Resin composition

By blending aromatic polyetherketone resin with polar engineering plastics, a homogeneous and high-heat-resistant resin composition is achieved, addressing the issue of insufficient heat resistance in PEEK resin blends.

JP2024146923APending Publication Date: 2024-10-15MITSUBISHI CHEM CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024057678
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-29
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

PEEK resin blends with high Tg materials fail to achieve homogeneous mixtures, resulting in insufficient heat resistance improvement due to the dominance of the lowest Tg in the resin composition.

Method used

A blend composition of aromatic polyetherketone resin with a predetermined polar engineering plastic, such as polyphenylsulfone, polyimide, or polyetherimide, is formulated to enhance heat resistance by ensuring compatibility and increasing the glass transition temperature of the resulting resin.

Benefits of technology

The resin composition achieves improved heat resistance, allowing for higher Tg values and enhanced mechanical properties, suitable for applications requiring thermal stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024146923000001
    Figure 2024146923000001
  • Figure 2024146923000002
    Figure 2024146923000002
  • Figure 2024146923000003
    Figure 2024146923000003
Patent Text Reader

Abstract

To address the issue where certain types of PAEK resin may lack sufficient heat resistance depending on the type and to provide a resin composition that avoids problems in crystallinity when used as a material.SOLUTION: A resin composition comprises a predetermined aromatic polyether ketone resin and at least one polar engineering plastic.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition. [Background technology]

[0002] Aromatic polyether ketone resins (hereinafter referred to as "PAEK resins") are so-called super engineering plastics (hereinafter referred to as "super engineering plastics") that have excellent mechanical properties such as heat resistance, chemical resistance, toughness, and dimensional stability, and are widely used in electrical and electronic parts, automotive parts, medical parts, fibers, films, and other applications.

[0003] For example, aromatic polyether ether ketone resin (hereinafter referred to as "PEEK resin"), which is one type of PAEK resin, has two ether moieties and one ketone moiety in the repeating structure of the resin, and is known to exhibit high mechanical properties as a partially crystalline resin due to their high order regularity (Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 54-90296 Summary of the Invention [Problem to be solved by the invention]

[0005] PEEK resin has a Tg of about 155°C, and when it is used in applications that require heat resistance, it is necessary to adjust the Tg higher. One way to improve the heat resistance of a material is to blend it with a material that has a higher Tg. When a resin composition has multiple Tgs, the practical heat resistance of the composition is often governed by the lowest Tg. However, when PEEK resin is blended with other resins having high Tgs, a homogeneous mixture is not obtained, and the resulting resin composition still has the Tg derived from PEEK, resulting in insufficient improvement in heat resistance.

[0006] That is, an object of the present invention is to solve the above-mentioned conventional problems, to improve the heat resistance of an aromatic polyether ketone resin, and to provide a resin composition having improved heat resistance. [Means for solving the problem]

[0007] Therefore, the present inventors have discovered that a resin composition with improved heat resistance can be obtained by blending a certain PAEK resin, which has insufficient heat resistance, with a certain other resin, and have completed the following invention.

[0008] That is, the gist of the present invention resides in the following [1] to [8]. [1] A resin composition comprising an aromatic polyether ketone resin containing a repeating unit represented by the following general formula (1) and at least one polar engineering plastic:

[0009] [ka] (In the formula (1), Structure A is any one selected from the group consisting of the following general formulae (2), (3) and (4), and Structure B is an optionally substituted divalent aromatic hydrocarbon ring.)

[0010] [ka]

[0011] [2] The resin composition according to [1], wherein Structure A is represented by the general formula (2). [3] The resin composition according to [1] or [2], wherein the polar engineering plastic has a functional group containing a heteroatom in its skeleton.

[0012] [4] The resin composition according to any one of [1] to [3], wherein the polar engineering plastic has one or more functional groups in the main chain selected from the group consisting of a sulfonyl group, a sulfinyl group, an ether group, a thioether group, an imide group, an amide group, an ester group, a carbonate group, and an imidazole ring. [5] The resin composition according to any one of [1] to [4], wherein the polar engineering plastic is substantially amorphous.

