Steel material
A low-hardness steel material with controlled ferrite and pearlite structures addresses the burr issue in cold forging, ensuring excellent cold workability and reduced burr height through optimized chemical composition and microstructure.
Patent Information
- Application Number
- JP2023060278
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-03
- Publication Date
- 2024-10-16
AI Technical Summary
The challenge in manufacturing automotive parts through cold forging is the occurrence of high burrs due to the ductility of steel materials, which can cause scratches and mold damage, and existing solutions do not adequately address burr height after cutting.
A low-hardness steel material with a specific chemical composition and controlled microstructure, including a ferrite and pearlite area ratio, average distance between pearlite blocks, and Vickers hardness, is developed to ensure excellent cold workability and reduce burr height.
The steel material achieves improved cold workability and significantly lowers burr height after cutting, even when hot-rolled, by optimizing the chemical composition and microstructure.
Smart Images

Figure 2024147332000001 
Figure 2024147332000002 
Figure 2024147332000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a steel material. [Background technology]
[0002] In recent years, from the viewpoint of energy saving, for example, in the manufacture of automotive parts such as gears, shafts, and bolts, the replacement of hot forging with cold forging has been considered.
[0003] When hot forging is switched to cold forging, the steel material has a problem of insufficient ductility. In order to solve this problem, the steel material to be subjected to cold forging is generally subjected to spheroidizing annealing (SA) before cold forging. Since spheroidizing annealing requires heating the steel material to a high temperature range and holding it there for a long time, heat treatment equipment such as a heating furnace is required, and energy is consumed for heating. Therefore, spheroidizing annealing increases manufacturing costs. From the viewpoint of improving productivity and saving energy, various techniques have been proposed to simplify and omit spheroidizing annealing.
[0004] For example, Patent Document 1 discloses a steel in which Ti carbide, Ti-containing composite carbide, and Ti nitride are finely precipitated, thereby suppressing the growth of austenite crystal grains during rolling or forging, increasing the amount of ferrite in the structure after rolling or forging, and making the ferrite grain size uniform, thereby improving the cold workability and heat treatment distortion characteristics.
[0005] Patent Document 2 discloses that by adding Zr and / or Hf as an element that generates a dynamic strain aging effect during cold working to increase deformation resistance and fixes free N that interferes with the hardenability effect of B, it is possible to omit softening annealing treatment before cold working and to perform good cold working in an unrefined state, and to obtain wire- or bar-shaped steel with excellent strength stability that can ensure stable strength even when heat treatment is performed after part forming.
[0006] Patent Document 3 discloses a hot-rolled steel bar or wire rod, which in an as-hot-rolled state has an average Vickers hardness of 240 or less, a Vickers hardness of a surface layer of 180 or less, a microstructure consisting of a ferrite-pearlite structure or a ferrite-pearlite-bainite structure with an area ratio of ferrite phase of 30% or more, and a maximum continuous length of the pearlite phase and / or bainite phase in the rolling direction of 600 μm or less. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Patent No. 3333697 [Patent Document 2] Patent No. 3949899 [Patent Document 3] Patent No. 4888277 Summary of the Invention [Problem to be solved by the invention]
[0008] When manufacturing the above-mentioned automotive parts, the steel material is cut to a predetermined length by a shear or saw. If high burrs are generated in the cut steel material, the burrs may bite into the steel material during cold forging, causing scratches on the steel material and the die. The metal structure of the steel material subjected to cold forging is mainly composed of ferrite, which has excellent ductility, in order to suppress cracking. However, this ferrite may not be destroyed during cutting, resulting in large burrs.
[0009] In the above Patent Documents 1 and 2, the metal structure is made ferrite and pearlite to ensure cold forgeability, but the burr height after cutting is not taken into consideration. In the above Patent Document 3, the occurrence of cracks during cutting using a shear is taken into consideration, but the cold forgeability may be improved by further reducing the hardness.
