Foam sheet
A foamed sheet with controlled properties, produced from an acrylic emulsion composition, addresses the issues of impact absorption and adhesion in thin configurations, enhancing protection for electronic devices.
Patent Information
- Application Number
- JP2023062988
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-07
- Publication Date
- 2024-10-18
AI Technical Summary
Existing foam sheets used in electronic and electrical equipment, particularly in display devices, lack sufficient point impact absorption and tape adhesion, especially in thin configurations, making them inadequate for protecting devices like organic EL displays.
A foamed sheet produced by foaming and curing an acrylic emulsion composition with controlled elution residual solidified material, specific thickness, density, and adhesive properties, incorporating an anionic surfactant and crosslinking agent, to enhance impact absorption and adhesion.
The solution provides a foam sheet with excellent point impact absorption and tape adhesion, ensuring effective protection for electronic devices by maintaining structural integrity and adhesion even under impact.
Smart Images

Figure 2024149234000003 
Figure 2024149234000004 
Figure 2024149234000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a foam sheet. [Background technology]
[0002] In recent years, as electronic and electrical devices become more precise, smaller, and more mobile, it has become important to prevent damage to the parts installed inside the devices. In particular, in the display devices of electronic and electrical devices, foams made of various materials are sandwiched as cushioning materials between the glass plate on the surface and the image display material to absorb shocks and vibrations and prevent damage. Furthermore, as the miniaturization progresses, the space for installing the above-mentioned cushioning materials is limited, making it impossible to give the cushioning materials a sufficient thickness, and so there is a demand for thin but sufficient shock absorption performance. In particular, organic EL displays use frit glass as a sealing material and do not have a backlight unit, so they are considered to be vulnerable to shocks, and the above-mentioned cushioning materials are required to have high shock resistance.
[0003] Patent Documents 1 and 2 propose a foam sheet as a cushioning material, and in particular, for electronic or electrical devices having a display unit, they propose using a foam sheet on the back of the display unit as a damage-preventing cushioning material. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 6366776 [Patent Document 2] JP 2020-015799 A DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]
[0005] An object of the present invention is to provide a foam sheet having excellent point impact absorbency and excellent tape adhesion (adhesion to adhesive tape / peel strength). [Means for solving the problem]
[0006] The present invention (1) is a foamed sheet obtained by foaming and curing an acrylic emulsion composition, characterized in that the amount of eluted residual solidified matter under the following elution conditions is 15 mg or less. (Elution conditions) 5 g of the foam sheet was added to 500 ml of water and boiled for 30 minutes, then filtered. 200 g of the filtrate was dried and the mass after drying was measured. The present invention (2) relates to the foam sheet according to the above-mentioned invention (1), which has a peel strength from an adhesive tape (85°C) of 5.0 N / 25 mm or more at an ambient temperature of 85°C. The present invention (3) relates to the foamed sheet according to any one of the above-mentioned inventions (1) to (2), wherein the above-mentioned acrylic emulsion composition is an acrylic emulsion composition obtained by emulsion polymerization of an acrylic monomer composition containing an acrylic monomer and a reactive emulsifier. The present invention (4) is the foamed sheet according to any one of the above inventions (1) to (3), wherein the emulsion composition contains 5 mass % or less of an anionic surfactant based on the mass (solid content) of the acrylic emulsion composition. The present invention (5) is an electronic / electrical device or a part thereof, comprising the foamed sheet according to any one of the above inventions (1) to (4).
[0007] According to the present invention, it is possible to provide a foamed sheet having excellent point impact absorbency and excellent tape adhesion (peel strength). [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a schematic diagram of a foamed sheet according to the present embodiment. [Diagram 2] FIG. 2 is a schematic diagram of a method for measuring the tape peel strength of a foam sheet against an adhesive tape. [Diagram 3] FIG. 3 is a schematic diagram showing the measurement of the point impact absorption rate using a drop type impact absorption tester.
[0009] 1. Foam sheet 1-1.Structure A preferred foam sheet according to the present invention is a foam sheet obtained by foaming and curing an acrylic emulsion composition, and characterized in that the amount of eluted residual solidified matter is 15 mg or less under the following elution conditions: Here, the foam sheet has a thickness of 0.03 mm or more and 1.0 mm or less, and an apparent density of 500 kg / m 3 More than 900kg / m 3 The thickness of the foamed sheet may be 0.01 MPa or less, the 25% compressive stress may be 0.01 MPa or more and 0.5 MPa or less, and the point impact absorption rate may be 5% or more. In this specification, the term "thickness of the foamed sheet" refers to the thickness of the foamed sheet only, and does not include the thickness of other layers including the adhesive layer, the substrate, and the release liner. In addition, when a plurality of foamed sheets are laminated, the sum of the thicknesses of the plurality of foamed sheets is referred to as the "thickness of the foamed sheet". The structure of the foamed sheet according to this embodiment will be described in detail below.
