Transfer type curable resin sheet, coating method, vehicle and vehicle component
The transfer-type curable resin sheet with angled protrusions and controlled peel strength addresses the issues of peeling and damage in decorative films, providing a seamless paint finish on three-dimensional surfaces.
Patent Information
- Application Number
- JP2024057103
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-15
AI Technical Summary
Decorative films used in painting and decoration often peel off at unintended interfaces, fail to follow three-dimensional shapes, and are prone to peeling or lifting, risking damage to the paint layer during removal.
A transfer-type curable resin sheet with a paint layer containing a curable resin composition and a transfer layer with thermoplastic resin, featuring protrusions angled at 30° or more, and a peel strength ratio of 0.5 or less between the transfer and paint layers, allowing for damage-free peeling.
The resin sheet enables seamless peeling of the transfer layer without damaging the paint layer, ensuring a smooth, intact decorative finish on complex surfaces.
Smart Images

Figure 2024146909000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a transfer-type curable resin sheet used for painting, a painting method using the transfer-type curable resin sheet, and a vehicle and vehicle part painted using the transfer-type curable resin sheet or by the painting method. [Background technology]
[0002] Furniture, steel plates, vehicle bodies, and the like are painted or decorated from the viewpoint of design and durability. It is known that decoration is performed using a film such as a decorative film. A decorative film is generally provided with a protective layer for protecting a resin layer for decoration and a release layer that serves as a base material when transferring the resin layer, and the resin layer is transferred to an object while peeling off the release layer and protective layer. In addition, in order to improve design and durability, the resin layer may have a multi-layer structure of two or more layers.
[0003] As described above, decorative films are composed of many layers, and therefore, when the protective layer or release layer is peeled off, it may peel off at an unintended interface, making application difficult. In addition, when the film is attached to an object having a three-dimensional shape, it may not be able to sufficiently follow the shape of the object. Furthermore, decorative films are generally attached to objects using an adhesive layer, and peeling or lifting from the object often occurs.
[0004] For example, Patent Document 1 discloses a transfer sheet as a decorative film, in which a releasable support, a peeling layer, a decorative layer, an adhesive layer, and a peeling film are laminated in this order. In this transfer sheet, the peeling layer contains an adhesive and either an ionizing radiation curable resin or a curable resin, and the peel strength between the releasable support and the peeling layer is greater than the peel strength between the release film and the adhesive layer. In addition, the transfer film is irradiated with ionizing radiation or heated before the releasable support is peeled off, thereby reducing the peel strength between the releasable support and the peeling layer. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2019-048426 A Summary of the Invention [Problem to be solved by the invention]
[0006] The decorative film described in Patent Document 1 has the peel strength between the releasable support and the release film adjusted as described above, which makes it possible to prevent unintended peeling at the interface when peeling off the releasable support or the release film. However, according to the method of Patent Document 1, after the decorative film is attached to the adherend, when the releasable support and the release film are peeled off, the decorative layer may be scratched by hand and damaged.
[0007] Therefore, an object of the present invention is to provide a transfer-type curable resin sheet that can peel off a transfer layer without damaging the paint layer, a painting method using the transfer-type curable resin sheet, and a vehicle and vehicle part that has been painted using the transfer-type curable resin sheet or by the painting method. [Means for solving the problem]
[0008] As a result of intensive research, the present inventors have found that the above-mentioned problems can be solved by providing a protrusion on the transfer type curable resin sheet and adjusting the peel strength of the transfer type curable resin sheet so as to satisfy a predetermined relationship, and have completed the present invention. [1] A transfer-type curable resin sheet comprising a paint layer containing a curable resin composition that can be cured by heat, active energy rays, or moisture, and a transfer layer containing a thermoplastic resin provided on one side of the paint layer, wherein the transfer-type curable resin sheet comprises a main body and a protrusion protruding in a planar direction from the main body, the protrusion having an inclined portion inclined at an angle of 30° or more with respect to the main body, and wherein the ratio (A / B) of the peel strength A (N / 25 mm) at the interface between the transfer layer and the paint layer to the peel strength B (N / 25 mm) at the interface between a coated steel plate test piece and the paint layer is 0.5 or less. [2] The transfer type curable resin sheet described in [1] above, wherein the protrusions are bent at an angle of 30° or more by shaping. [3] The transfer type curable resin sheet according to the above [2], wherein the protrusions are folded toward the transfer layer. [4] The transfer type curable resin sheet described in [1] above, wherein the protrusion has the inclined portion when attached to an object to be coated. [5] The transfer type curable resin sheet described in [4] above, wherein the inclined direction of the protrusions is toward the paint layer side. [6] The transfer type curable resin sheet according to any one of the above [1] to [5], wherein a peel strength A of the interface between the transfer layer and the paint layer is 2 N / 25 mm or less. [7] The transfer type curable resin sheet according to any one of the above [1] to [6], wherein the transfer layer has a loop stiffness of 0.05 to 1.0 N / 20 mm. [8] The transfer type curable resin sheet according to any one of the above [1] to [7], wherein the paint layer includes a clear layer that does not contain a colorant, and a color layer that contains a colorant and is provided on the opposite side of the clear layer from the transfer layer. [9] The transfer type curable resin sheet according to any one of the above [1] to [8], wherein the curable resin composition contains a (meth)acrylic resin (A) and a blocked isocyanate (B).
[10] The transfer type curable resin sheet according to any one of the above [1] to [9], which has a gel fraction of 50% or less.
[11] The transfer type curable resin sheet according to any one of the above [1] to
[10] , wherein the transfer layer contains at least one resin selected from the group consisting of cyclic olefin resin, polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polyvinyl chloride (PVC) resin, acrylonitrile-butadiene-styrene copolymer (ABS), polyethylene (PE) and polypropylene (PP).
[12] The transfer type curable resin sheet according to any one of the above [1] to
[11] , which is shaped into a three-dimensional shape.
[13] A coating method comprising the steps of attaching the transfer type curable resin sheet according to any one of the above [1] to
[12] to an object to be coated, and peeling the transfer layer from the object to be coated at the protrusions.
[14] The coating method described in
[13] above, wherein the transfer type curable resin sheet is attached to an object to be coated so as to form an inclined portion that is inclined at an angle of 30° or more relative to the main body portion.
[15] The coating method according to
[13] or
[14] above, further comprising a step of, after attaching the transfer type curable resin sheet to an object to be coated, wrapping the protrusion around to the back of the object to be coated.
[16] A vehicle painted using the transfer type curable resin sheet according to any one of [1] to
[12] above.
[17] A vehicle part coated with the transfer type curable resin sheet according to any one of the above [1] to
[12] .
[18] A vehicle painted by the painting method described in any one of
[13] to
[15] above.
[19] A vehicle part coated by the coating method according to any one of
[13] to
[15] above. Effect of the Invention
[0009] According to the present invention, it is possible to provide a transfer-type curable resin sheet that can peel off a transfer layer without damaging a paint layer, a coating method using the transfer-type curable resin sheet, and a vehicle and vehicle part that is coated with the transfer-type curable resin sheet or coated by the coating method. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1(a) is a plan view of a transfer type curable resin sheet according to a first embodiment of the present invention, and FIG. 1(b) is a cross-sectional view taken along line AA of FIG. 1(a). [Diagram 2] FIG. 2 is a diagram showing a modified example of the transfer type curable resin sheet according to the first embodiment of the present invention. [Diagram 3] FIG. 3 is a diagram showing a modified example of the transfer type curable resin sheet according to the first embodiment of the present invention. [Figure 4] 4(a) to (d) are diagrams illustrating a coating method using the transfer type curable resin sheet according to the first embodiment of the present invention. [Diagram 5] 5(a) and (b) are diagrams showing a transfer type curable resin sheet according to a second embodiment of the present invention. [Figure 6] 6(a) to (d) are diagrams illustrating a coating method using a transfer type curable resin sheet according to a second embodiment of the present invention. [Figure 7] FIG. 7(a) is a plan view of a modified example of the transfer type curable resin sheet of the first embodiment of the present invention, and FIG. 5(b) is a cross-sectional view taken along line AA of FIG. 5(a). [Figure 8] 8(a) and (b) are plan views of modified examples of the transfer type curable resin sheets of the first and second embodiments of the present invention. [Figure 9] FIG. 9 is a plan view of a modified example of the transfer type curable resin sheet according to the first and second embodiments of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] <First embodiment> [Transfer-type curable resin sheet] Hereinafter, the transfer type curable resin sheet according to the first embodiment of the present invention will be described with reference to FIG. 1. The transfer type curable resin sheet 1 according to the first embodiment of the present invention comprises a paint layer 10 containing a curable resin composition that can be cured by heat, active energy rays, or moisture, and a transfer layer 20 containing a thermoplastic resin provided on one surface of the paint layer 10. In this embodiment, the transfer type curable resin sheet 1 comprises a main body 2 and a protrusion 3 protruding from the main body 2 in the planar direction, and the protrusion 3 has an inclined portion inclined at an angle θ of 30° or more toward the transfer layer 20 side with respect to the main body 2. In addition, in this specification, the inclined portion also includes a shape bent at 90° or 180° with respect to the surface S. In addition, the ratio (A / B) of the peel strength A (N / 25mm) at the interface between the transfer layer 20 and the paint layer 10 to the peel strength B (N / 25mm) at the interface between the coated steel plate test piece and the paint layer 10 is 0.5 or less. With the above configuration, the transfer layer can be peeled off without damaging the paint layer.
