Processing method of wafer
The wafer processing method addresses unevenness in plasma etching by using a protective film to mask the groove sidewalls and forming a narrower second groove, enhancing processing quality and reducing thermal damage.
Patent Information
- Application Number
- JP2023060192
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-03
- Publication Date
- 2024-10-16
AI Technical Summary
The unevenness of the side surface of the processed groove formed by laser beam irradiation leads to a deterioration in the quality of the chip formed by plasma etching.
A wafer processing method that includes forming a protective film, irradiating it with a laser beam along the dividing line to remove the film and create a first machined groove, liquefying a part of the protective film with a solvent, covering the groove's sidewalls with the protective film, and using it as a mask for plasma etching, followed by forming a narrower second groove to expose the substrate.
This method suppresses unevenness on the side surface of the chip, improving processing quality by reducing thermal damage and the need for additional laser irradiation, while minimizing the use of protective film and maintaining chip integrity.
Smart Images

Figure 2024147276000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a wafer processing method for processing a wafer. [Background technology]
[0002] There is a known processing method for processing a wafer having a plurality of device regions defined by a plurality of dividing lines on the surface of a substrate by plasma etching. In this processing method, after a protective film is coated on the surface, the protective film is removed by irradiation with a laser beam to form a processing groove that exposes the substrate, and plasma etching is performed using the protective film as a mask (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent Publication No. 2022-052821 Summary of the Invention [Problem to be solved by the invention]
[0004] However, if the side surface of the groove formed by irradiation with a laser beam is uneven, the quality of the side surface of the chip formed by plasma etching deteriorates.
[0005] The present invention has been made in view of the above problems, and an object of the present invention is to provide a wafer processing method capable of improving processing quality in plasma etching. [Means for solving the problem]
[0006] In order to solve the above-mentioned problems and achieve the object, the wafer processing method of the present invention is a wafer processing method for processing a wafer having device regions partitioned by a plurality of planned dividing lines formed on the surface of a substrate along the planned dividing lines, and is characterized by comprising: a protective film forming step for forming a protective film on the surface; a first processing groove forming step for irradiating the protective film with a laser beam along the planned dividing lines to form a first processing groove that removes the protective film and exposes the substrate; a first processing groove covering step for liquefying at least a portion of the protective film with a solvent and covering the sidewall of the first processing groove with the protective film after the first processing groove covering step; and a plasma etching step for processing the substrate by plasma etching using the protective film as a mask with the sidewall of the first processing groove covered with the protective film after the first processing groove covering step.
[0007] In the first groove covering step, the bottom surface of the first groove is also covered with the protective film, and after the first groove covering step, a laser beam is irradiated onto the first groove to form a second groove narrower than the first groove, and the protective film covering the sidewall of the first groove is left in place while the protective film covering the bottom surface of the first groove is removed to expose the substrate, and the substrate may be processed along the second groove in the plasma etching step.
[0008] In the first groove coating step, the solvent may be supplied in the form of a spray.
[0009] In the first groove covering step, at least one of the wafer and the protective film may be heated.
[0010] In the first groove covering step, an external force of at least one of vibration and pressure may be applied to the protective film to promote movement of the protective film to the first groove. Effect of the Invention
[0011] In the present invention, the sidewalls of the first groove are covered with a protective film, and then the substrate exposed at the bottom surface of the first groove is etched. This allows the substrate exposed at the bottom surface of the first groove to be etched along the unevenness of the protective film, which is clearly smaller than the unevenness of the sidewalls of the first groove. This suppresses the generation of unevenness on the processed side surface during etching, thereby improving the processing quality in plasma etching. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a perspective view that typically shows a wafer to be processed by the wafer processing method according to the first embodiment. [Diagram 2] FIG. 2 is a cross-sectional view that typically shows a main part of the wafer shown in FIG. [Diagram 3] FIG. 3 is a flowchart showing the flow of the wafer processing method according to the first embodiment. [Figure 4] FIG. 4 is a cross-sectional view that illustrates a schematic view of a main part of the wafer after the protective film forming step in the wafer processing method illustrated in FIG. [Diagram 5] FIG. 5 is a cross-sectional view that illustrates a schematic view of a main part of a wafer after the first groove forming step of the wafer processing method illustrated in FIG. [Figure 6] FIG. 6 is a schematic partial cross-sectional view of a main portion of a wafer during a first groove covering step of the wafer processing method shown in FIG. [Figure 7] FIG. 7 is a schematic partial cross-sectional view showing an example of the first groove covering step of the wafer processing method shown in FIG. [Figure 8] FIG. 8 is a schematic partial cross-sectional view showing another example of the first processed groove covering step of the wafer processing method shown in FIG. [Figure 9] FIG. 9 is a cross-sectional view that diagrammatically shows a main part of a wafer during a plasma etching step of the wafer processing method shown in FIG. [Figure 10] FIG. 10 is a cross-sectional view that typically shows a main part of the wafer after the cleaning step of the wafer processing method shown in FIG. [Figure 11]FIG. 11 is a flowchart showing the flow of the wafer processing method according to the second embodiment. [Figure 12] FIG. 12 is a schematic partial cross-sectional view of a main portion of a wafer during a first groove covering step of the wafer processing method shown in FIG. [Figure 13] FIG. 13 is a schematic partial cross-sectional view of a main portion of a wafer after the second groove forming step of the wafer processing method shown in FIG. [Figure 14] FIG. 14 is a cross-sectional view that diagrammatically shows a main part of a wafer during a plasma etching step of the wafer processing method shown in FIG. [Figure 15] FIG. 15 is a cross-sectional view that typically shows a main part of a wafer after the cleaning step of the wafer processing method shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The form (embodiment) for carrying out the present invention will be described in detail with reference to the drawings. The present invention is not limited to the contents described in the following embodiment. Furthermore, the components described below include those that a person skilled in the art can easily imagine and those that are substantially the same. Furthermore, the configurations described below can be appropriately combined. Furthermore, various omissions, substitutions, or modifications of the configurations can be made without departing from the gist of the present invention.
