Polyphenylene sulfide hollow fiber membrane and manufacturing method of the same
By employing a solvent with specific boiling point and solubility parameters, the method addresses fiber breakage issues in polyphenylene sulfide hollow fiber membrane production, resulting in membranes with enhanced spinnability and strength for organic solvent applications.
Patent Information
- Application Number
- JP2023060480
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-03
- Publication Date
- 2024-10-16
AI Technical Summary
Existing methods for producing polyphenylene sulfide hollow fiber membranes face frequent fiber breakage due to the use of solvents with boiling points around 200°C, making it difficult to spin into hollow fibers effectively.
The method involves using a solvent with a boiling point higher than the phase separation temperature and a Hansen solubility parameter distance of 4 to 11 MPa to dissolve polyphenylene sulfide resin, forming a continuous porous structure in the hollow fiber membrane, which is achieved through a double-tubular nozzle process with controlled coagulation.
This approach enhances spinnability, preventing fiber breakage and enabling the production of polyphenylene sulfide hollow fiber membranes with improved organic solvent permeation performance and high membrane strength.
Smart Images

Figure 2024147452000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a polyphenylene sulfide hollow fiber membrane. [Background technology]
[0002] Membrane separation technology can be applied to the separation of chemical species having various molecular weights in liquid and gas phases, and is widely used in separation processes in various industrial fields.
[0003] Membrane separation processing technology in particular is widely applied to membrane separation of aqueous liquids, and is put to practical use in a variety of fields, including seawater desalination, removal of fine particles and viruses from river water and domestic wastewater, separation or concentration of heat-sensitive substances such as proteins and enzymes, clarification of fruit juice, production of unpasteurized sake, artificial dialysis, removal of viruses and proteins when producing pharmaceuticals and medical water, production of ultrapure water, recovery of electrodeposition paint, wastewater treatment from silk and pulp factories, treatment of oil-containing wastewater, and treatment of dye wastewater.
[0004] The separation membranes used in these membrane separation processing technologies are mainly polymer membranes, because they are relatively easy to mold, an inexpensive mass production process can be easily established, and they are lightweight, flexible, and easy to handle.
[0005] On the other hand, membrane separation technology has hardly been used for the separation of organic solvent-based liquids because there are no practical separation membranes that are resistant to organic solvents. Although there are many manufacturing processes in the chemical industry that use organic solvents, the separation operation of organic solvents is mainly performed by distillation, which consumes a lot of energy.
[0006] Among organic solvents, there are very few separation membranes that can be stably used for aprotic polar solvents such as acetone, tetrahydrofuran, N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), N-methyl-2-pyrrolidone (NMP), dimethyl sulfoxide (DMSO), and dichloromethane; and basic solvents such as triethylamine, aniline, pyridine, and monoethanolamine.
[0007] In the process of separating organic solvent-based liquids, there is a demand for the separation of particles or solutes of a wide range of sizes in the organic solvent-based liquid. However, it is difficult to produce a polymer membrane that has high separation performance, particularly at the ultrafiltration or nanofiltration level, and is also resistant to organic solvents. Even if such a membrane is obtained, there are problems in that the organic solvents that can be used are limited, or the organic solvent permeation rate is low.
[0008] Polyphenylene sulfide resin (hereinafter, also referred to as "PPS") is an example of a material that has extremely excellent resistance to a wide range of organic solvents including the above-mentioned organic solvents. Although several separation membranes made of PPS have been proposed, a PPS separation membrane that has high separation performance at the ultrafiltration or nanofiltration level in organic solvents and also has practical organic solvent permeability and membrane strength has not yet been developed.
[0009] For example, Patent Document 1 proposes a method for producing a polyphenylene sulfide hollow fiber membrane, in which a solution containing a polyphenylene sulfide resin is extruded from an annular nozzle while a coagulable liquid consisting of a mixture of a good solvent and a non-solvent for polyphenylene sulfide is introduced into the core part of the annular nozzle, and then the solution is coagulated. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] Japanese Patent Application Publication No. 60-248202 Summary of the Invention [Problem to be solved by the invention]
[0011] However, the manufacturing method described in Patent Document 1 uses a solvent that dissolves PPS, which has a boiling point of about 200°C and dissolves PPS under pressure. This causes frequent fiber breakage when the solution containing PPS is extruded through an annular nozzle under normal pressure, making it difficult to spin the solution into a hollow fiber membrane.
[0012] The present invention has been made to solve the above problems, and has an object to provide a method for producing a polyphenylene sulfide hollow fiber membrane having improved spinnability. [Means for solving the problem]
[0013] In order to solve the above problems, the present inventors have investigated the use of a solvent having a boiling point higher than the temperature at which PPS is compatible with PPS at standard atmospheric pressure as a membrane-forming solvent for dissolving PPS, but have found that it is difficult to improve the spinnability of hollow fiber membranes simply by using the solvent.
[0014] The inventors further studied the spinnability of hollow fiber membranes and found that hollow fiber membranes may have a spherulite structure or a continuous porous structure, and that hollow fiber membranes with a spherulite structure are brittle and prone to fiber breakage. FIG. 1 is a scanning electron micrograph (magnification: 5000 times) showing an example of a hollow fiber membrane with a continuous porous structure, and FIG. 2 is a scanning electron micrograph (magnification: 5000 times) showing an example of a hollow fiber membrane with a spherulite structure. In the present invention, the term "continuous porous structure" refers to a structure in which a resin component containing PPS is in the form of a three-dimensional network to form a large number of pores, and the pores are connected and penetrate each other, as shown in FIG. 1. In the present invention, the term "spherulite structure" refers to a structure in which a large number of spheres formed by a resin component containing PPS are aggregated, as shown in FIG. 2.
[0015] The present inventors further investigated membrane-forming solvents that dissolve PPS and found that by using an organic solvent whose boiling point at standard atmospheric pressure is sufficiently higher than the phase separation temperature with PPS and whose Hansen solubility parameter distance between PPS and the organic solvent is within a specific numerical range as a membrane-forming solvent, it is possible to form a hollow fiber membrane having a porous region with a continuous pore structure (hereinafter, simply referred to as "porous region"), thereby improving the spinnability of the hollow fiber membrane. The present invention was completed through further investigation based on this finding.
[0016] That is, the present invention provides the following aspects. Item 1. A first step of preparing a film-forming solution by dissolving a polyphenylene sulfide resin in a film-forming solvent; A second step of forming a hollow fiber membrane having a porous region with a continuous pore structure by discharging the membrane forming solution from an outer annular nozzle using a double-tube nozzle for producing hollow fibers having a double-tube structure and immersing the solution in a coagulation bath; and A third step of removing the solvent from the hollow fiber membrane formed in the second step; The membrane-forming solvent has a Hansen solubility parameter distance (A) between the polyphenylene sulfide resin and the membrane-forming solvent of 4 to 11 MPa. 0.5 and the boiling point at standard pressure is 20° C. or more higher than the phase separation temperature with the polyphenylene sulfide resin. Item 2. The polyphenylene sulfide hollow fiber membrane has a dense layer on the outer surface and the porous region on the inner surface and inside, Item 2. The method for producing a polyphenylene sulfide hollow fiber membrane according to Item 1, wherein the coagulating bath liquid has a Hansen solubility parameter distance (B) between the polyphenylene sulfide resin and the coagulating bath liquid that satisfies the following formula (1): Hansen solubility parameter distance (B)>Hansen solubility parameter distance (A)(1) Item 3. The method for producing a polyphenylene sulfide hollow fiber membrane according to Item 1, wherein in the second step, an internal coagulation liquid is further discharged from an inner nozzle of the double tubular nozzle. Item 4. The polyphenylene sulfide hollow fiber membrane has a porous region throughout the membrane, Item 4. The method for producing a polyphenylene sulfide hollow fiber membrane according to Item 3, wherein the coagulating bath liquid has a Hansen solubility parameter distance (B) between the polyphenylene sulfide resin and the coagulating bath liquid that satisfies the following formula (2), and the internal coagulating liquid has a Hansen solubility parameter distance (C) between the polyphenylene sulfide resin and the internal coagulating liquid that satisfies the following formula (3). Hansen solubility parameter distance (B) ≦ Hansen solubility parameter distance (A) (2) Hansen solubility parameter distance (C) ≦ Hansen solubility parameter distance (A) (3) Item 5. The polyphenylene sulfide hollow fiber membrane has a dense layer on the outer surface and the porous region on the inner surface and inside, Item 4. The method for producing a polyphenylene sulfide hollow fiber membrane according to Item 3, wherein the coagulating bath liquid has a Hansen solubility parameter distance (B) between the polyphenylene sulfide resin and the coagulating bath liquid that satisfies the following formula (1), and the internal coagulating liquid has a Hansen solubility parameter distance (C) between the polyphenylene sulfide resin and the internal coagulating liquid that satisfies the following formula (3). Hansen solubility parameter distance (B)>Hansen solubility parameter distance (A)(1) Hansen solubility parameter distance (C) ≦ Hansen solubility parameter distance (A) (3) Item 6. The polyphenylene sulfide hollow fiber membrane has a dense layer on the outer surface and the inner surface, and has the porous region inside, Item 4. The method for producing a polyphenylene sulfide hollow fiber membrane according to Item 3, wherein the coagulating bath liquid has a Hansen solubility parameter distance (B) between the polyphenylene sulfide resin and the coagulating bath liquid that satisfies the following formula (1), and the internal coagulating liquid has a Hansen solubility parameter distance (C) between the polyphenylene sulfide resin and the internal coagulating liquid that satisfies the following formula (4). Hansen solubility parameter distance (B)>Hansen solubility parameter distance (A)(1) Hansen solubility parameter distance (C)>Hansen solubility parameter distance (A)(4) Effect of the Invention
[0017] According to the method for producing a polyphenylene sulfide hollow fiber membrane of the present invention, a hollow fiber membrane having a porous region with a continuous pore structure can be formed, and as a result, fiber breakage during spinning of the hollow fiber membrane can be effectively suppressed, allowing the polyphenylene sulfide hollow fiber membrane to be produced with good productivity. [Brief description of the drawings]
[0018] [Figure 1] 1 is a scanning electron microscope photograph (magnification: 5000 times) showing an example of a hollow fiber membrane having a continuous porous structure. [Diagram 2] 1 is a scanning electron microscope photograph (magnification: 5000 times) showing an example of a hollow fiber membrane having a spherulite structure. [Diagram 3] FIG. 1 is a schematic diagram of an apparatus showing one embodiment of a method for producing a polyphenylene sulfide hollow fiber membrane of the present invention. [Figure 4] FIG. 1 is a schematic diagram of an apparatus used for measuring the NMP permeation amount and solute rejection rate of the polyphenylene sulfide hollow fiber membrane of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] In the present invention, when the term "ultrafiltration" or "ultrafiltration membrane" is used, it means a filtration membrane having a molecular weight cutoff set within a range of 1,000 to 1,000,000, and when the term "nanofiltration" or "nanofiltration membrane" is used, it means a filtration membrane having a molecular weight cutoff set within a range of 200 to 1,000, or a filtration membrane having a molecular weight cutoff within a range of 200 to 1,000.
