Paper mat and manufacturing method for paper mat
The paper-made mat with intertwined inorganic fiber bundles and binders addresses the issue of low surface pressure, ensuring effective sealing and structural integrity in exhaust gas purification systems.
Patent Information
- Application Number
- JP2024025479
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-09-11
- Filing Date
- 2024-02-22
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2044-02-22
AI Technical Summary
Existing paper-made mats used in exhaust gas purification systems suffer from low surface pressure due to broken alumina fibers and insufficient intertwining of lumpy agglomerated fibers, leading to reduced elasticity and difficulty in maintaining sufficient sealing performance.
A paper-made mat composed of inorganic fibers, with fiber bundles formed by intertwining ten or more fibers, having an average length of 5 to 15 mm and a width of 0.2 to 1.0 mm, and being in a curled state, which acts as a core material to resist deformation under pressure, and includes organic and inorganic binders to maintain shape and adhesion.
The mat achieves high surface pressure, preventing the exhaust gas treatment body from dislodging from the casing, enhancing sealing performance and maintaining structural integrity under pressure fluctuations.
Smart Images

Figure 2024147494000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a paper-made mat and a method for producing the same. [Background technology]
[0002] Exhaust gas emitted from internal combustion engines such as diesel engines contains particulate matter (hereinafter referred to as PM), and in recent years, the harm that this PM poses to the environment and human body has become a problem. In addition, exhaust gas also contains harmful gas components such as CO, HC, and NOx, and there are concerns about the impact that these harmful gas components have on the environment and human body.
[0003] In response to this, various exhaust gas purification devices have been proposed that capture PM in exhaust gas and purify harmful gas components, and are composed of an exhaust gas treatment body made of porous ceramics such as silicon carbide and cordierite, a casing that houses the exhaust gas treatment body, and a holding seal material (mat material) disposed between the exhaust gas treatment body and the casing. The main purpose of this holding seal material (mat material) is to prevent the exhaust gas treatment body from coming into contact with the casing that covers its outer periphery and being damaged by vibrations and impacts caused by the running of the automobile, and to prevent exhaust gas from leaking from between the exhaust gas treatment body and the casing.
[0004] In order to improve the force (surface pressure) with which the mat material holds the exhaust gas treatment body, Patent Document 1 discloses a mat material in which the surface pressure is improved by producing an alumina fiber aggregate using a specific spinning aid.
[0005] Patent Document 2 also discloses that a needled sheet is first produced, the needled sheet is dry-opened to obtain opened fibers containing agglomerated fibers, and a paper-made sheet material is produced using the opened fibers containing agglomerated fibers. Patent Document 2 also discloses that the inclusion of agglomerated fibers improves the surface pressure of the paper-made sheet material. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] International Publication No. 2018 / 012423 [Patent Document 2] JP 2008-82310 A Summary of the Invention [Problem to be solved by the invention]
[0007] The mat material described in Patent Document 1 has a problem in that the alumina fibers are easily broken, and the surface pressure is easily reduced. The papermaking sheet material described in Patent Document 2 is made by dry-spreading a needle ring sheet, so the spread fibers are short, and the fibers constituting the lumpy aggregated fibers are also short. Therefore, the fibers in the lumpy aggregated fibers are not sufficiently entangled with each other, and the lumpy aggregated fibers are not twisted. The length of the lumpy aggregated fibers is also short. Therefore, the elasticity of the lumpy aggregated fibers is not sufficiently high, and as a result, there is a problem that the surface pressure of the papermaking sheet material produced is difficult to be sufficiently high.
[0008] The present invention has been made in consideration of the above problems, and an object of the present invention is to provide a papermaking mat having a sufficiently high surface pressure. [Means for solving the problem]
[0009] That is, the papermaking mat of the present invention is a papermaking mat composed of inorganic fibers, the papermaking mat including fiber bundles formed by twisting and intertwining 10 or more of the inorganic fibers, and the inorganic fibers that do not constitute the fiber bundles, the average length of the fiber bundles is 5 to 15 mm, the average width of the fiber bundles is 0.2 to 1.0 mm, the fiber bundles include fiber bundles in a crimped state, and the tracing length of the fiber bundles in the crimped state measured by the tracing length measurement method described below is 0.1 mm or more longer than the length of the fiber bundles in the crimped state. How to measure trace length: The crimped fiber bundle is placed on a flat surface. The fiber bundle in the crimped state that has been left stationary is viewed from above, and a line is traced along the fiber bundle in the crimped state from one end of the fiber bundle in the crimped state to the other end, and the distance traced is defined as the "tracing length of the fiber bundle in the crimped state."
[0010] The papermaking mat of the present invention includes fiber bundles having a predetermined size. Such fiber bundles are formed by twisting and intertwining 10 or more inorganic fibers to have a predetermined length and width, and since they support each other, they are not easily deformed by pressure. Therefore, when pressure is applied to the papermaking mat, the fiber bundles act as a core material and can reduce the pressure on the inorganic fibers that do not constitute the fiber bundles. Therefore, it is possible to prevent the inorganic fibers that do not constitute the fiber bundles from breaking due to pressure. As a result, the surface pressure of the papermaking mat of the present invention is high.
[0011] In the papermaking mat of the present invention, the fiber bundles include fiber bundles in a crimped state, and the trace length of the fiber bundles in the crimped state measured by the above-mentioned trace length measurement method is at least 0.1 mm longer than the length of the fiber bundles in the crimped state. The fiber bundles in a crimped state are elastic, and a papermaking mat containing such fiber bundles is subject to high surface pressure.
[0012] The papermaking mat of the present invention preferably contains 0.1 to 20 parts by weight of an organic binder and 0.1 to 10 parts by weight of an inorganic binder per 100 parts by weight of inorganic fibers. The organic binder and the inorganic binder bond the inorganic fibers together and maintain the shape of the papermaking mat. When the contents of the organic binder and the inorganic binder are within the above ranges, the inorganic fibers are appropriately bonded to each other, and the paper mat can have both flexibility and shape retention. In addition, it is possible to prevent the inorganic fibers from falling off the paper mat and scattering.