[0014] [Embodiment 1] A wafer processing method according to a first embodiment of the present invention will be described with reference to the drawings. Fig. 1 is a perspective view that typically shows a wafer 1 to be processed by the wafer processing method according to the first embodiment. Fig. 2 is a cross-sectional view that typically shows a main part of the wafer 1 shown in Fig. 1. Fig. 3 is a flow chart showing the flow of the wafer processing method according to the first embodiment.
[0015] (Wafer) The wafer processing method according to the first embodiment is a method for processing a wafer 1 shown in Fig. 1. In the first embodiment, the wafer 1 is a wafer such as a disk-shaped semiconductor wafer having a substrate 2 made of silicon, glass, SiC, sapphire, gallium arsenide, or the like. As shown in Fig. 1, the wafer 1 has devices 5 formed in regions partitioned in a lattice pattern by a plurality of planned division lines 4 formed in a lattice pattern on a surface 3. Hereinafter, the region of the wafer 1 in which the devices 5 are formed is referred to as a device region.
[0016] The device 5 is, for example, an integrated circuit such as an IC (Integrated Circuit) or an LSI (Large Scale Integration), a CCD (Charge Coupled Device), or a memory (semiconductor memory device).
[0017] In the first embodiment, the wafer 1 has a functional layer 6 laminated on the surface of the substrate 2, as shown in Figures 1 and 2. The functional layer 6 includes a low dielectric constant insulator coating (hereinafter referred to as a low-k film) made of an inorganic film such as SiOF, BSG (SiOB), or an organic film such as a polymer film of a polyimide system or parylene system, or carbon-containing silicon oxide (SiOCH), and a circuit layer including a conductive metal pattern or metal film.
[0018] The low-k film is laminated with a circuit layer to form the device 5. The circuit layer constitutes the circuit of the device 5. For this purpose, the device 5 is constituted by the mutually laminated low-k films of the functional layer 6 laminated on the substrate 2, and the circuit layer laminated between the low-k films. At the planned division line 4, the functional layer 6 is constituted by the low-k film laminated on the substrate 2.
[0019] The functional layer 6 such as a low-k film is easily peeled off from the substrate 2 when the wafer 1 is cut from the front surface 3 side with a cutting blade. Thus, in the first embodiment, the wafer 1 has the device 5 formed on the front surface 3 by the functional layer 6 laminated on the substrate 2.
[0020] (Wafer Processing Method) The wafer processing method according to the first embodiment is a method of processing a wafer 1, on which a plurality of devices 5 are formed by a functional layer 6 laminated on the surface of a substrate 2, along a planned division line 4 that divides the plurality of devices 5. In the first embodiment, the wafer processing method is also a method of dividing (corresponding to processing) the wafer 1 along the planned division line 4 into individual device chips 10 (shown in FIG. 1). The device chip 10 includes a part of the substrate 2 and a device 5. Although all the embodiments are described with a configuration in which a functional layer 6 is laminated on the surface of the substrate 2, the functional layer 6 may not be formed.
[0021] As shown in Fig. 3, the wafer processing method includes a protective film forming step 101, a first processed groove forming step 102, a first processed groove covering step 103, a plasma etching step 104, and a cleaning step 105. In the wafer processing method according to the first embodiment, as shown in Fig. 1, a disk-shaped tape 11 having a larger diameter than the wafer 1 is attached to the back surface 9 behind the front surface 3, an annular frame 12 is attached to the outer edge of the tape 11, and the wafer 1 supported by the frame 12 is processed.
[0022] (Protective film formation step) Fig. 4 is a cross-sectional view showing a schematic view of a main part of the wafer 1 after the protective film forming step 101 of the wafer processing method shown in Fig. 3. The protective film forming step 101 is a step of forming a protective film 13 (shown in Fig. 4) on the front surface 3 of the wafer 1 before the first processed groove forming step 102 is performed.
[0023] In the first embodiment, in the protective film forming step 101, a resin coating device (not shown) suction-holds the back surface 9 of the wafer 1 on the holding surface of the spinner table via the tape 11, clamps the frame 12 with a clamping section, rotates the spinner table about its axis, and drips liquid water-soluble resin from a water-soluble resin supply nozzle onto the center of the front surface 3 of the wafer 1. The dripped water-soluble resin flows from the center to the outer periphery on the front surface 3 of the wafer 1 due to centrifugal force generated by the rotation of the spinner table, and is applied to the entire surface of the front surface 3 of the wafer 1. Note that although all the embodiments are described as including the frame 12, the frame 12 need not be used.
