Paper mat and manufacturing method for paper mat
The paper-made mat with fiber bundles and controlled bulk specific gravity addresses cracking and surface pressure issues, providing enhanced durability and sealing in exhaust gas treatment systems.
Patent Information
- Application Number
- JP2024025480
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-09-11
- Filing Date
- 2024-02-22
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2044-02-22
AI Technical Summary
Existing paper-made mats used for exhaust gas treatment systems are prone to cracking and have insufficient surface pressure due to the breakage of alumina fibers and low density of inorganic fibers, leading to reduced elasticity and holding force.
A paper-made mat composed of inorganic fibers formed into fiber bundles by twisting and entangling 10 or more fibers, with an average length exceeding 5 mm, and a bulk specific gravity of 0.012 to 0.035 g/cm³, which are oriented in a specific direction to enhance strength and prevent cracking.
The mat maintains high surface pressure and resistance to cracking when wrapped around a base material, ensuring effective sealing and durability in exhaust gas treatment systems.
Smart Images

Figure 2024147495000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a paper-made mat and a method for producing the same. [Background technology]
[0002] Exhaust gas emitted from internal combustion engines such as diesel engines contains particulate matter (hereinafter referred to as PM), and in recent years, the harm that this PM poses to the environment and human body has become a problem. In addition, exhaust gas also contains harmful gas components such as CO, HC, and NOx, and there are concerns about the impact that these harmful gas components have on the environment and human body.
[0003] In response to this, various exhaust gas purification devices have been proposed that capture PM in exhaust gas and purify harmful gas components, and are composed of an exhaust gas treatment body made of porous ceramics such as silicon carbide and cordierite, a casing that houses the exhaust gas treatment body, and a holding seal material (mat material) disposed between the exhaust gas treatment body and the casing. The main purpose of this holding seal material (mat material) is to prevent the exhaust gas treatment body from coming into contact with the casing that covers its outer periphery and being damaged by vibrations and impacts caused by the running of the automobile, and to prevent exhaust gas from leaking from between the exhaust gas treatment body and the casing.
[0004] In order to improve the force (surface pressure) with which the mat material holds the exhaust gas treatment body, Patent Document 1 discloses a mat material in which the surface pressure is improved by producing an alumina fiber aggregate using a specific spinning aid.
[0005] In addition, in Patent Document 2, the holding power (surface pressure) is improved by incorporating aggregated fibers, which are aggregated into aggregates having a diameter of 1 to 5 mm and a total length of 2 to 3 mm, into a papermaking sheet. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] International Publication No. 2018 / 012423 [Patent Document 2] JP 2008-82310 A Summary of the Invention [Problem to be solved by the invention]
[0007] The mat material described in Patent Document 1 has a problem in that the alumina fibers are easily broken, and the surface pressure is easily reduced. In addition, the mat material as described in Patent Documents 1 and 2 is wrapped around the exhaust gas treatment body when in use, but there is a problem in that cracks may occur in the mat material due to differences in the inner and outer circumferences of the mat material when wrapped. In particular, in the mat material described in Patent Document 2, the density of the inorganic fibers present between the aggregated fibers is low, and cracks tend to occur. In addition, the papermaking sheet material described in Patent Document 2 is dry-spread from a needled sheet, so the spread fibers are short, and the fibers constituting the lumpy aggregated fibers are also short. Therefore, the fibers in the lumpy aggregated fibers are not sufficiently entangled with each other, and the lumpy aggregated fibers are not twisted. The length of the lumpy aggregated fibers is also short. Therefore, the elasticity of the lumpy aggregated fibers is not sufficiently high, and as a result, there is a problem that the surface pressure of the papermaking sheet material produced is not sufficiently high.
[0008] The present invention has been made in consideration of the above problems, and an object of the present invention is to provide a papermaking mat that is less likely to crack even when wrapped around a substrate and has a sufficiently high surface pressure. [Means for solving the problem]
[0009] That is, the papermaking mat of the present invention is a papermaking mat composed of inorganic fibers, the papermaking mat includes fiber bundles formed by twisting and intertwining 10 or more of the inorganic fibers, and the inorganic fibers that do not constitute the fiber bundles, the average length of the fiber bundles exceeds 5 mm, and when the papermaking mat is opened by the papermaking mat opening method described below to obtain a slurry containing the inorganic fibers, the underwater bulk density of the inorganic fibers contained in the slurry is 0.012 to 0.035 g / cm 3 It is characterized in that: How to open the paper mat: The papermaking mat is heat treated at 600℃ for 1 hour. 5.0 g of fiber was measured out from the papermaking mat while loosening it, and the fiber was placed in a container containing 400 cc of water. After stirring for 10 minutes at a stirrer speed of 1000 rpm, the mixture is transferred to a measuring cylinder and water is added so that the total volume becomes 500 cc. After leaving it to stand for 30 minutes, the height of the settled fibers is read and the underwater bulk density is calculated using the following formula (1). Underwater bulk density (g / cm 3 ) = 5.0 (g) / Sedimentation volume of fiber (cm 3 ) · · · (1)
[0010] The papermaking mat of the present invention contains fiber bundles. Such fiber bundles are formed by twisting and intertwining 10 or more inorganic fibers, and since they support each other, they are not easily deformed by pressure. Therefore, when pressure is applied to the papermaking mat, the fiber bundles act as a core material and can reduce the pressure applied to the inorganic fibers that do not constitute the fiber bundles. Therefore, it is possible to prevent the inorganic fibers that do not constitute the fiber bundles from breaking due to pressure. As a result, the surface pressure of the papermaking mat of the present invention is high.
[0011] In the papermaking mat of the present invention, the average length of the fiber bundles exceeds 5 mm. The papermaking mat of the present invention is produced by flowing a slurry containing inorganic fibers in a certain direction and papering up the inorganic fibers. If the slurry contains fiber bundles having an average length of more than 5 mm, the produced papermaking mat of the present invention will also contain such fiber bundles. When a slurry containing such fiber bundles is made to flow in a certain direction, the fiber bundles are likely to be caught by other inorganic fibers and become oriented in a direction perpendicular to the flow direction of the slurry. Fiber bundles are stronger and less likely to bend than individual inorganic fibers, so a paper mat in which the fiber bundles are oriented in one direction is less likely to bend in the direction in which the fiber bundles are oriented, but is more likely to bend in the direction perpendicular to the direction in which the fiber bundles are oriented. Therefore, even if such a papermaking mat is bent in a direction perpendicular to the orientation of the fiber bundles, stress is unlikely to be generated, and cracks due to the stress are unlikely to occur. Therefore, even if the papermaking mat of the present invention is wrapped around a substrate, cracks are unlikely to occur.
