Joined body and electrostatic chuck
A joined body with controlled thermal expansion and reduced contact area between materials in a composite member minimizes thermal stress, addressing deformation and damage issues in electrostatic chucks.
Patent Information
- Application Number
- JP2023060570
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-04
- Publication Date
- 2024-10-17
AI Technical Summary
Existing joined bodies with materials having different thermal expansion coefficients suffer from deformation and damage due to thermal stress, particularly in applications like electrostatic chucks, where thermal expansion differences between materials like porous materials and metals cause joint defects.
A joined body comprising a ceramic member and a composite member made of multiple materials with controlled thermal expansion differences and particle sizes, where the thermal expansion coefficient difference is 10 ppm/K or more, and the particle size of the first material is 50 μm or less, with reduced contact length between materials to minimize thermal stress.
The solution effectively suppresses deformation and damage to the joined body by reducing thermal stress, ensuring durability and reliability, especially in electrostatic chucks, by controlling thermal expansion and contact area between materials.
Smart Images

Figure 2024147873000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a joint and an electrostatic chuck. [Background technology]
[0002] A bonded body in which two members having different thermal expansion coefficients are bonded to each other has been known. For example, Patent Document 1 discloses a bonded body in which a ceramic member is bonded to a base made of a combination of a porous material having a low thermal expansion coefficient and a metal material. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 11-163109 Summary of the Invention [Problem to be solved by the invention]
[0004] However, even with the prior art such as Patent Document 1, there is still room for improvement in the technology for suppressing damage to the bonded body due to the thermal expansion difference. For example, in the base of the bonded body of Patent Document 1, since the pores of the porous material are filled with a metal material, there is a thermal expansion difference between the porous material and the metal material in the base. For example, when the bonded body is used for a long time, the dimensions of the base change due to the thermal expansion difference between the porous material and the metal material, and the base is deformed. If the base is deformed, there is a problem in the bond with the ceramic member, and the bonded body may be damaged, so there has been a demand for a technology for suppressing damage to the bonded body due to the thermal expansion difference.
[0005] An object of the present invention is to provide a technique for suppressing breakage in a bonded structure. [Means for solving the problem]
[0006] The present invention has been made to solve at least part of the above-mentioned problems, and can be realized in the following forms.
[0007] (1) According to one aspect of the present invention, there is provided a joined body in which a ceramic member and a composite member are joined together, the composite member of this joined body includes a plurality of materials, a difference between a thermal expansion coefficient of a first material having a minimum thermal expansion coefficient and a thermal expansion coefficient of a second material having a maximum thermal expansion coefficient among the plurality of materials is 10 ppm / K or more, and a particle size of the first material included in a cross section of the composite member is 50 μm or less.
[0008] According to this configuration, the composite member bonded to the ceramic member in the bonded body contains multiple types of materials. Among the multiple types of materials contained in the composite member, the difference between the thermal expansion coefficient of the first material having the smallest thermal expansion coefficient and the thermal expansion coefficient of the second material having the largest thermal expansion coefficient is 10 ppm / K or more, and the particle size of the particles made of the first material contained in the cross section of the composite member is 50 μm or less. In this way, even if there is a relatively large difference in thermal expansion coefficient between the multiple types of materials contained in the composite member, by making the particle size of the first material having a relatively small thermal expansion coefficient relatively small, the thermal stress generated in the composite member due to the thermal expansion difference is reduced. As a result, the deformation of the composite member is suppressed, and therefore the damage to the bonded body due to the deformation of the composite member can be suppressed.
[0009] (2) In the bonded body of the above embodiment, the length of the portion where the first material and the second material are in contact in the cross section may be less than 100 μm. According to this configuration, the length of the portion where the first material and the second material are in contact in the cross section of the composite member is relatively short, less than 100 μm. That is, the contact area between the first material and the second material is relatively small. When the contact area is small, the thermal stress generated due to the difference in thermal expansion is also small, so that the deformation of the composite member is further suppressed. Therefore, the damage of the bonded body can be further suppressed.
