Polyethylene resin composition comprising polymeric ultraviolet absorber
A polyethylene resin composition with a high molecular weight UV absorber and specific polyethylene blends addresses UV barrier and bleed-out issues, providing effective long-term UV absorption and transparency for medical and food packaging.
Patent Information
- Application Number
- JP2023062796
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-07
- Publication Date
- 2024-10-18
AI Technical Summary
Existing polyethylene films for medical and food packaging lack effective UV barrier properties in the long-wave ultraviolet region (320-400 nm) without compromising transparency or durability, and organic UV absorbers tend to bleed or degrade over time, especially under high humidity conditions.
A polyethylene resin composition containing a specific polymeric UV absorber with a benzotriazole or benzophenone group, acrylic group, and a weight average molecular weight of 15,000 g/mol or more, blended with linear low-density and high-density polyethylene in specific ratios, ensuring excellent UV absorption and transparency while preventing bleed-out under high humidity.
The composition maintains high UV absorption and transparency in the long-wavelength region, preventing bleed-out even under high humidity conditions, thus ensuring long-term photostability and appearance of the film.
Smart Images

Figure 2024149110000001 
Figure 2024149110000002 
Figure 2024149110000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyethylene resin composition containing a polymeric ultraviolet absorber. [Background technology]
[0002] Medical films for packaging liquid medicines, blood, etc., and food films for packaging food ingredients are required to have transparency for visually checking the presence of liquid or contents and the presence or absence of foreign matter, and ultraviolet barrier properties for preventing deterioration of the active ingredients in the liquid or contents. In order to impart ultraviolet barrier properties to films, ultraviolet absorbers and light stabilizers are usually added, and ultraviolet absorbers and light stabilizers with various chemical structures are commercially available. In particular, inorganic ultraviolet absorbers and organic ultraviolet absorbers may be used as ultraviolet absorbers. Inorganic ultraviolet absorbers (see, for example, Patent Documents 1 to 3, etc.) have excellent durability such as light resistance and heat resistance, but the absorption wavelength is determined by the band gap of the compound, so there is little freedom of selection, and there is no inorganic ultraviolet absorber that can absorb up to the long-wave ultraviolet (UV-A) region of 320 to 400 nm, and those that absorb long-wave ultraviolet have absorption up to the visible region, so they are accompanied by coloring. In contrast, organic ultraviolet absorbers have a high degree of freedom in the structure design of the absorber, so that various absorption wavelengths can be obtained by devising the structure of the absorber. So far, systems using various organic ultraviolet absorbents such as benzotriazole, benzophenone, triazine, and cyan have been studied, and when absorbing up to the long-wave ultraviolet region, two methods have been considered: using one with a maximum absorption wavelength in the long-wave ultraviolet region, or increasing the concentration. However, those with a maximum absorption wavelength in the long-wave ultraviolet region described in Patent Documents 4 and 5, etc., have a problem of poor light resistance and decreasing absorption ability over time.
[0003] In contrast, benzotriazole-based UV absorbers have relatively good light resistance, and if the concentration is increased, they can relatively clearly cut even the long wavelength region (see, for example, Patent Document 6). However, since these UV absorbers generally have low molecular weights, when added at high concentrations, they bleed over time from the product surface or in environments where they come into contact with water, such as high-pressure steam sterilization, impairing the transparency and appearance of the product, and at the same time, it is known to be difficult to impart long-term light stability to the product.