[0013] [6] The resin composition according to any one of [1] to [5], wherein the polar engineering plastic is selected from the group consisting of polyphenylsulfone, polyimide, and polyetherimide. [7] The resin composition according to any one of [1] to [6], wherein Tg2-Tg1≧5(°C), where Tg1 is the glass transition temperature of the aromatic polyether ketone resin containing a repeating unit represented by the general formula (1) and Tg2 is the glass transition temperature of the resin composition.

[0014] [8] The resin composition according to any one of [1] to [7], wherein Tg2-Tg3≧1 (°C), where Tg3 is the calculated glass transition temperature of the aromatic polyether ketone resin containing a repeating unit represented by the general formula (1) and Tg2 is the glass transition temperature of the resin composition. Effect of the Invention

[0015] According to the present invention, a resin composition having improved heat resistance can be obtained by preparing a blend composition of a specific aromatic polyether ketone resin having insufficient heat resistance and at least one type of polar engineering plastic. By providing a resin composition with improved heat resistance, it becomes possible to suitably use the composition in applications requiring heat resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The present invention will be described in detail below, but the present invention is not limited to the following description, and can be modified in any manner without departing from the gist of the present invention. In this specification, when "A to B" is used with a numerical value or a physical property value between the front and back of the expression (A and B represent numerical values ​​or physical property values), this means "A or more and B or less," and preferably means "more than A but less than B."

[0017] Furthermore, the term "aromatic" encompasses "heteroaromatic" and also encompasses forms containing a heteroatom, which is an element other than carbon, in the ring structure.

[0018] The following describes in detail an embodiment of the present invention. The description of the components described below is an example (representative example) of an embodiment of the present invention, and the present invention is not limited to the following content as long as it does not exceed the gist of the present invention.

[0019] <Resin composition> The resin composition of the present invention is a resin composition comprising a specified aromatic polyether ketone resin and at least one type of polar engineering plastic.

[0020] (Aromatic polyether ketone resin) The predetermined aromatic polyether ketone resin in the present invention is an aromatic polyether ketone resin containing a repeating unit represented by the following general formula (1). Here, the term "polyetherketone" is not limited to polyetherketone in the narrow sense, which contains one ether bond and one ketone bond in one repeating unit, but refers to polyetherketone in the broad sense. The broad sense of polyetherketone means that it may include a resin skeleton that may have multiple ether bonds and multiple ketone bonds in one repeating unit, such as polyetherketone (PEK), polyetheretherketone (PEEK), polyetherketoneketone (PEKK), polyetheretherketoneketone (PEEKK), and polyetherketoneetherketoneketone (PEKEKK).

[0021] [ka]

[0022] In the formula (1), the structure A is any one selected from the group consisting of the following formulae (2), (3) and (4), and the structure B is an optionally substituted divalent aromatic hydrocarbon ring. In the figure, * indicates a binding site.

[0023] [ka]

[0024] Specific examples of the structure A include the following.

[0025] [ka]

[0026] The structure A is preferably the above general formula (2). In this way, by using PAEK (FDCA-PAEK) having furandicarboxylic acid (FDCA) as a structural unit as a component of the resin composition, the FDCA can be obtained from bio-derived raw materials, thereby reducing the environmental load.

[0027] The optionally substituted divalent aromatic hydrocarbon ring of structure B is preferably a substituted or unsubstituted aromatic hydrocarbon ring having 6 to 30 carbon atoms. A structure in which a plurality of aromatic hydrocarbon rings are linked may also be used, but the linkage of the aromatic hydrocarbon rings is preferably a direct linkage of the aromatic rings, or when the linkage is via a substituent, the substituent preferably does not contain an ether group. Moreover, it is more preferable that the aromatic hydrocarbon ring is unsubstituted.

[0028] Specifically, the structure B is preferably any one selected from the group consisting of the following general formulae (5) to (14).

[0029] [ka]

[0030] In formula (7), n1 is preferably 0 or 1. In formula (12), R1 and R2 are the same or different aliphatic or aromatic hydrocarbon groups, each of which may have an alicyclic skeleton or an aromatic skeleton and may have a substituent.

[0031] More specifically, the structure B includes the following formulae B-1 to B-17.

