Glass laminate manufacturing method and glass laminate

By controlling the bending rigidity ratio and material properties of the protective film and adhesive layer, the method prevents dent formation on glass members during bonding, ensuring high appearance and flexibility for applications like cover windows.

JP2024147967AInactive Publication Date: 2024-10-17NITTO DENKO CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023060759
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-04
Publication Date
2024-10-17
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Glass members, particularly thin glass, are prone to forming dents when foreign objects are trapped between the glass and a protective film during the bonding process, leading to poor appearance and reduced flexibility.

Method used

The method involves manufacturing a glass laminate by attaching a protective film to a glass member via an adhesive layer, ensuring the bending rigidity ratio of the protective film to the glass member (F1/F0) is 2.50 or less, along with specific ranges for the thickness and material properties of the protective film and adhesive layer to alleviate stress and prevent dent formation.

Benefits of technology

This approach effectively prevents dents on the glass member, maintaining its appearance and flexibility, making it suitable for applications requiring high visual quality, such as cover windows.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024147967000001_ABST
    Figure 2024147967000001_ABST
Patent Text Reader

Abstract

To prevent a dent from remaining in a glass member when subjecting the glass member to air-pressed bonding to another member.SOLUTION: A glass laminate includes at least a glass member having a first main surface and a second main surface. A method for manufacturing the glass laminate includes a first step of adhering a protective film to the first main surface with an adhesive layer interposed therebetween. Bending rigidity of the glass member is F0; bending rigidity of the protective film is F1; and the unit of F0 and F1 is N mm. A ratio of F1 to F0, F1 / F0, is 2.50 or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a glass laminate, including a glass member intended for a cover window, and to the glass laminate. [Background technology]

[0002] Patent Document 1 discloses a glass plate, an adhesive layer, and a film, which are arranged in this order toward one side in the thickness direction. The glass plate has a thickness of less than 40 μm; the average tan δ of the film at −100° C. to −50° C., as determined by a dynamic viscoelasticity test in a tensile mode at a frequency of 10 Hz and a heating rate of 2° C. / min, is 0.04 or more; The optical laminate proposed has an average tensile storage modulus E' of the film at -100°C to -50°C as determined by the dynamic viscoelasticity test of 3 GPa or more and 6 GPa or less. In addition to Patent Document 1, several optical laminates including a glass plate have been proposed (Patent Documents 2 to 4, etc.). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent Publication No. 2022-83323 [Patent Document 2] Patent Publication No. 2022-83324 [Patent Document 3] Patent Publication No. 2022-83325 [Patent Document 4] Patent Publication No. 2022-83326 Summary of the Invention [Problem to be solved by the invention]

[0004] Glass members such as thin glass are used in the processing step of products in the form of a glass laminate with a protective film in order to prevent scratches and ensure a certain degree of ease of handling. However, when the protective film is attached to the glass member, foreign matter may get between the glass member and the protective film. When the glass member and the protective film with the foreign matter sandwiched therebetween are pressure-bonded to another member such as a base film via an adhesive layer, the foreign matter may leave a dent on the glass member. [Means for solving the problem]

[0005] A first aspect of the present invention is a method for producing a glass laminate including at least a glass member having a first main surface and a second main surface, The manufacturing method includes: A first step of attaching a protective film to the first main surface via a pressure-sensitive adhesive layer, The bending stiffness of the glass member is F0; The bending rigidity of the protective film is F1; The units of F0 and F1 are N mm. The method for producing a glass laminate, wherein the ratio of F1 to F0: F1 / F0 is 2.50 or less.

[0006] A second aspect of the present invention provides a glass member having a first main surface and a second main surface; A protective film disposed on the first main surface side; An adhesive layer interposed between the glass member and the protective film, The bending stiffness of the glass member is F0; The bending rigidity of the protective film is F1; The units of F0 and F1 are N mm. The ratio of F1 to F0: F1 / F0 is less than or equal to 2.50. Effect of the Invention

[0007] This can prevent dents from being left on the glass member when the glass member is pressure-bonded to another member. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a schematic vertical cross-sectional view of a glass laminate according to an embodiment of the present disclosure. [Diagram 2] FIG. 2 is a schematic vertical cross-sectional view of a glass laminate according to another embodiment of the present disclosure. [Diagram 3] FIG. 2 is a schematic vertical cross-sectional view of a glass laminate according to still another embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Glass members such as thin glass are sometimes used for applications such as cover windows. Flexibility is required for cover windows. However, in cover windows using glass members such as thin glass, when the surface of the glass member is scratched, the flexibility is significantly reduced. On the other hand, glass members such as thin glass are easily bent, making them difficult to handle in the processing process into products. Therefore, a protective film may be attached to the glass member via an adhesive layer and used in the processing process. Generally, a large number of cullets generated during manufacturing or processing are attached to the glass member. Although the cullets can be removed by thoroughly cleaning the glass member, there is a risk that the glass member may be scratched by cleaning. Therefore, it is difficult to remove all the cullets without scratching the glass member. When a glass member with a protective film is pressure-bonded to another member via an adhesive layer with a foreign object such as cullet sandwiched between the protective film and the glass member, the foreign object may leave a dent on the glass member. When the protective film is peeled off from the glass member together with the adhesive layer, the dent appears on the surface, resulting in poor appearance of the glass member.