[0010] The present invention has been made in view of the above-mentioned circumstances, and has an object to provide a low-hardness steel material which can be subjected to cold working such as cold forging, cold rolling, cold heading, etc. without cracking even in the as-hot-rolled state, i.e., has excellent cold workability, and has a small burr height after cutting. [Means for solving the problem]
[0011] The gist of the present invention is as follows. (1) A steel material according to one embodiment of the present invention has a chemical composition, in mass%, Chemical composition, in mass%, C: 0.10-0.42%, Si: 0.01 to 0.30%, Mn: 0.20-1.00%, P: less than 0.050% S: 0.001 to 0.050%, Al: 0.001 to 0.200%, N: less than 0.020%, Cr: 0.01-1.50%, and O: Contains 0.0030% or less, the balance being Fe and impurities, In the metal structure at a position 0.50R from the surface, The area ratio of ferrite is 50% or more, and the area ratio of pearlite is 20% or more, The average distance between the centers of gravity of the pearlite blocks is 20 to 50 μm; The Vickers hardness is 170HV or less. (2) The steel material described in (1) above has a metal structure at a position 200 μm from the surface, The area ratio of ferrite is 50% or more, and the area ratio of pearlite is 20% or more, The average distance between the centers of gravity of the pearlite blocks is 20 to 50 μm; The Vickers hardness may be 170 HV or less. (3) A steel material according to another embodiment of the present invention has a chemical composition, in mass%, Chemical composition, in mass%, C: 0.10-0.42%, Si: 0.01 to 0.10%, Mn: 0.20-1.00%, P: less than 0.050% S: 0.001 to 0.050%, Al: 0.001 to 0.200%, N: less than 0.020%, Cr: 0.01-1.50%, and O: Contains 0.0030% or less, Further, it contains one or more selected from the group consisting of the following groups A, B, and C: the balance being Fe and impurities, In the metal structure at a position 0.50R from the surface, The area ratio of ferrite is 50% or more, and the area ratio of pearlite is 20% or more, The average distance between the centers of gravity of the pearlite blocks is 20 to 50 μm; The Vickers hardness is 170HV or less. [Group A] Mo: 0.30% or less V: 0.150% or less, Nb: 0.050% or less, and Ti: 0.100% or less, One or more selected from the group consisting of [Group B] Cu: 0.40% or less, Ni: 0.30% or less, Sn: 0.100% or less, and B: 0.0200% or less One or more selected from the group consisting of [Group C] Ca: 0.0050% or less, and Mg: 0.0050% or less One or two selected from the group consisting of (4) The steel material described in (3) above has a metal structure at a position 200 μm from the surface, The area ratio of ferrite is 50% or more, and the area ratio of pearlite is 20% or more, The average distance between the centers of gravity of the pearlite blocks is 20 to 50 μm; The Vickers hardness may be 170 HV or less. (5) The steel material described in (3) or (4) above may have a chemical composition containing, in mass %, the Group A. (6) The steel material according to (3) or (4) above may have a chemical composition containing, in mass %, the B group. (7) The steel material according to (3) or (4) above may have a chemical composition containing, in mass %, the C group. Effect of the Invention
[0012] According to the above-described aspects of the present invention, it is possible to provide a steel material having excellent cold workability even in an as-hot-rolled state, and having low hardness with low burr height after cutting. Furthermore, according to a preferred embodiment of the present invention, a steel material having the above-mentioned properties and having a smaller burr height after cutting can be provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, each requirement of the steel material according to this embodiment will be described in detail. First, the chemical composition of the steel material according to this embodiment will be described. In the following, the numerical ranges described with "~" include the lower and upper limits. Numerical values indicated as "less than" and "greater than" do not include the numerical range. All "%" in the chemical composition means "mass %".
[0014] The steel material according to the present embodiment is cut to a predetermined length by, for example, a shear or a saw, and then subjected to cold working such as cold forging, cold rolling, cold heading, etc. to form a part shape. First, the chemical composition of the steel material according to the present embodiment will be described. The steel material according to this embodiment has a chemical composition, in mass%, of C: 0.10-0.42%, Si: 0.01-0.30%, Mn: 0.20-1.00%, P: less than 0.050%, S: 0.001-0.050%, Al: 0.001-0.200%, N: less than 0.020%, Cr: 0.01-1.50%, O: 0.0030% or less, and the balance: Fe and impurities. Each element will be described below.
[0015] C: 0.10-0.42% C is an element that increases the hardness of steel. C is also an element that generates a desired amount of pearlite. If the C content is less than 0.10%, the desired amount of pearlite cannot be obtained, and the average distance between pearlite blocks cannot be controlled favorably, resulting in high burr height after cutting. Therefore, the C content is set to 0.10% or more. The C content is preferably 0.15% or more, and more preferably 0.20% or more. On the other hand, if the C content exceeds 0.42%, the amount of ferrite increases, the hardness of the steel material becomes too high, and the cold workability is deteriorated. Therefore, the C content is set to 0.42% or less. The C content is preferably 0.40% or less, 0.35% or less, 0.30% or less, less than 0.30%, 0.28% or less, and more preferably 0.26% or less.
