Molding mold, method for manufacturing resin molded product, and resin molded product
The molding die and method address residual stress and birefringence in resin molded products by positioning the resin gate on a non-design surface, enhancing optical properties and reducing warpage.
Patent Information
- Application Number
- JP2023061392
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-05
- Publication Date
- 2024-10-18
AI Technical Summary
Resin molded products, particularly optical products, suffer from residual stress-induced birefringence, which affects image formation and optical characteristics.
A molding die and method that incorporates a specific cavity design with a resin gate opening on a non-design surface, reducing residual stress and birefringence by allowing the resin gate to extend along a third molding surface, connected to first and second molding surfaces.
The solution effectively reduces residual stress and birefringence in resin molded products, improving optical properties and reducing warpage, with a demonstrated reduction in birefringence by about 30% compared to conventional methods.
Smart Images

Figure 2024148336000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a molding die, a method for manufacturing a resin molded product, and a resin molded product. [Background technology]
[0002] Glass has traditionally been used in optical products (transparent products) such as lenses, prisms, and display panels. In recent years, there has been a demand for such optical products to be lightweight. There has also been a demand for greater freedom in design. To meet these demands, the use of plastics (resins) has been considered.
[0003] Generally, injection molding is used as a manufacturing method for plastic products (Patent Document 1, Patent Document 2). Injection molding allows for the mass production of optical products with complex shapes in a short period of time by injecting heated and molten resin into a mold and then cooling it.
[0004] On the other hand, this injection molding has a problem that a phase difference occurs due to birefringence. Birefringence is induced by residual stress. When a phase difference occurs in an optical product, the image formation is disturbed, and the optical characteristics or visibility may be deteriorated. In order to solve such a problem, for example, development of a material or a mold that reduces birefringence is being promoted. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 10-027512 [Patent Document 2] Japanese Patent Application Publication No. 10-193397 Summary of the Invention [Problem to be solved by the invention]
[0006] Further reduction in birefringence (residual stress) is required for resin molded products such as optical products that use resin (plastic). The present disclosure has been made to solve such problems, and one object of the present disclosure is to provide a molding die that suppresses the occurrence of residual stress, another object of the present disclosure is to provide a method for producing a resin molded product that suppresses the occurrence of residual stress, and yet another object of the present disclosure is to provide such a resin molded product. [Means for solving the problem]
[0007] The molding die according to the present disclosure is a molding die including a first mold and a second mold in which one or more cavities including a cavity body for molding a resin molded product having a first molded surface, a second molded surface, and a third molded surface are formed, and the molding die includes a first molding surface, a second molding surface, a third molding surface, and a resin gate. The first molding surface is formed in the first mold and molds the first molded surface. The second molding surface is formed in the second mold arranged to face the first mold and molds the second molded surface. The third molding surface is formed to connect between the first molding surface and the second molding surface when the first mold and the second mold are in contact with each other, and molds the third molded surface. The resin gate feeds resin into the cavity body formed by the multiple molding surfaces including the first molding surface, the second molding surface, and the third molding surface when the first mold and the second mold are in contact with each other. The resin gate is formed so as to open to either the first or second molding surface which opposes each other when the first and second molds are in contact with each other, and to extend along the third molding surface.
[0008] The manufacturing method of a resin molded product according to the present disclosure is a manufacturing method of a resin molded product using a molding die in which a cavity body for molding a resin molded product having a first molded surface, a second molded surface, and a third molded surface is formed, and includes the following steps: A molding die having a first mold and a second mold is prepared. A cavity body of the molding die is filled with resin. A resin molded product molded by filling the cavity body is removed from the molding die. In the step of preparing a molding die, the following molding die is prepared. A first molding surface for molding the first molded surface is formed in the first mold. A second molding surface for molding the second molded surface is formed in the second mold. A third molding surface for molding the third molded surface is formed so as to connect between the first molding surface and the second molding surface when the first mold and the second mold are in contact with each other. With the first and second dies in contact with each other, a cavity body is formed by a plurality of molding surfaces including a first molding surface, a second molding surface, and a third molding surface that face each other. A resin gate is formed that opens on either the first molding surface or the second molding surface that face each other and that feeds resin into the cavity body so as to extend along the third molding surface. In the step of filling the cavity body with resin, the resin is filled into the cavity body from the resin gate in a manner that intersects with either the first molding surface or the second molding surface. In the step of removing the resin molded product from the molding die, a resin gate mark is left on either the first molded surface or the second molded surface of the resin molded product so as to extend along the third molded surface.
[0009] The resin molded product according to the present disclosure includes a first molded surface, a second molded surface, and a third molded surface. The second molded surface is positioned to face the first molded surface. The third molded surface connects the first molded surface and the second molded surface. A resin gate mark is left on either the first molded surface or the second molded surface so as to extend along the third molded surface. Effect of the Invention
[0010] According to the molding die of the present disclosure, the resin gate is formed so as to open to either the first molding surface or the second molding surface facing each other when the first mold and the second mold are in contact with each other, and to extend along the third molding surface, thereby reducing the residual stress in the resin molded product and reducing birefringence.
[0011] According to the method for producing a resin molded article according to the present disclosure, it is possible to reduce residual stress in a resin molded article, and to produce a resin molded article with reduced birefringence. Residual stress can be reduced.
