Exterior material for power storage device and power storage device using the same

The exterior material for power storage devices, featuring a base, barrier, and sealant layers with specific high-temperature components, addresses the heat resistance and adhesion issues in all-solid-state batteries, ensuring robust sealing and durability in high-temperature conditions.

JP2024147799AActive Publication Date: 2024-10-16TOPPAN HOLDINGS INC
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2024120916
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-10-16
Estimated Expiration
2039-12-27

AI Technical Summary

Technical Problem

Laminated all-solid-state batteries face issues with insufficient heat resistance and interlayer adhesion in high-temperature environments, leading to decreased heat seal strength and sealing performance due to the use of multilayer films as exterior materials.

Method used

An exterior material for power storage devices comprising a base layer, barrier layer, and sealant layer, where the sealant layer includes components with high melting points or glass transition temperatures, such as polyolefin units and polypropylene resins, ensuring excellent heat seal strength even in high-temperature conditions.

Benefits of technology

The proposed exterior material maintains sufficient heat-sealing strength at 200°C and ensures good interlayer adhesion, even in high-temperature environments, preventing moisture ingress and enhancing the durability of all-solid-state batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024147799000001_ABST
    Figure 2024147799000001_ABST
Patent Text Reader

Abstract

To provide an exterior material for a power storage device which can secure heat seal strength even under a high temperature environment.SOLUTION: An exterior material for a power storage device includes at least a base material layer, a barrier layer, and a sealant layer in this order, wherein the sealant layer contains component (A): a compound containing a polyolefin unit and having a melting point of 175°C or higher or a glass transition temperature of 75°C or higher; component (B): at least one kind of resin selected from the group consisting of a polyethylene-based resin and a polypropylene-based resin; component (C): a compatibilizer having a part compatible with the component (A) and a part compatible with the component (B), and the component (A) is incompatible with the component (B).SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present disclosure relates to an exterior material for a power storage device and a power storage device using the same. [Background technology]

[0002] Known examples of power storage devices include secondary batteries such as lithium-ion batteries, nickel-metal hydride batteries, and lead-acid batteries, as well as electrochemical capacitors such as electric double-layer capacitors. Due to the miniaturization of portable devices and limitations on installation space, there is a demand for further miniaturization of power storage devices, and lithium-ion batteries with high energy density have attracted attention. While metal cans have traditionally been used as the exterior materials for lithium-ion batteries, multilayer films have begun to be used, which are lightweight, have excellent heat dissipation properties, and can be produced at low cost.

[0003] Lithium-ion batteries that use the above multilayer film as an exterior material are called laminated lithium-ion batteries. The exterior material covers the battery contents (positive electrode, separator, negative electrode, electrolyte, etc.) and prevents moisture from penetrating into the battery. Laminated lithium-ion batteries are manufactured, for example, by forming a recess in part of the exterior material by cold forming, accommodating the battery contents in the recess, folding back the remaining part of the exterior material, and heat-sealing the edges (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Laid-Open No. 2013-101765 Summary of the Invention [Problem to be solved by the invention]

[0005] Meanwhile, research and development is being conducted on power storage devices known as all-solid-state batteries as the next generation of lithium-ion batteries. All-solid-state batteries are characterized by using a solid electrolyte instead of an organic electrolyte solution as the electrolyte material. While lithium-ion batteries cannot be used at temperatures higher than the boiling point of the electrolyte solution (approximately 80°C), all-solid-state batteries can be used at temperatures exceeding 100°C, and the conductivity of lithium ions can be increased by operating them under high temperature conditions (for example, 100 to 150°C).

[0006] However, when a laminated all-solid-state battery is manufactured using the above-mentioned multilayer film as an exterior material, if the heat resistance of the exterior material is insufficient, interlayer adhesion (adhesion between layers fused by heat sealing) in a high-temperature environment after heat sealing cannot be ensured, and the heat seal strength may decrease, resulting in a risk of a decrease in the hermeticity of the package of the all-solid-state battery.

[0007] The present disclosure has been made in view of the above-mentioned problems, and aims to provide an exterior packaging material for a power storage device that can ensure excellent heat seal strength even in a high-temperature environment, and a power storage device using the same. [Means for solving the problem]

[0008] In order to achieve the above object, the present disclosure provides an exterior packaging material for an electricity storage device comprising at least a base layer, a barrier layer, and a sealant layer in this order, wherein the sealant layer contains: (A) component: a compound containing a polyolefin unit and having a melting point of 175°C or higher or a glass transition temperature of 75°C or higher; and (B) component: at least one resin selected from the group consisting of polyethylene-based resins and polypropylene-based resins.

[0009] The packaging material for a power storage device, which includes a sealant layer having the above-described configuration, can ensure excellent heat seal strength even in a high-temperature environment. This is because the combination of the (A) component and the (B) component ensures good heat sealability through the (B) component, while the (A) component imparts excellent heat resistance to the sealant layer. Therefore, the packaging material can obtain sufficient heat seal strength at a heat seal temperature of about 200°C, and can maintain good interlayer adhesion (adhesion between the sealant layers fused by heat sealing) even in a high-temperature environment (for example, about 150°C) after heat sealing, ensuring excellent heat seal strength.

[0010] In the packaging material for a power storage device, the component (A) may contain a polyamide / polyolefin graft copolymer, and the content of the component (A) in the sealant layer may be 5 to 100 parts by mass per 100 parts by mass of the component (B). In this case, more sufficient heat seal strength can be obtained at a heat seal temperature of about 200°C, and excellent heat seal strength can be more sufficiently ensured even in a high-temperature environment.

[0011] In the packaging material for a power storage device, the component (A) may include a polyamide / polyethylene graft copolymer, the component (B) may include the polypropylene-based resin, and the sealant layer may further include a compatibilizer (component (C)) having a portion compatible with the polyamide / polyethylene graft copolymer and a portion compatible with the polypropylene-based resin. The component (A) may include a polyamide / polyethylene graft copolymer and the component (B) may include a polypropylene-based resin, thereby further improving the heat resistance of the sealant layer. Furthermore, although polyamide / polyethylene graft copolymers are dispersible in polypropylene-based resins, there is room for improvement in compatibility. Therefore, by incorporating the component (C), the compatibility between the components (A) and (B) can be improved, thereby further improving the heat seal strength.

[0012] In the packaging material for a power storage device, the component (A) may contain a cycloolefin copolymer, and the content of the component (A) in the sealant layer may be 5 to 100 parts by mass per 100 parts by mass of the component (B). In this case, more sufficient heat seal strength can be obtained at a heat seal temperature of about 200°C, and excellent heat seal strength can be more sufficiently ensured even in a high-temperature environment.

[0013] In the packaging material for a power storage device, the component (A) may include an ethylene / cycloolefin copolymer, the component (B) may include the polypropylene-based resin, and the sealant layer may further include a compatibilizer (C) having a portion compatible with the ethylene / cycloolefin copolymer and a portion compatible with the polypropylene-based resin. When the component (A) includes an ethylene / cycloolefin copolymer and the component (B) includes a polypropylene-based resin, the heat resistance of the sealant layer can be further improved. Furthermore, although ethylene / cycloolefin copolymers can be dispersed in polypropylene-based resins, there is room for improvement in compatibility. Therefore, by incorporating the component (C), the compatibility between the components (A) and (B) can be improved, thereby further improving heat seal strength.

[0014] In the above-mentioned casing material for a power storage device, a corrosion prevention treatment layer may be provided on one or both surfaces of the barrier layer. By providing the corrosion prevention treatment layer, corrosion of the barrier layer can be prevented, and the presence of the corrosion prevention treatment layer can increase the adhesion between the barrier layer and an adjacent layer. Furthermore, in all-solid-state batteries, sulfide-based materials are sometimes used as electrolytes. When moisture penetrates into the casing material, the sulfide-based compounds react with water to generate hydrogen sulfide (H2S). This H2S may reduce the adhesion between the barrier layer and an adjacent layer. However, when the above-mentioned casing material for a power storage device is used as a casing material for an all-solid-state battery, providing a corrosion prevention treatment layer on the surface of the barrier layer can impart H2S resistance to the barrier layer, thereby preventing a decrease in the adhesion between the barrier layer and an adjacent layer.

[0015] In the packaging material for a storage battery device, when the base layer side of the packaging material for a storage battery device is the outer side and the sealant layer side is the inner side, at least one of the layers arranged on the inner side of the barrier layer may contain a hydrogen sulfide adsorbent. As described above, there is a risk of hydrogen sulfide (H2S) being generated in an all-solid-state battery, but if at least one of the layers arranged on the inner side of the barrier layer contains a hydrogen sulfide adsorbent, the layer containing the hydrogen sulfide adsorbent can adsorb and detoxify H2S generated inside the packaging material, thereby enabling a higher level of protection from H2S to the barrier layer, the current collector (particularly copper foil), and a positive electrode containing Ni.

[0016] In the packaging material for a power storage device, the sealant layer may have a thickness of 10 to 100 μm, which allows a good balance between thinning the packaging material and improving the heat seal strength in a high-temperature environment.

[0017] The packaging material for a power storage device may be used for an all-solid-state battery.

[0018] The present disclosure also provides an electricity storage device including: an electricity storage device main body; a current extracting terminal extending from the electricity storage device main body; and an exterior material for an electricity storage device according to the present disclosure, the exterior material sandwiching the current extracting terminal and housing the electricity storage device main body. The electricity storage device may be an all-solid-state battery. [Effects of the Invention]

[0019] According to the present disclosure, it is possible to provide an exterior packaging material for a power storage device that can ensure excellent heat seal strength even in a high-temperature environment, and a power storage device using the same. [Brief explanation of the drawings]

[0020] [Figure 1] 1 is a schematic cross-sectional view of an exterior packaging material for a power storage device according to an embodiment of the present disclosure. [Figure 2] 1 is a schematic cross-sectional view of an exterior packaging material for a power storage device according to an embodiment of the present disclosure. [Figure 3]1 is a perspective view of an electricity storage device according to an embodiment of the present disclosure. [Figure 4] FIG. 2 is a schematic diagram illustrating a method for preparing a sample for measuring heat seal strength in the examples. DETAILED DESCRIPTION OF THE INVENTION

[0021] Preferred embodiments of the present disclosure will be described in detail below with reference to the drawings. In the drawings, identical or corresponding parts are designated by the same reference numerals, and duplicate explanations will be omitted. Furthermore, the dimensional ratios of the drawings are not limited to those shown.