[0004] In order to solve such problems, attempts have been made to increase the molecular weight of an ultraviolet absorber to which a group having a double bond such as a vinyl group has been added, thereby preventing the volatilization, thermal decomposition, leaching, etc. of the ultraviolet absorber (Patent Documents 7 to 9). However, even these polymeric ultraviolet absorbers, such as polyethylene, have problems such as reduced transparency and poor long-term light resistance. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 5-339033 [Patent Document 2] Japanese Patent Application Publication No. 5-345639 [Patent Document 3] Japanese Patent Application Publication No. 6-56466 [Patent Document 4] Japanese Patent Application Publication No. 6-145387 [Patent Document 5] JP 2003-177235 A [Patent Document 6] JP 2005-517787 A [Patent Document 7] Japanese Patent Application Publication No. 60-38411 [Patent Document 8] Japanese Patent Publication No. 181360 / 1983 [Patent Document 9] Japanese Patent Application Publication No. 3-281685 Summary of the Invention [Problem to be solved by the invention]
[0006] The object of the present invention is to provide a polyethylene resin composition which has excellent ultraviolet absorbency and transparency in the long-wave ultraviolet region around 340 nm and which is less prone to bleeding out even under high humidity conditions. [Means for solving the problem]
[0007] As a result of intensive research, the present inventors have found that a polyethylene resin composition containing a specific ultraviolet absorber and a specific amount of polyethylene can solve the above problems, and have completed the present invention. That is, the present invention relates to the following inventions. [1] A polyethylene resin composition comprising: 0.5 to 3.0 mass% of a polymeric ultraviolet absorber which contains a benzotriazole group or a benzophenone group, and also contains an acrylic group, and which has a weight-average molecular weight of 15,000 g / mol or more and a glass transition temperature of 40°C or more; and 97.0 to 99.5 mass% of polyethylene. [2] The polyethylene resin composition according to the above item [1], wherein the polyethylene comprises 40 to 90 mass% of a linear low-density polyethylene (A) satisfying the following properties (a) to (d) and 10 to 60 mass% of a high-density polyethylene (B) satisfying the following properties (e) to (g): (a) Density measured by the density gradient tube method in accordance with JIS K6922-1 is 890 to 915 kg / m 3 It is. (b) The melt mass flow rate (hereinafter referred to as MFR) measured in accordance with JIS K 6922-1 at 190° C. under a load of 21.18 N is 0.1 to 15 g / 10 min. (c) The ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) measured by gel permeation chromatography (hereinafter referred to as GPC) is 3.0 or less. (d) The n-heptane extractables at 50°C are 1.5% by mass or less. (e) Density measured by the density gradient tube method in accordance with JIS K6922-1 is 940 to 970 kg / m 3 It is. (f) The MFR measured in accordance with JIS K 6922-1 at 190°C under a load of 21.18 N is 0.1 to 15 g / 10 min. (g) The ratio (Mw / Mn) of weight average molecular weight (Mw) to number average molecular weight (Mn) measured by GPC is 3.0 or less. [3] The polyethylene resin composition according to the above [1] or [2], wherein, when the polyethylene resin composition is formed into a film having a thickness of 100 μm, the film has an ultraviolet ray transmittance of 5% or less at a wavelength of 340 nm and a visible light transmittance of 70% or more at a wavelength of 450 nm, and the ultraviolet absorber does not bleed out when stored for 28 days in an atmosphere having a temperature of 40° C. and a relative humidity of 75%. [4] A medical container comprising the polyethylene resin composition according to any one of the above [1] to [3]. Effect of the Invention
[0008] The polyethylene resin composition of one embodiment of the present invention has excellent ultraviolet absorbency and transparency in the long-wave ultraviolet region of around 340 nm, and is also resistant to bleeding out under high humidity, so that it can maintain high ultraviolet absorbency and good appearance for a long period of time. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The present invention will be described in detail below.
[0010] The polyethylene resin composition of one embodiment of the present invention contains 0.5 to 3.0 mass % of a polymeric ultraviolet absorber which contains a benzotriazole group or a benzophenone group, and also contains an acrylic group, and which has a weight-average molecular weight of 15,000 g / mol or more and a glass transition temperature of 40°C or more, and 97.0 to 99.5 mass % of polyethylene.
[0011] The polymeric ultraviolet absorber may be any polymeric ultraviolet absorber that contains a benzotriazole group or a benzophenone group, an acrylic group, a weight average molecular weight of 15,000 g / mol or more, and a glass transition temperature of 40° C. or more. Examples of such polymeric polymers include polymeric copolymers of a monomer having an ultraviolet absorbing molecular structure containing a benzotriazole group or a benzophenone group and a polymerizable monomer having an acrylic group. Specifically, examples of such polymeric polymers include polymeric copolymers obtained by copolymerizing a monomer having an ultraviolet absorbing molecular structure such as benzotriazole or benzophenone having a reactive unsaturated ethylene group in the molecular structure with a polymerizable monomer having an acrylic group such as (meth)acrylate or (meth)acrylamide. As a monomer having an ultraviolet absorbing molecular structure, a monomer having a benzotriazole group is more preferable in that it has good light resistance and can cut relatively clearly up to the long wavelength region. As a polymerizable monomer, methacrylate is more preferable in that the light resistance, heat resistance, and transparency of the obtained polymeric ultraviolet absorber are good, and the heat resistance of the obtained polymeric ultraviolet absorber is better. As the polymerizable monomer, vinyl ether, vinyl ester, siloxane, α-olefin, substituted styrene, etc. may be used in combination. The content of the polymerizable monomer in the polymeric ultraviolet absorber is preferably 30 to 90% by mass relative to 100% by mass of the polymeric ultraviolet absorber of this embodiment. When the content of the polymerizable monomer is 30% by mass or more, the copolymerization reactivity is better than when the content of the polymerizable monomer is less than 30% by mass, and a polymeric ultraviolet absorber with a high molecular weight can be obtained. When the content of the polymerizable monomer is 90% by mass or less, the ultraviolet absorbency of the obtained polymeric ultraviolet absorber is better than when the content of the polymerizable monomer is more than 90%. In addition, the copolymerization form of the polymeric ultraviolet absorbent is not particularly limited as long as it is possible to obtain a polymeric ultraviolet absorbent that contains a benzotriazole group or a benzophenone group, an acrylic group, a weight-average molecular weight of 15,000 g / mol or more, and a glass transition temperature of 40°C or more, and may be a block copolymer or a random copolymer.