[0010] (3) In the bonded body of the above embodiment, the thermal expansion coefficient of the second material may be 30 ppm / K or less. With this configuration, the thermal expansion coefficient of the second material having the maximum thermal expansion coefficient is reduced, so that the difference between the thermal expansion coefficient of the second material having the maximum thermal expansion coefficient and the thermal expansion coefficient of the first material having the minimum thermal expansion coefficient is reduced, and the thermal stress generated in the composite member is also reduced. This further suppresses deformation of the composite member, and therefore further suppresses damage to the bonded body.
[0011] (4) In the bonded structure of the above embodiment, the thermal expansion coefficient of the first material may be 3 ppm / K or more. With this configuration, the thermal expansion coefficient of the first material having the smallest thermal expansion coefficient is increased, so that the difference between the thermal expansion coefficient of the first material and the thermal expansion coefficient of the second material having the largest thermal expansion coefficient is reduced, and the thermal stress generated in the composite member is also reduced. This further suppresses deformation of the composite member, and therefore further suppresses damage to the bonded structure.
[0012] (5) In the bonded structure of the above embodiment, the composite member may contain the first material at 50% by volume or more. With this configuration, the first material, which has a small thermal expansion coefficient, occupies a large portion of the composite member. This suppresses dimensional changes in the composite member, thereby further suppressing damage to the bonded structure.
[0013] (6) According to another aspect of the present invention, there is provided an electrostatic chuck. The electrostatic chuck includes the above-mentioned bonded body, the ceramic member has a chuck electrode, and the composite member has a cooling function. According to this configuration, the electrostatic chuck holds an object using the chuck electrode of the ceramic member. At this time, heat generated in the ceramic member is transferred to the composite member, and the composite member repeats expansion and contraction due to temperature changes. In the composite member, the thermal stress generated due to the difference in thermal expansion between the first material and the second material is small, so that dimensional changes in the composite member are suppressed even when used for a long period of time. This makes it possible to suppress damage to the electrostatic chuck.
[0014] The present invention can be realized in various forms, for example, in the form of a method for manufacturing a composite member, a structure including a composite member, a method for manufacturing a joined body, an apparatus including a joined body, etc. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 is a perspective view of an electrostatic chuck according to a first embodiment. [Diagram 2] 1 is a cross-sectional view of an electrostatic chuck according to a first embodiment. [Diagram 3] 3 is a cross-sectional photograph of a composite member according to the first embodiment. [Figure 4] 1 is a schematic cross-sectional view of a composite member according to a first embodiment. FIG. [Diagram 5] FIG. 13 is a diagram illustrating the results of an evaluation test of a composite material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] First Embodiment FIG. 1 is a perspective view of an electrostatic chuck 100 according to a first embodiment. FIG. 2 is a cross-section of the electrostatic chuck 100 according to the first embodiment. The electrostatic chuck 100 according to the first embodiment is provided in, for example, an etching device, and holds a wafer W by electrostatic attraction. The electrostatic chuck 100 includes a bonded body 1 having a ceramic member 10, a composite member 20, and a bonding portion 30. As shown in FIG. 1, the bonded body 1 is stacked in the order of the ceramic member 10, the bonding portion 30, and the composite member 20 from the positive side in the z-axis direction (stacking direction). In this embodiment, the bonded body 1 is a columnar body having a substantially circular cross-sectional shape perpendicular to the stacking direction. Note that FIG. 1 and FIG. 2 show the arrangement of each part in a schematic manner, and do not show the exact ratio of the dimensions of each part.
