Coated paper

A coated paper with a partially saponified polyvinyl alcohol barrier layer addresses the permeability and recyclability issues of existing materials, offering improved barriers and mechanical strength for packaging sensitive foods, suitable for heat or cold sealing.

JP2024147660AActive Publication Date: 2024-10-16KOEHLER INNOVATION & TECH GMBH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024111982
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-10-16
Filing Date
2024-07-11
Publication Date
2024-10-16
Estimated Expiration
2041-10-14

AI Technical Summary

Technical Problem

Existing paper-based packaging materials face challenges such as high permeability to polar compounds like water, limited recyclability, and mechanical weaknesses, especially when used for oxidation-sensitive and fatty foods, often requiring halogen-containing compounds that cause equipment issues and are not recyclable.

Method used

A coated paper with a base paper and a barrier layer comprising partially saponified polyvinyl alcohol or copolymers, having an onset temperature below 210°C, which allows for improved barriers against oxygen, grease, and mineral oil, and is recyclable, compatible with water-based cold seal adhesives, and suitable for heat or cold sealing.

Benefits of technology

The coated paper provides enhanced barriers, improved tear resistance, and recyclability while maintaining food quality and being compatible with sealing processes, without the need for halogen-containing compounds, thus addressing the limitations of existing materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024147660000001
    Figure 2024147660000001
  • Figure 2024147660000002
    Figure 2024147660000002
  • Figure 2024147660000003
    Figure 2024147660000003
Patent Text Reader

Abstract

To provide coated paper comprising base paper and a barrier layer coated to the base paper.SOLUTION: The present invention relates to coated paper in which a barrier layer includes at least one polymer, wherein the polymer includes at least partially saponified polyvinyl alcohol and / or at least partially saponified polyvinyl alcohol copolymer, wherein each of the polymers has an onset temperature of less than 210°C as determined by DSC, and wherein a precoat including at least one inorganic pigment and a polymer binder is applied to a surface of the base paper and exists between the base paper and the barrier layer.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to coated paper, to a method for making such coated paper, to the use of the coated paper as a packaging material, and to packages containing the coated paper. [Background technology]

[0002] The term "packaging" generally refers to the covering or (partial or complete) wrapping of an object, especially to protect or better handle the object. Consequently, packaging material includes materials that form such packaging.

[0003] The packaging material may be based on, for example, paper, plastic and / or metal.The present invention relates to a paper-based packaging material.

[0004] The main requirement of packaging materials of all origins is to protect the packaged product from external influences and to prevent leakage of the packaged product. For this purpose, packaging materials should meet different criteria depending on the packaged product and the packaging process. In addition to so-called barrier properties, for example against water, grease, oxygen or mineral oil, suitable packaging materials should also meet mechanical and process-specific requirements. Depending on the packaging system, packaging materials should have sufficient tear resistance, suitable friction values ​​(friction coefficients) and flexibility, be compatible with heat-sealable or cold-sealable adhesives, be printable from the outside and should not lose their protective effect during the entire conversion and packaging process.

[0005] Depending on its composition and areal density, paper can meet many mechanical requirements, but its physical properties as well as its porous structure require additional coatings to provide, for example, heat sealability or a barrier.

[0006] Known paper-based coated packaging materials often contain compounds such as polyvinylidene chloride (containing halogens) or are composites of paper with metal foils or plastic films, and often require improvement in tear strength, which can lead to running problems on packaging equipment, and / or cannot be reused due to too high coating content, adhesive components, or the formation of so-called sticky foreign bodies through the paper fiber flow.

[0007] Polyvinyl alcohol is widely known as a linear water-soluble biodegradable barrier coating, including for paper, where such coatings exhibit good barrier properties against oil, grease, oxygen, solvents and other non-polar gases, liquids or solids. However, due to its hydrophilic nature, polyvinyl alcohol is very permeable to polar compounds such as water. This can affect the barrier effect against non-polar migration, since polyvinyl alcohol is very good at absorbing moisture, swelling and thus creating molecular-level pathways through the barrier coating.

[0008] Many attempts have been made to achieve barrier degradation at relative humidities above 50 or 60%, for example by adding pigments as disclosed in WO 2010 / 129032, or by cross-linking polymer chains as disclosed in WO 2020 / 109401 or US Pat. No. 6,444,750. However, not only are these microscopic defects detrimental to the use of polyvinyl alcohol as a barrier, but the occurrence of macroscopic defects due to mechanical stresses, especially in packaging and converting systems, also limits the scope of use of polyvinyl alcohol.

[0009] Polyvinyl alcohol is understood to mean fully saponified polyvinyl acetate, which is usually a (thermoplastic) plastic material of the following formula (I) synthesized by free radical polymerization of vinyl acetate:

[0010] [ka]

[0011] The ester groups in polyvinyl acetate can be relatively easily subjected to alkaline saponification, which converts the polymer into polyvinyl alcohol, which becomes hydrophilic and water-sensitive.

[0012] Partially saponified polyvinyl acetate is also called partially saponified polyvinyl alcohol.

[0013] In the present invention, the term "partially saponified polyvinyl acetate" may be used synonymously with the term "partially saponified polyvinyl alcohol."

[0014] In this case, the degree of saponification indicates the proportion of ester groups that have been saponified and are present as -OH groups. For example, polyvinyl alcohol with a degree of saponification of 90% is a vinyl acetate polymer in which 90% of the originally existing ester groups have been saponified. Therefore, this polyvinyl alcohol contains 90% OH groups and 10% ester groups. With a degree of saponification of 100%, all the originally existing ester groups have been saponified, so only OH groups remain.

[0015] In addition to the pure homopolymers, many copolymers of polyvinyl alcohol are also of great technological importance. Copolymers are understood to mean all polymers which consist of the greatest proportion (more than 50%) of vinyl alcohol or vinyl acetate units, despite the different number of monomers used in their synthesis.