[0012] The weight average molecular weight of the polymeric ultraviolet absorber is 15,000 g / mol or more, preferably 17,000 g / mol or more, and more preferably 20,000 g / mol or more, in order to obtain a polyethylene resin composition having good bleeding resistance under high temperature and high humidity. If the weight average molecular weight is less than 15,000 g / mol, bleeding tends to occur under high temperature and high humidity, and the polyethylene resin composition has poor bleeding resistance.
[0013] Moreover, the glass transition temperature of the polymeric ultraviolet absorber is 40° C. or higher, preferably 50° C. or higher, and more preferably 70° C. or higher, in order to obtain a polyethylene resin composition having good bleeding resistance under high temperature and high humidity conditions. If the glass transition temperature is less than 40° C., bleeding will be likely to occur under high temperature and high humidity conditions, and the bleeding resistance of the polyethylene resin composition will be poor.
[0014] The polymeric ultraviolet absorber may be a commercially available product, such as NCI-707S-30T (manufactured by Nikko Chemical Laboratory Co., Ltd.), NCI-707S-30BK (manufactured by Nikko Chemical Laboratory Co., Ltd.), or ULS-1935LH (manufactured by Lion Specialty Chemicals Co., Ltd.).
[0015] The polyethylene may be any polyethylene generally known as polyethylene, including high-density polyethylene, low-density polyethylene, linear low-density polyethylene, ethylene-α-olefin copolymers such as ethylene-propylene copolymers, ethylene-butene copolymers, ethylene-hexene copolymers, and ethylene-octene copolymers, ethylene-acrylic acid ester copolymers, ethylene-methacrylic acid ester copolymers, ethylene-vinyl acetate copolymers, etc., and may contain two or more of these. In particular, a specific amount of linear low-density polyethylene (A) and high-density polyethylene (B) having specific physical properties is preferably blended, since the resulting polyethylene resin composition has excellent heat resistance and transparency.
[0016] The amount of the polyethylene blended is preferably a polyethylene resin composition containing 40 to 90 mass% of linear low-density polyethylene (A) and 10 to 60 mass% of high-density polyethylene (B), and more preferably a polyethylene resin composition containing 50 to 80 mass% of linear low-density polyethylene (A) and 20 to 50 mass% of high-density polyethylene (B), since the resulting polyethylene resin composition is particularly excellent in heat resistance and transparency. The total of the linear low-density polyethylene (A) and high-density polyethylene (B) is 100 mass%.
[0017] Here, the linear low density polyethylene (A) is a copolymer of ethylene and an α-olefin. Specific examples of the copolymer of ethylene and an α-olefin include ethylene-hexene-1 copolymer, ethylene-butene-1 copolymer, and ethylene-octene-1 copolymer.
[0018] The linear low-density polyethylene (A) can be produced by a production method such as a high-pressure method, a solution method, a gas phase method, etc., according to the methods described in, for example, JP 2009-275059 A and JP 2013-81494 A. When producing the linear low-density polyethylene (A), a Ziegler catalyst consisting of a solid catalyst component containing magnesium and titanium and an organoaluminum compound, a metallocene catalyst consisting of an organotransition metal compound containing a cyclopentadienyl derivative and a compound and / or an organometallic compound that reacts with the organotransition metal compound to form an ionic complex, a vanadium-based catalyst, etc. can be used, and the linear low-density polyethylene (A) can be produced by copolymerizing ethylene and an α-olefin with the catalyst.
[0019] The linear low-density polyethylene (A) has an MFR of preferably 0.1 to 15 g / 10 min, more preferably 0.5 to 10 g / 10 min, and even more preferably 1.0 to 5.0 g / 10 min, as measured in accordance with JIS K6922-1 at 190° C. under a load of 2.16 kg, since this results in excellent moldability and excellent surface appearance of the resulting molded article.
[0020] The linear low-density polyethylene (A) has a density of 890 to 915 kg / m as measured according to JIS K6922-1, so that the resulting molded product has excellent transparency. 3 is preferably 895 to 910 kg / m 3 It is more preferable that:
[0021] It is particularly preferable that the linear low-density polyethylene (A) has the following properties (c) and (d), since the polyethylene resin composition has improved low elution properties when used as a medical container. The linear low-density polyethylene (A) having such properties can be produced by using the metallocene catalyst. (c) The ratio of weight average molecular weight (Mw) to number average molecular weight (Mn) (Mw / Mn) as determined by gel permeation chromatography is 3.0 or less. (d) The amount of n-heptane extractables at 50°C is 1.5 wt% or less.
