Method for producing porous molding, molding material, porous molding, and porous carbon material

Coating spherical phenol resin cured products with a liquid phenol resin and employing a nitrogen-containing resol resin enhances mechanical strength and productivity in porous molded bodies, addressing the weakness of existing methods.

JP2024147911APending Publication Date: 2024-10-17SUMITOMO BAKELITE CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023060648
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-04
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Existing methods for producing porous molded bodies using phenolic resins result in products with inadequate mechanical strength.

Method used

A method involving coating spherical phenol resin cured products with a liquid phenol resin, followed by low-pressure molding, using a molding material that includes a nitrogen-containing resol resin, which is optionally ethylene crosslinked, and incorporating an inorganic filler to enhance mechanical strength and productivity.

Benefits of technology

The method produces porous molded bodies with high bending strength and bending elastic modulus, enabling low-pressure molding and improved productivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024147911000001
    Figure 2024147911000001
  • Figure 2024147911000002
    Figure 2024147911000002
  • Figure 2024147911000003
    Figure 2024147911000003
Patent Text Reader

Abstract

To provide a method for producing a porous molding which can obtain a porous molding that has high bending strength and bending elastic modulus and excellent mechanical strength, enables low pressure molding and offers excellent productivity.SOLUTION: A method for producing a porous molding includes a step of coating the surface of a spherical phenolic resin cured product (A) with a liquid phenol resin (B), and a step of molding a molding material containing the obtained coated spherical phenolic resin cured product (AB), wherein the spherical phenolic resin cured product (A) is a cured product of a resol resin.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a porous molded body, a molding material, a porous molded body, and a porous carbon material. [Background technology]

[0002] Because of their excellent physical properties such as heat resistance, cured products of phenolic resins have been widely used in various products such as machine structural parts, automobile parts, electrical equipment parts, communication equipment parts, etc. Such products are generally produced by known molding methods using resin compositions obtained by blending phenolic resins with various additives, fillers, etc.

[0003] Patent Document 1 discloses a porous body formed by aggregating coated particles obtained by coating spherical particles with a thermosetting resin such as a phenolic resin, and curing the thermosetting resin. Specifically, this document describes the formation of coated particles by a hot melt method in which a phenolic resin is added to heated spherical particles and the particles are kneaded while being heated.

[0004] Patent Document 2 discloses a method for producing a porous molded body in which a spherical composite resin formed by providing a coating layer made of uncured phenolic resin on the surface of cured particles made of a cured product of a thermosetting resin such as phenolic resin is filled into a molding die and molded by heating under pressure to melt and cure the coating layer made of uncured thermosetting resin, and the cured particles and the spherical particles made of the cured coating layer formed by curing the coating layer on their surfaces are fused together at their contact points. In this document, the coating layer is melted and cured, and the phenolic resin constituting the coating layer is in a solid state. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2011-26435 A [Patent Document 2] JP 2016-145264 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, the porous bodies obtained by the methods described in Patent Documents 1 and 2 have room for improvement in terms of mechanical strength. [Means for solving the problem]

[0007] The present inventors have found that a porous molded body excellent in mechanical strength can be obtained by using a spherical cured phenolic resin coated with a liquid phenolic resin, and have completed the present invention. That is, the present invention can be shown as follows.

[0008] [1] A step of coating the surface of a spherical phenolic resin cured material (A) with a liquid phenolic resin (B); A step of molding a molding material containing the obtained coated spherical phenolic resin cured material (AB); Including, A method for producing a porous molded body, wherein the spherical phenolic resin cured product (A) is a cured product of a resol resin. [2] The method for producing a porous molded body according to [1], wherein the molding step is performed at a pressure ranging from normal pressure to a pressure less than 0.2 MPa. [3] The method for producing a porous molded body according to [1] or [2], wherein the resol resin contains a nitrogen-containing structure. [4] The method for producing a porous molded body according to any one of [1] to [3], wherein the resol resin is an ethylene crosslinked resin. [5] The method for producing a porous molded body according to any one of [1] to [4], wherein the spherical phenolic resin cured product (A) is infusible by heat. [6] The method for producing a porous molded body according to any one of [1] to [5], wherein the amount of the liquid phenol resin (B) is 2 to 50 parts by mass per 100 parts by mass of the spherical phenol resin cured product (A). [7] The method for producing a porous molded body according to any one of [1] to [6], wherein the molding material further contains an inorganic filler. [8] A coated spherical phenolic resin cured material (AB) in which the surface of a spherical phenolic resin cured material (A) is coated with a liquid phenolic resin (B), The spherical phenolic resin cured material (A) is a molding material that is a cured product of a resol resin. [9] The molding material according to [8], wherein the resol resin contains a nitrogen-containing structure.