[0010] The thickness of the foamed sheet according to the present embodiment is preferably 0.03 mm or more and 1.0 mm or less. The thickness of the foamed sheet can be determined according to the application and design requirements. When the thickness is within this range, a higher uniform dispersion of bubbles and a more sufficient impact absorption can be realized, and furthermore, it becomes possible to fit the foamed sheet into the limited space of a space-saving electronic or electrical device. The lower limit of the thickness of the foamed sheet according to the present embodiment is more preferably 0.05 mm, 0.055 mm, 0.06 mm, 0.065 mm, 0.07 mm, 0.075 mm, or 0.08 mm, and the upper limit is more preferably 0.5 mm, 0.4 mm, 0.3 mm, or 0.2 mm.
[0011] The foam sheet according to the present embodiment may be a single layer {FIG. 1(a)} or a laminate with a substrate {FIG. 1(b)}. In the figure, 1 is a foam sheet and 2 is a substrate. By forming a laminate with a substrate, it is possible to give strength to the foam sheet. The method of forming the laminate with the substrate is not particularly limited, and examples thereof include a method of directly applying a foam onto a substrate, a method of providing an adhesive layer and laminating the substrate, etc. Also, a laminate in which the substrate, adhesive layer, and release liner are arranged in this order may be formed in advance, and a foam may be integrally molded on the surface of the substrate opposite to the side where the adhesive layer is present.
[0012] A release agent layer may be provided on the surface of the substrate on the side where the foamed sheet is formed, thereby allowing the substrate to serve as a release liner.
[0013] Furthermore, a release agent layer may be provided on the surface of the substrate opposite to the foamed sheet forming side, whereby the foamed sheet can be wound into a roll, thereby saving space during transportation and storage and protecting the foamed sheet from damage.
[0014] The foamed sheet according to the present embodiment can have an adhesive layer on one or both sides of its surface (FIG. 1(c): 3 is the adhesive layer). By providing an adhesive layer, it becomes easier to fix the foamed sheet to electronic / electrical device parts or electronic / electrical devices.
[0015] The foam sheet having an adhesive layer on one or both surfaces can further have a release liner on the surface of the adhesive layer {FIG. 1(d): in the figure, 3 is the adhesive layer, and 4 is the release liner}. By providing a release liner, damage to the adhesive layer during transportation or before use can be prevented.
[0016] Here, the foam sheet according to the present embodiment may be formed by laminating a foam other than the foam sheet according to the present embodiment, a substrate, a pressure-sensitive adhesive layer, and other known layers in a desired number and in a desired order. Further, although an embodiment in which one layer of the foam sheet according to the present embodiment is provided is preferable, a foam sheet having a plurality of foam sheets according to the present embodiment, such as substrate / foam sheet according to the present embodiment / pressure-sensitive adhesive layer / foam sheet according to the present embodiment / pressure-sensitive adhesive layer, may be used.
[0017] 2.Each part 2-1.Foam 2-1-1. Raw materials The foam according to the present embodiment contains, as raw materials, for example, an acrylic emulsion, a foaming agent, a foam stabilizer, etc. (anionic surfactant, amphoteric surfactant, thickener), water as a dispersion medium, a crosslinking agent, and other additives as necessary (the foaming gas used in the foaming step will be described in the section on the foaming step).
[0018] 2-1-1-1. Acrylic emulsion The raw material of the emulsion composition used in producing the foam according to the present embodiment contains an acrylic emulsion.
[0019] The acrylic emulsion according to the present embodiment is an acrylic emulsion obtained by emulsion polymerization of an acrylic monomer composition containing an acrylic monomer and a reactive emulsifier. The acrylic emulsion will be described in detail below.
[0020] The acrylic emulsion (aqueous dispersion of acrylic resin) can be produced by copolymerizing, for example, a polymerizable monomer component essentially consisting of a (meth)acrylic acid ester monomer, and, if necessary, other polymerizable monomers copolymerizable with these monomers, and a reactive emulsifier, in the presence of a polymerization initiator, a reactive emulsifier, and, if necessary, a dispersion stabilizer. Here, the acrylic resin emulsion may be a commercially available one, and may be one in which resin particles are dispersed in water as a continuous phase, and may contain a dispersant such as a surfactant, if necessary. In this specification, when (meth)acrylic acid is described, it includes methacrylic acid and acrylic acid. For example, when (meth)acrylic acid is described as methyl (meth)acrylate, it includes methyl methacrylate and methyl acrylate.
[0021] 2-1-1-1―1. (Meth)acrylic acid ester monomer Examples of (meth)acrylic acid esters include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, octadecyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, cyclohexyl (meth)acrylate, nonyl (meth)acrylate, dodecyl (meth)acrylate, stearyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, phenyl (meth)acrylate, and benzyl (meth)acrylate.
