Method for manufacturing zircon-cast product and zircon-cast product

Optimizing zircon particle size distribution and adding alumina cement in zircon-based refractories addresses structure separation and cracking issues, producing a zircon cast product with enhanced mechanical properties.

JP2024148501AActive Publication Date: 2024-10-18YOTAI REFRACTORIES
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2023061684
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-05
Publication Date
2024-10-18
Estimated Expiration
2043-04-05

AI Technical Summary

Technical Problem

Existing zircon-based monolithic refractories face issues with structure separation and cracking during molding and drying due to differences in specific gravity, particularly in large or irregularly shaped products.

Method used

A method involving precise optimization of zircon particle size distribution, using 20 to 40% by mass of 1 to 5 mm particles, 25 to 45% by mass of 0.1 to 1 mm particles, 25 to 40% by mass of 0.1 mm or less particles, and 5 to 10% by mass of 10 μm or less particles, along with 2 to 3% by mass of alumina cement or hydraulic alumina, to enhance fluidity and strength, preventing structure separation and cracking.

Benefits of technology

The method effectively suppresses structure separation and cracking during drying, resulting in a zircon cast product with high mechanical properties and reliability, achieving compressive strengths of 140 MPa or more.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024148501000001
    Figure 2024148501000001
Patent Text Reader

Abstract

To provide: a method for manufacturing a zircon-cast product, capable of molding without separating the structure of the zircon-cast product, and capable of effectively inhibiting cracking that occurs during drying; and the zircon-cast product in which the separation of the structure and the occurrence of cracking are inhibited.SOLUTION: A method for manufacturing a zircon-cast product includes a casting step of casting a zircon-cast material, which is mainly composed of zircon, to obtain the zircon-cast product. The zircon-cast material contains: 20 to 40 mass% of zircon particles having a particle diameter of 1 to 5 mm; 25 to 45 mass% of zircon particles having a particle diameter of 0.1 to 1 mm; and 25 to 40 mass% of zircon particles having a particle diameter of 0.1 mm or less. A content of zircon particles having a particle diameter of 10 μm or less is 5 to 10 mass%.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a zircon casting that can be used in various furnaces and a method for producing the same. [Background technology]

[0002] Zircon refractories are used in steelmaking, glass manufacturing, etc., and are produced, for example, by firing zircon castings under appropriate conditions. By using the casting method, it is also possible to obtain large zircon refractories and irregularly shaped zircon refractories that are difficult to press mold.

[0003] For example, Patent Document 1 (JP Patent Publication No. 06-157150) proposes a zircon-based amorphous refractory for pouring, which is made by adding 0.2 to 2.0 weight percent of silica sol, calculated as SiO2, and 0.005 to 1.0 weight percent of light-burned magnesia to 100 weight percent of a refractory mixture whose main aggregate is zircon raw material.

[0004] In the zircon-based monolithic refractory for pouring described in the above Patent Document 1, the addition of light-burned magnesia as a hardening agent enables room temperature hardening, and it is said that components such as Al2O3, CaO, MgO, and Na2O, which easily react with zircon components, can be reduced as much as possible from the joints, thereby improving hot strength. In addition, it is said that by imparting appropriate fluidity and hardening properties, it is possible to suppress the deterioration of corrosion resistance due to the decrease in hot strength.

[0005] In addition, Patent Document 2 (JP Patent Publication 55-116680 A) proposes a slag-added zircon-based monolithic refractory in which 0.3 to 5 percent by weight of converter slag is added to a zircon-based monolithic refractory containing 40 to 90 percent by weight of zircon.

[0006] In the slag-added zircon-based monolithic refractory described in Patent Document 2 mentioned above, it is said that by adding converter slag to the zircon-based monolithic refractory, the adhesion and sintering properties are improved, and physical properties such as bending strength and compressive strength can be improved. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Japanese Patent Application Publication No. 06-157150 [Patent Document 2] Japanese Patent Application Publication No. 55-116680 Summary of the Invention [Problem to be solved by the invention]

[0008] However, in the pourable zircon-based monolithic refractory described in Patent Document 1 above and the slag-added zircon-based monolithic refractory described in Patent Document 2 above, no consideration is given to the separation of the structure during molding or the occurrence of cracks during drying, nor is casting of these refractory raw materials considered.

