Semiconductor light-emitting element and manufacturing method for semiconductor light-emitting element

The semiconductor light emitting device with a laminated structure of protective layers and a manufacturing method improves moisture resistance and reliability by preventing cracks during cutting, enabling its use without a package.

JP2024147982AActive Publication Date: 2024-10-17NIKKISO CO LTD

Patent Information

Application Number
JP2023060795
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-04
Publication Date
2024-10-17
Estimated Expiration
2043-04-04

AI Technical Summary

Technical Problem

Existing semiconductor light emitting devices lack adequate moisture resistance, which affects their reliability.

Method used

A semiconductor light emitting device with a laminated structure of a substrate, base layer, and protective layers, where the protective layers are made of oxide and nitride dielectric materials with decreasing thicknesses, and a method for manufacturing this device that includes forming electrodes and protective layers with specific openings and using a laser to separate elements, ensuring the outer peripheral region is cut without cracks.

Benefits of technology

The device achieves improved moisture resistance and reliability by preventing cracks during the cutting process, allowing it to be used without a package and enhancing its sealing performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024147982000001_ABST
    Figure 2024147982000001_ABST
Patent Text Reader

Abstract

To improve the reliability of a semiconductor light-emitting element.SOLUTION: A semiconductor light-emitting element 10 includes a substrate 20 having a first thickness t1, a base layer 22 having a second thickness t2 that is smaller than the first thickness t1, an n-type semiconductor layer 24 provided in an internal region W2 that is different from an outer peripheral region W1 on the base layer 22, an active layer 26, a p-type semiconductor layer 28, an n-side electrode 30, a p-side electrode 32, a first protection layer 34 covering the n-side electrode 30 and the p-side electrode 32, covering the n-type semiconductor layer 24, the active layer 26, and the p-type semiconductor layer 28, being in contact with the base layer 22 in the outer peripheral region W1, and having a third thickness t3 that is smaller than the second thickness t2 in the outer peripheral region W1, a second protection layer 36 covering the first protection layer 34, being in contact with the first protection layer 34 in the outer peripheral region W1, and having a fourth thickness t4 that is smaller than the third thickness t3 in the outer peripheral region W1, an n-side pad electrode 38, and a p-side pad electrode 40.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a semiconductor light-emitting device and a method for manufacturing the same. [Background technology]

[0002] The semiconductor light emitting device has an n-type semiconductor layer, an active layer, and a p-type semiconductor layer stacked on a substrate, an n-side electrode is provided on the n-type semiconductor layer, and a p-side electrode is provided on the p-type semiconductor layer. 2 , Al 2 O 3 A covering layer made of a dielectric material such as SiN is provided (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2020-113741 A Summary of the Invention [Problem to be solved by the invention]

[0004] In order to further improve the reliability of the semiconductor light emitting device, it is preferable to provide a protective layer having superior moisture resistance.

[0005] The present invention has been made in view of the above problems, and has an object to provide a technique for improving the reliability of semiconductor light-emitting devices. [Means for solving the problem]

[0006] A semiconductor light-emitting element according to one embodiment of the present invention includes a substrate having a first thickness, a base layer provided on the substrate and having a second thickness smaller than the first thickness, an n-type semiconductor layer provided in a region on the base layer different from a peripheral region and having a first upper surface and a second upper surface, an active layer provided on the first upper surface of the n-type semiconductor layer, a p-type semiconductor layer provided on the active layer, an n-side electrode provided on the second upper surface of the n-type semiconductor layer, a p-side electrode provided on the p-type semiconductor layer, a first n-side opening provided on the n-side electrode, a first p-side opening provided on the p-side electrode, the n-side electrode being covered at a location different from the first n-side opening, the p-side electrode being covered at a location different from the first p-side opening, and the n-type semiconductor layer having a first upper surface and a second upper surface. a first protective layer covering the body layer, the active layer and the p-type semiconductor layer and in contact with the base layer in the peripheral region, made of an oxide dielectric material and having a third thickness in the peripheral region that is smaller than the second thickness; a second protective layer having a second n-side opening provided on the n-side electrode and a second p-side opening provided on the p-side electrode, covering the first protective layer at a location different from the second n-side opening and the second p-side opening, in contact with the first protective layer in the peripheral region, made of a nitride dielectric material and having a fourth thickness in the peripheral region that is smaller than the third thickness; an n-side pad electrode connected to the n-side electrode at the second n-side opening; and a p-side pad electrode connected to the p-side electrode at the second p-side opening.

