Paper material with post-processable printing layer and producing method thereof

A post-processable layer with a post-processing aid and OP varnish on paperboard addresses the need for special printing plates by ensuring adhesion and preventing smearing, enhancing productivity and reducing costs in decorative printing.

JP2024148153APending Publication Date: 2024-10-17RENGO CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024049480
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-04
Filing Date
2024-03-26
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Existing methods for decorative printing on paperboard require special printing plates for overprint varnish (OP varnish) due to the need to protect the printed surface, which leads to reduced productivity and increased costs, and the application of OP varnish can hinder post-processing such as hot melt adhesive application.

Method used

A post-processable layer containing a post-processing aid and OP varnish is applied to the paper material using a flexographic printing method, reducing the amount of OP varnish in specific areas to allow for full-surface coating without affecting post-processing, using a polyvalent cation salt and humectant to ensure adhesion and prevent smearing.

Benefits of technology

This approach enhances productivity by eliminating the need for special printing plates, reduces costs, and ensures suitable adhesion of hot melt adhesives and printing inks, preventing smearing during transportation and maintaining the printed surface integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024148153000003
    Figure 2024148153000003
  • Figure 2024148153000004
    Figure 2024148153000004
  • Figure 2024148153000005
    Figure 2024148153000005
Patent Text Reader

Abstract

To improve productivity without changing printing plates and ensure suitability for post-processing into cardboard by applying OP varnish to the entire surface by flexographic printing using only one type of flat printing plate without unevenness, without being affected by changes in decorative printing patterns.SOLUTION: A post-processable layer containing a post-processing aid and overprint varnish is provided on part of the surface of a paper material with a printed layer provided on part or the entire surface of the paper material, and an overprint varnish layer is provided on the surface of the paper material with a printed layer other than the post-processable layer, and the post-processing aid is a post-processable paper material with a printed layer containing a polyvalent cationic salt.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a post-processable printed paper material and a method for producing the same. [Background technology]

[0002] Some corrugated boards are manufactured using a method called "preprinting," in which the boards are pasted together using base paper, a type of paperboard that has already been beautifully printed. Conventionally, the method of printing on the base paper has mainly been flexographic printing using relief printing. In this flexographic printing method, flexible and elastic resin or rubber printing plates (flexographic plates) are used depending on the number of colors. Furthermore, white paperboard, which is a type of paperboard that has been decoratively printed using techniques such as gravure printing or offset printing, is used for paper containers for packaging cosmetics, processed foods, and the like.

[0003] In response to this, in recent years, inkjet printing, which does not require printing plates, has been attracting attention as a method for performing decorative printing on paperboard. In this printing method, not only is a pattern formed by directly ejecting ink from an inkjet head onto a substrate, but for example, Patent Document 1 discloses a method in offset printing in which a dampening liquid is ejected onto a transfer material by inkjet to form a pattern, ink is applied onto the pattern, and the resulting image is transferred and imaged onto a medium. These methods make decorative printing possible without plates.

[0004] In addition, cardboard boxes and paper containers manufactured using decoratively printed paperboard produced by the preprinting method are usually subjected to post-processing by the user, such as applying hot melt adhesive to make the box and seal it after the contents are placed inside, and printing bar codes indicating product numbers and lot numbers using inkjet printing methods.

[0005] However, the printed surface of cardboard and paper containers can be damaged or contaminated due to physical effects during processing and transportation. To prevent this, overprint varnish (hereinafter sometimes abbreviated as "OP varnish") is generally applied to the printed surface. For cardboard, this OP varnish is mainly a water-based varnish that has little impact on the human body and the environment, and is low in cost, while for paper containers, UV varnish that hardens when exposed to UV light may be used.

[0006] The flexographic printing method, which can ensure the necessary amount of coating, is used for this OP varnish application. This flexographic printing method has also been used for surface printing on cardboard and other materials using water-based flexographic inks, but applying OP varnish makes it possible to protect the printed surface.

[0007] However, when the OP varnish is applied to the entire surface, it is possible to easily apply the OP varnish without affecting the change in the printing pattern, but there is a risk of it interfering with the above-mentioned post-processing. Specifically, when the above-mentioned hot melt adhesive is applied on the OP varnish coating film, the penetration of the hot melt adhesive into the paperboard may be hindered, and sufficient adhesion may not be obtained. Furthermore, when printing is performed on the OP varnish coating film, regardless of the type of ink used, which may be water-based or oil-based, the penetration of the ink into the paperboard may be hindered in either case, sufficient ink adhesion may not be obtained, and the printed part may be soiled due to vibration, friction, etc. during transportation.

[0008] Therefore, in order to prevent the application of OP varnish from interfering with post-processing, in actual manufacturing sites, flexographic printing is carried out using a dedicated printing plate for OP varnish that has a printing pattern with recesses so that OP varnish is not applied to positions where post-processing will be performed. In this case, since the positions and sizes of the post-processing differ for each box, a printing plate for OP varnish of a type corresponding to the printing pattern is required. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] JP 2014-117951 A Summary of the Invention [Problem to be solved by the invention]

[0010] In such a situation, when the decorative printing pattern is changed, the printing plate for the OP varnish needs to be replaced, which reduces productivity. In addition, a dedicated printing plate for the OP varnish is required for each decorative printing pattern, which leads to high costs.

[0011] As a method for eliminating the need to change the printing plate for the OP varnish, it is possible to change the OP varnish to one that has less effect on post-processing and print it on the entire surface. In other words, it is possible to use an OP varnish with a composition that allows the hot melt adhesive and printing ink for post-processing to penetrate and adhere to the paperboard. The present inventors have conducted extensive research into this issue, but have not been able to find an OP varnish formula that can achieve both print surface protection and post-processing suitability.

[0012] Also, to eliminate the need for a dedicated printing plate for OP varnish, it is possible to apply the OP varnish using inkjet printing, except in areas where post-processing will be performed, as in decorative printing, but to ensure the protection of the printed surface, a fairly large amount of OP varnish must be applied. However, the OP varnish coating liquid has a high viscosity, and in order to prevent it from drying and clogging the inkjet head, it is necessary to reduce the solid content concentration or add a moisturizing agent, making it difficult to use existing inkjet heads, which have a limited discharge volume. One solution would be to add more inkjet heads, but as the coating volume increases, drying becomes insufficient, making it difficult to practically apply this inkjet printing method.

