Metal oxide film
A metal oxide film with controlled crystallinity, evaluated through electron beam diffraction, addresses the challenges of high electrical properties and reliability in semiconductor devices, enhancing mass productivity.
Patent Information
- Application Number
- JP2024123143
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-04-12
- Filing Date
- 2024-07-30
- Publication Date
- 2024-10-18
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing metal oxide films in semiconductor devices face challenges in achieving high electrical properties, reliability, and mass productivity, while also lacking effective evaluation methods.
A metal oxide film containing indium, aluminum, gallium, yttrium, or tin, and zinc, with controlled crystallinity evaluated through electron beam diffraction, providing a distribution of interplanar spacing and electron diffraction patterns to assess crystallinity.
The solution results in a metal oxide film with high electrical properties, ensuring high reliability and suitability for semiconductor devices with improved electrical characteristics.
Smart Images

Figure 2024149553000001_ABST
Abstract
Description
[Technical field]
[0001] 1. Field of the Invention One embodiment of the present invention relates to a metal oxide film. One embodiment of the present invention relates to a semiconductor device including a metal oxide film. One embodiment of the present invention relates to a method for evaluating a metal oxide film.
[0002] Note that one embodiment of the present invention is not limited to the above technical field. Examples of the technical field of one embodiment of the present invention disclosed in this specification and the like include a semiconductor device, a display device, a light-emitting device, a power storage device, a memory device, an electronic device, a lighting device, an input device, an input / output device, a driving method thereof, or a manufacturing method thereof. A semiconductor device refers to any device that can function by utilizing semiconductor characteristics. [Background technology]
[0003] As a semiconductor material applicable to transistors, oxide semiconductors have been attracting attention. For example, Patent Document 1 discloses a semiconductor device in which a plurality of oxide semiconductor layers are stacked, and an oxide semiconductor layer serving as a channel among the plurality of oxide semiconductor layers contains indium and gallium, and the proportion of indium is made higher than the proportion of gallium, thereby increasing the field effect mobility (sometimes simply referred to as mobility, or μFE). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2014-7399 A Summary of the Invention [Problem to be solved by the invention]
[0005] An object of one embodiment of the present invention is to provide a metal oxide film having excellent electric properties.An object of one embodiment of the present invention is to provide a metal oxide film having high reliability.An object of one embodiment of the present invention is to provide a metal oxide film having excellent mass productivity.An object of one embodiment of the present invention is to provide a novel metal oxide film.
[0006] Another object of one embodiment of the present invention is to provide a semiconductor device to which a metal oxide film is applied and which has high electrical characteristics.An object of one embodiment of the present invention is to provide a semiconductor device to which a metal oxide film is applied and which has high reliability.
[0007] Another object of one embodiment of the present invention is to provide a novel analysis method, evaluation method, or analysis method for a metal oxide film.
[0008] Note that the description of these problems does not preclude the existence of other problems. Note that one embodiment of the present invention does not necessarily solve all of these problems. Note that problems other than these can be extracted from the description of the specification, drawings, claims, etc. [Means for solving the problem]
[0009] One aspect of the present invention is a metal oxide film containing indium, M (M is aluminum, gallium, yttrium, or tin), and zinc. The distribution of the interplanar spacing d of the metal oxide film determined by electron beam diffraction in which an electron beam is irradiated from a direction perpendicular to the film surface of the metal oxide film has a first peak and a second peak. The apex of the first peak is located at 0.25 nm to 0.30 nm, and the apex of the second peak is located at 0.15 nm to 0.20 nm. The distribution of the interplanar spacing d is obtained from a plurality of electron beam diffraction patterns in a plurality of regions of the metal oxide film. The electron beam diffraction is performed using an electron beam with a beam diameter of 0.3 nm to 10 nm.
[0010] In the above, it is preferable that the height of the apex of the first peak is higher than the height of the apex of the second peak, or in the above, it is preferable that the height of the apex of the first peak is lower than the height of the apex of the second peak.
[0011] Another embodiment of the present invention is a semiconductor device including a semiconductor layer, a gate electrode, and a gate insulating layer, in which the semiconductor layer includes any one of the above metal oxide films.
[0012] Another embodiment of the present invention is a method for evaluating a metal oxide film, comprising: irradiating a plurality of regions of the metal oxide film with an electron beam having a beam diameter of 0.3 nm or more and 10 nm or less in a direction perpendicular to a film surface of the metal oxide film, obtaining a plurality of electron beam diffraction patterns, calculating a lattice spacing d for a plurality of spots observed in the plurality of electron beam diffraction patterns, and evaluating the crystallinity of the metal oxide film from the shape of a frequency distribution of the lattice spacing d.
[0013] Another embodiment of the present invention is a method for evaluating a metal oxide film, comprising: irradiating a plurality of regions of the metal oxide film with an electron beam having a beam diameter of 0.3 nm or more and 10 nm or less in a direction perpendicular to a surface of the metal oxide film, obtaining a plurality of electron beam diffraction patterns; calculating an angle θ from a reference line for a plurality of spots observed in the plurality of electron beam diffraction patterns; and evaluating the crystallinity of the metal oxide film from the shape of the distribution of the angle θ. Effect of the Invention
[0014] According to one embodiment of the present invention, a metal oxide film having excellent electrical characteristics, a highly reliable metal oxide film, or a novel metal oxide film can be provided.
[0015] According to one embodiment of the present invention, a semiconductor device having excellent electrical characteristics by using a metal oxide film can be provided. Alternatively, a semiconductor device having high reliability by using a metal oxide film can be provided.
[0016] According to one embodiment of the present invention, a novel analysis method, evaluation method, or analysis method for a metal oxide film can be provided.
[0017] Note that the description of these effects does not preclude the existence of other effects. Note that one embodiment of the present invention does not necessarily have all of these effects. Note that effects other than these can be extracted from the description in the specification, drawings, claims, etc. [Brief description of the drawings]
[0018] [Figure 1] Figure 1A is a schematic diagram of a metal oxide film, Figures 1B and 1C are schematic diagrams of electron diffraction patterns, and Figures 1D and 1E are schematic diagrams of histograms. [Diagram 2] 2A to 2C are schematic diagrams of histograms. [Diagram 3] 3A and 3B are schematic diagrams of electron diffraction patterns. [Figure 4] Figure 4A is an electron diffraction pattern, and Figure 4B is a histogram of lattice spacing. [Diagram 5] Figure 5A is an electron diffraction pattern, and Figure 5B is a histogram of lattice spacing. [Figure 6] Figure 6A is an electron diffraction pattern, and Figure 6B is a histogram of lattice spacing. [Figure 7] Figure 7A is an electron diffraction pattern, and Figure 7B is a histogram of lattice spacing. [Figure 8] Figure 8A is an electron diffraction pattern, and Figure 8B is a histogram of lattice spacing. [Figure 9] Figure 9A is an electron diffraction pattern, and Figure 9B is a histogram of lattice spacing. [Figure 10] FIG. 10 is a diagram showing the frequency ratio of electron diffraction peaks. [Figure 11] 11A and 11B show the change in lattice spacing for each frame and the change in spot angle for each frame, respectively. [Figure 12] 12A and 12B show the change in lattice spacing for each frame and the change in spot angle for each frame, respectively. [Figure 13] 13A, 13B, and 13C are XRD spectra. [Figure 14] 14A, 14B, and 14C are XRD spectra. [Figure 15] 15A, 15B, and 15C are XRD spectra. [Figure 16] 16A, 16B, and 16C are XRD spectra. [Figure 17] FIG. 17 is a diagram showing the apex angles of X-ray diffraction peaks. [Figure 18] 18A to 18E are diagrams showing a calculation model. [Figure 19] 19A to 19E are diagrams showing a calculation model. [Figure 20] Fig. 20A is a diagram showing the relationship between temperature and average energy, and Fig. 20B is a diagram showing the relationship between temperature and the difference in average energy. [Figure 21] FIG. 21 is a diagram for explaining the generation energy of defects. [Figure 22] Fig. 22A is a diagram explaining the classification of IGZO crystal structures, Fig. 22B is a diagram explaining the XRD spectrum of quartz glass, Fig. 22C is a diagram explaining the XRD spectrum of crystalline IGZO, and Fig. 22D is a diagram explaining the ultrafine electron beam diffraction pattern of crystalline IGZO. [Figure 23] Fig. 23A is a top view of the semiconductor device, and Fig. 23B and Fig. 23C are cross-sectional views of the semiconductor device. [Figure 24] 24A and 24B are cross-sectional views of a semiconductor device. [Diagram 25] Fig. 25A is a top view of the semiconductor device, and Fig. 25B and Fig. 25C are cross-sectional views of the semiconductor device. [Figure 26] Fig. 26A is a top view of the semiconductor device, and Fig. 26B and Fig. 26C are cross-sectional views of the semiconductor device. [Figure 27] 27A and 27B are cross-sectional views of a semiconductor device. [Figure 28] 28A to 28C are diagrams showing configuration examples of a display device. [Figure 29] FIG. 29 is a diagram showing an example of a cross-sectional configuration of a display device. [Diagram 30] FIG. 30 is a diagram showing an example of a cross-sectional configuration of a display device. [Diagram 31] FIG. 31 is a diagram showing an example of a cross-sectional configuration of a display device. [Diagram 32] Fig. 32A is a block diagram of a display device, and Fig. 32B and Fig. 32C are circuit diagrams of the display device. [Diagram 33] Figures 33A, 33C and 33D are circuit diagrams of the display device, and Figure 33B is a timing chart. [Diagram 34] 34A and 34B show configuration examples of a display module. [Diagram 35] 35A to 35C are diagrams showing configuration examples of electronic devices. [Diagram 36] 36A to 36E are diagrams illustrating configuration examples of electronic devices. [Figure 37] 37A to 37G are diagrams showing configuration examples of electronic devices. [Figure 38] 38A to 38D are diagrams showing configuration examples of electronic devices. [Figure 39] 39A to 39D are diagrams showing the Id-Vg characteristics of a transistor. [Diagram 40] FIG. 40 is a diagram showing the reliability evaluation results of transistors. [Diagram 41] 41A to 41D are diagrams showing the Id-Vg characteristics of a transistor. [Diagram 42] FIG. 42 shows a HAADEF-STEM image and an EDX mapping image. [Diagram 43] 43A to 43D show the results of quantitative analysis of the composition of the metal oxide film. [Diagram 44] 44A-44C are compositional histograms of metal oxide films. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] Hereinafter, the embodiments will be described with reference to the drawings. However, it will be easily understood by those skilled in the art that the embodiments can be implemented in many different ways, and that the modes and details can be changed in various ways without departing from the spirit and scope of the present invention. Therefore, the present invention should not be interpreted as being limited to the description of the following embodiments.
[0020] In the configuration of the invention described below, the same parts or parts having similar functions are denoted by the same reference numerals in different drawings, and the repeated explanations are omitted. In addition, when referring to similar functions, the same hatch pattern may be used and no particular reference numeral may be used.
[0021] In addition, in each figure described in this specification, the size of each component, the thickness of a layer, or an area may be exaggerated for clarity, and therefore, the drawings are not necessarily limited to the scale.
[0022] In addition, ordinal numbers such as "first" and "second" in this specification are used to avoid confusion of components and do not limit the numbers.
[0023] A transistor is a type of semiconductor element that can amplify current or voltage, and perform switching operations to control conduction or non-conduction, etc. In this specification, the term "transistor" includes an IGFET (Insulated Gate Field Effect Transistor) and a thin film transistor (TFT).
[0024] In addition, the functions of "source" and "drain" may be interchangeable when transistors of different polarities are used, when the direction of current flow changes during circuit operation, etc. For this reason, in this specification, the terms "source" and "drain" may be used interchangeably.
[0025] In addition, in this specification and the like, the terms "film" and "layer" can be interchangeable. For example, the terms "conductive layer" and "insulating layer" can be interchangeable with the terms "conductive film" and "insulating film".
[0026] In this specification and the like, a display panel, which is one aspect of a display device, has a function of displaying (outputting) an image or the like on a display surface. Therefore, the display panel is one aspect of an output device.
[0027] In addition, in this specification, a display panel having a connector such as an FPC (Flexible Printed Circuit) or TCP (Tape Carrier Package) attached to the substrate, or a substrate having an IC mounted thereon using a COG (Chip On Glass) method or the like, may be referred to as a display panel module, display module, or simply a display panel.
[0028] In this specification and the like, a touch panel, which is one aspect of a display device, has a function of displaying an image or the like on a display surface and a function as a touch sensor that detects that a detectable object such as a finger or a stylus touches, presses, or approaches the display surface. Thus, the touch panel is one aspect of an input / output device.
[0029] The touch panel can also be called, for example, a display panel (or display device) with a touch sensor or a display panel (or display device) with a touch sensor function. The touch panel can have a display panel and a touch sensor panel. Alternatively, the touch panel can have a function as a touch sensor inside or on the surface of the display panel.
[0030] In addition, in this specification and the like, a touch panel substrate on which a connector and / or an IC are mounted may be referred to as a touch panel module, a display module, or simply a touch panel.
[0031] (Embodiment 1) In this embodiment, a metal oxide film according to one embodiment of the present invention and an evaluation method for the metal oxide film will be described.
[0032] [Metal oxide film] FIG. 1A shows a schematic diagram of a metal oxide film 11 formed on a substrate 10.
[0033] The metal oxide film 11 according to one embodiment of the present invention is an oxide film containing indium, M (M is aluminum, gallium, yttrium, or tin), and zinc. Such an oxide film is characterized by exhibiting semiconductor characteristics. The metal oxide film 11 is preferably a film formed by a sputtering method. In particular, it is preferable to use a polycrystalline metal oxide target as a sputtering target.
[0034] The metal oxide film 11 includes a plurality of extremely small (several nm or less) crystalline regions that are randomly oriented (also referred to as having no orientation). The metal oxide film 11 having such crystallinity has extremely high reliability compared to an amorphous metal oxide film. The metal oxide film 11 may be a film in which crystalline regions not having orientation and crystalline regions having orientation are mixed.
[0035] The metal oxide film 11 according to one embodiment of the present invention can be applied to a semiconductor device, for example, a semiconductor in which a channel of a transistor is formed.
[0036] The metal oxide film 11 is preferably an oxide film containing indium, gallium, and zinc. In addition, it is preferable to use a material having a high indium content among the metal elements contained in the metal oxide film 11. In particular, it is preferable to use a material having a higher indium content than the gallium content. By applying such a metal oxide film 11 to the semiconductor layer of a transistor, a transistor with high field effect mobility can be realized.
[0037] The crystallinity of the metal oxide film 11 can be controlled by changing the film formation conditions. For example, a film with high crystallinity can be formed by increasing the ratio of oxygen gas in the film formation gas (also referred to as oxygen flow ratio). On the other hand, a film with low crystallinity can be formed by decreasing the ratio of oxygen gas in the film formation gas or by using a film formation gas that does not contain oxygen gas. Alternatively, a film with high crystallinity can be formed by increasing the substrate temperature during film formation, and a film with low crystallinity can be formed by decreasing the substrate temperature or by forming the film without heating the substrate. The higher the crystallinity of the metal oxide film 11, the more stable the film is. On the other hand, the lower the crystallinity, the higher the field effect mobility can be when applied to a transistor.
[0038] [Electron diffraction] The metal oxide film 11 according to one embodiment of the present invention is a film in which the following characteristics appear in an electron beam diffraction pattern obtained by irradiating the film surface with an electron beam in a direction perpendicular to the film surface.
[0039] As the electron beam diffraction method, it is preferable to use the nano beam electron diffraction (NBED) method in which a converged electron beam is irradiated onto a sample, or the selected area electron diffraction (SAED) method in which a parallel electron beam is used to irradiate a micro area by narrowing the irradiation area.
[0040] When the electron beam diffraction pattern of the metal oxide film 11 having extremely small crystal regions is measured under conditions where the electron beam diameter is extremely small (e.g., 0.3 nm or more and 10 nm or less, or 5 nm or less), multiple spots distributed discretely in the circumferential direction (also called the θ direction) are observed. On the other hand, in the electron beam diffraction pattern under conditions where the beam diameter is large (e.g., 50 nm or more, or 100 nm or more), a ring-shaped (also called annular) pattern is observed.
[0041] 1B and 1C are schematic diagrams of electron beam diffraction patterns obtained by irradiating an electron beam having a beam diameter of several nm from a direction perpendicular to the film surface of the metal oxide film 11. An electron beam diffraction pattern 20a shown in Fig. 1B is an electron beam diffraction pattern in a region 12a shown in Fig. 1A, and an electron beam diffraction pattern 20b shown in Fig. 1C is an electron beam diffraction pattern in a region 12b different from the region 12a.
[0042] As shown in FIG. 1B, in the electron beam diffraction pattern 20a of the metal oxide film 11, a spot (direct spot 20) of the incident electron beam that has passed through the sample, a first spot 21 closer to the direct spot 20, and a second spot 22 farther from the direct spot 20 than the first spot 21 are observed.
[0043] The first spot 21 is observed in an annular first region 31 located at a distance r1 in the radial direction from the direct spot 20 and in the vicinity thereof. The second spot 22 is observed in an annular second region 32 located at a distance r2 in the radial direction from the direct spot 20 and in the vicinity thereof. The second region 32 is located outside the first region 31. In other words, the distance r2 is greater than the distance r1.
[0044] Furthermore, as shown in FIG. 1A, when the irradiation position of the electron beam is scanned parallel to the film surface direction of the metal oxide film 11 and the electron beam diffraction pattern of a region (region 12b) different from region 12a is observed, a first spot 21 is observed at a different position in the first region 31, and a second spot 22 is observed at a different position in the second region 32, as shown in FIG. 1C.
[0045] This shows that extremely small crystal regions are included in the metal oxide film 11. In addition, since the positions of the first spot 21 and the second spot 22 are different in different regions, it is shown that the small crystal regions included in the metal oxide film 11 do not have orientation.
[0046] In this way, by performing measurements while scanning the irradiation position of the electron beam parallel to the film surface direction of the metal oxide film 11, a plurality of electron beam diffraction patterns can be observed. From each of the plurality of electron beam diffraction patterns thus obtained, information such as the positions of the first spot 21 and the second spot 22 and the detected intensity can be obtained. The position information of the first spot 21 and the second spot 22 includes the distance r from the direct spot 20 and the angle θ from an arbitrarily determined reference line. From the information obtained from the plurality of electron beam diffraction patterns, a histogram (also called a distribution diagram or a frequency distribution diagram) for the distance r, the angle θ, the detected intensity, etc. can be obtained.
[0047] A method for evaluating a metal oxide film according to one embodiment of the present invention will be described. First, an electron beam having a beam diameter of 0.3 nm to 10 nm is irradiated to multiple regions of the metal oxide film in a direction perpendicular to the film surface of the metal oxide film to obtain multiple electron beam diffraction patterns. Next, the interplanar spacing d is calculated for multiple spots observed in the obtained multiple electron beam diffraction patterns. Then, the crystallinity of the metal oxide film can be evaluated from the shape of the frequency distribution of the calculated interplanar spacing d.
[0048] Similarly, the angle θ from a reference line is calculated for multiple spots observed in multiple electron beam diffraction patterns obtained, and the crystallinity of the metal oxide film can be evaluated from the shape of the distribution of the angle θ.
[0049] Similarly, the crystallinity of the metal oxide film can also be evaluated from information (eg, distribution shape) on the brightness (detection intensity) of a plurality of spots observed in a plurality of electron beam patterns obtained.
[0050] The more electron beam diffraction patterns are obtained, the more accurate the information will be, which is preferable. For example, it is preferable to obtain 50 or more electron beam diffraction patterns, preferably 100 or more, and more preferably 1000 or more. There is no particular upper limit, but even if the number is 10,000 or less, or 5,000 or less, sufficiently accurate information can be obtained.
[0051] A more specific example will be described below.
[0052] 1D shows an example of a histogram 30r showing the number (frequency) of spots observed in the electron diffraction pattern of the metal oxide film 11 versus the distance r from the direct spot 20. As shown in FIG 1D, the histogram 30r includes a peak of a first spot 21 having an apex in a first region 31 and a peak of a second spot 22 having an apex in a second region 32.
[0053] In the electron beam diffraction method, the value of the interplanar spacing d (hereinafter referred to as the d value) corresponding to the target spot can be calculated using the distance r from the center of the direct spot to the target spot according to the following formula (1).
[0054] [Number 1] d = Lλ / r (1) In equation (1), L is the camera distance and λ is the wavelength of the electron beam.
[0055] A histogram 30 created using the d values calculated in this manner is shown in FIG. 1E.
[0056] A histogram of d values obtained from an electron beam diffraction pattern of the metal oxide film 11 of one embodiment of the present invention has two peaks (a first peak 41 and a second peak 42 from the larger d value side) as shown in FIG. 1E.