[0024] The water-soluble resin contains a water-soluble resin such as polyvinyl alcohol (PVA) or polyvinylpyrrolidone (PVP). In the protective film forming step 101, the water-soluble resin applied to the entire surface of the front surface 3 of the wafer 1 is dried, so that the entire surface of the front surface 3 of the wafer 1 is covered with a protective film 13 containing the water-soluble resin, as shown in FIG. 4. Thus, in the first embodiment, the protective film 13 is made of a water-soluble resin. Furthermore, when dried, the water-soluble resin constituting the protective film 13 has a lower etching rate than the substrate 2 with respect to the plasma etching gas 18 (shown in FIG. 9) used in the plasma etching step 104, and has resistance.
[0025] In the protective film forming step 101, a protective film 13 of sufficient thickness is formed on the device region of the front surface 3 of the wafer 1 so that even if the protective film 13 on the device region of the front surface 3 of the wafer 1 becomes thin in the first processing groove covering step 103, the protective film 13 on the device region of the front surface 3 of the wafer 1 has a thickness that is effective as a mask in the plasma etching step 104.
[0026] (First machining groove forming step) Fig. 5 is a cross-sectional view showing a schematic view of a main part of the wafer 1 after the first groove forming step 102 of the wafer processing method shown in Fig. 3. The first groove forming step 102 is a step of irradiating a laser beam (not shown) from the front surface 3 of the wafer 1 along the division lines 4 to remove the protective film 13 and form a first groove 14 (shown in Fig. 5) that exposes the substrate 2. In the first embodiment, in the first groove forming step 102, the functional layer 6 formed on the division lines 4 is also removed by the irradiation of the laser beam.
[0027] In the first embodiment, in the first processed groove forming step 102, a laser processing device (not shown) suction-holds the back surface 9 side of the wafer 1 on the holding surface of a holding table via tape 11, and clamps the frame 12 with a clamp section. In the first processed groove forming step 102, the laser processing device images the front surface 3 side of the wafer 1 with an imaging unit (not shown), detects the planned division lines 4, and performs alignment to align the laser beam application unit with the planned division lines 4.
[0028] In the first embodiment, in the first groove forming step 102, the laser processing device irradiates the wafer 1 along the intended dividing lines 4 with a laser beam having a wavelength absorbed by the wafer 1 from the laser beam application unit while moving the wafer 1 and the laser beam application unit relatively along the intended dividing lines 4. Note that in the first embodiment, in the first groove forming step 102, the laser processing device sets the focal point of the laser beam on the surface of the protective film 13 or the surface of the substrate 2, and irradiates the wafer 1 with the laser beam along each of the intended dividing lines 4.
[0029] In embodiment 1, in the first processing groove formation step 102, a laser processing device performs ablation processing on the protective film 13, functional layer 6 and substrate 2 on each planned division line 4 to remove portions of these, thereby forming a first processing groove 14 that divides the protective film 13 and functional layer 6 at each planned division line 4, as shown in Figure 5.
[0030] In the first embodiment, in the first groove forming step 102, a laser beam is irradiated to both edges in the width direction of each division line 4 to form a groove by ablation processing on the protective film 13, the functional layer 6 and the substrate 2 on both edges in the width direction of each division line 4, and then a laser beam is irradiated between the grooves of each division line 4 to form a first groove 14 by ablation processing on the protective film 13, the functional layer 6 and the substrate 2 between the grooves of each division line 4. In the first groove forming step 102, a laser beam having a wavelength of 355 nm (not limited to 355 nm, but a wavelength in the ultraviolet region that is absorbent by the functional layer 6 and the substrate 2 is preferable) is irradiated.
[0031] In the first processed groove forming step 102, when the laser beam is branched to form two both edge processed grooves on both edges in the width direction of the dividing line 4 and ablation processing is performed, the average output of the laser beam is 0.5 W, the relative moving speed (hereinafter referred to as the processing feed speed) between the laser beam application unit and the wafer 1 is 100 mm / sec to 400 mm / sec, and the spot of the focusing point of the laser beam is a circle with a diameter of 5 μm. In the first processed groove forming step 102, when ablation processing is performed between the both edge processed grooves of the dividing line 4, the average output of the laser beam is 10.0 W, the processing feed speed is 200 mm / sec to 1000 mm / sec, and the spot of the focusing point of the laser beam is a rectangle with a width of 60 μm.
[0032] In the first embodiment, the widths 14-1 of all the first processed grooves 14 are the same.
[0033] (First machining groove covering step) Fig. 6 is a schematic partial cross-sectional view of a main part of the wafer 1 during the first groove covering step 103 of the wafer processing method shown in Fig. 3. The first groove covering step 103 is a step performed after the first groove forming step 102, in which at least a part of the protective film 13 is liquefied with a solvent 15 (shown in Fig. 6) and an inner side wall 14-2 of the first groove 14 is covered with the protective film 13.