[0012] According to the resin molded article according to the present disclosure, residual stress is reduced, and birefringence can be reduced. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a side view showing an example of an injection molding apparatus equipped with an injection mold according to each embodiment. [Diagram 2] FIG. 2 is a cross-sectional view showing an example of a structure of an injection molding die according to each embodiment. [Diagram 3] FIG. 1 is a first perspective view showing an example of a resin molded product molded by the injection mold according to each embodiment. [Figure 4] FIG. 2 is a second perspective view showing an example of a resin molded product molded by the injection mold according to each embodiment. [Diagram 5] FIG. 1 is an exploded perspective view showing an injection molding die according to a first embodiment. [Figure 6] 6 is a cross-sectional view taken along line VI-VI in FIG. 5 in the embodiment. [Figure 7] FIG. 4 is a cross-sectional view showing one step of a method for producing a resin molded body using an injection molding die in the embodiment. [Figure 8] 8 is a cross-sectional view showing a step performed after the step shown in FIG. 7 in the embodiment. [Figure 9]9 is a cross-sectional view showing a step performed after the step shown in FIG. 8 in the embodiment. [Figure 10] 10 is a cross-sectional view showing a step performed after the step shown in FIG. 9 in the embodiment. [Figure 11] FIG. 2 is a perspective view showing an example of a resin molded body manufactured using a mold for injection molding in the embodiment. [Figure 12] FIG. 4 is a partial cross-sectional view showing an injection molding die according to a comparative example. [Figure 13] FIG. 11 is a perspective view for explaining a problem with a resin molded body manufactured using an injection molding die according to a comparative example. [Figure 14] FIG. 2 is a perspective view for explaining the function and effect of a resin molded body manufactured using the injection molding die in the same embodiment. [Figure 15] FIG. 11 is a diagram showing evaluation results of retardation in the embodiment. [Figure 16] FIG. 11 is an exploded perspective view showing an injection molding die according to a second embodiment. [Figure 17] 17 is a cross-sectional view taken along line XVII-XVII in FIG. 16 in the embodiment. [Figure 18] FIG. 2 is a perspective view showing an example of a resin molded body manufactured using a mold for injection molding in the embodiment. [Figure 19] FIG. 11 is an exploded perspective view showing an injection molding die according to embodiment 3. [Figure 20] 20 is a cross-sectional view taken along line XX-XX in FIG. 19 in the embodiment. [Figure 21] FIG. 2 is a perspective view showing an example of a resin molded body manufactured using a mold for injection molding in the embodiment. [Figure 22] FIG. 11 is an exploded perspective view showing an injection molding die according to embodiment 4. [Figure 23] FIG. 13 is an exploded perspective view showing an injection molding die according to embodiment 5. [Figure 24] FIG. 24 is a cross-sectional view taken along line XXIV-XXIV in FIG. 23 in the embodiment. [Diagram 25] FIG. 13 is an exploded perspective view showing an injection molding die according to a sixth embodiment. [Figure 26] FIG. 2 is a perspective view showing an example of a resin molded body manufactured using a mold for injection molding in the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] First, an example of an injection molding apparatus equipped with an injection mold according to each embodiment will be described. As shown in Fig. 1, an injection molding apparatus 41 includes an injection mold 1 as a molding mold, a hopper 43, and a cylinder 45. The injection mold 1 includes a movable mold 3 as a first mold, and a fixed mold 19 as a second mold.
[0015] A resin material (not shown) is put into the hopper 43. In the cylinder 45, the put resin material is heated and melted. The melted resin material is injected from the cylinder 45 into the injection molding die 1 by a screw (not shown). The injected resin material is cooled by contacting the surface of the injection molding die 1. The resin material is held in the injection molding die 1 until cooling of the resin material is completed.
[0016] When the cooling of the resin material is completed, the injection mold 1 is opened. At this time, the movable mold 3 slides in a direction away from the fixed mold 19. The cooled and solidified resin material is taken out as a resin molded product. In this way, the molding of the resin material is completed.
[0017] Next, the injection molding die 1 will be described. As shown in Fig. 2, in the injection molding die 1, a cavity 29 is formed with a movable die 3 and a fixed die 5 in contact with each other. The cavity 29 includes a product molding section 30 as a cavity main body, an underwater gate section 33 as a communication passage section, and a runner section 31. In the fixed die 19, a cylindrical runner 27 for supplying resin to the runner section 31 is formed.
[0018] Resin supplied from the runner 27 to the runner section 31 flows through the diving gate section 33 and is sent from the resin gate 35 to the product molding section 30. The resin flows from the runner section 31 from above toward below in the direction of gravity to fill the product molding section 30. The movable mold 3 is provided with an ejector pin 18 that removes a molded body including a resin molded product molded in the cavity 29 from the movable mold 3. The specific structure of the injection molding die 1 will be described below in each embodiment.
[0019] Embodiment 1 An injection molding die 1 according to the first embodiment will be described. First, an example of a resin molded product molded by the injection molding die 1 will be described. As shown in Fig. 3 and Fig. 4, a resin molded product 51 is a type of optical component having a light transmitting portion 53 and a bezel 55. The bezel 55 is positioned so as to surround the periphery of the light transmitting portion 53.
[0020] The resin molded product 51 has a first molded surface 61, a second molded surface, and a third molded surface 65, each of which is molded by the injection molding die 1. The first molded surface 61 and the second molded surface 63 are positioned so as to face each other. The third molded surface 65 is positioned so as to connect between the first molded surface 61 and the second molded surface 63. The third molded surface 65 is positioned in the thickness direction of the resin molded product 51. A resin gate mark 57 corresponding to a resin gate provided in the injection molding die 1 is left on the first molded surface 61.
[0021] Next, an example of an injection molding die 1 for molding such a resin molded product 51 will be described. As shown in Figures 5 and 6, in the injection molding die 1, a cavity 29 is formed with a movable die 3 and a fixed die 19 in contact with each other. The cavity 29 includes a product molding portion 30 as a cavity main body, an underwater gate portion 33 as a communication passage portion, and a runner portion 31.
[0022] The movable side mold 3 is formed with a movable side first recess 7 as the first mold side first recess, a movable side second recess 13 as the first mold side second recess, and a movable side third recess 17 as the first mold side third recess. The movable side second recess 13 is formed deeper than each of the movable side first recess 7 and the movable side third recess 17. The fixed side mold 19 is formed with a fixed side convex portion 23 as a second mold side convex portion that faces the movable side second recess 13.
[0023] A first molding surface 9 for molding a first molded surface 61 of the resin molded product 51 is located on the bottom surface of the movable-side first recess 7. A third molding surface 11 (third molding surface 11a) for molding a third molded surface 65 of the resin molded product 51 is located on the side wall surface of the movable-side first recess 7. The fixed-side convex portion 23 includes a part (third molding surface 11b) of the third molding surface 11 for molding the third molded surface 65 of the resin molded product 51. A second molding surface 21 for molding a second molded surface 63 of the resin molded product 51 is located in the fixed-side mold 19.