[0010] In view of the above, (1) a manufacturing method for a glass laminate according to a first aspect of the present invention is a manufacturing method for a glass laminate including at least a glass member having a first main surface and a second main surface, the manufacturing method including a first step of attaching a protective film to the first main surface via an adhesive layer. The bending rigidity of the glass member is F0, and the bending rigidity of the protective film is F1. The units of F0 and F1 are N·mm. The ratio of F1 to F0: F1 / F0 is 2.50 or less. Hereinafter, the glass member to which the protective film is attached via an adhesive layer may be referred to as a "glass member with protective film".

[0011] According to the above (1), since the glass member and the protective film satisfy the relationship F1 / F0≦2.50, the protective film is sufficiently flexible compared to the glass member and can mitigate stress even when applied. Therefore, when a foreign object is sandwiched between the glass member and the protective film (more specifically, the adhesive layer), and the glass member with the protective film is pressurized and bonded to another member via the adhesive layer, it is possible to prevent the foreign object from leaving a dent on the glass member.

[0012] In this specification, the term "dent" refers to a dent that is formed on a main surface of a glass member due to localized pressure applied, for example, via a foreign object, and that does not disappear even over time.

[0013] (2) In the above (1), the glass laminate may further include a base film disposed on the second main surface side, and an adhesive layer interposed between the base film and the glass member. In such a glass laminate, dents are likely to remain when the protective film is bonded to the base film with a foreign object sandwiched between the protective film and the glass member. In the present invention, even in such a glass laminate, dents are suppressed from remaining by setting the F1 / F0 ratio to a specific range as described above.

[0014] (3) In the above (2), the manufacturing method of the glass laminate may further include a second step of attaching a substrate film to the second main surface under pressure via an adhesive layer after the first step. If a foreign object is sandwiched between the glass member and the protective film in the glass member with protective film formed in the first step, a dent is likely to be formed in the glass member when pressure is applied in the second step. In the present invention, even when the manufacturing method includes the second step, dents are prevented from remaining in the glass member by setting the F1 / F0 ratio in a specific range as described above.

[0015] (4) In the above (3), the manufacturing method of the glass laminate may include a third step of peeling the protective film and the adhesive layer from the first main surface after the second step. If a dent is formed on the glass member, the first main surface of the glass member is exposed when the protective film and the adhesive layer are peeled off from the glass member, revealing the dent and impairing the appearance. Even in such a case, the present invention reduces the dent itself, thereby maintaining the high appearance of the glass member.

[0016] (5) In any one of the above (1) to (4), the pressure-sensitive adhesive layer may have an indentation modulus of 50 MPa or more and 500 MPa or less at 25° C. In this case, the effect of suppressing dents by setting the F1 / F0 ratio in the above range is more likely to be exerted.

[0017] (6) In any one of the above (1) to (5), the thickness of the protective film may be 100 μm or less. When the thickness of the protective film is in this range, the protective film is easily deformed, and in addition to setting the F1 / F0 ratio in a specific range, stress due to foreign matter is easily alleviated, and dents in the glass member can be suppressed.

[0018] (7) In any one of the above (1) to (6), the thickness of the adhesive layer may be 5 μm or more. In this case, the adhesive layer and the protective film can reduce stress caused by foreign matter, thereby preventing dents from being formed in the glass member.

[0019] (8) In any one of the above (1) to (7), the glass member may have a thickness of 50 μm or less. When the glass member has a thickness of 50 μm or less, the influence of deformation due to foreign matter is more likely to become apparent than when the thickness exceeds 50 μm. Even in such a case, in the present invention, the F1 / F0 ratio is set within a specific range, thereby making it possible to suppress the formation of dents in the glass member.

[0020] (9) The present invention also includes a glass laminate. The glass laminate includes at least a glass member having a first main surface and a second main surface, a protective film disposed on the first main surface side, and an adhesive layer interposed between the glass member and the protective film. The bending rigidity of the glass member is F0, and the bending rigidity of the protective film is F1. The units of F0 and F1 are N·mm. The ratio of F1 to F0: F1 / F0 is 2.50 or less.

[0021] (10) In the above (9), the pressure-sensitive adhesive layer may have an indentation modulus at 25° C. of 50 MPa or more and 500 MPa or less.

[0022] (11) In the above (9) or (10), the protective film may have a thickness of 100 μm or less.

[0023] (12) In any one of the above (9) to (11), the pressure-sensitive adhesive layer may have a thickness of 5 μm or more.

[0024] (13) In any one of the above (9) to (12), the glass member may have a thickness of 50 μm or less.

[0025] (14) In any one of the above (9) to (13), the glass laminate may further include a base film disposed on the second main surface side, and an adhesive layer interposed between the base film and the glass member.

[0026] The manufacturing method of the glass laminate and the glass laminate of the present invention will be described in more detail below, including the above (1) to (14). At least one of the above (1) to (14) may be combined with at least one of the elements described below, provided that there is no technical contradiction.

[0027] When referring to the drawings, the shapes and dimensions of each component in each drawing are not shown to the same scale as in reality. In order to clarify the characteristics of each component, the relative relationship of these dimensions is shown diagrammatically and exaggeratedly.