[0022] [Exterior materials for energy storage devices] Fig. 1 is a cross-sectional view schematically illustrating one embodiment of an exterior packaging material for an energy storage device according to the present disclosure. As shown in Fig. 1, an exterior packaging material (exterior packaging material for an energy storage device) 10 of this embodiment is a laminate including a substrate layer 11, a first adhesive layer 12a provided on one side of the substrate layer 11, a barrier layer 13 provided on the side of the first adhesive layer 12a opposite the substrate layer 11 and having first and second corrosion prevention treatment layers 14a, 14b on both sides, a second adhesive layer 12b provided on the side of the barrier layer 13 opposite the first adhesive layer 12a, and a sealant layer 16 provided on the side of the second adhesive layer 12b opposite the barrier layer 13. The first corrosion prevention treatment layer 14a is provided on the surface of the barrier layer 13 facing the substrate layer 11, and the second corrosion prevention treatment layer 14b is provided on the surface of the barrier layer 13 facing the sealant layer 16. In the packaging material 10, the base material layer 11 is the outermost layer and the sealant layer 16 is the innermost layer. That is, the packaging material 10 is used with the base material layer 11 facing the exterior side of the electricity storage device and the sealant layer 16 facing the interior side of the electricity storage device. Each layer that makes up the packaging material 10 will be described in detail below.

[0023] <Base material layer 11> The base material layer 11 provides heat resistance in the sealing process when manufacturing the electricity storage device and plays a role in suppressing the occurrence of pinholes that may occur during molding and distribution. In particular, in the case of an exterior material for a large-scale electricity storage device, the base material layer 11 can also provide scratch resistance, chemical resistance, insulation, etc.

[0024] The base layer 11 is preferably a layer made of a resin film formed from an insulating resin. Examples of the resin film include stretched or unstretched films such as polyester film, polyamide film, and polypropylene film. The base layer 11 may be a single-layer film made of any of these resin films, or a laminated film made of two or more of these resin films.

[0025] Among these, polyester film and polyamide film are preferred as the base layer 11 due to their excellent formability, and polyamide film is more preferred. These films are preferably biaxially stretched films. Examples of polyester resins constituting polyester films include polyethylene terephthalate. Examples of polyamide resins constituting polyamide films include nylon 6, nylon 6,6, copolymers of nylon 6 and nylon 6,6, nylon 6,10, polymetaxylylene adipamide (MXD6), nylon 11, and nylon 12. Among these, nylon 6 (ONy) is preferred due to its excellent heat resistance, puncture strength, and impact strength.

[0026] Examples of the stretching method for the biaxially stretched film include sequential biaxial stretching, tubular biaxial stretching, simultaneous biaxial stretching, etc. From the viewpoint of obtaining better deep drawability, the biaxially stretched film is preferably one stretched by the tubular biaxial stretching method.

[0027] Furthermore, the substrate layer 11 preferably has a peak melting temperature higher than that of the sealant layer 16. When the sealant layer 16 has a multilayer structure, the peak melting temperature of the sealant layer 16 refers to the peak melting temperature of the layer with the highest peak melting temperature. The peak melting temperature of the substrate layer 11 is preferably 290°C or higher, more preferably 290 to 350°C. Examples of resin films that can be used as the substrate layer 11 and have a peak melting temperature within the above range include nylon film, PET film, polyamide film, and polyphenylene sulfide film (PPS film). A commercially available film may be used as the substrate layer 11, or the substrate layer 11 may be formed by coating (application of a coating liquid and drying). The substrate layer 11 may have a single-layer structure or a multilayer structure, and may be formed by coating a thermosetting resin. The substrate layer 11 may also contain various additives (e.g., flame retardants, slip agents, antiblocking agents, antioxidants, light stabilizers, tackifiers, etc.).

[0028] Melting peak temperature T of the base layer 11 11 and the melting peak temperature T of the sealant layer 16 16 The difference (T 11 -T 16 ) is preferably 20° C. or more. When this temperature difference is 20° C. or more, deterioration of the appearance of the packaging material 10 due to heat sealing can be more sufficiently suppressed.

[0029] The substrate layer 11 may be provided by directly applying it onto the barrier layer 13 or the first corrosion prevention treatment layer 14a described below. In this case, the first adhesive layer 12a described below is not necessary. The substrate layer 11 can be formed by applying a resin coating liquid such as urethane resin, acrylic resin, or polyester resin, followed by curing by ultraviolet irradiation, high-temperature heating, aging (curing), or the like. The application method is not particularly limited, and various methods such as gravure coating, reverse coating, roll coating, and bar coating can be used.

[0030] The thickness of the substrate layer 11 is preferably 5 to 50 μm, more preferably 6 to 40 μm, even more preferably 10 to 30 μm, and particularly preferably 12 to 30 μm. When the thickness of the substrate layer 11 is 5 μm or more, the pinhole resistance and insulating properties of the packaging material for an electricity storage device 10 tend to be improved. If the thickness of the substrate layer 11 exceeds 50 μm, the total thickness of the packaging material for an electricity storage device 10 increases, which is undesirable because it may be necessary to reduce the electrical capacity of the battery.

[0031] <First adhesive layer 12a> The first adhesive layer 12a is a layer that bonds the base material layer 11 and the barrier layer 13. Specific examples of materials that constitute the first adhesive layer 12a include polyurethane resins in which a bifunctional or higher isocyanate compound is allowed to react with a base material such as polyester polyol, polyether polyol, acrylic polyol, or carbonate polyol.

[0032] The various polyols described above can be used alone or in combination of two or more types depending on the functions and performance required of the packaging material.

[0033] Depending on the performance required of the adhesive, various other additives and stabilizers may be blended into the polyurethane resin described above.

[0034] The thickness of the first adhesive layer 12a is not particularly limited, but from the viewpoint of obtaining the desired adhesive strength, conformability, processability, etc., it is preferably, for example, 1 to 10 μm, more preferably 3 to 7 μm.

[0035] <Barrier layer 13> The barrier layer 13 has water vapor barrier properties that prevent moisture from penetrating into the interior of the electricity storage device. The barrier layer 13 also has extensibility for deep drawing. Examples of the barrier layer 13 that can be used include various metal foils such as aluminum, stainless steel, and copper, as well as metal vapor-deposited films, inorganic oxide vapor-deposited films, carbon-containing inorganic oxide vapor-deposited films, and films having these vapor-deposited films. Examples of films having vapor-deposited films that can be used include aluminum vapor-deposited films and inorganic oxide vapor-deposited films. These may be used alone or in combination of two or more. In terms of mass (specific gravity), moisture resistance, processability, and cost, metal foils are preferred for the barrier layer 13, and aluminum foil is more preferred.

[0036] As the aluminum foil, soft aluminum foil that has been annealed is particularly preferred because it can impart the desired ductility during molding. However, it is more preferable to use aluminum foil containing iron for the purpose of imparting further pinhole resistance and ductility during molding. The iron content in the aluminum foil is preferably 0.1 to 9.0 mass%, more preferably 0.5 to 2.0 mass%, based on 100 mass% of the aluminum foil. By having an iron content of 0.1 mass% or more, an exterior packaging material 10 having better pinhole resistance and ductility can be obtained. By having an iron content of 9.0 mass% or less, an exterior packaging material 10 having better flexibility can be obtained. As the aluminum foil, untreated aluminum foil may be used, but it is preferable to use aluminum foil that has been degreased to impart corrosion resistance. When the aluminum foil is degreased, the degreasing treatment may be performed on only one side of the aluminum foil, or on both sides.

[0037] The thickness of the barrier layer 13 is not particularly limited, but is preferably 9 to 200 μm, more preferably 15 to 100 μm, in consideration of barrier properties, pinhole resistance, and processability.

[0038] <First and second corrosion prevention treatment layers 14a, 14b> The first and second corrosion prevention treatment layers 14a and 14b are layers provided on the surface of the barrier layer 13 to prevent corrosion of the metal foil (metal foil layer) that constitutes the barrier layer 13. The first corrosion prevention treatment layer 14a serves to increase the adhesion between the barrier layer 13 and the first adhesive layer 12a. The second corrosion prevention treatment layer 14b serves to increase the adhesion between the barrier layer 13 and the second adhesive layer 12b. The first corrosion prevention treatment layer 14a and the second corrosion prevention treatment layer 14b may be layers of the same configuration or layers of different configurations. The first and second corrosion prevention treatment layers 14a and 14b (hereinafter simply referred to as "corrosion prevention treatment layers 14a and 14b") may be formed by, for example, degreasing treatment, hydrothermal conversion treatment, anodizing treatment, chemical conversion treatment, or a combination of these treatments.

[0039] Examples of degreasing treatments include acid degreasing and alkaline degreasing. Examples of acid degreasing include a method using an inorganic acid such as sulfuric acid, nitric acid, hydrochloric acid, or hydrofluoric acid, either alone or in combination. Furthermore, by using an acid degreasing agent prepared by dissolving a fluorine-containing compound such as monosodium ammonium difluoride in the inorganic acid, not only can the aluminum be degreased, but also a passive aluminum fluoride can be formed, which is effective in terms of corrosion resistance, particularly when an aluminum foil is used for the barrier layer 13. Examples of alkaline degreasing include a method using sodium hydroxide or the like.

[0040] An example of the hydrothermal modification treatment is boehmite treatment, in which aluminum foil is immersed in boiling water containing triethanolamine.

[0041] An example of the anodizing treatment is alumite treatment.

