Film for ultraviolet laser printing, printed matter and method for producing the same, and worked article
The ultraviolet laser printing film with titanium oxide and sealant layers addresses high costs and visibility issues in existing printing methods, offering clear and heat-sealable printing solutions for packages.
Patent Information
- Application Number
- JP2023062641
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-07
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-04-07
AI Technical Summary
Existing printing methods on packages using thermal printers, inkjet printers, and UV-curable inks face high running costs, printing errors, poor visibility due to dirt or uneven surfaces, and issues with print clarity and contamination from ink dust, while laser printing methods struggle with limited material choices and poor visibility of printed characters.
A film for ultraviolet laser printing with a film base material containing titanium oxide, a sealant layer, and optional barrier and resin layers, where the titanium oxide content is 0.2% by mass or more and crystallite size is 30 nm or more, ensuring excellent print clarity and heat sealability.
The film provides clear, high-visibility printing spots with excellent print clarity and heat sealability, reducing contamination and operational costs, and is suitable for various packaging applications.
Smart Images

Figure 2024149009000001 
Figure 2024149009000002 
Figure 2024149009000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a film for ultraviolet laser printing, a printed matter and a method for producing the same, and a processed product. [Background technology]
[0002] 2. Description of the Related Art Conventionally, labeling or inkjet printing has been used to display dates such as manufacturing dates and shipping dates, and variable information such as bar codes, on packaging such as containers that hold contents. A method of printing by irradiation with laser light has also been proposed. For example, Patent Document 1 discloses a laser-printing laminate manufactured by applying white ink, black ink and overprint varnish (OP varnish) to the aluminum-vapor-deposited surface of aluminum-vapor-deposited paper, with the aim of providing a laser-printing laminate and a printed body that can produce dark characters at high speed by irradiation with laser light and have printed areas that are excellent in various resistances. Furthermore, Patent Document 2 describes an ink composition used to form a laser marking layer that contains first titanium oxide particles having an average particle size of 150 nm or less and changes color when irradiated with an ultraviolet laser, with the aim of providing a technology that generates relatively little heat and is preferably applicable to laser marking of packaging materials. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 9-123607 [Patent Document 2] JP 2020-75943 A Summary of the Invention [Problem to be solved by the invention]
[0004] One method of printing on the surfaces of packages, labels, adhesive tapes, etc. is to directly apply ink to the surface of the package using a thermal printer or inkjet printer, which is currently widely used. However, consumables such as ink ribbons for thermal printers and ink for inkjet printers are expensive, and there is a problem that the running costs are high to print a lot of variable information. In addition, failure to replace these consumables may result in printing errors. Furthermore, variable information is also directly printed on the package by offset printing using UV-curable ink, but stains on the surface of the package or uneven thickness of the package may result in blurred printing or missing characters. In addition, the method described in Patent Document 1 can be performed at high speed, but since it is a technology in which the upper layer, which easily absorbs laser light, is removed by irradiating a CO2 laser light, the lower layer is exposed, and characters, etc. that are visible due to the difference in color between the upper layer and the lower layer are formed, the upper layer is limited to a material that easily absorbs laser light, and conversely, the lower layer is limited to a material that does not easily absorb laser light and has a color contrast with the upper layer. In other words, the upper layer is a carbon black-based material (black color) that easily absorbs laser light, and the lower layer is a titanium oxide-based material (white color), and the characters, etc. formed by irradiating the laser light are white characters on a black background, which is poor in visibility. In addition, when removing the upper layer, there is a problem that the ink in the upper layer turns into dust, which causes contamination of the working environment. Furthermore, when printing is performed with an ultraviolet laser on a coating layer prepared using the ink composition described in Patent Document 2, the printing clarity of each printing spot may be poor in some cases.
[0005] The present invention aims to provide a film for ultraviolet laser printing that, when irradiated with an ultraviolet laser, produces print spots with excellent print clarity for each point and has heat sealability. The present invention also aims to provide a printed matter and a method for producing the same, in which the irradiated area of the film for ultraviolet laser printing is discolored by irradiating the film with an ultraviolet laser. The present invention also aims to provide a processed product made using the film for ultraviolet laser printing or the printed matter. [Means for solving the problem]
[0006] The present inventors have discovered that the above problems can be solved in a film for ultraviolet laser printing having a sealant layer on at least one side of a film substrate to which titanium oxide is added, by setting the content of titanium oxide in the film to a specific value or more and setting the crystallite size of the titanium oxide to a specific value or more. The present invention relates to the following: <1> ~ <10> Regarding. <1> A film for ultraviolet laser printing comprising a film substrate having titanium oxide added thereto and a sealant layer on at least one surface of the film substrate, wherein the content of titanium oxide in the film substrate is 0.2 mass% or more and the crystallite size of the titanium oxide is 30 nm or more. <2> The crystallite size of the titanium oxide is 53 nm or less. <1> 2. A film for ultraviolet laser printing according to claim 1. <3> The titanium oxide is a rutile type titanium oxide, and the diffraction angle of the titanium oxide is 27.60° or less. <1> or <2> 2. A film for ultraviolet laser printing according to claim 1. <4> The resin constituting the film substrate is at least one selected from the group consisting of polyolefin, polyester, and polyvinyl chloride. <1> ~ <3> 10. A film for ultraviolet laser printing according to any one of claims 1 to 9. <5> The content of titanium oxide in the film substrate is 50% by mass or less. <1> ~ <4> 10. A film for ultraviolet laser printing according to any one of claims 1 to 9. <6> A barrier layer is provided between the film substrate and the sealant layer. <1> ~ <5> 10. A film for ultraviolet laser printing according to any one of claims 1 to 9. <7> <1> ~ <6> 1. A printed matter obtained from the ultraviolet laser printing film described in any one of claims 1 to 9, wherein the printed matter has, at least in a portion thereof, a printed area containing discolored titanium oxide, and the ratio of the Raman intensity originating from titanium oxide in the printed area to the Raman intensity originating from titanium oxide in the non-printed area is 0.70 or less. <8> <1> ~ <6> 2. A film for ultraviolet laser printing according to any one of the items 1 to 11, or <7> A processed product using the printed matter described in . <9> <1> ~ <6> irradiating an ultraviolet laser onto the ultraviolet laser printing film according to any one of the above items 1 to 3, thereby discoloring the irradiated area, thereby printing the film. A method for producing printed matter. <10> the printing step is a step of irradiating with an ultraviolet laser so that the ratio of the Raman intensity originating from titanium oxide in the printed area to the Raman intensity originating from titanium oxide in the non-printed area is 0.70 or less; <9> A method for producing a printed matter according to claim 1. Effect of the Invention
[0007] According to the present invention, a film for ultraviolet laser printing is provided that, when irradiated with an ultraviolet laser, print spots with excellent print clarity for each point are obtained and further has heat sealability. Also, according to the present invention, a printed matter in which the irradiated area is discolored by irradiating the film for ultraviolet laser printing with an ultraviolet laser and a method for producing the same are provided. Furthermore, according to the present invention, a processed product made of the film for ultraviolet laser printing or the printed matter is provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] [UV laser printing film] The ultraviolet laser printing film of the present invention (hereinafter simply referred to as "film" or "printing film") is a film for ultraviolet laser printing having a film substrate to which titanium oxide is added and a sealant layer on at least one side of the film substrate, wherein the content of titanium oxide in the film substrate is 0.2 mass% or more and the crystallite size of the titanium oxide is 30 nm or more. By adopting the above-mentioned constitution, there is provided a film for ultraviolet laser printing which, when irradiated with an ultraviolet laser, gives print spots which are excellent in print clarity for each individual point and have heat sealability. Although the detailed reasons why the above-mentioned effects are obtained are unclear, some of the reasons are thought to be as follows. By adding titanium oxide to the film substrate, the titanium oxide changes color by irradiation with an ultraviolet laser, making it possible to print. The color change of the titanium oxide is considered to be caused by the change in the ionic valence of the titanium oxide added to the film substrate from tetravalent to trivalent, which causes oxygen defects, and the color changes from white to black, which makes it visible. The ionic valence of titanium oxide is considered to change when it is irradiated with light energy corresponding to the band gap of titanium oxide. The band gap of titanium oxide varies depending on the crystal system, but is generally about 3.0 to 3.2 eV, and the wavelength of light corresponding to this is 420 nm or less. Therefore, even if a laser beam with a wavelength exceeding 420 nm (for example, 532 nm, 1064 nm, 10600 nm) is used, it is difficult to perform printing due to the change in the ionic valence of titanium oxide as in the present invention. In this case, by making the amount of titanium oxide added to the film substrate 0.2 mass % or more, excellent visibility can be obtained, and the printing clarity of each point is excellent. In addition, when the crystallite size of titanium oxide is 30 nm or more, there are few crystal defects, the recombination of excited electrons and holes is suppressed, and titanium oxide is easily reduced and discolored, which is thought to result in printed spots with excellent printing clarity for each dot. In the following description, "printable area" refers to the area (portion) where printing is possible due to discoloration of the titanium oxide contained in the film substrate, i.e., the titanium oxide in the portion irradiated with the ultraviolet laser changes color from white to black upon irradiation with the ultraviolet laser, and "printable area" refers to the portion of the printable area where the titanium oxide has actually changed color, i.e., the portion where the titanium oxide has changed color due to irradiation with the ultraviolet laser and become visible (the portion irradiated with the ultraviolet laser). Additionally, "non-printable area" refers to the area (portion) of the printable area where the titanium oxide has not changed color, i.e., the area (portion) not irradiated with the ultraviolet laser. Furthermore, by having a sealant layer on at least one side of the film substrate, heat sealability is imparted, and a film for ultraviolet laser printing having heat sealability is provided. Furthermore, by having a sealant layer, it is preferable that gas barrier properties are also imparted. Here, gas barrier properties mainly mean barrier properties against at least one selected from oxygen and water vapor, and may also have barrier properties against other gases. The printing film of this embodiment preferably has at least water vapor barrier properties, and in addition to this, it is preferable that it has oxygen barrier properties.
[0009] The ultraviolet laser printing film of this embodiment has a film substrate (film substrate layer) containing titanium oxide and a sealant layer on at least one side of the film substrate. The sealant layer is preferably provided on the top layer of at least one side of the printing film, and more preferably on the top layer of one side. The film substrate may have a sealant layer on the entire surface, or may have a sealant layer on a part of the film substrate that requires heat sealability. In addition, a barrier layer may be provided between the film substrate and the sealant layer, and an adhesive layer may be provided between the film substrate and the sealant layer, between the film substrate and the barrier layer, or between the barrier layer and the sealant layer. Furthermore, the printing film may have a sealant layer on one side of the film substrate and a resin layer on the other side for the purpose of protecting the film substrate. The resin layer is preferably excellent in transparency. An adhesive layer may be provided between the resin layer and the film substrate. The ultraviolet laser printable film of the present invention will be described in more detail below.
[0010] <Titanium oxide> The film of the present embodiment has a film substrate to which titanium oxide is added in order to obtain sufficient print density and improve the print clarity of each individual point, and the content of titanium oxide in the film substrate is 0.2% by mass or more, preferably 0.3% by mass or more, more preferably 0.5% by mass or more, even more preferably 1.0% by mass or more, and even more preferably 1.2% by mass or more, and from the viewpoint of suppressing smoke generation during ultraviolet laser printing, the content of titanium oxide is preferably 50% by mass or less, more preferably 30% by mass or less, even more preferably 15% by mass or less, even more preferably 10% by mass or less, and particularly preferably 5.0% by mass or less. When irradiating with an ultraviolet laser and printing, smoke may be generated, which is thought to be due to scattering of titanium oxide. When titanium oxide is heated by irradiation with an ultraviolet laser, it is thought that a phenomenon occurs in which discolored titanium oxide is detached from the film substrate, and smoke is generated due to such detachment. By setting the content of titanium oxide in the film substrate to the above upper limit or less, smoke generation is suppressed, which is preferable. It is sufficient that at least the printable region of the film substrate contains titanium oxide, and the non-printed region may have a titanium oxide content below the lower limit. From the viewpoint of ease of production, it is preferable that the entire region of the film substrate contains titanium oxide within the above range. The content of titanium oxide in the film substrate is measured by the method described in the Examples.
[0011] Titanium oxide is added internally to the film substrate, and more preferably is obtained by adding titanium oxide to a film substrate raw material and forming the film substrate into a sheet. The titanium oxide contained in the film substrate is represented by the composition formula TiO2, and is also called titanium dioxide or titania. In this embodiment, the crystallite size of titanium oxide in the film substrate of the ultraviolet laser printing film is 30 nm or more. If the crystallite size of titanium oxide in the film is less than 30 nm, there are many crystal defects, and the recombination of excited electrons and holes excited by ultraviolet laser irradiation is likely to occur, resulting in the titanium oxide being difficult to reduce, and the printing clarity of each point is poor. The crystallite size of titanium oxide is preferably 35 nm or more, more preferably 40 nm or more. In addition, the upper limit of the crystallite size of titanium oxide is not particularly limited, but from the viewpoint of the dispersibility of titanium oxide during the production of the film substrate and the resulting dispersibility in the film substrate, it is preferably 60 nm or less, more preferably 56 nm or less, and even more preferably 53 nm or less. If the upper limit of the crystallite size of titanium oxide is within the above range, the dispersion stability of titanium oxide during production is good, and as a result, the dispersibility in the film substrate and the printing uniformity are excellent, which is preferable. The crystallite size of titanium oxide is measured by the method described in the Examples. The crystallite size is determined by the Scherrer equation, and the Bragg angle is the measured value of the maximum intensity derived from the 101 plane in the case of anatase titanium oxide, or the 110 plane in the case of rutile titanium oxide.