[0032] [ka]

[0033] As the structure B, B-1, B-5, B-6, B-7, B-8, B-9, B-13, B-14, B-15, B-16, and B-17 are preferred, and among them, B-1, B-5, and B-6 are more preferred. The aromatic polyether ketone resin X containing the repeating unit represented by the general formula (1) may have two or more types of structures B, and among these, preferably, the aromatic polyether ketone resin X may contain two or more types selected from B-1, B-5, B-6, B-7, B-8, B-9, B-13, B-14, B-15, B-16, and B-17, and more preferably, the aromatic polyether ketone resin X may contain two or more types selected from B-1, B-5, and B-6.

[0034] Specific examples of the repeating unit represented by formula (1) are given below.

[0035] [ka]

[0036] [ka]

[0037] [ka]

[0038]

change

[0039]

change

[0040]

change

[0041]

change

[0042]

change

[0043]

change

[0044]

change

[0045]

change

[0046]

change

[0047]

change

[0048] Among the above specific examples, from the viewpoint that a homogeneous resin having the desired heat resistance can be easily obtained by using the resin composition of the present invention, the aromatic polyether ketone resin in the present invention preferably has repeating units represented by (1)-1, (1)-2, (1)-3, (1)-4, or (1)-5, and particularly preferably has repeating units represented by (1)-1 or (1)-2, or both repeating units of (1)-1 and (1)-2.

[0049] The reduced viscosity of the aromatic polyether ketone resin in the present invention is usually 0.6 dL / g or more. Also, it is preferably 0.8 dL / g or more, and particularly preferably 0.9 dL / g or more. By setting it in such a range, a resin or resin composition having sufficient mechanical strength can be obtained. On the other hand, the reduced viscosity of the aromatic polyether ketone resin in the present invention is usually 3.5 dL / g or less, preferably 3.0 dL / g or less, more preferably 2.5 dL / g or less, even more preferably 2.0 dL / g or less, particularly preferably 1.9 dL / g or less, particularly preferably 1.8 dL / g or less, particularly preferably 1.7 dL / g or less, and most preferably 1.6 dL / g or less. By setting it in such a range, it becomes easier to mix when mixed with other resins, and the resin and resin composition can be melt-molded under simple conditions. In addition, when the resin or resin composition is handled in a solution state, it becomes easier to handle it at a higher concentration, so the amount of organic solvent to be handled can be reduced, which is preferable from the viewpoint of reducing environmental load.

[0050] The reduced viscosity (ηsp / c) of the aromatic polyetherketone resin in the present invention is calculated by dissolving the resin in concentrated sulfuric acid at a concentration c=0.1 g / dL, measuring the specific viscosity (ηsp) at 25°C using an Ubbelohde viscometer (manufactured by Moritomo Rika Kogyo Co., Ltd.), and dividing the measured value by the concentration c. It is known that the reduced viscosity correlates with the molecular weight of the resin, and it is common to compare the molecular weight of aromatic polyetherketone resins relatively using reduced viscosity values. In other words, in the present invention, an aromatic polyetherketone resin with a reduced viscosity of 0.6 dL / g or more indicates that the molecular weight is sufficiently high to the extent that the properties are not significantly changed by molding processing.

[0051] (Polar Engineering Plastics) The resin composition of the present invention is a resin composition obtained by blending the above-mentioned specific aromatic polyether ketone resin with at least one type of polar engineering plastic. The resin composition of the present invention may contain one type of polar engineering plastic, or may contain two or more types of polar engineering plastics. The two or more types of polar engineering plastics may be, for example, a mixture of different resins, such as a mixture of polyetherimide and polyimide, which will be exemplified later, or a mixture of the same type of resins with different properties, such as a mixture of multiple types of polyetherimides of different grades (e.g., different molecular weights).

[0052] It is preferred that the polar engineering plastics have the following properties: -Prescribed glass transition temperature -Substantially amorphous -Has affinity with aromatic polyether ketone resin -Having a specified molecular weight

[0053] The glass transition temperature of the polar engineering plastic is preferably higher than the glass transition temperature of the aromatic polyether ketone resin, and in particular, it is preferably 150°C or higher and 300°C or lower, more preferably 160°C or higher and 280°C or lower, and even more preferably 170°C or higher and 270°C or lower.

