Plastic base material with film composed of photocured product of photosensitive resin composition, and method for producing the same
A photosensitive resin composition enables the production of temperature-responsive films on plastic substrates at room temperature, addressing the challenges of high-temperature baking and solvent compatibility, thereby facilitating the use of plastics in cell culture applications.
Patent Information
- Application Number
- JP2024057352
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-15
AI Technical Summary
Conventional methods for applying polymers to cell culture substrates face challenges with glass substrates due to alkali elution and reproducibility issues, and plastic substrates require high-temperature baking after light irradiation, making it difficult to use plastics for cell culture due to heat resistance and solvent compatibility.
A photosensitive resin composition is developed that allows for the production of a photocured film on plastic substrates at room temperature without high-temperature baking, using a polymer with aryl ketone residues and specific solvents, enabling patterning by photolithography.
The method enables the production of a film-coated plastic substrate with a glass transition temperature of 105°C or less, allowing for temperature-responsive patterns without dissolving the plastic, and provides a simple photolithography process for creating films on plastic surfaces.
Smart Images

Figure 2024146913000016 
Figure 2024146913000017 
Figure 2024146913000018
Abstract
Description
[Technical field]
[0001] The present invention relates to a film-attached plastic substrate made of a photocured product of a photosensitive resin composition, and to a film-attached plastic substrate and a method for producing the film-attached plastic substrate. [Background technology]
[0002] Poly(N-isopropylacrylamide) (PNIPAAm) is known as a polymer contained in a photosensitive resin composition. PNIPAAm can be easily obtained by polymerizing N-isopropylacrylamide (NIPAAm) with a radical initiator. An aqueous solution of PNIPAAm undergoes phase separation due to temperature changes, dissolving in water at 31°C or lower, and insolubilizing and precipitating at temperatures higher than that. A technology is known for manufacturing chips having dot patterns formed by photolithography using a photosensitive resin composition containing such a polymer. Photolithography technology, which processes substrates, etc., can manufacture fine pattern structures. Such fine pattern structures are useful when handling microscopic cells, etc.
[0003] In Patent Document 1, it is described in the Examples that a cell culture support is produced by patterning using a photolithography method from a photosensitive resin composition containing a monomer N-isopropylacrylamide. However, in Patent Document 1, the cell culture support is produced on a glass substrate in the Examples by performing post-exposure baking (PEB) in an oven at 80°C for 20 hours. Patent Document 2 describes a coating material that exhibits the ability to selectively culture and separate cells. However, Patent Document 2 describes that the polymer coating on the surface of the glass substrate is heated on a hot plate heated to 100° C. for 1 minute. Non-Patent Document 1 describes a study in which a polymer of N-isopropylacrylamide, methacrylic acid, and 4-methacryloylbenzophenone is plasma cleaned, and then surface-adsorbed onto a glass substrate silanized with a hexamethyldisilazane solution (Scheme 1), to create a responsive hydrogel thin film, and an atomic force microscope is used to examine the changes in structure and adhesion of the hydrogel thin film depending on temperature. However, in this study, the film is not cured, and the technique is only applicable to glass substrates. Non-Patent Document 2 describes a study on the possibility of modeling the swelling behavior of a film produced from a copolymer of poly(N-isopropylacrylamide) and methacryloylbenzophenone, evaluating the swelling behavior of the film by neutron reflectometry, and measuring the film thickness with temperature change. However, the film is produced on a quartz or silicon substrate, and is heated at 90°C for 10 minutes during the production of the film. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2016 / 068271 [Patent Document 2] International Publication No. 2019 / 013148 [Non-patent literature]
[0005] [Non-Patent Document 1] Langmuir 2010,26(10),7262-7269 [Non-Patent Document 2] Macromolecules 2008,41(3),919-924 Summary of the Invention [Problem to be solved by the invention]
[0006] Conventionally, when applying polymers to cell culture, a glass substrate was used instead of a plastic substrate because baking after light irradiation must be performed at high temperatures. However, when using a glass substrate for cell culture, the cured layer on the substrate is a thin film, so there is a problem that it is highly affected by alkaline elution of the glass substrate and it is difficult to achieve reproducibility. In addition, when trying to create a film on a silicon wafer instead of a plastic substrate, there are problems that the film does not become thick and the film thickness is not reproducible. In addition, in current cell culture, plastic products have replaced glass products as the mainstream because they are easy to use, have excellent impact resistance, are inexpensive, are lightweight, etc. Therefore, it has been desired to use plastic substrates instead of glass and silicon wafer products for cell culture using polymers.
[0007] On the other hand, plastics have problems such as low heat resistance and dissolution in some organic solvents. When using a plastic substrate for cell culture, it is required that the membrane or the like to be produced be prepared at room temperature or at most 50°C or lower, and that the solvent for the composition to be the membrane be an organic solvent that does not dissolve plastics. However, in the conventional technology, in order to cure a photosensitive resin composition containing N-isopropylacrylamide, it was necessary to maintain a high temperature of 80°C or more for a certain period of time as a post-light irradiation bake. Therefore, it was extremely difficult to select an organic solvent that does not dissolve plastics, select and prepare a composition that dissolves in this organic solvent and cures only by light irradiation, determine the wavelength and dose of light irradiation, and establish a manufacturing method. The present invention has been made in view of the above-mentioned circumstances, and an object of the present invention is to provide a photosensitive resin composition using a polymer that can produce a temperature-responsive pattern by photolithography in the field of cell culture. Another object of the present invention is to provide a photosensitive resin composition that can be processed at room temperature using a solvent that does not dissolve plastics, so that a plastic substrate can be used. [Means for solving the problem]
[0008] As a result of intensive research, the present inventors have found that a cured film can be prepared by irradiating a composition containing N-isopropylacrylamide and an aryl ketone with light, and that a cured film that can be processed at room temperature without high-temperature baking can be produced by patterning using a photolithography method, thus completing the invention. Furthermore, they have found that an organic solvent that does not dissolve plastics can be used as a solvent for the composition.
[0009] That is, the present invention relates to the following. According to a first aspect, there is provided a film-attached plastic substrate having a film (C) made of a photocured product of a composition on a surface of the plastic substrate, The composition contains a polymer (A) having a structural unit represented by the following formula (1): The composition may comprise an optionally substituted aryl ketone (B), When the aryl ketone (B) is not included in the composition, the polymer (A) has residues of the aryl ketone (B); When the aryl ketone (B) is contained in the composition, the polymer (A) may have a residue of the aryl ketone (B). [ka] (In formula (1), R 1 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, R 2 represents an optionally substituted alkyl group having 1 to 10 carbon atoms. As a second aspect, the present invention relates to a film-attached plastic substrate according to the first aspect, in which the aryl ketone (B) is an aryl ketone selected from the group consisting of acetophenone, benzophenone, anthraquinone, anthrone, a compound represented by the following formula (2), anthrone analogues in which any carbon atom on the ring of the compound represented by formula (2) is replaced with a heteroatom, and derivatives of these compounds. [ka] (In formula (2), R 3 to R 6 each independently represents a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, a hydroxy group, a sulfo group, a vinyl group, an acetoxy group, an aryl group having 6 to 14 carbon atoms which may be substituted with a hydroxy group, an amino group or a mono- or di-alkylamino group having 1 to 4 carbon atoms, X represents -O-, -S-, >CH2, >C=O or >N-R, and R represents a hydrogen atom, a hydrocarbon group or an acyl group, n1 represents 0 or 1, n2 to n5 each independently represent 0, 1, 2 or 3, and n2 + n3 ≤ 3, n4 + n5 ≤ 4 are satisfied.) As a third aspect, it relates to the plastic substrate with a film according to the first aspect, wherein the polymer (A) is a polymer having a structural unit represented by the following formula (3).