[0012] In addition, since the papermaking mat of the present invention contains fiber bundles, when the papermaking mat of the present invention is spread by the above-mentioned spreading method, the fiber bundles are not spread and remain in the same state. In the slurry after spreading, the density of the inorganic fibers in the part where the fiber bundles are formed is higher than that in the part where the fiber bundles are not formed. The bulk density in water of the inorganic fibers contained in the slurry after fiber spreading is 0.012 to 0.035 g / cm 3 This means that the proportion of fiber bundles contained in the papermaking mat is appropriate, and the effect of preventing the inorganic fibers that do not constitute the above-mentioned fiber bundles from being broken by pressure can be preferably exerted. The bulk density of the inorganic fibers in the slurry after fiber spreading is 0.012 g / cm 3 If it is less than this, the ratio of fiber bundles contained in the papermaking mat will be low, and the surface pressure of the papermaking mat will be low. The bulk density in water of the inorganic fibers contained in the slurry after fiber spreading is 0.035 g / cm 3 If the thickness exceeds this range, the proportion of fiber bundles contained in the mat increases, and the flexibility of the mat decreases.
[0013] The papermaking mat of the present invention preferably contains 0.1 to 20 parts by weight of an organic binder and 0.1 to 10 parts by weight of an inorganic binder per 100 parts by weight of inorganic fibers. The organic binder and the inorganic binder bond the inorganic fibers together and maintain the shape of the papermaking mat. When the contents of the organic binder and the inorganic binder are within the above ranges, the inorganic fibers are appropriately bonded to each other, and the paper mat can have both flexibility and shape retention. In addition, it is possible to prevent the inorganic fibers from falling off the paper mat and scattering.
[0014] In the papermaking mat of the present invention, the organic binder preferably has a glass transition temperature Tg of 5° C. or lower. When the glass transition temperature Tg of the organic binder is 5° C. or lower, the strength of the organic binder film formed by the organic binder can be increased, and the papermaking mat can have high film elongation and excellent flexibility.
[0015] In the papermaking mat of the present invention, the organic binder is preferably at least one selected from the group consisting of acrylic resin, acrylate-based latex, rubber-based latex, carboxymethyl cellulose, and polyvinyl alcohol which function as water-soluble organic polymers, styrene resin which functions as a thermoplastic resin, and epoxy resin which functions as a thermosetting resin. In the papermaking mat of the present invention, the inorganic binder preferably contains at least one of alumina, silica, silicon carbide, zirconia, boron nitride, diamond, and pumice. These organic binders and inorganic binders are suitable for bonding the inorganic fibers together and maintaining the shape of the papermaking mat.
[0016] In the papermaking mat of the present invention, the fiber bundle is formed by intertwining 10 or more of the inorganic fibers, and it is preferable that the average length of the fiber bundle formed by intertwining 10 or more of the inorganic fibers is more than 5 mm and not more than 15 mm, and the average width of the fiber bundle is 0.2 to 1.0 mm. When the fiber bundle is in this form, the fiber bundle has an appropriate strength as a core material, and the pressure applied to the inorganic fibers that do not constitute the fiber bundle can be reduced. Therefore, the inorganic fibers that do not constitute the fiber bundle can be more effectively prevented from breaking due to the pressure, and the surface pressure of the papermaking mat of the present invention can be increased.
[0017] In the papermaking mat of the present invention, the fiber bundle includes a fiber bundle in a crimped state, and it is preferable that the trace length of the fiber bundle in the crimped state measured by the trace length measurement method described below is at least 0.1 mm longer than the length of the fiber bundle in the crimped state. How to measure trace length: The crimped fiber bundle is placed on a flat surface. The fiber bundle in the crimped state that has been left stationary is viewed from above, and a line is traced along the fiber bundle in the crimped state from one end of the fiber bundle in the crimped state to the other end, and the distance traced is defined as the "tracing length of the fiber bundle in the crimped state." When the tracing length of the fiber bundle in the crimped state is at least 0.1 mm longer than the length of the fiber bundle in the crimped state, the elasticity of the fiber bundle in the crimped state increases, and the surface pressure of the paper mat is improved.
[0018] The method for producing a paper mat of the present invention includes a fiber-opening step of opening an inorganic fiber molded body containing aggregated inorganic fibers in water to prepare a slurry containing fiber bundles formed by entangling 10 or more of the inorganic fibers so as to be twisted and the inorganic fibers that do not constitute the fiber bundles, and a paper-making step of papermaking the slurry to produce a paper mat, wherein in the fiber-opening step, the average length of the fiber bundles exceeds 5 mm, and the bulk density in water of the inorganic fibers contained in the slurry is 0.012 to 0.035 g / cm. 3 The fiber is spread so that the fiber is spread as follows.
[0019] In the method for producing a papermaking mat of the present invention, an inorganic fiber molded body is opened in water to obtain inorganic fibers, which are then paper-made. When the inorganic fiber molded body is opened, the inorganic fibers may not be completely opened, resulting in fiber bundles in which 10 or more fibers are twisted and entangled. In the method for producing a paper mat of the present invention, such fiber bundles are intentionally produced. By producing a predetermined amount of such fiber bundles, the bulk density in water of the inorganic fibers contained in the slurry is increased to 0.012 to 0.035 g / cm 3 It can be said that: A paper mat produced in this manner is less likely to crack even when wrapped around a substrate, and has a sufficiently high surface pressure.
[0020] In the method for producing a papermaking mat of the present invention, the inorganic fiber molded body preferably includes a first inorganic fiber molded body derived from a needle mat and / or a second inorganic fiber molded body derived from a papermaking mat. Whether the inorganic fiber molded product is derived from a needle mat or a paper-formed mat, the first fiber bundle can be formed in the opening step. Effect of the Invention
[0021] According to the present invention, a papermaking mat that is unlikely to crack even when wrapped around a substrate and has a sufficiently high surface pressure can be provided. [Brief description of the drawings]
[0022] [Figure 1A] FIG. 1A is a perspective view showing an example of a papermaking mat of the present invention. [Figure 1B] FIG. 1B is an enlarged view of the dashed line portion of FIG. 1A. [Diagram 2] FIG. 2 is a schematic diagram of an example of a fiber bundle in a crimped state. [Diagram 3] FIG. 3 is a cross-sectional view that illustrates an example of an exhaust gas purification device of the present invention.