[0034] In the first embodiment, in the first groove covering step 103, the solvent supply nozzle 16 supplies the solvent 15 that liquefies the protective film 13 to the surface 3 of the wafer 1. The supplied solvent 15 liquefies at least a part of the protective film 13 formed on the surface 3 of the wafer 1. At least a part of the protective film 13 liquefied by the solvent 15 flows along the side wall 14-2 of the first groove 14. In the first groove covering step 103, the liquefied protective film 13 that flows along the side wall 14-2 of the first groove 14 is dried again, so that the side wall 14-2 of the first groove 14 is covered with the protective film 13 as shown in FIG. 6. In the first groove covering step 103, at least a part of the protective film 13 formed on the surface 3 of the wafer 1 is liquefied and flows along the side wall 14-2 of the first groove 14, so that the protective film 13 on the device region of the surface 3 of the wafer 1 becomes thin. Therefore, in the protective film forming step 101, even if the protective film 13 on the device region becomes thinner by the first processing groove covering step 103, a thickness that can sufficiently protect the device region without exposing it in the plasma etching step 104 is calculated, and the protective film 13 is covered with a thickness greater than or equal to that thickness.
[0035] In addition, the solvent 15 for liquefying the protective film 13 containing a water-soluble resin is, for example, pure water in embodiment 1, but is not limited to this in the present invention and may be a liquid mixture of pure water and the liquid protective film 13, or the liquid protective film 13 itself.
[0036] In the first embodiment, in the first groove covering step 103, a small amount of the solvent 15 is supplied in a spray (mist) form to the surface 3 of the wafer 1 to liquefy a small amount of the protective film 13. This suppresses the risk of removing the protective film 13 on the device region by the solvent 15 due to excessive supply of the solvent 15, and also suppresses the adhesion of the liquefied protective film 13 to the bottom surface 14-3 of the first groove 14 by liquefying a large amount of the protective film 13 due to excessive supply of the solvent 15, and thus the small amount of the solvent 15 that liquefies the small amount of the protective film 13 that maintains the exposure of the bottom surface 14-3 of the first groove 14 while covering the side wall 14-2 of the first groove 14 can be suitably supplied approximately uniformly to the surface 3 of the wafer 1. Therefore, there is no need to expose the bottom surface 14-3 of the first groove 14 by irradiating the laser beam again, and the substrate 2 exposed at the bottom surface 14-3 of the first groove 14 can be etched in the plasma etching step 104. Note that in order to detect the amount of solvent 15 that liquefies a small amount of protective film 13 that covers the side wall 14-2 of the first groove 14 while maintaining the bottom surface 14-3 of the first groove 14 exposed, a detection step may be provided in which the amount of solvent 15 is changed in multiple steps while the first groove covering step 103 is performed, the covering state of the first groove 14 is confirmed, and the optimum amount of solvent 15 is determined.
[0037] In the first processed groove covering step 103, at least one of the wafer 1 and the protective film 13 is heated, and the fluidity of the protective film 13 liquefied by supplying a solvent 15 is increased, so that the liquefied protective film 13 can easily flow along the side wall 14-2 of the first processed groove 14. At least one of the wafer 1 and the protective film 13 is heated, for example, by a heater provided in a holding table that holds the wafer 1, or by an infrared heater or a hot air supply unit provided at a position facing the protective film 13 formed on the front surface 3 of the wafer 1, or the like.
[0038] In addition, in the first processed groove covering step 103, by applying an external force to the protective film 13, it is possible to promote the liquefied protective film 13 to flow along the side wall 14-2 of the first processed groove 14. The external force applied to the protective film 13 is, for example, a centrifugal force generated by rotating the wafer 1, vibration along the surface direction, thickness direction, or oblique direction of the wafer 1, pressure brought about by blowing air, and pressure that presses the protective film 13 downwardly, which is generated by storing the wafer 1 in a vacuum chamber and applying positive pressure above the wafer 1 from below the wafer 1. In addition, by blowing hot air to the protective film 13 in the first processed groove covering step 103, both the effect of heating the protective film 13 and the effect of applying pressure, which is an external force, can be obtained.
[0039] Fig. 7 is a schematic partial cross-sectional view of an example of the first processed groove covering step 103 of the wafer processing method shown in Fig. 3. In the first embodiment, in the first processed groove covering step 103, for example, the solvent supply device 20-1 shown in Fig. 7 may hold the back surface 9 side of the wafer 1 on the holding surface 22 of the holding table 21 by suction via the tape 11, and may rotate the holding table 21 around its axis while heating the wafer 1 and the protective film 13 by the heater 23 provided in the holding table 21, and may supply the solvent 15 in a spray (mist) form to the protective film 13 formed on the front surface 3 of the wafer 1 from above the holding table 21 by the solvent supply nozzle 16.