[0013] In the papermaking mat of the present invention, the organic binder preferably has a glass transition temperature Tg of 5° C. or lower. When the glass transition temperature Tg of the organic binder is 5° C. or lower, the strength of the organic binder film formed by the organic binder can be increased, and the papermaking mat can have high film elongation and excellent flexibility.
[0014] In the papermaking mat of the present invention, the organic binder is preferably at least one selected from the group consisting of acrylic resin, acrylate-based latex, rubber-based latex, carboxymethyl cellulose, and polyvinyl alcohol which function as water-soluble organic polymers, styrene resin which functions as a thermoplastic resin, and epoxy resin which functions as a thermosetting resin. In the papermaking mat of the present invention, the inorganic binder preferably contains at least one of alumina, silica, silicon carbide, zirconia, boron nitride, diamond, and pumice. These organic binders and inorganic binders are suitable for bonding the inorganic fibers together and maintaining the shape of the papermaking mat.
[0015] In the papermaking mat of the present invention, the fiber bundles may include fiber bundles in a straight state. The straight fiber bundle can be obtained by opening, in water, a first inorganic fiber molded body derived from a needle mat and a second inorganic fiber molded body derived from a papermaking mat.
[0016] The method for producing a papermaking mat of the present invention includes a fiber-opening step of opening an inorganic fiber molding in water to produce a slurry containing the opened inorganic fibers, and a papermaking step of papermaking the slurry to form a papermaking mat, and is characterized in that in the fiber-opening step, the slurry contains fiber bundles formed by twisting and entangling 10 or more of the inorganic fibers, the fiber bundles having an average length of 5 to 15 mm and an average width of 0.2 to 1.0 mm, and the inorganic fibers that do not constitute the fiber bundles.
[0017] In the method for producing a papermaking mat of the present invention, an inorganic fiber molded body is opened in water to obtain inorganic fibers, which are then paper-made. When the inorganic fiber molded body is opened, the inorganic fibers may not be completely opened, resulting in fiber bundles in which a plurality of fibers are twisted and entangled. In the method for producing a paper mat of the present invention, such fiber bundles are intentionally produced. The number of inorganic fibers that are twisted and entangled in the fiber bundle, as well as the average length and average width of the fiber bundle, can be adjusted by adjusting the spreading conditions. The mat produced by this method has a high surface pressure.
[0018] In the method for producing a papermaking mat of the present invention, the inorganic fiber molded body preferably includes a first inorganic fiber molded body derived from a needle mat and / or a second inorganic fiber molded body derived from a papermaking mat. Whether the inorganic fiber molded product is derived from a needle mat or a paper-formed mat, it can form a fiber bundle in the opening step. Effect of the Invention
[0019] According to the present invention, a paper mat having a sufficiently high surface pressure can be provided. [Brief description of the drawings]
[0020] [Figure 1A] FIG. 1A is a perspective view showing an example of a papermaking mat of the present invention. [Figure 1B] FIG. 1B is an enlarged view of the dashed line portion of FIG. 1A. [Diagram 2] FIG. 2 is a schematic diagram of an example of a crimped fiber bundle contained in the papermaking mat of the present invention. [Diagram 3] FIG. 3 is a cross-sectional view that illustrates an example of an exhaust gas purification device of the present invention. [Figure 4A] FIG. 4A is a photograph of one of the straight fiber bundles contained in the papermaking mat of Example 1. FIG. [Figure 4B]FIG. 4B is a photograph illustrating the orientation of the fiber bundles shown in FIG. 4A. [Figure 5A] FIG. 5A is a photograph of one of the fiber bundles in a crimped state contained in the papermaking mat of Example 1. FIG. [Figure 5B] FIG. 5B is a photograph illustrating the orientation of the fiber bundles shown in FIG. 5A. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] The papermaking mat of the present invention will be specifically described below. However, the present invention is not limited to the following configuration, and can be appropriately modified and applied within the scope that does not change the gist of the present invention. In addition, the present invention also includes a combination of two or more of the individual preferred configurations of the present invention described below.
[0022] The papermaking mat according to the present invention will be described with reference to the drawings. FIG. 1A is a perspective view showing an example of a papermaking mat of the present invention. FIG. 1B is an enlarged view of the dashed line portion of FIG. 1A. As shown in FIG. 1A, a papermaking mat 10 is a papermaking mat made of inorganic fibers. The papermaking mat 10 has a rectangular shape in a plan view, with a protruding portion 11a provided at one end 11 and a recessed portion 12a provided at the other end 12.
[0023] As will be described in detail later, the papermaking mat 10 is wrapped around an exhaust gas treatment body and placed in the exhaust gas purification device. The convex portions 11a and the concave portions 12a are shaped to fit exactly together when the paper mat 10 is wrapped around the exhaust gas treatment body. The provision of such convex portions 11a and concave portions 12a improves the sealing performance when the papermaking mat 10 is placed in an exhaust gas purification device, which will be described later. The papermaking mat of the present invention does not necessarily have to have any protrusions or recesses at its ends.
[0024] As shown in FIG. 1B, the papermaking mat 10 includes fiber bundles 21 formed by twisting and entangling ten or more inorganic fibers 20, and inorganic fibers 22 that do not constitute the fiber bundles 21. The fiber bundle 21 may be in a straight state (denoted by reference symbol "21a" in FIG. 1B) or in a curled state (denoted by reference symbol "21b" in FIG. 1B). In the papermaking mat 10, the fiber bundles 21 include the fiber bundles 21b in a crimped state as an essential component.
[0025] In this specification, the term "straight state" means that the direction of the fiber bundle (the direction indicated by the arrow D1 in FIG. 1B) is linear. In addition, in this specification, the term "crimped" refers to a state in which the direction of the fiber bundle (the direction indicated by the arrow D2 in FIG. 1B) is curved at least once.