[0017] The ceramic member 10 is a substantially circular flat plate member made of alumina (Al2O3). The ceramic member 10 has a pair of main surfaces 10a, 10b (see FIG. 2). One of the pair of main surfaces 10a, 10b, the main surface 10a, is formed with a mounting surface on which a wafer W is mounted. The wafer W mounted on the mounting surface is attracted and fixed to the mounting surface by electrostatic attraction generated by a chuck electrode 11 of the ceramic member 10. A heater electrode (not shown) for heating the wafer W attracted and fixed to the mounting surface may be built in the ceramic member 10. The material for forming the ceramic member 10 may be aluminum nitride (AlN), zirconia (ZrO2), silicon nitride (Si3N4), silicon carbide (SiC), yttria (Y2O3), or the like.
[0018] The composite member 20 includes a plurality of types of materials. The composite member 20 includes silicon carbide (SiC) as a "first material" having the smallest thermal expansion coefficient among the plurality of types of materials included in the composite member 20, and aluminum (Al) as a "second material" having the largest thermal expansion coefficient. The thermal expansion coefficient of silicon carbide is 4.5 ppm / K, which is 3 ppm / K or more, and the thermal expansion coefficient of aluminum is 22 ppm / K, which is 30 ppm / K or less. As a result, in the composite member 20, the difference between the thermal expansion coefficient of silicon carbide and the thermal expansion coefficient of aluminum is 17.5 ppm / K, which is 10 ppm / K or more. The composite member 20 includes silicon carbide at 50 volume % or more. In this embodiment, the composite member 20 includes silicon carbide at 70 volume % and aluminum at 30 volume %. As a result, the thermal conductivity of the composite member 20 is 80 W / (m·K) or more. 2, the composite member 20 has a plurality of coolant flow paths 21 for allowing a coolant to flow therethrough, as a cooling function. In the electrostatic chuck 100, the composite member 20 functions as a heat dissipation base having electrical conductivity.
[0019] The joint 30 is disposed between the ceramic member 10 and the composite member 20. The joint 30 is made of gold (Au), silver (Ag), copper (Cu), nickel (Ni), platinum (Pt), palladium (Pd), or an alloy containing at least one of these metals. The joint 30 metallurgically joins the ceramic member 10 and the composite member 20. This can improve the thermal conductivity between the ceramic member 10 and the composite member 20. Note that the method for joining the ceramic member 10 and the composite member 20 is not limited to this.
[0020] Next, the features of the joined body 1 of this embodiment will be described. As described above, the composite member 20 included in the joined body 1 of this embodiment is made of multiple types of materials with different thermal expansion coefficients. Among the multiple types of materials included in the composite member 20, the difference between the thermal expansion coefficient of the first material (silicon carbide) having the smallest thermal expansion coefficient and the thermal expansion coefficient of the second material (aluminum) having the largest thermal expansion coefficient is 10 ppm / K or more. In the cross section of the composite member 20, the grains made of the first material (silicon carbide) have a grain size of 50 μm or less.
[0021] Fig. 3 is a cross-sectional photograph of the composite member 20 of this embodiment. Fig. 3 shows an example of a cross-sectional photograph of the composite member 20 taken using a scanning electron microscope (SEM), and is a photograph taken at a magnification of 500 times within a field of view of 550 μm × 750 μm. In the cross-sectional photograph shown in Fig. 3, the dark-colored portion A11 is a grain made of silicon carbide, and the light-colored portion A12 is aluminum.
[0022] FIG. 4 is a schematic cross-sectional view of the composite member 20 of the present embodiment. FIG. 4 is a diagram showing the relationship between silicon carbide and aluminum in the cross section of the composite member 20 based on the cross-sectional photograph shown in FIG. 3. In the composite member 20, as shown in FIG. 4, the particle size of the silicon carbide particles A11 included in the cross section is 50 μm or less. Here, the "particle size" refers to the longest distance between two points on the outline of the particles in the cross section. For example, in the silicon carbide particles A111 shown in FIG. 4, the longest distance D111 between two points on the outline L111 of the cross section is the particle size of the silicon carbide particles A111. Note that, as shown in FIG. 4, when a cross section includes a plurality of silicon carbide particles, the "particle size" of silicon carbide included in the cross section is the value (average particle size) obtained by dividing the sum of the particle sizes of the plurality of silicon carbide particles included in the cross section by the number of silicon carbide particles included in the cross section. The particle size of the silicon carbide particles can be calculated by performing image analysis on a cross-sectional photograph taken by the SEM method, such as that shown in FIG.