[0013] Therefore, this invention aims to apply OP varnish to the entire surface by flexographic printing using only one type of flat printing plate with no unevenness, without being affected by changes in the decorative printing pattern, thereby eliminating the need to change the printing plate for OP varnish, improving productivity, and reducing costs by eliminating the need for a dedicated printing plate for OP varnish.It also aims to ensure suitability for post-processing, for example by improving the adhesion of hot melt adhesives and inks, thereby maintaining adhesion and preventing the occurrence of smudges due to vibration or friction in the printed area. [Means for solving the problem]

[0014] The present invention solves the above-mentioned problems by providing a post-processable layer containing a post-processing aid and OP varnish on a part of the surface of a printed paper material, and the gist of the invention resides in the following [1] to [7].

[0015] [1] A post-processable layer containing a post-processing aid and overprint varnish is provided on part of the surface of a paper material with a printed layer, which has a printed layer provided on part or the entire surface of the paper material, and an overprint varnish layer is provided on the surface of the paper material with a printed layer other than the post-processable layer, and the post-processing aid is a post-processable paper material with a printed layer that contains a polyvalent cationic salt. [2] A post-processable paper material with a printed layer described in [1], in which the post-processable layer is provided on at least one surface selected from the surface of the printed layer and the surface of the paper material on which the printed layer is not provided. [3] The post-processable paper material with a printed layer according to [1] or [2], wherein the post-processing aid is the polyvalent cationic salt to which at least one agent selected from a thickener and a moisturizer has been added. [4] The paper material having a printed layer that can be post-processed according to [1] or [2], wherein the paper material is cardboard base paper, white paperboard or cardboard sheet.

[0016] [5] A method for producing a post-processable paper material with a printed layer, as described in [1] or [2], using a flexographic printing method, comprising supplying an aqueous solution of the post-processing aid to a portion of the flexographic plate corresponding to the portion where the post-processable layer is to be provided, transferring the overprint varnish supplied to an anilox roll to the flexographic plate, and transferring the post-processing aid and overprint varnish of the flexographic plate to the paper material with a printed layer. [6] The method for producing a post-processable printed paper material according to [5], wherein the post-processing aid is supplied to the flexographic plate by an inkjet method. [7] [4] A corrugated board with a post-processable printed layer, which is made by laminating the corrugated board base paper or white paperboard with a post-processable printed layer described in [7] [4] as a front liner, with a medium core and a back liner. Effect of the Invention

[0017] In the paper material with a post-processable printing layer according to the present invention, an aqueous solution of a post-processing aid is supplied to the flexographic plate corresponding to the portion where the post-processable layer is to be provided, i.e., the portion of the printing plate, and overprint varnish (OP varnish) is transferred and supplied to the upper surface of the flexographic plate via an anilox roll, so that the amount of OP varnish supplied to the portion where the post-processable layer is to be provided is reduced compared to the amount of OP varnish supplied to other portions. This reduction in the OP varnish disposed on the post-processable layer reduces the protective effect of the OP varnish on the printing layer. In other words, the reduction in the OP varnish can ensure post-processing suitability. For example, even if a hot melt adhesive is applied, the effect of suppressing the penetration of the OP varnish into the paper material is reduced, so that the adhesiveness of the hot melt adhesive can be ensured. In addition, even if post-printing is performed using a printing ink, whether the printing ink is water-based or oil-based, the effect of suppressing the penetration of the OP varnish into the paper material is reduced, so that the adhesion of the printing ink to the paper material is improved, and even if the printing portion is subjected to vibration, friction, etc. during transportation, it is possible to prevent the occurrence of smudges. As a result, flexographic printing plates for applying OP varnish do not require dedicated plates for each decorative printing pattern, so only a plate for full-surface coating is needed, which helps prevent productivity losses due to plate changes, etc. [Brief description of the drawings]

[0018] [Figure 1] (a) and (b) are cross-sectional views showing a post-processable printed paper material according to the present invention. [Diagram 2] (a) and (b) are cross-sectional views showing a post-processable layer according to the present invention. [Diagram 3] Schematic diagram showing the manufacturing process of the post-processable printed paper material (rolled paper material) according to the present invention. [Figure 4] Schematic diagram showing the manufacturing process of the post-processable printed paper material (flat paper material) according to the present invention. [Diagram 5] (a) and (b) are cross-sectional views showing a state in which a post-press processable layer is transferred to a paper material according to the present invention. [Figure 6] (a) and (b) are cross-sectional views showing a post-press processable layer on a paper material according to the present invention. [Figure 7] SEM photographs of the cross sections of the samples of Comparative Example 1 ((a)), Comparative Example 2 ((b)), and Example 6 ((c)) DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The present invention will be described below. The paper material with a printed layer that can be processed after the present invention is a paper material with a printed layer on the surface and an overprint varnish (OP varnish) layer and a post-processable layer on the printed layer side of the paper material. Examples of this paper material include regular liner, white liner, and other cardboard base paper, white cardboard, and cardboard sheets. 1(a) and 1(b), a printed layer 12 such as decorative printing is first provided on a part or the entire surface of a paper material 11a. This printed layer 12 can be printed by a printing method such as flexographic printing, gravure printing, or inkjet printing.

[0020] Then, a post-processable layer 13 is provided on a portion of the surface of the paper material 11a on which the printed layer 12 is provided, i.e., a portion of the outer surface of the printed layer 12 (Figure 1(a)), or a portion of the surface of the paper material 11a on the side on which the printed layer 12 is provided that does not have the printed layer 12 (Figure 1(b)). Also, an OP varnish layer 14 is provided on the printed layer side surface of the paper material 11a on which the printed layer 12 is provided, except for the portion on which the post-processable layer 13 is provided. Although not shown in the figure, the OP varnish layer 14 or the post-processable layer 13 may be provided on the surface of the paper material 11a on the side where the printed layer 12 is provided, straddling the part where the printed layer 12 is provided and the part of the surface of the paper material 11a where the printed layer 12 is not provided. Also, there may be a part on the surface of the paper material 11a where none of the printed layer 12, the OP varnish layer 14, or the post-processable layer 13 exists.