Chemical formula
Chemical formula
[0010] According to the present invention, it is possible to provide a film-coated plastic substrate, which has a film made of a photocured product on the surface of the plastic substrate at room temperature, using a photosensitive resin composition, without high-temperature baking after light irradiation. According to the present invention, a plastic substrate having a film made of a photocured product attached to the surface of a plastic substrate having a glass transition temperature of 105° C. or lower can be provided using a photosensitive resin composition. According to the present invention, by using an alcohol-based solvent, a plastic substrate with a film made of a photocured material can be produced without dissolving the plastic. According to the present invention, by using a photosensitive resin composition, a method for producing a plastic substrate with a film made of a photocured product by a simple photolithography method without baking after light irradiation can be provided. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a graph showing the sensitivity behavior of the photosensitive resin compositions obtained in Example 1, Example 2, and Comparative Example 1 on a polystyrene film. [Diagram 2] FIG. 2 is a graph showing the sensitivity behavior on a silicon wafer of the photosensitive resin compositions obtained in Example 1, Example 2, and Comparative Example 1. [Diagram 3] FIG. 3 is an electron microscope photograph of patterning performed on a polystyrene film using the photosensitive resin composition obtained in Example 1. [Figure 4] FIG. 4 is a differential thermal curve of the reaction product obtained in Synthesis Example 1 in pure water. [Diagram 5] FIG. 5 is a differential thermal curve of the reaction product obtained in Synthesis Example 2 in pure water. [Figure 6] FIG. 6 is a differential thermal curve of the reaction product obtained in Synthesis Example 1 in phosphate buffered saline. [Figure 7] FIG. 7 is a differential thermal curve of the reaction product obtained in Synthesis Example 2 in phosphate buffered saline. [Figure 8] FIG. 8 shows the change in film thickness of a photocured film prepared using composition 2 as a function of temperature. [Figure 9] Figures 9a to 9d are photographs of films of Composition 3 with thicknesses of 5 to 10 nm that were incubated and then placed on tables at temperatures ranging from 37°C to 22°C, taken at times ranging from 0 to 10 minutes (Figure 9a: optical microscope photograph after 0 minutes, Figure 9b: optical microscope photograph after 5 minutes, Figure 9c: overall photograph after 7 minutes, Figure 9d: overall photograph after 10 minutes). [Figure 10] Figures 10a and 10b show photographs of films of composition 3 with thicknesses of 11-22 nm that were subsequently incubated at 37°C (Figure 10a: optical microscope photograph, Figure 10b: overall photograph). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] <Photosensitive resin composition> The photosensitive resin composition (hereinafter, also referred to as the composition) of the present invention will be described. The composition contains a polymer (A) having a structural unit represented by the above formula (1), The composition may comprise an optionally substituted aryl ketone (B), When the aryl ketone (B) is not included in the composition, the polymer (A) has residues of the aryl ketone (B); When the aryl ketone (B) is contained in the composition, the polymer (A) may contain residues of the aryl ketone (B). Therefore, the photosensitive resin composition of the present invention is "(Composition I) a photosensitive resin composition comprising, in a polymer (A), a structural unit (main chain 1) represented by the above formula (1) and a structural unit (main chain 2) to which a residue of an aryl ketone (B) is bonded; (Composition II) a photosensitive resin composition comprising, in a polymer (A), a structural unit (main chain 1) represented by the above formula (1) and a structural unit (main chain 2) to which a residue of an aryl ketone (B) can be bonded but is not bonded, and further comprising an optionally substituted aryl ketone (B); (Composition III) is classified as a photosensitive resin composition which contains, in a polymer (A), a structural unit (main chain 1) represented by the above formula (1), a structural unit (main chain 2) to which a residue of an aryl ketone (B) is bonded, and a structural unit (main chain 2) to which a residue of an aryl ketone (B) can be bonded but is not bonded, and further contains an optionally substituted aryl ketone (B) bonded to the main chain 2. However, in the above (Compositions I) to III, the main chain 2 may be a derivative group of the main chain 1.
[0013] <Polymer (A)> Polymer (A) can contain a structural unit represented by the above formula (1) (main chain 1), a structural unit to which a residue of aryl ketone (B) is bonded (main chain 2), and a structural unit to which a residue of aryl ketone (B) can be bonded but is not bonded (main chain 2). The main chain 1 is also called the first monomer unit and is represented by the above formula (1). The main chain 2, also referred to as the second monomer unit, may have a residue of an aryl ketone (B) bonded thereto or may not have a residue of an aryl ketone (B) bonded thereto. A specific example of a compound having a residue of an aryl ketone (B) bonded thereto is shown on the right side of the above formula (3). A specific example of a case where the residue of an aryl ketone (B) can be bonded but is not bonded is shown by the following formula (7). [ka] (In formula (7), R 7 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, L 1 represents a group that reacts with and bonds to an aryl ketone (B).
[0014] <Aryl ketone (B)> An "aryl ketone (B)" is a compound containing an aryl group and a carbonyl group. As the aryl ketone of the present invention, benzophenone or a substituted derivative thereof (hereinafter also referred to as a "benzophenone compound") is preferable from the viewpoint that the lifetime of the lowest excited triplet is relatively long and photochemical reactions are easily caused. Examples of the benzophenone compound include 2,2'-dihydroxy-4-methoxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, 2,2',3,4-tetrahydroxybenzophenone, 2,2',4,4'-tetrahydroxybenzophenone, 2,2'3,4,4'-pentahydroxybenzophenone, 2,2'-dihydroxy-4-methoxybenzophenone, 2,3,3'4,4',5'-hexahydroxybenzophenone, 2 ,3,4,4'-Tetrahydroxybenzophenone, 2,3,4-Trihydroxybenzophenone, 2,4,4'-Trihydroxybenzophenone, 2,4,5-Trihydroxybenzophenone, 2,4,6-Trihydroxybenzophenone, 2,4-Dihydroxy-4'-diethylaminobenzophenone, 2,4-Dihydroxy-4'-dimethylaminobenzophenone, 2,4-Dihydroxybenzophenone, 4,4'-Dihydroxybenzophenone, 2-Hydroxy -4-(2-hydroxy-3-methacryloxy)propoxybenzophenone, 2-hydroxy-4'-dimethylaminobenzophenone, 2-hydroxy-4-i-octyloxybenzophenone, 2-hydroxy-4-n-octyloxybenzophenone, 2-hydroxy-4-octyloxybenzophenone, 2-hydroxy-4-acetoxyethoxybenzophenone, 2-hydroxy-4-octadecyloxybenzophenone, 2-hydroxy-4-dodecyloxybenzophenone, 2-hydroxy-4-methoxy-2'-carboxybenzophenone, 2,2'-dihydroxy-4,4' -dimethoxydisulfobenzophenone disodium, 2-hydroxy-4-methoxy-5-sulfobenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxybenzophenone, 4,4'-dihydroxybenzophenone, 4,4'-bis(diethylamino)benzophenone, 4,4'-bis(dimethylamino)benzophenone, 4',6-dihydroxy-2-naphthobenzophenone, 4-dodecyloxy-2-hydroxybenzophenone, 4-hydroxybenzophenone, N,N,N',N'-tetramethyl-4,4'-diaminobenzophenone, etc. Optionally substituted vinylbenzophenones are also included. Other examples of structures capable of abstracting hydrogen radicals upon irradiation with ultraviolet light include a benzyl group, an o-benzoylbenzoate group, a thioxanthone group, a 3-ketocoumarin group, a 2-ethylanthraquinone group, and a camphorquinone group. Compounds having these structures may also be used. In addition to the benzophenone compounds, specific preferred examples of the aryl ketones include aryl ketones selected from the group consisting of acetophenone, benzophenone, anthraquinone, anthrone, the compound represented by the above formula (2), anthrone analogues in which any carbon atom of the compound represented by formula (2) is substituted with a heteroatom, and derivatives of these compounds.
