Method for manufacturing airless tire

By applying adhesive to the hub and incorporating an annealing step, the method improves adhesive strength between the hub and spoke parts, addressing the bonding issues in airless tire manufacturing and increasing tire durability.

JP2024148508AInactive Publication Date: 2024-10-18SUMITOMO RUBBER INDUSTRIES LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023061692
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-05
Publication Date
2024-10-18
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The adhesive strength between the hub and spoke parts of an airless tire tends to decrease due to insufficient heat reaction during the injection molding process, leading to reduced bonding effectiveness.

Method used

A method involving the application of adhesive to the hub's outer surface, followed by injection of thermoplastic resin into a mold, and an annealing step to enhance adhesive strength, including surface roughening and controlled temperature application to activate reactive groups.

Benefits of technology

The method significantly increases the adhesive strength between the hub and spoke portions, enhancing the durability and integrity of the airless tire.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024148508000001_ABST
    Figure 2024148508000001_ABST
Patent Text Reader

Abstract

To provide a method for manufacturing an airless tire that can further increase an adhesive strength between a hub and a spoke part of a spoke complex.SOLUTION: A method for manufacturing an airless tire 1 includes: a coating step S3 of coating an outer peripheral surface 3a of a hub 3 with an adhesive 33; a placing step S5 of placing the hub 3 coated with the adhesive 33 in a cavity 20 of a mold 10; an injecting step S6 of injecting a thermoplastic resin 8 into the cavity 20 of the mold 10; a molding step S7 of molding a spoke complex 7 in which a spoke part 4 is connected to the hub 3 by curing the spoke part 4 in the cavity 20; and an annealing step S8 of increasing adhesive strength of the adhesive 33 of the spoke complex 7.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing an airless tire. [Background technology]

[0002] The following Patent Document 1 describes a method for manufacturing an airless tire. In this manufacturing method, a thermoplastic resin is injected into an integral molding die in which a hub and a tread ring are arranged. This forms spokes that connect the hub and the tread ring, and the airless tire is integrally molded. This manufacturing method also includes a step of applying an adhesive to the outer circumferential surface of the hub to enhance adhesion to the thermoplastic resin. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent Publication No. 2022-34665 Summary of the Invention [Problem to be solved by the invention]

[0004] Generally, when an injection-molded resin is bonded to a base material such as a metal with an adhesive, the resin hardens when cooled, and there is an insufficient amount of heat for the adhesive to react, which tends to reduce the adhesive strength.

[0005] The present invention has been devised in consideration of the above-mentioned circumstances, and has as its main object to provide a method for manufacturing an airless tire that can further increase the adhesive strength between the hub and the spoke portions of the spoke complex. [Means for solving the problem]

[0006] The present invention is a method for manufacturing an airless tire that includes a metal hub and spoke portions connected to the outer peripheral surface of the hub, the method including the steps of: applying an adhesive to the outer peripheral surface of the hub; placing the hub with the adhesive applied in a cavity of a mold; injecting a thermoplastic resin into the cavity of the mold; hardening the thermoplastic resin in the cavity to mold a spoke complex in which the spoke portions are connected to the hub; and an annealing step for increasing the adhesive strength of the adhesive of the spoke complex. Effect of the Invention

[0007] By employing the above-described configuration, the method for manufacturing an airless tire of the present invention can further increase the adhesive strength between the hub and the spoke portions of the spoke complex. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a perspective view of an airless tire manufactured by the manufacturing method of the present embodiment. [Diagram 2] FIG. 2 is an enlarged view of a cross section taken along line AA in FIG. [Diagram 3] FIG. [Figure 4] FIG. 2 is a flow diagram of a manufacturing method according to the present embodiment. [Diagram 5] FIG. 11 is a plan view of the mold in the placement process. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. The drawings include exaggerated expressions and expressions different from the dimensional ratio of the actual structure in order to facilitate understanding of the present invention. In addition, when there are multiple embodiments, the same or common elements are given the same reference numerals throughout the specification, and duplicated explanations are omitted.