[0026] The average length of the fiber bundles 21 (the average value of the lengths indicated by the symbol L in FIG. 1B) is 5 to 15 mm. The average length of the fiber bundles 21 is preferably 7 to 13 mm, and more preferably 8 to 10 mm. The average width of the fiber bundles 21 (the average value of the length indicated by the symbol W in FIG. 1B) is 0.2 to 1.0 mm. The average width of the fiber bundles 21 is preferably 0.2 to 0.8 mm. As shown in FIG. 1B, when the fiber bundle 21 is a straight fiber bundle 21a and when the fiber bundle 21 is a crimped fiber bundle 21b, the maximum width (the lengths indicated by the symbols Wa and Wb, respectively, in FIG. 1B) is the width of the fiber bundle 21.
[0027] The fiber bundles 21 are formed by twisting and intertwining 10 or more inorganic fibers 20, and since they support each other, they are not easily deformed by pressure. Therefore, when pressure is applied to the papermaking mat 10, the fiber bundles 21 act as a core material and can reduce the pressure on the inorganic fibers 22 that do not constitute the fiber bundles 21. Therefore, it is possible to prevent the inorganic fibers 22 that do not constitute the fiber bundles 21 from breaking due to pressure. As a result, the surface pressure of the papermaking mat 10 is high. In particular, when the fiber bundles 21 are crimped fiber bundles 21b, this effect is exhibited favorably, and the surface pressure of the papermaking mat 10 becomes higher.
[0028] If the average length of the fiber bundles is less than 5 mm, the fiber bundles are too short, making it difficult for the fiber bundles to act as a core material and to relieve the pressure applied to the inorganic fibers that do not constitute the fiber bundles. If the average length of the fiber bundle exceeds 15 mm, the fiber bundle is too long and when pressure is applied to the sides of the fiber bundle, it becomes easy to bend and does not function well as a core material.
[0029] If the average width of the fiber bundle is less than 0.2 mm, the strength of the fiber bundle will be low, the fiber bundle will be easily bent, and it will be difficult for the fiber bundle to function as a core material. If the average width of the fiber bundle exceeds 1.0 mm, the strength of the fiber bundle becomes too high, and the flexibility of the entire papermaking mat decreases.
[0030] In this specification, the term "fiber bundle" refers to a portion of the papermaking mat where inorganic fibers are concentrated and have a higher density than other portions. In this specification, the term "fiber bundle formed by intertwining inorganic fibers in a twisted manner" refers to the following fiber bundle. Although the details will be described later, the papermaking mat of the present invention is manufactured from a needle mat and inorganic fibers obtained by opening the papermaking mat. When the needle mat and the paper-made mat are opened, the inorganic fibers may not be completely opened, and fiber bundles in which a plurality of fibers are twisted and entangled may be produced. That is, when the needle mat is manufactured, the inorganic fibers are entangled with each other by the needles, so that the inorganic fibers are strongly entangled with each other in that portion. In addition, when the papermaking mat is manufactured, the inorganic fibers are bonded together with an organic binder, so that the inorganic fibers are not easily separated from each other. When the papermaking mat is manufactured by the papermaking method, the aggregate of the inorganic fibers is unevenly formed, and an aggregate of the inorganic fibers with high density is formed. In needle mats, the portions where the inorganic fibers are entangled by the needles, and in paper mats, the aggregated portions of the inorganic fibers with high density are difficult to open, and remain as twisted and entangled fiber bundles. In this manner, the fiber bundles remaining when the needle mat and the paper-made mat are opened are referred to as "fiber bundles in which the inorganic fibers are entangled so as to be twisted" in this specification. The papermaking mat of the present invention contains fiber bundles in which such inorganic fibers are entangled so as to be twisted.
[0031] The average length of the fiber bundle and the average width of the fiber bundle refer to values measured as follows. 150cm from papermaking mat 3 Cut out a test piece. The test piece is then fired at 600°C for one hour to thermally decompose the binder components. Next, the test piece is placed in a container, and the container is vibrated up and down and left and right to loosen the inorganic fibers that make up the test piece. A fiber bundle is taken out from the loosened test piece, and the length and width of the fiber bundle are measured. The same procedure is repeated three times, and the average length and width of the obtained fiber bundles are calculated. In calculating the average length and average width of the fiber bundles, fiber bundles consisting of less than 10 inorganic fibers are excluded from the calculation.
[0032] As long as the mat material of the present invention contains fiber bundles having an average length of 5 to 15 mm and an average width of 0.2 to 1.0 mm, it may contain fiber bundles having a length of less than 5 mm, a length of more than 15 mm, a width of less than 0.2 mm, or a width of more than 1.0 mm.
[0033] As described above, the papermaking mat 10 includes the crimped fiber bundles 21b as an essential component. The crimped fiber bundle 21b will be described in detail below with reference to the drawings. FIG. 2 is a schematic diagram of an example of a crimped fiber bundle contained in the papermaking mat of the present invention. The fiber bundle 21b in the crimped state shown in FIG. 2 has a trace length L t is preferably longer than the length L of the fiber bundle 21b in the crimped state, more preferably by 0.1 mm or more, and even more preferably by 0.2 to 0.6 mm.
[0034] (Method of measuring tracing length) The fiber bundle 21b in a crimped state is placed on a flat surface. Next, when the fiber bundle 21b in the crimped state that has been left stationary is viewed from above, one end P 1 to the other end P 2 The fiber bundle 21b in the crimped state is traced along the length L t is defined as the "tracing length of the fiber bundle in a crimped state."
[0035] The length L of the fiber bundle 21b in the crimped state t When the length L of the fiber bundles 21b in the crimped state is longer than the length L of the fiber bundles 21b in the crimped state, the elasticity of the fiber bundles 21b in the crimped state increases, and the surface pressure of the papermaking mat 10 increases.