[0022] The high-density polyethylene (B) is an ethylene homopolymer or a copolymer of ethylene and an α-olefin. Specific examples of the copolymer of ethylene and an α-olefin include an ethylene-hexene-1 copolymer, an ethylene-butene-1 copolymer, and an ethylene-octene-1 copolymer.
[0023] The high-density polyethylene (B) can be produced by a production method such as a slurry method, a solution method, a gas phase method, etc., according to the methods described in, for example, JP 2009-275059 A, JP 2013-81494 A, etc. When producing the high-density polyethylene (B), a Ziegler catalyst consisting of a solid catalyst component containing magnesium and titanium and an organoaluminum compound, a metallocene catalyst consisting of an organotransition metal compound containing a cyclopentadienyl derivative and a compound and / or an organometallic compound that reacts with the organotransition metal compound to form an ionic complex, a vanadium-based catalyst, etc. can be used, and the high-density polyethylene (B) can be produced by homopolymerizing ethylene or copolymerizing ethylene and an α-olefin using the catalyst.
[0024] The high-density polyethylene (B) has an MFR of preferably 0.1 to 15 g / 10 min, more preferably 0.5 to 10 g / 10 min, and even more preferably 1.0 to 5.0 g / 10 min, as measured in accordance with JIS K6922-1 at 190° C. under a load of 2.16 kg, since this results in excellent moldability and excellent surface appearance of the resulting molded article.
[0025] In addition, the high density polyethylene (B) has a density of 940 to 970 kg / m as measured according to JIS K6922-1, so that the resulting molded product has excellent transparency. 3 is preferably 950 to 965 kg / m 3 It is more preferable that:
[0026] It is particularly preferable that the high-density polyethylene (B) has the following characteristic (g), since the polyethylene resin composition has improved low elution properties when used as a medical container. The high-density polyethylene (B) having such characteristics can be produced by using the metallocene catalyst. (g) The ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) measured by gel permeation chromatography (hereinafter referred to as GPC) is 3.0 or less.
[0027] The blend amount of the polymeric ultraviolet absorber in the polyethylene resin composition according to one embodiment of the present invention is preferably 0.5 to 3.0 mass % and more preferably 0.7 to 2.0 mass % in the resin composition, since this particularly improves the dispersibility of the copolymer in the resin composition and results in a resin composition with excellent ultraviolet absorbency and transparency.
[0028] The polyethylene resin composition may contain other thermoplastic resins such as polyolefin-based resins, and resin additives (for example, stabilizers such as heat stabilizers and weather resistance stabilizers, crosslinking agents, crosslinking assistants, antistatic agents, slip agents, antiblocking agents, antifogging agents, lubricants, dyes, pigments, fillers, mineral oil-based softeners, petroleum resins, waxes, etc.) within the scope of the present invention.
[0029] The method for producing the polyethylene resin composition is not particularly limited as long as the polymeric ultraviolet absorbent can be dispersed in polyethylene. For example, the polyethylene resin composition can be produced by kneading the polymeric ultraviolet absorbent with a resin.
[0030] For kneading the polymeric ultraviolet absorber and the polyethylene, a kneading device that is usually used for kneading resins, such as a single screw extruder, a twin screw extruder, a multi-screw extruder, a Banbury mixer, a pressure kneader, a rotating roll, an internal mixer, etc. Furthermore, the polymeric ultraviolet absorber and the polyethylene can be kneaded by heating, for example, at 160 to 260°C.
[0031] The polymeric ultraviolet absorber and polyethylene may be kneaded after premixing using a tumbler or a Henschel mixer. Alternatively, the polymeric ultraviolet absorber and polyethylene may be kneaded to produce a master batch containing the polymeric ultraviolet absorber at a high concentration, and then the master batch and a resin may be kneaded to produce a resin composition. The resin composition obtained by kneading the polymeric ultraviolet absorber and polyethylene may be molded into a predetermined shape by a conventionally known method.
[0032] The polyethylene resin composition can be molded to obtain a desired shape. The molding method is not particularly limited, and examples thereof include inflation molding, blow molding, injection molding, extrusion molding, calendar molding, Engel molding, vacuum molding, compression molding, etc. Regardless of the molding method, a molded product can be obtained that blocks ultraviolet rays to prevent deterioration of the contents and has excellent bleeding resistance and does not contaminate the contents.