[0024] When the movable-side mold 3 and the fixed-side mold 19 are in contact with each other, a cavity 29 including a product molding portion 30 as a cavity main body, a runner portion 31, and a submerged gate portion 33 as a communicating passage portion, and a resin gate 35 are formed. The product molding portion 30 is formed by the first molding surface 9 and the third molding surface 11a of the movable-side first recess 7, the third molding surface 11b of the fixed-side protrusion 23, and the second molding surface 21 of the fixed-side mold 19.
[0025] The movable-side second recess 13 and the fixed-side protrusion 23 face each other with a gap therebetween, so that a resin gate 35 is formed on the first molding surface of the product molding section 30. The resin gate 35 that opens on the first molding surface 9 opens from a first position P1 where the third molding surface 11b is located to a second position P2 that is more inward than the first position P1, and is formed so as to extend along the first position P1. The runner section 31 is formed by the movable-side third recess 17. The submerged gate section 33 communicates between the runner section 31 and the resin gate 35 in a manner that it submerges toward the first molding surface 9 with respect to the product molding section 30.
[0026] Next, an example of a method for manufacturing a resin molded product using the above-mentioned injection mold 1 will be described. As shown in FIG. 7, the movable mold 3 and the fixed mold 19 are opposed to each other, and the movable mold 3 is brought close to the fixed mold 19, and as shown in FIG. 8, the movable mold 3 and the fixed mold 19 are brought into contact with each other. Next, as shown in FIG. 9, resin 47 is supplied from the runner 27 to the runner section 31. The resin 47 supplied to the runner section 31 flows through the diving gate section 33 and reaches the resin gate 35. As shown in FIG. 10, the resin 47 that has reached the resin gate 35 flows downward through the product molding section 30, and the product molding section 30 is gradually filled with the resin 47.
[0027] After the resin 47 filled in the product molding portion 30 has been sufficiently cooled, the movable mold 3 slides in a direction away from the fixed mold 19. The ejector pin 18 removes the molded product including the resin molded product 51 filled in the product molding portion 30 from the injection mold 1. Then, the part of the resin that was located in the runner portion 31 and the part of the resin that was located in the submerged gate portion are removed. In this way, the resin molded product 51 is molded, as shown in FIG.
[0028] A resin gate mark 57 corresponding to the resin gate 35 is left on the first molded surface 61 of the resin molded product 51 by removing a portion of the resin that was located at the submerged gate portion 33, etc. The resin gate mark 57 has a width from a position where the third molded surface 65 is located (corresponding to the first position P1) to a position inside that position (corresponding to the second position P2) on the first molded surface 61, and is left in a band shape extending along the third molded surface 65.
[0029] Here, it is assumed that the design surface of the resin molded product 51 is molded by the second molding surface 21 of the fixed mold 19, and the non-design surface of the resin molded product 51 is molded by the first molding surface 9 of the movable mold 3. Then, the first molded surface 61 of the resin molded product 51 molded by the first molding surface 9 is molded as the non-design surface. The resin gate mark 57 is left on the first molded surface 61, which is the non-design surface.
[0030] In the above-described injection molding die 1, the resin gate 35 opens to the first molding surface 9, thereby making it possible to reduce the residual stress in the resin molded product 51. This will be explained in comparison with an injection molding die according to a comparative example.
[0031] As shown in FIG. 12, in the injection molding die 101 relating to the comparative example, when the movable side die 103 and the fixed side die 119 are in contact with each other, a product molding portion 130, a communicating passage portion 133, and a runner portion 131 are formed as a cavity 129.
[0032] The movable side mold 103 is formed with a movable side first recess 107, a movable side second recess 113, and a movable side third recess 117. The movable side first recess 107, the movable side second recess 113, and the movable side third recess 117 are formed to have the same depth. The fixed side mold 119 is formed with a fixed side protrusion 123 that faces the movable side second recess 113.
[0033] A first molding surface 109 for molding a first molded surface 161 of a resin molded product 151 (see FIG. 13) is located on the bottom surface of the movable-side first recess 107. A part (third molding surface 111a) of a third molding surface 111 for molding a third molded surface 165 of the resin molded product 151 is located on the side wall surface of the movable-side first recess 107. A part (third molding surface 111b) of the third molding surface 111 is located on the side wall surface of the fixed-side convex portion 123. A second molding surface 121 for molding a second molded surface 163 of the resin molded product 151 is located in the fixed-side mold 119.
[0034] When the movable mold 103 and the fixed mold 119 are in contact with each other, a product molding section 130, a runner section 131, and a communicating passage section 133 are formed. A resin gate 135 that sends out resin to the product molding section 130 opens to the third molding surface 111 of the product molding section 130. In the injection molding die 101 according to the comparative example, resin supplied from the runner 127 to the runner section 131 flows through the communicating passage section 133 and reaches the resin gate 135.
[0035] The resin that reaches the resin gate 135 flows into product molding section 130 along first molding surface 109 (second molding surface 121), and the resin gradually fills product molding section 130. After the resin filled in product molding section 130 has been sufficiently cooled, molded article 173 (see FIG. 13) including resin molded article 151 filled in product molding section 130 is removed from the injection mold 101.
[0036] At this time, the molded product 173 taken out may be deformed as shown in Fig. 13. When the shape of the resin molded product 151 is rectangular, it often becomes warped in the direction of the long side. This will be explained.
[0037] Resin gate 135 is called a side gate because of the manner in which it is connected to product molding portion 130. Generally, in a side gate, a structure is often adopted in which the thickness of communication passage portion 133 becomes thinner as it approaches product molding portion 130, taking into consideration gate cut. In other words, communication passage portion 133 is formed so that the thickness of remaining resin portion 171 located in communication passage portion 133 is thinner than the thickness of resin molded product 151.
[0038] Therefore, in the molded product 173 taken out of the injection mold 101, the amount of warping of the relatively thick resin molded product 151 is greater than the amount of warping of the relatively thin remaining resin portion 171. Note that in Fig. 12, the amount of warping is exaggerated by a two-dot chain line. The warping of the remaining resin portion 171 cannot follow the warping of the resin molded product 151, and a difference occurs between the amount of warping of the resin molded product 151 and the amount of warping of the remaining resin portion 171.
