Polyphenylene ether, production method of the same, thermosetting composition, prepreg, and laminate

A polyphenylene ether with optimized repeating units and functional groups addresses solubility issues in ketone solvents, enabling improved thermosetting compositions and laminates for electronic applications.

JP2024149538AActive Publication Date: 2024-10-18ASAHI KASEI KOGYO KABUSHIKI KAISHA

Patent Information

Application Number
JP2024122248
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-01-25
Filing Date
2024-07-29
Publication Date
2024-10-18
Estimated Expiration
2041-12-15

Smart Images

  • Figure 2024149538000001
    Figure 2024149538000001
  • Figure 2024149538000002
    Figure 2024149538000002
  • Figure 2024149538000003
    Figure 2024149538000003
Patent Text Reader

Abstract

To provide a polyphenylene ether excellent in solubility in a general-purpose ketone-based solvent, a production method of the same, a thermosetting composition using the polyphenylene ether, prepreg, and laminate.SOLUTION: A polyphenylene ether includes: 5-85 mol% of a repeating unit derived from a phenol of formula (1); and 15-95 mol% of a repeating unit derived from a phenol of formula (2) based on 100 mol% of a total of the repeating unit derived from the phenol of formula (1) and the repeating unit derived from the phenol of formula (2), where the reduced viscosity (η sp / c) measured at 30°C by a chloroform solution of a concentration of 0.5 g / dL is 0.03-0.30 dL / g.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to polyphenylene ether, a method for producing the same, a thermosetting composition, a prepreg, and a laminate. [Background technology]

[0002] Polyphenylene ether (hereinafter, also referred to as "PPE") has excellent high-frequency characteristics, flame retardancy, and heat resistance, and is therefore widely used as a material for products and parts in the electrical and electronics, automotive, and food and packaging fields, as well as in various other industrial materials. In particular, in recent years, its low dielectric properties and heat resistance have been utilized to promote its application as a modifier in electronic materials such as substrate materials and in various other applications.

[0003] However, although high molecular weight polyphenylene ethers having repeating units derived from monohydric phenols, typically typified by 2,6-dimethylphenol, dissolve in highly toxic solvents such as chloroform, they have the problem that they are poorly soluble at high concentrations at room temperature in aromatic solvents such as toluene, which are known to be good solvents, and are insoluble in ketone solvents such as methyl ethyl ketone. For this reason, for example, when used as a wiring board material, it is difficult to handle resin varnish solutions in toluene, methyl ethyl ketone, etc.

[0004] Patent Document 1 discloses that polyphenylene ether having a low molecular weight and a specific particle size has excellent solubility in solvents such as methyl ethyl ketone. Furthermore, Patent Document 2 describes a modified polyphenylene ether compound having a specific polyphenylene ether moiety in its molecular structure and having at least one p-ethenylbenzyl group, m-ethenylbenzyl group, or the like at the molecular end. Furthermore, Patent Document 3 describes a modified polymer having a polyphenylene ether portion in its molecular structure and having a methacryl group at the molecular end. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2004-99824 A [Patent Document 2] JP 2004-339328 A [Patent Document 3] Special Publication No. 2008-510059 Summary of the Invention [Problem to be solved by the invention]

[0006] As described above, Patent Documents 1-3 disclose methods for producing polyphenylene ethers with reduced molecular weights in order to improve the solvent solubility of polyphenylene ethers, but the solubility at room temperature in general-purpose ketone solvents such as methyl ethyl ketone is not significantly improved by simply lowering the molecular weight of polyphenylene ether, and is still insufficient. In particular, a method for improving the long-term solvent solubility in ketone solvents is desired.

[0007] The present invention has been made in view of the above problems, and has an object to provide a polyphenylene ether having excellent solubility in a general-purpose ketone solvent and a method for producing the same, as well as a thermosetting composition, a prepreg, and a laminate using the polyphenylene ether. [Means for solving the problem]

[0008] That is, the present invention is as follows. [1] The repeating unit derived from a phenol represented by the following formula (1) contains 5 to 85 mol % of the repeating unit derived from a phenol represented by the following formula (1) and 15 to 95 mol % of the repeating unit derived from a phenol represented by the following formula (2), relative to 100 mol % in total of the repeating unit derived from a phenol represented by the following formula (1) and the repeating unit derived from a phenol represented by the following formula (2), The reduced viscosity (ηsp / c) measured in a chloroform solution with a concentration of 0.5 g / dL at 30°C is 0.03 to 0.30 dL / g. 1. A polyphenylene ether comprising: [ka] (In formula (1), R 11 each independently represents an optionally substituted saturated hydrocarbon group having 1 to 6 carbon atoms, an optionally substituted aryl group having 6 to 12 carbon atoms, or a halogen atom; R 12 are each independently a hydrogen atom, an optionally substituted hydrocarbon group having 1 to 6 carbon atoms, an optionally substituted aryl group having 6 to 12 carbon atoms, or a halogen atom. [ka] (In formula (2), R 22 each independently represents a hydrogen atom, an optionally substituted saturated or unsaturated hydrocarbon group having 1 to 20 carbon atoms, an optionally substituted aryl group having 6 to 12 carbon atoms, or a halogen atom; 22 are not both hydrogen atoms, R 21 is a partial structure represented by the following formula (3). [ka] (In formula (3), R 31 each independently represents an optionally substituted linear alkyl group having 1 to 8 carbon atoms, or two R 31 is a cyclic alkyl structure having 1 to 8 carbon atoms, R 32 each independently represents an optionally substituted alkylene group having 1 to 8 carbon atoms; each b independently represents 0 or 1; R 33 is a hydrogen atom, an optionally substituted alkyl group having 1 to 8 carbon atoms, or an optionally substituted phenyl group. [2] The polyphenylene ether according to [1], wherein the partial structure represented by the formula (3) is a t-butyl group. [3] The polyphenylene ether according to [1] or [2], having an average number of hydroxyl groups of less than 2.5 per molecule. [4] The polyphenylene ether according to any one of [1] to [3], having an average number of hydroxyl groups of less than 0.2 per molecule. [5] The polyphenylene ether according to any one of [1] to [4], which has at least one partial structure selected from the group consisting of the following formula (4), formula (5), formula (6), and formula (7), and has an average number of hydroxyl groups of less than 0.2 per molecule: [ka] [ka] [ka] (In formula (6), R 6 is a hydrogen atom or a saturated or unsaturated hydrocarbon group having 1 to 10 carbon atoms, and the saturated or unsaturated hydrocarbon may have a substituent within the limit of satisfying the condition of having 1 to 10 carbon atoms.) [ka] (In formula (7), R 7 is a saturated or unsaturated divalent hydrocarbon group having 1 to 10 carbon atoms, and the saturated or unsaturated divalent hydrocarbon may have a substituent within the limit of satisfying the condition of having 1 to 10 carbon atoms; R 8 is a hydrogen atom or a saturated or unsaturated hydrocarbon group having 1 to 10 carbon atoms, and the saturated or unsaturated hydrocarbon may have a substituent within the limit of satisfying the condition of having 1 to 10 carbon atoms.) [6] The polyphenylene ether according to any one of [1] to [5], comprising a repeating unit derived from a monohydric phenol having at least one unsaturated hydrocarbon group on a carbon atom at the ortho position to a carbon atom to which a phenol hydroxyl group is bonded. [7] The polyphenylene ether according to [6], wherein the monohydric phenol is 2-allylphenol or 2-methyl-6-allylphenol. [8] A method for producing the polyphenylene ether according to any one of [1] to [7], comprising a step of oxidatively polymerizing a phenol represented by the formula (1) and a phenol represented by the formula (2). [9] A polyphenylene ether solution comprising the polyphenylene ether according to any one of [1] to [7] and a ketone solvent.

[10] A thermosetting composition comprising the polyphenylene ether according to any one of [1] to [7].

[11] A prepreg comprising a substrate and the thermosetting composition according to

[10] .

[12] The prepreg according to

[11] , wherein the substrate is a glass cloth.

[13] A laminate comprising a cured product of the prepreg according to

[11] or

[12] and a metal foil. Effect of the Invention

[0009] According to the present invention, it is possible to provide a polyphenylene ether having excellent solubility in a general-purpose ketone solvent and a method for producing the same. It is also possible to provide a thermosetting composition, a prepreg, and a laminate using the polyphenylene ether. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, an embodiment for carrying out the present invention (hereinafter, referred to as "the present embodiment") will be described in detail. The following embodiment is an example for explaining the present invention, and the present invention is not limited to only this embodiment, and the present invention can be carried out by appropriately modifying it within the scope of the gist of the present invention.

[0011] In the present embodiment, polyphenylene ether in which some or all of the hydroxyl groups contained in the polyphenylene ether have been modified may be simply referred to as "polyphenylene ether". Therefore, when the term "polyphenylene ether" is used, it includes both unmodified polyphenylene ether and modified polyphenylene ether, unless there is a particular contradiction. In this specification, A (numeric value) to B (numeric value) mean greater than or equal to A and less than or equal to B. In addition, in this specification, examples of the substituent include a saturated or unsaturated hydrocarbon group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, and a halogen atom.

[0012] <Polyphenylene ether> The polyphenylene ether of the present embodiment contains at least a repeating unit derived from a phenol of the following formula (1) and a repeating unit derived from a phenol of the following formula (2), and the repeating units in the compound may consist only of the repeating unit derived from a phenol of the following formula (1) and the repeating unit derived from a phenol of the following formula (2). [ka] (In formula (1), R 11 each independently represents an optionally substituted saturated hydrocarbon group having 1 to 6 carbon atoms, an optionally substituted aryl group having 6 to 12 carbon atoms, or a halogen atom; R 12 are each independently a hydrogen atom, an optionally substituted hydrocarbon group having 1 to 6 carbon atoms, an optionally substituted aryl group having 6 to 12 carbon atoms, or a halogen atom. [ka] (In formula (2), R 22 each independently represents a hydrogen atom, an optionally substituted saturated or unsaturated hydrocarbon group having 1 to 20 carbon atoms, an optionally substituted aryl group having 6 to 12 carbon atoms, or a halogen atom; 22 are not both hydrogen atoms, R 21 is a partial structure represented by the following formula (3). [ka] (In formula (3), R 31 each independently represents an optionally substituted linear alkyl group having 1 to 8 carbon atoms, or two R 31 is a cyclic alkyl structure having 1 to 8 carbon atoms, R 32each independently represents an optionally substituted alkylene group having 1 to 8 carbon atoms; each b independently represents 0 or 1; R 33 is any one of a hydrogen atom, an optionally substituted alkyl group having 1 to 8 carbon atoms, and an optionally substituted phenyl group.

[0013] In the above formula (1), R 11 are each independently preferably a saturated hydrocarbon group having 1 to 6 carbon atoms or an aryl group having 6 to 12 carbon atoms, more preferably a methyl group or a phenyl group, and further preferably a methyl group. 11 Preferably, both have the same structure. Above R 11 Examples of the substituent in the saturated hydrocarbon group having 1 to 6 carbon atoms and the aryl group having 6 to 12 carbon atoms include a saturated or unsaturated hydrocarbon group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, and a halogen atom.

[0014] In the above formula (1), R 12 are each independently preferably a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms, more preferably a hydrogen atom or a methyl group. 12 are preferably different, and it is more preferable that one is a hydrogen atom and the other is a hydrocarbon group having 1 to 6 carbon atoms (preferably a methyl group). Above R 12 Examples of the substituent in the hydrocarbon group having 1 to 6 carbon atoms and the aryl group having 6 to 12 carbon atoms include a saturated or unsaturated hydrocarbon group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, and a halogen atom.

[0015] In the above formula (2), R 22 are each independently preferably a hydrogen atom, a saturated or unsaturated hydrocarbon group having 1 to 15 carbon atoms, or an aryl group having 6 to 12 carbon atoms which may be substituted with an alkyl group having 1 to 6 carbon atoms, more preferably a hydrogen atom, a hydrocarbon group having 1 to 6 carbon atoms, or an aryl group having 6 to 10 carbon atoms which may be substituted with an alkyl group having 1 to 6 carbon atoms, and even more preferably a hydrogen atom or a methyl group. 22are preferably different, and it is more preferable that one is a hydrogen atom and the other is a hydrocarbon group having 1 to 6 carbon atoms (preferably a methyl group). Above R 22 Examples of the substituent in the saturated or unsaturated hydrocarbon group having 1 to 20 carbon atoms and the aryl group having 6 to 12 carbon atoms include a saturated or unsaturated hydrocarbon group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, and a halogen atom.

[0016] The partial structure represented by the above formula (3) is preferably a group containing a secondary and / or tertiary carbon, such as an isopropyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a tert-amyl group, a 2,2-dimethylpropyl group, a cyclohexyl group, or a structure having a phenyl group at the terminal thereof, more preferably a tert-butyl group or a cyclohexyl group, and even more preferably a tert-butyl group. In addition, the above R 31 The substituent in the linear alkyl group having 1 to 8 carbon atoms, R 32 The substituents in the alkylene group having 1 to 8 carbon atoms and the above R 33 Examples of the substituent in the alkyl group having 1 to 8 carbon atoms and the phenyl group include a saturated or unsaturated hydrocarbon group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, and a halogen atom.

[0017] In this embodiment, the structure of polyphenylene ether can be identified by analyzing the polyphenylene ether by techniques such as NMR and mass spectrometry. As a specific method for identifying the structure of polyphenylene ether, field desorption mass spectrometry (FD-MS), which is known to be less likely to cause fragmentation, can be performed, and repeating units can be estimated based on the intervals between detected ions. In addition, there is a method for estimating the structure of polyphenylene ether by combining peak analysis of fragment ions by electron ionization (EI) and structural analysis by NMR.