[0010] [Basic structure of airless tires] FIG. 1 is a perspective view of one embodiment of an airless tire (hereinafter, may be simply referred to as "tire") 1 manufactured by the manufacturing method of this embodiment. FIG. 2 is an enlarged view of a cross section of tire 1 taken along line AA in FIG. 1. As shown in FIGS. 1 and 2, tire 1 includes a tread ring 2 having a contact surface 2a that contacts the road surface, a hub 3 disposed on the inner side in the tire radial direction, and spoke portions 4 connecting tread ring 2 and hub 3. Hub 3 is bonded to spoke portions 4 with adhesive 33, which will be described later. In this embodiment, tread ring 2 is bonded to spoke portions 4 with a second adhesive 34, which will be described later.

[0011] The tread ring 2 is an annular rubber member. Well-known rubber members such as natural rubber, butadiene rubber, and isoprene rubber are used as the rubber members. The tread ring 2 is formed of, for example, vulcanized rubber. Spoke portions 4 are connected to an inner peripheral surface 2b of the tread ring 2 in the tire radial direction.

[0012] The tread ring 2 may have, for example, a reinforcing cord 2c (shown in FIG. 3) disposed therein. The reinforcing cord 2c may be, for example, a plurality of organic fiber cords or steel cords oriented in a predetermined direction. A resin material may be added to or compounded with a part of the tread ring 2.

[0013] The hub 3 is connected to an axle (drive shaft) of a vehicle (not shown). The hub 3 in this embodiment is made of metal. Well-known metals such as aluminum, magnesium, copper and titanium are used as the metal. The hub 3 includes, for example, a disk portion 3a and a cylindrical portion 3b formed on the outer side in the tire radial direction. The disk portion 3a is disposed concentrically with the tread ring 2. The spoke portion 4 is connected to the outer peripheral surface 3e of the cylindrical portion 3b.

[0014] The spoke portion 4 in this embodiment is made of a thermoplastic resin 8. Such spoke portion 4 has a function of absorbing vibrations during running of the tire and improving ride comfort performance. As the thermoplastic resin 8, for example, polyolefin, polyvinyl chloride, methacrylic resin, etc. are preferable, and in particular, polyester resin, polyamide resin, or polyurethane resin is preferably adopted. It is to be noted that "resin" includes elastomer. In this embodiment, the spoke portion 4 is made of a hardened thermoplastic resin 8.

[0015] The complex modulus of the spoke portion 4 (cured thermoplastic resin 8) is desirably 80 MPa or more, more desirably 100 MPa or more, desirably 300 MPa or less, and even more desirably 250 MPa or less. Since the complex modulus is 80 MPa or more, the rigidity of the tire 1 is maintained. Since the complex modulus is 300 MPa or less, high ride comfort performance can be maintained. In this specification, the complex modulus is a value measured in accordance with JIS K6394 using a viscoelasticity spectrometer such as GABO's "Eplexer (registered trademark)" under the conditions shown below. Initial strain: 10% Amplitude: ±2% Frequency: 10Hz Deformation mode: tension Temperature: 70℃

[0016] The spoke portion 4 is integrally provided with, for example, an outer ring portion 4a on the outside in the tire radial direction, an inner ring portion 4b on the inside in the tire radial direction, and a plurality of spoke elements 4c. The outer ring portion 4a is, for example, an annular body connected to the inner peripheral surface 2b of the tread ring 2. The inner ring portion 4b is, for example, an annular body connected to the outer peripheral surface 3e of the cylindrical portion 3b of the hub 3. In this manner, the tread ring 2 is connected to the outside of the spoke portion 4 in the tire radial direction, and the hub 3 is connected to the inside of the spoke portion 4 in the tire radial direction. Each spoke element 4c is, for example, a plate-like body extending in the tire radial direction, and is connected to the outer ring portion 4a and the inner ring portion 4b. The spoke element 4c is not limited to the illustrated embodiment, and various well-known forms may be adopted.

