Manufacturing method of resin molded article, and resin molded article
The method of pulverizing, melting, and maintaining the molten state in a mold cavity with gravity separation of decorative particles addresses the issue of excessive man-hours and design deterioration in resin molded products, achieving efficient production with reduced decorative particle presence.
Patent Information
- Application Number
- JP2023060214
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-03
- Publication Date
- 2024-10-16
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods for manufacturing resin molded products using waste materials require excessive man-hours due to the need for two-stage pulverization and separation of resin base material from decorative layers, leading to potential design deterioration.
A method involving pulverization, melting, and molten state maintenance in a mold cavity to separate decorative particles by gravity, combined with optional mixing of virgin material, reduces the need for manual separation and maintains the molten state to minimize decorative particle presence on the design surface.
This approach reduces man-hours and effectively suppresses design deterioration in resin molded products while maintaining mechanical strength, by minimizing decorative particle presence on the design surface.
Smart Images

Figure 2024147292000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a resin molded product and the resin molded product. [Background technology]
[0002] Conventionally, a method has been proposed for producing a resin molded product by collecting waste materials made of resin products with painted surfaces, such as automobile bumpers, and reusing them as raw materials (see, for example, Patent Document 1). In this method, the waste materials are first crushed into particles of an appropriate size. The crushed waste materials are then further finely crushed. Most of the finely crushed waste materials are resin substrates and coatings. Since there is a difference in specific gravity between the resin substrates and coatings in the finely crushed waste materials, they are separated using a known specific gravity method. Then, a resin molded product is produced using only the separated resin substrate as raw material. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 8-309750 Summary of the Invention [Problem to be solved by the invention]
[0004] However, the above-mentioned method can suppress the deterioration of the design of the resin molded product using the waste material, but the waste material is crushed in two stages and only the resin base material is separated from the crushed waste material by using a known specific gravity method, which requires a large number of steps. Therefore, there is still room for improvement in terms of reducing the number of steps required to manufacture the resin molded product while suppressing the deterioration of the design of the resin molded product using the waste material. [Means for solving the problem]
[0005] Hereinafter, various aspects of a method for producing a resin molded product and a resin molded product for solving the above problems will be described. [Embodiment 1] A method for manufacturing a resin molded product, comprising: a fine grinding process for finely grinding waste material having a base material made of thermoplastic resin and a decorative layer provided on the surface of the base material into granules; a melting process for melting the granular waste material finely ground in the fine grinding process; a molten state holding process for injecting the waste material melted in the melting process into a cavity of a molding die and holding the molten state of the waste material in the cavity; and a molding process for molding a resin molded product by cooling the waste material held in a molten state in the molten state holding process.
[0006] According to the above method, the molten state of the waste material is maintained in the cavity in the molten state maintaining step, so that the molten waste material can be prevented from being instantly cooled and solidified by heat exchange with the molding die. The molten waste material contains decorative layer particles (foreign matter). In the molten waste material, the decorative layer particles have a higher specific gravity than the base material. Therefore, the decorative layer particles contained in the molten waste material in the molten state in the molten state maintaining step settle in the cavity due to gravity. This reduces the proportion of decorative layer particles present in the design surface side portion of the resin molded product. Therefore, it is possible to suppress a decrease in the design of the resin molded product using the waste material.
[0007] In addition, unlike Patent Document 1, in order to prevent the deterioration of the design of the resin molded product using the waste material, it is not necessary to further finely pulverize the waste material after pulverization and to separate the finely pulverized waste material into particles of the resin substrate and particles of the decorative layer in the fine pulverization process, which reduces the number of steps required to manufacture the resin molded product.
[0008] Therefore, it is possible to reduce the number of steps required to manufacture a resin molded product using waste materials while suppressing a decrease in the design quality of the resin molded product. [Aspect 2] A method for manufacturing a resin molded product as described in [Aspect 1], characterized in that prior to the melting step, a mixing step is provided in which granular virgin material made of the same thermoplastic resin as the base material is mixed with the granular waste material finely ground in the fine grinding step, and in the melting step, the mixed material obtained by mixing the waste material and the virgin material is melted.