[0023] In the composite member 20 of the present embodiment, the length of the portion where silicon carbide and aluminum are in contact in the cross section is less than 100 μm. Here, the "portion where silicon carbide and aluminum are in contact" refers to the portion where the silicon carbide grains and aluminum are in contact without voids or impurities. For example, in the silicon carbide grains A112 shown in FIG. 4, the length of the two-dot chain line L112 indicating the portion where the aluminum A122 around the grains A112 and the silicon carbide grains A112 are in contact is less than 100 μm. Note that, as shown in FIG. 4, when the cross section includes a plurality of silicon carbide grains, the "length of the portion where silicon carbide and aluminum are in contact" refers to the sum of the lengths of the portions of the plurality of silicon carbide grains included in the cross section that are in contact with aluminum, divided by the number of silicon carbide grains included in the cross section (average length). The length of the portion where silicon carbide and aluminum are in contact in the cross section can be calculated by performing image analysis on a cross-sectional photograph taken by SEM, in the same manner as the particle size of the silicon carbide grains.
[0024] In the composite member 20 of this embodiment, as described above, the length of the portion where the silicon carbide and aluminum are in contact in the cross section is less than 100 μm. This makes the difference between the change in size of the silicon carbide and the change in size of the aluminum due to thermal expansion, i.e., the thermal expansion difference, relatively small, and therefore the thermal stress generated due to the thermal expansion difference is relatively small. Therefore, deformation of the composite member 20 due to thermal stress can be suppressed, and damage to the joined body 1 can be suppressed.
[0025] Next, a method for manufacturing the composite member 20 will be described. In a first manufacturing method for the composite member 20, first, a porous body is manufactured using silicon carbide powder. Next, the manufactured porous body is machined and formed into a predetermined shape. The porous body formed into a predetermined shape and aluminum are set in a mold and hot pressed, so that the interior of the porous body is impregnated with molten aluminum. In this way, the composite member 20 is completed. In the composite member 20 of this embodiment, by adjusting the particle size of the silicon carbide powder when manufacturing the porous body, it is possible to make the particle size of the silicon carbide particles contained in the cross section 50 μm or less, and to make the length of the portion where the silicon carbide and aluminum are in contact in the cross section shorter than 100 μm.
[0026] In the second manufacturing method of the composite member 20, first, a predetermined amount of silicon carbide powder and aluminum powder are mixed. At this time, the silicon carbide powder and the aluminum powder may be mixed together with an organic binder. Next, the mixed powder is sintered by hot pressing to complete the composite member 20. In the second manufacturing method as well, by adjusting the particle size of the silicon carbide powder mixed with the aluminum powder, it is possible to make the particle size of the silicon carbide particles contained in the cross section 50 μm or less, and to make the length of the portion where the silicon carbide and the aluminum are in contact in the cross section shorter than 100 μm.
[0027] Next, an evaluation test of the composite member will be described. In this evaluation test, the relationship between the type of material contained in the composite member and the deformation amount of the composite member was evaluated.
[0028] In this evaluation test, a composite member sample having a length of 40 mm and a cross-sectional shape of a square with sides of 5 mm was produced according to the above-mentioned manufacturing method for composite member 20. In this evaluation test, the materials contained in the sample were combined with the material having the smallest thermal expansion coefficient and the material having the largest thermal expansion coefficient, and the composition was changed to investigate the effect of the material combination or composition on the deformation amount due to thermal expansion of the sample.