[10] The molding material according to [8] or [9], wherein the resol resin is an ethylene crosslinked resin.

[11] The molding material according to any one of [8] to

[10] , wherein the spherical phenolic resin cured product (A) is infusible by heat.

[12] The molding material according to any one of [8] to

[11] , comprising 2 to 50 parts by mass of liquid phenolic resin (B) per 100 parts by mass of the spherical phenolic resin cured product (A).

[13] The molding material according to any one of [8] to

[12] , further comprising an inorganic filler.

[14] A porous molded body comprising a cured product of the molding material according to any one of [8] to

[13] .

[15] Molded density is 0.4g / cm 3 ~1.2g / cm 3 The porous molded body according to

[14] ,

[16] A porous carbon material obtained by firing the porous molded body according to

[15] . Effect of the Invention

[0009] According to the present invention, a porous molded body having high bending strength and bending elastic modulus and excellent mechanical strength can be obtained, and further, a method for producing a porous molded body that allows low-pressure molding and is highly productive can be provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, the present invention will be described based on the embodiments. For example, "1 to 10" means "1 or more" to "10 or less" unless otherwise specified.

[0011] <Method of manufacturing porous body> The method for producing the porous body of this embodiment includes the following steps: Step a: The surface of a spherical cured phenolic resin (A) is coated with a liquid phenolic resin (B). Step b: The molding material containing the coated spherical cured phenolic resin (AB) obtained in step a is molded to obtain a porous molded body.

[0012] [Step a] In this process, the method is not particularly limited as long as the surface of the spherical phenolic resin cured material (A) can be coated with the liquid phenolic resin (B), and the liquid phenolic resin (B) can be attached to the surface of the spherical phenolic resin cured material (A) by a known mixing method. By using the liquid phenol resin (B), the contact area with the spherical phenol resin cured product (A) becomes large, and the porous molded body obtained in the step b described below has excellent mechanical strength.

[0013] Examples of the mixing method include a method using a mixer, a grinder, a kneader, a roll, a single-screw kneader, a twin-screw kneader, or the like.

[0014] Step a can be carried out in the atmosphere at room temperature (25° C.), and the mixing time is about 10 seconds to 10 minutes. In order to increase the fluidity of the liquid phenol resin (B), it may be heated or an organic solvent may be added thereto.

[0015] By this step, a coated spherical phenolic resin cured material (AB) is obtained. In this embodiment, the term "coated" refers not only to a case where the entire surface of the spherical phenolic resin cured material (A) is covered with the liquid phenolic resin (B), but also to a case where only a part of the surface is covered with the liquid phenolic resin (B). The components used in this step are described below.

[0016] (Spherical phenolic resin cured material (A)) In this embodiment, the spherical phenolic resin cured product (A) is a cured product of a resol resin. The resol resin preferably contains a nitrogen-containing structure, and specifically, contains at least one structural unit derived from an alkyleneamine represented by the following chemical formula (1) in the molecule.

[0017] [ka]

[0018] In the above general formula (1), R1 each independently represents a linear or branched alkylene group having 1 to 10 carbon atoms. The number of carbon atoms in the alkylene group of R1 is, for example, 1 to 10, preferably 2 to 6, and more preferably 2 to 4. By keeping it within the above range, the mechanical strength, such as bending strength and bending modulus of elasticity, of the cured body can be improved.

[0019] The resol resin may contain at least one structural unit derived from ethyleneamine represented by the following chemical formula (2) in the molecule.

[0020] [ka]

[0021] In this embodiment, the resol resin is preferably crosslinked with a structural unit derived from ethyleneamine represented by chemical formula (2), that is, is preferably an ethylene crosslinked product.

[0022] The lower limit of the content ratio of the structural unit derived from ethyleneamine in the resol resin is, for example, 3% by weight or more, preferably 5% by weight or more, more preferably 10% by weight or more. This improves the interfacial adhesion between the spherical phenolic resin cured product and the resol resin, and improves mechanical strength such as bending strength and bending modulus. On the other hand, the upper limit of the content ratio of the structural unit derived from ethyleneamine in the phenolic resin may be, for example, 50% by weight or less, preferably 45% by weight or less, more preferably 40% by weight or less. This allows the hardness of the spherical phenolic resin cured product to be appropriately adjusted. The content of the ethyleneamine-derived structure can be calculated based on the following formula: The nitrogen content (wt%) in the formula can be measured by elemental analysis. Ethyleneamine-derived structure content = Nitrogen content × (43 / 14)

[0023] The average particle size of the spherical phenolic resin cured product (A) of the present embodiment has an optimum range that varies depending on the application, and can be appropriately selected depending on the application. The lower limit of the average particle size of the spherical phenolic resin cured product (A) of this embodiment is, for example, preferably 0.1 μm or more, more preferably 1 μm or more, and even more preferably 5 μm or more. The upper limit of the average particle size of the spherical phenolic resin cured product (A) of this embodiment is, for example, preferably 1000 μm or less, and more preferably 500 μm or less.