[0023] The papermaking mat according to the present invention will be described with reference to the drawings. FIG. 1A is a perspective view showing an example of a papermaking mat of the present invention. FIG. 1B is an enlarged view of the dashed line portion of FIG. 1A. As shown in FIG. 1A, a papermaking mat 10 is a papermaking mat made of inorganic fibers. The papermaking mat 10 has a rectangular shape in a plan view, with a protruding portion 11a provided at one end 11 and a recessed portion 12a provided at the other end 12.
[0024] As will be described in detail later, the papermaking mat 10 is wrapped around an exhaust gas treatment body and placed in the exhaust gas purification device. The convex portions 11a and the concave portions 12a are shaped to fit exactly together when the paper mat 10 is wrapped around the exhaust gas treatment body. The provision of such convex portions 11a and concave portions 12a improves the sealing performance when the papermaking mat 10 is placed in an exhaust gas purification device, which will be described later. The papermaking mat of the present invention does not necessarily have to have any protrusions or recesses at its ends.
[0025] As shown in FIG. 1B, the papermaking mat 10 includes fiber bundles 21 formed by twisting and entangling ten or more inorganic fibers 20, and inorganic fibers 22 that do not constitute the fiber bundles 21. The fiber bundle 21 may be in a straight state (indicated by reference symbol "21a" in FIG. 1B) or in a crimped state (indicated by reference symbol "21b" in FIG. 1B).
[0026] In this specification, the fiber bundle means a portion of the papermaking mat where inorganic fibers are concentrated and entangled, and where the density is higher than other portions.
[0027] Here, the crimped fiber bundle 21b will be described in detail below with reference to the drawings. FIG. 2 is a schematic diagram of an example of a fiber bundle in a crimped state. The fiber bundle 21b in the crimped state shown in FIG. 2 has a trace length L t is preferably longer than the length L of the fiber bundle 21b in the crimped state, more preferably by 0.1 mm or more, and even more preferably by 0.2 to 0.6 mm.
[0028] (Method of measuring tracing length) The fiber bundle 21b in a crimped state is placed on a flat surface. Next, the fiber bundle 21b in the crimped state that has been left stationary is viewed from above, and a line is traced along the fiber bundle 21b in the crimped state from one end P1 to the other end P2 of the fiber bundle 21b in the crimped state, and the distance L t is defined as the "tracing length of the fiber bundle in a crimped state."
[0029] The length L of the fiber bundle 21b in the crimped state t When the length L of the fiber bundles 21b in the crimped state is longer than the length L of the fiber bundles 21b in the crimped state, the elasticity of the fiber bundles 21b in the crimped state increases, and the surface pressure of the papermaking mat 10 increases.
[0030] It is preferable that the papermaking mat 10 includes fiber bundles 21b in a crimped state such that, when measuring the "trace length of the fiber bundle in a crimped state" in the fiber bundles 21b in a crimped state shown in Figure 2, the fiber bundles 21b in a crimped state can be traced so as to cross the line segment S connecting end P1 and end P2 two or more times. The fiber bundles 21b in such a crimped state have an appropriate degree of crimping, and the elasticity of the fiber bundles 21b in the crimped state is increased, so that the surface pressure of the papermaking mat 10 is improved.
[0031] In the papermaking mat 10, the length L of the fiber bundle 21b in the crimped state is compared to the tracing length L of the fiber bundle 21b in the crimped state. t The ratio of L t It is preferable that / L=1.1 to 1.6.
[0032] In the papermaking mat 10, the value of the following formula (1) is preferably 0.1 or more, and more preferably 0.2 to 0.6. (L t -L) / Wb···(1) It should be noted that "Wb" refers to the width of the fiber bundle 21b in a crimped state.
[0033] In the papermaking mat 10, the fiber bundles 21b in a crimped state are placed on a flat surface, and the area of the fiber bundles 21b in a crimped state as viewed from above is 2.6 to 8.3 mm 2 It is preferable that:
[0034] In the papermaking mat 10, the proportion of the number of crimped fiber bundles 21b contained in the fiber bundles 21 is preferably 85% or less, more preferably 60% or less, even more preferably 30% or less, and even more preferably 10 to 30%.
[0035] The fiber bundles 21 are formed by intertwining a plurality of inorganic fibers 20, which support each other and are therefore resistant to deformation under pressure. Therefore, when pressure is applied to the papermaking mat 10, the fiber bundles 21 act as a core material and can reduce the pressure on the inorganic fibers 22 that do not constitute the fiber bundles 21. This prevents the inorganic fibers 22 that do not constitute the fiber bundles 21 from breaking under pressure. As a result, the surface pressure of the papermaking mat 10 is high.
[0036] Since the papermaking mat 10 contains fiber bundles 21, when the papermaking mat 10 is opened by the opening method described below, the fiber bundles are not opened and remain as they are. In the slurry after opening, the density of the inorganic fibers is higher in the part where the fiber bundles are formed than in the part where the fiber bundles are not formed.
[0037] How to open the paper mat: The papermaking mat is heat treated at 600℃ for 1 hour. 5.0 g of fiber was measured out from the papermaking mat while loosening it, and the fiber was placed in a container containing 400 cc of water. After stirring for 10 minutes at 1000 rpm using a stirrer (product name: SMT-101, manufacturer: ASONE), transfer the mixture to a measuring cylinder and add water until the total volume is 500 cc. After leaving it to stand for 30 minutes, the height of the settled fibers is read and the underwater bulk density is calculated using the following formula (1). Underwater bulk density (g / cm 3 ) = 5.0 (g) / Sedimentation volume of fiber (cm3 ) · · · (1)
[0038] The paper mat 10 is opened by the above-mentioned method for opening a paper mat to obtain a slurry containing inorganic fibers, and the inorganic fibers contained in the slurry have a bulk density in water of 0.012 to 0.035 g / cm. 3 The bulk density in water of the inorganic fibers contained in the slurry is 0.014 to 0.028 g / cm 3 It is more preferable that:
[0039] The bulk density in water of the inorganic fibers contained in the slurry after fiber spreading is 0.012 to 0.035 g / cm 3 This means that the proportion of fiber bundles 21 contained in the papermaking mat 10 is appropriate, and the effect of preventing the inorganic fibers 22 that do not constitute the fiber bundles 21 from being broken by pressure can be preferably exerted. The bulk density of the inorganic fibers in the slurry after fiber spreading is 0.012 g / cm 3 If it is less than this, the ratio of fiber bundles contained in the papermaking mat will be low, and the surface pressure of the papermaking mat will be low. The bulk density in water of the inorganic fibers contained in the slurry after fiber spreading is 0.035 g / cm 3 If the thickness exceeds this range, the proportion of fiber bundles contained in the mat increases, and the flexibility of the mat decreases.
