Membrane electrode assembly, manufacturing method thereof, and fuel cell
The membrane electrode assembly with a conductive fiber diffusion layer and catalyst membrane coverage addresses the output decrease in liquid fuel cells, enhancing performance by increasing catalyst surface area and reducing resistance.
Patent Information
- Application Number
- JP2023061716
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-05
- Publication Date
- 2024-10-18
AI Technical Summary
Fuel cells using liquid fuels, such as direct methanol and direct formic acid fuel cells, face a decrease in output when applying the conventional membrane electrode assembly structure, necessitating a design suitable for improved performance.
A membrane electrode assembly with a diffusion layer made of conductive fibers and a catalyst membrane interposed between the electrolyte membrane and the conductive fibers, where at least half of the conductive fibers on the first surface are covered by the catalyst membrane, enhancing the specific surface area and contact with liquid fuel.
This configuration increases the catalyst's specific surface area, improves fuel-cell output, and reduces internal resistance by ensuring efficient reaction with liquid fuels and minimizing thickness while maintaining a sufficient contact area.
Smart Images

Figure 2024148519000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a membrane electrode assembly, a method for producing the same, and a fuel cell. [Background technology]
[0002] A fuel cell such as a polymer electrolyte fuel cell has a membrane electrode assembly including an electrolyte membrane, an anode provided on one side of the electrolyte membrane, and a cathode provided on the other side of the electrolyte membrane. The fuel cell generates an electromotive force between the anode and the cathode by supplying a fuel to the anode of the membrane electrode assembly and an oxidant to the cathode, thereby generating electricity. In addition, the membrane electrode assembly may be provided with a diffusion layer made of a conductive porous material for the purpose of diffusing the fuel and the oxidant and promoting the electrode reaction at the anode and the cathode.
[0003] For example, Patent Document 1 describes a membrane-electrode assembly for a fuel cell in which a gas diffusion layer for a fuel cell is laminated on one or both sides of a catalyst layer-electrolyte membrane laminate in which a catalyst layer, an electrolyte membrane, and a catalyst layer are laminated in order. The gas diffusion layer for a fuel cell in the membrane-electrode assembly for a fuel cell has a conductive porous layer, and is laminated on the catalyst layer-electrolyte membrane laminate so that the catalyst layer and the conductive porous layer are in contact with each other. The conductive porous layer contains at least conductive carbon particles and a polymer having a glass transition temperature that satisfies at least one of the following conditions: a glass transition temperature of the hydrogen ion conductive polymer electrolyte contained in the catalyst layer is lower than that of the hydrogen ion conductive resin constituting the electrolyte membrane. The polymer in the conductive porous layer is present more densely on the surface in contact with the catalyst layer than on the surface not in contact with the catalyst layer. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2012-199237 A Summary of the Invention [Problem to be solved by the invention]
[0005] In recent years, fuel cells using liquid fuels, such as direct methanol fuel cells and direct formic acid fuel cells, have been developed. Liquid fuels are extremely useful because they are easier to handle and can have a higher energy density per unit volume than gases such as hydrogen gas. However, when the membrane-electrode assembly for fuel cells of Patent Document 1 is applied to a fuel cell using liquid fuel, there is a problem that the output of the fuel cell is reduced. Therefore, there is a demand for a membrane electrode assembly that has a structure suitable for a fuel cell using liquid fuel and can improve the output of the fuel cell.
[0006] The present invention has been made in view of the above problems, and aims to provide a membrane electrode assembly capable of improving the output of a fuel cell that uses a liquid fuel, a manufacturing method thereof, and a fuel cell including this membrane electrode assembly. [Means for solving the problem]
[0007] One aspect of the present invention is a membrane electrode assembly for use in a fuel cell configured to be capable of generating electricity using a liquid fuel, comprising: The membrane electrode assembly includes an electrolyte membrane and A diffusion layer formed of conductive fibers and provided on both sides of the electrolyte membrane; a catalyst film including a catalyst and interposed between the electrolyte membrane and the conductive fiber constituting the diffusion layer; The membrane electrode assembly includes the conductive fibers on a first surface of the diffusion layer facing the electrolyte membrane, the conductive fibers being covered with the catalyst membrane over at least half of the circumferential area thereof.
[0008] Another aspect of the present invention is a fuel cell comprising the membrane electrode assembly of the above aspect.
[0009] Yet another aspect of the present invention is a method for producing the membrane electrode assembly of the above aspect, comprising the steps of: forming the catalyst film by depositing catalyst particles containing the catalyst on one surface of the diffusion layer; Thereafter, the diffusion layer and the electrolyte membrane are stacked together so that the catalyst membrane and the electrolyte membrane are in contact with each other to form a laminate; The laminate is heat-pressed to obtain the membrane electrode assembly. Effect of the Invention
[0010] The diffusion layer in the membrane electrode assembly is made of conductive fibers, and the catalyst membrane is interposed between the electrolyte membrane and the conductive fibers constituting the diffusion layer. Also, conductive fibers are present on the first surface of the diffusion layer facing the electrolyte membrane, with more than half of the circumferential area covered by the catalyst membrane. In this way, by covering more than half of the circumferential area of the conductive fibers present on the first surface of the diffusion layer with the catalyst membrane, the specific surface area of the catalyst membrane can be increased. As a result, the liquid fuel and the catalyst membrane come into contact with each other more easily, and the liquid fuel and the catalyst can react more efficiently when a liquid fuel with relatively low diffusivity is used.
[0011] In addition, by increasing the specific surface area of the catalyst membrane, the area of the interface between the diffusion layer and the catalyst membrane can be increased. Furthermore, by increasing the specific surface area of the catalyst membrane, the thickness of the catalyst membrane can be reduced while ensuring a sufficient contact area between the diffusion layer and the catalyst membrane. As a result, the internal resistance of the fuel cell can be reduced.