[0021] The post-processable layer 13 is a layer containing a post-processing aid and an OP varnish, and is either one layer, two layers, or a heterogeneous layer in which the two components are mixed at the interface. That is, it has any of the layer structures among a two-layer layer in which a post-processing aid layer 15 and an OP varnish layer 14 are laminated as shown in Fig. 2(a), a layer consisting of only one layer 15a in which the post-processing aid and the OP varnish are mixed and integrated as shown in Fig. 2(b), and a heterogeneous layer in which the post-processing aid and the OP varnish are mixed at the interface and the post-processing aid, the OP varnish, and a mixture thereof are present (not shown). As described later, a polyvalent cationic salt is used as the post-processing aid. In this case, when an anionic component such as acrylic acid is used as a component of the OP varnish, the charge of this anionic component and the polyvalent cation may be neutralized at the interface between the post-processing aid layer 15 and the OP varnish layer 14, causing self-aggregation and thickening. In this case, the post-processable layer 13 may have a two-layer structure in which the post-processing aid layer 15 is laminated on top of the OP varnish layer 14, as shown in FIG. 2(a).

[0022] <Method of manufacturing a paper material with a printed layer that can be post-processed> The post-processable paper material with a printed layer can be manufactured by the following method. Specifically, when the paper material is a roll of paper that is not cut into use units, it can be manufactured by the flexographic printing method shown in Figure 3, and when the paper material is cut into use units and in the form of a flat sheet, it can be manufactured by the flexographic printing method shown in Figure 4. Generally, in flexographic printing, printing plates made of flexible and elastic resin or rubber are used, but metal or ceramic plates can also be used depending on the coating conditions.

[0023] (In the case of the paper material 11a, the paper material is a roll of paper that has not been cut into usage units) When using a paper material 11a consisting of a roll of paper that is not cut into use units, a flexographic printing method as shown in FIG. 3 can be used to produce a post-processable printed paper material. First, printing is performed on the paper material 11a by a printing process, which is not shown in Fig. 3. Specifically, decorative printing or other printing is performed on a part or all of the surface of the paper material 11a in the printing target area to provide a printed layer 12, thereby producing a printed-layer-attached paper material 11b.

[0024] Next, a pre-post-processable layer 13 ′ which serves as a post-processable layer and a pre-OP varnish layer 14 ′ which serves as an OP varnish layer are provided at specific positions on the flexographic plate 24 . Specifically, the OP varnish is supplied from a chamber 21 such as a varnish liquid pan to an anilox roll 22 to form a pre-OP varnish layer 14'. On the other hand, an aqueous solution of a post-processing aid is supplied from a post-processing aid supplying section 23 to a specific position of the flexographic plate 24 to form a pre-post-processing aid layer 15'. When the agent disposed on the surface of the plate 24 is transferred to the printing layer 12 side of the printing layer-attached paper material 11b, this position corresponds to the area where the post-processable layer 13 will be provided. When the inkjet method is used as a method for supplying the aqueous solution of the post-processing aid to a specific position on the flexographic plate 24, the aqueous solution can be efficiently supplied to any position on the flexographic plate 24 without the need for a plate, thereby achieving the advantage of improved productivity. In this case, a commercially available product can be used as the inkjet head, with a widthwise resolution of 300 to 600 dpi and a droplet volume of about 3 to 25 pL.

[0025] Then, after supplying an aqueous solution of a post-processing aid to a specific position of the flexographic plate 24, the pre-OP varnish layer 14' supplied to the anilox roll 22 is transferred to the flexographic plate 24. At this time, when the pre-OP varnish layer 14' is transferred to the position where the pre-post-processing aid layer 15' is present, the pre-post-processing aid layer 15' and the pre-OP varnish layer 14' are laminated or mixed to form the pre-post-processable layer 13'. Next, the agent on the flexographic plate 24 is transferred and coated onto the printed layer-attached paper material 11b. As a result, as shown in Figures 5(a) and (b), the pre-OP varnish layer 14' and the pre-post-processable layer 13' are formed on the printed layer-attached paper material 11b. Then, the pre-OP varnish layer 14' and the pre-post-processable layer 13' permeate the printed layer-attached paper material 11b, and a drying process is performed as described later, so that the OP varnish layer 14 and the post-processable layer 13 are formed.

[0026] (In the case of flat-sheet paper material 11c cut into units of use) When a flat-plate-shaped paper material 11c cut into usage units is used, a paper material with a print layer that can be post-processed is manufactured using a flexographic printing method shown in FIG. First, printing is performed on the flat-plate-shaped paper material 11c cut into usage units by a printing process (not shown in Fig. 4). Specifically, decorative printing or other printing is performed on a part or all of the surface of the paper material 11c in the printing target area to provide a printing layer 12, thereby producing a paper material with a printing layer 11d. This printed-layer-attached paper material 11d can be moved by a conveyor 25 shown in Fig. 4. The means for moving the printed-layer-attached paper material 11d is not limited to the conveyor 25, and is not particularly limited as long as it is a facility that can transport the printed-layer-attached paper material 11d.

[0027] Next, a pre-post-processable layer 13' serving as a post-processable layer and a pre-OP varnish layer 14' serving as an OP varnish layer are provided at specific positions on the flexographic plate 24'. Specifically, the OP varnish is supplied from a chamber 21' such as a varnish liquid pan to an anilox roll 22' to form a pre-OP varnish layer 14'. Meanwhile, an aqueous solution of a post-processing aid is supplied from a post-processing aid supplying section 23' to a specific position on the flexographic plate 24' to form a pre-post-processing aid layer 15'. This specific position is a position that corresponds to the portion where the post-processable layer 13 will be provided when the agent disposed on the surface of the flexographic plate 24' is transferred to the printing layer 12 side of the printing layer-attached paper material 11d. When the inkjet method is used as a method for supplying the post-processing aid to a specific position on the flexographic plate 24', the aid can be efficiently supplied to any position on the flexographic plate 24' without the need for a plate, thereby achieving the advantage of improved productivity. In this case, as the ink jet head, a commercially available product can be used, as described above.