[0012] The titanium oxide may have a crystalline structure or may be amorphous, and is preferably at least one selected from rutile titanium oxide, anatase titanium oxide, brookite titanium oxide, and amorphous titanium oxide. From the standpoint of availability and stability, it is more preferably at least one selected from rutile titanium oxide and anatase titanium oxide, and even more preferably rutile titanium oxide. The crystal form of titanium oxide can be determined by known methods, specifically, by analysis of Raman spectrum, XRD pattern, etc. For example, when identifying from Raman spectrum, the crystal form of rutile type is generally determined as 447±10 cm -1 , 609±10cm -1A peak was confirmed at 395±10cm for the anatase type. -1 , 516±10cm -1 , 637±10cm -1 A peak is observed at . The titanium oxide may be used alone or in combination of two or more kinds.
[0013] When the titanium oxide is rutile type titanium oxide, the diffraction angle of the titanium oxide is preferably 27.60° or less from the viewpoint of print clarity for each point. The Bragg angle of rutile type titanium oxide is originally 27.40°, but if the crystallinity is low, the diffraction angle tends to be high. If the diffraction angle of titanium oxide exceeds 27.60°, the crystallinity is low and discoloration is suppressed, so the print clarity for each point tends to be poor. When the titanium oxide is rutile type titanium oxide, the diffraction angle of the titanium oxide is preferably 27.60° or less, more preferably 27.55° or less, and even more preferably 27.50° or less. The diffraction angle of titanium oxide, in the case of rutile type, is the measured value of the maximum intensity resulting from the 110 plane, as described above.
[0014] The shape of the titanium oxide is not particularly limited, and may be any shape such as amorphous, spherical, rod-like, or needle-like. When the titanium oxide is amorphous or spherical, the particle size of the titanium oxide is not particularly limited, but from the viewpoint of obtaining a film substrate having excellent surface smoothness, it is preferably 0.01 μm or more, more preferably 0.05 μm or more, even more preferably 0.10 μm or more, still more preferably more than 0.15 μm, particularly preferably 0.16 μm or more, and is preferably 20.0 μm or less, more preferably 5.0 μm or less, even more preferably 1.0 μm or less, still more preferably 0.50 μm or less, particularly preferably 0.30 μm or less.
[0015] In addition, when titanium oxide is needle-shaped, the long diameter of titanium oxide is not particularly limited, but from the viewpoint of obtaining a film substrate having excellent surface smoothness, it is preferably 0.1 μm or more, more preferably 0.5 μm or more, even more preferably 1.5 μm or more, and preferably 50.0 μm or less, more preferably 30.0 μm or less, and even more preferably 15.0 μm or less. In addition, the short diameter is preferably 0.01 μm or more, more preferably 0.03 μm or more, even more preferably 0.05 μm or more, and preferably 3.0 μm or less, more preferably 1.5 μm or less, and even more preferably 1.0 μm or less. In addition, when titanium oxide is needle-shaped, the aspect ratio (long diameter / short diameter) is preferably 5 or more, more preferably 10 or more, even more preferably 15 or more, and preferably 300 or less, more preferably 100 or less, and even more preferably 30 or less. The average particle size, major axis, and minor axis of titanium oxide are measured by the method described in the Examples. The particle size, major axis, and minor axis values of titanium oxide used as a raw material may be adopted, or catalog values of the particle size, major axis, and minor axis of titanium oxide used as a raw material may be adopted.
[0016] <Binding resin> The resin constituting the film substrate (hereinafter also simply referred to as "resin") is not particularly limited as long as it can be processed into a film by incorporating titanium oxide, and may be appropriately selected from among known thermoplastic resins. Specific examples include polyester-based resins such as polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polylactic acid, and polybutylene succinate; polyolefin-based resins such as polyvinyl chloride, polyvinylidene chloride, polybutene, polybutadiene, ethylene-vinyl acetate copolymer, polyethylene, polypropylene, ethylene-propylene copolymer, and polymethylpentene; polycarbonate; polyurethane; polyamide; polyacrylonitrile; poly(meth)acrylate; and the like. Among these, the resin constituting the film substrate is preferably a polyolefin such as polyethylene, polypropylene, ethylene-propylene copolymer, polyester such as polyethylene terephthalate, polybutylene terephthalate, polylactic acid, polybutylene succinate, or polyvinyl chloride, from the viewpoint of being versatile, having high UV transmittance, and enabling discoloration of titanium oxide to the inside of the film substrate, more preferably at least one selected from the group consisting of polyethylene, polypropylene, ethylene-propylene copolymer, polyethylene terephthalate, polylactic acid, and polybutylene succinate, and even more preferably at least one selected from the group consisting of polyethylene, polypropylene, ethylene-propylene copolymer, polyethylene terephthalate, polylactic acid, and polybutylene succinate. The resin constituting the film substrate is more preferably a polyolefin, even more preferably at least one selected from the group consisting of polyethylene and polypropylene, and particularly preferably contains at least polypropylene. In addition, it is preferable to use a biodegradable resin, polyester, as the resin constituting the film substrate in terms of reducing the environmental load. Examples of such resins include polylactic acid and polybutylene succinate. These resins may be used alone or in combination of two or more.
[0017] The resin content in the film substrate is, from the viewpoints of improving print density, improving print clarity for each point, and suppressing smoke generation during irradiation with an ultraviolet laser, preferably 50% by mass or more, more preferably 70% by mass or more, even more preferably 85% by mass or more, still more preferably 90% by mass or more, particularly preferably 95.0% by mass or more, and is 99.8% by mass or less, preferably 99.7% by mass or less, more preferably 99.5% by mass or less, even more preferably 99.0% by mass or less, and still more preferably 98.8% by mass or less.
[0018] <Other ingredients> The film substrate of the present embodiment may contain other components in addition to the titanium oxide and resin described above. Examples of other components include inorganic particles other than titanium oxide. Examples of inorganic particles include kaolin, talc, calcium carbonate, calcium sulfite, gypsum, calcined kaolin, white carbon, amorphous silica, delaminated kaolin, diatomaceous earth, magnesium carbonate, aluminum hydroxide, calcium hydroxide, magnesium hydroxide, zinc oxide, zinc hydroxide, etc., and among these, calcium carbonate is preferred from the viewpoint of improving the whiteness of the film and improving the print density. The calcium carbonate may be heavy calcium carbonate or light calcium carbonate, and is not particularly limited. From the viewpoint of gloss, light calcium carbonate having a small particle size is preferable. Furthermore, by containing inorganic particles other than titanium oxide, preferably calcium carbonate, scattering of titanium oxide during irradiation with an ultraviolet laser is further suppressed, and smoke generation is also suppressed, which is preferable.
[0019] The shape of the inorganic particles is not particularly limited, and may be any shape such as amorphous, spherical, rod-like, or needle-like. When the inorganic particles are amorphous or spherical, the particle size of the inorganic particles is not particularly limited, but from the viewpoint of obtaining a film substrate having excellent surface smoothness and suppressing smoke generation, the particle size is preferably 0.1 μm or more, more preferably 0.3 μm or more, even more preferably 0.5 μm or more, and is preferably 5.0 μm or less, more preferably 4.0 μm or less, even more preferably 3.0 μm or less. In addition, when the inorganic particles are needle-shaped, the major axis of the inorganic particles is not particularly limited, but from the viewpoint of obtaining a film substrate with excellent surface smoothness and suppressing smoke generation, it is preferably 0.1 μm or more, more preferably 0.3 μm or more, even more preferably 0.5 μm or more, and preferably 50.0 μm or less, more preferably 30.0 μm or less, and even more preferably 15.0 μm or less. In addition, the minor axis is preferably 0.05 μm or more, more preferably 0.10 μm or more, even more preferably 0.3 μm or more, and preferably 5.0 μm or less, more preferably 4.0 μm or less, and even more preferably 3.0 μm or less. In addition, when the inorganic particles are needle-shaped, the aspect ratio (major axis / minor axis) is preferably 5 or more, more preferably 10 or more, even more preferably 15 or more, and preferably 300 or less, more preferably 100 or less, and even more preferably 50 or less.
[0020] As mentioned above, calcium carbonate is preferred as the inorganic particles. When the film substrate contains inorganic particles, the content of the inorganic particles, preferably calcium carbonate, in the film substrate is, from the viewpoint of improving printability and suppressing smoke generation, preferably 1 mass % or more, more preferably 2 mass % or more, even more preferably 3 mass % or more, and is preferably 60 mass % or less, more preferably 55 mass % or less, even more preferably 50 mass % or less, and even more preferably 45 mass % or less. The inorganic particles other than titanium oxide may be used alone or in combination of two or more. When two or more types are used in combination, the total content of the inorganic particles other than titanium oxide is preferably within the above range.
[0021] In the present embodiment, in addition to the components described above, other components may be added to the film substrate within a range that does not impair the effects of the present invention. Examples of such components include antistatic agents, antiblocking agents, antioxidants, UV absorbers, HALS, plasticizers, lubricants, flame retardants, release agents, and colorants.
[0022] [Thickness] From the viewpoint of improving strength, the thickness of the film substrate is preferably 10 μm or more, more preferably 20 μm or more, even more preferably 40 μm or more, even more preferably 50 μm or more, still more preferably 55 μm or more, and is preferably 700 μm or less, more preferably 500 μm or less, even more preferably 350 μm or less, and still more preferably 250 μm or less. When the thickness of the film substrate is within the above range, when the film substrate is irradiated with an ultraviolet laser, deterioration of the resin is observed near the surface of the film substrate, but since the thickness of the film substrate is sufficient, a decrease in the strength of the printed matter is suppressed, which is preferable. The thickness of the film substrate is measured by the method described in the Examples.
[0023] <Manufacturing method of film substrate> The film substrate can be obtained by preparing a raw material composition by melt-kneading at least titanium oxide and resin, and, if necessary, materials such as inorganic pigments other than titanium oxide, forming this into a film, and then appropriately stretching it. In preparing the raw material composition, a master batch containing titanium oxide or an inorganic pigment other than titanium oxide at a high concentration may be prepared and then mixed with the resin. Alternatively, materials that have been uniformly mixed in advance may be charged into the molding machine, or the materials may be mixed in a hopper or kneader that is integrated with the molding machine. The method for forming the composition into a film may be appropriately selected from conventionally known methods, such as melt extrusion, melt casting, and calendering. The film substrate may be prepared by mixing titanium oxide with the above-mentioned resin so that the content of titanium oxide in the printing region of the film substrate falls within the above range.
[0024] In the present embodiment, when the film substrate is stretched, the stretching may be uniaxial stretching or biaxial stretching. The stretching is preferably performed at least in the longitudinal direction, and may also be performed in the transverse direction.
[0025] [Sealant Layer] The printing film of this embodiment has a sealant layer on at least one surface of the film substrate. The sealant layer is a layer that melts and adheres by heating, ultrasonic waves, etc. The printing film of this embodiment may have a sealant layer on both surfaces of the film substrate. In addition, from the viewpoint of imparting heat sealability, the sealant layer is provided as the uppermost layer on at least one surface, and two or more sealant layers may be formed on one surface. The sealant layer may be provided at least on the surface of the film substrate opposite to the surface on which ultraviolet laser printing is performed, but may also be provided on the surface on which printing is performed.
[0026] The resin constituting the sealant layer (hereinafter also referred to as "sealant layer resin") is not particularly limited, and examples thereof include vinyl chloride resin, vinyl acetate resin, vinyl chloride-vinyl acetate copolymer, acrylic resin, polyester resin, olefin resin, styrene resin, styrene-acrylic resin (e.g., styrene-acrylic acid copolymer), ethylene-acrylic resin (ethylene-(meth)acrylic acid copolymer), and modified products thereof. The sealant layer resin may be used alone or in combination of two or more kinds.
[0027] The resin for the sealant layer may be either a synthetic product or a commercially available product. As the commercially available product, the one used in the examples may be used.
[0028] The sealant layer may be formed by laminating with melt extrusion, adhesive, etc., and may be formed by preparing a coating liquid for the sealant layer and applying the coating liquid. A known adhesive may be used as the adhesive. The sealant layer may be formed of two or more layers. When the sealant layer is laminated with a resin film for the sealant layer with an adhesive, etc., the resin film may be unstretched or may be uniaxially or biaxially stretched.
[0029] When the sealant layer is formed by lamination, from the viewpoints of heat sealability and gas barrier property, the resin for the sealant layer more preferably contains at least one selected from the group consisting of polyolefin resins, polyamide resins, polyester resins, and polyvinylidene chloride resins, more preferably contains a polyolefin resin, and even more preferably is a polyolefin resin. When the sealant layer is a laminated sealant layer consisting of two or more layers, from the viewpoint of heat sealability, the layer is preferably a polyolefin resin layer, more preferably a polyethylene resin layer.
[0030] From the viewpoint of heat sealability and gas barrier property, the polyolefin resin is more preferably at least one selected from the group consisting of polyethylene, polypropylene and an ethylene-propylene copolymer, and even more preferably at least one of polyethylene and polypropylene. The polyethylene may be low density polyethylene (LDPE), linear low density polyethylene (LLDPE), medium density polyethylene (MDPE), or high density polyethylene (HDPE).
