Manufacturing method for surface treatment sheet
The controlled use of toluene and ethyl acetate solvents with a triacetyl cellulose film and specific volatilization temperatures addresses the issues of adhesion durability and appearance in surface-treated sheets, resulting in improved reliability and appearance.
Patent Information
- Application Number
- JP2023060647
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-04
- Publication Date
- 2024-10-17
AI Technical Summary
Existing methods for producing surface-treated sheets using triacetyl cellulose films result in poor adhesion durability and appearance due to thickener aggregates and insufficient mixing of components, especially when polyester components with aromatic rings are present, leading to potential peeling and reduced reliability.
A manufacturing method involving the application of a coating liquid containing toluene and ethyl acetate solvents in specific ratios, along with a thickener, and volatilizing the solvent at controlled temperatures between 70°C and 100°C to ensure proper mixing and adhesion, while using a triacetyl cellulose film with a polyester component.
The method produces surface-treated sheets with improved adhesion durability and appearance, preventing thickener aggregation and ensuring effective mixing of components, thereby enhancing the reliability of the surface-treated film.
Smart Images

Figure 2024147910000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a surface-treated sheet that can be used as a member of an image display device, for example. [Background technology]
[0002] A method for producing a surface-treated sheet by performing a surface treatment on one surface of a base film has been known. The surface-treated sheet obtained by this type of production method is used, for example, as a member of an image display device.
[0003] As a method for producing such a surface-treated sheet, for example, a method is known which comprises a step of applying a coating liquid containing a specific number of components and a solvent to one side of a base film such as a triacetyl cellulose film, and a step of volatilizing the solvent after the step. In addition, the triacetyl cellulose film as the base film has been improved by changing the manufacturing process in order to increase the yield during production, to reduce the manufacturing cost, or to reduce the burden on the global environment during production. As a result of the improvement in the manufacturing process, some triacetyl cellulose films contain auxiliary components.
[0004] Specifically, a method for producing a surface-treated sheet is known in which a coating liquid containing low refractive index particles, a binder matrix, a functional compound, and a specific solvent is applied to a triacetyl cellulose film as a base film, the solvent in the coating liquid is volatilized, and then the coating film after the solvent has volatilized is hardened to produce an anti-reflective film as a surface-treated sheet (for example, Patent Document 1).
[0005] In the manufacturing method described in Patent Document 1, for example, when the solvent is evaporated, the temperature is first set to 20°C or more and 30°C or less, and then the solvent is further evaporated at 50°C or more and 150°C or less. The anti-reflection film obtained by the manufacturing method described in Patent Document 1 can have good hardness. In addition, according to the manufacturing method described in Patent Document 1, the solvent of the coating liquid dissolves or swells a part of the substrate film, so that the binder matrix and the solvent penetrate into the substrate film side to form a mixed layer. Therefore, by one coating, an anti-reflection film can be manufactured in which a multilayer structure having a low refractive layer containing low refractive particles and a hard coat layer formed by curing the mixed layer is formed on the surface part. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2013-205644 A Summary of the Invention [Problem to be solved by the invention]
[0007] In some cases, a surface-treated film is produced using a coating liquid that has been appropriately thickened by blending a thickener in order to suppress sedimentation of particulate components contained in the coating liquid as much as possible.
[0008] However, if the coating liquid containing the thickener and the solvent is simply applied to the triacetyl cellulose film, the thickener aggregates may cause the surface treatment film to have a poor appearance on the surface. In addition, the solvent of the coating liquid may not dissolve a part of the triacetyl cellulose film sufficiently, and the mixed layer may not be formed sufficiently, resulting in poor adhesion durability on the surface and easy peeling on the surface. The surface treatment film produced by such a method may have a low reliability as a product.
[0009] In addition, examples of the above-mentioned secondary components that may be contained in triacetyl cellulose film include certain polyester components, and these types of specific polyester components can also cause the problem of poor adhesion durability on the surface portion of the triacetyl cellulose film.
[0010] In order to prevent the above problems, it is conceivable to design the manufacturing method so as to improve the adhesion durability and appearance of the surface portion. However, it cannot be said that a method for producing a surface-treated sheet having good adhesion durability and appearance on the surface portion while using a triacetyl cellulose film containing the above-mentioned specific polyester component as a substrate has yet to be fully investigated.