[0018] The polyphenylene ether of this embodiment contains 5 to 85 mol % of the repeating units derived from phenol of formula (1) and 15 to 95 mol % of the repeating units derived from phenol of formula (2) relative to 100 mol % in total of the repeating units derived from phenol of formula (1) and the repeating units derived from phenol of formula (2). From the viewpoint of obtaining a polyphenylene ether having excellent solvent solubility and low dielectric tangent, the repeating units derived from phenol of formula (2) are preferably 18 mol % or more, more preferably 20 mol % or more. From the same viewpoint, the repeating units derived from phenol of formula (1) are preferably 82 mol % or less, more preferably 80 mol % or less. The repeating unit derived from the phenol of formula (1) contained in the polyphenylene ether of the present embodiment may be one or more kinds. The repeating unit derived from the phenol of formula (2) contained in the polyphenylene ether of the present embodiment may be one or more kinds.

[0019] With respect to 100 mol % of monomer units contained in the polyphenylene ether of the present embodiment (e.g., all monomer units derived from phenol contained in the polyphenylene ether), the total molar amount of the repeating units derived from phenol of formula (1) and the repeating units derived from phenol of formula (2) is preferably 75 mol % or more, more preferably 90 mol % or more, and even more preferably 95 mol % or more.

[0020] The ratio of the repeating unit derived from the phenol of formula (1) to the repeating unit derived from the phenol of formula (2) is, for example, 1 H NMR, 13 It can be determined using an analytical technique such as C NMR, and more specifically, it can be measured by the method described in the Examples below.

[0021] Since the phenol of formula (1) has no unsubstituted ortho positions (i.e., no hydrogen atoms are bonded to the carbon atoms in the two ortho positions to the carbon atom to which the hydroxyl group is bonded), it can react with another phenolic monomer only at the carbon atom in the para position to the phenolic hydroxyl group. Thus, the repeating unit derived from formula (1) includes a repeating unit having the structure of formula (8) below. [ka] (In formula (8), R 11 and R 12 is the same as equation (1).

[0022] In addition to the phenolic hydroxyl group, the phenol of formula (2) can react with another phenolic monomer at either the ortho or para position of the phenol. Thus, the repeat unit derived from the phenol of formula (2) has a monomer unit of formula (9), formula (10), or a combination thereof: [ka] [ka] (R in Equation (9) and Equation (10) 21 , R 22 is the same as equation (2).

[0023] The reduced viscosity of the polyphenylene ether in this embodiment measured in a chloroform solution having a concentration of 0.5 g / dL at 30° C. is preferably 0.03 to 0.30 dL / g, and more preferably 0.06 to 0.30 dL / g. The reduced viscosity can be appropriately selected depending on the application. For example, in order to improve the fluidity when dissolved in a solvent for preparing a varnish in a process of applying the composition to a substrate material, a low reduced viscosity is preferable. The reduced viscosity can be measured by the method described in the Examples below.

[0024] The polyphenylene ether in this embodiment may contain, as an impurity (sometimes simply referred to as "impurity A" in this specification), a ternary copolymer containing a structure derived from a dihydric phenol of the following formula (11) in addition to the phenol of formula (1) and the phenol of formula (2). The polyphenylene ether in this embodiment may be a mixture of the above polyphenylene ether and the above impurity A. The molar ratio of impurity A to 100 mol % of the polyphenylene ether in this embodiment is preferably 10 mol % or less, and more preferably 5 mol % or less. The above-mentioned impurity A can be synthesized, for example, as a terpolymer containing a structure derived from a dihydric phenol, where z=0 in formula (11), by reacting the following formula (12), which is generated as a by-product during the oxidative polymerization of a monohydric phenol, with a polyphenylene ether composed of a monohydric phenol. [ka] (In formula (11), R 11 and R 12 is the same as formula (1). z is 0 or 1, and Y is [ka] (In the formula, R 41 are each independently any one of an optionally substituted hydrocarbon group having 1 to 6 carbon atoms, an optionally substituted aryl group having 6 to 12 carbon atoms, and a halogen atom. [ka] (In formula (12), R 11 and R 12 is the same as equation (1).

[0025] In the present embodiment, the average number of hydroxyl groups in the polyphenylene ether is preferably less than 2.5 / molecule, more preferably less than 2.2 / molecule, and even more preferably less than 2.0 / molecule, in the case of unmodified polyphenylene ether. If the average number of hydroxyl groups exceeds 2.5 / molecule, it means that the polyphenylene ether is a multibranched unmodified polyphenylene ether whose structure cannot be controlled. The average number of hydroxyl groups can be measured by the method described in the Examples below.

[0026] The polyphenylene ether in this embodiment may be a modified polyphenylene ether in which a hydroxyl group contained in the polyphenylene ether is modified to a functional group (e.g., a functional group containing an unsaturated carbon bond, etc.). In the case of the modified polyphenylene ether, the average number of hydroxyl groups is preferably less than 0.2 per molecule, more preferably less than 0.1 per molecule, and even more preferably less than 0.01 per molecule.

[0027] The polyphenylene ether in this embodiment may have at least one partial structure selected from the group consisting of the following formulas (4), (5), (6), and (7). [ka] [ka] [ka] (In formula (6), R 6 is a hydrogen atom or a saturated or unsaturated hydrocarbon group having 1 to 10 carbon atoms, and the saturated or unsaturated hydrocarbon is R 6 may have a substituent within the range of a total carbon number of 1 to 10.) [ka] (In formula (7), R 7 is a saturated or unsaturated divalent hydrocarbon group having 1 to 10 carbon atoms, and the saturated or unsaturated divalent hydrocarbon is R7 may have a substituent within a range in which the total carbon number of R is 1 to 10; 8 is a hydrogen atom or a saturated or unsaturated hydrocarbon group having 1 to 10 carbon atoms, and the saturated or unsaturated hydrocarbon is R 8 may have a substituent within the range of a total carbon number of 1 to 10.) At least one partial structure selected from the group consisting of formula (4), formula (5), formula (6), and formula (7) may be directly bonded to a hydroxyl group contained in the polyphenylene ether.

[0028] The ratio of the repeating unit derived from phenol of formula (1) and the repeating unit derived from phenol of formula (2) contained in the modified polyphenylene ether into which at least one partial structure represented by the group consisting of the above formulas (4), (5), (6), and (7) has been introduced is, for example, 1 H NMR, 13 It can be determined using an analytical technique such as C NMR, and more specifically, it can be measured by the method described in the Examples below.

[0029] The polyphenylene ether in this embodiment may contain a monohydric phenol having at least one unsaturated hydrocarbon group on the carbon atom at the ortho position of the carbon atom to which the hydroxyl group of the phenol is bonded. The monohydric phenol preferably has one unsaturated hydrocarbon group bonded to the carbon atom at the ortho position of the carbon atom to which the hydroxyl group of the phenol is bonded. The unsaturated hydrocarbon may be bonded to each of the carbon atoms at the ortho positions of the carbon atom to which the hydroxyl group of the monohydric phenol is bonded, or may be bonded to one of the carbon atoms at the ortho position of the carbon atom to which the hydroxyl group of the phenol is bonded. The monohydric phenol having at least one unsaturated hydrocarbon group on the carbon atom at the ortho position of the carbon atom to which the hydroxyl group of the phenol is bonded refers to a monohydric phenol different from the phenol of the formula (1) or the phenol of the formula (2). The unsaturated hydrocarbon group is preferably an unsaturated hydrocarbon group having 3 to 10 carbon atoms, and more preferably an unsaturated hydrocarbon group having 3 to 5 carbon atoms. Examples of such unsaturated hydrocarbon groups include alkenyl groups (e.g., vinyl group, allyl group, etc.) and alkynyl groups (e.g., ethynyl group, 1-propynyl, 2-propynyl, etc.). The above unsaturated hydrocarbon may have a substituent as long as the condition of 3 to 10 carbon atoms is satisfied.

[0030] The introduction rate of the monohydric phenol having at least one unsaturated hydrocarbon group on a carbon atom in the ortho position to the carbon atom to which the phenol hydroxyl group is bonded may be appropriately adjusted in order to adjust the number of curable functional groups, but the monohydric phenol having at least one unsaturated hydrocarbon group on a carbon atom in the ortho position to the carbon atom to which the phenol hydroxyl group is bonded is preferably 0.1 to 30 mol %, and more preferably 0.1 to 25 mol %, relative to the total of phenol in formula (1) and the monohydric phenol having at least one unsaturated hydrocarbon group on a carbon atom in the ortho position to the carbon atom to which the phenol hydroxyl group is bonded. In the polyphenylene ether of the present embodiment, the molar ratio of the repeating units derived from the monohydric phenol having at least one unsaturated hydrocarbon group on a carbon atom in the ortho position to the carbon atom to which the hydroxyl group of the phenol is bonded to the sum of the repeating units derived from the phenol of formula (1) and the repeating units derived from the monohydric phenol having at least one unsaturated hydrocarbon group on a carbon atom in the ortho position to the carbon atom to which the hydroxyl group of the phenol is bonded is preferably 0.1 to 40 mol %, and more preferably 0.1 to 10 mol %.

[0031] <Production method of polyphenylene ether> The polyphenylene ether of the present embodiment can be obtained, for example, by a method including at least a step of oxidatively polymerizing a monohydric phenol compound represented by the above formula (1) or formula (2). The above oxidative polymerization step preferably includes oxidatively polymerizing a raw material including at least the above phenol of formula (1) and the phenol of formula (2).

[0032] Examples of the monohydric phenol compound represented by the above formula (1) include 2,6-dimethylphenol, 2-methyl-6-ethylphenol, 2,6-diethylphenol, 2-ethyl-6-n-propylphenol, 2-methyl-6-chlorophenol, 2-methyl-6-bromophenol, 2-methyl-6-n-propylphenol, 2-ethyl-6-bromophenol, 2-methyl-6-n-butylphenol, 2,6-di-n-propylphenol, 2-ethyl-6-chlorophenol, 2-methyl-6-phenylphenol, 2,6-diphenylphenol, 2-methyl-6-tolylphenol, 2,6-ditolylphenol, 2,3,6-trimethylphenol, 2,3-diethyl-6-n-propylphenol, 2,3,6-tributylphenol, 2,6-di-n-butyl-3-methylphenol, 2,6-dimethyl-3-n-butylphenol, and 2,6-dimethyl-3-t-butylphenol. Among these, 2,6-dimethylphenol, 2,3,6-trimethylphenol, and 2,6-diphenylphenol are particularly preferable since they are inexpensive and easily available. The monohydric phenol compound represented by the above formula (1) may be used alone or in combination of two or more kinds.

[0033] Examples of the monohydric phenol compound represented by the above formula (2) include 2-isopropyl-5-methylphenol, 2-cyclohexyl-5-methylphenol, 2-tert-butyl-5-methylphenol, 2-isobutyl-5-methylphenol, etc. From the viewpoint of suppressing multi-branching and gelation, 2-t-butyl-5-methylphenol and 2-cyclohexyl-5-methylphenol, which are bulky substituents, are more preferred. The monohydric phenol compound represented by the above formula (2) may be used alone or in combination of two or more kinds.

[0034] The step of carrying out the oxidative polymerization may be, for example, a step of carrying out oxidative polymerization of a raw material containing, in addition to the phenol of the formula (1) and the phenol of the formula (2), a monohydric phenol having at least one unsaturated hydrocarbon group on a carbon atom at the ortho position to the carbon atom to which the hydroxyl group of the phenol is bonded. The monohydric phenol having at least one unsaturated hydrocarbon group on the carbon atom in the ortho position relative to the carbon atom to which the phenol hydroxyl group is bonded is preferably a monohydric phenol in which at least one (preferably one) unsaturated hydrocarbon group is bonded to the carbon atom in the ortho position and hydrogen atoms are bonded to the carbon atoms in the meta and para positions, more preferably 2-allylphenol, 2-allyl-6-methylphenol, and even more preferably 2-allylphenol. The monohydric phenol having at least one unsaturated hydrocarbon group on the carbon atom at the ortho position relative to the carbon atom to which the phenol hydroxyl group is bonded may be used alone or in combination of two or more kinds.

[0035] Usually, in the oxidative polymerization of phenols having hydrogen atoms at the ortho positions (e.g., 2-methylphenol, 2,5-dimethylphenol, 2-phenylphenol), ether bonds can also be formed at the ortho positions, making it difficult to control the bonding positions of the phenol compounds during oxidative polymerization, resulting in high-molecular-weight polymers that are polymerized in a branched form with an average of 3 or more hydroxyl groups per molecule, and ultimately generating gel components that are insoluble in solvents (see the oxidative polymerization of 2,5-dimethylphenol and 2,6-dimethylphenol in Reference Example 1 below). On the other hand, when a phenol having a bulky substituent at the ortho-position on one side, as represented by the above formula (2), is used, it is possible to control the bonding position of the phenol compound during oxidative polymerization, despite the presence of a hydrogen atom at the ortho-position on the opposite side, and a polyphenylene ether having an average of less than 2.5 hydroxyl groups per molecule can be obtained. Furthermore, when a phenol having a bulky substituent at the ortho-position on one side represented by the above formula (2) is used, even when a monohydric phenol having a non-bulky substituent (e.g., a hydrogen atom, an allyl group, a methyl group, an ethyl group, a methoxy group, etc.) at the ortho-position of the oxygen atom of the phenol is used as the third component, gelation does not occur and a polyphenylene ether having an average of less than 2.5 hydroxyl groups per molecule can be obtained.