[0012] (Paint layer) The paint layer 10 contains a curable resin composition that can be cured by heat, active energy rays, or moisture. The curable resin composition may contain a curable resin that can be cured by heat, active energy rays, or moisture, but preferably contains a thermosetting resin that can be cured by heat. The curable resin composition may also contain an active energy ray-curable resin that can be cured by active energy rays, or a moisture-curable resin that can be cured by moisture. The curable resin is not particularly limited, but examples thereof include (meth)acrylic resin, polycarbonate resin, polyester resin, and epoxy resin, and among these, (meth)acrylic resin is preferred.
[0013] In the case of a thermosetting resin, the curable resin composition preferably contains a curing agent. The curing agent is not particularly limited, but is preferably an isocyanate compound, and more preferably a blocked isocyanate. On the other hand, in the case of a curable resin being an active energy ray curable resin or a moisture thermosetting resin, the curable resin composition does not need to contain a curing agent. Therefore, it is preferable that the curable resin composition for the paint layer 10 contains a (meth)acrylic resin and a blocked isocyanate. By containing a (meth)acrylic resin and a blocked isocyanate, the paint layer 10 is more likely to have the desired flexibility, and it is easier to improve the adhesion and adhesive strength to the object to be coated. In addition, it is easier to achieve high hardness after curing by heat curing, and the scratch resistance of the cured paint is also improved.
[0014] The (meth)acrylic resin used in the curable resin composition may be a (meth)acrylic resin having a plurality of functional groups. The functional group is a group capable of reacting with heat, active energy rays, or moisture. When the (meth)acrylic resin is a thermosetting resin, the functional group is preferably a functional group that reacts with a reactive group (e.g., an isocyanate group) contained in the curing agent, specifically, a hydroxyl group, an amino group, a carboxyl group, etc. The (meth)acrylic resin may have only one type of functional group, or may have two or more types. Among these, the (meth)acrylic resin preferably has a hydroxyl group. Therefore, the (meth)acrylic resin preferably contains a (meth)acrylic polyol having a plurality of hydroxyl groups. Furthermore, when the (meth)acrylic resin is an active energy ray-curable resin, examples of the group capable of reacting with active energy rays include groups having a reactive double bond, such as a (meth)acryloyl group.
[0015] In the case of a thermosetting resin, the (meth)acrylic resin is preferably an acrylic polymer obtained by polymerizing a monomer mixture containing a (meth)acrylic acid ester monomer and a functional group-containing monomer having the above-mentioned functional group such as a hydroxyl group, an amino group, or a carboxyl group. The monomer mixture may also contain monomers other than the (meth)acrylic acid ester monomer and the functional group-containing monomer, such as a styrene derivative monomer. Note that (meth)acrylic means methacryl or acrylic, and the same applies to other similar terms.
[0016] Examples of the (meth)acrylic acid ester monomer include (meth)acrylic acid ester monomers that do not have the above-mentioned functional group, such as alkyl (meth)acrylates having an alkyl group with about 1 to 18 carbon atoms, (meth)acrylates having an aromatic ring such as benzyl (meth)acrylate and phenoxydiethylene glycol (meth)acrylate, and 2-ethoxyethyl (meth)acrylate. Examples of functional group-containing monomers include (meth)acrylic acid ester monomers having a hydroxyl group such as 2-hydroxyethyl (meth)acrylate, (meth)acrylic acid ester monomers having an amino group such as 2-aminoethyl (meth)acrylate, and (meth)acrylic acid. Furthermore, as the (meth)acrylic resin, a copolymer obtained by block or graft polymerization of the above-mentioned acrylic polymer with another monomer or polymer may be used. Furthermore, as the (meth)acrylic resin, a (meth)acryloyl group may be contained in the acrylic polymer by reacting a (meth)acryloyl group-containing compound having a reactive group capable of reacting with the functional group and a (meth)acryloyl group with the functional group of the above-mentioned acrylic polymer.
[0017] The curable resin composition preferably contains, as the (meth)acrylic resin, a (meth)acrylic resin having a weight average molecular weight (Mw) of 50,000 or more and 1,000,000 or less, which is solid and has a plurality of functional groups (hereinafter also referred to as a high molecular weight (meth)acrylic resin). By containing a (meth)acrylic resin having a weight average molecular weight within the above range, it becomes easier to maintain the paint layer in a certain shape even before curing, and it becomes easier to properly form it on a transfer layer or the like. In addition, it becomes easier to impart tackiness and extensibility to the paint layer. By having tackiness and extensibility, the paint layer has good shape followability during vacuum molding, and color unevenness is also less likely to occur. Furthermore, when the weight average molecular weight is within the above range, it becomes easier to increase the hardness of the resin layer after curing. The weight average molecular weight is preferably 100,000 or more and 500,000 or less, more preferably 120,000 or more and 400,000 or less. In this specification, the weight average molecular weight (Mw) is measured by gel permeation chromatography (GPC) and is calculated as a standard polystyrene equivalent value. In addition, being solid means being solid at room temperature (23°C) and normal pressure (1 atm).
[0018] The high molecular weight (meth)acrylic resin is preferably a (meth)acrylic polyol having a plurality of hydroxyl groups. As described above, the (meth)acrylic polyol can be obtained, for example, by polymerizing a monomer mixture containing a (meth)acrylic acid ester monomer and a hydroxyl group-containing monomer. In the curable resin composition, the (meth)acrylic resin may be used alone or in combination of two or more kinds.
[0019] The content of the (meth)acrylic resin in the paint layer 10 relative to the total amount of the paint layer is not particularly limited, but is, for example, 15 mass% or more, preferably 18 mass% or more, and more preferably 22 mass% or more. By containing a certain amount or more of the (meth)acrylic resin, the paint layer 10 is easily able to improve the coatability, curability, etc. of the paint layer 10, and can also be prevented from becoming too flexible. The content of the (meth)acrylic resin in the coating layer 10 is not particularly limited, but is, for example, 75 mass % or less, preferably 65 mass % or less, and more preferably 55 mass % or less. By making the content of the (meth)acrylic resin equal to or less than the upper limit, it becomes easier to impart the desired curability by containing a plasticizing resin and a curing agent described below in a predetermined amount or more.
[0020] The curable resin composition may contain, as the curable resin, a resin having a weight average molecular weight of less than 50,000 (hereinafter also referred to as a plasticizing resin) in addition to the high molecular weight (meth)acrylic resin described above. The curable resin composition contains a plasticizing resin having a low weight-average molecular weight in addition to a high molecular weight (meth)acrylic resin, which makes it easier to achieve a good balance between coatability, curability, tackiness, extensibility, etc. Also, the wettability to the substrate can be improved, thereby increasing the adhesive strength to the substrate.
[0021] The plasticizing resin is preferably one that is compatible with the high molecular weight (meth)acrylic resin and has a functional group that is heat curable, active energy ray curable, or moisture curable. Examples of the resin used for the plasticizing resin include (meth)acrylic resin, polycarbonate resin, polyester resin, and epoxy resin, and among these, (meth)acrylic resin or polycarbonate resin is preferred. The (meth)acrylic resin used as the plasticizing resin may be an oligomer having a functional group such as a hydroxyl group, an amino group, or a carboxyl group in the case of a thermosetting resin. The (meth)acrylic resin used as the plasticizing resin may be, for example, as described above in the (meth)acrylic resin, and preferably, a (meth)acrylic polyol having a plurality of hydroxyl groups is used. Poly(meth)acrylate having a carboxyl group is also preferred. As the polycarbonate resin, polycarbonate polyol is preferred. On the other hand, in the case of active energy ray curing, the plasticizing resin may be a resin having a group with a reactive double bond such as a (meth)acryloyl group (preferably a (meth)acrylic resin). The weight average molecular weight of the plasticizing resin is preferably 450 or more and 30,000 or less, and more preferably 1000 or more and 20,000 or less. Moreover, it is desirable for the plasticizing resin to be liquid at room temperature and pressure. The plasticizing resin is preferably at least one of a (meth)acrylic polyol having a plurality of hydroxyl groups and a polycarbonate polyol.