[0054] It is preferable that the polar engineering plastic is substantially amorphous. Substantially amorphous means that it has no crystallinity at all, or that even if it has crystallinity, crystallization does not proceed under normal molding conditions or usage environments. Crystallinity may be evaluated by the magnitude of heat of fusion detected by differential scanning calorimetry (DSC), or by confirming the degree of crystallinity by a method such as X-ray diffraction. When no endotherm due to melting of the resin is observed during the temperature rise process in DSC evaluation, or the amount of endotherm is very small (for example, ≦3 J / g), or when no diffraction peak due to the crystalline phase is observed in X-ray diffraction, or the diffraction peak is very weak, the resin can be considered to be substantially amorphous.

[0055] It is preferable that the polar engineering plastic has a molecular weight of a certain level or more, and as a result, it is preferable that the melt viscosity is the same as that of aromatic polyether ketone resin. If it deviates from the above preferable range, it may cause problems such as poor flowability during melt molding, difficulty in mixing during kneading, and non-uniformity. For example, in the case of PPSU resin, the melt viscosity at 365°C measured in the same manner is preferably 100 to 1200 Pa·s, more preferably 200 to 1000 Pa·s, and even more preferably 400 to 800 Pa·s. In the case of PI resin, the melt viscosity at 345°C measured in the same manner is preferably 200 to 2000 Pa·s, more preferably 300 to 1800 Pa·s, and even more preferably 600 to 1500 Pa·s. In the case of PEI resin, the melt viscosity at 400°C measured in the same manner is preferably 100 to 1000 Pa·s, more preferably 200 to 800 Pa·s, and even more preferably 300 to 700 Pa·s.

[0056] Polar engineering plastic construction Polar engineering plastics is a general term for engineering plastics that have a polar skeleton in the molecular skeleton, and preferably have a functional group containing a heteroatom in the skeleton. Examples of these functional groups include sulfonyl groups, sulfinyl groups, ether groups, thioether groups, imide groups, amide groups, ester groups, carbonate groups, and imidazole rings, and polar engineering plastics preferably have one or more of these functional groups. In addition, among the functional groups containing heteroatoms, it is preferable to have a sulfonyl group, a sulfinyl group, an imide group, an amide group, an ester group, a carbonate group, and an imidazole ring.

[0057] As the polar engineering plastics, for example, preferably, polyphenylsulfone, polyimide, and polyetherimide are used, more preferably, polyimide and polyetherimide are used, and particularly preferably, polyetherimide is used.

[0058] (Composition of Resin Composition) The composition of the resin composition of the present invention can be adjusted depending on the desired glass transition temperature of the resin composition. In other words, by adjusting the composition of the resin composition, it is possible to set the glass transition temperature of the resulting resin composition to a desired value. In the composition of the resin composition of the present invention, the proportion of the aromatic polyether ketone resin containing a repeating unit represented by general formula (1) can be appropriately adjusted according to the desired glass transition temperature, to be 10 mass% or more and 90 mass% or less, 20 mass% or more and 80 mass% or less, 30 mass% or more and 70 mass% or less, or 40 mass% or more and 60 mass% or less, based on the entire resin composition. In order to obtain a resin composition that utilizes the properties of the aromatic polyether ketone resin, the composition preferably contains the aromatic polyether ketone as a main component. Specifically, the content of the aromatic polyether ketone resin is preferably 50% by mass or more, more preferably 60% by mass or more, and particularly preferably 70% by mass or more, based on the entire resin composition. The physical properties of homogeneous resin compositions are generally considered to be additive, and the Fox formula is known as a method for estimating the glass transition temperature. As a general rule, when the polar engineering plastic has a higher Tg, the more the amount of polar engineering plastic is increased, the higher the glass transition temperature of the resulting resin composition can be.

[0059] (Thermal properties of resin composition) The glass transition temperature (Tg) of the resin composition of the present invention was measured using a differential scanning calorimeter "DSC7020" (manufactured by Hitachi High-Tech Science Corporation) by heating about 2 mg of the resin composition from 30°C to 360°C at a rate of 10°C / min (1st heating), cooling from 360°C to 30°C at a rate of 10°C / min (1st cooling), and further heating from 30°C to 360°C at a rate of 10°C / min (2nd heating). When Tg could be measured in the first heating, the measured Tg was regarded as the Tg of the resin composition. When Tg could not be measured in the first heating, Tg was further measured in the second heating, and the measured Tg was regarded as the Tg of the resin composition.