[0040] Fig. 8 is a schematic partial cross-sectional view of another example of the first processed groove covering step 103 of the wafer processing method shown in Fig. 3. In the first embodiment, in the first processed groove covering step 103, for example, the solvent supply device 20-2 shown in Fig. 8 may hold the back surface 9 side of the wafer 1 on the holding surface 22 of the holding table 21 by suction via the tape 11, move the holding table 21 along a direction parallel to the holding surface 22 relative to the gas supply unit 24 while heating the wafer 1 and the protective film 13 by the heater 23 provided in the holding table 21, and supply the solvent 15 in a spray form (mist form) from above the holding table 21 to the protective film 13 formed on the front surface 3 of the wafer 1 by the solvent supply nozzle 16, and blow air 25 from above the holding table 21 to the protective film 13 formed on the front surface 3 of the wafer 1 by the gas supply unit 24. The gas supply unit 24 extends, for example, along one direction parallel to the holding surface 22 of the holding table 21 (a direction perpendicular to the paper surface of Figure 8), is formed to be longer than the diameter of the holding surface 22, and is provided above the holding surface 22.
[0041] (Plasma Etching Step) Fig. 9 is a cross-sectional view showing a schematic view of a main part of the wafer 1 during the plasma etching step 104 of the wafer processing method shown in Fig. 3. The plasma etching step 104 is a step of processing the substrate 2 by plasma etching using the protective film 13 as a mask in a state in which the side wall 14-2 of the first processed groove 14 is covered with the protective film 13 after the first processed groove covering step 103.
[0042] In the first embodiment, in the plasma etching step 104, a plasma etching device (not shown) holds the back surface 9 of the wafer 1 on the holding surface of a holding table via tape 11. In the first embodiment, in the plasma etching step 104, high frequency power for generating and maintaining plasma is applied to the upper electrode, and an etching gas 18 is supplied to the front surface 3 side of the wafer 1 while high frequency power for attracting ions is applied to the holding table, which is the lower electrode. In the first embodiment, the etching gas 18 in the plasma etching step 104 is, for example, fluorine-based gases SF6 and C4F8.
[0043] Then, in embodiment 1, in the plasma etching step 104, the plasma etching apparatus converts the etching gas 18 in the space between the holding table and the upper electrode into plasma, and this plasmatized etching gas 18 is drawn toward the wafer 1 side to etch (so-called plasma etching) the substrate 2 exposed at the bottom surface 14-3 (shown in Figures 5 and 6) of the first groove 14 formed in the protective film 13, which is a mask for the wafer 1, thereby progressing the first groove 14 toward the back surface 9 of the wafer 1.
[0044] Here, the protective film 13 supplied with the solvent 15 in the first processed groove covering step 103 plays the role of a mask in plasma etching, similar to the protective film 13 to which the solvent 15 is not supplied that is used in the conventional processing method, and has the effect of preventing adhesion of foreign matter such as debris to the device region on the front surface 3 of the wafer 1. For this reason, in the plasma etching step 104, similar to the case where the protective film 13 to which the solvent 15 is not supplied is used in the conventional processing method, no deterioration in the processing quality after plasma etching was observed, and no adhesion of foreign matter such as debris to the device region was observed.
[0045] In the first embodiment, in the plasma etching step 104, the plasma etching device plasma etches the wafer 1 until the first processed grooves 14 open on the back surface 9 side and the wafer 1 is divided into device chips 10, as shown in Fig. 9. Thus, in the first embodiment, in the plasma etching step 104, the wafer 1 is divided and a plurality of device chips 10 are manufactured.
[0046] (Washing step) Fig. 10 is a cross-sectional view showing a schematic view of a main part of the wafer 1 after the cleaning step 105 of the wafer processing method shown in Fig. 3. The cleaning step 105 is a step of cleaning and removing the protective film 13 after the plasma etching step 104 is performed.
[0047] In the first embodiment, in cleaning step 105, a cleaning device (not shown) suction-holds the back surface 9 of the wafer 1 on the holding surface of the spinner table via tape 11, clamps frame 12 with a clamp section, and supplies cleaning water consisting of pure water or pure water containing a surfactant from a cleaning water supply nozzle to the center of the front surface 3 of the wafer 1 while rotating the spinner table around its axis. The cleaning water supplied to the front surface 3 of the wafer 1 flows from the center to the outer periphery on the front surface 3 of the wafer 1 due to centrifugal force generated by the rotation of the spinner table, cleaning the front surface 3 of the wafer 1 and removing the protective film 13 containing a water-soluble resin from the front surface 3 of the wafer 1 together with foreign matter such as debris, as shown in FIG.
[0048] In the conventional processing method, when the substrate 2 on the bottom surface 14-3 of the first processed groove 14 is plasma etched, the protective film 13 and the functional layer 6 are removed to form the first processed groove 14, so irradiation with a high-power laser beam is required, and the thermal damage to the functional layer 6 is also large, causing unevenness on the inner side wall 14-2 of the first processed groove 14, particularly on the functional layer 6. For this reason, in the conventional processing method, when the substrate 2 on the bottom surface 14-3 of the first processed groove 14 is plasma etched, the substrate 2 is etched along the unevenness of the inner side wall 14-2 of the first processed groove 14, particularly on the functional layer 6, causing unevenness on the side surface of the device chip 10, which reduces the flexural strength of the device chip 10 and deteriorates the appearance of the device chip 10.