[0031] Examples of polyamide resins include nylon 6, nylon 11, nylon 12, nylon 66, nylon 610, and nylon 612.
[0032] Examples of polyester resins include polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polybutylene terephthalate (PBT), and derivatives thereof. Many of the biodegradable resins described below also fall under the category of polyester resins.
[0033] Polyvinylidene chloride resin (PVDC) is a synthetic resin obtained by polymerizing vinylidene groups containing chlorine, and may be a copolymer with vinyl chloride, acrylonitrile, or the like.
[0034] Examples of biodegradable resins include polylactic acid (PLA), polybutylene succinate (PBS), polybutylene succinate adipate (PBSA), and 3-hydroxybutanoic acid-3-hydroxyhexanoic acid copolymer (PHBH). Among these, polylactic acid (PLA) and polybutylene succinate (PBS) are preferred, and polybutylene succinate (PBS) is more preferred.
[0035] As the sealant layer, a laminate film in which two or more resins are laminated may be used, such as a polyethylene / polypropylene laminate film, a polyamide resin / polyvinylidene chloride resin laminate film, or a polyethylene / polyester resin laminate film.
[0036] When an adhesive is used to bond the sealant layer or a barrier layer described later, the adhesive used is not particularly limited and may be any of a solventless type, an organic solvent type, a water-based type, etc., but from the viewpoints of adhesion and ease of production, it is preferable to use an organic solvent type adhesive or a solventless type adhesive. Examples of the main component constituting the adhesive include (meth)acrylic acid ester copolymers, α-olefin copolymers, ethylene-vinyl acetate copolymers, polyvinyl alcohol, polyurethane, styrene-butadiene copolymers, polyvinyl chloride, epoxy resins, melamine resins, silicone resins, natural rubber, casein, starch, etc. Among these, from the viewpoints of easy availability and obtaining good adhesive properties, (meth)acrylic acid ester copolymers, ethylene-vinyl acetate copolymers, and polyurethanes are preferred, and polyurethanes are more preferred. As the adhesive, a commercially available adhesive may be used as appropriate, for example, a combination of Nipporan ID-816 (manufactured by Tosoh Corporation) and HARDENER 300 (manufactured by Tosoh Corporation), or a combination of Dikdry LX-500 (manufactured by DIC Corporation) and Dikdry KW-75 (manufactured by DIC Corporation). Note that, an adhesive may be applied to the sealant layer or barrier layer, and then the sealant layer or barrier layer and the film substrate may be laminated thereto, or an adhesive may be applied to the film substrate and then the sealant layer or barrier layer may be laminated thereto, or an adhesive may be applied to both the sealant layer or barrier layer and the film substrate and then the two may be laminated together; although there are no particular limitations, from the viewpoints of adhesion and ease of production, it is preferable to apply an adhesive to the sealant layer or barrier layer and then laminate the film substrate.
[0037] The method for applying the adhesive may be appropriately selected from conventionally known methods, and is not particularly limited. Examples of the method include a roll coater, a die coater, a gravure coater, and a spray coater. The amount of adhesive applied is not particularly limited, but the amount applied (coating amount) after drying is preferably 1 g / m from the viewpoint of enhancing the adhesion between the sealant layer or barrier layer and the film base layer. 2 More preferably, 2 g / m 2 More preferably, 3 g / m 2 and preferably 40 g / m 2 Less than 20 g / m, more preferably 20 g / m 2 More preferably, 10 g / m 2 The following is the result.
[0038] When the sealant layer is formed using a coating liquid, the resin for the sealant layer is not particularly limited as long as it has heat-sealing properties, but is more preferably one or more selected from styrene-butadiene copolymers; olefin-unsaturated carboxylic acid copolymers such as ethylene-acrylic acid copolymers and ethylene-methacrylic acid copolymers; biodegradable resins; polyolefin resins such as polyethylene and polypropylene; and acrylic resins such as methyl acrylate copolymers, methyl methacrylate copolymers, styrene-acrylic copolymers, and styrene-methacrylic copolymers.
[0039] Among these, it is more preferable that the resin is at least one selected from a styrene-acrylic acid copolymer and an olefin-unsaturated carboxylic acid copolymer. In this specification, the acrylic resin does not include an olefin-unsaturated carboxylic acid copolymer.
[0040] The olefin-unsaturated carboxylic acid copolymer may be a salt in which the carboxyl groups derived from the unsaturated carboxylic acid monomer are partially or completely neutralized with an alkali metal hydroxide, ammonia, an alkylamine, an alkanolamine, or the like. Examples of the olefin monomer of the olefin-unsaturated carboxylic acid copolymer include ethylene, propylene, butadiene, etc. These may be used alone or in combination of two or more. Among these, ethylene is preferred.
[0041] Examples of the unsaturated carboxylic acid monomer of the olefin-unsaturated carboxylic acid copolymer include unsaturated carboxylic acids such as acrylic acid, methacrylic acid, crotonic acid, cinnamic acid, itaconic acid, fumaric acid, maleic acid, and butene tricarboxylic acid; unsaturated polycarboxylic acid alkyl esters having at least one carboxy group such as itaconic acid monoethyl ester, fumaric acid monobutyl ester, and maleic acid monobutyl ester; unsaturated sulfonic acid monomers or salts thereof such as acrylamidopropanesulfonic acid, acrylic acid sulfoethyl sodium salt, and methacrylic acid sulfopropyl sodium salt; and the like. These may be used alone or in combination of two or more. Among these, unsaturated carboxylic acids are preferred, acrylic acid and methacrylic acid are more preferred, and acrylic acid is particularly preferred. Therefore, the olefin-unsaturated carboxylic acid copolymer is preferably at least one of an ethylene-acrylic acid copolymer and an ethylene-methacrylic acid copolymer.
[0042] The ethylene-unsaturated carboxylic acid copolymer is preferably obtained by emulsion polymerization of ethylene and the unsaturated carboxylic acid monomer. As the ethylene-unsaturated carboxylic acid copolymer, ethylene-acrylic acid copolymer and ethylene-methacrylic acid copolymer are preferable. As long as the effect of the present invention is not impaired, the copolymer may contain a monomer composed of another compound copolymerizable with ethylene and the unsaturated carboxylic acid monomer.
[0043] Specific examples of ethylene-unsaturated carboxylic acid copolymers include ZAIXXEN (registered trademark) A, ZAIXXEN (registered trademark) AC (both manufactured by Sumitomo Seika Chemicals Co., Ltd.), Chemipearl S series (manufactured by Mitsui Chemicals, Inc.), MFHS1279, MP498345N, MP4983R, MP4990R (all manufactured by Michaelman LLC).
[0044] The biodegradable resin is preferably one or more selected from polylactic acid (PLA), polybutylene succinate (PBS), polybutylene succinate adipate (PBSA), polybutylene adipate terephthalate (PBAT), and poly(3-hydroxybutyrate-co-hydroxyhexanoate) (PHBH), more preferably one or more selected from polylactic acid and polybutylene succinate, and particularly preferably polylactic acid. By using a biodegradable resin as the sealant layer in this embodiment, the environmental load can be reduced.
[0045] The polylactic acid may be either a commercially available product or a synthetic product. Examples of commercially available products include Randy PL-1000 and Randy PL-3000 (aqueous dispersion of polylactic acid, manufactured by Miyoshi Oil & Fat Co., Ltd.).
[0046] When the sealant layer is provided by coating, the coating liquid for the sealant layer may contain, in addition to the resin for the sealant layer (water-dispersible polymer), a lubricant, a pigment, an antifoaming agent, a viscosity adjuster, a surfactant, a leveling agent, a colorant, etc. Since these other components tend to deteriorate the heat sealability, the total content of the other components is preferably 30 mass % or less, more preferably 10 mass % or less, and even more preferably 5 mass % or less, of the solid content of the sealant layer.
[0047] From the viewpoint of obtaining high heat seal peel strength, the content of the resin for the sealant layer in the solid content of the coating liquid for the sealant layer is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more.
[0048] The device used for applying the coating liquid for the sealant layer is not particularly limited, and may be appropriately selected from commonly used coating devices, such as an air knife coater, a blade coater, a gravure coater, a rod blade coater, a roll coater, a reverse roll coater, a Mayer bar coater, a curtain coater, a die slot coater, a champlex coater, a metering blade type size press coater, a short dwell coater, a spray coater, a gate roll coater, and a lip coater.
[0049] The drying conditions for the sealant layer are not particularly limited, but the drying temperature is preferably 50 to 120° C., and the drying time is preferably 5 to 120 seconds. The drying equipment for drying the applied sealant layer is not particularly limited, and known equipment can be used. Examples of the drying equipment include a hot air dryer, an infrared dryer, an explosion-proof dryer, and a hot plate.
[0050] The amount of the sealant layer applied is preferably 1 g / m from the viewpoint of heat seal peel strength. 2 More preferably, 2 g / m 2 and preferably 30 g / m 2 Less than 20 g / m, more preferably 20 g / m 2 When the printing film has two or more sealant layers, the total amount of the sealant applied is preferably within the above range.
[0051] [Barrier Layer] The printing film of the present embodiment preferably has a barrier layer between the film substrate and the sealant layer. The barrier layer is a layer having a function of mainly preventing the permeation of oxygen gas. The barrier layer may be formed by applying a coating liquid containing a polymer selected from the group consisting of water-dispersible polymers and water-soluble polymers, by laminating a resin having a barrier property by melt extrusion, adhesive, or the like, by forming a vapor deposition layer selected from the group consisting of a metal vapor deposition layer and an inorganic vapor deposition layer, or by laminating a resin film having a vapor deposition layer selected from the group consisting of a metal vapor deposition layer and an inorganic vapor deposition layer.
[0052] (Water-suspended polymer) In this embodiment, the water-suspendable polymer used in the barrier layer is a polymer having a solubility of 10 g / L or less in water at 25° C. In this embodiment, the water-suspendable polymer is preferably derived from a polymer (particle) dispersed in an emulsion. The water-suspendable polymer and water-soluble resin used in the barrier layer are not particularly limited, but examples thereof include urethane-based resins, vinylidene chloride-based resins, olefin resins, polyester resins, nylon resins, epoxy resins, melamine resins, polyvinyl alcohol-based resins, acrylonitrile-based resins, polycarboxylic acid-based resins, and silicone resins. The water-suspendable polymer may be used alone or in combination of two or more. Among them, the water-suspendable polymer is preferably at least one selected from the group consisting of urethane-based resins and vinylidene chloride-based resins. By forming the barrier layer using these resins, excellent gas barrier properties (oxygen barrier properties) can be exhibited.
[0053] The urethane resin can be produced by a known production method. For example, the urethane resin can be obtained by reacting a polyisocyanate compound (e.g., a diisocyanate compound) with a polyhydroxy acid (e.g., a dihydroxy acid). In addition, for example, the urethane resin can be obtained by reacting a polyol compound (e.g., a polyester polyol, a polyether polyol) and / or a chain extender with the polyisocyanate compound and the polyhydroxy acid. The urethane resin preferably contains at least one selected from the group consisting of a structural unit derived from meta-xylylene diisocyanate and a structural unit derived from hydrogenated meta-xylylene diisocyanate. Such a urethane resin exhibits high cohesive strength due to hydrogen bonds and a stacking effect between xylylene groups, so that the barrier layer is likely to exhibit excellent gas barrier properties. The structural unit derived from meta-xylylene diisocyanate refers to a monomer unit in a urethane resin that is reacted with meta-xylylene diisocyanate. The same applies to the structural unit derived from hydrogenated meta-xylylene diisocyanate and the structural unit derived from polyisocyanate. The monomer unit refers to a form in which a monomer substance in a polymer is reacted.
[0054] In the urethane resin, the total mol% of the meta-xylylene diisocyanate-derived structural units and the hydrogenated meta-xylylene diisocyanate-derived structural units is preferably 50 mol% or more, more preferably 60 mol% or more, based on the total amount of polyisocyanate-derived structural units in the urethane resin. There is no particular upper limit, but it is preferably 95 mol% or less, more preferably 90 mol% or less. The mol% of the structural units is 1 The identification can be performed using known analytical techniques such as H-NMR.
[0055] The urethane resin may have a hydroxyl group, and the hydroxyl value is preferably 50 mgKOH / g or more, more preferably 100 mgKOH / g or more, and even more preferably 150 mgKOH / g or more. The upper limit of the hydroxyl value is not particularly limited, but is preferably 1000 mgKOH / g or less, more preferably 800 mgKOH / g or less, and even more preferably 600 mgKOH / g or less. When the hydroxyl value of the urethane resin is within the above range, the barrier layer is more likely to exhibit oxygen barrier properties. In addition, by setting the hydroxyl value of the urethane resin within the above range, the thermal fusion property of the barrier layer can be improved, and as a result, the heat sealability of the printing film can also be improved. The hydroxyl value is measured in accordance with JIS K0070-1992, and the number of milligrams of potassium hydroxide required to neutralize the acetic acid bonded to the hydroxyl group when 1 g of the sample is acetylated is measured.