[0029] In this evaluation test, the dimensional change of the sample was measured in a heat cycle test in which the sample was left at -50°C for 20 minutes, and then left at 150°C for 35 minutes, repeated 300 times. In this evaluation test, the rate of change in dimension after the heat cycle test compared to the dimension before the heat cycle test was calculated for each of multiple samples, and the calculated rate of change was classified into the following three levels. Less than 0.05(%): Rating A 0.05(%) or more but less than 0.1(%): Grade B 0.1(%) or more: Rating C
[0030] FIG. 5 is a diagram illustrating the results of the evaluation test of the composite member. In this evaluation test, the deformation amount was evaluated using 15 types of samples. In FIG. 5, for each of the 15 types of samples, the "composition (vol%)" of the material contained in the sample, the first material "M1" having the smallest thermal expansion coefficient among the materials contained in the sample, the thermal expansion coefficient of the first material "CTE_M1 (ppm / K)", the second material "M2" having the largest thermal expansion coefficient among the materials contained in the sample, and the thermal expansion coefficient of the second material "CTE_M2 (ppm / K)". In addition, FIG. 5 shows the difference "ΔCTE (ppm / K)" between the thermal expansion coefficient of the first material and the thermal expansion coefficient of the second material, the "particle size (μm)" of the particles made of the first material, the "contact length (μm)" which is the length of contact between the first material and the second material in the cross section of the sample, and the "evaluation result" based on the above-mentioned evaluation rule.
[0031] Regarding the particle size of the first material in the cross section of the sample, Sample 1, which has the same composition "Al-70SiC" and a particle size of 90 μm, was compared with Samples 2 and 3, which have particle sizes of 40 μm or 50 μm. As a result, Sample 1 was rated C, while Samples 2 and 3 were rated B or A. This revealed that by setting the particle size of the first material to 50 μm or less, the dimensional change of the composite material can be suppressed. Furthermore, as a result of comparing Sample 2, which has a particle size of 50 μm, with Sample 3, which has a particle size of 40 μm, Sample 2 was rated B, while Sample 3 was rated A. This revealed that by setting the particle size of the first material to 40 μm or less, the dimensional change of the composite material can be further suppressed.
[0032] Regarding the contact length between the first and second materials in the cross section of the sample, Sample 1, which has the same composition "Al-70SiC" and a contact length of 100 μm, was compared with Samples 2 and 3, which have a contact length of 50 μm or 60 μm. As a result, Sample 1 was rated C, while Samples 2 and 3 were rated B or A. From this result, it became clear that by making the contact length between the first and second materials in the cross section smaller than 100 μm, the dimensional change of the composite material can be suppressed. Furthermore, as a result of comparing Sample 2, which has a contact length of 60 μm, with Sample 3, which has a contact length of 50 μm, Sample 2 was rated B, while Sample 3 was rated A. From this result, it became clear that by making the contact length between the first and second materials in the cross section smaller, the dimensional change of the composite material can be further suppressed.
[0033] The thermal expansion coefficient of the first material having the smallest thermal expansion coefficient was compared among Sample 7 of "Mg-70SiC", Sample 13 of "Mg-70Si3N4", Sample 14 of "Mg-70AlN", and Sample 15 of "Mg-70Al2O3". Among the first materials silicon carbide, silicon nitride, aluminum nitride, and alumina, silicon nitride has a thermal expansion coefficient of 2.3 ppm / K, which is smaller than 3 ppm / K, and silicon carbide, aluminum nitride, and alumina all have a thermal expansion coefficient of 3 ppm / K or more (SiC: 4.5 ppm / K, AlN: 4.6 ppm / K, Al2O3: 7.2 ppm / K). As a result of comparing Samples 7, 13, 14, and 15, Sample 13, whose first material is silicon nitride, was evaluated as B, while Samples 7, 14, and 15, whose first material is other than silicon nitride, were evaluated as A. This tendency was also confirmed in the relationships between samples 5, 8, and 9, in which the second material was aluminum. These results demonstrate that the dimensional change of the composite member can be suppressed by setting the thermal expansion coefficient of the first material, which has the smallest thermal expansion coefficient, to 3 ppm / K or more.