[0049] Compared with such conventional processing methods, the above-described wafer processing method according to the first embodiment etches the substrate 2 exposed on the bottom surface 14-3 of the first processed groove 14 after covering the inner sidewall 14-2 of the first processed groove 14 with the protective film 13. For this reason, the wafer processing method according to the first embodiment etches the substrate 2 exposed on the bottom surface 14-3 of the first processed groove 14 along the unevenness of the protective film 13 that is obviously smaller than the unevenness of the functional layer 6 on the inner sidewall 14-2 of the first processed groove 14, thereby suppressing the unevenness generated on the side surface of the device chip 10, thereby suppressing the decrease in the bending strength of the device chip 10. In this way, the wafer processing method according to the first embodiment can improve the processing quality in plasma etching.
[0050] Moreover, in the wafer processing method according to the embodiment 1, the inner side wall 14-2 of the first groove 14 is covered with the protective film 13 so that the liquefied protective film 13 does not adhere to the bottom surface 14-3 of the first groove 14, and then the substrate 2 exposed at the bottom surface 14-3 of the first groove 14 is etched. For this reason, in the wafer processing method according to the embodiment 1, it is not necessary to expose the bottom surface 14-3 of the first groove 14 by irradiating the laser beam again, and the substrate 2 exposed at the bottom surface 14-3 of the first groove 14 can be etched in the plasma etching step 104.
[0051] In addition, in the wafer processing method according to the first embodiment, instead of the processing after the first processing groove covering step 103, a method including twice forming a protective film is considered, in which the protective film when the first processing groove for removing the functional layer is formed is cleaned, the protective film is covered again, and a second processing groove narrower than the first processing groove is formed. However, in this method, when the protective film is cleaned and covered again to form the second processing groove, the amount of the protective film used increases. However, in the wafer processing method according to the first embodiment, the protective film 13 when the first processing groove 14 is formed is suitably reused by supplying the solvent 15 in the first processing groove covering step 103, so that the protective film 13 used can be reduced compared to the method including twice forming the protective film as described above, as long as the protective film 13 formed in the protective film forming step 101 is not too thick, that is, as long as the protective film 13 is not formed to be twice as thick as the method including twice forming the protective film as described above.
[0052] In the wafer processing method according to the first embodiment, the solvent 15 may be supplied in a sprayed form in the first processed groove covering step 103. In this case, the wafer processing method according to the first embodiment can suppress the risk of excessively supplying the solvent 15 to wash and remove the protective film 13 with the solvent 15, and can suppress the excessive supply of the solvent 15 to liquefy a large amount of the protective film 13 and cause the liquefied protective film 13 to adhere to the bottom surface 14-3 of the first processed groove 14, and can suitably supply an appropriate amount of the solvent 15 to liquefy an appropriate amount of the protective film 13 that covers the side wall 14-2 of the first processed groove 14 while maintaining the exposure of the bottom surface 14-3 of the first processed groove 14, approximately uniformly to the front surface 3 of the wafer 1.
[0053] Furthermore, in the wafer processing method according to the first embodiment, at least one of the wafer 1 and the protective film 13 may be heated in the first groove covering step 103. In this case, the wafer processing method according to the first embodiment can supply the solvent 15 to increase the fluidity of the liquefied protective film 13, so that the liquefied protective film 13 can easily flow along the side wall 14-2 of the first groove 14.
[0054] In addition, in the wafer processing method of embodiment 1, in the first processing groove covering step 103, an external force of at least one of vibration and pressure may be applied to the protective film 13, in which case movement of the protective film 13 into the first processing groove 14 can be promoted.
[0055] [Embodiment 2] A wafer processing method according to the second embodiment will be described with reference to the drawings. FIG. 11 is a flow chart showing the flow of the wafer processing method according to the second embodiment. FIG. 12 is a schematic partial cross-sectional view of the main part of the wafer 1 in the first groove covering step 103 of the wafer processing method shown in FIG. 10. FIG. 13 is a schematic partial cross-sectional view of the main part of the wafer 1 after the second groove forming step 106 of the wafer processing method shown in FIG. 10. FIG. 14 is a cross-sectional view showing the main part of the wafer 1 in the plasma etching step 104 of the wafer processing method shown in FIG. 10. FIG. 15 is a cross-sectional view showing the main part of the wafer 1 after the cleaning step 105 of the wafer processing method shown in FIG. 10. In addition, in FIGS. 11, 12, 13, 14, and 15, the same parts as those in the first embodiment are denoted by the same reference numerals, and the description thereof will be omitted.
[0056] As shown in FIG. 11, the wafer processing method of embodiment 2 is the wafer processing method of embodiment 1 modified from the first machining groove covering step 103 onwards, and further modified to include a second machining groove forming step 106 after the first machining groove covering step 103 and before the plasma etching step 104.
[0057] The first groove covering step 103 in the second embodiment is a modification of the first groove covering step 103 in the first embodiment, in which the bottom surface 14-3 of the first groove 14 is also covered with the protective film 13.