[0056] Urethane resin has an oxygen permeability of 100.0 mL / (m2) at 23°C and 50% relative humidity when converted into a 25 μm thick sheet. 2 ·day·atm) or less, and 50.0mL / (m 2 ·day·atm) or less, and 25.0mL / (m 2 ·day·atm) or less, and more preferably 10.0 mL / (m 2 ·day·atm) or less, and more preferably 3.0 mL / (m 2 ·day·atm) or less. When converted into a 25 μm thick sheet, the oxygen permeability at 23°C and a relative humidity of 50% is 0 mL / (m 2 ·day·atm). The oxygen permeability converted to a 25 μm thick sheet is measured by forming a 25 μm thick sheet using the target urethane resin. In this specification, the oxygen permeability of the sheet is measured using an oxygen permeability measuring device (OX-TRAN2 / 22, manufactured by MOCON) at 23° C. and a relative humidity of 50%.
[0057] The glass transition temperature of the urethane resin is preferably 150° C. or less, more preferably 140° C. or less, and particularly preferably 135° C. or less. The glass transition temperature of the urethane resin is measured in accordance with JIS K 7122:2012.
[0058] As the urethane-based resin, a synthetic product may be used, and examples of the synthetic product include the urethane-based resins described in International Publication No. 2015 / 016069. As the urethane-based resin, a commercially available product may be used, and examples include "Takelac W series (product name)", "Takelac WPB series (product name)", and "Takelac WS series (product name)" manufactured by Mitsui Chemicals, Inc., and specifically, Takelac WPB-341 is exemplified. Other commercially available products include "HPU W-003" (hydroxyl value 235 mg KOH / g) manufactured by Dainichiseika Chemicals Co., Ltd.
[0059] The vinylidene chloride resin can be produced by a known production method. For example, the vinylidene chloride resin can be obtained from a homopolymer of vinylidene chloride (polyvinylidene chloride, PVDC), a copolymer of vinylidene chloride and a monomer copolymerizable with vinylidene chloride, etc. The monomer copolymerizable with vinylidene chloride is not particularly limited, but includes vinyl chloride, (meth)acrylic acid esters such as methyl (meth)acrylate, ethyl (meth)acrylate, and butyl (meth)acrylate, acrylonitrile, isobutylene, and vinyl acetate.
[0060] As the vinylidene chloride resin, commercially available products may be used, for example, "Saran Latex L549B" manufactured by Asahi Kasei Corporation, or Diofan B204 manufactured by Solvay.
[0061] The weight average molecular weight of the water-suspendable polymer is preferably from 1000 to 20,000,000, and more preferably from 5,000 to 5,000,000. The weight average molecular weight is measured by gel permeation chromatography and expressed in terms of polystyrene.
[0062] The average particle size of the water-suspendable polymer in the emulsion is preferably 0.001 μm or more and 100 μm or less, more preferably 0.01 μm or more and 10 μm or less. The average particle size can be measured by a dynamic light scattering method.
[0063] (Water-soluble polymer) A water-soluble polymer is a resin that can be dissolved in water. A water-soluble resin is a polymer whose skeleton polymer has a solubility in water at 25°C of more than 10 g / L. Examples of polymers that serve as the backbone of the water-soluble polymer include polyvinyl alcohol, modified polyvinyl alcohol, starch and its derivatives, cellulose derivatives, polyvinylpyrrolidone, polyacrylic acid and its salts, casein, polyethyleneimine, etc. Among these, from the viewpoint of improving the gas barrier property, the water-soluble polymer is preferably one or more selected from the group consisting of polyvinyl alcohol and modified polyvinyl alcohol, and more preferably modified polyvinyl alcohol. Examples of modified polyvinyl alcohol include ethylene-modified polyvinyl alcohol, carboxy-modified polyvinyl alcohol, silicon-modified polyvinyl alcohol, acetoacetyl-modified polyvinyl alcohol, diacetone-modified polyvinyl alcohol, etc. Among these, the modified polyvinyl alcohol is preferably one or more selected from the group consisting of ethylene-modified polyvinyl alcohol, carboxy-modified polyvinyl alcohol, silicon-modified polyvinyl alcohol, and acetoacetyl-modified polyvinyl alcohol, more preferably one or more selected from the group consisting of ethylene-modified polyvinyl alcohol and carboxy-modified polyvinyl alcohol, and even more preferably ethylene-modified polyvinyl alcohol. Polyvinyl alcohol and modified polyvinyl alcohol are available in fully saponified and partially saponified forms, with fully saponified being preferred. Fully saponified means that the degree of saponification is greater than 96%. The degree of saponification is a value measured according to a method in accordance with JIS K 6726:1994.
[0064] As the water-soluble polymer, a commercially available product may be used, for example, modified polyvinyl alcohol such as "Exceval (product name)" manufactured by Kuraray Co., Ltd.
[0065] From the viewpoint of improving the barrier properties, the content of the water-suspendable polymer and water-soluble polymer in the barrier layer is preferably 10 mass % or more, more preferably 30 mass % or more, even more preferably 50 mass % or more, and still more preferably 60 mass % or more, of the solid content of the barrier layer, with the upper limit being 100 mass %.
[0066] The barrier layer may be formed by applying the coating liquid for the barrier layer to a film substrate, or by laminating a resin film to which the coating liquid for the barrier layer has been applied in advance. The resin film may be a sealant layer.
[0067] When the barrier layer is formed by coating, it is preferable to contain a layered inorganic compound in addition to at least one selected from the water-suspendable polymer and the water-soluble polymer. That is, it is preferable that the barrier layer contains a water-suspendable polymer and a layered inorganic compound, or a water-soluble polymer and a layered inorganic compound. By containing a layered inorganic compound in the barrier layer, the barrier properties can be further improved (oxygen permeability can be further reduced).
[0068] The average length of the layered inorganic compound is preferably 1 μm or more and 100 μm or less, more preferably 2 μm or more and 50 μm or less, and even more preferably 3 μm or more and 20 μm or less. Here, the average length of the layered inorganic compound is the average length of the major axis in the planar direction of the layered inorganic compound. When the average length is 1 μm or more, the layered inorganic compound in the barrier layer is easily arranged parallel to the film substrate. Also, when the average length is 100 μm or less, there is less concern that a part of the layered inorganic compound will protrude from the barrier layer.
[0069] The aspect ratio of the layered inorganic compound is preferably 200 or more, more preferably 300 or more, even more preferably 500 or more, and even more preferably 800 or more. The upper limit of the aspect ratio of the layered inorganic compound is not particularly limited, but is preferably 10,000 or less, more preferably 5,000 or less, and even more preferably 2,000 or less. When the aspect ratio of the layered inorganic compound is within the above range, the barrier property is improved, and the coating amount of the barrier layer can be reduced, thereby making it possible to increase the weight of the printing film. Here, the aspect ratio is a value calculated from a microscopic magnified photograph of the cross section of the barrier layer, and is the average value (arithmetic mean value of 20 to 30 samples) of the length of the layered inorganic compound divided by its thickness.
[0070] The thickness of the layered inorganic compound is preferably 100 nm or less, more preferably 50 nm or less, and further preferably 30 nm or less. The lower limit of the thickness of the layered inorganic compound is not particularly limited, but is preferably 2 nm or more. Here, the thickness of the layered inorganic compound is the average thickness of the layered inorganic compound measured from a microscopic magnified photograph of the cross section of the barrier layer (arithmetic mean value of 20 to 30 samples). The thickness is measured in the direction perpendicular to the long axis of the layered inorganic compound. By setting the average thickness of the layered inorganic compound within the above range, the number of layers of the layered inorganic compound in the barrier layer increases, so that the barrier layer can exhibit higher oxygen barrier properties. In particular, when a layered inorganic compound having a large aspect ratio and a small thickness is used, the barrier layer forms a dense film without voids. This phenomenon can also be observed from a microscopic magnified photograph of the cross section of the barrier layer.
[0071] Specific examples of the layered inorganic compound include mica such as mica group and brittle mica group, bentonite, kaolinite (kaolin mineral, hereinafter also referred to as "kaolin"), pyrophyllite, talc, smectite, vermiculite, chlorite, septe chlorite, serpentine, stilpnomelane, montmorillonite, etc. Among these, from the viewpoint of improving the water vapor barrier property, the layered inorganic compound is preferably at least one selected from the group consisting of mica, bentonite, and kaolin, and more preferably at least one selected from mica and kaolin. Examples of mica include synthetic mica, white mica (muscovite), sericite (sericite), phlogopite mica (phlocopite), black mica (biotite), fluorine phlogopite (artificial mica), red mica, soda mica, vanadium mica, illite, chin mica, paragonite, brittle mica, etc. Among them, the mica is preferably swellable mica because of its high aspect ratio. The kaolin may be a natural product or a synthetic product (engineered kaolin). Among these, at least one selected from the group consisting of mica, bentonite and kaolin is preferable, and at least one selected from mica and kaolin is more preferable. By containing the layered inorganic compound as described above in the barrier layer, the barrier property of the printing film under high humidity conditions can be more effectively improved.
[0072] When a layered inorganic compound is contained in the barrier layer, the content of the layered inorganic compound is not particularly limited, but is preferably 0.5 parts by mass or more and 500 parts by mass or less, more preferably 1 part by mass or more and 300 parts by mass or less, even more preferably 2 parts by mass or more and 200 parts by mass or less, still more preferably 5 parts by mass or more and 150 parts by mass or less, and particularly preferably 10 parts by mass or more and 70 parts by mass or less, relative to 100 parts by mass of the water-suspendable polymer or water-soluble polymer in the barrier layer. By setting the content of the layered inorganic compound within the above range, the barrier property of the printing film under high humidity conditions can be more effectively improved.
[0073] The barrier layer may contain, in addition to at least one selected from a water-dispersible polymer and a water-soluble polymer and a layered inorganic compound, a pigment, a dispersant, a surfactant, a defoamer, a wetting agent, a dye, a color adjuster, a thickener, etc.
[0074] When the barrier layer is provided by coating, the coating amount of the coating solution for the barrier layer is preferably 0.1 g / m2 in terms of solid content. 2 More than 10g / m 2 Less than 0.5 g / m 2 More than 5g / m 2 The following is the result.
[0075] (Resin with barrier properties) When the barrier layer is formed by laminating a resin having a barrier property by melt extrusion, adhesive or the like, examples of the resin having a barrier property include ethylene-vinyl alcohol copolymer (EVOH) and MX nylon. As the EVOH, commercially available products may be used, for example, the EVAL series manufactured by Kuraray Co., Ltd. An example of MX nylon is MXD6 manufactured by Mitsubishi Gas Chemical Company, Inc.
[0076] (deposited layer) The barrier layer may be formed by forming a vapor deposition layer directly on the film substrate, or by laminating a resin film on which a vapor deposition layer has been formed. The vapor-deposited layer is selected from the group consisting of a metal vapor-deposited layer and an inorganic vapor-deposited layer. An example of the metal to be deposited in the metal deposition layer is aluminum (Al), and an example of the inorganic compound to be deposited in the inorganic deposition layer is silica (SiOx) or alumina (AlOx). The thickness of the metal vapor deposition layer is not particularly limited as long as the desired barrier properties are obtained.
[0077] As the barrier layer, an adhesive may be applied to a resin film provided with a vapor deposition layer, and the resin film may be laminated with a substrate. Examples of the resin film include polyester-based resin films such as polyethylene terephthalate (PET), polyamide-based resin films such as various nylons, polyethylene-based resins, polypropylene-based resins, cyclic polyolefin resins, polystyrene-based resins, acrylonitrile-styrene copolymers (AS resins), acrylonitrile-butadiene-styrene copolymers (ABS resins), polyolefin films such as polybutene resin films, polyvinyl chloride-based resins, polycarbonate-based resins, polyimide-based resins, polyamideimide-based resins, polyarylphthalate resins, silicone-based resins, polysulfone-based resins, polyphenylene sulfide-based resins, polyethersulfone-based resins, polyurethane-based resins, cellulose-based resins, poly(meth)acrylic resins, polyvinylidene chloride films, acetal-based resin films, fluorine-based resins, and the like. In particular, polypropylene-based resins, polyester-based resins, and polyamide-based resins are preferred.
[0078] [Resin Layer] The printing film of this embodiment may further have a resin layer on at least one surface of the film substrate. That is, a printing medium may be used in which a resin layer is provided in advance on a film substrate having a titanium oxide content and a titanium oxide crystallite size equal to or greater than a predetermined value. In particular, by configuring the film substrate to have a resin layer on the printing surface thereof, in which the content of titanium oxide and the crystallite size of titanium oxide are equal to or greater than a predetermined value, it is preferable since it has excellent printability and further suppresses smoke generation upon irradiation with an ultraviolet laser. It is believed that when titanium oxide is heated by irradiation with an ultraviolet laser, the discolored titanium oxide is detached from the film substrate. It is believed that by providing a resin layer on the film substrate in advance, the detachment of the discolored titanium oxide described above is suppressed, the print density is increased, and smoke generation is suppressed.
[0079] The total light transmittance of the resin layer is preferably 40% or more, more preferably 60% or more, even more preferably 70% or more, still more preferably 80% or more, and particularly preferably 90% or more, and is 100% or less. There is no particular upper limit. The total light transmittance is measured in accordance with JIS K 7361-1:1997.