[0040] In the papermaking mat 10, the average length of the fiber bundles 21 formed by entangling 10 or more inorganic fibers 20 (the average length indicated by the symbol L in FIG. 1B) exceeds 5 mm. The average length of the fiber bundles 21 is preferably more than 5 mm and not more than 15 mm, and more preferably 7 to 13 mm.
[0041] As will be described in detail later, the papermaking mat 10 is produced by pouring a slurry containing inorganic fibers in a certain direction and papering up the inorganic fibers. If the slurry contains fiber bundles 21 formed by entanglement of 10 or more inorganic fibers and having an average length exceeding 5 mm, the produced paper mat 10 will also contain such fiber bundles 21. When the slurry containing the fiber bundles 21 is made to flow in a certain direction, the fiber bundles 21 are caught by the other inorganic fibers (20, 22) and tend to be oriented in a direction perpendicular to the flow direction of the slurry. The fiber bundles 21 are stronger and less likely to bend than the inorganic fibers 22 alone. Therefore, the papermaking mat 10 in which the fiber bundles 21 are oriented in one direction is less likely to bend in the direction in which the fiber bundles 21 are oriented, but is easily bent in a direction perpendicular to the direction in which the fiber bundles 21 are oriented. Therefore, even if such a papermaking mat 10 is bent in a direction perpendicular to the orientation direction of the fiber bundles 21, stress is unlikely to occur. In addition, cracks due to the stress are unlikely to occur. Therefore, even if the papermaking mat 10 is wrapped around a substrate, cracks are unlikely to occur.
[0042] Furthermore, if the average length of the fiber bundles is 5 mm or less, the fiber bundles are too short, making it difficult for the fiber bundles to act as a core material and to alleviate the pressure applied to the inorganic fibers that do not constitute the fiber bundles. If the average length of the fiber bundles exceeds 15 mm, the fiber bundles are too long and, when pressure is applied to the sides of the fiber bundles, they tend to bend and are less able to function as a core material. Also, when the paper mat is bent, the fiber bundles tend to break, and when the fiber bundles break, cracks tend to form in the paper mat starting from that point.
[0043] In the papermaking mat 10, the average width (average length indicated by the symbol W in FIG. 1B) of fiber bundles 21 formed by entangling 10 or more inorganic fibers 20 is preferably 0.2 to 1.0 mm, and more preferably 0.2 to 0.8 mm. As shown in FIG. 1B, when the fiber bundle 21 is in a straight state 21a and when it is in a crimped state 21b, the maximum width (the lengths indicated by the symbols Wa and Wb, respectively, in FIG. 1B) is the width of the fiber bundle 21.
[0044] If the average width of the fiber bundle is less than 0.2 mm, the strength of the fiber bundle will be low, the fiber bundle will be easily bent, and it will be difficult for the fiber bundle to function as a core material. If the average width of the fiber bundle exceeds 1.0 mm, the strength of the fiber bundle becomes too high, and the flexibility of the entire papermaking mat decreases.
[0045] The average length of a fiber bundle formed by intertwining 10 or more inorganic fibers and the average width of a fiber bundle formed by intertwining 10 or more inorganic fibers refer to values measured as follows. 150cm from the papermaking mat 3 Cut out a test piece. The test piece is then fired at 600°C for one hour to thermally decompose the binder components. Next, the test piece is placed in a container, and the container is vibrated up and down and left and right to loosen the inorganic fibers that make up the test piece. A fiber bundle formed by intertwining 10 or more inorganic fibers is taken out from the loosened test piece, and the length and width of the fiber bundle are measured. The same procedure is repeated three times, and the average length and width of the obtained fiber bundles are calculated. In calculating the average length and average width of the fiber bundles, fiber bundles consisting of less than 10 inorganic fibers are excluded from the calculation.
[0046] In the papermaking mat 10, the fiber bundles 21 are preferably oriented in one direction. When the fiber bundles 21 are oriented in one direction, stress is unlikely to occur even if the papermaking mat 10 is bent in a direction perpendicular to the orientation of the fiber bundles 21. In addition, cracks due to the stress are unlikely to occur. Therefore, even if the papermaking mat 10 is wrapped around a substrate, cracks are unlikely to occur.
[0047] Whether or not the fiber bundles 21 are oriented in one direction is determined by the following method. First, as shown in Fig. 1B, a line segment is drawn connecting one end 21e1 to the other end 21e2 of the fiber bundle 21 on the first main surface of the papermaking mat 10. Next, the acute angle a formed by the line segment and an arbitrary direction d is measured. If the angle is 0 to 45°, the fiber bundle 21 from which the line segment originates is determined to be the fiber bundle 21 oriented in the direction d. In any area of length x width = 5 cm x 5 cm on the first main surface of the papermaking mat 10, if 50% or more of the entire fiber bundles 21 are fiber bundles 21 oriented in direction d, the entire fiber bundles 21 are determined to be oriented in direction d. When the fiber bundles 21 are in this state, it is determined that the "fiber bundles are oriented in one direction" in the papermaking mat.
[0048] As described above, in the papermaking process for producing the papermaking mat 10, if the slurry containing the fiber bundles 21 is flowed in a certain direction, the fiber bundles 21 will get caught on the other inorganic fibers (20, 22) and will tend to be oriented in a direction perpendicular to the flow direction of the slurry. This phenomenon in which the fiber bundles 21 are oriented in a direction perpendicular to the flow direction of the slurry occurs throughout the thickness direction of the papermaking mat 10. Therefore, when the fiber bundles 21 are oriented in one direction on the main surface of the papermaking mat 10, it can be determined that the fiber bundles 21 are also oriented in one direction throughout the papermaking mat 10.