[0033] The polyethylene resin composition according to one embodiment of the present invention preferably has an ultraviolet transmittance of 5% or less at a wavelength of 340 nm when made into a film having a thickness of 100 μm, since this makes it possible to prevent ultraviolet deterioration of the contents of a molded article in particular. Furthermore, preferably has a visible light transmittance of 70% or more at a wavelength of 450 nm when made into a film having a thickness of 100 μm, since this makes it possible to obtain a molded article in which the visibility of the contents is particularly good. The ultraviolet transmittance and the visible light transmittance can be measured using an ultraviolet-visible-near infrared spectrophotometer. Furthermore, preferably, the ultraviolet absorber does not bleed out when the film having a thickness of 100 μm is stored for 28 days in an atmosphere at a temperature of 40° C. and a relative humidity of 75%.
[0034] The medical container according to one embodiment of the present invention is made of the resin composition. The polyethylene resin composition has excellent ultraviolet absorption and transparency in the long-wave ultraviolet region around 340 nm, and is also resistant to bleeding out under high humidity, and therefore can be used for medical containers, food containers, cosmetic containers, etc. Examples of medical containers include infusion bags, kit preparation containers, plastic ampoules, eye drop containers, infusion bottles, infusion sets, oral medication containers, and dialysis fluid containers; examples of food containers include various beverage containers, concentrated beverage containers, seasoning containers, prepared food containers, dressing containers, mayonnaise and ketchup containers, various retort food containers, and baby bottles; examples of cosmetic containers include containers for hair styling products, hair products, perfumes, hair dyes, eye shadow, nail polish, lotions, creams, milky lotions, skin lotions, and perm solutions; and the medical containers such as infusion bags, kit preparation containers, plastic ampoules, eye drop containers, infusion bottles, infusion sets, oral medication containers, and dialysis fluid containers can be particularly suitably used. EXAMPLES
[0035] The present invention will be described in more detail below by showing examples, but the present invention is not limited to these examples.
[0036] The samples used in the examples and comparative examples were evaluated by the following methods. <Glass transition point, melting point> The melting point and heat of fusion were measured by a differential scanning calorimeter (DSC). After filling 5 mg of the sample into an aluminum pan, the sample was placed in the heat sink of a DSC apparatus (DSC 7000X, manufactured by Hitachi High-Tech Science Corporation, trade name) using an autosampler (AS-3, manufactured by Hitachi High-Tech Science Corporation, trade name). The temperature of the heater was set to -30°C. After raising the temperature of the heater from -30°C to 210°C at a rate of 10°C / min and holding for 5 min, then lowering the temperature to -30°C at a rate of 10°C / min and holding for 5 min, and then raising the temperature to 210°C again at a rate of 10°C / min, the glass transition point and melting point of the sample were measured. An empty aluminum pan was used as the reference substance. <Molecular weight, molecular weight distribution> The weight-average molecular weight (Mw), number-average molecular weight (Mn), and the ratio of weight-average molecular weight to number-average molecular weight (Mw / Mn) were measured by GPC. Using a GPC apparatus (HLC-8320GPC, manufactured by Tosoh Corporation, trade name) and columns (TSKgel GMHhr-H (6.0 mm I.D. × 4 cm) and TSKgel GMHhr-H (7.8 mm I.D. × 30 cm), manufactured by Tosoh Corporation, trade name), the column temperature was set to 40°C, and chloroform was used as the eluent for measurement. The measurement sample was prepared at a concentration of 0.002 - 1.0 mg / ml, and 0.3 ml was injected for measurement. The calibration curve for molecular weight was calibrated using polystyrene samples with known molecular weights. Note that Mw and Mn were determined as values in terms of linear polyethylene. <n-heptane extraction amount> Approximately 10 g of the pulverized sample passing through a 200-mesh sieve was precisely weighed, 400 ml of n-heptane was added, and extraction was carried out at 50°C for 2 hours. The percentage of the mass of the extract obtained by evaporating the solvent from the extract and drying and solidifying it with respect to the initial mass was calculated. <Density> The density was measured by the density gradient column method in accordance with JIS K6922-1. <mfr> The MFR was measured in accordance with JIS K6922-1.