[0020] In the present invention, the molecular weight cutoff is a value determined by the following method. A solution of a compound with a known molecular weight is used as the stock solution and filtered, and the liquid that permeates the membrane is collected. The concentration of the compound in the permeated liquid is measured, and the rejection rate is calculated according to the following formula. Rejection rates are calculated using compounds of various molecular weights, and based on these results, a graph is created showing the molecular weight of the compound used on the horizontal axis and the rejection rate of each compound on the vertical axis, and the molecular weight at the intersection of the obtained approximation curve and a rejection rate of 90% is determined as the molecular weight cutoff. Note that a dye compound or polyethylene glycol is used as the compound with a known molecular weight. Rejection rate (%) = [(concentration of compound in original solution - concentration of compound in permeate) / concentration of compound in original solution] x 100
[0021] 1. Manufacturing method of polyphenylene sulfide hollow fiber membrane The method for producing the polyphenylene sulfide hollow fiber membrane of the present invention includes the steps of: A first step of preparing a film-forming solution by dissolving a polyphenylene sulfide resin in a film-forming solvent; A second step of forming a hollow fiber membrane having a porous region with a continuous pore structure by discharging the membrane forming solution from an outer annular nozzle using a double-tube nozzle for producing hollow fibers having a double-tube structure and immersing the solution in a coagulation bath; and A third step of removing the solvent from the hollow fiber membrane formed in the second step; The membrane-forming solvent has a Hansen solubility parameter distance (A) between the polyphenylene sulfide resin and the membrane-forming solvent of 4 to 11 MPa. 0.5 and the boiling point at standard atmospheric pressure is at least 20° C. higher than the phase separation temperature with the polyphenylene sulfide resin.
[0022] Hereinafter, each step of the method for producing the polyphenylene sulfide hollow fiber membrane of the present invention will be described in detail.
[0023] [1st step] In the first step, a film-forming solution is prepared by dissolving a polyphenylene sulfide resin in a film-forming solvent.
[0024] In the present invention, the polyphenylene sulfide resin is a polymer containing 80 mol % or more of a structural unit represented by the following formula (1) (wherein the benzene ring may have one or more substituents selected from the group consisting of an alkyl group, an alkoxy group, a nitro group, a phenyl group, and a halogen group). From the viewpoint of improving the membrane strength of the polyphenylene sulfide hollow fiber membrane, the structural unit in the polyphenylene sulfide resin is preferably 90 mol % or more, more preferably 95 mol % or more, and even more preferably 100 mol %. [ka]
[0025] The polyphenylene sulfide resin may be a straight-chain type having no branched or crosslinked structure, or a branched type having a branched or crosslinked structure. From the viewpoints of ease of preparation of a membrane-forming solution and improvement of the membrane strength of a polyphenylene sulfide hollow fiber membrane, the straight-chain type is preferred.
[0026] When the polyphenylene sulfide resin contains the structural unit represented by the formula (1) and other structural units, the other structural units are not particularly limited, and examples thereof include structural units represented by the following formulas (2) to (6) (wherein the benzene ring may have one or more substituents selected from the group consisting of an alkyl group, an alkoxy group, a nitro group, a phenyl group, and a halogen group). One type of other structural unit may be contained, or two or more types may be contained. From the viewpoint of improving the membrane strength of the polyphenylene sulfide hollow fiber membrane, the other structural units in the polyphenylene sulfide resin are less than 20 mol%, preferably less than 10 mol%, more preferably less than 5 mol%, and even more preferably 0 mol%. [ka]
[0027] From the viewpoint of improving the formability and controllability of phase separation during production of the hollow fiber membrane, and from the viewpoint of imparting excellent shape stability to the hollow fiber membrane, the polyphenylene sulfide resin has a melt flow rate of preferably 200 g / 10 min or less, and more preferably 150 g / 10 min or less, under conditions of a test temperature of 316°C and a load of 5 kg.
[0028] The concentration of the polyphenylene sulfide resin in the membrane forming solution is not particularly limited, but is preferably 20 to 70% by weight, more preferably 25 to 65% by weight, even more preferably 30 to 60% by weight, and even more preferably 30 to 40% by weight. By adjusting the concentration of the polyphenylene sulfide resin in the membrane forming solution within the above range, it becomes easy to form a hollow fiber membrane, and it is possible to produce a polyphenylene sulfide hollow fiber membrane having a porosity and / or a polyphenylene sulfide hollow fiber membrane having a porous region with an average pore size, as described in the following "2. Polyphenylene sulfide hollow fiber membrane", and it is possible to obtain a polyphenylene sulfide hollow fiber membrane having excellent organic solvent permeability and high membrane strength.
[0029] The film-forming solution preferably does not contain any other resins other than polyphenylene sulfide resin, but may contain other resins within the range that does not impair the effects of the present invention. Examples of other resins include polyethylene terephthalate, polybutylene terephthalate, polyamide 6, polyamide 66, polyamide 46, polyamide 610, polyamide 612, polyamide 11, polyamide 12, polyamide MXD6, polyamide 4T, polyamide 6T, polyamide 9T, polyamide 10T, polycarbonate, polyphenylene oxide, polymethylpentene, polyethylene, polypropylene, polytetrafluoroethylene, polyether ether ketone, polysulfone, and polyether sulfone. These resins may be used alone or in combination of two or more. From the viewpoint of suppressing a decrease in the organic solvent permeability and membrane strength of the polyphenylene sulfide hollow fiber membrane, the content of the other resin in the membrane forming solution is preferably 20 parts by weight or less, more preferably 10 parts by weight or less, and even more preferably 5 parts by weight or less, per 100 parts by weight of the polyphenylene sulfide resin.
[0030] The membrane-forming solution may contain a filler as necessary within a range that does not impair the effects of the present invention. By adding a filler to the membrane-forming solution, the membrane strength of the resulting polyphenylene sulfide hollow fiber membrane can be improved. In particular, by containing a filler in the polyphenylene sulfide hollow fiber membrane, the effect of the polyphenylene sulfide hollow fiber membrane being less likely to deform even when high pressure is applied during filtration can be obtained. The type of filler to be added is not particularly limited, and examples thereof include fibrous fillers such as glass fiber, carbon fiber, potassium titanate whisker, zinc oxide whisker, calcium carbonate whisker, wollastonite whisker, aluminum borate whisker, aramid fiber, alumina fiber, silicon carbide fiber, ceramic fiber, asbestos fiber, gypsum fiber, and metal fiber; talc, hydrotalcite, wollastonite, zeolite, sericite, mica, kaolin, clay, pyrophyllite, bentonite, asbestos, and the like. Examples of the filler include silicates such as sulphur oxide and alumina silicate; metal compounds such as silicon oxide, magnesium oxide, alumina, zirconium oxide, titanium oxide, and iron oxide; carbonates such as calcium carbonate, magnesium carbonate, and dolomite; sulfates such as calcium sulfate and barium sulfate; metal hydroxides such as calcium hydroxide, magnesium hydroxide, and aluminum hydroxide; and inorganic materials such as non-fibrous fillers such as glass beads, glass flakes, glass powder, ceramic beads, boron nitride, silicon carbide, carbon black, silica, and graphite. These fillers may be used alone or in combination of two or more. Among these fillers, preferred are talc, hydrotalcite, silica, clay, and titanium oxide, and more preferred are talc and clay. The content of the filler in the film-forming solution is not particularly limited, but is, for example, 5 to 100 parts by weight, and preferably 10 to 50 parts by weight, per 100 parts by weight of the polyphenylene sulfide resin. By adding the filler to the membrane forming solution in such an amount, the membrane strength of the resulting polyphenylene sulfide hollow fiber membrane can be improved, and the pressure resistance can be improved.
[0031] The membrane-forming solvent that dissolves polyphenylene sulfide resin is selected from those having a Hansen solubility parameter distance (A) between the polyphenylene sulfide resin and the membrane-forming solvent of 4 to 11 MPa. 0.5 and has a boiling point at standard pressure that is 20°C or more higher than the phase separation temperature with the polyphenylene sulfide resin. By using a membrane-forming solvent that satisfies the above conditions, the hollow fiber membrane has a porous region with a continuous porous structure due to liquid-liquid phase separation, and the mechanical strength of the hollow fiber membrane is improved, so that the spinnability of the hollow fiber membrane is improved and, as a result, fiber breakage can be suppressed. The hollow fiber membrane may have a porous region in part or throughout. In addition, by using a membrane-forming solvent that satisfies the above conditions, a polyphenylene sulfide hollow fiber membrane having excellent organic solvent permeability and high membrane strength can be obtained. In addition, when the Hansen solubility parameter distance (A) is 4 MPa, 0.5 If a membrane-forming solvent with a Hansen solubility parameter distance (A) of less than 11 MPa is used, the hollow fiber membrane will have a spherulitic structure due to solid-liquid phase separation, and the mechanical strength of the hollow fiber membrane will decrease, resulting in frequent fiber breakage. 0.5 When a membrane-forming solvent exceeding this temperature is used, the phase separation temperature between the polyphenylene sulfide resin and the membrane-forming solvent becomes high, and therefore the types of membrane-forming solvents whose boiling points at standard pressure are 20°C or more higher than the phase separation temperature are very limited. In addition, deterioration of the membrane-forming solution due to high temperatures is likely to progress, which leads to a decrease in the mechanical strength of the hollow fiber membrane and fiber breakage.