[0058] In the second embodiment, in the first groove covering step 103, the solvent supply nozzle 16 supplies the solvent 15 for liquefying the protective film 13 to the front surface 3 of the wafer 1. The supplied solvent 15 liquefies at least a part of the protective film 13 formed on the front surface 3 of the wafer 1. At least a part of the protective film 13 liquefied by the solvent 15 flows along the side wall 14-2 of the first groove 14, and a further part of the liquefied protective film 13 flows to the bottom surface 14-3 of the first groove 14. In the first groove covering step 103, the liquefied protective film 13 that flows along the side wall 14-2 of the first groove 14 is dried again, so that the side wall 14-2 and bottom surface 14-3 of the first groove 14 are covered with the protective film 13, as shown in FIG. 12.
[0059] In embodiment 2, in the first groove covering step 103, the first groove 14 may be filled with a protective film 13 as shown in FIG. 12, or the side wall 14-2 and bottom surface 14-3 of the first groove 14 may be covered without filling the first groove 14 with the protective film 13.
[0060] In the second embodiment, in the first groove covering step 103, an appropriate amount of the solvent 15 is supplied in a spray (mist) form to the front surface 3 of the wafer 1 to liquefy an appropriate amount of the protective film 13. This suppresses the risk of the protective film 13 being washed away by the solvent 15 due to an excessive supply of the solvent 15, and makes it possible to suitably supply an appropriate amount of the solvent 15 that liquefies an appropriate amount of the protective film 13 that covers the side wall 14-2 and bottom surface 14-3 of the first groove 14 approximately uniformly to the front surface 3 of the wafer 1.
[0061] (Second machining groove forming step) The second groove forming step 106 is a step that follows the first groove covering step 103, in which a laser beam is applied along the first groove 14 to form a second groove 19 (shown in Figure 13) that is narrower (has a smaller width 19-1) than the first groove 14, and the protective film 13 covering the bottom surface 14-3 of the first groove 14 is removed while leaving the protective film 13 covering the side wall 14-2 of the first groove 14, thereby exposing the substrate 2 along the second groove 19.
[0062] In the second embodiment, in the second groove forming step 106, a laser processing device (not shown) suction-holds the back surface 9 of the wafer 1 on the holding surface of the holding table via tape 11, and clamps the frame 12 with a clamp section. In the second groove forming step 106, the laser processing device images the front surface 3 of the wafer 1 with an imaging unit (not shown), detects the planned division lines 4, and performs alignment to align the laser beam application unit with the planned division lines 4.
[0063] In the second embodiment, in the second groove forming step 106, the laser processing device irradiates the wafer 1 along the division lines 4 with a laser beam having a wavelength absorbed by the wafer 1 from the laser beam application unit while moving the wafer 1 and the laser beam application unit relatively along the division lines 4. Note that in the second groove forming step 106, the laser processing device sets the focal point of the laser beam on the protective film 13 or the surface of the substrate 2, and irradiates the wafer 1 with the laser beam along the first grooves 14 formed on each division line 4.
[0064] In embodiment 2, in the second processing groove formation step 106, a laser processing device performs ablation processing on the protective film 13 and substrate 2 on the bottom surface 14-3 of the first processing groove 14 formed at each planned division line 4, thereby removing part of them and forming a second processing groove 19 having a width 19-1 smaller than that of the first processing groove 14 on the bottom surface 14-3 of the first processing groove 14 that divides the functional layer 6 at each planned division line 4, as shown in Figure 13.
[0065] In the second embodiment, in the second groove forming step 106, a laser beam is irradiated to the center in the width direction of the first groove 14 formed on each of the planned division lines 4, and ablation is performed on the protective film 13 and the substrate 2 on the bottom surface 14-3 of the first groove 14 to form the second groove 19. In the second groove forming step 106, a laser beam having a wavelength of 355 nm (not limited to 355 nm, but a wavelength in the ultraviolet range is preferable) and a repetition frequency of 200 kHz to 1000 kHz is irradiated.
[0066] In the second processing groove forming step 106, the average output of the laser beam is 1.0 W, the processing feed rate is 200 mm / sec, and the spot of the focal point of the laser beam is a circle with a diameter of 25 μm to 40 μm. In the second processing groove forming step 106, the average output of the laser beam may be lower than the average output of the laser beam irradiated between the processing grooves in the first processing groove forming step 102. Thus, in the second processing groove forming step 106, the output of the irradiated laser beam is smaller than that in the first processing groove forming step 102. Alternatively, in the second processing groove forming step 106, the energy density of one spot of the laser beam irradiated in the second processing groove forming step 106 is lower than the energy density of one spot of the laser beam irradiated in the first processing groove forming step 102. In the second processing groove forming step 106, the width 19-1 of all the second processing grooves 19 is the same.
[0067] In the first groove forming step 102, it is necessary to remove the functional layer 6, which requires a laser beam with a high average power, while in the second groove forming step 106, it is sufficient to remove the protective film 13, which can be processed with a laser beam with a low average power. Therefore, in the second groove forming step 106 in the second groove forming step, the average power of the laser beam can be made lower than the average power of the laser beam irradiated between the grooves in the first groove forming step 102, so that the unevenness on the side wall 14-2 of the protective film 13 can be made clearly smaller than the unevenness on the side wall 14-2 of the functional layer 6.
