Sintering bonding sheet
The sintered bonding sheet with controlled adhesive load values addresses the insufficient transferability and fixation issues in semiconductor manufacturing, ensuring reliable bonding through a sintered bonding layer with conductive metal and organic binder.
Patent Information
- Application Number
- JP2024019696
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-06
- Filing Date
- 2024-02-13
- Publication Date
- 2024-10-18
AI Technical Summary
Existing semiconductor device manufacturing methods fail to achieve sufficient transferability and temporary fixation of a sintered bonding layer to semiconductor elements and their mounting areas on a substrate, lacking comprehensive studies in these critical characteristics.
A sintered bonding sheet with a sintered bonding layer containing conductive metal particles and an organic binder, where the minimum load values for the adhesive surfaces are set within specific ranges (-100μN to -35μN) to ensure both transferability and temporary fixation, utilizing nanoindentation methods for precise adhesion control.
The sintered bonding sheet achieves both sufficient transferability and temporary fixation of semiconductor elements to their mounting areas, enhancing the reliability and efficiency of semiconductor device assembly.
Smart Images

Figure 2024149387000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a sheet for sinter bonding. More specifically, the present invention relates to a sheet for sinter bonding having a sinter bonding layer for bonding a semiconductor element by sintering onto a substrate having a mounting area for the semiconductor element. [Background technology]
[0002] 2. Description of the Related Art Conventionally, in the manufacture of semiconductor devices, it is known to attach a semiconductor element to a substrate having a mounting area for the semiconductor element by using a sintered bonding layer (for example, see Patent Document 1 below). Moreover, Patent Document 1 below describes that the sintered bonding layer is configured as a layer containing sinterable particles and an organic binder.
[0003] The above-described semiconductor device is manufactured, for example, in the following procedure. (1) A dicing tape has a substrate and an adhesive layer laminated on the substrate. A semiconductor wafer is attached to the adhesive layer of the dicing tape. The semiconductor wafer attached to the adhesive layer is then diced into individual semiconductor elements. (2) After picking up a semiconductor element from the adhesive layer of the dicing tape using a tool such as a collet, the semiconductor element is pressed against a sintering bonding layer provided on a sintering bonding sheet to divide a portion of the sintering bonding layer into a size corresponding to the size of the semiconductor element. Then, the divided sintered bonding layer as described above is adhered to the one semiconductor element by an organic binder present on the contact surface side with the one semiconductor element, thereby transferring the divided sintered bonding layer to the one semiconductor element. (3) The semiconductor element to which the divided sintered bonding layer has been transferred is adhered to a mounting area of a semiconductor element on a substrate having mounting areas for a plurality of semiconductor elements by an organic binder present on the side opposite to the contact surface with the semiconductor element. That is, the one semiconductor element is temporarily fixed to the one semiconductor element mounting region of the substrate by the organic binder. (4) By carrying out the above steps (2) and (3) multiple times, each of the multiple semiconductor elements is temporarily fixed to each of the mounting areas of the multiple semiconductor elements on the substrate by each of the divided sintered bonding layers, thereby obtaining an intermediate semiconductor device product. (5) The intermediate product of the semiconductor device is heated at a temperature at which the sinterable particles in the sintered bonding layer can be sintered together, thereby sintering the sinterable particles in the sintered bonding layer and causing at least a portion of the organic binder to disappear from the sintered bonding layer, thereby bonding each of the multiple semiconductor elements to each mounting area of the semiconductor element on the substrate. After this process, each of the plurality of semiconductor elements is fixed to each of the mounting areas of the plurality of semiconductor elements on the substrate by sintering of the sinterable particles contained in the divided plurality of sintered bonding layers. That is, the plurality of semiconductor elements are fixed to the respective mounting regions of the substrate by a sintered body formed by sintering the sinterable particles together. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2020-150188 A Summary of the Invention [Problem to be solved by the invention]
[0005] In the manufacture of the semiconductor device as described above, it is preferable that the sintered bonding layer divided in the above steps (2) and (4) is transferred to the semiconductor element in a state of being sufficiently in close contact with the semiconductor element. Furthermore, in the manufacture of the above-described semiconductor device, in steps (3) and (4), it is preferable that the semiconductor element is temporarily fixed in a state in which it is sufficiently adhered to the mounting area of the semiconductor element on the substrate by the sintered bonding layer. In other words, in the manufacture of the above-described semiconductor device, it is preferable to simultaneously achieve sufficient transferability of the sintered bonding layer to the semiconductor element and sufficient temporary fixation of the semiconductor element to the mounting area of the semiconductor element on the substrate via the sintered bonding layer. However, in the manufacture of such semiconductor devices, it cannot be said that sufficient consideration has been given to achieving both of the above-mentioned two characteristics.
[0006] Therefore, an object of the present invention is to provide a sheet for sintering bonding that can achieve both sufficient transferability of a sintering bonding layer to a semiconductor element and sufficient temporary fixation of the semiconductor element to the mounting area of the semiconductor element on a substrate via the sintering bonding layer. [Means for solving the problem]
[0007] As a result of intensive research, the inventors have found that by providing a sheet for sintering bonding having a sintering bonding layer containing sinterable particles containing a conductive metal and an organic binder, and having the sintering bonding layer having a first adhesive surface adhered to one adherend and a second adhesive surface adhered to another adherend, and by setting the value of the minimum load reached during the unloading process in a load-displacement measurement by nanoindentation method for the first adhesive surface to b1 and the value of the minimum load reached during the unloading process in a load-displacement measurement by nanoindentation method for the second adhesive surface to b2, by making the values of b1 and b2 fall within a predetermined numerical range, it is possible to achieve both sufficient transferability of the sintering bonding layer to the semiconductor element and sufficient temporary fixation of the semiconductor element to the mounting area of the semiconductor element on the substrate via the sintering bonding layer. As a result, the present invention was achieved.
[0008] That is, the sinter-bonding sheet according to the present invention is A sintered bonding layer including sinterable particles containing a conductive metal and an organic binder, The sintered bonding layer has a first adhesive surface that is bonded to one adherend and a second adhesive surface that is bonded to another adherend, When the value of the minimum load reached during the unloading process in the load-displacement measurement by the nanoindentation method for the first adhesive surface is b1, and the value of the minimum load reached during the unloading process in the load-displacement measurement by the nanoindentation method for the second adhesive surface is b2, The b1 satisfies -100 μN≦b1≦-35 μN, The b2 satisfies -100 μN≦b2≦-35 μN. Effect of the Invention
[0009] According to the present invention, it is possible to provide a sheet for sintering bonding that can achieve both sufficient transferability of a sintering bonding layer to a semiconductor element and sufficient temporary fixation of the semiconductor element to the mounting area of the semiconductor element on a substrate via the sintering bonding layer. [Brief description of the drawings]
[0010] [Figure 1] 1 is a cross-sectional view showing a configuration of a sheet for sinter bonding according to an embodiment of the present invention. [Diagram 2] FIG. 4 is a cross-sectional view showing a configuration of a sheet for sinter bonding according to another embodiment of the present invention. [Figure 3A] 11 is a schematic cross-sectional view showing how the first semiconductor chip is lifted up from the dicing tape by a collet. [Figure 3B] 11 is a schematic cross-sectional view showing how the second semiconductor chip is lifted up from the dicing tape by the collet. FIG. [Figure 4A] 4 is a schematic cross-sectional view showing a state in which a part of a sintering bonding layer of the sintering bonding sheet according to the embodiment is transferred to a first semiconductor chip. FIG. [Figure 4B] 4 is a schematic cross-sectional view showing a state in which a part of the sintered bonding layer of the sheet for sinter bonding according to the embodiment is transferred to a second semiconductor chip. FIG. [Figure 5A] 11 is a schematic cross-sectional view showing how the first semiconductor chip with the divided pieces of the sintered bonding layer is lifted up by a collet. FIG. [Figure 5B] 13 is a schematic cross-sectional view showing how a second semiconductor chip with a divided body of the sintered bonding layer is lifted up by a collet. FIG. [Figure 6A] 4 is a schematic cross-sectional view showing a state in which a first semiconductor chip with a divided body of a sintered bonding layer is temporarily fixed to a first die pad of a lead frame substrate. FIG. [Figure 6B] 13 is a schematic cross-sectional view showing a state in which a second semiconductor chip with a divided body of the sintered bonding layer is temporarily fixed to a second die pad of a lead frame substrate. FIG. [Figure 7A] FIG. 11 is a schematic cross-sectional view showing an example of heating a lead frame substrate in which a first semiconductor chip is temporarily fixed to a first die pad and a second semiconductor chip is temporarily fixed to a second die pad via a divided body of a sintered bonding layer. [Figure 7B] FIG. 11 is a schematic cross-sectional view showing another example of heating a lead frame substrate in which a first semiconductor chip is temporarily fixed to a first die pad and a second semiconductor chip is temporarily fixed to a second die pad via a divided body of a sintered bonding layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, one embodiment of the present invention will be described. Note that, hereinafter, one embodiment of the present invention may be simply referred to as the present embodiment.
[0012] [Sintering bonding sheet] As shown in FIG. 1, a sintering bonding sheet 10 according to this embodiment has a sintering bonding layer 2 containing sinterable particles containing a conductive metal and an organic binder. In the example shown in FIG. 1, the sintered bonding layer 2 is laminated on the base layer 1. Moreover, the sheet 10 for sintering bonding according to this embodiment has, for example, a long strip shape, and is stored in a cylindrically wound state. In the sintering bonding sheet 10 according to this embodiment, the sintering bonding layer 2 has a first adhesive surface 2a that is bonded to one adherend, and a second adhesive surface 2b that is bonded to another adherend. In the sintering bonding sheet 10 of this embodiment, when the value of the minimum load reached during the unloading process in the load-displacement measurement by nanoindentation method for the first adhesive surface 2a is b1 and the value of the minimum load reached during the unloading process in the load-displacement measurement by nanoindentation method for the second adhesive surface 2b is b2, the b1 satisfies -100 μN≦b1≦-35 μN, and the b2 satisfies -100 μN≦b2≦-35 μN. In this specification, the term "conductive metal" refers to a metal having an electrical conductivity of 100 μS / cm or less as measured in accordance with JIS K 0130 (2008).