[0036] The molecular weight of the polyphenylene ether in this embodiment can be adjusted by the molar ratio of the repeating unit derived from the above formula (2) to the sum of the repeating unit derived from the above formula (1) and the repeating unit derived from the above formula (2). That is, when the molar ratio of the repeating unit derived from the above formula (2) is high, the molecular weight (reduced viscosity) can be lowered, and when the molar ratio of the repeating unit derived from the above formula (2) is low, the molecular weight (reduced viscosity) can be adjusted to be high. Although the reason is unclear, it is presumed that the bulky substitution at the ortho position of the above formula (2) suppresses the increase in molecular weight.

[0037] (Oxidative polymerization process) Here, in the method for producing polyphenylene ether, an aromatic solvent that is a good solvent for polyphenylene ether can be used as the polymerization solvent in the oxidative polymerization step. Here, a good solvent for polyphenylene ether is a solvent capable of dissolving polyphenylene ether. Examples of such solvents include aromatic hydrocarbons such as benzene, toluene, xylene (including o-, m-, and p-isomers) and ethylbenzene; halogenated hydrocarbons such as chlorobenzene and dichlorobenzene; and nitro compounds such as nitrobenzene.

[0038] As the polymerization catalyst used in this embodiment, a known catalyst system that can be generally used for the production of polyphenylene ether can be used. A generally known catalyst system is one that is composed of a transition metal ion having redox ability and an amine compound that can form a complex with the transition metal ion, such as a catalyst system composed of a copper compound and an amine compound, a catalyst system composed of a manganese compound and an amine compound, a catalyst system composed of a cobalt compound and an amine compound, etc. Since the polymerization reaction proceeds efficiently under slightly alkaline conditions, a small amount of alkali or an additional amine compound may be added thereto.

[0039] The polymerization catalyst preferably used in the present embodiment is a catalyst containing a copper compound, a halogen compound, and an amine compound as catalyst components, and more preferably a catalyst containing a diamine compound represented by the following formula (13) as the amine compound.

[0040] [ka] In formula (13), R 14 , R 15 , R 16 , R 17 are each independently a hydrogen atom or a linear or branched alkyl group having 1 to 6 carbon atoms, but are not all hydrogen atoms at the same time. 18 is a linear or methyl-branched alkylene group having 2 to 5 carbon atoms.

[0041] Examples of the copper compound of the catalyst component described herein are listed below. Suitable copper compounds include cuprous compounds, cupric compounds, and mixtures thereof. Examples of cupric compounds include, for example, cupric chloride, cupric bromide, cupric sulfate, and cupric nitrate. Examples of cuprous compounds include, for example, cuprous chloride, cuprous bromide, cuprous sulfate, and cuprous nitrate. Particularly preferred metal compounds among these are cuprous chloride, cupric chloride, cuprous bromide, and cupric bromide. These copper salts may be synthesized at the time of use from oxides (e.g., cuprous oxide), carbonates, hydroxides, and the like and corresponding halogens or acids. A method that is often used is to mix the cuprous oxide exemplified above with hydrogen halide (or a solution of hydrogen halide) to prepare the copper salt.

[0042] Examples of halogen compounds include hydrogen chloride, hydrogen bromide, hydrogen iodide, sodium chloride, sodium bromide, sodium iodide, potassium chloride, potassium bromide, potassium iodide, tetramethylammonium chloride, tetramethylammonium bromide, tetramethylammonium iodide, tetraethylammonium chloride, tetraethylammonium bromide, and tetraethylammonium iodide. These compounds can be used as aqueous solutions or solutions using appropriate solvents. These halogen compounds can be used alone as components, or in combination of two or more. Preferred halogen compounds are aqueous solutions of hydrogen chloride and hydrogen bromide.

[0043] The amount of these compounds used is not particularly limited, but is preferably 2 to 20 times the molar amount of halogen atoms relative to the molar amount of copper atoms, and the amount of copper atoms used is preferably in the range of 0.02 to 0.6 moles per 100 moles of the phenol compound added to the polymerization reaction.

[0044] Examples of the diamine compound of the catalyst component are as follows: N,N,N',N'-tetramethylethylenediamine, N,N,N'-trimethylethylenediamine, N,N'-dimethylethylenediamine, N,N-dimethylethylenediamine, N-methylethylenediamine, N,N,N',N'-tetraethylethylenediamine, N,N,N'-triethylethylenediamine, N,N'-diethylethylenediamine, N,N-diethylethylenediamine, N-ethylethylenediamine, N,N-dimethyl-N'-ethylethylenediamine, N,N'-dimethyl-N-ethylethylenediamine, Nn-propylethylenediamine, N,N'-n-propylethylenediamine, Ni-propylethylenediamine, N,N'-i-propylethylenediamine, Nn-butylethylenediamine, amine, N,N'-n-butylethylenediamine, Ni-butylethylenediamine, N,N'-i-butylethylenediamine, Nt-butylethylenediamine, N,N'-t-butylethylenediamine, N,N,N',N'-tetramethyl-1,3-diaminopropane, N,N,N'-trimethyl-1,3-diaminopropane, N,N'-dimethyl-1,3-diaminopropane, N-methyl-1,3-diaminopropane, N,N,N',N'-tetramethyl-1,3-diamino-1-methylpropane, N,N,N',N'-tetramethyl-1,3-diamino-2-methylpropane, N,N,N',N'-tetramethyl-1,4-diaminobutane, and N,N,N',N'-tetramethyl-1,5-diaminopentane. A preferred diamine compound for this embodiment is one in which the number of carbon atoms in the alkylene group connecting the two nitrogen atoms is 2 or 3. The amount of these diamine compounds used is not particularly limited, but is preferably in the range of 0.01 mol to 10 mol per 100 mol of the phenol compound added to the polymerization reaction.

[0045] In this embodiment, the polymerization catalyst may contain a primary amine and a secondary monoamine as a component. Examples of the secondary monoamine include, but are not limited to, dimethylamine, diethylamine, di-n-propylamine, di-i-propylamine, di-n-butylamine, di-i-butylamine, di-t-butylamine, dipentylamines, dihexylamines, dioctylamines, didecylamines, dibenzylamines, methylethylamine, methylpropylamine, methylbutylamine, cyclohexylamine, N-phenylmethanolamine, N-phenylethanolamine, N-phenylpropanolamine, N-(m-methylphenyl)ethanolamine, N-(p-methylphenyl)ethanolamine, N-(2',6'-dimethylphenyl)ethanolamine, N-(p-chlorophenyl)ethanolamine, N-ethylaniline, N-butylaniline, N-methyl-2-methylaniline, N-methyl-2,6-dimethylaniline, and diphenylamine.

[0046] The polymerization catalyst of the present embodiment may also contain a tertiary monoamine compound as a component thereof. The tertiary monoamine compound is an aliphatic tertiary amine including an alicyclic tertiary amine. Examples of the tertiary monoamine compound include trimethylamine, triethylamine, tripropylamine, tributylamine, triisobutylamine, dimethylethylamine, dimethylpropylamine, allyldiethylamine, dimethyl-n-butylamine, diethylisopropylamine, and N-methylcyclohexylamine. These tertiary monoamines may be used alone or in combination of two or more. The amount of these compounds used is not particularly limited, but is preferably in the range of 15 moles or less relative to 100 moles of the phenol compound added to the polymerization reaction.

[0047] In this embodiment, there is no limitation on adding a surfactant that has been known to have an effect of improving polymerization activity. Examples of such surfactants include trioctylmethylammonium chloride, known under the trade names Aliquat 336 and Capriquat. The amount of the surfactant used is preferably within a range not exceeding 0.1% by mass relative to the total amount (100% by mass) of the polymerization reaction mixture.

[0048] As the oxygen-containing gas in the polymerization of this embodiment, in addition to pure oxygen, a mixture of oxygen and an inert gas such as nitrogen in any ratio, air, and a mixture of air and an inert gas such as nitrogen in any ratio can be used. Normal pressure is sufficient for the pressure in the system during the polymerization reaction, but reduced or increased pressure can be used as necessary.

[0049] The polymerization temperature is not particularly limited, but if it is too low, the reaction does not proceed easily, and if it is too high, the reaction selectivity may decrease or gel may be formed, so it is in the range of 0 to 60°C, preferably 10 to 40°C.

[0050] In the process for producing polyphenylene ether, the polymerization can also be carried out in a poor solvent such as alcohol.

[0051] (Copper extraction and by-product removal process) In this embodiment, there is no particular restriction on the post-treatment method after the polymerization reaction is completed. Usually, an acid such as hydrochloric acid or acetic acid, or ethylenediaminetetraacetic acid (EDTA) and its salts, nitrilotriacetic acid and its salts, etc. are added to the reaction liquid to deactivate the catalyst. In addition, a method for removing and treating the dihydric phenol by-product generated by the polymerization of polyphenylene ether can be performed using a conventionally known method. If the metal ions, which are the catalyst, are substantially deactivated as described above, the mixture can be decolorized simply by heating it. Alternatively, a method of adding a required amount of a known reducing agent is also possible. Examples of known reducing agents include hydroquinone and sodium dithionite.

[0052] (Liquid-liquid separation process) In the method for producing polyphenylene ether, water may be added to extract the compound that has deactivated the copper catalyst, and then liquid-liquid separation may be performed into an organic phase and an aqueous phase, and the aqueous phase may be removed to remove the copper catalyst from the organic phase. This liquid-liquid separation step is not particularly limited, and may include methods such as static separation and separation using a centrifuge. In order to promote the liquid-liquid separation, a known surfactant or the like may be used.

[0053] (concentration / drying process) Next, in the method for producing polyphenylene ether of the present embodiment, the organic phase containing the polyphenylene ether after liquid-liquid separation may be concentrated and dried by volatilizing the solvent.

[0054] The method for volatilizing the solvent contained in the organic phase is not particularly limited, but examples thereof include a method of transferring the organic phase to a high-temperature concentration tank and distilling off the solvent to concentrate it, and a method of distilling off toluene using equipment such as a rotary evaporator to concentrate it.

[0055] The temperature of the drying treatment in the drying step is preferably at least 60° C. or higher, more preferably 80° C. or higher, even more preferably 120° C. or higher, and most preferably 140° C. or higher. When the polyphenylene ether is dried at a temperature of 60° C. or higher, the content of high-boiling-point volatile components in the polyphenylene ether powder can be efficiently reduced.

[0056] In order to obtain polyphenylene ether with high efficiency, a method of increasing the drying temperature, a method of increasing the degree of vacuum in the drying atmosphere, a method of stirring during drying, and the like are effective, but a method of increasing the drying temperature is particularly preferable from the viewpoint of production efficiency. In the drying step, it is preferable to use a dryer equipped with a mixing function. Examples of the mixing function include a stirring type dryer and a rolling type dryer. This allows the processing amount to be increased, and the productivity to be maintained at a high level.

[0057] The polyphenylene ether of this embodiment can also be produced by a redistribution reaction in which a polyphenylene ether derived from a phenol of formula (1) is equilibrated with a phenolic compound of formula (2) in the presence of an oxidizing agent. Redistribution reactions are known in the art and are described, for example, in U.S. Patent No. 3,496,236 to Cooper et al. and U.S. Patent No. 5,880,221 to Liska et al.

[0058] (Modification reaction process) There is no limitation on the method of introducing a functional group into the hydroxyl group of the unmodified polyphenylene ether. For example, the functional group can be obtained by an ester bond formation reaction between the hydroxyl group of the unmodified polyphenylene ether and a carboxylic acid having a carbon-carbon double bond (hereinafter, carboxylic acid). Various known methods can be used to form the ester bond. For example, a. reaction between a carboxylic acid halide and a hydroxyl group at the polymer terminal, b. formation of an ester bond by reaction with a carboxylic acid anhydride, c. direct reaction with a carboxylic acid, d. a method using an ester exchange reaction, etc. are listed. The reaction with a carboxylic acid halide is one of the most common methods. As the carboxylic acid halide, chlorides and bromides are generally used, but other halogens may also be used. The reaction may be either a direct reaction with a hydroxyl group or a reaction with an alkali metal salt of a hydroxyl group. Since an acid such as hydrogen halide is generated in the direct reaction between a carboxylic acid halide and a hydroxyl group, a weak base such as an amine may be coexisted in order to trap the acid. In the reaction with a carboxylic anhydride of b or the direct reaction with a carboxylic acid of c, a compound such as a carbodiimide or dimethylaminopyridine may be allowed to coexist in order to activate the reaction site and promote the reaction. In the case of the transesterification reaction of d, it is desirable to remove the generated alcohols as necessary. In addition, known metal catalysts may be allowed to coexist in order to promote the reaction. After the reaction, in order to remove by-products such as amine salts, the reaction product may be washed with water, an acidic or alkaline aqueous solution, or the polymer solution may be dropped into a poor solvent such as an alcohol to recover the target product by reprecipitation. In addition, after washing the polymer solution, the solvent may be distilled off under reduced pressure to recover the polymer.

[0059] The method for producing the modified polyphenylene ether of the present embodiment is not limited to the method for producing the polyfunctional modified polyphenylene ether of the present embodiment described above, and the order and number of the above-mentioned oxidative polymerization step, copper extraction and by-product removal step, liquid-liquid separation step, and concentration and drying step may be appropriately adjusted.