[0016] Silicon: 0.01 to 0.30% Silicon is an element that enhances the hardenability of steel. If the silicon content is less than 0.01%, the desired hardness cannot be obtained in the part. Therefore, the silicon content is set to 0.01% or more. The silicon content is preferably 0.02% or more, and more preferably 0.04% or more. On the other hand, if the Si content exceeds 0.30%, the hardness of the steel material becomes too high, resulting in poor cold workability. Therefore, the Si content is set to 0.30% or less. The Si content is preferably 0.25% or less, and more preferably 0.15% or less.
[0017] Mn: 0.20-1.00% Mn is an element that increases the hardness of steel materials. If the Mn content is less than 0.20%, the hardness decreases and the burr height increases after cutting. Therefore, the Mn content is set to 0.20% or more. The Mn content is preferably 0.25% or more, and more preferably 0.40% or more. On the other hand, if the Mn content exceeds 1.00%, the hardness of the steel material becomes too high, resulting in poor cold workability. Therefore, the Mn content is set to 1.00% or less. The Mn content is preferably 0.80% or less, and more preferably 0.70% or less.
[0018] P: Less than 0.050% P is an element that may be contained in steel even if it is not intentionally added. P is likely to segregate in steel, causing localized reduction in ductility. In particular, if the P content is 0.050% or more, the localized reduction in ductility becomes significant. Therefore, the P content is set to less than 0.050%. The P content is preferably 0.030% or less. The lower limit of the P content is not particularly limited, but may be 0% or more, or may be more than 0% or 0.002% or more.
[0019] S: 0.001 to 0.050% S is an element that may be contained in steel even if it is not intentionally added. S combines with Mn in steel to form MnS, which causes cracks during hot rolling. Therefore, the S content is set to 0.050% or less. The S content is preferably 0.040% or less, and more preferably 0.030% or less. Since excessive reduction in the S content significantly increases the cost of desulfurization, the S content is set to 0.001% or more, preferably 0.005% or more, and more preferably 0.010% or more.
[0020] Al: 0.001 to 0.200% Al is an element effective as a deoxidizer. If the Al content is less than 0.001%, the effect as a deoxidizer cannot be obtained. Therefore, the Al content is set to 0.001% or more. The Al content is preferably 0.005% or more, and more preferably 0.010% or more. On the other hand, if the Al content exceeds 0.200%, coarse nitrides are formed in the rolled material, which become the starting points for cracks during cold working. Therefore, the Al content is set to 0.200% or less. The Al content is preferably 0.150% or less, and more preferably 0.100% or less.
[0021] N: Less than 0.020% N is an element that may be contained in steel even if it is not intentionally added. If the N content is 0.020% or more, the toughness of the part deteriorates significantly. Therefore, the N content is set to less than 0.020%. The N content is preferably 0.018% or less, and more preferably 0.015% or less. The lower limit of the N content is not particularly limited, but may be 0% or more, or may be more than 0% or 0.005% or more.
[0022] Cr: 0.01~1.50% Cr is an element that increases the hardenability of steel and increases the hardness of parts. If the Cr content is less than 0.01%, the desired hardness cannot be obtained in the parts. Therefore, the Cr content is set to 0.01% or more. The Cr content is preferably 0.50% or more, and more preferably 0.90% or more. On the other hand, if the Cr content exceeds 1.50%, the hardness becomes too high and the cold workability deteriorates. Therefore, the Cr content is set to 1.50% or less. The Cr content is preferably 1.40% or less, and more preferably 1.30% or less.
[0023] O: 0.0030% or less If the O content in steel is large, it forms coarse oxides that become the starting points of fracture and deteriorates the cold workability of the steel. Therefore, the O content is set to 0.0030% or less. The O content is preferably 0.0020% or less, and more preferably 0.0015% or less. The lower limit of the O content is not particularly limited, but may be 0% or more, or may be more than 0% or 0.0005% or more.