[0036] In the papermaking mat 10, when the "trace length of the fiber bundle in the crimped state" is measured for the fiber bundle 21b in the crimped state shown in FIG. 1 and end P 2 It is preferable that the fiber bundles 21b include fiber bundles 21b in a crimped state such that the fiber bundles 21b in a crimped state can be traced so as to cross the line segment S connecting the fiber bundles 21b and the line segment S two or more times. The fiber bundles 21b in such a crimped state have an appropriate degree of crimping, and the elasticity of the fiber bundles 21b in the crimped state is increased, so that the surface pressure of the papermaking mat 10 is improved.
[0037] In the papermaking mat 10, the length L of the fiber bundle 21b in the crimped state is compared to the tracing length L of the fiber bundle 21b in the crimped state. t The ratio of L t It is preferable that / L=1.1 to 1.6.
[0038] In the papermaking mat 10, the value of the following formula (1) is preferably 0.1 or more, and more preferably 0.2 to 0.6. (L t -L) / Wb···(1)
[0039] In the papermaking mat 10, the fiber bundles 21b in a crimped state are placed on a flat surface, and the area of the fiber bundles 21b in a crimped state as viewed from above is 2.6 to 8.3 mm 2 It is preferable that:
[0040] In the papermaking mat 10, the proportion of the number of crimped fiber bundles 21b contained in the fiber bundles 21 is preferably 85% or less, more preferably 60% or less, even more preferably 30% or less, and even more preferably 10 to 30%.
[0041] The inorganic fibers 20 constituting the papermaking mat 10 preferably contain at least one type selected from alumina fibers, silica fibers, alumina-silica fibers, mullite fibers, glass fibers, and biosoluble fibers. If the papermaking mat 10 is made of these inorganic fibers, it has sufficient heat resistance.
[0042] The inorganic fibers 20 constituting the papermaking mat 10 preferably have an average fiber diameter of 2 to 10 μm and an average fiber length of 0.01 to 5.0 mm.
[0043] The bulk density of the paper mat 10 is 0.05 to 0.30 g / cm 3 It is preferable that: The bulk density of the paper mat 10 is 0.05 g / cm 3 If the thickness is less than this, the inorganic fibers will not be entangled well and will be prone to peeling, making it difficult to maintain the desired shape of the paper-made mat. The bulk density of the paper mat 10 is 0.30g / cm 3 If it exceeds this value, the mat becomes hard, the wrapping property decreases, and the mat is easily torn.
[0044] The papermaking mat 10 preferably contains 0.1 to 20 parts by weight, and more preferably 0.5 to 10 parts by weight, of the organic binder per 100 parts by weight of the inorganic fibers 20. The inorganic binder is preferably contained in an amount of 0.1 to 10 parts by weight, more preferably 0.5 to 3.0 parts by weight, per 100 parts by weight of the inorganic fibers 20. The organic binder and the inorganic binder bond the inorganic fibers together and maintain the shape of the papermaking mat. When the contents of the organic binder and the inorganic binder are within the above ranges, the inorganic fibers are appropriately bonded to each other, and the paper mat can have both flexibility and shape retention. In addition, it is possible to prevent the inorganic fibers from falling off the paper mat and scattering.
[0045] In the papermaking mat 10, the glass transition temperature Tg of the organic binder is preferably 5°C or lower, and more preferably -35 to 5°C. When the glass transition temperature Tg of the organic binder is 5° C. or lower, the strength of the organic binder film formed by the organic binder can be increased, and the resulting papermaking mat has high film elongation and excellent flexibility. In addition, the mat is less likely to tear when it is wrapped around the exhaust gas treatment body, etc. Furthermore, since the organic binder film does not become too hard, when the inorganic fibers are broken, it has the effect of binding the inorganic fibers together, and it is possible to suppress scattering of the inorganic fibers. If the glass transition temperature Tg of the organic binder exceeds 5° C., the flexibility of the papermaking mat decreases, and the breaking elongation may decrease.
[0046] In the papermaking mat of the present invention, the organic binder may be a water-soluble organic polymer, a thermoplastic resin, or a thermosetting resin. Examples of water-soluble organic polymers include acrylic resins, acrylate-based latexes, rubber-based latexes, carboxymethyl cellulose, and polyvinyl alcohol. Examples of thermoplastic resins include styrene resins. Examples of epoxy resins function as thermosetting resins.
[0047] In the papermaking mat 10, the inorganic binder preferably contains at least one of alumina, silica, silicon carbide, zirconia, boron nitride, diamond, and pumice.
[0048] These organic binders and inorganic binders are suitable for bonding the inorganic fibers together and maintaining the shape of the papermaking mat.
[0049] Next, the method for producing the paper-made mat of the present invention will be described. The method for producing a papermaking mat of the present invention includes (1) a fiber-opening step and (2) a papermaking step. In the following explanation, we will describe the case where both a first inorganic fiber molding derived from a needle mat and a second inorganic fiber molding derived from a papermaking mat are used as inorganic fiber moldings, but in the manufacturing method of a papermaking mat of the present invention, either one of the inorganic fiber moldings may be used. Each step is described in detail below.
[0050] (1) Opening process In this step, the first inorganic fiber molded body derived from the needle mat and the second inorganic fiber molded body derived from the papermaking mat are opened in water to prepare a slurry containing the opened inorganic fibers. In this process, the slurry is opened so that it contains fiber bundles formed by twisting and entangling 10 or more of the inorganic fibers and having an average length of 5 to 15 mm and an average width of 0.2 to 1.0 mm, and the inorganic fibers that do not constitute fiber bundles. In this step, it is preferable not to perform dry opening.