[0032] Here, Hansen solubility parameters (hereinafter referred to as "HSP") are parameters used to evaluate the solubility and affinity of substances. HSP consists of three parameters: dispersion term δD, polarity term δP, and hydrogen bond term δH. These three parameters can be considered as coordinates in a three-dimensional space (Hansen space). When the HSPs of two substances are placed in Hansen space, the closer the distance between two HSP points, the easier it is for the substances to dissolve in each other.
[0033] The HSPs of various compounds are described, for example, in Hansen Solubility Parameters: A user's handbook, Second Edition. Boca Raton, Fla: CRC Press. (Hansen, Charles (2007)).
[0034] In the present invention, the HSP distance (A) represented by the following formula is used as a quantitative index of the closeness of the HSP between the polyphenylene sulfide resin and the membrane-forming solvent. HSP distance (A)={4(δD1-δD2) 2 +(δP1-δP2) 2 +(δH1-δH2) 2} 0.5 In the above formula, δD1, δP1, and δH1 are the dispersion term, polar term, and hydrogen bond term of the polyphenylene sulfide resin, and δD2, δP2, and δH2 are the dispersion term, polar term, and hydrogen bond term of the membrane-forming solvent.
[0035] When a mixed solvent is used as a membrane-forming solvent, the HSP of the mixed solvent is an average weighted by the volume ratio (1 atmosphere, 25°C). For example, when the mixed solvent is a mixture of solvent 1 and solvent 2 with a volume ratio of v1 (volume %):v2 (volume %) (total 100 volume %), the HSP of the mixed solvent is expressed by the following formula. δDm=(v1×δDs1+v2×δDs2) / (v1+v2) δPm=(v1×δPs1+v2×δPs2) / (v1+v2) δHm=(v1×δHs1+v2×δHs2) / (v1+v2) In the above formula, δDm, δPm, and δHm are the dispersion term, polar term, and hydrogen bond term of the HSP of the mixed solvent containing two types of solvents, δDs1, δPs1, and δHs1 are the dispersion term, polar term, and hydrogen bond term of the HSP of solvent 1, and δDs2, δPs2, and δHs2 are the dispersion term, polar term, and hydrogen bond term of the HSP of solvent 2. The HSP of a mixed solvent containing three or more solvents is also an average weighted by volume ratio in the same manner as above.
[0036] Table 1 shows δD, δP, and δH of PPS with CAS Registry Number 25212-74-2.
[0037] [Table 1]
[0038] In addition, Tables 2 and 3 show ΔD, ΔP, and ΔH of various solvents.
[0039] [Table 2]
[0040] [Table 3]
[0041] In addition, ΔD, ΔP, and ΔH of various mixed solvents are shown in Table 4. Note that the ratios in Table 4 are volume ratios (1 atmospheric pressure, 25° C.).
[0042] [Table 4]
[0043] When the δD, δP, and δH of the polyphenylene sulfide resin and the solvent used are unknown, values calculated from the physical properties of the compound, values calculated from a solubility test, values calculated by the atomic group contribution method, etc. can be used. The method of obtaining these calculated values is described in the aforementioned Hansen Solubility Parameters: A user's handbook, Second Edition. Boca Raton, Fla: CRC Press. (Hansen, Charles (2007)).
[0044] The membrane-forming solvent is selected based on the HSP of the polyphenylene sulfide resin used, and the HSP distance (A) is set to 4 to 11 MPa. 0.5 Any solvent that satisfies the above condition may be appropriately selected and used.
[0045] The membrane-forming solvent has an HSP distance (A) of preferably 5 to 10 MPa from the viewpoint of further improving the spinnability of the hollow fiber membrane and further suppressing fiber breakage, and from the viewpoint of obtaining a polyphenylene sulfide hollow fiber membrane having superior organic solvent permeability and high membrane strength. 0.5 , more preferably 5 to 9 MPa 0.5 , more preferably 5 to 8 MPa 0.5 As the membrane-forming solvent, it is preferable to use one solvent or a mixed solvent of two or more solvents selected from the group consisting of sulfolane (SFL), diphenyl sulfone (DPS), diphenyl ketone (DPK), benzoin (BZ), dibutyl sebacate (DBS), and di-2-ethylhexyl phthalate (DEHP).
[0046] In addition to the condition of the HSP distance (A), the membrane-forming solvent must have a boiling point at standard pressure that is 20°C or more higher than the phase separation temperature with the polyphenylene sulfide resin. By using a membrane-forming solvent whose boiling point at standard pressure is 20°C or more higher than the phase separation temperature with the polyphenylene sulfide resin, a membrane-forming stock solution in which the polyphenylene sulfide resin is uniformly dissolved at standard pressure can be prepared. This improves the spinnability of the hollow fiber membrane and suppresses fiber breakage.
[0047] In the present invention, the phase separation temperature refers to a temperature at which liquid-liquid phase separation or solid-liquid phase separation by crystal precipitation occurs when a mixture of a polyphenylene sulfide resin and a membrane-forming solvent at a sufficiently high temperature is gradually cooled. The phase separation temperature can be measured using a microscope equipped with a hot stage or the like.
[0048] Tables 2 and 3 show the boiling points of various solvents at standard atmospheric pressure. For solvents whose boiling points at standard atmospheric pressure are unknown, the boiling point at standard atmospheric pressure is calculated from the boiling point at reduced pressure using a boiling point conversion table. When the membrane-forming solvent is a mixed solvent, the boiling point of the component with the lowest boiling point among the solvents contained therein is taken as the boiling point of the mixed solvent. When the boiling point of the membrane-forming solvent to be used at standard atmospheric pressure is actually measured, it can be measured using a boiling point measuring device.
[0049] From the viewpoint of further improving the spinnability of the hollow fiber membrane and further suppressing fiber breakage, and from the viewpoint of obtaining a polyphenylene sulfide hollow fiber membrane having superior organic solvent permeability and high membrane strength, the boiling point of the membrane-forming solvent at standard atmospheric pressure is preferably 20 to 100°C higher, more preferably 20 to 80°C higher, and even more preferably 20 to 50°C higher, than the phase separation temperature with the polyphenylene sulfide resin.
[0050] To the membrane-forming solution, additives such as thickeners, antioxidants, surface modifiers, lubricants, and surfactants may be added as necessary for controlling the pore size and improving the membrane performance.
[0051] [Second process] In the second step, a double-tube nozzle for producing hollow fibers having a double-tube structure is used, and the membrane-forming solution is discharged from the outer annular nozzle and immersed in a coagulation bath liquid to form a hollow fiber membrane having a porous region with a continuous pore structure.
[0052] As the double tubular nozzle for producing hollow fibers, a spinneret having a double annular structure such as that used for producing a core-sheath type composite fiber in melt spinning can be used. The diameter of the outer annular nozzle and the diameter of the inner nozzle of the double tubular nozzle for producing hollow fibers may be appropriately set according to the inner and outer diameters of the polyphenylene sulfide hollow fiber membrane.
[0053] As the coagulation bath liquid, any known coagulation liquid can be used without any particular limitation as long as it can form a hollow fiber membrane having at least a porous region. For example, aqueous solvents such as water and aqueous solutions having a water content of 10% by volume or more; monohydric alcohols such as ethanol, 1-propanol, 2-propanol, isobutanol, etc.; polyhydric alcohols such as ethylene glycol, propylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, glycerin, etc.; polyethylene glycols with a molecular weight of 300 or more; polypropylene glycols with a molecular weight of 400 or more; diethylene glycol diethyl ether, triethylene glycol monomethyl ether, tetraethylene glycol, Examples of the coagulation liquid include glycol ethers such as glycol dimethyl ether and propylene glycol monoethyl ether; glycol acetates such as triacetin and propylene glycol monoethyl ether acetate; amides such as dimethylformamide, dimethylacetamide, N-methyl-2-pyrrolidone and N-cyclohexyl-2-pyrrolidone; phthalates such as dimethyl phthalate and diethyl phthalate; fatty acid esters such as methyl oleate and isopropyl palmitate; dibutyl maleate, dibutyl sebacate, benzyl benzoate, diphenyl ketone, acetone, methyl ethyl ketone, dimethyl sulfoxide, toluene, and xylene. These coagulation liquids may be used alone or in combination of two or more.
[0054] In the second step, an internal coagulation liquid may be discharged from the inner nozzle of the double tubular nozzle in order to facilitate the formation of a porous region on the inner surface of the hollow fiber membrane, or to make the structure of the inner surface of the hollow fiber membrane different from that of the outer surface, etc. As the internal coagulation liquid, any known coagulation liquid may be used without particular limitation, and examples thereof include the coagulation liquids exemplified above.