[0080] The resin constituting the resin layer is not particularly limited as long as it preferably has a total light transmittance of 40% or more and can be provided on a film substrate; however, from the viewpoints of transparency and ease of providing the resin layer, when the resin layer and the film substrate are attached via an adhesive layer or laminated by lamination, the resin is preferably at least one selected from polyethylene, polypropylene, polyethylene terephthalate, polyvinyl alcohol, and starch, more preferably at least one selected from polyethylene, polypropylene, polyethylene terephthalate, and polyvinyl alcohol, even more preferably polyethylene or polypropylene, and particularly preferably polyethylene. When the resin layer is provided by coating, examples of the resin include acrylic resins, styrene-maleic acid resins, water-soluble polyurethane resins, and water-soluble polyester resins. Examples of acrylic resins include resins obtained by copolymerizing (meth)acrylic acid with other monomers, such as alkyl esters thereof, styrene, unsaturated carboxylic acids other than (meth)acrylic acid, ethylene, and propylene. Specific examples include ethylene-(meth)acrylic acid copolymers and styrene-acrylic acid-maleic acid resins, with ethylene-(meth)acrylic acid copolymers being preferred.
[0081] The resin layer and the film substrate may be laminated by any method, and there is no particular limitation. From the viewpoint of ease of production, however, it is preferable to attach the resin layer and the film substrate via an adhesive layer, or to laminate them, or to apply the paint in the form of a liquid paint. When the resin layer is provided locally, it is preferable to attach it via an adhesive from the viewpoint of ease of production, whereas when the resin layer is provided over a wide area, it is preferable to use a lamination process. The adhesive layer is not particularly limited and may be appropriately selected from known adhesive layers. Specific examples include the pressure-sensitive adhesive layer described in JP2012-57112A.
[0082] The thickness of the resin layer is not particularly limited, but from the viewpoints of improving print density, improving print clarity for each individual point, ease of handling of the printed matter and print medium, and suppressing smoke generation during irradiation with an ultraviolet laser, it is preferably 5 μm or more, more preferably 10 μm or more, even more preferably 15 μm or more, and is preferably 100 μm or less, more preferably 75 μm or less, even more preferably 50 μm or less.
[0083] <Uses of printing films and printed matter, and processed products> The ultraviolet laser printable film of the present embodiment can be printed by irradiating it with an ultraviolet laser, and can be used for a variety of purposes. The ultraviolet laser printing film of the present embodiment and the printed matter printed on the film by an ultraviolet laser are processed into various processed products for use. That is, the processed products of the present embodiment are made using the ultraviolet laser printing film or the printed matter of the present embodiment. Examples of processed products using the ultraviolet laser printing film or printed matter of this embodiment include packaging, labels, adhesive tapes, etc. It is also preferable to mold the printing film and printed matter of this embodiment directly into packaging for use. Examples of packaging bodies include outer bags and outer boxes; liquid containers for beverages such as milk cartons and cups (preferably liquid containers for beverages); food containers such as food trays and food cups (bowl-shaped), and skin packs. Examples of labels include label sheets, adhesive labels, and adhesive sheets. Examples of adhesive tapes include adhesive tapes and craft tapes. Among these, since the film can be directly molded, it is preferable to use it for packaging, and it is particularly preferable to use it for food containers. That is, food containers made of the ultraviolet laser printing film or printed matter of this embodiment are a preferred embodiment. By irradiating the surface of the packaging with an ultraviolet laser, it is possible to print characters such as dates, barcodes, and various information about the contents (contents, raw material names, content volume, manufacturer name).
[0084] [Printed matter and method of manufacturing printed matter] The printed matter of the embodiment is a printed matter obtained from the above-mentioned ultraviolet laser printing film, and has a printed area having discolored titanium oxide in at least a part. The ratio of the Raman intensity originating from titanium oxide in the printed area to the Raman intensity originating from titanium oxide in the non-printed area is preferably 0.70 or less. The printed area having discolored titanium oxide is an area containing titanium oxide discolored by irradiation with an ultraviolet laser, and is an ultraviolet laser irradiated area, i.e., a printed area. The method for producing a printed matter of the present embodiment also includes a step of irradiating the above-mentioned ultraviolet laser printing film with an ultraviolet laser to discolor the irradiated area, thereby printing. The film used in the printed matter and the method for producing printed matter of this embodiment can be exemplified by the above-mentioned UV laser printing film, and the preferred range is also the same.In addition, in the printed matter and the method for producing printed matter of this embodiment, the titanium oxide content and the crystallite size of titanium oxide in at least UV laser irradiation area are sufficient to be equal to or greater than a predetermined value, and the titanium oxide content and the crystallite size of titanium oxide in non-irradiation area are not particularly limited, but since titanium oxide is added to the film, it is preferable that the titanium oxide content and the crystallite size of titanium oxide in non-irradiation area are equal to or greater than the above-mentioned predetermined amount.
[0085] The ultraviolet laser is preferably irradiated so that the ratio of the Raman intensity derived from titanium oxide in the printed area to the Raman intensity derived from titanium oxide in the non-printed area is 0.70 or less. That is, in the printed matter of this embodiment, the ratio of the Raman intensity derived from titanium oxide in the printed area to the Raman intensity derived from titanium oxide in the non-printed area is preferably 0.70 or less. In addition, in the printed matter, the printed area means an area (part) in the printable area that contains discolored titanium oxide, and is an area (part) that is printed with an ultraviolet laser. The non-printed area means an area (part) that is not printed in the printable area. Furthermore, the printable area means the entire area containing titanium oxide in the ultraviolet laser printing film or printed matter, including the area that can be printed with an ultraviolet laser and the printed area printed with an ultraviolet laser, if any, and the non-printable area means an area other than the printable area in the ultraviolet laser printing film or printed matter. It is preferable to print so that the ratio of the Raman intensity derived from titanium oxide in the printed area to the Raman intensity derived from titanium oxide in the non-printed area (Raman intensity of the printed area / Raman intensity of the non-printed area) is 0.70 or less. By keeping the ratio of Raman intensities within the above range, a printed matter with excellent visibility can be obtained. The ratio of the above Raman intensities (Raman intensity in the printed area / Raman intensity in the non-printed area) is 447±10 cm when rutile titanium oxide is used as the titanium oxide, which is the Raman intensity derived from titanium oxide. -1 In addition, when anatase-type titanium oxide is used as the titanium oxide, the Raman intensity at 516±10 cm is compared. -1 The Raman intensities of the maximum values in the wavenumber range are compared. In addition, when rutile titanium oxide and anatase titanium oxide coexist, the Raman intensity derived from rutile titanium oxide is used for comparison.
[0086] In the printed matter of this embodiment, it is preferable that the non-printed areas are white and the printed areas are black. The non-printed areas preferably have a value of 10 on the Munsell color system, i.e., are white. On the other hand, the printed areas preferably have a value of any one of 0 to 8 on the Munsell color system, more preferably 0 to 6, and even more preferably 0 to 4. In order to obtain a color in the Munsell color system described above, it is preferable to appropriately adjust the titanium oxide content in the film, the crystallite size of the titanium oxide, other characteristics of the film (such as resin type and film thickness), and irradiation conditions of the ultraviolet laser (for example, average output, repetition frequency, wavelength, etc.).
[0087] [UV laser irradiation conditions] From the viewpoint of improving the visibility of the printed area, the wavelength of the ultraviolet laser is preferably 370 nm or less, more preferably 365 nm or less, even more preferably 360 nm or less, and is preferably 260 nm or more, more preferably 340 nm or more, even more preferably 350 nm or more.
[0088] From the viewpoint of improving the visibility of the printed area, the average output of the ultraviolet laser is preferably 0.3 W or more, more preferably 0.8 W or more, even more preferably 1.2 W or more, and even more preferably 1.8 W or more, and from the viewpoint of economy, it is preferably 30 W or less, more preferably 25 W or less, even more preferably 20 W or less, even more preferably 15 W or less, even more preferably 10 W or less, and even more preferably 6 W or less.
[0089] From the viewpoint of improving the visibility of the printed area, the repetition frequency (frequency) of the ultraviolet laser is preferably 10 kHz or more, more preferably 20 kHz or more, even more preferably 30 kHz or more, and is preferably 100 kHz or less, more preferably 80 kHz or less, even more preferably 60 kHz or less.
[0090] From the viewpoint of obtaining a dark printed image and ease of printing, the spot diameter of the ultraviolet laser is preferably 10 μm or more, more preferably 20 μm or more, even more preferably 30 μm or more, and is preferably 300 μm or less, more preferably 240 μm or less, even more preferably 180 μm or less, even more preferably 120 μm or less.
[0091] From the viewpoints of high-speed printing and visibility of the printed area, the scanning speed of the ultraviolet laser is preferably 500 mm / sec or more, more preferably 1000 mm / sec or more, even more preferably 2000 mm / sec or more, and is preferably 7000 mm / sec or less, more preferably 6000 mm / sec or less, even more preferably 5000 mm / sec or less.
[0092] From the viewpoint of obtaining a dark printed image and of the ease of availability of the equipment, the filling interval (line pitch) of the ultraviolet laser is preferably 10 μm or more, more preferably 20 μm or more, even more preferably 30 μm or more, and is preferably 300 μm or less, more preferably 250 μm or less, even more preferably 200 μm or less.
[0093] [Embodiments of the method for producing printed matter] The method for producing a printed matter according to the present embodiment can be carried out in various modes. Various examples of the printed matter manufacturing method of the present embodiment are described below, but the printed matter manufacturing method of the present embodiment is not limited to the following examples. The information to be printed is not particularly limited, but is preferably variable information. The method for producing a printed matter according to the present embodiment is preferably carried out in-line. (1) Direct printing on packaging A first embodiment of the method for producing printed matter of this embodiment is a method for printing information on a packaging body having the printing film of this embodiment, and includes a step of printing directly on the packaging body using an ultraviolet laser while it is moving on a packaging line or while it is intermittently stopped. In the method for producing a printed matter according to the first embodiment, a package is produced using a printing medium having the printing film according to the present embodiment, and is directly printed with an ultraviolet laser. Note that at least the outermost layer of the package may be produced using the printing medium having the film, or a printing medium having a resin layer on the film. Furthermore, the packaging material is exemplified by food containers, and it is preferable to print directly on the side or back of the packaging material with an ultraviolet laser.
[0094] (2) Printing on labels A second embodiment of the method for producing a printed matter of this embodiment is a method for printing information on a label having a film containing a predetermined amount of titanium oxide, the crystallite size of the titanium oxide being equal to or larger than a predetermined value. The printing medium constituting the printing surface of the label may be made of a printing medium having the above-mentioned film, or a printing medium having a resin layer on the film. The printed label is preferably applied to the package using a label application device, of which various types of label application devices have been proposed. The first label application device applies adhesive to a rolled label sheet and then applies it to an article. More specifically, a roll labeler includes a cutting means for cutting the rolled label sheet into a predetermined length one by one, a gluing conveying means for receiving the label sheet cut by the cutting means with a label sheet holder coated with adhesive and applying the adhesive to the back surface of the label sheet, and an application means for receiving the label sheet (label) with adhesive applied from the gluing conveying means and applying it to an article such as a container. An example of the roll labeler is one in which a rotary conveying means having a label holding surface on its outer surface is provided between the cutting means and the gluing conveying means, as disclosed in Japanese Patent Application Laid-Open No. 6-64637. Other examples include a roll labeler that has a cutting means for cutting the rolled-up label sheet to a specified length, a transfer roll that passes the label sheet to the application roll, and a gluing roll that applies glue to the label sheet held by the application roll, as well as an embodiment that does not require the transfer roll. The ultraviolet laser irradiation is preferably performed before cutting the rolled label sheet to a specified length, or after cutting and before transferring to the next roll, etc. Depending on the type of roll labeler, the front or back surface of the rolled label sheet will become the front or back surface when affixed to a package, so the ultraviolet laser irradiation is performed accordingly.
[0095] The second labelling device uses adhesive label rolls as the labels. In the case of using an adhesive label roll with a release paper, for example, an application device having a release paper separating means for separating the adhesive label from the release paper, a delivery roll for receiving the adhesive label from which the release paper has been separated, and an application roll for sucking the adhesive label from the delivery roll and applying it to an article (package) is exemplified. Irradiation with an ultraviolet laser is preferably performed before separating the release paper, or after separating the release paper and before the label is carried by the application roll. Another example is an apparatus that sets an adhesive label roll with a release paper, has a mechanism for separating the adhesive label from the release paper, and has a mechanism for attaching a label immediately after separation, and performs printing with an ultraviolet laser before the release paper is separated from the set adhesive label roll. The above-mentioned adhesive label attachment method is also called flow attachment. Further, a label application device is exemplified that has a mechanism for setting an adhesive label roll with a release paper, separating the release paper from the adhesive label, and attaching the adhesive label to an article (package), the mechanism being a syringe type, an air jet type, or a robot arm type. Irradiation with an ultraviolet laser is preferably performed until the release paper is separated from the set adhesive label roll with the release paper.
[0096] The labels may be linerless adhesive labels. Linerless adhesive labels are labels without release paper, and have the advantages of being cheaper and having more labels per roll than when using an adhesive label roll with release paper, since there is no release paper. An example of a label application device using linerless adhesive labels is a device that has a mechanism for setting a linerless label roll, a cutting mechanism for cutting the linerless labels one by one, and an application mechanism for applying the cut linerless labels to an article (package), and the application mechanism is of a cylinder type or a robot arm type. Printing by irradiation with an ultraviolet laser is preferably performed between the mechanism for setting the linerless label roll and the cutting mechanism, or while the cut linerless labels are being sent to the application mechanism.
[0097] The third label application device applies a print medium having a sheet medium containing at least a predetermined amount of titanium oxide to an article (package), and then prints with an ultraviolet laser. For the method of attaching the label, reference is made to the first and second devices described above.