[0022] 2-1-1-1―2. Other polymerizable monomers Examples of other polymerizable monomers include unsaturated bond-containing monomers having a carboxyl group, such as acrylic acid, methacrylic acid, β-carboxyethyl (meth)acrylate, 2-(meth)acryloylpropionic acid, crotonic acid, itaconic acid, maleic acid, fumaric acid, itaconic acid half ester, maleic acid half ester, maleic anhydride, and itaconic anhydride; glycidyl group-containing polymerizable monomers, such as glycidyl (meth)acrylate and allyl glycidyl ether; 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and the like. Examples of such monomers include hydroxyl group-containing polymerizable monomers such as acrylate, polyethylene glycol mono(meth)acrylate, and glycerol mono(meth)acrylate; ethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, diallyl phthalate, divinylbenzene, allyl (meth)acrylate; and styrene.
[0023] 2-1-1-1―3. Reactive emulsifiers The reactive emulsifier according to this embodiment is preferably an emulsifier having a radically polymerizable double bond, and may be an anionic emulsifier or a nonionic emulsifier. A plurality of types of reactive emulsifiers may be used. The reactive emulsifier is preferably an anionic reactive emulsifier having a double bond (e.g., an allyl group) and an anionic group. Here, examples of the anionic group include a sulfonic acid group, a carboxylic acid group, a phosphoric acid group, a sulfate group, and salts thereof. A specific example of the anionic reactive emulsifier is sodium alkylaryl sulfosuccinate.
[0024] 2-1-1-1―4. Amount of reactive emulsifier The amount of the reactive emulsifier is preferably 0.8 parts by mass or more and 5.0 parts by mass or less, more preferably 0.8 parts by mass or more and 3.5 parts by mass or less, and even more preferably 1.0 parts by mass or more and 3.5 parts by mass or less, based on 100 parts by mass of the (meth)acrylic acid ester monomer (+other polymerizable monomers).
[0025] 2-1-1-1-5.Solid content of acrylic emulsion The solid content of the acrylic emulsion is preferably 30% by mass or more, more preferably 40% by mass or more, and even more preferably 50% by mass or more. The upper limit is, for example, 95% by mass, 90% by mass, 80% by mass, or 70% by mass.
[0026] 2-1-1-2. Dispersion medium The dispersion medium of the emulsion composition according to the present embodiment is essentially water. However, it may be a mixture of water and a water-soluble solvent. The water-soluble solvent may be, for example, alcohols such as methyl alcohol, ethyl alcohol, isopropyl alcohol, ethyl carbitol, ethyl cellosolve, and butyl cellosolve, polar solvents such as N-methylpyrrolidone, and a mixture of one or more of these may be used.
[0027] 2-1-1-3. Foaming agents (anionic surfactants) Anionic surfactants (foaming anionic surfactants) function as foaming agents for emulsion compositions. Specific examples of anionic surfactants include sodium laurate, sodium myristate, sodium stearate, ammonium stearate, sodium oleate, potassium oleate soap, potassium castor oil soap, potassium coconut soap, sodium lauroyl sarcosine, sodium myristoyl sarcosine, sodium oleyl sarcosine, sodium cocoyl sarcosine, sodium coconut alcohol sulfate, sodium polyoxyethylene lauryl ether sulfate, sodium alkyl sulfosuccinate, sodium lauryl sulfoacetate, sodium alkyl benzene sulfonate, sodium α-olefin sulfonate, etc. In particular, sodium alkyl sulfosuccinate is preferred.
[0028] In order to facilitate dispersion in the emulsion composition, the anionic surfactant used in this embodiment preferably has an HLB value of 10 or more, more preferably 20 or more, and particularly preferably 30 or more. Here, the HLB value is a value measured by the Water Number method.
[0029] 2-1-1-4. Foam stabilizer In addition to the anionic surfactant, it is preferable to use a bubble stabilizer as the surfactant according to this embodiment in order to make the bubbles fine and uniform. Here, an amphoteric surfactant is preferable as the bubble stabilizer. When an anionic surfactant and an amphoteric surfactant are used in combination, the charges of the hydrophilic groups of the anionic surfactant molecules repel each other, and the anionic surfactant molecules maintain a certain distance from each other. Meanwhile, the electrically neutral amphoteric surfactant enters between the molecules of the anionic surfactant, thereby further stabilizing the bubbles and reducing the size of the bubbles. Here, the amphoteric surfactant is not particularly limited, and examples thereof include amphoteric surfactants of amino acid type, betaine type, and amine oxide type. Betaine type amphoteric surfactants are preferable because they have a higher effect as described above. Furthermore, C10-12 is preferable in terms of ease of entering between the molecules of the anionic surfactant.
[0030] 2-1-1-5. Crosslinking agent (hardening agent) The crosslinking agent (curing agent) according to the present embodiment includes, for example, an isocyanurate compound. Here, the isocyanurate compound is a compound having an isocyanurate ring.
[0031] Examples of the isocyanurate compound include an isocyanurate compound of an aliphatic diisocyanate, an isocyanurate compound of an aliphatic isocyanate silane, a (meth)acrylic compound having an isocyanurate ring, a thiol compound having an isocyanurate ring, and a glycidyl compound having an isocyanurate ring.