[0012] Therefore, the membrane electrode assembly can improve the output of a fuel cell that uses a liquid fuel.
[0013] Furthermore, since the fuel cell has the membrane electrode assembly, it is possible to obtain high output using liquid fuel.
[0014] In the manufacturing method, catalyst particles are first deposited on one side of the diffusion layer to form a catalyst film. By depositing catalyst particles on the diffusion layer in this manner, the catalyst film is formed along the surface of the diffusion layer and can also penetrate between the conductive fibers exposed on the surface of the diffusion layer. After forming such a catalyst film on the diffusion layer, the electrolyte membrane and the diffusion layer are joined via the catalyst film to easily obtain the membrane electrode assembly.
[0015] As described above, according to the above aspects, it is possible to provide a membrane electrode assembly capable of improving the output of a fuel cell that uses a liquid fuel, a manufacturing method thereof, and a fuel cell including this membrane electrode assembly. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a partial cross-sectional view that illustrates a schematic view of a main portion of a membrane electrode assembly in accordance with the first embodiment. [Diagram 2] FIG. 2 is a cross-sectional view that typically shows a diffusion layer on which a catalyst membrane is formed in the method for producing a membrane / electrode assembly of the first embodiment. [Diagram 3] FIG. 3 is a cross-sectional view that illustrates a stack in the method for producing a membrane / electrode assembly of the first embodiment. [Figure 4] FIG. 4 is a cross-sectional view showing a main part of a fuel cell including the membrane electrode assembly of the first embodiment. [Diagram 5] FIG. 5 is a partial cross-sectional view showing a main part of a membrane electrode assembly in Comparative Example 1. As shown in FIG. [Figure 6] FIG. 6 is a cross-sectional view that illustrates a process for laminating a catalyst layer and a diffusion layer in the method for producing a membrane electrode assembly in Comparative Example 1. As shown in FIG. [Figure 7] FIG. 7 is a partial cross-sectional view showing a main part of a diffusion layer in Comparative Example 2. As shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] (Embodiment 1) An embodiment of the membrane / electrode assembly and the method for producing the same will be described with reference to FIGS. 1 to 3. FIG.
[0018] A. Membrane electrode assembly As shown in Fig. 1, a membrane electrode assembly (hereinafter referred to as MEA) 1 of this embodiment has an electrolyte membrane 2, a diffusion layer 3 composed of conductive fibers 311 and provided on both sides of the electrolyte membrane 2, and a catalyst membrane 4 containing a catalyst and interposed between the electrolyte membrane 2 and the conductive fibers 311 constituting the diffusion layer 3. The MEA 1 is configured so as to be applicable to a polymer electrolyte fuel cell that uses a liquid fuel, such as a direct methanol fuel cell that uses methanol as a fuel and a direct formic acid fuel cell that uses formic acid as a fuel. The configuration of the MEA 1 will be described in more detail below.
[0019] The electrolyte membrane 2 has electrical insulation properties and is + The cation exchange resin is made of a cation exchange resin that is configured to selectively allow permeation of cations such as cations of 1 to 100 carbon atoms. Examples of such cation exchange resins include perfluoroalkylsulfonic acid polymers (e.g., Nafion (registered trademark) manufactured by DuPont).
[0020] Diffusion layers 3 are provided on both sides of the electrolyte membrane 2. The diffusion layers 3 are composed of a plurality of conductive fibers 311. As the conductive fibers 311 constituting the diffusion layer 3, for example, conductive carbon fibers such as PAN-based carbon fibers obtained by carbonizing polyacrylonitrile fibers and pitch-based carbon fibers obtained by carbonizing pitch fibers can be used.
[0021] More specifically, the diffusion layer 3 may be made of carbon paper, which is a composite material of conductive carbon fibers and carbon, or carbon cloth, which is a woven material of conductive carbon fibers. The diffusion layer 3 is preferably made of carbon cloth. Carbon cloth has appropriate gaps between the conductive carbon fibers that make up the carbon cloth, so that the liquid fuel can quickly penetrate into the gaps between the conductive carbon fibers due to surface tension. Therefore, by using carbon cloth as the diffusion layer 3, the liquid fuel can be more easily diffused into the diffusion layer 3.
[0022] When carbon cloth is used as the diffusion layer 3, the warp and weft of the carbon cloth may be monofilaments, but are preferably twisted yarns of conductive carbon fibers. By forming the carbon cloth from twisted yarns of conductive carbon fibers, more gaps are formed in the diffusion layer 3, and the diffusibility of the liquid fuel in the diffusion layer 3 can be further improved. In addition, on the surface of the carbon cloth, parts where the warp yarns are exposed and parts where the weft yarns are exposed are alternately present, and the conductive carbon fibers extend in approximately the same direction in each of the parts where the warp yarns are exposed and the parts where the weft yarns are exposed. Therefore, by forming the catalyst film 4 on such a diffusion layer 3, the catalyst film 4 can more easily enter the gaps between the conductive carbon fibers. As a result, the specific surface area of the catalyst film 4 can be more easily increased.
[0023] There is no particular limitation on the weave structure of the carbon cloth serving as the diffusion layer 3. For example, the carbon cloth may have various weave structures such as plain weave, varied plain weave, twill weave, and varied twill weave.