[0098] (3) Printing on adhesive tape A third embodiment of the method for producing a printed matter of the present embodiment is an embodiment in which a printing medium having a film containing a predetermined amount or more of titanium oxide, in which the crystallite size of the titanium oxide is a predetermined value or more, is made into an adhesive tape. That is, the method for producing a printed matter of the third embodiment includes a step of attaching an adhesive tape made from a printing medium having the film to an item (packaging material), and a step of printing with an ultraviolet laser before or after the attaching step. Also, a printing device incorporating an ultraviolet laser printer in a cardboard sealing machine may be used. Specifically, the printing device has a mechanism for setting the adhesive tape winding, a conveyor for transporting the cardboard, a mechanism for folding the flaps of the cardboard, a mechanism for sealing the cardboard by applying adhesive tape, and a mechanism for printing on the adhesive tape with an ultraviolet laser during or after the application of the adhesive tape.
[0099] The printed matter and the method for producing the printed matter of the present embodiment are not limited to the above-mentioned aspects, and can be applied to various uses where printing is required.
[0100] In this embodiment, the printed matter obtained by the method for producing a printed matter is suitable for use as packaging materials, labels, adhesive tapes, and the like. Examples of packaging bodies include outer boxes; liquid containers for beverages such as milk cartons and cups (preferably paper containers for liquid beverages); food containers such as food trays and food cups (bowl-shaped), skin packs, pillow packaging, standing pouches, three-side / four-side sealed packaging, etc. Examples of labels include label sheets, adhesive labels, and adhesive sheets, and examples of adhesive tapes include adhesive tapes and craft tapes. Among these, since films can be directly molded, it is preferable that the printed matter be a package, and in particular, a food container. EXAMPLES
[0101] The features of the present invention will be described in more detail below with reference to examples and comparative examples. The materials, amounts used, ratios, processing contents, processing procedures, etc. shown in the following examples can be changed as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the specific examples shown below. In addition, "parts" and "%" mean "parts by mass" and "% by mass" unless otherwise specified.
[0102] [Titanium oxide] The titanium oxides used in the examples and comparative examples are as shown in Table 1 below.
[0103] [Table 1]
[0104] <Synthesis method of titanium oxide C, F~H> Titanium oxide (amorphous) was synthesized by hydrolysis and condensation polymerization of titanium tetraisopropoxide (TTIP), and was crystallized by calcination. Specifically, the synthesis was carried out according to the following steps (1) to (6). (1) The following solutions A to C were prepared using TTIP (Tokyo Chemical Industry Co., Ltd., product code: T0133), isopropanol (Tokyo Chemical Industry Co., Ltd., purity 99.5% or higher, product code: I0163), and ion-exchanged water. Solution A: 35.6 parts by weight of TTIP, 200 parts by weight of isopropanol Solution B: 200 parts by weight of isopropanol, 6.3 parts by weight of ion-exchanged water Solution C: 200 parts by weight of isopropanol, 24.4 parts by weight of ion-exchanged water (2) While stirring solution A with a Teflon (registered trademark) stirring blade, solution B was slowly added dropwise, and stirring was continued for 10 minutes. (3) Solution C was slowly added dropwise to the mixture of Solution A and Solution B obtained in (2) above, and the mixture was stirred for 1 minute and then allowed to stand at room temperature for 24 hours. (4) The precipitate was separated into solid and liquid using a membrane filter (manufactured by Advantec, material: cellulose acetate). (5) After washing with isopropanol, it was dried at 100°C for 5 hours to obtain titanium oxide (amorphous). (6) The mixture was fired in a muffle furnace to crystallize the titanium oxide. The firing was performed at the temperatures shown in the table, with a temperature rise rate of 10° C. / min and firing for 2 hours after the temperature rise.
[0105] [resin] Polypropylene (PP): PH943B (SunAllomer Co., Ltd.) Polyethylene (PE): Novatec (registered trademark) LC522 (manufactured by Japan Polyethylene Co., Ltd.) Polyethylene terephthalate (PET): SA-8339P, manufactured by Unitika Ltd. Polylactic acid (PLA): REVODE190 (manufactured by Zhejiang Hisun Biomaterials Co., Ltd.) Polybutylene succinate (PBS): ZM9B02 (manufactured by Mitsubishi Chemical Corporation)
[0106] [Examples 1 to 16, Comparative Examples 1 to 3] <Masterbatch manufacturing method> Following the example of JP 2015-96568 A, the film was prepared in the following manner. 60 parts of a resin shown in Table 3 and 40 parts of titanium oxide shown in Table 3 were mixed in a tumbler mixer (TM-65S, manufactured by Eishin Co., Ltd.) at 45 rpm for 1 hour, and then melt-kneaded in a twin-screw extruder (TEX30XCT, L / D=42, manufactured by The Japan Steel Works, Ltd.) at a screw rotation speed of 250 rpm and a cylinder temperature under the conditions in Table 2 below, extruded into a strand shape, cooled in a water tank, and then pelletized using a pelletizer into columnar shapes with an average shaft diameter of 2.0 mm and an average shaft length of 3.0 mm to obtain a master batch.
[0107] <Manufacturing method of film substrate> The master batch and the resin in Table 3 were fed into a single screw extruder (50C150, manufactured by Toyo Seiki Seisakusho Co., Ltd.) so that the titanium oxide concentration was the value in the table, and melt-extruded to a thickness of 60 μm, and then rapidly cooled while being sandwiched between cooling rolls adjusted to 20° C. to obtain a UV printing medium. The melting temperature of each resin was as shown in Table 2 below. Table 2 below shows the cylinder temperature during the production of the master batch and the melt temperature during the production of the film.
[0108] [Table 2]
[0109] <Formation of sealant layer> PE (low density polyethylene, manufactured by Japan Polyethylene Co., Ltd., Novatec (registered trademark) LD LC522) was fed into a single screw extruder (manufactured by Toyo Seiki Seisakusho Co., Ltd., D2025), and extrusion laminated (melt laminated) onto one side of the film substrate so that the resin had a thickness of 15 μm, and then rapidly cooled while being sandwiched between cooling rolls adjusted to 20° C. to provide a sealant layer, thereby obtaining a film for ultraviolet laser printing. The melting temperature of the resin in the extrusion lamination was 320° C.
[0110] [Example 17] <Manufacturing of film substrate> A film substrate was produced in the same manner as in Example 4. <Barrier layer formation> EVOH (ethylene-vinyl alcohol copolymer, EVAL E105B, manufactured by Kuraray Co., Ltd.) was put into a single screw extruder (D2025, manufactured by Toyo Seiki Seisakusho Co., Ltd.) and extrusion laminated (melt laminated) onto one side of the film substrate so that the resin had a thickness of 15 μm, and then it was quickly quenched while being sandwiched between cooling rolls adjusted to 20°C to form a barrier layer. The melting temperature of the resin in the extrusion lamination was 215°C. <Formation of sealant layer> A sealant layer was provided in the same manner as in Example 4 to obtain a film for ultraviolet laser printing.
[0111] [Example 18] <Manufacturing of film substrate> A film substrate was produced in the same manner as in Example 4. <Barrier layer formation> To 100 parts of an aqueous solution of ethylene-modified polyvinyl alcohol (fully saponified, Kuraray Co., Ltd., Exeval AQ-4104) with a solid content concentration of 15 mass%, 50 parts of an aqueous dispersion of a layered inorganic compound (layered inorganic compound=synthetic mica (swellable mica, average length: 6.3 μm, aspect ratio: about 1000, thickness: about 5 nm), solid content concentration of 6 mass%, Topy Industries, Ltd., NTO-05) was added, and dilution water was further added thereto to adjust the solid content concentration to 10 mass%, to prepare a coating liquid for a barrier layer. The coating liquid for a barrier layer was applied in a coating amount of 2.0 g / m 2 The coating was then dried in a hot air dryer at 120° C. for 1 minute to form a barrier layer. <Formation of sealant layer> Water was added to a water-based heat sealant (ethylene-acrylic acid copolymer (Et-AA in the table), Michaelman, MFHS1279, solids concentration 42%) to dilute it to a solids concentration of 20%, and the coating amount (solids content) was 5 g / m on the barrier layer. 2The coating was applied using a Mayer bar so that the coating solution had a thickness of 100 μm and then dried at 120° C. for 60 seconds to form a sealant layer, thereby obtaining a film for ultraviolet laser printing.
[0112] [Example 19] <Manufacturing of film substrate> A film substrate was produced in the same manner as in Example 4. <Barrier layer formation> A water dispersion of a layered inorganic compound (layered inorganic compound = synthetic mica (swellable mica, average length: 6.3 μm, aspect ratio: approximately 1000, thickness: approximately 5 nm), solid content concentration 6 mass%, manufactured by Topy Industries, Ltd., NTO-05) was mixed with a urethane emulsion (solid content concentration 30 mass%, glass transition temperature 130°C, oxygen permeability when formed into a 25 μm thick sheet was 2.0 mL / (m 2 1.0 g / m2 (Takelac WPB-341, manufactured by Mitsui Chemicals, Inc.) was added to the mixture so that the mass ratio of solids (layered inorganic compound:urethane resin) was 2:10, and the mixture was stirred. Further, dilution water was added so that the solids concentration was 20 mass %, to prepare a coating liquid for a barrier layer. The coating liquid for a barrier layer was diluted with 1.0 g / m2 of the mixture so that the coating amount of the barrier layer was 2.0 g / m2. 2 After coating one surface of the film substrate with a Mayer bar so as to obtain the above coating composition, the coating was dried in a hot air dryer at 120° C. for 1 minute to form a barrier layer. <Formation of sealant layer> In the same manner as in Example 18, a sealant layer was formed on the barrier layer to obtain a film for ultraviolet laser printing.
[0113] [Example 20] <Manufacturing of film substrate> A film substrate was produced in the same manner as in Example 4. <Barrier layer formation> Aluminum-deposited PP film (base material = CPP (non-oriented polypropylene film), manufactured by Mitsui Chemicals Tocello Co., Ltd., product name: ML, thickness 20 μm, water vapor permeability 0.2 g / m 2 ·day, oxygen permeability 50mL / m 2On the surface of the PP film of the 100-m2 ... 2 After coating, the coating was attached to one side of a film substrate. <Formation of sealant layer> A sealant layer was formed on the barrier layer in the same manner as in Example 4 to obtain a film for ultraviolet laser printing.
[0114] [Example 21] In forming the barrier layer, an aluminum-deposited PET film (substrate: PET (polyethylene terephthalate), manufactured by Mitsui Chemicals Tohcello Co., Ltd., product name: ML, thickness: 12 μm, water vapor permeability: 1 g / m) was used instead of an aluminum-deposited PP film. 2 ·day, oxygen permeability 10mL / m 2 A film for ultraviolet laser printing was obtained in the same manner as in Example 20, except that a 1000-milliliter (1.0-1.0-g / kg) ... was used. The adhesive was applied to the substrate (PET) side.
[0115] [Example 22] In forming the barrier layer, a silica-deposited PP film (substrate: PP, manufactured by Toppan Printing Co., Ltd., product name: GL-LP, thickness: 17 μm, water vapor permeability: 0.5 g / m) was used instead of an aluminum-deposited PP film. 2 ·day, oxygen permeability 1mL / m 2 A film for ultraviolet laser printing was obtained in the same manner as in Example 20, except that a 1000-milliliter (1.0-1.0-g / kg) ... was used. The adhesive was applied to the substrate (PP) side.
[0116] [Example 23] In forming the barrier layer, a silica-deposited PET film (substrate: PET, manufactured by Toppan Printing Co., Ltd., product name: GL-AE, thickness: 12 μm, deposition layer thickness: 400 nm, water vapor permeability: 0.6 g / m) was used instead of an aluminum-deposited PP film. 2 ·day, oxygen permeability 0.2mL / m 2A film for ultraviolet laser printing was obtained in the same manner as in Example 20, except that a 1000-milliliter (1.0-1.0-g / kg) ... was used. The adhesive was applied to the substrate (PET) side.
[0117] [Example 24] In forming the barrier layer, an alumina-deposited PET film (substrate: PET, manufactured by Mitsui Chemicals Tohcello Co., Ltd., product name: TL, thickness: 12 μm, water vapor permeability: 1.5 g / m) was used instead of an aluminum-deposited PP film. 2 ·day, oxygen permeability 15mL / m 2 A film for ultraviolet laser printing was obtained in the same manner as in Example 20, except that a 1000-milliliter (1.0-1.0-g / kg) ... was used. The adhesive was applied to the substrate (PET) side.
[0118] [Example 25] In forming the barrier layer, instead of aluminum-deposited PP film, a PET film coated with PVDC (polyvinylidene chloride) (manufactured by Mitsui Chemicals Tohcello Co., Ltd., product name: V Barrier, thickness 12 μm, water vapor permeability 0.2 g / m) was used. 2 ·day, oxygen permeability 0.8mL / m 2 A film for ultraviolet laser printing was obtained in the same manner as in Example 20, except that a 1000-milliliter (1.0-1.0-g / kg) ... was used. The adhesive was applied to the substrate (PET) side.
[0119] [Comparative Example 4] An ultraviolet laser printing film was obtained in the same manner as in Example 4, except that the sealant layer was not formed.
[0120] [Measurement and Evaluation] The ultraviolet laser printing films and various raw materials obtained in the examples and comparative examples were subjected to the following measurements and evaluations.