[0032] Examples of the isocyanurate compound of an aliphatic diisocyanate include isocyanurate compounds of an aliphatic diisocyanate such as hexamethylene diisocyanate (HDI), pentamethylene diisocyanate, trimethylhexamethylene diisocyanate (TMHDI), lysine diisocyanate, and norbornane diisocyanate (NBDI).
[0033] Examples of the isocyanurate compound of an aliphatic isocyanate silane include compounds obtained by isocyanating an aliphatic isocyanate silane such as isocyanate propyl triethoxy silane and isocyanate propyl trimethoxy silane.
[0034] Examples of the (meth)acrylic compound having an isocyanurate ring include ethoxylated isocyanuric acid triacrylate, ε-caprolactone-modified tris(2-acryloxyethyl)isocyanurate, and compounds obtained by reacting an aliphatic diisocyanate such as hexamethylene diisocyanate (HDI), pentamethylene diisocyanate, trimethylhexamethylene diisocyanate (TMHDI), lysine diisocyanate, or norbornane diisocyanate (NBDI) with a hydroxyl group-containing acrylamide monomer such as hydroxyethylacrylamide, or a hydroxyl group-containing acrylate such as 4-hydroxybutyl acrylate.
[0035] Examples of thiol compounds having an isocyanurate ring include tris(ethyl-3-mercaptopropionate)isocyanurate and 1,3,5-tris(3-mercaptobutyryloxyethyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione.
[0036] An example of the glycidyl compound having an isocyanurate ring is 1,3,5-tris(2,3-epoxypropyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione.
[0037] These isocyanurate compounds can be used alone or in combination of two or more.
[0038] Among these isocyanurate compounds, aliphatic or alicyclic diisocyanate isocyanurate compounds are preferred, and aliphatic isocyanurate compounds are more preferred. By using these isocyanurate compounds, the time at which the reaction mixture liquid after mechanical stirring is discharged can be made appropriate, and by using a trimer, the mechanical properties of the foamed sheet can be made appropriate, and a foamed sheet with excellent point impact absorption can be obtained.
[0039] 2-1-2.Composition The amount (solid content) of the resin raw material (raw material composition containing an acrylic emulsion as an essential component) in the liquid medium is preferably 30 parts by mass or more and 80 parts by mass or less per 100 parts by mass of the liquid medium. By setting the amount in this range, it is possible to obtain an effect of molding a more stable foam. In addition, the preferred blend ratio of the foam according to this embodiment will be explained below. In addition, the blend amounts and blend ratios in the following description are based on the solid content unless otherwise specified.
[0040] 2-1-2-1. Mixture ratio in emulsion composition First, the components constituting the "solid content" of the acrylic emulsion referred to in this specification are the components excluding the dispersion medium from the emulsion. Specifically, in addition to the resin, it contains a surfactant and, in some cases, a filler, etc.
[0041] Based on the total amount of the acrylic emulsion (the sum of the solid content and non-solid content is 100 parts by mass), the content of the acrylic emulsion (solid content) is preferably more than 10 parts by mass and not more than 90 parts by mass, more preferably 20 parts by mass or more and not more than 80 parts by mass, even more preferably 30 parts by mass or more and not more than 70 parts by mass, and particularly preferably 50 parts by mass or more and not more than 60 parts by mass.
[0042] The amount of the anionic surfactant in the acrylic emulsion composition is preferably 1.0 part by mass or more and 10 parts by mass or less, and more preferably 3 parts by mass or more and 10 parts by mass or less, based on the total amount of the emulsion (the sum of the solid content and non-solid content being 100 parts by mass).
[0043] The amount of the amphoteric surfactant in the emulsion composition is preferably 0.5 parts by mass or more and 10 parts by mass or less, and more preferably 1 part by mass or more and 5 parts by mass or less, based on the total amount of the emulsion (the sum of the solid content and non-solid content being 100 parts by mass).
[0044] Regarding the amount of the crosslinking agent (curing agent) blended, the mass ratio of the crosslinking agent to the acrylic emulsion (solid content) in the acrylic emulsion composition (the crosslinking agent / the acrylic emulsion) is preferably 0.01 or more and 0.12 or less, and more preferably 0.025 or more and 0.05 or less.
[0045] 2-1-3. Manufacturing method The method for producing a foamed sheet according to the present embodiment includes a raw material preparation step, and a foaming / curing step (a step of foaming an acrylic emulsion composition containing at least an acrylic emulsion and a foaming agent by using a mechanical froth method to form a foam, and curing the foam). The acrylic emulsion composition may further contain a crosslinking agent. In this case, application of energy crosslinks the resin constituting the acrylic emulsion via the crosslinking agent, thereby accelerating curing. Each step will be described in detail below.
[0046] 2-1-3-1. Raw material preparation process The raw material preparation step is a step of preparing an emulsion composition, which is a raw material mixture for a foamed sheet, by mixing the raw materials described above. The mixing method is not particularly limited, and may be, for example, a method of mixing the components while stirring them in a container such as a mixing tank.