[0028] [Glass laminate] A glass laminate according to one aspect of the present invention includes at least a glass member having a first principal surface and a second principal surface, a protective film disposed on the first principal surface side, and an adhesive layer interposed between the glass member and the protective film, where the bending rigidity of the glass member is F0 (unit: N mm), and the bending rigidity of the protective film is F1 (unit: N mm).

[0029] In the present invention, the ratio of F1 to F0: F1 / F0 is 2.50 or less. By setting the F1 / F0 ratio in such a range, the formation of dents on the first main surface of the glass member due to the inclusion of foreign matter is reduced. From the viewpoint of further reducing the formation of dents, the F1 / F0 ratio may be 2.20 or less, or may be 2.00 or less. The F1 / F0 ratio may be greater than 0 (e.g., greater than 0.00) and greater than or equal to 0.10. The F1 / F0 ratio may be, for example, greater than 0 and less than or equal to 2.50, or greater than or equal to 0.10 and less than or equal to 2.50. F1 and F0 are adjusted by selecting the thickness and material of the protective film and the glass member, the layer structure of the protective film, and the like.

[0030] The product of the tensile modulus E0 (unit: GPa) of the glass member and the thickness T0 (unit: m) is R0 (unit: N / m), and the product of the tensile modulus E1 (unit: GPa) of the protective film and the thickness T1 (unit: m) is R1 (unit: N / m). In this case, the ratio of R1 to R0: R1 / R0 may be 0.20 or less, 0.19 or less, or 0.18 or less. R0 and R1 each indicate the hardness or stiffness of the glass member and the protective film. When the R1 / R0 ratio, which is the relationship between the hardness of the glass member and the protective film, is in the above-mentioned range, the formation of dents on the first main surface of the glass member due to the inclusion of foreign matter is further reduced. The R1 / R0 ratio may be 0.01 or more, or 0.05 or more. The R1 / R0 ratio may be, for example, 0.01 or more and 0.20 or less, or 0.05 or more and 0.20 or less. The tensile moduli E0 and E1 are adjusted by selecting the materials of the glass member and the protective film, as well as the layer structure of the protective film.

[0031] (Glass components) The bending stiffness F0 of the glass member is 2.0×10 6 N mm or more 7.3×10 7 N·mm or less, 2.0×10 6 N mm or more 9.1×10 6 N·mm or less. When the bending rigidity of the glass member is in this range, appropriate bendability is obtained, but the glass member is easily deformed and dents are easily formed. In the present disclosure, by setting the F1 / F0 ratio in a specific range, it is possible to suppress the formation of dents even when the bending rigidity of the glass member is in this range.

[0032] The glass member may be, for example, a glass film. The glass film is also generally referred to as thin glass. The glass member preferably has a uniform thickness.

[0033] Glass films such as thin glass have high flexibility and may be supplied in a rolled form. Therefore, a long glass member (such as a glass film) may be used in the glass laminate. However, this is not limited to this case, and for example, a large-sized glass member may be used. When multiple large-sized glass members are used, they may all be the same glass members, or different glass members may be arranged in different positions depending on the purpose.

[0034] The composition of the glass constituting the glass member is not particularly limited. Examples of the glass include soda-lime glass, borate glass, aluminosilicate glass, and quartz glass. The glass may be non-alkali glass or low-alkali glass. The total content of alkali metal components (e.g., Na2O, K2O, Li2O) in the glass may be 15 mass% or less, or 10 mass% or less.

[0035] The thickness of the glass member may be 100 μm or less. From the viewpoint of easily obtaining the effect of keeping the F1 / F0 ratio in a specific range, the thickness of the glass member is preferably 50 μm or less, and may be 35 μm or less or 30 μm or less. The thickness of the glass member may be 10 μm or more.

[0036] In this specification, the thickness of each component of the glass laminate is the average value of thicknesses measured at any multiple locations (for example, five locations) unless otherwise specified.

[0037] The glass member is manufactured by any suitable method. Typically, the glass film is manufactured by melting a mixture containing ceramics (silica, alumina, etc.) as a main raw material, an antifoaming agent (mirabilite, antimony oxide, etc.), and a reducing agent (carbon, etc.) at a temperature of 1400°C to 1600°C, forming it into a film, and then cooling it. Examples of the glass film forming method include the slot downdraw method, the fusion method, and the float method. The glass film obtained by these methods may be chemically polished with a solvent such as hydrofluoric acid as necessary to further reduce the thickness or improve the smoothness of the surface and edge.

[0038] The surface of the glass member may be subjected to a surface treatment in order to improve adhesion between the glass member and an adhesive layer or pressure-sensitive adhesive layer that comes into contact with the glass member. The surface treatment is not particularly limited, and examples thereof include a corona treatment, a plasma treatment, and a coupling treatment.

[0039] If necessary, a surface coating layer having various functions may be provided on at least a part of the first main surface of the glass member.

[0040] Examples of the surface coating layer include a fingerprint-resistant coating layer, a hard coating layer, an anti-reflection layer, an anti-glare layer, an anti-stain layer, an anti-sticking layer, a hue adjustment layer, an antistatic layer, an easy-adhesion layer, a component-dispersion prevention layer, an impact absorption layer, and a shatterproof layer. The surface coating layer can be made of various materials, and for example, the fingerprint-resistant coating layer includes a fluororesin, a silicone resin, and the like. Other surface coating layers are formed, for example, of an acrylic coating agent, a melamine coating agent, a urethane coating agent, an epoxy coating agent, a silicone coating agent, and an inorganic coating agent. The coating agent may include an additive. Examples of the additive include a silane coupling agent, a colorant, a dye, a pigment, a filler, a surfactant, a plasticizer, an antistatic agent, a surface lubricant, a leveling agent, an antioxidant, a light stabilizer, an ultraviolet absorber, a polymerization inhibitor, and an antifouling agent.