[0009] According to the above method, since virgin materials have a smaller specific gravity than waste materials, the ratio of waste materials to the design surface side of the resin molded product can be reduced. This reduces the number of particles (foreign matter) in the decorative layer near the design surface of the resin molded product. This makes it possible to more effectively prevent the design of the resin molded product using waste materials from deteriorating.
[0010] [Embodiment 3] A method for manufacturing a resin molded product, comprising: a fine grinding process for finely grinding waste material having a thermoplastic resin molded body colored with a pigment into granules; a melting process for melting the granular waste material finely ground in the fine grinding process; a molten state holding process for injecting the waste material melted in the melting process into a cavity of a molding die and holding the molten state of the waste material in the cavity; and a molding process for molding a resin molded product by cooling the waste material held in a molten state in the molten state holding process.
[0011] According to the above method, the molten state of the waste material is maintained in the cavity in the molten state maintaining step, so that the molten waste material can be prevented from being instantly cooled and solidified by heat exchange with the molding die. The molten waste material contains pigment particles (foreign matter). In the molten waste material, the pigment particles have a higher specific gravity than the thermoplastic resin that constitutes the molded body. Therefore, the pigment particles contained in the molten waste material in the molten state in the molten state maintaining step settle in the cavity due to gravity. This reduces the proportion of pigment particles present in the design surface side of the resin molded product. Therefore, it is possible to suppress a decrease in the design of the resin molded product using the waste material.
[0012] In addition, unlike Patent Document 1, in order to prevent the deterioration of the design of the resin molded product using the waste material, it is not necessary to further finely pulverize the waste material after pulverization and separate the finely pulverized waste material into resin base material particles and pigment particles in the fine pulverization step, which reduces the number of steps required to manufacture the resin molded product.
[0013] Therefore, it is possible to reduce the number of steps required to manufacture a resin molded product using waste materials while suppressing a decrease in the design quality of the resin molded product. [Aspect 4] A method for manufacturing a resin molded product as described in [Aspect 3], characterized in that prior to the melting step, a mixing step is provided in which granular virgin material made of the same thermoplastic resin as the molded body and having a different color from the waste material is mixed with the granular waste material that has been finely ground in the fine grinding step, and in the melting step, a mixed material in which the waste material and the virgin material are mixed is melted.
[0014] According to the above method, since virgin materials have a smaller specific gravity than waste materials, it is possible to reduce the proportion of waste materials in the design surface side of the resin molded product. This makes it possible to reduce the amount of pigment particles (foreign matter) present in the vicinity of the design surface of the resin molded product. Therefore, it is possible to more effectively prevent the deterioration of the design of the resin molded product using waste materials.
[0015] [Embodiment 5] A resin molded product having a base material made of a thermoplastic resin and particles dispersed in the base material and having a different color than the base material, characterized in that the proportion of the particles present in the portion of the base material on the design surface side is lower than the proportion of the particles present in portions of the base material other than the portion on the design surface side.