[0011] Therefore, an object of the present invention is to provide a method for producing a surface-treated sheet that can produce a surface-treated sheet having good adhesion durability and appearance in the surface portion even when a triacetyl cellulose film containing a specific polyester component is used as a substrate. [Means for solving the problem]
[0012] In order to solve the above problems, the manufacturing method of the surface treatment sheet according to the present invention comprises the steps of: A step of applying a coating liquid containing at least a solvent and a thickener to a triacetyl cellulose film; and volatilizing the solvent from the coating liquid, The triacetyl cellulose film contains a polyester component having an aromatic ring at a molecular end, the solvent contains at least toluene and ethyl acetate, and the content of the ethyl acetate in the solvent is 7% by mass or more and 11% by mass or less; The step of volatilizing the solvent is characterized in that the solvent is volatilized under temperature conditions in which the maximum temperature is 70° C. or higher and 100° C. or lower. Effect of the Invention
[0013] According to the method for producing a surface treatment sheet of the present invention, even if a triacetyl cellulose film containing a polyester component having an aromatic ring at the molecular end is used as a substrate, a surface treatment sheet having good adhesion durability and appearance at the surface portion can be produced. [Brief description of the drawings]
[0014] [Figure 1] 1A to 1C are schematic diagrams illustrating a state in which an example of a method for producing a surface treatment sheet is carried out. [Figure 2A] FIG. 3 is a cross-sectional view illustrating a state before a coating step is performed in the manufacturing method of the present embodiment. [Figure 2B] FIG. 3 is a cross-sectional view illustrating a state immediately after a coating step in the manufacturing method of the present embodiment. [Figure 2C] FIG. 4 is a cross-sectional view illustrating a state after a volatilization step is performed in the manufacturing method of the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, an embodiment of the method for producing a surface treatment sheet according to the present invention will be described with reference to the drawings. Note that each figure in the drawings is a schematic view, and the aspect ratio is not necessarily the same as that of the actual product.
[0016] The method for producing the surface-treated sheet 10 of this embodiment includes a step of applying a coating liquid Y containing at least a solvent and a thickener to a triacetyl cellulose film X (hereinafter, sometimes simply referred to as a TAC film) (hereinafter, referred to as a coating step); and a step of volatilizing the solvent from the coating solution Y (hereinafter, referred to as the volatilization step). The triacetyl cellulose film X contains a polyester component having an aromatic ring at a molecular end. The solvent contains at least toluene and ethyl acetate, and the content of the ethyl acetate in the solvent is 7% by mass or more and 11% by mass or less. In the volatilization step, the solvent is volatilized under temperature conditions in which the maximum temperature is 70° C. or higher and 100° C. or lower.
[0017] Preferably, the coating liquid Y further contains a curable component and a polymerization initiator, etc., and the manufacturing method of the surface treatment sheet 10 of this embodiment includes the coating process, the volatilization process, and a process of curing the curable component (hereinafter referred to as a curing process).
[0018] For example, as shown in FIG. 1, the manufacturing method of the surface treatment sheet 10 of this embodiment can be carried out using a manufacturing apparatus 100 equipped with a coating section 2 for carrying out the above-mentioned coating process, a heating section 3 having a heating means for carrying out the above-mentioned volatilization process, and a hardening processing section 4 for carrying out the above-mentioned hardening treatment process. The manufacturing method of the surface-treated sheet 10 of this embodiment may further include a pre-treatment section 1 for pre-annealing the TAC film X, if necessary. In the pre-treatment section 1, for example, in order to sufficiently reduce wrinkles in the TAC film X or to sufficiently reduce foreign matter attached to the surface of the TAC film X, a pre-annealing process may be performed in the pre-treatment section 1. In the manufacturing method of the surface treatment sheet 10 of this embodiment, a long strip-shaped TAC film X is continuously supplied to a coating section 2, while passing through a heating section 3 and a hardening processing section 4, etc., to continuously produce the surface treatment sheet 10 obtained.