[0039] Due to the difference in the amount of warping, stress tends to concentrate at the connection (seam) between the resin molded product 151 and the remaining resin part 171. This connection part corresponds to the position of the resin gate 135. If the stress concentrated at the connection part remains in the resin molded product 151 after the remaining resin part 171 is removed, birefringence is likely to be induced, and a phase difference may occur. As a result, it is expected that the optical properties of the resin molded product 151 will deteriorate.
[0040] Unlike the injection molding die 101 according to the comparative example, in the injection molding die 1 according to the first embodiment, the resin gate 35 that sends out resin to the product molding portion 30 opens to the first molding surface 9, not the third molding surface 11 in the product molding portion 30. Therefore, as shown in Fig. 14, in the molded product 73 removed from the injection molding die 1, the remaining resin portion 71 is connected to the first molded surface 61 of the resin molded product 51.
[0041] As a result, compared to a structure in which the remaining resin portion 171 is connected to the third molded surface 165 of the resin molded product 151, the warping of the remaining resin portion 71 is more likely to follow the warping of the resin molded product 51. In addition, since the remaining resin portion 71 extending in the longitudinal direction is connected to the first molded surface 61 of the resin molded product 51 which tends to warp in the longitudinal direction, the warping of the resin molded product 51 can be suppressed. Therefore, the amount of warping of the resin molded product 51 and the amount of warping of the remaining resin portion 71 are smaller than those in the comparative example. In FIG. 14, the amount of warping smaller than that in the comparative example is indicated by a two-dot chain line.
[0042] The reduction in the amount of warping of the resin molded product 51 and the amount of warping of the remaining resin portion 71 makes it possible to suppress stress concentration at the connection portion between the resin molded product 51 and the remaining resin portion 71. As a result, the stress remaining in the resin molded product 51 after the remaining resin portion 71 is removed is reduced, making it possible to suppress deterioration of the optical properties of the resin molded product 51 due to the residual stress.
[0043] Next, the results of evaluating the birefringence of the resin molded product 51 according to the first embodiment and the resin molded product 151 according to the comparative example will be described. As shown in FIG. 15, the length L1 in the longitudinal direction of the resin molded product 51 according to the embodiment is 200 mm, the length L2 in the lateral direction is 120 mm, and the width W of the resin remaining part 71, i.e., the width W of the resin gate 35, is 80 mm. On the other hand, the length CL1 in the longitudinal direction of the resin molded product 151 according to the comparative example is 200 mm, the length CL2 in the lateral direction is 120 mm, and the width CW of the resin remaining part 171, i.e., the width CW of the resin gate 135, is 80 mm. In both cases, the size of the light transmitting part is 180 mm×100 mm.
[0044] The resin used was polycarbonate resin, which is prone to birefringence among transparent resins. The retardation values of the light-transmitting area (180 mm x 100 mm) in the resin molded product 51 were measured, and the magnitude relationship of the average retardation values was expressed by the degree of density of the hatching. Similarly, the retardation values of the light-transmitting area (180 mm x 100 mm) in the resin molded product 151 were measured, and the magnitude relationship of the average retardation values was expressed by the degree of density of the hatching.
[0045] The retardation value is a value indicating the degree of change in phase difference when light passes through the resin molded product 51 (resin molded product 151). Generally, nm is used as a unit. It can be said that the lower the retardation value, the lower the birefringence. As a result of the evaluation, it was found that the average retardation value of the resin molded product 51 according to the embodiment was 42 nm. On the other hand, it was found that the average retardation value of the resin molded product 151 according to the comparative example was 59 nm. It was demonstrated that the resin molded product according to the embodiment can reduce birefringence by about 30% compared to the comparative example by using the injection molding die 1 in which the resin gate 35 opens on the first molding surface.
[0046] The size of the resin molded product 51 is not limited to the above-mentioned size. The size of the resin molded product 51 molded by the injection mold die 1 can be larger than 200×120 (L1: 200 mm, L2: 120 mm). The inventors molded a resin molded product having a size of 300×150 (L1: 300 mm, L2: 150 mm) and confirmed that the birefringence reduction effect was obtained similarly to the resin molded product 51 of the above-mentioned size.
[0047] Incidentally, in the portion where resin gate 35 is located, it is considered desirable that angle θ (see FIG. 6) between the side wall surface of fixed-side convex portion 23 and first molding surface 9 of movable-side first recess 7 is an angle of about 90°. If angle θ is sufficiently larger than 90°, there is a concern that resin may not be sufficiently filled in product molding portion 30. On the other hand, if angle θ is sufficiently smaller than 90°, there is a concern that the effect of reducing birefringence may be halved, since the structure approaches that of the side gate according to the comparative example.
[0048] It is also considered desirable that the width W of the resin gate 35 be at least 1 / 5 of the longitudinal length L1 (see FIG. 5) of the product molding section 30. This is because, if the width W of the resin gate 35 is shorter than 1 / 5 of the length L1, more pressure (molding pressure) will be required to send the resin to the product molding section 30, and it is expected that molding of the resin molded product 51 itself will become difficult. If there is no problem with the fluidity of the resin, it is desirable that the width W of the resin gate 35 is short. This is because the length of the resin gate mark 57 will be shorter if the width W of the resin gate 35 is short.
[0049] A banana gate is known as one of the resin gate structures. The banana gate opens at a pinpoint in the cavity body corresponding to the product molding part. That is, the banana gate has a structure in which a substantially circular gate opens on the molding surface of the cavity body. As a result, a substantially circular resin gate mark remains on a resin molded product molded using an injection molding die that employs a banana gate.
[0050] On the other hand, as described above, in the resin molded product 51 molded using the injection molding die 1 according to the first embodiment, the resin gate mark 57 is left so as to extend in a strip shape. Therefore, the resin gate mark of the resin molded product 51 according to the first embodiment is clearly different in structure from the resin gate mark of a resin molded product molded by an injection molding die employing a banana gate. That is, by checking the resin gate mark of the resin molded product, it is possible to determine whether the resin molded product 51 is manufactured using the injection molding die 1. Note that, as a method for manufacturing the resin molded product 51 using the injection molding die 1, the resin 47 may be injected under an arrangement in which the product molding portion 30 (cavity body) is horizontal.