[0013] The sintering bonding layer 2 of the sintering bonding sheet 10 is temporarily fixed to a substrate or transferred to a semiconductor chip by the organic binder contained in the sintering bonding layer 2. That is, when the sintered bonding layer 2 is temporarily fixed to the substrate or transferred to the semiconductor chip, the organic binder remains in the sintered bonding layer 2. On the other hand, the sintered bonding layer 2 serves to bond the semiconductor chip to the substrate by sintering the sinterable particles contained in the sintered bonding layer 2 to each other. That is, in the state where the semiconductor chip is bonded to the substrate, at least a part of the organic binder in the sintered bonding layer 2 disappears. Furthermore, from the viewpoint of bonding the semiconductor chip to the substrate by sintering the sinterable particles together as described above, it is preferable that the amount of the organic binder remaining in the sintered bonding layer 2 be as small as possible. That is, it is preferable that almost no organic binder remains in the sintered bonding layer 2, and it is more preferable that no organic binder remains at all.
[0014] The minimum load value b1 reached during the unloading process in load-displacement measurement by nanoindentation method for the first adhesive surface 2a, and the minimum load value b2 reached during the unloading process in load-displacement measurement by nanoindentation method for the second adhesive surface 2b can be determined using a nanoindenter (for example, product name "Triboindenter", manufactured by Hysitron) as a measuring device. The load-displacement measurement by the nanoindentation method using the nanoindenter can be carried out under the following conditions. Indenter used: Berkovich (triangular pyramid) type diamond indenter (radius of curvature: 10nm to 100nm) Measurement mode: Single indentation measurement ·Measurement temperature: normal temperature (23±2℃) - Press depth setting: 2μm Maximum load reached during load application (set value): 500μN - Pressing speed of the indenter during load application: 100μN / sec Indenter withdrawal speed during unloading: 100μN / sec Measurement sample: sintered bonded layer 2 with a planar dimension of 10 mm square The load-displacement measurement by the nanoindentation method using the nanoindenter is performed by fixing the measurement sample onto a SUS plate (stainless steel plate) having a diameter of 15 mm, and then fixing the SUS plate with the measurement sample fixed thereto onto a stage provided in the nanoindenter. Furthermore, the SUS plate on which the measurement sample is fixed is fixed onto the stage by a magnet provided on the stage.
[0015] The smaller the minimum load value b1 of the first adhesive surface 2a and the minimum load value b2 of the second adhesive surface 2b, the higher the adhesiveness is indicated, and the larger the minimum load value b1 and the lower the adhesiveness is indicated. Therefore, if the minimum load value b1 and the minimum load value b2 are too small, the adhesion of the sintered bonding layer 2 to the adherend such as a semiconductor chip or substrate is improved, but the sintered bonding layer 2 may be separated from the base layer 1, for example, when peeling it off. Furthermore, if the minimum load value b1 and the minimum load value b2 are too large, the adhesiveness decreases, and it may become impossible to sufficiently bond the sintered bonding layer 2 to the adherend, such as a semiconductor chip or a substrate. In contrast, in the sintering bonding sheet 10 of this embodiment, the minimum load value b1 of the first adhesive surface 2a and the final load value b2 of the second adhesive surface 2b of the sintering bonding layer 2 are suitably adjusted, thereby achieving sufficient transferability to the semiconductor chip and sufficient temporary fixation to the substrate.
[0016] The minimum load value b1 of the first adhesive surface 2a and the minimum load value b2 of the second adhesive surface 2b can be adjusted by changing the content of the organic binder in the sintered bonding layer 2. In addition, the minimum load value b1 of the first adhesive surface 2a and the minimum load value b2 of the second adhesive surface 2b can also be adjusted by appropriately changing the degree of release treatment of the base material layer 1 to be laminated to the first adhesive surface 2a and the second adhesive surface 2b. For example, by performing a release treatment on the base layer 1 so as to increase the difference between the surface free energy of the sintered bonding layer 2 and the surface free energy of the base layer 1, the minimum load value b1 and the minimum load value b2 can be reduced. Furthermore, the minimum load value b1 and the minimum load value b2 can also be adjusted by roughening the surface of the base layer 1 by embossing or the like.
[0017] Examples of the conductive metal include gold, silver, copper, palladium, tin, and nickel. The conductive metal may be an alloy of two or more metals selected from the group consisting of gold, silver, copper, palladium, tin, and nickel. Additionally, the conductive metal may be a metal oxide, such as silver oxide, copper oxide, palladium oxide, and tin oxide. In the sintering bonding sheet 10 according to this embodiment, the sinterable particles preferably contain, as the conductive metal, at least one selected from the group consisting of silver, copper, silver oxide, and copper oxide. Since the sinterable particles contain at least one conductive metal selected from the group consisting of silver, copper, silver oxide, and copper oxide, the bonding strength of the divided sintered bonding layer 2 (division 2' of the sintered bonding layer) can be sufficiently enhanced when a semiconductor element is bonded to a mounting area of a substrate for the semiconductor element via the divided sintered bonding layer 2 (division 2' of the sintered bonding layer), as described below. In order for the sintered bonding layer 2 to have high electrical conductivity and high heat dissipation properties, the sinterable particles preferably contain silver or copper as the conductive metal. Furthermore, in consideration of oxidation resistance, it is preferable to use silver as the conductive particles. For example, when bonding a semiconductor element such as a semiconductor chip to a die pad of a lead frame substrate by sintering the sinterable particles together in a divided sintered bonding layer 2 (divided body 2' of the sintered bonding layer), if the conductive particles are copper, the bonding must be performed in an inert environment such as a nitrogen atmosphere, but if the conductive particles are silver, the bonding can be suitably performed even in an air atmosphere. In the sintering bonding sheet 10 according to the present embodiment, the sinterable particles may be particles having a core-shell structure having a core portion and a shell portion covering the core portion. The conductive metal constituting the core portion may contain copper as a main component, and the conductive metal constituting the shell portion may contain gold or silver as a main component.
[0018] Examples of the shape of the sinterable particles include flakes, needles, filaments, spheres, and flats (including scales). Among these, it is preferable to use spherical sinterable particles. By using spherical sinterable particles, the dispersibility of the sinterable particles can be improved in the varnish for obtaining the sintered bonding layer 2 described below.
[0019] The sinterable particles may be sinterable at a heating temperature of 400° C. or less. Sinterable at a heating temperature of 400° C. or less means that necking is observed between the outer surfaces of the particles when heated at a temperature of 400° C. or less. The sintering temperature of the sinterable particles can be measured using a thermogravimetric differential thermal analyzer. Specifically, measurements are performed under the following conditions using a thermogravimetric differential thermal analyzer (e.g., Rigaku's TG8120 differential thermal balance) to obtain a Tg curve and a DTA curve, and the sintering temperature of the sinterable particles can be obtained by determining the temperature of the largest peak in the DTA curve observed near the bottom of the Tg curve. <Measurement conditions> Heating rate: 10℃ / min Measurement atmosphere: Air Measurement temperature range: Room temperature (23±2℃) to 500℃
[0020] The sinterable particles containing the conductive metal such as gold, silver, copper, palladium, tin, nickel, and alloys thereof can be sintered by heating at a temperature of 400° C. or less.
[0021] The average particle size of the sinterable particles is preferably 1 nm or more, more preferably 10 nm or more, and even more preferably 50 nm or more. When the average particle size of the sinterable particles is equal to or greater than the above lower limit, the dispersibility of the sinterable particles in the varnish for obtaining the sintered bonding layer 2 described below can be increased. As a result, the sintered bonding layer 2 obtained has the sinterable particles suitably dispersed therein. The average particle size of the sinterable particles is preferably 10,000 nm or less, more preferably 3,000 nm or less, even more preferably 1,000 nm or less, and even more preferably 500 nm or less. When the average particle size of the sinterable particles is equal to or less than the upper limit, the surface of the sintered bonding layer 2 can be made relatively smooth. The average particle size of the sinterable particles can be determined by observing a cross section of the sintered bonding layer 2 using a scanning electron microscope (SEM). Specifically, it can be obtained according to the following procedure. (1) Prepare a sintered bonding layer 2 having planar dimensions of 10 mm×10 mm and a thickness of 50 μm (0.05 mm). (2) A sintered bonding layer 2 and a chip (planar dimensions 10 mm × 10 mm, thickness 0.2 mm) having a second electrode part are arranged in this order on a substrate (planar dimensions 10 mm × 10 mm, thickness 3 mm) having a first electrode part on one surface to obtain a laminate, and then the laminate is subjected to a sintering process to obtain a sintered bonded body. The sintering process is performed under the conditions of heating from 80°C to 300°C at a heating rate of 1.5°C / sec under a pressure of 10 MPa, and then holding at 300°C for 2.5 minutes. The sintered bonding layer 2 is disposed on the substrate so as to be in contact with the first electrode portion, and the chip is disposed so that the second electrode portion is in contact with the exposed surface of the sintered bonding layer 2. (3) The entire outer surface of the sintered bonded body is embedded in an embedding resin (for SEM), and then the outer surface of the embedded sintered bonded body is polished to be smooth. (4) Using a milling device, the sintered bonded body with the surfaces adjusted is cut in the thickness direction to obtain a sample for SEM observation. (5) The cut surface of the SEM observation sample is observed using an SEM to obtain an image of the cut surface, and the obtained image is then subjected to image analysis to determine the average particle size of the sinterable particles. The image is acquired at an accelerating voltage of 3 kV. The image analysis is performed using SEM images at a magnification of 10,000 or 100,000 depending on the size of the sinterable particles. The image analysis can be performed by binarizing the acquired image so that each of the sinterable particles included in the cut surface can be identified. Then, the circle-equivalent diameter of each of the sinterable particles included in the cut surface is calculated, and the calculated circle-equivalent diameters are arithmetically averaged to obtain the average particle size of the sinterable particles. Sinterable particles whose entire outer shape is not visible on the cut surface are excluded from the calculation of the circle-equivalent diameter. The circle-equivalent diameter is a diameter obtained by calculating the area of the sinterable particle on the cut surface and then converting it into the diameter of a perfect circle having an area equivalent to the calculated area.