[0016] Such polyvinyl alcohol copolymers preferably include polyethylene vinyl alcohol.

[0017] In a narrower sense, saponification here refers to the hydrolysis of esters with aqueous solutions of hydroxides, such as sodium hydroxide, or with special enzymes (esterases). In contrast to acid ester hydrolysis (the reverse reaction of esterification), these are irreversible, since carboxylic acids lack the protons required for esterification. The reaction products formed are the salts of the alcohol and acid of which the ester was composed (carboxylation). In a broader sense, any hydrolysis of an ester can be called saponification. [Prior art documents] [Patent documents]

[0018] [Patent Document 1] International Publication No. 2010 / 129032 Brochure [Patent Document 2] International Publication No. 2020 / 109401 Brochure [Patent Document 3] U.S. Patent No. 6,444,750 Summary of the Invention [Problem to be solved by the invention]

[0019] The object of the present invention is to overcome the drawbacks of known materials and to provide a material suitable as a packaging material, especially for oxidation-sensitive and fatty foods, which can be used for the manufacture of packages such as tubular bags by heat-sealing or cold-sealing processes. Moreover, the material does not contain a barrier layer based on halogen-containing compounds. Furthermore, the material according to the present invention shall have one or more of the following properties compared to known packaging materials:

[0020] Improved oxygen barrier, improved grease barrier, improved mineral oil barrier, improved wrinkle resistance / flexibility, recyclability through waste paper cycle, improved heat seal properties,

[0021] It should have improved cold seal properties (compatibility with sealing media such as water-based cold seal adhesives), high tear resistance, no change in the taste of the packaged contents, aroma seal, and be printable on the outside. The material should also have an improved water vapor barrier, and the sealing seams should be as resistant to moisture as possible. The packaging material should also be suitable for metallization, especially in the micrometer and nanometer range, to further optimize the barrier properties if necessary. Finally, the material should be as economical to manufacture as possible. [Means for solving the problem]

[0022] This object is addressed by a coated paper according to claim 1, i.e. a coated paper comprising a base paper and a barrier layer applied to the base paper, characterized in that the barrier layer comprises at least one polymer, the polymer comprising an at least partially saponified polyvinyl alcohol and / or an at least partially saponified polyvinyl alcohol copolymer, each of which has an onset temperature determined by DSC of less than 210°C.

[0023] The onset temperature was determined by DSC as follows:

[0024] The (extrapolated) onset temperature (according to DIN EN ISO 11357-1:2010-03) is the intersection of the extrapolated baseline and the inflection tangent at the beginning of the melting or crystallization peak in a DSC measurement. The baseline and the inflection tangent are determined from the temperature-dependent heat flow signal. For pure, homogeneous materials, the initial temperature can be defined as the melting temperature. In contrast to the peak temperature, the onset temperature is less dependent on the heating rate and the sample mass. Furthermore, the onset temperature is often used for the temperature calibration of DSC.

[0025] The papers coated in this way are particularly suitable as packaging materials for oxidation-sensitive and fatty objects, especially food, and are particularly characterized in that they can be used to produce bags by heat or cold sealing, making it possible to use water-based cold seal adhesives for the cold sealing process. Moreover, the presence of a barrier layer based on a halogen-containing compound is not necessary.

[0026] Partially saponified polyvinyl alcohol has the advantage that the optimum sealing temperature is much lower in the heat sealing process than fully saponified polyvinyl alcohol (PVOH) or polyethylene vinyl alcohol (EVOH). The sealing seam strength is not adversely affected by this. Furthermore, partially saponified polyvinyl alcohol has a slightly lower viscosity, otherwise at the same concentration. In this case, the high viscosity is rather disadvantageous, since the PVOH solution needs to be diluted to a higher degree and therefore a larger amount of water has to be dried in the coating process. This is not only costly in terms of energy and therefore requires coating equipment with a higher drying capacity, but can also be difficult to realize in terms of application technology, depending on the desired coating weight. Furthermore, the diffusion of water molecules at high viscosity and therefore the drying process itself is slower. Furthermore, the accumulation of gaseous water in the coating is more likely, which can lead to the formation of macroscopic coating defects.

[0027] Thus, partially saponified polyvinyl alcohol or partially saponified polyvinyl alcohol copolymers, such as polyethylene vinyl alcohol, are preferred over the fully saponified variants.

[0028] The coated papers according to the invention are also characterized by improved oxygen barrier, improved grease barrier, improved mineral oil barrier and improved water vapor barrier.

[0029] The coated paper according to the invention also has improved crease resistance without compromising the barrier effect and is also characterized by high tear strength.

[0030] The coated paper according to the invention can also be recycled through the waste paper cycle.

[0031] When the coated paper according to the invention is used as a packaging material for food, it is particularly characterized in that it does not affect and / or change the taste of the packaged food.

[0032] The coated papers according to the invention are furthermore heat sealable, exhibit improved cold seal properties (compatible with sealing media such as water-based cold seal adhesives) and the sealed seams each have sufficient moisture resistance.

[0033] The coated paper according to the invention is also easy to print on the uncoated side (outside).

[0034] The coated paper according to the invention is also suitable for metallization in the micrometer and nanometer range in order to further optimize the barrier properties if required.

[0035] Finally, coated papers according to the invention can be produced relatively easily at low coating weights and can be recycled through the waste paper cycle. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0036] Hereinafter, the term "comprise" can also mean "consisting of".

[0037] The term "hydrophobic" refers to a material that cannot be mixed with water or can be wetted by water only with the use of a surfactant. The term "hydrophilic" refers to a material that can be mixed with water or can be wetted by water without the use of a surfactant. Hydrophobic polymers are also called non-polar polymers and hydrophilic polymers are also called polar polymers.

