Anode catalyst, water electrolysis cell, and water electrolysis cell stack

A perovskite-structured anode catalyst with specific ion combinations and radius differences enhances the catalytic activity and longevity of water electrolysis cells by stabilizing the catalyst in the oxidizing environment.

JP2024148374AActive Publication Date: 2024-10-18TOKYO GAS CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023061468
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-05
Publication Date
2024-10-18
Estimated Expiration
2043-04-05

AI Technical Summary

Technical Problem

Anode catalysts used in water electrolysis suffer from high catalytic activity but have a short lifespan due to dissolution of elements like ruthenium and iridium in the strong oxidizing atmosphere during the process.

Method used

An anode catalyst with a perovskite structure containing alkaline earth metal ions in the A site and tetravalent metal ions, such as zirconium or titanium, and iridium in the B site, with a specific ionic radius difference, is developed to maintain high catalytic activity and extend the catalyst's life.

Benefits of technology

The anode catalyst maintains high catalytic activity and current density over a prolonged period, outperforming traditional catalysts by retaining performance and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024148374000007
    Figure 2024148374000007
  • Figure 2024148374000008
    Figure 2024148374000008
  • Figure 2024148374000001
    Figure 2024148374000001
Patent Text Reader

Abstract

To provide an anode catalyst having both a high catalytic activity and a long life.SOLUTION: The anode catalyst includes perovskite type oxide including an alkali earth metal ion in an A site ion and a tetravalent metal ion and an Ir ion in a B site ion thereof, with the alkali earth metal ion included in the A site ion including a Ca ion and an Sr ion, the Ca ion and a Ba ion, or the Ca ion, the Sr ion and the Ba ion, and the tetravalent metal ion included in the B site ion including a Zr ion and / or a Ti ion, a mol concentration of the Ir ion included in the B site ion being 35 mol% or more, and an ion radius difference (rA-rCa) defined by the formula shown below being from 0.0175 to 0.2616Å, provided that rA represents an ion radius of the A site ion, ri represents an ion radius of the alkali earth metal ion included in the A site ion, mi represents a mol concentration of the alkali earth metal ion, and rca represents the Ca ion.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to an anode catalyst, a water electrolysis cell, and a water electrolysis cell stack. [Background technology]

[0002] Water electrolysis (hereinafter sometimes referred to as "water electrolysis") is a method for producing hydrogen and oxygen from water by electrolysis. For example, among technologies that utilize hydrogen as an energy source, water electrolysis is a promising technology for sustainable hydrogen production.

[0003] A water electrolysis cell used for water electrolysis includes an anode separator, an anode gas diffusion layer, an anode catalyst, an electrolyte membrane, a cathode catalyst, a cathode gas diffusion layer, a cathode separator, etc. Regarding the anode catalyst and cathode catalyst, catalysts suitable for water electrolysis are being studied.

[0004] For example, Patent Document 1 discloses PdRu solid solution nanoparticles containing palladium (Pd) and ruthenium (Ru), and discloses that the nanoparticles are used as a catalyst for water electrolysis reactions. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2018 / 159644 Summary of the Invention [Problem to be solved by the invention]

[0006] Anode catalysts containing elements having anode activity, such as ruthenium and iridium, have high catalytic activity. However, since the anode catalyst is exposed to a strong oxidizing atmosphere during water electrolysis, elements such as ruthenium and iridium are easily dissolved, resulting in a short lifespan.

[0007] For example, in a water electrolysis catalyst containing ruthenium as disclosed in Patent Document 1, there is a risk that ruthenium will dissolve and the catalyst will have a shortened lifespan.

[0008] An object of the present disclosure is to provide an anode catalyst that combines high catalytic activity with a long life, and a water electrolysis cell and a water electrolysis cell stack including the anode catalyst. [Means for solving the problem]

[0009] The present disclosure includes the following aspects. <1> The present invention includes an oxide having a perovskite structure, the A site ions of which include alkaline earth metal ions, and the B site ions of which include tetravalent metal ions and iridium ions, the alkaline earth metal ions contained in the A site ions include a combination of calcium ions and strontium ions, a combination of calcium ions and barium ions, or a combination of calcium ions, strontium ions and barium ions; the tetravalent metal ions contained in the B site ions include at least one selected from zirconium ions and titanium ions, the molar concentration of the iridium ions contained in the B site ions is 35 mol % or more; The ionic radius of the A site ion is r A , and the ionic radius of the alkaline earth metal ion contained in the A site ion is r i , the molar concentration of the alkaline earth metal ions is m i , and the ionic radius of the calcium ion is r ca In this case, the ionic radius difference between the A site ion and the calcium ion (r A -r Ca ) is 0.0175 Å to 0.2616 Å.

[0010]

number

[0011] <2> The difference in ionic radius (r A -r Ca ) is 0.0474Å to 0.2316Å <1> The anode catalyst according to claim 1, <3> The difference in ionic radius (r A -r Ca ) is 0.0668Å to 0.2122Å <1> The anode catalyst according to claim 1, <4> an anode gas diffusion layer; <1> ~ <3> 13. A water electrolysis cell comprising: the anode catalyst according to any one of claims 1 to 12; an electrolyte membrane; a cathode catalyst; a cathode gas diffusion layer; and a separator. <5> <4> A water electrolysis cell stack in which a plurality of water electrolysis cells according to claim 1 are stacked. Effect of the Invention

[0012] According to the present disclosure, there are provided an anode catalyst that combines high catalytic activity with a long life, and a water electrolysis cell and a water electrolysis cell stack including the anode catalyst. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a schematic cross-sectional view of a water electrolysis cell. [Diagram 2] FIG. 2 is a graph showing the relationship between the ionic radius difference (rA-rCa) and the current density in each of the examples and comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, the embodiments of the present disclosure will be described in detail. The present disclosure is not limited to the following embodiments, and can be implemented with appropriate modifications within the scope of the object of the present disclosure. The dimensional ratios in the drawings do not necessarily represent the actual dimensional ratios.

[0015] In the present disclosure, a numerical range expressed using "to" means a range that includes the numerical values ​​before and after "to" as the lower and upper limits.

[0016] In the present disclosure, the upper limit value described in a certain numerical range may be replaced with the upper limit value of another numerical range described in a certain numerical range, and the lower limit value described in a certain numerical range may be replaced with the lower limit value of another numerical range described in a certain numerical range. In the present disclosure, the upper limit value or lower limit value described in a certain numerical range may be replaced with a value shown in the examples.

[0017] In the present disclosure, combinations of two or more preferred embodiments are more preferred embodiments.