[0007] Another aspect of the present invention is a method for manufacturing a semiconductor light-emitting device, the method including the steps of forming a base layer having a second thickness smaller than the first thickness on a substrate having a first thickness, sequentially forming an n-type semiconductor layer, an active layer, and a p-type semiconductor layer on the base layer, removing the active layer and the p-type semiconductor layer in a partial region to expose an upper surface of the n-type semiconductor layer, forming an n-side electrode on the upper surface of the n-type semiconductor layer, forming a p-side electrode on the p-type semiconductor layer, removing the n-type semiconductor layer in an element isolation region to expose an upper surface of the base layer, forming a first protective layer that covers the n-side electrode, the p-side electrode, the n-type semiconductor layer, the active layer, and the p-type semiconductor layer, is in contact with an upper surface of the base layer in the element isolation region, is made of an oxide dielectric material, and has a third thickness smaller than the second thickness, removing the first protective layer on the n-side electrode to form a first n-side opening, and removing the first protective layer on the p-side electrode to expose an upper surface of the base layer. forming a second protective layer covering the first protective layer, covering the n-side electrode in the first n-side opening, covering the p-side electrode in the first p-side opening, in contact with the first protective layer in the element isolation region, made of a nitride dielectric material, and having a fourth thickness smaller than the third thickness; removing the second protective layer over the n-side electrode to form a second n-side opening; removing the second protective layer over the p-side electrode to form a second p-side opening; forming an n-side pad electrode connecting to the n-side electrode in the second n-side opening; forming a p-side pad electrode connecting to the p-side electrode in the second p-side opening; irradiating a laser into the substrate in the element isolation region to form a modified portion; and pressing a blade against the second protective layer in the element isolation region to cut the second protective layer, the first protective layer, the base layer, and the substrate. Effect of the Invention

[0008] According to the present invention, the reliability of the semiconductor light emitting element can be improved. [Brief description of the drawings]

[0009] [Figure 1] 1 is a cross-sectional view illustrating a schematic configuration of a semiconductor light emitting device according to an embodiment. [Diagram 2]3A to 3C are diagrams illustrating a manufacturing process of the semiconductor light emitting device according to the embodiment. [Diagram 3] 3A to 3C are diagrams illustrating a manufacturing process of the semiconductor light emitting device according to the embodiment. [Figure 4] 3A to 3C are diagrams illustrating a manufacturing process of the semiconductor light emitting device according to the embodiment. [Diagram 5] 3A to 3C are diagrams illustrating a manufacturing process of the semiconductor light emitting device according to the embodiment. [Figure 6] 3A to 3C are diagrams illustrating a manufacturing process of the semiconductor light emitting device according to the embodiment. [Figure 7] 3A to 3C are diagrams illustrating a manufacturing process of the semiconductor light emitting device according to the embodiment. [Figure 8] 3A to 3C are diagrams illustrating a manufacturing process of the semiconductor light emitting device according to the embodiment. [Figure 9] 3A to 3C are diagrams illustrating a manufacturing process of the semiconductor light emitting device according to the embodiment. [Figure 10] 3A to 3C are diagrams illustrating a manufacturing process of the semiconductor light emitting device according to the embodiment. [Figure 11] 3A to 3C are diagrams illustrating a manufacturing process of the semiconductor light emitting device according to the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, the embodiments of the present invention will be described in detail with reference to the drawings. In the description, the same elements are given the same reference numerals, and duplicated descriptions will be omitted as appropriate. In addition, in order to facilitate understanding of the description, the dimensional ratios of the components in each drawing do not necessarily match the dimensional ratios of the actual light-emitting element.

[0011] The semiconductor light-emitting device according to this embodiment is configured to emit "deep ultraviolet light" with a central wavelength λ of about 360 nm or less, and is a so-called DUV-LED (Deep UltraViolet-Light Emitting Diode) chip. In order to output deep ultraviolet light of such a wavelength, an aluminum gallium nitride (AlGaN)-based semiconductor material with a bandgap of about 3.4 eV or more is used. In this embodiment, in particular, the case of emitting deep ultraviolet light with a central wavelength λ of about 240 nm to 320 nm is shown.

[0012] In this specification, the "AlGaN-based semiconductor material" refers to a semiconductor material containing at least aluminum nitride (AlN) and gallium nitride (GaN), and includes semiconductor materials containing other materials such as indium nitride (InN). Therefore, the "AlGaN-based semiconductor material" referred to in this specification can be represented by the composition of In 1-x-y Al x Ga y N (0 < x + y ≤ 1, 0 < x < 1, 0 < y < 1), and includes AlGaN or InAlGaN. The "AlGaN-based semiconductor material" in this specification has, for example, a molar fraction of each of AlN and GaN of 1% or more, preferably 5% or more, 10% or more, or 20% or more.