[0057] As shown in FIG. 1E, the metal oxide film 11 is preferably a film in which the shape of the frequency distribution of the d value has a first peak 41 located in a d value range of 0.25 nm or more and 0.30 nm or less, and a second peak 42 located in a d value range of 0.15 nm or more and 0.20 nm or less.
[0058] The first spots 21 constituting the first peak 41 include spots due to scattered electrons originating from the medium-range order structure of minute crystalline clusters contained in the metal oxide film 11. The first spots 21 include scattered electrons due to diffraction with different interplanar spacings in the crystalline clusters and scattered electrons from crystalline clusters with different structures, and therefore the scattering angle varies, and as a result, the width of the region in which the d value of the first spots 21 can be observed increases. Therefore, the full width at half maximum of the first peak 41 tends to be larger than the full width at half maximum of the second peak 42.
[0059] The first spot 21 may include a spot formed by diffracted electrons diffracted by a minute crystal region contained in the metal oxide film 11.
[0060] The second spots 22 constituting the second peak 42 are spots formed by diffracted electrons diffracted by minute crystalline regions contained in the metal oxide film 11. For example, if the crystalline regions are made of InGaZnO 4 When the crystal structure is the same as that of a crystal, the second spot 22 is presumably derived from electrons diffracted by the (110) plane and crystal planes equivalent thereto.
[0061] The shapes and heights of the first peak 41 and the second peak 42 in the histogram 30 reflect the crystallinity of the metal oxide film 11. Therefore, it is possible to evaluate the crystallinity of the metal oxide film 11 from the shape of the frequency distribution of the histogram 30.
[0062] As an example, histograms 30 of metal oxide films 11 having different crystallinity are shown in FIGS. 2A, 2B, and 2C, respectively.
[0063] The histogram 30a shown in Fig. 2A is an example of a metal oxide film 11 with low crystallinity. Fig. 2A shows a peak value P1 which is the apex value of a first peak 41, and a peak value P2 which is the apex value of a second peak 42. Note that the heights and positions of the peak values P1 and P2 change according to the division width (class width) of the data of the histogram 30a, and therefore the class width can be set to an appropriate width. Typically, it is preferable to set the number of classes to about the square root of the total number of data.
[0064] In the histogram 30a, the peak value P2 of the second peak 42 is lower than the peak value P1 of the first peak 41. In a metal oxide film 11 having an even lower crystallinity than the first peak 41, the second peak 42 may be barely observed.
[0065] The histogram 30b shown in FIG. 2B is an example of a metal oxide film 11 having higher crystallinity than that shown in FIG. 2A. The improved crystallinity increases the number of second spots 22 resulting from diffracted electrons, and the peak value P2 of the second peak 42 becomes higher than that shown in FIG. 2A. On the other hand, the proportion of low-order regions in the metal oxide film 11 decreases, and the number of first spots 21 decreases, and the peak value P1 of the first peak 41 becomes lower. As a result, the difference between the peak value P1 of the first peak 41 and the peak value P2 of the second peak 42 becomes smaller than that shown in FIG. 2A.
[0066] Histogram 30c shown in Fig. 2C is an example of a metal oxide film 11 with even higher crystallinity than that of Fig. 2B. As the crystallinity improves, the number of second spots 22 further increases and the number of first spots 21 decreases, so that the magnitude relationship between peak value P1 of first peak 41 and peak value P2 of second peak 42 is reversed, and peak value P2 becomes larger than peak value P1.
[0067] The above is an example of a histogram. According to the evaluation method described here, it is possible to evaluate the crystallinity of the metal oxide film 11 from the shape of the frequency distribution of the histogram. In addition, by comparing the shapes of the frequency distribution of the histograms for metal oxide films 11 formed under different film formation conditions, it is also possible to compare their crystallinity.
[0068] The metal oxide film 11 may be a film in which regions with low crystallinity and regions with high crystallinity are mixed. When the electron beam diffraction pattern of such a metal oxide film 11 is measured while scanning the electron beam parallel to the film surface direction as described above, the electron beam diffraction pattern derived from the region with low crystallinity and the electron beam diffraction pattern derived from the region with high crystallinity may appear alternately.
[0069] FIG. 3A shows an example of an electron beam diffraction pattern 20c obtained when a region of low crystallinity in the metal oxide film 11 is measured.
[0070] In the electron beam diffraction pattern 20c, a plurality of first spots 21 are observed in the first region 31. The first spots 21 vary in their radial positions (specifically, the distance from the direct spot 20 to the first spots 21). In addition, although not shown here, the detected intensity of the first spots 21 also varies.
[0071] In the electron beam diffraction pattern 20c, the second spots 22 are observed in the second region 32. The second spots 22 have smaller radial variations than the first spots 21. Since the second region 32 is low in crystallinity, the number of the second spots 22 observed is often smaller than the number of the first spots 21. Furthermore, the detected intensity may be relatively small.
[0072] FIG. 3B shows an example of an electron beam diffraction pattern 20d obtained when a highly crystalline region of the metal oxide film 11 is measured.
[0073] In the electron beam diffraction pattern 20d, six first spots 21 are observed in the first region 31. The angle θ1 between two adjacent first spots 21 with the direct spot 20 as the center is approximately 60 degrees. That is, the six first spots 21 are observed to satisfy six-fold symmetry with the direct spot 20 as the center. Furthermore, the radial positions and detected intensities of the first spots 21 have smaller variations than those of the electron beam diffraction pattern 20c.
[0074] In the electron beam diffraction pattern 20d, six second spots 22 are observed in the second region 32. Like the first spots 21, the second spots 22 are observed to satisfy six-fold symmetry, and the angle θ2 between two adjacent second spots 22 is approximately 60 degrees.
[0075] Moreover, the angle θ3 between the first spot 21 and the second spot 22 with the direct spot 20 at the center is approximately 30 degrees. This shows that the highly crystalline region of the metal oxide film 11 has six-fold symmetry with respect to the axis perpendicular to the film surface.
[0076] The crystalline region included in the metal oxide film 11 is InGaZn 2 O 5 In the case where the crystalline region has a crystal structure similar to that of InGaZnO, it is presumed that the first spot 21 originates from diffracted electrons due to the (100) plane and crystal planes equivalent thereto. 4 If the crystal structure is similar to that of InGaZnO, the (100) plane satisfies the extinction rule, so in principle no diffracted electrons are observed. 4 Even if a material has a crystal structure similar to that of a crystal, the entire crystalline region is not a perfect crystal, but is in an incomplete state that includes lattice distortion, which violates the extinction rule and results in the observation of diffracted electrons from the (100) plane that would not normally be observed.
[0077] Furthermore, when the crystal structure of the crystalline region contained in the metal oxide film 11 is classified as a hexagonal crystal system, the electron beam diffraction pattern 20d obtained by irradiating an electron beam perpendicular to the film surface has six-fold symmetry, and therefore it can be inferred that the crystal orientation of the crystalline region contained in the metal oxide film 11 is such that the c-axis is oriented in the film thickness direction.
[0078] [Method of forming metal oxide film] A method for forming a metal oxide film according to one embodiment of the present invention will be described below.
[0079] The metal oxide film of one embodiment of the present invention can be formed by a sputtering method with or without heating the substrate.
[0080] When forming a film by heating the substrate, the substrate temperature may be from room temperature to 250° C., preferably from room temperature to 200° C., and more preferably from room temperature to 140° C. For example, the substrate temperature is from room temperature to less than 140° C., which is preferable because it increases productivity.
[0081] When a film is formed without heating the substrate, the substrate temperature is initially at room temperature or a temperature close to room temperature. Note that the substrate may be heated by energy imparted to the substrate by sputtering particles or the like during film formation. In addition, since a mechanism for heating the substrate is not required in an apparatus for forming a metal oxide film, the apparatus can be simplified and costs can be reduced.
[0082] The film may be formed in an atmosphere containing oxygen. For example, the ratio of the flow rate of oxygen to the total flow rate of the film forming gas supplied to the film forming chamber of the film forming apparatus (hereinafter referred to as the oxygen flow rate ratio) can be set to an appropriate value in the range of 0% to 100%. The crystallinity of the metal oxide film to be formed can be controlled by adjusting the oxygen flow rate. Specifically, the higher the oxygen flow rate ratio, the higher the crystallinity of the metal oxide film can be, and the lower the oxygen flow rate ratio, the lower the crystallinity of the metal oxide film can be. As the gas other than oxygen contained in the film forming gas, for example, a rare gas such as argon can be used. By forming the film in an atmosphere containing oxygen, oxygen deficiency in the metal oxide film can be reduced. Alternatively, the atmosphere may be free of oxygen.
[0083] As an oxide target that can be used for forming a metal oxide film, for example, an In-M-Zn oxide (M is Al, Ga, Y, or Sn) can be applied. In particular, it is preferable to use an In-Ga-Zn oxide.
[0084] In addition, as an oxide target that can be used for forming a metal oxide film, In-M-based oxides, In-Zn-based oxides, etc. can also be used. In-Ga oxides are particularly preferred because they are less likely to form oxygen vacancies.
[0085] Here, the metal oxide contained in the oxide target preferably has a high In content. For example, when the sum of the compositions of In, M, and Zn is 1 (100%), it is preferable to use a metal oxide target in which the ratio of In is 33% or more and 60% or less, preferably 40% or more and 50% or less. Representatively, In:Ga:Zn=1:1:1 and oxides in the vicinity thereof, In:Ga:Zn=4:2:3 and oxides in the vicinity thereof, In:Ga:Zn=4:2:4.1 and oxides in the vicinity thereof, In:Ga:Zn=5:1:3 and oxides in the vicinity thereof, In:Ga:Zn=5:3:4 and oxides in the vicinity thereof, or In:Ga:Zn=10:1:3 and oxides in the vicinity thereof can be used.
[0086] As a result, the formed metal oxide film can be a metal oxide film with a high In content. Here, the composition of the formed metal oxide film and the oxide target may not necessarily be the same. In particular, the formed metal oxide film tends to have a lower Zn content than the oxide target.
[0087] In this manner, a metal oxide film can be formed.
[0088] The method for forming the metal oxide film is not limited to the above. Other methods may be used, such as plasma enhanced chemical vapor deposition (PECVD), thermal chemical vapor deposition (thermal CVD), atomic layer deposition (ALD), vacuum deposition, pulsed laser deposition (PLD), and liquid phase methods (spin coating, spraying, etc.). An example of the thermal CVD method is metal organic chemical vapor deposition (MOCVD).
[0089] The above is a description of the method for forming the metal oxide film.
[0090] [Metal oxide film evaluation example] The results of analysis of the metal oxide film of one embodiment of the present invention using the evaluation methods exemplified above will be described below.
[0091] Nanobeam electron diffraction analysis and X-ray diffraction (XRD) analysis were performed on the metal oxide films prepared by different methods to evaluate their crystallinity. Samples (sample A1 to sample A6) in which a metal oxide film with a thickness of 40 nm was formed on a silicon wafer were used for the evaluation. In-Ga-Zn oxide was used as the metal oxide film, and the deposition conditions for the metal oxide film were varied between the samples.
[0092] [Sample preparation] The metal oxide film was formed by sputtering using an In-Ga-Zn oxide target (In:Ga:Zn=4:2:4.1 [atomic ratio]). The film composition of the sample formed using a target with a composition of In:Ga:Zn=4:2:4.1 [atomic ratio] is approximately In:Ga:Zn=4:2:3 [atomic ratio].
[0093] The deposition conditions for the metal oxide films of samples A1 to A6 are shown in Table 1. In Table 1, the substrate temperature during deposition of the metal oxide films is Tsub, the oxygen flow rate is O 2 / (Ar+O 2 ), pressure is written as Pressure, and power source power is written as Power.
[0094] [Table 1]
[0095] For sample A1, the substrate temperature during deposition of the metal oxide film was room temperature (hereinafter also referred to as RT). A mixture of oxygen gas and argon gas was used as the deposition gas, and the oxygen flow rate ratio was 10%. The pressure during deposition was 0.6 Pa, and the power supply power was 2.5 kW.
[0096] For sample A2, the substrate temperature during deposition of the metal oxide film was room temperature (RT). A mixture of oxygen gas and argon gas was used as the deposition gas, with the oxygen flow rate ratio set to 30%. The pressure during deposition was 0.6 Pa, and the power supply power was 2.5 kW.
[0097] For sample A3, the substrate temperature during deposition of the metal oxide film was room temperature (RT). A mixture of oxygen gas and argon gas was used as the deposition gas, with the oxygen flow rate ratio set to 40%. The pressure during deposition was 0.6 Pa, and the power supply power was 2.5 kW.
[0098] For sample A4, the substrate temperature during deposition of the metal oxide film was room temperature (RT). A mixture of oxygen gas and argon gas was used as the deposition gas, with the oxygen flow rate ratio set to 50%. The pressure during deposition was 0.6 Pa, and the power supply power was 2.5 kW.
[0099] For sample A5, the substrate temperature during deposition of the metal oxide film was set to 100°C. A mixture of oxygen gas and argon gas was used as the deposition gas, with the oxygen flow rate ratio set to 10%. The pressure during deposition was set to 0.6 Pa, and the power supply power was set to 2.5 kW.
[0100] For sample A6, the substrate temperature during deposition of the metal oxide film was set to 100°C. A mixture of oxygen gas and argon gas was used as the deposition gas, with the oxygen flow rate ratio set to 30%. The pressure during deposition was set to 0.6 Pa, and the power supply power was set to 2.5 kW.
[0101] [Nanobeam Electron Diffraction] Each of the samples A1 to A6 was sliced in a direction parallel to the surface on which the metal oxide film was formed, to a thickness of about 20 nm to 30 nm. The sliced samples included the surface of the metal oxide film when the metal oxide film was formed.
[0102] Next, an electron beam with an acceleration voltage of 200 kV (wavelength: about 2.51 pm) and a beam diameter of 1 nm was incident on the metal oxide film from a direction perpendicular to the surface on which the film was to be formed, and multiple electron diffraction patterns were obtained. Multiple electron diffraction patterns were obtained by taking a video of the electron diffraction pattern while moving the electron beam irradiation point. The video was taken while moving the electron beam irradiation point by about 0.08 nm to 0.10 nm per frame, and about 3700 frames were obtained for each sample. A 200 pixel x 200 pixel imaging plate was used to take the electron diffraction patterns. The magnitude (q) of the scattering vector for one pixel was 0.082426 / nm / pixel.
[0103] Next, the spots were analyzed for each frame of the video.
[0104] The nanobeam electron diffraction results for sample A1 are shown in Figures 4A and 4B. The nanobeam electron diffraction results for sample A2 are shown in Figures 5A and 5B. The nanobeam electron diffraction results for sample A3 are shown in Figures 6A and 6B. The nanobeam electron diffraction results for sample A4 are shown in Figures 7A and 7B. The nanobeam electron diffraction results for sample A5 are shown in Figures 8A and 8B. The nanobeam electron diffraction results for sample A6 are shown in Figures 9A and 9B.
[0105] Figures 4A, 5A, 6A, 7A, 8A, and 9A each show the electron diffraction pattern of the final frame in the movie of each sample. In each figure, the upper horizontal axis and the right vertical axis show the pixel coordinates (denoted as pixel) of the imaging plate with the lower left as the reference point. The lower horizontal axis and the left vertical axis show the magnitude of the scattering vector (q [ / nm]). In addition, each point shown in each figure is shown in a darker color when the spot intensity (detection intensity) is higher, and in a lighter color when the intensity is lower.
[0106] The positions and intensity values of the spots (first spots) observed in the region of 30 to 90 pixels from the center of the electron diffraction pattern were obtained. In Fig. 4A, Fig. 5A, Fig. 6A, Fig. 7A, Fig. 8A, and Fig. 9A, the region of 30 pixels from the center and the region of 90 pixels from the center are indicated by solid line circles. The region of 30 to 90 pixels from the center of the electron diffraction pattern corresponds to a lattice spacing (d) of 0.13348 nm to 0.4044 nm. In addition, only spots with a spot intensity (0 to 255) of 64 or more and an area of 2 pixels or more were evaluated. In Fig. 4A, Fig. 5A, Fig. 6A, Fig. 7A, Fig. 8A, and Fig. 9A, the center of the electron diffraction pattern and each spot are connected by a solid line. The center of the electron diffraction pattern was the center of the spot of the incident electron beam that was transmitted through the sample without diffracting (also called a direct spot).
[0107] 4B, 5B, 6B, 7B, 8B, and 9B are histograms (frequency distribution diagrams) of the lattice spacing (d) in all frames of the video acquired for each sample. In each diagram, the horizontal axis indicates the lattice spacing (d [nm]), and the vertical axis indicates the frequency (Frequency [count]). In this embodiment, the data interval (class width) of the histogram is set to lattice spacing (d) = 0.002 nm.
[0108] As shown in Figures 4B, 5B, 6B, 7B, 8B, and 9B, under all conditions, there is a peak (first peak) having an apex in the range of 0.25 nm or more and 0.30 nm or less in terms of lattice spacing (d), and a peak (second peak) having an apex in the range of 0.15 nm or more and 0.20 nm or less.
[0109] Here, for samples A1 to A4, the ratio (P2 / P1) of the value of the apex of the second peak (peak value P2) to the value of the apex of the first peak (peak value P1) is shown in FIG. 10. In FIG. 10, the horizontal axis represents the oxygen flow rate ratio (O 2 / (Ar+O 2 10 shows the ratio of peak value P2 to peak value P1 (P2 / P1) on the vertical axis. Note that in Fig. 10, the frequency at d = 0.278 nm is used as peak value P1, and the frequency at d = 0.168 nm is used as peak value P2.
[0110] Comparing samples A1 to A4, there is a tendency for the second peak to increase as the oxygen flow rate ratio increases. Also, in samples A1 to A3, the value of the apex of the first peak (peak value P1) is higher than the value of the apex of the second peak (peak value P2). On the other hand, in sample A4, which has the highest oxygen flow rate ratio, the relationship between these magnitudes is reversed, and the value of the apex of the second peak (peak value P2) exceeds the value of the apex of the first peak (peak value P1), and the value of P2 / P1 shown in FIG. 10 also exceeds 1.
[0111] Similarly, when comparing sample A5 and sample A6, the value of the apex of the first peak is higher than the value of the apex of the second peak in sample A5, which is under the condition of a low oxygen flow ratio, whereas the value of the apex of the second peak is higher than the value of the apex of the first peak in sample A6, which is under the condition of a high oxygen flow ratio. This confirms that the higher the oxygen flow ratio, the more improved the crystallinity.
[0112] In addition, when comparing sample A1 and sample A5, which were formed under the same oxygen flow ratio, the second peak is larger in sample A5. The same is true for sample A2 and sample A6. This confirms that even under the same oxygen flow ratio, the higher the substrate temperature during film formation, the better the crystallinity.
[0113] In the evaluation method according to one embodiment of the present invention, information about the crystallinity of the metal oxide film can be obtained not only from the histogram but also from data for each frame regarding the position and brightness of the detected spots.
[0114] The change in lattice spacing (d) for each frame of sample A1 is shown in Figure 11A. In Figure 11A, the horizontal axis shows the frame number (Frame No.) and the vertical axis shows the lattice spacing (d [nm]). Also, in Figure 11A, the points are shown in darker colors when the spot intensity is higher and in lighter colors when the intensity is lower.
[0115] The change in the spot angle (Angle) for each frame of sample A1 is shown in Figure 11B. In Figure 11B, the horizontal axis shows the frame number (Frame No.) and the vertical axis shows the spot angle (Angle [°]). In addition, each point in Figure 11B is shown in a darker color when the spot intensity (Intensity) is higher, and in a lighter color when the intensity is lower.
[0116] As shown in FIG. 11A, in sample A1, the first spot was observed in the region where the lattice spacing (d) was 0.25 nm to 0.35 nm, and the second spot was observed in the region where the lattice spacing (d) was 0.15 nm to 0.20 nm. As shown in FIG. 11A, the first spot was observed continuously regardless of the measurement position, whereas the second spot was observed discretely. It is presumed that the position where the second spot was observed is a region with relatively high crystallinity compared to other positions. From this, it can be confirmed that the metal oxide film does not have uniform crystallinity, but has a mixture of regions with relatively high crystallinity and regions with relatively low crystallinity.
[0117] As shown in Fig. 11B, the spot has almost no angle dependence in sample A1, which suggests that most of the crystalline regions in sample A1 are randomly oriented without any orientation.
[0118] Next, FIG. 12A shows the change in lattice spacing (d) for each frame of sample A6, and FIG. 12B shows the change in spot angle for each frame.