[0018] [Anode catalyst] The anode catalyst of the present disclosure includes an oxide having a perovskite structure including alkaline earth metal ions as A site ions and tetravalent metal ions and iridium ions as B site ions, the alkaline earth metal ions included in the A site ions include a combination of calcium ions and strontium ions, a combination of calcium ions and barium ions, or a combination of calcium ions, strontium ions and barium ions, the tetravalent metal ions included in the B site ions include at least one selected from zirconium ions and titanium ions, the molar concentration of the iridium ions included in the B site ions is 35 mol % or more, and the ionic radius of the A site ions is r A , and the ionic radius of the alkaline earth metal ion contained in the A site ion is r i , the molar concentration of the alkaline earth metal ions is m i , and the ionic radius of the calcium ion is r ca In this case, the ionic radius difference between the A site ion and the calcium ion (r A -r Ca ) is 0.0175 Å to 0.2616 Å. The anode catalyst of the present disclosure is an anode catalyst that combines high catalytic activity with a long life. Here, "long life" means that high catalytic activity is unlikely to be lost for a long period of time.

[0019]

number

[0020] The anode catalyst of the present disclosure includes an oxide having a perovskite structure, and the molar concentration of iridium ions contained in the B-site ions of the oxide having a perovskite structure is relatively high at 35 mol% or more, and therefore tends to have high catalytic activity. In addition, the anode catalyst of the present disclosure tends not to lose its high catalytic activity for a long period of time, since the perovskite structure is a stable crystal structure. Furthermore, the anode catalyst of the present disclosure has a higher catalytic activity and tends not to lose its high catalytic activity for a long period of time, since the alkaline earth metal ions contained in the A-site ions of the oxide having a perovskite structure are of a specific type, combination, and mixing ratio, and the ionic radius difference between the A-site ions and calcium ions is within the above-mentioned numerical range. The anode catalyst of the present disclosure makes it possible to increase the current density of a water electrolysis cell and to maintain the increased current density satisfactorily for a long period of time.

[0021] <Oxides with perovskite structure> The anode catalyst of the present disclosure includes an oxide having a perovskite structure. Oxides having a perovskite structure are generally represented by the chemical formula ABO3. Some oxides with a perovskite structure have oxygen instability. The amount of oxygen in an oxide with a perovskite structure may be deficient or excessive compared to 3. The A-site ions and B-site ions may be partially substituted with different elements.

[0022] The A-site ions of the perovskite structure include alkaline earth metal ions, and the alkaline earth metal ions include a combination of calcium (Ca) ions and strontium (Sr) ions, a combination of calcium ions and barium (Ba) ions, or a combination of calcium ions, strontium ions, and barium ions. The alkaline earth metal ions contained in the A site ions of the perovskite structure preferably include a combination of calcium ions and strontium ions or a combination of calcium ions and barium ions, and more preferably a combination of calcium ions and strontium ions or a combination of calcium ions and barium ions.

[0023] The A-site ions in the perovskite structure may contain metal ions other than alkaline earth metal ions. Examples of the metal ions include trivalent metal ions. Examples of the trivalent metal ions include ions of metals such as aluminum (Al), chromium (Cr), and iron (Fe). From the viewpoint of better achieving the effects of the present disclosure, it is preferable that the A-site ions in the perovskite structure do not contain metal ions other than alkaline earth metal ions.

[0024] The A-site ions in the perovskite structure may or may not contain alkaline earth metal ions other than calcium ions, strontium ions, and barium ions. When the A-site ions of the perovskite structure contain an alkaline earth metal ion other than a calcium ion, a strontium ion, or a barium ion, examples of the alkaline earth metal ion include a beryllium (Be) ion and a magnesium (Mg) ion.

[0025] The B-site ions in the perovskite structure include a tetravalent metal ion and an iridium (Ir) ion, and the tetravalent metal ion includes at least one selected from a zirconium ion and a titanium ion. The B-site ions in the perovskite structure may include zirconium (Zr) ions and iridium ions, may include titanium (Ti) ions and iridium ions, or may include zirconium ions, titanium ions and iridium ions. Both zirconium ions and titanium ions are stable elements and contribute to extending the life of the anode catalyst. The tetravalent metal ion is preferably at least one selected from zirconium ions and titanium ions, and more preferably zirconium ions or titanium ions.

[0026] The B-site ions in the perovskite structure may or may not contain tetravalent metal ions other than zirconium ions and titanium ions.

[0027] The B-site ions in the perovskite structure may or may not contain metal ions other than tetravalent metal ions and iridium ions. When the B site ion of the perovskite structure contains a metal ion other than a tetravalent metal ion and an iridium ion, the metal ion is not particularly limited as long as it is an ion that can be located at the B site, and examples of the metal ion include ions of metals such as vanadium (V), niobium (Nb), tantalum (Ta), chromium (Cr), molybdenum (Mo), tungsten (W), manganese (Mn), iron (Fe), ruthenium (Ru), cobalt (Co), nickel (Ni), gallium (Ga), and tin (Sn).

[0028] The molar concentration of the tetravalent metal ions contained in the B site ions of the perovskite structure (when there are two or more types of metal ions, the total molar concentration of the two or more types of metal ions) may be 1 mol% to 65 mol%, 20 mol% to 65 mol%, or 33 mol% to 65 mol%.

[0029] The molar concentration of iridium ions contained in the B-site ions of the perovskite structure is 35 mol% or more from the viewpoint of catalytic activity of the anode catalyst. The upper limit of the molar concentration of iridium ions contained in the B-site ions of the perovskite structure is preferably 99 mol% or less, more preferably 80 mol% or less, and even more preferably 67 mol% or less, from the viewpoint of extending the life of the anode catalyst, for example. In one embodiment, the molar concentration of iridium ions contained in the B site ions of the perovskite structure may be 35 mol % to 99 mol %, 35 mol % to 80 mol %, or 35 mol % to 67 mol %.

[0030] The metal ions contained in the oxide having a perovskite structure and their concentrations can be identified by analytical methods such as high-frequency inductively coupled plasma optical emission spectrometry, energy dispersive X-ray spectrometry, electron beam microanalyzer, and X-ray photoelectron spectrometry.

[0031] In the oxide having a perovskite structure contained in the anode catalyst of the present disclosure, the ionic radius difference (r A -r Ca ) is 0.0175 Å to 0.2616 Å.

[0032]

number

[0033] In the above formula, r A is the ionic radius of the A-site ion, and r Ca is the ionic radius of the calcium ion, and r i is the ionic radius of the alkaline earth metal ion contained in the A site ion, and m i is the molar concentration of alkaline earth metal ions in the A site ions.

[0034] r Ameans the average ionic radius (Å) of the A-site ions on a molar basis. r Ca is 1.34 Å. The right-hand side of the above equation is calculated by subtracting the ionic radius (Å) of the calcium ion from the sum of the values ​​obtained by multiplying the ionic radius (Å) of the alkaline earth metal ion (i) by the molar concentration of the alkaline earth metal ion. In the present disclosure, the value of the "ionic radius" is the value described in the literature "RD Shannon, Revised effective ionic radii and systematic studies of interatomic distances in halides and chalcogenides, Acta Crystallogr. Sect. A 32, 751 (1976)."