[0013] In addition, in order to distinguish materials that do not contain AlN, there is sometimes referred to as a "GaN-based semiconductor material". The "GaN-based semiconductor material" includes GaN and InGaN. Similarly, in order to distinguish materials that do not contain GaN, there is sometimes referred to as an "AlN-based semiconductor material". The "AlN-based semiconductor material" includes AlN and InAlN.

[0014] FIG. 1 is a cross-sectional view schematically showing the configuration of a semiconductor light-emitting device 10 according to an embodiment. The semiconductor light-emitting device 10 includes a substrate 20, a base layer 22, an n-type semiconductor layer 24, an active layer 26, a p-type semiconductor layer 28, an n-side electrode 30, a p-side electrode 32, a first protective layer 34, a second protective layer 36, an n-side pad electrode 38, and a p-side pad electrode 40.

[0015] 1, the direction indicated by arrow A may be referred to as the "up-down direction" or "thickness direction." Furthermore, when viewed from the substrate 20, the direction away from the substrate 20 may be referred to as the upper side, and the direction toward the substrate 20 may be referred to as the lower side.

[0016] The substrate 20 is made of a material that is transparent to the deep ultraviolet light emitted by the semiconductor light emitting element 10. The substrate 20 is made of an oxide dielectric material, for example, sapphire (Al 2 O 3 The substrate 20 has a first thickness t1 that is 50 μm or more, for example, not less than 100 μm and not more than 500 μm.

[0017] The base layer 22 is provided on the substrate 20. The base layer 22 is made of a nitride material. The base layer 22 is made of, for example, undoped AlN, and is, for example, a high temperature grown AlN (HT-AlN) layer. The second thickness t2 of the base layer 22 is smaller than the first thickness t1, and is, for example, half or less of the first thickness t1. The second thickness t2 is 1 μm or more and 3 μm or less, for example, 1.5 μm or more and 2.5 μm or less, and is, for example, about 2 μm.

[0018] The n-type semiconductor layer 24 is provided on the base layer 22. The n-type semiconductor layer 24 is provided in the inner region W2 excluding the peripheral region W1 on the base layer 22. The n-type semiconductor layer 24 is made of an n-type AlGaN-based semiconductor material, and is doped with, for example, Si as an n-type impurity. The n-type semiconductor layer 24 is, for example, an n-type AlGaN layer. The AlN mole fraction of the n-type semiconductor layer 24 is 25% or more, 40% or more, 50% or more, or 60% or more. The AlN mole fraction of the n-type semiconductor layer 24 is 80% or less, or 70% or less. The thickness of the n-type semiconductor layer 24 is 1 μm or more and 3 μm or less, for example, 1.5 μm or more and 2.5 μm or less, for example, about 2 μm. The n-type semiconductor layer 24 has a first upper surface 24a and a second upper surface 24b.

[0019] The active layer 26 is provided on the first upper surface 24a of the n-type semiconductor layer 24. The active layer 26 is made of an AlGaN-based semiconductor material and is sandwiched between the n-type semiconductor layer 24 and the p-type semiconductor layer 28 to form a double heterostructure. The active layer 26 has, for example, a single-layer or multi-layer quantum well structure, and includes a barrier layer made of an undoped AlGaN-based semiconductor material and a well layer made of an undoped AlGaN-based semiconductor material. The active layer 26 includes, for example, a first barrier layer in contact with the n-type semiconductor layer 24 and a first well layer provided on the first barrier layer. One or more pairs of a barrier layer and a well layer may be additionally provided between the first well layer and the p-type semiconductor layer 28. Each of the barrier layer and the well layer has a thickness of 1 nm or more and 20 nm or less, for example, a thickness of 2 nm or more and 10 nm or less.

[0020] An electron blocking layer may be further provided between the active layer 26 and the p-type semiconductor layer 28. The electron blocking layer is composed of an undoped or p-type AlGaN-based semiconductor material. The AlN mole fraction of the electron blocking layer is 40% or more, 50% or more, 60% or more, 70% or more, or 80% or more. The electron blocking layer may be an AlN layer. The thickness of the electron blocking layer is 1 nm or more and 10 nm or less, for example, 2 nm or more and 5 nm or less.

[0021] The p-type semiconductor layer 28 is formed on the active layer 26. The p-type semiconductor layer 28 is a p-type AlGaN-based semiconductor material layer or a p-type GaN-based semiconductor material layer, for example, an AlGaN layer or a GaN layer doped with magnesium (Mg) as a p-type impurity. The p-type semiconductor layer 28 has a thickness of, for example, 20 nm or more and 400 nm or less.