[0041] The surface coating layer may be formed on the first main surface of the glass member before the protective film is disposed on the glass member, or may be formed after the protective film and the pressure-sensitive adhesive layer are peeled off.

[0042] (Protective film) The protective film is disposed on the first main surface of the glass member via a pressure-sensitive adhesive layer in order to ensure ease of handling of the glass member, etc. Such a protective film is sometimes referred to as a first protective film.

[0043] The first protective film is not particularly limited, and may be composed of, for example, a resin film. The resin constituting the resin film may be a thermoplastic resin or a thermosetting resin. Examples of the thermoplastic resin are polyethersulfone-based resin, polycarbonate-based resin, acrylic-based resin, polyester-based resin, polyolefin-based resin, cycloolefin-based resin, polyimide-based resin, polyamide-based resin, polyimideamide-based resin, polyarylate-based resin, polysulfone-based resin, and polyetherimide-based resin. Examples of the polyester-based resin are aromatic polyester-based resin (polyalkylene arylate resin, etc.). Examples of the polyalkylene arylate resin are polyethylene terephthalate (PET) resin, polybutylene terephthalate resin, and polyethylene naphthalate resin. Examples of the cycloolefin-based resin are norbornene-based resin. Examples of the thermosetting resin are epoxy-based resin, urethane-based resin, and silicone-based resin. However, these resins are merely examples, and the resin constituting the resin film is not limited to these. The resin film may contain one type of resin or may contain two or more types of resin in combination. The first protective film may be a single layer or may be multi-layered. Each layer constituting the multi-layered first protective film may contain one type of resin or may contain two or more types of resin in combination. In consideration of transportability and strength, a film made of PET resin is preferable.

[0044] The thickness of the first protective film may be 200 μm or less, 110 μm or less, or 100 μm or less. When the F1 / F0 ratio is within a specific range and the thickness of the first protective film is relatively small, such as 110 μm or less or 100 μm or less, the film is easily deformed, and stress caused by foreign matter is easily alleviated. Thus, the formation of dents in the glass member can be further reduced. The thickness of the first protective film may be 10 μm or more, 20 μm or more, 35 μm or more, or 38 μm or more. The thickness of the first protective film may be, for example, 10 μm or more to 200 μm or less, 20 μm or more to 110 μm or less, or 20 μm or more to 100 μm or less.

[0045] The tensile modulus E1 of the protective film is 0.4×10 5 N / m or more 8.0×10 5 When the tensile modulus E1 of the protective film is in such a range, it is easy to adjust the R1 / R0 ratio to the above range.

[0046] (Adhesive layer) The adhesive layer is interposed between the glass member and the protective film, and may be referred to as a first adhesive layer.

[0047] In the present disclosure, the pressure-sensitive adhesive layer is composed of a pressure-sensitive adhesive. The pressure-sensitive adhesive layer is non-curable and has fluidity. On the other hand, the adhesive layer is formed by curing a coating of the adhesive. Therefore, the adhesive layer does not have substantial fluidity. Thus, in the present disclosure, the adhesive layer and the pressure-sensitive adhesive layer are distinguished from each other.

[0048] The storage modulus of the first pressure-sensitive adhesive layer at 25°C is, for example, 10 MPa or less, and is usually 1 MPa or less. The storage modulus of the first pressure-sensitive adhesive layer at 25°C may be 0.2 MPa or less or 0.1 MPa or less. When the storage modulus of the first pressure-sensitive adhesive layer is in such a range, the protective film is easily attached to the glass member and fixed, and the first pressure-sensitive adhesive layer together with the protective film can be relatively easily peeled off from the glass member. The storage modulus of the first pressure-sensitive adhesive layer at 25°C may be 0.001 MPa or more. The storage modulus of the first adhesive layer at 25°C may be greater than 10 MPa and may be 100 MPa or more, and is usually about 1 GPa. The first pressure-sensitive adhesive layer is also distinguished from the adhesive layer by its storage modulus.

[0049] The first pressure-sensitive adhesive layer may have an indentation modulus of 50 MPa or more and 500 MPa or less at 25° C. In this case, the effect of suppressing dents by setting the F1 / F0 ratio in the above range is more likely to be exerted.

[0050] The adhesive constituting the first adhesive layer is not particularly limited, and examples thereof include acrylic adhesives, rubber adhesives, silicone adhesives, urethane adhesives, vinyl alkyl ether adhesives, polyvinylpyrrolidone adhesives, polyacrylamide adhesives, and cellulose adhesives.

[0051] Each adhesive may contain, for example, a base polymer, a crosslinking agent, additives (e.g., tackifiers, coupling agents, polymerization inhibitors, crosslinking retarders, catalysts, plasticizers, softeners, fillers, colorants, metal powders, UV absorbers, light stabilizers, antioxidants, deterioration inhibitors, surfactants, antistatic agents, surface lubricants, leveling agents, corrosion inhibitors, particles of inorganic or organic materials (metal compound particles (such as metal oxide particles), resin particles, etc.)). However, the components of an adhesive are not limited to these.