[0024] The balance of the chemical composition of the steel material according to the present embodiment may be Fe and impurities. In the present embodiment, the impurities include elements that are mixed in from raw materials such as ore and scrap, or from the manufacturing environment, during industrial production of steel materials, and are permissible within a range that does not impair the properties of the steel material according to the present embodiment.
[0025] The chemical composition of the steel material according to this embodiment may further contain, as an optional element, one or more elements selected from the group consisting of the following groups A, B, and C, instead of a portion of Fe. When the following optional elements are not contained, the content is 0%. [Group A] Mo: 0.30% or less V: 0.150% or less, Nb: 0.050% or less, and Ti: 0.100% or less, One or more selected from the group consisting of [Group B] Cu: 0.40% or less, Ni: 0.30% or less, Sn: 0.100% or less, and B: 0.0200% or less One or more selected from the group consisting of [Group C] Ca: 0.0050% or less, and Mg: 0.0050% or less One or two selected from the group consisting of
[0026] Mo: 0.30% or less Mo is an element that improves the strength of steel materials by precipitation strengthening. Mo may be added as necessary to obtain this effect. However, if the Mo content exceeds 0.30%, the cracking sensitivity of the slab increases, which may make the slab difficult to handle. Therefore, the Mo content is preferably 0.30% or less. The Mo content may be 0%.
[0027] V:0.150% or less V is an element that improves the strength of steel materials by precipitation strengthening. V may be added as necessary to obtain this effect. However, if the V content exceeds 0.150%, a large amount of carbonitrides may precipitate, deteriorating the cold workability of the steel material. Therefore, the V content is preferably 0.150% or less. The V content may be 0%.
[0028] Nb: 0.050% or less Nb is an element that improves the strength of steel by refining the grain size and strengthening the precipitation of NbC. Nb may be added as necessary to obtain this effect. However, even if the Nb content exceeds 0.050%, the above effect is saturated. Therefore, the Nb content is preferably 0.050% or less. The Nb content may be 0%.
[0029] Ti:0.100% or less Ti is an element that improves the strength of steel materials by refining the crystal grain size and precipitation strengthening of TiC. If the Ti content exceeds 0.100%, coarse TiN may be formed, which may deteriorate the toughness of parts. Therefore, the Ti content is preferably 0.100% or less. The Ti content is more preferably 0.030% or less. The Ti content may be 0%.
[0030] Cu:0.40% or less Cu is an element that increases the hardness of parts. Cu may be contained as necessary to obtain this effect. The Cu content may be 0%, but in order to reliably obtain this effect, it is preferable that the Cu content be 0.02% or more. However, if the Cu content exceeds 0.40%, the toughness of the part may decrease. Therefore, the Cu content is preferably 0.40% or less, and more preferably 0.25% or less.
[0031] Ni: 0.30% or less Ni is an element that increases the hardness of parts. Ni may be contained as necessary to obtain this effect. The Ni content may be 0%, but to ensure this effect, the Ni content is preferably 0.02% or more. However, if the Ni content exceeds 0.30%, the toughness of the part may deteriorate. Therefore, the Ni content is preferably 0.30% or less, and more preferably 0.25% or less.
[0032] Sn: 0.100% or less Sn is an element that suppresses the coarsening of crystal grains and improves the strength of steel. Sn may be contained as necessary to obtain this effect. However, if the Sn content exceeds 0.100%, the steel becomes brittle and easily breaks during hot rolling. Therefore, the Sn content is preferably 0.100% or less. The Sn content may be 0%.
[0033] B: 0.0200% or less B is an element that combines with N in steel to form nitrides. If the B content exceeds 0.0200%, coarse nitrides may be formed, which may deteriorate the toughness of the part. Therefore, the B content is preferably 0.0200% or less. The B content is more preferably 0.0030% or less. Since it is preferable that B is not contained, the B content may be 0%.
[0034] Ca: 0.0050% or less Ca is an element that fixes S in steel as spherical CaS and suppresses the generation of elongated inclusions such as MnS, thereby improving the formability of the steel material. Ca may be added as necessary to obtain this effect. However, even if the Ca content exceeds 0.0050%, the above effect is saturated. Therefore, the Ca content is preferably 0.0050% or less. The Ca content may be 0%.
[0035] Mg: 0.0050% or less Mg has the effect of improving the formability of steel by adjusting the shape of inclusions in steel to a preferred shape. Mg may be added as necessary to obtain this effect. However, if the Mg content exceeds 0.0050%, excessive inclusions are generated in the steel, which may actually reduce the formability of the steel. Therefore, the Mg content is preferably 0.0050% or less. The Mg content may be 0%.