[0119] In FIG. 12A, the second spots observed in the region where the lattice spacing (d) is 0.15 nm to 0.20 nm are continuously observed regardless of the position (frame), so it can be confirmed that sample A6 has extremely high crystallinity compared to sample A1. In addition, when focusing on the first spots observed in the region where the lattice spacing (d) is 0.25 nm to 0.35 nm, it can be confirmed that a region with small variation (for example, a range from 0 to 200 frames) and a region with large variation (for example, a range from 300 to 500 frames) appear alternately. In addition, in the region where the variation of the first spots is small, the variation of the second spots also tends to be small. From this, it is inferred that a crystal region with a large size exists in the metal oxide film.
[0120] Furthermore, according to Fig. 12B, in the region in Fig. 12A where the variation of the first spots is small, it can be confirmed that the spots are observed discretely at intervals of about 30 degrees. Also, looking at Fig. 9A, it can be seen that six first spots and six second spots outside of them are observed to be located at the vertices of a regular hexagon, and an electron beam diffraction pattern having six-fold symmetry is shown. From this, it is inferred that a single crystal region having six-fold symmetry is observed in the region in Fig. 12A and Fig. 12B where the variation of the first spots is small.
[0121] In this manner, according to the evaluation method of one aspect of the present invention, the crystallinity of metal oxide films can be evaluated and compared with high accuracy.
[0122] [X-ray diffraction] Next, X-ray diffraction (XRD) analysis was carried out on sample A1 to sample A6.
[0123] The XRD analysis was performed using the GIXRD (Grazing-Incidence XRD) method, which is a type of out-of-plane method. The GIXRD method is also called the thin film method or the Seemann-Bohlin method. The GIXRD method is a method in which the incidence angle of X-rays is fixed at a very shallow angle, and the angle of a detector provided opposite to the X-ray source is changed to measure the X-ray diffraction intensity. In this embodiment, the incidence angle is set to 0.70 degrees. In addition, CuKα rays with a wavelength of 0.15418 nm are used as the X-ray source, the scanning range is 2θ=15 degrees to 70 degrees, and the step width is 0.01 degrees.
[0124] The XRD measurement results of samples A1 to A3 are shown in Figures 13A to 13C, and the XRD measurement results of samples A4 to A6 are shown in Figures 14A to 14C.
[0125] 13A to 14C, the horizontal axis represents 2θ, and the vertical axis represents intensity. In addition, in FIG. 13A to FIG. 14C, 2θ=33 degrees (written as deg.) and 2θ=55 degrees are indicated by dashed lines as auxiliary lines.
[0126] As shown in Figures 13A to 14C, diffraction peaks were observed in the vicinity of 2θ = 33 degrees and 2θ = 55 degrees in all samples. The diffraction peak in the vicinity of 2θ = 33 degrees corresponds to a lattice spacing (d) of about 0.27 nm, and is considered to correspond to the first peak in the above-mentioned electron beam diffraction. In addition, a peak was observed in the vicinity of 2θ = 55 degrees. The sharp peak observed in the vicinity of 2θ = 51 degrees is a peak due to diffraction from the silicon wafer, which is the substrate.
[0127] For the diffraction peak observed in each sample near 2θ=33 degrees, the angle (2θ) of the apex of the diffraction peak was calculated by fitting a Lorentzian function. The least squares method was used for fitting the Lorentzian function. Enlarged views of Figures 13A, 13B, and 13C are shown in Figures 15A, 15B, and 15C. Enlarged views of Figures 14A, 14B, and 14C are shown in Figures 16A, 16B, and 16C. The angle (2θ) of the apex of the diffraction peak in each sample is shown in Figure 17. In Figure 17, the horizontal axis represents the oxygen flow rate ratio (O 2 / (Ar+O 2 17 shows the diffraction peak angle (2θ [deg.]) on the vertical axis, and the diffraction peak angle (2θ [deg.]) on the vertical axis. In addition, in Fig. 17, the samples with the substrate temperature set to room temperature (Tsub = RT) are plotted with circles, and the samples with the substrate temperature set to 100°C (Tsub = 100°C) are plotted with triangles.
[0128] As shown in Figures 15A to 16C and Figure 17, as the oxygen flow rate ratio during deposition of the metal oxide film increases, the 2θ of the apex of the diffraction peak tends to decrease. In addition, as the substrate temperature during deposition of the metal oxide film increases, the 2θ of the apex of the diffraction peak tends to decrease. This is because the crystallinity of the metal oxide film increases, and the diffraction peak near 2θ = 31 degrees (InGaZnO 4 This is presumably due to an increase in the intensity of the (009) peak in the crystal.
[0129] As shown in Fig. 17, information regarding the crystallinity of a metal oxide film can be obtained by XRD analysis. Therefore, by combining the evaluation method using electron beam diffraction described above with the evaluation method using XRD exemplified here to perform a multi-faceted analysis, more detailed information regarding the crystallinity of a metal oxide film can be obtained.
[0130] [Stability of nc film] In this section, we explain the stability of metal oxide films with extremely small crystalline regions (hereafter also referred to as nc films) using the results of first-principles calculations.
[0131] In order to explain the stability of the nc film, two calculation models (calculation model 1A and calculation model 2A) were prepared. Calculation model 1A is a calculation model with a crystalline region, and is a calculation model that mimics the nc film. Calculation model 2A is a calculation model without a crystalline region, and is a calculation model that mimics the amorphous film. The crystalline region will be described later.
[0132] [How to create calculation model 1A] A method for creating the calculation model 1A will be described below.
[0133] First, a hexagonal columnar region (called a crystal region) is cut out from the crystal structure of an In-Ga-Zn oxide with an atomic ratio of In:Ga:Zn:O=1:1:1:4, and the crystal region is placed at the center of the calculation model. The number of atoms placed in the crystal region is 87. Hereinafter, the atoms located in the crystal region refer to the 87 atoms placed in the crystal region. In addition, one or more of the atoms located in the crystal region may move to the periphery of the crystal region by a calculation performed later.
[0134] Next, a plurality of In atoms, a plurality of Ga atoms, a plurality of Zn atoms, and a plurality of O atoms are randomly arranged on the periphery of the crystal region. The numbers of In atoms, Ga atoms, Zn atoms, and O atoms arranged on the periphery, and the size of the periphery are set so that the atomic ratio of the atoms arranged on the crystal region and the periphery is In:Ga:Zn:O=1:1:1:4, and the density of the calculation model is 6.1 g / cm. 3 The number of atoms arranged on the periphery is 291. Therefore, the number of atoms included in the calculation model is 378. In addition, one or more of the atoms arranged on the periphery may move to the crystal region by a calculation performed later.
[0135] Next, the coordinates of the atoms located in the crystal region are fixed, and calculations are performed to melt the outer periphery. Specifically, the temperature is set to 3500 K, the time step size is set to 1 fs, and the number of steps is set to 6000. Hereinafter, calculations performed by setting the temperature, time step size, and number of steps may be referred to as first-principles molecular dynamics calculations or quantum molecular dynamics calculations.
[0136] The first-principles calculation software VASP (The Vienna Ab initio simulation package) was used for the calculation. Calculation conditions other than the above-mentioned conditions are shown in Table 2. In the above-mentioned first-principles molecular dynamics calculation, the calculation conditions are set to Condition 1 shown in Table 2.
[0137] [Table 2]
[0138] The electronic state pseudopotential was generated by the Projector Augmented Wave (PAW) method, and the functional was GGA / PBE (Generalized-Gradient-Approximation / Perdew-Burke-Ernzerhof).
[0139] In the first-principles molecular dynamics calculation performed in this embodiment and in the calculation for optimizing the structure of the calculation model (also called optimization calculation), which will be described later, the 3d state or 4d state is not considered as a valence band in the potentials of In, Ga, and Zn. Also, the lattice vectors (axis lengths and angles between axes) of the calculation model are fixed. That is, the first-principles molecular dynamics calculation is performed under conditions (NVT ensemble) where the number of particles (N), volume (V), and temperature (T) are constant. Also, in the first-principles molecular dynamics calculation, a Nose-Hoover thermostat is used as a method for controlling the temperature.
[0140] Next, a calculation is performed to cool the melted outer peripheral part to a temperature of 500K. The cooling rate is set to 500K / ps. Specifically, first, the coordinates of the atoms located in the crystal region are fixed, the time step width is set to 1 fs, the number of steps is set to 1000, and other calculation conditions are set to Condition 1 shown in Table 2. Then, for the calculation model obtained by the calculation to melt the outer peripheral part, a first-principles molecular dynamics calculation is performed with a temperature set to 3500K. Next, for the calculation model obtained after the calculation, a first-principles molecular dynamics calculation is performed with a temperature set to 3000K. Next, for the calculation model obtained after the calculation, a first-principles molecular dynamics calculation is performed with a temperature set to 2500K. Next, for the calculation model obtained after the calculation, a first-principles molecular dynamics calculation is performed with a temperature set to 2000K. Next, for the calculation model obtained after the calculation, a first-principles molecular dynamics calculation is performed with a temperature set to 1500K. Next, for the calculation model obtained after the calculation, a first-principles molecular dynamics calculation is performed with a temperature set to 1000K. Next, a first-principles molecular dynamics calculation is performed on the calculation model obtained after the calculation, with the temperature set to 500 K. This completes the calculation for cooling the outer periphery.
[0141] Next, calculations are performed to relax the structure of the cooled peripheral part. Specifically, for the calculation model obtained in the calculation to cool the peripheral part, the coordinates of the atoms located in the crystalline region are fixed, the temperature is set to 300 K, the time step size is set to 1 fs, the number of steps is set to 5000, and other calculation conditions are set to Condition 1 in Table 2, and ab initio molecular dynamics calculations are performed.
[0142] Next, the calculation conditions are set to Condition 2 shown in Table 2, and the coordinates of the atoms located in the crystalline region are fixed for the calculation model obtained by the calculation for relaxing the structure of the periphery, and a calculation is performed to optimize the structure of the periphery. After that, the coordinates of the atoms located in the periphery and the coordinates of one In atom present at the center of the crystalline region are fixed for the calculation model obtained after the calculation, and a calculation is performed to optimize the structure of the crystalline region. After that, the coordinates of only the In atom are fixed for the calculation model obtained after the calculation, and a calculation is performed to optimize the structure of the entire calculation model (crystalline region and periphery). After that, the calculation conditions are set to Condition 3 shown in Table 2, and the coordinates of only the In atom are fixed for the calculation model obtained after the calculation, and a calculation is performed to optimize the structure of the entire calculation model.
[0143] A calculation model 1A is created by the above method. The created calculation model 1A is shown in Figs. 18A to 18D. Figs. 18A and 18C are diagrams showing an overall image of the calculation model 1A. Figs. 18B and 18D are diagrams showing the crystal region of the calculation model 1A. Figs. 18A and 18B are diagrams showing the side view of the hexagonal columnar region, and Figs. 18C and 18D are diagrams showing the top view of the hexagonal columnar region.
[0144] [How to create calculation model 2A] The method for creating the calculation model 2A will be described below. The calculation conditions shown in Table 2 are used for the calculations for creating the calculation model 2A.
[0145] First, calculations are performed to melt the crystal region and the periphery of calculation model 1 A. Specifically, calculation model 1 A is prepared, and ab initio molecular dynamics calculations are performed without fixing the coordinates of all atoms, with the temperature set to 3500 K, the time step size to 1 fs, the number of steps to 6000, and other calculation conditions set to Condition 1 in Table 2.
[0146] Next, a calculation is performed to cool the entire melted calculation model to a temperature of 500K. The cooling rate is set to 500K / ps. Specifically, first, the coordinates of all atoms are not fixed, the time step width is set to 1fs, the number of steps is set to 1000, and other calculation conditions are set to Condition 1 shown in Table 2. Then, a first-principles molecular dynamics calculation is performed on the calculation model obtained by the calculation to melt the crystal region and the outer periphery, with the temperature set to 3500K. Next, a first-principles molecular dynamics calculation is performed on the calculation model obtained after the calculation, with the temperature set to 3000K. Next, a first-principles molecular dynamics calculation is performed on the calculation model obtained after the calculation, with the temperature set to 2500K. Next, a first-principles molecular dynamics calculation is performed on the calculation model obtained after the calculation, with the temperature set to 2000K. Next, a first-principles molecular dynamics calculation is performed on the calculation model obtained after the calculation, with the temperature set to 1500K. Next, a first-principles molecular dynamics calculation is performed on the calculation model obtained after the calculation, with the temperature set to 1000K. Next, a first-principles molecular dynamics calculation is performed on the calculation model obtained after the calculation, with the temperature set to 500 K. This completes the calculation for cooling the entire calculation model.
[0147] Next, calculations are performed to relax the structure of the entire cooled calculation model. Specifically, for the calculation model obtained by the calculation to cool the entire calculation model, the coordinates of all atoms are not fixed, and a first-principles molecular dynamics calculation is performed under the following conditions: temperature 300 K, time step size 1 fs, number of steps 5000, and other calculation conditions are set to Condition 1 in Table 2.
[0148] Next, the calculation conditions are set to Condition 2 shown in Table 2, and a calculation is performed to optimize the structure of the entire calculation model without fixing the coordinates of all atoms for the calculation model obtained by the calculation to relax the entire calculation model. After that, the calculation conditions are set to Condition 3 shown in Table 2, and a calculation is performed to optimize the structure of the entire calculation model without fixing the coordinates of all atoms for the calculation model obtained after the calculation.
[0149] In this manner, calculation model 2A is created. An overall image of calculation model 2A is shown in FIG.
[0150] The total energy was calculated for each of the calculation models 1A and 2A created by the above method, and compared. Specifically, the calculation conditions were set to condition 3 shown in Table 2, and for calculation model 1A, the coordinates of only one In atom present at the center of the crystal region were fixed, and a one-point calculation was performed, while for calculation model 2A, the coordinates of all atoms were not fixed, and a one-point calculation was performed. The total energies calculated in these calculations were compared.
[0151] As a result of the above calculation, the value of the total energy of the calculation model 1A was smaller than that of the calculation model 2A, specifically, 6.83 eV smaller. Therefore, it can be seen that the calculation model 1A having a crystalline region is more stable than the calculation model 2A having no crystalline region. In other words, it is suggested that the nc film is stabilized by having a crystalline region.
[0152] Next, a calculation model 3A is prepared for comparison with the calculation model 1A. The structure of the calculation model 3A is a single crystal structure.
[0153] Introduction, InGaZnO 4 The single crystal structure (space group is R-3m) has an atomic ratio of In:Ga:Zn:O=1:1:1:4 and a density of 6.36 g / cm 3A calculation model including 112 atoms is prepared. Next, the k-point grid is set to 2x2x3, and other calculation conditions are set to Condition 3 shown in Table 2, and calculations are performed to optimize the atomic coordinates of the calculation model. Through the above steps, calculation model 3A is created.
[0154] The total energy is calculated for the calculation model 3A created by the above method. Specifically, a one-point calculation is performed by setting the k-point grid to 2×2×3 and setting other calculation conditions to condition 3 shown in Table 2. The total energy calculated by this calculation is multiplied by 3.375 (=378 / 112) to obtain the total energy value of the calculation model of the single crystal structure.
[0155] As a result of the above calculation, the total energy value of the calculation model of the single crystal structure was smaller than that of the calculation model 1A, specifically, it was 54.88 eV smaller. In other words, it is found that the film becomes energetically stable by improving the crystallinity in the film.
[0156] From the above, although calculation model 1A has a higher energy than the calculation model of the single crystal structure, it is more stable than calculation model 2A, suggesting that the presence of crystalline regions contributes to the stabilization of the nc film.
[0157] This concludes the explanation of the stability of the nc membrane.
[0158] [Thermal stability of nc films] In this section, we explain the thermal stability of the nc film using the results of first-principles calculations. The thermal stability of the nc film is evaluated using the internal energy, which will be described later.
[0159] Here, the internal energy will be explained. In this specification, the internal energy U is calculated using the following formula.
[0160]
number
[0161] Here, M I is the mass of the I-th atomic nucleus (I is a natural number), m is the mass of the electron, and v I is the velocity of the I-th nucleus. In other words, the first term on the right-hand side of the above equation represents the kinetic energy of the nucleus, and the third term on the right-hand side of the above equation represents the kinetic energy of the electron.
[0162] Also, Z I is the charge of the I-th nucleus, and e is the charge of the electron. Also, r IJ is the distance between the I-th nucleus and the J-th nucleus (J is an integer greater than I), and r ij is the distance between the i-th electron (i is a natural number) and the j-th electron (j is an integer greater than i). In other words, the second term on the right-hand side of the above equation is the potential energy related to the interaction between nuclei, the fourth term on the right-hand side of the above equation is the potential energy related to the interaction between electrons, and the fifth term on the right-hand side of the above equation is the potential energy related to the interaction between nuclei and electrons.
[0163] From the above, the internal energy U is calculated as the sum of the kinetic energy and the potential energy.
[0164] The stability of a phase in an equilibrium state is described by the Helmholtz free energy F. Here, the Helmholtz free energy F is the value obtained by subtracting the product of the temperature T and the entropy S from the internal energy U (F=U-TS). However, since it is difficult to evaluate the entropy S, in this specification, the internal energy U is used to verify the thermodynamic phase stability.
[0165] This concludes the explanation of the internal energy. Next, we will explain the specific method for evaluating the thermal stability of the nc film.
[0166] For each of the above-mentioned calculation models 1A and 2A, the temperature is set to 300K, 673K, 1000K, 1500K, or 2000K, and a first-principles molecular dynamics calculation is performed. When calculation model 1A is used, the coordinates of one In atom present at the center of the crystal region are fixed, and the first-principles molecular dynamics calculation is performed. When calculation model 2A is used, the coordinates of all atoms are not fixed, and the first-principles molecular dynamics calculation is performed. In the first-principles molecular dynamics calculation, the time step size is set to 1 fs, the number of steps is set to 10,000, and other calculation conditions are set to Condition 2 shown in Table 2.
[0167] Next, for each of the above-mentioned calculation models 1A and 2A, the internal energy is calculated for each calculation model (10 types in total) after first-principles molecular dynamics calculations are performed at each temperature. Specifically, the average value of the internal energy from step 9001 to 10000 is calculated. Note that the average value of the internal energy obtained by performing first-principles molecular dynamics calculations for calculation model 1A at a temperature of 300K is set as the reference (0.0 eV), and this is referred to as the average energy.
[0168] The relationship between temperature and the average energy calculated by the above method is shown in Figure 20A. In Figure 20A, the horizontal axis is temperature [K] and the vertical axis is average energy [eV]. The plots shown by black diamonds in Figure 20A are plots of average energy when calculation model 1A is used, and the plots shown by white squares are plots of average energy when calculation model 2A is used.
[0169] Next, for each of the calculation models (total of five types) obtained by performing first-principles molecular dynamics calculations at each temperature setting for calculation model 1A, calculation conditions are set to Condition 2 shown in Table 2, and calculations are performed to optimize the structure of the calculation models. Note that this optimization calculation is performed by fixing the coordinates of one In atom present at the center of the crystal region. Thereafter, for each of the calculation models (total of five types) obtained by performing this optimization calculation, calculation conditions are set to Condition 3 shown in Table 2, and calculations are performed to optimize the structure of the calculation models.
[0170] Some of the calculation models (5 types in total) obtained by the above calculation are shown in Fig. 19A to Fig. 19E. Fig. 19A to Fig. 19E show the arrangement of 87 atoms arranged in the crystal region before placing atoms on the periphery of the crystal region in the calculation model. Fig. 19A is a calculation model obtained by performing first-principles molecular dynamics calculations and optimization calculations with the temperature set to 300K, Fig. 19B is a calculation model obtained by performing first-principles molecular dynamics calculations and optimization calculations with the temperature set to 673K, Fig. 19C is a calculation model obtained by performing first-principles molecular dynamics calculations and optimization calculations with the temperature set to 1000K, Fig. 19D is a calculation model obtained by performing first-principles molecular dynamics calculations and optimization calculations with the temperature set to 1500K, and Fig. 19E is a calculation model obtained by performing first-principles molecular dynamics calculations and optimization calculations with the temperature set to 2000K.
[0171] 19A to 19D, the lattice arrangement of the crystal region is maintained in the calculation model obtained by performing the first-principles molecular dynamics calculation and the optimization calculation with the temperature set to 1500 K or less. Also, in FIG. 19E, the crystal structure is destroyed in the calculation model obtained by performing the first-principles molecular dynamics calculation and the optimization calculation with the temperature set to 2000 K. Also, in FIG. 19D, the lattice arrangement of the crystal region is maintained in the calculation model obtained by performing the first-principles molecular dynamics calculation and the optimization calculation with the temperature set to 1500 K, but compared to the calculation model obtained by performing the first-principles molecular dynamics calculation and the optimization calculation with the temperature set to 1000 K, the atomic arrangement is greatly disturbed, and there are signs that the crystal structure is starting to collapse.