[0028] Then, after an aqueous solution of a post-processing aid is supplied to a specific position on the flexographic plate 24', the OP varnish layer 14' supplied to the anilox roll 22' is transferred to the flexographic plate 24'. At this time, when the pre-OP varnish layer 14' is transferred to the location of the pre-post-processing aid layer 15', the pre-post-processing aid layer 15' and the pre-OP varnish layer 14' are laminated or the two layers are mixed to form a pre-post-processable layer 13'. Next, the agent on the flexographic plate 24' is transferred and coated onto the printed layer-attached paper material 11d. As a result, the pre-OP varnish layer 14' and the pre-post-processable layer 13' are formed on the printed layer-attached paper material 11b, as shown in Figures 5(a) and (b). The pre-OP varnish layer 14' and the post-pre-processable layer 13' are then attached to the printed layer-attached paper material 11. b, and a drying step is carried out as described below, so that an OP varnish layer 14 and a post-processable layer 13 are formed.

[0029] (Paper material with a printed layer that can be post-processed) The pre-post-processable layer 13' formed on the post-processable printed layer-bearing paper material 11b manufactured by the above-mentioned method is formed on the surface layer of the printed layer 12 (Figure 5(a)) or the surface layer of the paper material 11a (Figure 5(b)). At this time, the layer formed on the flexographic plate 24, 24' containing only OP varnish (pre-OP varnish layer 14') and the layer containing both the aqueous solution of post-processing aid and OP varnish (pre-post-processable layer 13') will be of approximately uniform thickness, so that the amount of OP varnish in the surface portion of the printed layer-attached paper material 11b transferred and coated from the portion of the flexographic plate 24, 24' to which the aqueous solution of post-processing aid was supplied, i.e., the pre-post-processable layer 13', will be reduced by the amount of the aqueous solution of post-processing aid.

[0030] Although not shown in the figure, a post-press processable layer 13' may be provided on the surface of the paper material 11a on which the printed layer 12 is provided, spanning the portion on which the printed layer 12 is provided and the portion on the surface of the paper material 11a on which the printed layer 12 is not provided.

[0031] The pre-post-processable layer 13' is a layer containing an aqueous solution of a post-processing aid and an OP varnish, and is either one layer, two layers, or a non-uniform layer in which the two components are mixed at the interface. That is, it has any of the layer structures among a layer consisting of two layers, a pre-post-processing aid layer 15' and a pre-OP varnish layer 14', as shown in Fig. 6(a), a layer consisting of only one layer, layer 15b, in which the aqueous solution of the post-processing aid and the OP varnish are mixed and integrated, as shown in Fig. 6(b), and a non-uniform layer in which the post-processing aid and the OP varnish are mixed at the interface and the post-processing aid, the OP varnish, and a mixture thereof are present, although not shown. As a post-processing aid, a polyvalent cationic salt is used, as described later. In this case, when an anionic component such as acrylic acid is used as a component of the OP varnish, the charge of this anionic component and the polyvalent cation may be neutralized at the interface between the pre-post-processing aid layer 15' and the pre-OP varnish layer 14', causing self-aggregation and thickening. In this case, the pre-post-processing layer 13' may have a two-layer structure in which the pre-OP varnish layer 14' is laminated on top of the pre-post-processing aid layer 15', as shown in Figure 6(a).

[0032] The pre-processable layer 13' and pre-OP varnish layer 14' penetrate to a certain extent into the printed-layer-attached paper material 11b. In addition, a drying process is performed by any drying method such as hot air drying to evaporate the aqueous medium contained in the aqueous solution of the post-processing aid. As a result, a printed-layer-attached paper material that can be post-processed can be obtained, with the post-processable layer 13 and OP varnish layer 14 provided on the surface layer on the printed layer 12 side. Incidentally, when the paper material used is a corrugated board sheet (paper material 11c), it can be used as it is as a printed corrugated board. Also, when the paper material used is a base paper for corrugated board such as a general liner or a white liner, or a white paperboard (paper material 11a), the obtained paper material with a printed layer that can be processed afterwards can be used as a front or back liner, and by bonding it to a medium and another liner by any method, the printed corrugated board that can be processed afterwards according to the present invention can be manufactured and used.

[0033] The OP varnish that constitutes part of the pre-OP varnish layer 14' and the pre-post-processable layer 13', and the aqueous solution of the post-processing aid that constitutes part of the pre-post-processable layer 13' all penetrate into the printed layer-attached paper material 11b, 11d, but since the pre-post-processable layer 13' contains the post-processing aid, the amount of OP varnish remaining on the surface of the printed layer-attached paper material 11b, 11d is reduced, making it difficult for the OP varnish to form a film. Furthermore, the aqueous medium of the aqueous solution of the post-processing aid evaporates due to drying, and after drying, the aqueous solution of the post-processing aid becomes only the main agent, and the post-processing aid is not easily formed. The effect on the surface of the printed layer-attached paper materials 11b and 11d is smaller. For these reasons, a portion of the pre-OP varnish layer 14' penetrates into the printed layer-attached paper materials 11b and 11d, and the portion remaining on the surface of the printed layer-attached paper materials 11b and 11d becomes the OP varnish layer 14. Also, a portion of the pre-post-processable layer 13' penetrates into the printed layer-attached paper materials 11b and 11d, and the aqueous medium evaporates due to drying, and the portion remaining on the surface of the printed layer-attached paper materials 11b and 11d becomes the post-processable layer 13. As a result, as shown in Figures 1(a) and (b), the post-processable layer 13 becomes a layer with less OP varnish than the OP varnish layer 14.

[0034] [Overprint varnish (OP varnish)] The OP varnish layer 14 is a layer that covers the surface of the printed layer 12 to protect the printed layer 12 and prevent damage and contamination of the printed layer 12. Examples of the OP varnish material that constitutes the OP varnish layer 14 include acrylic resins, styrene-acrylic resins, and the like.