[0015] <Optionally Substituted Aryl Ketone (B)> Examples of the substituent that the "optionally substituted aryl ketone (B)" may have include a halogen atom, an amino group, a mono- or di-alkylamino group having 1 to 4 carbon atoms, a nitro group, a cyano group, an oxo group, a hydroxy group, a sulfanyl group, an alkoxy group having 1 to 4 carbon atoms, an alkoxycarbonyl group having 1 to 4 carbon atoms, a formyl group, and an aryl group having 6 to 14 carbon atoms. The aforementioned "halogen atom" includes fluorine, chlorine, bromine and iodine. Examples of the "mono- or di-alkylamino group having 1 to 4 carbon atoms" include a methylamino group, an ethylamino group, a propylamino group, an isopropylamino group, a butylamino group, a dimethylamino group, a diethylamino group, a dipropylamino group, a dibutylamino group, and an n-ethyl-n-methylamino group.
[0016] The "alkoxy group" may be either linear or branched. Examples of the "alkoxy group having 1 to 4 carbon atoms" include a methoxy group, an ethoxy group, a propoxy group, an isopropoxy group, a butoxy group, an isobutoxy group, a sec-butoxy group, and a tert-butoxy group. The "alkoxycarbonyl group having 1 to 4 carbon atoms" is an organic group in which a carbonyl group -C(=O)- is bonded to the "alkoxy group having 1 to 4 carbon atoms". Examples of the "aryl group having 6 to 14 carbon atoms" include a phenyl group, a 1-naphthyl group, a 2-naphthyl group, a 1-anthryl group, a 2-anthryl group, and a 9-anthryl group.
[0017] <Anthrone analogue in which any carbon atom of the compound represented by formula (2) is replaced with a heteroatom> The term "anthrone analog" refers to a compound having a composition in which an atom or atomic group of anthrone is replaced with another heteroatom. The "anthrone analog" of the present invention is "a compound represented by the formula (2) The term "anthrone analogues" refers to "anthrone analogues in which any carbon atom of the compound represented is replaced with a heteroatom." Heteroatoms include nitrogen, oxygen, sulfur, phosphorus, chlorine, iodine, bromine, and the like. <Derivatives of these compounds> The above-mentioned "these compounds" refer to acetophenone, benzophenone, anthraquinone, anthrone, the compound represented by the above formula (2), and anthrone analogues in which any carbon atom of the compound represented by formula (2) is replaced with a heteroatom. The term "derivatives of these compounds" refers to the substitution of an atom or an atomic group of the aforementioned "these compounds" with another substituent. The substituents that can be substituted are the same as those shown in the aforementioned <Optionally substituted aryl ketone (B)>.
[0018] <Molecular weight of aryl ketone (B)> The "optionally substituted aryl ketone" may have a molecular weight of 500 or more. However, in consideration of ease of handling of the composition and ease of curing of the film, the molecular weight is preferably 500 or less, more preferably 400 or less, and even more preferably 300 or less.
[0019] <Residue of aryl ketone (B)> An aryl ketone residue is a group of a compound (monoaryl ketone or diaryl ketone) in which one or two aryl groups are directly bonded to a carbonyl group [-C(=O)-], an ether group [-O-], an alkylene group, etc., and this aryl ketone residue acts as a photoreactive group and can be activated by light of a specific wavelength, such as ultraviolet light, to cause a crosslinking reaction. As used herein, the term "residue" of a compound refers to an organic group in which a hydrogen atom bonded to a carbon atom or heteroatom (such as a nitrogen, oxygen, or sulfur atom) constituting the compound is replaced with a bond for covalent bonding. The residue of the aryl ketone does not constitute the main chain, but constitutes a side chain of the polymer that is one embodiment of the present invention, via a suitable linking group. As used herein, the term "backbone" refers to the longest series of covalently bonded atoms that together form a continuous chain of a molecule. The term "side chain" is used herein to broadly encompass chemical groups that are covalently attached to a main chain and pendant laterally, and is used synonymously with so-called pendant molecular chains. Examples of the residue of an aryl ketone include the monovalent groups of an optionally substituted aryl ketone shown above as the optionally substituted aryl ketone (B). These aryl ketone residues (monovalent groups) form covalent bonds such as -O- bonds, ester bonds (-O-CO- or -CO-O-), amide bonds (-NH-CO- or -CO-NH-), urethane bonds (-NH-CO-O- or -O-CO-NH-), carbonate bonds (-O-CO-O-), and urea bonds (-NH-CO-NH-) with the bonding groups in the polymer (for example, those included in L in formula (3)), thereby forming side chains of the polymer. Therefore, "L" in the formula (3) is the bonding group or a group in which the bonding group is bonded to one or more groups selected from an alkylene group having 1 to 3 carbon atoms, an alkenylene group having 1 to 3 carbon atoms, and a carbonyl group. In addition, "L 1 " is a group in which a hydrogen atom is bonded in place of the aryl ketone bonded to the above "L". The "alkylene group having 1 to 3 carbon atoms" includes a divalent group having a straight or branched chain, such as a methylene group, an ethylene group, or a propylene group. The "alkenylene group having 1 to 3 carbon atoms" includes a divalent group having a double bond and a straight or branched chain, and refers to a group in which one or more carbon-carbon bonds of the alkylene group having 1 to 3 carbon atoms are double bonds.
[0020] R shown in the above formula (1) 1 contains an alkyl group having 1 to 3 carbon atoms. The above-mentioned "alkyl group having 1 to 3 carbon atoms" includes those having a straight or branched chain, such as a methyl group, an ethyl group, an n-propyl group, and an isopropyl group.