[0047] 2-1-3-2. Foaming and curing process The foaming and curing step is a step of adding a predetermined foaming gas to the emulsion composition obtained in the raw material preparation step and thoroughly mixing them to produce a state in which a large number of bubbles exist in the emulsion composition (foamed emulsion composition). This foaming and curing step can usually be carried out by thoroughly mixing the raw material mixture obtained in the raw material preparation step with the foaming gas using a mixing device such as a mixing head.
[0048] 2-1-3-2-1. Foaming gas The foaming gas mixed into the emulsion composition in the stirring and foaming step in the foaming and curing step forms bubbles (cells) in the foam. The amount of foaming gas mixed in determines the expansion ratio and density of the resulting foam. In order to adjust the density of the foamed sheet, the weight of the raw material for the foamed sheet required is calculated from the desired density of the foamed sheet and the volume of the raw material for the foamed sheet (for example, the internal volume of the mold into which the raw material for the foamed sheet is injected), and the amount of the foaming gas is determined so that the desired volume is obtained for this weight. In addition, air is mainly used as the type of foaming gas, but other inert gases such as nitrogen, carbon dioxide, helium, and argon can also be used.
[0049] 2-1-3-2-2. Foaming method and conditions In the foaming and curing process, the foaming method and foaming conditions are not particularly limited, and examples thereof include the mechanical froth method and a method using a chemical foaming agent, with the mechanical froth method being preferred. The mechanical froth method is a method in which air in the atmosphere is mixed into the emulsion composition by stirring the emulsion composition with a stirring blade or the like, thereby foaming the emulsion composition. The stirring device is not particularly limited as long as it is a stirring device generally used in the mechanical froth method, and for example, a homogenizer, a dissolver, a mechanical froth foaming machine, etc. can be used. According to this mechanical froth method, a foamed sheet with a density suitable for various applications can be obtained by adjusting the mixing ratio of the emulsion composition and the air.
[0050] The time for mixing the emulsion composition with air is not particularly limited, and is usually 1 to 10 minutes, preferably 2 to 6 minutes. The mixing temperature is also not particularly limited, and is usually room temperature. The stirring speed in the above mixing is preferably 200 rpm or more (more preferably 500 rpm or more) in order to make the bubbles finer, and is preferably 2000 rpm or less (more preferably 800 rpm or less) in order to smoothly discharge the foam from the foaming machine.
[0051] 2-1-3-2-3. Formation of foam The emulsion composition foamed as described above (foamed emulsion composition) is formed into a sheet-like foam (foamed sheet) having a desired thickness by known means such as a doctor knife or a doctor roll.
[0052] 2-1-3-2-4.Curing The foam curing method is, for example, a known method. Preferably, the resin constituting the emulsion is cured by applying energy and crosslinking (through a crosslinking agent). Furthermore, when the emulsion is a self-crosslinking type, a crosslinking agent may or may not be used. The step of applying energy is not particularly limited, and may be, for example, a heating step (thermal crosslinking).
[0053] In the heating step, the dispersion medium in the molded foamed emulsion composition is evaporated. The drying method is not particularly limited, and for example, hot air drying may be used. The drying temperature and drying time are also not particularly limited, and for example, the drying temperature and drying time may be about 80°C for about 1 to 3 minutes.
[0054] In this heating step, the dispersion medium evaporates from the foamed emulsion composition. The path through which the steam escapes is connected from the inside to the outside of the foamed sheet. Therefore, the path through which the steam escapes remains as open cells, so that at least a part of the bubbles present in the foamed sheet becomes open cells. Here, if the foaming gas mixed in the stirring and foaming step remains as it is, the bubbles in the obtained foamed sheet become closed cells, and if the mixed foaming gas is connected when the steam escapes in this step, the bubbles in the obtained foamed sheet become open cells. That is, in this case, the foamed sheet has a structure in which some of the bubbles in the foamed sheet are open cells and the remaining bubbles are closed cells, and thus has a semi-open cell structure in which open cells and closed cells are mixed.
[0055] When a crosslinking agent is added, the crosslinking (curing) reaction of the raw materials proceeds and is completed in the heating step. Specifically, the raw materials are crosslinked with each other by the above-mentioned crosslinking agent, and a hardened foamed sheet is formed. The heating means at this time is not particularly limited, and for example, a tunnel-type heating furnace or the like can be used. The heating temperature and heating time may be any temperature and time that can crosslink (cur) the raw materials, and may be, for example, 80 to 150°C (particularly, about 120°C is preferable) for about 1 to 3 minutes.
[0056] 2-1-4.Characteristics 2-1-4-1. Apparent density The apparent density of the foamed sheet according to the present embodiment is preferably 100 kg / m 3 More than 900kg / m 3 The apparent density can be measured in accordance with JIS K7222. The lower limit of the apparent density is, for example, 200 kg / m 3 , 300kg / m 3 , 400kg / m 3 , 500kg / m 3 , 550kg / m 3 , 600kg / m 3 and the upper limit of the apparent density is, for example, 900 kg / m 3 , 875kg / m 3 , 850kg / m3 , 825kg / m 3 , 800kg / m 3 It is.