[0055] In one embodiment of the method for producing a polyphenylene sulfide hollow fiber membrane of the present invention, when the HSP distance (B) between the polyphenylene sulfide resin and the coagulation bath liquid satisfies the following formula (1) and no internal coagulation liquid is discharged, a hollow fiber membrane having a dense layer on the outer surface and a porous region on the inner surface and inside is easily obtained. In the present invention, the HSP distance (B) is a quantitative index of the closeness of the HSP between the polyphenylene sulfide resin and the coagulation bath liquid, and is a value calculated in the same manner as the HSP distance (A). In the present invention, the "dense layer" refers to a region where dense micropores are gathered and where the presence of pores is substantially not observed in a scanning electron microscope (SEM) photograph at a magnification of 10,000 times. HSP distance (B) > HSP distance (A) (1)
[0056] In addition, as one embodiment of the method for producing a polyphenylene sulfide hollow fiber membrane of the present invention, in the coagulation bath liquid, when the HSP distance (B) between the polyphenylene sulfide resin and the coagulation bath liquid satisfies the following formula (2) and the internal coagulation liquid is not discharged, a porous region is likely to be formed throughout the hollow fiber membrane. HSP distance (B)≦HSP distance (A) (2)
[0057] In one embodiment of the method for producing a polyphenylene sulfide hollow fiber membrane of the present invention, when the HSP distance (B) between the polyphenylene sulfide resin and the coagulating bath liquid satisfies the following formula (2), and the HSP distance (C) between the polyphenylene sulfide resin and the internal coagulating liquid satisfies the following formula (3), a porous region is easily formed throughout the hollow fiber membrane. In the present invention, the HSP distance (C) is a quantitative index of the closeness of the HSP between the polyphenylene sulfide resin and the internal coagulating liquid, and is a value calculated in the same manner as the HSP distance (A). HSP distance (B)≦HSP distance (A) (2) HSP distance (C)≦HSP distance (A) (3)
[0058] In one embodiment of the method for producing a polyphenylene sulfide hollow fiber membrane of the present invention, when the coagulating bath liquid has an HSP distance (B) between the polyphenylene sulfide resin and the coagulating bath liquid that satisfies the following formula (1), and the internal coagulating liquid has an HSP distance (C) between the polyphenylene sulfide resin and the internal coagulating liquid that satisfies the following formula (3), a hollow fiber membrane having a dense layer on the outer surface and a porous region on the inner lumen surface and inside is easily obtained. HSP distance (B) > HSP distance (A) (1) HSP distance (C)≦HSP distance (A) (3)
[0059] In one embodiment of the method for producing a polyphenylene sulfide hollow fiber membrane of the present invention, when the coagulating bath liquid has an HSP distance (B) between the polyphenylene sulfide resin and the coagulating bath liquid that satisfies the following formula (2) and the internal coagulating liquid has an HSP distance (C) between the polyphenylene sulfide resin and the internal coagulating liquid that satisfies the following formula (4), a hollow fiber membrane having porous regions on the outer surface and in the interior and having a dense layer on the lumen side surface is easily obtained. HSP distance (B)≦HSP distance (A) (2) HSP distance (C) > HSP distance (A) (4)
[0060] In one embodiment of the method for producing a polyphenylene sulfide hollow fiber membrane of the present invention, when the coagulating bath liquid has an HSP distance (B) between the polyphenylene sulfide resin and the coagulating bath liquid that satisfies the following formula (1), and the internal coagulating liquid has an HSP distance (C) between the polyphenylene sulfide resin and the internal coagulating liquid that satisfies the following formula (4), a hollow fiber membrane having dense layers on the outer surface and the inner lumen surface and a porous region inside is easily obtained. HSP distance (B) > HSP distance (A) (1) HSP distance (C) > HSP distance (A) (4)
[0061] The coagulation bath liquid for forming the porous region has an HSP distance (B) of preferably 2 to 10 MPa from the viewpoint of further improving the spinnability of the hollow fiber membrane and further suppressing fiber breakage, and from the viewpoint of obtaining a polyphenylene sulfide hollow fiber membrane having superior organic solvent permeability and high membrane strength. 0.5 , more preferably 3 to 9 MPa 0.5 , more preferably 3 to 8 MPa 0.5 Examples of the coagulation bath liquid that satisfies the HSP distance (B) include N-methyl-2-pyrrolidone (NMP), an aqueous solution containing more than 90% by weight of NMP, triacetin, bis(2-ethylhexyl) phthalate, dibutyl sebacate, and ethyl oleate.
[0062] The coagulation bath liquid for forming the dense layer has an HSP distance (B) of preferably 10 to 60 MPa from the viewpoint of further improving the spinnability of the hollow fiber membrane and further suppressing fiber breakage, and from the viewpoint of obtaining a polyphenylene sulfide hollow fiber membrane having excellent organic solvent permeability, excellent solute blocking performance, and high membrane strength. 0.5 , more preferably 12 to 50 MPa 0.5 , and more preferably 13 to 45 MPa 0.5 Examples of the coagulation bath liquid that satisfies the HSP distance (B) include water, an aqueous solution containing 90% by weight or less of NMP, ethylene glycol, and propylene glycol.
[0063] The internal coagulation liquid for forming the porous region has an HSP distance (C) of preferably 2 to 10 MPa from the viewpoint of further improving the spinnability of the hollow fiber membrane and further suppressing fiber breakage, and from the viewpoint of obtaining a polyphenylene sulfide hollow fiber membrane having superior organic solvent permeability and high membrane strength. 0.5 , more preferably 3 to 9 MPa 0.5 , more preferably 3 to 7 MPa 0.5 , and even more preferably 3 to 5 MPa 0.5Examples of the internal coagulation liquid that satisfies the HSP distance (C) include benzyl benzoate (BB), a mixed solvent of 20 to 40% by weight of tetraethylene glycol dimethyl ether (TEGDM) and 60 to 80% by weight of diphenyl ketone (DPK), triacetin, bis(2-ethylhexyl) phthalate, dibutyl sebacate, and ethyl oleate.
[0064] The internal coagulation liquid for forming the dense layer has an HSP distance (C) of preferably 10 to 30 MPa from the viewpoint of further improving the spinnability of the hollow fiber membrane and further suppressing fiber breakage, and from the viewpoint of obtaining a polyphenylene sulfide hollow fiber membrane having excellent organic solvent permeability, excellent solute blocking performance, and high membrane strength. 0.5 , more preferably 12 to 25 MPa 0.5 , more preferably 12 to 23 MPa 0.5 Examples of the internal coagulation liquid that satisfies the HSP distance (C) include tetraethylene glycol dimethyl ether (TEGDM), a mixed solvent of 60 to 80% by weight of tetraethylene glycol dimethyl ether (TEGDM) and 20 to 40% by weight of diphenyl ketone (DPK), ethylene glycol, diethylene glycol, triethylene glycol, and sulfolane.
[0065] In forming a hollow fiber membrane, since the temperature of the double tubular nozzle during membrane production reaches 100°C or higher, it is preferable to use a liquid having a boiling point exceeding 100°C as the internal coagulation liquid.
[0066] In the second step, the temperature of the coagulation bath is appropriately adjusted depending on the composition of the membrane-forming raw solution, the composition of the coagulation solution, and the desired membrane pore size.
[0067] The flow rate of the membrane-forming stock solution discharged from the outer annular nozzle of the hollow fiber production double tubular nozzle is not particularly limited, and may be, for example, 2 to 40 g / min, preferably 5 to 30 g / min, and more preferably 8 to 20 g / min. The flow rate of the internal coagulation liquid is appropriately set in consideration of the diameter of the inner nozzle of the hollow fiber production double tubular nozzle, the type of the internal coagulation liquid used, the flow rate of the membrane-forming stock solution, and the like, and may be, for example, 0.1 to 2 times, preferably 0.2 to 1 times, and more preferably 0.2 to 0.7 times, the flow rate of the membrane-forming stock solution.
[0068] [3rd step] In the third step, the solvent (the solvent of the membrane-forming solution and the coagulation liquid) is removed from the hollow fiber membrane formed in the second step. The method of removing the solvent from the hollow fiber membrane is not particularly limited, and for example, a method of immersing the hollow fiber membrane in an extraction solvent that dissolves the solvent of the membrane-forming solution and the coagulation liquid can be mentioned. The extraction solvent needs to be appropriately selected according to the solvent of the membrane-forming solution used and the coagulation liquid, and examples thereof include acetone, methyl ethyl ketone, N-methyl-2-pyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, tetrahydrofuran, 1-chloronaphthalene, chloroform, toluene, and xylene. These may be used alone or in combination of two or more. In order to effectively extract and remove the organic solvent remaining in the polyphenylene sulfide hollow fiber membrane, the extraction solvent may be replaced, stirred, or heated.
[0069] After the third step, the polyphenylene sulfide hollow fiber membrane is preferably dried to remove the extraction solvent, which can be performed by a known drying process such as natural drying, hot air drying, reduced pressure drying, or vacuum drying.
[0070] Prior to the drying step, the polyphenylene sulfide hollow fiber membrane may be treated with a modifier. The modifier is a low-volatility organic liquid. Examples of the modifier include synthetic oil, mineral oil, vegetable oil, higher alcohol, glycerin, glycol, or derivatives thereof. Examples of the solvent for dissolving the modifier include alcohol, ketone, hydrocarbon, or a mixture thereof. The use of the modifier maintains a suitable pore structure during drying and improves flexibility and handling.
[0071] An additional heat treatment may be performed simultaneously with or after drying. The heat treatment can improve the dimensional stability and strength of the polyphenylene sulfide hollow fiber membrane. The heat treatment can also be used to adjust the rejection rate of a solute. The polyphenylene sulfide hollow fiber membrane after drying may be heated, for example, at 100 to 300°C for 1 to 120 minutes.
[0072] An additional stretching treatment may be performed simultaneously with, before, or after drying. The stretching can improve the organic solvent permeability and membrane strength of the polyphenylene sulfide hollow fiber membrane.