[0022] The p-type semiconductor layer 28 may be composed of multiple layers. The p-type semiconductor layer 28 may have, for example, a p-type cladding layer and a p-type contact layer. The p-type cladding layer is in contact with the active layer 26 or the electron blocking layer. The AlN mole fraction of the p-type cladding layer is 25% or more, for example, 40% or more, 50% or more, 60% or more, 70% or more, or 80% or more. The thickness of the p-type cladding layer is 10 nm or more and 100 nm or less, for example, 15 nm or more and 70 nm or less. The p-type contact layer is in contact with the p-side electrode 32. The AlN mole fraction of the p-type contact layer is 20% or less, for example, 10% or less, 5% or less, or 0%. The thickness of the p-type contact layer is 5 nm or more and 30 nm or less, for example, 10 nm or more and 20 nm or less.

[0023] The n-side electrode 30 is provided on the second upper surface 24b of the n-type semiconductor layer 24. The n-side electrode 30 includes an n-side contact electrode 42 and an n-side current diffusion layer 44. The n-side contact electrode 42 has, for example, a layered structure of Ti / Al / Ti / TiN. The n-side current diffusion layer 44 covers the upper surface and side surface of the n-side contact electrode 42. The n-side current diffusion layer 44 has, for example, a layered structure of Ti / TiN / Ti / Rh / TiN / Ti / Au in which a Ti layer, a first TiN layer, a Ti layer, a Rh layer, a second TiN layer, a Ti layer, and an Au layer are layered in this order. The n-side current diffusion layer 44 may have a plurality of Ti layers and a plurality of Rh layers alternately stacked between the first TiN layer and the second TiN layer.

[0024] The p-side electrode 32 is provided on the p-type semiconductor layer 28. The p-type semiconductor layer 28 includes a p-side contact electrode 46 and a p-side current diffusion layer 48. The p-side contact electrode 46 includes, for example, an Rh layer. The p-side contact electrode 46 may be composed of only an Rh layer. The p-side contact electrode 46 is made of tin oxide (SnO 2The p-side contact electrode 46 may be made of a transparent conductive oxide (TCO) such as TiN, zinc oxide (ZnO), or indium tin oxide (ITO). The p-side contact electrode 46 may have a Ni / Au laminated structure. The p-side current spreading layer 48 covers the upper surface and side surface of the p-side contact electrode 46. The p-side current spreading layer 48 has a Ti / TiN / Ti / Rh / TiN / Ti / Au laminated structure in which a Ti layer, a first TiN layer, a Ti layer, a Rh layer, a second TiN layer, a Ti layer, and an Au layer are laminated in this order. The p-side current spreading layer 48 may have a plurality of Ti layers and a plurality of Rh layers alternately laminated between the first TiN layer and the second TiN layer.

[0025] The first protective layer 34 is provided so as to cover the entire upper portion of the element. The first protective layer 34 covers the n-type semiconductor layer 24, the active layer 26, the p-type semiconductor layer 28, the n-side electrode 30, and the p-side electrode 32. The first protective layer 34 contacts the upper surface 22a of the base layer 22 in the peripheral region W1 and covers the upper surface 22a of the base layer 22. The first protective layer 34 covers, for example, the entire upper surface 22a of the base layer 22 in the peripheral region W1. The first protective layer 34 has a first n-side opening 34n provided on the n-side electrode 30 and a first p-side opening 34p provided on the p-side electrode 32. The first protective layer 34 covers the n-side electrode 30 at a location different from the first n-side opening 34n, and covers the p-side electrode 32 at a location different from the first p-side opening 34p. The first protective layer 34 is made of silicon oxide (SiO 2 ), aluminum oxide (Al 2 O 3 ), hafnium oxide (HfO 2 The first protective layer 34 is preferably made of an oxide dielectric material such as SiO 2 The third thickness t3 of the first protective layer 34 is smaller than the second thickness t2, for example, half or less of the second thickness t2. The third thickness t3 is 0.5 μm or more and 1.5 μm or less, for example, 0.7 μm or more and 1.2 μm or less, for example, 0.8 μm or more and 1 μm or less.

[0026] The second protective layer 36 is provided so as to cover the entire upper portion of the element. The second protective layer 36 is provided so as to cover the entire surface of the first protective layer 34. The second protective layer 36 has a second n-side opening 36n provided on the n-side electrode 30 and a second p-side opening 36p provided on the p-side electrode 32. The second protective layer 36 covers the first protective layer 34 at a location different from the second n-side opening 36n and the second p-side opening 36p. The second protective layer 36 covers the inner peripheral surface 34a of the first protective layer 34 that defines the first n-side opening 34n. The second protective layer 36 covers the inner peripheral surface 34b of the first protective layer 34 that defines the first p-side opening 34p. The second protective layer 36 contacts the first protective layer 34 in the outer peripheral region W1 and overlaps the first protective layer 34. The second protective layer 36 does not contact the base layer 22. The second protective layer 36 is made of a nitride dielectric material such as silicon nitride (SiN). The second protective layer 36 has a fourth thickness t4 which is smaller than the third thickness t3, for example, half or less of the third thickness t3. The fourth thickness t4 is 0.1 μm or more and 0.4 μm or less, for example, 0.15 μm or more and 0.3 μm or less, for example, about 0.2 μm.