[0057] 2-1-4-2.25% compressive stress (CLD) The 25% compressive stress of the foamed sheet according to the present embodiment is preferably 0.01 MPa or more, more preferably 0.05 MPa or more, even more preferably 0.075 MPa or more, and particularly preferably 0.1 MPa or more. The upper limit of the 25% compressive stress is not particularly limited, and is, for example, 0.5 MPa, 0.75 MPa, or 1 MPa. Here, the 25% compressive stress at 25°C is a value measured by the method described in JIS K6254-2:2016 "Vulcanized rubber and thermoplastic rubber - Determination of stress-strain characteristics".
[0058] 2-1-4-3.Point impact absorption rate The point impact absorption rate of the foamed sheet according to the present embodiment is preferably 5% or more, more preferably 7.5% or more, even more preferably 10% or more, and particularly preferably 20% or more. The upper limit is not particularly limited, and is, for example, 40%, 50%, or 60%. Here, the value of the point impact absorption rate in this specification is a value measured using a drop type impact absorption tester shown in FIG. 1. Specifically, a foamed sheet 11 processed to a size of φ50 mm is placed on a sample stage, and an impactor (steel ball) 10 weighing 32 g is dropped from a height of 10 cm in an environment of an air temperature of 23° C. The point impact absorption rate is calculated based on Equation 1. Point impact absorption rate (%) = {(fa0-fa1) / fa0} x 100 (Equation 1)
[0059] In the formula 1, fa0 is the impact load when the impact absorption test is performed without placing the sample on the sample stage, and fa1 is the impact load when the impact absorption test is performed with the sample placed on the sample stage. The impact load is measured by a sensor placed on the sample stage.
[0060] 2-1-4-4.Tensile strength The tensile strength of the foamed sheet according to the present embodiment is preferably 1.0 MPa or more, more preferably 1.25 MPa or more, even more preferably 1.35 MPa or more, and most preferably 1.5 MPa or more. The upper limit of the tensile strength is not particularly limited, and is, for example, 10 MPa, 5 MPa, or 2.5 MPa. Here, the tensile strength of the foamed sheet in this specification is a value measured in accordance with JIS K6251:2010 "Vulcanized rubber and thermoplastic rubber - Determination of tensile properties".
[0061] 2-1-4-5.Tape peel strength The tape peel strength (85°C) of the foamed sheet according to the present embodiment against the adhesive tape at an ambient temperature of 85°C is preferably 3.0N / 25mm or more, 3.5N / 25mm or more, 4.5N / 25mm or more, 5.0N / 25mm or more, 5.5N / 25mm or more, 6.0N / 25mm or more, 6.5N / 25mm or more, or 7.0N / 25mm or more. The lower limit of the tape peel strength is not particularly limited, and is, for example, 50.0N / 25mm, 30.0N / 25mm, 20.0N / 25mm, or 10.0N / 25mm. Here, the tape peel strength in this specification refers to a value measured by the method described in the examples.
[0062] Furthermore, the ratio of the tape peel strength (85°C) after 14 days of curing at 50°C to the tape peel strength (85°C) before curing at 50°C of the foamed sheet according to the present embodiment is preferably 0.5 or more, 0.55 or more, 0.6 or more, 0.65 or more, 0.7 or more, 0.75 or more, 0.8 or more, 0.85 or more, or 0.9 or more. The lower limit of the ratio is not particularly limited and is, for example, 1.
[0063] 2-1-4-6. Elution residual solidified matter The foamed sheet according to the present embodiment preferably has an eluted residual solidified matter of 15 mg or less, more preferably 12.5 mg or less, 10 mg or less, 9.5 mg or less, 9 mg or less, 8.5 mg or less, 8 mg or less, 7.5 mg or less, 7 mg or less, 6.5 mg or less, 6 mg or less, 5.5 mg or less, or 5 mg or less. The lower limit is not particularly limited, and is, for example, 0 mg. Here, the value of the eluted residual solidified matter is a value measured under the following elution conditions. It is presumed that the bleeding of the non-reactive emulsifier of the emulsion produced by the forced emulsification method and the surfactant added as a foaming agent onto the foam surface is the cause of the decrease in adhesion to the tape (tape peel strength). It is understood that the reason why the short-term and long-term adhesion to the tape is excellent when the eluted residual solidified matter is small is that the bleeding is reduced.
[0064] (Elution conditions) 5 g of the foam sheet is added to 500 ml of water and boiled for 30 minutes. After boiling, filtration is performed, 200 g of the filtrate is dried, and the mass after drying is measured, and the measured value is the value of the eluted residual solidified matter. Here, the filtration is performed, for example, using filter paper.
[0065] 2-2. Base material The material of the substrate is not particularly limited, and a known substrate can be used. For example, a resin film or paper can be used. The thickness of the substrate can be selected according to the application, design requirements, etc., and can be, for example, 10 μm or more and 100 μm or less.