[0073] The polyphenylene sulfide hollow fiber membrane of the present invention can be produced through the above-mentioned first to third steps. The apparatus used for the production is not particularly limited, but a general apparatus used for dry-wet spinning as shown in FIG. 3 is preferably used. The production flow of the polyphenylene sulfide hollow fiber membrane is outlined below using the apparatus shown in FIG. 3 as an example. The membrane-forming stock solution prepared in the first step is contained in a container 3. Alternatively, the first step may be performed in the container 3 to prepare the membrane-forming stock solution. The membrane-forming stock solution contained in the container 3 and the internal coagulation liquid introduced from the internal coagulation liquid inlet 5 are each metered by a metering pump 4 and sent to a double tubular nozzle (spinneret) 6 for hollow fiber production. The membrane-forming stock solution discharged from the double tubular nozzle (spinneret) 6 for hollow fiber production is introduced into a coagulation bath liquid 7 through a small air gap and cooled to solidify. Phase separation occurs during the process of cooling and solidifying the membrane forming solution, resulting in a hollow fiber membrane 8 having an island-in-a-sea structure. The hollow fiber membrane 8 thus obtained is wound up by a winding machine 9, and is then wound up by a bobbin winding machine 10 equipped with a bobbin. The wound hollow fiber membrane 8 is subjected to an extraction solvent to remove solvents such as the coagulation liquid, thereby obtaining a polyphenylene sulfide hollow fiber membrane.
[0074] 2. Polyphenylene sulfide hollow fiber membrane The polyphenylene sulfide hollow fiber membrane of the present invention is formed from a polyphenylene sulfide resin, It has a dense layer on its outer surface and a porous region on its inner surface and inside, The permeation rate of N-methyl-2-pyrrolidone at 25°C is 0.04 L / (m 2 ·bar·h) or more, When a solution containing N-methyl-2-pyrrolidone as a solvent and polyethylene glycol 10000 as a solute is filtered, the rejection rate of polyethylene glycol 10000 is 85% or more, and The polyphenylene sulfide hollow fiber membrane of the present invention is characterized by having a tensile strength of 8 MPa or more at 25° C. and a relative humidity of 60%. The polyphenylene sulfide hollow fiber membrane of the present invention will be described in detail below.
[0075] The raw materials for the polyphenylene sulfide hollow fiber membrane of the present invention are as described above in "1. Production method of polyphenylene sulfide hollow fiber membrane", and therefore the description here is omitted.
[0076] The polyphenylene sulfide hollow fiber membrane of the present invention has a dense layer formed on the outer surface. In the present invention, the "dense layer" is a region where dense micropores are gathered, as described in "1. Manufacturing method of polyphenylene sulfide hollow fiber membrane" above, and is a region where the presence of pores is not substantially observed in a scanning electron microscope (SEM) photograph at a magnification of 10,000 times. In the polyphenylene sulfide hollow fiber membrane of the present invention, the thickness of the dense layer is not particularly limited, but is, for example, 0.05 to 2.0 μm, preferably 0.05 to 1.0 μm, and more preferably 0.05 to 0.6 μm. If the thickness of the dense layer is within the above range, defects are unlikely to occur in the dense layer, and excellent organic solvent permeability can be obtained due to small filtration resistance. In the present invention, the thickness of the dense layer is a value obtained by measuring the distance (thickness) of areas where substantially no pores are present in 10 or more locations in an SEM photograph of the cross section of a hollow fiber membrane at a magnification of 10,000 times and calculating the average value.
[0077] In the polyphenylene sulfide hollow fiber membrane of the present invention, the regions other than the dense layer, that is, the lumen side surface and the inside, are porous regions.
[0078] The average pore size of the pores in the porous region is not particularly limited, but from the viewpoint of achieving both practical organic solvent permeability and membrane strength, it is preferably 0.1 to 1.5 μm, more preferably 0.2 to 1.0 μm, and even more preferably 0.3 to 0.6 μm. In detail, if the average pore size is 0.1 μm or more, the flow path of the fluid becomes wider to some extent, and the filtration resistance becomes smaller, so that it is easier to suppress the decrease in organic solvent permeability, and if the average pore size is 1.5 μm or less, it is easier to suppress the decrease in membrane strength. The pores in the porous region can be observed with a scanning electron microscope (SEM), and are recesses in an image of a cross section of a polyphenylene sulfide hollow fiber membrane photographed using an SEM, and are dark areas in the SEM image. In the present invention, the average pore size of the pores in the porous region is a value calculated by the following formula from the average area obtained by measuring the area of any 100 dark areas (recesses) in an SEM image using image analysis software. Average pore diameter (μm) = 2 × (average area (μm 2 ) / pi) 0.5
[0079] The porosity of the polyphenylene sulfide hollow fiber membrane of the present invention is not particularly limited, but is preferably 40 to 70%, more preferably 45 to 65%, and even more preferably 50 to 65%. The porosity represents the degree of the pore volume of the hollow fiber membrane. If the porosity is too high, it is difficult to obtain sufficient membrane strength against the pressure applied in the filtration operation, and the membrane is likely to collapse in the case of external pressure filtration and to break in the case of internal pressure filtration. On the other hand, if the porosity is too low, the number of flow paths through which the fluid can pass through the hollow fiber membrane is likely to decrease, and the organic solvent permeation rate is likely to decrease. If the porosity is within the above range, it is easier to obtain a sufficient organic solvent permeation rate while having a membrane strength that can withstand high pressure. In the present invention, the porosity is the average value of the values calculated by the following formula for five samples of the hollow fiber membrane. Porosity (%) = {1-(weight of hollow fiber membrane (g) / apparent volume of hollow fiber membrane (cm 3 ) × density of polyphenylene sulfide resin (g / cm 3 ))}×100 Apparent membrane volume (cm 3): {(Outer diameter of hollow fiber membrane (cm) / 2) 2 - (inner diameter of hollow fiber membrane (cm) / 2) 2} × Pi × length of hollow fiber membrane (cm)
[0080] The polyphenylene sulfide hollow fiber membrane of the present invention has a permeation rate of N-methyl-2-pyrrolidone (NMP) of 0.04 L / (m 2 ·bar·h) or more.
[0081] In one embodiment of the polyphenylene sulfide hollow fiber membrane of the present invention, when it is an ultrafiltration membrane, the NMP permeation rate at 25° C. is preferably 0.2 L / (m 2 ·bar·h), preferably 0.5L / (m 2 ·bar·h) or more, more preferably 2.0L / (m 2 ·bar·h) or more. In the case of an ultrafiltration membrane, the upper limit of the NMP permeability is usually 100 L / (m 2 ·bar·h).
[0082] In one embodiment of the polyphenylene sulfide hollow fiber membrane of the present invention, when it is a nanofiltration membrane, the NMP permeation amount at 25° C. is preferably 0.06 L / (m 2 ·bar·h), preferably 0.08L / (m 2 ·bar·h) or more, more preferably 0.10L / (m 2 ·bar·h) or more. In the case of nanofiltration membranes, the upper limit of the NMP permeability is usually 5L / (m 2 ·bar·h).
[0083] The NMP permeation amount of the polyphenylene sulfide hollow fiber membrane of the present invention is a value measured by external pressure filtration, and is a value measured by the following procedure. First, 10 hollow fiber membranes are cut to a length of 30 cm, and prepared by arranging and bundling them. Next, a polybutylene terephthalate (PBT) tube with an outer diameter of 12.7 mm, an inner diameter of 9.5 mm, a length of 200 mm, and two holes for liquid passage on the side is prepared, and a silicone tube with an inner diameter of 12 mm and a length of about 50 mm is inserted about 15 mm into one end opening of the tube to connect it, and a rubber plug with a length of about 20 mm is inserted on the side opposite to the side inserted into the PBT tube of the silicone tube to plug the one end opening. Next, a two-liquid mixed epoxy resin is injected from the opening on the opposite side of the connecting tube from the side where the rubber plug is inserted, and the space inside the tube is filled with the epoxy resin. Thereafter, one end of the bundle of hollow fiber membranes prepared above is heat sealed to prevent the epoxy resin from penetrating into the hollow portion, and the end is inserted into the tube filled with the epoxy resin until the tip of the end touches the rubber stopper, and the epoxy resin is cured in this state. Next, the region of the cured epoxy resin on the rubber stopper side is cut together with the tube to open the hollow portion. The other end is similarly sealed with epoxy resin to produce a crossflow module with an open hollow portion at one end of the hollow fiber membrane. The prepared cross-flow module 13 is connected to an external pressure separation treatment line shown in FIG. 4, and the flowing liquid is continuously passed through the cross-flow module 13 by the liquid supply circulation pump 11. NMP is used as the flowing liquid. In the module, the pressures of the primary pressure gauge 16 and the secondary pressure gauge 17 are adjusted by the regulator 12 so that the arithmetic mean value of the pressures of the primary pressure gauge 16 and the secondary pressure gauge 17 is 10 bar. Of the flowing liquid passing through the module, that which has passed through the pores of the hollow fiber membrane is recovered as a permeated liquid separated from the flowing liquid, and the remainder is circulated again to the separation treatment line. The NMP that has flowed out of the cross-flow module 13 between 3 and 4 hours after the start of circulation is recovered in the receiver 15, and the NMP permeation amount (L / (m 2 Calculate the value of 1.5 bar h). NMP permeation amount = volume of NMP permeated to the inner side of the hollow fiber membrane (L) / [outer diameter of hollow fiber membrane (m) x 3.14 x effective filtration length of hollow fiber membrane (m) x 10 (pieces) x pressure Force (bar) x time (h)] Effective filtration length of hollow fiber membrane: The length of the outer surface of the hollow fiber membrane in the module that is not covered with epoxy resin.
[0084] In one embodiment of the polyphenylene sulfide hollow fiber membrane of the present invention, when it is an ultrafiltration membrane, the permeation amount of NMP at 25° C. is preferably 0.5 L / (m 2 ·bar·h) or more, preferably 3.0L / (m 2 ·bar·h) or more, more preferably 6.0 L / (m 2 ·bar·h), and even more preferably 9.0 L / (m 2 In the case of an ultrafiltration membrane, when the measurement is performed by applying a pressure so that the arithmetic mean value of the pressure of the primary pressure gauge 16 and the pressure of the secondary pressure gauge 17 is 1 bar, the upper limit of the permeation amount of NMP at 25°C depends on the pore size, but is usually 100 L / (m 2 ·bar·h).
[0085] The polyphenylene sulfide hollow fiber membrane of the present invention has a rejection rate of polyethylene glycol 10000 of 85% or more when a solution containing polyethylene glycol 10000 as a solute and NMP as a solvent is filtered. That's all.