[0035] The coating amount of the OP varnish of the OP varnish layer 14 is 1 g / m2 in terms of solid content. 2 Above 2g / m 2 More than 1g / m is preferable. 2 If it is less than this, it becomes difficult to adequately protect the printed surface. 2 Less than 3g / m 2 Less than 4g / m is preferred. 2 More is acceptable, but not more than 4 g / m 2 This is enough to protect the printing surface, so 4g / m 2 The following will suffice: The amount of OP varnish applied does not include the amount of OP varnish applied to the post-preprocessable layer 13'.

[0036] [Post-processing aids] It is preferable that the post-processing aid be an agent that, by being present in advance at a specific position on the flexographic plate, reduces the amount of OP varnish transferred from the anilox roll to the flexographic plate, i.e., the amount of OP varnish in the pre-post-processable layer 13', and does not impair the adhesiveness of the hot melt adhesive or the adhesion of the printing ink without preventing a portion of the hot melt adhesive or printing ink used in post-processing from penetrating into the paper material. As the post-processing aid, a polyvalent cationic salt can be used. Examples of the polyvalent cationic salt include divalent or higher polyvalent metal salts. Examples of metal salts constituting the polyvalent metal salt include magnesium salts, calcium salts, and aluminum salts, with calcium salts being preferred. Examples of counter ions of the polyvalent metal salt include chloride ions, bromide ions, nitrate ions, hypophosphite ions, formate ions, acetate ions, and propionate ions. Specific examples of the polyvalent metal salt include calcium chloride, magnesium chloride, calcium nitrate, calcium hypophosphite, calcium bromide, magnesium bromide, calcium formate, calcium acetate, calcium propionate, and aluminum chloride.

[0037] The polyvalent cationic salt is dissolved in an aqueous medium to be used as an aqueous solution of the polyvalent cationic salt. Examples of the aqueous medium include water, organic solvents compatible with water such as methanol and ethanol, and mixtures thereof. The concentration of the aqueous solution of the polyvalent cationic salt is preferably 0.35 mol / L or more, more preferably 0.40 mol / L or more, and more preferably 0.45 mol / L or more. If the concentration is less than 0.35 mol / L, the pre-post-processing aid layer 15' is likely to move on the flexographic plate, and the boundary between the pre-post-processing layer 13' and the pre-OP varnish layer 14' may become unclear. On the other hand, the concentration of the aqueous solution of the polyvalent cationic salt is preferably 2.5 mol / L or less, and more preferably 1.5 mol / L or less. If the concentration is more than 2.5 mol / L, the salt is likely to precipitate during or after coating, which may impair the coating suitability or cause the formation of foreign matter.

[0038] In addition to the polyvalent cationic salt which is the main component, the post-processing auxiliary may contain, as necessary, a thickener, a moisturizing agent, a surfactant, a preservative, a pH adjuster, a water repellent, an anti-rust agent, and the like. The thickener is suitable for adjusting viscosity as a post-processing aid, and therefore has the characteristic that it can be added at a low concentration and has little effect even if it remains on the flexographic plate. Examples of the thickener include aqueous resins, etc. Examples of the aqueous resin include polyethylene glycol, polypropylene glycol, polyvinyl alcohol, polyvinylpyrrolidone, poly-N-vinylacetamide, sodium carboxymethylcellulose, and polyacrylamide.

[0039] The humectant has the advantage that the viscosity can be adjusted and that clogging of the nozzles of the inkjet head can be suppressed. Examples of the moisturizing agent include polyhydric alcohols, glycol ethers, etc. Examples of the polyhydric alcohols include glycerin, 1,4-butanediol, 1,5-heptanediol, etc. Examples of the glycol ethers include diethylene glycol monobutyl ether, etc. These thickeners and moisturizing agents may be used alone or in combination of two or more.

[0040] The amount of the thickener used is preferably 0.1% by weight or more, and preferably 0.5% by weight or more, in terms of the concentration of the aqueous solution of the polyvalent cationic salt. If it is less than 0.1% by weight, the thickening effect may not be fully exhibited. On the other hand, it is preferably 10.0% by weight or less, preferably 5.0% by weight or less, and more preferably 4.0% by weight or less. If it is more than 10.0% by weight, the viscosity may become high, making it difficult to eject the inkjet, and there is also a risk of salt precipitation.

[0041] The amount of the humectant used is preferably 1% by weight or more, more preferably 3% by weight or more, and more preferably 5% by weight or more, in terms of the concentration of the aqueous solution of the polyvalent cationic salt. If it is less than 3% by weight, the inkjet head tends to dry out and become clogged due to insufficient moisturizing effect. On the other hand, it is preferably 30% by weight or less, more preferably 25% by weight or less, and more preferably 20% by weight or less. If it is more than 30% by weight, the drying is slow, and there is a risk that the drying on the surface of the paper material will be insufficient.

[0042] The types of surfactants include acetylene-based, silicone-based, and mineral oil-based surfactants, and the amount added must be within a prescribed range for the surface tension of the post-processing aid, but is generally 0.05 to 1% by weight, and preferably 0.1 to 0.5% by weight. Use of the water repellent agent can enhance the effect of inhibiting the transfer of OP varnish.

[0043] The surface tension of the aqueous solution of the post-processing aid is preferably 20 mN / m or more and 40 mN / m or less at 25° C. If the surface tension of the post-processing aid is less than 20 mN / m at 25° C., it is difficult to eject the post-processing aid from the inkjet head, and if it is more than 40 mN / m, the flow inside the inkjet head deteriorates, resulting in unstable ejection from the inkjet head. The surface tension of the aqueous solution of the post-processing aid can be adjusted by adding a surfactant.

[0044] The content of the aqueous solution of the post-processing aid in the pre-post-processable layer 13' (the amount of the aqueous solution of the post-processing aid supplied to the flexographic plate 24, 24') is, in terms of solid content, 1 g / m of OP varnish contained in the pre-post-processable layer 13'. 2 The amount should be less than 0.5g / m 2 The amount of OP varnish contained in the post-processable layer 13' is preferably 1 g / m 2 If the amount is greater, the amount of OP varnish supplied to the pre-post-processable layer 13' will increase, resulting in too much OP varnish in the post-processable layer 13 that is applied, which may reduce the adhesion of the hot melt adhesive to the paper material and the adhesion of the printing ink to the paper material. The lower limit of the amount of OP varnish contained in the post-processing layer 13' is preferably as low as possible, and is preferably 0 g / m 2 In addition, when the above-mentioned method for producing a post-processable printed paper material is used, a small amount of OP varnish is applied.