[0038] Hydrophobicity or hydrophilicity can be defined, for example, by the log P value. The n-octanol / water partition coefficient K ow (also commonly and accurately written as n-octanol / water partition coefficient) is a dimensionless partition coefficient known to those skilled in the art, which indicates the ratio of the concentration of a chemical in a two-phase system formed by n-octanol and water, and is therefore a measure of the hydrophobicity or hydrophilicity of a substance. The log P value is the n-octanol-water partition coefficient K ow is the decimal logarithm of , where the following holds:

[0039]

number

[0040] In the formula, c o Si = concentration of chemical in the octanol-rich phase, and

[0041] c w Si = concentration of chemical in the water-rich phase.

[0042] K ow is greater than 1 if a substance is more soluble in a fat-like solvent such as n-octanol, and less than 1 if it is more soluble in water. Thus, log P is positive for hydrophobic / lipophilic substances and negative for hydrophilic / lipophilic substances.

[0043] The low permeability of polyvinyl alcohols to oxygen, mineral oil, fats and other non-polar transporters is due to their relatively high hydrophilicity.

[0044] Furthermore, ethylene-containing polymers such as (saponified) polyethylene vinyl alcohol have lower water vapor permeability, which can be attributed to the ethylene content and the associated lower hydrophilicity.

[0045] The base paper used for the coated paper according to the invention is in principle not limited.

[0046] However, the base paper is 20 to 120 g / m 2 , preferably 40 to 100 g / m 2 It is preferred that the surface density of the substrate is 0.1 to 1.0 μm.

[0047] It is further preferred that the paper has a composition with a long fibre content of from 10 to 80% by weight, preferably from 20 to 50% by weight, and a short fibre content of from 20 to 90% by weight, preferably from 50 to 80% by weight.

[0048] Long fibres are understood to mean fibres having a fibre length of 2.6 to 4.4 mm, short fibres are understood to mean fibres having a fibre length of 0.7 to 2.2 mm.

[0049] It may further contain GCC (ground calcium carbonate), known for example under the trade name Hydrocarb 60 or Hydrolex 60, PCC (precipitated calcium carbonate), known for example under the trade name Precarb 105, natural kaolin and / or talc, 0% to 20%, preferably 0% to 5%, of fillers, the value 0% being preferably excluded, as well as the usual auxiliaries such as retention agents and / or sizing agents.

[0050] The advantages of such a base paper are, on the one hand, its high flexibility and, on the other hand, its good processability in existing packaging machines for flexible materials such as plastic material films, maintaining high machine availability and achieving the required puncture resistance.

[0051] Common packaging machines are vertical and horizontal form-fill-seal machines for producing e.g. stand-up pouches, flow packs, pillow packs etc., machines that join two webs of the same or different material and join them by heat sealing, e.g. tray sealers, chamber belt equipment (also using vacuum), bag fill seal machines, thermoforming packaging machines, linear filling machines that apply a lid by heat sealing to seal the package, packaging machines with a final heat sealing step, blister packaging machines and X-fold packaging machines.

[0052] The coated paper according to the invention is further preferably characterised in that a precoat comprising at least one inorganic pigment and a polymeric binder is present between the base paper and the barrier layer.

[0053] Inorganic pigments are preferably in the form of flakes and include in particular talc, precipitated calcium carbonates or silicates, preferably phyllosilicates, very particularly preferably kaolin.

[0054] Suitable polymer binders include, in particular, acrylate-based or styrene / butadiene-based binders. In principle, all polymers that can be used as binders for pigment coatings in the paper industry are suitable. Starch-based binders (solutions of modified starch, dispersions of crosslinked starch, so-called biolatexes) and polymer-starch hybrid latexes are also considered.

[0055] The polymer binder preferably comprises a polyacrylate-based polymer binder.

[0056] The precoat may be a generally hydrophobic precoat.

[0057] In another embodiment, the precoat is generally hydrophilic.

[0058] The precoat preferably contains 1-70% by weight of polymer binder, preferably 5-50% by weight, this amount relating to the dry precoat in the final product.

[0059] It is further preferred that the precoat comprises 50-95% by weight, preferably 80-90% by weight, of inorganic pigment, said amount relating to the dry precoat in the final product.

[0060] Additionally, the precoat may contain additives such as thickeners, e.g., acrylate-based thickeners, surfactants, and / or rheology modifiers. The use of crosslinking agents is also contemplated. Preferably, the precoat contains a zirconium-based crosslinking agent, itself crosslinked with formaldehyde.

[0061] Each of these additives is preferably present in an amount of 0 to 2% by weight, preferably greater than 0 to 2% by weight, the value 0% being preferably excluded. This amount relates to the dry precoat in the final product.

[0062] The amount of precoat applied is 1 to 10 g / m 2 is preferable, and 2 to 6 g / m 2 is especially preferred. This amount refers to the dry precoat in the final product.

[0063] When such a precoat (also called primer) is applied, this has the advantage that, for example, the paper surface is sealed and a further barrier layer coated thereon migrates only slightly into the paper, thus resulting in sufficient interlayer adhesion. Moreover, this precoat reduces the average roughness depth of the base paper, providing an advantageous "hold-out" characterized by an application covering the entire surface and a defined surface energy, so that the applied barrier layer can be optimally formed. Furthermore, the precoat mediates interlayer adhesion between the base paper and the barrier layer, which can be important for subsequent sealing applications.

[0064] The barrier layer applied to the precoat comprises at least partially saponified polyvinyl alcohol and / or at least partially saponified polyvinyl alcohol copolymer. The formulation used in the processing process preferably comprises the polymer in an amount of 10-100% by weight, particularly preferably 50-99.8% by weight.