[0027] The n-side pad electrode 38 is connected to the n-side electrode 30 at the second n-side opening 36n. The n-side pad electrode 38 is provided so as to close the second n-side opening 36n and to overlap the second protective layer 36. The p-side pad electrode 40 is connected to the p-side electrode 32 at the second p-side opening 36p. The p-side pad electrode 40 is provided so as to close the second p-side opening 36p and to overlap the second protective layer 36. The n-side pad electrode 38 and the p-side pad electrode 40 include, for example, a stacked structure of Ni / Au, Ti / Au, or Ti / Pt / Au. The thickness of each of the n-side pad electrode 38 and the p-side pad electrode 40 is 0.1 μm or more, for example, 0.2 μm or more and 2 μm or less.

[0028] Next, a method for manufacturing the semiconductor light emitting device 10 according to the embodiment will be described. Figures 2 to 11 show schematic diagrams of the manufacturing process of the semiconductor light emitting device 10 according to the embodiment. First, in Figure 2, a base layer 22 is formed on a substrate 20. Next, an n-type semiconductor layer 24, an active layer 26, and a p-type semiconductor layer 28 are formed in this order on the base layer 22. The base layer 22, the n-type semiconductor layer 24, the active layer 26, and the p-type semiconductor layer 28 can be formed using a well-known epitaxial growth method such as a metal organic vapor phase epitaxy (MOVPE) method or a molecular beam epitaxy (MBE) method.

[0029] Next, as shown in FIG. 3, for example, an etching mask is used to remove the p-type semiconductor layer 28 and the active layer 26 in a partial region W3 by dry etching or the like, thereby exposing the second upper surface 24b of the n-type semiconductor layer 24.

[0030] Next, as shown in Fig. 4, for example, an n-side electrode 30 and a p-side electrode 32 are formed using a lift-off mask. An n-side contact electrode 42 is formed on the second upper surface 24b of the n-type semiconductor layer 24, and the n-side contact electrode 42 is annealed after the formation of the n-side contact electrode 42. A p-side contact electrode 46 is formed on the upper surface of the p-type semiconductor layer 28, and the p-side contact electrode 46 is annealed. Thereafter, an n-side current diffusion layer 44 that covers the n-side contact electrode 42 is formed, and a p-side current diffusion layer 48 that covers the p-side contact electrode 46 is formed. The n-side electrode 30 and the p-side electrode 32 can be formed by a vapor deposition method or a sputtering method.

[0031] Next, as shown in FIG. 5, for example, an etching mask is used to remove the n-type semiconductor layer 24 in the element isolation region W4 by dry etching or the like, thereby exposing the upper surface 22a of the base layer 22.

[0032] 6, a first protective layer 34 is formed so as to cover the entire upper surface of the element. The first protective layer 34 can be formed by using a plasma enhanced chemical vapor deposition (PECVD) method, an atomic layer deposition (ALD) method, a sputtering method, or the like.

[0033] Next, as shown in FIG. 7, the first protective layer 34 on the n-side electrode 30 and the p-side electrode 32 is removed by dry etching or the like using, for example, an etching mask to form a first n-side opening 34n and a first p-side opening 34p.

[0034] 8, a second protective layer 36 is formed so as to cover the entire upper portion of the element. The second protective layer 36 can be formed by using a method such as PECVD, ALD, or sputtering.

[0035] Next, as shown in FIG. 9, the second protective layer 36 on the n-side electrode 30 and the p-side electrode 32 is removed by dry etching or the like using, for example, an etching mask to form a second n-side opening 36n and a second p-side opening 36p.

[0036] 10, an n-side pad electrode 38 is formed to connect to the n-side electrode 30 in the second n-side opening 36n. Also, a p-side pad electrode 40 is formed to connect to the p-side electrode 32 in the second p-side opening 36p. The n-side pad electrode 38 and the p-side pad electrode 40 can be formed by a vapor deposition method or a sputtering method.

[0037] 11, in the element isolation region W4, the substrate 20 is irradiated with a laser to form a modified portion 50 inside the substrate 20. The modified portion 50 can be formed, for example, by irradiating the substrate 20 with a high-intensity short-pulse laser in a transparent wavelength band. The modified portion 50 may be formed, for example, at a plurality of locations inside the substrate 20 in the thickness direction.