[0035] The difference in ionic radius between the A-site ion and calcium ion (r A -r Ca From the viewpoint of the catalytic activity of the anode catalyst, the thickness of the anode electrode is 0.0175 Å to 0.2616 Å, preferably 0.0474 Å to 0.2316 Å, and more preferably 0.0668 Å to 0.2122 Å.

[0036] For example, when the alkaline earth metal ions contained in the A site ions are a combination of calcium ions and strontium ions, the ionic radius difference between the A site ions and the calcium ions (r A -r Ca ) is preferably 0.0091 Å to 0.1113 Å, more preferably 0.0258 Å to 0.0947 Å, and further preferably 0.0385 Å to 0.0820 Å. For example, when the alkaline earth metal ions contained in the A site ions are a combination of calcium ions and barium ions, the ionic radius difference between the A site ions and the calcium ions (r A -r Ca) is preferably 0.0176 Å to 0.2639 Å, more preferably 0.0478 Å to 0.2336 Å, and further preferably 0.0674 Å to 0.2140 Å.

[0037] The anode catalyst of the present disclosure may contain components (so-called other components) other than the oxide having the perovskite structure described above in the present disclosure. Examples of other components include components having catalytic activity other than oxides having a perovskite structure, unreacted components of the raw materials used in producing the oxides having a perovskite structure, and side reaction components.

[0038] The content of the oxide having the perovskite structure in the anode catalyst of the present disclosure is not particularly limited, but is, for example, preferably 50 mass % to 100 mass %, more preferably 70 mass % to 100 mass %, and further preferably 90 mass % to 100 mass %, relative to the total amount of the anode catalyst.

[0039] The content of the oxide having the perovskite structure in the anode catalyst of the present disclosure can be measured by X-ray diffraction. The content of the oxide having the perovskite structure in the anode catalyst of the present disclosure being 50 mass % or more relative to the total amount of the anode catalyst means that the oxide having the perovskite structure in the present disclosure is contained as a main phase of the anode catalyst of the present disclosure.

[0040] The anode catalyst may include a catalyst supported on a support. Supports include, for example, titanium oxide and tin oxide. The catalyst may be in the form of particles.

[0041] The primary particle size of the anode catalyst is not particularly limited, but is, for example, preferably from 1 nm to 10 μm, more preferably from 2 nm to 1 μm, and further preferably from 5 nm to 100 nm. When the primary particle size of the anode catalyst is 1 nm or greater, the mixing ratio of the ionomer required to increase the contact area does not become too large, and many electron conduction paths can be secured inside the anode catalyst layer, which tends to make it difficult to increase the resistance. If the primary particle size of the anode catalyst is 10 μm or less, the reduction in the contact area with the ionomer is suppressed, and therefore it tends to be difficult to achieve high resistance. The primary particle size of the anode catalyst can be measured using a scanning electron microscope or a transmission electron microscope.

[0042] An oxide having a perovskite structure containing alkaline earth metal ions as A-site ions and tetravalent metal ions and iridium ions as B-site ions, wherein the alkaline earth metal ions contained in the A-site ions include a combination of calcium ions and strontium ions, a combination of calcium ions and barium ions, or a combination of calcium ions, strontium ions and barium ions, and the tetravalent metal ions contained in the B-site ions include at least one selected from zirconium ions and titanium ions, can be prepared by a conventionally known method. The oxide having the perovskite structure can be prepared by, for example, a conventionally known solid phase method, liquid phase method, or the like. An example of the solid phase method is a method based on a direct reaction of solid raw materials. Examples of the liquid phase method include the Pezzini method, the complex polymerization method, and the hydrothermal synthesis method.

[0043] [Water electrolysis cell] The water electrolysis cell according to the present disclosure includes an anode gas diffusion layer, the anode catalyst according to the present disclosure described above, an electrolyte membrane, a cathode catalyst, a cathode gas diffusion layer, and a separator.

[0044] The anode catalyst of the present disclosure is as described above, and therefore description thereof will be omitted here. The anode gas diffusion layer, the electrolyte membrane, the cathode catalyst, the cathode gas diffusion layer and the separator may be made of materials used in conventionally known water electrolysis cells.

[0045] For example, the anode gas diffusion layer and the cathode gas diffusion layer may each independently be made of a material that allows fluid to flow within the layer, such as a porous material, a powder sintered material, a fiber sintered material, a metal mesh, or a felt.

[0046] The anode gas diffusion layer may be coated with a corrosion-resistant conductive material (so-called coating material) from the viewpoint of suppressing an increase in resistance due to oxidation. Examples of the coating material include platinum, gold, silver, titanium nitride, titanium carbide, and titanium carbonitride.

[0047] The electrolyte membrane may be selected from known electrolyte membranes (which may be ion exchange membranes) used in water electrolysis. The electrolyte membrane is a membrane that can exchange protons (H + ) is preferably selectively permeable. The electrolyte membrane may be, for example, a polymer electrolyte membrane (PEM). The polymer electrolyte membrane may be, for example, a perfluorocarbon membrane having a sulfonic acid group. The perfluorocarbon membrane having a sulfonic acid group may be, for example, a Nafion membrane.

[0048] The electrolyte membrane is a polymer having proton conductivity due to the presence of ionic groups. The electrolyte membrane may be, for example, a fluorine-based polymer electrolyte or a hydrocarbon-based polymer electrolyte.

[0049] Here, the fluorine-based polymer electrolyte means one in which most or all of the hydrogen atoms in the alkyl groups and / or alkylene groups in the polymer have been substituted with fluorine atoms. Representative examples of fluorine-based polymer electrolytes having ionic groups include commercially available products such as "Nafion" (registered trademark) (manufactured by Chemours), "Aquivion" (registered trademark) (manufactured by Solvay), "Flemion" (registered trademark) (manufactured by AGC Corporation), and "Aciplex" (registered trademark) (manufactured by Asahi Kasei Corporation).

[0050] The hydrocarbon electrolyte is preferably an aromatic hydrocarbon polymer having an aromatic ring in the main chain. Here, the aromatic ring may include not only a hydrocarbon aromatic ring consisting of only carbon atoms and hydrogen atoms such as a benzene ring or a naphthalene skeleton, but also a heterocycle such as a pyridine ring, an imidazole ring, or a thiol ring. In addition, a part of the polymer may be composed of an aliphatic unit together with the aromatic ring unit.