[0065] The barrier layer may further contain additives such as thickeners, e.g., acrylate-based thickeners, surfactants, e.g., sulfosuccinates, extensional rheology aids, e.g., polyacrylamides, carboxymethylcellulose, polyvinyl alcohol, and / or crosslinkers, e.g., aldehydes and polyaldehydes, zirconates, polyepoxides, epichlorohydrin resins, and / or hydrazides.

[0066] Each of these additives is preferably contained in an amount of 0.1 to 1% by weight based on the total weight of the barrier layer.

[0067] In one embodiment, the coated paper according to the invention is further preferably characterized in that the at least partially saponified polyvinyl alcohol and / or the at least partially saponified polyvinyl alcohol copolymer has an average molecular weight of less than 100,000 g / mol.

[0068] In another embodiment, the coated paper according to the invention is further preferably characterized in that the at least partially saponified polyvinyl alcohol and / or the at least partially saponified polyvinyl alcohol copolymer has an average molecular weight of more than 30,000 g / mol, or more than 40,000 g / mol, or more than 50,000 g / mol, or more than 60,000 g / mol, or more than 70,000 g / mol.

[0069] In one embodiment, the coated paper according to the invention is further preferably characterized in that the at least partially saponified polyvinyl alcohol and / or the at least partially saponified polyvinyl alcohol copolymer has a degree of saponification between 30% and 100%.

[0070] In another embodiment, the coated paper according to the invention is further preferably characterized in that the at least partially saponified polyvinyl alcohol and / or the at least partially saponified polyvinyl alcohol copolymer has a degree of saponification of from 30% to less than 100%.

[0071] In another embodiment, the coated paper according to the invention is further preferably characterized in that the at least partially saponified polyvinyl alcohol and / or the at least partially saponified polyvinyl alcohol copolymer has a degree of saponification of less than 95% or between 30% and 95%.

[0072] In another embodiment, the coated paper according to the invention is further preferably characterized in that the at least partially saponified polyvinyl alcohol and / or the at least partially saponified polyvinyl alcohol copolymer has a degree of saponification of 95% to 100%.

[0073] In another embodiment, the coated paper according to the invention is further preferably characterized in that the at least partially saponified polyvinyl alcohol and / or the at least partially saponified polyvinyl alcohol copolymer has a degree of saponification of 95% to less than 100%.

[0074] In another embodiment, the coated paper according to the invention is further preferably characterized in that the at least partially saponified polyvinyl alcohol and / or the at least partially saponified polyvinyl alcohol copolymer has an onset temperature, determined by DSC, of ​​less than 200°C.

[0075] The coated paper according to the present invention is further preferably characterized in that the at least one polymer comprises a partially saponified polyvinyl alcohol having a degree of saponification less than 95% or between 30% and 95%, an average molecular weight between 0 and less than 100,000 g / mol, and an onset temperature determined by DSC less than 200°C.

[0076] In another embodiment, the coated paper according to the invention is further preferably characterized in that the at least one polymer comprises a partially saponified polyvinyl alcohol having a degree of saponification between 95% and 100%, an average molecular weight of more than 70,000 g / mol and an onset temperature determined by DSC of less than 200° C.

[0077] In another embodiment, the coated paper according to the invention is further preferably characterized in that at least one polymer is a partially saponified polyvinyl alcohol copolymer, preferably a partially saponified polyethylene vinyl alcohol, having a degree of saponification between 95% and 100%, an average molecular weight of more than 60,000 g / mol and an onset temperature determined by DSC of less than 210° C.

[0078] Partially saponified polyvinyl alcohol copolymers, such as polyethylene vinyl alcohol, have generally been shown to be more flexible than polyvinyl alcohol.

[0079] In another embodiment, the coated paper according to the invention is preferably characterized in that at least one polymer is a mixture of partially saponified polyvinyl alcohol with a degree of saponification of 1% to 95%, an average molecular weight between 0 and less than 100,000 g / mol and an onset temperature below 200° C., determined by DSC, partially saponified polyvinyl alcohol with a degree of saponification of 95% to 100%, an average molecular weight above 70,000 g / mol and an onset temperature below 200° C., and / or partially saponified polyvinyl alcohol copolymers, preferably partially saponified polyethylene vinyl alcohols, with a degree of saponification of 95% to 100%, an average molecular weight above 60,000 g / mol and an onset temperature below 210° C., determined by DSC.

[0080] The degree of saponification was determined according to DIN EN ISO 3681 as follows:

[0081] PVOH (1 g) is mixed with distilled water (70 mL) and neutralized ethanol (30 mL) and heated under reflux until complete dissolution. After cooling, the solution is neutralized with potassium hydroxide solution (0.1 M). In the case of partially saponified PVOH types, additional potassium hydroxide solution (50 mL, 0.1 M) is added and heated under reflux (60 min). In the case of fully saponified PVOH types, a smaller amount of potassium hydroxide solution (25 mL, 0.1 M) is additionally used to prevent the absorption of carbon dioxide under excess potassium and also to reduce the reflux time (30 min). The excess potassium is then back-titrated with hydrochloric acid (0.1 M) using phenolphthalein as an indicator. A blind test is carried out in parallel.

[0082] The degree of saponification (%) is calculated according to the following formula:

[0083]

number

[0084] The ester number can be calculated according to Equation 2:

[0085]

number

[0086] Request according to.

[0087] The average molecular weight was determined by size exclusion chromatography (GPC) under the following conditions:

[0088] Eluent: DMSO / +0.1M LiCl; Precolumn: 10μm, Guard, id 8.00mm x 50.00mm; Column: 10μm, 30Å, id 8.00mm x 300.00mm; 10μm, 3000Å, id 8.00mm x 300.00mm; 10μm, 3000Å, id 8.00mm x 300.00mm; Pump: 1260 HPLC pump; Flow rate: 1.0mL / min; Injector: 1260 Autosampler; Injection volume: 200μL; Sample concentration: 5.0g / L; Temperature: 80℃; Detector: SECcurity 2Refractive index detector (RI) - WEG eta 1001 HT viscometer; Calculation: WinGPC UniChrom version 8.33

[0089] The samples were dissolved in the solvent (5 mg / mL) at a temperature of 80° C. for 3 h and injected by an autosampler.