[0022] When the conductive metal is silver, that is, when the sinterable particles are silver particles, the silver particles may be silver particles composed of silver element and other elements (metal elements, etc.) contained as unavoidable impurity elements, or may be silver particles that have been subjected to a surface treatment (for example, silane coupling treatment). Examples of the surface treatment agent for silver particles include fatty acid-based, amine-based, and epoxy-based coating agents. In the following, silver particles that have been surface-treated with a coating agent such as a fatty acid-based, amine-based, or epoxy-based coating agent may be referred to as coating agent-treated silver particles. By using coated silver particles as the sinterable particles, it is possible to increase the affinity between the organic binder and the sinterable particles in the sintered bonding layer 2 before at least a portion of the organic binder is lost by heat treatment during the manufacture of a semiconductor device, as described below. This makes it easier to disperse the sinterable metal particles in the sintered bonding layer 2 before at least a portion of the organic binder is lost. At least a part of the organic binder is removed from the sintered bonding layer 2 by heating the sintered bonding layer 2 to a predetermined temperature or higher, as will be explained in the manufacturing process of the semiconductor device described later.
[0023] In the sintering bonding sheet 10 according to the present embodiment, the content SC of the sinterable particles in the sintering bonding layer 2 is preferably 60% by mass or more, more preferably 65% by mass or more, even more preferably 70% by mass or more, and even more preferably 85% by mass or more. The content SC of the sinterable particles is preferably 99% by mass or less, more preferably 98% by mass or less, and even more preferably 97% by mass or less. When the content SC of the sinterable particles is within the above numerical range, the sinterable particles can be sintered together in the sintered bonding layer 2, and highly reliable bonding can be achieved when a semiconductor element such as a semiconductor chip is bonded to the die pad of a lead frame substrate.
[0024] The content SC of the sinterable particles in the sintered bonding layer 2 can be determined from the amount of ash remaining after the sintered bonding layer 2 is burned. The content SC of the sinterable particles can be measured, for example, by using a thermogravimetric analyzer (eg, TG209F1). The measurement using the thermogravimetric analyzer can be carried out, for example, according to the following procedure. (1) About 50 mg of the sintered bonding layer 2 is used as a measurement sample, and the temperature of the measurement sample is increased from room temperature (23±2° C.) to 650° C. (2) The organic binder in the sintered bonding layer 2 is thermally decomposed by holding the material at a temperature of 650° C. for 30 minutes. (3) Calculate the ratio of the mass of the remaining components (ash) to the mass of the measurement sample before heat treatment (approximately 50 mg). The measurement using the thermogravimetric analyzer may be carried out under an air flow or a nitrogen flow. Since copper particles are easily affected by oxidation at the temperatures used during the analysis as described above, when the sintered bonding layer 2 contains copper particles as the sinterable particles, it is preferable to carry out the measurement using the thermogravimetric analyzer under a nitrogen gas flow.
[0025] In the sintering bonding sheet 10 according to this embodiment, the sintering bonding layer 2 preferably contains, as the organic binder, a first organic binder and a second organic binder having a smaller molecular weight than the first organic binder.
[0026] The first organic binder is preferably a thermally decomposable polymer binder, which is thermally decomposed in a high-temperature heating process for forming a sintered bond by sintering sinterable particles together. The thermally decomposable polymer binder contributes to maintaining the sintered bonding layer 2 in a sheet shape before the high-temperature heating process. From the viewpoint of ensuring the function of maintaining the sintered bonding layer 2 in a sheet shape, the thermally decomposable polymer binder is preferably a material that is solid at room temperature (23±2° C.). Examples of such thermally decomposable polymer binders include polycarbonate resins and acrylic resins. That is, the sintered bonding layer 2 preferably contains at least one of the polycarbonate resin and the acrylic resin as the first organic binder. Moreover, the sintered bonding layer 2 may contain only the polycarbonate resin as the first organic binder.
[0027] Examples of the polycarbonate resin include aliphatic polycarbonates having aliphatic chains without containing aromatic compounds such as benzene rings between the carbonate esters (-OCOO-) in the main chain, and aromatic polycarbonates having the aromatic compounds between the carbonate esters (-OCOO-) in the main chain. Examples of the aliphatic polycarbonate include polyethylene carbonate and polypropylene carbonate. The aromatic polycarbonate may, for example, be a polycarbonate containing a bisphenol A structure in the main chain.
[0028] The acrylic resin may be, for example, at least one of a polymer of an acrylic acid ester and a polymer of a methacrylic acid ester having a linear or branched alkyl group having 4 to 18 carbon atoms. Hereinafter, "(meth)acrylic" refers to at least one of "acrylic" and "methacrylic", and "(meth)acrylate" refers to at least one of "acrylate" and "methacrylate". Examples of the alkyl group of the (meth)acrylic acid ester for constituting the acrylic resin as the thermally decomposable polymer binder include a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, a t-butyl group, an isobutyl group, an amyl group, an isoamyl group, a hexyl group, a heptyl group, a cyclohexyl group, a 2-ethylhexyl group, an octyl group, an isooctyl group, a nonyl group, an isononyl group, a decyl group, an isodecyl group, an undecyl group, a lauryl group, a tridecyl group, a tetradecyl group, a stearyl group, and an octadecyl group.
[0029] The acrylic resin may be a polymer containing a monomer unit derived from a monomer other than the above-mentioned (meth)acrylic acid ester. Examples of the other monomers include carboxy group-containing monomers, acid anhydride monomers, hydroxy group-containing monomers, sulfonic acid group-containing monomers, and phosphoric acid group-containing monomers. The carboxy group-containing monomer may be acrylic acid, methacrylic acid, carboxyethyl acrylate, carboxypentyl acrylate, itaconic acid, maleic acid, fumaric acid, or crotonic acid. The acid anhydride monomers include, for example, maleic anhydride or itaconic anhydride. Examples of the hydroxy group-containing monomer include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and 4-(hydroxymethyl)cyclohexylmethyl (meth)acrylate. Examples of the sulfonic acid group-containing monomer include styrenesulfonic acid, allylsulfonic acid, 2-(meth)acrylamide-2-methylpropanesulfonic acid, (meth)acrylamidepropanesulfonic acid, sulfopropyl(meth)acrylate, and (meth)acryloyloxynaphthalenesulfonic acid. The phosphate group-containing monomer may, for example, be 2-hydroxyethyl acryloyl phosphate.
[0030] The first organic binder preferably has a mass average molecular weight of 10,000 or more. The mass average molecular weight of the first organic binder is a value calculated by measuring using gel permeation chromatography (GPC) and converting the measured value into polystyrene equivalent value.
[0031] The second organic binder is preferably a low boiling point binder. The low boiling point binder is a binder component having a boiling point lower than the thermal decomposition starting temperature of the thermally decomposable polymer binder. In this embodiment, the low-boiling point binder has a viscosity of 1×10 at 23° C. measured using a dynamic viscoelasticity measuring device (trade name “HAAKE MARS III”, manufactured by Thermo Fisher Scientific). 5 A substance that has a viscosity of Pa·s or less and is in a liquid or semi-liquid state. In this viscosity measurement, parallel plates with a diameter of 20 mm were used as a jig, the gap between the plates was set to 100 μm, and the shear rate in the rotational shear was set to 1 s -1 Let us assume that.
[0032] Examples of the low boiling point binder include terpene alcohols, alcohols other than terpene alcohols, alkylene glycol alkyl ethers, and ethers other than alkylene glycol alkyl ethers. Examples of the terpene alcohols include isobornylcyclohexanol, citronellol, geraniol, nerol, carveol, and α-terpineol. Examples of the alcohols other than the terpene alcohols include pentanol, hexanol, heptanol, octanol, 1-decanol, ethylene glycol, diethylene glycol, propylene glycol, butylene glycol, and 2,4-diethyl-1,5-pentanediol. Examples of alkylene glycol alkyl ethers include ethylene glycol butyl ether, diethylene glycol methyl ether, diethylene glycol ethyl ether, diethylene glycol butyl ether, diethylene glycol isobutyl ether, diethylene glycol hexyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, diethylene glycol butyl methyl ether, diethylene glycol isopropyl methyl ether, triethylene glycol methyl ether, triethylene glycol dimethyl ether, triethylene glycol butyl methyl ether, propylene glycol propyl ether, dipropylene glycol methyl ether, dipropylene glycol ethyl methyl ether, dipropylene glycol propyl ether, dipropylene glycol butyl ether, and tripropylene glycol dimethyl ether. Examples of the ethers other than the alkylene glycol alkyl ethers include ethylene glycol ethyl ether acetate, ethylene glycol butyl ethyl acetate, diethylene glycol ethyl ether acetate, diethylene glycol butyl ethyl acetate, and dipropylene glycol methyl ether acetate. The low boiling point binder may be used alone or in combination of two or more kinds. As the low boiling point binder, it is preferable to use the terpene alcohols from the viewpoint of stability at room temperature. Among the terpene alcohols, it is preferable to use isobornylcyclohexanol.