[0016] According to the above-mentioned configuration, the particles are less likely to appear on the design surface of the base material, so that deterioration of the design of the resin molded product can be suppressed. Effect of the Invention
[0017] The present invention has an effect of reducing the number of steps required to manufacture a resin molded product using waste materials while suppressing deterioration in the design of the resin molded product. [Brief description of the drawings]
[0018] [Figure 1] FIG. 1 is a schematic cross-sectional view showing one embodiment of a resin molded product. [Diagram 2] 2 is a flowchart showing a method for manufacturing the resin molded product of FIG. 1. [Diagram 3] 2 is a schematic cross-sectional view showing a state where a molten mixed material is injected into a mold for molding the resin molded product of FIG. 1. FIG. [Figure 4] 4 is a schematic cross-sectional view showing a state where decorating particles contained in the molten mixed material in FIG. 3 have settled down. FIG. [Diagram 5] 2 is a schematic cross-sectional view showing a state when the molding die is opened after molding of the resin molded product in FIG. 1. [Figure 6] FIG. 11 is a schematic cross-sectional view showing a molding die according to a modified example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] An embodiment will now be described with reference to the drawings. <Resin molded product 11> 1, the resin molded product 11 is, for example, an exterior part such as a bumper cover for a vehicle. The resin molded product 11 has a base material 12 made of a thermoplastic resin and decorative particles 13 as an example of particles dispersed in the base material 12. The base material 12 is made of, for example, polypropylene (PP).
[0020] The decorative particles 13 are formed by pulverizing a decorative layer contained in, for example, scrap material of a vehicle bumper cover. Examples of the decorative layer include a coating film, a plating layer, a hot stamp layer, a film layer, a vapor deposition layer, and a printing layer. The maximum particle size of the decorative particles 13 is, for example, 300 μm. The decorative particles 13 have a different color from the base material 12.
[0021] The resin molded product 11 has a planar design surface 14. The resin molded product 11 has a structure having a first region 15 constituting the portion on the design surface 14 side, and a second region 16 constituting the portion other than the first region 15. The second region 16 contains most of the decorative particles 13. The first region 15 contains almost no decorative particles 13. The proportion of the decorative particles 13 present in the first region 15 is significantly lower than the proportion of the decorative particles 13 present in the second region 16.
[0022] Next, a method for producing the resin molded product 11 will be described. As shown in FIG. 2, the method for producing the resin molded product 11 includes a pulverizing step, a mixing step, a melting step, a molten state maintaining step, a molding step, and a removal step.
[0023] <Fine grinding process> In the pulverization process, a waste material (not shown) having a base material made of a thermoplastic resin and a decorative layer provided on the surface of the base material is pulverized into granules by a known pulverizer. The waste material is, for example, a bumper cover of a vehicle.
[0024] <Mixing process> In the mixing step, granular virgin material made of the same thermoplastic resin as the base material is mixed with granular waste material that has been finely pulverized in the fine pulverization step (both not shown).
[0025] <Melting process> In the melting process, the mixture of the virgin material and the waste material in the mixing process is poured into the cylinder of a known injection molding machine, and the mixture in the cylinder is heated by passing electricity through a heater, thereby raising the temperature of the mixture to a temperature equal to or higher than the melting point of the thermoplastic resin, and melting the mixture.
[0026] <Molten state maintaining process> As shown in Fig. 3, in the molten state maintaining step, the mixed material molten in the melting step is injected from the cylinder into the cavity 18 of the molding die 17 in the clamped state, and the molten state of the mixed material in the cavity 18 is maintained. The molding die 17 includes a first die 20 having a molding surface 19 for forming the design surface 14 of the resin molded product 11, and a second die 21. The first die 20 and the second die 21 are molds that are opened and closed in the vertical direction. The first die 20 is disposed above the second die 21.
[0027] The molten state of the mixed material in the cavity 18 is maintained by flowing pressurized hot water through a heat transfer medium flow path 22 provided in the mold 17 in order to control the temperature of the cavity 18. In other words, by flowing pressurized hot water through the heat transfer medium flow path 22 provided in the mold 17, the molten mixed material in the cavity 18 is prevented from being instantly cooled and solidified by heat exchange with the mold 17. The molten mixed material in the cavity 18 contains waste material including the base material and decorative particles 13, but the decorative particles 13 have a larger specific gravity than the base material and virgin material.
[0028] 4, when the mixed material is maintained in a molten state in the cavity 18, the decorative particles 13 contained in the mixed material are precipitated by gravity to the lower side opposite the molding surface 19. As a result, the decorative particles 13 present in the upper part of the mixed material on the molding surface 19 side are almost completely removed.