[0021] R shown in formula (1) 2represents an optionally substituted alkyl group having 1 to 10 carbon atoms. The "alkyl group having 1 to 10 carbon atoms" includes those having a straight chain or a branched chain, such as a methyl group, an ethyl group, an n-propyl group, an i-propyl group, an n-butyl group, an i-butyl group, an s-butyl group, a t-butyl group, an n-pentyl group, a 1-methyl-n-butyl group, a 2-methyl-n-butyl group, a 3-methyl-n-butyl group, a 1,1-dimethyl-n-propyl group, a 1,2-dimethyl-n-propyl group, a 2,2-dimethyl-n-propyl group, a 1-ethyl-n-propyl group, an n-hexyl group, a 1-methyl-n-pentyl group, a 2 ... Examples of such alkyl groups include butyl, 3-methyl-n-pentyl, 4-methyl-n-pentyl, 1,1-dimethyl-n-butyl, 1,2-dimethyl-n-butyl, 1,3-dimethyl-n-butyl, 2,2-dimethyl-n-butyl, 2,3-dimethyl-n-butyl, 3,3-dimethyl-n-butyl, 1-ethyl-n-butyl, 2-ethyl-n-butyl, 1,1,2-trimethyl-n-propyl, 1,2,2-trimethyl-n-propyl, 1-ethyl-1-methyl-n-propyl and 1-ethyl-2-methyl-n-propyl groups.
[0022] Examples of the substituent that the "optionally substituted alkyl group having 1 to 10 carbon atoms" may have include a halogen atom, an amino group, a mono- or di-alkylamino group having 1 to 4 carbon atoms, a nitro group, a cyano group, an oxo group, a hydroxy group, a sulfanyl group, an alkoxy group having 1 to 4 carbon atoms, an alkoxycarbonyl group having 1 to 4 carbon atoms, a formyl group, and an aryl group having 6 to 14 carbon atoms.
[0023] The "alkyl group having 1 to 10 carbon atoms" and the "aryl group having 6 to 14 carbon atoms" shown in formula (2) are the same as those described above. The "alkoxy group having 1 to 10 carbon atoms" shown in formula (2) represents a group in which the "alkyl group having 1 to 10 carbon atoms" is bonded to -O-. The "aryl group having 6 to 14 carbon atoms which may be substituted with a hydroxy group" shown in formula (2) represents a group in which a hydroxy group is bonded in place of any hydrogen of the "aryl group having 6 to 14 carbon atoms". The "hydrocarbon group" shown in formula (2) represents an alkyl group, an alkenyl group, and an aryl group. The "acyl group" shown in formula (2) is R 11 -C(=O)-, and "R 11 " represents a hydrogen atom, an alkyl group, an alkenyl group, and an aryl group.
[0024] The "alkyl group having 1 to 3 carbon atoms" and the "optionally substituted alkyl group having 1 to 10 carbon atoms" shown in formula (3) are the same as those described in formula (1). Further, when there is a description of "alkyl group having 1 to 3 carbon atoms", "optionally substituted alkyl group having 1 to 10 carbon atoms", or "optionally substituted" below, unless otherwise specified, it is the same as the above-described content. In formulas (4) to (6), the above-mentioned "R 3 ~R 6 , X and n1 to n5" are the same as those in formula (2).
[0025] In formula (3), x and y are each any number satisfying x + y ≤ 1, 0 < x < 1, and 0 < y < 1, and x and y are the molar ratios of their constituent units. Further, x and y can satisfy 0.01 ≤ y / x ≤ 0.2, preferably satisfy 0.02 ≤ y / x ≤ 0.18, and more preferably satisfy 0.03 ≤ y / x ≤ 0.15. For example, what "0.03 ≤ y / x ≤ 0.15" means is that the number of moles of y is 3 mol% to 15 mol% with respect to the number of moles of x. This indicates that for the left-side constituent unit represented by formula (3), the right-side constituent unit is sufficient at 3 mol% to 15 mol%. That is, although the left-side constituent unit of formula (3) is important as a polymer, the right-side constituent unit of formula (3) is required to promote crosslinking by light. In the present invention, since the film thickness and the degree of curing can be adjusted by the exposure amount and this x:y ratio, this x:y ratio becomes an important index. のモル数は3モル%~15モル%であることを示している。これは、式(3)で表される、左側の構成単位に対し、右側の構成単位は3モル%~15モル%で足りることを示している。つまり、ポリマーとしては、式(3)の左側の構成単位が重要であるが、光による架橋を促進するためには、式(3)の右側の構成単位が必要となることを示している。本発明においては、露光量とこのx:yの比によって膜の厚み及び硬化度の調製ができるため、このx:yの比が重要な指標となる。 Additionally, "x+y≦1" can also be "x+y=1" or "x+y<1." When "x+y=1," the polymer is composed only of the left and right structural units shown in formula (3). When "x+y<1," the polymer contains other polymer structural units in addition to the polymer structural units shown on the right and left sides of formula (3).
[0026] <Alcohol-based solvent> The "alcohol-based solvent" used in the present invention is an alcohol having 2 to 10 carbon atoms which may be substituted. The "alcohol having 2 to 10 carbon atoms" may be linear or branched. Specific examples include ethanol, 1-propanol, 2-propanol, 1-butanol, tert-butanol, 1-pentanol, 2-pentanol, 3-pentanol, 2-methyl-1-butanol, 3-methyl-2-butanol, 2-ethyl-1-butanol, 2,3-dimethyl-2-butanol, 2-methyl-2-pentanol, 4-methyl-2-pentanol, tert-pentyl alcohol, propylene glycol monopropyl ether, tert-butyl cellosolve, cyclohexanol, 4-tert-butylhexanol, α-terpineol, 1-methoxy-2-propanol, 1-ethoxy-2-propanol, diethylene glycol mono-tert-butyl ether, and diacetone alcohol.
[0027] The substituent that the "alcohol having 2 to 10 carbon atoms which may be substituted" may have is the same as the substituent that the "alkyl group having 1 to 10 carbon atoms which may be substituted" may have. In particular, when the substituent is a hydroxyl group, the alcohol becomes a polyhydric alcohol. Examples of the polyhydric alcohol include dihydric polyhydric alcohols such as ethylene glycol, propylene glycol, butanediol, pentanediol, dimethylbutanediol, hexanediol, octanediol, and decanediol, and trihydric or higher polyhydric alcohols such as glycerin, pentaerythritol, and trimethylolpropane. The present invention is not limited to only these examples. These alcohols may be used alone or in combination of two or more kinds. In the present invention, the content of the alcohol-based solvent is preferably 50 to 99.5 parts by mass, more preferably 55 to 95 parts by mass or 60 to 90 parts by mass, and even more preferably 60 to 80 parts by mass, relative to 100 parts by mass of the total mass of the photosensitive resin composition, in order to control the film thickness and to obtain good patterning characteristics.
[0028] <Crosslinking agent> The photosensitive resin composition of the present invention may contain a crosslinking agent within the range not impairing the effects of the present invention. Examples of the crosslinking agent include glycoluril compounds, melamine compounds, and bisazide compounds. Examples of glycoluril compounds include 1,3,4,6-tetrakis(methoxymethyl)glycoluril, 1,3,4,6-tetrakis(ethoxymethyl)glycoluril, 1,3,4,6-tetrakis(propoxymethyl)glycoluril, and 1,3,4,6-tetrakis(butoxymethyl)glycoluril. Examples of the melamine compound include hexamethoxymethylmelamine, hexaethoxymethylmelamine, hexapropoxymethylmelamine, and hexabutoxymethylmelamine. When a crosslinking agent is used, in order to obtain good patterning characteristics and sufficient temperature responsiveness, the content thereof is usually preferably 50 parts by mass or less, 30 parts by mass or less, or even 10 parts by mass or less, relative to 100 parts by mass of the total mass of the polymer (A) (resin component).