[0042] The chemical conversion treatment may be an immersion type or a coating type. Examples of the immersion type chemical conversion treatment include chromate treatment, zirconium treatment, titanium treatment, vanadium treatment, molybdenum treatment, calcium phosphate treatment, strontium hydroxide treatment, cerium treatment, ruthenium treatment, and various chemical conversion treatments consisting of a mixture of these. On the other hand, an example of the coating type chemical conversion treatment is a method in which a coating agent having corrosion prevention properties is applied to the barrier layer 13.

[0043] When forming at least a part of the corrosion prevention treatment layer by any of these corrosion prevention treatments, i.e., hydrothermal conversion treatment, anodizing treatment, and chemical conversion treatment, it is preferable to perform the above-mentioned degreasing treatment beforehand. Note that when a degreased metal foil, such as a metal foil that has been subjected to an annealing process, is used as the barrier layer 13, there is no need to perform a degreasing treatment again when forming the corrosion prevention treatment layers 14a and 14b.

[0044] The coating agent used in the spray-type chemical conversion treatment preferably contains trivalent chromium and may also contain at least one polymer selected from the group consisting of cationic polymers and anionic polymers, which will be described later.

[0045] Among the above treatments, hydrothermal conversion treatment and anodizing, in particular, dissolve the aluminum foil surface with a treatment agent to form aluminum compounds (boehmite, anodized aluminum) with excellent corrosion resistance. Therefore, a bicontinuous structure is formed from the aluminum foil barrier layer 13 to the corrosion prevention treatment layers 14a, 14b, and these treatments are included in the definition of chemical conversion treatment. On the other hand, as described below, it is also possible to form the corrosion prevention treatment layers 14a, 14b using a pure coating method, which is not included in the definition of chemical conversion treatment. One example of such a method is the use of a sol of a rare earth oxide, such as cerium oxide, with an average particle size of 100 nm or less, which has an aluminum corrosion prevention effect (inhibitor effect) and is environmentally friendly. Using this method, it is possible to impart corrosion prevention effects to metal foils such as aluminum foil using a conventional coating method.

[0046] Examples of the rare earth element oxide sol include sols using various solvents such as water-based, alcohol-based, hydrocarbon-based, ketone-based, ester-based, ether-based, etc. Of these, water-based sols are preferred.

[0047] In order to stabilize the dispersion of the rare earth element oxide sol, inorganic acids such as nitric acid, hydrochloric acid, phosphoric acid, or their salts, or organic acids such as acetic acid, malic acid, ascorbic acid, and lactic acid are usually used as dispersion stabilizers. Of these dispersion stabilizers, phosphoric acid in particular is expected to have the following effects on the exterior packaging material 10: (1) stabilization of the sol dispersion, (2) improvement of adhesion to the barrier layer 13 by utilizing the aluminum chelating ability of phosphoric acid, and (3) improvement of the cohesion of the corrosion prevention treatment layers 14a, 14b (oxide layers) due to the tendency of phosphoric acid to undergo dehydration condensation even at low temperatures.

[0048] Examples of the phosphoric acid or its salt include orthophosphoric acid, pyrophosphoric acid, metaphosphoric acid, or their alkali metal salts or ammonium salts. Among these, condensed phosphoric acids such as trimetaphosphoric acid, tetrametaphosphoric acid, hexametaphosphoric acid, and ultrametaphosphoric acid, or their alkali metal salts or ammonium salts, are preferred for functional expression in the exterior packaging material 10. Furthermore, when considering the drying film-forming properties (drying capacity, heat quantity) when forming the corrosion prevention treatment layers 14a, 14b made of rare earth element oxides using the rare earth element oxide sol by various coating methods, sodium salts are more preferred because of their excellent dehydration condensation properties at low temperatures. Water-soluble salts are preferred as phosphates.

[0049] The compounding ratio of phosphoric acid (or a salt thereof) to rare earth element oxide is preferably 1 to 100 parts by mass per 100 parts by mass of rare earth element oxide. If the compounding ratio is 1 part by mass or more per 100 parts by mass of rare earth element oxide, the rare earth element oxide sol becomes more stable, and the functionality of the packaging material 10 becomes better. The compounding ratio is more preferably 5 parts by mass or more per 100 parts by mass of rare earth element oxide. Furthermore, if the compounding ratio is 100 parts by mass or less per 100 parts by mass of rare earth element oxide, the functionality of the rare earth element oxide sol is improved. The compounding ratio is more preferably 50 parts by mass or less, and even more preferably 20 parts by mass or less, per 100 parts by mass of rare earth element oxide.

[0050] Since the corrosion prevention treatment layers 14a, 14b formed from the rare earth element oxide sol are aggregates of inorganic particles, the cohesive strength of the layers themselves may be reduced even after the dry-cure process. Therefore, in this case, the corrosion prevention treatment layers 14a, 14b are preferably compounded with the following anionic polymer or cationic polymer to compensate for the cohesive strength.

[0051] Examples of anionic polymers include polymers having a carboxy group, such as poly(meth)acrylic acid (or a salt thereof) or a copolymer copolymerized with poly(meth)acrylic acid as the main component. The copolymerization components of this copolymer include alkyl(meth)acrylate monomers (alkyl groups include methyl, ethyl, n-propyl, i-propyl, n-butyl, i-butyl, t-butyl, 2-ethylhexyl, and cyclohexyl groups); (meth)acrylamide, N-alkyl(meth)acrylamide, N,N-dialkyl(meth)acrylamide (alkyl groups include methyl, ethyl, n-propyl, i-propyl, n-butyl, i-butyl, t-butyl, 2-ethylhexyl, and cyclohexyl groups); N-alkoxy(meth)acrylamide, N,N-dialkoxy(meth)acrylamide, and (alkoxy)acrylamide. Examples of the oxy group include a methoxy group, an ethoxy group, a butoxy group, and an isobutoxy group. Examples of the oxy group include amide group-containing monomers such as N-methylol(meth)acrylamide and N-phenyl(meth)acrylamide; hydroxyl group-containing monomers such as 2-hydroxyethyl(meth)acrylate and 2-hydroxypropyl(meth)acrylate; glycidyl group-containing monomers such as glycidyl(meth)acrylate and allyl glycidyl ether; silane-containing monomers such as (meth)acryloxypropyltrimethoxysilane and (meth)acryloxypropyltriethoxylane; and isocyanate group-containing monomers such as (meth)acryloxypropylisocyanate.

[0052] These anionic polymers improve the stability of the corrosion-resistant treated layers 14a, 14b (oxide layers) obtained using the rare earth element oxide sol. This is achieved by protecting the hard and brittle oxide layer with the acrylic resin component and by capturing ionic contaminants (especially sodium ions) derived from the phosphate contained in the rare earth element oxide sol (as a cation catcher). In other words, if the corrosion-resistant treated layers 14a, 14b obtained using the rare earth element oxide sol contain alkali metal ions, particularly sodium, or alkaline earth metal ions, the corrosion-resistant treated layers 14a, 14b are prone to degradation originating from the locations containing these ions. Therefore, by immobilizing the sodium ions and other ions contained in the rare earth element oxide sol using the anionic polymer, the durability of the corrosion-resistant treated layers 14a, 14b is improved.

[0053] The corrosion prevention treatment layers 14a, 14b, which combine anionic polymers and rare earth oxide sols, have corrosion prevention performance equivalent to that of corrosion prevention treatment layers 14a, 14b formed by chromate treatment of aluminum foil. The anionic polymer preferably has a structure in which an essentially water-soluble polyanionic polymer is crosslinked. Examples of crosslinking agents used to form this structure include compounds having an isocyanate group, a glycidyl group, a carboxyl group, or an oxazoline group.

[0054] Examples of compounds having an isocyanate group include diisocyanates such as tolylene diisocyanate, xylylene diisocyanate or hydrogenated products thereof, hexamethylene diisocyanate, 4,4'-diphenylmethane diisocyanate or hydrogenated products thereof, and isophorone diisocyanate; or polyisocyanates such as adducts obtained by reacting these isocyanates with polyhydric alcohols such as trimethylolpropane, biuret compounds obtained by reacting these isocyanates with water, or trimer isocyanurates; and blocked polyisocyanates obtained by blocking these polyisocyanates with alcohols, lactams, oximes, or the like.

[0055] Examples of compounds having a glycidyl group include epoxy compounds obtained by reacting epichlorohydrin with glycols such as ethylene glycol, diethylene glycol, triethylene glycol, polyethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, polypropylene glycol, 14a,14b-butanediol, 1,6-hexanediol, and neopentyl glycol; epoxy compounds obtained by reacting epichlorohydrin with polyhydric alcohols such as glycerin, polyglycerin, trimethylolpropane, pentaerythritol, and sorbitol; and epoxy compounds obtained by reacting epichlorohydrin with dicarboxylic acids such as phthalic acid, terephthalic acid, oxalic acid, and adipic acid.

[0056] Examples of compounds having a carboxy group include various aliphatic or aromatic dicarboxylic acids, etc. Poly(meth)acrylic acid and alkali (earth) metal salts of poly(meth)acrylic acid may also be used.

[0057] Examples of compounds having an oxazoline group include low molecular weight compounds having two or more oxazoline units, and when a polymerizable monomer such as isopropenyloxazoline is used, copolymers of acrylic monomers such as (meth)acrylic acid, alkyl (meth)acrylates, and hydroxyalkyl (meth)acrylates.

[0058] Alternatively, an anionic polymer may be reacted with a silane coupling agent, more specifically, by selectively reacting the carboxyl groups of the anionic polymer with the functional groups of the silane coupling agent to form siloxane bonds at the crosslinking points. In this case, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-chloropropylmethoxysilane, vinyltrichlorosilane, γ-mercaptopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, N-β(aminoethyl)-γ-aminopropyltrimethoxysilane, γ-isocyanatopropyltriethoxysilane, etc. can be used. Among these, epoxysilanes, aminosilanes, and isocyanatesilanes are preferred, especially in terms of reactivity with anionic polymers or their copolymers.