[0033] The isobornylcyclohexanol is a compound represented by the following formula (1). The isobornylcyclohexanol is an organic compound with a boiling point of 308 to 318°C. When heated from room temperature (23±2°C) to 600°C under a nitrogen gas flow of 200mL / min at a temperature increase rate of 10°C / min, it has the property that it undergoes a large mass loss from 100°C or higher and volatilizes at 245°C (no further mass loss is observed). Furthermore, it has the property of exhibiting an extremely high viscosity of 1,000,000 mPa·s at 25°C, but a relatively low viscosity of 1,000 mPa·s or less at 60°C. The mass loss is a value when the mass loss rate at the measurement start temperature (room temperature) is set to 0%. In this way, isobornylcyclohexanol exhibits extremely high viscosity at 25°C as described above, and therefore can maintain the sheet shape at room temperature. On the other hand, it exhibits relatively low viscosity at 60°C as described above, and therefore has tackiness. That is, the sintering bonding sheet 10 having the sintering bonding layer 2 containing isobornylcyclohexanol has excellent sheet shape retention at room temperature, and has tackiness at temperatures of 60°C or higher. Incidentally, when mounting a semiconductor element attached to one surface of the sintered bonding layer 2 on a lead frame substrate or the like, the semiconductor element is usually temporarily attached (temporarily fixed) to an adherend such as a lead frame substrate via the sintered bonding layer 2 at a temperature of 60 to 80° C. Here, isobornylcyclohexanol becomes tacky at 60° C. or higher as described above. Therefore, in the sintering bonding sheet 10 according to the present embodiment, when the sintering bonding layer 2 contains isobornylcyclohexanol as the second organic binder, the sintering bonding layer 2 has improved temporary fixation to an adherend such as a lead frame substrate. That is, in the temporarily fixed state, the attachment position of the semiconductor element is prevented from shifting, and the sintering bonding layer 2 is prevented from lifting off the adherend.
[0034] [ka]
[0035] When the sintered bonding layer 2 contains, as the organic binder, the first organic binder and the second organic binder having a smaller molecular weight than the first organic binder, the content of the first organic binder is BC 1 % by mass, and the content of the second organic binder is BC 2 When expressed as mass%, the BC 1 and the aforementioned B.C. 2 is B.C. 1 :BC 2 It is preferable that the relationship of 0.5:9.5 is satisfied. Said B.C. 1 and the B.C. 2 is B.C. 1 :BC 2 It is more preferable that the relationship satisfies BC = 5:5 to 1:9. 1 :BC 2 It is more preferable that the relationship of 4:6 to 2:8 is satisfied.
[0036] The content BC of the first organic binder 1 is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, even more preferably 0.10% by mass or more, and even more preferably 0.20% by mass or more. Furthermore, the content BC of the first organic binder 1is preferably 20% by mass or less, more preferably 10% by mass or less, still more preferably 7.5% by mass or less, and even more preferably 5.0% by mass or less.
[0037] The content BC of the second organic binder 2 is preferably 0.5% by mass or more, more preferably 1.0% by mass or more, still more preferably 1.5% by mass or more, and even more preferably 2.0% by mass or more. Also, the content BC of the second organic binder 2 is preferably 20% by mass or less, more preferably 15% by mass or less, and still more preferably 10% by mass or less.
[0038] The value b1 of the minimum load for the first bonding surface 2a preferably satisfies -100 μN ≤ b1 ≤ -45 μN, more preferably satisfies -95 μN ≤ b1 ≤ -50 μN, and still more preferably satisfies -90 μN ≤ b1 ≤ -55 μN. The value b2 of the minimum load for the second bonding surface 2b preferably satisfies -90 μN < b2 ≤ -39 μN, and more preferably satisfies -85 μN ≤ b2 ≤ -45 μN.
[0039] It is preferable that b1 and b2 satisfy b1 ≤ b2. Also, b2 is preferably a value that is 1.00 times or more of b1, more preferably 1.05 times or more of b1, and still more preferably 1.10 times or more of b1. b2 is preferably a value that is 2.00 times or less of b1, more preferably 1.50 times or less of b1, and still more preferably 1.20 times or less of b1.
[0040] As shown in FIG. 2, the sintered joint layer 2 may include a first sintered joint layer 2A and a second sintered joint layer 2B laminated on the first sintered joint layer 2A. That is, the sintered joint layer 2 may be a laminate in which two or more sintered joint layers are laminated. When the sintered bonding layer 2 is a laminate as shown in FIG. 2, the first sintered bonding layer 2A and the second sintered bonding layer 2B have a first organic binder content BC 1 The content of the second organic binder B 2 It is preferable that the sinterable particles have different contents SC. The composition of the first sintered bonding layer 2A and the composition of the second sintered bonding layer 2B may be the same as each other. That is, the first sintered bonding layer 2A and the second sintered bonding layer 2B may have a first organic binder content B 1 The content of the second organic binder is the same, and the content of the second organic binder is 2 may be the same and the content SC of sinterable particles may be the same.
[0041] In the sheet 10 for sintering bonding according to this embodiment, the thickness of the sintering bonding layer 2 is preferably 5 μm or more, and more preferably 10 μm or more. In the sintering bonding sheet 10 according to this embodiment, the thickness of the sintering bonding layer 2 is preferably 300 μm or less, and more preferably 150 μm or less. The thickness of the sintered bonding layer 2 can be determined, for example, by measuring the thickness at five randomly selected locations using a dial gauge (manufactured by PEACOCK, model R-205) and calculating the arithmetic average of these thicknesses.
[0042] The sintered bonding layer 2 can be produced, for example, by preparing a varnish by dissolving or suspending the sinterable particles and the organic binder in an organic solvent, applying the varnish onto the base layer 1 to form a coating film of a predetermined thickness, and then drying the coating film. As the organic solvent for preparing the varnish, for example, alcohols such as ethanol, or ketones such as methyl ethyl ketone (MEK) can be used.
[0043] The substrate layer 1 functions as a support in the sinter-bonding sheet 10. The substrate layer 1 is made of, for example, a plastic substrate. As the plastic substrate, it is preferable to use a plastic film. Examples of the constituent material of the plastic substrate include polyolefin resin, polyester resin, polyurethane resin, polycarbonate resin, polyether ether ketone resin, polyimide resin, polyetherimide resin, polyamide resin, wholly aromatic polyamide resin, polyvinyl chloride resin, polyvinylidene chloride resin, polyphenyl sulfide resin, aramid resin, fluororesin, cellulose-based resin, and silicone resin. Examples of the polyolefin resin include low-density polyethylene resin, linear low-density polyethylene resin, medium-density polyethylene resin, high-density polyethylene resin, very low-density polyethylene resin, random copolymer polypropylene resin, block copolymer polypropylene resin, homopolypropylene resin, polybutene resin, polymethylpentene resin, ethylene-vinyl acetate copolymer resin, ionomer resin, ethylene-butene copolymer resin, and ethylene-hexene copolymer resin. Examples of the polyester resin include polyethylene terephthalate resin, polyethylene naphthalate resin, and polybutylene terephthalate resin. The base layer 1 may be composed of one type of constituent material, or may be composed of two or more types of constituent materials. The base layer 1 may have a single-layer structure, or may have a multi-layer structure. The term "single-layer structure" refers to a structure made of one type of constituent material. For example, a structure in which two or more layers made of one type of constituent material are laminated is classified as a single-layer structure. On the other hand, a multi-layer structure refers to a structure in which two or more layers made of different constituent materials are laminated. When the base layer 1 is made of a plastic film, the base layer 1 may be made of a non-stretched film or a stretched film. The stretched film may be a uniaxially stretched film or a biaxially stretched film. In addition, when manufacturing a semiconductor device using the sintering bonding sheet 10 as described below, the base layer 1 may function as a release sheet that can easily peel off the divided sintering bonding layer 2 (divided body 2' of the sintering bonding layer). When the base layer 1 functions as a release sheet, the surface of the base layer 1 that comes into contact with the sintered bonding layer 2 may be coated with a release agent.
[0044] The thickness of the base layer 1 is preferably 10 μm or more, more preferably 20 μm or more, and even more preferably 30 μm or more. The thickness of the base layer 1 is preferably 5000 μm or less, more preferably 4000 μm or less, and even more preferably 3000 μm or less. The thickness of the base layer 1 can be determined, for example, by measuring the thickness at five randomly selected locations using a dial gauge (manufactured by PEACOCK, model R-205) and calculating the arithmetic average of these thicknesses.
[0045] (Method of manufacturing a semiconductor device) Next, an example of a method for manufacturing a semiconductor device using the sheet for sinter bonding 10 according to this embodiment will be described with reference to FIGS. 3A to 7B.
[0046] The manufacturing method of the semiconductor device according to this embodiment is carried out using a substrate having a plurality of semiconductor chips and a plurality of mounting areas on which the plurality of semiconductor chips are mounted, a sintering bonding sheet 10 according to this embodiment, and a first pressing member that presses the semiconductor chips toward the substrate with a portion of the sintering bonding layer 2 of the sintering bonding sheet 10 interposed therebetween, thereby adhering the plurality of semiconductor chips to the plurality of mounting areas. In the method for manufacturing a semiconductor device according to this embodiment, the semiconductor chips are pressed in sequence by the first pressing member to be temporarily fixed to the mounting regions.
[0047] In the following, a case will be described in which the substrate is a lead frame substrate, the mounting area is a die pad, and the first pressing member is a collet.
[0048] First, a semiconductor wafer is cut on a dicing tape C to obtain a plurality of semiconductor chips (see FIG. 3A). Next, as shown in FIG. 3A, a collet A lifts up one semiconductor chip B1 (hereinafter also referred to as a first semiconductor chip B1) out of the plurality of semiconductor chips from a dicing tape C. Incidentally, the semiconductor chip is usually in the shape of a flat rectangular plate, more specifically, in the shape of a flat square plate. The thickness of the semiconductor chip is, for example, 10 μm or more and 500 μm or less, and preferably 20 μm or more and 400 μm or less. The area of a semiconductor chip in plan view is, for example, 0.01 mm 2 More than 1000mm 2 The area of a semiconductor chip in plan view is 0.04 mm 2 More than 500mm 2 It is preferable that: The planar dimensions of the collet A on the side that contacts the semiconductor chip correspond to the chip size. That is, the area S1 of the surface of the collet A that contacts the semiconductor chip in a planar view (hereinafter also referred to as the collet area S1) corresponds to the area S2 of the semiconductor chip in a planar view (hereinafter also referred to as the chip area S2). More specifically, the collet area S1 is 0.9 to 1.1 times the chip area S2.