[0060] (Polyphenylene ether solution) The polyphenylene ether solution of the present embodiment contains at least the polyphenylene ether of the present embodiment and a ketone-based solvent, and may further contain other components. In addition, the solution may contain a solvent other than the ketone-based solvent. Examples of the ketone solvent include acetone, methyl ethyl ketone, methyl propyl ketone, methyl isobutyl ketone, diisobutyl ketone, and cyclohexanone. The ratio of the total mass of the polyphenylene ether and the ketone-based solvent to 100 mass% of the polyphenylene ether solution is preferably 80 mass% or more, more preferably 90 mass% or more, even more preferably 95 mass% or more, and particularly preferably 100 mass%. The mass ratio of the polyphenylene ether to 100% by mass of the polyphenylene ether solution is preferably 1 to 40% by mass, and the mass ratio of the ketone solvent to 100% by mass of the polyphenylene ether solution is preferably 60 to 99% by mass. The polyphenylene ether solution can be produced, for example, by mixing the polyphenylene ether, the ketone solvent, and any other components, other solvents, and the like.

[0061] <Thermosetting composition> The polyphenylene ether of this embodiment can be used as a raw material for a thermosetting composition. The thermosetting composition is not particularly limited as long as it contains polyphenylene ether, but it is preferable that the thermosetting composition further contains a crosslinking agent and an organic peroxide, and if desired, it can further contain a thermoplastic resin, a flame retardant, other additives, a silica filler, a solvent, etc. The components of the thermosetting composition of this embodiment will be described below.

[0062] (Polyphenylene ether) As described above, the polyphenylene ether of the present embodiment may be used as a sole resin in the thermosetting composition, or may be used in combination with polyphenylene ethers having other structures, or may be used in combination with various known additives. When used in combination with other components, the content of polyphenylene ether in the thermosetting composition is preferably 0.5 to 95 mass %, more preferably 20 to 93 mass %, and even more preferably 40 to 90 mass %.

[0063] (Crosslinking agent) Any crosslinking agent capable of initiating or facilitating a crosslinking reaction can be used in the thermosetting composition of the present embodiments. The crosslinking agent preferably has a number average molecular weight of not more than 4000. When the number average molecular weight of the crosslinking agent is not more than 4000, an increase in the viscosity of the thermosetting composition can be suppressed, and good resin fluidity can be obtained during heat molding. The number average molecular weight may be a value measured by a general molecular weight measurement method, specifically, a value measured by GPC, etc.

[0064] From the viewpoint of the crosslinking reaction, the crosslinking agent preferably has an average of two or more carbon-carbon unsaturated double bonds per molecule. The crosslinking agent may be composed of one type of compound or two or more types of compounds. In addition, the term "carbon-carbon unsaturated double bond" as used herein refers to a double bond located at an end branched from the main chain when the crosslinking agent is a polymer or oligomer. An example of the carbon-carbon unsaturated double bond is a 1,2-vinyl bond in polybutadiene.

[0065] When the number average molecular weight of the crosslinking agent is less than 600, the number (average value) of carbon-carbon unsaturated double bonds per molecule of the crosslinking agent is preferably 2 to 4. When the number average molecular weight of the crosslinking agent is 600 or more and less than 1,500, the number (average value) of carbon-carbon unsaturated double bonds per molecule of the crosslinking agent is preferably 4 to 26. When the number average molecular weight of the crosslinking agent is 1,500 or more and less than 4,000, the number (average value) of carbon-carbon unsaturated double bonds per molecule of the crosslinking agent is preferably 26 to 60. When the number average molecular weight of the crosslinking agent is within the above range, the number of carbon-carbon unsaturated double bonds is equal to or more than the specific value, so that the thermosetting composition of this embodiment has a higher reactivity of the crosslinking agent and a higher crosslink density of the cured product of the thermosetting composition, and as a result, it can provide better heat resistance. On the other hand, when the number average molecular weight of the crosslinking agent is within the above range, the number of carbon-carbon unsaturated double bonds is equal to or less than the specific value, so that it can provide better resin fluidity during hot molding.

[0066] Examples of the crosslinking agent include trialkenyl isocyanurate compounds such as triallyl isocyanurate (TAIC), trialkenyl cyanurate compounds such as triallyl cyanurate (TAC), polyfunctional methacrylate compounds having two or more methacrylic groups in the molecule, polyfunctional acrylate compounds having two or more acrylic groups in the molecule, polyfunctional vinyl compounds having two or more vinyl groups in the molecule such as polybutadiene, vinylbenzyl compounds such as divinylbenzene having a vinylbenzyl group in the molecule, and polyfunctional maleimide compounds having two or more maleimide groups in the molecule such as 4,4'-bismaleimide diphenylmethane. These crosslinking agents are used alone or in combination of two or more. Of these, the crosslinking agent preferably contains at least one compound selected from the group consisting of triallyl cyanurate, triallyl isocyanurate, and polybutadiene. When the crosslinking agent contains at least one or more of the compounds described above, the thermosetting composition has better compatibility between the crosslinking agent and the polyphenylene ether, and better coatability, and when mounted on an electronic circuit board, the board properties tend to be better.

[0067] The mass ratio of polyphenylene ether to the crosslinking agent (polyphenylene ether:crosslinking agent) is preferably 25:75 to 95:5, and more preferably 32:68 to 85:15, from the viewpoints of improving the compatibility between the crosslinking agent and the modified polyphenylene ether, the coatability of the thermosetting composition, and achieving even better properties of the mounted electronic circuit board.

[0068] (organic peroxide) In this embodiment, any organic peroxide capable of promoting the polymerization reaction of the thermosetting composition comprising the polyphenylene ether and the crosslinking agent can be used. Examples of organic peroxides include benzoyl peroxide, cumene hydroperoxide, 2,5-dimethylhexane-2,5-dihydroperoxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexyne-3, di-t-butyl peroxide, t-butylcumyl peroxide, di(2-t-butylperoxyisopropyl)benzene, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, dicumyl peroxide, di-t-butylperoxyisophthalate, t-butylperoxybenzoate, 2,2-bis(t-butylperoxy)butane, 2,2-bis(t-butylperoxy)octane, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, di(trimethylsilyl)peroxide, and trimethylsilyltriphenylsilyl peroxide. Radical generators such as 2,3-dimethyl-2,3-diphenylbutane can also be used as reaction initiators for thermosetting compositions. Among them, 2,5-dimethyl-2,5-di(t-butylperoxy)hexyne-3, di(2-t-butylperoxyisopropyl)benzene, and 2,5-dimethyl-2,5-di(t-butylperoxy)hexane are preferred from the viewpoint of providing a cured product having excellent heat resistance and mechanical properties and a low dielectric tangent (and preferably a low dielectric constant).

[0069] The one-minute half-life temperature of the organic peroxide is preferably 155 to 185° C., more preferably 160 to 180° C., and even more preferably 165 to 175° C. When the one-minute half-life temperature of the organic peroxide is within the range of 155 to 185° C., the compatibility of the organic peroxide with the modified PPE, the coatability of the thermosetting composition, and the properties of the mounted electronic circuit board tend to be further improved. In this specification, the one-minute half-life temperature is the temperature at which the organic peroxide decomposes and the amount of active oxygen is reduced to half in one minute. The one-minute half-life temperature is a value confirmed by a method in which an organic peroxide is dissolved in a solvent inactive against radicals, such as benzene, to a concentration of 0.05 to 0.1 mol / L, and the organic peroxide solution is thermally decomposed in a nitrogen atmosphere.

[0070] Examples of organic peroxides having a one-minute half-life temperature in the range of 155 to 185°C include t-hexylperoxyisopropyl monocarbonate (155.0°C), t-butylperoxy-3,5,5-trimethylhexanoate (166.0°C), t-butylperoxylaurate (159.4°C), t-butylperoxyisopropyl monocarbonate (158.8°C), t-butylperoxy2-ethylhexyl monocarbonate (161.4°C), t-hexylperoxybenzoate (160.3°C), 2,5-dimethyl-2,5-di(benzoylperoxy)hexane (158.2°C), and the like. ), t-butyl peroxyacetate (159.9°C), 2,2-di-(t-butylperoxy)butane (159.9°C), t-butyl peroxybenzoate (166.8°C), n-butyl 4,4-di-(t-butylperoxy)valerate (172.5°C), di(2-t-butylperoxyisopropyl)benzene (175.4°C), dicumyl peroxide (175.2°C), di-t-hexyl peroxide (176.7°C), 2,5-dimethyl-2,5-di(t-butylperoxy)hexane (179.8°C), and t-butylcumyl peroxide (173.3°C).

[0071] The content of the organic peroxide, based on 100 parts by mass in total of the polyphenylene ether and the crosslinking agent, is preferably 0.05 parts by mass or more, more preferably 0.5 parts by mass or more, even more preferably 1 part by mass or more, and still more preferably 1.5 parts by mass or more, from the viewpoint of achieving even better compatibility between the organic peroxide and the modified PPE and even better coatability of the thermosetting composition; and is preferably 5 parts by mass or less, more preferably 4.5 parts by mass or less, from the viewpoint of achieving excellent board properties when the thermosetting composition is mounted on an electronic circuit board.

[0072] (thermoplastic resin) The thermoplastic resin is preferably at least one selected from the group consisting of a block copolymer of a vinyl aromatic compound and an olefin-based alkene compound and a hydrogenated product thereof (a hydrogenated block copolymer obtained by hydrogenating a block copolymer of a vinyl aromatic compound and an olefin-based alkene compound), and a homopolymer of a vinyl aromatic compound. From the viewpoint of achieving better compatibility with polyphenylene ether, resin fluidity, coatability of the thermosetting composition, and heat resistance during curing, the weight average molecular weight of the thermoplastic resin is preferably more than 50,000 and not more than 780,000, more preferably 60,000 to 750,000, and even more preferably 70,000 to 700,000. When the thermosetting composition contains polyphenylene ether, a crosslinking agent, an organic peroxide, and a thermoplastic resin having the type and weight-average molecular weight described above, the compatibility of the modified PPE with the other components and the coatability onto substrates tend to be good, and thus the substrate properties when incorporated into an electronic circuit board may also be excellent. The weight average molecular weight can be determined by the method described in the Examples below.

[0073] The content of the vinyl aromatic compound-derived unit in the block copolymer or its hydrogenated product is preferably 20% by mass or more, more preferably 22% by mass or more, 24% by mass or more, 26% by mass or more, 28% by mass or more, 30% by mass or more, or 32% by mass or more. The upper limit is preferably 70% by mass or less, more preferably 69% by mass or less, 68% by mass or less, or 67% by mass or less. When the content of the vinyl aromatic compound-derived unit in the block copolymer or its hydrogenated product is 20 to 70% by mass, the compatibility with the modified polyphenylene ether tends to be further improved, and / or the adhesive strength with the metal foil tends to be further improved.

[0074] The vinyl aromatic compound may be any compound having an aromatic ring and a vinyl group in the molecule, and examples thereof include styrene. The olefin-based alkene compound may be any alkene having a linear or branched structure in the molecule, and examples thereof include ethylene, propylene, butylene, isobutylene, butadiene, and isoprene. From the viewpoint of having even better compatibility with polyphenylene ether, the thermoplastic resin is preferably at least one selected from the group consisting of styrene-butadiene block copolymers, styrene-ethylene-butadiene block copolymers, styrene-ethylene-butylene block copolymers, styrene-butadiene-butylene block copolymers, styrene-isoprene block copolymers, styrene-ethylene-propylene block copolymers, styrene-isobutylene block copolymers, hydrogenated styrene-butadiene block copolymers, hydrogenated styrene-ethylene-butadiene block copolymers, hydrogenated styrene-butadiene-butylene block copolymers, hydrogenated styrene-isoprene block copolymers, and homopolymers of styrene (polystyrene), and more preferably at least one selected from the group consisting of styrene-butadiene block copolymers, hydrogenated styrene-butadiene block copolymers, and polystyrene.

[0075] The hydrogenation rate in the hydrogenated product is not particularly limited, and some of the carbon-carbon unsaturated double bonds derived from the olefin-based alkene compound may remain.

[0076] The content of the thermoplastic resin is preferably 2 to 20 parts by mass, more preferably 3 to 19 parts by mass, further preferably 4 to 18 parts by mass, and particularly preferably 5 to 17 parts by mass, based on 100 parts by mass of the total of the polyphenylene ether and the crosslinking agent. By having this content within the above numerical range, the thermosetting composition of the present embodiment has better compatibility between the thermoplastic resin and the modified polyphenylene ether and better coatability, and tends to have better board properties when mounted on an electronic circuit board.

[0077] The thermosetting composition of the present embodiment may also contain a thermoplastic resin other than the thermoplastic resin having the type and weight average molecular weight described above.

[0078] (Flame retardant) The thermosetting composition of the present embodiment preferably contains a flame retardant. The flame retardant is not particularly limited as long as it is incompatible with other components contained in the thermosetting composition after the thermosetting composition is cured, from the viewpoint of improving heat resistance. Preferably, the flame retardant is incompatible with the polyphenylene ether and / or the crosslinking agent in the thermosetting composition after the thermosetting composition is cured. Examples of the flame retardant include inorganic flame retardants such as antimony trioxide, aluminum hydroxide, magnesium hydroxide, and zinc borate; aromatic bromine compounds such as hexabromobenzene, decabromodiphenylethane, 4,4-dibromobiphenyl, and ethylene bistetrabromophthalimide; and phosphorus-based flame retardants such as resorcinol bis-diphenyl phosphate and resorcinol bis-dixylenyl phosphate. These flame retardants may be used alone or in combination of two or more. Among these, the flame retardant is preferably decabromodiphenylethane from the viewpoints of compatibility between the flame retardant and the modified PPE, coatability of the thermosetting composition, and superior properties of the mounted electronic circuit board.