[0017] [Manufacturing method of airless tires] Next, a method for manufacturing the tire 1 will be described. A mold 10 is used to manufacture the tire 1. FIG. 3 is a cross-sectional view of one embodiment of the mold 10. As shown in FIG. 3, the mold 10 includes a lower mold 10A and an upper mold 10B that is movable in the vertical direction relative to the lower mold 10A. The lower mold 10A includes a cavity 20 formed of a cylindrical recess and a mating surface 11 with which the upper mold 10B is mated. Specifically, FIG. 3 is a cross-sectional view of the upper mold 10B and the lower mold 10A when they are closed and cut at the mating surface 11, and shows the lower mold 10A and a portion 10e of the upper mold 10B located below the mating surface 11. The mold 10 includes, for example, an injection gate 26 of a known structure for injecting a thermoplastic resin 8 into the cavity 20.

[0018] The cavity 20 includes, for example, an area in which the tread ring 2 and the hub 3 are disposed, and an area in which the thermoplastic resin 8 for molding the spoke portion 4 is filled. As described above, in this embodiment, the mold 10 has a well-known structure.

[0019] Fig. 4 is a flow diagram of the manufacturing method of this embodiment. As shown in Fig. 4, in this embodiment, the manufacturing method includes a coating step (hereinafter referred to as a "first coating step") S3, a placement step S5, an injection step S6, a molding step S7, and an annealing step S8. The manufacturing method also includes, for example, a preparation step S1, a treatment step S2, and a second coating step S4.

[0020] In the manufacturing method of this embodiment, first, a preparation step S1 is performed. In the preparation step S1, for example, a tread ring 2 and a hub 3 are prepared. The tread ring 2 is obtained, for example, according to a conventional method, by molding an unvulcanized rubber member, a reinforcing cord 2c, etc. into a predetermined shape and vulcanizing it in a mold or the like. On the other hand, the hub 3 is manufactured by various well-known methods such as casting, forging, cutting, etc. (not shown).

[0021] Next, a treatment step S2 is performed. The treatment step S2 is, for example, a step of blasting the outer peripheral surface 3e (shown in FIG. 2) of the hub 3. The blasting step is, for example, a step of roughening the outer peripheral surface 3e by spraying non-metallic particles or metallic particles at high speed onto the outer peripheral surface 3e. This can increase the adhesive strength between the hub 3 and the spoke portion 4. In the treatment step S2 in this embodiment, the inner peripheral surface 2b of the tread ring 2 may be blasted. Note that in the manufacturing method of the present invention, a well-known roughening treatment step other than the blasting treatment may be performed, or the treatment step may be omitted.

[0022] Next, a first application step S3 is performed. In the first application step S3, in this embodiment, an adhesive 33 (shown in FIG. 2) is applied to the outer circumferential surface 3e of the hub 3. In this embodiment, the adhesive 33 is applied to the outer circumferential surface 3e by a well-known method.

[0023] The adhesive 33 is preferably a vulcanizing adhesive to increase adhesive strength. Specifically, the adhesive 33 is preferably manufactured by Lord Far East Corporation under the trade names "Chemlock 218E" and "IMB1040" or manufactured by Toyo Kagaku Kenkyusho Co., Ltd. under the trade names "Metalock UA" and "Metalock C-12".

[0024] In the first application step S3, it is desirable that the adhesive 33 be applied to a thickness d1 (shown in FIG. 2) of 30 to 100 μm. Since the thickness d1 is 30 μm or more, the adhesive 33 is sufficiently applied to the outer peripheral surface 3e, and therefore the adhesive strength can be ensured. Since the thickness d1 is 100 μm or less, the adhesive 33 is prevented from being swept away by the thermoplastic resin 8 when the thermoplastic resin 8 is injected in the injection step, and the adhesive strength can be increased. The adhesive 33 applied to the thickness d1 remains in the same thickness range even after the molding step S7.

[0025] In the first application step S3, it is preferable to apply the adhesive 33 that has been preheated in advance to the outer circumferential surface 3e of the hub 3. This allows the adhesive 33 to be spread and improves adhesion to the metal hub 3, and also makes it possible to remove the solvent contained in the adhesive 33. The adhesive 33 is heated to 30 to 150°C by a known heater (not shown) for a preheating time of 10 to 60 minutes, for example.