[0024] By having the average particle size of the spherical phenolic resin cured product (A) within the above numerical range, the dispersibility of the spherical phenolic resin cured product (A) in the phenolic resin composition and in the cured product can be improved, and the cured product can have excellent mechanical strengths, such as bending strength and bending modulus. From the viewpoint of the effects of the present invention, the spherical phenolic resin cured product (A) may contain at least one type of spherical phenolic resin cured product having a different average particle size. The average particle size of the spherical phenolic resin cured product (A) can be measured by a laser scattering particle size distribution analyzer.

[0025] The lower limit of the bulk density of the spherical phenolic resin cured product (A) is, for example, preferably 0.10 g / ml or more, more preferably 0.15 g / ml or more, and even more preferably 0.20 g / ml or more. The upper limit of the bulk density of the spherical phenolic resin cured material (A) is, for example, preferably 1.00 g / ml or less, more preferably 0.90 g / ml or less, and even more preferably 0.80 g / ml or less. In this embodiment, the bulk density of the spherical phenolic resin cured material (A) can be evaluated using, for example, a powder tester PT-X manufactured by Hosokawa Micron Corporation.

[0026] In this embodiment, the spherical phenolic resin cured material (A) is preferably infusible by heat, which means the heat (heating temperature) during the production of the porous molded body and the heat (sintering temperature) during the production of the porous carbon material by sintering the porous molded body. Since the spherical phenolic resin cured product (A) is infusible by heat, the resulting porous molded product can withstand the heat and pressure during molding and maintain its porous structure, making it suitable for use in desired applications.

[0027] [Method for producing spherical phenolic resin cured product (A)] The spherical phenolic resin cured material (A) can be produced by the following method. The method for producing the spherical phenolic resin cured material (A) of this embodiment includes the steps of: A preparation step of preparing a mixed liquid containing a phenol, an aldehyde, and a hydrophilic polymer; The method includes a reaction step of stirring the mixture to react the phenols with the aldehydes to form suspended particles, and a hardening step. Each step will be described in detail below.

[0028] (preparation process) In the preparation step, a mixed liquid containing a phenol, an aldehyde, a hydrophilic polymer, and a hydrophilic solvent is prepared. Each component of the mixture will be described in detail below.

[0029] (Phenols) The phenols are not limited, and specific examples thereof include phenol; dihydroxybenzenes such as o-dihydroxybenzene (i.e., catechol), m-dihydroxybenzene (i.e., resorcinol, i.e., resorcin), and p-dihydroxybenzene (i.e., hydroquinone); trihydroxybenzenes such as 1,2,3-trihydroxybenzene (i.e., pyrogallol); cresols such as o-cresol, m-cresol, p-cresol, and oxocresol; alkylphenols such as ethylphenol, butylphenol, octylphenol, and nonylphenol; xylenol; and phenols contained in cashew oil such as 3-pentadecylphenol, 3-pentadecylphenol monoene, 3-pentadecylphenol diene, and 3-pentadecylphenol triene. Components containing cardol such as 1,3-dihydroxy-5-pentadecylbenzene, 1,3-dihydroxy-5-pentadecylbenzenemonoene, 1,3-dihydroxy-5-pentadecylbenzenediene, and 1,3-dihydroxy-5-pentadecylbenzenetriene; components containing methyl cardol such as 2-methyl-1,3-dihydroxy-5-pentadecylbenzene, 2-methyl-1,3-dihydroxy-5-pentadecylbenzenemonoene, 2-methyl-1,3-dihydroxy-5-pentadecylbenzenediene, and 2-methyl-1,3-dihydroxy-5-pentadecylbenzenetriene; urushiol; bisphenols such as bisphenol A, bisphenol F, and bisphenol S; p-phenylphenol; and styrenated phenol. As the phenols, one or more of the above specific examples can be used in combination. As the phenol, it is preferable to use one or more selected from the group consisting of phenol, cresol, and alkylphenol, among the above specific examples, and it is more preferable to use phenol, which can improve the mechanical strength such as bending strength and bending modulus of elasticity of the cured body.

[0030] (Aldehydes) The aldehydes are not limited, and specifically include formaldehyde, paraformaldehyde, acetaldehyde, paraaldehyde, butylaldehyde, crotonaldehyde, benzaldehyde, hydroxybenzaldehyde, terephthalaldehyde, salicylaldehyde, furfural, glyoxal, etc. As the aldehydes, one or more of the above specific examples can be used in combination. In addition, a compound that is a source of aldehyde compounds, such as hexamethylenetetramine, may be used. As the aldehydes, it is preferable to use one or more of the above specific examples selected from the group consisting of formaldehyde, paraformaldehyde, and acetaldehyde, and it is more preferable to use formaldehyde. This makes it easier to control the degree of curing.