[0079] The content of the flame retardant is not particularly limited, but from the viewpoint of maintaining flame retardancy at the V-0 level of UL Standard 94, it is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 15 parts by mass or more, relative to 100 parts by mass of the total of the polyphenylene ether and the crosslinking agent. Moreover, from the viewpoint of maintaining a low dielectric tangent of the obtained cured product (preferably also maintaining a low dielectric constant), the content of the flame retardant is preferably 50 parts by mass or less, more preferably 45 parts by mass or less, and even more preferably 40 parts by mass or less.

[0080] (Silica filler) The thermosetting composition of the present embodiment may contain a silica filler. Examples of the silica filler include natural silica, fused silica, synthetic silica, amorphous silica, aerosil, and hollow silica. The content of the silica filler may be 10 to 100 parts by mass relative to 100 parts by mass of the total of the polyphenylene ether and the crosslinking agent. The silica filler may be surface-treated with a silane coupling agent or the like.

[0081] The thermosetting composition of the present embodiment may further contain additives such as a heat stabilizer, an antioxidant, a UV absorber, a surfactant, and a lubricant, a solvent, and the like, in addition to the flame retardant and silica filler. When the thermosetting composition of the present embodiment contains a solvent, it can be in the form of a varnish in which the solid components in the thermosetting composition are dissolved or dispersed in the solvent, and a resin film can be formed from the thermosetting composition of the present embodiment.

[0082] (solvent) From the viewpoint of solubility, the solvent is preferably an aromatic compound such as toluene or xylene, methyl ethyl ketone (MEK), cyclopentanone, cyclohexanone, chloroform, etc. These solvents may be used alone or in combination of two or more.

[0083] <Prepreg> The prepreg of the present embodiment includes a substrate and the thermosetting composition of the present embodiment described above, and is preferably a composite including the substrate and the thermosetting composition of the present embodiment impregnated or applied to the substrate. The prepreg can be obtained, for example, by impregnating a substrate such as a glass cloth with a varnish of the thermosetting composition, and then drying and removing the solvent with a hot air dryer or the like.

[0084] Examples of the substrate include various glass cloths such as roving cloth, cloth, chopped mat, and surfacing mat; asbestos cloth, metal fiber cloth, and other synthetic or natural inorganic fiber cloths; woven or nonwoven fabrics obtained from liquid crystal fibers such as fully aromatic polyamide fibers, fully aromatic polyester fibers, and polybenzoxazole fibers; natural fiber cloths such as cotton cloth, linen cloth, and felt; natural cellulose-based substrates such as carbon fiber cloth, craft paper, cotton paper, and cloth obtained from paper-glass mixed fiber yarn; and polytetrafluoroethylene porous films. Among these, glass cloth is preferable. These substrates may be used alone or in combination of two or more.

[0085] The proportion of the solid content of the thermosetting composition of this embodiment in the prepreg (components other than the solvent of the thermosetting composition) is preferably 30 to 80 mass %, more preferably 40 to 70 mass %. When the proportion is 30 mass % or more, the insulation reliability tends to be more excellent when the prepreg is used for electronic boards, etc. When the proportion is 80 mass % or less, the mechanical properties such as flexural modulus tend to be more excellent in applications such as electronic boards.

[0086] <Laminate> The laminate of the present embodiment includes the cured product of the prepreg of the present embodiment and a metal foil, and is preferably a metal-clad laminate obtained by laminating and curing the thermosetting composition of the present embodiment or the prepreg of the present embodiment and the metal foil. The metal-clad laminate preferably has a configuration in which the cured product of the prepreg (hereinafter also referred to as a "cured product composite") and the metal foil are laminated and adhered to each other, and is suitably used as a material for electronic substrates. Examples of the metal foil include aluminum foil and copper foil. Among these, copper foil is preferred because of its low electrical resistance. The cured composite to be combined with the metal foil may be one or more sheets, and depending on the application, the composite is processed into a laminate by overlaying metal foil on one or both sides thereof.

[0087] Examples of methods for producing a metal-clad laminate include a method in which a composite (e.g., the above-mentioned prepreg) is formed from a thermosetting composition and a substrate, this is layered with metal foil, and the thermosetting composition is cured to obtain a laminate in which the cured laminate and the metal foil are laminated together. One particularly preferred application of the metal-clad laminate is a printed wiring board, which is preferably formed by removing at least a portion of the metal foil from the metal-clad laminate.

[0088] <Printed wiring board> At least a part of the metal foil can be removed from the metal-clad laminate to form a printed wiring board. The printed wiring board can typically be formed by a method of pressurizing and hot molding using the prepreg of the present embodiment described above. Examples of the substrate include the same as those described above for the prepreg. The printed wiring board contains the thermosetting composition of the present embodiment, and thus has excellent heat resistance and electrical properties (low dielectric tangent and / or low dielectric constant), can suppress fluctuations in electrical properties due to environmental changes, and has excellent insulation reliability and mechanical properties. EXAMPLES

[0089] Hereinafter, the present embodiment will be described in more detail based on examples, but the present embodiment is not limited to the following examples.

[0090] First, the measurement methods and evaluation criteria for each physical property will be described below.

[0091] (1) The molar ratio of the repeating units derived from phenol of formula (1) or formula (2) to the total of the repeating units derived from phenol of formula (1) and the repeating units derived from phenol of formula (2) contained in the unmodified polyphenylene ether The unmodified polyphenylene ether obtained in the Examples and Comparative Examples was dissolved in deuterated chloroform, and tetramethylsilane was used as an internal standard. 1H-NMR measurement (JEOL 500MHz) was performed. Prior to the measurement, the polyphenylene ether was kept at 140°C and 1mmHg for 8 hours to remove volatile components such as toluene and water, and the measurement was performed as dry unmodified polyphenylene ether. The signals of the units derived from phenol in formula (1) and formula (2) were identified, and the respective proportions were calculated. For example, in the unmodified polyphenylene ethers obtained in the Examples and Comparative Examples, the signal derived from the repeating unit derived from phenol of formula (1), i.e., the 2,6-dimethylphenol-derived structure (2,6-dimethylphenylene unit), and the signal derived from the repeating unit derived from phenol of formula (2), i.e., the 2-tert-butyl-5-methylphenol-derived structure (2-tert-butyl-5-methylphenylene unit), were assigned as follows. The peaks of the repeating units derived from each phenol appear in the following regions. Peaks derived from hydrogen atoms of the methyl groups of the 2,6-dimethylphenylene unit and the 2-tert-butyl-5-methylphenylene unit (6H and 3H, respectively): 1.60 to 2.50 ppm (excluding peaks derived from hydrogen atoms of the methyl group of toluene) Peaks (9H) derived from hydrogen atoms of the tert-butyl group of the 2-tert-butyl-5-methylphenylene unit: 1.00 to 1.52 ppm (excluding peaks derived from hydrogen atoms of water) The integral value of the above signal is examined, and the integral value per proton of the peak derived from the hydrogen atom of the methyl group of the 2,6-dimethylphenylene unit can be calculated using the following formula (1). E = {C - 3 × (D / 9)} / 6 Formula (1) C: Integration value of the peaks derived from the methyl of the 2,6-dimethylphenylene unit and the 2-tert-butyl-5-methylphenylene unit D: Integration value of the peak derived from the tert-butyl of the 2-tert-butyl-5-methylphenylene unit E: integral per proton of the peak derived from the methyl of the 2,6-dimethylphenylene unit Furthermore, the proportion (mol %) of the repeating units derived from the phenol of formula (1) or formula (2) can be calculated using the following formulas (2) and (3). Proportion of repeating units derived from phenol in formula (1) (mol%) = E / {(D / 9) + E} × 100 ··· Formula (2) Proportion (mol%) of repeating units derived from phenol in formula (2) = (D / 9) / {(D / 9)+E}×100 Formula (3)

[0092] (2) The molar ratio of the repeating unit derived from impurity A to the total of the repeating unit derived from phenol of formula (1), the repeating unit derived from phenol of formula (2), and the repeating unit derived from impurity A contained in the unmodified polyphenylene ether. The unmodified polyphenylene ether obtained in the Examples and Comparative Examples was dissolved in deuterated chloroform, and tetramethylsilane was used as an internal standard. 1 H-NMR measurement (JEOL 500MHz) was performed. Prior to the measurement, the polyphenylene ether was kept at 140°C and 1mmHg for 8 hours to remove volatile components such as toluene and water, and the measurement was performed as dry unmodified polyphenylene ether. The signals of the units derived from phenol in formula (1), formula (2), and impurity A were identified, and their respective proportions were calculated. For example, in the unmodified polyphenylene ether obtained in the examples and comparative examples, a signal derived from a repeating unit derived from phenol of formula (1), i.e., a structure derived from 2,6-dimethylphenol (2,6-dimethylphenylene unit), a signal derived from a repeating unit derived from phenol of formula (2), i.e., a structure derived from 2-tert-butyl-5-methylphenol (2-tert-butyl-5-methylphenylene unit), and a signal derived from a repeating unit derived from impurity A, i.e., R 11 = methyl group, R 12 The assignment of signals derived from the repeating unit with z=hydrogen atom and z=0 was analyzed as follows. The peaks of the repeating units derived from each phenol appear in the following regions. 2,6-dimethylphenylene unit, 2-tert-butyl-5-methylphenylene unit, and R in formula (11) 11 = methyl group, R 12 = hydrogen atom, peaks derived from the hydrogen atoms of the methyl groups of the signals derived from the repeating unit where z = 0 (6H, 3H, and 12H, respectively): 1.60 to 2.50 ppm (excluding the peaks derived from the hydrogen atoms of the methyl groups of toluene) Peaks (9H) derived from hydrogen atoms of the tert-butyl group of the 2-tert-butyl-5-methylphenylene unit: 1.00 to 1.52 ppm (excluding peaks derived from hydrogen atoms of water) R in Equation (11) 11 = methyl group, R 12 = hydrogen atom, peak due to hydrogen atom of methyl group of repeating unit where z = 0 (4H): 7.35 ppm The integral value of the above signal is examined, and the integral value per proton of the peak derived from the hydrogen atom of the methyl group of the 2,6-dimethylphenylene unit can be calculated using the following formula (4). E = {C - 3 × (D / 9) - 12 × (F / 4)} / 6 Formula (4) C: Integration value of the peaks derived from the methyl of the 2,6-dimethylphenylene unit and the 2-tert-butyl-5-methylphenylene unit D: Integration value of the peak derived from the tert-butyl of the 2-tert-butyl-5-methylphenylene unit F: R in formula (11) 11 = methyl group, R 12 = hydrogen atom, integral value of the peak due to hydrogen atoms in the benzene ring of the repeating unit where z=0 E: integral per proton of the peak derived from the methyl of the 2,6-dimethylphenylene unit Furthermore, according to the following formula (5), R in formula (11) 11 = methyl group, R 12 = hydrogen atom, and the proportion (mol%) of structures where z=0 can be calculated. R in Equation (11) 11 = methyl group, R 12= Proportion of repeating units with hydrogen atoms and z=0 (mol%) = (F / 4) / {(D / 9)+E+(F / 4)}×100 Formula (5)

[0093] (3) The molar ratio of repeating units derived from a monohydric phenol having at least one unsaturated hydrocarbon group on a carbon atom in the ortho position to the carbon atom to which the hydroxyl group of the phenol is bonded to the sum of repeating units derived from the phenol of formula (1) contained in the unmodified polyphenylene ether and repeating units derived from the monohydric phenol having at least one unsaturated hydrocarbon group on a carbon atom in the ortho position to the carbon atom to which the hydroxyl group of the phenol is bonded. The unmodified polyphenylene ether obtained in the Examples and Comparative Examples was dissolved in deuterated chloroform, and tetramethylsilane was used as an internal standard. 1 H-NMR measurements (JEOL 500MHz) were performed. Prior to the measurements, the polyphenylene ether was kept at 140°C and 1mmHg for 8 hours to remove volatile components such as toluene and water, and the measurements were performed as dry, unmodified polyphenylene ether. The signals of the repeating unit derived from phenol of formula (1), the repeating unit derived from phenol of formula (2), and the repeating unit derived from a monohydric phenol having at least one unsaturated hydrocarbon group on the carbon atom ortho to the carbon atom to which the hydroxyl group of the phenol is bonded were identified, and the respective proportions were calculated. For example, in the unmodified polyphenylene ethers obtained in the Examples and Comparative Examples, a signal derived from a repeating unit derived from a phenol of formula (1), i.e., a structure derived from 2,6-dimethylphenol (2,6-dimethylphenylene unit), a signal derived from a repeating unit derived from a phenol of formula (2), i.e., a structure derived from 2-tert-butyl-5-methylphenol (2-tert-butyl-5-methylphenylene unit), and a signal derived from a repeating unit derived from a monohydric phenol having at least one unsaturated hydrocarbon group on a carbon atom in the ortho position to the carbon atom to which the hydroxyl group of the phenol is bonded, i.e., a structure derived from 2-allylphenol (2-allylphenylene unit), appear in the following regions. Peaks derived from hydrogen atoms of the methyl groups of the 2,6-dimethylphenylene unit and the 2-tert-butyl-5-methylphenylene unit (6H and 3H, respectively): 1.60 to 2.50 ppm (excluding peaks derived from hydrogen atoms of the methyl group of toluene) Peaks (9H) derived from hydrogen atoms of the tert-butyl group of the 2-tert-butyl-5-methylphenylene unit: 1.00 to 1.52 ppm (excluding peaks derived from hydrogen atoms of water) Peak due to hydrogen atoms of methylene groups of 2-allylphenylene units (2H): 3.40 ppm The integral value of the above signal is examined, and the integral value per proton of the peak derived from the hydrogen atom of the methyl group of the 2,6-dimethylphenylene unit can be calculated using the following formula (6). E = {C - 3 × (D / 9)} / 6 Formula (6) C: Integration value of the peaks derived from the methyl of the 2,6-dimethylphenylene unit and the 2-tert-butyl-5-methylphenylene unit D: Integration value of the peak derived from the tert-butyl of the 2-tert-butyl-5-methylphenylene unit E: integral per proton of the peak derived from the methyl of the 2,6-dimethylphenylene unit Furthermore, the proportion (mol %) of 2-allylphenylene units can be calculated using the following formula (7). Proportion of 2-allylphenylene units (mol%) = (G / 2) / {E+(G / 2)}×100 Formula (7) G: integral per proton of the peak derived from the methylene group of the 2-allylphenylene unit