[0090] To obtain the calibration curve, several PMMA standards with different molecular weights were measured and the calibration curve was converted to a universal calibration curve by measuring the intrinsic viscosity.

[0091] The coated paper according to the invention is further preferably characterized in that the polyvinyl alcohol dry content of 4% has a viscosity of less than 30 mPa·s or less than 20 mPa·s, particularly preferably less than 15 mPa·s.

[0092] Viscosity is determined at 23°C using a Brookfield viscometer at 100 rpm.

[0093] This range of viscosity has the advantage that a higher solids content can be used for application and therefore less energy needs to be used for drying. Furthermore, higher process speeds can be achieved. In addition to the economic advantages, this is also reflected in the use of a larger drying window in the coating equipment.

[0094] The coated paper according to the invention preferably has a breaking strength in the running direction of more than 80 N 15 mm, preferably more than 90 N 15 mm, and transversely to the running direction of the paper of more than 40 N 15 mm, preferably more than 50 N 15 mm.

[0095] The coated paper according to the invention further preferably has a dynamic coefficient of friction of less than 0.7, preferably less than 0.6, particularly preferably less than 0.5, which refers to the friction of coated side against coated side (coating against coating).

[0096] The coated paper according to the present invention further preferably has a coating density of the barrier layer of 5 to 20 g / m2 for the dried final product (air-dried). 2 , preferably 8 to 12 g / m 2 It is characterized in that:

[0097] The coated paper according to the invention is further preferably characterized in that the barrier layer is wettable by common water-based cold seal adhesives. For this purpose, the surface energy of the barrier coating is more than 40 mN / m, preferably more than 50 mN / m, particularly preferably more than 55 mN / m.

[0098] Such wettability of the barrier layer has the advantage that no uncoated areas are formed during the application and drying process of the cold seal adhesive, and also provides sufficient adhesion for application.

[0099] The coated paper according to the present invention is more preferably 10 cm 3 / m 2 / d, preferably less than 5cm 3 / m 2 / d (at 23°C and 0% relative humidity).

[0100] The coated paper according to the present invention is more preferably 10 cm 3 / m 2 / d, preferably less than 5cm 3 / m 2 / d (at 23°C and 50% relative humidity).

[0101] The coated paper according to the present invention is more preferably 20 cm 3 / m 2 / d, preferably less than 10cm 3 / m 2 / d (at 23°C and relative humidity 70%).

[0102] The coated paper according to the present invention is more preferably 25 g / m 2 / d, preferably less than 15 g / m 2 / d (at 23°C and relative humidity 80%).

[0103] Oxygen transmission rate (or oxygen transmission rate - OTR) is determined according to ISO 15105-2.

[0104] The coated paper according to the invention is further preferably characterized in that it has a grease barrier corresponding to test condition I according to DIN 53116.

[0105] The coated paper according to the invention also does not lose this grease barrier due to the mechanical stress of a 180° fold, preferably by a roller applying a load of 330 g / cm to the resulting fold, the coating being either on the inside (inner fold) or on the outside (outer fold).

[0106] The coated paper according to the present invention is more preferably 10 g / m 2 / d of mineral oil barrier (hexane).

[0107] The mineral oil barrier is determined by pouring hexane into a beaker (solvent resistant), sealing with coated paper, and following the weight loss over time.

[0108] The coated paper according to the invention is further preferably characterised in that the coated paper has a water vapour barrier, which is maintained even when the coating comes into contact with grease, although this is not the case for all water vapour barriers.

[0109] The coated paper according to the invention is further preferably characterised by being crease-resistant in the uncreased state, on the inside crease and on the outside crease.

[0110] The coated paper according to the invention is characterised by its recyclability through the waste paper cycle.

[0111] The coated paper according to the invention is heat sealable and at the optimum sealing temperature preferably gives a sealing seam strength of more than 3.5 N / 15 mm, particularly preferably more than 5.0 N / 15 mm, the sealing seam strength of the coated paper being determined as follows:

[0112] The coated papers were sealed transversely to the running direction of the paper at 3.3 bar for 0.3 s in the temperature range 100°C–230°C, and the sealing seam strength was determined according to DIN 55529 (2012).

[0113] The term "heat sealing" is preferably understood to mean joining two layers of coated paper by localized heat input and / or pressure. In a further embodiment, the coated side of the paper can also be joined by heat sealing to the opposite side of a paper that is not itself heat-sealable, or to another paper.

[0114] Furthermore, the coated paper according to the invention is also cold-sealable due to its compatibility with common cold-seal media. Cold-sealing is generally understood to mean that a cold-seal adhesive is applied to a portion of a flat packaging material that is sealed by a pressure-based process. Cold-seal adhesives have the property that they only develop an adhesive effect under increased pressure between the sealing jaws of a packaging machine, otherwise they have no or limited tack.

[0115] Both heat seal and cold seal papers are characterized by high moisture resistance of the sealing seam.

[0116] The coated paper according to the present invention is also tear resistant.

[0117] The coated paper according to the invention is further characterized in that the taste of food packaged therein is not affected.

[0118] The coated paper according to the invention is characterized by the presence of nanometer-range particles, e.g. Al 2 O 3 Alternatively, it can be metallized with Al.

[0119] The coated paper according to the invention is further preferably characterised in that a further layer comprising a metal, in particular aluminium, and / or a metal oxide, in particular aluminium oxide and / or silicon oxide, is applied to the barrier layer.