[0031] The amounts of phenols and aldehydes added in the mixed solution can be, for example, such that the molar ratio of aldehydes to phenols (aldehydes / phenols) is 0.8 to 4.0. This allows the phenols and aldehydes to react with each other to form a resol-type phenolic resin, and further a crosslinked body of the resol-type phenolic resin in part, which can be dispersed in the mixed solution in the form of particles.

[0032] (Hydrophilic polymer) The method for producing the spherical phenolic resin cured material (A) of this embodiment is a wet method. The hydrophilic polymer is necessary to adhere to the surface of the phenols and aldehydes, to disperse the phenols and aldehydes in a spherical shape in the hydrophilic solvent, as if the phenols and aldehydes and the hydrophilic solvent were dispersed as if they were an O / W emulsion. This allows the production of suspended particles of a desired shape.

[0033] The hydrophilic polymer is not limited, and specific examples thereof include water-soluble cellulose derivatives such as hydroxyethyl cellulose, hydroxypropyl cellulose, carboxymethyl cellulose, and cationized hydroxyethyl cellulose; polyvinyl alcohol; alginic acid; guar gum; and gum arabic. The hydrophilic polymer may be one or more of the above specific examples. The hydrophilic polymer may be one or more of the above specific examples selected from the group consisting of hydroxyethyl cellulose, guar gum, and gum arabic, and more preferably hydroxyethyl cellulose. This allows the particle size of the spherical phenolic resin cured material (A) to be within a desired numerical range.

[0034] (Reaction process) In the reaction step, the mixture is stirred to react the phenols with the aldehydes to form suspended particles. The method of reacting the phenols with the aldehydes to form suspended particles can be carried out by stirring the mixture.

[0035] The reaction between the phenols and the aldehydes is carried out, for example, under a basic catalyst. In the reaction process, the phenols and the aldehydes react to form a resol-type phenolic resin, and further, a part of the resol-type phenolic resin crosslinks with each other to form a crosslinked body. In the reaction process, the crosslinking does not proceed completely, and in the curing process described below, the crosslinking proceeds further and the product is cured. That is, the suspended particles include, for example, a resol-type phenolic resin and a crosslinked body of the resol-type phenolic resin.

[0036] After forming the suspended particles, the suspended particles may be washed to remove the hydrophilic polymer on the surface of the suspended particles, which can further improve the handling properties of the spherical cured phenolic resin (A) by preventing aggregation and adhesion between the particles.

[0037] The washing method is not limited, but for example, a method of dispersing the suspended particles in a large amount of hydrophilic solvent such as pure water can be used. This allows the hydrophilic solvent to be removed from the surface of the suspended particles. As a washing method, for example, washing is preferably performed three or more times, more preferably five or more times, with a hydrophilic solvent in an amount from 1 to 2 times the mass of the suspended particles. This is preferable in that the content of impurities can be reduced to a desired numerical range, and it can be used in applications requiring a high degree of cleanliness. It is preferable to perform washing many times within a range that does not complicate the production process, but the upper limit of the number of washing times may be, for example, 10 times or less.

[0038] (basic catalyst) The basic catalyst is not limited as long as it is one that has been used in the reaction between phenols and aldehydes to prepare a conventional resol-type phenolic resin. Specific examples of the basic catalyst include hydroxides of alkali metals such as sodium hydroxide, lithium hydroxide, and potassium hydroxide; oxides and hydroxides of alkaline earth metals such as calcium, magnesium, and barium; and amines such as sodium carbonate, aqueous ammonia, N-(2-aminoethyl)propanolamine, triethylamine, ethylenediamine, diethylenetriamine, triethylenetetramine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, polyethyleneimine, N-(2-aminoethyl)ethanolamine, and hexamethylenetetramine (i.e., hexamine). The basic catalyst may be one or more of the above specific examples in combination.

[0039] As the basic catalyst, amines capable of introducing a nitrogen-containing structure are preferred, and ethylenediamine, diethylenetriamine, triethylenetetramine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, polyethyleneimine, N-(2-aminoethyl)ethanolamine, and hexamethylenetetramine are more preferred. This allows a porous molded body to be obtained that has excellent adhesion to the liquid phenolic resin due to the highly reactive nitrogen-containing structure and has excellent mechanical strength.

[0040] As the basic catalyst, ethylenediamine, diethylenetriamine, triethylenetetramine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, and polyethyleneimine are particularly preferred, which can introduce ethylene crosslinks into the cured product, thereby making it possible to increase the amount of deformation strain when subjected to stress and to obtain a porous molded product with excellent mechanical strength.