[0037] In the examples and comparative examples, resins produced by the following methods and commercially available products were used. (1) Ultraviolet absorbers The following commercially available products were used. (X)-1: NCI-707S-30T (product name) manufactured by Nikko Chemical Laboratory Co., Ltd. (ultraviolet absorbing part: benzotriazole group, contained acrylic group: methacrylate, glass transition temperature = 78 ° C, Mw = about 20000 g / mol) (X)-2: NCI-707S-30BK (product name) manufactured by Nikko Chemical Laboratory Co., Ltd. (ultraviolet absorbing part: benzotriazole group, contained acrylic group: methacrylate, glass transition temperature = 78 ° C, Mw = about 20000 g / mol) (X)-3: RUVA-93 (product name) manufactured by Otsuka Chemical Co., Ltd. (ultraviolet absorbing part: benzotriazole group, contained acrylic group: none, melting point = 98 ° C, molecular weight = 323 g / mol) (X)-4: Adeka STAB (registered trademark) LA-36 (product name) manufactured by ADEKA CORPORATION (ultraviolet absorbing portion: benzotriazole group, contained acrylic group: none, melting point = 140°C, molecular weight = 315 g / mol) (X)-5: Adeka STAB (registered trademark) LA-31RG (product name) manufactured by ADEKA CORPORATION (ultraviolet absorbing portion: benzotriazole group, contained acrylic group: none, melting point = 195°C, molecular weight = 659 g / mol) (2) Linear low-density polyethylene (A)-1 [Preparation of denatured clay] 30 ml of 37% hydrochloric acid and 106 g of N,N-dimethyl-behenylamine were added to 1,500 ml of water to prepare an aqueous solution of N,N-dimethyl-behenylammonium hydrochloride. 300 g of montmorillonite with an average particle size of 7.8 μm (prepared by pulverizing Kunipia F, a product of Kunimine Industries, with a jet pulverizer) was added to the aqueous solution of hydrochloride and reacted for 6 hours. After the reaction was completed, the reaction solution was filtered and the resulting cake was dried under reduced pressure for 6 hours to obtain 370 g of a modified clay compound.
[0038] [Preparation of polymerization catalyst] In a 20L stainless steel container under nitrogen atmosphere, 3.3L of heptane, 1.13mol (0.9L) of a heptane solution of triethylaluminum (20% by mass diluted product) per aluminum atom, and 50g of the modified clay compound obtained above were added and stirred for 1 hour. Diphenylmethylene (4-phenyl-indenyl) (2,7-di-t-butyl-9-fluorenyl) zirconium dichloride was added at 1.25mmol per zirconium atom and stirred for 12 hours. 5.8L of an aliphatic saturated hydrocarbon solvent (Idemitsu Petrochemicals, product name IP Solvent 2835) was added to the resulting suspension to prepare a catalyst. (Zirconium concentration 0.125mmol / L) [Production of (A)-1] A tank-type reactor equipped for high-temperature, high-pressure polymerization was used, and ethylene and 1-hexene were continuously injected into the reactor, with the total pressure set at 90 MPa, the 1-hexene concentration at 18 mol%, and the hydrogen concentration at 5 mol%. The reactor was then stirred at 1,500 rpm, and the polymerization catalyst obtained above was continuously fed from the reactor's feed port, and the polymerization reaction was carried out while maintaining the average temperature at 200°C. The obtained linear low-density polyethylene ((A)-1) had an MFR of 2.0 g / 10 min and a density of 907 kg / m 3 The results of the evaluation of the basic characteristics of (A)-1 are shown in Table 1.
[0039] (A)-2 [Preparation of denatured clay] A modified clay compound was prepared in the same manner as in (A)-1.
[0040] [Preparation of polymerization catalyst] A polymerization catalyst was prepared in the same manner as in (A)-1.
[0041] [Production of (A)-2] A tank-type reactor equipped for high-temperature, high-pressure polymerization was used, and ethylene and 1-hexene were continuously injected into the reactor, with the total pressure set at 90 MPa, the 1-hexene concentration at 20 mol%, and the hydrogen concentration at 15 mol%. The reactor was then stirred at 1,500 rpm, and the polymerization catalyst obtained above was continuously fed from the reactor's feed port, and the polymerization reaction was carried out while maintaining the average temperature at 200°C. The obtained linear low-density polyethylene ((A)-2) had an MFR of 12 g / 10 min and a density of 907 kg / m 3 The results of the evaluation of the basic characteristics of (A)-2 are shown in Table 1.
[0042] (A)-3 [Preparation of denatured clay] A modified clay compound was prepared in the same manner as in (A)-1.
[0043] [Preparation of polymerization catalyst] A polymerization catalyst was prepared in the same manner as in (A)-1.
[0044] [Production of (A)-3] Using a tank-type reactor equipped for high-temperature, high-pressure polymerization, ethylene and 1-hexene were continuously injected into the reactor, and the total pressure was set to 90 MPa, the 1-hexene concentration to 18 mol%, and the hydrogen concentration to 7 mol%. The reactor was then stirred at 1,500 rpm, and the polymerization catalyst obtained above was continuously fed from the reactor's feed port, and the polymerization reaction was carried out while maintaining the average temperature at 200°C. The obtained linear low-density polyethylene ((A)-3) had an MFR of 3.5 g / 10 min and a density of 910 kg / m 3 The results of the evaluation of the basic characteristics of (A)-3 are shown in Table 1.