[0019] The triacetyl cellulose film X (TAC film) contains triacetyl cellulose, which is a cellulose monosaccharide unit in which three hydroxyl groups are acetylated, as a main component, and a polyester component having an aromatic ring at the molecular end as a minor component. The content of the polyester component in the TAC film X is usually from 1% by mass to 10% by mass.
[0020] The polyester component having an aromatic ring at the molecular end is mixed into the TAC film during the process of producing the TAC film X. The polyester component is, for example, an esterification reaction product of terephthalic acid, adipic acid, and propylene glycol.
[0021] A commercially available product can be used as the TAC film X. Commercially available TAC film products are available from, for example, Konica Minolta.
[0022] The coating solution Y used in the production method of the present embodiment contains at least toluene and ethyl acetate as a solvent, and further contains a thickener, a curable component, and a polymerization initiator. The coating solution Y may further contain a particulate additive, a leveling agent, or the like, as necessary.
[0023] In the above-mentioned Coating Fluid Y, the content of ethyl acetate in the solvent is preferably 8% by mass or more, more preferably 9% by mass or more, and even more preferably more than 9% by mass. Note that such a content is a mass ratio in the total amount of the solvent. In addition, in the above-mentioned Coating Fluid Y, the mass ratio of toluene to ethyl acetate is preferably equal to or greater than 8. Moreover, such a mass ratio is preferably equal to or less than 13, and more preferably equal to or less than 11.
[0024] The coating solution Y may contain a solvent other than toluene and ethyl acetate, such as cyclopentanone or methoxypropanol. However, in terms of making the curable component (e.g., a resin) more easily soluble or making it possible to more thoroughly disperse the thickener in Coating Liquid Y, the proportion of toluene and ethyl acetate in the total amount of the solvent is preferably 95 mass% or more, more preferably 98 mass% or more, and even more preferably 100 mass%.
[0025] Examples of the thickener for the coating solution Y used in this embodiment include particulate clay minerals. Examples of such clay minerals include smectite, talc, bentonite, montmorillonite, and kaolinite. The clay mineral is preferably an organically modified clay mineral (organoclay). As the particulate clay mineral, commercially available products can be used, such as the "Lucentite Series" manufactured by Co-op Chemical Co., Ltd., the "Esben Series" manufactured by Hojun Co., Ltd., or the "Sumecton Series" manufactured by Kunimine Kogyo Co., Ltd.
[0026] The coating solution Y may contain 0.3% by mass or more, or 0.5% by mass or more of a thickener (non-volatile content). The coating solution Y may contain 3.0% by mass or less, or 1.0% by mass or less of a thickener (non-volatile content). In the above coating liquid Y, the ratio of the thickener to the non-volatile content other than the solvent may be 0.5 mass% or more, 1.0 mass% or more, or 1.5 mass% or more. The ratio of the thickener to the non-volatile content other than the solvent may be 5.0 mass% or less, or 3.0 mass% or less. The non-volatile content is a component other than the solvent that will constitute a part of the surface treatment sheet.
[0027] Examples of the curable component of the coating liquid Y include (meth)acrylate monomers. The term "(meth)acrylate" includes both "acrylate" and "methacrylate".
[0028] Examples of the (meth)acrylate monomer include polyfunctional (meth)acrylate monomers, oligomers derived from polyfunctional (meth)acrylate monomers, and prepolymers derived from polyfunctional (meth)acrylate monomers.
[0029] Examples of polyfunctional (meth)acrylate monomers include tricyclodecane dimethanol diacrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, trimethylolpropane triacrylate, pentaerythritol tetra(meth)acrylate, dimethylolpropane tetraacrylate, dipentaerythritol hexa(meth)acrylate, 1,6-hexanediol (meth)acrylate, 1,9-nonanediol diacrylate, 1,10-decanediol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, dipropylene glycol diacrylate, isocyanuric acid tri(meth)acrylate, ethoxylated glycerin triacrylate, and ethoxylated pentaerythritol tetraacrylate.
[0030] The polyfunctional (meth)acrylate monomer may include a urethane (meth)acrylate or an oligomer of a urethane (meth)acrylate. The urethane (meth)acrylate is, for example, a urethane reaction product of a hydroxy (meth)acrylate having an --OH group, a diisocyanate, and a polyol.