[0049] Next, as shown in FIG. 4A, the sheet for sintering bonding 10 is placed on a stage G so that the sintering bonding layer 2 of the sheet for sintering bonding 10 faces upward. Then, the first semiconductor chip B1 is pressed against the sintered bonding layer 2 on the sintered bonding sheet 10 by the collet A, thereby transferring a part of the sintered bonding layer 2 to the first semiconductor chip B1. This results in the first semiconductor chip B1 having a divided sintered bonding layer 2 (hereinafter also referred to as a divided body 2' of the sintered bonding layer). The pressure with which the first semiconductor chip B1 is pressed against the sintered bonding layer 2 is preferably 0.01 MPa or more and 10 MPa or less, and more preferably 0.1 MPa or more and 5 MPa or less. Furthermore, the temperature of the collet A or the stage G when the first semiconductor chip B1 is pressed against the sintered bonding layer 2 is preferably 40°C or higher and 150°C or lower, and more preferably 50°C or higher and 130°C or lower. By setting the temperature of the collet A or the stage G within the above range, the divided body 2' of the sintered bonding layer can be suitably transferred to the first semiconductor chip B1.
[0050] Next, as shown in FIG. 5A, the first semiconductor chip B1 with the divided body 2' of the sintered bonding layer attached thereto is lifted up from the sheet 10 for sintering bonding with a collet A.
[0051] Next, as shown in FIG. 6A, the lead frame substrate D is placed on the stage H. While the collet A is held at any temperature within a range of 25° C. to 100° C., the collet A is lowered vertically downward to bring the divided body 2' of the sintered bonding layer of the first semiconductor chip B1 with the divided body 2' of the sintered bonding layer into contact with the first die pad E1 of the lead frame substrate D. Then, the first semiconductor chip B1 with the divided body 2' of the sintered bonding layer is pressed (pressed) by the collet A. More specifically, the first semiconductor chip B1 is pressed by the collet A to attach the divided body 2' of the sintered bonding layer to the first die pad E1 of the lead frame substrate D. As a result, the first semiconductor chip B1 is temporarily fixed to the first die pad E1 of the lead frame substrate D via the divided body 2' of the sintered bonding layer (see FIG. 6A). The pressure applied when pressing the first semiconductor chip B1 with the divided body 2' of the sintered bonding layer against the first die pad E1 of the lead frame substrate D from the divided body 2' side of the sintered bonding layer is preferably 0.01 MPa or more and 50 MPa or less, and more preferably 0.1 MPa or more and 30 MPa or less.
[0052] As described above, after the first semiconductor chip B1 is temporarily fixed to the first die pad E1 of the lead frame substrate D, another semiconductor chip B2 (hereinafter also referred to as the second semiconductor chip B2) among the multiple semiconductor chips is lifted from the dicing tape C by a collet A, as shown in FIG. 3B.
[0053] 4B, the second semiconductor chip B2 is pressed against the sintered bonding layer 2 of the sintered bonding sheet 10 by a collet A, thereby transferring a part of the sintered bonding layer 2 to the second semiconductor chip B2. This results in the second semiconductor chip B2 having a divided body 2' of the sintered bonding layer attached thereto.
[0054] Next, as shown in FIG. 5B, the second semiconductor chip B2 with the divided body 2' of the sintered bonding layer is lifted up from the sintering bonding sheet 10 by the collet A. Next, while holding the collet A at any temperature within the range of 25°C or higher and 150°C or lower, the second semiconductor chip B2 with the divided body 2' of the sintered bonding layer is abutted against another die pad E2 (second die pad E2) on the lead frame substrate D from the divided body 2' side of the sintered bonding layer. Then, the second semiconductor chip B2 having the divided body 2' of the sintered bonding layer attached thereto is pressed (pressed) by the collet A. As a result, the second semiconductor chip B2 is temporarily fixed to the second die pad E2 of the lead frame substrate D via the divided body 2' of the sintered bonding layer (see FIG. 6B). The above steps are repeated in sequence until semiconductor chips are temporarily fixed to all the die pads of the lead frame substrate D.
[0055] In addition, after temporarily fixing the first semiconductor chip B1 to the first die pad E1 of the lead frame substrate D, or after temporarily fixing the second semiconductor chip B2 to the second die pad E2 of the lead frame substrate D, the collet A may be heated to a temperature at which the sinterable particles (sinterable particles contained in the divided body 2' of the sintered bonding layer) can be sintered, thereby performing primary sintering of the sinterable particles to each other in the divided body 2' of the sintered bonding layer. In other words, if there are semiconductor chips other than the first semiconductor chip B1 and the second semiconductor chip B2 to be temporarily fixed to the die pad of the lead frame substrate D, the primary sintering may also be performed on the sinterable particles contained in each of the divided bodies 2' of the sintered bonding layer used to temporarily fix the other semiconductor chips to each die pad.
[0056] When the sinterable particles contained in the divided body 2' of the sintered bonding layer are sinterable particles that can be sintered at a heating temperature of 400°C or less, it is preferable to heat the collet A to a temperature of 200°C or more. By heating collet A to a temperature of 200°C or higher, the sinterable particles can be more thoroughly sintered together, so that each semiconductor chip can be more firmly attached to each die pad of lead frame substrate D with the divided bodies 2' of the sintered bonding layer interposed therebetween. That is, the connection reliability of a semiconductor chip such as the first semiconductor chip B1 or the second semiconductor chip B2 to a substrate such as the lead frame substrate D can be improved.
[0057] Furthermore, when the primary sintering is carried out, it is preferable that collet A is rapidly heated (in about 5 seconds) to a temperature at which the sinterable particles become sinterable. Collet A is preferably heated at 30° C. / sec or more, and more preferably heated at 45° C. / sec or more, to a temperature at which the sinterable particles become sinterable. The primary sintering may be performed by heating the collet A and also by heating the stage H to a temperature equal to or higher than the temperature at which the sinterable particles can be sintered. This allows heating from both sides of the divided body 2' of the sintered bonding layer, so that the sinterable particles can be sintered more thoroughly in the divided body 2' of the sintered bonding layer. As a result, the semiconductor chips can be attached more firmly to the die pads of the lead frame substrate D with the divided body 2' of the sintered bonding layer interposed therebetween. That is, the connection reliability of a semiconductor chip such as the first semiconductor chip B1 or the second semiconductor chip B2 to a substrate such as the lead frame substrate D can be further improved. The temperature to which the stage H is heated is preferably equal to or lower than the temperature that suppresses oxidation of the lead frame substrate D. For example, when the lead frame substrate D is made of a Cu alloy (Cu-Cr-Zr, Cu-Cr-Sn-Zn, Cu-Ni-Si-Mg, etc.), the temperature to which the stage H is heated is preferably equal to or lower than 150°C.
[0058] As described above, when primary sintering is performed on the divided body 2' of the sintered bonding layer, it is preferable to lower the temperature of collet A to a temperature (e.g., 50°C) at which the sinterable particles become difficult to sinter by lifting collet A and separating it from the semiconductor chip attached to the divided body 2' of the sintered bonding layer after the primary sintering is performed.
[0059] Furthermore, when semiconductor chips are attached to all the die pads of the lead frame substrate D, if the primary sintering is performed on each of the divided bodies 2' of the sintered bonding layer, bonding wires may be bonded to necessary locations.
[0060] In the manufacturing method of the semiconductor device of this embodiment, as described above, a portion of the sintered bonding layer 2 of the sintered bonding sheet 10 of this embodiment is transferred to an adherend such as a semiconductor chip, and the semiconductor chip is temporarily fixed to the die pad of the lead frame substrate via the portion of the sintered bonding layer 2. Furthermore, in the sintering bonding layer 2 of the sintering bonding sheet 10 of this embodiment, when the minimum load value reached during the unloading process in the load-displacement measurement by nanoindentation method for the first adhesive surface 2a is b1 and the minimum load value reached during the unloading process in the load-displacement measurement by nanoindentation method for the second adhesive surface 2b is b2, the b1 satisfies -100 μN≦b1≦-35 μN and the b2 satisfies -100 μN≦b2≦-35 μN. That is, both the first adhesive surface 2a and the second adhesive surface 2b have a suitable adhesiveness. Therefore, in the manufacturing method of a semiconductor device according to this embodiment, in addition to being able to achieve sufficient transferability of the sintered bonding layer 2 to the semiconductor chip, it is also possible to achieve sufficient temporary fixation of the semiconductor chip to the mounting area of the semiconductor chip, such as a die pad, via the sintered bonding layer 2.
[0061] In the manufacturing method of a semiconductor device according to this embodiment, after the multiple semiconductor chips are pressed in sequence to temporarily fix them to the multiple mounting areas, a heating process may be carried out in which the substrate to which the multiple semiconductor chips are attached is heated to a temperature at which the sinterable particles can be sintered. In the heating step, the heating may be performed by pressing only some or all of the plurality of semiconductor chips against the substrate. In the heating step, the heating may be performed without pressing any of the plurality of semiconductor chips against the substrate. In addition, as described above, in the case where heating (primary heating) is performed for primary sintering of the sinterable particles contained in the divided body 2' of the sintered bonding layer, the above heating process becomes a secondary heating process.