[0024] The warp density, weft density, thickness, and mass per unit area of the carbon cloth as the diffusion layer 3 may be appropriately selected according to the desired diffusion characteristics. For example, the thickness of the carbon cloth may be 0.1 mm or more and 1 mm or less. The mass per unit area of the carbon cloth may be 50 g / m 2 More than 300g / m 2It is sufficient that the volume resistivity of the carbon cloth in the thickness direction is 1 Ωcm or less. From the viewpoint of reducing the internal resistance in the fuel cell, the lower the volume resistivity of the carbon cloth in the thickness direction, the more preferable.
[0025] Furthermore, the diffusion layer 3 may be previously subjected to a surface treatment such as a water-repellent treatment.
[0026] Specifically, the diffusion layer 3 in this embodiment is a carbon cloth made of twisted conductive carbon fibers.
[0027] A catalyst-containing catalyst film 4 is interposed between the electrolyte membrane 2 and the conductive fibers 311 that constitute the diffusion layer 3. The catalyst contained in the catalyst film 4 may be, for example, a precious metal catalyst such as palladium (Pd) or platinum (Pt), or a catalyst-supported carbon in which such a precious metal catalyst is supported on carbon.
[0028] The catalyst membrane 4 may further contain an electrolyte. The electrolyte contained in the catalyst membrane 4 is, like the electrolyte membrane 2, an electrolyte that has electrical insulation properties and can store hydrogen ions (H + A cation exchange resin configured to be selectively permeable to cations such as cation exchange resin (e.g., Nafion (registered trademark) manufactured by DuPont) can be used. Examples of such cation exchange resins include perfluoroalkylsulfonic acid polymers (e.g., Nafion (registered trademark) manufactured by DuPont). The catalyst content and electrolyte content in the catalyst membrane 4 may be appropriately set according to the desired electrode characteristics, etc.
[0029] The catalyst film 4 is attached to the surface of the conductive fibers 311 that constitute the diffusion layer 3. The amount of the catalyst film 4 attached per unit area of the diffusion layer 3 is, for example, 0.1 to 3 mg / cm. 2 The range can be appropriately set.
[0030] At least a portion of the catalyst membrane 4 is in contact with both the conductive fibers 311 and the electrolyte membrane 2. This allows hydrogen ions generated in the catalyst membrane 4 of the anode of the fuel cell to move to the catalyst membrane 4 of the cathode.
[0031] Moreover, among the conductive fibers 311a present on the first surface 32 of the diffusion layer 3 on the electrolyte membrane 2 side, at least a half of the area in the circumferential direction of at least a part of the conductive fibers 311a is covered with the catalyst membrane 4. By attaching the catalyst membrane 4 to more than half of the area in the circumferential direction of the surface of the conductive fibers 311a present on the first surface 32 of the diffusion layer 3 in this manner, the specific surface area of the catalyst membrane 4 can be increased, and the contact area between the liquid fuel and the catalyst membrane 4 can be increased. Furthermore, by increasing the specific surface area of the catalyst membrane 4, the resistance caused by the movement of hydrogen ions and electrons generated by the electrode reaction can be reduced. As a result, the internal resistance of the fuel cell can be reduced, and the output can be improved.
[0032] The state of adhesion of the catalyst film 4 to the conductive fiber 311a can be determined, for example, as follows. First, the MEA 1 is cut along a plane perpendicular to the extension direction of the conductive fiber 311a to expose a cross section perpendicular to the extension direction of the conductive fiber 311a. A scanning electron microscope is used to obtain an enlarged photograph of this cross section. Then, based on the enlarged photograph, the ratio of the length of the area where the conductive fiber 311a and the catalyst film 4 are in contact with each other to the circumferential length of the conductive fiber 311a is calculated. If this value is 0.5 or more, it can be determined that the catalyst film 4 is attached to more than half of the area in the circumferential direction of the surface of the conductive fiber 311a.
[0033] From the viewpoint of further enhancing the above-mentioned effect, it is preferable that the entire circumferential surface of at least some of the conductive fibers 311a present on the first surface 32 of the diffusion layer 3 is covered by the catalyst film 4. That is, it is preferable that the enlarged photograph of the diffusion layer 3 obtained by the above-mentioned method includes conductive fibers 311a whose entire circumferential surface is in contact with the catalyst film 4.
[0034] In addition, the catalyst film 4 is preferably distributed such that the amount of the catalyst film 4 present in the diffusion layer 3 in a region 35 from the first surface 32 to the center 34 in the thickness direction of the diffusion layer 3 is greater than the amount of the catalyst film 4 present in a region 36 from the second surface 33, which is the back surface of the first surface 32, to the center 34 in the thickness direction of the diffusion layer. In this way, by attaching more catalyst film 4 to the conductive fibers 311 present in the region 35 relatively close to the electrolyte membrane 2 among the conductive fibers 311 constituting the diffusion layer 3, the average distance between the electrolyte membrane 2 and the catalyst film 4 can be further shortened, and the resistance caused by the movement of hydrogen ions can be further reduced. As a result, the internal resistance of the fuel cell can be further reduced.
[0035] Whether or not the catalyst film 4 has the above-mentioned distribution can be determined, for example, by the following method. First, the MEA 1 is cut along a plane perpendicular to the extension direction of the conductive fibers 311a to expose a cross section perpendicular to the extension direction of the conductive fibers 311a. An enlarged photograph of this cross section is obtained using a scanning electron microscope. Then, based on the enlarged photograph, the area ratio of the catalyst film 4 present in the region 35 from the first surface 32 of the diffusion layer 3 to the center in the thickness direction, and the area ratio of the catalyst film 4 present in the region 36 from the second surface 33 of the diffusion layer 3 to the center in the thickness direction are calculated. By comparing the area ratios of the catalyst film 4 in each region calculated in this way, it is possible to determine whether or not the catalyst film 4 has the above-mentioned distribution.