[0031] Examples of the polyol include ethylene glycol, 1,3-propylene glycol, 1,2-propylene glycol, diethylene glycol, dipropylene glycol, neopentyl glycol, 1,3-butanediol, 1,4-butanediol, 1,6-hexanediol, 1,9-nonanediol, 1,10-decanediol, 2,2,4-trimethyl-1,3-pentanediol, 3-methyl-1,5-pentanediol, hydroxypivalic acid neopentyl glycol ester, tricyclodecane dimethylol, 1,4-cyclohexanediol, spiroglycol, hydrogenated bisphenol A, ethylene oxide-added bisphenol A, propylene oxide-added bisphenol A, trimethylolethane, trimethylolpropane, glycerin, 3-methylpentane-1,3,5-triol, pentaerythritol, dipentaerythritol, tripentaerythritol, and glucoses.
[0032] The above (meth)acrylate monomers may be used alone or in combination of two or more. As the curable component such as the above (meth)acrylate monomer, a commercially available product can be used.
[0033] The above-mentioned coating liquid Y may contain a photopolymerization initiator or a thermal polymerization initiator in order to sufficiently cure the above-mentioned curable component. As the photopolymerization initiator or the thermal polymerization initiator, a commercially available product can be used.
[0034] In the above-mentioned Coating Solution Y, the ratio of the curable component to the non-volatile content other than the solvent may be 70.0% by mass or more and 90.0% by mass or less. In addition, in the above-mentioned Coating Solution Y, the ratio of the polymerization initiator to the non-volatile content other than the solvent may be 1.0% by mass or more and 10.0% by mass or less.
[0035] Examples of the particulate additive in the coating liquid Y include polymer particles and inorganic particles. Examples of the polymer particles include polymethyl methacrylate particles (PMMA particles), silicone polymer particles, polystyrene particles, polycarbonate particles, acrylic styrene particles, benzoguanamine particles, melamine resin particles, polyolefin particles, polyester particles, polyamide particles, polyimide particles, polyethylene fluoride particles, etc. The polymer in the particles may be in a crosslinked state. Examples of inorganic particles include silicon oxide particles, titanium oxide particles, aluminum oxide particles, zinc oxide particles, tin oxide particles, calcium carbonate particles, barium sulfate particles, talc particles, kaolin particles, and calcium sulfate particles. The above particles may be used alone or in combination of two or more kinds. Commercially available products may be used as the above particles.
[0036] The average particle diameter of the particulate additive is, for example, 1 μm or more and 10 μm or less. The average particle diameter is obtained by measuring the diameter of 50,000 particulate additives (e.g., polystyrene particles) using a flow-type image analyzer and arithmetically averaging the measured values. When the particles in the image at the time of measurement are not perfectly circular but elliptical, the major axis of each particle is measured.
[0037] The coating solution Y may contain 1.0% by mass or more, or 2.0% by mass or more, of a particulate additive (solid). The coating solution Y may contain 10.0% by mass or less, or 5.0% by mass or less, of a thickener (non-volatile content). In the above-mentioned Coating Fluid Y, the proportion of the particulate additive in the non-volatile content other than the solvent may be 5.0% by mass or more. Such a proportion may be 20.0% by mass or less, or may be 15.0% by mass or less.
[0038] The coating liquid Y preferably contains 10% by mass or more and 20% by mass or less of polystyrene particles having an average particle size of 1 μm or more and 5 μm or less, so that the produced surface-treated sheet can have better antiglare properties.
[0039] In the above coating step, a coating liquid Y is applied to one side of a TAC film X by a coating unit 2. In the coating step, a general coating method can be used, such as a die coating method, a bar coating method, a roll coating method, a gravure coating method, a rod coating method, a slot orifice coating method, a curtain coating method, a fountain coating method, or a comma coating method.
[0040] The time period from the end of coating in the coating step to the start of heating in the volatilization step is preferably 10 seconds or more and 30 seconds or less.