[0051] Embodiment 2 An example of an injection molding die according to embodiment 2 will be described. As shown in Fig. 16 and Fig. 17, a movable side first recess 7, a movable side second recess 13, and a movable side third recess 17 are formed in a movable side die 3 of an injection molding die 1. A fixed side protrusion 23 that faces the movable side second recess 13 is formed in a fixed side die 19.
[0052] When the movable-side mold 3 and the fixed-side mold 19 are in contact with each other, a cavity 29 including a product molding portion 30, a runner portion 31 and a submerged gate portion 33, and a resin gate 35 are formed. The movable-side second recess 13 and the fixed-side protrusion 23 face each other with a gap between them, so that the resin gate 35 is formed on the first molding surface 9 of the product molding portion 30.
[0053] The resin gate 35 opening into the first molding surface 9 is formed so as to open from a third position P3 on the first molding surface 9 which is more inward than the first position P1 where the third molding surface 11b is located, to a fourth position P4 which is more inward than the third position P3, and to extend along the first position P1.
[0054] The product molding portion 30 is formed by the first molding surface 9a (first molding surface 9) and the third molding surface 11a (third molding surface 11) of the movable-side first recess 7, the third molding surface 11b (third molding surface 11) and the first molding surface 9b (first molding surface 9) of the fixed-side protrusion 23, and the second molding surface 21 of the fixed-side mold 19. Note that other configurations are similar to those of the injection molding die 1 shown in Figures 5 and 6, so the same members are denoted by the same reference numerals, and description thereof will not be repeated unless necessary.
[0055] Next, a method for manufacturing a resin molded product using the above-mentioned injection molding die 1 will be described. The manufacturing method using the above-mentioned injection molding die 1 is similar to the manufacturing method using the injection molding die 1 described in embodiment 1. As shown in Fig. 17, with the movable die 3 and the fixed die 19 in contact with each other, resin is injected from the resin gate 35 into the product molding section 30, thereby molding a resin molded product 51.
[0056] 18, a resin gate mark 57 corresponding to the resin gate 35 is left on the first molded surface 61 of the molded resin molded product 51. The resin gate mark 57 has a width from a position on the first molded surface 61 that is more inward than the position where the third molded surface 65 is located (corresponding to the third position P3) to a position more inward than that position (corresponding to the fourth position P4), and is left in a band shape extending along the third molded surface 65. The resin gate mark 57 is left on the first molded surface 61, which is a non-design surface.
[0057] In the injection mold 1 described above, the resin gate 35 opens on the first molding surface 9 in the product molding portion 30. As a result, similar to the description in the first embodiment, the residual stress of the resin molded product 51 is reduced, and birefringence can be reduced. In particular, the resin gate 35 opens on the first molding surface 9 from the third position P3, which is on the inside of the first position P1 where the third molding surface 11b is located, to the fourth position P4, which is on the inside of the third position P3, making it easier to fill the resin in the product molding portion 30, which can contribute to further reducing birefringence. Note that the resin gate 35 needs to be opened at a desired position that does not affect the light transmitting portion 53 in the resin molded product 51.
[0058] Embodiment 3 An example of an injection molding die according to embodiment 3 will be described. As shown in Fig. 19 and Fig. 20, a movable side first recess 7, a movable side convex portion 15 as a first die side convex portion, and a movable side third recess 17 are formed in a movable side die 3 of an injection molding die 1. A fixed side recess 25 as a second die recess that faces the movable side convex portion 15 is formed in a fixed side die 19.
[0059] When the movable-side mold 3 and the fixed-side mold 19 are in contact with each other, a cavity 29 including a product molding portion 30, a runner portion 31 and a communication passage portion 34, and a resin gate 35 are formed. The movable-side convex portion 15 and the fixed-side concave portion 25 face each other with a gap between them, so that the resin gate 35 is formed on the second molding surface 21 of the product molding portion 30. Also, unlike the submerged gate portion 33, the communication passage portion 34 is formed in a manner that it climbs over the movable-side convex portion 15.
[0060] The resin gate 35 that opens into the second molding surface 21 is formed so as to open on the second molding surface 21 from a fifth position P5 where the third molding surface 11c is located to a sixth position P6 that is more inward than the fifth position P5, and to extend along the fifth position P5.
[0061] The product molding portion 30 is formed by the first molding surface 9 and the third molding surface 11a (third molding surface 11) of the movable-side first recess 7, the third molding surface 11c (third molding surface 11) of the movable-side protrusion 15, and the second molding surface 21 of the fixed-side mold 19. Note that other configurations are similar to the configuration of the injection molding die 1 shown in Figures 5 and 6, so the same members are given the same reference numerals and descriptions thereof will not be repeated unless necessary.
[0062] Next, a method for manufacturing a resin molded product using the above-mentioned injection molding die 1 will be described. The manufacturing method using the above-mentioned injection molding die 1 is similar to the manufacturing method using the injection molding die 1 described in embodiment 1. As shown in Fig. 20, with the movable die 3 and the fixed die 19 in contact with each other, resin is injected from the resin gate 35 into the product molding section 30, thereby molding a resin molded product 51.
[0063] 21, a resin gate mark 57 corresponding to the resin gate 35 is left on the second molded surface 63 of the molded resin molded product 51. The resin gate mark 57 is left in a band shape on the second molded surface 63, having a width from a position where the third molded surface 65 is located (corresponding to the fifth position P5) to a position inside that position (corresponding to the sixth position P6), and extending along the third molded surface 65. In this resin molded product 51, the resin gate mark 57 is left on the second molded surface 63, which is the design surface.