[0036] From a similar viewpoint, it is more preferable that the catalyst film 4 has a distribution such that, when the diffusion layer 3 is divided into three or more regions in its thickness direction, the amount of catalyst film 4 present in the region closest to the first surface 32 is greatest, and the amount of catalyst film 4 present in the region increases as the region is further away from the first surface 32.
[0037] The method for determining whether the catalyst film 4 has the above-mentioned distribution is the same as that described above, except that the number of regions for calculating the area ratio of the catalyst film 4 is changed from two, region 35 and region 36, to three or more.
[0038] When the diffusion layer 3 is made of carbon cloth as in this embodiment, the interface 21 between the catalyst membrane 4 and the electrolyte membrane 2 preferably has unevenness along the surface of the conductive fiber 311a. That is, in a portion where the warp yarn is exposed on the first surface 32 of the diffusion layer 3, the interface 21 between the catalyst membrane 4 and the electrolyte membrane 2 preferably has unevenness in a direction perpendicular to the extension direction of the warp yarn. Similarly, in a portion where the weft yarn is exposed on the first surface 32 of the diffusion layer 3, the interface 21 between the catalyst membrane 4 and the electrolyte membrane 2 preferably has unevenness in a direction perpendicular to the extension direction of the weft yarn. In this way, by forming unevenness extending in stripes at the interface 21 between the catalyst membrane 4 and the electrolyte membrane 2 by utilizing the gaps in the conductive carbon fibers constituting the carbon cloth, the contact area between the catalyst membrane 4 and the electrolyte membrane 2 can be increased and the internal resistance of the fuel cell can be further reduced.
[0039] B. Manufacturing method of membrane electrode assembly The MEA 1 of this embodiment is obtained by depositing catalyst particles containing a catalyst on one side of the diffusion layer 3 to form a catalyst film 4, as shown in Fig. 2, then overlapping the diffusion layer 3 and the electrolyte membrane 2 so that the catalyst film 4 and the electrolyte membrane 2 are in contact with each other to form a laminate 10 shown in Fig. 3, and then heat pressing the laminate 10. The manufacturing process of the MEA 1 will be described in more detail below.
[0040] (1) Formation of catalyst film 4 In the manufacturing method, catalyst particles are deposited on one side of the diffusion layer 3 to form a catalyst film 4 on the surface of the conductive fibers 311 that constitute the diffusion layer 3. The catalyst particles contain at least a catalyst. The catalyst particles may further contain an electrolyte.
[0041] As a method for depositing catalyst particles on the diffusion layer 3, for example, a method can be adopted in which a catalyst ink in which a catalyst is dispersed in a dispersion medium is prepared, and the catalyst ink is sprayed onto the diffusion layer 3. When the catalyst ink is sprayed, catalyst particles consisting of droplets containing the catalyst ink and the dispersion medium are formed, and move toward the diffusion layer 3. During this movement, the dispersion medium in the catalyst particles gradually evaporates, and catalyst particles made of a substantially solid state are deposited on the diffusion layer 3. By depositing the catalyst particles in a substantially solid state on the diffusion layer 3 in this manner, the catalyst film 4 can be reliably formed on one side of the diffusion layer 3.
[0042] Alternatively, instead of the above method, it is also possible to form the catalyst film 4 on one side of the diffusion layer 3 by, for example, spraying a powder containing a catalyst onto the diffusion layer.
[0043] In the above-mentioned manufacturing method, it is preferable that the catalyst membrane 4 formed on the diffusion layer 3 has gaps in a plan view seen from the thickness direction of the diffusion layer 3. In this case, after bonding with the electrolyte membrane 2, the unevenness resulting from the above-mentioned gaps can be more easily formed at the interface between the electrolyte membrane 2 and the catalyst membrane 4. As a result, the contact area between the electrolyte membrane 2 and the catalyst membrane 4 can be increased, and the internal resistance of the fuel cell can be further reduced.
[0044] Furthermore, after the catalyst film 4 is formed on the diffusion layer 3, it is preferable that no catalyst particles are present on the back surface of the diffusion layer 3 opposite the surface having the catalyst film 4. In this case, the ratio of the portion of the catalyst film 4 of the MEA 1 that is in contact with both the electrolyte membrane 2 and the conductive fibers 311 can be increased.
[0045] (2) Heat pressing of the diffusion layer 3 and the catalyst film 4 In the above-mentioned manufacturing method, after forming the catalyst membrane on the diffusion layer 3, the diffusion layer 3 may be heat-pressed before the diffusion layer 3 and the electrolyte membrane 2 are laminated together. By thus heat-pressing the diffusion layer 3 provided with the catalyst membrane 4, the catalyst membrane 4 can be softened and the catalyst membrane 4 can be more reliably inserted between the conductive fibers 311 constituting the diffusion layer 3. As a result, the conductive fibers 311a present on the first surface 32 of the diffusion layer 3 can be more easily covered with the catalyst membrane 4.
[0046] When the diffusion layer 3 is heat-pressed, the temperature during heat pressing can be appropriately set depending on the composition of the catalyst film 4. For example, when the catalyst film 4 includes a catalyst film and an electrolyte, the temperature during heat pressing is preferably 120° C. or more and 160° C. or less, and more preferably 140° C. or more and 160° C. or less. The pressure during heat pressing is preferably 0.6 MPa or more and 2.6 MPa or less. The pressing time during heat pressing varies depending on the pressing method, heating temperature, and pressing pressure, but can be appropriately set within the range of, for example, 1 minute or more and 15 minutes or less.