[0045] [Table 1]
[0046] (3) High-density polyethylene (B)-1 [Preparation of denatured clay] Dimethylbehenylamine (C22H45)(CH3)2N (354 g) and 37% hydrochloric acid (83.3 mL) were added to a mixed solvent of 4.8 L of deionized water and 3.2 L of ethanol to prepare a dimethylbehenylamine hydrochloride solution. Synthetic hectorite (1,000 g) was added to this solution and stirred overnight. The reaction solution was filtered, and the solid was thoroughly washed with water. The solid was dried to obtain 1,180 g of an organically modified clay compound. The liquid content measured with an infrared moisture meter was 0.8%. Next, this organically modified clay compound was pulverized to adjust the average particle size to 6.0 μm. [Preparation of polymerization catalyst] In a 5L flask, 450g of the organic modified clay compound obtained above and 1.4kg of hexane were added, followed by 1.78kg (1.8mol) of a 20% by mass solution of triisobutylaluminum in hexane and 7.32g (18mmol) of bis(n-butyl-cyclopentadienyl)zirconium dichloride, which were then heated to 60°C and stirred for 1 hour. The reaction solution was cooled to 45°C, allowed to stand for 2 hours, and the supernatant was removed by decantation. Next, 1.78kg (0.09mol) of a 1% by mass solution of triisobutylaluminum in hexane was added, and the reaction was carried out at 45°C for 30 minutes. The reaction solution was allowed to stand for 2 hours at 45°C, and the supernatant was removed by decantation, and 0.45kg (0.45mol) of a 20% by mass solution of triisobutylaluminum in hexane was added, and the mixture was diluted again with hexane to a total volume of 4.5L to prepare a polymerization catalyst.
[0047] [Production of (B)-1] To a 300 L polymerization vessel, 135 kg / h of hexane, 20.0 kg / h of ethylene, 0.3 kg / h of butene-1, 5 NL / h of hydrogen, and the polymerization catalyst obtained in the above section were continuously fed. In addition, triisobutylaluminum was continuously fed as a co-catalyst so that the concentration in the liquid was 0.93 mmol / kg hexane. The polymerization temperature was controlled at 85°C. The obtained high density polyethylene ((B)-1) had an MFR of 1.0 g / 10 min and a density of 952 kg / m 3 The results of the evaluation of the basic characteristics of (B)-1 are shown in Table 2.
[0048] (B)-2 [Preparation of denatured clay] A modified clay compound was prepared in the same manner as in (B)-1.
[0049] [Preparation of polymerization catalyst] A polymerization catalyst was prepared in the same manner as in (B)-1. [Production of (B)-2] Ethylene was continuously fed at 20.0 kg / h, butene-1 at 0.4 kg / h, hydrogen at 8 NL / h, and the polymerization catalyst obtained in the section "Preparation of polymerization catalyst". In addition, triisobutylaluminum was continuously fed as a co-catalyst so that the concentration in the liquid was 0.93 mmol / kg hexane. The polymerization temperature was controlled at 85°C. The obtained high density polyethylene ((B)-2) had an MFR of 3.0 g / 10 min and a density of 945 kg / m 3 The results of the evaluation of the basic characteristics of (B)-2 are shown in Table 2.
[0050] [Table 2]
[0051] The films used in the examples and comparative examples were produced by the following method. The samples used and the evaluation results are shown in Tables 3 and 4.
[0052] [Table 3]
[0053] [Table 4]
[0054] <Example 1> [Production of polyethylene resin composition] The ultraviolet absorber (X-1) was mixed at 5% by mass and the polyethylene (Y-1) was mixed at 95% by mass, and the mixture was kneaded in a single-screw extruder (manufactured by Toyo Seiki Seisakusho, Ltd., product name: Labo Plastomill D2025N) using a full-flight screw with a compression ratio of 3 at a heating temperature of 180°C and a rotation speed of 40 rpm. After cooling, the mixture was cut into pellets using a pelletizer to obtain a master batch.
[0055] The obtained master batch was mixed to 25% by mass and polyethylene (Y-1) to 75% by mass, and the mixture was kneaded using a full-flight screw with a compression ratio of 3 in a single-screw extruder (manufactured by Toyo Seiki Seisakusho, Ltd., product name: Labo Plastomill 2D25S) under conditions of a heating temperature of 180°C and a rotation speed of 40 rpm. The kneaded product was cooled and then cut into pellets using a pelletizer to obtain a polyethylene resin composition.
[0056] [Film manufacturing] The above polyethylene resin composition was compressed in a compression molding machine AWFA.50 (manufactured by Shinto Metal Industries Co., Ltd.) at a heating temperature of 180°C and a heating pressure of 190 kgf / cm 2 After heating and compressing for 6 minutes, the mixture was immersed in cold water at a temperature of 15° C. and rapidly cooled and solidified to obtain a film having a thickness of 100 μm.