[0049] The inorganic fibers 20 constituting the papermaking mat 10 preferably contain at least one type selected from alumina fibers, silica fibers, alumina-silica fibers, mullite fibers, glass fibers, and biosoluble fibers. If the papermaking mat 10 is made of these inorganic fibers, it has sufficient heat resistance.
[0050] The inorganic fibers 20 constituting the papermaking mat 10 preferably have an average fiber diameter of 3 to 50 μm and an average fiber length of 100 to 100,000 μm.
[0051] The bulk density of the paper mat 10 is 0.05 to 0.30 g / cm 3 It is preferable that: The bulk density of the paper mat 10 is 0.05 g / cm 3 If the thickness is less than this, the inorganic fibers will not be entangled well and will be prone to peeling, making it difficult to maintain the desired shape of the paper-made mat. The bulk density of the paper mat 10 is 0.30g / cm 3If it exceeds this value, the mat becomes hard, the wrapping property decreases, and the mat is easily torn.
[0052] The papermaking mat 10 preferably contains 0.1 to 20 parts by weight, and more preferably 0.5 to 10 parts by weight, of the organic binder per 100 parts by weight of the inorganic fibers 20. The inorganic binder is preferably contained in an amount of 0.1 to 10 parts by weight, more preferably 0.5 to 3.0 parts by weight, per 100 parts by weight of the inorganic fibers 20. The organic binder and the inorganic binder bond the inorganic fibers together and maintain the shape of the papermaking mat. When the contents of the organic binder and the inorganic binder are within the above ranges, the inorganic fibers are appropriately bonded to each other, and the paper mat can have both flexibility and shape retention. In addition, it is possible to prevent the inorganic fibers from falling off the paper mat and scattering.
[0053] In the papermaking mat 10, the glass transition temperature Tg of the organic binder is preferably 5°C or lower, and more preferably -35 to 5°C. When the glass transition temperature Tg of the organic binder is 5° C. or lower, the strength of the organic binder film formed by the organic binder can be increased, and the resulting papermaking mat has high film elongation and excellent flexibility. In addition, the mat is less likely to tear when it is wrapped around the exhaust gas treatment body, etc. Furthermore, since the organic binder film does not become too hard, when the inorganic fibers are broken, it has the effect of binding the inorganic fibers together, and it is possible to suppress scattering of the inorganic fibers. If the glass transition temperature Tg of the organic binder exceeds 5° C., the flexibility of the papermaking mat decreases, and the breaking elongation may decrease.
[0054] In the papermaking mat of the present invention, the organic binder may be a water-soluble organic polymer, a thermoplastic resin, or a thermosetting resin. Examples of water-soluble organic polymers include acrylic resins, acrylate-based latexes, rubber-based latexes, carboxymethyl cellulose, and polyvinyl alcohol. Examples of thermoplastic resins include styrene resins. Examples of epoxy resins function as thermosetting resins.
[0055] In the papermaking mat 10, the inorganic binder preferably contains at least one of alumina, silica, silicon carbide, zirconia, boron nitride, diamond, and pumice.
[0056] These organic binders and inorganic binders are suitable for bonding the inorganic fibers together and maintaining the shape of the papermaking mat.
[0057] Next, the method for producing the paper-made mat of the present invention will be described. The method for producing a papermaking mat of the present invention includes (1) a fiber-opening step and (2) a papermaking step. In the following explanation, we will describe the case where both a first inorganic fiber molding derived from a needle mat and a second inorganic fiber molding derived from a papermaking mat are used as inorganic fiber moldings, but in the manufacturing method of a papermaking mat of the present invention, either one of the inorganic fiber moldings may be used. Each step is described in detail below.
[0058] (1) Opening process In this step, the first inorganic fiber molded body derived from the needle mat and the second inorganic fiber molded body derived from the papermaking mat are opened in water to prepare a slurry containing the opened inorganic fibers. In this process, the bulk density in water of the inorganic fibers contained in the slurry is 0.012 to 0.035 g / cm 3 The fibers are opened so that In this step, it is preferable not to perform dry fiber-spreading before or after the underwater fiber-spreading.
[0059] When the needle mat and the paper-made mat are opened, the inorganic fibers may not be completely opened, resulting in fiber bundles in which a plurality of fibers are entangled. The reason why such fiber bundles are formed will be explained below.
[0060] When the needle mat is manufactured, the inorganic fibers are entangled with each other by needles, so that the inorganic fibers are strongly entangled with each other in that portion. In addition, when the papermaking mat is manufactured, the inorganic fibers are bonded together with an organic binder, so that the inorganic fibers are not easily separated from each other. When the papermaking mat is manufactured by the papermaking method, the aggregate of the inorganic fibers is unevenly formed, and an aggregate of the inorganic fibers with high density is formed. When such a first inorganic fiber forming body derived from a needle mat and a second inorganic fiber forming body derived from a papermaking mat are opened, the parts of the needle mat where the inorganic fibers have been entangled by the needles and the parts of the papermaking mat where the inorganic fibers are concentrated at high density are difficult to open and remain as twisted fiber bundles. In the method for producing a paper mat of the present invention, such fiber bundles are intentionally produced. That is, in the method for producing a paper mat of the present invention, fiber bundles are formed, and the fiber bundles are spread so that the average length of the fiber bundles exceeds 5 mm. By producing a predetermined amount of such fiber bundles, the bulk density in water of the inorganic fibers contained in the slurry is increased to 0.012 to 0.035 g / cm 3 It can be said that:
[0061] The bulk density in water of the inorganic fibers contained in the slurry can be measured by the following method. First, the slurry is completely dried, and 5.0 g of fibers are measured out from the dried slurry while loosening it, and the fibers are placed in a container containing 400 cc of water. Next, after stirring at 1000 rpm for 10 minutes, the mixture is transferred to a measuring cylinder and water is added so that the total volume becomes 500 cc. After leaving it to stand for 30 minutes, the height of the settled fibers is read and the underwater bulk density is calculated using the following formula (1). Underwater bulk density (g / cm 3 ) = 5.0 (g) / Sedimentation volume of fiber (cm 3 ) · · · (1)
[0062] The fiber bundles contained in the slurry are formed by entangling 10 or more inorganic fibers, and preferably have an average length of 5 to 15 mm and an average width of 0.2 to 1.0 mm.