[0062] More specifically, after the semiconductor chips have been temporarily fixed to all of the die pads of the lead frame substrate D, as shown in FIG. 7A, without pressing any or all of the semiconductor chips attached to all of the die pads of the lead frame substrate D, the stage H may be heated (a heating process may be performed) to a temperature at which the sinterable particles contained in the divided body 2' of the sintered bonding layer can be sintered (for example, any temperature in the range of 200°C or higher and 400°C or lower). Note that Figure 7A shows an example in which heating is performed without pressing any of the semiconductor chips (first semiconductor chip B1 and second semiconductor chip B2) attached to all of the die pads (first die pad E1 and second die pad E2) of the lead frame substrate D. By carrying out such a heating step, the sinterable particles can be sintered together, so that the semiconductor chip can be firmly attached to the substrate (lead frame substrate D) with the divided body 2' of the sintered bonding layer interposed therebetween. This improves the connection reliability of the semiconductor chip to the substrate. Also, the equipment used in the heating step can be simple and does not include a pressing member. When such a heating step is performed, bonding wires may be bonded to required locations after the heating step.
[0063] On the other hand, in the manufacturing method of the semiconductor device according to this embodiment, in the heating process in which the sinterable particles are heated at a temperature at which they can be sintered, the heating may be carried out while pressing some or all of the multiple semiconductor chips against the substrate. In the method for manufacturing a semiconductor device according to the present embodiment, in the heating step, heating may be performed while pressing all of the plurality of semiconductor chips against the substrate.
[0064] More specifically, after the semiconductor chips are temporarily fixed to all the die pads of the lead frame substrate D, as shown in Fig. 7B, a heating and pressurizing device F is used that has two flat plates (parallel flat plates) arranged so as to sandwich from above and below some or all of the semiconductor chips attached to all the die pads of the lead frame substrate D. Then, using the heating and pressurizing device F, some or all of the semiconductor chips attached to all the die pads of the lead frame substrate D may be heated to a sinterable temperature while being pressurized (pressed). Note that Figure 7B shows an example in which all of the semiconductor chips (first semiconductor chip B1 and second semiconductor chip B2) attached to all of the die pads (first die pad E1 and second die pad E2) of the lead frame substrate D are heated while being pressed against each other. By carrying out such a heating step, it is possible to heat some or all of the semiconductor chips while pressing them against the substrate (lead frame substrate D), so that some or all of the semiconductor chips can be firmly attached to the substrate (lead frame substrate D) with the divided bodies 2' of the sintered bonding layer interposed therebetween. This improves the connection reliability of the semiconductor chips to the substrate. Even when such a heating step is performed, bonding wires may be bonded to required locations after the heating step.
[0065] Various known lead frame substrates can be used as the lead frame substrate D. Examples of the various known lead frame substrates include a lead frame substrate in which a Cu lead frame substrate is plated with Ag, or a lead frame substrate in which a Cu lead frame substrate is plated with Ni, Pd, and Au in this order (Palladium Pre Plated Lead Frame, Pd-PPF).
[0066] The matters disclosed in this specification include the following.
[0067] (1) The sintered bonding layer includes sinterable particles containing conductive particles and an organic binder, The sintered bonding layer has a first adhesive surface that is bonded to one adherend and a second adhesive surface that is bonded to another adherend, When the value of the minimum load reached during the unloading process in the load-displacement measurement by the nanoindentation method for the first adhesive surface is b1, and the value of the minimum load reached during the unloading process in the load-displacement measurement by the nanoindentation method for the second adhesive surface is b2, The b1 satisfies -100 μN≦b1≦-35 μN, A sheet for sintering joining, wherein b2 satisfies -100 μN≦b1≦-35 μN.
[0068] (2) The b1 satisfies -100 μN≦b1≦-45 μN, The said b2 satisfies -90 μN < b2 ≦ -39 μN, The sintering bonding sheet according to the above (1).
[0069] (3) The said b1 and the said b2 satisfy the relation of b1 ≦ b2, The sintering bonding sheet according to the above (1) or (2).
[0070] (4) The said organic binder includes a first organic binder and a second organic binder having a molecular weight smaller than that of the first organic binder, When the content rate of the first organic binder in the sintering bonding layer is BC 1 in mass %, and the content rate of the second organic binder is BC 2 in mass %, the said BC 1 and the said BC 2 are such that BC 1 : BC 2 = 6:4 to 0.5:9.5 is satisfied, The sintering bonding sheet according to any one of the above (1) to (3).
[0071] (5) The content rate SC of the sinterable particles in the sintering bonding layer is 85 mass % or more and 97 mass % or less, The sintering bonding sheet according to any one of the above (1) to (4).
[0072] (6) The sintering bonding layer includes a first sintering bonding layer and a second sintering bonding layer laminated on the first sintering bonding layer, The first sintering bonding layer includes the sinterable particles and at least one of a first organic binder or a second organic binder having a molecular weight smaller than that of the first organic binder as the organic binder, The second sintering bonding layer includes the sinterable particles and at least one of the first organic binder or the second organic binder as the organic binder, The first sintered bonding layer and the second sintered bonding layer have a first organic binder content BC 1 , the content of the second organic binder BC 2 At least one of the sinterable particle contents SC is different from each other; The sinter bonding sheet according to any one of (1) to (5) above.
[0073] (7) The sinterable particles contain, as the conductive metal, at least one selected from the group consisting of silver, copper, silver oxide, and copper oxide. The sinter bonding sheet according to any one of (1) to (6) above.
[0074] (8) A first release sheet is attached to the first adhesive surface, and a second release sheet is attached to the second adhesive surface. A sheet for sintering bonding according to any one of (1) to (7) above.
[0075] The sinter-bonding sheet according to the present invention is not limited to the above-described embodiment. Moreover, the sheet for sinter bonding according to the present invention is not limited to the above-mentioned functions and effects. Furthermore, the sheet for sinter bonding according to the present invention can be modified in various ways without departing from the gist of the present invention. EXAMPLES
[0076] The present invention will now be described in more detail with reference to examples. The following examples are provided to further explain the present invention in detail, and are not intended to limit the scope of the present invention.
[0077] [Example 1A] The first silver particles (average particle diameter 60 nm, manufactured by DOWA Electronics Co., Ltd.), the second silver particles (average particle diameter 1100 nm, manufactured by Mitsui Mining and Smelting Co., Ltd.), a polycarbonate resin (product name "QPAC40", manufactured by Empower Materials Corporation), and isobornylcyclohexanol (product name "Tersolve MTPH", manufactured by Nippon Terpene Chemical Industry Co., Ltd.) were dissolved and suspended in methyl ethyl ketone (MEK) in the blending ratio shown in Table 1 below, to prepare a first varnish. The above components were dissolved and suspended in methyl ethyl ketone by stirring and mixing for 3 minutes using a hybrid mixer (model "HM-500", manufactured by Keyence Corporation) in stirring mode. The first varnish was applied to the release-treated surface of a first release-treated film (product name "MRA38", manufactured by Mitsui Resin Co., Ltd.) to a thickness of 200 μm to form a coating layer, and the coating layer was heated at a temperature of 110° C. for 3 minutes to form a sintered bonding layer on the first release-treated film. This produced a first laminate sheet. Next, two of the first laminate sheets were laminated together to obtain a sheet for sinter bonding according to Example 1A. The exposed surfaces of the sintered bonding layers of the two first laminate sheets were placed against each other (hereinafter, the exposed surface after the varnish application when the sintered bonding layer was formed may be simply referred to as the exposed surface or the exposed surface after application). The first and second silver particles are classified as sinterable particles. The polycarbonate resin is classified as a first organic binder (thermally decomposable polymer binder). Isobornylcyclohexanol is classified as a second organic binder (low boiling point binder). In the following Table 1, the blending amount of the sinterable particles is shown as an ash content value, and the blending amounts of the first silver particles and the second silver particles are shown as amounts at the time of charging. The same applies to the following Tables 2 and 3.
[0078] [Example 2A] The first varnish was applied to the release-treated surface of a second release-treated film (product name "SRD38", manufactured by Toyobo Co., Ltd.) to a thickness of 200 μm to form a coating layer, and the coating layer was heated at a temperature of 110° C. for 3 minutes to form a sintered bonding layer on the second release-treated film. This produced a second laminate sheet. Next, two second laminate sheets were laminated together to obtain a sheet for sinter bonding according to Example 2A. The exposed surfaces of the two second laminate sheets were placed against each other.
[0079] [Example 3A] A sheet for sinter bonding according to Example 3A was obtained by overlapping one first laminate sheet and one second laminate sheet. The exposed surfaces of one first laminate sheet and one second laminate sheet were placed against each other.
[0080] [Example 4A] Three first laminate sheets were stacked together to obtain a sheet for sinter bonding according to Example 4A. The three second laminate sheets were laminated according to the following procedure. (1) Two first laminate sheets are laminated together with their exposed surfaces in contact with each other to obtain a laminate having a first release-treated film on both sides (top and bottom). (2) The first release-treated film is peeled off from one surface of the laminate to expose the one surface of the laminate. (3) The laminate and the remaining first laminate sheet are superimposed so that their exposed surfaces abut each other.
[0081] [Comparative Example 1A] Two first laminate sheets were overlapped to obtain a sheet for sinter bonding according to Comparative Example 1A. The two first laminate sheets were laminated according to the following procedure. (1) The first release-treated film is peeled off from one first laminate sheet to obtain an exposed surface (hereinafter referred to as a release-formed exposed surface). (2) The first laminate sheet is laminated so that the release-forming exposed surface of the first laminate sheet having the release-forming exposed surface abuts against the exposed surface of the remaining first laminate sheet.
[0082] [Comparative example 2A] Two second laminate sheets were overlapped to obtain a sheet for sinter bonding according to Comparative Example 2A. The two first laminate sheets were laminated according to the following procedure. (1) The first release-treated film is peeled off from each of the two first laminate sheets to obtain an exposed release surface. (2) Two first laminate sheets having release-forming exposed surfaces are stacked together so that the release-forming exposed surfaces abut against each other.