[0059] The ratio of these crosslinking agents to the anionic polymer is preferably 1 to 50 parts by mass, more preferably 10 to 20 parts by mass, per 100 parts by mass of the anionic polymer. When the ratio of the crosslinking agent is 1 part by mass or more per 100 parts by mass of the anionic polymer, a crosslinked structure is easily formed sufficiently. When the ratio of the crosslinking agent is 50 parts by mass or less per 100 parts by mass of the anionic polymer, the pot life of the coating liquid is improved.

[0060] The method for crosslinking the anionic polymer is not limited to the above-mentioned crosslinking agents, and may also be a method for forming ionic crosslinks using titanium or zirconium compounds.

[0061] Examples of cationic polymers include polymers containing amines, such as polyethyleneimine, ionic polymer complexes consisting of polyethyleneimine and a polymer containing carboxylic acid, primary amine-grafted acrylic resins in which a primary amine is grafted onto an acrylic backbone, polyallylamine or derivatives thereof, and cationic polymers such as aminophenol. Examples of polyallylamine include homopolymers or copolymers of allylamine, allylamine amide sulfate, diallylamine, and dimethylallylamine. These amines may be free amines or stabilized with acetic acid or hydrochloric acid. Furthermore, maleic acid, sulfur dioxide, and the like may be used as copolymer components. Furthermore, types in which the primary amine is partially methoxylated to impart thermal crosslinking properties can also be used, and aminophenols can also be used. Allylamine or its derivatives are particularly preferred.

[0062] The cationic polymer is preferably used in combination with a crosslinking agent having a functional group capable of reacting with amine / imine, such as a carboxy group or a glycidyl group. As the crosslinking agent to be used in combination with the cationic polymer, a polymer having a carboxylic acid that forms an ionic polymer complex with polyethyleneimine can also be used, and examples thereof include polycarboxylic acid (salts) such as polyacrylic acid or its ionic salts, copolymers thereof with comonomers introduced therein, and polysaccharides having a carboxy group, such as carboxymethylcellulose or its ionic salts.

[0063] Cationic polymers are more preferred materials in terms of improving adhesion. Furthermore, like the anionic polymers, cationic polymers are also water-soluble, so it is more preferred to form a crosslinked structure to impart water resistance. The crosslinking agent used to form the crosslinked structure in the cationic polymer can be the same as the crosslinking agent described in the anionic polymer section. When a rare earth element oxide sol is used as the corrosion prevention treatment layers 14a and 14b, a cationic polymer may be used as the protective layer instead of the anionic polymer.

[0064] A corrosion-preventing treatment layer formed by chemical conversion treatment, such as chromate treatment, is formed by treating aluminum foil with a chemical conversion treatment agent, particularly a combination of hydrofluoric acid, hydrochloric acid, nitric acid, sulfuric acid, or their salts, followed by the application of a chromium or non-chromium compound to form a chemical conversion treatment layer on the aluminum foil. However, since the above-mentioned chemical conversion treatment uses an acid in the chemical conversion treatment agent, it can lead to deterioration of the working environment and corrosion of the coating equipment. On the other hand, unlike chemical conversion treatments such as chromate treatment, the aforementioned coating-type corrosion-preventing treatment layers 14a and 14b do not require the formation of a gradient structure relative to the barrier layer 13 using aluminum foil. Therefore, the properties of the coating agent are not restricted by acidity, alkalinity, neutrality, etc., and a good working environment can be achieved. In addition, chromate treatments using chromium compounds are preferred because alternatives are needed for environmental hygiene reasons.

[0065] From the above, examples of combinations of the above-mentioned coating-type corrosion prevention treatments include (1) rare earth element oxide sol only, (2) anionic polymer only, (3) cationic polymer only, (4) rare earth element oxide sol + anionic polymer (laminated composite), (5) rare earth element oxide sol + cationic polymer (laminated composite), (6) (rare earth element oxide sol + anionic polymer: laminated composite) / cationic polymer (multilayered), and (7) (rare earth element oxide sol + cationic polymer: laminated composite) / anionic polymer (multilayered). Among these, (1) and (4) to (7) are preferred, and (4) to (7) are particularly preferred. However, this embodiment is not limited to the above combinations. For example, as an example of the selection of corrosion prevention treatment, cationic polymers are very preferable materials in that they have good adhesion to the modified polyolefin resins mentioned in the description of the second adhesive layer, adhesive resin layer, or sealant layer described below. Therefore, when the second adhesive layer, adhesive resin layer, or sealant layer is made of a modified polyolefin resin, it is possible to design the surface in contact with the second adhesive layer, adhesive resin layer, or sealant layer by providing a cationic polymer (for example, structures (5) and (6)).

[0066] Furthermore, the corrosion prevention treatment layers 14a, 14b are not limited to the layers described above. For example, they may be formed using a treatment agent that combines phosphoric acid and a chromium compound with a resin binder (such as aminophenol), as in the case of a known paint-type chromate. Using this treatment agent makes it possible to obtain a layer that combines both corrosion prevention functionality and adhesion. Furthermore, although the stability of the coating liquid must be considered, a coating agent that combines a rare earth element oxide sol with a polycationic polymer or a polyanionic polymer in advance as a one-component can be used to obtain a layer that combines corrosion prevention functionality and adhesion.

[0067] The mass per unit area of ​​the corrosion prevention treatment layers 14a and 14b is 0.005 to 0.200 g / m 2 regardless of whether the layer has a multi-layer structure or a single-layer structure. 2 is preferable, and 0.010 to 0.100 g / m 2It is more preferable that the mass per unit area is 0.005 g / m 2 If the mass per unit area is 0.200 g / m or more, it is easy to impart a corrosion prevention function to the barrier layer 13. 2 Even if the thickness exceeds this range, the corrosion prevention function does not change significantly. On the other hand, when a rare earth element oxide sol is used, if the coating is thick, the heat curing during drying may be insufficient, which may result in a decrease in cohesive force. The thickness of the corrosion prevention treatment layers 14a and 14b can be calculated from their specific gravity.

[0068] From the viewpoint of easily maintaining the adhesion between the sealant layer and the barrier layer, the corrosion prevention treatment layers 14a, 14b may be in an embodiment containing, for example, cerium oxide, 1 to 100 parts by mass of phosphoric acid or a phosphate salt per 100 parts by mass of the cerium oxide, and a cationic polymer, or may be formed by subjecting the barrier layer 13 to a chemical conversion treatment, or may be formed by subjecting the barrier layer 13 to a chemical conversion treatment and contain a cationic polymer.

[0069] <Second adhesive layer 12b> The second adhesive layer 12b is a layer that bonds the barrier layer 13, on which the second corrosion prevention treatment layer 14b is formed, to the sealant layer 16. A general adhesive for bonding a barrier layer and a sealant layer can be used for the second adhesive layer 12b.

[0070] When the second corrosion prevention treatment layer 14b has a layer containing at least one polymer selected from the group consisting of the above-mentioned cationic polymers and anionic polymers, the second adhesive layer 12b is preferably a layer containing a compound (hereinafter also referred to as a "reactive compound") that is reactive with the above-mentioned polymer contained in the second corrosion prevention treatment layer 14b.

[0071] For example, if the second corrosion prevention treatment layer 14b contains a cationic polymer, the second adhesive layer 12b contains a compound reactive with the cationic polymer. If the second corrosion prevention treatment layer 14b contains an anionic polymer, the second adhesive layer 12b contains a compound reactive with the anionic polymer. If the second corrosion prevention treatment layer 14b contains both a cationic polymer and an anionic polymer, the second adhesive layer 12b contains a compound reactive with the cationic polymer and a compound reactive with the anionic polymer. However, the second adhesive layer 12b does not necessarily have to contain both of these compounds; it may also contain a compound reactive with both the cationic polymer and the anionic polymer. Here, "reactive" means forming a covalent bond with the cationic polymer or the anionic polymer. The second adhesive layer 12b may also contain an acid-modified polyolefin resin.

[0072] The compound reactive with the cationic polymer may be at least one compound selected from the group consisting of a polyfunctional isocyanate compound, a glycidyl compound, a compound having a carboxy group, and a compound having an oxazoline group.

[0073] Examples of these polyfunctional isocyanate compounds, glycidyl compounds, compounds having a carboxy group, and compounds having an oxazoline group include the polyfunctional isocyanate compounds, glycidyl compounds, compounds having a carboxy group, and compounds having an oxazoline group exemplified above as crosslinking agents for forming a crosslinked structure from a cationic polymer. Among these, polyfunctional isocyanate compounds are preferred because they have high reactivity with cationic polymers and are easy to form a crosslinked structure.

[0074] The compound reactive with anionic polymers includes at least one compound selected from the group consisting of glycidyl compounds and compounds having an oxazoline group. These glycidyl compounds and compounds having an oxazoline group include the glycidyl compounds and compounds having an oxazoline group exemplified above as crosslinking agents for forming a crosslinked structure in cationic polymers. Among these, glycidyl compounds are preferred because of their high reactivity with anionic polymers.

[0075] When the second adhesive layer 12b contains an acid-modified polyolefin resin, the reactive compound preferably also has reactivity with the acidic groups in the acid-modified polyolefin resin (i.e., forms a covalent bond with the acidic groups). This further enhances adhesion to the second corrosion prevention treatment layer 14b. In addition, the acid-modified polyolefin resin forms a crosslinked structure, further improving the solvent resistance of the exterior packaging material 10.

[0076] The content of the reactive compound is preferably from 1 to 10 times the amount of the acidic groups in the acid-modified polyolefin resin. If the amount is equal to or greater than 10 times, the reactive compound will react sufficiently with the acidic groups in the acid-modified polyolefin resin. On the other hand, if the amount exceeds 10 times, the crosslinking reaction with the acid-modified polyolefin resin will be fully saturated, resulting in the presence of unreacted material, which may lead to a decrease in various performances. Therefore, for example, the content of the reactive compound is preferably 5 to 20 parts by mass (solid content ratio) per 100 parts by mass of the acid-modified polyolefin resin.