[0009] Because zircon has a high specific gravity, it is extremely difficult to cast raw materials containing 25% or more by mass of zircon, and a serious problem has been that the difference in specific gravity during casting causes the raw material to separate into upper and lower parts, resulting in the formation of different structures. This problem is particularly pronounced for large or irregularly shaped products that are difficult to press mold. In other words, the reality is that there is no manufacturing method for zircon castings that can be molded without structure separation and that can effectively prevent cracks that occur during drying, and no zircon castings that prevent structure separation and cracks.

[0010] In view of the problems in the prior art as described above, an object of the present invention is to provide a method for producing a zircon casting which can be molded without causing structural separation and which can effectively suppress cracks that occur during drying, and to provide a zircon casting in which structural separation and cracks are suppressed. [Means for solving the problem]

[0011] In order to achieve the above object, the present inventors have conducted extensive research into the composition of zircon-based casting raw materials, and have discovered that it is extremely important to precisely optimize the grain size composition of the zircon raw material, thereby arriving at the present invention.

[0012] That is, the present invention provides: A casting process is provided for casting a zircon-based casting material containing zircon as a main component to obtain a zircon-based casting product, The zircon casting raw material contains 20 to 40 mass% of zircon particles having a particle diameter of 1 to 5 mm, 25 to 45 mass% of zircon particles having a particle diameter of 0.1 to 1 mm, and 25 to 40 mass% of zircon particles having a particle diameter of 0.1 mm or less, The content of zircon particles having a particle size of 10 μm or less is 5 to 10 mass %. The present invention provides a method for producing a zircon casting, comprising the steps of:

[0013] By including 20-40% by mass of zircon particles with a particle size of 1-5 mm, 25-45% by mass of zircon particles with a particle size of 0.1-1 mm, and 25-40% by mass of zircon particles with a particle size of 0.1 mm or less, the amount of added water and the amount of fine powder are optimized, and it is possible to suppress separation of the structure and cracks during drying. In addition, by including 5-10% by mass of zircon particles with a particle size of 10 μm or less, the fluidity is improved, and it is possible to reduce water and achieve dense packing, thereby imparting high strength while suppressing separation of the structure.

[0014] In the method for producing a zircon-based casting of the present invention, it is preferable to add alumina cement and / or hydraulic alumina to the zircon-based casting raw material so that the total content of the alumina cement and / or hydraulic alumina is 2 to 3 mass %. By adding 2 to 3 mass % of alumina cement and / or hydraulic alumina, it is possible to impart even higher strength to a fired zircon-based casting obtained by firing the zircon-based casting.

[0015] The present invention also provides a method for producing a semiconductor device comprising the steps of: The zircon particles have a particle size of 1 to 5 mm in an amount of 20 to 40 mass%, the zircon particles have a particle size of 0.1 to 1 mm in an amount of 25 to 45 mass%, and the zircon particles have a particle size of 0.1 mm or less in an amount of 25 to 40 mass%, Contains 5 to 10 mass % of zircon particles having a particle size of 10 μm or less; Also provided is a zircon casting, characterized in that

[0016] The zircon casting of the present invention can be suitably obtained by the method for producing the zircon casting of the present invention, and although the zircon casting is mainly composed of zircon particles having a large specific gravity, the grain size composition of the zircon particles is precisely optimized, so that the occurrence of separation of the structure and cracks is extremely effectively suppressed. As a result, by firing the zircon casting of the present invention under appropriate firing conditions, a fired zircon casting having excellent mechanical properties and reliability can be obtained.

[0017] The zircon casting of the present invention preferably contains alumina cement and / or hydraulic alumina, and the total content of the alumina cement and / or hydraulic alumina is preferably 2 to 3 mass %. By adding 2 to 3 mass % of alumina cement and / or hydraulic alumina, it is possible to impart even higher strength to a fired zircon casting obtained by firing the zircon casting. Effect of the Invention

[0018] According to the present invention, it is possible to provide a method for producing a zircon casting that can be molded without causing structural separation and that can effectively suppress cracks that occur during drying, and a zircon casting in which structural separation and cracks are suppressed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] Representative embodiments of the method for producing a zircon casting and the zircon casting of the present invention will be described in detail below, but the present invention is not limited to these.

[0020] 1. Manufacturing method of zircon castings The method for producing a zircon casting of the present invention involves casting a zircon casting material containing zircon as a main component to obtain a zircon casting. The method for producing a zircon casting of the present invention will be described in detail below.