[0063] The fiber-spreading conditions are not particularly limited. For example, when the fiber-spreading is performed in water using a stirrer, the rotation speed and time of the stirrer can be adjusted to make the bulk density in water of the inorganic fibers contained in the slurry 0.012 to 0.035 g / cm. 3 In addition, by adjusting the rotation speed and time of the stirrer, the average length and average width of the fiber bundle can also be adjusted.
[0064] In addition, the fiber bundles produced in this step are preferably derived from needle marks on the first inorganic fiber molded body. When manufacturing the needle mat, the inorganic fibers are entangled by needle punching. When such a needle mat is opened in water, inorganic fibers including fiber bundles in which a plurality of inorganic fibers are entangled are obtained. The fiber bundles are crimped fiber bundles. By adjusting the needle punching conditions, the bulk density in water of the inorganic fibers contained in the slurry can be easily adjusted to 0.012 to 0.035 g / cm 3 It can be said that: In other words, the papermaking mat of the present invention can be easily produced by going through a process of opening a predetermined needle mat.
[0065] Examples of the fiber opening include the following methods. First, the first inorganic fiber molded body and the second inorganic fiber molded body are fired at 500 to 1200°C for 0.5 to 10.0 hours. The firing temperature is preferably 800 to 950°C. This allows the organic binder contained in the first inorganic fiber molded body and the second inorganic fiber molded body to be thermally decomposed, making it easier to open up the first inorganic fiber molded body and the second inorganic fiber molded body.
[0066] Next, the fired first inorganic fiber molded body and second inorganic fiber molded body are left to stand until they reach room temperature, and then the first inorganic fiber molded body and second inorganic fiber molded body are loosened by hand.
[0067] Next, the first inorganic fiber molded body and the second inorganic fiber molded body are placed in water in an amount of 50 to 400 times by weight, and the mixture is stirred to open the fibers, thereby producing a slurry containing inorganic fibers. For example, when preparing a 10 L slurry, it is preferable to use a stirrer (product name: SMT-101, manufacturer: ASONE) and stir at a rotation speed of 500 to 1000 rpm for a stirring time of 200 to 900 seconds. Preferably, the rotation speed is 650 to 850 rpm, the stirring time is 500 to 700 seconds, and more preferably, the rotation speed is 700 to 800 rpm, and the stirring time is 500 to 650 seconds. This allows the bulk density of the inorganic fibers in the slurry to be 0.012 to 0.035 g / cm 3 and the average length of the fiber bundles can be greater than 5 mm.
[0068] Next, the organic and inorganic binders are added to the slurry. The organic binder is added to the produced paper mat in an amount of preferably 0.1 to 20 parts by weight, and more preferably 0.5 to 15.0 parts by weight, per 100 parts by weight of the inorganic fibers. The inorganic binder is preferably added in an amount of 0.1 to 15.0 parts by weight, and more preferably 0.5 to 10 parts by weight, per 100 parts by weight of the inorganic fibers in the produced paper mat. Since the preferred types of organic binders and inorganic binders have already been described, the description thereof will be omitted here.
[0069] (2) Papermaking process Next, the slurry is poured into a molding machine having a filtering mesh formed on the bottom surface thereof, and the solvent in the slurry is removed to obtain an inorganic fiber aggregate, which is then dehydrated and dried.
[0070] In the papermaking process, the inorganic fiber aggregate may be dried by heating and pressing. During the heating and pressing, a heat treatment may be performed in which hot air is passed through the inorganic fiber aggregate to dry it, or the inorganic fiber aggregate may be left in a wet state without being subjected to a heat treatment. When heat treatment is performed, the heating temperature or hot air temperature is preferably 100 to 250°C to prevent deterioration of the organic binder due to heat. In the range of 100 to 250°C, moisture can be removed from the inorganic fiber aggregate while suppressing deterioration of the organic binder. If the heating temperature or hot air temperature is less than 100°C, the temperature does not reach the center of the inorganic fiber aggregate, and the drying time becomes long. Furthermore, if it exceeds 250°C, the organic binder is deteriorated and the binding force between the fibers is reduced, making it difficult to control the thickness of the inorganic fiber aggregate.
[0071] Through the above steps, the papermaking mat of the present invention can be manufactured. In addition, since no new fiber bundles are generated in the papermaking process, the obtained papermaking mat is opened by the above-mentioned papermaking mat opening method to obtain a slurry containing inorganic fibers. The bulk density in water of the inorganic fibers contained in the slurry is 0.012 to 0.035 g / cm. 3 It becomes.
[0072] In the method for producing a papermaking mat of the present invention, it is preferable to carry out batch papermaking or continuous papermaking in the papermaking step. The sheet mat of the present invention can be easily obtained by batch or continuous sheet making.
[0073] Next, a method for using the papermaking mat of the present invention will be described. FIG. 3 is a cross-sectional view that illustrates an example of an exhaust gas purification device of the present invention. 3, the exhaust gas purification device 100 includes a metal casing 30, an exhaust gas treatment body 40 housed in the metal casing 30, and a paper mat 10 disposed between the exhaust gas treatment body 40 and the metal casing 30. The paper mat 10 is the paper mat of the present invention. The exhaust gas treatment body 40 is a columnar structure in which a large number of cells 41 are arranged in parallel in the longitudinal direction with cell walls 42 separating them. Note that, to the ends of the metal casing 30, an inlet pipe for introducing exhaust gas discharged from the internal combustion engine and an outlet pipe for discharging exhaust gas that has passed through the exhaust gas purification device to the outside are connected as necessary. In the exhaust gas purification device 100 shown in FIG. 3, an exhaust gas filter (honeycomb filter) in which one of the cells is sealed with a plugging material 43 is used as the exhaust gas treatment body 40, but a catalyst carrier in which none of the end faces are sealed with a plugging material may also be used.
[0074] As shown in Fig. 3, exhaust gas discharged from an internal combustion engine and flowing into the exhaust gas purification device 100 (in Fig. 3, the exhaust gas is indicated by G, and the flow of the exhaust gas is indicated by arrows) flows into one cell 41 opening at an exhaust gas inlet end face 40a of the exhaust gas treatment body (honeycomb filter) 40, and passes through a cell wall 42 separating the cells 41. At this time, PM in the exhaust gas is captured by the cell wall 42, and the exhaust gas is purified. The purified exhaust gas flows out from another cell 41 opening at an exhaust gas outlet end face 40b, and is discharged to the outside.