[0051] Specific examples of aromatic hydrocarbon polymers include polymers having a structure selected from the group consisting of polysulfone, polyethersulfone, polyphenylene oxide, polyarylene ether, polyphenylene sulfide, polyphenylene sulfide sulfone, polyparaphenylene, polyarylene, polyarylene ketone, polyether ketone, polyarylene phosphine oxide, polyether phosphine oxide, polybenzoxazole, polybenzothiazole, polybenzimidazole, polyamide, polyimide, polyetherimide, and polyimide sulfone in the main chain together with an aromatic ring. Note that polysulfone, polyethersulfone, polyether ketone, etc. referred to here are general terms for structures having sulfone bonds, ether bonds, ketone bonds, etc. in the molecular chain, and include polyether ketone ketone, polyether ether ketone, polyether ether ketone ketone, polyether ketone ether ketone ketone, polyether ketone sulfone, etc. The aromatic hydrocarbon polymer may have a plurality of these structures. As the aromatic hydrocarbon polymer, a polymer having a polyetherketone skeleton, that is, a polyetherketone polymer, is particularly preferred.

[0052] The electrolyte membrane may be combined with a reinforcing material. By using the reinforcing material, gas leakage and short circuits in the electrodes caused by the membrane being damaged are less likely to occur when the electrolyte membrane and the electrodes are joined by, for example, a hot press method.

[0053] Specific examples of reinforcing materials include homogeneous porous films made of fluorine-based polymers such as PTFE (polytetrafluoroethylene), PFA (tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer), PVDF (polyvinylidene fluoride), and FEP (tetrafluoroethylene-hexafluoropropylene copolymer); thermoplastic resins such as PE (polyethylene) and PP (polypropylene); and engineering plastics such as PI (polyimide), PSF (polysulfone), PES (polyethersulfone), PEEK (polyetheretherketone), PPSS (polyphenylene sulfide sulfone), PPO (polyphenylene oxide), PEK (polyetherketone), PBI (polybenzimidazole), PPS (polyphenylene sulfide), PPP (polyparaphenylene), PPQ (polyphenylquinoxaline), polybenzoxazole (PBO), polybenzothiazole (PBT), and polyparaphenylene terephthalamide (PPTA).

[0054] The cathode catalyst may be selected from known catalysts used in water electrolysis. Examples of catalyst components include platinum, gold, silver, palladium, iridium, rhodium, ruthenium, tin, iron, cobalt, nickel, molybdenum, tungsten, vanadium, alloys thereof, and oxides thereof. The cathode catalyst may include a catalyst supported on a carrier. Examples of the carrier include carbon black. The catalyst may be in the form of particles.

[0055] The water electrolysis cell may include an anode catalyst layer containing an anode catalyst (preferably anode catalyst particles) and an ionomer, or may include a cathode catalyst layer containing a cathode catalyst (preferably cathode catalyst particles) and an ionomer, which increases the contact area between the catalyst and the ionomer in the catalyst layer and tends to promote the reaction.

[0056] Examples of the separator include an anode separator disposed on the anode gas diffusion layer side, and a cathode separator disposed on the cathode gas diffusion layer side. Examples of the material for the separator include titanium, stainless steel, and carbon. The anode separator preferably contains titanium from the viewpoint of suppressing oxidation due to oxygen generated on the anode side. The anode separator may be coated with a corrosion-resistant conductive material (so-called coating material) to prevent the anode separator from becoming highly resistive due to oxidation. Examples of the coating material include platinum, gold, silver, titanium nitride, titanium carbide, and titanium carbonitride.

[0057] The water electrolysis cell may further include other components. The other components may be selected from known water electrolysis cell components. Other components include, for example, gaskets and seals.

[0058] The arrangement of each component in the water electrolysis cell may be determined with reference to known water electrolysis cells. In the water electrolysis cell, the electrolyte membrane is preferably located between the anode catalyst and the cathode catalyst. In the water electrolysis cell, the electrolyte membrane, the anode catalyst and the cathode catalyst are preferably located between the anode gas diffusion layer and the cathode gas diffusion layer. In the water electrolysis cell, the electrolyte membrane, the anode catalyst and the cathode catalyst, and the anode gas diffusion layer and the cathode gas diffusion layer are preferably located between two separators.

[0059] An example of a water electrolysis cell is shown in Fig. 1. Fig. 1 is a schematic cross-sectional view of a water electrolysis cell. As shown in Fig. 1, a water electrolysis cell 100 includes, in order from the top of Fig. 1, an anode separator 60, an anode gas diffusion layer 20, an anode catalyst 12, an electrolyte membrane 11, a cathode catalyst 13, a cathode gas diffusion layer 30, and a cathode separator 70. Furthermore, in the water electrolysis cell 100, a gasket 40 is disposed between the anode separator 60 and the electrolyte membrane 11, and a gasket 50 is disposed between the cathode separator 70 and the electrolyte membrane 11.

[0060] [Water electrolysis device] The water electrolysis device according to the present disclosure may be a water electrolysis cell stack formed by stacking a plurality of the above-described water electrolysis cells according to the present disclosure, or may be a device including the water electrolysis cell stack or the water electrolysis cell according to the present disclosure and other components.

[0061] The other components may be selected from known water electrolysis device components. Examples of other components include auxiliary equipment such as a power conditioner, a water pump, an ion exchange resin, a heat exchanger, and a dehumidifier. EXAMPLES

[0062] The present disclosure will be described in detail below with reference to examples. However, the present disclosure is not limited to the following examples. The matters shown in the following examples may be appropriately changed without departing from the spirit of the present disclosure.

[0063] <Example 1> Using the Pezzini method, a catalyst powder was produced that contains an oxide with a perovskite structure, in which the A-site ions include a combination of alkaline earth metal ions, calcium ions and barium ions, and the B-site ions include iridium ions and tetravalent metal ions, zirconium ions. The starting materials were barium carbonate (BaCO3), calcium carbonate (CaCO3), zirconium oxide chloride octahydrate (ZrOCl2·8H2O), and potassium hexachloroiridate (K2IrCl6). 0.9869g of BaCO3, 0.0556g of CaCO3, 0.1917g of ZrOCl2·8H2O, 0.1920g of K2IrCl6, 4.708g of citric acid monohydrate (C6H8O7·H2O), 2mL of nitric acid (1.38), and 8mL of ethylene glycol (C2H6O2) were weighed and added to 20mL of pure water, mixed, and then stirred at room temperature ("20°C"; the same applies below) for 15 minutes or more to dissolve. The resulting mixed solution was stirred and mixed at 75°C for 3 hours or more using a hot stirrer. The resulting mixed solution was then transferred to a zirconia crucible and heat-treated at 180°C for 12 hours, 200°C for 6 hours, 300°C for 6 hours, 500°C for 3 hours, 600°C for 6 hours, and 700°C for 6 hours. The powder obtained by the heat treatment was then collected and placed in a beaker containing 50 mL of 1M aqueous hydrochloric acid solution, and stirred for 3 hours or more to remove unreacted components. The mixed solution from which the unreacted components had been removed was then washed with water using a suction filter, and then dried in an oven at 60°C to obtain a catalyst powder. When the obtained catalyst powder was subjected to X-ray diffraction measurement, a diffraction pattern derived from a perovskite structure was obtained. The resulting catalyst powder was analyzed for its constituent elements using an energy dispersive X-ray analyzer attached to a field emission scanning electron microscope. Specifically, the catalyst powder was applied to a carbon tape, and mapping analysis was carried out on three image areas at a magnification of 10,000 times, and the average element concentration of the constituent elements in each image was evaluated. As a result, the molar concentration of iridium ions in the B site was 40 mol%, and the molar concentration of barium ions in the A site (m Ba ) is 90 mol%, and the molar concentration of calcium ions at the A site (m Ca ) was 10 mol%. From the above, it was confirmed that the obtained catalyst was Ba, an oxide having a perovskite structure. 0.9 Ca 0.1 Zr 0.6 Ir 0.4 It was confirmed that it contains O3. The ionic radius of the calcium ion at the A site (r ca ) is 1.34 Å, and the ionic radius of the A-site barium ion (r Ba ) is 1.61 Å. Ionic radius of A-site ions (average ionic radius on a molar basis, r A ) is 1.5830 Å, and the ionic radius difference between the A-site ions and calcium ions (r A -r Ca ) was 0.2430 Å.