[0041] (hardening process) In the curing step, the suspended particles (phenolic resin particles) are heat-treated at a temperature of more than 50° C. and less than 200° C. to cure the suspended particles and obtain a spherical cured phenolic resin product (A).

[0042] Specifically, the resol type phenolic resin in the suspended particles is further crosslinked by heat treatment to form a crosslinked body, and is then cured. From the viewpoint of suitably reducing the density of the spherical phenolic resin cured material (A), for example, it is preferable that a part of the resol type phenolic resin remains without being crosslinked. That is, it is preferable that the spherical phenolic resin cured material (A) contains, for example, a resol type phenolic resin and a crosslinked body of the resol type phenolic resin. The method of heat treatment is not limited, and can be a conventionally known method such as under atmospheric pressure, under reduced pressure, in a gas, in a liquid, etc. Heating may be continued in the reaction step to harden the composition.

[0043] The upper limit of the temperature of the heat treatment in the curing step is less than 200° C., and for example, is preferably less than 170° C., and is preferably 150° C. or less, more preferably 135° C. or less, and even more preferably 130° C. or less. This can suppress oxidation of the spherical phenolic resin cured product (A) and improve compatibility with the phenolic resin.

[0044] The lower limit of the temperature of the heat treatment in the curing step is more than 50° C., and is preferably, for example, 80° C. or higher, and more preferably 110° C. or higher, which can suppress fusion between phenolic resin particles and improve handleability.

[0045] The upper limit of the heat treatment time in the curing step is, for example, 24 hours or less, preferably 12 hours or less, more preferably 8 hours or less, and even more preferably 6 hours or less, which allows the hardness of the phenolic resin particles to be adjusted within an appropriate range.

[0046] The lower limit of the heat treatment time in the curing step is, for example, more than 0 minutes, preferably 30 minutes or more, more preferably 1 hour or more, and even more preferably 2 hours or more, whereby the resol-type phenolic resins in the phenolic resin particles are crosslinked with each other, and the spherical phenolic resin cured product (A) is appropriately cured.

[0047] If necessary, a drying step may be provided. The suspended particles (phenol resin particles) are heat-treated at a temperature of 60° C. or more and 150° C. or less to remove the hydrophilic solvent from the suspended particles. The heat treatment method is not limited, and any conventionally known method can be used as long as it is performed in a gas under atmospheric pressure or under reduced pressure.

[0048] As described above, the curing step and the drying step can be performed by a conventional method as long as they are continuously performed in the atmosphere or under reduced pressure. From the viewpoint of continuously performing the drying step and the curing step, it is preferable to use, for example, a hot air dryer or a reduced pressure stirring drying device as a method for performing the drying step and the curing step.

[0049] In order to improve the uniformity of the composition, the spherical phenolic resin cured product (A) may be further crushed after drying, if necessary. Examples of the crushing method include impact crushers such as pin mills, knife mills, and hammer mills, and airflow crushers such as jet mills and counter jet mills.

[0050] (Liquid phenolic resin (B)) The liquid phenolic resin (B) is a phenolic resin that is liquid at room temperature (25°C). The term "liquid" means that the liquid has fluidity at room temperature (25°C). The viscosity is not particularly limited as long as it can be mixed with the spherical phenolic resin cured product (A) described below. From the viewpoint of production efficiency, however, it is preferably, for example, 10 Pa s or less.

[0051] In this embodiment, by using the liquid phenolic resin (B) which is liquid at room temperature (25°C), the adhesive area with the spherical phenolic resin cured material (A) is increased compared to that of a solid phenolic resin, and therefore the mechanical strength of the resulting porous molded body is improved. As the liquid phenol resin (B), any known liquid phenol resin can be used as long as the effects of the present invention are achieved.

[0052] The liquid phenolic resin (B) is one that contains a methylol group (-CH2-OH) in the resin skeleton, and examples thereof include liquid resol resins synthesized using a basic catalyst or a weak acid catalyst. These may be used alone or in combination of two or more kinds.

[0053] In this step a, the liquid phenolic resin (B) can be used in an amount of 2 to 50 parts by mass, preferably 5 to 30 parts by mass, and more preferably 10 to 20 parts by mass, per 100 parts by mass of the spherical phenolic resin cured product (A). In general, liquid phenolic resins often contain solvents such as water and organic solvents, so the amount of liquid phenolic resin (B) is calculated as the amount of active ingredient. The amount of active ingredient of the liquid phenolic resin can be calculated based on the non-volatile content as described in JIS K 6910.