[0086] In one embodiment of the polyphenylene sulfide hollow fiber membrane of the present invention, when it is an ultrafiltration membrane, the rejection rate of the polyethylene glycol 10,000 is more preferably 90% or more, even more preferably 92% or more, still more preferably 95% or more, and particularly preferably 99% or more.
[0087] In one embodiment of the polyphenylene sulfide hollow fiber membrane of the present invention, when it is a nanofiltration membrane, the rejection rate of the polyethylene glycol 10000 is more preferably more than 99%.
[0088] In one embodiment of the polyphenylene sulfide hollow fiber membrane of the present invention, the rejection rate of polyethylene glycol 4000 when a solution containing NMP as a solvent and polyethylene glycol 4000 as a solute is filtered is preferably 80% or more.
[0089] In one embodiment of the polyphenylene sulfide hollow fiber membrane of the present invention, when it is an ultrafiltration membrane, the rejection rate of the polyethylene glycol 4000 is more preferably 84% or more, and further preferably 90% or more.
[0090] In one embodiment of the polyphenylene sulfide hollow fiber membrane of the present invention, when it is a nanofiltration membrane, the rejection rate of the polyethylene glycol 4000 is more preferably more than 99%.
[0091] In one embodiment of the polyphenylene sulfide hollow fiber membrane of the present invention, when it is a nanofiltration membrane, the rejection rate of Brilliant Blue R when a solution in which the solvent is NMP and the solute is Brilliant Blue R is filtered is preferably 90% or more, more preferably 93% or more, even more preferably 96% or more, and still more preferably 98% or more.
[0092] In one embodiment of the polyphenylene sulfide hollow fiber membrane of the present invention, when it is a nanofiltration membrane, the rejection rate of Acid Red 52 when a solution containing NMP as a solvent and Acid Red 52 as a solute is filtered is preferably 85% or more, more preferably 87% or more, even more preferably 88% or more, and still more preferably 90% or more.
[0093] In the polyphenylene sulfide hollow fiber membrane of the present invention, the rejection rates of polyethylene glycol 10000, polyethylene glycol 4000, Brilliant Blue R, and Acid Red 52 are values measured by external pressure filtration, and are values measured by the same procedure as in the measurement of the NMP permeation amount. Specifically, the prepared cross-flow module 13 is connected to an external pressure separation processing line shown in FIG. 4, and the flowing liquid is continuously passed through the cross-flow module 13 by the liquid supply circulation pump 11. As the flowing liquid, an NMP solution of polyethylene glycol 10000 (100 ppm), an NMP solution of polyethylene glycol 4000 (100 ppm), an NMP solution of brilliant blue R (100 ppm), or an NMP solution of acid red 52 (100 ppm) is used. In the module, the pressure of the primary pressure gauge 16 and the pressure of the secondary pressure gauge 17 are adjusted by the regulator 12 so that the arithmetic mean value of the pressure of the primary pressure gauge 16 and the pressure of the secondary pressure gauge 17 is 1 bar in the case of the NMP solution of polyethylene glycol 10000 and the NMP solution of polyethylene glycol 4000, and 10 bar in the case of the NMP solution of brilliant blue R and the NMP solution of acid red 52. Of the flowing liquid passing through the module, that which has passed through the pores of the hollow fiber membrane is collected as a permeated liquid separated from the flowing liquid, and the remainder is circulated again to the separation treatment line. The permeated liquid flowing out of the cross flow module 13 between 3 and 4 hours after the start of circulation is collected in a receiver 15, and the solute concentrations of the resulting permeated liquid and flowing liquid are measured using an absorbance meter in the case of Brilliant Blue R and Acid Red 52, and using high performance liquid chromatography in the case of polyethylene glycol 10000 and polyethylene glycol 4000, and the rejection rate is calculated from the following formula. Rejection rate = 100 - (solute concentration of permeate / solute concentration of flow-through liquid) x 100
[0094] The polyphenylene sulfide hollow fiber membrane of the present invention has a tensile strength of 8 MPa or more at 25°C and a relative humidity of 60%, and is excellent in membrane strength. The tensile strength at 25°C and a relative humidity of 60% is preferably 10 MPa or more, more preferably 12 MPa or more, even more preferably 13 MPa or more, and even more preferably 14 MPa or more. In the present invention, the tensile strength of the polyphenylene sulfide hollow fiber membrane is a value measured using a tensile tester under conditions of an atmosphere of 25°C and a relative humidity of 60%, a gauge length of 50 mm, and a pulling speed of 50 mm / min. The tensile strength is an average value of five measurements.
[0095] The polyphenylene sulfide hollow fiber membrane of the present invention is formed of polyphenylene sulfide resin and has the above-mentioned membrane structure, and therefore has the property of suppressing changes in membrane strength and stably maintaining the membrane structure (organic solvent resistance) even when it comes into contact with various types of organic solvents used industrially. Therefore, the polyphenylene sulfide hollow fiber membrane of the present invention can be suitably used for ultrafiltration or nanofiltration of organic solvent-based liquids. Specifically, the polyphenylene sulfide hollow fiber membrane of the present invention has resistance to organic solvents such as aprotic polar solvents, basic solvents, alcohols, hydrocarbons, higher fatty acids, ketones, esters, and ethers.
[0096] The polyphenylene sulfide hollow fiber membrane of the present invention has excellent resistance, particularly to aprotic polar solvents, and is therefore preferably used for ultrafiltration or nanofiltration of aprotic polar solvent-based liquids.
[0097] Examples of aprotic polar solvents include ketones such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; ethers such as diethyl ether, tetrahydrofuran, 1,4-dioxane, and anisole; esters such as methyl acetate, ethyl acetate, butyl acetate, ethylene carbonate, and propylene carbonate; N-substituted amides such as DMF, DMAc, and NMP; organic sulfur compounds such as dimethyl sulfoxide and sulfolane; nitriles such as acetonitrile and acrylonitrile; alkyl halides such as dichloromethane and trichloromethane; and mixed solvents thereof.
[0098] Furthermore, since the polyphenylene sulfide hollow fiber membrane of the present invention has excellent resistance, particularly to basic solvents and basic components, it is preferably used for ultrafiltration or nanofiltration of basic solvent-based liquids and liquids containing basic components.
[0099] Examples of the basic solvent include aliphatic amines such as ethylamine, diethylamine, triethylamine, ethylenediamine, diethylenetriamine, triethylenetetramine, etc., aromatic amines such as aniline, toluidine, etc., heterocyclic amines such as pyrrolidine, piperidine, pyridine, quinoline, morpholine, etc., alkanolamines such as monoethanolamine, diethanolamine, triethanolamine, etc., and mixed solvents thereof. Examples of the basic component include metal alkoxides such as sodium methoxide, sodium ethoxide, etc.
[0100] Specifically, the organic solvent resistance of the polyphenylene sulfide hollow fiber membrane of the present invention is such that when immersed in an organic solvent such as an aprotic polar solvent (e.g., acetone, NMP, DMF, DMSO, etc.) or a basic solvent (e.g., ethylenediamine, pyridine, monoethanolamine, etc.) at 25° C. for 30 days, the strength retention of the polyphenylene sulfide hollow fiber membrane after immersion is preferably 90% or more, more preferably 93% or more, even more preferably 95% or more, and even more preferably 97% or more. In the present invention, the strength retention is a value calculated by the following formula. Strength retention rate (%) = (tensile strength of hollow fiber membrane after immersion / tensile strength of hollow fiber membrane before immersion) x 100
[0101] The outer diameter of the polyphenylene sulfide hollow fiber membrane of the present invention is appropriately set depending on the application, liquid permeability, etc., but in consideration of the relationship between the effective membrane area when packed in a module, the membrane strength, the pressure loss of the fluid flowing through the hollow part, and the buckling pressure, the outer diameter of the hollow fiber membrane is usually 100 to 4000 μm, preferably 200 to 3000 μm, and more preferably 300 to 1000 μm. The inner diameter of the polyphenylene sulfide hollow fiber membrane of the present invention is not particularly limited, but may be, for example, 50 to 3000 μm, preferably 100 to 2500 μm, more preferably 100 to 2000 μm, and even more preferably 100 to 1000 μm. In the present invention, the outer diameter and inner diameter of the hollow fiber membrane are values obtained by observing 10 hollow fiber membranes with an optical microscope at a magnification of 200 times, measuring the outer diameter and inner diameter of each hollow fiber membrane (both at the point where the diameter is maximum), and calculating the average value of each.
[0102] The thickness of the polyphenylene sulfide hollow fiber membrane of the present invention is appropriately set depending on the use and shape of the hollow fiber membrane, the liquid permeability to be provided, etc., and is, for example, 50 to 600 μm, preferably 100 to 350 μm. In the present invention, the thickness of the hollow fiber membrane is a value calculated by subtracting the inner diameter from the outer diameter and dividing the value by 2.
[0103] The polyphenylene sulfide hollow fiber membrane of the present invention is preferably used by being incorporated into a hollow fiber membrane module described below.
[0104] The polyphenylene sulfide hollow fiber membrane of the present invention is not particularly limited by its production method, so long as it can be produced having the above-mentioned membrane structure and properties. For example, it can be produced by the method described in the above "1. Production method of polyphenylene sulfide hollow fiber membrane".
[0105] 3. Hollow fiber membrane module The polyphenylene sulfide hollow fiber membrane of the present invention is housed in a module case equipped with an inlet for a liquid to be treated, an outlet for a permeated liquid, etc., and used as a hollow fiber membrane module.
[0106] Specifically, the hollow fiber membrane module may have a structure in which the polyphenylene sulfide hollow fiber membranes of the present invention are bundled and housed in a module case, and one or both ends of the hollow fiber membranes are sealed and fixed with a potting agent. The hollow fiber membrane module may have an opening connected to a flow path passing through the outer wall surface side of the hollow fiber membranes and an opening connected to the hollow part of the hollow fiber membrane, as an inlet for the liquid to be treated or an outlet for the filtrate.