[0120] Coated papers according to the invention can be obtained economically using known manufacturing methods.

[0121] However, the coated paper according to the invention is preferably obtained by a process in which an aqueous suspension comprising the starting materials for the barrier layer is applied to the base paper, the aqueous application suspension having a solids content of 5 to 50% by weight, preferably 10 to 30% by weight, and is applied by a curtain coating process, preferably a double curtain coating process, at an operating speed of the coating installation of at least 200 m / min.

[0122] This method is particularly advantageous from an economic standpoint and for uniform application to the paper web.

[0123] Solids values ​​below about 10% by weight lead to poor economic efficiency, since large amounts of water must be removed by short, gentle drying, which has a negative effect on the coating speed, whereas values ​​above 50% by weight only increase the technical effort to ensure the stability of the coating curtain material during the coating process and drying of the applied film, since in this case the machine must be operated very quickly again.

[0124] In the curtain coating process, a free-falling curtain of coating dispersion is formed. The coating dispersion in the form of a thin film (curtain) is applied to the substrate by "pouring" it by free fall onto the substrate. Document DE 10196052 T1 discloses the use of the curtain coating process in the production of information recording materials, whereby a multi-layer recording layer is realized by applying a curtain of multiple coating dispersion films to the substrate.

[0125] In a preferred embodiment of the method according to the invention, the aqueous degassed coating suspension has a viscosity of about 100 to about 800 mPa·s (Brookfield, 100 rpm, 20° C.). If the viscosity is below a value of about 100 mPa·s or above a value of about 800 mPa·s, the coating composition is difficult to pass through the coating unit. Particularly preferably, the viscosity of the aqueous degassed coating suspension is about 200 to about 500 mPa·s.

[0126] In a preferred embodiment, the surface tension of the aqueous coating suspension can be adjusted to about 25 to about 70 mN / m, preferably about 35 to about 60 mN / m (measured according to the standard for bubble pressure tensiometry (ASTM D 3825-90) as described below) in order to optimize the process. Better control over the coating process can be obtained by determining the dynamic surface tension of the coating material and adjusting the dynamic surface tension in a targeted manner by selecting an appropriate surfactant and by determining the amount of surfactant required.

[0127] Polyvinyl alcohol solutions have been shown to require significantly less surfactant to produce the same surface tension compared to dispersions, especially those with smaller particle sizes and therefore larger particle surface areas.

[0128] Dynamic surface tension is measured by a bubble pressure tensiometer. The maximum internal pressure of a bubble formed in a liquid through a capillary is measured. The internal pressure p (Laplace pressure) of a spherical bubble depends on the radius of curvature r and the surface tension σ according to the Young-Laplace equation:

[0129]

number

[0130] When a bubble is generated at the tip of a capillary in a liquid, the curvature first increases and then decreases again, resulting in a maximum pressure. The maximum curvature, and therefore the maximum pressure, occurs when the radius of curvature is equal to the radius of the capillary.

[0131] Pressure curve during bubble pressure measurement, position of pressure maximum:

[0132] The radius of the capillary is determined by a reference measurement made with a liquid of known surface tension, usually water. So, with the radius known, the surface tension can be calculated from the maximum pressure pmax. Since the capillary is immersed in the liquid, the hydrostatic pressure p0 resulting from the immersion depth and density of the liquid must be subtracted from the measured pressure (this is done automatically in the case of modern measuring equipment). This gives the following equation for the bubble pressure method:

[0133]

number

[0134] The measurements correspond to the surface tension at a given surface lifetime, which is the time from the onset of bubble formation to the occurrence of maximum pressure. By varying the rate at which bubbles form, the dependence of surface tension on surface lifetime can be recorded, resulting in a curve in which surface tension is plotted against time.

[0135] This dependence plays an important role in the use of surfactants, since in many processes the interfacial tension never reaches the equilibrium value, due to the sometimes low diffusion and adsorption rates of the surfactants.

[0136] The individual coatings can be applied in separate coating processes either on-line at the paper machine equipped with a coating unit or off-line at the coating machine.

[0137] In a further embodiment, the individual layers can be applied to the base paper using the following method.

[0138] The barrier layer can be applied to the base paper and / or existing precoat by a printing method.

[0139] The barrier layer can be applied to the base paper and / or an existing precoat by extrusion.

[0140] This technique has the advantage that significantly more material can be applied, which is only important if the entire product does not need to be recyclable as paper, while the disadvantages are lower application speeds, higher energy consumption and higher minimum application weights.

[0141] The barrier layer may be applied, for example, by laminating the paper in the form of a plastic material film applied to the base paper and / or an existing precoat.

[0142] The barrier layer and precoat may also be applied sequentially over multiple application steps.

[0143] The present invention further relates to a coated paper obtainable by the above process.

[0144] Due to its relatively high polarity, the barrier layer is also suitable for applying a further barrier in the form of an aqueous polymer solution or dispersion by melt extrusion or lamination with the film.

[0145] The barrier layer can be improved, if necessary, for all barriers, by applying an ultra-thin metal layer, metal oxide layer, or other inorganic compound by deposition or especially vacuum deposition. Such thin barrier layers are only effective if they do not contain particles (e.g. inorganic pigments) and are adhered to very smooth and flexible substrates on which a closed layer can be formed. The relatively high surface energy of the barrier layer, especially the surface energy of generic polymers, favors the adhesion of layers of polar materials such as metal oxides and other inorganic oxides, as well as polarizable conductive materials such as metals. The paper thus obtained can then be made sealable by applying a heat seal layer or a cold seal adhesive.

[0146] The present invention also relates to the use of a coated paper as described above or obtainable by the process described above as packaging material.

[0147] Finally, the invention also relates to the use of a coated paper as described above or obtainable by the process described above, as packaging material for food products, in particular fatty and oxidation-sensitive food products.