[0022] The content of the plasticizing resin in the paint layer 10 relative to the total amount of the paint layer is not particularly limited, but is, for example, 2% by mass or more, preferably 5% by mass or more, more preferably 6% by mass or more, and is, for example, 35% by mass or less, preferably 30% by mass or less, more preferably 25% by mass or less. When the paint layer 10 contains a certain amount or more of the plasticizing resin, the glass transition temperature of the paint layer 10 is easily lowered. Furthermore, when the content of the plasticizing resin is set to be equal to or more than the lower limit value and equal to or less than the upper limit value, various performances are easily balanced and favorable. Furthermore, the wettability to the coated object is improved, and the peel strength to the coated object is easily increased.
[0023] In addition, when the curable resin is a moisture-curable resin, the following moisture-curable resin may be used instead of the curable resin described above. Examples of moisture-curable resins include prepolymers having an isocyanate group at the end. Examples of prepolymers having an isocyanate group at the end include those obtained by reacting polyisocyanate with an active hydrogen-containing compound and / or an active hydrogen-containing polymer. Examples of the polyisocyanate used in preparing the prepolymer having an isocyanate group at its terminal include tolylene diisocyanate, crude tolylene diisocyanate, diphenylmethane diisocyanate, polymethylene polyphenyl isocyanate, carbadiimidized diphenylmethane diisocyanate, phenylene diisocyanate, 1,5-naphthalene diisocyanate, xylylene diisocyanate, and hexamethylene diisocyanate. Polymethylene polyphenyl isocyanate is preferably used.
[0024] As the above-mentioned active hydrogen-containing compound and active hydrogen-containing polymer, for example, the following are used. Active hydrogen-containing compounds such as ethylene glycol, diethylene glycol, propylene glycol, dipropylene glycol, glycerin, trimethylolethane, trimethylolpropane, castor oil, diglycerin, sorbitol, pentaerythritol, and dipentaerythritol, and active hydrogen-containing polymers having two or more terminal hydroxyl groups and an average molecular weight of 3,000 or less, an average functional group number of 2 or more, preferably an average molecular weight of 200 to 1,000, and an average functional group number of 2 to 2.5, obtained by addition polymerization of the above-mentioned active hydrogen-containing compounds and alkylene oxides such as ethylene oxide, propylene oxide, butylene oxide, styrene oxide, and tetrahydrofuran, alone or in combination, are used. Other active hydrogen-containing polymers that can be used in combination include polyester polyols, oil-modified polyester polyols, polyε-caprolactone polyols, polycarbonate diols, acrylic polyols, polyamines, polyamides, urea resins, and melamine resins, and have an average molecular weight of 3,000 or less and an average number of functional groups of 1.5 or more, and preferably an average molecular weight of 200 to 1,000 and an average number of functional groups of 2 to 2.5. The prepolymer having a terminal isocyanate group has, for example, an effective NCO content of 1 to 15 mass %, preferably 8 to 13 mass %.
[0025] The prepolymer having a terminal isocyanate group can be synthesized by carrying out a urethane reaction of the above-mentioned polyisocyanate and a conventional polyol including the above-mentioned active hydrogen-containing polymer under conditions of excess isocyanate at a temperature of 40°C to 90°C, preferably 55°C to 75°C, in a system that is kept away from moisture.
[0026] The above-mentioned urethane reaction is usually carried out in an organic solvent, and examples of such solvents include ketone-based solvents such as methyl ethyl ketone, ester-based solvents such as ethyl acetate, aromatic solvents such as toluene and xylene, and other solvents generally used for paints. The urethane reaction can also be carried out using a catalyst, and examples of such catalysts include tertiary amine-based catalysts such as triethylamine and dimethylaniline, and metal-based catalysts such as tin and zinc. These also serve as catalysts when reacting with moisture in the air during coating film formation.
[0027] The blocked isocyanate used as a curing agent is a compound in which an isocyanate group is blocked with a protecting group, and when exposed to high temperatures, the protecting group (blocking portion) is thermally dissociated and removed, causing a curing reaction between the resulting isocyanate group and the functional group in the curable resin (typically, a hydroxyl group in a polyol). The blocked isocyanate can be obtained, for example, by reacting an isocyanate compound having two or more isocyanate groups in one molecule with a blocking agent. The isocyanate compound having two or more isocyanate groups in one molecule is not particularly limited, but examples thereof include tolylene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, pentamethylene diisocyanate, isophorone diisocyanate, xylylene diisocyanate, hydrogenated xylylene diisocyanate, and modified products thereof. Examples of blocking agents include pyrazoles, phenols, oximes, lactams, and malonic acid esters. The content of the blocked isocyanate in the curable resin composition is preferably adjusted so that the ratio of the number of functional groups in the curable resin to the number of isocyanate groups in the blocked isocyanate is preferably 0.4 to 1.8, more preferably 0.6 to 1.5.
[0028] The content of the blocked isocyanate in the coating layer 10 relative to the total amount of the coating layer is not particularly limited, but is, for example, 15% by mass or more, preferably 20% by mass or more, more preferably 25% by mass or more, and is, for example, 65% by mass or less, preferably 60% by mass or less, more preferably 55% by mass or less. By making the content of the blocked isocyanate equal to or more than the lower limit, it becomes easier to lower the glass transition temperature while improving the curability. In addition, by making it equal to or less than the upper limit, it is possible to prevent the glass transition temperature from being lowered more than necessary and various physical properties from being deteriorated.
[0029] The curable resin composition for the paint layer 10 may contain, in addition to the curable resin and curing agent, appropriate components according to the performance required for the coating formed from the paint layer 10. For example, when the coating formed from the paint layer 10 is to be a colored coating, a colorant such as a pigment, dye, or luster material may be contained to make the paint layer 10 a colored layer. When the coating formed from the paint layer 10 is to be a heat-shielding coating, a heat-shielding material may be contained in the curable resin composition to make the paint layer 10 a heat-shielding layer. The paint layer 10 may also be made of a clear layer, which will be described later. Among these, it is preferable that the curable resin composition contains at least a colorant.
[0030] Examples of pigments used in the colorant include, but are not limited to, metal oxide pigments such as titanium oxide and iron oxide; inorganic pigments such as carbon black, clay, kaolin, barium sulfate, barium carbonate, calcium carbonate, talc, silica, and alumina white; and organic pigments such as azo pigments, quinacridone pigments, diketopyrrolopyrrole pigments, perylene pigments, perinone pigments, benzimidazolone pigments, vat pigments, isoindoline pigments, isoindolinone pigments, metal chelate azo pigments, phthalocyanine pigments, indanthrone pigments, dioxane pigments, and indigo pigments. As the dye, known dyes can be used, and examples of the dye include azo dyes, anthraquinone dyes, indigoid dyes, and stilbene dyes. The lustrous material is a compound capable of imparting lustrous properties to the paint layer 10 and imparting the property of exhibiting luster when observed from multiple directions. The lustrous material is not particularly limited, but examples thereof include compounds in which a titanium oxide layer is provided on the surface of natural mica, synthetic mica, alumina flakes, glass flakes, etc. The paint layer 10 preferably contains at least one of a pigment or a luster material as a colorant, and more preferably contains a pigment. The paint layer 10 also preferably contains both a pigment and a luster material. The content of the colorant in the curable resin composition is not particularly limited, but is, for example, based on the solid content, 0.5 mass % or more, preferably 1 mass % or more, more preferably 2 mass % or more, and preferably 25 mass % or less, more preferably 20 mass % or less, and even more preferably 12 mass % or less. In addition to the colorant and the heat-shielding material, the curable resin composition may appropriately contain additives such as an inorganic filler, a curing catalyst, a curing accelerator, a surface conditioner, an antifoaming agent, a crosslinking agent, a dispersant, an antiaging agent, an antioxidant, a rust inhibitor, and a flame retardant.
[0031] The thickness of the paint layer 10 is not particularly limited, but is, for example, from 10 μm to 200 μm, and preferably from 20 μm to 100 μm.