[0054] The liquid phenolic resin (B) has excellent fluidity, and when used in the specified amount, it can adequately coat the spherical phenolic resin cured product (A). Furthermore, it has excellent adhesion to the spherical phenolic resin cured product (A). Therefore, when used in the specified amount, a porous molded body having high bending strength, bending modulus, and excellent mechanical strength can be obtained.

[0055] [Step b] In this step, a molding material containing the coated spherical cured phenolic resin (AB) obtained in step a is prepared, and the molding material is molded to obtain a porous molded body.

[0056] The molding method for the molded body is not particularly limited, but examples thereof include transfer molding, compression molding, and press molding.

[0057] Since the coated spherical cured phenolic resin (AB) is coated with the liquid phenolic resin (B), the molding material containing the coated spherical cured phenolic resin (AB) can be molded at low pressure, and can be molded at a pressure of normal pressure or less than 0.2 MPa, preferably normal pressure or 0.15 MPa or less. Since the molding material can be molded at low pressure, a porous structure can be obtained stably, and the productivity of the porous molded body is excellent.

[0058] The step b can be carried out in air at a molding temperature of 100°C to 250°C for a molding time of about 10 to 60 minutes. Furthermore, a post-curing step can be carried out on the porous molded body. The post-curing step can be carried out at a heating temperature of 100°C to 250°C for a heating time of about 2 to 9 hours.

[0059] The molding material of the present embodiment may further contain a curing agent. The curing agent can be appropriately selected depending on the type of liquid phenolic resin (B), and is preferably at least one selected from the group consisting of hexamethylenetetramine, isocyanate resin, epoxy resin, hexamethoxymethylolmelamine, and resol resin. Among these, it is preferable to use hexamethylenetetramine and resol resin.

[0060] The molding material of the present embodiment may further contain a filler. Examples of the filler include fibrous base materials, organic fillers, and inorganic fillers. The fibrous base materials are fillers having a fibrous form. The organic fillers and inorganic fillers may each be either granular fillers or plate-like fillers. The plate-like fillers are fillers having a plate shape. The granular fillers are fillers having shapes other than fibrous and plate shapes, including irregular shapes. These may be used alone or in combination of two or more.

[0061] As the granular filler, for example, a granular inorganic filler can be used, such as glass beads, glass powder, calcium carbonate, talc, silica, aluminum hydroxide, clay, and mica.

[0062] Examples of the fibrous filler include fibrous inorganic fillers such as glass fibers, carbon fibers, asbestos fibers, metal fibers, wollastonite, attapulgite, sepiolite, rock wool, aluminum borate whiskers, potassium titanate fibers, calcium carbonate whiskers, titanium oxide whiskers, and ceramic fibers; and fibrous organic fillers such as aramid fibers, polyimide fibers, and poly(paraphenylene benzobisoxazole fibers). These may be used alone or in combination of two or more.

[0063] Examples of the plate-like filler and granular filler include talc, kaolin clay, calcium carbonate, zinc oxide, calcium silicate hydrate, mica, glass flakes, glass powder, magnesium carbonate, silica, titanium oxide, alumina, aluminum hydroxide, magnesium hydroxide, barium sulfate, calcium sulfate, calcium sulfite, zinc borate, barium metaborate, aluminum borate, calcium borate, sodium borate, aluminum nitride, boron nitride, silicon nitride, and pulverized products of the fibrous fillers.

[0064] The molding material of the present embodiment (100% by mass) may contain the filler in an amount of preferably 1 to 70% by mass, more preferably 5 to 50% by mass, and even more preferably 10 to 40% by mass.

[0065] The molding material of the present embodiment may contain other components depending on the application and the needs. Examples of other components include curing accelerators, other resin components, release agents, pigments, dyes, flame retardants, adhesion improvers, coupling agents, toughness imparting agents, and foaming agents.

[0066] The curing accelerator is not particularly limited, and a conventional curing accelerator can be used. Examples of the curing accelerator include oxides or hydroxides of alkaline earth metals such as magnesium oxide, sodium hydroxide, calcium hydroxide, and barium hydroxide; organic acids such as succinic acid, salicylic acid, benzoic acid, and paratoluenesulfonic acid; and inorganic acids such as hydrochloric acid, sulfuric acid, nitric acid, and phosphoric acid.

[0067] Examples of the other resin components include urea resins, resins having a triazine ring such as melamine resins, bismaleimide resins, polyurethane resins, silicone resins, resins having a benzoxazine ring, cyanate ester resins, polyvinyl butyral resins, and polyvinyl acetate resins. If necessary, a combination of two or more of these resins may be used.

[0068] Examples of the release agent include stearic acid, calcium stearate, zinc stearate, and polyethylene. An example of the pigment is carbon black.