[0029] <Other additives> The photosensitive resin composition of the present invention may contain other additives commonly used in the art, as long as the effects of the present invention are not impaired. Examples of the other additives include antireflection agents, polymerization initiators, ultraviolet absorbers, antioxidants, light stabilizers, sensitizers, surfactants, leveling agents, and silane coupling agents. When other additives are used, it is usually preferable that the total amount of the other additives is blended in a ratio of 30 parts by mass or less, 20 parts by mass or less, 10 parts by mass or less, or even 5 parts by mass or less per 100 parts by mass of the total mass of the polymer (A) (resin component).
[0030] <Synthesis of Polymer (A)> In the case of (Composition I), a predetermined amount of a monomer having a structural unit represented by the above formula (1) (e.g., N-isopropylacrylamide) and a predetermined amount of a monomer having a structural unit to which a residue of an aryl ketone (B) is bonded (e.g., 4-benzoylphenyl methacrylate); In the case of (composition II), a predetermined amount of a monomer having a structural unit represented by the above formula (1) (e.g., N-isopropylacrylamide) and a predetermined amount of a monomer having a structural unit to which a residue of an aryl ketone (B) can be bonded but is not bonded (e.g., methacrylic acid); In the case of (composition III), a predetermined amount of a monomer having a structural unit represented by the above formula (1) (e.g., N-isopropylacrylamide), a predetermined amount of a monomer having a structural unit to which a residue of an aryl ketone (B) is bonded (e.g., 4-benzoylphenyl methacrylate), and a predetermined amount of a monomer having a structural unit to which a residue of an aryl ketone (B) can be bonded but is not bonded (e.g., methacrylic acid). After dissolving any of the above in an alcohol-based solvent, the temperature is raised, for example, to 50 to 80°C or higher, and if necessary, a crosslinking agent and other additives are added, followed by reaction at 50 to 80°C for 12 hours or more to obtain a solution of polymer (A). The weight average molecular weight (mw) of the obtained polymer, calculated as standard polystyrene, is preferably 10,000 or more, more preferably 20,000 or more, 30,000 or more, 40,000 or more, or 50,000 or more, since a low value leads to a low sensitivity of temperature response, and is preferably 300,000 or less, more preferably 200,000 or less, 150,000 or less, 100,000 or less, 90,000 or less, or 80,000 or less, since a high value is likely to lead to a low solubility or resolution. The mw value in the present invention is measured by gel permeation chromatography (GPC).
[0031] <Content of polymer (A)> In order to achieve good patterning characteristics, the polymer content may be 50 to 99 parts by mass, 60 to 98 parts by mass, or even 70 to 97 parts by mass or less per 100 parts by mass of the total solid content of the photosensitive resin composition excluding alcohol-based solvents.
[0032] <Plastic substrate> Examples of materials for the plastic substrate include resins (plastics). The resin may be any of natural resins, modified natural resins, and synthetic resins. Examples of natural resins include cellulose. Examples of modified natural resins include cellulose triacetate and cellulose with fixed dextran sulfate. Examples of synthetic resins include polyethylene, polypropylene, polyvinyl chloride, polystyrene, ABS, polyamide 6, polyamide 66, polyurethane, polylactic acid, polyacrylonitrile, polyvinylidene fluoride, polybutylene terephthalate, polyethylene terephthalate, polyvinyl acetate, poly(vinyl alcohol), ... Examples of the polyacrylate include butyl polyacrylate, ethyl polyacrylate, methyl polyacrylate, methyl polymethacrylate, polyester-based polymer alloys, polyvinyl alcohol, polyester, and polyethersulfone.
[0033] The plastic substrate used in the present invention may be a plastic having a glass transition temperature of 105° C. or lower. In particular, examples of "plastic having a glass transition temperature of 105° C. or lower" include polyethylene, polypropylene, polyvinyl chloride, polystyrene, ABS, polyamide 6, polyamide 66, polylactic acid, polyacrylonitrile, polyvinylidene fluoride, polybutylene terephthalate, polyethylene terephthalate, polyvinyl acetate, polybutyl acrylate, polyethyl acrylate, polymethyl acrylate, polymethyl methacrylate, etc. Among these plastics, polystyrene is preferable.
[0034] <Method for producing film (C) made of photocured composition and film-coated plastic substrate> The present invention provides a film (C) made of a photocured product of the photosensitive resin composition of the polymer (A), a plastic substrate with a film, a patterned plastic substrate with a film, and a method for producing the same. The film (C) made of a photocured product of the photosensitive resin composition of the polymer (A) is patterned to form a patterned film and the plastic substrate with a film. The film (C), the plastic substrate with a film, and the patterned plastic substrate with a film can be produced, for example, by the method described below. Step (1): A step of applying a solution containing the composition and an alcohol-based solvent to the surface of the plastic substrate to form a film. The photosensitive resin composition containing the polymer (A) of the present invention is dissolved in the alcohol-based solvent to obtain a solution containing the polymer (A) and the alcohol-based solvent. This solution is applied to a plastic substrate by a method such as spin coating or slit coating, and the solvent is removed to form a film. Step (2): Irradiating the film with light When light of a certain wavelength is irradiated through a mask using an aligner to obtain a desired pattern, photocuring occurs only in the light-irradiated portions. Step (3): Developing the film after light irradiation The film after the light irradiation is developed with a developer or the like, and the parts not irradiated with light (uncured parts of the coating film) are removed. Through these steps, a patterned plastic substrate with a film can be manufactured. Note that, regardless of whether or not the film is patterned, anything after the film is applied to the plastic substrate is referred to as a "plastic substrate with a film". Therefore, a patterned plastic substrate with a film is included in the category of plastic substrates with a film. According to the above-mentioned production method, a film made of a photocured product of the photosensitive resin composition of the polymer (A), a plastic substrate with a film, and a patterned plastic substrate with a film can be produced.
[0035] In "step (2): step of irradiating the film with light" of the production method of the present invention, the amount of exposure is adjusted according to the required film thickness and rate of curing. The light to be irradiated is preferably ultraviolet light or visible light of 600 nm or less, more preferably ultraviolet light. The wavelength is preferably 150 nm or more and 600 nm or less, more preferably 150 nm or more and 500 nm or less, and even more preferably 200 nm or more and 380 nm or less. The exposure dose is preferably 10 to 5,000 mj / cm. 2 , more preferably 50 to 3,000 mj / cm 2 , and more preferably 100 to 2,000 mj / cm 2 It is. The above-described production method of the present invention can provide a film made of a photocured product of a photosensitive resin composition as a temperature-responsive film having a desired response temperature, a plastic substrate with said film, and a patterned plastic substrate with a film. The film-attached plastic substrate and the patterned film-attached plastic of the present invention are also The film on the substrate may be on both sides of the plastic substrate, not just on one side.
[0036] <Patterning shape> There is no particular limit to the shape of the pattern formed on the patterned film, and examples of the shape include a square, a circle, a line, and a line and space when observed from above the substrate. There is no particular limit to the size of the pattern observed from above and the thickness (height) observed from the cross section of the pattern. The size of one side of the pattern is, for example, 0.1 μm to 1,000 mm, and the thickness (height) of the pattern is, for example, 5 nm to 1,000 μm. The shape of these patterns can be controlled by using multiple masks with different shapes of transmitted light during light irradiation.