[0121] [Average particle size of titanium oxide] The average particle size of titanium oxide was measured by the following method. The film substrate was scraped off from the ultraviolet laser printing films obtained in the Examples and Comparative Examples using an industrial razor (Feather Safety Razor Co., Ltd., product number: 099769), and the collected film substrate was used as a sample, and calculations were performed from SEM images (secondary electron images) obtained with a scanning electron microscope (SEM, Hitachi High-Tech Corporation, SU7000, etc.) of the ash obtained by burning in a muffle furnace. The ash was obtained by burning at 450°C using a muffle furnace (Yamato Scientific Co., Ltd., model number FO300) and incinerating. Next, the mixture was dispersed in ethanol for 5 minutes using an ultrasonic cleaner (such as LSC-63, manufactured by AS ONE Corporation) to obtain a 0.1% by mass slurry, and 0.1 mL of the mixture was cast onto an aluminum dish and dried at 100°C to prepare a measurement sample. The aluminum dish was subjected to observation using a scanning electron microscope (SEM, such as SU7000, manufactured by Hitachi High-Tech Corporation), and particles that were clearly distinguishable from adjacent particles were visually selected, and the particle size was calculated from the geometric mean of the major and minor axes of one particle. In this case, if primary particles and secondary particles in an aggregated state were mixed but were clearly distinguishable, each was counted as one particle, and the average diameter of 100 randomly selected particles was taken as the average particle size. The magnification during SEM image observation was appropriately selected depending on the particle size of titanium oxide, and was set to about 20,000 times. When particles other than titanium oxide were contained, particles containing titanium element were measured using an energy dispersive X-ray analyzer attached to the SEM (Horiba, Ltd., EMAX, etc.). In the case of needle-shaped particles, the major axis of 100 particles was measured, and the average was taken as the average particle diameter.
[0122] [Crystallite size calculation method] <Measuring sample preparation method> From the ultraviolet laser printing films obtained in the examples and comparative examples, the film substrate was shaved off using an industrial razor (manufactured by Feather Safety Razor Co., Ltd., product number: 099769), and the collected film substrate was used as a sample and calculated from the SEM image (secondary electron image) obtained from a scanning electron microscope (SEM, manufactured by Hitachi High-Tech Corporation, SU7000, etc.) of the ash obtained by burning in a muffle furnace. The ash was obtained by firing at 450 °C using a muffle furnace (manufactured by Yamato Scientific Co., Ltd., model number FO300) and ashing.
[0123] <Measurement by X-ray diffraction method> The test sample obtained by ashing was filled into a sample holder and measured using a high-speed detector. During filling, the height adjustment jig was appropriately used according to the sample amount so that the sample measurement surface was always at the same height as the edge of the sample holder. (Measurement conditions) X-ray diffractometer: manufactured by Rigaku Corporation, RINT-Ultima III Voltage: 40 kV Current: 40 mA Optical system: parallel beam (CBO) Detector: high-speed detector D / teX Ultra 2 manufactured by Rigaku Corporation Goniometer: Ultima III horizontal goniometer Tube target: Cu Wavelength: 1.541 Å (Kα1) Scan mode: CONTINUOUS Scan speed: 1.0000 deg / min Step width: 0.0500 deg Scan axis: 2Theta / Theta Scan range: 5.0000 ~ 60.0000 deg Incident slit: 1.0 mm Longitudinal limiting slit: 10 mm Light receiving slit 1: open Light receiving slit 2: open Sample holder: ASC-6 sample holder (product number 2455E442) Material: aluminum Dimensions: φ23 mm × 2.0 mm Holder height adjustment jig: Transparent disc-shaped plate (self-made) Material: Methyl polyacrylate Dimensions: φ23 mm × 0.8 mm
[0124] <Processing of data obtained by X-ray diffraction> For the obtained diffraction profile, background processing and profile fitting processing were performed using integrated powder X-ray analysis software (manufactured by Rigaku Corporation, PDXL2). Regarding the settings for data processing, all those without specific description were performed with the default settings of the software. Based on the information on the peak position and peak intensity of the diffraction profile, the crystal phase was identified using a database (ICDD).
[0125] <Calculation of crystallite size based on data obtained by X-ray diffraction> The full width at half maximum (FWHM) and Bragg angle (θ) of the strongest diffraction line obtained from the diffraction profile after data processing were substituted into the Scherrer equation to calculate the crystallite size. The X-ray diffraction peaks of titanium oxide used in the calculation are as follows. Anatase: 101 plane Rutile: 110 plane The Scherrer equation is as follows.
[0126]
Equation
[0127] D: Crystallite size (nm) K: Scherrer constant λ: Wavelength of X-ray (nm) B: FWHM (rad) θ: Bragg angle (rad) The value of K was 0.89, B was the value of FWHM obtained by measurement, the value of λ was 0.154, and the value of θ was the measured value of the maximum intensity derived from the 101 plane in the case of anatase and the 110 plane in the case of rutile.
[0128] [Titanium oxide content] <Measurement of moisture in substrate> The moisture content of the film was measured according to JIS P 8203:2010 (ISO 638:2008). <Preparation of test specimen> As a pretreatment, layers other than the film substrate (sealant layer, barrier layer, resin layer, etc.) were removed from the ultraviolet laser printing films obtained in the examples and comparative examples using a grinding device (manufactured by Sagawa Corporation, grinding wheel dimensions φ50.8 × 12.7 mm). The obtained film substrate was conditioned by the method of JIS P 8111:1998, and then cut into a suitable size to prepare a sample (test piece), and the area and mass of the cut piece were recorded.
[0129] <Dissolution of test specimen> A mixed solvent of nitric acid:hydrofluoric acid = 50:5 (volume %) and the test piece were placed in a Teflon (registered trademark) container of an autoclave device (MARS5, manufactured by CEM Japan), and the test piece was dissolved by autoclaving at 210°C for 120 minutes. The mass of the test piece may be changed as appropriate, and if the test piece remains undissolved, the ratio of nitric acid and hydrofluoric acid, the treatment temperature, the treatment time, etc. may be changed as appropriate. After dissolving the test piece, the solution was accurately adjusted to a fixed volume using ultrapure water.
[0130] <Measurement of titanium oxide content in solution> (1) The ICP apparatus and measurement conditions are as follows: ICP device: ICP-OEC device (Rigaku Corporation, CIROS1-20) Measurement conditions: Carrier gas: Argon gas Argon gas flow rate: 0.9L / min Plasma gas flow rate: 14 L / min Plasma power 1400W Pump RPM: 2 ·Measurement wavelength Ti: 334.941nm (2) Preparation of calibration curve A general-purpose mixed standard solution (manufactured by SPEX, XSTC-622B) was accurately measured to give the following concentrations, and subjected to measurement under the above measurement conditions, and the intensity at 334.941 nm, which corresponds to the emission wavelength of titanium atoms, was measured. Concentrations for creating calibration curves: 0 ppm, 0.01 ppm, 0.05 ppm, 0.1 ppm, 0.5 ppm, 1.0 ppm, 3.0 ppm, 5.0 ppm (3) Measurement of titanium oxide content in the solution The solution in which the test pieces were dissolved was diluted with ultrapure water so that the solution was within the range of the above calibration curve, and then subjected to ICP measurement. (4) Titanium dioxide content calculation method The titanium oxide content was calculated using the following formula: (molecular weight of titanium oxide / atomic weight of titanium) ≈ 1.669. Titanium oxide content (g / m 2 ) = ICP measured concentration (ppm) × dilution ratio × fixed volume (L) × 1.669 × 1000 ÷ area (m 2 ) Titanium oxide content (mass%) = ICP measured concentration (ppm) x dilution ratio x fixed volume (L) x 1.669 ÷ test piece mass (mg) x (1 - moisture content) x 100
[0131] [Thickness of film substrate and sealant] The thicknesses of the film substrate and the sealant layer were measured from image data obtained from a scanning electron microscope. (1) Preparation of measurement samples The sample was embedded in a photocurable resin (D-800, manufactured by Toagosei Co., Ltd.), and the cross section of the printing film was extracted using an ultramicrotome. A diamond knife was used for cutting at room temperature. The cut cross section was coated with gold vapor deposition to a thickness of about 20 nm and subjected to measurement using a scanning electron microscope. (2) Measurement equipment and conditions Measuring device: S-3600 (Hitachi High-Tech Corporation) Measurement conditions: 2000x magnification The type of scanning microscope is not limited to the above, but an apparatus that displays a scale bar was used. When the film layer or sealant layer was thin, an appropriate magnification was selected to acquire image data. (3)Measurement method Image data was obtained at a magnification of 2000 times using a scanning electron microscope. After printing the obtained image data on printing paper, the thickness of the target film substrate and sealant layer (the length from the boundary to the boundary with other layers) was measured with a ruler, and the actual thickness of the film layer and sealant layer (coating layer or laminate layer) was measured by comparing with the scale bar. Image data of five randomly selected points was obtained from one measurement sample, and the thickness of the thickest point of the film substrate and the thinnest point of the film substrate were measured from the image data of one point, and the average of the total of 10 points was taken as the thickness of the film substrate. The observation magnification may be changed depending on the thickness of the film substrate to be observed. In addition, the thickness of the thickest point of the sealant layer and the thinnest point of the sealant layer were measured, and the average of the total of 10 points was taken as the thickness of the sealant layer. The observation magnification may be changed depending on the thickness of the sealant layer to be observed. When a barrier layer is further provided between the sealant layer and the film substrate, the thickness of the barrier layer can also be measured in the same manner.
[0132] [Measurement of Raman spectrum] The Raman spectrum was measured by the following method: In this example, the Raman spectrum was measured on a print obtained by the clarity of a single printed dot described below. <Measurement conditions> The measurement conditions for Raman spectrum are as follows, but if the laser used for measurement causes damage to the printed matter, if the fluorescence is strong, if the peak intensity is weak, etc., the measurement conditions below such as laser output and irradiation time can be changed as appropriate. However, the Raman intensities of the printed and non-printed areas are measured under the same conditions. Equipment: Renishaw inVia Raman microscope QUONTOR Excitation laser: 532nm Laser power: 50mW (at 100% output) Laser power: 50% Measurement mode: Confocal mode Irradiation time: 2.0sec Number of times: 30 Laser spot diameter: 2.5μm Objective lens: 20x
[0133] <Measurement method> The measurements were carried out by the following method. (1) The Raman shift position was calibrated using a standard sample (single crystal silicon, manufactured by Renishaw) (520.5 cm for single crystal silicon). -1 ). (2) The sheet-shaped sample was placed on the sample stage. If necessary, a presser was installed to keep the sheet flat. (3) The device was focused and observed (the focus was set to the smallest using the simulated laser). When measuring the printed area, the darkest part that could be visually confirmed was measured to be at the center of the guide displayed during measurement. When measuring the non-printed area, the measurement was made at a distance of 300 μm or more from the printed area. (4) The obtained Raman spectrum was subjected to baseline correction (intelligent correction) using the processing software attached to the device (Renishaw, Wire5.2). The baseline was corrected using polynomial 11 of the processing software. (5) Rutile titanium dioxide: 447±10cm -1 , 516±10cm for anatase titanium dioxide -1 The maximum value (maximum intensity) in the wavenumber range was read, and the Raman intensity ratio was calculated according to the following formula. Raman intensity ratio = maximum intensity in printed area ÷ maximum intensity in non-printed area (6) Ten points were measured in each of the printed area (printed portion) and non-printed area (non-printed portion), and the average value was used as the measurement result. From the viewpoint of suppressing the variation of the measured values, it is preferable to measure the Raman intensity count of the printed area in a range of 10,000 or less. Therefore, the measurement conditions were appropriately changed so that the Raman intensity count of the printed area was in a range of 10,000 or less. In addition, 10 measurements were performed under the following measurement conditions, and values that deviated beyond the average value ± 2SD (standard deviation) were excluded, and the average was calculated again to obtain the average value of the Raman intensity. The Raman intensity ratio was evaluated according to the following criteria. A: Raman intensity ratio is 0.3 or less B: Raman intensity ratio is greater than 0.3 and less than or equal to 0.7 C: Raman intensity ratio exceeds 0.7
[0134] [Clarity of a single printed point] <Laser marking method> For the printing films obtained in the Examples and Comparative Examples, a 10 mm square was printed on the sample surface using an ultraviolet laser irradiation machine (manufacturer: Keyence Corporation, model number: MD-U1020C). (Printing conditions) Wavelength: 355nm Output: 80% (2.5W at 100% output) Frequency: 40kHz Focal length: 300mm (focusing is performed using the height correction included with the device) Spot diameter: 40μm (when focused) Fill spacing: 0.3mm Scan speed: 5000mm / sec Spot variable: 100
[0135] <Clarity evaluation> A digital microscope (manufacturer: Keyence Corporation, model number: VHX-8000) was used to obtain depth composite images of the area near the printed area to be evaluated. A depth stacking image is an image that is created by capturing multiple images by changing the focal length, extracting the in-focus parts from each image, and reconstructing them into a single image. Depth stacking images were captured using the live depth stacking function built into a digital microscope. After that, the brightness extraction mode of the automatic area measurement function was used to measure the area of the printed area that was darker than the threshold. The brightness extraction mode is a mode that classifies the brightness level of the image from -255 to 255 and extracts areas above or below an arbitrary threshold. Regarding the printed portion, the more areas with a luminance level lower than the threshold value, the darker the print is considered to be. (Settings when taking images) Shutter speed: Auto mode (set value 70) Gain: 0dB Magnification: 500x Lighting: Ring lighting (Brightness Extraction Mode Settings) Magnification when acquiring depth stacking image: 500x Illumination: 100% coaxial epi-illumination Shutter speed: Auto mode 70 Gain: 0dB Threshold: -10 Extraction area: Inside a circle with a radius of 60 μm from the center of the printed area (Evaluation criteria for print density) A: The area of the area with a brightness level lower than -10 is 70% or more of the extracted area. B: The area of the area with a luminance level lower than -10 is between 60% and 70% of the extracted area C: The area of the area with a luminance level lower than -10 is between 50% and 60% of the extracted area D: The area of the area with a luminance level lower than -10 is less than 50% of the extracted area.