[0077] The acid-modified polyolefin resin is a polyolefin resin into which an acidic group has been introduced. Examples of the acidic group include a carboxyl group, a sulfonic acid group, and an acid anhydride group, with a maleic anhydride group and a (meth)acrylic acid group being particularly preferred. For example, the acid-modified polyolefin resin may be the same as the modified polyolefin resin (a) used in the first sealant layer 16a, which will be described later.

[0078] The second adhesive layer 12b may contain various additives such as a flame retardant, a slip agent, an antiblocking agent, an antioxidant, a light stabilizer, and a tackifier.

[0079] From the viewpoint of suppressing a decrease in laminate strength and further suppressing a decrease in insulating properties, the second adhesive layer 12b may contain, for example, an acid-modified polyolefin and at least one curing agent selected from the group consisting of a polyfunctional isocyanate compound, a glycidyl compound, a compound having a carboxy group, a compound having an oxazoline group, and a carbodiimide compound. Examples of the carbodiimide compound include N,N'-di-o-toluylcarbodiimide, N,N'-diphenylcarbodiimide, N,N'-di-2,6-dimethylphenylcarbodiimide, N,N'-bis(2,6-diisopropylphenyl)carbodiimide, N,N'-dioctyldecylcarbodiimide, N-triyl-N'-cyclohexylcarbodiimide, N,N'-di-2,2-di-t-butylphenylcarbodiimide, N-triyl-N'-phenylcarbodiimide, N,N'-di-p-nitrophenylcarbodiimide, N,N'-di-p-aminophenylcarbodiimide, N,N'-di-p-hydroxyphenylcarbodiimide, N,N'-di-cyclohexylcarbodiimide, and N,N'-di-p-toluylcarbodiimide.

[0080] Furthermore, as the adhesive for forming the second adhesive layer 12b, for example, a polyurethane adhesive containing a polyester polyol made of a hydrogenated dimer fatty acid and a diol, and a polyisocyanate may be used.

[0081] The thickness of the second adhesive layer 12b is not particularly limited, but is preferably 1 to 10 μm, more preferably 3 to 7 μm, from the viewpoint of obtaining the desired adhesive strength and processability.

[0082] <Sealant layer 16> The sealant layer 16 is a layer that imparts heat-sealing properties to the exterior packaging material 10. The sealant layer 16 is a layer that contains: (A) component: a compound that contains a polyolefin unit and has a melting point of 175°C or higher or a glass transition temperature of 75°C or higher; and (B) component: at least one resin selected from the group consisting of polyethylene-based resins and polypropylene-based resins.

[0083] When the sealant layer is a single layer as shown in Figure 1, the sealant layer is a layer containing the above-mentioned components (A) and (B). When the sealant layer has two or more layers, it is sufficient that at least one layer contains the above-mentioned components (A) and (B), and it is preferable that at least the innermost layer (the layer located farthest from the base layer 11) is a layer containing the above-mentioned components (A) and (B). In addition, the sealant layer 16 may further contain component (C): a compatibilizer having a portion compatible with component (A) and a portion compatible with component (B). In addition, the sealant layer 16 may further contain a hydrogen sulfide adsorbing substance.

[0084] (Component (A)) Component (A) is a compound containing a polyolefin unit and having a melting point (Tm) of 175°C or higher or a glass transition temperature (Tg) of 75°C or higher. Examples of the polyolefin unit include a polyethylene unit, a polypropylene unit, and a polybutylene unit. Component (A) is preferably a copolymer of an olefin and another copolymerizable monomer. Examples of component (A) include a polyamide / polyolefin graft copolymer and a cycloolefin / olefin copolymer (cycloolefin copolymer).

[0085] An example of the polyamide / polyolefin graft copolymer is a polyamide / polyethylene graft copolymer. Commercially available polyamide / polyolefin graft copolymers include "Aporya LP2" (melting point: 216°C) and "Aporya LP21H" (melting point: 216°C) manufactured by Arkema.

[0086] An example of a cycloolefin copolymer is an ethylene / cycloolefin copolymer. Commercially available cycloolefin copolymers include "APEL" manufactured by Mitsui Chemicals, Inc. and "TOPAS" manufactured by TOPAS Advanced Polymers GmbH. Examples of "APEL" include "APL6509" (Tg: 80°C), "APL6011T" (Tg: 105°C), "APL6013T" (Tg: 125°C), and "APL6015T" (Tg: 145°C).

[0087] Component (A) is a compound having a melting point of 175°C or higher or a glass transition temperature of 75°C or higher. By using component (A) having a melting point of 175°C or higher or a glass transition temperature of 75°C or higher, the sealant layer 16 can obtain sufficient heat seal strength at a heat seal temperature of about 200°C and maintain sufficient heat seal strength even in a high-temperature environment (for example, about 150°C). Component (A) may be a compound having a melting point of 175°C or higher and a glass transition temperature of 75°C or higher. On the other hand, if a compound having a melting point below 175°C and a glass transition temperature below 75°C, a compound having a melting point below 175°C and no glass transition temperature, or a compound having a glass transition temperature below 75°C and no melting point is used, sufficient heat seal strength cannot necessarily be ensured in a high-temperature environment (about 150°C).

[0088] From the viewpoint of further improving heat seal strength in a high-temperature environment (for example, about 150°C), the melting point of component (A) may be 180°C or higher, 190°C or higher, 200°C or higher, or 210°C or higher. Furthermore, from the viewpoint of obtaining sufficient heat seal strength at a heat seal temperature of about 200°C, the melting point of component (A) may be 250°C or lower, or 240°C or lower.

[0089] From the viewpoint of further improving heat seal strength in a high-temperature (for example, about 150°C) environment, the glass transition temperature of component (A) may be 80°C or higher, 90°C or higher, 100°C or higher, or 120°C or higher. Furthermore, from the viewpoint of obtaining sufficient heat seal strength at a heat seal temperature of about 200°C, the glass transition temperature of component (A) may be 200°C or lower, or 180°C or lower.

[0090] The content of component (A) in sealant layer 16 is preferably 5 to 100 parts by mass, more preferably 10 to 90 parts by mass, and even more preferably 20 to 80 parts by mass, per 100 parts by mass of component (B). When the content of component (A) is 5 parts by mass or more, excellent heat seal strength can be more sufficiently ensured even in high-temperature environments, and when the content is 100 parts by mass or less, more sufficient heat seal strength can be obtained at a heat seal temperature of about 200°C, and a decrease in flexibility of the sealant layer and the resulting embrittlement can be suppressed.

[0091] ((B) component) The component (B) is at least one resin selected from the group consisting of polyethylene resins and polypropylene resins. The component (B) is a component that serves as the base resin of the sealant layer 16.

[0092] Examples of polyethylene resins include high-density polyethylene, branched low-density polyethylene, linear low-density polyethylene, etc. Among these, from the viewpoint of film formability, branched low-density polyethylene and linear low-density polyethylene are preferred, and branched low-density polyethylene is more preferred.

[0093] Polypropylene-based resins are resins obtained from polymerized monomers containing propylene. Examples of polypropylene-based resins include homopolypropylene and random polypropylene. From the viewpoint of basic performance of packaging materials such as heat seal strength, the polypropylene-based resin is preferably random polypropylene, and more preferably propylene-ethylene random copolymer. Since propylene-ethylene random copolymers have excellent heat sealability at low temperatures, the use of component (A) can suppress an increase in the heat seal temperature required to obtain sufficient heat seal strength, and more sufficient heat seal strength can be obtained at a heat seal temperature of about 200°C.

[0094] In the propylene-ethylene random copolymer, the ethylene content is preferably 0.1 to 10% by mass, more preferably 1 to 7% by mass, and even more preferably 2 to 5% by mass. When the ethylene content is 0.1% by mass or more, copolymerization of ethylene tends to provide impact resistance and improve seal strength and mold whitening resistance. When the ethylene content is 10% by mass or less, excessive lowering of the melting point tends to be prevented, and the occurrence of over-sealed portions tends to be more sufficiently prevented. The ethylene content can be calculated from the mixing ratio of the monomers during polymerization.

[0095] The melting point of the propylene-ethylene random copolymer is preferably 120 to 160° C., more preferably 125 to 160° C. When the melting point is 120° C. or higher, the occurrence of excess sealed portions tends to be more sufficiently suppressed.

[0096] The propylene-ethylene random copolymer may be acid-modified, for example, an acid-modified propylene-ethylene random copolymer graft-modified with maleic anhydride. By using the acid-modified propylene-ethylene random copolymer, adhesion to the tab lead can be maintained even without a tab sealant.

[0097] The propylene-ethylene random copolymers can be used alone or in combination of two or more.

[0098] ((C) component) To improve the compatibility between the (A) and (B) components, the sealant layer 16 may further contain, as the (C) component, a compatibilizer having a portion compatible with the (A) component and a portion compatible with the (B) component. The (C) component is preferably used when the (A) component is incompatible with the (B) component. When the (A) component is incompatible with the (B) component, the sealant layer 16 has a sea-island structure in which the (A) component is dispersed in the (B) component, which is the base resin. Adding the compatibilizer to the sea-island structure can improve the adhesion strength at the interface, thereby further improving the heat seal strength.

[0099] When the component (B) is a polypropylene-based resin such as a propylene-ethylene random copolymer, and the component (A) is a copolymer containing a polyethylene unit such as a polyamide / polyethylene graft copolymer or an ethylene / cycloolefin copolymer, a compatibilizer having a moiety compatible with the polypropylene-based resin and a moiety compatible with the copolymer containing the polyethylene unit can be used as the component (C).