[0047] (3) Preparation and bonding of laminates In the manufacturing method, after forming the catalyst membrane 4 on the diffusion layer 3, as shown in FIG. 3, the diffusion layer 3 and the electrolyte membrane 2 are overlapped so that the catalyst membrane 4 and the electrolyte membrane 2 are in contact with each other to form the laminate 10. Then, the laminate 10 is heat-pressed to bond the diffusion layer 3 and the electrolyte membrane 2. In this manner, the MEA 1 can be obtained. The temperature and pressure in the heat press of the laminate 10 can be appropriately set according to the type of electrolyte contained in the electrolyte membrane 2 and the composition of the catalyst membrane 4. For example, the temperature in the heat press of the laminate 10 is preferably in the range of 135° C. to 165° C., and more preferably in the range of 135° C. to 155° C. In addition, the pressure in the heat press of the laminate 10 is preferably in the range of 0.6 MPa to 2.6 MPa. In addition, the press time in the heat press of the laminate 10 can be appropriately set, for example, in the range of 1 minute to 15 minutes.
[0048] C. Fuel cell 5 FIG. 4 shows an example of a fuel cell 5 having an MEA1. The fuel cell 5 has an MEA1 having an electrolyte membrane 2, a catalyst membrane 4, and a diffusion layer 3, a first separator 51 provided on one side of the MEA1, and a second separator 52 provided on the other side of the MEA1. The first separator 51 is configured to be able to supply liquid fuel to the MEA1, and the second separator 52 is configured to be able to supply an oxidant to the MEA1. That is, the fuel cell 5 is configured such that the catalyst membrane 4 on the first separator 51 side of the MEA1 becomes the anode 4a, and the catalyst membrane 4 on the second separator 52 side becomes the cathode 4c. The fuel cell 5 can generate power by supplying liquid fuel from the first separator 51 to the anode 4a and supplying an oxidant from the second separator 52 to the cathode 4c, thereby causing an electrode reaction on the anode 4a and the cathode 4c. Note that in FIG. 5, the structure of the catalyst membrane 4 is simplified for convenience.
[0049] The liquid fuel used in the fuel cell 5 may be any liquid containing carbon atoms. For example, the fuel cell 5 may be configured as a direct formic acid fuel cell using formic acid as fuel, or may be configured as a direct methanol fuel cell using methanol as fuel. In addition, the oxidant supplied to the fuel cell 5 may be, for example, air or oxygen gas. From the viewpoint of further increasing the energy density of the fuel cell 5, it is preferable that the liquid fuel is formic acid.
[0050] The fuel cell 5 may have one or more unit cells 50 including an MEA 1, a first separator 51, and a second separator 52. For example, when the fuel cell 5 is composed of one unit cell 50 as shown in FIG. 4, the catalyst membrane 4 serving as the anode 4a and the catalyst membrane 4 serving as the cathode 4c may be electrically connected to an external load, and a current may be drawn from each electrode. Although not shown in the figure, when the fuel cell 5 has a plurality of unit cells 50, these unit cells 50 may be stacked together to form a cell stack. In this case, each unit cell 50 may be electrically connected in series or in parallel with the other unit cells 50.
[0051] The first separator 51 may be made of an electric conductor such as a metal material such as gold-plated stainless steel, a conductive nonmetallic material such as conductive carbon, a conductive composite material, etc. The first separator 51, which is electrically conductive, functions as a current collector that collects electrons generated by the electrode reaction in the MEA 1, and can conduct the electric power generated in the MEA 1 to the outside.
[0052] The electrode contact surface 511 of the first separator 51, which contacts the diffusion layer 3, is provided with a fuel flow channel 512 configured to be able to supply fuel to the anode 4a. The shape and arrangement of the fuel flow channel 512 may take various forms. For example, the fuel flow channel 512 may be a groove provided in the first separator 51, having a cross-sectional shape such as a rectangular, triangular, or semicircular shape. The fuel flow channel 512 may have, for example, a plurality of straight portions arranged in parallel to each other and a folded portion connecting an end of each straight portion to an end of a straight portion adjacent to the straight portion, and may be arranged in a meandering manner in a plan view seen from the contact surface side, but other arrangements may also be used.
[0053] A first sealant 53 made of an elastomer may be provided around the electrode contact surface 511 of the first separator 51. The first sealant 53 is disposed so as to be in close contact with each of the first separator 51 and the MEA 1. By providing the first sealant 53 between the first separator 51 and the MEA 1, unintended leakage of fuel from the internal space of the fuel cell 5 to the outside can be suppressed. As the elastomer used for the first sealant 53, for example, a polymer material having rubber elasticity, such as ethylene-propylene-diene rubber (i.e., EPDM), can be used.
[0054] The second separator 52 may be made of an electric conductor such as a metal material, such as gold-plated stainless steel, a conductive nonmetallic material, such as conductive carbon, or a conductive composite material, similar to the first separator 51. The second separator 52, which is electrically conductive, functions as a current collector that supplies electrons generated in the anode 4a and passed through an external load to the cathode 4c, and can conduct the electric power generated in the MEA 1 to the outside.
[0055] An oxidant flow channel 522 is provided on an electrode contact surface 521 of the second separator 52 that contacts the diffusion layer 3. The shape and arrangement of the oxidant flow channel 522 may take various forms, similar to the fuel flow channel 512. For example, the oxidant flow channel 522 may have a cross-sectional shape such as a rectangular, triangular, or semicircular shape, and may be a groove provided in the second separator 52. The oxidant flow channel 522 may have, for example, a plurality of straight portions arranged in parallel to each other and a folded portion connecting an end of each straight portion to an end of a straight portion adjacent to the straight portion, and may be arranged in a meandering manner in a plan view seen from the contact surface side, but may also be arranged in other ways.