[0032] (Transfer layer) The transfer layer 20 in the transfer type curable resin sheet 1 is a member that protects the paint layer 10 from scratches and adhesion of foreign matter, and also serves as a support when the paint layer 10 is attached to an object to be coated 30 (see FIG. 4). The transfer layer 20 is preferably formed from a resin film. The resin used for the resin film is a thermoplastic resin. Specific examples of resins used in the resin film include cyclic polyolefin resins, polyolefin resins, polyester resins such as polybutylene terephthalate (PBT) and polyethylene terephthalate (PET), polyamide resins, polycarbonate resins, acrylic resins, fluororesins, polyvinyl chloride resins (PVC) such as soft vinyl chloride resins, polymethylpentene resins, tetrafluoroethylene resins, and acrylonitrile-butadiene-styrene copolymer (ABS) resins. Cyclic polyolefin resins are polymers containing structural units derived from cyclic olefins. Polyolefin resins are polyolefin resins other than cyclic polyolefin resins, specifically, polypropylene resins (PP) and polyethylene resins (PE). Polyethylene resins include low-density polyethylene, medium-density polyethylene, high-density polyethylene, linear low-density polyethylene (LLDPE), and the like. These resins may be used alone or in combination of two or more. Among these resins, cyclic olefin resins, PET, PBT, PVC, ABS, PE and PP are preferred from the viewpoints of vacuum moldability and transferability.
[0033] At least one surface of the transfer layer 20 may be release-treated with a release agent such as a silicone-based release agent, a fluorine-based release agent, etc. When the transfer layer 20 is release-treated, it is preferable that the release-treated surface constitutes the surface on the paint layer 10 side. However, the transfer layer 20 does not need to be release-treated as long as it can be peeled off from the paint layer 10. The thickness of the transfer layer 20 is not particularly limited, but is, for example, 10 μm or more and 1000 μm or less, preferably 20 μm or more and 600 μm or less, and more preferably 30 μm or more and 400 μm or less.
[0034] The loop stiffness of the transfer layer 20 is preferably 0.05 to 1.0 N / 20 mm. When the loop stiffness of the transfer layer 20 is 0.05 N / 20 mm or more, the transfer type curable resin sheet 1 has an inclined portion, so that a restoring force is appropriately generated, and the transfer layer 20 is easily peeled off from the paint layer 10. When the loop stiffness of the transfer layer 20 is 1.0 N / 20 mm or less, the transfer type curable resin sheet 1 is easily handled. From this viewpoint, the loop stiffness of the transfer layer 20 is more preferably 0.06 to 0.8 N / 20 mm, and further preferably 0.07 to 0.6 N / 20 mm. The loop stiffness is a physical property related to the rigidity of a film. The loop stiffness of the transfer layer 20 can be measured by the method described in the examples below. The loop stiffness of the transfer layer 20 can be adjusted by the thickness of the transfer layer 20, the type of resin constituting the transfer layer 20, and the like.
[0035] (Main body) After the main body 2 of the transfer type curable resin sheet 1 in the first embodiment of the present invention is attached to an object to be coated, the transfer layer 20 is peeled off, thereby coating the object.
[0036] (protrusion) The protrusions 3 of the transfer curable resin sheet 1 in the first embodiment of the present invention protrude from the main body 2 in the planar direction, and are formed as inclined parts by shaping and trimming in advance to an angle θ of 30° or more toward the transfer layer 20 side with respect to the main body 2. Here, the angle θ is specifically the angle between a virtual surface S formed by extending the surface 112 (i.e., the surface to be attached to the object to be coated) opposite the surface of the transfer layer side of the paint layer 10 in the main body 2 along the surface 112 toward the protrusion side, and a surface 113 opposite the surface of the paint layer 10 in the protrusion 3 toward the transfer layer side. If the angle θ is less than 30°, the restoring force generated by the inclined part does not act sufficiently, making it difficult to peel the transfer layer 20 from the paint layer 10 at the protrusion 3, and there is a risk of damaging the paint layer 10 when peeling the transfer layer 20 from the paint layer 10. From this viewpoint, the angle θ of the protrusion 3 relative to the main body 2 is preferably 40° or more, more preferably 60° or more, and even more preferably 70° or more. The angle θ of the protrusion 3 relative to the main body 2 may be 180° or less, but is preferably 150° or less, more preferably 120° or less, and even more preferably 90° or less. As the angle becomes larger, the restoring force becomes larger, but from the viewpoint of ease of molding by vacuum molding or the like, it is preferable that the angle be 90° or less. The protrusions 3 can be formed by, for example, cutting, laser processing, or the like. The protrusions 3 may be molded into a bent shape by molding. The molding may be performed by thermoforming such as vacuum molding, compressed air molding, and press molding. In addition, it is preferable that not only the protrusions 3 but also the main body 2 of the transfer type curable resin sheet 1 are shaped to correspond to the shape of the object to be coated.
[0037] The length of the protrusion 3 in the direction protruding from the main body is not particularly limited as long as the protrusion 3 can be peeled off by pinching it with fingers or a peeling device, but is preferably 5 to 50 mm, and more preferably 7 to 30 mm. The length of the protrusion 3 in the direction perpendicular to the direction protruding from the main body, i.e., the width of the protrusion 3, is not particularly limited as long as the protrusion 3 can be peeled off by pinching it with fingers or a peeling device, but is preferably 5 to 50 mm, and more preferably 7 to 30 mm.
[0038] The protrusions 3 of the transfer-type curable resin sheet 1 in the first embodiment of the present invention may be folded two or more times by shaping. For example, as shown in Fig. 2, the protrusions 3 of the transfer-type curable resin sheet 1 may be folded twice by shaping. In this case, the angle θ of the inclined portion is the angle of the folded portion located farthest from the main body portion 2 as shown in Fig. 2.
[0039] (peel strength) In the transfer type curable resin sheet 1 in the first embodiment of the present invention, the ratio (A / B) of the peel strength A (N / 25 mm) at the interface between the transfer layer 20 and the paint layer 10 to the peel strength B (N / 25 mm) at the interface between the coated steel plate test piece and the paint layer 10 is 0.5 or less. If the peel strength ratio (A / B) is greater than 0.5, when the transfer layer 20 is peeled off from the paint layer starting from the protrusion 3 after the transfer type curable resin sheet 1 is attached to the paint layer, the paint layer 10 may peel off together. From this viewpoint, the peel strength ratio (A / B) is preferably 0.45 or less, more preferably 0.1 or less, even more preferably 0.05 or less, and even more preferably 0.02 or less. The lower limit of the range of the peel strength ratio (A / B) is not particularly limited, but is, for example, 0.001, preferably 0.005. The peel strength can be measured by the method described in the examples described later. The above peel strength ratio (A / B) can be appropriately adjusted, for example, by the composition of the resin in the transfer layer and the composition of the resin in the paint layer.
[0040] In the transfer type curable resin sheet 1 in the first embodiment of the present invention, the peel strength A of the interface between the transfer layer 20 and the paint layer 10 is preferably 2N / 25mm or less. If the peel strength A of the interface between the transfer layer 20 and the paint layer 10 is 2N / 25mm or less, the transfer layer 20 can be easily peeled off from the paint layer 10 after the transfer type curable resin sheet 1 is attached to the object to be coated. From this viewpoint, the peel strength A of the interface between the transfer layer 20 and the paint layer 10 is more preferably 1.5N / 25mm or less, more preferably 1.0N / 25mm or less, and even more preferably 0.8N / 25mm or less. From the viewpoint of suppressing the transfer layer 20 from peeling off from the paint layer 10 before attaching the transfer type curable resin sheet 1 to the object to be coated, the peel strength A of the interface between the transfer layer 20 and the paint layer 10 is preferably 0.05N / 25mm or more, more preferably 0.1N / 25mm or more, and even more preferably 0.15N / 25mm or more. The peel strength can be measured by the method described in the Examples below. The peel strength can be appropriately adjusted by the composition of the resin in the transfer layer, the composition of the resin in the paint layer, and the like.
[0041] (Gel fraction) The gel fraction of the transfer curable resin sheet in the first embodiment of the present invention is preferably 50% or less. When the gel fraction of the transfer curable resin sheet is 50% or less, the adhesion of the transfer curable resin sheet to the object to be coated is further improved. From this viewpoint, the gel fraction of the transfer curable resin sheet in the first embodiment of the present invention is more preferably 40% or less, and further preferably 30% or less. The lower limit of the range of the gel fraction of the transfer curable resin sheet in the first embodiment of the present invention is not particularly limited and may be 0%. The gel fraction of the transfer curable resin sheet can be measured by the method described in the examples below. The gel fraction of the transfer curable resin sheet can be adjusted by the heating conditions when curing the paint layer in the initial curing, the conditions for drying the paint layer, the irradiation conditions of active energy rays, and the environmental conditions of temperature and humidity.