[0041] In the volatilization step, the triacetyl cellulose film X coated with the coating liquid Y is heat-treated at a predetermined temperature for a predetermined time. The minimum temperature in the heat treatment is, for example, 45° C., and the coating liquid Y after coating is heated under temperature conditions with a maximum temperature of 70° C. or higher and 100° C. or lower, thereby volatilizing the solvent in the coating liquid Y.
[0042] The maximum temperature during the heat treatment in the volatilization step may be set to 75°C or higher, 80°C or higher, 85°C or higher, or 90°C or higher. By increasing the heating temperature, the time required for the polyester component to be eluted from the TAC film is shortened. The adhesion durability of the surface portion of the manufactured surface-treated sheet can be improved to the extent that the amount of the polyester component eluted is reduced. The maximum temperature during the heat treatment may be set to 95°C or lower. The duration of the maximum temperature set as above may be 5 seconds or more, or may be 10 seconds or more, and the duration of the maximum temperature set as above may be 30 seconds or less, or may be 20 seconds or less.
[0043] The heat treatment time in the volatilization step (total time for which the heat treatment is continued) is preferably 60 seconds or more, and more preferably 80 seconds or more. By increasing the heat treatment time, the solvent can be more sufficiently volatilized from Coating Solution Y. The heat treatment time is preferably 120 seconds or less, and more preferably 100 seconds or less. By shortening the heat treatment time, the volatilization step can be completed in a shorter time. The minimum temperature set in the heat treatment is preferably 45°C, and more preferably 50°C.
[0044] The heat treatment time in the volatilization step can be adjusted, for example, by increasing or decreasing the speed at which the TAC film X passes through the heating section 3. In the volatilization step, it is preferable to set the maximum temperature in the heat treatment as described above, and to continue the heat treatment at such maximum temperature for 10 seconds or more and 20 seconds or less.
[0045] In the manufacturing method of this embodiment, a curing process step is carried out in the curing unit 4. In the curing unit 4, the curing process step is carried out in order to cure the curable component remaining after the solvent has evaporated.
[0046] The curing unit 4 includes a light irradiation device capable of irradiating light such as ultraviolet light. When the coating solution Y contains a curable component that can be cured by light irradiation, the curable component can be cured by light irradiation from the light irradiation device. When the coating solution Y contains a curable component that can be cured by heat treatment, the curable component can be cured by heat treatment.
[0047] In the light irradiation in the curing treatment step, for example, the dried coating film after the solvent has evaporated is irradiated with active energy rays such as ultraviolet rays to cure the dried coating film. As the active energy ray, for example, ultraviolet light, visible light, or infrared light is used. As the active energy ray, radiation such as α-ray, β-ray, γ-ray, electron beam, neutron beam, or X-ray may be used. It is preferable to irradiate with light including ultraviolet light, since it is relatively safe for the human body and has a relatively large amount of energy.
[0048] The surface treatment sheet 10 manufactured through the hardening treatment step is, for example, rolled up and stored.
[0049] In the manufacturing method of this embodiment, in the coating step, the coating liquid Y is applied to one side of the TAC film X (see FIG. 2A) (see FIG. 2B). In the volatilization step, the coating liquid Y applied to the TAC film X is heated, so that the solvent in the coating liquid Y volatilizes. As shown in FIG. 2C, the manufactured surface treatment sheet 10 has, for example, a surface layer 13, a base layer 11 located inside the surface layer 13, and a mixed layer 12 (also called a compatible layer) located between the surface layer 13 and the base layer 11 and in which a part of the components constituting the surface layer 13 and a part of the components constituting the base layer 11 are compatible with each other. That is, the manufactured surface treatment sheet 10 is also a multilayer sheet having a surface portion having a structure in which multiple layers are laminated.