[0107] The shape of the hollow fiber membrane module is not particularly limited, and may be a dead-end type module or a cross-flow type module.Specific examples of the module include a dead-end type module in which a hollow fiber membrane bundle is folded into a U-shape and packed, and the ends of the hollow fiber membrane bundle are sealed and then cut to open; a dead-end type module in which a hollow fiber membrane bundle is packed straight, with the hollow opening at one end closed by heat sealing or the like, and the end of the hollow fiber membrane bundle that is open is sealed and then cut to open; a dead-end type module in which a hollow fiber membrane bundle is packed straight, both ends of the hollow fiber membrane bundle are sealed, and only one end is cut to expose the opening; and a cross-flow type module in which a hollow fiber membrane bundle is packed straight, both ends of the hollow fiber membrane bundle are sealed, and the sealed parts at both ends of the hollow fiber membrane bundle are cut to create two flow paths on the side of the filter case.
[0108] The packing rate of the hollow fiber membranes inserted into the module case is not particularly limited, but may be, for example, 15 to 75 volume %, preferably 25 to 65 volume %, and more preferably 35 to 55 volume % of the volume of the hollow fiber membranes, including the volume of the hollow portion relative to the volume inside the module case. By satisfying such a packing rate, it is possible to ensure a sufficient filtration area, while facilitating the packing operation of the hollow fiber membranes into the module case and allowing the potting agent to easily flow between the hollow fiber membranes.
[0109] The potting agent used in the manufacture of the hollow fiber membrane module is not particularly limited, but when the hollow fiber membrane module is used for treating an organic solvent, it is desirable that the potting agent has organic solvent resistance, and examples of such potting agents include polyamide, silicone resin, polyurethane resin, epoxy resin, melamine resin, polyethylene, polypropylene, phenolic resin, polyimide, polyurea resin, etc. Among these potting agents, those that shrink or swell little when cured and are not too hard are preferred, and suitable examples include polyamide, silicone resin, epoxy resin, and polyethylene. These potting agents may be used alone or in combination of two or more.
[0110] The material of the module case used in the hollow fiber membrane module is not particularly limited, but when the hollow fiber membrane module is used to treat an organic solvent, it is desirable that the module case has resistance to the organic solvent, and examples of the material of such a module case include polyamide, polyester, polyethylene, polypropylene, polyvinylidene fluoride, polytetrafluoroethylene, polyvinyl chloride, polysulfone, polyethersulfone, polycarbonate, polyarylate, polyphenylene sulfide, etc. Among these, preferred are polyamide, polyethylene, polypropylene, polytetrafluoroethylene, polycarbonate, polysulfone, polyethersulfone, and more preferred are polyamide, polyethylene, polypropylene, and polytetrafluoroethylene. EXAMPLES
[0111] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0112] 1. Measurement and evaluation methods [Phase separation temperature between polyphenylene sulfide resin and membrane-forming solvent] The polyphenylene sulfide resin and each membrane-forming solvent were mixed to a total amount of 20 g to prepare a membrane-forming stock solution composition shown in Tables 5 to 8, and heated to dissolve the polyphenylene sulfide resin to prepare a homogeneous solution. The prepared homogeneous solution was cooled at a rate of 10°C / min, and the temperature at which liquid-liquid phase separation or solid-liquid phase separation due to crystal precipitation occurred was measured using a microscope equipped with a hot stage, and the temperature obtained by the measurement was taken as the phase separation temperature.
[0113] [Structure of hollow fiber membrane] The internal structure of the hollow fiber membrane was observed by cutting the hollow fiber membrane perpendicular to the longitudinal direction with a scanning electron microscope at a magnification of 10,000 times. The structures of the outer surface and the lumen side surface of the hollow fiber membrane were observed by cutting the hollow fiber membrane horizontally to the longitudinal direction with a scanning electron microscope at a magnification of 10,000 times. The presence or absence of a dense layer, a porous region with a continuous pore structure, and a spherulite structure was confirmed.
[0114] [Spinnability] The spinnability of the hollow fiber membrane was evaluated according to the following criteria. A: When the polyphenylene sulfide resin dissolves in the membrane-forming solvent and the hollow fiber membrane can be wound up without fiber breakage. B: When the polyphenylene sulfide resin does not dissolve in the membrane-forming solvent, or when the hollow fiber membrane cannot be wound up due to frequent fiber breakage.
[0115] [Outer diameter, inner diameter, and thickness of hollow fiber membrane] Ten hollow fiber membranes were observed under an optical microscope at a magnification of 200 times, and the outer and inner diameters of each hollow fiber membrane (both at the maximum diameter points) were measured and averaged to obtain the thickness of the hollow fiber membrane. The thickness of the hollow fiber membrane was calculated by subtracting the inner diameter from the outer diameter and dividing the result by 2.
[0116] [Porosity of hollow fiber membrane] The hollow fiber membrane was cut to a length of 100 mm, and the porosity of the hollow fiber membrane was calculated by the following formula: The porosity is the average value of five hollow fiber membrane samples. Porosity (%) = {1-(weight of hollow fiber membrane (g) / apparent volume of hollow fiber membrane (cm3 ) × density of polyphenylene sulfide resin (g / cm 3 ))}×100 Apparent membrane volume (cm 3 ): {(Outer diameter of hollow fiber membrane (cm) / 2) 2 - (inner diameter of hollow fiber membrane (cm) / 2) 2} × Pi × length of hollow fiber membrane (cm)
[0117] [Thickness of the dense layer of the hollow fiber membrane] After freezing the hollow fiber membrane using liquid nitrogen, the membrane surface was cut in a vertical direction, and the membrane cross section was observed with a scanning electron microscope (SEM) (SU8020, manufactured by Hitachi High-Technologies Corporation). In the SEM observation, the membrane cross section was observed at a magnification of 10,000 times with the outer surface side end of the hollow fiber membrane as the center of the microscope field of view. There were areas in the SEM photograph where the presence of pores was substantially not observed, confirming the presence of a dense layer. Then, the thickness of 10 random points of the dense layer was measured, and the average value of these values was taken as the thickness of the dense layer.
[0118] [Average pore size of the porous region of the hollow fiber membrane] In the SEM observation, the cross-section of the membrane was photographed at a magnification of 5000 times with the center of the membrane thickness as the center of the microscope field of view. The photographed image was binarized using the image analysis software ImageJ, and then processed in the Analyze Particles command with size set to 0.01-Infinity and circularity set to 0.00-1.00 to extract the contours of 100 arbitrary pores and calculate the area value of each pore. The average pore size was calculated from the average area of the obtained pores using the following formula. Average pore diameter (μm) = 2 × (average area (μm 2 ) / pi) 0.5
[0119] [Tensile strength of hollow fiber membrane] A sample with a length of 100 mm was cut out from the hollow fiber membrane, and a tensile test was performed in the longitudinal direction of the hollow fiber membrane using a tensile tester (Shimadzu Corporation, Autograph AG-H) under conditions of 25°C, relative humidity 60%, gauge length 50 mm, and tensile speed 50 mm / min. The tensile test was repeated five times, and the tensile strength was calculated as the average value of the five tests.
[0120] [Strength retention rate] A sample of 100 mm in length was cut out from the hollow fiber membrane and left to stand at 25°C for 30 days while immersed in a test solvent in a sealed container. Acetone, NMP, DMF, DMSO, ethylenediamine, pyridine, and monoethanolamine were used as the test solvent. The sample was then taken out, the test solvent was washed away with pure water, and the sample was naturally dried. The tensile strength of the dried sample was measured using the tensile strength measurement procedure described above, and the strength retention rate was calculated using the following formula. The strength retention rate is the average value of five samples. Strength retention rate (%) = (tensile strength of hollow fiber membrane after immersion / tensile strength of hollow fiber membrane before immersion) x 100
[0121] [NMP permeation amount] Ten hollow fiber membranes were cut to a length of 30 cm, and bundled together to prepare a tube. Next, a polybutylene terephthalate (PBT) tube with an outer diameter of 12.7 mm, an inner diameter of 9.5 mm, a length of 200 mm, and two holes for liquid passage on the side was prepared, and a silicone tube with an inner diameter of 12 mm and a length of about 50 mm was inserted about 15 mm into one end opening of the tube to connect it, and a rubber stopper with a length of about 20 mm was inserted on the side opposite to the side where the silicone tube was inserted into the PBT tube to plug the one end opening. Next, a two-liquid mixed epoxy resin was injected from the opening on the opposite side of the rubber stopper of the connecting tube to fill the inner space of the tube with the epoxy resin. Then, one end of the bundle of hollow fiber membranes prepared as above was heat sealed to prevent the epoxy resin from penetrating into the hollow part, and the end tip was inserted into the tube filled with the epoxy resin until it touched the rubber stopper, and the epoxy resin was cured in this state. Next, the region of the cured epoxy resin on the rubber plug side was cut together with the tube to open the hollow part. The other end was similarly sealed with epoxy resin to produce a cross-flow module with an open hollow part at one end of the hollow fiber membrane. The prepared cross-flow module 13 was connected to an external pressure separation treatment line shown in FIG. 4, and the flowing liquid was continuously passed through the cross-flow module 13 by the liquid supply circulation pump 11. NMP was used as the flowing liquid. In the module, the pressure of the primary pressure gauge 16 and the pressure of the secondary pressure gauge 17 were adjusted by the regulator 12 so that the arithmetic mean value of the pressure of the primary pressure gauge 16 and the pressure of the secondary pressure gauge 17 was 1 bar or 10 bar. Of the flowing liquid passing through the module, that which passed through the pores of the hollow fiber membrane was collected as a permeated liquid separated from the flowing liquid, and the remainder was circulated again to the separation treatment line. The NMP that flowed out of the cross-flow module 13 between 3 hours and 4 hours after the start of circulation was collected in the receiver 15, and the NMP permeation amount (L / (m 2 ·bar·h) was calculated. NMP permeation amount = volume of NMP permeated to the inner side of the hollow fiber membrane (L) / [outer diameter of hollow fiber membrane (m) x 3.14 x effective filtration length of hollow fiber membrane (m) x 10 (pieces) x pressure Force (bar) x time (h)] Effective filtration length of hollow fiber membrane: This is the length of the part of the outer surface of the hollow fiber membrane in the module that is not covered with epoxy resin.