[0083] [Comparative example 3A] The first silver particles, the second silver particles, polycarbonate, and isobornylcyclohexanol were dissolved and suspended in methyl ethyl ketone (MEK) in the blending ratio shown in Table 1 below to prepare a second varnish. The above components were stirred and mixed in the same manner as described in Example 1, and dissolved and suspended in methyl ethyl ketone. The second varnish was applied to the release-treated surface of the first release-treated film to form a coating layer, and the coating layer was then heated at a temperature of 110° C. for 3 minutes to form a sintered bonding layer on the first release-treated film, thereby obtaining a third laminate sheet. In Comparative Example 3A, the third laminate sheet was used as a sheet for sinter bonding.
[0084] [Comparative example 4A] The third varnish was prepared by dissolving and suspending the first silver particles, the second silver particles, and isobornylcyclohexanol in methyl ethyl ketone (MEK) at the blending ratio shown in the following Table 1. In other words, the third varnish did not contain polycarbonate. The above components were dissolved and suspended in methyl ethyl ketone by stirring and mixing in the same manner as described in Example 1A. The third varnish was applied to the release-treated surface of the first release-treated film to form a coating layer, and the coating layer was heated at a temperature of 110° C. for 3 minutes to form a sintered bonding layer on the first release-treated film, thereby obtaining a fourth laminate sheet. Next, two of the fourth laminate sheets were overlapped to obtain a sheet for sinter bonding according to Comparative Example 4A. The two fourth laminate sheets were placed together with their exposed surfaces facing each other.
[0085] [Table 1]
[0086] [Example 1B] First, a first laminate sheet was obtained as described in Example 1A. Next, the first silver particles, the second silver particles, polycarbonate, and isobornylcyclohexanol were dissolved and suspended in methyl ethyl ketone in the blending ratio shown in Table 2 below to prepare a fourth varnish. The above components were dissolved and suspended in methyl ethyl ketone by stirring and mixing in the same manner as described in Example 1A. The fourth varnish was applied to the release-treated surface of the first release-treated film to form a coating layer, and the coating layer was heated at a temperature of 110° C. for 3 minutes to form a sintered bonding layer on the first release-treated film, thereby obtaining a fifth laminate sheet. Next, one first laminate sheet and one fifth laminate sheet were laminated together to obtain a sheet for sinter bonding according to Example 1B. The exposed surfaces of one first laminate sheet and one fifth laminate sheet were placed against each other.
[0087] [Example 2B] First, the first silver particles, the second silver particles, polycarbonate, and isobornylcyclohexanol were dissolved and suspended in methyl ethyl ketone in the blending ratio shown in Table 2 below to prepare a fifth varnish. The above components were dissolved and suspended in methyl ethyl ketone by stirring and mixing in the same manner as described in Example 1A. The fifth varnish was applied to the release-treated surface of the first release-treated film to form a coating layer, and the coating layer was heated at a temperature of 110° C. for 3 minutes to form a sintered bonding layer on the first release-treated film, thereby obtaining a sixth laminate sheet. Next, the first silver particles, the second silver particles, polycarbonate, and isobornylcyclohexanol were dissolved and suspended in methyl ethyl ketone in the blending ratio shown in Table 2 below to prepare a sixth varnish. The above components were dissolved and suspended in methyl ethyl ketone by stirring and mixing in the same manner as described in Example 1A. The sixth varnish was applied to the release-treated surface of the first release-treated film to form a coating layer, and the coating layer was heated at a temperature of 110° C. for 3 minutes to form a sintered bonding layer on the first release-treated film, thereby obtaining a seventh laminate sheet. Next, one sixth laminate sheet and one seventh laminate sheet were laminated together to obtain a sheet for sinter bonding according to Example 2B. The exposed surfaces of one sixth laminate sheet and one seventh laminate sheet were placed against each other.
[0088] [Example 3B] First, a first laminate sheet was obtained as described in Example 1A. Next, the first silver particles, the second silver particles, polycarbonate, and isobornylcyclohexanol were dissolved and suspended in methyl ethyl ketone at the blending ratio shown in Table 2 below to prepare a seventh varnish. The above components were dissolved and suspended in methyl ethyl ketone by stirring and mixing in the same manner as described in Example 1A. The seventh varnish was applied to the release-treated surface of the first release-treated film to form a coating layer, and the coating layer was heated at a temperature of 110° C. for 3 minutes to form a sintered bonding layer on the first release-treated film, thereby obtaining the eighth laminate sheet. Next, one first laminate sheet and one eighth laminate sheet were laminated together to obtain a sheet for sinter bonding according to Example 3B. The exposed surfaces of one first laminate sheet and one eighth laminate sheet were placed against each other.
[0089] [Example 4B] First, an eighth laminate sheet was obtained as described in Example 3B. Next, the first silver particles, the second silver particles, polycarbonate, and isobornylcyclohexanol were dissolved and suspended in methyl ethyl ketone at the blending ratio shown in Table 2 below to prepare an eighth varnish. The above components were dissolved and suspended in methyl ethyl ketone by stirring and mixing in the same manner as described in Example 1A. The eighth varnish was applied to the release-treated surface of the first release-treated film to form a coating layer, and the coating layer was heated at a temperature of 110° C. for 3 minutes to form a sintered bonding layer on the first release-treated film. This produced the ninth laminate sheet. Next, one eighth laminate sheet and one ninth laminate sheet were laminated together to obtain a sheet for sinter bonding according to Example 4B. The exposed surfaces of one eighth laminate sheet and one ninth laminate sheet were placed against each other.
[0090] [Comparative example 1B] First, a first laminate sheet was obtained as described in Example 1A. Next, the first silver particles, the second silver particles, polycarbonate, and isobornylcyclohexanol were dissolved and suspended in methyl ethyl ketone at the blending ratio shown in Table 2 below to prepare a ninth varnish. The above components were dissolved and suspended in methyl ethyl ketone by stirring and mixing in the same manner as described in Example 1A. The ninth varnish was applied to the release-treated surface of the first release-treated film to form a coating layer, and the coating layer was heated at a temperature of 110° C. for 3 minutes to form a sintered bonding layer on the first release-treated film. This produced a tenth laminate sheet. Next, one first laminate sheet and one tenth laminate sheet were laminated together to obtain a sheet for sinter bonding according to Comparative Example 1B. The exposed surfaces of one first laminate sheet and one tenth laminate sheet were placed against each other.
[0091] [Comparative Example 2B] First, the tenth varnish was prepared by dissolving and suspending the first silver particles, the second silver particles, and isobornylcyclohexanol in methyl ethyl ketone (MEK) at the blending ratio shown in the following Table 2. In other words, the tenth varnish did not contain polycarbonate. The above components were dissolved and suspended in methyl ethyl ketone by stirring and mixing in the same manner as described in Example 1A. The tenth varnish was applied to the release-treated surface of the first release-treated film to form a coating layer, and the coating layer was heated at a temperature of 110° C. for 3 minutes to form a sintered bonding layer on the first release-treated film. This produced an eleventh laminate sheet. Next, a tenth laminate sheet was obtained as described in the section of Comparative Example 1B. Then, one eleventh laminate sheet and one tenth laminate sheet were laminated together to obtain a sheet for sinter bonding according to Comparative Example 2B. The exposed surfaces of one eleventh laminate sheet and one tenth laminate sheet were placed against each other.
[0092] [Table 2]
[0093] [Example 1C] First, the first silver particles, the second silver particles, polycarbonate, and isobornylcyclohexanol were dissolved and suspended in methyl ethyl ketone (MEK) in the blending ratio shown in Table 3 below to prepare an eleventh varnish. The above components were dissolved and suspended in methyl ethyl ketone by stirring and mixing in the same manner as described in Example 1A. The 11th varnish was applied to the release-treated surface of the 1st release-treated film to form a coating layer, and the coating layer was heated at a temperature of 110° C. for 3 minutes to form a sintered bonding layer on the 1st release-treated film. This produced a 12th laminate sheet. Next, a first laminate sheet was obtained as described in Example 1A. Then, one twelfth laminate sheet and one first laminate sheet were laminated together to obtain a sheet for sinter bonding according to Example 1C. The exposed surfaces of one twelfth laminate sheet and one first laminate sheet were placed against each other.
[0094] [Example 2C] First, a first laminate sheet was obtained as described in Example 1A. Next, the first silver particles, the second silver particles, polycarbonate, and isobornylcyclohexanol were dissolved and suspended in methyl ethyl ketone (MEK) at the blending ratio shown in Table 3 below to prepare a twelfth varnish. The above components were dissolved and suspended in methyl ethyl ketone by stirring and mixing in the same manner as described in Example 1A. The 12th varnish was applied to the release-treated surface of the 1st release-treated film to form a coating layer, and the coating layer was heated at a temperature of 110° C. for 3 minutes to form a sintered bonding layer on the 1st release-treated film. This produced the 13th laminate sheet. Then, one first laminate sheet and one thirteenth laminate sheet were laminated together to obtain a sheet for sinter bonding according to Example 2C. The exposed surfaces of one first laminate sheet and one thirteenth laminate sheet were placed against each other.
[0095] [Example 3C] The first silver particles, the second silver particles, polycarbonate, and isobornylcyclohexanol were dissolved and suspended in methyl ethyl ketone (MEK) in the blending ratio shown in Table 3 below to prepare a thirteenth varnish. The above components were dissolved and suspended in methyl ethyl ketone by stirring and mixing in the same manner as described in Example 1A. The 13th varnish was applied to the release-treated surface of the 1st release-treated film to form a coating layer, and the coating layer was heated at a temperature of 110° C. for 3 minutes to form a sintered bonding layer on the 1st release-treated film. This produced the 14th laminate sheet. Then, two of the fourteenth laminate sheets were overlapped to obtain a sheet for sinter bonding according to Example 3C. The two No. 14 laminate sheets were placed together with their exposed surfaces facing each other.
[0096] [Example 4C] First, a first laminate sheet was obtained as described in Example 1A. Next, a seventh laminate sheet was obtained as described in Example 2B. Then, one first laminate sheet and one seventh laminate sheet were laminated together to obtain a sheet for sinter bonding according to Example 4C. The exposed surfaces of one first laminate sheet and one seventh laminate sheet were placed against each other.