[0172] Here, the difference between the average energy of calculation model 1A and the average energy of calculation model 2A is calculated at each temperature, and the thermal stability of calculation model 1A is compared with that of calculation model 2A. The relationship between temperature and the average energy of calculation model 1A and calculation model 2A is as shown in FIG. 20A.
[0173] The relationship between temperature and the value obtained by subtracting the average energy of calculation model 2A from the average energy of calculation model 1A (also called the average energy difference) is shown in Figure 20B. In Figure 20B, the horizontal axis is temperature [K] and the vertical axis is the average energy difference [eV].
[0174] From FIG. 20B, when the temperature is set to 2000K, the difference in average energy is close to zero, and the average energy when using the calculation model 1A is almost equal to the average energy when using the calculation model 2A. On the other hand, when the temperature is set to 1500K or less, the difference in average energy is a negative value at any temperature, and the average energy when using the calculation model 1A is smaller than the average energy when using the calculation model 2A. In other words, at a temperature where the lattice arrangement of the crystalline regions is maintained, it is estimated that the calculation model having the crystalline regions is more stable against heat than the calculation model without the crystalline regions. Therefore, it is suggested that the thermal stability of the film is improved by the presence of the crystalline regions, except in the high temperature range.
[0175] This concludes the explanation of the thermal stability of the nc film.
[0176] [H in nc film O Ease of generating In this section, we explain the ease of defect formation in nc films using the results of first-principles calculations. Specifically, defects in which hydrogen is inserted into oxygen vacancies (hereafter referred to as V O H or H O The formation energy of this reaction, sometimes referred to as , is calculated using first-principles calculations.
[0177] H O In some cases, electrons that act as carriers are generated. For this reason, H O When H is generated, the electrical characteristics of the transistor change, for example, the transistor tends to be normally on. O It is preferable that the production of is suppressed.
[0178] Here, the defect formation energy will be explained. In this specification, the defect formation energy is calculated using the following formula. It can be said that the smaller the defect formation energy is, the more easily the defect is formed.
[0179]
number
[0180] Here, E form (defect) is the defect formation energy, E(defect) is the total energy of the calculation model including one defect, E(no defect) is the total energy of the calculation model including no defect, atom X is the atom that is increased or decreased by forming a defect, μ(X) is the chemical potential of atom X, and n X is the number of atoms X that are increased or decreased. For example, if the defect is H O X is an oxygen atom (O) or a hydrogen atom (H), and nO is -1, and n H is +1.
[0181] In addition, the chemical potential μ(O) of the oxygen atom and the chemical potential μ(H) of the hydrogen atom are calculated using the following formula.
[0182]
number
[0183] Here, E(O 2 ) is an oxygen molecule (O 2 ) and E(H 2 O) is a water molecule (H 2 O).
[0184] In addition, E(O 2 ) is one O 2 Molecules at 1 nm 3 The calculation conditions are set to Condition 2 in Table 2. 2 It is calculated by performing a calculation to optimize the molecular structure, and then performing a single point calculation on the calculation model obtained after the calculation. Also, E(H 2 O) is one H 2 O molecule 1 nm 3 The calculation conditions are set to Condition 2 in Table 2, and H 2 It is calculated by performing calculations to optimize the structure of the O molecule, and then performing a single-point calculation on the calculation model obtained after the calculations.
[0185] The above is an explanation of the defect formation energy.
[0186] In order to calculate the formation energy of defects, a calculation model 3A was prepared. The method for creating the calculation model 3A will be described below. The calculation conditions shown in Table 2 are used for the calculation to create the calculation model 3A.
[0187] First, calculation model 1A is prepared, and calculations are performed to relax the structure of the outer periphery of calculation model 1A. Specifically, calculation model 1A is prepared, the coordinates of the atoms located in the crystal region are fixed, and a first-principles molecular dynamics calculation is performed with the temperature set to 1000 K, the time step size to 1 fs, the number of steps to 10000, and other calculation conditions set to Condition 2 shown in Table 2.
[0188] Next, while the calculation conditions are set to Condition 2 shown in Table 2, the coordinates of the atoms located in the crystalline region are fixed for the calculation model obtained by the calculation for relaxing the structure of the circumferential portion, and a calculation is performed to optimize the structure of the circumferential portion. After that, the coordinates of the atoms located in the circumferential portion and the coordinates of one In atom present at the center of the crystalline region are fixed for the calculation model obtained after the calculation, and a calculation is performed to optimize the structure of the crystalline region. After that, the coordinates of one In atom present at the center of the crystalline region are fixed for the calculation model obtained after the calculation, and a calculation is performed to optimize the structure of the entire calculation model. After that, the calculation conditions are set to Condition 3 shown in Table 2, and the coordinates of one In atom present at the center of the crystalline region are fixed for the calculation model obtained after the calculation, and a calculation is performed to optimize the structure of the entire calculation model.
[0189] Using the above method, calculation model 3A is created.
[0190] Using the calculation model 3A created by the above method, H O Specifically, by replacing one oxygen atom in the calculation model 3A with one hydrogen atom, the formation energy of H O A calculation model containing one oxygen atom is prepared. Note that the number of oxygen atoms in calculation model 3A is 216, so H O There are 216 computational models, each of which contains one H O The calculation model that does not include is calculation model 3A itself.
[0191] H O A computational model with one OFor each of the calculation models that do not include H, the calculation conditions are set to Condition 3 in Table 2, and calculations are performed to optimize the structure of the entire calculation model. O The total energy of the calculation model including one defect is defined as E(defect), and the energy obtained after the calculation is H O The total energy of the calculation model that does not include H is defined as E(no defect). O By performing the calculation on a computational model that includes one O may be converted to other defects (e.g., oxygen vacancies and hydrogen).
[0192] Using E(defect) and E(no defect) calculated by the above method, H O Calculate the energy of formation of H O The energy of formation of is shown in Fig. 21. In Fig. 21, the horizontal axis is the distance from the In atom at the center of the crystal region to the H atom placed in the calculation model before the calculation to optimize the structure of the entire calculation model is performed. O The vertical axis is the distance to the target (Distance) [Å], and the vertical axis is H O The formation energy [eV] of H is shown in Fig. 21. The black squares (■) in Fig. 21 indicate the formation energy of H located in the region near In in the crystalline region (also called the core region of the crystal). O The white squares in Fig. 21 indicate the formation energy of H located in the region other than the core region of the crystal (also called the shell region of the crystal). O The cross marks in Figure 21 indicate the formation energy of H O The number of oxygen atoms located in the core region of the crystal is 12, and the number of oxygen atoms located in the shell region of the crystal is 38.
[0193] H located in the core region of the crystal O , H located in the shell region of the crystal O , H located on the outer periphery O The average formation energies of were 2.75 eV, 2.60 eV, and 2.14 eV, respectively.
[0194] As shown in Fig. 21, the shell region of the crystal has a larger amount of H than the core region of the crystal. O The variation in the formation energy of H O The value of the formation energy of H is small. O This is presumably because the structure is distorted even in the crystalline region near the interface between the crystalline region and the outer periphery.
[0195] In addition, compared to the crystalline regions (core and shell regions of the crystal), the H O The variation in the formation energy of H O The value of the formation energy of H is small. O This is presumably because the peripheral area with low crystallinity has a larger fluctuation in bond length and a larger number of oxygen atoms with weaker bond strength with metal atoms than the crystalline area.
[0196] From the above, the crystalline region is H O In the region with low crystallinity (the outer periphery), H O Therefore, the presence of crystalline regions suggests that H O Therefore, by using the nc film in a transistor, the change in the electrical characteristics of the transistor can be suppressed.
[0197] The above is the H O This explains the ease of generating
[0198] [Metal oxide structures] Oxide semiconductors (metal oxides) are classified into single-crystal oxide semiconductors and other non-single-crystal oxide semiconductors, such as c-axis aligned crystalline oxide semiconductors (CAAC-OS), polycrystalline oxide semiconductors, nanocrystalline oxide semiconductors (nc-OS), amorphous-like oxide semiconductors (a-like OS), and amorphous oxide semiconductors.
[0199] CAAC-OS has a c-axis orientation and a distorted crystal structure in which multiple nanocrystals are connected in the ab-plane direction. The distortion refers to a portion where the lattice orientation changes between a region with a uniform lattice arrangement and a region with a different uniform lattice arrangement in the region where multiple nanocrystals are connected.
[0200] Nanocrystals are basically hexagonal, but may be non-regular hexagonal. In addition, the lattice arrangement of the distortion may be pentagonal, heptagonal, or the like. In the CAAC-OS, it is difficult to confirm clear grain boundaries even in the vicinity of the distortion. That is, it is found that the formation of grain boundaries is suppressed by the distortion of the lattice arrangement. This is because the CAAC-OS can tolerate distortion because the arrangement of oxygen atoms in the ab-plane direction is not dense, and the bond distance between atoms changes due to the substitution of metal elements. A crystal structure in which clear grain boundaries are confirmed is called a polycrystal. The grain boundaries are likely to become recombination centers, trapping carriers and causing a decrease in the on-current of a transistor or a decrease in the field effect mobility. Therefore, the CAAC-OS in which clear grain boundaries are not confirmed is one of the crystalline oxides having a crystal structure suitable for the semiconductor layer of a transistor. In addition, a structure containing Zn is preferable for forming the CAAC-OS. For example, In-Zn oxide and In-Ga-Zn oxide are preferable because they can suppress the generation of crystal grain boundaries more effectively than In oxide.
[0201] CAAC-OS also tends to have a layered crystal structure (also referred to as a layered structure) in which a layer containing indium and oxygen (hereinafter, In layer) and a layer containing element M, zinc, and oxygen (hereinafter, (M, Zn) layer) are stacked. Note that indium and element M can be substituted for each other, and when element M in an (M, Zn) layer is substituted for indium, it can also be expressed as an (In, M, Zn) layer. When indium in an In layer is substituted for element M, it can also be expressed as an (In, M) layer.
[0202] CAAC-OS is a metal oxide with high crystallinity. On the other hand, it is difficult to confirm clear crystal boundaries in CAAC-OS, so it can be said that the decrease in electron mobility caused by crystal boundaries is unlikely to occur. In addition, since the crystallinity of metal oxides can be decreased by the inclusion of impurities or the generation of defects, CAAC-OS can be said to be a metal oxide with few impurities and defects (oxygen vacancies, etc.). Therefore, metal oxides with CAAC-OS have stable physical properties. As a result, metal oxides with CAAC-OS are resistant to heat and highly reliable.
[0203] The nc-OS has periodic atomic arrangement in a microscopic region (for example, a region of 1 nm to 10 nm, particularly a region of 1 nm to 3 nm). In addition, the nc-OS does not show regularity in the crystal orientation between different nanocrystals. Therefore, no orientation is seen throughout the film. Therefore, depending on the analysis method, the nc-OS may be indistinguishable from an a-like OS or an amorphous oxide semiconductor.
[0204] In-Ga-Zn oxide (hereinafter referred to as IGZO), a type of metal oxide containing indium, gallium, and zinc, may have a stable structure when made into the above-mentioned nanocrystals. In particular, since IGZO tends to have difficulty in crystal growth in the atmosphere, it may be structurally more stable when made into small crystals (for example, the above-mentioned nanocrystals) rather than large crystals (here, crystals of several mm or several cm).
[0205] The a-like OS is a metal oxide having a structure between the nc-OS and an amorphous oxide semiconductor. The a-like OS has a pore or low-density region. That is, the a-like OS has lower crystallinity than the nc-OS and CAAC-OS.
[0206] Oxide semiconductors (metal oxides) have a variety of structures and each structure has different characteristics. The oxide semiconductor of one embodiment of the present invention may include two or more of an amorphous oxide semiconductor, a polycrystalline oxide semiconductor, an a-like OS, an nc-OS, and a CAAC-OS.
[0207] Alternatively, a cloud-aligned composite (CAC)-OS may be used as the non-single-crystal oxide semiconductor. Note that the CAC-OS relates to a material structure.
[0208] [Metal oxide composition] CAC-OS is a material in which some of the material has a conductive function and some of the material has an insulating function, and the material as a whole functions as a semiconductor. When CAC-OS is used in the active layer of a transistor, the conductive function is a function of allowing electrons (or holes) to flow as carriers, and the insulating function is a function of not allowing electrons to flow as carriers. By making the conductive function and the insulating function act in a complementary manner, it is possible to give the CAC-OS a switching function (on / off function). By separating the respective functions in CAC-OS, it is possible to maximize both functions.
[0209] The CAC-OS has a conductive region and an insulating region. The conductive region has the above-mentioned conductive function, and the insulating region has the above-mentioned insulating function. In the material, the conductive region and the insulating region may be separated at the nanoparticle level. In addition, the conductive region and the insulating region may be unevenly distributed in the material. In addition, the conductive region may be observed to be connected in a cloud shape with a blurred periphery.
[0210] In addition, in the CAC-OS, the conductive regions and the insulating regions may each be dispersed in the material with a size of 0.5 nm or more and 10 nm or less, preferably 0.5 nm or more and 3 nm or less.
[0211] In addition, the CAC-OS is composed of components having different band gaps. For example, the CAC-OS is composed of a component having a wide gap due to an insulating region and a component having a narrow gap due to a conductive region. In this configuration, when carriers are caused to flow, the carriers mainly flow in the component having the narrow gap. In addition, the component having the narrow gap acts complementarily to the component having the wide gap, and carriers also flow in the component having the wide gap in conjunction with the component having the narrow gap. Therefore, when the above-mentioned CAC-OS is used in the channel formation region of a transistor, a high current driving force, that is, a large on-current and a high field effect mobility can be obtained in the on-state of the transistor.
[0212] That is, CAC-OS can also be called a matrix composite or a metal matrix composite.
[0213] In addition, when focusing on the crystal structure, oxide semiconductors may be classified differently from the above. Here, the classification of crystal structures in oxide semiconductors will be described with reference to Fig. 22A. Fig. 22A is a diagram for explaining the classification of crystal structures of oxide semiconductors, typically IGZO (metal oxide containing In, Ga, and Zn).
[0214] As shown in FIG. 22A, IGZO is broadly classified into Amorphous, Crystalline, and Crystal. Amorphous includes completely amorphous. Crystalline includes CAAC, nc, and CAC. Crystalline excludes single crystal, poly crystal, and completely amorphous. Crystal includes single crystal and poly crystal.
[0215] The structure in the bold frame shown in FIG. 22A is an intermediate state between Amorphous and Crystal, and belongs to a new boundary region (New crystalline phase). This structure is in the boundary region between Amorphous and Crystal. In other words, this structure can be said to be a structure that is completely different from Amorphous, which is energetically unstable, or Crystal.
[0216] The crystal structure of the film or substrate can be evaluated using an X-ray diffraction (XRD) image. Here, XRD spectra of quartz glass and IGZO (also called crystalline IGZO) having a crystal structure classified as Crystalline are shown in Fig. 22B and Fig. 22C. Fig. 22B shows the XRD spectrum of quartz glass, and Fig. 22C shows the XRD spectrum of crystalline IGZO. The composition of the crystalline IGZO shown in Fig. 22C is near In:Ga:Zn=4:2:3 [atomic ratio]. The thickness of the crystalline IGZO shown in Fig. 22C is 500 nm.
[0217] As shown by the arrows in FIG. 22B, the shape of the peak in the XRD spectrum of silica glass is almost symmetric. On the other hand, as shown by the arrows in FIG. 22C, the shape of the peak in the XRD spectrum of crystalline IGZO is asymmetric. The asymmetric shape of the peak in the XRD spectrum clearly indicates the presence of crystals. In other words, if the shape of the peak in the XRD spectrum is not symmetric, it cannot be said to be amorphous. Note that FIG. 22C clearly shows the crystal phase (IGZO crystal phase) at or near 2θ=31°. It is presumed that the reason why the shape of the peak in the XRD spectrum is asymmetric is due to the crystal phase (microcrystals).
[0218] Specifically, the XRD spectrum of crystalline IGZO shown in FIG. 22C has a peak at or near 2θ=34°. Microcrystals have a peak at or near 2θ=31°. When an oxide semiconductor film is evaluated using an X-ray diffraction image, the spectrum width on the low-angle side is wider than the peak at or near 2θ=34°, as shown in FIG. 22C. This suggests that the oxide semiconductor film contains microcrystals having a peak at or near 2θ=31°.
[0219] The crystal structure of the film can be evaluated from the diffraction pattern (also called the nanobeam electron diffraction pattern) observed by nanobeam electron diffraction (NBED). Figure 22D shows the diffraction pattern of an IGZO film formed at room temperature on the substrate. The IGZO film shown in Figure 22D was formed by sputtering using an oxide target with an In:Ga:Zn=1:1:1 [atomic ratio]. In the nanobeam electron diffraction method, electron diffraction was performed with a probe diameter of 1 nm.
[0220] As shown in Figure 22D, a spot-like pattern, not a halo, is observed in the diffraction pattern of the IGZO film deposited at room temperature. Therefore, it is presumed that the IGZO film deposited at room temperature is in an intermediate state, neither crystalline nor amorphous, and it cannot be concluded that it is in an amorphous state.
[0221] This embodiment mode can be implemented by appropriately combining at least a part of it with other embodiment modes described in this specification.
[0222] (Embodiment 2) In this embodiment, a structure example of a semiconductor device including a metal oxide film according to one embodiment of the present invention will be described below using a transistor as an example.
[0223] [Configuration example 1] [Configuration Example 1-1] FIG. 23A is a top view of the transistor 300, FIG. 23B corresponds to a cross-sectional view of the cut surface taken along dashed line A1-A2 in FIG. 23A, and FIG. 23C corresponds to a cross-sectional view of the cut surface taken along dashed line B1-B2 in FIG. 23A. The dashed line A1-A2 direction corresponds to the channel length direction, and the dashed line B1-B2 direction corresponds to the channel width direction. Note that FIG. 23A omits some of the components of the transistor 300 (such as a gate insulating layer). As with FIG. 23A, the top views of the transistors in the following drawings omit some of the components.
[0224] The transistor 300 is provided over a substrate 302 and includes a conductive layer 304, an insulating layer 306, a semiconductor layer 308, a conductive layer 312a, a conductive layer 312b, and the like. The insulating layer 306 is provided to cover the conductive layer 304. The semiconductor layer 308 has an island shape and is provided over the insulating layer 306. The conductive layers 312a and 312b are in contact with a top surface of the semiconductor layer 308 and are provided apart from each other on the semiconductor layer 308. An insulating layer 314 is provided to cover the insulating layer 306, the conductive layer 312a, the conductive layer 312b, and the semiconductor layer 308, and an insulating layer 316 is provided over the insulating layer 314.
[0225] The metal oxide film described in Embodiment 1 can be used for the semiconductor layer 308.
[0226] There are no significant limitations on the material of the substrate 302, but the substrate must have at least sufficient heat resistance to withstand subsequent heat treatment. For example, a single crystal semiconductor substrate made of silicon or silicon carbide, a polycrystalline semiconductor substrate, a compound semiconductor substrate such as silicon germanium, an SOI substrate, a glass substrate, a ceramic substrate, a quartz substrate, a sapphire substrate, or the like may be used as the substrate 302. Furthermore, any of these substrates on which a semiconductor element is provided may be used as the substrate 302.
[0227] A flexible substrate may be used as the substrate 302, and the semiconductor device may be formed directly on the flexible substrate. Alternatively, a peeling layer may be provided between the substrate 302 and the semiconductor device. The peeling layer can be used to separate the semiconductor device from the substrate 302 after a part or whole of the semiconductor device is completed thereon, and to transfer the semiconductor device to another substrate. In this case, the semiconductor device can be transferred to a substrate having poor heat resistance or a flexible substrate.
[0228] The conductive layer 304 functions as a gate electrode. A part of the insulating layer 306 functions as a gate insulating layer. The conductive layer 312a functions as one of a source electrode and a drain electrode, and the conductive layer 312b functions as the other. A region of the semiconductor layer 308 overlapping with the conductive layer 304 functions as a channel formation region. The transistor 300 is a so-called bottom-gate transistor in which a gate electrode is provided closer to the formation surface than the semiconductor layer 308. Here, the surface of the semiconductor layer 308 opposite to the conductive layer 304 side may be referred to as a back channel side surface. The transistor 300 is a transistor with a so-called channel etch structure in which a protective layer is not provided between the back channel side of the semiconductor layer 308 and the source electrode and drain electrode.
[0229] The semiconductor layer 308 may have a stacked structure of two or more layers. In this case, the semiconductor film constituting the semiconductor layer 308 preferably contains a metal oxide. In the case where the semiconductor layer 308 has a two-layer structure, the semiconductor film located on the back channel side is preferably a film having higher crystallinity than the semiconductor film located on the conductive layer 304 side. This can prevent a part of the semiconductor layer 308 from being etched and lost when the conductive layer 312a and the conductive layer 312b are processed.