[0069] The porous molded body of the present embodiment obtained as described above contains a cured product of the molding material. From the viewpoint of the effect of the present invention, the porous molded body preferably has a molded specific gravity of 0.4 g / cm 3 ~1.2g / cm 3 , more preferably 0.5 g / cm 3 ~1.0g / cm 3 , and more preferably 0.6 g / cm 3 ~0.9g / cm 3 It can be said that: The molded specific gravity was measured from a rectangular molded test piece (g / cm 3 ) = weight of test piece (g) / volume of test piece (cm 3 ) can be measured.

[0070] The elastic modulus of the porous molded body of this embodiment can be 1 GPa to 10 GPa, preferably 2 GPa to 8 GPa. Thus, the porous molded body has excellent mechanical strength and can be suitably used for various applications.

[0071] <Porous carbon material> The porous carbon material of this embodiment is obtained by firing the above-mentioned porous molded body. In the firing step, the firing temperature can be 400 to 2000° C., and the firing time can be 1 to 200 hours.

[0072] The porous molded body and porous carbon material of the present embodiment can be used, for example, in molded articles used in automobiles, aircraft, railway vehicles, ships, general-purpose machines, household electrical appliances, and peripheral parts thereof, or in molded articles, grinding wheels, friction materials, and the like used in housings, structural / mechanical parts, and electrical / electronic parts thereof.

[0073] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can be adopted as long as they do not impair the effects of the present invention. EXAMPLES

[0074] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these.

[0075] (Production Example 1) First, 1000 parts by mass of phenol, which is a phenol, 1120 parts by mass of 37% formaldehyde aqueous solution, which is an aldehyde, 200 parts by mass of 2% hydroxyethylcellulose aqueous solution, which is a hydrophilic polymer, 41 parts by mass of ethylene glycol, which is a hydrophilic solvent, and 235 parts by mass of pure water were prepared as raw material components of the mixed liquid. Next, the raw material components were charged into a reaction vessel and mixed uniformly to prepare a mixed liquid. Next, 270 parts by mass of 33% triethylenetetramine aqueous solution, which is a basic catalyst, was added successively over 60 minutes, and the temperature was raised to 95°C to react with phenol and formaldehyde, and the mixed liquid was reacted and cured for 6 hours. The reaction between phenol and formaldehyde was carried out while stirring the mixed liquid. As a result, suspended particles of phenol and formaldehyde were prepared. The resulting suspended particles were then filtered using a suction funnel, and the cycle of immersion in pure water, washing, and suction filtration was repeated five times, after which the particles were placed in a box-shaped container and dried and hardened at 110°C for 24 hours using a hot air circulation system. The moisture content of the dried and hardened suspended particles was 0.5%. The moisture content is (100-X)% when the weight change rate when the dried suspension particles are treated at 135° C. for 1 hour is X%. The moisture content was measured separately from the process of producing the phenolic resin particles of Example 1. The mixture was then crushed using a hammer mill to obtain a spherical cured phenolic resin A. The average particle size was 358 μm, and the nitrogen content determined by elemental analysis was 3%. Next, 7 parts of liquid phenolic resin (liquid at room temperature of 25°C, PR-55331, manufactured by Sumitomo Bakelite Co., Ltd.) (5 parts as the amount of active resin component) and 100 parts of the obtained spherical phenolic resin cured product were kneaded using a mixer DM type (Shinagawa Kogyosho Co., Ltd.) to obtain a coated spherical phenolic resin cured product A (molding material A) in which the spherical phenolic resin cured product was coated with the liquid phenolic resin.

[0076] (Production Example 2) The same procedure was carried out except that a 1% polyvinyl alcohol aqueous solution was used instead of the 2% hydroxyethyl cellulose aqueous solution of Production Example 1, and 20 parts of triethylamine was used instead of the 33% triethylenetetramine aqueous solution, to obtain a spherical phenolic resin cured product B. The average particle size was 320 μm, and the nitrogen content was 0%. Next, the same procedure as in Production Example 1 was carried out to obtain a coated spherical phenolic resin cured product B (molding material B).

[0077] (Production Examples 3 to 5) Coated spherical phenolic resin cured materials C to E (molding materials C to E) were obtained in the same manner as in Production Example 1, except that the amount of active ingredient of liquid phenolic resin (liquid at room temperature of 25°C, PR-55331, Sumitomo Bakelite Co., Ltd.) per 100 parts of spherical phenolic resin cured material A was changed as shown in Table 1.