[0042] (protective layer) The transfer type curable resin sheet according to the first embodiment of the present invention may further include a protective layer 40 provided on the side of the paint layer 10 opposite the transfer layer 20 side, as shown in FIG. 3. The protective layer 40 is a member that protects the paint layer 10 from scratches and adhesion of foreign matter. The protective layer 40 is preferably formed from a resin film. Specific examples of thermoplastic resins used in the protective layer 40 are the same as those usable in the transfer layer 20, and among these, polyester resins are preferred. The resin film forming the protective layer 40 may be a single-layer film consisting of one layer, or a multi-layer film consisting of two or more layers. The resin film used for the protective layer 40 may be a stretched resin film or a non-stretched resin film, but is preferably a non-stretched resin film. The protective layer 40 may have at least one surface that has been release-treated with a release agent such as a silicone-based release agent or a fluorine-based release agent. When the protective layer 40 is release-treated, it is preferable that the release-treated surface constitutes the surface on the paint layer 10 side. By being release-treated, the protective layer 40 is easily peeled off from the paint layer 10. However, the protective layer 40 does not need to be release-treated as long as it can be peeled off from the paint layer 10. The thickness of the protective layer 40 is not particularly limited, but is, for example, 10 μm or more and 1000 μm or less, preferably 30 μm or more and 700 μm or less, and more preferably 50 μm or more and 500 μm or less. It is advisable to peel and remove the protective layer 40 from the paint layer before attaching the transfer type curable resin sheet to the object to be coated.
[0043] (Method for manufacturing transfer type curable resin sheet) The method for producing the transfer type curable resin sheet in the first embodiment of the present invention is not particularly limited, but it is preferable to first prepare a curable resin composition for forming a paint layer, and then form a paint layer from the curable resin composition on the transfer layer. Here, when forming the paint layer on the transfer layer, it is preferable to apply the curable resin composition and dry it as necessary to form a resin layer. Moreover, a protective layer may be further laminated on the paint layer formed on the transfer layer. However, the paint layer does not need to be formed directly on the transfer layer. For example, a paint layer may be formed from a curable resin composition on a protective layer, and the paint layer with the protective layer formed thereon may be laminated to the transfer layer.
[0044] The curable resin composition is preferably diluted with a solvent from the viewpoint of improving workability such as coating property. Examples of the solvent include ethyl acetate, butyl acetate, toluene, etc. In addition, the drying performed after applying the curable resin composition on the transfer layer or the protective layer is preferably drying that includes at least the main drying step described later, and more preferably drying that performs the pre-drying step and the main drying step described later in this order.
[0045] The drying temperature in the pre-drying step is preferably 50° C. or more and 70° C. or less, and more preferably 55° C. or more and 65° C. or less. The drying time in the pre-drying step is preferably 1 minute or more and 30 minutes or less, and more preferably 2 minutes or more and 15 minutes or less. The drying temperature in this drying step is preferably 85° C. or higher and 130° C. or lower, and more preferably 90° C. or higher and 120° C. or lower. When the drying temperature is equal to or higher than these lower limits, the solvent is easily removed appropriately, and the solvent is prevented from evaporating and causing bubbles when the resin layer is cured. In addition, by setting the drying temperature to the upper limit or lower, the curable resin composition can be prevented from being cured more than necessary during drying. The drying time in this drying step is preferably 1 minute or more and 30 minutes or less, more preferably 2 minutes or more and 15 minutes or less. By setting the drying time to the above lower limit or more, the solvent is easily removed appropriately, and the solvent is prevented from evaporating and generating bubbles when the resin layer is cured. In addition, by setting the drying time to the above upper limit or less, the curable resin composition can be prevented from being cured more than necessary during drying.
[0046] In addition, the paint layer after drying may be subjected to initial curing as necessary. Initial curing refers to curing the curable resin composition constituting the paint layer to a semi-cured state. The initial curing can be performed, for example, by heating, and is preferably performed under conditions of a heating temperature of 90°C or higher and 150°C or lower, and a heating time of about 2 minutes or higher and 5 minutes or lower.
[0047] The laminate in which the paint layer, or the paint layer and the protective layer are laminated on the transfer layer, is preferably preformed and shaped into a three-dimensional shape by vacuum forming, press forming, compressed air forming, etc. The shaping may be performed to form the inclined portion as described above, but it is preferable to form the main body portion in a shape corresponding to the shape of the object to be coated by forming the inclined portion as well. By forming the main body of the transfer-type curable resin sheet into a three-dimensional shape, the transfer-type curable resin sheet can be easily adhered to the object to be coated, even if the object has a complex shape. Among the above methods, the preforming is preferably performed by vacuum forming. The preforming may be performed by pressing the laminate against a jig or a mold by vacuum forming, and shaping the laminate into a shape corresponding to the surface shape of the adherend while stretching the laminate by the jig or the mold. Here, the vacuum forming is preferably TOM forming. TOM stands for "Three dimension Overlay Method", and when TOM forming is applied, it is possible to form a complex shape.
[0048] (Painting method) The transfer type curable resin sheet in the first embodiment of the present invention is a sheet for forming a decorative body such as a coating on various articles (subjects to be coated), and is used by being attached to the subject to be coated. Specifically, the transfer type curable resin sheet in the first embodiment of the present invention is attached to the subject to be coated via a paint layer, and the transfer type curable resin sheet attached to the subject to be coated may be heated. The paint layer is cured by heating the transfer type curable resin sheet, and the decorative body is formed by the cured paint layer. In addition, the transfer layer is peeled off from the paint layer after the transfer curable resin sheet is attached to the substrate via the paint layer, so that the transfer layer serves as a support for the paint layer when the transfer curable resin sheet is attached to the substrate. Furthermore, the transfer layer may be peeled off at room temperature or at a temperature close to room temperature (about 15 to 35° C.), but may also be peeled off after the coating layer has been cooled. When a protective layer is provided on the transfer type curable resin sheet, it is advisable to peel off the protective layer before attaching the sheet to the object to be coated.
[0049] A coating method using the transfer type curable resin sheet 1 in the first embodiment of the present invention is shown in Fig. 4. Hereinafter, the coating method will be described in more detail with reference to Fig. 4. As shown in Fig. 4(a), the main body 2 of the transfer type curable resin sheet 1 is attached to the object 30 via the paint layer 10. At this time, the attachment of the main body 2 to the object 30 is not particularly limited, and may be performed by hand attachment using a squeegee or the like, or may be performed using a laminating device. At this time, since the protrusions 3 have inclined portions, they tend to be positioned at a position separated from the object 30 as shown in Fig. 4(a), but it is preferable to hold down the protrusions 3 and attach them to the object 30 as shown in Fig. 4(b).
[0050] Next, the transfer layer 20 of the protrusion 3 is pinched and the transfer layer 20 is peeled off. At this time, the transfer layer 20 of the protrusion 3 naturally peels off before being pinched, or easily peels off from the paint layer 10, due to the restoring force of the transfer layer 20 trying to return to its bent state, as shown in Fig. 4(c). Therefore, the transfer layer 20 of the main body 20 can also be easily peeled off, using the peeled transfer layer 20 of the protrusion 3 as the peeling starting point.
[0051] The temperature at which the transfer layer 20 is peeled off is not particularly limited, and may be room temperature or a temperature around it, but may be performed after cooling the paint layer 10. Cooling the paint layer 10 hardens the paint layer 10, and in particular, cooling the paint layer 10 to a temperature below the glass transition temperature makes the paint layer 10 even harder, making it easier to peel the transfer layer 20 from the paint layer 10 without causing peeling problems. The temperature of the paint layer 10 when it is cooled and peeled off is preferably at least the glass transition temperature or lower. Specifically, it is preferably 15° C. or lower, more preferably 10° C. or lower, and even more preferably 5° C. or lower. In addition, the temperature of the paint layer 10 when it is cooled and peeled off is preferably a certain temperature or higher from the viewpoint of reducing energy and time loss, specifically, for example, −20° C. or higher, and preferably −10° C. or higher.
[0052] Of the paint layer 10 remaining after the transfer layer 20 has been peeled off, the paint layer 10 on the protrusion 3 may be removed, but does not have to be removed. For example, by arranging the paint layer 10 on the protrusion 3 in a portion that is difficult to see from the outside, it is possible to prevent the design from being impaired even if it is not removed.