[0230] For example, the semiconductor layer 308 preferably contains indium, M (wherein M is one or more selected from gallium, aluminum, silicon, boron, yttrium, tin, copper, vanadium, beryllium, titanium, iron, nickel, germanium, zirconium, molybdenum, lanthanum, cerium, neodymium, hafnium, tantalum, tungsten, and magnesium), and zinc. In particular, M is preferably aluminum, gallium, yttrium, or tin.
[0231] In particular, it is preferable to use an oxide containing indium, gallium, and zinc for the semiconductor layer 308.
[0232] Each of the conductive layers 312a and 312b has a layered structure in which a conductive layer 313a and a conductive layer 313b are layered in this order from the formation surface side.
[0233] The conductive layer 313b is preferably made of a low-resistance conductive material containing copper, silver, gold, aluminum, or the like. In particular, the conductive layer 313b preferably contains copper or aluminum. This allows the conductive layer 312a and the conductive layer 312b to have extremely low resistance.
[0234] The conductive layer 313a can be formed using a conductive material different from that of the conductive layer 313b. For example, the conductive layer 313a is preferably formed using a conductive material containing titanium, tungsten, molybdenum, chromium, tantalum, zinc, indium, platinum, ruthenium, or the like.
[0235] In this manner, by providing the conductive layer 313a between the conductive layer 313b containing copper, aluminum, or the like and the semiconductor layer 308, a metal element contained in the conductive layer 313b can be prevented from diffusing into the semiconductor layer 308, thereby achieving a highly reliable transistor 300. In addition, the conductive layer 313a preferably functions as a barrier layer that prevents oxygen in the semiconductor layer 308 from diffusing into the conductive layer 313b.
[0236] Note that the structure of the conductive layer 312a and the conductive layer 312b is not limited to a two-layer structure, and may be a three-layer structure or a four-layer structure including a conductive layer containing copper, silver, gold, or aluminum. For example, the conductive layer 312a and the conductive layer 312b may be a three-layer structure in which a conductive layer containing a conductive material similar to that of the conductive layer 313a is stacked on the conductive layer 313b. This can suppress oxidation of the top surface of the conductive layer 313b and prevent metal elements contained in the conductive layer 313b from scattering to the surroundings, thereby realizing a highly reliable transistor.
[0237] Any of the above-mentioned conductive materials which can be used for the conductive layer 313a or the conductive layer 313b can be used as the conductive layer 304. In particular, it is preferable to use a conductive material containing copper.
[0238] An insulating material containing an oxide is preferably used for the insulating layer 306 and the insulating layer 314 in contact with the semiconductor layer 308. When the insulating layer 306 and the insulating layer 314 have a stacked structure, an insulating material containing an oxide is used for the layer in contact with the semiconductor layer 308.
[0239] Alternatively, a nitride insulating film such as silicon nitride or aluminum nitride may be used for the insulating layer 306. When an insulating material not containing oxide is used, it is preferable to form a region containing oxygen by performing a treatment for adding oxygen to the upper part of the insulating layer 306. Examples of the treatment for adding oxygen include heat treatment or plasma treatment in an atmosphere containing oxygen, and ion doping treatment.
[0240] The insulating layer 316 functions as a protective layer that protects the transistor 300. For the insulating layer 316, an inorganic insulating material such as silicon nitride, silicon nitride oxide, silicon oxide, silicon oxynitride, aluminum oxide, or aluminum nitride can be used. In particular, using a material through which oxygen does not easily diffuse, such as silicon nitride or aluminum oxide, for the insulating layer 316 is preferable because oxygen can be prevented from being released from the semiconductor layer 308 or the insulating layer 314 to the outside through the insulating layer 316 due to heat or the like applied during a manufacturing process.
[0241] Alternatively, an organic insulating material that functions as a planarizing film may be used as the insulating layer 316. Alternatively, the insulating layer 316 may be a stacked film of a film containing an inorganic insulating material and a film containing an organic insulating material.
[0242] The semiconductor layer 308 may have a pair of low-resistance regions that function as a source region and a drain region and are located in the vicinity of and in contact with the conductive layer 312a and the conductive layer 312b. The regions are part of the semiconductor layer 308 and have a lower resistance than the channel formation region. The low-resistance region can also be referred to as a region with a high carrier concentration or an n-type region. In the semiconductor layer 308, a region that is sandwiched between the pair of low-resistance regions and overlaps with the conductive layer 304 functions as a channel formation region.
[0243] [Configuration Example 1-2] In the following, a configuration example of a transistor that is partially different from the above-mentioned configuration example 1-1 will be described. Note that in the following, a description of parts that overlap with the above-mentioned configuration example 1-1 may be omitted.
[0244] FIG. 24A is a cross-sectional view of the transistor 300A in the channel length direction, and FIG. 24B is a cross-sectional view of the transistor 300A in the channel width direction.
[0245] The transistor 300A differs from configuration example 1-1 mainly in that a conductive layer 320 is provided on an insulating layer 314.
[0246] The conductive layer 320 has a region overlapping with the semiconductor layer 308 with the insulating layer 314 interposed therebetween.
[0247] In the transistor 300A, the conductive layer 304 functions as a first gate electrode (also referred to as a bottom gate electrode), and the conductive layer 320 functions as a second gate electrode (also referred to as a top gate electrode). Part of the insulating layer 314 functions as a second gate insulating layer.
[0248] 24B, the conductive layer 320 may be electrically connected to the conductive layer 304 through an opening 342 provided in the insulating layer 314 and the insulating layer 306. This allows the conductive layer 320 and the conductive layer 304 to be supplied with the same potential, thereby realizing a transistor with high on-state current.
[0249] 24B, in the channel width direction, the conductive layer 304 and the conductive layer 320 preferably extend outward beyond the end of the semiconductor layer 308. In this case, as shown in FIG 24B, the entire semiconductor layer 308 in the channel width direction is covered with the conductive layer 304 and the conductive layer 320.
[0250] With such a structure, the semiconductor layer 308 can be electrically surrounded by an electric field generated by the pair of gate electrodes. In particular, it is preferable to apply the same potential to the conductive layer 304 and the conductive layer 320. This makes it possible to effectively apply an electric field for inducing a channel in the semiconductor layer 308, thereby increasing the on-state current of the transistor 300A. As a result, the transistor 300A can also be miniaturized.
[0251] Note that the conductive layer 304 and the conductive layer 320 may not be connected. In this case, a constant potential may be applied to one of the pair of gate electrodes, and a signal for driving the transistor 300A may be applied to the other. In this case, the threshold voltage when the transistor 300A is driven by the other gate electrode can be controlled by the potential applied to one gate electrode.
[0252] Alternatively, the conductive layer 320 may be electrically connected to either the conductive layer 312a or the conductive layer 312b. In particular, it is preferable that the conductive layer 320 is electrically connected to one of the conductive layers 312a and 312b to which a constant potential is supplied (for example, a source electrode).
[0253] The above is a description of configuration example 1.
[0254] [Configuration example 2] In the following, examples of transistor configurations different from the above configuration example 1 will be described.
[0255] [Configuration Example 2-1] Fig. 25A is a top view of transistor 350, Fig. 25B corresponds to a cross-sectional view of the cut surface taken along dashed line A3-A4 shown in Fig. 25A, and Fig. 25C corresponds to a cross-sectional view of the cut surface taken along dashed line B3-B4 shown in Fig. 25A. The dashed line A3-A4 direction corresponds to the channel length direction, and the dashed line B3-B4 direction corresponds to the channel width direction.
[0256] The transistor 350 is provided over a substrate 352 and includes an insulating layer 353, a semiconductor layer 358, an insulating layer 360, a metal oxide layer 364, a conductive layer 362, an insulating layer 368, and the like. The island-shaped semiconductor layer 358 is provided over the insulating layer 353. The insulating layer 360 is provided in contact with an upper surface of the insulating layer 353 and an upper surface and side surfaces of the semiconductor layer 358. The metal oxide layer 364 and the conductive layer 362 are stacked in this order over the insulating layer 360 and have a portion overlapping with the semiconductor layer 358. The insulating layer 368 is provided to cover an upper surface of the insulating layer 360, a side surface of the metal oxide layer 364, and an upper surface of the conductive layer 362.
[0257] The metal oxide film described in Embodiment 1 can be used for the semiconductor layer 358.
[0258] 25A and 25B, the transistor 350 may include a conductive layer 370a and a conductive layer 370b over the insulating layer 368. The conductive layer 370a and the conductive layer 370b function as a source electrode and a drain electrode. The conductive layer 370a and the conductive layer 370b are electrically connected to the low-resistance region 358n through an opening 391a and an opening 391b provided in the insulating layer 368 and the insulating layer 360, respectively.
[0259] A part of the conductive layer 362 functions as a gate electrode. A part of the insulating layer 360 functions as a gate insulating layer. The transistor 350 is a so-called top-gate transistor in which a gate electrode is provided over the semiconductor layer 358.
[0260] The conductive layer 362 and the metal oxide layer 364 are processed so that their top surface shapes roughly match each other.
[0261] In this specification, the phrase "top surface shapes roughly match" refers to at least a portion of the contours of stacked layers overlapping. For example, this includes cases where the upper and lower layers are processed using the same mask pattern, or where a portion of the mask pattern is the same. However, strictly speaking, the contours may not overlap, and the upper layer may be located inside the lower layer, or outside the lower layer, and in this case, it is also called "top surface shapes roughly match."
[0262] The metal oxide layer 364 located between the insulating layer 360 and the conductive layer 362 functions as a barrier film that prevents oxygen contained in the insulating layer 360 from diffusing toward the conductive layer 362. The metal oxide layer 364 also functions as a barrier film that prevents hydrogen and water contained in the conductive layer 362 from diffusing toward the insulating layer 360. The metal oxide layer 364 is preferably made of a material that is less permeable to oxygen and hydrogen than the insulating layer 360, for example.
[0263] The metal oxide layer 364 can prevent oxygen from diffusing from the insulating layer 360 to the conductive layer 362 even when the conductive layer 362 is made of a metal material that easily absorbs oxygen, such as aluminum or copper. Even when the conductive layer 362 contains hydrogen, the metal oxide layer 364 can prevent hydrogen from diffusing from the conductive layer 362 to the semiconductor layer 358 through the insulating layer 360. As a result, the carrier density in the channel formation region of the semiconductor layer 358 can be made extremely low.
[0264] An insulating material or a conductive material can be used as the metal oxide layer 364. When the metal oxide layer 364 has insulating properties, the metal oxide layer 364 functions as a part of the gate insulating layer. On the other hand, when the metal oxide layer 364 has conductive properties, the metal oxide layer 364 functions as a part of the gate electrode.
[0265] It is preferable to use an insulating material having a higher dielectric constant than silicon oxide as the metal oxide layer 364. In particular, it is preferable to use an aluminum oxide film, a hafnium oxide film, a hafnium aluminate film, or the like, because the driving voltage can be reduced.
[0266] A conductive oxide such as indium oxide, indium tin oxide (ITO), or silicon-containing indium tin oxide (ITSO) can also be used as the metal oxide layer 364. In particular, a conductive oxide containing indium is preferable because of its high conductivity.
[0267] In addition, it is preferable to use an oxide material containing one or more elements that are the same as those of the semiconductor layer 358 for the metal oxide layer 364. In particular, it is preferable to use an oxide semiconductor material that can be used for the semiconductor layer 358. In this case, it is preferable to use a metal oxide film formed using the same sputtering target as that for the semiconductor layer 358 for the metal oxide layer 364, because this allows the use of common equipment.
[0268] The metal oxide layer 364 is preferably formed using a sputtering apparatus. For example, when an oxide film is formed using a sputtering apparatus, oxygen can be suitably added to the insulating layer 360 and the semiconductor layer 358 by forming the oxide film in an atmosphere containing oxygen gas.
[0269] The semiconductor layer 358 has a region overlapping with the conductive layer 362 and a pair of low-resistance regions 358n sandwiching the region. The region of the semiconductor layer 358 overlapping with the conductive layer 362 functions as a channel formation region of the transistor 350. On the other hand, the low-resistance region 358n functions as a source region or drain region of the transistor 350.
[0270] The low-resistance region 358n can also be referred to as a region having a lower resistance than the channel formation region, a region with a high carrier concentration, a region with a high density of oxygen defects, a region with a high impurity concentration, or an n-type region.
[0271] The low-resistance region 358n of the semiconductor layer 358 is a region containing an impurity element. Examples of the impurity element include hydrogen, boron, carbon, nitrogen, fluorine, phosphorus, sulfur, arsenic, aluminum, and rare gases. Representative examples of rare gases include helium, neon, argon, krypton, and xenon. In particular, it is preferable that the low-resistance region 358n contains boron or phosphorus. Two or more of these elements may be contained.
[0272] The treatment of adding an impurity to the low-resistance region 358n can be performed through the insulating layer 360 by using the conductive layer 362 as a mask. As the treatment of adding an impurity to the low-resistance region 358n, a plasma ion doping method or an ion implantation method can be preferably used.
[0273] The low resistance region 358n has an impurity concentration of 1×10 19 atoms / cm 3 That's it, 1×10 23 atoms / cm 3 Less than or equal to 5×10 19 atoms / cm 3 That's it, 5 x 10 22 atoms / cm 3 Less than or equal to 1×10 20 atoms / cm 3 That's it, 1×10 22 atoms / cm 3 It is preferred to include a region in which:
[0274] The concentration of impurities contained in the low resistance region 358n can be analyzed by, for example, secondary ion mass spectrometry (SIMS), X-ray photoelectron spectroscopy (XPS), etc. When using XPS analysis, the concentration distribution in the depth direction can be known by combining ion sputtering from the front side or back side with XPS analysis.
[0275] In addition, in the low-resistance region 358n, the impurity element is preferably present in an oxidized state. For example, it is preferable to use an easily oxidized element such as boron, phosphorus, magnesium, aluminum, or silicon as the impurity element. Since such an easily oxidized element can exist stably in an oxidized state by bonding with oxygen in the semiconductor layer 358, even if a high temperature (for example, 400°C or higher, 600°C or higher, or 800°C or higher) is applied in a later process, desorption is suppressed. Furthermore, the impurity element removes oxygen from the semiconductor layer 358, and many oxygen vacancies are generated in the low-resistance region 358n. The oxygen vacancies are bonded with hydrogen in the film to become a carrier supply source, so that the low-resistance region 358n has an extremely low resistance state.
[0276] For example, when boron is used as an impurity element, the boron contained in the low resistance region 358n can exist in a state of being bonded to oxygen. 2 O 3 This can be confirmed by observing the spectral peaks due to bonding. In addition, in XPS analysis, the spectral peaks due to the existence of elemental boron are not observed, or the peak intensity becomes so small that it is buried in the background noise at the lower limit of measurement.
[0277] The insulating layer 360 has a region in contact with a channel formation region of the semiconductor layer 358, that is, a region overlapping with the conductive layer 362. The insulating layer 360 also has a region in contact with a low-resistance region 358n of the semiconductor layer 358 and not overlapping with the conductive layer 362.
[0278] The region of the insulating layer 360 overlapping with the low-resistance region 358n may contain the above-mentioned impurity element. In this case, like the low-resistance region 358n, the impurity element in the insulating layer 360 is preferably present in a state of being bonded to oxygen. Since such an element that is easily oxidized can be stably present in an oxidized state by bonding with oxygen in the insulating layer 360, even if a high temperature is applied in a later process, the element is prevented from being desorbed. In particular, when the insulating layer 360 contains oxygen (also referred to as excess oxygen) that can be desorbed by heating, the excess oxygen and the impurity element are bonded to be stabilized, so that the supply of oxygen from the insulating layer 360 to the low-resistance region 358n can be prevented. In addition, a part of the insulating layer 360 containing an oxidized impurity element is in a state where oxygen is difficult to diffuse, and therefore, the supply of oxygen to the low-resistance region 358n from above the insulating layer 360 through the insulating layer 360 can be prevented from becoming high-resistance.
[0279] The insulating layer 368 functions as a protective layer that protects the transistor 350. For example, an inorganic insulating material such as an oxide or a nitride can be used as the insulating layer 368. More specific examples of the inorganic insulating material that can be used include silicon oxide, silicon oxynitride, silicon nitride, silicon nitride oxide, aluminum oxide, aluminum oxynitride, aluminum nitride, hafnium oxide, and hafnium aluminate.
[0280] [Configuration Example 2-2] 26A is a top view of the transistor 350A, FIG. 26B is a cross-sectional view of the transistor 350A in the channel length direction, and FIG. 26C is a cross-sectional view of the transistor 350A in the channel width direction.
[0281] The transistor 350A differs from the transistor 350 illustrated in Structural example 2-1 mainly in that the insulating layer 360 has a different configuration and that an insulating layer 366 is included.
[0282] The insulating layer 360 is processed so that its top surface shape generally matches those of the conductive layer 362 and the metal oxide layer 364. The insulating layer 360 can be formed by processing using a resist mask for processing the conductive layer 362 and the metal oxide layer 364, for example.
[0283] The insulating layer 366 is provided in contact with the top surface and side surfaces of the semiconductor layer 358 that are not covered with the conductive layer 362, the metal oxide layer 364, and the insulating layer 360. The insulating layer 366 is provided to cover the top surface of the insulating layer 353, the side surfaces of the insulating layer 360, the side surfaces of the metal oxide layer 364, and the top surface and side surfaces of the conductive layer 362.
[0284] The insulating layer 366 has a function of lowering the resistance of the low-resistance region 358n. As such an insulating layer 366, an insulating film capable of supplying impurities into the low-resistance region 358n by heating during or after the formation of the insulating layer 366 can be used. Alternatively, an insulating film capable of generating oxygen vacancies in the low-resistance region 358n by heating during or after the formation of the insulating layer 366 can be used.
[0285] For example, an insulating film that functions as a supply source for supplying impurities to the low-resistance region 358n can be used as the insulating layer 366. In this case, the insulating layer 366 is preferably a film that releases hydrogen by heating. By forming such an insulating layer 366 in contact with the semiconductor layer 358, impurities such as hydrogen can be supplied to the low-resistance region 358n, and the resistance of the low-resistance region 358n can be reduced.
[0286] The insulating layer 366 is preferably formed using a gas containing an impurity element such as a hydrogen element as a deposition gas. By increasing the deposition temperature of the insulating layer 366, a large amount of impurity elements can be effectively supplied to the semiconductor layer 358. The deposition temperature of the insulating layer 366 can be, for example, 200° C. to 500° C., preferably 220° C. to 450° C., more preferably 250° C. to 400° C.
[0287] Furthermore, by forming the insulating layer 366 under reduced pressure and by heating, it is possible to promote desorption of oxygen from the regions that become the low-resistance regions 358n in the semiconductor layer 358. By supplying impurities such as hydrogen to the semiconductor layer 358 in which many oxygen vacancies are formed, the carrier density in the low-resistance regions 358n is increased, and the resistance of the low-resistance regions 358n can be more effectively reduced.
[0288] For example, an insulating film containing a nitride, such as silicon nitride, silicon nitride oxide, silicon oxynitride, aluminum nitride, or aluminum nitride oxide, can be suitably used as the insulating layer 366. In particular, silicon nitride has a blocking property against hydrogen and oxygen, and can therefore prevent both diffusion of hydrogen from the outside to the semiconductor layer and elimination of oxygen from the semiconductor layer to the outside, thereby realizing a highly reliable transistor.
[0289] The insulating layer 366 may be an insulating film that has a function of absorbing oxygen in the semiconductor layer 358 and generating oxygen vacancies. In particular, the insulating layer 366 is preferably formed using a metal nitride.
[0290] In addition, when a metal nitride is used, it is preferable to use a nitride of aluminum, titanium, tantalum, tungsten, chromium, or ruthenium. In particular, it is particularly preferable to include aluminum or titanium. For example, an aluminum nitride film formed by a reactive sputtering method using aluminum as a sputtering target and a gas containing nitrogen as a deposition gas can be made into a film having extremely high insulating properties and extremely high blocking properties against hydrogen and oxygen by appropriately controlling the flow rate of nitrogen gas relative to the total flow rate of the deposition gas. Therefore, by providing an insulating film containing such a metal nitride in contact with a semiconductor layer, not only can the resistance of the semiconductor layer be reduced, but also oxygen can be suitably prevented from being released from the semiconductor layer and hydrogen can be suitably prevented from diffusing into the semiconductor layer.