[0052] The thickness of the first adhesive layer may be 3 μm or more. The thickness of the first adhesive layer is preferably 5 μm or more, more preferably 15 μm or more or 20 μm or more. In these cases, the first adhesive layer as well as the first protective film relieves stress caused by foreign matter, further reducing the formation of dents on the glass member. The thickness of the first adhesive layer may be 50 μm or less.

[0053] (others) The glass laminate may further include a base film disposed on the second main surface side of the glass member, and an adhesive layer interposed between the base film and the glass member. A second protective film may be disposed on the main surface of the base film opposite the glass member via a second adhesive layer. The glass laminate may further include a second protective film and a second adhesive layer in addition to the base film and the adhesive layer. However, the glass laminate is not limited to such a configuration, and a desired layer may be provided on the main surface of the base film opposite the glass member depending on the application of the glass laminate. For the second protective film and the second adhesive layer, the explanations for the first protective film and the first adhesive layer can be referred to, respectively.

[0054] (Base film) The substrate film is not particularly limited and may be selected according to the application of the glass laminate. The substrate film may be selected from the resin film and the optical film exemplified for the protective film. The second substrate film may be a single layer film or a multilayer film. The second substrate film may be, for example, a multilayer film including an optical film. Such a multilayer film may be a multilayer film including an optical film and a substrate film (such as the above-mentioned resin film), a multilayer film including two or more optical films, or a multilayer film including one or more optical films and a separator. Each film constituting the multilayer film may be directly bonded or may be bonded via a pressure-sensitive adhesive layer or an adhesive layer.

[0055] The optical film is not particularly limited, but may be, for example, a polarizing plate, a retardation plate, or an isotropic film. Examples of materials constituting the optical film include polyvinyl alcohol resins, polyolefin resins, cyclic olefin resins, polycarbonate resins, cellulose resins, polyester resins, polyvinyl alcohol resins, polyamide resins, polyimide resins, polyether resins, polystyrene resins, (meth)acrylic resins, (meth)acrylic urethane resins, polysulfone resins, acetate resins, epoxy resins, and silicone resins. The optical film may be a metal oxide film (metal film, ITO film, etc.), or a laminate film of a metal film and a resin film.

[0056] The thickness of the substrate film may be 5 μm or more and 300 μm or less.

[0057] At least a part of the surface layer of the substrate film on the side opposite to the glass member may be provided with a surface coating layer having various functions, if necessary. For the surface coating layer, the description of the surface coating layer formed on the surface of the glass member may be referred to. The surface coating layer may be provided after or before laminating the substrate film on the glass member.

[0058] (adhesive layer) The adhesive layer is interposed between the base film and the glass member. The adhesive layer is formed by applying an adhesive to at least one of the main surface of the base film facing the glass member and the second main surface of the glass member, stacking the glass member and the base film so as to sandwich the adhesive therebetween, and then pressing and bonding them together. More specifically, the adhesive layer is formed by sandwiching the adhesive between the glass member and the base film, and curing the adhesive while pressing them in the thickness direction.

[0059] The adhesive is not particularly limited, and any suitable adhesive may be used. Examples of the adhesive include an adhesive containing a resin having a cyclic ether group (such as an epoxy group, a glycidyl group, or an oxetanyl group), an adhesive containing an acrylic resin, and an adhesive containing a silicone resin. The adhesive may be a thermosetting type or a photosetting type (such as an ultraviolet ray curing type).

[0060] The thickness of the adhesive layer may be 0.5 μm or more and 20 μm or less, 1 μm or more and 20 μm or less, or 1 μm or more and 5 μm or less.

[0061] <Method of measuring physical properties> (A) Bending rigidity of glass components and protective films The bending rigidity of the glass member and the protective film is measured in accordance with JIS K 7171: 2022. The bending rigidity is measured using test pieces (length 50 mm × width 6 mm) made from each of the glass member and the protective film under conditions of a test speed of 2 mm / min, a support distance of 25 mm, and an indenter radius of 5 mm.

[0062] (B) Tensile modulus of glass member and protective film The tensile modulus (GPa) of the glass member and the protective film is measured using an autograph (for example, a precision universal testing machine manufactured by Shimadzu Corporation).

[0063] (C) Indentation modulus of adhesive layer The indentation elastic modulus of the pressure-sensitive adhesive layer can be measured by a nanoindenter method using a measurement sample by pressing the pressure-sensitive adhesive layer of the measurement sample from the side with an indenter under the following conditions and analyzing the obtained load-displacement curve. Equipment: Triboindenter (manufactured by Hysitron Inc.) Sample size: 10mm length x 10mm width Indenter: Concial (spherical indenter: radius of curvature 10μm) Measurement method: Single indentation measurement Measurement temperature: 25℃ Indenter depth: 5000nm Analysis: Oliver Pharr analysis based on load-displacement curve

[0064] The measurement sample is a sample obtained by subjecting the side of a laminate of a first protective film and a first adhesive layer (or a laminate of a second protective film and a second adhesive layer) to focused ion beam (FIB) processing. The size of the sample is 10 mm length x 10 mm width. If the protective film and the adhesive constituting the adhesive layer for the above-mentioned laminate to be analyzed cannot be obtained, a sample may be prepared by cutting a glass laminate to the above-mentioned size and subjecting the side to FIB processing. The FIB processing is performed under the following conditions. FIB processing equipment: Thermo Fisher Scientific, Helios G4 UX Acceleration voltage: FIB 30kV Processing temperature: -160℃ After processing, the sample is returned to room temperature and removed from the apparatus, and then the indentation elastic modulus is measured by pressing an indenter into the side of the FIB-processed adhesive layer.