[0060] In a resin composition formed by blending multiple resins, when the resin composition has multiple glass transition temperatures, the practical heat resistance of the resin composition is governed by the lowest glass transition temperature. Therefore, even if a resin composition is formed by mixing a resin component A having a low glass transition temperature and a resin component B having a high glass transition temperature, if the resin composition is not a homogeneous mixture, the practical heat resistance of the resin composition will depend on the low glass transition temperature of the resin component A or the phase mainly containing the resin component A.

[0061] In the resin composition of the present invention, a compatible resin composition (mixture) can be obtained by mixing a specific aromatic polyether ketone resin with at least one polar engineering plastic. This makes it possible to improve the practical heat resistance of the resulting resin composition. Here, "compatible" includes "homogeneous compatibility" and "partial compatibility". A "homogeneously compatible resin composition" means that a single phase is formed by mixing and that a single Tg is shown in the DSC measurement by the above method. A "partially compatible resin composition" means that the composition is in a multiphase state with some remaining non-uniform regions, and that a single or multiple Tg is observed in the DSC measurement depending on the content ratio of the current resin in each phase. In either case, the Tg of the composition is generally considered to appear between the Tg of the raw aromatic polyether ketone resin and the Tg of the polar engineering plastic. The resin composition of the present invention is preferably a homogeneous, compatible resin composition.

[0062] When the glass transition temperature detected when the aromatic polyether ketone resin containing the repeating unit represented by the general formula (1) is measured alone is Tg1, and the glass transition temperature of the resin composition (the lowest temperature when multiple glass transition temperatures are observed) is Tg2, it is preferable that Tg2-Tg1 ≧ 5 (°C), it is preferable that Tg2-Tg1 ≧ 6 (°C), it is more preferable that Tg2-Tg1 ≧ 10 (°C), it is more preferable that Tg2-Tg1 ≧ 11 (°C), it is more preferable that Tg2-Tg1 ≧ 15 (°C), it is particularly preferable that Tg2-Tg1 ≧ 20 (°C), and it is most preferable that Tg2-Tg1 ≧ 25 (°C). By setting it in such a range, a resin composition having sufficiently improved practical heat resistance can be obtained compared to the aromatic polyether ketone resin before composition.

[0063] When polyether ether ketone resin (PEEK), which is a type of aromatic polyether ketone resin, is mixed with polar engineering plastics, it is difficult to obtain a homogeneous mixture, and the resulting resin composition tends to still exhibit a low glass transition temperature derived from PEEK. For this reason, the practical heat resistance of the resin composition remains low. In contrast, the resin composition of the present invention can be made into a resin mixture that exhibits a higher Tg than the raw aromatic polyether ketone resin as described above. The inventors of the present invention presume that the reason for this is that the polarity of the specific aromatic polyether ketone resin constituting the resin composition of the present invention is greater than that of PEEK and is easily mixed with polar engineering plastics, and therefore a homogeneous mixture is formed.

[0064] The glass transition temperature of the resin composition of the present invention is preferably 150°C or higher, more preferably 160°C or higher, and even more preferably 170°C or higher, and is adjusted to a desired range depending on the application of the resin composition. By designing it to be above such a lower limit, a resin composition having sufficiently high practical heat resistance can be obtained. In addition, the upper limit of the glass transition temperature can also be appropriately set, and is preferably 300°C or lower, more preferably 280°C or lower, even more preferably 250°C or lower, particularly preferably 230°C or lower, and especially preferably 210°C or lower. By setting it below such an upper limit, it becomes possible to melt mold under relatively mild conditions, and it becomes possible to suppress thermal deterioration of the resin composition during molding and reduce process costs.

[0065] As a method for estimating the glass transition temperature of a homogeneous resin composition, various empirical formulas are known, and for example, it can be estimated by the Fox formula according to the method described in the Examples. The glass transition temperature of the resin composition of the present invention is preferably higher than the calculated Tg value (Tg3) calculated based on the Fox formula. Specifically, using the Tg2, it is preferable that Tg2-Tg3≧1 (°C), more preferably Tg2-Tg3≧3 (°C), even more preferably Tg2-Tg3≧5 (°C), particularly preferably Tg2-Tg3≧7 (°C), and most preferably Tg2-Tg3≧8 (°C). By being in such a range, it can be said that the blending design of the resin composition provides an effect of improving heat resistance that exceeds empirical expectations.