[0036] The chemical composition of the above-mentioned steel material may be measured by a general analytical method. For example, it may be measured by ICP-AES (Inductively Coupled Plasma-Atomic Emission Spectrometry). Note that C and S may be measured by the combustion-infrared absorption method, N by the inert gas fusion-thermal conductivity method, and O by the inert gas fusion-non-dispersive infrared absorption method. The content of each element is determined by rounding off the measured value based on the significant figures specified in this embodiment to the minimum digit of the content of each element specified in this embodiment.
[0037] Next, the metal structure of the steel material according to this embodiment will be described. In the steel material according to this embodiment, in the metal structure at a position 0.50R from the surface, the area ratio of ferrite is 50% or more, the area ratio of pearlite is 20% or more, and the average distance between the centers of gravity of pearlite blocks is 20 to 50 μm. In addition, the "R" in "a position 0.50R from the surface" refers to the radius if the steel material is a bar, and refers to 1 / 2 the plate thickness if the steel material is a steel plate.
[0038] Ferrite area ratio: 50% or more Ferrite is a structure with relatively low hardness and high deformability. If the area ratio of ferrite is less than 50%, the hardness of the steel material becomes too high, and the cold workability deteriorates. Therefore, the area ratio of ferrite is set to 50% or more. The area ratio of ferrite is preferably 55% or more, and more preferably 60% or more. The upper limit of the area ratio of ferrite is not particularly limited, but may be 80% or less in relation to the area ratio of pearlite described later.
[0039] Perlite area ratio: 20% or more In the steel material according to the present embodiment, the average distance between the centers of gravity of the pearlite blocks is controlled to reduce the burr height after cutting, and therefore, pearlite is an important structure in the present embodiment. If the area ratio of pearlite is less than 20%, the burr height after cutting cannot be reduced. Therefore, the area ratio of pearlite is set to 20% or more. The area ratio of pearlite is preferably 25% or more, and more preferably 30% or more. The upper limit of the area ratio of pearlite is not particularly limited, but may be 50% or less in relation to the area ratio of ferrite.
[0040] remnant tissue The metal structure of the steel material according to this embodiment may contain bainite and martensite as a remaining structure other than ferrite and pearlite. The area ratio of the remaining structure is preferably 5% or less in order to secure a desired amount of ferrite and pearlite. The area ratio of the remaining structure is more preferably 1% or less, and even more preferably 0%.
[0041] The area ratios of ferrite and pearlite are measured by the following method. A sample is taken from the surface of the steel material at a position 0.50R away from the rolling direction so that the cross section perpendicular to the rolling direction can be observed. The cross section of this sample is then mirror-finished.
[0042] After polishing the observation surface of the sample, the observation surface is etched for 10 seconds using 3% by volume nitric acid alcohol (Nital etching solution). A microstructure photograph is taken of the observation field (0.3 mm x 0.4 mm) of the etched observation surface using an optical microscope at 400x magnification. In the taken microstructure photograph, phases are identified by contrast. In the microstructure photograph, ferrite, pearlite, bainite, and martensite can be easily distinguished by contrast. Ferrite is observed as a white area. Pearlite is observed as a phase with a lamellar structure or as black and gray areas. The area ratio of ferrite is obtained by calculating the area ratio of the area observed as ferrite. The area ratio of pearlite is also obtained by calculating the area ratio of the area observed as pearlite. Bainite and martensite are observed as regions with lower brightness than ferrite. The area ratio of each phase may be measured using a general-purpose image analysis software such as WinROOF.
[0043] Average distance between the centers of gravity of pearlite blocks: 20~50μm If the average distance between the centers of gravity of the pearlite blocks at the 0.50R position from the surface is less than 20 μm, the hardness of the steel material increases due to the refinement of the structure, and the cold workability deteriorates. Therefore, the average distance between the centers of gravity of the pearlite blocks is set to 20 μm or more. The average distance between the centers of gravity of the pearlite blocks is preferably 30 μm or more, and more preferably 35 μm or more. On the other hand, if the average distance between the centers of gravity of the perlite blocks exceeds 50 μm, the perlite blocks are unevenly distributed, resulting in high burr height after cutting. Therefore, the average distance between the centers of gravity of the perlite blocks is set to 50 μm or less. The average distance between the centers of gravity of the perlite blocks is preferably 45 μm or less, more preferably 40 μm or less.