[0136] [Printing uniformity] For the ultraviolet laser printing films obtained in the Examples and Comparative Examples, a 10 mm square was printed on the sample surface using an ultraviolet laser irradiation machine (manufacturer: Keyence Corporation, model number: MD-U1020C). (Printing conditions) Wavelength: 355nm Output: 80% (2.5W at 100% output) Frequency: 40kHz Focal length: 300mm (focusing is performed using the height correction included with the device) Spot diameter: 40μm (when focused) Fill interval (line pitch): 0.05mm Scan speed: 3000mm / sec Spot variable: -100
[0137] (Print uniformity evaluation) 100 squares were printed, and the printing uniformity was evaluated according to the following criteria based on the number of squares that had a visually noticeable difference in shading (printing non-uniformity). A: The number of squares with shading differences is less than 3 out of 100 squares. B: Out of 100 squares, the number of squares with shading differences is between 3 and 5 C: Out of 100 squares, the number of squares with shading differences is between 5 and 10 D: There are 10 or more squares with different shading out of 100 squares.
[0138] [Smoke generation] When evaluating the printing uniformity, a 10 mm x 10 mm square was printed on the surface of the sample by irradiation with an ultraviolet laser, and the smoke generation was evaluated according to the following criteria. (Judgment criteria) A: No visible smoke or very little visible smoke B: Smoke can be visually confirmed, but the amount of smoke is small. C: Smoke can be seen with the naked eye, but it is not enough to affect printing. D: Smoke is easily visible and is so great that it scatters the ultraviolet laser light and affects printing.
[0139] [Water vapor barrier properties] Measurements were performed in accordance with JIS-Z-0208:1976 (cup method) Method B (40°C ± 0.5°C, relative humidity 90% ± 2%) with the sealant layer facing inward. The water vapor barrier property was evaluated according to the following criteria. (Evaluation criteria for water vapor barrier properties) A: Water vapor permeability is 5g / m 2 ·day or less B: Water vapor permeability is 5g / m 2 · More than 10g / m 2 ·day or less C: Water vapor permeability is 10g / m 2 · Over 15g / m 2 ·day or less D: Water vapor permeability is 15g / m 2 ·Over the day
[0140] Laser irradiation was also carried out under the conditions described below, and the water vapor permeability of the ultraviolet laser print after laser irradiation was similarly measured. <Laser irradiation> For the ultraviolet laser printing films obtained in the examples and comparative examples, a 10 cm square was printed on the sample surface (printing layer side) using an ultraviolet laser irradiator (manufacturer: Keyence Corporation, model number: MD-U1020C) under the conditions described below. Printing conditions Wavelength: 355nm Output: 80% (2.5W at 100% output) Frequency: 40kHz Focal length: 300mm (focusing is performed using the height correction included with the device) Spot diameter: 40μm (when focused) Fill spacing: 0.04mm Scan speed: 1000mm / sec Spot variable: 0
[0141] [Oxygen Barrier Properties] The oxygen permeability of the films for ultraviolet laser printing of Examples 17 to 25 was measured using an oxygen permeability measuring device (OX-TRAN2 / 22, manufactured by MOCON) under conditions of a temperature of 23° C. and a relative humidity of 85%. Specifically, the oxygen transmission rate of the ultraviolet laser printing film was measured at a temperature of 23° C. and a relative humidity of 85% in accordance with JIS K7126-2:2006. The lower the oxygen permeability value, the better the oxygen barrier property. The oxygen barrier property was evaluated according to the following criteria. (Evaluation criteria for oxygen barrier properties) A: Oxygen permeability is 3.0mL / m 2 ·day · atm or less B: Oxygen permeability is 3.0mL / m 2 ·day·atm, 5.0mL / m 2 ·day · atm or less C: Oxygen permeability is 5.0mL / m 2 ·day·atm, 15mL / m 2 ·day · atm or less D: Oxygen permeability is 15mL / m 2 ·day·exceeds ATM
[0142] Laser irradiation was also carried out under the following conditions, and the oxygen permeability of the ultraviolet laser print after laser irradiation was similarly measured. <Laser irradiation> For the ultraviolet laser printing films obtained in the examples and comparative examples, a 10 cm square was printed on the sample surface (printing layer side) using an ultraviolet laser irradiator (manufacturer: Keyence Corporation, model number: MD-U1020C) under the conditions described below. Printing conditions Wavelength: 355nm Output: 80% (2.5W at 100% output) Frequency: 40kHz Focal length: 300mm (focusing is performed using the height correction included with the device) Spot diameter: 40μm (when focused) Fill spacing: 0.04mm Scan speed 1000mm / sec Spot variable: 0
[0143] [Barrier property reduction rate after UV laser irradiation (barrier property reduction rate)] The decrease in barrier property (barrier property decrease rate) due to ultraviolet laser irradiation was evaluated based on the water vapor permeability and oxygen permeability before and after ultraviolet laser irradiation according to the following evaluation criteria. (Evaluation criteria for barrier property deterioration rate) A: The rate of decrease (reduction) in water vapor permeability and oxygen permeability is 5.0% or less B: The decrease (reduction rate) of water vapor permeability and / or oxygen permeability exceeds 5.0%. The rate of decrease in water vapor permeability is calculated as follows. Decrease rate of water vapor permeability = (water vapor permeability after UV laser irradiation (g / m 2 ·day)-Water vapor permeability before UV laser irradiation (g / m 2 ·day) / Water vapor permeability before UV laser irradiation (g / m 2 ·day)×100 Similarly, the decrease in oxygen permeability is calculated as follows. Decrease rate of oxygen permeability = (oxygen permeability after UV laser irradiation (mL / m 2 ·day·atm)-Oxygen permeability before UV laser irradiation (mL / m 2 ·day·atm) / Oxygen permeability before UV laser irradiation (mL / m 2 ·day·atm)×100
[0144] [Heat seal peel strength and rate of decrease in heat seal peel strength (rate of decrease in peel strength)] Two sheets of UV laser printing film were stacked with the sealant layers facing each other, and heat sealed at 160°C, 0.2 MPa, and 1 second using a heat seal tester (Tester Sangyo, TP-701-B). The heat-sealed test piece was left to stand for more than 4 hours in a room with a temperature of 23°C ± 1°C and a humidity of 50% ± 2%. The heat-sealed test piece was then cut to a width of 15 mm and T-peeled at a tensile speed of 300 mm / min using a tensile tester, and the maximum load recorded was taken as the heat seal peel strength. The heat seal peel strength was evaluated according to the following criteria. (Evaluation criteria for heat seal peel strength) A: Heat seal peel strength is 10N / 15mm or more B: Heat seal peel strength is 6.0N / 15m or more and less than 10N / 15mm C: Heat seal peel strength is 3.0N / 15mm or more and less than 6.0N / 15mm D: Heat seal peel strength is less than 3.0N / 15mm <Laser irradiation> For the ultraviolet laser printing films obtained in the Examples and Comparative Examples, a 10 cm square was printed on the sample surface using an ultraviolet laser irradiator (manufacturer: Keyence Corporation, model number: MD-U1020C) under the conditions described below. Printing conditions Wavelength: 355nm Output: 80% (2.5W at 100% output) Frequency: 40kHz Focal length: 300mm (focusing is performed using the height correction included with the device) Spot diameter: 40μm (when focused) Fill spacing: 0.04mm Scan speed 1000mm / sec Spot variable: 0 (Evaluation criteria for heat seal peel strength reduction rate) The heat seal peel strength reduction rate due to ultraviolet laser irradiation was evaluated based on the heat seal peel strength before and after ultraviolet laser irradiation according to the following evaluation criteria: Note that for Comparative Example 4, the heat seal peel strength before ultraviolet laser irradiation was evaluated as D, so it was not measured. (Evaluation criteria for the rate of decrease in heat seal peel strength) A: Heat seal peel strength reduction rate (reduction rate) is 5.0% or less B: The rate of decrease (reduction) in heat seal peel strength exceeds 5.0%. The rate of decrease in heat seal peel strength is calculated as follows. Reduction rate of heat seal peel strength = (heat seal peel strength before UV laser irradiation (N / 15mm) - heat seal peel strength after UV laser irradiation (N / 15mm)) / heat seal peel strength before UV laser irradiation (N / 15mm) x 100
[0145] [Table 3-1]
[0146] [Table 3-2]
[0147] As shown in Table 3, by directly printing with an ultraviolet laser onto an ultraviolet laser printing film containing a specific amount of titanium oxide or more and having a titanium oxide crystallite size of a specific value or more, a print with excellent printing clarity for each individual point was obtained. Furthermore, the films had heat sealability and excellent water vapor barrier properties. The ultraviolet laser printing films of Examples 17 to 25, in which a barrier layer was formed, also had excellent oxygen barrier properties. Furthermore, the deterioration of the barrier properties and heat sealability due to printing with an ultraviolet laser was suppressed. In Example 6, which used titanium oxide with a relatively large crystallite size of 55.3 nm, a decrease in print uniformity was observed, which was thought to be due to a decrease in dispersibility. In Example 8, which used titanium oxide with a diffraction angle of 27.74° and relatively low crystallinity, a slight decrease in print clarity was observed for each individual point. The printing films of Comparative Examples 1 and 2, which used titanium oxide with a crystal size of less than 30 nm, produced prints with poor print clarity for each individual point. The ultraviolet laser printing film of Comparative Example 3, which contained titanium oxide at 0.05% by mass and less than 0.2% by mass, produced print spots with poor print clarity for each individual point when irradiated with an ultraviolet laser. Moreover, when the printing film of Comparative Example 4, which did not have a sealant layer, was used, the heat sealability and water vapor barrier property were not obtained. [Industrial Applicability]
[0148] The ultraviolet laser printing film of the present invention can provide a printed matter with excellent visibility by discoloring titanium oxide by irradiation with an ultraviolet laser, and further suppresses smoke generation during irradiation with an ultraviolet laser. The ultraviolet laser printing film and printed matter of the present invention are suitably applied to processed products such as packages (preferably food containers), labels, and adhesive tapes on which variable information such as dates and bar codes are printed. Furthermore, the method for producing printed matter of the present invention is suitably applied to printing variable information on packages, labels, adhesive tapes, etc.
Claims
1. A film for ultraviolet laser printing comprising a film substrate having titanium oxide added thereto, and a sealant layer on at least one surface of the film substrate, The content of titanium oxide in the film substrate is 0.2% by mass or more, The crystallite size of the titanium oxide is 30 nm or more. UV laser printing film.
2. 2. The film for ultraviolet laser printing according to claim 1, wherein the crystallite size of the titanium oxide is 53 nm or less.
3. 2. The film for ultraviolet laser printing according to claim 1, wherein the titanium oxide is rutile titanium oxide, and the diffraction angle of the titanium oxide is 27.60° or less.
4. 2. The film for ultraviolet laser printing according to claim 1, wherein the resin constituting the film substrate is at least one selected from the group consisting of polyolefins, polyesters, and polyvinyl chlorides.
5. 2. The film for ultraviolet laser printing according to claim 1, wherein the content of titanium oxide in the film substrate is 50% by mass or less.
6. 2. The film for ultraviolet laser printing according to claim 1, further comprising a barrier layer between the film substrate and the sealant layer.
7. A printed matter obtained from the ultraviolet laser printing film according to any one of claims 1 to 6, the printed matter has, at least in part, a printed area containing discolored titanium oxide; A printed matter, in which the ratio of the Raman intensity originating from titanium oxide in a printed area to the Raman intensity originating from titanium oxide in a non-printed area is 0.70 or less.
8. A processed product obtained by using the film for ultraviolet laser printing according to any one of claims 1 to 6.
9. A processed product obtained by using the printed matter according to claim 7.
10. A step of printing by irradiating the ultraviolet laser printing film according to any one of claims 1 to 6 with an ultraviolet laser to discolor the irradiated area, A method for producing printed matter.
11. 11. The method for producing a printed matter according to claim 10, wherein the printing step is a step of irradiating with an ultraviolet laser so that the ratio of the Raman intensity derived from titanium oxide in the printed area to the Raman intensity derived from titanium oxide in the non-printed area is 0.70 or less.
Citation Information
Patent Citations
Thermoplastic resin composition for laser marking, resin molded article and method for laser marking
JP1998237319A
Polyacetal resin composition for laser-marking and laser-marked molded article
JP2001089632A
Resin composition for laser processing and joined resin member comprising the same
JP2006291196A
Polyamide resin composition for laser marking and laser-marked polyamide resin molding
JP2007098939A
Resin composition for laser marking and molded article using the same
JP2007118416A