[0065] (D) Storage modulus (D-1) Storage modulus of adhesive layer The storage modulus of the adhesive layer can be measured in a torsion mode in accordance with JIS K 7244-1: 1998. Specifically, the adhesive coating is sandwiched between parallel plates, and the viscoelasticity is measured under the following conditions using a dynamic viscoelasticity measuring device (for example, "Advanced Rheometric Expansion System (ARES)" manufactured by Rheometric Scientific), to determine the storage modulus at 25°C. The measurement may be performed five or more times to determine the average value.

[0066] Measurement conditions Deformation mode: Torsion Measurement frequency: 1Hz Measurement temperature: -40℃~+150℃ Heating rate: 5℃ / min

[0067] (D-2) Storage modulus of adhesive layer The storage modulus of the adhesive layer can be measured as the tensile storage modulus in accordance with JIS K 7244-1:1998. Specifically, the adhesive is first formed into a film and cured to produce a cured film having a thickness of about 20 μm. This film is cut to a predetermined size to produce a test piece. Viscoelasticity is measured for this test piece using a dynamic viscoelasticity measuring device (for example, a multi-function dynamic viscoelasticity measuring device "DMS6100" manufactured by Hitachi High-Tech Science Corporation) under the following conditions to determine the tensile storage modulus at 25°C. The measurement may be performed five or more times to obtain an average value.

[0068] Measurement conditions Temperature range: -100℃~+200℃ Heating rate: 2℃ / min Mode: Tensile Sample width: 10mm Chuck distance: 20mm Frequency: 10Hz Distortion amplitude: 10μm Atmosphere: Air (250ml / min) Data acquisition interval: 0.5 min (every 1°C)

[0069] [Method of manufacturing glass laminate] An example of a method for producing a glass laminate according to the present disclosure will be described below. For components of the glass laminate, the above description of the glass laminate can be referred to.

[0070] The method for manufacturing a glass laminate includes a first step of attaching a protective film (first protective film) to a first main surface of a glass member via an adhesive layer (first adhesive layer), where the bending rigidity F0 of the glass member and the bending rigidity F1 of the protective film (first protective film) satisfy the relationship F1 / F0≦2.50 as described above.

[0071] The method for producing a glass laminate may further include a second step of attaching the base film to the second main surface under pressure via the adhesive layer after the first step, and a third step of peeling the protective film (first protective film) and the pressure-sensitive adhesive layer (first pressure-sensitive adhesive layer) from the first main surface after the second step.

[0072] (1st step) In the first step, an adhesive may be applied to at least one of the first main surface of the glass member and the main surface of the first protective film facing the glass member to form an adhesive layer, and the glass member and the first protective film may be attached via the adhesive layer. Alternatively, the first protective film on which the adhesive layer is formed (sometimes referred to as the first protective film with adhesive layer) may be attached to the first main surface of the glass member so that the adhesive layer is sandwiched between the first protective film and the glass member. In this case, the first protective film with adhesive layer is prepared prior to attachment to the glass member. The first protective film with adhesive layer may be a commercially available product, or may be formed by applying an adhesive to one main surface of the protective film.

[0073] (2nd process) In the second step, a glass laminate is obtained that includes a base film disposed on the second main surface side of the glass member and an adhesive layer interposed between the base film and the glass member in addition to the configuration of the glass member, the first adhesive layer, and the first protective film. More specifically, in the second step, an adhesive is applied to at least one of the second main surface of the glass member and one main surface of the base film, and the glass member and the base film are pressurized and bonded with the adhesive interposed between them. The adhesive is cured while the glass member and the base film are pressed in the thickness direction to form an adhesive layer. In this way, the above-mentioned glass laminate is formed. The adhesive may be cured by heating or by light irradiation depending on the type of adhesive.

[0074] If a foreign object is sandwiched between the glass member and the first protective film (more specifically, the first pressure-sensitive adhesive layer), the foreign object is likely to cause a dent in the first main surface of the glass member when the glass member is pressurized and bonded to the base film in step 2. In the present disclosure, by setting the F1 / F0 ratio within a specific range, the formation of a dent in the glass member in step 2 is reduced.

[0075] The base film may be adhered to the glass member as a laminate with one or more other layers. After adhering the base film to the glass member, one or more other layers may be laminated on the main surface of the base film opposite the glass member. For example, the base film and the glass member may be pressure-adhered in a laminate state of the base film, the second protective film, and the second pressure-sensitive adhesive layer interposed therebetween.

[0076] (3rd step) In the third step, after the second step, the first protective film and the adhesive layer (first adhesive layer) are peeled off from the first main surface of the glass member. This results in a laminate in which the base film and the glass member are bonded via the adhesive layer. As described above, other layers may be laminated on the base film. By peeling off the first protective film and the first adhesive layer, the first main surface of the glass member is exposed. In the present disclosure, the formation of dents due to foreign matter is reduced, so that excellent appearance is ensured even if the first main surface of the glass member is exposed. Therefore, the glass member can be used for applications requiring excellent appearance, such as a cover window.