[0021] (1) Zircon casting material The zircon casting material used in the method for producing a zircon casting product of the present invention is most characterized in that the particle size and content of zircon particles are controlled.

[0022] (1-1) Main component (zircon particles) The zircon casting raw material contains 20-40 mass% zircon particles with a particle diameter of 1-5 mm, 25-45 mass% zircon particles with a particle diameter of 0.1-1 mm, and 25-40 mass% zircon particles with a particle diameter of 0.1 mm or less. The content of zircon particles with a particle diameter of 10 μm or less is 5-10 mass%. Note that zircon particles with a particle diameter of 10 μm or less are included in zircon particles with a particle diameter of 0.1 mm or less.

[0023] By including 20-40% by mass of zircon particles with a particle size of 1-5 mm, 25-45% by mass of zircon particles with a particle size of 0.1-1 mm, and 25-40% by mass of zircon particles with a particle size of 0.1 mm or less, the amount of added water and the amount of fine powder are optimized, and it is possible to suppress separation of the structure and cracks during drying. In addition, by including 5-10% by mass of zircon particles with a particle size of 10 μm or less, the fluidity is improved, and it is possible to densely pack the material while reducing water, and it is possible to impart high compressive strength while suppressing separation of the structure.

[0024] The content of zircon particles having a particle diameter of 1 to 5 mm is preferably 20 to 40 mass%, more preferably 25 to 35 mass%. The content of zircon particles having a particle diameter of 0.1 to 1 mm is preferably 25 to 45 mass%, more preferably 30 to 40 mass%. The content of zircon particles having a particle diameter of 0.1 mm or less is preferably 25 to 40 mass%, more preferably 30 to 40 mass%. The content of zircon particles having a particle diameter of 10 μm or less is preferably 8 to 10 mass%. If fine zircon particles having a particle diameter of 10 μm or less are added in an amount exceeding 10 mass%, the fine zircon particles may float up and cause separation.

[0025] The zircon particles may have any particle size and content within the specified range. The manufacturing method and particle shape of the zircon particles are not particularly limited as long as they do not impair the effects of the present invention, and various conventionally known zircon particles can be used.

[0026] For example, when it is difficult to obtain coarse zircon particles derived from natural minerals, zircon pellets having a particle size of 1 to 5 mm obtained by artificially crushing, granulating, firing, crushing, and classifying zircon sand may be used as coarse particles. For zircon particles having a particle size of 0.1 to 1 mm, crushed zircon pellets and / or crushed zircon brick waste can be used. For zircon particles having a particle size of 0.1 mm or less, zircon sand can be used, and for fine zircon particles having a particle size of 10 μm or less, zircon flower, zircon pax, etc. can be used.

[0027] (1-2) Optional additives Alumina cement and / or hydraulic alumina can be added as an optional additive component. The total content of alumina cement and / or hydraulic alumina is preferably 2 to 3 mass%. By adding 2 to 3 mass% of alumina cement and / or hydraulic alumina, it is possible to impart even higher strength to the zircon-based cast sintered product obtained by firing the zircon-based cast product. By making the total content 2 mass% or more, it is possible to achieve the effect of improving strength, and by making it 3 mass% or less, it is possible to suppress a decrease in the load-softening point of the zircon-based cast sintered product obtained by firing the zircon-based cast product.

[0028] In addition, alumina, alumina-silica, and silica may be used in combination as the zircon casting raw material. The particles used as the alumina, alumina-silica, and silica are not particularly limited as long as they do not impair the effects of the present invention, and various conventionally known particles may be used.

[0029] In addition, clay may be added as necessary. The amount of clay added may be adjusted as appropriate, but may be, for example, 0.5 to 1.5% by mass. By adding 0.5 to 1.5% by mass of clay, separation of tissues can be reduced.

[0030] (2) Casting process The zircon casting material described above can be cast into a desired mold to give it any desired shape, and after a drying process, the zircon casting of the present invention can be obtained.

[0031] In order to realize smooth casting during the casting process, it is preferable to adjust the fluidity of the zircon casting material by adding an appropriate amount of water. For example, by adding 3 to 8 mass% of water and kneading the raw materials, a good zircon casting material can be obtained. Note that the added water is later removed by drying, and is therefore not included in the components of the zircon casting of the present invention.