[0050] The coating solution Y used in the coating step contains at least ethyl acetate and toluene as a solvent, and the solvent contains ethyl acetate and toluene at a predetermined content respectively. Since ethyl acetate easily dissolves TAC in the TAC film, a part of TAC, which is the main component of the base layer 11, dissolves and migrates to the mixed layer 12, and a mixed layer containing TAC can be reliably formed. Therefore, the presence of the mixed layer between the surface layer 13 and the base layer 11 can improve adhesion durability. However, if the content of ethyl acetate in the solvent is too high, the thickener is difficult to disperse in the solvent of the coating liquid Y, so that agglomerates of the thickener are likely to occur in the surface layer 13 or the mixed layer 12, and the appearance of the surface portion of the surface-treated sheet 10 may be poor. On the other hand, toluene can disperse the thickener sufficiently, so that the thickener can be prevented from agglomerating. Therefore, the appearance of the surface-treated sheet 10 can be improved. However, if the content of toluene in the solvent is too high, TAC becomes difficult to dissolve in the solvent, so that the formation of the mixed layer 12 containing TAC may be insufficient. Therefore, the adhesion durability between the surface layer 13 and the base layer 11 may be poor.
[0051] Moreover, the heat treatment temperature (particularly the maximum temperature) in the volatilization step is within the predetermined range as described above. If the heat treatment temperature for volatilizing the solvent is too high, most of the solvent will volatilize before the solvent sufficiently dissolves the TAC after the coating solution Y is applied onto the TAC film (before the TAC is sufficiently dissolved in the mixed layer 12), which may result in poor adhesion durability between the surface layer 13 and the base layer 11. On the other hand, if the heat treatment temperature (especially the maximum temperature) when volatilizing the solvent is too low, it will take a relatively long time for the solvent to volatilize. Although the solvent can sufficiently dissolve the TAC, it will take a long time for all of the solvent to volatilize, which may result in poor production efficiency. In addition, when the TAC film contains a relatively large amount of the above-mentioned polyester component, if the time until the solvent of the coating solution Y evaporates is too long, the polyester component may dissolve from the TAC film and segregate between the base layer 11 and the mixed layer 12. The segregated polyester component may deteriorate the adhesion between the base layer 11 and the mixed layer 12. This causes the adhesion durability between the surface layer 13 and the base layer 11 to become poor.
[0052] In the manufacturing method of this embodiment, the coating solution Y contains ethyl acetate and toluene in an organic solvent at a predetermined content, and the organic solvent of the coating solution Y is volatilized at a predetermined heating temperature, so that both the poor adhesion durability between the surface layer 13 and the base layer 11 and the aggregation of the thickener can be suppressed. Therefore, a surface-treated sheet 10 having good adhesion durability and appearance at the surface portion can be manufactured.
[0053] The manufacturing method of the surface treatment sheet of this embodiment is as exemplified above, but the present invention is not limited to the manufacturing method of the surface treatment sheet exemplified above. That is, various forms used in general methods for producing surface treatment sheets can be adopted as long as they do not impair the effects of the present invention.
[0054] The matters disclosed in this specification include the following. (1) A step of applying a coating liquid containing at least a solvent and a thickener to a triacetyl cellulose film; and volatilizing the solvent from the coating liquid, The triacetyl cellulose film contains a polyester component having an aromatic ring at a molecular end, the solvent contains at least toluene and ethyl acetate, and the content of the ethyl acetate in the solvent is 7% by mass or more and 11% by mass or less; In the step of volatilizing the solvent, the solvent is volatilized under a temperature condition in which the maximum temperature is 70°C or higher and 100°C or lower. (2) The method for producing a surface-treated sheet according to (1) above, wherein the content of the polyester component in the triacetyl cellulose film is 10% by mass or less. (3) The method for producing a surface-treated sheet according to (1) or (2) above, wherein the coating liquid contains the thickener (non-volatile content) in an amount of 0.3% by mass or more and 3.0% by mass or less. (4) The method for producing a surface-treated sheet according to any one of (1) to (3) above, wherein the coating liquid contains 1.0 mass % to 10.0 mass % of polystyrene particles having an average particle diameter of 1 μm to 5 μm. (5) The method for producing a surface-treated sheet according to any one of (1) to (4) above, wherein the coating liquid further contains a curable component, and the curable component contains a polyfunctional (meth)acrylate monomer. (6) The method for producing a surface-treated sheet according to any one of (1) to (5) above, wherein the thickener contains a particulate clay mineral. (7) The method for producing a surface-treated sheet according to any one of (1) to (6) above, wherein in the step of volatilizing the solvent, the solvent is volatilized by maintaining a temperature condition in which the maximum temperature is 70°C or higher and 100°C or lower for 10 seconds or longer and 20 seconds or shorter. (8) The method for producing a surface-treated sheet according to (7) above, wherein in the step of volatilizing the solvent, a temperature condition of 45°C or higher is maintained for 60 seconds or more and 120 seconds or less, and the solvent is volatilized by continuing a temperature condition of the maximum temperature being 70°C or higher and 100°C or lower for 10 seconds or more and 20 seconds or less. EXAMPLES
[0055] The present invention will now be described in more detail with reference to experimental examples, but the present invention is not limited thereto.