[0291] When aluminum nitride is used as the metal nitride, the thickness of the insulating layer containing the aluminum nitride is preferably 5 nm or more. Even with such a thin film, it is possible to achieve both high blocking properties against hydrogen and oxygen and a function of reducing the resistance of the semiconductor layer. The thickness of the insulating layer may be as thick as desired, but in consideration of productivity, it is preferable to set the thickness to 500 nm or less, preferably 200 nm or less, and more preferably 50 nm or less.
[0292] When an aluminum nitride film is used for the insulating layer 366, the composition formula is AlN x (x is a real number greater than 0 and equal to or less than 2, preferably, x is a real number greater than 0.5 and equal to or less than 1.5) is preferably used. This allows the film to have excellent insulating properties and excellent thermal conductivity, thereby improving the dissipation of heat generated when the transistor 350A is driven.
[0293] By providing such an insulating layer 366 in contact with the low-resistance region 358n, the insulating layer 366 can absorb oxygen in the low-resistance region 358n and form oxygen vacancies in the low-resistance region 358n. In addition, by performing heat treatment after forming such an insulating layer 366, many oxygen vacancies can be formed in the low-resistance region 358n, and the resistance can be reduced. In addition, when a film containing a metal oxide is used for the insulating layer 366, as a result of the insulating layer 366 absorbing oxygen in the semiconductor layer 358, a layer containing an oxide of a metal element (e.g., aluminum) contained in the insulating layer 366 may be formed between the insulating layer 366 and the low-resistance region 358n.
[0294] Here, when a metal oxide film containing indium is used as the semiconductor layer 358, a region where indium oxide is precipitated or a region with a high concentration of indium may be formed near the interface of the low-resistance region 358n on the insulating layer 366 side. This allows the low-resistance region 358n to have an extremely low resistance. The presence of such a region may be observed by an analysis method such as X-ray photoelectron spectroscopy (XPS).
[0295] [Configuration Example 2-3] 27A shows a cross-sectional view of a transistor 350B, in which the cross section in the channel length direction is shown to the left of the dashed dotted line, and the cross section in the channel width direction is shown to the right of the dashed dotted line.
[0296] The transistor 350B differs from the transistor 350B in configuration example 2-1 mainly in that a conductive layer 356 is provided between a substrate 352 and an insulating layer 353. The conductive layer 356 has a region overlapping with a semiconductor layer 358 and a conductive layer 362.
[0297] In the transistor 350B, the conductive layer 362 functions as a second gate electrode (also referred to as a top gate electrode), and the conductive layer 356 functions as a first gate electrode (also referred to as a bottom gate electrode). Part of the insulating layer 360 functions as a second gate insulating layer, and part of the insulating layer 353 functions as a first gate insulating layer.
[0298] A portion of the semiconductor layer 358 that overlaps with at least one of the conductive layer 362 and the conductive layer 356 functions as a channel formation region. Note that for ease of description, hereinafter, a portion of the semiconductor layer 358 that overlaps with the conductive layer 362 may be referred to as a channel formation region; however, in reality, a channel can also be formed in a portion that does not overlap with the conductive layer 362 and overlaps with the conductive layer 356 (a portion including the low-resistance region 358n).
[0299] 27A, the conductive layer 356 may be electrically connected to the conductive layer 362 through an opening 392 provided in the metal oxide layer 364, the insulating layer 360, and the insulating layer 353. This allows the conductive layer 356 and the conductive layer 362 to be applied with the same potential.
[0300] The conductive layer 356 may be electrically connected to either the conductive layer 370a or the conductive layer 370b.
[0301] The conductive layer 356 can be formed using a material similar to that of the conductive layer 362, the conductive layer 370a, or the conductive layer 370b. In particular, it is preferable to use a material containing copper for the conductive layer 356 because wiring resistance can be reduced.
[0302] 27A shows a case where the insulating layer 353 has a layered structure in which an insulating layer 353a and an insulating layer 353b are stacked from the conductive layer 356 side. In this case, the insulating layer 353a located on the conductive layer 356 side is preferably an insulating film that does not easily diffuse metal elements contained in the conductive layer 356. For example, an inorganic insulating film such as a silicon nitride film, a silicon nitride oxide film, an aluminum oxide film, or a hafnium oxide film is preferably used. In addition, an insulating film containing oxygen is preferably used for the insulating layer 353b in contact with the semiconductor layer 358. For example, a silicon oxide film, a silicon oxynitride film, or the like is preferably used.
[0303] 27A, in the channel width direction, it is preferable that the conductive layer 362 and the conductive layer 356 protrude outward beyond the end portion of the semiconductor layer 358. In this case, as shown in FIG 27A, the entire semiconductor layer 358 in the channel width direction is covered with the conductive layer 362 and the conductive layer 356 via the insulating layer 360 and the insulating layer 353.
[0304] With such a structure, the semiconductor layer 358 can be electrically surrounded by an electric field generated by the pair of gate electrodes. In particular, it is preferable to apply the same potential to the conductive layer 356 and the conductive layer 362. This makes it possible to effectively apply an electric field for inducing a channel in the semiconductor layer 358, thereby increasing the on-state current of the transistor 350B. Therefore, the transistor 350B can also be miniaturized.
[0305] Note that the conductive layer 362 and the conductive layer 356 may not be connected to each other. In this case, a constant potential may be applied to one of a pair of gate electrodes, and a signal for driving the transistor 350B may be applied to the other. In this case, the threshold voltage when the transistor 350B is driven by the other gate electrode can also be controlled by the potential applied to one gate electrode.
[0306] [Configuration Example 2-4] 27B shows a cross-sectional view of transistor 350C, in which the cross section in the channel length direction is shown to the left of the dashed dotted line, and the cross section in the channel width direction is shown to the right of the dashed dotted line.
[0307] The transistor 350C is an example in which the conductive layer 356 functioning as a second gate electrode, as exemplified in Structural example 2-3, is provided in the transistor 350A exemplified in Structural example 2-2.
[0308] With such a structure, a transistor with high on-state current can be obtained, or a transistor whose threshold voltage can be controlled can be obtained.
[0309] At least a part of the configuration examples exemplified in this embodiment and the corresponding drawings can be implemented in appropriate combination with other configuration examples or drawings.
[0310] This embodiment mode can be implemented by appropriately combining at least a part of it with other embodiment modes described in this specification.
[0311] (Embodiment 3) In this embodiment, a structural example of a display device that can be manufactured using a semiconductor device including a metal oxide film according to one embodiment of the present invention will be described.
[0312] 28A is a schematic top view of a display device 700. The display device 700 has a flexible substrate 762. The substrate 762 is provided with a display portion 702, a pair of circuit portions 763, a circuit portion 764, wiring 704, and a connection terminal 703a and a connection terminal 703b.
[0313] The circuit portion 763 and the circuit portion 764 have a function of driving the display portion 702. Two circuit portions 763 are provided on either side of the display portion 702. The circuit portion 764 is provided between the display portion 702 and the wiring 704. The circuit portion 763 has a function as, for example, a gate driver, and the circuit portion 764 has a function as, for example, a source driver or a part thereof. For example, the circuit portion 764 may include a buffer circuit or a demultiplexer circuit.
[0314] The above-mentioned various display elements, such as a liquid crystal element or a light-emitting element, can be used as the display element provided in the display unit 702. In particular, it is preferable to use an organic EL element as the display element.
[0315] The substrate 762 has a top surface shape in which a portion where the wiring 704, the connection terminal 703a, and the connection terminal 703b are provided protrudes more than other portions. In other words, the width of the portion of the substrate 762 where the wiring 704, the connection terminal 703a, and the connection terminal 703b are provided is smaller than the width of a portion where the display portion 702 is provided.
[0316] The protruding portion of the substrate 762 has a region (curved portion 761a) that can be curved in a region overlapping with the wiring 704. The substrate 762 has a pair of regions (curved portions 761b) that can be curved in a region where the display unit 702 is provided. As shown in FIG. 28A, by having a portion of the substrate 762 have a protruding shape, the curving direction of the curving portion 761a and the curving direction of the curving portion 761b can be set to intersect.
[0317] The connection terminal 703a functions as a terminal to which an FPC (Flexible Printed Circuit) is connected, and the connection terminal 703b functions as a terminal to which an IC is connected.
[0318] 28B and 28C are perspective views of the display device 700 when the substrate 762 is bent on the side opposite the display surface side at the curved portions 761a and 761b. Fig. 28B is a perspective view including the display surface side, and Fig. 28C is a perspective view including the side opposite the display surface side. Fig. 28C also clearly shows the FPC 706 connected to the connection terminal 703a and the IC 707 connected to the connection terminal 703b.
[0319] 28B, by curving both sides of display unit 702, curved display units can be provided on both sides of the electronic device when display device 700 is incorporated into the electronic device. This makes it possible to realize an electronic device with high functionality.
[0320] 28B and 28C, a part of the substrate 762 can be folded back to the opposite side to the display surface side by the curved portion 761a. Specifically, the protruding portion of the substrate 762 can be folded back so that the wiring 704 is on the outside. This allows the connection terminals 703a and 703b to be disposed on the opposite side to the display surface side, and further allows the FPC 706 to be disposed on the opposite side to the display surface side. This makes it possible to reduce the area of the non-display portion when the display device 700 is incorporated into an electronic device.
[0321] The substrate 762 is provided with a notch 765. The notch 765 is a portion where, for example, a camera lens, various sensors such as an optical sensor, a lighting device, or a design of the electronic device can be arranged. By cutting out a part of the display unit 702, an electronic device with a higher design quality can be realized. This also increases the occupancy rate of the screen relative to the surface of the housing.
[0322] [Cross-section example] An example of a cross-sectional configuration of a display device will be described below.
[0323] [Configuration Example 1] Fig. 29 is a schematic cross-sectional view of the display device 700. Fig. 29 shows a cross section including the display portion 702, the circuit portion 763, the curved portion 761a, and the connection terminal 703a of the display device 700 shown in Fig. 28A. The display portion 702 is provided with a transistor 750 and a capacitor 790. The circuit portion 763 is provided with a transistor 752.
[0324] The transistor 750 and the transistor 752 are transistors in which an oxide semiconductor is used for a semiconductor layer in which a channel is formed. Note that the present invention is not limited to this, and a transistor in which silicon (amorphous silicon, polycrystalline silicon, or single crystal silicon) or an organic semiconductor is used for the semiconductor layer can also be used.
[0325] The transistor used in this embodiment has an oxide semiconductor film that is highly purified and in which formation of oxygen vacancies is suppressed. The off-state current of the transistor can be significantly reduced. Therefore, a pixel including such a transistor can hold an electric signal such as an image signal for a long time and can set a long interval for writing an image signal or the like. Thus, the frequency of a refresh operation can be reduced, leading to reduced power consumption.
[0326] In addition, the transistor used in this embodiment mode can achieve a relatively high field-effect mobility and thus can be driven at high speed. For example, by using such a transistor capable of high speed driving in a display device, a switching transistor of a pixel and a driver transistor used in a circuit portion can be formed over the same substrate. That is, a configuration without using a driver circuit formed of a silicon wafer or the like is also possible, and the number of components of the display device can be reduced. In addition, by using a transistor capable of high speed driving in a pixel, a high-quality image can be provided.
[0327] The capacitor 790 has a lower electrode formed by processing the same film as the first gate electrode of the transistor 750, and an upper electrode formed by processing the same metal oxide film as the semiconductor layer. The upper electrode has a low resistance like the source and drain regions of the transistor 750. A part of an insulating film functioning as the first gate insulating layer of the transistor 750 is provided between the lower electrode and the upper electrode. That is, the capacitor 790 has a stacked structure in which an insulating film functioning as a dielectric film is sandwiched between a pair of electrodes. A wiring obtained by processing the same film as the source and drain electrodes of the transistor 750 is connected to the upper electrode.
[0328] An insulating layer 770 functioning as a planarization film is provided over the transistor 750, the transistor 752, and the capacitor 790.
[0329] The transistor 750 in the display portion 702 and the transistor 752 in the circuit portion 763 may have different structures. For example, a top-gate transistor may be used for one of them, and a bottom-gate transistor may be used for the other. Note that the circuit portion 764 is similar to the circuit portion 763.
[0330] Note that the structures of the transistors 750 and 752 can be those of the above-described Embodiment 2.
[0331] The connection terminal 703a has a part of the wiring 704. As shown in Fig. 29, the connection terminal 703a preferably has a laminated structure in which a plurality of conductive films are laminated, because the electrical conductivity and mechanical strength of the connection terminal 703a are increased. The connection terminal 703a is electrically connected to the FPC 706 via a connection layer 780. The connection layer 780 may be made of, for example, an anisotropic conductive material.
[0332] The display device 700 includes a substrate 762 and a substrate 740 each functioning as a support substrate. As the substrate 762 and the substrate 740, for example, a flexible substrate such as a glass substrate or a plastic substrate can be used.
[0333] The transistor 750, the transistor 752, the capacitor 790, and the like are provided over an insulating layer 744. The substrate 762 and the insulating layer 744 are attached to each other with an adhesive layer 742.
[0334] The display device 700 also includes a light-emitting element 782, a colored layer 736, a light-shielding layer 738, and the like.
[0335] The light-emitting element 782 includes a conductive layer 772, an EL layer 786, and a conductive layer 788. The conductive layer 772 is electrically connected to a source electrode or a drain electrode of the transistor 750. The conductive layer 772 is provided over the insulating layer 770 and functions as a pixel electrode. In addition, an insulating layer 730 is provided to cover an end portion of the conductive layer 772, and an EL layer 786 and a conductive layer 788 are stacked over the insulating layer 730 and the conductive layer 772.
[0336] The conductive layer 772 can be formed using a material that is reflective to visible light. For example, a material containing aluminum, silver, or the like can be used. The conductive layer 788 can be formed using a material that transmits visible light. For example, an oxide material containing indium, zinc, tin, or the like can be used. Therefore, the light-emitting element 782 is a top-emission light-emitting element that emits light to the side opposite to the surface where the light is formed (the side of the substrate 740).
[0337] The EL layer 786 may include organic compounds or inorganic compounds such as quantum dots, etc. The EL layer 786 includes a light-emitting material that emits light when a current is passed through it.
[0338] Examples of the luminescent material include fluorescent materials, phosphorescent materials, thermally activated delayed fluorescence (TADF) materials, inorganic compounds (quantum dot materials, etc.), etc. Examples of the material that can be used for the quantum dot include colloidal quantum dot materials, alloy type quantum dot materials, core-shell type quantum dot materials, core type quantum dot materials, etc.
[0339] The light-shielding layer 738 and the colored layer 736 are provided on one surface of the insulating layer 746. The colored layer 736 is provided at a position overlapping with the light-emitting element 782. The light-shielding layer 738 is provided in a region of the display portion 702 that does not overlap with the light-emitting element 782. The light-shielding layer 738 may also be provided to overlap with the circuit portion 763 and the like.
[0340] The substrate 740 is bonded to the other surface of the insulating layer 746 by an adhesive layer 747. The substrate 740 and the substrate 762 are bonded to each other by a sealing layer 732.
[0341] Here, a light-emitting material that emits white light is used as the EL layer 786 of the light-emitting element 782. The white light emitted by the light-emitting element 782 is colored by the coloring layer 736 and emitted to the outside. The EL layer 786 is provided across pixels that exhibit different colors. By arranging pixels, each of which is provided with a coloring layer 736 that transmits any of red (R), green (G), or blue (B), in a matrix form in the display unit 702, the display device 700 can perform full-color display.
[0342] A conductive film having transparency and reflectivity may be used as the conductive layer 788. In this case, a microresonator (microcavity) structure may be realized between the conductive layer 772 and the conductive layer 788, and a configuration may be adopted in which light of a specific wavelength is intensified and emitted. In this case, an optical adjustment layer for adjusting the optical distance may be disposed between the conductive layer 772 and the conductive layer 788, and the thickness of the optical adjustment layer may be made different between pixels of different colors, thereby increasing the color purity of the light emitted from each pixel.
[0343] When the EL layer 786 is formed in an island shape for each pixel or in a stripe shape for each pixel row, that is, when the EL layer 786 is formed by coloring, the colored layer 736 and the optical adjustment layer described above may not be provided.
[0344] Here, an inorganic insulating film functioning as a barrier film with low moisture permeability is preferably used for each of the insulating layers 744 and 746. By sandwiching the light-emitting element 782, the transistor 750, and the like between the insulating layers 744 and 746, deterioration of the light-emitting element 782, the transistor 750, and the like can be suppressed, and a highly reliable display device can be realized.
[0345] [Configuration Example 2] Fig. 30 shows a cross-sectional view of display device 700 having a configuration partially different from that of Fig. 29. Fig. 30 also clearly shows a configuration in which part of display device 700 is curved at curved portion 761a and folded back to the side opposite the display surface side.
[0346] A display device 700 shown in Fig. 30 includes a resin layer 743 between the adhesive layer 742 and the insulating layer 744 shown in Fig. 29. Also, a protective layer 749 is provided instead of the substrate 740.
[0347] The resin layer 743 is a layer containing an organic resin such as polyimide or acrylic. The insulating layer 744 contains an inorganic insulating film such as silicon oxide, silicon oxynitride, or silicon nitride. The resin layer 743 and the substrate 762 are attached to each other by an adhesive layer 742. The resin layer 743 is preferably thinner than the substrate 762.
[0348] The protective layer 749 is attached to the sealing layer 732. As the protective layer 749, a glass substrate, a resin film, or the like can be used. As the protective layer 749, an optical member such as a polarizing plate (including a circular polarizing plate) or a scattering plate, an input device such as a touch sensor panel, or a configuration in which two or more of these are laminated may be applied. Furthermore, the protective layer 749 may include a member that constitutes a part of the housing of the electronic device (for example, a part that becomes a screen).
[0349] In addition, the EL layer 786 of the light-emitting element 782 is provided in an island shape over the insulating layer 730 and the conductive layer 772. By forming the EL layer 786 so that each subpixel has a different light emission color, color display can be realized without using the coloring layer 736.
[0350] A protective layer 741 is provided to cover the light-emitting element 782. The protective layer 741 has a function of preventing impurities such as water from diffusing into the light-emitting element 782. The protective layer 741 has a layered structure in which an insulating layer 741a, an insulating layer 741b, and an insulating layer 741c are layered in this order from the conductive layer 788 side. In this case, it is preferable to use an inorganic insulating film having a high barrier property against impurities such as water for the insulating layer 741a and the insulating layer 741c, and an organic insulating film functioning as a planarization film for the insulating layer 741b. It is also preferable that the protective layer 741 is provided so as to extend to the circuit portion 763 and the like.
[0351] In addition, it is preferable that the organic insulating film covering the transistor 750, the transistor 752, and the like is formed in an island shape inside the sealing layer 732. In other words, it is preferable that the end of the organic insulating film is located inside the sealing layer 732 or in a region overlapping with the end of the sealing layer 732. FIG. 30 shows an example in which the insulating layer 770, the insulating layer 730, and the insulating layer 741b are processed into an island shape. For example, in a portion overlapping with the sealing layer 732, the insulating layer 741c and the insulating layer 741a are provided in contact with each other. In this way, the surface of the organic insulating film covering the transistor 750 and the transistor 752 is not exposed outside the sealing layer 732, so that water or hydrogen can be suitably prevented from diffusing from the outside to the transistor 750 and the transistor 752 through the organic insulating film. This suppresses fluctuations in the electrical characteristics of the transistors, and a display device with extremely high reliability can be realized.
[0352] 30, curved portion 761a has a portion where inorganic insulating films such as insulating layer 744 are not provided, in addition to substrate 762 and adhesive layer 742. Curved portion 761a has a configuration in which insulating layer 770 containing an organic material covers wiring 704 to prevent wiring 704 from being exposed. In the configuration shown in FIG. 30, curved portion 761a has a layered structure in which resin layer 743, wiring 704, and insulating layer 770 are layered.
[0353] By providing as little inorganic insulating film as possible in the curved portion 761a and stacking only a conductive layer containing a metal or alloy and a layer containing an organic material, it is possible to prevent cracks from occurring when the display device 700 is bent. Also, by not providing a substrate 762 in the curved portion 761a, a part of the display device 700 can be bent with an extremely small radius of curvature.
[0354] In addition, in a region overlapping with the connection terminal 703a, the resin layer 743 is bonded to the support 720 via an adhesive layer 748. The support 720 may be made of a material having higher rigidity than the substrate 762 or the like. Alternatively, the support 720 may be a part of the housing of the electronic device, or a part of a member disposed inside the electronic device.
[0355] 30, a conductive layer 761 is provided over the protective layer 741. The conductive layer 761 can be used as a wiring or an electrode.
[0356] Furthermore, when a touch sensor is provided overlapping the display device 700, the conductive layer 761 can function as an electrostatic shielding film for preventing electrical noise generated when a pixel is driven from being transmitted to the touch sensor. In this case, a predetermined constant potential may be applied to the conductive layer 761.