[0053] The paint layer 10 attached to the substrate 30 may be cured by heating. The curing may be performed by heating the substrate 30 to which the paint layer 10 is attached using a heating device (not shown). The heating temperature is, for example, from 90° C. to 170° C., and preferably from 100° C. to 160° C. The heating time is, for example, from 5 minutes to 120 minutes, and preferably from 15 minutes to 90 minutes. The heating device for heating the paint layer 10 may be an oven, an infrared heater, or the like. The coating layer 10 may be cured before or after the transfer layer 20 is peeled off.
[0054] The paint layer 10 hardens by heating to become a decorative body laminated on the object to be coated. In the first embodiment of the present invention, as described above, the paint layer 10 is properly adhered to the object to be coated 30, and no peeling failure occurs when the transfer layer 20 is peeled off. Therefore, for example, peeling or floating does not occur at the interface between the object to be coated 30 and the paint layer 10, and a decorative body with good appearance can be obtained. In the above description, the paint layer attached to the substrate is heated to harden the paint layer. However, the paint layer may be hardened by irradiating the paint layer attached to the substrate with active energy rays, or by leaving the paint layer attached to the substrate in an environment of predetermined temperature and humidity.
[0055] The object to be coated to which the transfer type curable resin sheet of the first embodiment of the present invention is attached is not particularly limited, and examples thereof include electric appliances, vehicles such as automobiles and railways, vehicle parts, sundries, heavy machinery, ships, aircraft, and the like, exterior materials for houses and buildings, exterior walls or roofing materials, bridges, steel frames, plants, wind power generation blades, and the like. Examples of vehicle parts include vehicle interior materials and vehicle exterior materials. Among these, vehicles and vehicle parts are preferred, vehicle parts are more preferred, and vehicle exterior materials are even more preferred. Examples of vehicle exterior materials include aero parts, hoods, roofs, door panels, bumpers, fuel filler panels, trunk lids, rear gates, and the like. When the transfer type curable resin sheet is attached to a vehicle exterior material, it may be attached to the exterior material attached to the vehicle body, or it may be attached to the exterior material before being attached to the vehicle body. The material of the object to be coated is not particularly limited, and may be any of resin materials, inorganic materials such as ceramics, and metal materials such as steel, among which metal materials such as steel are preferred. Metal materials such as steel are difficult to coat simultaneously with molding of the object to be coated by insert molding, and coating with a resin sheet is difficult, but by using the transfer-type curable resin sheet of the first embodiment of the present invention, such materials can be easily coated.
[0056] <Second embodiment> In the transfer type curable resin sheet in the first embodiment of the present invention, the protrusions are bent at an angle of 30° or more with respect to the main body by forming or the like before being attached to the object to be coated, and an inclined portion is formed. However, in the second embodiment, when the transfer type curable resin sheet is attached to the object to be coated, the transfer layer of the protrusions is bent at an angle of 30° or more with respect to the main body, and has an inclined portion. The second embodiment will be described in detail below. Note that the parts different from the transfer type curable resin sheet in the first embodiment will be mainly described.
[0057] Before being attached, the protrusions 3 do not have an inclined portion inclined at an angle of 30° or more as shown in Fig. 5(a), but when attached to the object to be coated, they are bent to fit the shape of the object to be coated as shown in Fig. 5(b), and thus preferably have an inclined portion inclined at an angle θ of 30° or more relative to the main body. In this case, the protrusions 3 are preferably bent toward the paint layer 10 side when attached, as shown in Fig. 5(b). That is, in the second embodiment, the protrusions 3 are not shaped and may be arranged, for example, on the same plane as the main body 2 before being attached to the substrate 30, but may be bent at an angle of 30° or more toward the paint layer 10 when attached to the substrate 30 in accordance with the shape of the substrate 30. The protrusions, when attached to the substrate, may have an inclined portion that is inclined toward the paint layer and at an angle of 30° or more relative to the main body. The transfer curable resin sheet according to the second embodiment described above may be applied to the same coating method as in the first embodiment. In the second embodiment, the transfer layer 20 of the protrusion 3 may be pinched and peeled off, but at this time, the transfer layer 20 of the protrusion 3 naturally peels off before being pinched due to a restoring force that tries to return it to its original state, or it easily peels off from the paint layer 10. Therefore, the transfer layer 20 of the main body 20 can also be easily peeled off, using the peeled transfer layer 20 of the protrusion 3 as the peeling starting point.
[0058] In the second embodiment, the angle θ may be 30° or more, but is preferably 60° or more, more preferably 90° or more, even more preferably 120° or more, and even more preferably 150° or more. The angle θ is typically 180° or less, but may be greater than 180°, for example, 270° or less, depending on the shape of the workpiece.
[0059] In the second embodiment, as shown in Fig. 6, it is preferable to attach the protrusions 3 to the object to be coated by wrapping them around the back of the object. Although Fig. 6 shows an example in which the protrusions 3 are bent at 180°, when wrapping around the back, it is preferable to bend them at an angle greater than 90°. By wrapping the protrusions 3 around the back, a repulsive force is more likely to be generated. Also, since the protrusions 3 are positioned in a position that is difficult to see, the design can be improved.
[0060] For example, when the transfer type curable resin sheet 1C is used to paint the object 30, the transfer type curable resin sheet 1C may be attached to the object 30, and then the protrusions 3 may be wrapped around the back of the object 30, as shown in FIG. 6(a). As a result, as shown in FIG. 6(b), the transfer layer 20 of the protrusions 3 is easily peeled off from the paint layer 10 due to its high restoring force. Therefore, as shown in FIG. 6(c), the transfer layer 20 can be easily peeled off from the paint layer 10, with the transfer layer 20 of the protrusions 3 as the peeling starting point. In addition, as shown in FIG. 6(c), the end of the main body 2 can be arranged at the end of the object 30, so that the transfer type curable resin sheet 1C can be used to paint the object 30 up to the end.
[0061] In the second embodiment, as shown in FIG. 5(a), the protrusion portion 3 is exemplified as being arranged on the same plane as the main body portion 2 before being attached to the substrate, but it does not have to be arranged on the same plane, and may be shaped and bent before being attached as in the first embodiment.
[0062] [Variations] The transfer type curable resin sheets in the first and second embodiments of the present invention can be modified as follows. (Variation 1) In the transfer type curable resin sheets according to the first and second embodiments of the present invention, the paint layer is a single layer, but the paint layer may have a multi-layer structure of two or more layers. When the paint layer 10 has a multi-layer structure, each layer may be made of the above-mentioned curable resin composition. Each layer may contain a coloring agent to form a color layer, a heat-shielding material to form a heat-shielding layer, or a clear layer that does not substantially contain a coloring agent.
[0063] In the case of a multi-layer structure, the paint layer 10 preferably has at least a color layer and a clear layer. In the case of having a color layer and a clear layer, the paint layer 10 may include a clear layer 11 that does not contain a colorant, and a color layer 12 that contains a colorant and is provided on the opposite side of the clear layer 11 from the transfer layer 20 side, as in the transfer type curable resin sheet 1D shown in FIG. 7. By having the color layer 12, the paint layer 10 can color the object to be painted by the paint formed by the paint layer 10. Furthermore, by providing the clear layer 11 in addition to the color layer 12, the color layer 12 can be protected and glossy. The color layer 12 preferably contains a pigment as a coloring agent. In this case, the clear layer 11 is a layer that does not contain a pigment.
[0064] The color layer 12 and the clear layer 11 may both be made of the above-mentioned curable resin composition, and the curable resin composition for the color layer 12 may contain a colorant as described above. When a (meth)acrylic resin is used as the curable resin, the curable resin composition for the color layer 12 may contain at least a high molecular weight (meth)acrylic resin, but preferably contains both a high molecular weight (meth)acrylic resin and a plasticizing resin. On the other hand, the clear layer 11 is a transparent layer, and it is sufficient that the clear layer 11 has a transparency to such an extent that the color of the color layer 12 can be seen from the outside through the clear layer 11, and for example, the transmittance of light with a wavelength of 450 nm is preferably 80% or more. The clear layer 11 is preferably a coating film that does not contain a colorant, but may contain a small amount of a colorant as long as it does not impair its function. In addition, when a (meth)acrylic resin is used as the curable resin, the curable resin composition for the clear layer may contain at least a high molecular weight (meth)acrylic resin, and in that case, it may or may not contain a plasticizing resin.
[0065] Of course, when the paint layer 10 has a multi-layer structure, it is not limited to a two-layer structure of a clear layer and a color layer, and various laminated structures are possible, and a three-layer or more structure may be formed by providing two or more color layers and one or more clear layers, or a structure consisting of two color layers without the clear layer. Also, two or more clear layers may be provided. Also, a three-layer or more structure may be formed by providing a heat-shielding layer or the like between the clear layer and the color layer.