[0056] A second sealant 54 made of an elastomer may be provided around the electrode contact surface 521 of the second separator 52. The second sealant 54 is disposed so as to be in close contact with each of the second separator 52 and the MEA 1. By providing the second sealant 54 between the second separator 52 and the MEA 1, unintended leakage of the oxidant from the internal space of the fuel cell 5 to the outside can be suppressed. As the elastomer used for the second sealant 54, for example, a polymer material having rubber elasticity, such as ethylene-propylene-diene rubber (i.e., EPDM), can be used.
[0057] In manufacturing the fuel cell 5 of this embodiment, the first separator 51, the first sealant 53, the MEA 1, the second sealant 54, and the second separator 52 are stacked in this order.
[0058] As shown in Fig. 1, the diffusion layer 3 in the MEA 1 of this embodiment is composed of conductive fibers 311, and the catalyst membrane 4 is interposed between the electrolyte membrane 2 and the conductive fibers 311 constituting the diffusion layer 3. In addition, conductive fibers 311a are present on the first surface 32 of the diffusion layer 3 on the electrolyte membrane 2 side, and more than half of the area in the circumferential direction is covered with the catalyst membrane 4. In this way, by covering more than half of the area in the circumferential direction of the conductive fibers 311a present on the first surface 32 of the diffusion layer 3 with the catalyst membrane 4, the specific surface area of the catalyst membrane 4 can be increased. As a result, the internal resistance of the fuel cell 5 can be reduced.
[0059] (Comparative form 1) 5, an MEA 901 of this comparative embodiment has an electrolyte membrane 91, catalyst layers 92 containing a catalyst and laminated on both sides of the electrolyte membrane 2, and a diffusion layer 93 laminated on the catalyst layer 92. The configuration of the electrolyte membrane 91 in the MEA 901 is similar to the configuration of the electrolyte membrane 2 in the first embodiment.
[0060] The catalyst layer 92 in the MEA 901 is formed in a layer shape on the surface of the electrolyte membrane 91. The composition of the catalyst layer 92 in the MEA 901 is similar to the composition of the catalyst membrane 4 in the first embodiment.
[0061] A diffusion layer 93 made of conductive fibers 931 is laminated on the catalyst layer 92. Of the conductive fibers 931 constituting the diffusion layer 93, conductive fibers 931a present on the surface on the electrolyte membrane 91 side are in contact with the surface of the catalyst layer 92. Of the conductive fibers 931 constituting the diffusion layer 93, conductive fibers 931b other than the conductive fibers 931a present on the surface on the electrolyte membrane 91 side are not in contact with the catalyst layer 92. That is, the catalyst layer 92 of this embodiment hardly penetrates into the gaps between the conductive fibers 931 constituting the diffusion layer 93, and is present only in the region between the electrolyte membrane 91 and the diffusion layer 93 in the thickness direction of the MEA 901.
[0062] The manufacturing method of the MEA 901 of this comparative embodiment is as follows. First, as shown in Fig. 6, a catalyst ink containing a catalyst is applied onto a substrate 94 to form a catalyst layer 92 on the substrate 94. Then, the catalyst layer 92 on the substrate 94 is superimposed on a diffusion layer 93, and the catalyst layer 92 is transferred from the substrate 94 to the diffusion layer 93 to form a laminate of the diffusion layer 93 and the catalyst layer 92. The laminate is joined to a separately prepared electrolyte membrane 91 to obtain the MEA 901.
[0063] When the catalyst ink is applied onto the substrate 94 as in this comparative embodiment, a relatively dense catalyst layer 92 is formed on the substrate. The catalyst layer 92 thus formed hardly penetrates into the gaps between the conductive fibers 931 constituting the diffusion layer 93 even after it is transferred to the diffusion layer 93 or bonded to the electrolyte membrane 91, and the layered structure is maintained. Therefore, the proportion of the area where the catalyst layer 92 and the conductive fibers 931a in this comparative embodiment are in contact with each other is less than half in the circumferential direction of the conductive fibers 931a.
[0064] (Comparative form 2) 7, the MEA 902 of the present comparative embodiment has an electrolyte membrane 91, a diffusion layer 93 composed of conductive fibers 931 and laminated on the electrolyte membrane 91, and a catalyst membrane 95 containing a catalyst and attached to the surface of conductive fibers 931b present inside in the thickness direction of the diffusion layer 93. The configuration of the electrolyte membrane 91 in the MEA 901 is similar to that of the electrolyte membrane 2 in the first embodiment.
[0065] The diffusion layer 93 of this embodiment is laminated on the electrolyte membrane 91 , and the conductive fibers 931 a present on the surface of the diffusion layer 93 facing the electrolyte membrane 91 are in contact with the electrolyte membrane 91 .
[0066] The catalyst film 95 in this embodiment is attached to the surfaces of the conductive fibers 931b present inside the diffusion layer 93 in the thickness direction. On the other hand, the catalyst film 95 is hardly attached to the conductive fibers 931a present on the surface of the diffusion layer 93.
[0067] The manufacturing method of the MEA 902 of this comparative embodiment is as follows. First, a catalyst ink containing a catalyst and a dispersion medium is prepared, and the liquid catalyst ink is applied onto the diffusion layer 93 using a slit die coater, a blade coater, a doctor blade, or the like. When the liquid catalyst ink is applied onto the diffusion layer 93 in this manner, the catalyst ink quickly penetrates between the conductive fibers 931 due to surface tension, and spreads throughout the diffusion layer 93. When the catalyst ink is dried in this state, the dispersion medium gradually evaporates from the outside of the diffusion layer 93, and the solid content in the catalyst ink is concentrated in the center of the diffusion layer 93 in the thickness direction. As a result of the above, a diffusion layer is obtained in which the catalyst film 95 is hardly attached to the conductive fibers 931a present on the surface of the diffusion layer 93, and the catalyst film 95 is attached to the surface of the conductive fibers 931b present in the center of the diffusion layer 93 in the thickness direction. The diffusion layer 93 obtained in this manner is then joined to the electrolyte membrane 91 to obtain the MEA 902.