[0038] Next, as shown in FIG. 11, a first protective sheet 52 is placed in contact with the n-side pad electrode 38 and the p-side pad electrode 40. The first protective sheet 52 is a resin sheet having adhesiveness and elasticity. A second protective sheet 54 is placed in contact with the substrate 20. The second protective sheet 54 is a resin sheet having no adhesiveness and no elasticity. The first protective sheet 52 includes an elastic layer made of a soft resin such as polyolefin or polyvinyl chloride, and an adhesive layer made of an acrylic or silicone resin adhesive. The second protective sheet 54 includes a resin layer made of a hard resin such as polyolefin or polyester. The thickness of the first protective sheet 52 and the second protective sheet 54 is not particularly limited, but is, for example, 0.2 mm or less, 0.15 mm or less, or 0.1 mm or less. With the first protective sheet 52 and the second protective sheet 54 in place, a blade 56 is pressed against the first protective sheet 52 in the thickness direction as indicated by an arrow 58 toward the element isolation region W4. When the blade 56 is pressed, the modified portion 50 becomes the starting point and the substrate 20, the base layer 22, the first protective layer 34, and the second protective layer 36 are broken in the element isolation region W4. This causes the substrate 20 to be divided into individual pieces, resulting in the semiconductor light emitting elements 10 shown in FIG.

[0039] According to this embodiment, the outer periphery of the semiconductor light-emitting element 10 is formed by a laminated structure of the substrate 20, the base layer 22, the first protective layer 34 and the second protective layer 36, thereby improving the sealing property of the light-emitting structure including the n-type semiconductor layer 24, the active layer 26 and the p-type semiconductor layer 28.

[0040] According to this embodiment, in the outer periphery region W1 (or the element isolation region W4), a structure is formed in which the substrate 20, the base layer 22, the first protective layer 34, and the second protective layer 36 are laminated in this order, and the thickness decreases in this order from the substrate 20 toward the second protective layer 36 (i.e., t1>t2>t3>t4). As a result, in the process of cutting the element isolation region W4 into individual pieces, it is possible to prevent cracks from occurring in the cut portions. In particular, it is possible to suppress the occurrence of cracks compared to the case where a thin layer is inserted in the middle of the laminated structure of the outer periphery region W1 (or the element isolation region W4). This makes it possible to form a highly reliable sealing structure.

[0041] According to this embodiment, the first protective sheet 52 having adhesiveness and elasticity is placed on the n-side pad electrode 38 and the p-side pad electrode 40, and the blade 56 is pressed against the first protective sheet 52 to cut the element isolation region W4, thereby preventing cracks from occurring in the cut portion. By using the first protective sheet 52 having adhesiveness and elasticity, it is possible to prevent the blade 56 from being displaced from the element isolation region W4 during cutting. This makes it possible to prevent the blade 56 from being pressed against a portion outside the element isolation region W4, which would damage the semiconductor layer and electrodes.

[0042] The semiconductor light emitting device 10 according to this embodiment has excellent moisture resistance and can be used without being sealed in a package. The semiconductor light emitting device 10 can be used while being energized with the second protective layer 36 exposed to the external environment, and can be used, for example, in the form of a chip on submount (CoS).

[0043] The present invention has been described above based on the embodiments. It will be understood by those skilled in the art that the present invention is not limited to the above-mentioned embodiments, that various design changes are possible, that various modifications are possible, and that such modifications are also within the scope of the present invention.

[0044] Several aspects of the present invention will now be described.

[0045] A first aspect of the present invention includes a substrate having a first thickness, a base layer provided on the substrate and having a second thickness smaller than the first thickness, an n-type semiconductor layer provided in a region on the base layer different from an outer periphery region and having a first upper surface and a second upper surface, an active layer provided on the first upper surface of the n-type semiconductor layer, a p-type semiconductor layer provided on the active layer, an n-side electrode provided on the second upper surface of the n-type semiconductor layer, a p-side electrode provided on the p-type semiconductor layer, a first n-side opening provided on the n-side electrode, a first p-side opening provided on the p-side electrode, covering the n-side electrode at a position different from the first n-side opening, covering the p-side electrode at a position different from the first p-side opening, and a gate insulating film formed on the n-type semiconductor layer, the active layer and a front surface of the n-type semiconductor layer, a first protective layer covering the p-type semiconductor layer, contacting the base layer in the peripheral region, made of an oxide dielectric material, and having a third thickness in the peripheral region that is smaller than the second thickness, a second protective layer having a second n-side opening provided on the n-side electrode, a second p-side opening provided on the p-side electrode, covering the first protective layer at a location different from the second n-side opening and the second p-side opening, contacting the first protective layer in the peripheral region, made of a nitride dielectric material, and having a fourth thickness in the peripheral region that is smaller than the third thickness, an n-side pad electrode connecting to the n-side electrode in the second n-side opening, and a p-side pad electrode connecting to the p-side electrode in the second p-side opening. According to the first aspect, the thicknesses of the substrate, base layer, first protective layer, and second protective layer stacked in the peripheral region become smaller in the stacking order, so that it is possible to prevent cracks from occurring in the cut portion in the process of cutting the peripheral region to separate the semiconductor light-emitting elements. This can improve the reliability of the sealing structure in which the substrate, the base layer, the first protective layer, and the second protective layer are laminated.