[0034] The thermal expansion coefficient of the second material having the largest thermal expansion coefficient was compared between sample 4 of "Zn-70SiC" and sample 7 of "Mg-70SiC". Of the second materials, zinc and magnesium, the thermal expansion coefficient of zinc is 40 ppm / K, which is greater than 30 ppm / K, and the thermal expansion coefficient of magnesium is 26 ppm / K, which is less than 30 ppm / K. As a result of comparing samples 4 and 7, sample 4, whose second material is zinc, was evaluated as B, while sample 7, whose second material is magnesium, was evaluated as A. This tendency was also confirmed in the relationship between samples 8, 11, and 14, whose first material is aluminum nitride, and in the relationship between samples 9, 12, and 15, whose first material is alumina. From these results, it became clear that the dimensional change of the composite member can be suppressed by setting the thermal expansion coefficient of the second material having the largest thermal expansion coefficient to 30 ppm / K or less. It was also revealed that sample 10 made of "Zn-70Si3N4" in which the thermal expansion coefficient of the first material was smaller than 3 ppm / K and the thermal expansion coefficient of the second material was larger than 30 ppm / K was rated B.
[0035] Regarding the composition of the first material having the smallest thermal expansion coefficient, sample 3, "Al-70SiC" containing 70 volume% silicon carbide, was compared with sample 6, "Al-40SiC" containing 40 volume% silicon carbide. As a result, sample 6 was given an evaluation of B, while sample 3 was given an evaluation of A. This revealed that by making the composition of the first material 70 volume% or more, and at least 50 volume% or more, it is possible to suppress dimensional changes in the composite member.
[0036] According to the joined body 1 of the present embodiment described above, the composite member 20 joined to the ceramic member 10 in the joined body 1 contains a plurality of types of materials. Among the plurality of types of materials contained in the composite member 20, the difference between the thermal expansion coefficient of silicon carbide having the smallest thermal expansion coefficient and the thermal expansion coefficient of aluminum having the largest thermal expansion coefficient is 10 ppm / K or more, and the grain size of the silicon carbide grains contained in the cross section of the composite member 20 is 50 μm or less. In this way, even if there is a relatively large difference in thermal expansion coefficient between the plurality of types of materials contained in the composite member 20, the grain size of the silicon carbide grains having a relatively small thermal expansion coefficient is made relatively small, so that the thermal stress generated in the composite member 20 due to the thermal expansion difference is reduced. As a result, the deformation of the composite member 20 is suppressed, and therefore the ceramic member 10 joined to the composite member 20 can be suppressed from cracking or warping due to the deformation of the composite member 20. Therefore, damage to the joined body 1 can be suppressed.
[0037] Furthermore, according to the joined body 1 of the present embodiment, the length of the portion where the silicon carbide and aluminum are in contact with each other in the cross section of the composite member 20 is relatively short, being smaller than 100 μm. That is, the contact area between the silicon carbide and the aluminum is relatively small. When the contact area is small, the thermal stress generated due to the difference in thermal expansion is also small, so that the deformation of the composite member 20 is further suppressed. Therefore, the damage of the joined body 1 can be further suppressed.
[0038] Furthermore, according to the joined body 1 of the present embodiment, the thermal expansion coefficient of aluminum, which has the largest thermal expansion coefficient among the multiple types of materials contained in the composite member 20, is 22 ppm / K, and the difference between this and the thermal expansion coefficient of silicon carbide, which has the smallest thermal expansion coefficient. In this way, the difference in thermal expansion coefficient between the multiple types of materials contained in the composite member 20 is reduced, and thus the thermal stress generated within the composite member 20 is also reduced. This further suppresses deformation of the composite member 20, and therefore further suppresses damage to the joined body 1.