[0045] The content of the aqueous solution of the post-processing aid in the pre-post-processable layer 13' can be adjusted by appropriately adjusting the amount of the post-processing aid supplied to a specific position of the flexographic plate 24, 24' and the amount of the OP varnish supplied to the anilox roll 22.

[0046] <Features of post-processable printed paper materials> The paper material with a printed layer that can be post-processed obtained by the above-mentioned method is protected by the OP varnish layer 14, which prevents damage or dirt from occurring even if forces such as vibration or friction are applied to the printed surface when used as a cardboard box or paper container, and protects the condition of the printed surface. Furthermore, even if a hot melt adhesive is adhered to the post-processable layer 13, the adhesive strength is sufficient, and if an attempt is made to peel off the adhesive portion, material destruction occurs on the surface of the cardboard, rather than peeling at the adhesive interface. Furthermore, when the post-processable layer 13 is printed or imprinted with water-based ink or oil-based ink, even if the printed or imprinted portion is rubbed after a specified time has passed, the portion is hardly soiled and the printed or imprinted state is maintained. EXAMPLES

[0047] The present invention will be described in more detail below using examples, but the present invention is not limited to the following examples. First, the raw materials and evaluation methods used in the present examples and comparative examples will be described.

[0048] <Ingredients> [Paper materials (cardboard base paper, white paperboard)] · White cardboard…Rengo Co., Ltd.: CRC230 White liner: Nippon Paper Industries Co., Ltd.: NCW210 General liner: Rengo Co., Ltd.: RKA210

[0049] [Paper materials (cardboard base paper, white paperboard) (with pre-coating)] The following precoat agent was applied to the above paper materials (cardboard base paper, white paperboard) at a concentration of 0.06 g / m using a tabletop automatic test coater (RK Print Coat Instruments: Flexiproof 100 / UV). 2 After coating (solid content), the material was dried in a dryer at 100° C. for 5 seconds to give paper material (cardboard base paper, white paperboard) (with precoat). [Pre-coat agent] To 94 parts by mass of water, 3 parts by mass of calcium chloride (reagent manufactured by Kishida Chemical Co., Ltd.) and 3 parts by mass of acrylic resin emulsion (Vinyblan 2687 manufactured by Nissin Chemical Industry Co., Ltd.) were added and stirred to obtain a precoat agent.

[0050] [Paper materials (corrugated cardboard sheets)] E-flute with white paperboard front liner (manufactured by Rengo Co., Ltd.)…Front liner (white paperboard: CRC230g) / Corner (KS120g) / Back liner (general liner: CN160g) E-flute with white outer liner (manufactured by Rengo Co., Ltd.)...Outer liner (white liner: CWA170g) / Centre (KS120g) / Inner liner (regular liner: CN160g) E-flute with standard outer liner (manufactured by Rengo Co., Ltd.)...Outer liner (standard liner: CN160g) / core (KS120g) / inner liner (white liner: CWA170g) The cardboard components mentioned above, "white cardboard: CRC230g," "medium core: KS120g," and "general liner: CN160g," are all manufactured by Rengo Co., Ltd., while "white liner: CWA170g" is manufactured by Nippon Paper Industries Co., Ltd.

[0051] [Post-processing aids - polyvalent cationic salts] Calcium chloride: Calcium chloride manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., hereafter referred to as "Ca chloride". Magnesium chloride: Magnesium chloride (anhydrous), manufactured by Kishida Chemical Co., Ltd.; hereinafter referred to as "Mg chloride". Calcium hypophosphite: Manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.: Calcium hypophosphite, hereafter referred to as "Ca hypophosphite". Calcium bromide: Calcium bromide manufactured by Kanto Chemical Co., Ltd., hereinafter referred to as "Ca bromide". Calcium formate: Calcium formate manufactured by Asahi Chemical Industry Co., Ltd., hereinafter referred to as "Ca formate".

[0052] (Sodium salt used in comparison example) Sodium chloride: Sodium chloride manufactured by Kishida Chemical Co., Ltd., hereinafter referred to as "Na chloride." Sodium propionate: Sodium propionate manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., hereinafter referred to as "Na propionate."

[0053] [Thickener] Polyethylene glycol: PEG20000 manufactured by Katayama Chemical Industry Co., Ltd., hereinafter referred to as "PEG." Polyvinyl alcohol: Fujifilm Wako Pure Chemical Industries, Ltd.: PVA1500, hereafter referred to as "PVA". Polyvinylpyrrolidone: PVP K-90 manufactured by Ashland Japan Co., Ltd., hereafter referred to as "PVP". Poly-N-vinylacetamide: GE191-104, manufactured by Showa Denko K.K., hereinafter referred to as "PNVA." Carboxymethylcellulose sodium salt: Daicel Miraize Co., Ltd.: CMC1330, hereinafter referred to as "CMC".

[0054] [Moisturizer] Glycerin...Kishida Chemical Co., Ltd. [Other additives] Surfactant: Olfine E1004 (acetylene-based surfactant) manufactured by Nissin Chemical Industry Co., Ltd.

[0055] [OP varnish] New FK MR OP Varnish N-2000…Manufactured by Sakata Inx Corporation, acrylic resin, hereafter referred to as “N-2000”. FK ACV G-902: Acrylic resin manufactured by Sakata Inx Corporation. Hereinafter referred to as "G-902". Hydric FCG OP Varnish: Styrene-acrylic resin manufactured by Dainichiseika Color & Chemicals Mfg. Co., Ltd., hereafter referred to as "FCG."

[0056] <Evaluation method> [Viscosity measurement of post-processing aids] For the post-processing aids obtained in each of the Examples and Comparative Examples, the shear viscosity (mPa·s) was measured at 25°C and a shear rate of 100 s-1 using a viscoelasticity measuring device (Anton Paar: Rheometer MCR102).