[0078] (Production Example 6) 100 parts of spherical phenolic resin cured product A was mixed with a varnish prepared by dissolving 5 parts of solid phenolic resin (solid at room temperature 25°C, PR-50099, Sumitomo Bakelite Co., Ltd.) in 20 parts of methanol, and the mixture was kneaded using a DM-type mixer. The mixture was then spread in a metal container to a thickness of 5 mm or less and dried at 40°C for 24 hours while ventilating, removing the solvent by evaporation and solidifying the resin on the surface of the spherical phenolic resin cured product. After drying, the aggregates were broken down into independent particles using a crusher (Feather Mill FM, Hosokawa Micron Co., Ltd.), and a coated spherical phenolic resin cured product F (molding material F) was obtained in which the phenolic resin cured product was coated with solid phenolic resin.

[0079] [Examples 1 to 5, Comparative Example 1] The coated spherical phenolic resin cured products A to F (molding materials A to F) obtained in Production Examples 1 to 6 were press molded using a press molding machine under the conditions of a molding temperature of 180°C, a molding load of 0.1 MPa, and a molding time of 30 minutes. The physical properties of the obtained porous molded bodies A to F (Examples 1 to 5 and Comparative Example 1, respectively) are shown in Table 1. Furthermore, the porous molded bodies A to F were post-cured by heating at 180°C for 6 hours to obtain porous molded bodies A' to F' (Examples 1 to 5 and Comparative Example 1, respectively). The physical properties of the porous molded bodies A' to F' are shown in Table 1. The spherical phenolic resin cured products A and B were infusible against the heat during press molding and the heat during post-curing.

[0080] (Molding specific gravity) The molded specific gravity of the porous molded bodies obtained in Examples 1 to 5 and Comparative Example 1 was calculated by the following formula. Formula: Molding specific gravity (g / cm 3 ) = weight of test piece (g) / volume of test piece (cm 3 )

[0081] (Flexural strength (flexural stress), flexural modulus) The flexural strength and elastic modulus at room temperature (25°C) of the porous molded bodies obtained in Examples 1 to 5 and Comparative Example 1 were evaluated in accordance with JIS K 6911. The porous molded bodies were cut to a width of 10 mm, a thickness of 4 mm, and a length of 100 mm, and tested using a universal testing machine (Autograph AG-IS, Shimadzu Corporation) with a 5 kN load cell at a span of 64 mm and a head speed of 2 mm / min to measure the flexural strength and flexural modulus.

[0082] [Table 1]

[0083] The porous bodies of the Examples according to the present invention had higher bending strength and bending modulus of elasticity and were superior in mechanical strength compared to the porous bodies of the Comparative Examples.

Claims

1. A step of coating the surface of the spherical phenolic resin cured material (A) with a liquid phenolic resin (B); A step of molding a molding material containing the obtained coated spherical phenolic resin cured material (AB); Including, A method for producing a porous molded body, wherein the spherical phenolic resin cured product (A) is a cured product of a resol resin.

2. The method for producing a porous molded body according to claim 1 , wherein the molding step is performed at a pressure ranging from normal pressure to a pressure less than 0.2 MPa.

3. The method for producing a porous molded body according to claim 1 , wherein the resol resin contains a nitrogen-containing structure.

4. The method for producing a porous molded body according to claim 1 , wherein the resol resin is an ethylene crosslinked resin.

5. The method for producing a porous molded body according to claim 1 , wherein the spherical phenolic resin cured product (A) is infusible by heat.

6. 2. The method for producing a porous molded body according to claim 1, wherein the amount of the liquid phenolic resin (B) is 2 to 50 parts by mass based on 100 parts by mass of the spherical phenolic resin cured product (A).

7. The method for producing a porous molded body according to any one of claims 1 to 6, wherein the molding material further contains an inorganic filler.

8. The present invention includes a coated spherical phenolic resin cured material (AB) in which the surface of a spherical phenolic resin cured material (A) is coated with a liquid phenolic resin (B), The spherical phenolic resin cured material (A) is a molding material which is a cured product of a resol resin.

9. The molding material according to claim 8 , wherein the resole resin comprises a nitrogen-containing structure.

10. The molding material according to claim 8 , wherein the resol resin is an ethylene crosslinked resin.

11. The molding material according to claim 8 , wherein the spherical phenolic resin cured material (A) is infusible by heat.

12. The molding material according to claim 8, comprising 2 to 50 parts by mass of the liquid phenolic resin (B) per 100 parts by mass of the spherical phenolic resin cured material (A).

13. The molding material according to claim 8 , further comprising an inorganic filler.

14. A porous molded body comprising a cured product of the molding material according to any one of claims 8 to 13.

15. Molding density is 0.4g / cm 3 ~1.2g / cm 3 The porous molded body according to claim 14,

16. A porous carbon material obtained by firing the porous molded body according to claim 15.

Citation Information

Patent Citations

  • Porous body and method for manufacturing the same

    JP2011026435A

  • Porous molded article, method for manufacturing the same, porous carbonized material, and porous active carbon

    JP2016145264A