[0066] The thickness of the clear layer is not particularly limited, but is, for example, 10 μm to 100 μm, preferably 15 μm to 50 μm. The thickness of the color layer is not particularly limited, but is, for example, 10 μm to 100 μm, preferably 15 μm to 50 μm.
[0067] When the paint layer has a multi-layer structure, the paint layer may be formed by sequentially laminating resin layers on the transfer layer. Alternatively, at least one of the resin layers constituting the paint layer may be formed on the transfer layer, and at least one of the resin layers constituting the paint layer may be formed on the protective layer, and the transfer layer having the resin layer and the protective layer having the resin layer may be bonded together to form a paint layer having a plurality of resin layers.
[0068] (Variation 2) In the transfer type curable resin sheet in the first and second embodiments of the present invention, the shape of the protrusion 3 is triangular. However, the shape of the protrusion 3 is not limited to a triangle as long as the protrusion 3 can be pinched with a finger or a peeling device. For example, the shape of the protrusion 3 may be rectangular as in the transfer type curable resin sheet 1E shown in FIG. 8(a), or the shape of the protrusion 3 may be semi-elliptical as in the transfer type curable resin sheet 1F shown in FIG. 8(b). In addition, when the shape of the protrusion is triangular, the angle of the tip is preferably 90° or less. Furthermore, when the protrusion is R-shaped, the width of the protrusion at a position 5 mm from the tip in the protruding direction toward the opposite direction to the protruding direction is preferably 7 mm or less.
[0069] (Variation 3) In the transfer type curable resin sheets according to the first and second embodiments of the present invention, the position of the protrusion 3 is the center of the main body 2. However, the position of the protrusion 3 is not limited to the center of the main body 2 as long as the protrusion 3 can be held by fingers or a peeling device. For example, as in the transfer type curable resin sheet 1G shown in FIG. 9, the protrusion 3 may be located on the edge side of the center of the main body 2.
[0070] (Variation 4) In the transfer type curable resin sheets in the first and second embodiments of the present invention, a configuration is shown in which the entire protrusion 3 is an inclined portion, but the entire protrusion 3 does not need to be an inclined portion, and only a part of the protrusion 3 may be an inclined portion. That is, in each of the above embodiments, the protrusion 3 is bent from the connection portion between the main body 2 and the protrusion 3, but it is not necessary to be bent from the connection portion, and any part of the protrusion 3 may be bent from the start point.
[0071] Two or more of the transfer type curable resin sheets according to the first and second embodiments of the present invention and the first to fourth modifications thereof can be combined.
[0072] The transfer-type curable resin sheet of the first and second embodiments of the present invention and its modifications 1 to 4 are merely examples of the transfer-type curable resin sheet of the present invention, and therefore the transfer-type curable resin sheet of the present invention is not limited to the transfer-type curable resin sheet of the first and second embodiments of the present invention and its modifications 1 to 4.
[0073] The coating method of the present invention can be applied to various applications. The coating method of the present invention can be applied to, for example, electrical appliances, vehicles such as automobiles and railways, vehicle parts, miscellaneous goods, heavy machinery, ships, aircraft, exterior materials such as exterior walls or roofing materials for houses and buildings, bridges, steel frames, plants, wind power generation blades, etc. Examples of vehicle parts include vehicle interior materials and vehicle exterior materials. Among these, vehicles and vehicle parts are preferred, vehicle parts are more preferred, and vehicle exterior materials are even more preferred. Examples of vehicle exterior materials include aero parts, hoods, roofs, door panels, bumpers, fuel filler panels, trunk lids, rear gates, etc.
[0074] [Vehicles, vehicle parts] The vehicle and vehicle parts of the present invention are those coated with the transfer type curable resin sheet of the present invention, or those coated by the coating method of the present invention. EXAMPLES
[0075] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way.
[0076] The measurement and evaluation methods in the present invention are as follows. (Loop Stiffness) A rectangular sample 20 mm wide and 15 cm long was prepared, and both ends were joined together to make a loop, which was then set into the device, and compression measurements were performed to crush the loop of the test piece. A flat compression tool much larger than the sample was used to press the sample at a speed of 50 mm / min, and the repulsive force at the position where the displacement was 20 mm was read, and this was taken as the loop stiffness value, which indicates the stiffness of the transfer film. A general universal testing machine can be used as the compression measurement device.
[0077] (Peel strength A) The transfer type curable resin sheet obtained in the examples and comparative examples was processed to a width of 25 mm and a length of 100 mm. The transfer layer side of the 25 mm wide transfer type curable resin sheet was attached to a 70 mm x 150 mm painted steel plate via a double-sided tape (product name "WT♯550TL5B5", manufactured by Sekisui Chemical Co., Ltd., PET base material 18 μm, adhesive layer on both sides 12 μm). In addition, after peeling the protective layer from the transfer type curable resin sheet, a single-sided tape (product name "3803BS", manufactured by Sekisui Chemical Co., Ltd., PET base material 18 μm, adhesive layer 12 μm) was attached to the surface of the color layer. Next, the peel strength A was obtained when the single-sided tape was peeled from the transfer layer together with the paint layer (clear layer and color layer) under the conditions of a peel angle of 90° and a peel speed of 300 mm / min.
[0078] (Peel strength B) The transfer-type curable resin sheet (a laminate of the transfer layer and the paint layer (color layer and clear layer)) peeled off from the protective layer as described above was attached to the painted surface of a 70 mm × 150 mm painted steel plate, and the transfer layer was peeled off. Next, a single-sided tape (product name "3803BS", manufactured by Sekisui Chemical Co., Ltd., PET base material 18 μm, adhesive layer 12 μm) was attached to the surface of the clear layer (i.e., the surface of the paint on the side where the transfer layer was provided). Next, the peel strength B was obtained when the single-sided tape was peeled off from the painted steel plate together with the paint layer (clear layer and color layer) under the conditions of a peel angle of 90 ° and a peel speed of 300 mm / min. The above peel strengths A and B were measured under an environment of 23 ° C. and humidity 50% RH. As the painted steel plate, a SPCC-SD automotive painted test piece (urethane white + urethane clear) manufactured by Standard Test Piece Co., Ltd. was used.
[0079] (Gel fraction) The transfer type curable resin sheet is cut into a flat rectangular shape of 50 mm x 100 mm to prepare a test piece. The test piece is immersed in toluene at 23°C for 24 hours, then removed from the toluene and dried at 110°C for 1 hour. The weight of the test piece after drying is measured, and the gel fraction is calculated using the following formula. Note that no protective layer is laminated on the test piece. Gel fraction (wt%) = 100 × (W 2 -W 0 ) / (W 1 -W 0 ) (W 0 : Weight of transfer layer, W 1 : weight of test piece before immersion, W 2 (Weight of test piece after immersion and drying)
[0080] (Transfer layer peelability) The transfer-type curable resin sheet from which the protective layer had been peeled off was attached to a coated steel plate measuring 1 mm in thickness × 70 mm × 150 mm using a squeegee and water at 23° C. After that, the transfer layer was peeled off in a 23° C. environment, and the peelability was evaluated according to the following evaluation criteria. ⊚: After application, the release layer at the protruding portion of the transfer-type curable resin sheet naturally peeled off. ◯: The release layer at the protrusions did not peel off naturally, but when the tip of the protrusion was lightly scratched with a fingernail, the release layer at the protrusions of the transfer-type curable resin sheet was easily peeled off. ×: Even when the tip of the protrusion was scratched with a fingernail, the release layer at the protrusion of the transfer-type curable resin sheet did not peel off, and the clear layer and the color layer also peeled off.