[0029] The time for which the mixed material is kept in the molten state in the cavity 18 in the molten state holding step is set to a time for which the decorative particles 13 contained in the mixed material are sufficiently precipitated by gravity (for example, about 30 to 60 seconds). This time is determined in advance by conducting experiments and simulations.
[0030] <Forming process> In the molding process, the mixed material kept in a molten state in the molten state keeping process is cooled to mold a resin molded product 11 (see FIG. 5). That is, in the molding process, cold water is passed through the heat transfer medium flow path 22 instead of pressurized hot water to cool and solidify the mixed material in the cavity 18.
[0031] <Removal process> As shown in FIG. 5, in the removal step, molding die 17 is opened, and resin molded article 11 molded in the molding step is removed from second die .
[0032] <Operation of the embodiment> As shown in Fig. 1, the first region 15 constituting the portion on the design surface 14 side of the resin molded product 11 molded using waste materials contains almost no decorative particles 13. This makes it difficult for the decorative particles 13 to appear on the design surface 14. This prevents the decorative particles 13 from deteriorating the design of the resin molded product 11.
[0033] <Effects of the embodiment> According to the embodiment described above in detail, the following effects are achieved. (1) The method for producing the resin molded article 11 includes a pulverizing step, a melting step, a molten state maintaining step, and a molding step.
[0034] According to the above method, the molten state of the waste material is maintained in the cavity 18 in the molten state maintaining step, so that the molten waste material can be prevented from being instantly cooled and solidified by heat exchange with the molding die 17. Therefore, the decorative particles 13 contained in the molten waste material in the molten state maintaining step settle in the cavity 18 due to gravity. This reduces the proportion of the decorative particles 13 present in the portion of the resin molded product 11 on the design surface 14 side. Therefore, it is possible to suppress a decrease in the design of the resin molded product 11 using the waste material.
[0035] In addition, unlike Patent Document 1, in order to suppress deterioration of the design of the resin molded product 11 using the waste material, there is no need to further finely pulverize the waste material after pulverizing it in the fine pulverizing step, and to separate the finely pulverized waste material into resin base material particles and decorative particles 13. Therefore, the number of steps required to manufacture the resin molded product 11 can be reduced.
[0036] Therefore, the number of steps required to manufacture the resin molded product 11 using waste materials can be reduced while preventing deterioration in the design of the resin molded product 11. (2) The method for producing the resin molded product 11 includes a mixing step prior to the melting step, in which a mixture of waste material and virgin material is melted.
[0037] According to the above method, since virgin materials have a smaller specific gravity than waste materials, it is possible to reduce the proportion of waste materials in the portion of the resin molded product 11 on the design surface 14 side. This makes it possible to reduce the number of decorative particles 13 present in the vicinity of the design surface 14 (first region 15) of the resin molded product 11. This makes it possible to more effectively prevent the deterioration of the design of the resin molded product 11 using waste materials.
[0038] In addition, since the resin molded product 11 contains virgin material, the mechanical strength of the resin molded product 11 can be increased compared to when the resin molded product 11 is formed from only waste materials. <Example of change> The above embodiment can be modified as follows: The above embodiment and the following modifications can be combined with each other as long as they are not technically inconsistent.
[0039] As shown in Fig. 6, a heat insulating layer 23 may be provided on the cavity surface of the mold 17. The heat insulating layer 23 is made of a material with low thermal conductivity. Examples of materials with low thermal conductivity include metal materials with relatively low thermal conductivity such as austenitic stainless steel (SUS304, etc.), polyimide, and ceramics. In this way, the molten state of the mixed material in the cavity 18 can be maintained without flowing a heating fluid through the heat transfer medium flow path 22 of the mold 17 in the molten state maintaining step, so that the heat transfer medium flow path 22 can be omitted from the mold 17.