[0044] The average distance between the centers of gravity of the pearlite blocks is measured by the following method. Using the same method as in the above-mentioned area ratio measurement method, ferrite and pearlite are identified from a structural photograph taken with a 100x optical microscope. The measurement field of view is 0.5 mm x 1.0 mm. The image is binarized so that the identified pearlite appears black and the ferrite appears white. The obtained binarized image is used to identify the center of gravity of each pearlite grain, and the average distance between the center of gravity coordinates of adjacent pearlite grains is measured. The analysis from binarization to measurement of the average distance between the centers of gravity can be performed using a commonly used image analysis software such as WinROOF manufactured by Mitani Shoji Co., Ltd.
[0045] The steel material according to this embodiment has a Vickers hardness of 170Hv or less at a position 0.50R from the surface. By setting the Vickers hardness to 170Hv or less, the hardness does not become too high and cold workability can be improved. The Vickers hardness is preferably 160Hv or less, more preferably 150Hv or less. The lower limit of the Vickers hardness is not particularly limited, but may be 100Hv or more, or 120Hv or more.
[0046] The Vickers hardness of the steel material is measured by the following method. A test piece is taken from the steel material, and the cross section of the plate thickness is polished with waterproof abrasive paper. Next, after buffing with a diamond suspension, the Vickers hardness is measured at 10 or more points 50 μm deep from the surface in accordance with JIS Z 2244-1:2020. The applied load is 300 gf. The Vickers hardness is obtained by calculating the average of the obtained measured values. In addition, the standard deviation of the Vickers hardness is obtained by calculating the standard deviation from the obtained measured values. The Vickers hardness is measured using a micro Vickers hardness tester.
[0047] In the steel material according to this embodiment, in the metal structure at a position 200 μm from the surface, the area ratio of ferrite may be 50% or more, the area ratio of pearlite may be 20% or more, the average distance between the centers of gravity of pearlite blocks may be 20 to 50 μm, and the Vickers hardness may be 170 HV or less. By having the above metal structure at a position 200 μm from the surface in addition to the position 0.50R from the surface, the burr height after cutting can be further reduced. The measurement can be performed at different measurement positions in the same manner as for the metal structure at a position 0.50R from the surface.
[0048] Next, a preferred method for manufacturing the steel material according to the present embodiment will be described. According to the manufacturing method described below, the steel material according to the present embodiment can be stably manufactured. Note that the temperature described below refers to the surface temperature of the slab or steel plate.
[0049] A preferred method for producing the steel material according to this embodiment comprises the following steps. In the finish rolling of the hot rolling, the passing time between stands is less than 1.0 second, the finish rolling completion temperature is 800 to 950°C, and the total rolling reduction in the temperature range of 800 to 950°C is 10% or more and less than 30%. The average cooling rate V from the finish rolling completion temperature to 500°C is set to 0.05 to 1.00°C / sec. Each step will be described below.
[0050] The slab to be subjected to hot rolling may be produced by a general method, for example, by melting steel having the above-mentioned chemical composition. However, in order to favorably control the metal structure at a position 200 μm from the surface, it is preferable to immerse the high-temperature slab after continuous casting in water at 20 to 70 ° C, set the surface temperature T0 of the slab immediately before the start of immersion to 630 to 800 ° C, and set the immersion time t0 to 10 to 30 seconds. The steel material produced by immersion under these conditions and by the manufacturing method described below can favorably control the metal structure not only at a position 0.50R from the surface but also at a position 200 μm from the surface. The slab produced in the continuous casting process is not allowed to cool to room temperature, but is immersed in water at a high temperature of 20 to 70 ° C. At this time, the surface temperature T0 of the slab immediately before the start of immersion is set to 630 to 800 ° C, and the immersion time t0 is set to 10 to 30 seconds. The surface layer of the slab immersed in water is rapidly cooled, and the surface layer temperature drops to 470 ° C or less. On the other hand, the temperature does not drop so much in the inner region of the slab, and is maintained at a temperature higher than the surface layer temperature. Next, the slab after immersion is heated in a heating furnace. During this process, reverse transformation from ferrite to austenite occurs in the surface layer, resulting in finer crystal grains. This suppresses the formation of coarse sulfides in the surface layer. Meanwhile, the internal region of the slab is kept at a high temperature even during immersion, and is heated in the heating furnace. This promotes the growth of sulfides in the internal region of the slab.