[0081] The components of the release layer film, protective layer film, and resin layer used in the examples and comparative examples are as follows. <Transfer layer film> Convenience store PE: Non-oriented polyethylene / EVA multilayer film (Okamoto's "Convenience store PE transparent", thickness 300μm), tensile breaking elongation at 100℃ (MD=350%, TD=400%) PP: Polypropylene (Okamoto Corporation's "Aromer Film", thickness 100 μm) Decofit Q17CK: Non-oriented cyclic polyolefin film (Toray "Decofit Q17CK", thickness 100μm) A-PET: Non-stretched polyethylene terephthalate film (A-PET) ("A-PET" manufactured by Nakamoto Pax Co., Ltd., thickness 200 μm) PBT: Polybutylene terephthalate (OG Film Co., Ltd. "Hard PBT", thickness 100 μm) Soft PVC: Soft polyvinyl chloride (Okamoto Corporation's "New Celeb", thickness 200 μm) ABS: Acrylonitrile-butadiene-styrene copolymer ("ABS film" manufactured by Okamoto Corporation, thickness 200 μm) <Protective layer film> Unstretched polyethylene terephthalate film (A-PET) ("A-PET" manufactured by Nakamoto Pax Co., Ltd., thickness 400 μm), tensile breaking elongation at 100°C (MD = 1200%, TD = 980%)
[0082] <(Meth)acrylic resin (A1)> Acrylic polyol (1): weight average molecular weight 250,000, glass transition temperature (Tg) 40°C, hydroxyl value 80 mgKOH / g, solid content concentration (NV) = 23.3 mass% (solvent: ethyl acetate) Acrylic polyol (2): weight average molecular weight 250,000, glass transition temperature (Tg) 40°C, hydroxyl value 170 mgKOH / g, solid content concentration (NV) = 29.6 mass% (solvent: ethyl acetate) <Plasticized resin (A2)> Acrylic polyol (3): weight average molecular weight 2500, glass transition temperature (Tg) -50°C, hydroxyl value 120 mgKOH / g, solid content (NV) = 100% by mass Polycarbonate diol: hydroxyl value 204-244 mg KOH / g, weight average molecular weight 500, "PH-50", manufactured by UBE Corporation Carboxyl-containing acrylic polymer, "UC-3000", manufactured by Toagosei Co., Ltd., adhesive strength regulator
[0083] <Compound (B) Having a Blocked Isocyanate Group> Hexamethylene diisocyanate-based blocked isocyanate (HDI-based), Mitsui Chemicals' "Takenate B-882N", blocking agent type: 2-butanone oxime (MEKO), NV=70%, solvent is petroleum naphtha, contains a small amount of urethane catalyst <Urethane catalyst> "XK-639", manufactured by Kusumoto Chemicals Co., Ltd.
[0084] <Pigments> "NSP-UP 841B" manufactured by Nikko Vicks Co., Ltd., effective pigment concentration = 9% by mass, NV = 24% by mass <Shining material> Merck's "Xiramic T60-10 WNT Crystal Silver" Alumina flakes coated with at least one layer of metal oxide, including titanium dioxide
[0085] <Surface conditioner> Silicone acrylic copolymer, "BYK-3550", manufactured by BYK <Antifoaming agent> Silicone-based defoamer, "TSA750", manufactured by Nissho Sangyo Co., Ltd.
[0086] [Preparation of Thermosetting Resin Compositions A to D] Each component was added in the proportions shown in Table 1, and ethyl acetate was added as a solvent to prepare diluted solutions of curable resin compositions A to D so that the solid content concentration was 40 mass %.
[0087] [Example 1] Thermosetting resin composition A was applied onto the surface of the film for the transfer layer shown in Table 2 using an applicator, and then a pre-drying process was carried out under conditions of a drying temperature of 60°C and a drying time of 30 minutes, followed by a main drying process under conditions of a drying temperature of 90°C and a drying time of 30 minutes, thereby forming a 30 μm-thick clear layer on the transfer layer. Next, thermosetting resin composition B was applied onto the surface of the film for the protective layer using an applicator, and then a pre-drying process was carried out under conditions of a drying temperature of 60°C and a drying time of 30 minutes, and then a main drying process was carried out under conditions of a drying temperature of 90°C and a drying time of 30 minutes, thereby forming a color layer with a thickness of 30 μm on the protective layer. The clear layer on the transfer layer and the color layer on the protective layer were attached and laminated at 25°C to obtain a transfer type curable resin sheet having the transfer layer, clear layer, color layer, and protective layer laminated in that order. In order to vacuum mold the obtained transfer type curable resin sheet, a wooden mold was made so that the parts that would become the protrusions would be at a specified angle. Next, the transfer type curable resin sheet was vacuum molded, and an ultrasonic cutter was used to produce a transfer type curable resin sheet with a main body and protrusions as shown in Figure 1(a).
[0088] [Examples 2 to 10, Comparative Examples 1 to 3] The same procedure as in Example 1 was carried out, except that the formulation of the curable resin composition was changed as shown in Tables 1 and 2. The evaluation results are shown in Table 2.
[0089] [Table 1] *Table 1 shows the amount of each component in thermosetting resin compositions A to D based on the solid content, and the solid content of the total thermosetting composition is taken as 100 parts by mass. *The amount of active pigment ingredient is the value in Table 1 multiplied by 9 / 24.
[0090] [Table 2]
[0091] In the transfer type curable resin sheets of Examples 1 to 10, the protrusions were folded at an angle of 30° or more, and the ratio (A / B) of peel strength A to peel strength B was 0.5 or less, so the releasability of the transfer layer was good. On the other hand, in the transfer type curable resin sheets of Comparative Examples 1 and 2, the protrusions were not folded or were folded at an angle of less than 30°, so the releasability of the transfer layer was poor. In addition, in the transfer type curable resin sheet of Comparative Example 3, the ratio (A / B) of peel strength A to peel strength B was greater than 0.5, so the releasability of the transfer layer was poor. [Explanation of symbols]
[0092] 1,1A~1G Transfer type curable resin sheet 2 Main unit 3 Projection (slanted part) 10 paint layers 11 Clear layer 12 Color Layers 20 Transfer layer 30 Object to be painted 40 protective layer
Claims
1. A transfer type curable resin sheet comprising a paint layer containing a curable resin composition that can be cured by heat, active energy rays, or moisture, and a transfer layer that is provided on one surface of the paint layer and contains a thermoplastic resin, The transfer type curable resin sheet includes a main body and a protrusion protruding from the main body in a planar direction, The protrusion portion has an inclined portion inclined at an angle of 30° or more with respect to the main body portion, A transfer type curable resin sheet in which the ratio (A / B) of the peel strength A (N / 25 mm) at the interface between the transfer layer and the paint layer to the peel strength B (N / 25 mm) at the interface between a coated steel plate test piece and the paint layer is 0.5 or less.
2. The transfer type curable resin sheet according to claim 1 , wherein the protrusions are bent at an angle of 30° or more by shaping.
3. The transfer type curable resin sheet according to claim 2 , wherein the protrusions are folded toward the transfer layer.
4. The transfer type curable resin sheet according to claim 1 , wherein the protrusions have the inclined portions when attached to an object to be coated.
5. The transfer type curable resin sheet according to claim 4 , wherein the protrusions are inclined toward the paint layer side.
6. 2. The transfer type curable resin sheet according to claim 1, wherein a peel strength A of the interface between the transfer layer and the paint layer is 2 N / 25 mm or less.
7. 2. The transfer type curable resin sheet according to claim 1, wherein the transfer layer has a loop stiffness of 0.05 to 1.0 N / 20 mm.
8. The transfer type curable resin sheet according to claim 1 , wherein the paint layer includes a clear layer that does not contain a colorant, and a color layer that contains a colorant and is provided on the opposite side of the clear layer from the transfer layer.
9. The transfer type curable resin sheet according to claim 1 , wherein the curable resin composition comprises a (meth)acrylic resin (A) and a blocked isocyanate (B).
10. 2. The transfer type curable resin sheet according to claim 1, which has a gel fraction of 50% or less.
11. The transfer layer comprises at least one resin selected from the group consisting of cyclic olefin resin, polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polyvinyl chloride (PVC) resin, acrylonitrile-butadiene-styrene copolymer (ABS), polyethylene (PE) and polypropylene (PP). The transfer type curable resin sheet according to claim 1, comprising at least one resin.
12. The transfer type curable resin sheet according to claim 1 , which is shaped into a three-dimensional shape.
13. A step of attaching the transfer type curable resin sheet according to claim 1 to an object to be coated; and A coating method comprising the step of peeling off the transfer layer from the workpiece at the protrusions.
14. The coating method according to claim 13, wherein the transfer type curable resin sheet is attached to the workpiece so as to form an inclined portion that is inclined at an angle of 30° or more with respect to the main body portion.
15. The coating method according to claim 13, further comprising a step of, after attaching the transfer type curable resin sheet to the object to be coated, causing the protrusions to be fitted around the back of the object to be coated.
16. A vehicle painted with the transfer type curable resin sheet according to any one of claims 1 to 12.
17. A vehicle part coated with the transfer type curable resin sheet according to any one of claims 1 to 12.
18. A vehicle coated by the coating method according to any one of claims 13 to 15.
19. A vehicle part coated by the coating method according to any one of claims 13 to 15.
Citation Information
Patent Citations
Transfer sheet and method of manufacturing decorative sheet