[0046] A second aspect of the present invention is the semiconductor light-emitting device according to the first aspect, in which the second thickness is half or less of the first thickness, the third thickness is half or less of the second thickness, and the fourth thickness is half or less of the third thickness. According to the second aspect, the thicknesses of the substrate, base layer, first protective layer, and second protective layer stacked in the peripheral region are half or less in the stacking order, so that it is possible to suitably prevent cracks from occurring at the cut portion in the process of cutting the peripheral region to separate the semiconductor light-emitting devices. This improves the reliability of the sealing structure in which the substrate, base layer, first protective layer, and second protective layer are stacked.

[0047] A third aspect of the present invention is the semiconductor light-emitting element according to the first or second aspect, wherein the second thickness is 1 μm or more and 3 μm or less, the third thickness is 0.5 μm or more and 1.5 μm or less, and the third thickness is 0.1 μm or more and 0.4 μm or less. According to the third aspect, by appropriately setting the thicknesses of the base layer, the first protective layer, and the second protective layer, it is possible to improve the reliability of the sealing structure in which the substrate, the base layer, the first protective layer, and the second protective layer are laminated.

[0048] A fourth aspect of the present invention includes a step of forming a base layer having a second thickness smaller than the first thickness on a substrate having a first thickness, a step of forming an n-type semiconductor layer, an active layer, and a p-type semiconductor layer in order on the base layer, a step of removing the active layer and the p-type semiconductor layer in a partial region to expose an upper surface of the n-type semiconductor layer, a step of forming an n-side electrode on the upper surface of the n-type semiconductor layer, a step of forming a p-side electrode on the p-type semiconductor layer, a step of removing the n-type semiconductor layer in an element isolation region to expose an upper surface of the base layer, a step of forming a first protective layer that covers the n-side electrode, the p-side electrode, the n-type semiconductor layer, the active layer, and the p-type semiconductor layer, is in contact with the upper surface of the base layer in the element isolation region, is made of an oxide dielectric material, and has a third thickness smaller than the second thickness, a step of removing the first protective layer on the n-side electrode to form a first n-side opening, and a step of removing the first protective layer on the p-side electrode to form a first p-side opening. forming a second protective layer covering the first protective layer, covering the n-side electrode in the first n-side opening, covering the p-side electrode in the first p-side opening, in contact with the first protective layer in the element isolation region, made of a nitride dielectric material, and having a fourth thickness smaller than the third thickness; removing the second protective layer over the n-side electrode to form a second n-side opening; removing the second protective layer over the p-side electrode to form a second p-side opening; forming an n-side pad electrode connected to the n-side electrode in the second n-side opening; forming a p-side pad electrode connected to the p-side electrode in the second p-side opening; irradiating a laser into the substrate in the element isolation region to form a modified portion; and pressing a blade against the second protective layer in the element isolation region to cut the second protective layer, the first protective layer, the base layer, and the substrate. According to the fourth aspect, the thicknesses of the substrate, base layer, first protective layer, and second protective layer stacked in the element isolation region become smaller in the stacking order, so that it is possible to prevent cracks from occurring at the cut portion in the process of cutting the element isolation region to separate the semiconductor light emitting devices, thereby improving the reliability of the sealing structure in which the substrate, base layer, first protective layer, and second protective layer are stacked.

[0049] A fifth aspect of the present invention is the method for manufacturing a semiconductor light-emitting element according to the fourth aspect, further comprising a step of placing an adhesive and stretchable sheet on the n-side pad electrode and the p-side pad electrode, and pressing the blade against the sheet in the cutting step. According to the fifth aspect, by using an adhesive and stretchable sheet, it is possible to prevent the blade from being misaligned with respect to the element isolation region during cutting. This makes it possible to prevent the blade from being pressed against a portion outside the element isolation region, which would otherwise damage the semiconductor layer or the electrodes. [Explanation of symbols]

[0050] 10...semiconductor light-emitting element, 20...substrate, 22...base layer, 22a...top surface, 24...n-type semiconductor layer, 24a...first top surface, 24b...second top surface, 26...active layer, 28...p-type semiconductor layer, 30...n-side electrode, 32...p-side electrode, 34...first protective layer, 34n...first n-side opening, 34p...first p-side opening, 36...second protective layer, 36n...second n-side opening, 36p...second p-side opening, 38...n-side pad electrode, 40...p-side pad electrode, 50...modified portion, 52...first protective sheet, 56...blade, W1...peripheral region, W2...inner region, W4...element isolation region.