[0064] Generally, resin molded products are molded so that resin gate marks remain on the non-design surface. In cases where the resin gate marks remain on the design surface, the above-described injection molding die 1 may be used to mold a resin molded product 51 in which resin gate marks 57 remain on the second molded surface 63, which is the design surface. In this case, the communication passage portion 34 is formed in such a manner that it climbs over the movable-side convex portion 15, so that the structure of the communication passage portion 34 is simpler than that of the submerged gate portion 33. This makes it possible to reduce the amount of resin remaining in the communication passage portion 34, and therefore the amount of resin to be discarded.
[0065] Furthermore, in the above-mentioned injection molding die 1, the resin gate 35 opens to the second molding surface 21 in the product molding portion 30, so that the residual stress in the resin molded product 51 is reduced, and birefringence can be reduced, as described in embodiment 1.
[0066] Embodiment 4 An example of an injection molding die according to embodiment 4 will be described. As shown in Fig. 22, a movable side first recess 7, a movable side second recess 13, and a movable side third recess 17 are formed in a movable side die 3 of an injection molding die 1. A fixed side protrusion 23 that faces the movable side second recess 13 is formed in a fixed side die 19.
[0067] 6, when the movable-side mold 3 and the fixed-side mold 19 are in contact with each other, a cavity 29 including a product molding portion 30, a runner portion 31 and a submerged gate portion 33, and a resin gate 35 are formed. The resin gate 35 is formed on the first molding surface 9 of the product molding portion 30 by the movable-side second recess 13 and the fixed-side protrusion 23 facing each other with a gap therebetween.
[0068] The resin gate 35 opening into the first molding surface 9 is formed so as to open from a first position P1 on the first molding surface 9 where the third molding surface 11b is located to a second position P2 which is more inward than the first position P1, and to extend along the first position P1.
[0069] The runner portion 31 and the submerged gate portion 33 are formed in a trapezoidal shape with a width gradually increasing from width W1 to width W2 from the runner portion 31 toward the submerged gate portion 33 when the first molding surface 9 is viewed in plan. Note that other configurations are similar to the configuration of the injection molding die 1 shown in Figures 5 and 6, so the same members are denoted by the same reference numerals and description thereof will not be repeated unless necessary.
[0070] Next, a method for manufacturing a resin molded product using the above-mentioned injection molding die 1 will be described. The manufacturing method using the above-mentioned injection molding die 1 is similar to the manufacturing method using the injection molding die 1 described in embodiment 1. As shown in Fig. 6, resin is injected from the resin gate 35 into the product molding section 30 with the movable die 3 and the fixed die 19 in contact with each other, thereby molding a resin molded product 51.
[0071] 11, a resin gate mark 57 corresponding to the resin gate 35 is left on the first molded surface 61 of the molded resin molded product 51. The resin gate mark 57 is left in a band shape on the first molded surface 61, having a width from a position where the third molded surface 65 is located (corresponding to the first position P1) to a position inside that position (corresponding to the second position P2), and extending along the third molded surface 65. The resin gate mark 57 is left on the first molded surface 61, which is a non-design surface.
[0072] In the above-mentioned injection molding die 1, the resin gate 35 opens to the first molding surface 9 in the product molding portion 30, so that the residual stress in the resin molded product 51 is reduced and birefringence can be reduced, as described in embodiment 1.
[0073] Furthermore, when the first molding surface 9 is viewed in a plan view, the runner portion 31 and the submerged gate portion 33 are formed in a trapezoidal shape with a width gradually increasing from the runner portion 31 toward the submerged gate portion 33. In particular, since the submerged gate portion 33 is formed in a trapezoidal shape in a plan view, the amount of resin remaining in the submerged gate portion 33 can be reduced, which can contribute to reducing the amount of resin to be discarded.
[0074] In order to efficiently send resin from resin gate 35 to product molding section 30, it is desirable for the opening shape of resin gate 35 to have a shape that widens from the first position P1 to the second position P2 (see Figure 22).
[0075] Embodiment 5. An example of an injection molding die according to embodiment 5 will be described. As shown in Fig. 23 and Fig. 24, a movable side first recess 7, a movable side second recess 13, and a movable side third recess 17 are formed in a movable side die 3 of an injection molding die 1. A fixed side convex portion 23 that faces the movable side second recess 13 is formed in a fixed side die 19.
[0076] When the movable-side mold 3 and the fixed-side mold 19 are in contact with each other, a cavity 29 including a product molding portion 30, a runner portion 31 and a submerged gate portion 33, and a resin gate 35 are formed. The movable-side second recess 13 and the fixed-side protrusion 23 face each other with a gap between them, so that the resin gate 35 is formed on the first molding surface 9 of the product molding portion 30.
[0077] The resin gate 35 opening into the first molding surface 9 is formed so as to open from a first position P1 on the first molding surface 9 where the third molding surface 11b is located to a second position P2 which is more inward than the first position P1, and to extend along the first position P1.
[0078] The submerged gate portion 33 is formed so that its cross section in the direction in which the resin flows from the runner portion 31 toward the resin gate 35 and in the direction perpendicular to the first molding surface 9 and the second molding surface 21 is curved. The submerged gate portion 33 is formed so as to describe a circular arc. Note that the rest of the configuration is similar to that of the injection molding die 1 shown in Figures 5 and 6, so the same members are denoted by the same reference numerals, and description thereof will not be repeated unless necessary.
[0079] Next, a method for manufacturing a resin molded product using the above-mentioned injection molding die 1 will be described. The manufacturing method using the above-mentioned injection molding die 1 is similar to the manufacturing method using the injection molding die 1 described in embodiment 1. As shown in Fig. 24, with the movable die 3 and the fixed die 19 in contact with each other, resin is injected from the resin gate 35 into the product molding section 30, thereby molding a resin molded product 51.
[0080] 11, a resin gate mark 57 corresponding to the resin gate 35 is left on the first molded surface 61 of the molded resin molded product 51. The resin gate mark 57 is left in a band shape on the first molded surface 61, having a width from a position where the third molded surface 65 is located (corresponding to the first position P1) to a position inside that position (corresponding to the second position P2), and extending along the third molded surface 65. The resin gate mark 57 is left on the first molded surface 61, which is a non-design surface.
[0081] In the above-mentioned injection molding die 1, the resin gate 35 opens to the first molding surface 9 in the product molding portion 30, so that the residual stress in the resin molded product 51 is reduced and birefringence can be reduced, as described in embodiment 1.