[0039] Furthermore, according to the joined body 1 of the present embodiment, silicon carbide, which has the smallest thermal expansion coefficient among the multiple types of materials contained in the composite member 20, has a thermal expansion coefficient of 4.5 pm / K, and the difference between this and the thermal expansion coefficient of aluminum, which has the largest thermal expansion coefficient, is small. In this way, the difference in thermal expansion coefficient between the multiple types of materials contained in the composite member 20 is reduced, and thus the thermal stress generated within the composite member 20 is also reduced. This further suppresses deformation of the composite member 20, and therefore further suppresses damage to the joined body 1.
[0040] Furthermore, according to the joined body 1 of the present embodiment, the composite member 20 contains 70 volume % silicon carbide, which has a small thermal expansion coefficient, and accounts for a large portion of the materials contained in the composite member 20. This suppresses dimensional changes in the composite member 20, and therefore damage to the joined body 1 can be further suppressed.
[0041] Moreover, according to the electrostatic chuck 100 of this embodiment, the electrostatic chuck 100 holds an object by using a chuck electrode of the ceramic member. At this time, heat generated in the ceramic member 10 is transferred to the composite member 20, so that the composite member 20 repeatedly expands and contracts due to temperature changes. In the composite member 20, thermal stress caused by the difference in thermal expansion between silicon carbide and aluminum is small, so that dimensional changes in the composite member 20 are suppressed even when used for a long period of time. As a result, damage to the electrostatic chuck 100 can be suppressed.
[0042] <Modifications of this embodiment> The present invention is not limited to the above-described embodiment, and can be embodied in various forms without departing from the spirit and scope of the invention. For example, the following modifications are also possible.
[0043] [Variation 1] In the above embodiment, the bonded body 1 is used in the electrostatic chuck 100, but the application field of the bonded body 1 is not limited thereto. Also, the bonded body 1 has the chuck electrode 11 and the coolant flow passage 21, but these may be omitted.
[0044] [Variation 2] In the above embodiment, the composite member 20 is made of a plurality of materials including silicon carbide and aluminum. The combination of materials forming the composite member 20 is not limited to this. Among the plurality of materials, the first material having the smallest thermal expansion coefficient may be AlN, Al2O3, Si3N4, etc., and the second material having the largest thermal expansion coefficient may be Zn, Mg, etc. It is sufficient that the difference between the thermal expansion coefficient of the first material having the smallest thermal expansion coefficient and the thermal expansion coefficient of the second material having the largest thermal expansion coefficient is 10 ppm / K or more.
[0045] [Variation 3] In the above embodiment, the length of the portion where silicon carbide and aluminum are in contact in the cross section of the composite member 20 is smaller than 100 μm. However, the length of the portion where silicon carbide and aluminum are in contact is not limited to this. When the length of the portion where silicon carbide and aluminum are in contact is smaller than 100 μm, the thermal expansion difference is reduced, and the thermal stress generated due to the thermal expansion difference is relatively reduced, and deformation of the composite member 20 due to the thermal stress can be suppressed.
[0046] [Variation 4] In the above embodiment, the composite member 20 contains aluminum with a thermal expansion coefficient of 22 ppm / K, which is less than 30 ppm / K. However, the thermal expansion coefficient of the "second material" contained in the composite member 20 is not limited to this. A material with a thermal expansion coefficient greater than 30 ppm / K may be used, but the smaller the thermal expansion coefficient of the second material having the maximum thermal expansion coefficient, the smaller the thermal stress generated due to the difference in thermal expansion coefficient with the first material. This makes it possible to suppress deformation of the composite member 20 due to thermal stress.