[0064] <Example 2> In Example 2, the same procedure as in Example 1 was carried out except that the amount of BaCO3 used was changed to 0.8224 g and the amount of CaCO3 used was changed to 0.1390 ​​g, to obtain a catalyst powder. When the obtained catalyst powder was subjected to X-ray diffraction measurement, a diffraction pattern derived from the perovskite structure was obtained. Furthermore, when the obtained catalyst powder was analyzed in the same manner as in Example 1, the molar concentration of the iridium ions in the B site was 40 mol %, and the molar concentration of the barium ions in the A site (m Ba ) is 75 mol% and the molar concentration of calcium ions at the A site (m Ca ) was 25 mol%. From the above, it was confirmed that the obtained catalyst was Ba, an oxide having a perovskite structure. 0.75 Ca 0.25 Zr 0.6 Ir 0.4 It was confirmed that it contains O3. The ionic radius of the A-site ions (average ionic radius on a molar basis, r A ) and the ionic radius difference between the A site ion and calcium ion (r A -r Ca ) were as shown in Table 1.

[0065] <Example 3> In Example 3, the same procedure as in Example 1 was carried out except that the amount of BaCO3 used was changed to 0.1097 g and the amount of CaCO3 used was changed to 0.5005 g, to obtain a catalyst powder. When the obtained catalyst powder was subjected to X-ray diffraction measurement, a diffraction pattern derived from the perovskite structure was obtained. Furthermore, when the obtained catalyst powder was analyzed in the same manner as in Example 1, the molar concentration of the iridium ions in the B site was 40 mol %, and the molar concentration of the barium ions in the A site (m Ba ) is 10 mol% and the molar concentration of calcium ions at the A site (m Ca ) was 90 mol%. From the above, it was confirmed that the obtained catalyst was Ba, an oxide having a perovskite structure. 0.1 Ca 0.9 Zr 0.6 Ir 0.4 It was confirmed that it contains O3. The ionic radius of the A-site ions (average ionic radius on a molar basis, r A ) and the ionic radius difference between the A site ion and calcium ion (r A -r Ca ) were as shown in Table 1.

[0066] <Example 4> In Example 4, the starting material was changed from BaCO3 to SrCO3 in an amount of 0.7383 g, and the amount of CaCO3 was changed to 0.0556 g, but the same procedure as in Example 1 was carried out to obtain a catalyst powder. When the obtained catalyst powder was subjected to X-ray diffraction measurement, a diffraction pattern derived from the perovskite structure was obtained. Furthermore, when the obtained catalyst powder was analyzed in the same manner as in Example 1, the molar concentration of iridium ions in the B site was 40 mol %, and the molar concentration of strontium ions in the A site (m Ba ) is 90 mol%, and the molar concentration of calcium ions at the A site (m Ca ) was 10 mol%. From the above, it was confirmed that the obtained catalyst was a Sr oxide having a perovskite structure. 0.9 Ca 0.1 Zr 0.6 Ir 0.4 It was confirmed that it contains O3. The ionic radius (r Sr ) is 1.44 Å. The ionic radius of the A-site ions (average ionic radius on a molar basis, r A ) and the ionic radius difference between the A site ion and calcium ion (r A -r Ca ) were as shown in Table 1.

[0067] <Example 5> In Example 5, the same procedure as in Example 4 was carried out except that the amount of SrCO3 used was changed to 0.6153 g and the amount of CaCO3 used was changed to 0.1391 g, to obtain a catalyst powder. When the obtained catalyst powder was subjected to X-ray diffraction measurement, a diffraction pattern derived from the perovskite structure was obtained. Furthermore, when the obtained catalyst powder was analyzed in the same manner as in Example 1, the molar concentration of iridium ions in the B site was 40 mol %, and the molar concentration of strontium ions in the A site (m Ba ) is 75 mol%, and the molar concentration of calcium ions at the A site (m Ca ) was 25 mol%. From the above, it was confirmed that the obtained catalyst was a Sr oxide having a perovskite structure. 0.75 Ca 0.25 Zr 0.6 Ir 0.4 It was confirmed that it contains O3. The ionic radius of the A-site ions (average ionic radius on a molar basis, r A ) and the ionic radius difference between the A site ion and calcium ion (r A -r Ca ) were as shown in Table 1.

[0068] <Example 6> In Example 6, the same procedure as in Example 4 was carried out except that the amount of SrCO3 used was changed to 0.4102 g and the amount of CaCO3 used was changed to 0.2781 g, to obtain a catalyst powder. When the obtained catalyst powder was subjected to X-ray diffraction measurement, a diffraction pattern derived from the perovskite structure was obtained. Furthermore, when the obtained catalyst powder was analyzed in the same manner as in Example 1, the molar concentration of iridium ions in the B site was 40 mol %, and the molar concentration of strontium ions in the A site (m Ba ) is 50 mol%, and the molar concentration of calcium ions at the A site (m Ca ) was 50 mol%. From the above, it was confirmed that the obtained catalyst was a Sr oxide having a perovskite structure. 0.5 Ca 0.5 Zr 0.6 Ir 0.4 It was confirmed that it contains O3. The ionic radius of the A-site ions (average ionic radius on a molar basis, r A ) and the ionic radius difference between the A site ion and calcium ion (r A -r Ca ) were as shown in Table 1.