[0057] [Surface tension measurement of post-processing aids] For the post-processing aids obtained in each of the Examples and Comparative Examples, the surface tension (mN / m) was calculated by the Young-Laplace method from the contour shape and density difference of droplets formed at 25° C. using a fully automatic contact angle meter (DM-701, manufactured by Kyowa Interface Science Co., Ltd.). The liquid density of the post-processing aid was measured at 25° C. using a density meter (DMA5000, manufactured by Anton Paar).

[0058] [Suitable for water-based inks] The test specimens obtained in each of the Examples and Comparative Examples were attached to a cardboard sheet, and a barcode was printed at the position of a specific layer described below using an inkjet printer (Graphica Minikey MKHP4-401WQP, manufactured by Yamazaki Sangyo Co., Ltd.). After each set period of time (2 minutes, 5 minutes, and 10 minutes after printing), the printed area was rubbed with the cotton ball of a cotton swab, and the print quality and staining were judged according to the following criteria.

[0059] (1) Print quality: The state of the print was evaluated by comparing it with an area not coated with OP varnish. ◎: The color is equal to or greater than the original color, and the outline is clear. ○: The color is the same and the outline is clear. △: The color intensity and the sharpness of the outline are insufficient. ×: Ink bleeds on the printed surface.

[0060] (2) Soiling: The result of rubbing 10 minutes after printing was evaluated. ◎: Barcode is almost not stained. ○: The barcode is almost completely undamaged and the printed content is legible. △: The barcode is heavily soiled and the printed contents are difficult to read. ×: The barcode is so badly soiled that the printed content is completely unreadable.

[0061] [Oil-based ink suitability evaluation] As the oil-based black ink, 2 g of oil-based ink for inkjet printers (BLACK81K01, manufactured by Yamazaki Sangyo Co., Ltd.) was taken, soaked into a Kimtowel placed on a petri dish, and pressed against a rotary stamp (Techno Touch, manufactured by Sanby Co., Ltd.) to collect the black ink, which was then stamped at the specific layer positions described below on the test specimens obtained in each of the examples and comparative examples. After each set time (2 minutes, 5 minutes, and 10 minutes after stamping), the stamped area was rubbed with the cotton ball of a cotton swab to check for any staining and judged according to the following criteria.

[0062] (1) Print quality: The state of the print was evaluated in comparison with an area not coated with OP varnish. ○: The color is the same and the outline is clear. ×: The color intensity and the sharpness of the outline are insufficient.

[0063] (2) Soiling: The results of rubbing the stamp 10 minutes after it was stamped were evaluated. ○: Almost no staining on the stamped area. △: The imprinted part is very dirty and the imprinted contents are difficult to read. ×: The stamped area is severely soiled and the stamped content is completely unrecognizable.

[0064] [Hot melt adhesive suitability (HM suitability)] The adhesive properties of hot melt adhesives were evaluated assuming a situation in which vertical and horizontal flaps are glued together when assembling a cardboard box. The test specimens obtained in each of the Examples and Comparative Examples were cut into a size of 70 mm x 50 mm so that the running direction of the paper material during printing was the longitudinal direction, to obtain sheet A. From the cardboard sheets (B flute: RKLP120 [front liner] / S140 [core] / RKLP120 [back liner]: all base papers are manufactured by Rengo Co., Ltd.) prepared in advance, one piece each was cut out measuring 100 mm x 50 mm, with the lamination direction and width direction being the long directions, to obtain Sheet B. (Note that the lamination direction was the direction intersecting the corrugations of the cardboard sheet, and the width direction was the direction parallel to the corrugations of the cardboard sheet.)

[0065] Double-sided tape was attached to the back surface of sheet A and the front liner side of sheet B, which was cut with the lamination direction as the long side, and the edges were aligned and bonded to obtain sheet AB. Sheet B was cut out with the width direction as the longitudinal direction, and 0.1 g of an olefin-based hot melt adhesive (RH-115, manufactured by Rengo Co., Ltd.) melted at 150°C was applied to the back liner side of sheet B using a hot melt applicator (manufactured by Nordson) to obtain sheet B'. Approximately one second after the hot melt adhesive was applied, the position of the specific layer described below on the surface of sheet A of the AB sheets bonded to the cardboard sheet was aligned long-side up with the surface of sheet B' to which the hot melt adhesive had been applied, and a 1 kg weight was placed on top and pressed together for three seconds. The test specimens thus obtained were stored in an environment of 5°C for 24 hours, and then using a thermostatic tensile testing machine (manufactured by Tester Sangyo Co., Ltd.), the ends of each cardboard sheet of the test specimen were gripped with a chuck and T-shaped peeled off at a speed of 100 mm / min while still at 5°C. The material failure rate of the hot melt adhesive joint of Sheet A was measured and judged according to the following criteria. ○: Material destruction rate is 80% or more. △: Material destruction rate is 50% or more. ×: Material destruction rate is less than 50%.

[0066] [Evaluation of abrasion resistance of printed surface] In accordance with JIS P 8136, a Gakushin type friction tester (made by Nippon TMC Co., Ltd.: abrasion resistance tester for paper materials) was used. A test specimen was attached to a sliding table, and the same type of unprocessed paper material as the test specimen was attached to the friction section, which was placed so that it was in contact with the printed surface (excluding the position of the specific layer described below). A load of 500 gf was applied and the specimen was slid back and forth 500 times, after which the peeling of the color on the printed surface was visually judged according to the following criteria. ◯: No or only slight color peeling on the printed surface. ×: Color peeling of the printed surface is noticeable.

[0067] (Examples 1 to 20) [Manufacturing of post-processing aids] The polyvalent cation salt, additives and solvent shown in Table 1 were mixed in the amounts shown in Table 1 to produce a post-processing aid.

[0068] [Manufacturing of test specimens] Using the above-mentioned automatic tabletop test coater as a substitute for the flexographic printing apparatus shown in FIG. 3, a test specimen was produced in the following manner. First, an inkjet head (600 dpi) was used as the post-processing aid supplying section 23, and the post-processing aid having the aqueous resin shown in Table 1 was applied to a predetermined position of the roll of the flexographic plate 24 by an inkjet method at a rate of 0.4 g / m 2 (Solids) discharged.