[0148] The present invention further preferably relates to the use of a coated paper as described above, or obtainable by the process described above, as packaging material for, for example, cereal bars, chocolate, chocolate-containing products, or potato chips.

[0149] In a further preferred embodiment of the invention, the coated paper according to the invention is applied to cardboard or paperboard, in particular by lamination or bonding.

[0150] Finally, the invention also relates to the use of a composite in which the coated paper according to the invention is applied, in particular by lamination or bonding, to cardboard or paperboard as packaging material for food, in particular for fatty and oxidation-sensitive food.

[0151] In this way, packaging materials having the advantages of both material components, for example the increased strength and stiffness of cardboard or paperboard compared to coated paper, as well as the described advantages of coated paper, can be produced in a simple and economical manner. Application can be carried out, for example, using starch or aqueous dispersion adhesives.

[0152] Thus, the coated paper may preferably be a component of a packaging material based on cardboard or paperboard.

[0153] These packaging materials according to the invention allow heavier food products to be packaged particularly safely and attractively presented to customers in upright packaging at retail outlets.

[0154] These packaging materials preferably have a mass fraction of homogeneous material type paper, cardboard or paperboard of more than 95%. A further advantage of the present invention here is that these packaging materials according to the invention are not composite packaging according to § 3(5) of the German Packaging Act, so that this embodiment of the present invention contributes significantly to reducing the environmental impact of packaging waste.

[0155] The present invention also relates to packaging comprising the coated paper as described above or in a composite with cardboard or paperboard as described above.

[0156] The features of the use according to the invention apply analogously to the packaging according to the invention.

[0157] The packaging can be a cold seal packaging. Cold seal packaging is preferably suitable for packaging foodstuffs such as chocolate, chocolate-containing products, bars, e.g. cereal bars and / or other confectionery products. This is due to the heat sensitivity of chocolate and the possible higher machine speeds. Packaging machines based on cold sealing can be operated faster, since it takes a relatively long time to heat the heat-sealing medium.

[0158] The packaging can also be a heat-sealed packaging, preferably suitable for use as secondary packaging or packaging for containers on a dosing and filling scale.

[0159] The packaging may also be a cold seal packaging.

[0160] The packaging may further be a form-fill-seal packaging, in particular a cold sealed or cold sealed form-fill-seal packaging.

[0161] The invention will now be explained in more detail with reference to the following non-limiting examples. EXAMPLES

[0162] The following coatings were applied to 60g / m2 with 40% long fibre content and 60% short fibre content.2 It was applied to the base paper.

[0163] Precoat / Primer:

[0164] The precoat contains 75.9% pigment (phyllosilicate), 22.8% latex (styrene-butadiene latex) and 1.3% rheology modifiers (0.2% acrylate thickener, 1.1% zirconium crosslinker).

[0165] Barrier Layer:

[0166] Polyvinyl alcohol was used in Examples 1 to 5 and Comparative Example 1. Polyethylene vinyl alcohol was used in Examples 6 and 7.

[0167] The barrier layers of Examples 1-7 and Comparative Example 1 comprise a pure polymer coating. Example 1' comprises 99.8% polyvinyl alcohol (Example 1; saponification degree: 87%; M w :50900) and a polymer coating containing 0.2% rheology modifier (Na-docusate).

[0168] For this purpose, a blade was used to apply the precoat. The barrier layers of Examples 1 to 7 and Comparative Example 1 were applied with a doctor blade. In contrast to Example 1, the barrier layer of Example 1' was applied with a curtain coater.

[0169] The following properties were investigated:

[0170] Coating weight: Barrier coating application weight (g / m 2 ), which is determined by the weight difference between coated and uncoated paper.

[0171] Viscosity: The viscosity was measured using a Brookfield viscometer at 23° C. and a speed of 100 rpm at a dry content of 4%.

[0172] WVTR: Water vapor transmission rate determined according to ISO 15106-2.

[0173] OTR: Oxygen transmission rate according to DIN 15105-2

[0174] HVTR: Hexane Vapor Transmission Rate, where n-hexane is filled into a beaker (solvent resistant), sealed with the test sample and the weight loss is monitored over time. For creased samples, a 180° crease is generated with a roller that applies a load of 330 g / cm to the resulting crease, and the coating can be placed on the inside (inner crease) or outside (outer crease).

[0175] Palm kernel oil test: similar to DIN 53116. For creased samples, a 180° crease is created using a roller that applies a load of 330 g / cm to the resulting crease; the crease can be positioned on the inside (inner crease) or outside (outer crease).

[0176] Indicator paper: Evaluation of indicator paper as described in DIN 53116, where grease penetration points with a diameter (d) > / < 1 mm are counted.

[0177] Sample paper: Evaluation of the reverse side of the sample paper as described in DIN 53116. This is not part of the standard but was done to improve differentiation.

[0178] Sealing seam strength: The samples are sealed crosswise to the running direction of the paper at 3.3 bar for 0.3 seconds in the temperature range 100°C to 220°C and the sealing seam strength is determined according to DIN 55529 (2012). The optimum sealing temperature and, for comparison, the sealing force at 150°C (optimum sealing temperature of Example 1) are recorded.

[0179] DSC melting temperature / onset: DSC curves were measured with a Mettler DSC 20 S in cold welded aluminium crucibles and perforated lids. The heating rate was 10 K / min in the range 30° C.-280° C. The melting temperature was determined by the peak-minimum of the melting process.

[0180] Surface tension or energy Contact angle measuring device OCA 20 (DataPhysics) and software SCA 20

[0181] Measurement principle: OWRK method (Owens, Wendt, Rabel, Kaelble)

[0182] The test solution used and the starting material constants were entered:

[0183] Water and diiodomethane (according to Buscher) and 1,5-pentanediol (according to Gebhardt)

[0184] The resulting coated papers were examined and the results are shown in the table below.