[0056] Using a manufacturing apparatus as shown in FIG. 1, a method for manufacturing a surface-treated sheet was carried out as follows.
[0057] <Raw materials for surface treatment sheets> (Triacetyl cellulose film) (Contains approximately 8% by mass of polyester components with aromatic rings at the molecular ends) Product name: "KC4UA" (Konica Minolta) Thickness: 40μm (Coating fluid) Organic solvent: ethyl acetate (concentration in solvent shown in Table 1) and toluene (remainder in solvent) · Thickener: Clay minerals (organic smectite, mainly composed of montmorillonite) Product name: "Sumecton SAN" (manufactured by Kunimine Kogyo Co., Ltd.) Uses a pre-prepared thickening solution (containing 4.6% clay minerals by weight) Photopolymerization initiator: Product name "OMNIRAD907" (manufactured by BASF) Particulate additive: Cross-linked polystyrene particles with an average particle size of 3.5 μm Product name "SX-350H" (manufactured by Soken Chemical Co., Ltd.) Curing component: UV-curable urethane acrylate resin solution Product name: "LUXYDIR 17-806" (DIC Corporation) (non-volatile content 80% by mass) Leveling agent: Fluorosurfactant Product name: "Megafac F-556" (DIC Corporation) (non-volatile content 40% by mass)
[0058] <Preparation of coating liquid (amount of each raw material)> - Thickening solution containing the above thickening agent (non-volatile content 4.6% by mass): 2.5 parts by mass Cross-linked polystyrene particles: 14 parts by weight Photopolymerization initiator: 5 parts by weight The above raw materials were mixed by stirring in a disperser for 15 minutes, and then further stirred in a homomixer for 20 minutes (rotation speed: 2500 rpm) to prepare an intermediate mixed liquid. Furthermore, the following raw materials were added to the intermediate mixture and mixed by stirring with a disper for 15 minutes, and then further stirred with a homomixer for 20 minutes (rotation speed: 2500 rpm) to prepare a coating liquid. Organic solvent: Amount that results in 32% non-volatile matter in the coating liquid UV-curable urethane acrylate resin solution (non-volatile content 80% by weight): 100 parts by weight Leveling agent (non-volatile content 40% by mass): 0.5 parts by mass
[0059] <Manufacturing conditions for surface treatment sheet> (Pretreatment process) Pre-annealing is performed for 15 seconds in the pre-treatment section. (Coating process) Coating section: Equipped with die coating device The coating liquid was applied to one surface of a triacetyl cellulose film so that the thickness of the coating film before curing treatment would be 6 μm. (Volatilization process) Volatilization section: Equipped with a heater that can heat the object passing through the internal space to a specified temperature (length of the section where the heating process is performed by the heater: 30m) The solvent contained in the coating liquid was evaporated by heating to form a dry coating film with a thickness of 6 μm. Details of the heat treatment time are as follows. Total heating time: 80 to 120 seconds (minimum heating temperature setting: 50°C), Duration of maximum temperature: 15 seconds (The maximum temperature setting for heat treatment is shown in Table 1) (Hardening process) Hardening treatment section: Equipped with high pressure mercury lamps The cumulative light intensity on the dried coating after the solvent has evaporated is 245 mJ / cm 2 The sample was irradiated with ultraviolet light having a wavelength of 365 nm so as to obtain the following:
[0060] The production conditions in each Example and Comparative Example are shown in Table 1. Unless otherwise specified, the production conditions in each Example and Comparative Example are the same.