[0069] <Example 7> In Example 7, the same procedure as in Example 4 was carried out except that the amount of SrCO3 used was changed to 0.2051 g and the amount of CaCO3 used was changed to 0.4172 g, to obtain a catalyst powder. When the obtained catalyst powder was subjected to X-ray diffraction measurement, a diffraction pattern derived from the perovskite structure was obtained. Furthermore, when the obtained catalyst powder was analyzed in the same manner as in Example 1, the molar concentration of iridium ions in the B site was 40 mol %, and the molar concentration of strontium ions in the A site (m Ba ) is 25 mol%, and the molar concentration of calcium ions at the A site (m Ca ) was 75 mol%. From the above, it was confirmed that the obtained catalyst was a Sr oxide having a perovskite structure. 0.25 Ca 0.75 Zr 0.6 Ir 0.4 It was confirmed that it contains O3. The ionic radius of the A-site ions (average ionic radius on a molar basis, r A) and the ionic radius difference between the A site ion and calcium ion (r A -r Ca ) were as shown in Table 1.

[0070] <Example 8> In Example 8, the same procedure as in Example 1 was carried out except that the amount of BaCO3 used was changed to 0.4174 g, the amount of CaCO3 used was changed to 0.2743 g, and the amount of ZrOCl2·8H2O used was changed to 0.0626 g, to obtain a catalyst powder. When the obtained catalyst powder was subjected to X-ray diffraction measurement, a diffraction pattern derived from the perovskite structure was obtained. Furthermore, when the obtained catalyst powder was analyzed in the same manner as in Example 1, the molar concentration of iridium ions in the B site was 67 mol %, and the molar concentration of barium ions in the A site (m Ba ) is 25 mol% and the molar concentration of calcium ions at the A site (m Ca ) was 75 mol%. From the above, it was confirmed that the obtained catalyst was Ba, an oxide having a perovskite structure. 0.25 Ca 0.75 Zr 0.33 Ir 0.67 It was confirmed that it contains O3. The ionic radius of the A-site ions (average ionic radius on a molar basis, r A ) and the ionic radius difference between the A site ion and calcium ion (r A -r Ca ) were as shown in Table 1.

[0071] <Example 9> In Example 9, a catalyst powder was produced by the Pezzini method, which contains an oxide having a perovskite structure, in which the A-site ions include a combination of alkaline earth metal ions, calcium ions and strontium ions, and the B-site ions include an iridium ion and a tetravalent metal ion, titanium ion. The starting materials were SrCO3, CaCO3, K2IrCl6, and tetrabutoxytitanium (C 16 H 36O4Ti). 0.0474g of SrCO3, 0.2095g of CaCO3, 0.08g of K2IrCl6, 0.28g of C6H8O7·H2O, and 0.3mL of nitric acid (1.38) were weighed out and added to 10mL of pure water, mixed, and then stirred at room temperature for 15 minutes or more to dissolve. The resulting mixed solution was named solution A. C 16 H 36 0.1047g of O4Ti was weighed out and put into 4mL of C2H6O2, and then stirred for 15 minutes or more to dissolve. The resulting mixed solution was designated as solution B. After putting solution A into solution B, it was stirred and mixed at 70°C for 3 hours or more using a hot stirrer. Next, the resulting mixed solution was transferred to a zirconia crucible and heat-treated at 180°C for 12 hours, 200°C for 6 hours, 300°C for 6 hours, 500°C for 3 hours, and 600°C for 6 hours. Next, the powder obtained by the heat treatment was collected and put into a beaker containing 50mL of a 1M aqueous hydrochloric acid solution, and then stirred for 3 hours or more to remove unreacted components. Next, the mixed solution from which the unreacted components had been removed was washed with water using a suction filter, and then dried in an oven at 60°C to obtain a catalyst powder. When the obtained catalyst powder was subjected to X-ray diffraction measurement, a diffraction pattern derived from the perovskite structure was obtained. Furthermore, when the obtained catalyst powder was analyzed in the same manner as in Example 1, the molar concentration of iridium ions in the B site was 35 mol %, and the molar concentration of strontium ions in the A site (m Ba ) is 75 mol%, and the molar concentration of calcium ions at the A site (m Ca ) was 25 mol%. From the above, it was confirmed that the obtained catalyst was a Sr oxide having a perovskite structure. 0.75 Ca 0.25 Ti 0.65 Ir 0.35 It was confirmed that it contains O3. The ionic radius of the A-site ions (average ionic radius on a molar basis, r A ) and the ionic radius difference between the A site ion and calcium ion (r A -r Ca ) were as shown in Table 1.

[0072] <Comparative Example 1> In Comparative Example 1, the same procedure as in Example 1 was carried out, except that BaCO3 was not used as the starting material, and the amount of CaCO3 used was changed to 0.5562 g, to obtain a catalyst powder. When the obtained catalyst powder was subjected to X-ray diffraction measurement, a diffraction pattern derived from the perovskite structure was obtained. Furthermore, when the obtained catalyst powder was analyzed in the same manner as in Example 1, the molar concentration of iridium ions in the B site was 40 mol %, and the molar concentration of calcium ions in the A site (m Ca ) was 100 mol%. From the above, it was confirmed that the obtained catalyst was a CaZr oxide having a perovskite structure. 0.6 Ir 0.4 It was confirmed that it contains O3. The ionic radius of the A-site ions (average ionic radius on a molar basis, r A ) and the ionic radius difference between the A site ion and calcium ion (r A -r Ca ) were as shown in Table 1.

[0073] <Comparative Example 2> In Comparative Example 2, the same operation as in Example 1 was carried out except that the amount of BaCO3 used was changed to 0.0110 g and the amount of CaCO3 used was changed to 0.5506 g, to obtain a catalyst powder. When the obtained catalyst powder was subjected to X-ray diffraction measurement, a diffraction pattern derived from the perovskite structure was obtained. Furthermore, when the obtained catalyst powder was analyzed in the same manner as in Example 1, the molar concentration of the iridium ions in the B site was 40 mol %, and the molar concentration of the barium ions in the A site (m Ba ) is the molar concentration of calcium ions at the A site (m Ca ) was 99 mol%. From the above, it was confirmed that the obtained catalyst was Ba, an oxide having a perovskite structure. 0.01 Ca 0.99 Zr 0.6 Ir 0.4 It was confirmed that it contains O3. The ionic radius of the A-site ions (average ionic radius on a molar basis, r A ) and the ionic radius difference between the A site ion and calcium ion (r A -r Ca ) were as shown in Table 1.

[0074] <Comparative Example 3> In Comparative Example 3, the same operation as in Example 4 was carried out except that the amount of SrCO3 used was changed to 0.0082 g and the amount of CaCO3 used was changed to 0.5506 g, to obtain a catalyst powder. When the obtained catalyst powder was subjected to X-ray diffraction measurement, a diffraction pattern derived from the perovskite structure was obtained. Furthermore, when the obtained catalyst powder was analyzed in the same manner as in Example 1, the molar concentration of iridium ions in the B site was 40 mol %, and the molar concentration of strontium ions in the A site (m Ba ) is 1 mol%, and the molar concentration of calcium ions at the A site (m Ca ) was 99 mol%. From the above, it was confirmed that the obtained catalyst was a Sr oxide having a perovskite structure. 0.01 Ca 0.99 Zr 0.6 Ir 0.4 It was confirmed that it contains O3. The ionic radius of the A-site ions (average ionic radius on a molar basis, r A ) and the ionic radius difference between the A site ion and calcium ion (r A -r Ca ) were as shown in Table 1.