[0185] [Table 1]

[0186] The partially saponified polyvinyl alcohol used has very low hexane and oxygen permeabilities, probably due to its relatively high hydrophilicity.

[0187] Polyvinyl alcohols with a higher degree of saponification are characterized in coating materials by a higher viscosity at the same dry content. From a chemical point of view, this only makes sense because, due to their higher polarity, each molecule interacts more strongly with the surrounding solvent (water).

[0188] This is a significant disadvantage, because a large amount of water must be dried at a low dry content in the coating process. This is not only costly in terms of energy, but also can be difficult to achieve in terms of application technology, depending on the desired coating weight. Furthermore, the diffusion of water molecules, and therefore the drying itself, is slowed down. Furthermore, this can lead to the accumulation of gaseous water in the coating, which can lead to the formation of macroscopic coating defects.

[0189] The water vapor permeability of the polyethylene vinyl alcohol investigated was lower than that of polyvinyl alcohol, presumably due to the ethylene content and associated lower hydrophilicity.

[0190] In general, fully saponified PVOH should be weaker than partially saponified PVOH due to the greater number of hydrogen bonds that can be formed. The same is true for Comparative Example 1 (see palm kernel oil test).

[0191] This has not yet been demonstrated in Example 2. The reason for this is believed to be the high molecular weight. It has already been shown for polyvinyl alcohol fibers that different molecular weights of otherwise identical polyvinyl alcohols have a significant effect on their physical properties (e.g. Gotoh et al., Polymer Journal, vol. 32, no. 12 (2000), pp. 1049-1051: "Molecular Weight Dependence of Tensile Properties in Poly(vinyl alcohol) Fibers"). For example, the breaking elongation of higher weight polyvinyl alcohol is lower, but the force required for this is many times higher.

Claims

1. 1. A coated paper comprising a base paper and a barrier layer applied to the base paper, wherein the barrier layer comprises at least one polymer, wherein the polymer comprises an at least partially saponified polyvinyl alcohol and / or an at least partially saponified polyvinyl alcohol copolymer, each of which has an onset temperature determined by DSC of less than 210°C, the onset temperature being defined by DSC according to DIN EN ISO 11357-1:2010-03 as the intersection of an extrapolated baseline and an inflection tangent at the onset of a melting or crystallization peak, a precoat comprising at least one inorganic pigment and a polymer binder is applied to a surface of the base paper and is present between the base paper and the barrier layer; A coated paper characterized by:

2. 2. The coated paper of claim 1, characterized in that the inorganic pigment is in the form of platelets and comprises talc, precipitated calcium carbonate or silicate, and / or the polymer binder comprises a polyacrylate-based polymer binder.

3. 3. The coated paper according to claim 1 or 2, characterized in that the at least one polymer comprises a partially saponified polyvinyl alcohol having a degree of saponification between 30% and 95%, an average molecular weight between >0 and <100,000 g / mol, and an onset temperature determined by DSC below 200°C.

4. 4. Coated paper according to any one of claims 1 to 3, characterized in that the at least one polymer comprises a partially saponified polyvinyl alcohol having a degree of saponification of more than 95% to 100%, an average molecular weight of more than 70,000 g / mol and an onset temperature determined by DSC of less than 200°C.

5. 5. Coated paper according to any one of claims 1 to 4, characterized in that the at least one polymer is a partially saponified polyvinyl alcohol copolymer having a degree of saponification between 95% and 100%, an average molecular weight of more than 60,000 g / mol and an onset temperature, determined by DSC, of ​​less than 210°C.

6. 3. Coated paper according to claim 1 or claim 2, characterized in that the at least one polymer comprises a mixture of a polyvinyl alcohol according to claim 3, a polyvinyl alcohol according to claim 4 and a polyvinyl alcohol copolymer according to claim 5.

7. 7. Coated paper according to claim 1, characterized in that the partially saponified polyvinyl alcohol and / or the partially saponified polyvinyl alcohol copolymer with a dry content of 4% has a viscosity of less than 30 mPa.s.

8. The coating density of the barrier layer is 5 to 20 g / m2 for the dried final product (air-dried). 2 The coated paper according to any one of claims 1 to 7, characterized in that

9. Coated paper according to any one of claims 1 to 8, characterized in that it is free of halogen-containing compounds.

10. The base paper has a thickness of 20 to 120 g / m 2 10. Coated paper according to claim 1, characterized in that it has an areal density of

11. 11. The coated paper according to claim 1, characterized in that the base paper has a long fiber content of 10-80% by weight and a short fiber content of 20-90% by weight, the long fibers being fibers with a fiber length of 2.6-4.4 mm and the short fibers being fibers with a fiber length of 0.7-2.2 mm.

12. Coated paper according to any one of the preceding claims, characterised in that a further layer comprising a metal and / or a metal oxide is applied to the barrier layer.

13. Method for producing coated paper according to any one of claims 1 to 12, characterized in that an aqueous suspension comprising starting materials for the barrier layer is applied to the base paper, the aqueous suspension having a solids content of 5-50% by weight and applied by a curtain coating process at a working speed of the coating installation of at least 200 m / min.

14. Use of the coated paper according to any one of claims 1 to 11 as a packaging material or as a component of a packaging material.

15. A packaging comprising the coated paper according to any one of claims 1 to 11, the packaging being a cold seal packaging or a heat seal packaging.

Citation Information

Patent Citations

  • Laminated sheet

    JP2006272655A

  • Barrier paper packaging material

    WO2013069788A1

  • Heat-sealable barrier paper

    WO2019158566A1

  • PVOH-based coating solutions

    US6444750B1

  • Barrier coatings post-treated with multi-valent metal cations

    WO2010129032A1