[0037] <Cell culture support and method for producing same> The cell culture support of the present invention is a film made of a photocured film of a photosensitive resin composition containing a polymer, or a film which has been further patterned. The present invention also provides the cell culture support and a method for producing the same. The method for producing a cell culture support in the present invention is the same as the above-mentioned <Method for producing a film and a film-attached plastic substrate> using a photosensitive resin composition containing a polymer. The method is characterized by including a step of forming a coating film on a plastic substrate and irradiating the coating film with light to form a film made of a cured product or a further patterned film. The photosensitive resin composition does not contain an acid generator, and it is preferable that high-temperature baking is not performed after light irradiation. The photosensitive resin composition may also contain a crosslinking agent or other additives. The thickness (height) of the membrane as a cell culture support is preferably 1 to 100 nm, more preferably 2 to 50 nm, and even more preferably 3 to 30 nm, so that the cells are attached to the membrane during culture and the cultured cells are detached from the membrane by changing the temperature of the culture system when the cultured cells are recovered. There is no particular limitation on the size of the membrane observed from above, and the size of one side of the cured layer is, for example, 0.1 to 1,000 mm.
[0038] <Lower critical point temperature> In the present invention, the cell culture support has a lower critical solution temperature (LCST) in order to attach cells to the membrane during culture, and to detach the cultured cells from the membrane by changing the temperature of the culture system when recovering the cultured cells. The lower critical solution temperature is the temperature at which a solution separates into two phases above a certain temperature. In other words, in a system having a lower critical solution temperature, it is said that at temperatures below that temperature, multiple components exist in one phase regardless of their composition. The lower critical point temperature (LCST) value was determined by dissolving a polymer solution in phosphate buffered saline (Sigma-Aldrich) at a concentration of 2 wt %. Under a nitrogen atmosphere, the temperature of the aqueous solution was lowered at 1° C. / min, while measuring the differential heat with respect to the air using a differential scanning calorimetry (DSC) (DSC7020, SII Nano Technology Co., Ltd.), and the temperature showing the peak top of the measurement curve was calculated as the lower critical point temperature (LCST) of the polymer. The cell culture support of the present invention can be manufactured by changing the constituent units of the temperature-responsive polymer, so that the cell culture support has a lower critical temperature (LCST) of 15°C or more and less than 45°C. The cell culture support is a photosensitive resin composition using a temperature-responsive polymer containing two or more kinds of constituent units having different temperature responsiveness, and may have a pattern with two or more kinds of response temperatures. The cell culture support of the present invention can be any of the above cell culture supports.
[0039] <Cell culture method for cell culture support, etc.> In the present invention, the method and conditions for culturing cells on the cell culture support are not particularly limited, and cells can be cultured by a method known per se. The method for culturing cells uses the plastic substrate with the film, seeds cells on the cell culture support which is the film, and incubates the cells at a temperature suitable for culturing and higher than the lower critical point temperature of the cell culture support, thereby culturing the cells. Then, the temperature of the cured product layer is adjusted to a temperature lower than the lower critical point temperature of the polymer, and the cells are detached from the cell culture support and recovered to perform the culturing.
[0040] In the present invention, the cells are not particularly limited, and various cells can be cultured. Examples of the cells include epithelial cells and endothelial cells that constitute each tissue and organ in the body; skeletal muscle cells, smooth muscle cells, and cardiomyocytes that exhibit contractility; neurons and glial cells that constitute the nervous system; fibroblasts; hepatocytes, non-parenchymal liver cells, and adipocytes related to metabolism in the body; stem cells present in various tissues, as well as bone marrow cells and ES cells, etc. In the present invention, there is no particular limitation on the method for seeding cells or the method for recovering the cultured cells detached from the cell culture support, and a method known per se can be used.
Examples
[0041] Hereinafter, the present invention will be described more specifically with reference to examples. However, the present invention is not limited by the following examples, and it is of course possible to appropriately modify and implement it within the range that can conform to the above and below gists, and all of them are included in the technical scope of the present invention.
[0042] <a. Synthesis of polymer and monomer> <Synthesis Example 1> 10 g of N-isopropylacrylamide and 0.73 g of 4-benzoylphenyl methacrylate were dissolved in 25.3 g of 1-propanol, and the temperature was raised to 70° C. Then, while maintaining the reaction solution at 70° C., 0.11 g of azobisisobutyronitrile was added, and the mixture was reacted at 70° C. for 24 hours to obtain a solution of a copolymerized polymer compound of N-isopropylacrylamide and 4-benzoylphenyl methacrylate. When the obtained copolymerized polymer compound was subjected to GPC analysis, the weight average molecular weight was 75,600 in terms of standard polystyrene. [ka]
[0043] <Synthesis Example 2> 10 g of N-isopropylacrylamide and 0.24 g of 4-benzoylphenyl methacrylate were dissolved in 24.1 g of 1-propanol, and the temperature was raised to 70° C. Then, while maintaining the reaction solution at 70° C., 0.10 g of azobisisobutyronitrile was added, and the mixture was reacted at 70° C. for 24 hours to obtain a solution of a copolymerized polymer compound of N-isopropylacrylamide and 4-benzoylphenyl methacrylate. When the obtained copolymerized polymer compound was subjected to GPC analysis, the weight average molecular weight was 57,700 in terms of standard polystyrene. [ka] <Synthesis Example 3> 25 g of N-isopropylacrylamide and 0.3 g of 4-benzoylphenyl methacrylate were dissolved in 59.6 g of 1-propanol, and the temperature was raised to 70° C. Then, while maintaining the reaction solution at 70° C., 0.25 g of azobisisobutyronitrile was added, and the mixture was reacted at 70° C. for 24 hours to obtain a solution of a copolymerized polymer compound of N-isopropylacrylamide and 4-benzoylphenyl methacrylate. When the obtained copolymerized polymer compound was subjected to GPC analysis, the weight average molecular weight was 44,200 in terms of standard polystyrene. [ka]
[0044] <Comparative Synthesis Example 1> After dissolving 20 g of N-isopropylacrylamide in 47.6 g of 1-propanol, the temperature was raised to 75°C. Then, while maintaining the reaction solution at 75°C, 0.4 g of azobisisobutyronitrile was added and reacted at 75°C for 24 hours to obtain a solution of the N-isopropylacrylamide polymer compound. When GPC analysis of the obtained copolymerized polymer compound was performed, the weight average molecular weight in terms of standard polystyrene was 30,800.
Chemical formula
[0045] <Comparative Synthesis Example 2> After dissolving 20 g of N-isopropylacrylamide and 5.13 g of 2-hydroxyethyl acrylate in 101.5 g of 1-propanol, the temperature was raised to 80°C. Then, while maintaining the reaction solution at 80°C, 0.25 g of azobisisobutyronitrile was added and reacted at 80°C for 24 hours to obtain a solution of the copolymerized polymer compound of N-isopropylacrylamide and 2-hydroxyethyl acrylate. When GPC analysis of the obtained copolymerized polymer compound was performed, the weight average molecular weight in terms of standard polystyrene was 23,000.