[0075] <Comparative Example 4> In Comparative Example 4, the same procedure as in Comparative Example 1 was carried out except that the amount of CaCO3 used was changed to 0.5560 g and the amount of ZrOCl2·8H2O used was changed to 0.5120 g, to obtain a catalyst powder. When the obtained catalyst powder was subjected to X-ray diffraction measurement, a diffraction pattern derived from the perovskite structure was obtained. Furthermore, when the obtained catalyst powder was analyzed in the same manner as in Example 1, the molar concentration of iridium ions in the B site was 20 mol %, and the molar concentration of calcium ions in the A site (m Ca ) was 100 mol%. From the above, it was confirmed that the obtained catalyst was a CaZr oxide having a perovskite structure. 0.8 Ir 0.2 It was confirmed that it contains O3. The ionic radius of the A-site ions (average ionic radius on a molar basis, r A ) and the ionic radius difference between the A site ion and calcium ion (r A -r Ca ) were as shown in Table 1.

[0076] <Comparative Example 5> In Comparative Example 5, the same procedure as in Example 1 was carried out except that the amount of BaCO3 used was changed to 0.8230 g, the amount of CaCO3 used was changed to 0.1391 g, and the amount of ZrOCl2·8H2O used was changed to 0.5120 g, to obtain a catalyst powder. When the obtained catalyst powder was subjected to X-ray diffraction measurement, a diffraction pattern derived from the perovskite structure was obtained. Furthermore, when the obtained catalyst powder was analyzed in the same manner as in Example 1, the molar concentration of the iridium ions in the B site was 20 mol %, and the molar concentration of the barium ions in the A site (m Ba ) is 75 mol%, and the molar concentration of calcium ions at the A site (m Ca ) was 25 mol%. From the above, it was confirmed that the obtained catalyst was Ba, an oxide having a perovskite structure. 0.75 Ca 0.25 Zr 0.8 Ir 0.2 It was confirmed that it contains O3. The ionic radius of the A-site ions (average ionic radius on a molar basis, r A ) and the ionic radius difference between the A site ion and calcium ion (r A -r Ca) were as shown in Table 1.

[0077] <Comparative Example 6> In Comparative Example 6, the same procedure as in Comparative Example 5 was carried out except that the amount of BaCO3 used was changed to 0.5487 g and the amount of CaCO3 used was changed to 0.2783 g, to obtain a catalyst powder. When the obtained catalyst powder was subjected to X-ray diffraction measurement, a diffraction pattern derived from the perovskite structure was obtained. Furthermore, when the obtained catalyst powder was analyzed in the same manner as in Example 1, the molar concentration of the iridium ions in the B site was 20 mol %, and the molar concentration of the barium ions in the A site (m Ba ) is 50 mol% and the molar concentration of calcium ions at the A site (m Ca ) was 50 mol%. From the above, it was confirmed that the obtained catalyst was Ba, an oxide having a perovskite structure. 0.5 Ca 0.5 Zr 0.8 Ir 0.2 It was confirmed that it contains O3. The ionic radius of the A-site ions (average ionic radius on a molar basis, r A ) and the ionic radius difference between the A site ion and calcium ion (r A -r Ca ) were as shown in Table 1.

[0078] <Comparative Example 7> In Comparative Example 7, the same procedure as in Comparative Example 5 was carried out except that the amount of BaCO3 used was changed to 0.2744 g and the amount of CaCO3 used was changed to 0.4175 g, to obtain a catalyst powder. When the obtained catalyst powder was subjected to X-ray diffraction measurement, a diffraction pattern derived from the perovskite structure was obtained. Furthermore, when the obtained catalyst powder was analyzed in the same manner as in Example 1, the molar concentration of the iridium ions in the B site was 20 mol %, and the molar concentration of the barium ions in the A site (m Ba ) is 25 mol% and the molar concentration of calcium ions at the A site (m Ca) was 75 mol%. From the above, it was confirmed that the obtained catalyst was Ba, an oxide having a perovskite structure. 0.25 Ca 0.75 Zr 0.8 Ir 0.2 It was confirmed that it contains O3. The ionic radius of the A-site ions (average ionic radius on a molar basis, r A ) and the ionic radius difference between the A site ion and calcium ion (r A -r Ca ) were as shown in Table 1.

[0079] <Comparative Example 8> In Comparative Example 8, the same procedure as in Comparative Example 5 was carried out except that CaCO3 was not used as the starting material and the amount of BaCO3 used was changed to 1.0973 g, to obtain a catalyst powder. When the obtained catalyst powder was subjected to X-ray diffraction measurement, a diffraction pattern derived from the perovskite structure was obtained. Furthermore, when the obtained catalyst powder was analyzed in the same manner as in Example 1, the molar concentration of iridium ions in the B site was 20 mol %, and the molar concentration of calcium ions in the A site (m Ca ) was 0 mol%. From the above, it was confirmed that the obtained catalyst was BaZr 0.8 Ir 0.2 It was confirmed that it contains O3. The ionic radius of the A-site ions (average ionic radius on a molar basis, r A ) and the ionic radius difference between the A site ion and calcium ion (r A -r Ca ) were as shown in Table 1.

[0080] <Comparative Example 9> Commercially available ruthenium dioxide (RuO2) with a rutile structure was used.

[0081] [evaluation] The catalyst powders containing an oxide having a perovskite structure obtained in Examples 1 to 9, the catalyst powders containing an oxide having a perovskite structure obtained in Comparative Examples 1 to 8, and the catalyst powder containing an oxide having a rutile structure of Comparative Example 9 were each used as an anode catalyst, and the following evaluations were performed.

[0082] 1. Current density measurement The relationship between the current density and the voltage of the catalyst was evaluated at room temperature by the rotating disk electrode method. 10 mg of catalyst powder, 0.1 mL of 5 mass% Nafion dispersion solution, 0.4 mL of 2-propanol, and 1.5 mL of pure water were weighed and transferred to a glass container, and mixed for 30 minutes or more using a homogenizer. 10 μL of the resulting mixed solution was taken out and applied to a glassy carbon electrode with a diameter of 5 mm. After drying, it was set using a rotating disk electrode device to form a working electrode. A platinum wire was used as the counter electrode, and an aqueous Ag / AgCl reference electrode was used as the reference electrode. These and the working electrode were placed in a beaker containing 0.5 M sulfuric acid aqueous solution. After holding the circuit open for 10 minutes or more, cyclic voltammetry measurements were performed for 10 cycles at room temperature in the range of 0.05 V to 1.4 V based on the reversible hydrogen electrode (RHE), at a sweep speed of 100 mV / sec, and at a rotation speed of 1,600 rpm (revolution per minute; the same applies below), and electrochemical cleaning of the catalyst surface was performed. Then, 30 cycles of cyclic voltammetry measurements were performed under conditions of a range of 1.2 V to 1.6 V on the RHE basis, a sweep rate of 5 mV / s, and a rotation rate of 1,600 rpm, and the current at 1.6 V in the first cycle and the 30th cycle was measured. The current value was divided by the area of ​​the glassy carbon electrode to obtain the current density (unit: mA / cm 2 The measurement results of the current density in the first cycle and the current density in the 30th cycle are shown in Table 1. The current density in the 30th cycle and the ion radius difference (r A -r Ca ) is shown in Figure 2.