[0032] In addition, a dispersant may be added as necessary. The amount of dispersant added may be adjusted appropriately, and for example, 0.01 to 0.1% of dispersant may be added. The type of dispersant is not particularly limited as long as it does not impair the effects of the present invention, and various conventionally known dispersants may be used.

[0033] In the method for producing a zircon casting of the present invention, although the main component is zircon grains with a large specific gravity, the grain size composition of the zircon grains is precisely optimized, so that separation of the structure during the casting process can be extremely effectively suppressed.

[0034] (3) Drying process The zircon casting of the present invention can be obtained by drying the zircon casting formed in the casting process to remove water. Since the separation of the structure during the casting process is suppressed, the occurrence of cracks during the drying process can also be suppressed very effectively.

[0035] The drying conditions are not particularly limited as long as they do not impair the effects of the present invention, and may be appropriately adjusted depending on the composition, shape, size, etc. of the zircon casting. For example, the casting may be cured at 50°C for one day, removed from the frame, and then dried at 70°C for one day, at 140°C for two days, and at 180°C for two days.

[0036] By firing the zircon casting of the present invention under appropriate conditions, it is possible to obtain a fired zircon casting which not only has a homogeneous structure but also is free of defects such as cracks and exhibits high compressive strength.

[0037] 2. Zircon castings The zircon casting of the present invention is obtained by the method for producing a zircon casting of the present invention.

[0038] The main components and optional added components of the zircon casting are as described above, but by containing 20 to 40 mass% zircon particles with a particle size of 1 to 5 mm, 25 to 45 mass% zircon particles with a particle size of 0.1 to 1 mm, 25 to 40 mass% zircon particles with a particle size of 0.1 mm or less, and 5 to 10 mass% zircon particles with a particle size of 10 μm or less, separation of the structure and the occurrence of cracks are extremely effectively suppressed.

[0039] As a result, by sintering the zircon casting of the present invention under appropriate sintering conditions, it is possible to obtain a sintered zircon casting having excellent mechanical properties and reliability. More specifically, a sintered zircon casting sintered under appropriate sintering conditions can be imparted with a compressive strength of 140 MPa or more, and by optimizing the composition of the zircon casting, the compressive strength can be increased to 180 MPa or more.

[0040] Representative embodiments of the present invention have been described above, but the present invention is not limited to these, and various design modifications are possible, all of which are included in the technical scope of the present invention. EXAMPLES

[0041] Example The raw materials were prepared in the ratios shown in Table 1 as Examples 1 to 8, and zircon casting raw materials were obtained. The values ​​shown in Table 1 are in mass %. Then, water and a dispersant were added to each raw material, and the mixture was thoroughly kneaded. The amount of water added was constant at 5.5 mass %, and the amount of dispersant added was constant at 0.05 mass %. Then, the zircon casting raw material having appropriate fluidity was cast into a mold, and a plate-shaped zircon casting product of 230 mm x 114 mm x 65 mm was obtained.

[0042] Next, each of the obtained zircon castings was cured at 50°C for one day, removed from the frame, and then dried at 70°C for one day, at 140°C for two days, and at 180°C for two days to obtain the zircon castings according to the present invention. Next, each of the zircon castings was fired at 1500°C for five hours to obtain fired zircon castings.

[0043] [Table 1]

[0044] [evaluation] The castability of the zircon casting feedstock having each composition, the state of the zircon castings, and the strength of the fired zircon castings were evaluated.

[0045] (1) Separation of top and bottom during casting The appearance of the cast surface of the fired product was used to evaluate the state of separation between the top and bottom during casting. A ◎ was given if no layer of separated fine powder was observed on the cast surface, a ◯ was given if a layer of separated fine powder was observed on the cast surface with a thickness of <1mm, and an × was given if a layer of separated fine powder was observed on the cast surface with a thickness of ≥1mm. The results are shown in Table 1.

[0046] (2) Presence or absence of cracks after drying The appearance of the dried castings and the condition of the cut surface were used to evaluate the presence or absence of cracks. A rating of ◯ was given for cases where no cracks were found on either the appearance or the cut surface, and a rating of × was given for cases where cracks were found on the appearance or the cut surface. The results are shown in Table 1.

[0047] (3) Compressive strength The compressive strength of the zircon-based cast sintered products after firing was measured based on JIS R2206 (Testing method for compressive strength of refractory bricks). The results are shown in Table 1.