[0100] Examples of component (C) include block copolymers composed of polyethylene units composed of polyethylene or ethylene-α-olefin copolymer and polypropylene units composed of polypropylene or propylene-α-olefin copolymer; block copolymers composed of polyethylene units and ethylene-butylene copolymer units; and block copolymers composed of polyethylene units and ethylene-1-octene copolymer units. Such block copolymers may have a diblock, triblock, or multiblock copolymer structure. When component (B) is the polypropylene-based resin and component (A) is a copolymer containing the polyethylene units, using the block copolymer as component (C) results in compatibility between the polypropylene-based resin (component (B)) and the polypropylene units, ethylene-butylene copolymer units, or ethylene-1-octene copolymer units of component (C), and compatibility between the polyethylene units of component (A) and the polyethylene units of component (C).

[0101] The above-mentioned compatibilizers may be used singly or in combination of two or more.

[0102] When the sealant layer 16 contains the (C) component, the content of the (C) component in the sealant layer 16 is preferably 1 to 40 parts by mass, more preferably 2 to 25 parts by mass, even more preferably 2 to 20 parts by mass, and particularly preferably 7 to 15 parts by mass, relative to 100 parts by mass of the total of the (A) and (B) components. When the (C) component content is 1 part by mass or more, it is easy to improve the adhesion strength of the sea-island interface, and it is easy to obtain an improved effect in heat seal strength. On the other hand, when the (C) component content is 40 parts by mass or less, it is easy to suppress a decrease in the cohesive strength and heat seal strength of the sealant layer 16 as a whole.

[0103] When the sealant layer 16 is composed of multiple layers, it is preferable that component (C) be added to all layers. However, if component (C) is added to at least one layer, the aforementioned effect of improving the heat seal strength can be obtained.

[0104] (Hydrogen sulfide adsorbent) The sealant layer 16 may further contain a hydrogen sulfide adsorbent. By including the hydrogen sulfide adsorbent in the sealant layer 16, hydrogen sulfide that may be generated in an all-solid-state battery using a sulfide-based solid electrolyte can be captured and rendered harmless by the sealant layer 16. Although the same effect as described above can be achieved even when the hydrogen sulfide adsorbent is added to the second adhesive layer 12b or the adhesive resin layer 15 described below, a more excellent hydrogen sulfide adsorption effect can be achieved by including the hydrogen sulfide adsorbent in the sealant layer 16, which is the innermost layer. When the substrate layer 11 side of the packaging material 10 is the outer side and the sealant layer 16 side is the inner side, the hydrogen sulfide adsorbent is preferably contained in at least one of the layers disposed inside the barrier layer 13. However, the hydrogen sulfide adsorbent may also be contained in at least one of the layers disposed outside the barrier layer 13. For example, the first adhesive layer 12a may contain the hydrogen sulfide adsorbent.

[0105] Examples of hydrogen sulfide adsorbents include zinc oxide, amorphous metal silicates (mainly those containing copper or zinc), hydrates of zirconium and lanthanoid elements, tetravalent metal phosphates (particularly those containing copper), mixtures of zeolite and zinc ions, mixtures of zeolite, zinc oxide, and copper(II) oxide, potassium permanganate, sodium permanganate, silver sulfate, and silver acetate. Among these, zinc oxide is preferred because it can more easily neutralize hydrogen sulfide and is cost-effective and easy to handle. The hydrogen sulfide adsorbents can be used singly or in combination.

[0106] When the sealant layer 16 contains a hydrogen sulfide adsorbing substance, the content of the hydrogen sulfide adsorbing substance in the sealant layer 16 is preferably 0.01 to 30 mass %, and more preferably 0.1 to 20 mass %, based on the total solid content of the sealant layer 16. If the content of the hydrogen sulfide adsorbing substance is less than 0.01 mass %, the effect of detoxifying hydrogen sulfide is small, whereas if it exceeds 30 mass %, the physical properties of the sealant layer 16, such as the sealing strength, tend to decrease.

[0107] (Additional ingredients) The sealant layer 16 may further contain additive components other than those described above. Examples of additive components include polyolefin elastomers. The polyolefin elastomer may be compatible or incompatible with component (B), and may contain both compatible polyolefin elastomers and incompatible polyolefin elastomers. "Compatible" means that the polyolefin elastomer disperses in component (B) with a dispersed phase size of 1 nm or more and less than 500 nm. "Incompatible" means that the polyolefin elastomer disperses in component (B) with a dispersed phase size of 500 nm or more and less than 20 μm.

[0108] When component (B) is a polypropylene resin, examples of the compatible polyolefin elastomer include propylene-butene-1 random copolymer, and examples of the incompatible polyolefin elastomer include ethylene-butene-1 random copolymer. The polyolefin elastomers can be used alone or in combination of two or more.

[0109] When the sealant layer 16 contains a polyolefin elastomer, the content of the polyolefin elastomer in the sealant layer 16 may be 5 to 40 mass % or 10 to 40 mass % based on the total solid content of the sealant layer 16. When the content of the polyolefin elastomer is 5 mass % or more, the effect of improving the sealing properties can be more sufficiently obtained, and when it is 40 mass % or less, a decrease in the heat resistance of the sealant layer 16 can be suppressed.

[0110] The sealant layer 16 may also contain additives such as slip agents, antiblocking agents, antioxidants, light stabilizers, and flame retardants. The content of these additives is preferably 5 parts by mass or less, assuming that the total mass of the sealant layer 16 is 100 parts by mass.

[0111] The thickness of the sealant layer 16 is not particularly limited, but from the viewpoint of the volumetric energy density of the battery, it is preferably in the range of 5 to 150 μm, more preferably in the range of 10 to 120 μm, and even more preferably in the range of 20 to 100 μm.

[0112] The above describes in detail a preferred embodiment of the exterior packaging material for a power storage device of this embodiment, but the present disclosure is not limited to such a specific embodiment, and various modifications and variations are possible within the scope of the gist of the present disclosure as set forth in the claims.

[0113] For example, Figure 1 shows a case where corrosion prevention treatment layers 14a and 14b are provided on both sides of the barrier layer 13, but only one of the corrosion prevention treatment layers 14a and 14b may be provided, or no corrosion prevention treatment layer may be provided.

[0114] While Fig. 1 shows a case where the barrier layer 13 and the sealant layer 16 are laminated using the second adhesive layer 12b, the barrier layer 13 and the sealant layer 16 may be laminated using an adhesive resin layer 15, as in the packaging material 20 for an electricity storage device shown in Fig. 2. Furthermore, in the packaging material 20 for an electricity storage device shown in Fig. 2, the second adhesive layer 12b may be provided between the barrier layer 13 and the adhesive resin layer 15.

[0115] <Adhesive resin layer 15> The adhesive resin layer 15 is generally composed of an adhesive resin composition as a main component and additive components as necessary. The adhesive resin composition is not particularly limited, but preferably contains a modified polyolefin resin.

[0116] The modified polyolefin resin is preferably a polyolefin resin graft-modified with an unsaturated carboxylic acid derivative derived from an unsaturated carboxylic acid, or an acid anhydride or ester thereof.

[0117] Examples of polyolefin resins include low-density polyethylene, medium-density polyethylene, high-density polyethylene, ethylene-α-olefin copolymer, homopolypropylene, block polypropylene, random polypropylene, and propylene-α-olefin copolymer.

[0118] The modified polyolefin resin is preferably a polyolefin resin modified with maleic anhydride. Suitable modified polyolefin resins include, for example, "Admer" manufactured by Mitsui Chemicals, Inc. and "Modic" manufactured by Mitsubishi Chemical Corporation. Such modified polyolefin resins have excellent reactivity with various metals and polymers having various functional groups, and this reactivity can be utilized to impart adhesion to the adhesive resin layer 15. Furthermore, the adhesive resin layer 15 may contain various additives, such as compatible and incompatible elastomers, flame retardants, slip agents, antiblocking agents, antioxidants, light stabilizers, and tackifiers, as needed.

[0119] The thickness of the adhesive resin layer 15 is not particularly limited, but is preferably the same as or smaller than that of the sealant layer 16 from the viewpoint of stress relaxation and moisture permeation.

[0120] In addition, in the packaging material 20 for a storage battery device, the total thickness of the adhesive resin layer 15 and the sealant layer 16 is preferably in the range of 5 to 150 μm, and more preferably in the range of 20 to 100 μm, from the viewpoint of achieving both a thin film and improved heat seal strength in a high-temperature environment.

[0121] [Exterior material manufacturing method] Next, a description will be given of an example of a method for manufacturing the packaging material 10 shown in Fig. 1. Note that the method for manufacturing the packaging material 10 is not limited to the following method.

[0122] The manufacturing method of the exterior material 10 of this embodiment is roughly composed of the steps of providing corrosion prevention treatment layers 14a, 14b on the barrier layer 13, bonding the base material layer 11 and the barrier layer 13 together using the first adhesive layer 12a, further laminating the sealant layer 16 via the second adhesive layer 12b to produce a laminate, and, if necessary, aging the obtained laminate.

[0123] (Step of Laminating Anti-Corrosion Treatment Layers 14a and 14b on Barrier Layer 13) This step is a step of forming corrosion prevention treatment layers 14a and 14b on the barrier layer 13. As described above, examples of the method for forming the corrosion prevention treatment layers 14a and 14b include degreasing treatment, hydrothermal treatment, anodizing treatment, and chemical conversion treatment on the barrier layer 13, and applying a coating agent having corrosion prevention properties.

[0124] Furthermore, when the corrosion prevention treatment layers 14a, 14b are multi-layered, for example, the coating liquid (coating agent) constituting the lower corrosion prevention treatment layer (barrier layer 13 side) may be applied to the barrier layer 13 and baked to form a first layer, and then the coating liquid (coating agent) constituting the upper corrosion prevention treatment layer may be applied to the first layer and baked to form a second layer.

[0125] Degreasing treatment can be performed by spraying or immersion. Hydrothermal conversion treatment and anodizing treatment can be performed by immersion. Chemical conversion treatment can be performed by immersion, spraying, coating, or other methods appropriately selected depending on the type of chemical conversion treatment.

[0126] As a method for applying a coating agent having corrosion prevention properties, various methods such as gravure coating, reverse coating, roll coating, and bar coating can be used.