[0068] When liquid catalyst ink is applied onto the diffusion layer 93 as in this comparative embodiment, the catalyst is concentrated in the center in the thickness direction of the diffusion layer 93, so that almost no catalyst film 95 is formed between the electrolyte membrane 91 and the diffusion layer 93. Therefore, the proportion of the area where the catalyst film 95 and the conductive fibers 931a in this comparative embodiment are in contact with each other is less than half in the circumferential direction of the conductive fibers 931a.
[0069] (Experimental Example) In this example, MEAs (specimens A1, B1, and B2) having the same structures as those of the first embodiment, the first comparative embodiment, and the second comparative embodiment were fabricated, and the power generation output of the resulting membrane electrode assemblies was evaluated. The detailed configurations and manufacturing methods of the specimens used in the evaluation of the power generation output are as follows.
[0070] [Test specimen A1] In preparing the specimen A1, first, an electrolyte membrane 2, a carbon cloth as a diffusion layer 3, and a catalyst ink containing a catalyst were prepared. The electrolyte membrane 2 used in preparing the specimen A1 was made of a perfluoroalkylsulfonic acid polymer and had a thickness of about 10 to 200 μm. The diffusion layer 3 used in preparing the specimen A1 was a carbon cloth made of twisted yarns made by twisting together conductive carbon fibers having a diameter of about 10 to 30 μm. The catalyst ink was made of a perfluoroalkylsulfonic acid polymer as an electrolyte, a precious metal catalyst, and a dispersion medium for dispersing the electrolyte and the precious metal catalyst. The solid content of the catalyst ink was 5 to 20 mass%.
[0071] Next, a catalyst ink was sprayed onto one side of the diffusion layer 3 using an ultrasonic spray coater. This caused catalyst particles to deposit on one side of the diffusion layer 3, forming a catalyst film 4. The coating amount of the catalyst film 4 per unit area of the diffusion layer 3 was 0.1 to 3 mg / cm. 2 Although not shown in the figure, when catalyst film 4 was formed under such conditions, the surface of catalyst film 4 had stripe-like irregularities along the surface of the conductive carbon fiber. Furthermore, in a plan view seen from the thickness direction of diffusion layer 3, gaps were formed on the surface of catalyst film 4.
[0072] After the catalyst film 4 was deposited on the diffusion layer 3, the diffusion layer 3 was heat pressed. The heating temperature in the heat press of the diffusion layer 3 was 160°C, the pressure was 2 MPa, and the pressing time was 3 minutes. Although not shown in the figure, the unevenness and gaps on the surface of the catalyst film 4 described above were still present even after the heat press.
[0073] After the diffusion layer 3 was heat pressed, the diffusion layer 3 and the electrolyte membrane 2 were overlapped so that the catalyst membrane 4 and the electrolyte membrane 2 were in contact with each other to form a laminate 10. The laminate 10 was heat pressed to bond the electrolyte membrane 2 and the diffusion layer 3 via the catalyst membrane 4. The heating temperature in the heat press of the laminate 10 was 140° C. The pressing pressure was appropriately set within the range of 0.5 to 2 MPa.
[0074] As a result, a specimen A1 was obtained having a structure similar to that of the MEA1 of embodiment 1. Although not shown in the figure, the interface between the catalyst membrane 4 and the electrolyte membrane 2 in the specimen A1 had irregularities along the surfaces of the conductive fibers 311a.
[0075] [Test specimen B1] The same electrolyte membrane 91, diffusion layer 93, and catalyst ink as those of the specimen A1 were used to prepare the specimen B1. In preparing the specimen B1, first, a liquid catalyst ink was applied to a fluororesin sheet serving as a substrate 94 using an ultrasonic spray coater. The catalyst ink was then dried to remove the dispersion medium from the catalyst ink, thereby forming a catalyst layer 92 on the substrate 94. The mass per unit area of the catalyst layer 92 was 0.1 to 3 mg / cm. 2 It was decided.
[0076] Next, the catalyst layer 92 formed on the substrate 94 was transferred onto one side of the diffusion layer 93. Thereafter, the diffusion layer 93 and the electrolyte membrane 91 were overlapped so that the catalyst layer 92 and the electrolyte membrane 91 were in contact with each other to form a laminate. The laminate was heat pressed to bond the electrolyte membrane 91 and the diffusion layer 93 via the catalyst layer 92. The heating temperature in the heat press of the laminate was 140°C. The pressing pressure was appropriately set within the range of 0.5 to 2 MPa.
[0077] As a result of the above, a specimen B1 having a structure similar to that of MEA901 of Comparative Example 1 was obtained.
[0078] [Test specimen B2] The same electrolyte membrane 91, diffusion layer 93, and catalyst ink as those of the specimen A1 were used to prepare the specimen B2. In preparing the specimen B2, first, a liquid catalyst ink was applied to one side of the diffusion layer 93 using a slit die coater. Thereafter, the catalyst ink was dried to remove the dispersion medium from the catalyst ink, thereby adhering the catalyst film 95 to the surface of the conductive carbon fiber present inside the diffusion layer 93. The amount of the catalyst film 95 applied per unit area of the diffusion layer 93 was 0.1 to 3 mg / cm. 2 It was decided.