[0357] Alternatively, the conductive layer 761 can be used as, for example, an electrode of a touch sensor. This allows the display device 700 to function as a touch panel. For example, the conductive layer 761 can be used as an electrode or wiring of a capacitive touch sensor. In this case, the conductive layer 761 can be used as a wiring or electrode to which a detection circuit is connected or a wiring or electrode to which a sensor signal is input. In this manner, by forming a touch sensor over the light-emitting element 782, the number of components can be reduced, and the manufacturing costs of electronic devices and the like can be reduced.
[0358] The conductive layer 761 is preferably provided in a portion that does not overlap with the light-emitting element 782. For example, the conductive layer 761 can be provided in a portion that overlaps with the insulating layer 730. As a result, there is no need to use a transparent conductive film with relatively low conductivity as the conductive layer 761, and a metal or alloy with high conductivity can be used, which can improve the sensitivity of the sensor.
[0359] Note that the type of the touch sensor that can be configured using the conductive layer 761 is not limited to the capacitance type, and various types such as a resistive film type, a surface acoustic wave type, an infrared type, an optical type, and a pressure sensitive type can be used. Alternatively, two or more of these types may be used in combination.
[0360] [Configuration Example 3] Fig. 31 is a schematic cross-sectional view of a display device 700a in which a liquid crystal element is used as a display element, and Fig. 31 shows a cross-sectional view of a region including a circuit portion 763, a display portion 702, and a connection terminal 703a.
[0361] 31 includes a transistor 721, a transistor 722, a liquid crystal element 710, and the like between a substrate 701 and a substrate 705. The substrate 701 and the substrate 705 are attached to each other with a sealing layer 732.
[0362] Here, bottom-gate transistors are used as the transistor 721 and the transistor 722.
[0363] The liquid crystal element 710 includes a conductive layer 711, a liquid crystal 712, and a conductive layer 713. The conductive layer 713 is provided over a substrate 701. One or more insulating layers are provided over the conductive layer 713, and the conductive layer 711 is provided over the insulating layer. The liquid crystal 712 is located between the conductive layer 711 and the substrate 705. The conductive layer 713 is electrically connected to a wiring 723 and functions as a common electrode. The conductive layer 711 is electrically connected to a transistor 721 and functions as a pixel electrode. A common potential is applied to the wiring 723.
[0364] 31 is a liquid crystal element to which a lateral electric field mode (for example, FFS mode) is applied. The conductive layer 711 has a top surface shape having a comb shape or slits. In the liquid crystal element 710, the alignment state of the liquid crystal 712 is controlled by an electric field generated between the conductive layer 711 and the conductive layer 713.
[0365] In addition, a capacitor 790 functioning as a storage capacitor is formed by a stacked structure of the conductive layers 711, 713, and one or more insulating layers sandwiched between the conductive layers 711 and 713. Therefore, there is no need to provide a separate capacitor, and the aperture ratio can be increased.
[0366] A material that transmits visible light or a material that reflects visible light can be used for the conductive layer 711 and the conductive layer 713. As a light-transmitting material, for example, an oxide material containing indium, zinc, tin, or the like can be used. As a reflective material, for example, a material containing aluminum, silver, or the like can be used.
[0367] When a reflective material is used for either or both of the conductive layers 711 and 713, the display device 700a becomes a reflective liquid crystal display device. On the other hand, when a light-transmitting material is used for both the conductive layers 711 and 713, the display device 700a becomes a transmissive liquid crystal display device. In the case of a reflective liquid crystal display device, a polarizing plate is provided on the viewing side. On the other hand, in the case of a transmissive liquid crystal display device, a pair of polarizing plates is provided to sandwich a liquid crystal element.
[0368] 31 shows an example of a transmissive liquid crystal display device. A polarizing plate 755 and a light source 757 are provided on the outer side of a substrate 701, and a polarizing plate 756 is provided on the outer side of a substrate 705. The light source 757 functions as a backlight.
[0369] A light-shielding layer 738 and a colored layer 736 are provided on the surface of the substrate 705 facing the substrate 701. An insulating layer 734 functioning as a planarizing layer is provided to cover the light-shielding layer 738 and the colored layer 736. A spacer 727 is provided on the surface of the insulating layer 734 facing the substrate 701.
[0370] The liquid crystal 712 is located between an alignment film 725 that covers the conductive layer 711 and an alignment film 726 that covers the insulating layer 734. Note that the alignment films 725 and 726 do not have to be provided if they are not necessary.
[0371] 31, optical members (optical films) such as a retardation film and an anti-reflection film, a protective film, an antifouling film, etc. may be appropriately provided outside the substrate 705. Examples of the anti-reflection film include an AG (Anti Glare) film and an AR (Anti Reflection) film.
[0372] Thermotropic liquid crystal, low molecular liquid crystal, polymer liquid crystal, polymer dispersed liquid crystal (PDLC), polymer network liquid crystal (PNLC), ferroelectric liquid crystal, antiferroelectric liquid crystal, etc. can be used for the liquid crystal 712. In addition, when the in-plane switching mode is adopted, liquid crystal exhibiting a blue phase without using an alignment film may be used.
[0373] In addition, the liquid crystal element modes that can be used include TN (Twisted Nematic) mode, VA (Vertical Alignment) mode, IPS (In-Plane-Switching) mode, FFS (Fringe Field Switching) mode, ASM (Axially Symmetric aligned Micro-cell) mode, OCB (Optically Compensated Birefringence) mode, ECB (Electrically Controlled Birefringence) mode, and guest-host mode.
[0374] Also, a scattering type liquid crystal using a polymer dispersed type liquid crystal, a polymer network type liquid crystal, or the like can be used as the liquid crystal 712. In this case, a configuration for performing black and white display without providing the colored layer 736, or a configuration for performing color display using the colored layer 736 can be used.
[0375] Furthermore, as a method for driving the liquid crystal element, a time-division display method (also called a field sequential driving method) that performs color display based on a time-division additive color mixing method may be applied. In this case, the coloring layer 736 may not be provided. When the time-division display method is used, there is an advantage that the aperture ratio of the pixel can be improved and the resolution can be increased because there is no need to provide sub-pixels that exhibit the respective colors of R (red), G (green), and B (blue).
[0376] The display device 700a shown in FIG. 31 has a structure in which an organic insulating film functioning as a planarizing layer is not provided on the formation surface side of the conductive layer 711 functioning as a pixel electrode and the conductive layer 713 functioning as a common electrode. In addition, bottom-gate transistors that can be manufactured in a relatively short process are used as the transistors 721 and the like included in the display device 700a. In addition, the wiring 704, the connection terminals 703a, and the like can be manufactured in a common process with the manufacturing process of the transistors, the liquid crystal element, and the like without adding any special process. With such a structure, the manufacturing cost can be reduced and the manufacturing yield can be increased, making it possible to provide a highly reliable display device at a low cost.
[0377] At least a part of the configuration examples exemplified in this embodiment and the corresponding drawings can be implemented in appropriate combination with other configuration examples or drawings.
[0378] This embodiment mode can be implemented by appropriately combining at least a part of it with other embodiment modes described in this specification.
[0379] (Embodiment 4) In this embodiment, a display device including a semiconductor device of one embodiment of the present invention will be described with reference to FIGS. 32A to 32C.
[0380] 32A includes a pixel portion 502, a driver circuit portion 504, a protective circuit 506, and a terminal portion 507. Note that the protective circuit 506 does not necessarily have to be provided.
[0381] The transistor of one embodiment of the present invention can be applied to the transistors included in the pixel portion 502 and the driver circuit portion 504. The transistor of one embodiment of the present invention can also be applied to the protection circuit 506.
[0382] The pixel section 502 has a plurality of pixel circuits 501 arranged in X rows and Y columns (X and Y are each independently a natural number of 2 or more). Each pixel circuit 501 has a circuit for driving a display element.
[0383] The driver circuit unit 504 has driver circuits such as a gate driver 504a that outputs scanning signals to the gate lines GL_1 to GL_X and a source driver 504b that supplies data signals to the data lines DL_1 to DL_Y. The gate driver 504a may have at least a shift register. The source driver 504b is configured using, for example, a plurality of analog switches. The source driver 504b may also be configured using a shift register.
[0384] The terminal portion 507 refers to a portion provided with terminals for inputting power, control signals, image signals, and the like from an external circuit to the display device.
[0385] The protection circuit 506 is a circuit that, when a potential outside a certain range is applied to a wiring connected to the protection circuit 506, brings the wiring into a conductive state with another wiring. The protection circuit 506 shown in Fig. 32A is connected to various wirings, such as a gate line GL that is a wiring between the gate driver 504a and the pixel circuit 501, or a data line DL that is a wiring between the source driver 504b and the pixel circuit 501. Note that in Fig. 32A, the protection circuit 506 is hatched to distinguish it from the pixel circuit 501.
[0386] In addition, the gate driver 504a and the source driver 504b may be provided on the same substrate as the pixel unit 502, or a substrate on which a gate driver circuit or a source driver circuit is separately formed (e.g., a drive circuit substrate formed of a single crystal semiconductor or a polycrystalline semiconductor) may be mounted on the substrate by COG or TAB (Tape Automated Bonding).
[0387] 32B and 32C show an example of a pixel circuit configuration that can be applied to pixel circuit 501. In FIG.
[0388] 32B includes a liquid crystal element 570, a transistor 550, and a capacitor 560. The pixel circuit 501 is connected to a data line DL_n, a gate line GL_m, a potential supply line VL, and the like.
[0389] The potential of one of a pair of electrodes of the liquid crystal element 570 is set as appropriate according to the specifications of the pixel circuit 501. The orientation state of the liquid crystal element 570 is set by written data. Note that a common potential (common potential) may be applied to one of the pair of electrodes of the liquid crystal element 570 included in each of the multiple pixel circuits 501. Also, different potentials may be applied to one of the pair of electrodes of the liquid crystal element 570 in the pixel circuits 501 in each row.
[0390] 32C includes a transistor 552, a transistor 554, a capacitor 562, and a light-emitting element 572. The pixel circuit 501 is connected to a data line DL_n, a gate line GL_m, a potential supply line VL_a, a potential supply line VL_b, and the like.
[0391] A high power supply potential VDD is applied to one of the potential supply lines VL_a and VL_b, and a low power supply potential VSS is applied to the other. A current flowing through the light emitting element 572 is controlled in accordance with a potential applied to the gate of the transistor 554, thereby controlling the light emission luminance of the light emitting element 572.
[0392] At least a part of the configuration examples exemplified in this embodiment and the corresponding drawings can be implemented in appropriate combination with other configuration examples or drawings.
[0393] This embodiment mode can be implemented by appropriately combining at least a part of it with other embodiment modes described in this specification.
[0394] (Embodiment 5) A pixel circuit including a memory for correcting a gray scale displayed in a pixel and a display device including the pixel circuit will be described below. The transistor including a metal oxide film described in Embodiment 1 can be used as a transistor used in the pixel circuit described below.
[0395] [Circuit configuration] 33A shows a circuit diagram of a pixel circuit 400. The pixel circuit 400 includes a transistor M1, a transistor M2, a capacitor C1, and a circuit 401. The pixel circuit 400 is connected to a wiring S1, a wiring S2, a wiring G1, and a wiring G2.
[0396] The transistor M1 has a gate connected to the wiring G1, one of a source and a drain connected to the wiring S1, and the other connected to one electrode of the capacitor C1. The transistor M2 has a gate connected to the wiring G2, one of a source and a drain connected to the wiring S2, and the other connected to the other electrode of the capacitor C1 and the circuit 401.
[0397] The circuit 401 is a circuit including at least one display element. Various elements can be used as the display element, but typically, a light-emitting element such as an organic EL element or an LED element, a liquid crystal element, or a MEMS (Micro Electro Mechanical Systems) element can be used.
[0398] The node connecting the transistor M1 and the capacitor C1 is referred to as a node N1, and the node connecting the transistor M2 and the circuit 401 is referred to as a node N2.
[0399] In the pixel circuit 400, the potential of the node N1 can be maintained by turning off the transistor M1. Also, the potential of the node N2 can be maintained by turning off the transistor M2. Also, by writing a predetermined potential to the node N1 via the transistor M1 while the transistor M2 is in the off state, the potential of the node N2 can be changed according to the change in the potential of the node N1 due to capacitive coupling via the capacitor C1.
[0400] Here, the transistor including an oxide semiconductor, as exemplified in Embodiment 1, can be used as one or both of the transistor M1 and the transistor M2. Therefore, the potentials of the nodes N1 and N2 can be held for a long period of time due to an extremely low off-state current. Note that when the period during which the potentials of the nodes are held is short (specifically, when the frame frequency is 30 Hz or more), a transistor including a semiconductor such as silicon may be used.
[0401] [Driving method example] Next, an example of an operation method of pixel circuit 400 will be described with reference to Fig. 33B. Fig. 33B is a timing chart relating to the operation of pixel circuit 400. Note that, for ease of explanation, the influence of various resistances such as wiring resistance, parasitic capacitances of transistors and wiring, threshold voltages of transistors, and the like will not be taken into consideration here.
[0402] 33B, one frame period is divided into a period T1 and a period T2. The period T1 is a period in which a potential is written to the node N2, and the period T2 is a period in which a potential is written to the node N1.
[0403] [Period T1] In the period T1, a potential that turns on the transistor is applied to both the wiring G1 and the wiring G2. In addition, a constant potential V ref is supplied to the line S2, and the first data potential V w supplies.
[0404] The node N1 is connected to a potential V ref The node N2 is supplied with a first data potential V w Therefore, the capacitance C1 has a potential difference V w -V ref is held.
[0405] [Period T2] In the next period T2, a potential that turns on the transistor M1 is applied to the wiring G1, and a potential that turns off the transistor M2 is applied to the wiring G2. data A predetermined constant potential is applied to the wiring S2, or the wiring S2 may be in a floating state.
[0406] The node N1 receives a second data potential V data At this time, the second data potential V data In response to this, the potential of the node N2 changes by a potential dV. w The potential obtained by adding the second data potential V to the potential dV is input. Note that although the potential dV is shown to be a positive value in FIG. 33B, it may be a negative value. data is the potential V ref It may be lower.
[0407] Here, the potential dV is roughly determined by the capacitance value of the capacitor C1 and the capacitance value of the circuit 401. When the capacitance value of the capacitor C1 is sufficiently larger than the capacitance value of the circuit 401, the potential dV is equal to the second data potential V data The potential becomes close to
[0408] In this manner, the pixel circuit 400 can combine two types of data signals to generate a potential to be supplied to the circuit 401 including a display element, and therefore, gray scale correction can be performed within the pixel circuit 400.
[0409] In addition, the pixel circuit 400 can generate a potential that exceeds the maximum potential that can be supplied to the wirings S1 and S2. For example, when a light-emitting element is used, high dynamic range (HDR) display or the like can be performed. When a liquid crystal element is used, overdrive driving or the like can be realized.
[0410] [Example of application] [Example using liquid crystal element] The pixel circuit 400LC shown in Fig. 33C includes a circuit 401LC. The circuit 401LC includes a liquid crystal element LC and a capacitor C2.
[0411] The liquid crystal element LC has one electrode connected to the node N2 and one electrode connected to the capacitance C2, and the other electrode connected to the potential V com2 The capacitor C2 is connected to the wiring that has the potential V com1 Connect with the wiring given.
[0412] The capacitor C2 functions as a storage capacitor. If the capacitor C2 is not required, it can be omitted.
[0413] The pixel circuit 400LC can supply a high voltage to the liquid crystal element LC, and therefore can, for example, realize high-speed display by overdrive driving, apply a liquid crystal material with a high driving voltage, etc. In addition, by supplying a correction signal to the wiring S1 or wiring S2, it is possible to correct the gradation according to the operating temperature, the deterioration state of the liquid crystal element LC, etc.
[0414] [Example using light-emitting element] The pixel circuit 400EL shown in Fig. 33D includes a circuit 401EL. The circuit 401EL includes a light-emitting element EL, a transistor M3, and a capacitor C2.
[0415] The transistor M3 has a gate connected to the node N2 and one electrode of the capacitor C2, and one of its source and drain connected to the potential V H The other electrode of the capacitor C2 is connected to a wiring to which a potential V com The light-emitting element EL has the other electrode connected to a wiring that is supplied with a potential V L Connect with the wiring given.
[0416] The transistor M3 has a function of controlling the current supplied to the light-emitting element EL. The capacitor C2 functions as a storage capacitor. The capacitor C2 can be omitted if not required.
[0417] In this embodiment, the anode side of the light-emitting element EL is connected to the transistor M3, but the cathode side of the light-emitting element EL may be connected to the transistor M3. H and potential V L The value of can be changed appropriately.
[0418] In the pixel circuit 400EL, a large current can be passed through the light-emitting element EL by applying a high potential to the gate of the transistor M3, and thus, for example, HDR display can be realized. In addition, by supplying a correction signal to the wiring S1 or the wiring S2, it is also possible to correct variations in the electrical characteristics of the transistor M3 and the light-emitting element EL.
[0419] It should be noted that the circuits are not limited to those illustrated in FIGS. 33C and 33D, and may be configured to include additional transistors, capacitors, and the like.
[0420] This embodiment mode can be implemented by appropriately combining at least a part of it with other embodiment modes described in this specification.
[0421] (Embodiment 6) In this embodiment, a display module that can be manufactured using one embodiment of the present invention will be described.
[0422] A display module 6000 shown in FIG. 34A has a display device 6006 connected by an FPC 6005, a frame 6009, a printed circuit board 6010, and a battery 6011 between an upper cover 6001 and a lower cover 6002.
[0423] For example, a display device manufactured using one embodiment of the present invention can be used as the display device 6006. The display device 6006 can provide a display module with extremely low power consumption.
[0424] The shape and dimensions of the upper cover 6001 and the lower cover 6002 can be changed appropriately according to the size of the display device 6006.
[0425] The display device 6006 may have a function as a touch panel.
[0426] The frame 6009 may have a function of protecting the display device 6006, a function of blocking electromagnetic waves generated by the operation of the printed circuit board 6010, a function as a heat sink, and the like.
[0427] The printed circuit board 6010 includes a power supply circuit, a signal processing circuit for outputting a video signal and a clock signal, a battery control circuit, etc.
[0428] FIG. 34B is a cross-sectional schematic diagram of a display module 6000 with an optical touch sensor.
[0429] The display module 6000 has a light emitting section 6015 and a light receiving section 6016 provided on a printed circuit board 6010. Also, in an area surrounded by an upper cover 6001 and a lower cover 6002, a pair of light guiding sections (light guiding section 6017a, light guiding section 6017b) are provided.
[0430] The display device 6006 is provided so as to overlap a printed circuit board 6010 and a battery 6011 with a frame 6009 interposed therebetween. The display device 6006 and the frame 6009 are fixed to a light guiding portion 6017a and a light guiding portion 6017b.
[0431] Light 6018 emitted from the light-emitting unit 6015 passes through the light-guiding unit 6017a, the upper part of the display device 6006, and the light-guiding unit 6017b to reach the light-receiving unit 6016. When the light 6018 is blocked by a detection object such as a finger or a stylus, a touch operation can be detected.
[0432] A plurality of light emitting units 6015 are provided, for example, along two adjacent sides of the display device 6006. A plurality of light receiving units 6016 are provided at positions facing the light emitting units 6015. This makes it possible to obtain information on the position where a touch operation is performed.
[0433] The light emitting unit 6015 may be a light source such as an LED element, and it is particularly preferable to use a light source that emits infrared light. The light receiving unit 6016 may be a photoelectric element that receives the light emitted by the light emitting unit 6015 and converts it into an electric signal. Preferably, a photodiode that can receive infrared light may be used.
[0434] The light guiding portion 6017a and the light guiding portion 6017b that transmit light 6018 allow the light emitting portion 6015 and the light receiving portion 6016 to be disposed below the display device 6006, and it is possible to prevent external light from reaching the light receiving portion 6016 and causing the touch sensor to malfunction. In particular, if a resin that absorbs visible light and transmits infrared light is used, it is possible to more effectively prevent the touch sensor from malfunctioning.
[0435] This embodiment mode can be implemented by appropriately combining at least a part of it with other embodiment modes described in this specification.
[0436] (Embodiment 7) In this embodiment, examples of electronic devices to which the display device of one embodiment of the present invention can be applied will be described.
[0437] Electronic device 6500 shown in FIG. 35A is a portable information terminal that can be used as a smartphone.
[0438] The electronic device 6500 includes a housing 6501, a display portion 6502, a power button 6503, a button 6504, a speaker 6505, a microphone 6506, a camera 6507, and a light source 6508. The display portion 6502 has a touch panel function.
[0439] The display device of one embodiment of the present invention can be applied to the display portion 6502.