[0040] As a method for heating the cavity 18 in the molten state maintaining step, in addition to the method using pressurized hot water described above, a steam heating method, a heated oil method, a high-frequency induction heating method, a radiant heating method, an electric heating method, a cartridge heater method, a capillary heater method, etc. may be used.
[0041] The molding die 17 may be provided with separate heat transfer medium flow paths 22 for flowing pressurized hot water and for flowing cold water. The mixing step may be omitted. In this case, the resin molded product 11 is produced using only waste materials.
[0042] The base material 12 is not limited to polypropylene, and may be made of other thermoplastic resins such as polyethylene terephthalate. The resin molded product 11 is not limited to an exterior component such as a bumper cover for a vehicle, but may also be embodied as an interior component for a vehicle, such as an instrument panel.
[0043] In the pulverizing step of the above embodiment, the waste material having a base material made of a thermoplastic resin and a decorative layer provided on the surface of the base material is pulverized into granules, but the waste material having a molded body made of a thermoplastic resin colored with a pigment may be pulverized into granules. In this case, in the mixing step, a granular virgin material made of the same thermoplastic resin as the molded body and having a different color from the waste material is mixed with the granular waste material pulverized in the pulverizing step. Then, the melting step, the molten state maintaining step, and the molding step may be performed in the same manner as in the above embodiment. Even in this way, the same action and effect as in the above embodiment can be obtained. The mixing step may be omitted. [Explanation of symbols]
[0044] 11…Resin molded products 12...Base material 13...Decorative particles 14…Design surface 15...First area 16…Second area 17…Mold 18…Cavity 19…molding surface 20...Type 1 21…2nd type 22...Heat medium flow path 23…Thermal insulation layer
Claims
1. A fine pulverizing process for pulverizing a waste material having a base material made of a thermoplastic resin and a decorative layer provided on a surface of the base material into granules; a melting step of melting the granular waste material pulverized in the fine pulverization step; a molten state maintaining step of injecting the waste material melted in the melting step into a cavity of a molding die and maintaining the molten state of the waste material in the cavity; a molding step of molding a resin molded product by cooling the waste material held in a molten state in the molten state holding step; A method for producing a resin molded product comprising:
2. Prior to the melting step, a mixing step is provided in which a granular virgin material made of the same thermoplastic resin as the base material is mixed with the granular waste material finely pulverized in the fine pulverization step; 2. The method for producing a resin molded product according to claim 1, wherein the melting step melts a mixture of the waste material and the virgin material.
3. a fine grinding step of finely grinding waste material having a thermoplastic resin molded body colored with a pigment into granules; a melting step of melting the granular waste material pulverized in the fine pulverization step; a molten state maintaining step of injecting the waste material melted in the melting step into a cavity of a molding die and maintaining the molten state of the waste material in the cavity; a molding step of molding a resin molded product by cooling the waste material held in a molten state in the molten state holding step; A method for producing a resin molded product comprising:
4. A mixing step is provided prior to the melting step, in which a granular virgin material made of the same thermoplastic resin as the molded body and having a different color from the waste material is mixed with the granular waste material finely pulverized in the fine pulverization step, 4. The method for producing a resin molded product according to claim 3, wherein in the melting step, a mixture of the waste material and the virgin material is melted.
5. A base material made of a thermoplastic resin; Particles dispersed in the base material and having a different color from that of the base material; A resin molded product having the following structure: A resin molded product, characterized in that the proportion of the particles present in the portion of the base material on the design surface side is lower than the proportion of the particles present in portions of the base material other than the portion on the design surface side.
Citation Information
Patent Citations
Process for producing molded article of reclaimed thermoplastic resin
CN1622873A
System for re-commercializing electrical household appliance and OA equipment product
JP2001038729A
Method for manufacturing exterior parts for car
JP2001341173A
Method for injection-molding recycled resin
JP2001353742A
Resin molded article and molding method therefor
JP2002337179A