Claims

1. a substrate having a first thickness; a base layer disposed on the substrate and having a second thickness less than the first thickness; an n-type semiconductor layer provided in an inner region on the base layer that is different from an outer periphery region, the n-type semiconductor layer having a first upper surface and a second upper surface; an active layer provided on the first upper surface of the n-type semiconductor layer; a p-type semiconductor layer provided on the active layer; an n-side electrode provided on the second upper surface of the n-type semiconductor layer; a p-side electrode provided on the p-type semiconductor layer; a first protective layer having a first n-side opening provided on the n-side electrode, a first p-side opening provided on the p-side electrode, covering the n-side electrode at a location different from the first n-side opening, covering the p-side electrode at a location different from the first p-side opening, covering the n-type semiconductor layer, the active layer and the p-type semiconductor layer, in contact with the base layer in the peripheral region, being made of an oxide dielectric material, and having a third thickness in the peripheral region that is smaller than the second thickness; a second protective layer having a second n-side opening provided on the n-side electrode and a second p-side opening provided on the p-side electrode, covering the first protective layer at a location different from the second n-side opening and the second p-side opening, in contact with the first protective layer in the peripheral region, being made of a nitride dielectric material, and having a fourth thickness in the peripheral region that is smaller than the third thickness; an n-side pad electrode connected to the n-side electrode in the second n-side opening; a p-side pad electrode connected to the p-side electrode in the second p-side opening.

2. the second thickness is less than or equal to half of the first thickness; the third thickness is less than or equal to half of the second thickness; The semiconductor light emitting element according to claim 1 , wherein the fourth thickness is equal to or less than half of the third thickness.

3. The second thickness is equal to or greater than 1 μm and equal to or less than 3 μm, the third thickness is equal to or greater than 0.5 μm and equal to or less than 1.5 μm; The semiconductor light emitting element according to claim 1 , wherein the third thickness is not less than 0.1 μm and not more than 0.4 μm.

4. forming a base layer on a substrate having a first thickness, the base layer having a second thickness less than the first thickness; forming an n-type semiconductor layer, an active layer, and a p-type semiconductor layer in this order on the base layer; removing the active layer and the p-type semiconductor layer in a partial region to expose an upper surface of the n-type semiconductor layer; forming an n-side electrode on the top surface of the n-type semiconductor layer; forming a p-side electrode on the p-type semiconductor layer; removing the n-type semiconductor layer in an element isolation region to expose an upper surface of the base layer; forming a first protective layer covering the n-side electrode, the p-side electrode, the n-type semiconductor layer, the active layer, and the p-type semiconductor layer, in contact with the upper surface of the base layer in the element isolation region, the first protective layer being made of an oxide dielectric material and having a third thickness smaller than the second thickness; removing the first protective layer on the n-side electrode to form a first n-side opening; removing the first protective layer on the p-side electrode to form a first p-side opening; forming a second protective layer covering the first protective layer, covering the n-side electrode at the first n-side opening, covering the p-side electrode at the first p-side opening, in contact with the first protective layer in the element isolation region, the second protective layer being made of a nitride dielectric material and having a fourth thickness less than the third thickness; removing the second protective layer on the n-side electrode to form a second n-side opening; removing the second protective layer on the p-side electrode to form a second p-side opening; forming an n-side pad electrode connected to the n-side electrode in the second n-side opening; forming a p-side pad electrode connected to the p-side electrode in the second p-side opening; forming a modified portion in the element isolation region by irradiating a laser into the substrate; and pressing a blade against the second protective layer from above in the element isolation region to cut the second protective layer, the first protective layer, the base layer, and the substrate.

5. a step of disposing an adhesive and stretchable sheet on the n-side pad electrode and the p-side pad electrode, The method for manufacturing a semiconductor light emitting device according to claim 4 , wherein in the cutting step, the blade is pressed against the sheet from above.

Citation Information

Patent Citations

  • Semiconductor light emitting device and image display device

    JP2004040124A

  • Infrared device

    JP2017228628A

  • Semiconductor light-emitting element and method of manufacturing semiconductor light-emitting element

    JP2022106572A

  • Semiconductor light emitting element and method for manufacturing semiconductor light emitting element

    JP2023020627A

  • Thin film light emitting diode

    US20100207145A1

Cited By

  • Semiconductor light emitting device and method for manufacturing semiconductor light emitting device

    JP2026013565A

  • Semiconductor light-emitting element and method for manufacturing semiconductor light-emitting element

    JP7684488B1