[0082] Further, the submerged gate portion 33 has a cross-sectional shape curved like a circular arc along the direction in which the resin flows from the runner portion 31 toward the resin gate 35. This allows the movable mold 3 to be slid and released from the fixed mold relatively easily after the resin filled in the product molding portion 30 has been sufficiently cooled.
[0083] Embodiment 6 An example of an injection molding die according to the sixth embodiment will be described. As shown in Fig. 25, the movable side die 3 in the injection molding die 1 is formed with the movable side first recess 7, the movable side second recess 13a, the movable side second recess 13b, the movable side third recess 17a and the movable side third recess 17b. The fixed side die 19 is formed with the fixed side convex portion 23a which faces the movable side second recess 13a and the fixed side convex portion 23b which faces the movable side second recess 13b.
[0084] When the movable side mold 3 and the fixed side mold 19 are in contact with each other, a cavity 29 including a product molding portion 30, a runner portion 31a, a runner portion 31b, a submerged gate portion 33a and a submerged gate portion 33b, and a resin gate 35a and a resin gate 35b are formed.
[0085] The movable-side second recess 13a and the fixed-side protrusion 23a face each other with a gap therebetween, so that a resin gate 35a is formed on the first molding surface 9 of the product molding section 30. The movable-side second recess 13b and the fixed-side protrusion 23b face each other with a gap therebetween, so that a resin gate 35b is also formed on the first molding surface 9 of the product molding section 30.
[0086] That is, in the injection molding die 1, two resin gates 35a and 35b are formed for one product molding portion 30. The resin gates 35a and 35b are disposed at positions corresponding to two light transmitting portions formed in one resin molded product, respectively.
[0087] Other than this, the configuration is similar to that of the injection molding die 1 shown in Figures 5 and 6, so the same members are given the same reference numerals and the description thereof will not be repeated unless necessary.
[0088] Next, a method for manufacturing a resin molded product using the above-mentioned injection molding die 1 will be described. The manufacturing method using the above-mentioned injection molding die 1 is similar to the manufacturing method using the injection molding die 1 described in embodiment 1. With the movable die 3 and the fixed die 19 in contact with each other, resin is injected into the product molding section 30 from each of the resin gates 35a and 35b, thereby molding a resin molded product 51.
[0089] 26, two light transmitting portions, 53a and 53b, are formed in the molded resin molded product 51. A resin gate mark 57a corresponding to the resin gate 35a and a resin gate mark 57b corresponding to the resin gate 35b are left on a first molded surface 61 of the resin molded product 51. The resin gate mark 57a is left at a position corresponding to the light transmitting portion 53a. The resin gate mark 57b is left at a position corresponding to the light transmitting portion 53b.
[0090] In the above-mentioned injection molding die 1, the resin gates 35a and 35b open to the first molding surface 9 in the product molding portion 30, and thus, as described in embodiment 1, the residual stress in the resin molded product 51 is reduced, thereby making it possible to reduce birefringence.
[0091] In the injection mold 1, resin is filled into one product molding portion 30 from each of resin gates 35a and 35b. When the resin filled from resin gate 35a and the resin filled from resin gate 35b join together, a weld line may occur in the product molding portion 30. When a weld line occurs, a line appears on the surface of the resin molded product 51.
[0092] If a line appears in light transmitting portion 53a or light transmitting portion 53b in resin molded product 51, the image may be distorted when light passes through. For this reason, resin gate 35a and resin gate 35a need to be formed at a position relative to product molding portion 30 where no weld line will occur.
[0093] In addition to optical products such as lenses or display panels, the resin molded product 51 can also be applied to optical products such as prisms by changing the shape of the product molding part. The injection molding dies explained in each embodiment can be variously combined as necessary.
[0094] The embodiments disclosed herein are illustrative and are not limited thereto. The present disclosure is not limited to the above-described scope, but is defined by the scope of the claims, and is intended to include all modifications within the meaning and scope equivalent to the scope of the claims. [Industrial Applicability]
[0095] The present disclosure is effectively utilized for injection molding dies. [Explanation of symbols]
[0096] 1 injection molding die, 3 movable side die, 7 movable side first recess, 9, 9a, 9b first molding surface, 11, 11a, 11b, 11c third molding surface, 13, 13a, 13b movable side second recess, 15 movable side first convex portion, 17, 17a, 17b movable side third recess, 18 ejector pin, 19 fixed side die, 21 second molding surface, 23, 23a, 23b fixed side convex portion, 25 fixed side recess, 27 runner, 29 cavity, 30 product molding portion, 31, 31a, 31b runner portion, 33, 33a, 33b submerged gate portion, 34 communication passage portion, 35, 35a, 35b resin gate, 41 injection molding device, 43 hopper, 45 cylinder, 47 resin, 51 resin molded product, 53 Light transmission part, 55 bezel, 57 resin gate marks, 61 first molded surface, 63 second molded surface, 65 third molded surface, 71 remaining resin, 73 molded product, P1, P2, P3, P4, P5 positions.
Claims
1. A molding die including a first die and a second die, in which one or more cavities including a cavity body for molding a resin molded product having a first molded surface, a second molded surface, and a third molded surface are formed, a first molding surface formed in the first mold and configured to mold the first molded surface; a second molding surface that is formed in the second mold disposed so as to face the first mold and that molds the second molded surface; a third molding surface that is formed to connect between the first molding surface and the second molding surface when the first mold and the second mold are in contact with each other and that molds the third molded surface; a resin gate that feeds resin into the cavity main body that is formed by a plurality of molding surfaces including the first molding surface, the second molding surface, and the third molding surface while the first mold and the second mold are in contact with each other; Equipped with a molding die, the resin gate being formed so as to open to either the first molding surface or the second molding surface which face each other when the first mold and the second mold are in contact with each other, and to extend along the third molding surface.
2. the resin gate opens onto the first molding surface, 2. The molding die according to claim 1, wherein, when the first die and the second die are in contact with each other, the resin gate is formed so as to open on the first molding surface from a first position where the third molding surface is located to a second position that is more inward than the first position, and to extend along the first position.