[0057] <Example 2> [Production of polyethylene resin composition] The ultraviolet absorber (X-1) was mixed at 1.3% by mass and the polyethylene (Y-1) was mixed at 98.7% by mass, and the mixture was kneaded in a single-screw extruder (manufactured by Toyo Seiki Seisakusho, Ltd., product name: Labo Plastomill D2025N) using a full-flight screw with a compression ratio of 3 at a heating temperature of 180°C and a rotation speed of 40 rpm. The kneaded mixture was cooled and then cut into pellets using a pelletizer to obtain a resin composition.
[0058] [Film manufacturing] A film was produced in the same manner as in Example 1.
[0059] <Examples 3 to 7 and Comparative Examples 1 to 6> A resin composition was produced in the same manner as in Example 2, except that the raw materials in Example 2 were changed to the raw materials and blending amounts shown in Table 4, and a film was produced using the resin composition. <Film evaluation> The films were evaluated by the following methods.
[0060] (UV absorption) A test piece measuring 10 mm in width and 50 mm in length was cut out from the prepared film, and the ultraviolet light transmittance at a wavelength of 340 nm was measured in pure water using an ultraviolet-visible spectrophotometer (model V-730, manufactured by JASCO Corporation). When the ultraviolet light transmittance was below 5%, the ultraviolet light absorbency was judged to be good (evaluated as ◯), and otherwise it was rated as ×.
[0061] ○: Good UV absorption ×: Poor UV absorption (transparency) A test piece measuring 10 mm wide x 50 mm long was cut out from the prepared film, and the visible light transmittance at a wavelength of 450 nm was measured in pure water using an ultraviolet-visible spectrophotometer (model V-730, manufactured by JASCO Corporation). When the visible light transmittance was more than 70%, the transparency was judged to be good (evaluated as ◯), and otherwise it was rated as ×.
[0062] ○: Good transparency ×: Poor transparency (Bleeding resistance) The prepared film was placed in a thermo-hygrostat (Hitachi Appliances, Inc., model EC26-MHHP) and stored for one month (28 days) under conditions of a temperature of 40°C and a relative humidity of 75%. After that, an arbitrarily selected spot on the film surface was observed with an optical microscope (Nikon Corporation, model LV100ND) set at an observation magnification of 50x to observe the presence or absence of bleeding. When no precipitate (copolymer or ultraviolet absorber) was present on the film surface in the entire observation image, the bleeding resistance was judged to be good (evaluated as ◯), and otherwise was evaluated as ×.
[0063] ○: Good bleeding resistance ×: Poor bleeding resistance< / mfr>
Claims
1. A polyethylene resin composition comprising: 0.5 to 3.0 mass % of a polymeric ultraviolet absorber which contains a benzotriazole group or a benzophenone group, and also contains an acrylic group, and has a weight average molecular weight of 15,000 g / mol or more and a glass transition temperature of 40° C. or more; and 97.0 to 99.5 mass % of polyethylene.
2. The polyethylene resin composition according to claim 1, wherein the polyethylene is 40 to 90 mass% of a linear low-density polyethylene (A) satisfying the following properties (a) to (d) and 10 to 60 mass% of a high-density polyethylene (B) satisfying the following properties (e) to (g). (a) A density of 890 to 915 kg / m as measured by a density gradient tube method in accordance with JIS K6922-1 3 It is. (b) The melt mass flow rate (hereinafter referred to as MFR) measured in accordance with JIS K 6922-1 at 190° C. and a load of 21.18 N is 0.1 to 15 g / 10 min. (c) The ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) measured by gel permeation chromatography (hereinafter referred to as GPC) is 3.0 or less. (d) the amount of n-heptane extractables at 50° C. is 1.5% by mass or less. (e) A density of 940 to 970 kg / m as measured by a density gradient tube method in accordance with JIS K6922-1. 3 It is. (f) The MFR measured in accordance with JIS K 6922-1 at 190° C. under a load of 21.18 N is from 0.1 to 15 g / 10 min. (g) The ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) measured by GPC is 3.0 or less.
3. 2. The polyethylene resin composition according to claim 1, wherein, when the polyethylene resin composition is formed into a film having a thickness of 100 μm, the film has an ultraviolet transmittance of 5% or less at a wavelength of 340 nm and a visible light transmittance of 70% or more at a wavelength of 450 nm, and the ultraviolet absorber does not bleed out when stored for 28 days in an atmosphere having a temperature of 40° C. and a relative humidity of 75%.
4. A medical container comprising the polyethylene resin composition according to any one of claims 1 to 3.
Citation Information
Patent Citations
Ultraviolet absorbing polymer comprising 2-hydroxy-5-acrylyloxyalkylphenyl-2h-benzotriazoles
JP1985038411A
High polymer material composition having improved light stability
JP1987181360A
Ultraviolet absorber for plastic
JP1991281685A
Manufacture of uv shielding glass and window glass for automobile and window glass for building
JP1993339033A
Solution composition for forming transparent zinc oxide film
JP1993345639A