[0051] When the needle mat and the paper-made mat are opened, the inorganic fibers may not be completely opened, and fiber bundles in which a plurality of fibers are twisted and entangled may be produced. More specifically, it is as follows. When the needle mat is manufactured, the inorganic fibers are entangled with each other by needles, so that the inorganic fibers are strongly entangled with each other in that portion. In addition, when the papermaking mat is manufactured, the inorganic fibers are bonded together with an organic binder, so that the inorganic fibers are not easily separated from each other. When the papermaking mat is manufactured by the papermaking method, the aggregate of the inorganic fibers is unevenly formed, and an aggregate of the inorganic fibers with high density is formed. In needle mats, the portions where the inorganic fibers are entangled by the needles, and in paper mats, the aggregated portions of the inorganic fibers with high density are difficult to open, and remain as twisted and entangled fiber bundles. In the method for producing a paper mat of the present invention, such fiber bundles are intentionally produced. The number of inorganic fibers that are twisted and entangled in the fiber bundle, as well as the average length and average width of the fiber bundle, can be adjusted by adjusting the spreading conditions.
[0052] The fiber-spreading conditions are not particularly limited. For example, when fiber-spreading is performed using a stirrer in water, the number of inorganic fibers that are entangled so as to be twisted in the fiber bundle, as well as the average length and average width of the fiber bundle, can be adjusted by adjusting the rotation speed and time of the stirrer.
[0053] If dry spreading is performed in this step, the inorganic fibers are easily broken and the length of the fiber bundle is shortened, resulting in a shortened length of the obtained fiber bundle and making it impossible to obtain a fiber bundle having a desired shape. Therefore, it is preferable not to perform dry opening in this step.
[0054] The fiber bundles produced in this step may be derived from either the first inorganic fiber molded body or the second inorganic fiber molded body. Whether the inorganic fiber molded body is derived from a first inorganic fiber molded body (derived from a needle mat) or a second inorganic fiber molded body (derived from a paper-made mat), a fiber bundle can be formed in the opening step.
[0055] Examples of the fiber opening include the following methods. First, the first inorganic fiber molded body and the second inorganic fiber molded body are fired at 700 to 1000°C for 1.0 to 8.0 hours. The firing temperature is preferably 800 to 950°C. This allows the organic binder contained in the first inorganic fiber molded body and the second inorganic fiber molded body to be thermally decomposed, making it easier to open up the first inorganic fiber molded body and the second inorganic fiber molded body.
[0056] Next, the fired first inorganic fiber molded body and second inorganic fiber molded body are left to stand until they reach room temperature, and then the first inorganic fiber molded body and second inorganic fiber molded body are loosened by hand.
[0057] Next, the first inorganic fiber molded body and the second inorganic fiber molded body are placed in water in an amount of 50 to 400 times by weight and stirred to open the fibers, thereby preparing a slurry containing inorganic fibers. The weight ratio is preferably 100 to 200 times. For example, when preparing a 10 L slurry, it is preferable to use a stirrer (product name: SMT-101, manufacturer: ASONE) and stir at a rotation speed of 500 to 1000 rpm for a stirring time of 200 to 900 seconds. Preferably, the rotation speed is 650 to 850 rpm, the stirring time is 500 to 700 seconds, and more preferably, the rotation speed is 700 to 800 rpm, and the stirring time is 500 to 650 seconds. At this time, the slurry is opened so that, when the slurry is dried, 10 or more of the inorganic fibers are twisted and entangled to form a fiber bundle having an average length of 5 to 15 mm and an average width of 0.2 to 1.0 mm.
[0058] Next, the organic and inorganic binders are added to the slurry. The organic binder is preferably added in an amount of 0.1 to 20 parts by weight, and more preferably 0.5 to 15.0 parts by weight, per 100 parts by weight of the inorganic fibers in the produced paper mat. The inorganic binder is preferably added in an amount of 0.1 to 15.0 parts by weight, and more preferably 0.5 to 10 parts by weight, per 100 parts by weight of the inorganic fibers in the produced paper mat. Since the preferred types of organic binders and inorganic binders have already been described, the description thereof will be omitted here.
[0059] (2) Papermaking process Next, the slurry is poured into a molding machine having a filtering mesh formed on the bottom surface, and the solvent in the slurry is removed to obtain an inorganic fiber aggregate. The inorganic fiber aggregate is then dehydrated and dried to obtain the papermaking mat of the present invention.
[0060] In the papermaking process, the inorganic fiber aggregate may be dried by heating and pressing. During the heating and pressing, a heat treatment may be performed in which hot air is passed through the inorganic fiber aggregate to dry it, or the inorganic fiber aggregate may be left in a wet state without being subjected to a heat treatment. When carrying out the heat treatment, the heating temperature or hot air temperature is preferably 150 to 210° C. in order to prevent deterioration of the organic binder due to heat. In the range of 150 to 210°C, moisture can be removed from the inorganic fiber assembly while suppressing deterioration of the organic binder. If the heating temperature or hot air temperature is less than 150°C, the temperature does not reach the center of the inorganic fiber assembly, and the drying time becomes longer. If the temperature exceeds 210°C, the organic binder is deteriorated and the binding force between the fibers is reduced, making it difficult to control the thickness of the inorganic fiber assembly.
[0061] In the method for producing a papermaking mat of the present invention, it is preferable to carry out batch papermaking or continuous papermaking in the papermaking step. The sheet mat of the present invention can be easily obtained by batch or continuous sheet making.
[0062] Next, a method for using the papermaking mat of the present invention will be described. FIG. 3 is a cross-sectional view that illustrates an example of an exhaust gas purification device of the present invention. 3, the exhaust gas purification device 100 includes a metal casing 30, an exhaust gas treatment body 40 housed in the metal casing 30, and a paper mat 10 disposed between the exhaust gas treatment body 40 and the metal casing 30. The paper mat 10 is the paper mat of the present invention. The exhaust gas treatment body 40 is a columnar structure in which a large number of cells 41 are arranged in parallel in the longitudinal direction with cell walls 42 separating them. Note that, to the ends of the metal casing 30, an inlet pipe for introducing exhaust gas discharged from the internal combustion engine and an outlet pipe for discharging exhaust gas that has passed through the exhaust gas purification device to the outside are connected as necessary. In the exhaust gas purification device 100 shown in FIG. 3, an exhaust gas filter (honeycomb filter) in which one of the cells is sealed with a plugging material 43 is used as the exhaust gas treatment body 40, but a catalyst carrier in which none of the end faces are sealed with a plugging material may also be used.