[0066] (Additives, etc.) The resin composition of the present invention may be mixed with additives other than the aromatic polyether ether ketone resin containing the repeating unit of the general formula (1) and polar engineering plastics as long as the effects of the present invention are not impaired, depending on the application, required performance, etc. The components such as additives used may be used alone or in combination of two or more kinds.

[0067] The additive is not particularly limited and can be appropriately selected according to the purpose, and examples thereof include inorganic fillers and organic fillers. The shape of the filler is not particularly limited and examples thereof include particulate, plate-like, fibrous, and other fillers. Among fibrous fillers, carbon fiber and glass fiber are preferred because they have a wide range of industrial applications.

[0068] Furthermore, there are no particular limitations on the additives other than the filler, and additives such as heat stabilizers, antioxidants, lubricants, antiblocking agents, nucleating agents, colorants, pigments, ultraviolet absorbers, light stabilizers, modifiers, crosslinking agents, etc. may be contained.

[0069] <Molded object, application> The resin composition of the present invention can be molded into a molded article by a melt molding method such as injection molding or extrusion molding, or by a method of handling the resin composition as a solution using an appropriate good solvent, depending on the application and required performance. Specific examples of the shape and application of the molded article include films, fibers, pipes, rods, rings, gears, bearings, coating materials, and in vivo implant materials. As for the form of the molded article, the composition of the present invention alone may be used to construct the molded article, but it may also be combined with other materials in any shape as long as the properties of the composition can be exhibited, and used as a laminate, for example. EXAMPLES

[0070] The following examples of the resin composition of the present invention are given, but the present invention is not limited to these examples as long as the gist of the invention is not exceeded. The methods for measuring the various properties are as follows. <Thermal properties of resin composition or resin (glass transition temperature: Tg)> The thermal properties of the resin composition or resin were measured using a differential scanning calorimeter "DSC7020" (manufactured by Hitachi High-Tech Science Corporation) by heating approximately 2 mg of the resin composition or resin from 30°C to 360°C at a rate of 10°C / min (1st heating), then cooling from 360°C to 30°C at a rate of 10°C / min (1st cooling), and further heating from 30°C to 360°C at 10°C / min (2nd heating). Tg was measured in the first heating and was regarded as the Tg of the resin composition or resin. If Tg could not be measured in the first heating, Tg was measured in the second heating and was regarded as the Tg of the resin composition or resin.

[0071] <Synthesis Example 1> In a reaction vessel equipped with an agitator, a nitrogen inlet / vacuum inlet, and a heater, 7.09 parts by mass of bisfluorobenzoylfuran (BFBF), 2.50 parts by mass of hydroquinone (HQ), 3.17 parts by mass of potassium carbonate, 27.2 parts by mass of diphenyl sulfone, and 1.5 parts by mass of triglyme were charged. Nitrogen gas was introduced into the vessel while stirring the contents of the reaction vessel, and the system was placed under a nitrogen atmosphere by vacuum replacement. Next, the temperature was raised to 200°C while stirring the system, and the reaction was carried out at this temperature for 1 hour. Thereafter, the temperature was raised to 280°C over 5 minutes, and polycondensation was continued at this temperature for 2 hours. The polymerization product was removed from the reaction vessel and crushed with a hammer to make it into a powder form, and then washed by solid-liquid extraction with 157 parts by mass of acetone at room temperature for 15 minutes to recover the solid components. Washing with acetone was carried out again under the same conditions. Subsequently, washing by solid-liquid extraction with 200 parts by mass of water at 60°C for 15 minutes was carried out to recover the solid components. The mixture was washed again with water under the same conditions. After that, the mixture was washed by solid-liquid extraction with 103 parts by mass of N-methyl-2-pyrrolidone at 120°C for 30 minutes to recover the solid component. The filtered solid component was vacuum dried at 120°C for 6 hours in a vacuum dryer to obtain the target PAEK1.