[0069] In addition, the OP varnish shown in Table 1 was placed in the chamber 21 and transferred to the anilox roll 22 . Next, 3 seconds after the post-processing aid was discharged onto the flexographic plate 24, the OP varnish transferred to the anilox roll 22 was transferred to the flexographic plate 24, and then the paper material with the decorative design applied to its surface was attached to the impression roll and transferred to its printing layer side. In this way, the post-processing aid and OP varnish were applied to the predetermined positions on the printing layer side of the paper material with the decorative design applied to its surface. After coating, the coating was dried in a hot air dryer at 105°C for 5 seconds, and then stored in an environment with a temperature of 23°C and a humidity of 50% for 24 hours to obtain a test specimen. The layer in which the post-processing aid is disposed is referred to as a "specific layer." The above-mentioned evaluations were carried out using the obtained test specimens, and the results are shown in Table 1. In Table 1, the solid content of the post-processing aid refers to the solid content of the post-processing aid applied to a specific layer, and the solid content of the OP varnish refers to the solid content of the OP varnish applied to areas other than the specific layer. The solid content of the OP varnish in a specific layer is 0.3 g / m for white board. 2 , 0.7g / m for white liner and general liner 2 (with or without precoat).

[0070] (Examples 21 to 23) Test specimens were produced in the same manner as in Example 1, except that a flexographic printing device (manufactured by Tritec Corporation) shown in FIG. 4 was used instead of the desktop automatic test coater, and the amounts of post-processing aids and OP varnish shown in Table 1 were used for the paper materials shown in Table 1. The above-mentioned evaluations were carried out using the obtained test specimens. The results are shown in Table 1.

[0071] (Comparative Examples 1 and 15) Comparative Examples 1 and 15 were white paperboard and corrugated cardboard sheets that were not coated with post-processing aids or OP varnish.

[0072] (Comparative Examples 2 to 4 and 16) Test specimens were obtained in the same manner as in Examples 1 and 21, except that no post-processing aid was used and the OP varnish shown in Table 2 was used for coating. The results are shown in Table 2.

[0073] (Comparative Examples 5 to 14) Test specimens were obtained in the same manner as in Example 1, except that the paper material shown in Table 2 was coated with purified water instead of the post-processing aid and with the OP varnish shown in Table 2. The results are shown in Table 2.

[0074] In addition, for Example 6, Comparative Example 1, and Comparative Example 2, cross sections were prepared for the obtained samples using a CROSS SECTION POLISHER (manufactured by JEOL Ltd.), and the cross sections were observed under an electron microscope (JSM6010 PLUS / LA type scanning electron microscope, manufactured by JEOL Ltd., 5000x magnification). The SEM photographs are shown in Figures 7(a) to (c). The results are as follows: First, Comparative Example 1 in Figure 7(a) is a control sample that does not use the post-processing aid or OP varnish of the present invention. Since no OP varnish was used, this sample had good suitability for water-based inks, oil-based inks, and HM, but the abrasion resistance of the printed surface was poor. Next, Comparative Example 2 in Figure 7(b) is an example in which only OP varnish was used without using the post-processing aid of the present invention. In this case, it can be seen that the OP varnish forms a layer on the paper material. Therefore, the suitability for water-based ink, oil-based ink, and HM was poor, but the abrasion resistance of the printed surface was good. In contrast, Example 6 in Figure 7(c) is an example in which the post-processing aid and OP varnish of the present invention were used, in which no OP varnish was observed on the paper material, and the suitability for water-based inks, suitability for HM, and abrasion resistance of the printed surface were all good.

[0075] [Table 1]

[0076] [Table 2] [Explanation of symbols]

[0077] 11a, 11c paper material 11b, 11d Paper material with printing layer 12 printing layer 13 Post-processable layer 13' Pre-processable layer 14 OP varnish layer 14' Pre-OP varnish layer 15 Post-processing aid layer 15' Pre-processing aid layer 15a Layer where post-processing aid and OP varnish are mixed and integrated 15b Layer in which the aqueous solution of post-processing aid and OP varnish are mixed and integrated 21, 21' Chamber (varnish pan) 22, 22' Anilox Roll 23, 23' Post-processing auxiliary supply section 24, 24' flexo plate 25 Conveyor

Claims

1. A post-processable layer containing a post-processing aid and an overprint varnish is provided on a part of the surface of the paper material having a printed layer provided on a part or the entire surface of the paper material, An overprint varnish layer is provided on the surface of the printed layer-bearing paper material other than the post-processable layer, The post-processing aid is a post-processable printed paper material containing a polyvalent cationic salt.

2. The post-processable paper material with a printed layer according to claim 1, wherein the post-processable layer is provided on at least one surface selected from the surface of the printed layer and a surface of the paper material on which the printed layer is not provided.

3. 3. The post-processable paper material with a printed layer according to claim 1, wherein the post-processing aid is a polyvalent cationic salt to which at least one agent selected from the group consisting of a thickener and a moisturizer has been added.

4. 3. The post-processable printed paper material according to claim 1, wherein the paper material is a cardboard base paper, a white paperboard, or a cardboard sheet.

5. A method for producing a post-processable printed paper material according to claim 1 or 2, using a flexographic printing method, providing an aqueous solution of the post-processing aid to a portion of the flexographic plate corresponding to a portion where the post-processable layer is to be formed; The overprint varnish supplied to the anilox roll is transferred to the flexographic plate; A method for producing a post-processable paper material with a printed layer, comprising transferring the post-processing aid and overprint varnish of the flexographic plate to the paper material with a printed layer.

6. The method for producing a post-processable printed paper material according to claim 5, wherein the post-processing aid is supplied to the flexographic plate by an inkjet method.

7. 5. A post-processable printed corrugated board, comprising the post-processable printed corrugated board base paper or white paperboard as claimed in claim 4 as a front liner, laminated with a corrugating medium and a back liner.

Citation Information

Patent Citations

  • System and method for ink-based digital printing

    JP2014117951A