[0077] (others) When the glass laminate further includes a second protective film and a second pressure-sensitive adhesive layer, the second protective film and the second pressure-sensitive adhesive layer may be peeled off from the other main surface of the base film, if necessary.

[0078] Each of Figs. 1 to 3 is a schematic vertical cross-sectional view showing an embodiment of a glass laminate according to the present disclosure. 1 has a glass member 1, a first protective film 2, and a first pressure-sensitive adhesive layer 3 interposed therebetween. Glass member 1 has a first main surface and a second main surface, and first pressure-sensitive adhesive layer 3 is in contact with the first main surface.

[0079] 2 has a base film 4 provided on the second main surface side of the glass member 1 in addition to the configuration in Fig. 1. More specifically, the glass laminate 111 has a glass member 1, a first protective film 2 attached to the first main surface of the glass member 1 via a first pressure-sensitive adhesive layer, and a base film 4 attached to the second main surface of the glass member 1 via an adhesive layer 5.

[0080] 2, glass laminate 211 in Fig. 3 has a second protective film 12 on the side of base film 4 opposite to glass member 1. More specifically, glass laminate 211 has glass member 1, a first protective film 2 attached to a first main surface of glass member 1 via a first pressure-sensitive adhesive layer, base film 4 attached to a second main surface of glass member 1 via adhesive layer 5, and a second protective film attached to a main surface of base film 4 opposite to glass member 1 via a second pressure-sensitive adhesive layer 13.

[0081] [Example] The present invention will be specifically described below based on examples and comparative examples, but the present invention is not limited to the following examples.

[0082] Examples 1-2 and Comparative Examples 1-2 A glass laminate having the layer structure shown in FIG. 3 was produced by the following procedure. (1) Preparation of materials for each layer The following materials were prepared: (First protective film) A PET film ("Diafoil S100 (registered trademark)" manufactured by Mitsubishi Chemical Corporation) having the thickness, tensile modulus E1, R1, and bending rigidity F1 shown in Table 1 was prepared.

[0083] (glass film) An ultra-thin glass sheet ("G-leaf (registered trademark)" manufactured by Nippon Electric Glass Co., Ltd.) was prepared having the thickness, tensile modulus E0, R0, and bending rigidity F0 shown in Table 1. The glass film had a rectangular shape in a plan view and a size of 280 mm long x 368 mm wide.

[0084] (Adhesive for the first adhesive layer) An acrylic adhesive was prepared according to the following procedure. (Preparation of Acrylic Oligomer) 60 parts by mass of dicyclopentanyl methacrylate and 40 parts by mass of methyl methacrylate as monomer components, 3.5 parts by mass of α-thioglycerol as a chain transfer agent, and 100 parts by mass of toluene as a polymerization solvent were mixed and stirred at 70°C for 1 hour under a nitrogen atmosphere. Next, 0.2 parts by mass of 2,2'-azobisisobutyronitrile was added as a thermal polymerization initiator, and reacted at 70°C for 2 hours, and then heated to 80°C and reacted for 2 hours. Thereafter, the reaction liquid was heated to 130°C, and toluene, the chain transfer agent, and unreacted monomers were dried and removed to obtain a solid acrylic oligomer. The weight average molecular weight of the acrylic oligomer was 5100, and the glass transition temperature (Tg) was 130°C.

[0085] (Preparation of Base Polymer Composition) 43 parts by weight of lauryl acrylate, 44 parts by weight of 2-ethylhexyl acrylate, 6 parts by weight of 4-hydroxybutyl acrylate, and 7 parts by weight of N-vinyl-2-pyrrolidone were mixed with 0.015 parts by weight of "Omnirad 184" manufactured by IGM Resins BV as a photopolymerization initiator, and the mixture was polymerized by irradiating with ultraviolet light to obtain a base polymer composition (polymerization rate: approximately 10%).

[0086] (Preparation of acrylic adhesive) An acrylic adhesive was prepared by adding 0.07 parts by mass of 1,6-hexanediol diacrylate, 1 part by mass of the acrylic oligomer described above, and 0.3 parts by mass of a silane coupling agent ("KBM403J" manufactured by Shin-Etsu Chemical Co., Ltd.) to 100 parts by mass of the above base polymer composition and mixing them uniformly.

[0087] (Base film, second adhesive layer, and second protective film) As a substrate film, a PET film having a thickness of 50 μm (Diafoil S100 (registered trademark) manufactured by Mitsubishi Chemical Corporation) was prepared. The above acrylic adhesive was applied to one main surface of a 50 μm-thick PET film (Diafoil S100 (registered trademark) manufactured by Mitsubishi Chemical Corporation) as a second protective film to form a 5 μm-thick second adhesive layer, thereby producing a protective film with an adhesive layer. This protective film with an adhesive layer was attached to a substrate film to produce a laminate having a substrate film.