Chemical formula
[0046] <b. Preparation of Composition> <Compositions 1 - 2> After adding 16.7 g of 1-propanol to 3.3 g of the solution containing 1.0 g of the reaction product obtained in Synthesis Examples 1 - 2, filtration was performed using a polyethylene microfilter with a pore size of 0.10 μm to prepare a photocurable resin composition solution. <Composition 3> After adding 33.5 g of 1-propanol to 1.0 g of the solution containing 0.3 g of the reaction product obtained in Synthesis Example 3, filtration was performed using a polyethylene microfilter with a pore size of 0.10 μm to prepare a photocurable resin composition solution. <Composition 4> After adding 41.9 g of 1-propanol to 2.0 g of a solution containing 0.6 g of the reaction product obtained in Synthesis Example 3, the mixture was filtered using a polyethylene microfilter with a pore size of 0.10 μm to prepare a photocurable resin composition solution.
[0047] <Comparative Composition 1> After adding 16.7 g of 1-propanol to 3.3 g of a solution containing 1.0 g of the reaction product obtained in Comparative Synthesis Example 1, the mixture was filtered using a polyethylene microfilter with a pore size of 0.10 μm to prepare a photocurable resin composition solution.
[0048] <Comparative Composition 2> To 10 g of a solution containing 2 g of the reaction product obtained in Comparative Synthesis Example 2, 0.1 g of α-(methylsulfonyloxyimino)-4-methoxybenzyl cyanide (trade name: PAI-1001, manufactured by Midori Chemical Co., Ltd.), 0.03 g of 1,3,4,6-tetrakis(methoxymethyl) glycoluril, and 0.52 g of 1-propanol were added, and the mixture was filtered using a polyethylene microfilter with a pore size of 1.0 μm to prepare a photocurable resin composition solution.
[0049] <c. Preparation of plastic substrate (polystyrene film)> Polystyrene petri dish (IWAKI 35 mm Non treated Dish) was dissolved in propylene glycol monomethyl ether acetate and filtered using a polyethylene microfilter with a pore size of 1.0 μm to prepare a 3.5 wt% polystyrene solution. The solution was applied onto a silicon wafer substrate by a spinner. It was baked on a hot plate at 180 °C for 1 minute to form a coating film with a film thickness of 100 nm. The obtained film was exposed to 1-propanol for 1 minute, then spin-dried and baked at 100 °C for 1 minute. When the film thickness was measured, it showed 100 nm, indicating resistance to exposure to 1-propanol.
[0050] <d. Sensitivity measurement> The photocurable resin composition solutions prepared from Compositions 1 to 2 and Comparative Composition 1 were applied onto a silicon wafer and a polystyrene film prepared at c using a spinner. On a hot plate They were baked at 50 °C for 1 minute to form a coating film with a film thickness of 330 nm. (The coating films formed from Compositions 1 to 2 were used as Examples 1 to 2, and the coating film formed from Comparative Composition 1 was used as Comparative Example 1.) After irradiating with 254 nm light by an aligner while changing the exposure dose, the remaining film thickness was measured after development with 1-propanol. In Examples 1 and 2, the remaining film thickness was not stable for each exposure dose on the silicon wafer, but on the polystyrene film, it was stable and showed good sensitivity behavior with a high remaining film ratio. In Comparative Example 1 having no benzophenone structure, no remaining film was shown. Comparative Composition 2 was applied onto a polystyrene substrate. It was baked at 50 °C for 1 minute on a hot plate, irradiated with 365 nm light by an aligner (PLA-501 manufactured by Canon) while changing the exposure dose, then post-exposure bake (PEB) was performed, and a photocured film was formed by developing with 1-propanol. However, in PEB, a temperature of 100 °C or higher was required, exceeding the heat resistance temperature of the polystyrene petri dish, so deformation of the polystyrene petri dish was observed during PEB. The sensitivity behavior on the polystyrene film is shown in Fig. 1. The sensitivity behavior on the silicon wafer is shown in Fig. 2.
[0051] <e. Patterning test> The polymer solution of Synthesis Example 1 was filtered using a polyethylene microfilter with a pore size of 1.0 μm to prepare a photocurable resin composition solution. The prepared solution was applied onto a polystyrene film prepared at c using a spinner. It was baked at 50 °C for 1 minute on a hot plate to form a coating film with a film thickness of 3.4 μm. Through a mask with a dot pattern (dot / space = 10 μm / 15 μm) drawn by an aligner, it was irradiated with 254 nm light at 1000 mJ / cm2. Then, after developing with 1-propanol for 3 minutes, it was spin-dried, and the pattern was observed with an electron microscope. The electron micrograph is shown in Fig. 3. As a result, good patterning performance was shown.
[0052] <Erosion test of polystyrene Petri dish> The comparative composition 2 was put into a polystyrene Petri dish (35 mm Non treated Dish manufactured by IWAKI), and an attempt was made to coat it, but the Petri dish dissolved. In Compositions 1 to 2 and Comparative Composition Example 1 in which 1-propanol was changed from propylene glycol monomethyl ether, the Petri dish was not dissolved.
[0053] <G. Measurement of lower critical solution temperature of reaction product> The reaction products obtained in Synthesis Examples 1 and 2 were each dissolved in pure water at a concentration of 10% by weight. Under a nitrogen atmosphere, differential thermal measurement was performed using a differential scanning calorimeter (Differential scanning calorimetry, DSC) (SII NanoTechnology Inc. "DSC7020") while raising the temperature of the aqueous solution at 1 °C / min, and the temperature at the peak top of the obtained measurement curve was calculated as the lower critical solution temperature (LCST) of the reaction product in pure water. The obtained measurement curves are shown in FIGS. 4 and 5. The lower critical solution temperatures (LCST) of the reaction products obtained in Synthesis Examples 1 and 2 in pure water were 23.8 °C and 28.9 °C, respectively. In addition, measurement was performed in the same manner as above except that pure water was changed to phosphate buffered saline (PBS), and the lower critical solution temperatures (LCST) of the reaction products obtained in Synthesis Examples 1 and 2 in phosphate buffered saline were calculated. The obtained measurement curves are shown in FIGS. 6 and 7. The lower critical solution temperatures (LCST) of the reaction products obtained in Synthesis Examples 1 and 2 in phosphate buffered saline were 21.6 °C and 26.6 °C, respectively.
[0054] <H. Measurement of swelling degree of photocured film> The photocurable resin composition solution prepared with Composition 2 was applied onto the polystyrene film prepared at c using a spinner. It was baked on a hot plate at 50°C for 1 minute to form a coating film with a film thickness of 11 μm. After irradiating with 254 nm light at 3000 mJ / cm2 using an aligner, it was developed with 1-propanol for 3 minutes and then spin-dried. Next, the substrate was scratched with a diamond pen and split, and it was set on the temperature-controlled stage of an inverted microscope (Olympus Corporation, IX71) so that the cross-sectional direction faced downward. Thereafter, phosphate buffered saline (PBS) was dropped, and while the cross-sectional part was immersed in the phosphate buffered saline, the substrate temperature was changed and the change in film thickness was observed. The observation results are shown in Fig. 8. At 36°C, which is higher than the lower critical solution temperature (LCST) of 26.6°C in phosphate buffered saline of the reaction product obtained in Synthesis Example 2 constituting the photocured film, the film thickness was 11 μm, whereas when the temperature was lowered to 18°C, which is lower than the lower critical solution temperature (LCST), swelling occurred and the film thickness increased to 100 μm. The swelling degree (film thickness at swelling / film thickness at shrinkage) was 909%. Subsequently, when the temperature was raised again to 36°C, which is higher than the lower critical solution temperature (LCST), shrinkage occurred and the film thickness returned to 11 μm. This swelling and shrinkage could be reversibly repeated. Also, observation was carried out in the same manner as above except that the photocurable resin composition solution prepared with Composition 2 was changed to the photocurable resin composition solution prepared with Composition 1, and the swelling degree of the photocured film prepared using Composition 1 was determined. At 36°C, which is higher than the lower critical solution temperature (LCST) of 21.6°C in phosphate buffered saline of the reaction product obtained in Synthesis Example 1 constituting the photocured film, the film thickness was 11 μm, whereas when the temperature was lowered to 18°C, which is lower than the lower critical solution temperature (LCST), swelling occurred and the film thickness increased to 30 μm. The swelling degree (film thickness at swelling / film thickness at shrinkage) was 272%. Subsequently, when the temperature was raised again to 36°C, which is higher than the lower critical solution temperature (LCST), shrinkage occurred and the film thickness returned to 11 μm. This swelling and shrinkage could be reversibly repeated.