3. The cavity is a runner portion to which the resin is supplied; a communication passage portion that communicates with the resin gate from the runner portion and sends the supplied resin to the resin gate; Including, The first mold includes: a first mold-side first recess having a bottom surface that becomes the first molding surface and a side wall surface that becomes the third molding surface; a second recess on a first mold side that is deeper than the first recess on the first mold side; a third recess on the first mold side that is shallower than the second recess on the first mold side; are formed, respectively, The second mold has a second mold convex portion formed therein, the second mold convex portion facing the first mold second concave portion and including a part of the third molding surface; In a state in which the first mold and the second mold are in contact with each other, the cavity main body is formed by the first molding surface and the third molding surface of the first recess of the first mold, the part of the third molding surface of the second mold convex portion, and the second molding surface of the second mold, The runner portion is formed by the third recess portion on the first mold side, The molding die according to claim 2, wherein the first die side second recess and the second die side convex portion face each other with a gap therebetween, thereby forming the communication passage portion that communicates the runner portion and the resin gate.
4. the resin gate opens onto the first molding surface, 2. The molding die according to claim 1, wherein, when the first mold and the second mold are in contact with each other, the resin gate is formed so as to open on the first molding surface from a third position spaced a distance inward from the third molding surface to a fourth position more inward than the third position, and to extend along the first position where the third molding surface is located.
5. The cavity is a runner portion to which the resin is supplied; a communication passage portion that communicates with the resin gate from the runner portion and sends the supplied resin to the resin gate; Including, The first mold includes: a first mold-side first recess having a bottom surface that becomes the first molding surface and a side wall surface that becomes the third molding surface; a second recess on a first mold side that is deeper than the first recess on the first mold side; a third recess on the first mold side that is shallower than the second recess on the first mold side; are formed, respectively, the second mold has a second mold convex portion formed therein, the second mold convex portion facing the first mold second concave portion and including a part of the third molding surface and a part of the first molding surface; In a state in which the first mold and the second mold are in contact with each other, the cavity main body is formed by the first molding surface and the third molding surface of the first recess of the first mold, the part of the third molding surface and the part of the first molding surface of the second mold convex portion, and the second molding surface of the second mold, The runner portion is formed by the first mold third recess, The molding die according to claim 4, wherein the first die side second recess and the second die side convex portion face each other with a gap therebetween, thereby forming the communication passage portion that communicates the runner portion and the resin gate.
6. the resin gate opens to the second molding surface, 2. The molding die according to claim 1, wherein, when the first die and the second die are in contact with each other, the resin gate is formed so as to open on the second molding surface from a fifth position where the third molding surface is located to a sixth position that is more inward than the fifth position, and to extend along the fifth position.
7. The cavity is a runner portion to which the resin is supplied; a communication passage portion that communicates with the resin gate from the runner portion and sends the supplied resin to the resin gate; Including, The first mold includes: a first mold-side first recess having a bottom surface that becomes the first molding surface and a side wall surface that becomes the third molding surface; a first mold side protrusion that protrudes toward the second mold and includes a part of the third molding surface; A third recess on the first mold side; are formed, respectively, The second mold has a second mold recess formed therein, the second mold recess facing the first mold protrusion of the first mold, In a state in which the first mold and the second mold are in contact with each other, the cavity main body is formed by the first molding surface and the third molding surface of the first recess of the first mold, the part of the third molding surface of the first mold convex portion, and the second molding surface of the second mold, The runner portion is formed by the first mold third recess, The molding die according to claim 6, wherein the first die side convex portion and the second die side concave portion face each other with a gap therebetween, thereby forming the communication passage portion that communicates between the runner portion and the resin gate.
8. The molding die according to claim 3, wherein, when the first molding surface is viewed in a plane, the runner portion and the communicating passage portion are formed to have a trapezoidal shape with a width increasing from the runner portion toward the cavity main body.
9. The molding die according to claim 3 , wherein the communication passage portion is formed in such a manner that a cross section along a direction in which the resin flows from the runner portion toward the resin gate is curved.
10. The molding die according to any one of claims 1 to 9, wherein the cavity includes a first resin gate as the resin gate and a second resin gate as the resin gate, each of which feeds the resin into the cavity body.
11. A method for manufacturing a resin molded product using a molding die having a cavity body for molding a resin molded product having a first molded surface, a second molded surface, and a third molded surface, comprising the steps of: providing the molding die having a first die and a second die; filling the cavity body of the molding die with resin; removing the resin molded product filled in the cavity body from the molding die; Equipped with In the step of preparing a molding die, The first mold has a first molding surface that molds the first molded surface, The second mold has a second molding surface that molds the second molded surface, a third molding surface that molds the third molded surface is formed so as to connect between the first molding surface and the second molding surface when the first mold and the second mold are in contact with each other; When the first mold and the second mold are in contact with each other, the cavity body is formed by a plurality of molding surfaces including the first molding surface, the second molding surface, and the third molding surface, which are opposed to each other; a molding die is prepared, the molding die having a resin gate formed therein, the resin gate opening in either the first molding surface or the second molding surface facing each other and extending along the third molding surface for feeding resin into the cavity body; In the step of filling the cavity body with the resin, the resin is filled into the cavity body from the resin gate in a manner that intersects with either the first molding surface or the second molding surface, A method for manufacturing a resin molded product, wherein in a process of removing the resin molded product from the molding die, a resin gate mark is left on either the first molded surface or the second molded surface of the resin molded product, extending along the third molded surface.
12. A first molded surface; A second molded surface positioned opposite the first molded surface; a third molded surface connecting the first molded surface and the second molded surface; Equipped with A resin molded product, wherein a resin gate mark is left on either the first molded surface or the second molded surface so as to extend along the third molded surface.
Citation Information
Patent Citations
Sprue structure for injection mold and injection mold
CN212400208U
Molding method
JP1993000425A
Underside pin gate injection mold
JP1994143351A
Die for light guide plate, its manufacture, polarized light source device, and liquid crystal display device
JP1998027512A
Mold for injection molding and injection molding method
JP1998193397A