[0063] As shown in Fig. 3, exhaust gas discharged from an internal combustion engine and flowing into the exhaust gas purification device 100 (in Fig. 3, the exhaust gas is indicated by G, and the flow of the exhaust gas is indicated by arrows) flows into one cell 41 opening at an exhaust gas inlet end face 40a of the exhaust gas treatment body (honeycomb filter) 40, and passes through a cell wall 42 separating the cells 41. At this time, PM in the exhaust gas is captured by the cell wall 42, and the exhaust gas is purified. The purified exhaust gas flows out from another cell 41 opening at an exhaust gas outlet end face 40b, and is discharged to the outside.
[0064] As described above, the surface pressure of the papermaking mat 10 is high. Therefore, in the exhaust gas purification device 100, even if the exhaust gas treatment body 40 is subjected to high pressure from the exhaust gas, the exhaust gas treatment body 40 can be prevented from falling off the metal casing 30.
[0065] The exhaust gas treatment body 40 may be made of a non-oxidizing porous ceramic such as silicon carbide or silicon nitride, or may be made of an oxidizing porous ceramic such as sialon, alumina, cordierite, mullite, etc. Among these, silicon carbide is preferable.
[0066] When the exhaust gas treatment body 40 is made of porous ceramics made of silicon carbide, the porosity of the porous ceramics is not particularly limited, but is preferably 35 to 60%. If the porosity is less than 35%, the exhaust gas treatment body may easily become clogged, whereas if the porosity is more than 60%, the strength of the exhaust gas treatment body may decrease and the body may easily be destroyed.
[0067] The average pore size of the porous ceramic is preferably 5 to 30 μm. If the average pore size is less than 5 μm, PM may easily cause clogging. If the average pore diameter exceeds 30 μm, PM may pass through the pores, making it impossible to capture PM and thus unable to function as a filter. The porosity and pore size can be measured by a conventionally known method using a scanning electron microscope (SEM).
[0068] The cell density in the cross section of the exhaust gas treatment body 40 is not particularly limited, but the preferred lower limit is 31.0 cells / cm 2 (200 pieces / inch 2 ), the preferred upper limit is 93.0 particles / cm 2 (600 pieces / inch 2 ) A more preferable lower limit is 38.8 particles / cm 2 (250 pieces / inch 2 ), and a more preferable upper limit is 77.5 particles / cm 2 (500 pieces / inch 2 ).
[0069] The exhaust gas treatment body 40 may support a catalyst for purifying the exhaust gas. The catalyst to be supported is preferably a precious metal such as platinum, palladium, or rhodium, and among these, platinum is more preferable. In addition, other catalysts such as alkali metals such as potassium or sodium, or alkaline earth metals such as barium may also be used. These catalysts may be used alone or in combination of two or more kinds. When these catalysts are supported, PM can be easily burned and removed, and toxic exhaust gas can also be purified.
[0070] (Metal casing) The metal casing 30 is generally cylindrical. The inner diameter of the metal casing 30 (the inner diameter of the portion that houses the exhaust gas treatment body) is preferably slightly shorter than the diameter of the exhaust gas treatment body 40 around which the papermaking mat 10 is wrapped.
[0071] The metal casing 30 is preferably made of, but not limited to, stainless steel. EXAMPLES
[0072] EXAMPLES Hereinafter, examples that more specifically disclose the present invention will be described, however, the present invention is not limited to these examples.
[0073] Example 1 Al 2 O 3 :SiO 2 It is made of alumina-silica fibers with a weight ratio of 72:28 and has a bulk density of 0.17 g / cm 3 The density of needle marks is 21 / cm 2 A first inorganic fiber molding derived from a needle mat having a density of 1000 g / m2 was prepared. In addition, Al 2 O 3 :SiO 2 It is made of alumina-silica fibers with a weight ratio of 72:28 and has a bulk density of 0.12 g / cm 3 A second inorganic fiber molded body derived from a papermaking mat was prepared.
[0074] Next, the first inorganic fiber molded body and the second inorganic fiber molded body were fired at 800° C. for 1 hour to thermally decompose the organic binder contained in the first inorganic fiber molded body and the second inorganic fiber molded body.
[0075] Next, the fired first inorganic fiber molded body and second inorganic fiber molded body were left to stand until they reached room temperature, and then the first inorganic fiber molded body and second inorganic fiber molded body were loosened by hand.
[0076] Next, 5.0 g of the first inorganic fiber molded body and 5.0 g of the second inorganic fiber molded body were taken out and placed in 0.4 L of water. After that, the mixture was stirred at a rotation speed of 1000 rpm for a stirring time of 10 minutes using a stirrer (product name: SMT-101, manufacturer: ASONE) to open the fibers, thereby producing an inorganic fiber slurry.
[0077] In order to confirm whether fiber bundles were formed in the slurry, a portion of the slurry was taken out and dried, and it was confirmed that fiber bundles were formed in which 10 or more inorganic fibers were twisted together.
[0078] Next, an organic binder was added to the slurry in an amount of 0.5 to 10 parts by weight relative to 100 parts by weight of the inorganic fibers. Further, an inorganic binder was added to the slurry in an amount of 0.5 to 3.0 parts by weight per 100 parts by weight of the inorganic fibers.
[0079] Next, the slurry was poured into a molding machine with a filtering mesh formed on the bottom surface, and the solvent in the slurry was removed to obtain an inorganic fiber aggregate. The inorganic fiber aggregate was then dehydrated and dried at 150 to 210°C for 5 minutes to 1 hour to produce a papermaking mat according to Example 1.