[0048] Comparative Example Zircon casting raw material, zircon casting products, and zircon casting fired products were obtained in the same manner as in the Examples, except that the raw materials were adjusted in the proportions shown in Table 1 as Comparative Examples 1 to 5. Evaluations were also performed in the same manner as in the Examples. The obtained results are shown in Table 1.

[0049] From the evaluation results shown in Table 1, it can be seen that in all Examples (Examples 1 to 8), separation between the top and bottom (separation of the structure) during casting is extremely effectively suppressed. In particular, Examples 1 to 6, which contain 8 mass% of fine zircon particles with a particle size of 10 μm or less, were evaluated as ⊚. On the other hand, Example 7, in which the content of fine zircon particles with a particle size of 10 μm or less is 5 mass%, and Example 8, in which the content of fine zircon particles with a particle size of 10 μm or less is 10 mass%, are evaluated as ◯, but all Comparative Examples (Comparative Examples 1 to 5) are evaluated as ×, so that the clear separation suppression effect of the present invention is recognized. Here, in Example 7, the content of the fine zircon particles is small, so the expression of the separation suppression effect is not sufficient compared to Examples 1 to 6, and in Example 8, the content of the fine zircon particles is large, so that the fine zircon particles float slightly, and therefore Examples 7 and 8 are evaluated as ◯.

[0050] In addition, the evaluation of the presence or absence of cracks after drying was ◯ in all the examples, confirming a remarkable crack suppression effect. On the other hand, in Comparative Example 3 and Comparative Example 4, in which the content of fine zircon particles having a particle size of 10 μm or less is less than 5 mass%, cracks after drying are suppressed, but separation between the top and bottom during casting cannot be suppressed. In Comparative Example 1 and Comparative Example 2, fine zircon particles having a particle size of 10 μm or less are contained at 8 mass%, but the ratio of zircon particles having other particle sizes is not optimized, and the evaluation is × from the viewpoints of both separation between the top and bottom during casting and cracks after drying.

[0051] From the above results, in order to suppress both separation of the upper and lower parts during casting and cracks after drying, it is extremely important that the zircon casting raw material contains 20-40 mass% zircon particles with a particle size of 1-5 mm, 25-45 mass% zircon particles with a particle size of 0.1-1 mm, 25-40 mass% zircon particles with a particle size of 0.1 mm or less, and the content of zircon particles with a particle size of 10 μm or less is 5-10 mass%. Also, from the results in Table 1, it is found that the zircon casting fired product obtained by firing the zircon casting product of the present invention has a compressive strength of 140 MPa or more.

Claims

1. A casting process is provided for casting a zircon-based casting material containing zircon as a main component to obtain a zircon-based casting product, The zircon casting raw material contains 20 to 40 mass % of zircon particles having a particle diameter of 1 to 5 mm, 25 to 45 mass % of zircon particles having a particle diameter of 0.1 to 1 mm, and 25 to 40 mass % of zircon particles having a particle diameter of 0.1 mm or less, The content of zircon particles having a particle diameter of 10 μm or less is 5 to 10 mass %; A method for producing a zircon casting, comprising the steps of:

2. adding alumina cement and / or hydraulic alumina to the zircon casting raw material; The total content of the alumina cement and / or the hydraulic alumina is 2 to 3 mass %; 2. A method for producing a zircon casting according to claim 1, comprising the steps of:

3. The zircon particles have a particle diameter of 1 to 5 mm in an amount of 20 to 40 mass %, the zircon particles have a particle diameter of 0.1 to 1 mm in an amount of 25 to 45 mass %, and the zircon particles have a particle diameter of 0.1 mm or less in an amount of 25 to 40 mass %, Contains 5 to 10 mass % of zircon particles having a particle size of 10 μm or less; Zircon castings characterized by:

4. Contains alumina cement and / or hydraulic alumina, The total content of the alumina cement and / or the hydraulic alumina is 2 to 3 mass %; 4. The zircon casting of claim 3, wherein

Citation Information

Patent Citations

  • Stamping material for molten bath

    JP1982191277A

  • Lining material for dielectric melting furnace

    JP1983045173A

  • Solenoid spring clutch

    JP1985018625A

  • Semizircon flow-in monolithic refractories for pouring ladle

    JP1986158874A

  • Flow-in monolithic refractories for ladle slag line

    JP1986286270A