[0075] As described above, the surface pressure of the papermaking mat 10 is high. Therefore, in the exhaust gas purification device 100, even if the exhaust gas treatment body 40 is subjected to high pressure from the exhaust gas, the exhaust gas treatment body 40 can be prevented from falling off the metal casing 30.
[0076] The exhaust gas treatment body 40 may be made of a non-oxidizing porous ceramic such as silicon carbide or silicon nitride, or may be made of an oxidizing porous ceramic such as sialon, alumina, cordierite, mullite, etc. Among these, silicon carbide is preferable.
[0077] When the exhaust gas treatment body 40 is made of porous ceramics made of silicon carbide, the porosity of the porous ceramics is not particularly limited, but is preferably 35 to 60%. If the porosity is less than 35%, the exhaust gas treatment body may easily become clogged, whereas if the porosity is more than 60%, the strength of the exhaust gas treatment body may decrease and the body may easily be destroyed.
[0078] The average pore size of the porous ceramic is preferably 5 to 30 μm. If the average pore size is less than 5 μm, PM may easily cause clogging. If the average pore diameter exceeds 30 μm, PM may pass through the pores, making it impossible to capture PM and thus unable to function as a filter. The porosity and pore size can be measured by a conventionally known method using a scanning electron microscope (SEM).
[0079] The cell density in the cross section of the exhaust gas treatment body 40 is not particularly limited, but the preferred lower limit is 31.0 cells / cm 2 (200 pieces / inch 2 ), the preferred upper limit is 93.0 particles / cm 2 (600 pieces / inch 2 ) A more preferable lower limit is 38.8 particles / cm 2 (250 pieces / inch 2 ), and a more preferable upper limit is 77.5 particles / cm 2 (500 pieces / inch 2 ).
[0080] The exhaust gas treatment body 40 may support a catalyst for purifying the exhaust gas. The catalyst to be supported is preferably a precious metal such as platinum, palladium, or rhodium, and among these, platinum is more preferable. In addition, other catalysts such as alkali metals such as potassium or sodium, or alkaline earth metals such as barium may also be used. These catalysts may be used alone or in combination of two or more kinds. When these catalysts are supported, PM can be easily burned and removed, and toxic exhaust gas can also be purified.
[0081] (Metal casing) The metal casing 30 is generally cylindrical. The inner diameter of the metal casing 30 (the inner diameter of the portion that houses the exhaust gas treatment body) is preferably slightly shorter than the diameter of the exhaust gas treatment body 40 around which the papermaking mat 10 is wrapped.
[0082] The metal casing 30 is preferably made of, but not limited to, stainless steel. EXAMPLES
[0083] EXAMPLES Hereinafter, examples that more specifically disclose the present invention will be described, however, the present invention is not limited to these examples.
[0084] Example 1 It is made of alumina-silica fibers with a weight ratio of Al2O3:SiO2 = 72:28, and has a bulk density of 0.17 g / mm 3 The density of needle marks is 21 / cm 2 A first inorganic fiber molding derived from a needle mat having a density of 1000 g / m2 was prepared. It is made of alumina-silica fibers with a weight ratio of Al2O3:SiO2 = 72:28, and has a bulk density of 1.2 g / mm 3 A second inorganic fiber molded body derived from a papermaking mat was prepared.
[0085] Next, the first inorganic fiber molded body and the second inorganic fiber molded body were fired at 800° C. for 1 hour to thermally decompose the organic binder contained in the first inorganic fiber molded body and the second inorganic fiber molded body.
[0086] Next, the fired first inorganic fiber molded body and second inorganic fiber molded body were left to stand until they reached room temperature, and then the first inorganic fiber molded body and second inorganic fiber molded body were loosened by hand.
[0087] Next, 5.0 g of the first inorganic fiber molded body and 5.0 g of the second inorganic fiber molded body were taken out and placed in 0.4 L of water. After that, the mixture was stirred at a rotation speed of 1000 rpm for a stirring time of 10 minutes using a stirrer (product name: SMT-101, manufacturer: ASONE) to open the fibers, thereby producing an inorganic fiber slurry.
[0088] In addition, in order to confirm whether fiber bundles were formed in the slurry, a portion of the slurry was taken out and dried, and it was confirmed that fiber bundles were formed in which 10 or more inorganic fibers were twisted and entangled.
[0089] Next, an organic binder was added to the slurry in an amount of 0.5 to 10 parts by weight relative to 100 parts by weight of the inorganic fibers. Further, an inorganic binder was added to the slurry in an amount of 0.3 to 3.0 parts by weight per 100 parts by weight of the inorganic fibers.
[0090] Next, the slurry was poured into a molding machine with a filtering mesh formed on the bottom surface, and the solvent in the slurry was removed to obtain an inorganic fiber aggregate. The inorganic fiber aggregate was then dehydrated and dried at 150 to 210°C for 5 minutes to 1 hour to produce a paper mat according to Example 1. The thickness of the paper mat according to Example 1 was 13 mm.
[0091] Comparative Example 1 A papermaking mat according to Comparative Example 1 was produced in the same manner as in Example, except that the first inorganic fiber molded body and the second inorganic fiber molded body were sufficiently loosened by hand without using a stirrer. The thickness of the papermaking mat in Comparative Example 1 was 12.9 mm.
[0092] (Measurement of bulk density in water) The papermaking mats according to Example 1 and Comparative Example 1 were heat treated at 600° C. for 1 hour. Then, 5.0 g of fiber was measured out while loosening it, and the fiber was placed in a container containing 400 cc of water. After stirring at 1000 rpm for 10 minutes, the mixture was transferred to a measuring cylinder and water was added to bring the total volume to 500 cc. After leaving it to stand for 30 minutes, the height of the settled fibers was read and the bulk density in water was calculated using the following formula (1). The results are shown in Table 1. Underwater bulk density (g / cm 3 ) = 5.0 (g) / Sedimentation volume of fiber (cm 3 ) · · · (1)
[0093] [Table 1]
[0094] (Observation of fiber bundles) From the paper mats according to Example 1 and Comparative Example 1, 3 A test piece was cut out. The test pieces were then fired at 600°C for 1 hour to thermally decompose the binder components. Next, the test piece was placed in a container, and the container was vibrated up and down and left and right to loosen the inorganic fibers that constituted the test piece. A fiber bundle formed by twisting and intertwining 10 or more inorganic fibers was taken out from the loosened test piece, and the length of the fiber bundle and the width of the inorganic fibers were measured. The same operation was repeated three times, and the average values of the fiber bundle length and fiber bundle width were calculated. The results are shown in Table 1.