[0080] (Observation of fiber bundles 1) From the papermaking mat according to Example 1, 150 cm 3 A test piece was cut out. The test pieces were then fired at 600°C for 1 hour to thermally decompose the binder components. Next, the test piece was placed in a container, and the container was vibrated up and down and left and right to loosen the inorganic fibers that constituted the test piece. Fiber bundles were randomly taken out from the unraveled test piece, and the length and width of the fiber bundles were measured. The same operation was repeated three times, and the average values of the fiber bundle length and fiber bundle width were calculated. As a result, the average length of the fiber bundle was 8 mm, and the average width of the fiber bundle was 0.393 mm.
[0081] Photographs of the fiber bundles contained in the papermaking mat of Example 1 are shown in Figures 4A and 5A, and the directions of the fiber bundles are shown in Figures 4B and 5B.
[0082] FIG. 4A is a photograph of one of the straight fiber bundles contained in the papermaking mat of Example 1. FIG. FIG. 4B is a photograph illustrating the orientation of the fiber bundles shown in FIG. 4A. FIG. 5A is a photograph of one of the fiber bundles in a crimped state contained in the papermaking mat of Example 1. FIG. FIG. 5B is a photograph illustrating the orientation of the fiber bundles shown in FIG. 5A.
[0083] The fiber bundle shown in FIG. 4B was in a straight state, and the direction of the fiber bundle was along the arrow D1. The fiber bundle shown in FIG. 5B was in a crimped state, and the direction of the fiber bundle was along the arrow D2.
[0084] (Example 2) and (Comparative Example 1) and (Comparative Example 2) The papermaking mats of Example 2 and Comparative Examples 1 and 2 were produced in the same manner as Example 1, except that the stirring time was changed when each inorganic fiber molding was opened with a stirrer to prepare an inorganic fiber slurry, and the average length of the fiber bundles contained in the produced papermaking mat was adjusted to the length shown in Table 1.
[0085] [Table 1]
[0086] Comparative Example 3 The composition ratio of the inorganic fiber after firing is Al 2 O 3 :SiO 2The silica sol was mixed so that the weight ratio was 72:28, and an appropriate amount of an organic polymer (polyvinyl alcohol) was further added to prepare a mixed liquid. The resulting mixture was concentrated to obtain a spinning mixture, which was then spun by a blowing method (spinning atmosphere temperature: 120° C.) to produce an alumina fiber precursor. Next, the obtained inorganic fiber precursor was compressed to prepare a continuous sheet-like material, which was then placed in a heating furnace and fired to produce an inorganic fiber aggregate. Next, the inorganic fiber aggregate was stirred and opened using a stirrer (product name: SMT-101, manufacturer: AS ONE) at a rotation speed of 1000 rpm for a stirring time of 10 minutes.
[0087] In order to confirm whether fiber bundles were formed in the slurry, a portion of the slurry was taken out and dried. Although it was confirmed that fiber bundles were formed, the fiber bundles were not twisted.
[0088] Next, the slurry was poured into a molding machine with a filtering mesh formed on the bottom surface, and the solvent in the slurry was removed to obtain an inorganic fiber aggregate. The inorganic fiber aggregate was then dehydrated and dried at 150 to 210°C for 5 minutes to 1 hour to produce a papermaking mat according to Comparative Example 3. When the papermaking mat of Comparative Example 3 was observed using a method similar to that described above in "(Fiber bundle observation 1)," it was found to contain untwisted fiber bundles, with the average length of the fiber bundles being 20 mm and the average width of the fiber bundles being 0.37 mm.
[0089] (Measurement of surface pressure) The papermaking mats according to Examples 1 and 2 and Comparative Examples 1 to 3 were set in a testing machine (product name: SMT-101, manufacturer: ASONE) and the void bulk density (GBD) was 0.40 mm 3 The material was compressed at a rate of 25.4 mm / min until the void bulk density (GBD) was 0.40 mm 3 The mixture was kept at this temperature for 10 min. The contact pressure of each mat was then measured, and the results are shown in Table 1.
[0090] As shown in Table 1, it was found that the sheet-formed mats according to the respective examples had a high surface pressure.
[0091] Comparative Example 4 In an aqueous solution of basic aluminum chloride with an aluminum content of 70 g / l and an atomic ratio of Al / Cl of 1.8, alumina fibers with a composition of Al 2 O 3 :SiO 2 Silica sol was mixed so that the ratio of sol to fiber was 72:28 to form an alumina-based fiber precursor. Next, an organic polymer such as polyvinyl alcohol was added to the alumina-based fiber precursor. This liquid was then concentrated to form a spinning solution, which was then used for spinning by a blowing method. The alumina-based fiber precursor was then folded and laminated to produce an alumina-based fiber laminate sheet. Next, a needling process was performed on this laminate sheet. The needling process was performed at 50 pieces / 100 cm. 2 Two sets of needle boards with needles of 10 ... 2 As a result, a laminated sheet having an interwoven point density of about
[0092] The obtained laminated sheet was then continuously fired from room temperature to a maximum temperature of 1250°C to obtain a needling sheet material with a thickness of approximately 7 mm.
[0093] Next, the needling sheet material was roughly cut into pieces measuring 200 mm x 200 mm or less, which were then placed in a feather mill (FM-1, manufactured by Hosokawa Micron Corporation) and dry-spread to obtain cotton-like spread fibers with a diameter of approximately 150 mm.
[0094] Next, to prepare the raw material slurry, 1200g of the obtained spread fibers and 120,000g of water were placed in a mixer and stirred for 1 minute. Next, 60g of organic binder (latex) was added to this solution and stirred for another 1 minute. Next, 12g of inorganic binder (alumina sol) was added to this solution and stirred for another 1 minute. Finally, 6g of coagulant (Percol 292) was added and stirred for 1 minute to obtain the raw material slurry.