[0072] <Synthesis Example 2> In a reaction vessel equipped with an agitator, a nitrogen inlet / vacuum inlet, and a heater, 22.7 parts by mass of bisfluorobenzoylfuran (BFBF), 0.80 parts by mass of hydroquinone (HQ), 14.0 parts by mass of 4,4'-dihydroxybenzophenone (DHBP), 10.1 parts by mass of potassium carbonate, 87.0 parts by mass of diphenylsulfone, and 4.8 parts by mass of triglyme were charged. Here, the molar ratio of BFBF / HQ / DHBP is 100 / 10 / 90. While stirring the contents of the reaction vessel, nitrogen gas was introduced into the vessel, and the system was placed under a nitrogen atmosphere by vacuum replacement. Next, the temperature was raised to 200°C while stirring the system, and the reaction was carried out at this temperature for 1 hour. After that, the temperature was raised to 280°C over 5 minutes, and polycondensation was continued at this temperature for 1 hour. The polymerization product was removed from the reaction vessel and crushed with a hammer to obtain a powder, after which it was washed by solid-liquid extraction with 784 parts by mass of acetone at room temperature for 15 minutes to recover the solid component. Washing with acetone was performed again under the same conditions. Then, washing with solid-liquid extraction was performed for 15 minutes with 1000 parts by mass of water at 60°C to recover the solid component. Washing with water was performed again under the same conditions. Then, washing with solid-liquid extraction was performed for 30 minutes with 309 parts by mass of N-methyl-2-pyrrolidone at 120°C to recover the solid component. The filtered solid component was vacuum dried at 120°C for 6 hours in a vacuum dryer to obtain the target PAEK2. The molar ratio of the constituent units derived from BFBF / HQ / DHBP, respectively, determined from the 1H-NMR spectrum, was 100 / 11 / 89.

[0073] <Example 1> As component A, PAEK1 synthesized in Synthesis Example 1 above, which has 2,5-bis(4-fluorobenzoyl)furan (BFBF) and hydroquinone (HQ) as structural units, was used as an aromatic polyether ketone resin containing a repeating unit of formula (1), and as component B, Ultem 1000 (manufactured by SABIC), which is a polyetherimide (PEI), was used. 70 parts by mass of PAEK1 (component A) and 30 parts by mass of Ultem 1000 (component B) were weighed out and dissolved in 2710 parts by mass of pentafluorophenol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), and then 5500 parts by mass of chloroform (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were added to obtain a uniform resin solution. This resin solution was dropped into a large excess of methanol, and the precipitated solid resin composition was collected and dried in vacuum, after which it was subjected to the measurement of the above thermal properties. Table 1 shows the results of the Tg measurement.

[0074] <Example 2> A solid resin composition was obtained in the same manner as in Example 1, except that the resin (component B) mixed with PAEK1 (component A) was changed from Ultem 1000 to Extem VH 1003-1000 (PI, manufactured by SABIC) shown in Table 1 and mixed in the composition shown in Table 1, and Tg was measured. Table 1 shows the results of the thermal property measurement.

[0075] <Example 3> As shown in Table 1, a solid resin composition was obtained in the same manner as in Example 1, except that PAEK2 synthesized in Synthesis Example 2 was used as Component A, and the above thermal properties were measured. Table 1 shows the results of the Tg measurement. PAEK2 was synthesized according to Synthesis Example 2 and is an aromatic polyether ketone resin containing a repeating unit of formula (1). The aromatic polyether ketone resin has 2,5-bis(4-fluorobenzoyl)furan (BFBF), 4,4'-dihydroxybenzophenone (DHBP) and hydroquinone (HQ) as constituent units, with the molar ratio of DHBP to HQ being 89:11.

[0076] <Comparative Example 1> The Tg was measured using only the aromatic polyether ketone resin PAEK1. Table 2 shows the results of the Tg measurement. <Comparative Example 2> The Tg was measured using only PAEK2, which is an aromatic polyether ketone resin. Table 2 shows the results of the Tg measurement.

[0077] <Comparative Example 3> Tg was measured using only Victrex PEEK 650G (manufactured by Victrex), which is a polyether ether ketone resin (PEEK). Table 2 shows the results of the Tg measurement.

[0078] <Comparative Example 4> As shown in Table 1, Victrex PEEK 650G, which is a polyether ether ketone resin (PEEK), was used as component A, Ultem 1000 (PEI, manufactured by SABIC) was used as component B, and these were mixed in the composition shown in Table 2. A solid resin composition was obtained in the same manner as in Example 1, and Tg was measured. Table 2 shows the results of the Tg measurement.