[0026] Next, the second application step S4 is performed. In the second application step S4, in this embodiment, the second adhesive 34 (shown in FIG. 2) is applied to the inner circumferential surface 2b of the tread ring 2. In this embodiment, the second adhesive 34 is applied to the inner circumferential surface 2b by a well-known method. The second adhesive 34 may be, for example, the same as the adhesive 33. In addition, the second adhesive 34 may be a vulcanization adhesive different from the adhesive 33. Specifically, the second adhesive 34 is preferably manufactured by Lord Far East Corporation under the trade names "Chemlock 210" and "Chemlock 6108" or manufactured by Toyo Kagaku Kenkyusho Co., Ltd. under the trade names "Metalock UA" and "Metalock C-12". Note that the second application step S4 may be performed between the treatment step S2 and the arrangement step S5.

[0027] The thickness d2 of the second adhesive 34 may be smaller than the thickness d1 of the adhesive 33. In general, due to the flow path of the thermoplastic resin 8, the adhesion between the spoke portion 4 formed of the thermoplastic resin 8 and the tread ring 2 formed of vulcanized rubber is delayed from the adhesion between the spoke portion 4 and the metal hub 3. As a result, the pressure of the thermoplastic resin 8 adhering to the tread ring 2 is relatively small, and the second adhesive 34 flowed by the thermoplastic resin 8 is small. Therefore, by making the thickness d2 of the second adhesive 34 smaller than the thickness d1 of the adhesive 33, the adhesive strength between the spoke portion 4 and the tread ring 2 and the adhesive strength between the spoke portion 4 and the hub 3 can be made approximately equal while reducing the amount of the second adhesive 34 used. From this viewpoint, it is desirable that the second adhesive 34 is applied to a thickness d2 of 10 to 50 μm in the second application step S4.

[0028] Next, the arrangement step S5 is performed. FIG. 5 is a plan view of the lower die 10A of the mold 10 in the arrangement step S5. As shown in FIG. 5, in the arrangement step S5, in this embodiment, the hub 3 to which the adhesive 33 is applied is arranged at a predetermined position in the cavity 20 of the lower die 10A. Also, in the arrangement step S5, for example, the tread ring 2 to which the second adhesive 34 is applied may be arranged in the cavity 20. This tread ring 2 is arranged at a predetermined position in the cavity 20, for example. Thereafter, the upper die 10B is fitted into the lower die 10A, and the mold 10 is closed.

[0029] Next, the injection process S6 is performed. In the injection process S6, in this embodiment, the thermoplastic resin 8 is injected into the cavity 20. In the injection process S6, for example, the thermoplastic resin 8 is filled into a predetermined position in the cavity 20 through an injection gate 26 (shown in FIG. 3).

[0030] To inject the thermoplastic resin 8, for example, an injection molding machine (not shown) of a known structure is used. This injection molding machine includes a cylinder (not shown) for heating the thermoplastic resin 8, and a screw (not shown) that rotates inside the cylinder and injects the thermoplastic resin 8 while applying pressure to it. The cylinder is configured so that its temperature can be controlled by a heating means such as a heater. As a result, the thermoplastic resin 8 is injected in a state softened by heating.

[0031] The temperature of the cylinder is desirably 180° C. or higher, more desirably 200° C. or higher, desirably 300° C. or lower, and desirably 220° C. or lower. Since the temperature of the cylinder is controlled to 300° C. or lower, it is possible to prevent the thermoplastic resin 8 from being heated to a temperature higher than necessary, and therefore it is possible to prevent thermal deterioration of the tread ring 2, the adhesive 33, and the second adhesive 34. Since the temperature of the cylinder is controlled to 180° C. or higher, the heat of the thermoplastic resin 8 is imparted to the adhesive 33 and the second adhesive 34, which enhances the activity of the reactive groups, thereby improving the adhesive strength.

[0032] Next, a molding step S7 is performed. In this embodiment, the molding step S7 involves hardening the thermoplastic resin 8 in the cavity 20 to form the spoke portions 4. This results in a spoke complex 7 in which the spoke portions 4 are connected to the hub 3 (as shown in FIG. 2). In this embodiment, the thermoplastic resin 8 is hardened by cooling, for example, by natural cooling. In this embodiment, the spoke complex 7 is formed by connecting the outer circumferential surface 3e of the cylindrical portion 3b and the inner ring portion 4b via an adhesive 33. A well-known method is used to harden the thermoplastic resin 8.