[0095] Next, in order to form a compact, the raw material slurry thus prepared was transferred to a molding machine having dimensions of 930 mm length × 515 mm width × 400 mm depth and equipped with a filtration wire mesh (30 mesh) at the bottom, and dewatered by using a suction pump to forcibly suck the water out of the raw material slurry from the bottom side of the molding machine through the filtration wire mesh.
[0096] Next, the molded body was removed from the molding machine and compressed and dried at 120°C and 70 kPa for 30 minutes. Through this process, a thickness of 13 mm and a density of 0.19 g / cm3 were obtained. 3 A papermaking mat according to Comparative Example 4 was produced.
[0097] When the papermaking mat of Comparative Example 4 was observed using a method similar to that described above in "(Fiber bundle observation 1)," it was found to contain untwisted fiber bundles, with the average length of the fiber bundles being 3 mm and the average width of the fiber bundles being 1.43 mm.
[0098] (Observation of fiber bundles 2) From the paper mat according to Example 1 and the paper mat according to Comparative Example 4, 150 cm 3 A test piece was cut out. The test pieces were then fired at 600°C for 1 hour to thermally decompose the binder components. Next, the test piece was placed in a container, and the container was vibrated up and down and left and right to loosen the inorganic fibers that constituted the test piece. Thirteen fiber bundles were taken out at random from the test piece derived from the papermaking mat of Example 1, and four fiber bundles were taken out at random from the test piece derived from the papermaking mat of Comparative Example 4.
[0099] The fiber bundles taken out from the test piece derived from the papermaking mat of Example 1 contained 9 crimped fiber bundles and 4 straight fiber bundles. The average length L of these crimped fiber bundles was 6.78 mm. The average area was 4.95 mm. 2 It was. The average length L of the straight fiber bundles was 7.97 mm. The average area was 2.83 mm. 2 It was.
[0100] The fiber bundles taken out from the test pieces derived from the papermaking mat of Comparative Example 4 were all straight fiber bundles. The average length L of the straight fiber bundles was 3.23 mm. The average area was 3.41 mm. 2 It was.
[0101] For each fiber bundle in the crimped state of Example 1, place the fiber bundle on a flat surface, and when viewed from above, measure the trace length L of the fiber bundle. t was measured and the average value was calculated. And the length L of the fiber bundle and the tracing length L of the fiber bundle t The difference (L t -L) and the ratio (L t / L) was calculated. The results are shown in Table 2.
[0102] [Table 2] [Explanation of symbols]
[0103] 10 Paper mat 11 One end 11a Convex part 12 The other end 12a Recess 20 Inorganic Fibers 21 Fiber bundle 21a Straight fiber bundle 21b Curly fiber bundle 22 Inorganic fibers not constituting fiber bundles 30 Metal Casing 40 Exhaust gas treatment body 40a Exhaust gas inlet end 40b Exhaust gas exhaust side end 41 Cell 42 Cell Wall 43 Encapsulating materials 100 Exhaust gas purification equipment
Claims
1. A paper mat made of inorganic fibers, The papermaking mat includes fiber bundles formed by twisting and intertwining 10 or more of the inorganic fibers, and the inorganic fibers that do not constitute the fiber bundles, The average length of the fiber bundle is 5 to 15 mm; The average width of the fiber bundle is 0.2 to 1.0 mm; The fiber bundle includes a crimped fiber bundle, The paper mat is characterized in that the traced length of the fiber bundle in the crimped state, as measured by the following traced length measuring method, is at least 0.1 mm longer than the length of the fiber bundle in the crimped state. How to measure trace length: The crimped fiber bundle is placed on a flat surface. The fiber bundle in a crimped state that has been placed still is viewed from above, and a line is traced along the fiber bundle in a crimped state from one end of the fiber bundle to the other end, and the distance traced is defined as the "tracing length of the fiber bundle in a crimped state."
2. 2. The papermaking mat according to claim 1, comprising 0.1 to 20 parts by weight of an organic binder and 0.1 to 10 parts by weight of an inorganic binder, based on 100 parts by weight of the inorganic fibers.
3. The papermaking mat according to claim 2 , wherein the organic binder has a glass transition temperature Tg of 5° C. or lower.
4. The papermaking mat according to claim 2 or 3, wherein the organic binder is at least one selected from the group consisting of acrylic resin, acrylate-based latex, rubber-based latex, carboxymethyl cellulose, and polyvinyl alcohol, which function as water-soluble organic polymers, styrene resin, which functions as a thermoplastic resin, and epoxy resin, which functions as a thermosetting resin.
5. 4. The papermaking mat according to claim 2, wherein the inorganic binder contains at least one of alumina, silica, silicon carbide, zirconia, boron nitride, diamond, and pumice.
6. The papermaking mat according to claim 1 or 2, wherein the fiber bundles include straight fiber bundles.
7. a fiber-opening step of opening the inorganic fiber molded body in water to prepare a slurry containing the opened inorganic fibers; A method for producing a paper mat, comprising: a papermaking step of papermaking the slurry to produce a paper mat, The method for producing a paper mat is characterized in that in the fiber-opening step, the slurry contains fiber bundles formed by twisting and intertwining 10 or more of the inorganic fibers, the fiber bundles having an average length of 5 to 15 mm and an average width of 0.2 to 1.0 mm, and inorganic fibers that do not constitute the fiber bundles.
8. The method for producing a paper mat according to claim 7 , wherein the inorganic fiber molded body includes a first inorganic fiber molded body derived from a needle mat and / or a second inorganic fiber molded body derived from a paper mat.
Citation Information
Patent Citations
Sheet member, manufacturing method of the same, and exhaust gas processing device
JP2008082310A
Matting, exhaust gas purification device, and method for manufacturing matting
JP2022156707A
Alumina fiber aggregate and production method therefor
WO2018012423A1