[0083] 2. Current density maintenance rate Based on the current density in the first cycle and the current density in the 30th cycle measured above, the current density retention rate (unit: %) was calculated. The results are shown in Table 1.

[0084] [Table 1]

[0085] As shown in Table 1, the current density retention rate was higher in Examples 1 to 9 compared to Comparative Examples 1 to 8. This shows that the catalysts containing an oxide having a perovskite structure shown in Examples 1 to 9 have a longer life than the catalysts containing an oxide having a perovskite structure shown in Comparative Examples 1 to 8. Furthermore, it was found that the catalysts containing an oxide having a perovskite structure shown in Examples 1 to 9 have a higher current density at the 30th cycle and maintain excellent catalytic activity compared to the catalysts containing an oxide having a perovskite structure shown in Comparative Examples 1 to 8. In Comparative Example 9, the current density was significantly inferior to that of Comparative Examples 1 to 8. The reason for this is believed to be that the rutile structure is unstable at a high potential of 1.6 V based on the RHE standard, and therefore the catalyst components are dissolved and deactivated.

[0086] FIG. 2 shows the ionic radius difference (r A -r Ca 2 is a graph showing the relationship between the ionic radius of the A-site ion and the calcium ion and the current density. As shown in Figure 2, it was found that a high current density tends to be obtained by adjusting the difference in ionic radius between the A-site ion and the calcium ion within an appropriate range. According to Examples 1 to 9, the ionic radius difference between the A site ion and the calcium ion (r A -r Ca The relationship between the current density and the approximation Y=-1559.1X 2 +435.22X+22.9, for example, if the current density is 30mA / cm 2 More than 40mA / cm 2 At threshold 1, which is less than A -r Ca) is 0.0175 Å to 0.2616 Å, and the current density is 40 mA / cm 2 More than 45mA / cm 2 At threshold 2, which is less than A -r Ca ) is 0.0474 Å to 0.2316 Å, and the current density is 45 mA / cm 2 At threshold 3, where the ion radius difference (r A -r Ca The ionic radius difference (r A -r Ca It was found that a high current density can be obtained by gradually narrowing the numerical range of . The feature of the anode catalyst becoming highly efficient by adjusting the ionic radius difference is unique to catalysts with a perovskite structure that contains metal ions with different valences at the A site and B site.

[0087] In addition, when the alkaline earth metal ions contained in the A site ions are a combination of calcium ions and strontium ions, the ionic radius difference between the A site ions and calcium ions (r A -r Ca The relationship between the current density and the approximation Y=-7006X 2 +844.08X+22.9, for example, if the current density is 30mA / cm 2 More than 40mA / cm 2 At threshold 1, which is less than A -r Ca ) is 0.0091 Å to 0.1113 Å, and the current density is 40 mA / cm 2 More than 45mA / cm 2 At threshold 2, which is less than A -r Ca ) is 0.0258 Å to 0.0947 Å, and the current density is 45 mA / cm 2 At threshold 3, where the ion radius difference (r A -r Ca ) was 0.0385 Å to 0.0820 Å. In addition, when the alkaline earth metal ions contained in the A site ions are a combination of calcium ions and barium ions, the ionic radius difference between the A site ions and the calcium ions (r A -r Ca The relationship between the current density and the approximation Y=-1532.2X 2 +431.2X+22.9, for example, if the current density is 30mA / cm 2 More than 40mA / cm 2 At threshold 1, which is less than A -r Ca ) is 0.0176 Å to 0.2639 Å, and the current density is 40 mA / cm 2 More than 45mA / cm 2 At threshold 2, which is less than A -r Ca ) is 0.0478 Å to 0.2336 Å, and the current density is 45 mA / cm 2 At threshold 3, where the ion radius difference (r A -r Ca ) was 0.0674 Å to 0.2140 Å. [Explanation of symbols]

[0088] 11: Electrolyte membrane 12: Anode catalyst 13: Cathode catalyst 20: Anode gas diffusion layer 30: Cathode gas diffusion layer 40: Gasket 50: Gasket 60: Anode separator 70: Cathode separator 100: Water electrolysis cell

Claims

1. The oxide has a perovskite structure and contains alkaline earth metal ions as A-site ions and tetravalent metal ions and iridium ions as B-site ions; the alkaline earth metal ions contained in the A site ions include a combination of calcium ions and strontium ions, a combination of calcium ions and barium ions, or a combination of calcium ions, strontium ions, and barium ions; the tetravalent metal ion contained in the B site ion includes at least one selected from a zirconium ion and a titanium ion, the molar concentration of the iridium ions contained in the B site ions is 35 mol % or more; The ionic radius of the A site ion is r A , and the ionic radius of the alkaline earth metal ion contained in the A site ion is r i , the molar concentration of the alkaline earth metal ion is m i , and the ionic radius of the calcium ion is r ca In this case, the ionic radius difference (r A -r Ca ) is 0.0175 Å to 0.2616 Å. [0010]

2. The ionic radius difference (r A -r Ca 2. The anode catalyst according to claim 1, wherein the surface area of ​​the anode is 0.0474 Å to 0.2316 Å.

3. The ionic radius difference (r A -r Ca 2. The anode catalyst according to claim 1, wherein the thickness of the first anode electrode is 0.0668 Å to 0.2122 Å.

4. A water electrolysis cell comprising: an anode gas diffusion layer; the anode catalyst according to any one of claims 1 to 3; an electrolyte membrane; a cathode catalyst; a cathode gas diffusion layer; and a separator.

5. A water electrolysis cell stack comprising a plurality of water electrolysis cells according to claim 4 stacked together.

Citation Information

Patent Citations

  • Pd-Ru SOLID SOLUTION NANOPARTICLES, PRODUCTION METHOD AND CATALYST THEREFOR, METHOD FOR CONTROLLING CRYSTAL STRUCTURE OF Pt-Ru SOLID SOLUTION NANOPARTICLES, Au-Ru SOLID SOLUTION NANOPARTICLES, AND METHOD FOR MANUFACTURING SAME

    WO2018159644A1