[0097] [Example 5C] First, a first laminate sheet was obtained as described in Example 1A. Next, an eighth laminate sheet was obtained as described in Example 3B. Then, one first laminate sheet and one eighth laminate sheet were laminated together to obtain a sheet for sinter bonding according to Example 5C. The exposed surfaces of one first laminate sheet and one eighth laminate sheet were placed against each other.
[0098] [Example 6C] Two eighth laminate sheets were obtained as described in Example 3B. Next, two of the eighth laminate sheets were overlapped to obtain a sheet for sinter bonding according to Example 6C. The two eighth laminate sheets were placed together with their exposed surfaces facing each other.
[0099] [Table 3]
[0100] <Measurement of minimum load> For both sides (first adhesive surface and second adhesive surface) of the sheet for sinter bonding according to each example, the minimum load reached during the unloading process in load-displacement measurement by nanoindentation method was determined. The minimum load was measured according to the method described in the embodiment section above. The results are shown in Table 4 below.
[0101] In addition, the sintering bonding sheet of Example 1A, the sintering bonding sheet of Example 2A, the sintering bonding sheet of Example 4A, the sintering bonding sheet of Comparative Example 2A, and the sintering bonding sheet of Comparative Example 4A are all constructed by stacking the same laminated sheets on top of each other, so that one exposed surface obtained by peeling off the release treatment film is the first adhesive surface, and the other exposed surface is the second adhesive surface. In the sheet for sinter bonding according to Example 3A, the surface facing the second laminate sheet was the first adhesive surface, and the surface facing the first laminate sheet was the second adhesive surface. Furthermore, in the sintering bonding sheet of Comparative Example 1A, the exposed surface (exposed surface after application) is the first adhesive surface, and the exposed surface (exposed surface formed by peeling off the first release treatment film) obtained by peeling off the first release treatment film is the second adhesive surface. In addition, in the sintering bonding sheet of Comparative Example 3A, the exposed surface (peeling-formed exposed surface) obtained by peeling off the first release treatment film is the first adhesive surface, and the exposed surface (exposed surface after application) is the second adhesive surface.
[0102] In the sinter bonding sheet according to Example 1B, the surface on the first laminate sheet side was the first adhesive surface, and the surface on the fifth laminate sheet side was the second adhesive surface. In the sinter bonding sheet according to Example 2B, the surface on the sixth laminate sheet side was the first adhesive surface, and the surface on the seventh laminate sheet side was the second adhesive surface. In the sheet for sinter bonding according to Example 3B, the surface on the first laminate sheet side was the first adhesive surface, and the surface on the eighth laminate sheet side was the second adhesive surface. In the sheet for sinter bonding according to Example 4B, the surface on the eighth laminate sheet side was the first adhesive surface, and the surface on the ninth laminate sheet side was the second adhesive surface. In the sinter bonding sheet according to Comparative Example 1B, the surface on the first laminate sheet side was the first adhesive surface, and the surface on the tenth laminate sheet side was the second adhesive surface. In the sheet for sinter bonding according to Comparative Example 2B, the surface on the eleventh laminate sheet side was the first adhesive surface, and the surface on the tenth laminate sheet side was the second adhesive surface.
[0103] In addition, in the sheet for sinter bonding according to Example 1C, the surface facing the twelfth laminate sheet was the first adhesive surface, and the surface facing the first laminate sheet was the second adhesive surface. In the sinter bonding sheet according to Example 2C, the surface on the first laminate sheet side was the first adhesive surface, and the surface on the thirteenth laminate sheet side was the second adhesive surface. In the sheet for sinter bonding according to Example 4C, the surface on the first laminate sheet side was the first adhesive surface, and the surface on the seventh laminate sheet side was the second adhesive surface. In the sheet for sinter bonding according to Example 5C, the surface facing the eighth laminate sheet was the first adhesive surface, and the surface facing the first laminate sheet was the second adhesive surface. In addition, the sintering bonding sheet of Example 3C and the sintering bonding sheet of Example 6C are constructed by stacking the same laminated sheets on top of each other, so that one exposed surface obtained by peeling off the release treatment film is the first adhesive surface, and the other exposed surface is the second adhesive surface.
[0104] [Table 4]
[0105] <Evaluation of transferability and temporary fixation> For each example of the sheet for sinter bonding, the transferability of the first adhesive surface was evaluated, and the temporary fixability of the second adhesive surface was also evaluated.
[0106] The transferability was evaluated according to the following procedure. (1) For the sinter bonding sheet according to each example, the release treatment film is peeled off from the first adhesive surface to expose the first adhesive surface. (2) Five 5 mm square Si chips (Ag plated, 200 μm thick) are placed at 5 mm intervals on the first adhesive surface of the sinter bonding sheet of each example. (3) The sinter bonding sheet according to each example, with five Si chips arranged on the first bonding surface, is passed through a laminator equipped with a bonding roll to bond the five Si chips to the first bonding surface. The bonding is performed under the conditions of a temperature of 70°C, a roll pressure of 0.5 MPa, and a roll speed of 10 mm / sec. (4) For each example of the sinter bonding sheet, the release treatment film is peeled off from the second adhesive surface side. Then, the size of the sinter bonding layer of the sinter bonding sheet that has been transferred is visually observed, and the transferability is evaluated according to the following criteria. Excellent: The sintered bonding layer is transferred to the same size as the Si chip. Defective: The sintered bonding layer was not transferred due to poor adhesion to the Si chip.
[0107] The temporary fixation property was evaluated according to the following procedure. (1) After cutting the sinter bonding sheet according to each example into a 10 mm square, the release film is peeled off from the second adhesive surface to expose the second adhesive surface. (2) The second adhesive surface of the sinter bonding sheet according to each example cut into a 10 mm square is placed on the surface of a solid copper (Cu) substrate, and then pressed for 10 seconds under conditions of a temperature of 50°C and pressures of 0.1 MPa and 0.5 MPa. This produces a test specimen for evaluating temporary fixation. (3) The specimen for evaluating the temporary fixation is held so that the surface direction of the pure copper substrate is aligned vertically. Then, the temporary fixation is evaluated according to the following criteria. Excellent: The sintered bonded sheet does not fall even under a pressure of 0.1 MPa. Good: The sintered sheet falls under the pressure condition of 0.1 MPa, but does not fall under the pressure condition of 0.5 MPa. Poor: The sintered sheet falls even under a pressure of 0.5 MPa. Or, separation of the sintered bonding layer is observed when the second adhesive surface is exposed.
[0108] For the sheets for sinter bonding according to each example, the results of evaluating the transferability of the first adhesive surface and the results of evaluating the temporary fixability of the second adhesive surface are shown in Table 5 below.
[0109] [Table 5]
[0110] From Table 5, it can be seen that the sintering bonding sheets of each Example gave good results in terms of both transferability and temporary fixation, whereas the sintering bonding sheets of each Comparative Example gave poor evaluation results in terms of at least one of transferability and temporary fixation. [Explanation of symbols]
[0111] 1 Base material layer, 2 Sintered bonding layer, 10 Sintered bonding sheet, 2a first adhesive surface, 2b second adhesive surface, 2A first sintered bonding layer, 2B second sintered bonding layer.
Claims
1. a sintered bonding layer including sinterable particles containing a conductive metal and an organic binder; the sintered bonding layer has a first adhesive surface that is bonded to one adherend and a second adhesive surface that is bonded to another adherend, When the value of the minimum load reached during the unloading process in the load-displacement measurement by nanoindentation method for the first adhesive surface is defined as b1, and the value of the minimum load reached during the unloading process in the load-displacement measurement by nanoindentation method for the second adhesive surface is defined as b2, The b1 satisfies −100 μN≦b1≦−35 μN, The b2 satisfies −100 μN≦b2≦−35 μN. Sheet for sinter bonding.
2. The b1 satisfies −100 μN≦b1≦−45 μN, The b2 satisfies −90 μN<b2≦−39 μN. The sinter-bonding sheet according to claim 1 .
3. The b1 and the b2 satisfy the relationship b1≦b2. The sinter-bonding sheet according to claim 1 or 2.
4. the organic binder includes a first organic binder and a second organic binder having a molecular weight smaller than that of the first organic binder; The content of the first organic binder in the sintered bonding layer is defined as BC 1 % by mass, and the content of the second organic binder is BC 2 When expressed as mass%, the BC 1 and the BC 2 is B.C. 1 :BC 2 = 6:4 to 0.5:9.
5. The sinter-bonding sheet according to claim 1 or 2.
5. The content SC of the sinterable particles in the sintered bonding layer is 85% by mass or more and 97% by mass or less. The sinter-bonding sheet according to claim 1 or 2.
6. the sintered bonding layer includes a first sintered bonding layer and a second sintered bonding layer stacked on the first sintered bonding layer, the first sintered bonding layer contains the sinterable particles and at least one of a first organic binder and a second organic binder having a molecular weight smaller than that of the first organic binder, the second sintered bonding layer contains the sinterable particles and at least one of the first organic binder and the second organic binder as the organic binder, The first sintered bonding layer and the second sintered bonding layer have a first organic binder content BC 1 , the content BC of the second organic binder 2 and at least one of the sinterable particle contents SC is different from each other; The sinter-bonding sheet according to claim 1 or 2.
7. The sinterable particles contain, as the conductive metal, at least one selected from the group consisting of silver, copper, silver oxide, and copper oxide. The sinter-bonding sheet according to claim 1 or 2.
8. a first release sheet is attached to the first adhesive surface, and a second release sheet is attached to the second adhesive surface; The sinter-bonding sheet according to claim 1 or 2.
Citation Information
Patent Citations
Sintering joint sheet and sintering joint sheet with base material
JP2020150188A
Cited By
Temporary joining composition and method for producing joined body
WO2026204138A1