[0033] Furthermore, since the tread ring 2 is placed in the mold 10 in the placement step S5, the tread ring 2 is connected to the spoke complex 7 in the molding step S7 of this embodiment. In the molding step S7, for example, the inner circumferential surface 2b of the tread ring 2 and the outer ring portion 4a of the spoke portion 4 are connected via the second adhesive 34. As a result, in the molding step S7 of this embodiment, a tire 1 is formed in which the tread ring 2, the hub 3, and the spoke portion 4 are integrally molded.

[0034] Next, the annealing step S8 is performed. In the annealing step S8, heat is supplied to the spoke complex 7. As a result, the reactive groups of the adhesive 33, which tend to be insufficiently reacted with the heat from the thermoplastic resin 8 in the injection step S6, are sufficiently activated by the heat supply in the annealing step S8. Therefore, the manufacturing method of the airless tire 1 of the present invention can further increase the adhesive strength of the adhesive 33 of the spoke complex 7. In addition, the annealing step S8 increases the activity of the reactive groups of the second adhesive 34.

[0035] In the annealing step S8, in this embodiment, the spoke composite 7, or in this embodiment, the tire 1, is placed in an atmosphere of 50 to 100° C. for 10 to 90 minutes. This increases the adhesive strength and suppresses deterioration of the thermoplastic resin 8 and deformation of the spoke portion 4.

[0036] The annealing step S8 is performed, for example, after the spoke complex 7, or in this embodiment, the tire 1, is removed from the mold 10. This ensures that the spoke complex 7 is cooled. Furthermore, cooling the spoke complex 7 within the mold 10 prevents the thermoplastic resin 8 from sticking to the mold 10. In the annealing step, at least one tire 1, and preferably multiple tires 1, are placed in a heating device of known structure, such as a hot air dryer, and annealed.

[0037] Although a particularly preferred embodiment of the present invention has been described above in detail, the present invention is not limited to the illustrated embodiment and can be modified and embodied in various ways. In this embodiment, the tire 1 in which the hub 3, the tread ring 2, and the spoke portion 4 made of thermoplastic resin 8 are integrally molded in a mold 10 is annealed. However, for example, only the spoke complex 7 in which the hub 3 and the spoke portion 4 made of thermoplastic resin 8 are integrally molded is annealed. Then, the tread ring 2 to which the second adhesive 34 is applied may be bonded to the annealed spoke complex 7 to mold the tire 1 (not shown). Also, the annealed spoke complex 7 and the tread ring 2 to which the second adhesive 34 is applied may be placed in the mold 10, and the thermoplastic resin 8 may be injected between the spoke complex 7 and the tread ring 2 to mold the tire 1 (not shown). EXAMPLES

[0038] An airless tire (corresponding to a tire size of 145 / 70R12) having the basic structure shown in Fig. 1 and Fig. 2 was prototyped. Then, the durability of each test tire was tested. The test method was as follows.

[0039] <Durability> Using a drum tester, each tire was run under the following conditions until damage such as peeling occurred between the hub and the spokes. The results were evaluated using a speed (called the breaking speed) that was 10 km / h lower than the speed at which the tire was damaged, and an index was used with the breaking speed of the example being set at 100. Load: 3.4kN From the initial speed of 100km / h, 10km / h is added every 10 minutes. In both the examples and the comparative examples, the tire structure and the manufacturing method except for the annealing step are the same. The results of the tests are shown in Table 1.

[0040] [Table 1]

[0041] As a result of the tests, it is understood that the tires of the examples have higher adhesive strength between the hub and the spokes and are more durable than the tires of the comparative examples.

[0042] [Note] The present invention includes the following aspects.