[0127] As described above, the various treatments may be applied to either one or both sides of the metal foil, but in the case of one-side treatment, the treated side is preferably the side on which the sealant layer 16 is laminated. If desired, the above treatments may also be applied to the surface of the base layer 11.

[0128] The amount of coating agent applied to form the first layer and the second layer is 0.005 to 0.200 g / m 2 is preferable, and 0.010 to 0.100 g / m 2 is more preferred.

[0129] Furthermore, if dry curing is required, it can be carried out at a base material temperature in the range of 60 to 300° C. depending on the drying conditions of the corrosion prevention treatment layers 14a and 14b used.

[0130] (Step of bonding the base layer 11 and the barrier layer 13) This step is a step of bonding the barrier layer 13 provided with the corrosion prevention treatment layers 14a and 14b to the base material layer 11 via the first adhesive layer 12a. The bonding method may be dry lamination, non-solvent lamination, wet lamination, or the like, and the two are bonded together using the material that constitutes the first adhesive layer 12a described above. The first adhesive layer 12a has a dry coating amount of 1 to 10 g / m. 2 range, more preferably 3 to 7 g / m 2 It is set within the range.

[0131] (Laminating step of second adhesive layer 12b and sealant layer 16) This step is a step of bonding the sealant layer 16 via the second adhesive layer 12b to the second corrosion prevention treatment layer 14b side of the barrier layer 13. Examples of bonding methods include a wet process and dry lamination.

[0132] In the case of a wet process, a solution or dispersion of the adhesive that constitutes the second adhesive layer 12b is applied onto the second corrosion prevention treatment layer 14b, and the solvent is evaporated at a predetermined temperature (a temperature equal to or higher than the melting point of the adhesive if the adhesive contains an acid-modified polyolefin resin), followed by drying to form a film, or a baking process is performed as necessary after the drying to form a film. Thereafter, the sealant layer 16 is laminated to produce the exterior packaging material 10. Examples of the coating method include the various coating methods exemplified above.

[0133] In this case, the sealant layer 16 can be produced by a melt extrusion molding machine using a resin composition for forming a sealant layer, which contains the above-mentioned components (A) and (B), and optionally the component (C), a hydrogen sulfide adsorbent, and additional components, etc. From the viewpoint of productivity, the processing speed of the melt extrusion molding machine can be set to 80 m / min or more.

[0134] (Aging treatment process) This step is a step of aging (curing) the laminate. By aging the laminate, it is possible to promote adhesion between the barrier layer 13, the second corrosion prevention treatment layer 14b, the second adhesive layer 12b, and the sealant layer 16. The aging treatment can be carried out at a temperature ranging from room temperature to 100°C. The aging time is, for example, 1 to 10 days.

[0135] In this manner, the packaging material 10 of this embodiment as shown in FIG. 1 can be manufactured.

[0136] Next, a description will be given of an example of a method for manufacturing the exterior packaging material 20 shown in Fig. 2. Note that the method for manufacturing the exterior packaging material 20 is not limited to the following method.

[0137] The manufacturing method of the packaging material 20 of this embodiment is generally composed of the steps of providing corrosion prevention treatment layers 14a, 14b on the barrier layer 13, bonding the base material layer 11 and the barrier layer 13 together using the first adhesive layer 12a, further laminating the adhesive resin layer 15 and the sealant layer 16 to prepare a laminate, and, if necessary, heat treating the obtained laminate. Note that the steps up to the step of bonding the base material layer 11 and the barrier layer 13 can be carried out in the same manner as the manufacturing method of the packaging material 10 described above.

[0138] (Laminating Step of Adhesive Resin Layer 15 and Sealant Layer 16) This step is a step of forming an adhesive resin layer 15 and a sealant layer 16 on the second corrosion prevention treatment layer 14b formed in the previous step. Examples of methods include sand lamination of the adhesive resin layer 15 together with the sealant layer 16 using an extrusion laminator. Furthermore, lamination can also be performed using a tandem lamination method or a co-extrusion method in which the adhesive resin layer 15 and the sealant layer 16 are extruded. When forming the adhesive resin layer 15 and the sealant layer 16, for example, the components are blended so as to satisfy the above-described structures of the adhesive resin layer 15 and the sealant layer 16. The above-described resin composition for forming a sealant layer is used to form the sealant layer 16.

[0139] This process produces a laminate in which the layers are stacked in the following order: base layer 11 / first adhesive layer 12a / first corrosion prevention treatment layer 14a / barrier layer 13 / second corrosion prevention treatment layer 14b / adhesive resin layer 15 / sealant layer 16, as shown in Figure 2.

[0140] The adhesive resin layer 15 may be formed by directly extruding dry-blended materials having the above-described material composition using an extrusion laminator. Alternatively, the adhesive resin layer 15 may be formed by extruding granules obtained by previously melt-blending the materials using a melt-kneading device such as a single-screw extruder, a twin-screw extruder, or a Brabender mixer, and then extruding the granules using an extrusion laminator.

[0141] The sealant layer 16 may be formed by directly extruding materials dry-blended to the composition described above as the constituent components of the resin composition for forming a sealant layer using an extrusion laminator. Alternatively, the adhesive resin layer 15 and the sealant layer 16 may be formed by a tandem lamination method in which the granules obtained by melt-blending the resin composition using a melt-kneading device such as a single-screw extruder, a twin-screw extruder, or a Brabender mixer are extruded into the adhesive resin layer 15 and the sealant layer 16 using an extrusion laminator, or by a co-extrusion method. Alternatively, a sealant monolayer may be formed in advance as a cast film using the resin composition for forming a sealant layer, and this film may be laminated together with an adhesive resin by sand lamination. The formation speed (processing speed) of the adhesive resin layer 15 and the sealant layer 16 may be, for example, 80 m / min or more from the viewpoint of productivity.

[0142] (Heat treatment process) This step is a step of heat-treating the laminate. Heat-treating the laminate can improve adhesion between the barrier layer 13, the second corrosion prevention treatment layer 14b, the adhesive resin layer 15, and the sealant layer 16. As a method of heat treatment, it is preferable to treat at a temperature at least equal to or higher than the melting point of the adhesive resin layer 15.

[0143] In this manner, the exterior packaging material 20 of this embodiment as shown in FIG. 2 can be manufactured.

[0144] The above describes in detail preferred embodiments of the exterior packaging material for a power storage device of the present disclosure, but the present disclosure is not limited to such specific embodiments, and various modifications and variations are possible within the scope of the gist of the present disclosure as set forth in the claims.

[0145] The packaging material for an electricity storage device according to the present disclosure can be suitably used as a packaging material for an electricity storage device such as a secondary battery such as a lithium ion battery, a nickel-metal hydride battery, or a lead-acid battery, and an electrochemical capacitor such as an electric double layer capacitor. In particular, the packaging material for an electricity storage device according to the present disclosure is suitable as a packaging material for an all-solid-state battery using a solid electrolyte.

[0146] [Electricity storage device] FIG. 3 is a perspective view showing one embodiment of an electricity storage device fabricated using the above-described exterior material. As shown in FIG. 3, the electricity storage device 50 includes a battery element (electricity storage device main body) 52, two metal terminals (current extraction terminals) 53 for extracting current from the battery element 52 to the outside, and an exterior material 10 that hermetically encases the battery element 52. The exterior material 10 is the exterior material 10 according to the present embodiment described above. In the exterior material 10, the base material layer 11 is the outermost layer, and the sealant layer 16 is the innermost layer. That is, the exterior material 10 is configured to encase the battery element 52 by folding one laminate film in half and heat-sealing it, or by overlapping and heat-sealing two laminate films, so that the base material layer 11 is on the exterior side of the electricity storage device 50 and the sealant layer 16 is on the interior side of the electricity storage device 50. Note that the electricity storage device 50 may use an exterior material 20 instead of the exterior material 10.

[0147] Battery element 52 has an electrolyte interposed between a positive electrode and a negative electrode. Metal terminal 53 is a part of the current collector that is taken out from exterior packaging 10, and is made of metal foil such as copper foil or aluminum foil.

[0148] The electricity storage device 50 of this embodiment may be an all-solid-state battery. In this case, a solid electrolyte such as a sulfide-based solid electrolyte is used as the electrolyte of the battery element 52. The electricity storage device 50 of this embodiment uses the packaging material 10 of this embodiment, and therefore can ensure excellent heat seal strength even when used in a high-temperature environment. [Example]

[0149] Hereinafter, the present disclosure will be described more specifically based on examples, but the present disclosure is not limited to the following examples.

[0150] [Materials used] The materials used in the examples and comparative examples are shown below.

[0151] <Base layer (thickness 25 μm)> A polyethylene terephthalate film was used, one side of which had been subjected to a corona treatment.

[0152] <First adhesive layer (thickness 4 μm)> A polyurethane adhesive (manufactured by Toyo Ink Co., Ltd.) containing a polyester polyol-based base resin and a tolylene diisocyanate adduct curing agent was used.

[0153] <First corrosion prevention treatment layer (base layer side) and second corrosion prevention treatment layer (sealant layer side)> (CL-1): "Sodium polyphosphate-stabilized cerium oxide sol" was used, adjusted to a solids concentration of 10% by mass using distilled water as the solvent. The sodium polyphosphate-stabilized cerium oxide sol was obtained by blending 100 parts by mass of cerium oxide with 10 parts by mass of sodium phosphate. (CL-2): A composition consisting of 90% by mass of "polyallylamine (manufactured by Nitto Boseki Co., Ltd.)" adjusted to a solid content concentration of 5% by mass using distilled water as a solvent and 10% by mass of "polyglycerol polyglycidyl ether (manufactured by Nagase ChemteX Corporation)" was used.

[0154] <Barrier layer (thickness 40 μm)> Annealed and degreased soft aluminum foil (manufactured by Toyo Aluminum Co., Ltd., "8079 material") was used.

[0155] <Second adhesive layer (thickness 3 μm)> An epoxy adhesive was used, prepared by diluting a mixture of 100 parts by mass of epoxy resin (manufactured by Adeka Corporation, product name: EP4100) and 25 parts by mass of polyamidoamine curing agent (manufactured by Adeka Corporation, product name: EH4602) with ethyl acetate to a solids content of 30% by mass.