[0051] The immersed cast slab or the cast slab produced by a general method without immersion is heated and subjected to hot rolling. The hot rolling start temperature (the entry temperature of the first stand of rough rolling) is preferably 1000°C or higher, since this allows nitrides to be sufficiently dissolved and improves the cold workability of the steel. The upper limit of the hot rolling start temperature may be, for example, 1300°C or lower.
[0052] Passing time between stands: less than 1.0 second, and finishing rolling completion temperature: 800 to 950°C, and total rolling reduction in the temperature range of 800 to 950°C: 10% or more, less than 30% In the finish rolling of the hot rolling, it is preferable that the passing time between each stand in the finish rolling is less than 1.0 second, the finish rolling completion temperature is 800 to 950°C, and the total rolling reduction in the temperature range of 800 to 950°C is 10% or more and less than 30%. The time between the stands is the time from rolling at one stand to rolling at the next stand. By making the time between the stands shorter than 1.0 second, the generation of coarse grains due to strain recovery can be suppressed. As a result, the average distance between the centers of gravity of the pearlite blocks can be favorably controlled.
[0053] By setting the finish rolling completion temperature (the temperature at the exit side of the final stand of the finish rolling) at 800°C or higher, it is possible to prevent the ferrite from becoming finer and the hardness from becoming too high, which would cause deterioration of cold workability. Also, by setting the finish rolling completion temperature at 950°C or lower, it is possible to prevent the average distance between the centers of gravity of the pearlite blocks from becoming longer. As a result, it is possible to reduce the burr height after cutting.
[0054] The average distance between the centers of gravity of pearlite blocks can be preferably controlled by setting the total reduction rate in the temperature range of 800 to 950° C. to 10% or more. In addition, by setting the total reduction rate in the temperature range of 800 to 950° C. to less than 30%, deterioration of cold workability due to excessive hardness can be suppressed. The total rolling reduction in the temperature range of 800 to 950°C can be expressed as {(t0-t1) / t0} x 100(%), where t0 is the entrance thickness before the first rolling in this temperature range, and t1 is the exit thickness after the final rolling stage in this temperature range.
[0055] Average cooling rate V:0.05~1.00℃ / sec After the finish rolling is completed, it is preferable to cool the steel at an average cooling rate V of 0.05 to 1.00°C / sec in the temperature range from the finish rolling completion temperature to 500°C. By setting the average cooling rate V to 0.05°C / sec or more, it is possible to suppress the generation of coarse ferrite, and as a result, it is possible to suppress the average distance between the centers of gravity of pearlite blocks from increasing. In addition, by setting the average cooling rate V to 1.00°C / sec or less, it is possible to suppress the increase in hardness due to the generation of bainite, and it is possible to suppress the deterioration of cold workability.
[0056] By the manufacturing method described above, the steel material according to this embodiment can be stably manufactured. EXAMPLES
[0057] Next, an embodiment of the present invention will be described, but the conditions in the embodiment are merely an example of conditions adopted to confirm the feasibility and effects of the present invention, and the present invention is not limited to this example of conditions. Various conditions can be adopted in the present invention as long as they do not deviate from the gist of the present invention and the object of the present invention is achieved.
[0058] By continuous casting, steel slabs having the chemical compositions shown in Table 1 were obtained. Some of the slabs were immersed in hot water at 20 to 70°C under the conditions shown in Table 2. The other slabs were not immersed. The obtained steel slab was subjected to hot rolling and cooling under the conditions shown in Table 2 to obtain a steel bar (steel material) shown in Table 3. The average cooling rate V shown in Table 2 is the average cooling rate from the finish rolling completion temperature to 500°C.
[0059] For the obtained steel bars, the area ratios of ferrite and pearlite, the average distance between the centers of gravity of pearlite blocks, and Vickers hardness were measured at positions 0.50R from the surface and 200 μm from the surface using the methods described above. The results obtained are shown in Table 3.