[0066] Here, a release agent layer may be provided on the surface of the substrate. The material of the release agent layer may be a known material, such as dimethylsiloxane.
[0067] 2-3. Adhesive layer The material of the adhesive layer is not particularly limited, and any known adhesive can be used, for example, an acrylic adhesive, a urethane adhesive, a silicone adhesive, a rubber adhesive, etc. can be selected according to the type of adherend, the application, the design requirements, etc.
[0068] The thickness of the adhesive layer is not particularly limited and can be, for example, from 1 μm to 100 μm, and can be selected according to the type of adhesive, the application, design requirements, and the like.
[0069] The pressure-sensitive adhesive layer may be in the form of a uniform film, or may have a structure such as a film having grooves or through holes, a dot shape, a fiber shape, or a lattice shape.
[0070] 2-4.Release liner When the foamed sheet according to the present embodiment is provided with the pressure-sensitive adhesive layer, a release liner that protects the pressure-sensitive adhesive layer until use may be further provided on the surface of the pressure-sensitive adhesive layer. The material of the release liner and the release agent applied to the surface are not particularly limited and can be selected from known materials. For example, the material may be a resin film or paper, and the release agent may be dimethylsiloxane.
[0071] Here, the thickness of the release liner is not particularly limited and can be, for example, 10 μm or more and 100 μm or less.
[0072] 3. Uses and usage of foam sheets The foamed sheet according to the present embodiment has extremely high impact absorbing performance and is therefore useful as an impact absorbing sheet for protecting electronic / electrical devices or parts thereof (for example, an organic EL display panel). EXAMPLES
[0073] Next, the present invention will be described in more detail with reference to examples. However, the present invention is not limited to these examples. In addition, unless otherwise specified, "%" representing the content means mass%.
[0074] [Raw materials] Acrylic emulsion 1: Acrylic copolymer {butyl acrylate-styrene-2-ethylhexyl acrylate, pH 8.4, solids content 55%, reactive emulsifier (ethylenically unsaturated double bond-containing compound) used} Acrylic emulsion 2: Acrylic copolymer {Ethyl acrylate-methyl methacrylate-butyl acrylate, pH 7.2, solids content 57%, reactive emulsifier with ethylenically unsaturated double bonds (compound containing ethylenically unsaturated double bonds)} Acrylic Emulsion 3: Acrylic copolymer (butyl acrylate-styrene-2-ethylhexyl acrylate, pH 8.6, solids 55%, non-reactive emulsifier) Anionic surfactant: Ammonium stearate, solids content 30% Nonionic surfactant: Myristyl dimethylaminoacetate, solid content 30% Crosslinker: Hydrophobic HDI isocyanurate (functional group number 3.5) Solid content 100% ·Thickener: Water-soluble polyurethane (product name: VISCOLAM PS202) solid content 20% The composition and physical properties of the acrylic emulsion are summarized in Table 1.
[0075] [Table 1]
[0076] [Preparation example of foam raw material] The foam raw material of Example 1 was prepared by mixing 4.5 parts by mass of anionic foaming agent 1 (anionic surfactant), 0.5 parts by mass of amphoteric surfactant 1, 1.0 part by mass of thickener, and 2 parts by mass of crosslinking agent with 100 parts by mass of acrylic emulsion 1. The foam raw materials of Examples 2 to 6 and Comparative Example 1 were prepared in the same manner as the foam raw material of Example 1, except that the raw materials were blended in the components and ratios shown in Table 2.
[0077] [Sheet formation] An inert gas such as air or nitrogen gas was added to the foam raw material of each Example and Comparative Example, and the foam was foamed by a mechanical froth method (foaming conditions: 100 to 1000 rpm), cast onto a PET release liner, and then heat-treated (in an oven or drying furnace) to obtain a foam sheet of each Example and Comparative Example.
[0078] [Evaluation test] Next, the measurements and evaluations of Examples 1 to 6 and Comparative Example 1 are shown in Table 2.
[0079] Thickness The thickness was measured by a thickness gauge.
[0080] ·density It was measured by calculating the weight per unit volume.