[0122] [Solute rejection rate] The solute rejection rate was measured in the same manner as the NMP permeation rate. Specifically, the prepared cross-flow module 13 was connected to an external pressure separation processing line shown in FIG. 4, and the flowing liquid was continuously passed through the cross-flow module 13 by the liquid sending circulation pump 11. As the flowing liquid, an NMP solution of polyethylene glycol 20000 (100 ppm), an NMP solution of polyethylene glycol 10000 (100 ppm), an NMP solution of polyethylene glycol 4000 (100 ppm), an NMP solution of brilliant blue R (100 ppm), an NMP solution of acid red 52 (100 ppm), or an NMP solution of methyl orange (100 ppm) was used. In the module, the pressure of the primary pressure gauge 16 and the pressure of the secondary pressure gauge 17 were adjusted by the regulator 12, so that the arithmetic average value of the pressure of the primary pressure gauge 16 and the pressure of the secondary pressure gauge 17 was 1 bar in the case of the NMP solution of polyethylene glycol 20000 (100 ppm), the NMP solution of polyethylene glycol 10000, and the NMP solution of polyethylene glycol 4000, and was 10 bar in the case of the NMP solution of brilliant blue R, the NMP solution of acid red 52, and the NMP solution of methyl orange. Of the flowing liquid permeating through the module, the one that permeated the pores of the hollow fiber membrane was recovered as a permeated liquid separated from the flowing liquid, and the remainder was circulated again to the separation treatment line. The permeate flowing out of the cross-flow module 13 within 3 to 4 hours after the start of circulation was collected in a receiver 15, and the solute concentrations of the permeate and flowing liquid obtained were measured using an absorbance spectrometer in the case of Brilliant Blue R, Acid Red 52, and Methyl Orange, and using high performance liquid chromatography in the case of polyethylene glycol 20000, polyethylene glycol 10000, and polyethylene glycol 4000, and the rejection rate was calculated from the following formula. Rejection rate = 100 - (solute concentration of permeate / solute concentration of flow-through liquid) x 100
[0123] 2. Test Example [Example 1] Polyphenylene sulfide resin (PPS) chip (Solvay, Ryton QC210N, density: 1.34 g / cm 3 300 g of polyphenylene sulfide (PPS) (CAS registration number: 25212-74-2) and 700 g of a mixture of sulfolane (SFL):diphenyl sulfone (DPS) = 20:80 (volume ratio) were mixed under a nitrogen atmosphere and stirred at 250 ° C for 1 hour to dissolve, then the stirring speed was reduced and degassed for 1 hour to prepare a membrane-forming stock solution (PPS concentration: 30 wt%). The membrane-forming stock solution was sent to a double-ring nozzle kept at 250 ° C via a metering pump, and benzyl benzoate (BB) was poured as an internal coagulation liquid. The extruded membrane-forming stock solution was poured into a coagulation bath solution of N-methyl-2-pyrrolidone (NMP) at 25 ° C, and cooled and solidified to form a hollow fiber membrane. The wound hollow fiber membrane was immersed in acetone for 24 hours to extract the solvent, and then naturally dried to obtain a polyphenylene sulfide hollow fiber membrane. The measurements and evaluation results of the obtained polyphenylene sulfide hollow fiber membrane are shown in Table 5.
[0124] [Examples 2 to 25, Comparative Examples 2 to 8] Polyphenylene sulfide hollow fiber membranes were produced in the same manner as in Example 1, except that the production conditions were changed as shown in Tables 5 to 8. The measurement and evaluation results of the obtained polyphenylene sulfide hollow fiber membranes are shown in Tables 5 to 8. In addition, the measurement results of the polyphenylene sulfide hollow fiber membranes produced in Examples 3, 7, 14 to 17, and 25 are shown in Table 9.
[0125] [Comparative Example 1] Polyphenylene sulfide resin (PPS) chip (Solvay, Ryton QC200P, density: 1.34 g / cm 3 300 g of polyphenylene sulfide (CAS registration number: 25212-74-2) and 700 g of sulfolane (SFL) were mixed under a nitrogen atmosphere and stirred at 250° C. for 1 hour. However, the polyphenylene sulfide resin did not dissolve in the sulfolane, so the test was discontinued.
[0126] [Table 5]
[0127] [Table 6]
[0128] [Table 7]
[0129] [Table 8]
[0130] In Examples 1 to 25, the HSP distance (A) between the polyphenylene sulfide resin and the membrane-forming solvent is 4 to 11 MPa. 0.5 Since the membrane-forming solvent used had a boiling point at standard pressure that was 20°C or more higher than the phase separation temperature with the polyphenylene sulfide resin, the hollow fiber membrane had a porous region with a continuous pore structure, and thus no fiber breakage occurred during spinning of the hollow fiber membrane. On the other hand, in Comparative Example 1, the HSP distance (A) between the polyphenylene sulfide resin and the membrane-forming solvent was 11 MPa. 0.5 In Comparative Examples 2 to 8, the HSP distance (A) between the polyphenylene sulfide resin and the membrane-forming solvent was 4 MPa or more. 0.5 Since a membrane-forming solvent having a viscosity of less than 1000 nm was used, the hollow fiber membrane had a spherulitic structure and the mechanical strength of the hollow fiber membrane was reduced, resulting in frequent fiber breakage during spinning of the hollow fiber membrane.
[0131] [Table 9]
[0132] The polyphenylene sulfide hollow fiber membranes of Examples 3, 7, 14 to 17, and 25 had excellent separation performance at the ultrafiltration or nanofiltration level in membrane separation of NMP solution, and also had practical NMP permeation performance and membrane strength. [Explanation of symbols]
[0133] 1: Stirring motor 2: Pressurized gas inlet 3: Container 4: Metering pump 5: Internal coagulation liquid inlet 6: Double tubular nozzle (spinneret) for hollow fiber production 7: Coagulation bath liquid 8: Polyphenylene sulfide hollow fiber membrane 9: Winding machine 10: Bobbin winding machine 11: Liquid circulation pump 12: Regulator 13: Crossflow module 14: Fluid tank 15: Tray 16: Primary pressure gauge 17: Secondary pressure gauge
Claims
1. A first step of preparing a film-forming solution by dissolving a polyphenylene sulfide resin in a film-forming solvent; A second step of forming a hollow fiber membrane having a porous region with a continuous pore structure by discharging the membrane forming solution from an outer annular nozzle using a double-tube nozzle for producing hollow fibers having a double-tube structure and immersing the solution in a coagulation bath; and A third step of removing the solvent from the hollow fiber membrane formed in the second step; The membrane-forming solvent has a Hansen solubility parameter distance (A) between the polyphenylene sulfide resin and the membrane-forming solvent of 4 to 11 MPa. 0.5 and the boiling point at standard pressure is 20° C. or more higher than the phase separation temperature with the polyphenylene sulfide resin.
2. The polyphenylene sulfide hollow fiber membrane has a dense layer on an outer surface thereof, and has the porous region on an inner surface thereof and inside thereof, The method for producing a polyphenylene sulfide hollow fiber membrane according to claim 1, wherein the coagulation bath liquid has a Hansen solubility parameter distance (B) between the polyphenylene sulfide resin and the coagulation bath liquid that satisfies the following formula (1): Hansen solubility parameter distance (B)>Hansen solubility parameter distance (A) (1)
3. The method for producing a polyphenylene sulfide hollow fiber membrane according to claim 1 , wherein in the second step, an internal coagulation liquid is further discharged from an inner nozzle of the double tubular nozzle.
4. The polyphenylene sulfide hollow fiber membrane has a porous region throughout the membrane, The method for producing a polyphenylene sulfide hollow fiber membrane according to claim 3, wherein the coagulating bath liquid has a Hansen solubility parameter distance (B) between the polyphenylene sulfide resin and the coagulating bath liquid that satisfies the following formula (2), and the internal coagulating liquid has a Hansen solubility parameter distance (C) between the polyphenylene sulfide resin and the internal coagulating liquid that satisfies the following formula (3). Hansen solubility parameter distance (B) ≦ Hansen solubility parameter distance (A) (2) Hansen solubility parameter distance (C) ≦ Hansen solubility parameter distance (A) (3)
5. The polyphenylene sulfide hollow fiber membrane has a dense layer on an outer surface thereof, and has the porous region on an inner surface thereof and inside thereof, The method for producing a polyphenylene sulfide hollow fiber membrane according to claim 3, wherein the coagulating bath liquid has a Hansen solubility parameter distance (B) between the polyphenylene sulfide resin and the coagulating bath liquid that satisfies the following formula (1), and the internal coagulating liquid has a Hansen solubility parameter distance (C) between the polyphenylene sulfide resin and the internal coagulating liquid that satisfies the following formula (3). Hansen solubility parameter distance (B)>Hansen solubility parameter distance (A) (1) Hansen solubility parameter distance (C) ≦ Hansen solubility parameter distance (A) (3)
6. The polyphenylene sulfide hollow fiber membrane has a dense layer on an outer surface and an inner surface, and has the porous region inside, The method for producing a polyphenylene sulfide hollow fiber membrane according to claim 3, wherein the coagulating bath liquid has a Hansen solubility parameter distance (B) between the polyphenylene sulfide resin and the coagulating bath liquid that satisfies the following formula (1), and the internal coagulating liquid has a Hansen solubility parameter distance (C) between the polyphenylene sulfide resin and the internal coagulating liquid that satisfies the following formula (4). Hansen solubility parameter distance (B)>Hansen solubility parameter distance (A) (1) Hansen solubility parameter distance (C)>Hansen solubility parameter distance (A) (4)
Citation Information