[0061] [Table 1]
[0062] <Performance evaluation of the manufactured surface-treated film> (Surface adhesion durability (durable peeling prevention performance)) Test pieces of each of the surface-treated sheets produced as described above were irradiated with ultraviolet light for a long period of time as described below, and then the adhesion of the surface portion was evaluated. -Evaluation of long-term light exposure conditions and adhesion The surface layer side of the test sample was irradiated with light using an ultraviolet long-life fade meter (manufactured by Suga Test Instruments Co., Ltd., model: U48HB). Temperature: 40℃ Humidity: 20%RH Lamp: (wavelength) 300nm~700nm, (illuminance) 500W / m 2 Continuous light exposure time: 144 hours, 192 hours After the ultraviolet irradiation was performed as described above, the adhesion of the surface of the surface-treated sheet was evaluated. Specifically, the test pieces 144 hours after the start of ultraviolet irradiation and the test pieces 192 hours after (reference experiment) were subjected to the following cross-cut peeling test. In the cross-cut test, 100 small sections (masks) of 1 mm square were formed in a cross-cut pattern (10 x 10) on the surface layer of each test piece using a cutter knife. Next, an adhesive tape (manufactured by Sekisui Chemical Co., Ltd., product name "Cellotape (registered trademark) No. 252") was attached to the surface layer, and the adhesive tape was peeled off. This operation was repeated twice, and the number of small sections peeled off together with the adhesive tape was counted. 0 (zero): (Excellent) No peeling of small areas on the surface is observed △: (Good) Only a part of a small area has peeled off (partial peeling). ×: (Failure) One or more small sections are completely peeled off (one or more small sections are completely peeled off) (Appearance: Visual inspection) In a dark room, the coated surface of a surface-treated film (rectangle of 150 mm x 100 mm) was irradiated with light from a three-wavelength fluorescent lamp and the light was reflected, and the coating surface was visually inspected for the presence of aggregates, etc. The absence of aggregates was judged as good (○), and the presence of aggregates was judged as poor (×).
[0063] As can be seen from Table 1, in the surface-treated sheet manufactured by the manufacturing method of the Example, even when a triacetyl cellulose film containing a polyester component having an aromatic ring at the molecular end was used as a substrate, both the adhesion durability and the appearance of the surface portion (surface layer) were good. On the other hand, in the surface-treated sheet manufactured by the manufacturing method of the Comparative Example, neither the adhesion durability nor the appearance of the surface portion (surface layer) was good. [Industrial Applicability]
[0064] The method for producing a surface-treated sheet of the present invention is preferably used for producing a member of an image display device. Such a member is, for example, an optical sheet, specifically, an anti-reflection sheet, an anti-glare sheet, an anti-glare protection sheet, an anti-fingerprint sheet, etc. [Explanation of symbols]
[0065] 10: Surface treatment sheet, 11: Base layer, 12: Mixed layer, 13: Surface layer, X: triacetyl cellulose film, Y: coating liquid, 100: Manufacturing equipment, 1: pre-treatment section, 2: coating section, 3: heating section, 4: curing section.
Claims
1. A step of applying a coating liquid containing at least a solvent and a thickener to a triacetyl cellulose film; and volatilizing the solvent from the coating liquid, The triacetyl cellulose film contains a polyester component having an aromatic ring at a molecular end, the solvent contains at least toluene and ethyl acetate, and the content of the ethyl acetate in the solvent is 7% by mass or more and 11% by mass or less; In the step of volatilizing the solvent, the solvent is volatilized under a temperature condition in which the maximum temperature is 70° C. or higher and 100° C. or lower.
2. The method for producing a surface-treated sheet according to claim 1 , wherein the content of the polyester component in the triacetyl cellulose film is 10% by mass or less.
3. The method for producing a surface-treated sheet according to claim 1 or 2, wherein the coating liquid contains the thickener in an amount of 0.3 mass % or more and 3.0 mass % or less.
4. The method for producing a surface-treated sheet according to claim 1 or 2, wherein the coating liquid contains 1.0 mass % or more and 10.0 mass % or less of polystyrene particles having an average particle diameter of 1 μm or more and 5 μm or less.
Citation Information
Patent Citations
Curable composition for forming antireflection film, antireflection film and method for manufacturing the same, polarizing plate, and display device
JP2013205644A