[0060] The burr height at the time of cutting the obtained steel bars was evaluated by the following method. Using a general band saw cutting machine, the obtained steel bars were cut at room temperature in a plane perpendicular to the rolling direction to a length of 50 mm. The burr height of the obtained cut material was measured using a microscope. Specifically, the burr was photographed at a magnification of 50 times from the opposite direction to the cut surface. The maximum burr height when 10 pieces were cut for each steel bar was regarded as the burr height. When the burr height was 50 μm or less, the burr height after cutting was deemed low and the product was judged as pass, whereas when the burr height was more than 50 μm, the burr height after cutting was deemed high and the product was judged as fail.
[0061] When the obtained Vickers hardness was 170 Hv or less, it was judged that the cold workability was excellent even in the as-hot-rolled state, and it was judged as passing.On the other hand, when the obtained Vickers hardness was more than 170 Hv, it was judged that the cold workability was poor, and it was judged as failing.
[0062] [Table 1]
[0063] [Table 2]
[0064] [Table 3]
[0065] It can be seen from Tables 1 to 3 that the steel materials according to the examples of the present invention have excellent cold workability, and have low burr height and low hardness after cutting. It can also be seen that the steel materials in which the metal structure is favorably controlled have even lower burr height after cutting at a position 200 μm from the surface. On the other hand, it is clear that the steel material according to the comparative example is deteriorated in any of the characteristics. [Industrial Applicability]
[0066] According to the above-described aspects of the present invention, it is possible to provide a steel material having excellent cold workability even in an as-hot-rolled state, and having low hardness with low burr height after cutting.
Claims
1. The chemical composition, in mass%, is C: 0.10-0.42%, Si: 0.01-0.30%, Mn: 0.20-1.00%, P: less than 0.050%; S: 0.001-0.050%, Al: 0.001-0.200%, N: less than 0.020%; Cr: 0.01 to 1.50%, and O: Contains 0.0030% or less, The balance is Fe and impurities, In the metal structure at a position 0.50R from the surface, The area ratio of ferrite is 50% or more, and the area ratio of pearlite is 20% or more, The average distance between the centers of gravity of the pearlite blocks is 20 to 50 μm; A steel material having a Vickers hardness of 170 HV or less.
2. In the metal structure at a position 200 μm from the surface, The area ratio of ferrite is 50% or more, and the area ratio of pearlite is 20% or more, The average distance between the centers of gravity of the pearlite blocks is 20 to 50 μm; 2. The steel material according to claim 1, characterized in that it has a Vickers hardness of 170 HV or less.
3. The chemical composition, in mass%, is C: 0.10-0.42%, Si: 0.01 to 0.10%, Mn: 0.20-1.00%, P: less than 0.050%; S: 0.001-0.050%, Al: 0.001-0.200%, N: less than 0.020%; Cr: 0.01 to 1.50%, and O: Contains 0.0030% or less, Further, the composition contains one or more selected from the group consisting of the following groups A, B, and C: The balance is Fe and impurities, In the metal structure at a position 0.50R from the surface, The area ratio of ferrite is 50% or more, and the area ratio of pearlite is 20% or more, The average distance between the centers of gravity of the pearlite blocks is 20 to 50 μm; A steel material having a Vickers hardness of 170 HV or less. [Group A] Mo: 0.30% or less, V: 0.150% or less, Nb: 0.050% or less, and Ti: 0.100% or less, One or more selected from the group consisting of [Group B] Cu: 0.40% or less, Ni: 0.30% or less, Sn: 0.100% or less, and B: 0.0200% or less One or more selected from the group consisting of [Group C] Ca: 0.0050% or less, and Mg: 0.0050% or less One or two selected from the group consisting of
4. In the metal structure at a position 200 μm from the surface, The area ratio of ferrite is 50% or more, and the area ratio of pearlite is 20% or more, The average distance between the centers of gravity of the pearlite blocks is 20 to 50 μm; 4. The steel material according to claim 3, characterized in that it has a Vickers hardness of 170 HV or less.
5. The steel material according to claim 3 or 4, having a chemical composition containing, in mass %, the Group A elements.
6. The steel material according to claim 3 or 4, having a chemical composition containing, in mass %, the B group.
7. The steel material according to claim 3 or 4, having a chemical composition containing, in mass %, the C group.
Citation Information
Patent Citations
JP1973088277A
Steel excellent in cold workability and heat treatment distortion, and method for producing the same
JP3333697B2
Linear or bar steel with excellent cold workability and strength stability after heat treatment, its manufacturing method, and machine parts
JP3949899B2