[0055] <i. Cell detachment test on the photocured film> The photocurable resin composition solutions prepared in Compositions 3 and 4 were applied to a 35 mm polystyrene cell culture dish (Corning, 353001) using a spinner. The dish was baked on a hot plate at 50°C for 1 minute to form a coating film with a thickness of 5-10 nm or 11-22 nm. After irradiating the dish with 254 nm light at 1000 mJ / cm2 using an aligner, the dish was developed with 1-propanol for 1 minute, washed with pure water, and dried at 50°C. Mouse-derived fibroblast cells (KAC Co., Ltd., EC99072801-F0, 10T1 / 2 cells) were used. The medium used was Basal Medium Eagle (Thermo Fisher Scientific, 21010-046) supplemented with 10v / v% FETAL BOVINE SERUM (Nichirei Biosciences, 175012) and 1v / v% Penicillin-Streptomycin-Glutamine (Thermo Fisher Scientific, 10378-016). 6 Cells were seeded at 35 cells / 35 mm petri dish and cultured at 37°C and 5% CO2 for 24 hours. After culture, the 35 mm petri dish was placed on a 22°C stand, and the cell adhesion state was confirmed 0 to 10 minutes later using an optical microscope and visual inspection. [Figures 9a to 9d are photographs of a 5-10 nm thick film of composition 3 placed on a 22°C stand from 37°C to 0 to 10 minutes later. Figures 9a and 9b are optical microscope photographs of the upper left periphery of the petri dish, and Figures 9c and 9d are photographs of the entire petri dish. Figures 10a and 10b are optical microscope photographs of a 11-22 nm thick film of composition 3 placed at 37°C (Figure 10a) and a photograph of the entire petri dish (Figure 10b). As a result, as shown in Figure 9, when the film thickness was 5-10 nm, 10T1 / 2 cells adhered to a 35 mm petri dish coated with Composition 3 at 37°C, and when the temperature was lowered to 22°C, the cells began to detach from the edge of the dish (Figure 9b), and after 10 minutes, they were completely detached (Figure 9d). On the other hand, when the film thickness was 11-22 nm, no adhesion of 10T1 / 2 cells was observed even at 37°C (Figure 10b). [Explanation of symbols]
[0056] 1. Phosphate Buffered Saline (PBS) 2 Membrane 3. Substrate
Claims
1. A film-attached plastic substrate having a film (C) made of a photocured product of a composition on a surface of the plastic substrate, The composition contains a polymer (A) having a structural unit represented by the following formula (1): The composition may comprise an optionally substituted aryl ketone (B), When the aryl ketone (B) is not included in the composition, the polymer (A) has a residue of the aryl ketone (B); When the aryl ketone (B) is contained in the composition, the polymer (A) may have a residue of the aryl ketone (B). 【Chemistry 1】 (In formula (1), R 1 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, R 2 represents an optionally substituted alkyl group having 1 to 10 carbon atoms.
2. The film-attached plastic substrate according to claim 1, wherein the aryl ketone (B) is an aryl ketone selected from the group consisting of acetophenone, benzophenone, anthraquinone, anthrone, a compound represented by the following formula (2), an anthrone analogue in which any carbon atom on the ring of the compound represented by formula (2) is replaced with a heteroatom, and derivatives of these compounds. 【Chemistry 2】 (In formula (2), R 3 ~R 6 each independently represents a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, a hydroxy group, a sulfo group, a vinyl group, an acetoxy group, an aryl group having 6 to 14 carbon atoms which may be substituted with a hydroxy group, an amino group, or a mono- or di-alkylamino group having 1 to 4 carbon atoms, X is -O-, -S-, >CH 2 , >C=O or >N-R, where R represents a hydrogen atom, a hydrocarbon group or an acyl group; n1 represents 0 or 1, and n2 to n5 each independently represent 0, 1, 2, or 3, and n2 + n3 ≦ 3, n4 + n5 ≦ 4 are satisfied.
3. The film-attached plastic substrate according to claim 1 , wherein the polymer (A) is a polymer having a structural unit represented by the following formula (3): 【Chemistry 3】 【Chemistry 4】 In formula (3), Ar represents a group represented by formula (4), formula (5), or formula (6), R 1 and R 7 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, R 2 represents an optionally substituted alkyl group having 1 to 10 carbon atoms, L represents a divalent linking group; x and y are arbitrary numbers satisfying x+y≦1, 0<x<1, and 0<y<1, respectively. In formulas (4) to (6), * represents a bond to L. R 3 ~R 6 each independently represents a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, a hydroxy group, a sulfo group, a vinyl group, an acetoxy group, an aryl group having 6 to 14 carbon atoms which may be substituted with a hydroxy group, an amino group, or a mono- or di-alkylamino group having 1 to 4 carbon atoms, X is -O-, -S-, >CH 2 , >C=O or >N-R, where R represents a hydrogen atom, a hydrocarbon group or an acyl group; n1 represents 0 or 1, and n2 to n5 each independently represent 0, 1, 2, or 3, and n2 + n3 ≦ 3, n4 + n5 ≦ 4 are satisfied.
4. The film-attached plastic substrate according to claim 3 , wherein in the formula (3), 0.01≦y / x≦0.2 is satisfied.
5. The film-attached plastic substrate according to claim 1 , wherein the optionally substituted aryl ketone (B) has a molecular weight of 500 or less.
6. The film-attached plastic substrate according to claim 1 , wherein the film (C) is a patterned film.
7. The film-attached plastic substrate according to claim 1 or 6, wherein the plastic substrate has a glass transition temperature of 105°C or lower.
8. A method for producing a film-coated plastic substrate, comprising: a step (1) of applying a solution containing the composition and an alcohol-based solvent to a surface of the plastic substrate to form a coating film; and a step (2) of irradiating the coating film with light.
9. The method for producing a film-coated plastic substrate according to claim 8, further comprising a step (3) of developing the coating film after the light irradiation.
10. The method for producing a film-coated plastic substrate according to claim 8 or 9, wherein the wavelength of the light in the step (2) is 150 nm or more and 600 nm or less.
Citation Information
Patent Citations
Photosensitive composition, patterned substrate, cell culture support, and cultured cell production method
WO2016068271A1
Substrate covered with polymers for selective separation of cells or for cell culturing