[0094] (4) The molar ratio of the repeating units derived from phenol of formula (1) or formula (2) to the total of the repeating units derived from phenol of formula (1) and the repeating units derived from phenol of formula (2) contained in the modified polyphenylene ether. The modified polyphenylene ether was prepared as follows. The modified polyphenylene ether obtained in the examples and comparative examples was dissolved in a measurement solvent (deuterated chloroform with one drop of deuterium oxide added to eliminate the hydroxyl group), and tetramethylsilane was used as an internal standard. 1 H-NMR measurement (JEOL 500MHz) was performed. Prior to the measurement, the polyphenylene ether was kept at 80°C and 1mmHg for 8 hours to remove volatile components such as toluene and water, and the measurement was performed as a dry modified polyphenylene ether. The signals of the units derived from phenol in formula (1) and formula (2) were identified, and their respective proportions were calculated. For example, in the modified polyphenylene ethers obtained in the Examples and Comparative Examples, the signal derived from the repeating unit derived from phenol of formula (1), i.e., the 2,6-dimethylphenol-derived structure (2,6-dimethylphenylene unit), the signal derived from the repeating unit derived from phenol of formula (2), i.e., the 2-tert-butyl-5-methylphenol-derived structure (2-tert-butyl-5-methylphenylene unit), and the signal derived from a partial structure selected from the group consisting of formula (4), formula (5), formula (6), or formula (7), i.e., the signal derived from a methacryl group-derived structure, were assigned as follows. The peaks of the repeating units derived from each phenol appear in the following regions. Peaks derived from hydrogen atoms of the 2,6-dimethylphenylene unit, 2-tert-butyl-5-methylphenylene unit, and methyl group of the methacryl group (6H, 3H, and 3H, respectively): 1.60 to 2.50 ppm (excluding peaks derived from hydrogen atoms of the methyl group of toluene) Peaks (9H) derived from hydrogen atoms of the tert-butyl group of the 2-tert-butyl-5-methylphenylene unit: 1.00 to 1.52 ppm (excluding peaks derived from hydrogen atoms of water) Peak due to one hydrogen atom of the methylene group of the methacryl group (1H): 4.4-5.8 ppm The integral value of the above signal is examined, and the integral value per proton of the peak derived from the hydrogen atom of the methyl group of the 2,6-dimethylphenylene unit can be calculated using the following formula (8). E = {C - 3 × (D / 9) - 3 × (H / 1)} / 6 Formula (8) C: Integration value of the peaks derived from the methyl of the 2,6-dimethylphenylene unit and the 2-tert-butyl-5-methylphenylene unit D: Integration value of the peak derived from the tert-butyl of the 2-tert-butyl-5-methylphenylene unit E: integral per proton of the peak derived from the methyl of the 2,6-dimethylphenylene unit H: Integral value of the peak derived from one hydrogen atom of the methylene group of the methacryl group Furthermore, the proportion (mol %) of the repeating units derived from the phenol of formula (1) or (2) can be calculated using the following formulas (9) and (10). Proportion of repeating units derived from phenol in formula (1) (mol%) = E / {(D / 9) + E} × 100 Formula (9) Proportion (mol%) of repeating units derived from phenol in formula (2) = (D / 9) / {(D / 9)+E}×100 Formula (10)

[0095] (5) The molar ratio of the repeating unit derived from impurity A to the total of the repeating unit derived from phenol of formula (1), the repeating unit derived from phenol of formula (2), and the repeating unit derived from impurity A contained in the modified polyphenylene ether. The unmodified polyphenylene ether obtained in the examples and comparative examples was dissolved in a measurement solvent (deuterated chloroform to which one drop of heavy water was added to eliminate the hydroxyl group), and tetramethylsilane was used as an internal standard. 1 H-NMR measurement (JEOL 500MHz) was performed. Prior to the measurement, the polyphenylene ether was kept at 80°C and 1mmHg for 8 hours to remove volatile components such as toluene and water, and the measurement was performed as dry unmodified polyphenylene ether. The signals of the units derived from phenol in formula (1), formula (2), and impurity A were identified, and their respective proportions were calculated. For example, in the unmodified polyphenylene ether obtained in the examples and comparative examples, a signal derived from a repeating unit derived from phenol of formula (1), i.e., a 2,6-dimethylphenol-derived structure (2,6-dimethylphenylene unit), a signal derived from a repeating unit derived from phenol of formula (2), i.e., a 2-tert-butyl-5-methylphenol-derived structure (2-tert-butyl-5-methylphenylene unit), a signal derived from a partial structure selected from the group consisting of formula (4), formula (5), formula (6) or formula (7), i.e., a signal derived from a methacryl group-derived structure, and a signal derived from a repeating unit derived from impurity A, i.e., R 11 = methyl group, R 12 The assignment of signals derived from the repeating unit with z=hydrogen atom and z=0 was analyzed as follows. The peaks of the repeating units derived from each phenol appear in the following regions. 2,6-dimethylphenylene unit, 2-tert-butyl-5-methylphenylene unit, R in formula (11) 11 = methyl group, R 12 = Hydrogen atom, repeating unit where z = 0, peaks derived from hydrogen atoms of methyl groups of signals derived from methacryl groups (6H, 3H, 12H, and 3H, respectively): 1.60 to 2.50 ppm (excluding peaks derived from hydrogen atoms of methyl groups of toluene) Peaks (9H) derived from hydrogen atoms of the tert-butyl group of the 2-tert-butyl-5-methylphenylene unit: 1.00 to 1.52 ppm (excluding peaks derived from hydrogen atoms of water) R in Equation (11) 11 = methyl group, R 12 = hydrogen atom, peak due to hydrogen atom of methyl group of repeating unit where z = 0 (4H): 7.35 ppm Peak due to one hydrogen atom of the methylene group of the methacryl group (1H): 4.4-5.8 ppm The integral value of the above signal is examined, and the integral value per proton of the peak derived from the hydrogen atom of the methyl group of the 2,6-dimethylphenylene unit can be calculated using the following formula (11). E = {C - 3 × (D / 9) - 12 × (F / 4) - 3 × (H / 1)} / 6 Formula (11) C: Integration value of the peaks derived from the methyl of the 2,6-dimethylphenylene unit and the 2-tert-butyl-5-methylphenylene unit D: Integration value of the peak derived from the tert-butyl of the 2-tert-butyl-5-methylphenylene unit F: R in formula (11) 11 = methyl group, R 12 = hydrogen atom, integral value of the peak due to hydrogen atoms in the benzene ring of the repeating unit where z=0 E: integral per proton of the peak derived from the methyl of the 2,6-dimethylphenylene unit H: Integral value of the peak derived from one hydrogen atom of the methylene group of the methacryl group Furthermore, according to the following formula (12), R in formula (11) 11 = methyl group, R 12 = hydrogen atom, and the proportion (mol%) of structures where z=0 can be calculated. R in Equation (11) 11 = methyl group, R 12 = hydrogen atom, z=0 repeating unit ratio (mol%) = (F / 4) / {(D / 9)+E+(F / 4)}×100 Formula (12)

[0096] (6) Reduced viscosity (ηsp / c) A 0.5 g / dL chloroform solution of polyphenylene ether was prepared, and the reduced viscosity (ηsp / c) (dL / g) at 30° C. was determined using an Ubbelohde viscosity tube.

[0097] (7) Average number of hydroxyl groups in polyphenylene ether 5.0 mg of polyphenylene ether was weighed out. Then, this weighed polyphenylene ether was dissolved in 25 mL of methylene chloride. After adding 150 μL of 2 mass% tetraethylammonium hydroxide (TEAH) ethanol solution to 2.0 mL of the prepared solution, the absorbance (Abs) at 318 nm was measured using a UV spectrophotometer (Hitachi: U-3210 type) (using an absorbance measurement cell with a cell length of 1 cm). Then, based on the measurement results, the hydroxyl equivalent obtained from the absorbance was calculated by the following mathematical formula (13). In addition, the average number of hydroxyl groups per molecule of polyphenylene ether was calculated using the number average molecular weight (details are described in (8) below) obtained by gel permeation chromatography. Hydroxyl equivalent (g / mol) obtained from absorbance = [(ε × 5) / (25 × Abs)] Formula (13) (Here, ε is the extinction coefficient, which is 4700 L / mol cm.) Average number of hydroxyl groups per molecule of polyphenylene ether (groups / molecule) = (number average molecular weight obtained by gel permeation chromatography) / (hydroxyl equivalent obtained from absorbance) Formula (14)

[0098] (8) Number average molecular weight (Mn) As a measuring device, a gel permeation chromatography System 21 manufactured by Showa Denko K.K. was used, and a calibration curve was prepared using standard polystyrene and ethylbenzene, and the number average molecular weight (Mn) of the obtained modified polyphenylene ether was measured using this calibration curve. The standard polystyrenes used had molecular weights of 3,650,000, 2,170,000, 1,090,000, 681,000, 204,000, 52,000, 30,200, 13,800, 3,360, 1,300, and 550. The columns used were two Showa Denko K-805L columns connected in series. The solvent used was chloroform, with a solvent flow rate of 1.0 mL / min and a column temperature of 40°C. A 1 g / L chloroform solution of modified polyphenylene ether was prepared and used as the measurement sample. The UV wavelength of the detection unit was 254 nm for standard polystyrene and 283 nm for polyphenylene ether. The number average molecular weight (Mn) (g / mol) was calculated from the peak area ratio based on the curve showing the molecular weight distribution obtained by GPC based on the above measurement data.

[0099] (9) Long-term solubility in methyl ethyl ketone (MEK solubility) 1.5 g of polyphenylene ether and 8.5 g of methyl ethyl ketone were weighed into a transparent glass screw tube. They were mixed at 20°C using a stirrer and a magnetic stirrer. After one day, if the solution maintained its transparency, it was judged as "Good." If it was clearly not dissolved or if there was a large amount of insoluble matter, it was judged as "Poor." If there was some residual dissolution (some turbidity), it was judged as "△."

[0100] (10) Long-term solubility in toluene (TL solubility) 2 g of polyphenylene ether and 8 g of toluene were weighed into a transparent glass screw tube. They were mixed at 20°C using a stirrer and a magnetic stirrer. After one day, if the solution maintained its transparency, it was judged as "Good." If it was clearly not dissolved or if there was a large amount of insoluble matter, it was judged as "Poor." If there was some residual dissolution (some turbidity), it was judged as "△."

[0101] (11) Dielectric tangent of the cured product of the thermosetting composition The dielectric loss tangent at 10 GHz of the laminates manufactured in the examples and comparative examples was measured by a cavity resonance method. As a measuring device, a network analyzer (N5230A, manufactured by Agilent Technologies) and a cavity resonator (Cavity Resornator CP series) manufactured by Kanto Electronics Application Development Co., Ltd. were used. The laminates were cut into strips with a width of about 2 mm, a length of 50 mm, and a thickness of about 0.5 mm so that the warp of the glass cloth was the long side. Next, the laminates were placed in an oven at 105°C ± 2°C and dried for 2 hours, and then left to stand for 24 ± 5 ​​hours in an environment of 23°C and relative humidity of 50 ± 5%. Thereafter, the dielectric loss tangent was measured using the above measuring device in an environment of 23°C and relative humidity of 50 ± 5%.

[0102] The methods for producing polyphenylene ether in each of the Examples and Comparative Examples will be described below.

[0103] Example 1 A 40-liter jacketed polymerization tank equipped with a sparger, stirring turbine blades and baffles for introducing oxygen-containing gas at the bottom of the polymerization tank and a reflux condenser on the vent gas line at the top of the polymerization tank was charged with 2.4 g of cupric oxide, 18.1 g of 47% by mass aqueous hydrogen bromide solution, 5.8 g of di-t-butylethylenediamine, 28.1 g of di-n-butylamine, 85.6 g of butyldimethylamine, 17.9 kg of toluene, 1497 g of 2,6-dimethylphenol, and 503 g of 2-tert-butyl-5-methylphenol to obtain a homogeneous solution while blowing nitrogen gas at a flow rate of 17.1 L / min. Next, dry air was introduced into the polymerization tank from the sparger at a rate of 10.5 L / min to start polymerization. Dry air was aerated for 120 minutes to obtain a polymerization mixture. The internal temperature was controlled to be 20°C during polymerization. The polymerization mixture (polymerization liquid) at the end of polymerization was in a homogeneous solution state. The dry air flow was stopped, and 25.9 g of tetrasodium ethylenediaminetetraacetate (a reagent manufactured by Dojindo Laboratories) was added to the polymerization mixture as an aqueous solution in 2 kg of water. The polymerization mixture was stirred at 70° C. for 150 minutes, then allowed to stand for 20 minutes, and the organic phase and the aqueous phase were separated by liquid-liquid separation. The organic phase was concentrated by a rotary evaporator until the polymer concentration was 25% by mass. The above solution was mixed with methanol such that the ratio of methanol to polymer solution was 6, and polymer precipitation was performed. Wet polyphenylene ether was obtained by filtration under reduced pressure using a glass filter. The wet polyphenylene ether was further washed with an amount of methanol such that the ratio of methanol to wet polyphenylene ether was 3. The above washing operation was performed three times. Next, the wet polyphenylene ether was kept at 140°C and 1 mmHg for 120 minutes, and dry polyphenylene ether was obtained. The polyphenylene ether thus obtained was subjected to the respective measurements by the methods described above. The results of the respective analyses are shown in Table 1.