[0043] [Invention 1] A method for manufacturing an airless tire including a metal hub and a spoke portion connected to an outer peripheral surface of the hub, comprising: a coating step of coating an adhesive on the outer peripheral surface of the hub; placing the adhesive coated hub into a mold cavity; injecting a thermoplastic resin into the cavity of the mold; hardening the thermoplastic resin in the cavity to form a spoke composite in which the spoke portions are connected to the hub; and an annealing step to increase the adhesive strength of the adhesive of the spoke composite. A method for manufacturing airless tires. [Invention 2] The method for producing an airless tire according to the first aspect of the present invention, wherein the annealing step is carried out after the spoke complex is removed from the mold. [Invention 3] 3. The method for producing an airless tire according to claim 1 or 2, wherein in the annealing step, the spoke complex is placed in an atmosphere at 50 to 100° C. for 10 to 90 minutes. [Invention 4] The method for producing an airless tire according to any one of Inventions 1 to 3, wherein in the coating step, the adhesive is coated to a thickness of 30 to 100 μm. [Invention 5] 5. The method for producing an airless tire according to any one of claims 1 to 4, further comprising a step of blasting the outer peripheral surface of the hub prior to the coating step. [Invention 6] 6. The method for producing an airless tire according to any one of claims 1 to 5, wherein the adhesive is a vulcanizing adhesive. [Invention 7] The method for producing an airless tire according to any one of Inventions 1 to 6, wherein the thermoplastic resin includes a polyester resin, a polyamide resin, or a polyurethane resin. [Invention 8] 8. The method for producing an airless tire according to claim 7, wherein the thermoplastic resin has a complex modulus of elasticity of 80 to 300 MPa after curing. [The present invention 9] The airless tire includes a tread ring connected to an outer side of the spoke portion in a tire radial direction, The method further includes a second application step of applying a second adhesive to an inner circumferential surface of the tread ring; The placing step further includes placing the tread ring to which the second adhesive has been applied in the cavity, 9. The method for producing an airless tire according to any one of claims 1 to 8, wherein in the molding step, the tread ring is connected to the spoke complex. [The present invention 10] The method for producing an airless tire according to claim 9, further comprising a step of blasting the inner circumferential surface of the tread ring prior to the second application step. [Explanation of symbols]

[0044] 1. Airless tires 3. Hub 4 Spoke section 7 spoke complex 8 Thermoplastic resin 10. Mold 20 Cavity 33 Adhesive S3 Coating process S5 Placement process S6 Injection process S7 Molding process S8 Annealing process

Claims

1. A method for manufacturing an airless tire including a metal hub and a spoke portion connected to an outer peripheral surface of the hub, comprising: a coating step of coating an adhesive on the outer peripheral surface of the hub; placing the adhesive coated hub into a mold cavity; injecting a thermoplastic resin into the cavity of the mold; hardening the thermoplastic resin in the cavity to form a spoke composite in which the spoke portions are connected to the hub; and an annealing step to increase the adhesive strength of the adhesive of the spoke composite. A method for manufacturing airless tires.

2. The method of claim 1 , wherein the annealing step is performed after the spoke composite is removed from the mold.

3. 3. The method for producing an airless tire according to claim 2, wherein in the annealing step, the spoke composite is placed in an atmosphere of 50 to 100° C. for 10 to 90 minutes.

4. The method for producing an airless tire according to any one of claims 1 to 3, wherein in the coating step, the adhesive is coated to a thickness of 30 to 100 µm.

5. The method for producing an airless tire according to claim 1 , further comprising a step of blasting the outer circumferential surface of the hub prior to the coating step.

6. The method for manufacturing an airless tire according to claim 1 , wherein the adhesive is a vulcanizing adhesive.

7. The method for producing an airless tire according to claim 1 , wherein the thermoplastic resin includes a polyester resin, a polyamide resin, or a polyurethane resin.

8. The method for producing an airless tire according to claim 7, wherein the complex modulus of the thermoplastic resin after curing is 80 to 300 MPa.

9. The airless tire includes a tread ring connected to an outer side of the spoke portion in a tire radial direction, The method further includes a second application step of applying a second adhesive to an inner circumferential surface of the tread ring; The placing step further includes placing the tread ring to which the second adhesive has been applied in the cavity, The method for manufacturing an airless tire according to claim 1 , wherein in the molding step, the tread ring is connected to the spoke complex.

10. The method for producing an airless tire according to claim 9 , further comprising a step of blasting the inner circumferential surface of the tread ring prior to the second applying step.

Citation Information

Patent Citations

  • Method for manufacturing airless tire

    JP2022034665A