[0088] (Adhesive for adhesive layer) An epoxy adhesive was prepared by blending 70 parts by mass of an aliphatic alicyclic epoxy resin (Celloxide 2021P, epoxy equivalent 128 to 133 g / eq., manufactured by Daicel Corporation), 5 parts by mass of a trifunctional aliphatic epoxy resin (EHPE3150, epoxy equivalent 170 to 190 g / eq., manufactured by Daicel Corporation), 19 parts by mass of an oxetane resin (Aron Oxetane (registered trademark), manufactured by Toa Gosei Co., Ltd.), 4 parts by mass of a silane coupling agent (KBM-403, 3-glycidoxypropyltrimethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd.), and 2 parts by mass of a photoacid generator (CPI101A, triarylsulfonium salt, manufactured by San-Apro Ltd.).

[0089] (2) Formation of glass laminate An acrylic adhesive was applied to one main surface of the first protective film, and the first protective film was attached to the first main surface of the glass film. An adhesive was applied to both the main surface of the base film of the laminate having the base film and the second main surface of the glass film to form a coating film, and the laminates were then bonded together. The obtained laminate was pressed in the thickness direction, and irradiated with UV light to harden the adhesive, forming an adhesive layer. In this way, a glass laminate was formed.

[0090] (3) Evaluation The evaluation of foreign matter and dents was carried out according to the following procedure. The first protective film and the first adhesive layer were peeled off from the glass laminate to expose the glass film. The first adhesive layer and the first main surface of the glass film were observed, and the number of foreign objects and the number of dents were counted. 2The number of foreign objects and the number of dents per unit area were calculated. The number of dents was divided by the number of foreign objects (= number of dents / number of foreign objects) to evaluate the degree of inhibition of dent formation. When the value of number of dents / number of foreign objects was 0.7 or less, it was determined that the formation of dents was inhibited.

[0091] The results of the Examples and Comparative Examples are shown in Table 1. In Table 1, A1 and A2 correspond to Examples 1 and 2, and B1 and B2 correspond to Comparative Examples 1 and 2.

[0092] [Table 1]

[0093] As shown in Table 1, in the examples that satisfied F1 / F0≦2.50, the ratio of the number of dents to the number of foreign bodies was low, which means that the formation of dents in the glass member was suppressed. In contrast, in the comparative examples that satisfied F1 / F0<2.50, dents were formed in most of the locations where foreign bodies had been present. [Industrial Applicability]

[0094] The glass laminate of the present disclosure suppresses dents in the glass member caused by foreign matter. Therefore, the glass laminate is suitable for applications requiring flexibility and excellent appearance of the glass member, such as for cover windows. However, the applications of the glass laminate are not limited to these. [Explanation of symbols]

[0095] 1 Glass components 2 Protective film 3 First adhesive layer 4. Base film 5 Adhesive layer 11, 111, 211 Glass laminate 12 Second protective film 13 Second adhesive layer

Claims

1. A method for producing a glass laminate including at least a glass member having a first main surface and a second main surface, The manufacturing method includes: A first step of attaching a protective film to the first main surface via a pressure-sensitive adhesive layer, The bending stiffness of the glass member is F0, The bending rigidity of the protective film is F1; The units of F0 and F1 are N mm. A method for producing a glass laminate, wherein a ratio of F1 to F0: F1 / F0 is 2.50 or less.

2. 2 . The method for producing a glass laminate according to claim 1 , wherein the glass laminate further includes a base film disposed on the second main surface side, and an adhesive layer interposed between the base film and the glass member.

3. 3. The method for producing a glass laminate according to claim 2, further comprising, after the first step, a second step of attaching the base film to the second main surface under pressure via the adhesive layer.

4. The method for producing a glass laminate according to claim 3 , further comprising, after the second step, a third step of peeling the protective film and the pressure-sensitive adhesive layer from the first main surface.

5. The method for producing a glass laminate according to claim 1 or 2, wherein the pressure-sensitive adhesive layer has an indentation modulus at 25°C of 50 MPa or more and 500 MPa or less.

6. The method for producing a glass laminate according to claim 1 or 2, wherein the protective film has a thickness of 100 μm or less.

7. The method for producing a glass laminate according to claim 1 or 2, wherein the pressure-sensitive adhesive layer has a thickness of 5 μm or more.

8. The method for producing a glass laminate according to claim 1 or 2, wherein the glass member has a thickness of 50 μm or less.

9. a glass member having a first major surface and a second major surface; A protective film disposed on the first main surface side; An adhesive layer interposed between the glass member and the protective film, The bending stiffness of the glass member is F0, The bending rigidity of the protective film is F1; The units of F0 and F1 are N mm. A glass laminate, wherein the ratio of F1 to F0: F1 / F0 is 2.50 or less.

10. The glass laminate according to claim 9 , wherein the pressure-sensitive adhesive layer has an indentation modulus at 25° C. of 50 MPa or more and 500 MPa or less.

11. The glass laminate according to claim 9 or 10, wherein the protective film has a thickness of 100 μm or less.

12. The glass laminate according to claim 9 or 10, wherein the pressure-sensitive adhesive layer has a thickness of 5 μm or more.

13. 11. The glass laminate according to claim 9, wherein the glass member has a thickness of 50 μm or less.

14. moreover, A base film disposed on the second main surface side; The glass laminate according to claim 9 or 10, further comprising: an adhesive layer interposed between the substrate film and the glass member.

Citation Information

Patent Citations

  • Optical laminate and optical laminate having adhesive layer

    JP2022083323A

  • Optical laminate

    JP2022083324A

  • Optical laminate

    JP2022083325A

  • Optical laminate

    JP2022083326A