[0047] [Variation 5] In the above embodiment, the composite member 20 includes silicon carbide with a thermal expansion coefficient of 4.5 ppm / K, which is equal to or greater than 3 ppm / K. However, the thermal expansion coefficient of the "first material" included in the composite member 20 is not limited to this. A material with a thermal expansion coefficient smaller than 3 ppm / K may be used, but the smaller the thermal expansion coefficient of the first material having the smallest thermal expansion coefficient, the smaller the thermal stress generated due to the difference in thermal expansion coefficient with the second material becomes. This makes it possible to suppress deformation of the composite member 20 due to thermal stress.
[0048] [Variation 6] In the above embodiment, the composite member 20 contains 50 volume % or more of silicon carbide. However, the volume percentage of the first material in the composite member is not limited to this. The volume percentage of the first material in the composite member may be less than 50 volume %. By containing a large amount of the first material, which has a relatively small thermal expansion coefficient, dimensional changes in the composite member can be suppressed.
[0049] Although the present aspect has been described above based on the embodiment and modified examples, the above-mentioned embodiment of the aspect is intended to facilitate understanding of the present aspect and does not limit the present aspect. The present aspect may be modified or improved without departing from the spirit and scope of the claims, and equivalents are included in the present aspect. Furthermore, if a technical feature is not described as essential in this specification, it may be deleted as appropriate.
[0050] [Application example 1] A bonded body in which a ceramic member and a composite member are bonded, The composite member is It contains multiple materials, Among the plurality of materials, a difference between a thermal expansion coefficient of a first material having a minimum thermal expansion coefficient and a thermal expansion coefficient of a second material having a maximum thermal expansion coefficient is 10 ppm / K or more; The particle size of the particles of the first material contained in the cross section of the composite material is 50 μm or less. A conjugate characterized in that [Application example 2] The bonded body according to Application Example 1, In the cross section, the length of the portion where the first material and the second material are in contact is less than 100 μm. A conjugate characterized in that [Application example 3] The bonded body according to Application Example 1 or Application Example 2, The thermal expansion coefficient of the second material is 30 ppm / K or less; A conjugate characterized in that [Application example 4] The bonded structure according to any one of Application Examples 1 to 3, The thermal expansion coefficient of the first material is 3 ppm / K or more; A conjugate characterized in that [Application example 5] The bonded structure according to any one of Application Examples 1 to 4, The composite member contains 50% by volume or more of the first material. A conjugate characterized in that [Application Example 6] 1. An electrostatic chuck comprising: The joint body according to any one of Application Examples 1 to 5 is provided, The ceramic member has a chuck electrode, The composite member has a cooling function. Electrostatic chuck characterized by: [Explanation of symbols]
[0051] 1...Zygote 10...Ceramic component 11...Electrostatic chuck 20...Composite material 21... Coolant flow path D111: Fluid particle size L112…Length 100...Electrostatic chuck
Claims
1. A bonded body in which a ceramic member and a composite member are bonded, The composite member is It contains multiple materials, Among the plurality of types of materials, a difference between a thermal expansion coefficient of a first material having a smallest thermal expansion coefficient and a thermal expansion coefficient of a second material having a largest thermal expansion coefficient is 10 ppm / K or more; The particle size of the particles made of the first material contained in the cross section of the composite material is 50 μm or less. A conjugate characterized in that
2. The joint body according to claim 1 , In the cross section, the length of a portion where the first material and the second material are in contact is less than 100 μm. A conjugate characterized in that
3. The bonded body according to claim 1 or 2, The thermal expansion coefficient of the second material is 30 ppm / K or less. A conjugate characterized in that
4. The bonded body according to claim 1 or 2, The thermal expansion coefficient of the first material is 3 ppm / K or more. A conjugate characterized in that
5. The bonded body according to claim 1 or 2, The composite member contains the first material at 50% by volume or more. A conjugate characterized in that
6. 1. An electrostatic chuck comprising: The joint body according to claim 1 or 2 is provided, The ceramic member has a chuck electrode, The composite member has a cooling function. Electrostatic chuck characterized by:
Citation Information
Patent Citations
Wafer holding device
JP1999163109A