[0079] <Comparative Example 5> A solid resin composition was obtained and its Tg was measured in the same manner as in Comparative Example 4, except that component B was changed from Ultem 1000 to Extem VH1003-1000 (PI, manufactured by SABIC) shown in Table 1. Table 2 shows the results of the Tg measurement.

[0080] [Table 1]

[0081] [Table 2]

[0082] In Table 2, Tg may be shown in two rows, one above the other, where the values ​​in the upper row are derived from the PEEK phase or a phase mainly composed of PEEK in the resin composition, and the values ​​in the lower row are derived from the polar engineering plastic phase or a phase mainly composed of polar engineering plastic in the resin composition. In the table, "nd" means "not detected," meaning that no quantifiable signal was observed. The calculated Tg values ​​shown in Tables 1 and 2 are values ​​calculated based on the Fox equation shown in general formula (15). The Fox equation is usually used to estimate the Tg of random copolymers, but it may also be used for homogeneous miscible resin blend compositions.

[0083]

number

[0084] The Tg of each of the resins used is as follows: PAEK1: 148℃ PAEK2: 155℃ PEEK: 151℃ ·Extem VH1003-1000: 242℃ Ultem 1000: 215℃

[0085] <Evaluation Results> As shown in Table 1, in Examples 1 to 3, the obtained resin compositions were compatible mixtures and showed a single Tg, and the Tg of each resin composition was higher than the Tg of PAEK1 itself, 148° C., or the Tg of PAEK2 itself, 155° C., of Component A. In addition, the measured Tg value of the resin composition was higher than the calculated Tg value, indicating that a higher heat resistance improvement effect was exhibited than predicted by the empirical formula.

[0086] In contrast, the resin composition of Comparative Example 5 did not become a compatible mixture, and the resin composition still showed the Tg of component A. Therefore, it was found that these resin compositions have poor practical heat resistance due to the influence of the low Tg. In Comparative Example 4, a compatible mixture was obtained, but the measured Tg of the resin composition was lower than the calculated Tg value, and the heat resistance improvement effect was poor.

[0087] As described above, in Examples 1 to 3 of the present application, the resin compositions obtained were compatible mixtures. It is believed that PAEK1 and PAEK2 of Component A have a higher polarity than PEEK, and therefore are easily compatible with the polar engineering plastic of Component B.

Claims

1. A resin composition comprising an aromatic polyether ketone resin containing a repeating unit represented by the following general formula (1) and at least one polar engineering plastic: 【Chemistry 1】 (In formula (1), structure A is any one selected from the group consisting of the following general formulae (2), (3) and (4), and structure B is an optionally substituted divalent aromatic hydrocarbon ring.) 【Chemistry 2】

2. The resin composition according to claim 1, wherein the structure A is the general formula (2).

3. The resin composition according to claim 1 or 2, wherein the polar engineering plastic has a functional group containing a heteroatom in its skeleton.

4. 3. The resin composition according to claim 1, wherein the polar engineering plastic has one or more functional groups in the main chain selected from the group consisting of a sulfonyl group, a sulfinyl group, an ether group, a thioether group, an imide group, an amide group, an ester group, a carbonate group, and an imidazole ring.

5. The resin composition according to claim 1 or 2, wherein the polar engineering plastic is substantially amorphous.

6. 3. The resin composition according to claim 1, wherein the polar engineering plastic is selected from the group consisting of polyphenylsulfone, polyimide, and polyetherimide.

7. The resin composition according to claim 1 or 2, wherein Tg2-Tg1 is greater than or equal to 5 (°C), where Tg1 is the glass transition temperature of the aromatic polyether ketone resin containing the repeating unit represented by the general formula (1) and Tg2 is the glass transition temperature of the resin composition.

8. The resin composition according to claim 1 or 2, wherein Tg2-Tg3≧1 (°C) is satisfied, where Tg3 is the calculated glass transition temperature of the aromatic polyether ketone resin containing the repeating unit represented by the general formula (1) and Tg2 is the glass transition temperature of the resin composition.

Citation Information

Patent Citations

  • Thermoplastic polyether aromatic ketone

    JP1979090296A