[0104] Example 2 The same operation as in Example 1 was carried out except that the phenol raw materials were 1269 g of 2,6-dimethylphenol and 731 g of 2-tert-butyl-5-methylphenol. The analytical results are shown in Table 1.

[0105] Example 3 The same procedure as in Example 1 was repeated except that the phenol raw materials were 853 g of 2,6-dimethylphenol and 1147 g of 2-tert-butyl-5-methylphenol. The analytical results are shown in Table 1.

[0106] Example 4 The same procedure as in Example 1 was repeated except that the phenol raw materials were 454 g of 2,6-dimethylphenol and 1517 g of 2-tert-butyl-5-methylphenol. The analytical results are shown in Table 1.

[0107] Example 5 The same operation as in Example 1 was carried out except that the phenol raw materials were 765 g of 2,6-dimethylphenol, 1142 g of 2-tert-butyl-5-methylphenol, and 93 g of 2-allylphenol. The analytical results are shown in Table 1.

[0108] Example 6 The same operation as in Example 1 was carried out except that the phenol raw materials were 503 g of 2,6-dimethylphenol, 1128 g of 2-tert-butyl-5-methylphenol, and 369 g of 2-allylphenol. The analytical results are shown in Table 1.

[0109] Example 7 Oxidative polymerization, copper extraction, liquid-liquid separation, and concentration by a rotary evaporator were carried out in the same manner as in Example 3, and the polymer solution having a polymer concentration of 25% by mass was used as a stock solution for the modification reaction. A 500mL three-neck flask equipped with a line for introducing nitrogen gas at the top of the reactor and a reflux condenser at the vent gas line at the top of the reactor was charged with 200g of unmodified polyphenylene ether solution and 0.64g of 4-dimethylaminopyridine after replacing the inside of the reactor with nitrogen. 21mL of triethylamine was added using a syringe while stirring. Then, 10.9mL of methacryloyl chloride was collected in a syringe and dropped into the system at room temperature. After the dropwise addition was completed, the flask was heated in an oil bath and stirring was continued at 90°C for 1 hour. Then, the reaction was continued under reflux by heating in an oil bath. Heating was stopped 4 hours after the start of reflux, and after returning to room temperature, 8g of methanol was added to stop the reaction. Next, the reaction solution was filtered using a glass filter to obtain a solution from which the by-product triethylammonium salt had been removed. The above solution was mixed with methanol in a ratio of 10 to the polymer solution, and the polymer was precipitated. Wet polyphenylene ether was obtained by vacuum filtration using a glass filter. The wet polyphenylene ether was further washed with an amount of methanol such that the ratio of methanol to wet polyphenylene ether was 2.5. The above washing operation was repeated three times. Next, the wet polyphenylene ether was kept at 100°C and 1 mmHg for 8 hours to obtain a dry polyphenylene ether. The average number of hydroxyl groups in the polyphenylene ether was measured by the above-mentioned method, and it was confirmed that the average number of hydroxyl groups derived from the polyphenylene ether was less than 0.2 per molecule. In addition, 1 By performing H NMR measurement and confirming the proton peak derived from the olefin of the methacryl group, it was determined that the hydroxyl group had been modified to a methacryl group. The analytical results are shown in Table 2.

[0110] Example 8 Oxidative polymerization, copper extraction, liquid-liquid separation, and concentration by a rotary evaporator were carried out in the same manner as in Example 3, and the polymer solution having a polymer concentration of 25% by mass was used as a stock solution for the modification reaction. In a 500 mL three-neck flask equipped with a temperature controller, a stirrer, a cooling device, and a dropping funnel, 200 g of the unmodified polyphenylene ether solution, 24 g of chloromethylstyrene (p-chloromethylstyrene and m-chloromethylstyrene in a ratio of 50 / 50, manufactured by Tokyo Chemical Industry Co., Ltd.), and 1.0 g of tetra-n-butylammonium bromide were added. The mixture was then stirred and dissolved, and the liquid temperature was adjusted to 85°C. A sodium hydroxide aqueous solution (4.2 g of sodium hydroxide / 104 g of water) was dropped into the mixture over 1 hour, and stirring was continued for another 5 hours at 85°C. Next, the obtained water layer was removed using a separatory funnel, and a toluene layer containing a polymer (polymer solution) was obtained. The polymer solution was mixed with methanol in a ratio of 10 to methanol, and the polymer was precipitated. Wet polyphenylene ether was obtained by filtration under reduced pressure using a glass filter. Furthermore, the wet polyphenylene ether was washed with a washing solvent (methanol:water=80:20) in an amount such that the ratio of the washing solvent (methanol:water=80:20) to the wet polyphenylene ether was 2.5. After the washing operation with the above-mentioned methanol-water mixed solvent was carried out three times, the wet polyphenylene ether was washed with an amount of methanol such that the ratio of methanol to the wet polyphenylene ether was 2.5. After the washing operation with the above-mentioned methanol was carried out twice, the wet polyphenylene ether was kept at 100°C and 1 mmHg for 8 hours to obtain a dry polyphenylene ether. The average number of hydroxyl groups of the polyphenylene ether was measured by the above-mentioned method, and it was confirmed that the average number of hydroxyl groups derived from the polyphenylene ether was less than 0.2 per molecule. In addition, 1 H NMR measurement confirmed the proton peaks derived from styryl groups at 5 to 7 ppm, and it was determined that the hydroxyl groups had been modified to styryl groups. The analytical results are shown in Table 2.

[0111] Example 9 The mixture was subjected to oxidation polymerization, copper extraction, liquid-liquid separation, and concentration by a rotary evaporator in the same manner as in Example 3, and then kept at 100° C. and 1 mmHg for 2 hours to obtain a dry polyphenylene ether. The dry polyphenylene ether was used as a raw material for the modification reaction. Into a 500 mL three-neck flask equipped with a temperature controller, a stirrer, a cooling device, and a dropping funnel, 50 g of unmodified polyphenylene ether, 150 g of tetrahydrofuran, 12.6 g of allyl bromide, and 0.8 g of benzyltributylammonium bromide were placed and stirred at a liquid temperature of 25° C. An aqueous sodium hydroxide solution (4.2 g of sodium hydroxide / 100 mL of water) was added dropwise to the mixture over 60 minutes, and stirring was continued at 25° C. for an additional 12 hours. Next, the contents of the flask were neutralized with a 10% aqueous hydrochloric acid solution, and then mixed with methanol such that the ratio of methanol to the polymer solution was 10, and the polymer was precipitated. Wet polyphenylene ether was obtained by filtration under reduced pressure using a glass filter. Furthermore, the wet polyphenylene ether was washed with a washing solvent (methanol:water=80:20) in an amount such that the ratio of the washing solvent (methanol:water=80:20) to the wet polyphenylene ether was 2.5. After the washing operation with the above-mentioned methanol-water mixed solvent was performed three times, the wet polyphenylene ether was washed with an amount of methanol such that the ratio of methanol to the wet polyphenylene ether was 2.5. After the washing operation with the above-mentioned methanol was performed twice, the wet polyphenylene ether was then kept at 100°C and 1 mmHg for 8 hours to obtain polyphenylene ether in a dry state. The average number of hydroxyl groups of the polyphenylene ether was measured by the above-mentioned method, and it was confirmed that the average number of hydroxyl groups derived from the polyphenylene ether was less than 0.2 per molecule. In addition, 1 1 H NMR measurement confirmed the proton peaks derived from allyl groups at 3.5 to 6.5 ppm, and it was determined that the hydroxyl groups had been modified to allyl groups. The analytical results are shown in Table 2.

[0112] Example 10 As in Example 5, oxidative polymerization, copper extraction, liquid-liquid separation, and concentration by a rotary evaporator were performed, and the mixture was further held at 100°C and 1 mmHg for 2 hours to obtain a dry polyphenylene ether. Methacrylic modification was performed as in Example 7, except that the dry polyphenylene ether was used as a raw material for the modification reaction. The average number of hydroxyl groups in the polyphenylene ether was measured by the above-mentioned method, and it was confirmed that the average number of hydroxyl groups derived from the polyphenylene ether was less than 0.2 per molecule. Also 1 By performing H NMR measurement and confirming the proton peak derived from the olefin of the methacryl group, it was determined that the hydroxyl group had been modified to a methacryl group. The analytical results are shown in Table 2.

[0113] Example 11 To 79 parts by mass of the polyphenylene ether described in Example 7, 20 parts by mass of TAIC (manufactured by Nippon Kasei Co., Ltd.) and 1 part by mass of organic peroxide (Perbutyl P, manufactured by NOF Corp.) were added to toluene, stirred and dissolved to obtain a varnish (solid content concentration 58% by mass). After impregnating L glass cloth (manufactured by Asahi Schwebel Co., Ltd., style: 2116) with this varnish, the excess varnish was scraped off by passing it through a specified slit, and the prepreg was obtained by drying for a specified time in a drying oven at 105°C and removing the toluene. This prepreg was cut to a specified size, and the solid content of the thermosetting composition in the prepreg was calculated by comparing the mass of the prepreg with the mass of a glass cloth of the same size, and was found to be 52% by mass. A predetermined number of these prepregs were stacked, and copper foil (GTS-MP foil, 35 μm thick, manufactured by Furukawa Electric Co., Ltd.) was placed on both sides of the stacked prepregs, and the resulting laminate was vacuum pressed to obtain a copper-clad laminate. In this vacuum pressing process, the laminate was first heated from room temperature at a temperature increase rate of 2°C / min while applying a pressure of 40 kg / cm. 2 After the temperature reached 200°C, the pressure was increased to 40 kg / cm while maintaining the temperature at 200°C. 2 and duration of 60 minutes were adopted. Next, the copper foil was removed from the copper-clad laminate by etching to obtain a laminate (thickness: about 0.5 mm). The analytical results are shown in Table 3.

[0114] Example 12 A laminate was obtained in the same manner as in Example 11, except that the polyphenylene ether described in Example 10 was used as the raw material. The analytical results are shown in Table 3.

[0115] Comparative Example 1 A 1.5-liter jacketed reactor equipped with a sparger for introducing an oxygen-containing gas at the bottom of the reactor, stirring turbine blades and baffles, and a reflux condenser on the vent gas line at the top of the reactor was charged with a mixture of 0.15 g of cuprous oxide and 1.12 g of 47% hydrogen bromide, 0.36 g of N,N'-di-t-butylethylenediamine, 5.31 g of dimethyl-n-butylamine, 1.74 g of di-n-butylamine, and 491.3 g of toluene, which had been previously prepared. Then, while vigorously stirring, air was introduced into the reactor from the sparger at a rate of 1.05 L / min, and oxygen was introduced at the same time. A mixed solution of 98.7 g of 2,6-dimethylphenol, 1.34 g of 2-tert-butyl-5-methylphenol, and 400.0 g of toluene was added to the solution over 60 minutes. The polymerization temperature was adjusted to maintain 40°C by passing a heat medium through the jacket. 130 minutes after the start of air introduction, the aeration was stopped, the inside of the reactor was replaced with nitrogen gas, and then a 20% methanol solution in which 1.03 g of hydroquinone (a reagent manufactured by Wako Pure Chemical Industries, Ltd.) was dissolved was added little by little. 30 minutes after the addition of the methanol solution of hydroquinone, 1.61 g of tetrasodium ethylenediaminetetraacetate tetrahydrate (a reagent manufactured by Dojindo Laboratories, Ltd.) was added as an aqueous solution of 200 g of water. The mixture was heated to 70°C, and copper extraction was carried out at 70°C for 2 hours. Thereafter, the mixture was separated into an unmodified polyphenylene ether solution (organic phase) and an aqueous phase to which the catalyst metal had been transferred by static separation. The above solution was mixed with methanol in a ratio of 10 to the polymer solution, and the polymer was precipitated. Wet polyphenylene ether was obtained by filtration under reduced pressure using a glass filter. Furthermore, the wet polyphenylene ether was washed with an amount of methanol in a ratio of 2.5 to the wet polyphenylene ether. The above washing operation was carried out three times. The wet polyphenylene ether was then kept at 140° C. and 1 mmHg for 120 minutes to obtain dry polyphenylene ether. The polyphenylene ether thus obtained was subjected to the respective measurements by the methods described above. The results of the respective analyses are shown in Table 1.

[0116] Comparative Example 2 The same procedure as in Example 1 was repeated except that the phenol raw materials were 1973 g of 2,6-dimethylphenol and 26.8 g of 2-tert-butyl-5-methylphenol. The analytical results are shown in Table 1.

[0117] Comparative Example 3 The same procedure as in Example 1 was repeated except that the phenol raw materials were 1740 g of 2,6-dimethylphenol and 260 g of 2-tert-butyl-5-methylphenol. The analytical results are shown in Table 1.