[0095] (Measurement of surface pressure) The papermaking mats according to Example 1 and Comparative Example 1 were set in a testing machine (product name: SMT-101, manufacturer: ASONE) and the void bulk density (GBD) was 0.40 mm 3 The material was compressed at a rate of 25.4 mm / min until the void bulk density (GBD) was 0.40 mm 3 The mixture was kept at this temperature for 10 min. The contact pressure of each mat was then measured, and the results are shown in Table 1.
[0096] (Wrapping property evaluation) The papermaking mats of Example 1 and Comparative Example 1 were cut into rectangular pieces with a longitudinal length of 350 mm and a lateral length of 30 mm to prepare test pieces. In this case, the test pieces were cut so that the direction in which the slurry was poured into the molding machine during the papermaking process for producing the paper mat coincided with the longitudinal direction of the test pieces.
[0097] Next, a cylinder with a diameter of 100 mm was prepared, and each test piece was wound around the cylinder so that the longitudinal direction of each test piece coincided with the winding direction. Then, each test piece was visually observed to see if it had any cracks. The evaluation criteria were as follows. The results are shown in Table 1. A: No cracks were observed. ×: Cracks were observed.
[0098] As shown in Table 1, it was found that the papermaking mat of Example 1 had a high surface pressure and was less likely to crack even when wrapped around a substrate. [Explanation of symbols]
[0099] 10 Paper mat 11 One end 11a Convex part 12 The other end 12a Recess 20 Inorganic Fibers 21 Fiber bundle 21a Straight fiber bundle 21b Curly fiber bundle 22 Inorganic fibers not constituting fiber bundles 30 Metal Casing 40 Exhaust gas treatment body 40a Exhaust gas inlet end 40b Exhaust gas exhaust side end 41 Cell 42 Cell Wall 43 Encapsulating materials 100 Exhaust gas purification equipment
Claims
1. A paper mat made of inorganic fibers, The papermaking mat includes fiber bundles formed by twisting and intertwining 10 or more of the inorganic fibers, and the inorganic fibers that do not constitute the fiber bundles, The average length of the fiber bundles is greater than 5 mm; The paper mat is opened by the following paper mat opening method to obtain a slurry containing the inorganic fibers, and the inorganic fibers contained in the slurry have a bulk density in water of 0.012 to 0.035 g / cm 3 A paper-made mat characterized by: How to open a paper mat: The paper mat is heat treated at 600° C. for 1 hour. 5.0 g of fibers are weighed out from the papermaking mat while loosening it, and the fibers are placed in a container containing 400 cc of water. After stirring for 10 minutes at a stirrer speed of 1000 rpm, the mixture is transferred to a measuring cylinder and water is added so that the total volume becomes 500 cc. After leaving it to stand for 30 minutes, the height of the settled fibers is read and the bulk density in water is calculated using the following formula (1). Bulk density in water (g / cm 3 ) = 5.0 (g) / Sedimentation volume of fiber (cm 3 ) ... (1)
2. 2. The papermaking mat according to claim 1, comprising 0.1 to 20 parts by weight of an organic binder and 0.1 to 10 parts by weight of an inorganic binder, based on 100 parts by weight of the inorganic fibers.
3. The papermaking mat according to claim 2 , wherein the organic binder has a Tg of 5° C. or less.
4. The papermaking mat according to claim 2 or 3, wherein the organic binder is at least one selected from the group consisting of acrylic resin, acrylate-based latex, rubber-based latex, carboxymethyl cellulose, and polyvinyl alcohol, which function as water-soluble organic polymers, styrene resin, which functions as a thermoplastic resin, and epoxy resin, which functions as a thermosetting resin.
5. 4. The papermaking mat according to claim 2, wherein the inorganic binder contains at least one of alumina, silica, silicon carbide, zirconia, boron nitride, diamond, and pumice.
6. The fiber bundle is formed by intertwining 10 or more of the inorganic fibers, The fiber bundle formed by intertwining 10 or more inorganic fibers has an average length of more than 5 mm and 15 mm or less, 3. The paper mat according to claim 1, wherein the fiber bundle formed by intertwining 10 or more inorganic fibers has an average width of 0.2 to 1.0 mm.
7. The fiber bundle includes a crimped fiber bundle, 3. The paper mat according to claim 1 or 2, wherein the trace length of the fiber bundle in the crimped state, as measured by the following trace length measuring method, is at least 0.1 mm longer than the length of the fiber bundle in the crimped state. How to measure trace length: The crimped fiber bundle is placed on a flat surface. The fiber bundle in a crimped state that has been placed still is viewed from above, and a line is traced along the fiber bundle in a crimped state from one end of the fiber bundle to the other end, and the distance traced is defined as the "tracing length of the fiber bundle in a crimped state."
8. an opening step of opening an inorganic fiber molded body in which inorganic fibers are aggregated in water to prepare a slurry containing fiber bundles formed by intertwining 10 or more of the inorganic fibers in a twisted manner and the inorganic fibers that do not constitute the fiber bundles; A method for producing a paper mat, comprising: a papermaking step of papermaking the slurry to produce a paper mat, In the fiber-spreading step, the average length of the fiber bundle exceeds 5 mm, and the bulk density in water of the inorganic fibers contained in the slurry is 0.012 to 0.035 g / cm 3 The method for producing a paper mat is characterized in that the fibers are opened so that the fibers are formed as follows.
9. The method for producing a paper mat according to claim 8 , wherein the inorganic fiber molded body includes a first inorganic fiber molded body derived from a needle mat and / or a second inorganic fiber molded body derived from a paper mat.
Citation Information
Patent Citations
Sheet member, manufacturing method of the same, and exhaust gas processing device
JP2008082310A
Holding seal material and process of manufacture of holding seal material
JP2016089776A
Holding seal material, exhaust emission control device, and method of manufacturing holding seal material
JP2016108987A
Holding material for catalytic converter, method for manufacturing holding material for catalytic converter, catalytic converter and method for manufacturing catalytic converter
JP2017177005A
Matting, exhaust gas purification device, and method for manufacturing matting
JP2022156707A