[0081] 25% compressive stress (CLD) at 25℃ The 25% compressive stress at 25℃ is based on JIS K6254-2:2016 "Vulcanized rubber and The stress-strain characteristic of the thermoplastic rubber was evaluated according to the following criteria: ○: 25% compressive stress at 25℃ is more than 0.020MPa △: 25% compressive stress at 25℃ is 0.015MPa or more and 0.020MPa or less ×: 25% compressive stress at 25°C is less than 0.015 MPa
[0082] Tape peel strength (Example of test piece creation) The method for measuring the tape peel strength will be described with reference to FIG. 1. Cut out the tape material {adhesive component: acrylic adhesive (methyl methacrylate / butyl acrylate / 2-ethylhexyl acrylate) = 2 / 72 / 26 (monomer molar ratio); base material: polyimide / 7 x 8 cm; total thickness: 55 μm)} and attach a lead PET to the edge 1 cm. 2. Apply the tape to side A of the test sample (the side not facing the PET release liner) 3. Peel off the PET release liner from the test sample and apply tape to side B (the side with the PET release liner). 4. Cut the sample into pieces 25 mm wide and create 3 samples. 5. Lamination: 2kg roller x 3 times, leave for 24 hours after tape application (Test Method) 1. Leave the test piece at 85℃ (measurement temperature) for 10 minutes 2. Peel speed: evaluated at 300mm / min (180° peel) (Evaluation Criteria) ◎: More than 8N / 25mm 〇: More than 6N / 25mm and less than 8N / 25mm △: 4N / 25mm or more, 6N / 25mm or less ×: Less than 4N / 25mm
[0083] Tensile strength The tensile strength of the foamed sheets of each Example and Comparative Example was measured in accordance with JIS K6251:2010 "Vulcanized and thermoplastic rubber - Determination of tensile properties." Specifically, the foamed sheets of each Example and Comparative Example were punched into dumbbell-shaped No. 3 test pieces, and tensile tests were performed using an Instron material testing machine (Shimadzu Corporation, Autograph) at a crosshead speed of 200 mm / min. 〇:More than 1.5MPa △: 1.0MPa or more and 1.5MPa or less ×: Less than 1.0MPa
[0084] Point impact absorption rate The point impact absorption rate was calculated by the following formula 1 for the measurement results under each measurement condition, using a drop type impact absorption tester (Fig. 3). In the figure, 11 is a test sample, 12 is a sample stage (SUS), and 13 is a sensor. The measurement was performed by placing a foamed sheet (0.10 mm) of each Example and Comparative Example processed to a size of φ50 mm on the sample stage, and then dropping an impactor (steel ball) weighing 32 g from a height of 10 cm in an environment with an air temperature of 23°C. The point impact absorption rate was calculated based on formula 1. Point impact absorption rate (%) = {(fa0-fa1) / fa0} x 100 (Equation 1) In formula 1, fa0 is the impact load when the impact absorption test was performed without placing the sample on the sample stage, and fa1 is the impact load when the impact absorption test was performed with the sample placed on the sample stage. The impact load was measured by a sensor {Toyo Corporation product name: PCB sensor (Model: 482A21)} placed on the sample stage. The point impact absorption rate was evaluated according to the following criteria. ○: Point impact absorption rate is over 10% △: Point impact absorption rate is 5% to 10% ×: Point impact absorption rate is less than 5%
[0085] ·Elution residual solidified matter 5 g of the foamed sheet (sample) according to the examples and comparative examples was added to 500 ml of water and boiled for 30 minutes. After boiling, filtration was performed using filter paper, 200 g of the filtrate was dried, and the mass after drying was measured. The filter paper used here was ADVANTEC (registered trademark) No. 2 {JIS P 3801: Type 2 / mass (g / m 2 ):125 / Thickness(mm):0.26 / Drainage time(s):80 / Water absorption(cm):8 / Burst strength(kPa):122 / Wet burst strength(kPa):8 / Particle size retention(μm):5 / Ash content(%):0.1 / Maximum operating temperature(℃):120 / pH range:0~12 / Size(mm):φ125 / Complies with RoHS2(EU)2015 / 863}. ◎: Less than 5 mg 〇: 5mg or more but less than 8mg △: 8mg to 15mg ×: More than 15 mg
[0086] ·Moldability ○: 0 defects / m 2 △: 1 cosmetic defect / m 2 ×: 2 or more defects in appearance / m 2
[0087] Overall Judgment Criteria ◎:×0 pieces, △0 pieces, ◎3 or more pieces 〇:×0 pieces, △0 pieces, ◎0-2 pieces △:×0 pieces, △1 or more pieces ×:×1 or more
[0088] The results are shown in Table 2.
[0089] [Table 2]
Claims
1. A foamed sheet obtained by foaming and curing an acrylic emulsion composition, the foamed sheet having an eluted residual solidified matter of 15 mg or less under the following elution conditions: (Elution conditions) 5 g of the foam sheet was added to 500 ml of water and boiled for 30 minutes, then filtered, 200 g of the filtrate was dried, and the mass after drying was measured.
2. 2. The foam sheet according to claim 1, which has a tape peel strength (85°C) from an adhesive tape at an atmospheric temperature of 85°C of 5.0 N / 25 mm or more.
3. 2. The foamed sheet according to claim 1, wherein the acrylic emulsion composition is an acrylic emulsion composition obtained by emulsion polymerization of an acrylic monomer composition containing an acrylic monomer and a reactive emulsifier.
4. 2. The foamed sheet according to claim 1, wherein the emulsion composition contains 5% by mass or less of an anionic surfactant based on the mass (solid content) of the acrylic emulsion composition.
5. An electronic or electric device or a part thereof, comprising the foamed sheet according to any one of claims 1 to 4.
Citation Information