[0079] Thereafter, the electrolyte membrane 91 and the diffusion layer 93 on which the catalyst membrane 95 was formed were stacked to form a laminate. The laminate was heat pressed to bond the electrolyte membrane 91 and the diffusion layer 93. The heating temperature in the heat press of the laminate was 140° C. The pressing pressure was appropriately set within the range of 0.5 to 2 MPa.
[0080] As a result of the above, a specimen B2 having a structure similar to that of the MEA902 of Comparative Example 2 was obtained.
[0081] The evaluation method for the power generation outputs of the test specimen A1 and the test specimens B1 and B2 is as follows.
[0082] [Method of measuring power output] A fuel cell 5 was assembled using the specimen A1 and specimens B1 and B2, and the fuel cell 5 was connected to an external load. In this state, the resistance of the external load was changed while generating power from the fuel cell 5, and a current-power curve was obtained. The maximum value of the power in this current-power curve was divided by the area of the anode of the specimen to calculate the maximum power density. The concentration of formic acid supplied as fuel was set to one of three levels: a standard concentration, a concentration 1.5 times the standard concentration, and a concentration 2.0 times the standard concentration.
[0083] Table 1 shows the ratio of the maximum power density of each test specimen to the maximum power density when test specimen B1 was supplied with formic acid of a reference concentration as fuel.
[0084] [Table 1]
[0085] The first surface 32 of the diffusion layer 3 of the specimen A1 has conductive fibers 311a whose half or more of the circumferential area is covered with the catalyst film 4. Therefore, as shown in Table 1, the specimen A1 exhibited a higher maximum power density than the specimen B1 having a dense catalyst layer 92, regardless of the concentration of formic acid used.
[0086] On the other hand, in the case of the test specimen B2, the catalyst film 95 was formed inside the diffusion layer 93, and there was almost no catalyst film 95 between the electrolyte membrane 91 and the diffusion layer 93. Therefore, regardless of the concentration of formic acid used, the test specimen B2 showed a lower maximum power density than the test specimen A1.
[0087] The above describes aspects of the membrane electrode assembly, its manufacturing method, and fuel cell according to the present invention based on the embodiments and experimental examples. However, the specific aspects of the membrane electrode assembly, its manufacturing method, and fuel cell according to the present invention are not limited to the aspects of the above-mentioned embodiments and experimental examples, and the configurations can be appropriately changed without departing from the gist of the invention. [Explanation of symbols]
[0088] 1 Membrane electrode assembly 2 Electrolyte membrane 3. Diffusion Layer 31 First surface 311 Conductive Fiber 4 Catalyst membrane
Claims
1. A membrane electrode assembly for use in a fuel cell configured to be capable of generating electricity using liquid fuel, comprising: The membrane electrode assembly includes an electrolyte membrane and A diffusion layer formed of conductive fibers and provided on both sides of the electrolyte membrane; a catalyst film including a catalyst and interposed between the electrolyte membrane and the conductive fiber constituting the diffusion layer; a membrane electrode assembly, the diffusion layer having a first surface on the electrolyte membrane side, the conductive fiber having a circumferential half or more area covered by the catalyst membrane.
2. 2 . The membrane electrode assembly according to claim 1 , wherein the entire surface in the circumferential direction of at least a portion of the conductive fibers present on the surface of the diffusion layer facing the electrolyte membrane is covered with the catalyst membrane.
3. 2. The membrane electrode assembly according to claim 1, wherein the catalyst film has a distribution such that an amount of the catalyst film present in a region of the diffusion layer from the first surface to a center in a thickness direction of the diffusion layer is greater than an amount of the catalyst film present in a region from a second surface, which is a back surface of the first surface, to the center in the thickness direction of the diffusion layer.
4. 4. The membrane electrode assembly according to claim 3, wherein, when the diffusion layer is divided into three or more regions in a thickness direction, the catalyst film has a distribution such that an amount of the catalyst film present in a region closest to the first surface is greatest, and an amount of the catalyst film present in a region that is farther away from the first surface decreases.
5. 2. The membrane electrode assembly of claim 1, wherein the diffusion layer is a carbon cloth.
6. 6. The membrane electrode assembly according to claim 5, wherein the carbon cloth is made of twisted conductive carbon fibers.
7. The membrane electrode assembly according to claim 5 , wherein an interface between the catalyst membrane and the electrolyte membrane has projections and recesses that follow the surfaces of the conductive fibers.
8. A fuel cell comprising the membrane electrode assembly according to any one of claims 1 to 7.
9. 9. The fuel cell according to claim 8, which is configured to be capable of using formic acid as the liquid fuel.
10. A method for producing a membrane electrode assembly according to any one of claims 1 to 7, comprising the steps of: forming the catalyst film by depositing catalyst particles containing the catalyst on one surface of the diffusion layer; Thereafter, the diffusion layer and the electrolyte membrane are stacked together so that the catalyst membrane and the electrolyte membrane are in contact with each other to form a laminate; and heat pressing the laminate to obtain the membrane electrode assembly.
11. The method for producing a membrane electrode assembly according to claim 10 , wherein the catalyst film formed on the diffusion layer has gaps in a plan view seen in a thickness direction of the diffusion layer.
12. The method for producing a membrane electrode assembly according to claim 10 , wherein the catalyst particles are not present on a back surface of the diffusion layer opposite to the surface having the catalyst membrane.
13. 11. The method for producing a membrane electrode assembly according to claim 10, further comprising the steps of: forming the catalyst membrane on the diffusion layer; heat pressing the diffusion layer; and stacking the heat pressed diffusion layer and the electrolyte membrane to form the laminate.
Citation Information
Patent Citations
Fuel cell membrane-electrode assembly, method of manufacturing the same, and solid polymer fuel cell using membrane-electrode assembly
JP2012199237A