[0118] Comparative Example 4 A 40-liter jacketed polymerization tank equipped with a sparger, stirring turbine blades and baffles for introducing oxygen-containing gas at the bottom of the polymerization tank and a reflux condenser on the vent gas line at the top of the polymerization tank was charged with 4.57 g of cupric oxide, 24.18 g of 47% by mass aqueous hydrogen bromide solution, 11.00 g of di-t-butylethylenediamine, 62.72 g of di-n-butylamine, 149.92 g of butyldimethylamine, 20.65 kg of toluene, and 3.12 kg of 2,6-dimethylphenol while blowing nitrogen gas at a flow rate of 0.5 L / min, and stirred until a homogeneous solution was formed and the internal temperature of the polymerization tank reached 25 ° C. Next, dry air was introduced into the polymerization tank from the sparger at a rate of 32.8 NL / min to start polymerization. Dry air was aerated for 140 minutes to obtain a polymerization mixture. The internal temperature was controlled to be 40 ° C. during polymerization. At the end of the polymerization, the polymerization mixture (polymerization liquid) was in a homogeneous solution state. The supply of dry air was stopped, and 10 kg of a 2.5% by mass aqueous solution of tetrasodium ethylenediaminetetraacetate (a reagent manufactured by Dojindo Laboratories) was added to the polymerization mixture. The polymerization mixture was stirred at 70° C. for 150 minutes, then allowed to stand for 20 minutes, and separated into an organic phase and an aqueous phase by liquid-liquid separation. The separated organic phase was a toluene solution containing 13.1% by mass of polyphenylene ether. The above solution was placed in a jacketed stirring vessel, and a heat medium at 120°C was passed through the jacket to heat it. The generated steam, mainly composed of toluene, was cooled by a condenser, and the toluene was extracted from the system, and the polymer concentration in the stirring vessel was concentrated until it reached 30% by mass. Next, methanol was mixed so that the ratio of methanol to the polymer solution was 1.0, and the polymer was precipitated. Wet polyphenylene ether was obtained by filtration under reduced pressure using a glass filter. The wet polyphenylene ether was further washed with an amount of methanol such that the ratio of methanol to the wet polyphenylene ether was 2.5. The above washing operation was repeated three times. Next, the wet polyphenylene ether was kept at 140°C and 1 mmHg for 120 minutes, and dry polyphenylene ether was obtained. The polyphenylene ether thus obtained was subjected to the measurements by the methods described above. The measurement results are shown in Table 1.

[0119] Comparative Example 5 In a 40-liter jacketed polymerization tank equipped with a sparger, stirring turbine blades and baffles for introducing oxygen-containing gas at the bottom of the polymerization tank and a reflux condenser on the vent gas line at the top of the polymerization tank, 4.02 g of cupric oxide, 29.876 g of 47 mass% aqueous hydrogen bromide solution, 9.684 g of di-t-butylethylenediamine, 46.88 g of di-n-butylamine, 122.28 g of butyldimethylamine, 17.53 kg of toluene, and 1.5 kg of 2,6-dimethylphenol were added while blowing nitrogen gas at a flow rate of 0.5 L / min, and the mixture was stirred until a homogeneous solution was obtained and the internal temperature of the polymerization tank reached 25° C. Next, dry air was introduced into the polymerization tank from the sparger at a rate of 32.8 NL / min, and at the same time, a solution consisting of 1.62 kg of 2,6-dimethylphenol and 3.12 kg of toluene was added to the polymerization tank over 30 minutes from the plunger pump. Dry air was passed through for 86 minutes to obtain a polymerization mixture. The internal temperature was controlled to be 40°C during the polymerization. The polymerization mixture (polymerization liquid) at the end of the polymerization was in a homogeneous solution state. The same operation as in Comparative Example 1 was carried out. The analytical results are shown in Table 1.

[0120] Comparative Example 6 The same operation as in Example 1 was carried out, except that the phenol raw material was 2 kg of 2,6-dimethylphenol, and the air supply was stopped 117 minutes after the start of air introduction. The analytical results are shown in Table 1.

[0121] Comparative Example 7 In a 4.1-liter jacketed reactor equipped with a sparger for introducing oxygen-containing gas at the bottom of the reactor, stirring turbine blades and baffles, and a reflux condenser on the vent gas line at the top of the reactor, 0.88 g of cupric chloride dihydrate, 3.76 g of 35% hydrochloric acid, 33.57 g of N,N,N',N'-tetramethylpropanediamine, 850 g of n-butanol, 1982 g of methanol, and 630 g of 2,6-dimethylphenol were placed. The composition weight ratio of the solvent used was n-butanol:methanol=30:70. Next, oxygen was introduced into the reactor from the sparger at a rate of 410 mL / min while vigorously stirring, and at the same time, the polymerization temperature was adjusted by passing a heat medium through the jacket to maintain it at 40°C. The polymerization liquid gradually took on the form of a slurry. 200 minutes after the start of oxygen introduction, the aeration of the oxygen-containing gas was stopped, and a 50% aqueous solution of 4.56 g of ethylenediaminetetraacetic acid tripotassium salt (a reagent manufactured by Dojindo Laboratories) was added to the polymerization mixture, followed by the addition of a 20% methanol solution of 8.52 g of hydroquinone (a reagent manufactured by Wako Pure Chemical Industries) little by little. The obtained polymerization liquid was transferred to a 4.1-liter jacketed reactor equipped with stirring turbine blades and baffles, and a reflux condenser on the vent gas line at the top of the reactor, and reacted at 60°C for 3 hours. After the reaction was completed, the mixture was filtered and washed three times with a methanol washing liquid (b) in an amount such that the mass ratio (b / a) of the washed polyphenylene ether (a) to the methanol washing liquid (b) was 4, to obtain wet polyphenylene ether. The mixture was then vacuum-dried at 120°C for 4 hours to obtain dry polyphenylene ether. The analysis results of the obtained polyphenylene ether are shown in Table 1.

[0122] Comparative Example 8 The same procedure as in Example 1 was repeated except that the phenol raw material was 2 kg of 2-tert-butyl-5-methylphenol. The analytical results are shown in Table 1.

[0123] (Production Example 1) A 1.5-liter jacketed reactor equipped with a sparger for introducing an oxygen-containing gas at the bottom of the reactor, stirring turbine blades and baffles, and a reflux condenser on the vent gas line at the top of the reactor was charged with a mixture of 0.092 g of cuprous oxide and 0.69 g of 47% hydrogen bromide, which had been previously prepared, 0.22 g of N,N'-di-t-butylethylenediamine, 3.27 g of dimethyl-n-butylamine, 1.07 g of di-n-butylamine, 714.65 g of toluene, 65.03 g of 2,6-dimethylphenol, and 14.97 g of 2,2-bis(3,5-dimethyl-4-hydroxyphenyl)propane. Then, air was introduced into the reactor from the sparger at a rate of 0.84 L / min while vigorously stirring, and the polymerization temperature was adjusted by passing a heat medium through the jacket to maintain it at 20°C. 150 minutes after the start of air introduction, the air flow was stopped and the inside of the reactor was replaced with nitrogen gas, and then 0.99 g of ethylenediaminetetraacetic acid tetrasodium salt tetrahydrate (a reagent manufactured by Dojindo Laboratories) was added to the polymerization mixture as an aqueous solution of 160 g of water. The mixture was then heated to 70°C, and copper extraction was carried out at 70°C for 2 hours. After that, the mixture was separated by standing to separate into an unmodified polyphenylene ether solution (organic phase) and an aqueous phase to which the catalyst metal had been transferred. The unmodified polyphenylene ether thus obtained was used to obtain a modified polyphenylene ether in the same manner as in Example 7. The analytical results are shown in Table 2.

[0124] Comparative Example 10 A laminate was obtained in the same manner as in Example 11, except that the polyphenylene ether described in Production Example 1 was used as the raw material. The analytical results are shown in Table 3.

[0125] (Reference example 9) A 1.5-liter jacketed reactor equipped with a sparger for introducing an oxygen-containing gas at the bottom of the reactor, stirring turbine blades and baffles, and a reflux condenser on the vent gas line at the top of the reactor was charged with a mixture of 0.15 g of cuprous oxide and 1.12 g of 47% hydrogen bromide, 0.36 g of N,N'-di-t-butylethylenediamine, 5.31 g of dimethyl-n-butylamine, 1.74 g of di-n-butylamine, 891.3 g of toluene, 50.0 g of 2,6-dimethylphenol, and 50.0 g of 2,5-dimethylphenol. Then, air was introduced into the reactor from the sparger at a rate of 1.05 L / min while vigorously stirring, and the polymerization temperature was adjusted by passing a heat medium through the jacket to maintain it at 40°C. 120 minutes after the start of air introduction, the entire solution became highly viscous and gel was generated.

[0126] [Table 1]

[0127] [Table 2]

[0128] [Table 3]

[0129] As shown in Tables 1 and 2, in comparison with the Comparative Examples, by using the polyphenylene ethers of the Examples, it was possible to obtain polyphenylene ethers having various reduced viscosities with improved solvent solubility in methyl ethyl ketone. [Industrial Applicability]

[0130] The polyphenylene ether of the present invention has excellent solvent solubility and is therefore industrially valuable as an electronic material and a modifier.

Claims

1. The repeating unit is derived from a phenol represented by the following formula (1) in an amount of 5 to 85 mol % and a repeating unit is derived from a phenol represented by the following formula (2) in an amount of 15 to 95 mol % relative to a total of 100 mol % of the repeating unit derived from a phenol represented by the following formula (1) and the repeating unit derived from a phenol represented by the following formula (2): The reduced viscosity (ηsp / c) measured in a chloroform solution having a concentration of 0.5 g / dL at 30° C. is 0.03 to 0.30 dL / g.

1. A polyphenylene ether comprising: 【Chemistry 1】 (In formula (1), R 11 each independently represents an optionally substituted saturated hydrocarbon group having 1 to 6 carbon atoms, an optionally substituted aryl group having 6 to 12 carbon atoms, or a halogen atom; R 12 are each independently a hydrogen atom, an optionally substituted hydrocarbon group having 1 to 6 carbon atoms, an optionally substituted aryl group having 6 to 12 carbon atoms, or a halogen atom. 【Chemistry 2】 (In formula (2), R 22 each independently represents a hydrogen atom, an optionally substituted saturated or unsaturated hydrocarbon group having 1 to 20 carbon atoms, an optionally substituted aryl group having 6 to 12 carbon atoms, or a halogen atom; 22 are not both hydrogen atoms, R 21 is a partial structure represented by the following formula (3). 【Chemistry 3】 (In formula (3), R 31 each independently represents an optionally substituted linear alkyl group having 1 to 8 carbon atoms, or two R 31 is a cyclic alkyl structure having 1 to 8 carbon atoms bonded to R 32 each independently represents an optionally substituted alkylene group having 1 to 8 carbon atoms; each b independently represents 0 or 1; R 33 is a hydrogen atom, an optionally substituted alkyl group having 1 to 8 carbon atoms, or an optionally substituted phenyl group.

2. The polyphenylene ether according to claim 1, wherein the partial structure represented by the formula (3) is a t-butyl group.

3. 3. The polyphenylene ether according to claim 1, having an average number of hydroxyl groups per molecule of less than 2.

5.

4. The polyphenylene ether according to any one of claims 1 to 3, having an average number of hydroxyl groups of less than 0.2 per molecule.

5. The polyphenylene ether according to any one of claims 1 to 4, having at least one partial structure selected from the group consisting of the following formulas (4), (5), (6), and (7), and having an average number of hydroxyl groups of less than 0.2 per molecule. 【Chemistry 4】 【Chemistry 5】 【Chemistry 6】 (In formula (6), R 6 is a hydrogen atom or a saturated or unsaturated hydrocarbon group having 1 to 10 carbon atoms, and the saturated or unsaturated hydrocarbon may have a substituent within the range satisfying the condition of having 1 to 10 carbon atoms. 【Chemistry 7】 (In formula (7), R 7 is a saturated or unsaturated divalent hydrocarbon group having 1 to 10 carbon atoms, and the saturated or unsaturated divalent hydrocarbon may have a substituent within the range satisfying the condition of having 1 to 10 carbon atoms; R 8 is a hydrogen atom or a saturated or unsaturated hydrocarbon group having 1 to 10 carbon atoms, and the saturated or unsaturated hydrocarbon may have a substituent within the range satisfying the condition of having 1 to 10 carbon atoms.

6. The polyphenylene ether according to any one of claims 1 to 5, comprising a repeating unit derived from a monohydric phenol having at least one unsaturated hydrocarbon group on a carbon atom at the ortho position to a carbon atom to which a phenol hydroxyl group is bonded.

7. 7. The polyphenylene ether of claim 6, wherein the monohydric phenol is 2-allylphenol or 2-methyl-6-allylphenol.

8. The method for producing the polyphenylene ether according to any one of claims 1 to 7, comprising a step of oxidatively polymerizing the phenol of the formula (1) and the phenol of the formula (2).

9. A polyphenylene ether solution comprising the polyphenylene ether according to any one of claims 1 to 7 and a ketone solvent.

10. A thermosetting composition comprising the polyphenylene ether of any one of claims 1 to 7.

11. A prepreg comprising a substrate and the thermosetting composition of claim 10.

12. The prepreg according to claim 11 , wherein the substrate is a glass cloth.

13. A laminate comprising a cured product of the prepreg according to claim 11 or 12 and a metal foil.

Citation Information

Patent Citations

  • Preparation of polyphenyleneeether copolymer

    JP1981104935A

  • Novel polyphenyleneeether resin composition

    JP1981104961A

  • Polyphenylene oxide composition

    JP1982149351A

  • Method for producing low-molecular weight polyphenylene ether

    JP2006335806A

  • Polyphenylene ether

    JP2012082343A

Cited By

  • Polyphenylene ether, method for producing the same, thermosetting composition, prepreg, and laminate

    JP2023183317A

  • Resin composition, resin film, prepreg, and metal-clad laminate

    JP2025071800A

  • Resin composition, resin film, prepreg and metal-clad laminate

    JP7612942B1

  • Polyphenylene ether, method for producing the same, thermosetting composition, prepreg, and laminate

    JP7836229B2