[0156] <Sealant layer> The following materials were prepared as components constituting the resin composition for forming a sealant layer.

[0157] ((B) component) B-1: Propylene-ethylene random copolymer (glass transition temperature: -5°C, melting point: 135°C). B-2: Branched low-density polyethylene resin (glass transition temperature: -125°C, melting point: 105°C).

[0158] (Component (A)) A-1: Aporya LP2 (trade name, manufactured by Arkema, melting point: 216°C) A-2: APL6013T (product name, manufactured by Mitsui Chemicals, Inc., glass transition temperature: 125°C) A-3: APL6509T (product name, manufactured by Mitsui Chemicals, Inc., glass transition temperature: 80°C)

[0159] (Component (A')) A'-1: Aporya LC3 (trade name, manufactured by Arkema, melting point: 130°C, glass transition temperature: none) A'-2: Vylon RN-9300 (product name, Toyobo Co., Ltd., melting point: 198°C, glass transition temperature: 73°C, crystalline polyester resin containing no polyolefin units)

[0160] ((C) component) C-1: INTUNE (product name, manufactured by DOW) C-2: DYNARON (product name, manufactured by JSR) C-3: BIOLLOY NM110NP (product name, manufactured by JSR Corporation, polyester / polyolefin compatibilizer)

[0161] (Hydrogen sulfide adsorbent) Zinc oxide (Sakai Chemical Industry Co., Ltd.)

[0162] [Fabrication of exterior materials] Example 1 First, first and second corrosion prevention treatment layers were formed on the barrier layer by the following procedure: (CL-1) was applied to both surfaces of the barrier layer in a dry coating amount of 70 mg / m 2 The resulting layer was coated by microgravure coating so that the coating amount was 20 mg / m, and then baked in a drying unit at 200°C. 2By applying the coating by microgravure coating so that the coating was as follows, a composite layer consisting of (CL-1) and (CL-2) was formed as the first and second corrosion prevention treatment layers. This composite layer exhibits corrosion prevention performance by combining the two types of (CL-1) and (CL-2).

[0163] Next, the first corrosion prevention treatment layer side of the barrier layer provided with the first and second corrosion prevention treatment layers was attached to the substrate layer by dry lamination using a polyurethane adhesive (first adhesive layer). Next, the second corrosion prevention treatment layer side of the barrier layer provided with the first and second corrosion prevention treatment layers was attached by dry lamination using an epoxy adhesive (second adhesive layer) to a sealant layer (80 μm thick) that had been previously formed as a cast film, thereby producing an exterior material (a laminate of substrate layer / first adhesive layer / first corrosion prevention treatment layer / barrier layer / second corrosion prevention treatment layer / second adhesive layer / sealant layer). The sealant layer was formed using a resin composition for forming a sealant layer having the composition shown in Table 1. The barrier layer and sealant layer were laminated by applying an epoxy adhesive to the second corrosion prevention treatment layer side of the barrier layer in an amount (mass per unit area) of 3 g / m after drying. 2 (thickness 3 μm), dried at 80°C for 1 minute, laminated with a sealant layer, and aged at 120°C for 3 hours. The numerical values ​​in the column for sealant layer in Table 1 indicate the content (unit: parts by mass) of each component in the resin composition for forming a sealant layer. The content of each component in the formed sealant layer is equal to the content of each component in the resin composition for forming a sealant layer.

[0164] (Examples 2 to 8 and 11 to 13) Except for changing the composition of the resin composition for forming the sealant layer as shown in Table 1, the exterior materials of Examples 2 to 8 and 11 to 13 (laminates of substrate layer / first adhesive layer / first corrosion prevention treatment layer / barrier layer / second corrosion prevention treatment layer / second adhesive layer / sealant layer) were produced in the same manner as in Example 1.

[0165] Example 9 The exterior material of Example 9 (a laminate of substrate layer / first adhesive layer / barrier layer / second adhesive layer / sealant layer) was produced in the same manner as in Example 5, except that the first and second corrosion prevention treatment layers were not provided on the barrier layer.

[0166] Example 10 An exterior material of Example 10 (a laminate of substrate layer / first adhesive layer / barrier layer / second adhesive layer / sealant layer) was produced in the same manner as in Example 9, except that a hydrogen sulfide-adsorbing substance was added to the resin composition for forming a sealant layer as shown in Table 1.

[0167] (Comparative Examples 1 to 5) Except for changing the composition of the resin composition for forming the sealant layer as shown in Table 1, the exterior materials of Comparative Examples 1 to 5 (laminates of substrate layer / first adhesive layer / first corrosion prevention treatment layer / barrier layer / second corrosion prevention treatment layer / second adhesive layer / sealant layer) were prepared in the same manner as in Example 1.

[0168] [Heat seal strength measurement] The packaging material was cut into a size of 120 mm x 60 mm, folded in half so that the sealant layer was on the inside, and the end opposite the folded part was heat-sealed over a width of 10 mm at 0.5 MPa for 3 seconds at the heat-sealing temperature shown in Table 1. Note that the heat-sealing temperatures in Comparative Examples 1 to 3 were set lower than those in the other examples in accordance with the composition of the sealant layer. This was because when the packaging materials of Comparative Examples 1 to 3 were heat-sealed at 220°C, the sealant layer would flow too much, causing the sealant layer thickness in the sealed area to become too thin, which could result in problems with insulation, etc.

[0169] Next, the heat-sealed packaging material was stored at room temperature for 6 hours, and then a 15 mm wide x 30 mm long sample was cut out from the longitudinal center of the heat-sealed portion (see Figure 4) to prepare a sample for measuring heat-seal strength. This sample was then left in a test environment at room temperature (25°C) and 150°C for 5 minutes, after which a T-peel test was performed on the heat-sealed portion of the sample using a tensile tester (manufactured by Shimadzu Corporation) at a pulling rate of 50 mm / min under these temperature conditions. This allowed for the measurement of heat-seal strength under room temperature and high-temperature environments. The heat-seal strength obtained was then evaluated according to the following criteria: A or B indicates passing, and C indicates failing. The results are shown in Table 1. A: Heat seal strength at room temperature and at 150°C is 35N / 15mm or more B: Heat seal strength at room temperature is 35N / 15mm or more, or heat seal strength at 150℃ is 20N / 15mm or more C: At least one of the heat seal strengths at room temperature and at 150°C is less than 20N / 15mm

[0170] [Measurement of H2S adsorption] A 10 cm2 sealant layer formed using the resin composition for forming a sealant layer having the composition shown in Table 1 was placed in a Tedlar (registered trademark) bag with a capacity of 2 L. 2 A sample of an 80 μm-thick sealant layer was sealed inside the bag. 2 L of 5 ppm hydrogen sulfide gas by volume was poured into the bag, and the bag was left at room temperature (25°C) for 24 hours. The hydrogen sulfide concentration was then measured using a gas detector tube. The lower the hydrogen sulfide concentration, the better the H2S adsorption ability of the sealant layer. The results are shown in Table 1.

[0171] [Table 1] [Industrial Applicability]

[0172] According to the present disclosure, there are provided an exterior packaging material for a power storage device that has excellent heat resistance and can ensure excellent heat seal strength even in a high-temperature environment, and a power storage device using the same. [Explanation of symbols]

[0173] 10, 20...outer packaging material for electricity storage device, 11...substrate layer, 12a...first adhesive layer, 12b...second adhesive layer, 13...barrier layer, 14a...first corrosion prevention treatment layer, 14b...second corrosion prevention treatment layer, 15...adhesive resin layer, 16...sealant layer, 50...electricity storage device, 52...battery element, 53...metal terminal.

Claims

1. An exterior material for an electricity storage device comprising at least a base layer, a barrier layer, and a sealant layer in this order, The sealant layer comprises: (A) a compound containing a polyolefin unit and having a melting point of 175° C. or higher or a glass transition temperature of 75° C. or higher; Component (B): at least one resin selected from the group consisting of polyethylene-based resins and polypropylene-based resins; Component (C): a compatibilizer having a portion compatible with component (A) and a portion compatible with component (B); Contains The exterior material for an electricity storage device, wherein the component (A) is incompatible with the component (B).

2. The component (A) contains a polyamide / polyolefin graft copolymer, 2. The exterior material for a storage battery device according to claim 1, wherein a content of the component (A) in the sealant layer is 5 to 100 parts by mass per 100 parts by mass of the component (B).

3. The component (A) contains a cycloolefin copolymer, 2. The exterior material for a storage battery device according to claim 1, wherein a content of the component (A) in the sealant layer is 5 to 100 parts by mass per 100 parts by mass of the component (B).

4. The packaging material for a power storage device according to any one of claims 1 to 3, wherein a corrosion prevention treatment layer is provided on one or both surfaces of the barrier layer.

5. 5. The packaging material for a storage battery device according to claim 1, wherein, when the base material layer side of the packaging material for a storage battery device is an outer side and the sealant layer side is an inner side, at least one of layers arranged on the inner side of the barrier layer contains a hydrogen sulfide adsorption substance.

6. The packaging material for a storage battery device according to any one of claims 1 to 5, wherein the sealant layer has a thickness of 10 to 100 µm.

7. The exterior material for a storage battery device according to any one of claims 1 to 6, which is for an all-solid-state battery.

8. A power storage device main body; a current extracting terminal extending from the power storage device body; The exterior material for an electricity storage device according to any one of claims 1 to 7, which holds the current extracting terminal and houses the electricity storage device main body; A power storage device comprising:

Citation Information

Patent Citations

  • One-piece type leak-proof battery

    JP1999162418A

  • Packaging material for lithium ion battery

    JP2004319414A

  • Mixture of polyamide block graft copolymer and flexible polyolefin

    JP2004510865A

  • All-solid battery for household electric appliance

    JP2008103292A

  • Battery packaging material

    JP2013206878A