[0068] The plasma etching step 104 in the second embodiment is a modification of the plasma etching step 104 in the first embodiment, in which the substrate 2 is processed along the second groove 19 formed in the second groove formation step 106. In the plasma etching step 104 in the second embodiment, similarly to the plasma etching step 104 in the first embodiment, in a state in which the sidewall 14-2 of the first groove 14 is covered with the protective film 13, the substrate 2 is processed by plasma etching using the protective film 13 as a mask.
[0069] In embodiment 2, in the plasma etching step 104, the plasmatized etching gas 18 is drawn into the wafer 1 side to plasma etch the substrate 2 exposed at the bottom of the second groove 19 formed in the protective film 13, which serves as a mask for the wafer 1, thereby causing the second groove 19 to progress toward the back surface 9 of the wafer 1.
[0070] The cleaning step 105 in the embodiment 2 is the same as the cleaning step 105 in the embodiment 1 except that the cleaning target is changed. In the cleaning step 105 in the embodiment 2, similarly to the embodiment 1, the cleaning water supplied to the front surface 3 of the wafer 1 flows from the center side to the outer periphery side on the front surface 3 of the wafer 1 by the centrifugal force generated by the rotation of the spinner table, cleaning the front surface 3 of the wafer 1, and removing the protective film 13 containing the water-soluble resin from the front surface 3 of the wafer 1 together with foreign matter such as debris, as shown in FIG.
[0071] The wafer processing method of embodiment 2 having the above-mentioned configuration is the wafer processing method of embodiment 1, modified in that in the first machining groove covering step 103, the bottom surface 14-3 of the first machining groove 14 is also covered with a protective film 13, and further includes a second machining groove forming step 106 after the first machining groove covering step 103, in which a laser beam is irradiated onto the first machining groove 14 to form a second machining groove 19 narrower than the first machining groove 14, and the protective film 13 covering the side wall 14-2 of the first machining groove 14 is removed to expose the substrate 2 while leaving the protective film 13 covering the bottom surface 14-3 of the first machining groove 14, and the substrate 2 is processed along the second machining groove 19 in the plasma etching step 104. Therefore, the wafer processing method of embodiment 2 has the same effect as embodiment 1, except that the first groove covering step 103 is performed so that the liquefied protective film 13 does not adhere to the bottom surface 14-3 of the first groove 14, thereby maintaining the bottom surface 14-3 of the first groove 14 exposed.
[0072] It is also possible to coat the protective film 13 again after forming the first groove 14 without cleaning the protective film 13, form a second groove 19 narrower than the first groove 14, and perform plasma etching step 104 on the second groove 19 using the recoated protective film 13 as a mask. This method eliminates the need for cleaning the protective film 13 to form the second groove 19, and therefore reduces the amount of protective film 13 used compared to the case where the protective film 13 is cleaned and then coated again.
[0073] It should be noted that the present invention is not limited to the above-described embodiment, and various modifications can be made without departing from the gist of the present invention. [Explanation of symbols]
[0074] 1 wafer 2. Board 3 surface 4. Planned division line 5 Devices 10 Device Chip 13 Protective film 14 1st machining groove 14-1 Width 14-2 Side wall 14-3 Bottom 15 Solvents 19 2nd machining groove 19-1 Width 101 Protective film formation step 102 First machining groove forming step 103 First machining groove covering step 104 Plasma Etching Step 105 Wash Step 106 Second machining groove forming step
Claims
1. A wafer processing method for processing a wafer having a substrate on a surface thereof, the substrate having device regions defined by a plurality of dividing lines, along the dividing lines, the method comprising the steps of: a protective film forming step of forming a protective film on the surface; a first groove forming step of irradiating the protective film with a laser beam along the intended division line to form a first groove for removing the protective film and exposing the substrate; a first groove covering step of liquidizing at least a portion of the protective film with a solvent after the first groove forming step, and covering a side wall of the first groove with the protective film; a plasma etching step of processing a substrate by plasma etching using the protective film as a mask in a state in which the sidewall of the first groove is covered with the protective film after the first groove covering step; A wafer processing method comprising the steps of:
2. In the first groove covering step, the bottom surface of the first groove is also covered with the protective film; The method further includes a second groove forming step of irradiating a laser beam onto the first groove after the first groove covering step to form a second groove narrower than the first groove, and removing the protective film covering the bottom surface of the first groove while leaving the protective film covering the sidewall of the first groove, thereby exposing the substrate, 2. The wafer processing method according to claim 1, wherein in the plasma etching step, the substrate is processed along a second processing groove.
3. 3. The wafer processing method according to claim 1, wherein in the first groove covering step, the solvent is supplied in a spray form.
4. 3. The wafer processing method according to claim 1, wherein in the first groove covering step, at least one of the wafer and the protective film is heated.
5. A wafer processing method as described in claim 1 or 2, characterized in that in the first groove covering step, an external force of at least one of vibration or pressure is applied to the protective film to promote movement of the protective film into the first groove.
Citation Information
Patent Citations
Processing method of work piece
JP2020027889A
Manufacturing method of device chip
JP2022052821A
Protective film agent and machining method for workpiece
JP2023041313A