[0440] The display portion 6502 has a cutout portion, and a camera 6507 and a light source 6508 are provided so as to engage with the cutout portion. With this structure, the area occupied by the display portion 6502 with respect to the housing 6501 can be increased.
[0441] 35B shows an example in which the display portion 6502 has an opening, and a camera 6507 and a ring-shaped light source 6509 surrounding the camera 6507 are disposed inside the opening. A speaker 6505 is provided so as to engage with a notch in the display portion 6502. The display portion 6502 may be used as a light source for illuminating a subject. With this configuration, the area occupied by the display portion 6502 relative to the housing 6501 can be made larger.
[0442] FIG. 35C is a schematic cross-sectional view including the end of the housing 6501 on the microphone 6506 side.
[0443] A light-transmitting protective member 6510 is provided on the display surface side of the housing 6501, and a display panel 6511, optical members 6512, a touch sensor panel 6513, a printed circuit board 6517, a battery 6518, etc. are arranged in the space surrounded by the housing 6501 and the protective member 6510.
[0444] A display panel 6511, an optical member 6512, and a touch sensor panel 6513 are fixed to the protective member 6510 by adhesive layers (not shown).
[0445] A part of the display panel 6511 is folded back in an area outside the display unit 6502. An FPC 6515 is connected to the folded back part. An IC 6516 is mounted on the FPC 6515. The FPC 6515 is connected to a terminal provided on a printed circuit board 6517.
[0446] The flexible display panel of one embodiment of the present invention can be applied to the display panel 6511. Therefore, an extremely lightweight electronic device can be realized. In addition, since the display panel 6511 is extremely thin, a large-capacity battery 6518 can be mounted thereon while keeping the thickness of the electronic device small. In addition, by folding back a part of the display panel 6511 and arranging a connection portion with the FPC 6515 on the back side of the pixel portion, an electronic device with a narrow frame can be realized.
[0447] This embodiment mode can be implemented by appropriately combining at least a part of it with other embodiment modes described in this specification.
[0448] (Embodiment 8) In this embodiment, electronic devices including a display device manufactured according to one embodiment of the present invention will be described.
[0449] The electronic devices exemplified below each have a display device according to one embodiment of the present invention in a display portion. Therefore, the electronic devices have high resolution. In addition, the electronic devices can have both high resolution and a large screen.
[0450] The display portion of the electronic device according to one embodiment of the present invention can display images with a resolution of, for example, full high definition, 4K2K, 8K4K, 16K8K, or higher.
[0451] Examples of electronic devices include electronic devices with relatively large screens such as television devices, notebook personal computers, monitor devices, digital signage, pachinko machines, and game machines, as well as digital cameras, digital video cameras, digital photo frames, mobile phones, portable game machines, personal digital assistants, and audio playback devices.
[0452] An electronic device to which one embodiment of the present invention is applied can be incorporated along a flat or curved surface of an inner or outer wall of a house or building, or the interior or exterior of an automobile or the like.
[0453] FIG. 36A is a diagram showing the appearance of the camera 8000 with the viewfinder 8100 attached.
[0454] The camera 8000 includes a housing 8001, a display unit 8002, an operation button 8003, a shutter button 8004, etc. In addition, a detachable lens 8006 is attached to the camera 8000.
[0455] In addition, the camera 8000 may have the lens 8006 and the housing integrated together.
[0456] The camera 8000 can capture an image by pressing a shutter button 8004 or touching a display unit 8002 that functions as a touch panel.
[0457] The housing 8001 has a mount having electrodes, and can be connected to a finder 8100 as well as a strobe device or the like.
[0458] The finder 8100 includes a housing 8101, a display portion 8102, a button 8103, and the like.
[0459] The housing 8101 is attached to the camera 8000 by a mount that engages with the mount of the camera 8000. The viewfinder 8100 can display an image received from the camera 8000 on a display unit 8102.
[0460] The button 8103 has a function such as a power button.
[0461] The display device of one embodiment of the present invention can be applied to a display portion 8002 of a camera 8000 and a display portion 8102 of a viewfinder 8100. Note that the camera 8000 may have a built-in viewfinder.
[0462] FIG. 36B is a diagram showing the external appearance of the head mounted display 8200.
[0463] The head mounted display 8200 includes a mounting portion 8201, a lens 8202, a main body 8203, a display portion 8204, and a cable 8205. The mounting portion 8201 includes a built-in battery 8206.
[0464] A cable 8205 supplies power from a battery 8206 to a main body 8203. The main body 8203 includes a wireless receiver or the like and can display received video information on a display portion 8204. The main body 8203 also includes a camera and can use information on the movements of the user's eyeballs and eyelids as an input means.
[0465] The mounting unit 8201 may have a function of recognizing the line of sight by providing a plurality of electrodes at positions that contact the user, capable of detecting a current that flows with the movement of the user's eyeballs. The mounting unit 8201 may also have a function of monitoring the user's pulse rate based on the current that flows through the electrodes. The mounting unit 8201 may also have various sensors, such as a temperature sensor, a pressure sensor, and an acceleration sensor, and may have a function of displaying the user's biological information on the display unit 8204 and a function of changing the image displayed on the display unit 8204 according to the movement of the user's head.
[0466] The display device of one embodiment of the present invention can be applied to the display portion 8204.
[0467] 36C, 36D, and 36E are diagrams showing the external appearance of a head mounted display 8300. The head mounted display 8300 includes a housing 8301, a display unit 8302, a band-shaped fixture 8304, and a pair of lenses 8305.
[0468] A user can view the display on the display unit 8302 through the lens 8305. Note that it is preferable to arrange the display unit 8302 in a curved manner because the user can feel a high sense of presence. In addition, by viewing another image displayed in a different area of the display unit 8302 through the lens 8305, it is possible to perform three-dimensional display using parallax. Note that the present invention is not limited to a configuration in which one display unit 8302 is provided, and two display units 8302 may be provided, with one display unit being provided for each eye of the user.
[0469] Note that the display device of one embodiment of the present invention can be applied to the display portion 8302. A display device including the semiconductor device of one embodiment of the present invention has extremely high definition, so that a user cannot see pixels even when the image is enlarged using a lens 8305 as in FIG. 36E, and a more realistic image can be displayed.
[0470] The electronic device shown in Figures 37A to 37G has a housing 9000, a display unit 9001, a speaker 9003, operation keys 9005 (including a power switch or an operation switch), a connection terminal 9006, a sensor 9007 (including a function to measure force, displacement, position, speed, acceleration, angular velocity, rotation speed, distance, light, liquid, magnetism, temperature, chemical substance, sound, time, hardness, electric field, current, voltage, power, radiation, flow rate, humidity, gradient, vibration, odor or infrared rays), a microphone 9008, etc.
[0471] The electronic device shown in Fig. 37A to Fig. 37G has various functions. For example, it can have a function of displaying various information (still images, videos, text images, etc.) on the display unit, a touch panel function, a function of displaying a calendar, date or time, a function of controlling processing by various software (programs), a wireless communication function, a function of reading and processing a program or data recorded on a recording medium, etc. The functions of the electronic device are not limited to these, and it can have various functions. The electronic device may have multiple display units. In addition, the electronic device may have a function of providing a camera or the like to capture still images and videos and store them on a recording medium (external or built-in to the camera), a function of displaying the captured images on the display unit, etc.
[0472] Details of the electronic device shown in FIGS. 37A to 37G will be described below.
[0473] 37A is a perspective view showing a television device 9100. The television device 9100 can incorporate a display unit 9001 having a large screen, for example, 50 inches or more, or 100 inches or more.
[0474] FIG. 37B is a perspective view showing a mobile information terminal 9101. The mobile information terminal 9101 can be used as, for example, a smartphone. The mobile information terminal 9101 may be provided with a speaker 9003, a connection terminal 9006, a sensor 9007, and the like. The mobile information terminal 9101 can display text and image information on a plurality of surfaces. FIG. 37B shows an example in which three icons 9050 are displayed. Information 9051 shown in a dashed rectangle can also be displayed on another surface of the display unit 9001. Examples of the information 9051 include notifications of incoming e-mail, SNS, and phone calls, titles of e-mail and SNS, sender names, date and time, time, remaining battery level, and antenna reception strength. Alternatively, icons 9050 and the like may be displayed at the position where the information 9051 is displayed.
[0475] 37C is a perspective view showing a mobile information terminal 9102. The mobile information terminal 9102 has a function of displaying information on three or more sides of the display unit 9001. Here, an example is shown in which information 9052, information 9053, and information 9054 are displayed on different sides. For example, a user can check information 9053 displayed in a position that can be observed from above the mobile information terminal 9102 while the mobile information terminal 9102 is stored in a breast pocket of clothes. The user can check the display without taking the mobile information terminal 9102 out of the pocket and decide, for example, whether or not to answer a call.
[0476] FIG. 37D is a perspective view showing a wristwatch-type mobile information terminal 9200. The mobile information terminal 9200 can be used as, for example, a smart watch. The display surface of the display unit 9001 is curved, and display can be performed along the curved display surface. The mobile information terminal 9200 can also perform hands-free conversation by communicating with, for example, a headset capable of wireless communication. The mobile information terminal 9200 can also perform data transmission and charging with another information terminal through a connection terminal 9006. Note that charging may be performed by wireless power supply.
[0477] 37E, 37F, and 37G are perspective views showing a foldable mobile information terminal 9201. FIG. 37E is a perspective view of the mobile information terminal 9201 in an unfolded state, FIG. 37G is a perspective view of the mobile information terminal 9201 in a folded state, and FIG. 37F is a perspective view of the mobile information terminal 9201 in a state in the middle of changing from one of FIG. 37E and FIG. 37G to the other. The mobile information terminal 9201 has excellent portability in a folded state, and has excellent viewability of the display due to a seamless wide display area in an unfolded state. The display unit 9001 of the mobile information terminal 9201 is supported by three housings 9000 connected by hinges 9055. For example, the display unit 9001 can be bent with a curvature radius of 1 mm or more and 150 mm or less.
[0478] 38A shows an example of a television device. A television device 7100 has a display unit 7500 built into a housing 7101. Here, the housing 7101 is supported by a stand 7103.
[0479] 38A can be operated using an operation switch provided on the housing 7101 or a separate remote control 7111. Alternatively, a touch panel may be applied to the display unit 7500, and the television set 7100 may be operated by touching the touch panel. The remote control 7111 may have a display unit in addition to operation buttons.
[0480] The television device 7100 may also include a television broadcast receiver and a communication device for network connection.
[0481] 38B shows a laptop personal computer 7200. The laptop personal computer 7200 includes a housing 7211, a keyboard 7212, a pointing device 7213, an external connection port 7214, and the like. A display unit 7500 is incorporated in the housing 7211.
[0482] 38C and 38D show an example of digital signage.
[0483] 38C includes a housing 7301, a display unit 7500, and a speaker 7303. The digital signage 7300 may further include an LED lamp, an operation key (including a power switch or an operation switch), a connection terminal, various sensors, a microphone, and the like.
[0484] 38D shows a digital signage 7400 attached to a cylindrical pole 7401. The digital signage 7400 has a display unit 7500 provided along the curved surface of the pole 7401.
[0485] The larger the display unit 7500, the more information can be provided at one time, and the larger the display area, the more easily it catches people's attention, which has the effect of increasing the effectiveness of advertising, for example.
[0486] It is preferable to apply a touch panel to the display unit 7500 so that the user can operate it. This allows the display unit 7500 to be used not only for advertising purposes, but also for providing information desired by the user, such as route information, traffic information, and commercial facility guide information.
[0487] 38C and 38D, it is preferable that the digital signage 7300 or the digital signage 7400 can be linked to an information terminal 7311 such as a smartphone carried by a user via wireless communication. For example, advertising information displayed on the display unit 7500 can be displayed on the screen of the information terminal 7311, or the display on the display unit 7500 can be switched by operating the information terminal 7311.
[0488] Furthermore, a game using the information terminal 7311 as an operation means (controller) can be executed on the digital signage 7300 or the digital signage 7400. This allows an unspecified number of users to simultaneously participate in and enjoy the game.
[0489] The display device of one embodiment of the present invention can be applied to the display portion 7500 in FIGS. 38A to 38D.
[0490] Although the electronic device in this embodiment has a display portion, one embodiment of the present invention can also be applied to an electronic device that does not have a display portion. EXAMPLES
[0491] In this example, a transistor including a metal oxide film of one embodiment of the present invention was manufactured, and the results of evaluating the electrical characteristics of the transistor are described.
[0492] [Sample preparation] The structure of the manufactured transistor can be that of Structural example 2-3 of Embodiment 2 and the transistor 350B illustrated in FIG. 27A.
[0493] First, a tungsten film with a thickness of about 100 nm was formed on a glass substrate by sputtering, and then processed to obtain a first gate electrode. Next, a laminated film with a thickness of about 300 nm, which is a first gate insulating layer, was formed by laminating a silicon nitride film and a silicon oxynitride film by plasma CVD.
[0494] Next, a metal oxide film with a thickness of about 30 nm was formed on the first gate insulating layer, and the film was processed to obtain a semiconductor layer. The metal oxide film was formed by a sputtering method using a metal oxide target with an atomic ratio of metal elements of In:Ga:Zn=4:2:4.1 [atomic ratio]. A mixed gas of argon gas and oxygen gas was used as the film formation gas. Four samples (Sample B1 to Sample B4) were fabricated under different film formation conditions for the metal oxide film.
[0495] The metal oxide film of Sample B1 was formed under the condition that the ratio of the flow rate of oxygen gas to the total flow rate of the film-forming gas (oxygen flow rate ratio) was 10%. The film formation was also performed without heating the substrate.
[0496] The metal oxide film of Sample B2 was formed under the condition of an oxygen flow rate ratio of 30% without heating the substrate.
[0497] The metal oxide film of Sample B3 was formed under the condition of an oxygen flow rate ratio of 40% without heating the substrate.
[0498] The metal oxide film of Sample B4 was formed under the condition of an oxygen flow rate ratio of 50% without heating the substrate.
[0499] The metal oxide films of Sample B1 to Sample B4 were formed under the same conditions as those of the metal oxide films of Sample A1 to Sample A4 described in the above-mentioned embodiment 1, respectively.
[0500] After the semiconductor layer was formed, heat treatment was performed at 350° C. for 1 hour in a nitrogen gas atmosphere, and then heat treatment was performed at 350° C. for 1 hour in a mixed atmosphere of nitrogen gas and oxygen gas.
[0501] Subsequently, a silicon oxynitride film having a thickness of about 150 nm was formed as a second gate insulating layer by a plasma CVD method.
[0502] Next, a metal oxide film with a thickness of about 20 nm was formed on the second gate insulating layer by sputtering. The metal oxide film was formed in an oxygen-containing atmosphere using a metal oxide target with an atomic ratio of metal elements of In:Ga:Zn=4:2:4.1 [atomic ratio]. After that, a heat treatment was performed at 350°C for 1 hour in a nitrogen-containing atmosphere.
[0503] Next, a molybdenum film with a thickness of about 100 nm was formed on the metal oxide film by sputtering, and then the molybdenum film and the metal oxide film were partially removed by etching to obtain a second gate electrode and a metal oxide layer.
[0504] Next, using the second gate electrode as a mask, a process of adding boron as an impurity element was performed. A plasma ion doping device was used to add the impurity. The gas used to supply boron was B 2 H 6 Gas was used.
[0505] Next, a silicon oxynitride film with a thickness of about 300 nm was formed by plasma CVD as a protective insulating layer covering the transistor. After that, a part of the protective insulating layer and the second gate insulating layer was opened by etching, and a molybdenum film was formed by sputtering, and then processed to obtain a source electrode and a drain electrode. After that, an acrylic film with a thickness of about 1.5 μm was formed as a planarizing layer, and a heat treatment was performed at 250° C. for 1 hour in a nitrogen atmosphere.
[0506] Through the above steps, Samples B1 to B4, each having a transistor formed on a glass substrate, were obtained.
[0507] [Transistor Id-Vg characteristics] Next, the Id-Vg characteristics of the transistor fabricated as described above were measured.
[0508] As for the measurement conditions of the Id-Vg characteristics of the transistor, the voltage (also called the gate voltage (Vg)) applied to the gate electrodes (first gate electrode and second gate electrode) was applied in increments of 0.25 V from −15 V to +20 V. The voltage (also called the source voltage (Vs)) applied to the source electrode was set to 0 V, and the voltage (also called the drain voltage (Vd)) applied to the drain electrode was set to 0.1 V and 10 V.
[0509] The transistors measured had a design value of a channel length of 2 μm and a channel width of 3 μm.
[0510] 39A to 39D show the Id-Vg characteristics of Samples B1 to B4. In each figure, the horizontal axis shows the gate voltage (Vg) and the vertical axis shows the drain current (Id). In each figure, the dashed line shows the field effect mobility (μFE) calculated from the Id-Vg characteristics when the drain voltage (Vd) is 10 V.
[0511] 39A to 39D, favorable electrical characteristics were obtained for all the samples. This suggests that the influence on electrical characteristics of the transistor using the metal oxide film of one embodiment of the present invention is minimal even if there is variation in the deposition conditions of the metal oxide film (particularly, the oxygen flow rate ratio), and thus it was confirmed that the transistor has excellent mass productivity.
[0512] [Reliability assessment] Next, the reliability of Samples B1 to B4 was evaluated. A gate bias stress test (GBT test) was performed to evaluate the reliability. In the GBT test, the substrate on which the transistors were formed was held at 60°C, and a voltage of 0V was applied to the source and drain of the transistor, and a voltage of 20V or -20V was applied to the gate, and this state was held for one hour. Here, the results of the PBTS test and the NBTIS test are shown in particular. Note that the light irradiation in the NBTIS was performed using white LED light of about 3400lx. The transistors measured here were designed to have a channel length of 2μm and a channel width of 3μm.
[0513] Fig. 40 shows the variation (ΔVth) of threshold voltage before and after the PBTS test and the NBTIS test for Samples B1 to B4. As an example, Fig. 41A to Fig. 41D show the transition of Id-Vg characteristics before and after the GBT test for Samples B1 and B4. Fig. 41A shows the results of the PBTS test for Sample B1, Fig. 41B shows the results of the PBTS test for Sample B4, Fig. 41C shows the results of the NBTIS test for Sample B1, and Fig. 41D shows the results of the NBTIS test for Sample B4.
[0514] As shown in FIG. 40 and FIG. 41A to FIG. 41D, it was confirmed that the variation in threshold voltage was small for all the samples, making them highly reliable transistors.
[0515] From the above results, it was confirmed that a transistor including a metal oxide film of one embodiment of the present invention has favorable transistor characteristics even with a short channel length and is a highly reliable transistor. EXAMPLES
[0516] In this example, the results of investigating the composition of a metal oxide film of one embodiment of the present invention are described.
[0517] [Sample preparation] The sample used in this example was a metal oxide film formed on a glass substrate by sputtering. A metal oxide target with an atomic ratio of metal elements of In:Ga:Zn=4:2:4.1 [atomic ratio] was used for forming the metal oxide film. A mixed gas of argon gas and oxygen gas was used as the film formation gas. The metal oxide film was formed without heating the substrate. Three samples (Sample C1 to Sample C3) were prepared under different conditions for forming the metal oxide film.
[0518] The metal oxide film of Sample C1 was formed under the condition that the ratio of the oxygen gas flow rate to the total flow rate of the film formation gas (oxygen flow rate ratio) was 10%. The metal oxide film of Sample C2 was formed under the condition that the oxygen flow rate ratio was 30%. The metal oxide film of Sample C3 was formed under the condition that the oxygen flow rate ratio was 50%.
[0519] [HAADF-STEM observation and EDX analysis] The three samples prepared were observed using high-angle annular dark field scanning transmission electron microscopy (HAADF-STEM) and their composition was analyzed using energy dispersive X-ray spectroscopy (EDX).
[0520] The HAADF-STEM image and the EDX mapping images for In, Ga, and Zn for each sample are shown in Figure 42. For each sample, the HAADF-STEM image and the EDX mapping image are the results of observing the same region.
[0521] In HAADF-STEM images, contrast proportional to the square of the atomic number is obtained, so brighter areas indicate the presence of heavier atoms. In EDX mapping images, bright areas correspond to areas where the corresponding element is abundant, and dark areas correspond to areas where the corresponding element is scarce.
[0522] As shown in the EDX mapping images in Figure 42, light and dark shading was observed in all of Sample C1, Sample C2, and Sample C3. This confirmed that In, Ga, and Zn were not present uniformly within a range of several nanometers.
[0523] [Quantitative analysis of composition] Next, for each sample, quantitative analysis was performed for In, Ga, and Zn in the bright areas (In-rich areas) and dark areas (In-poor areas) in the EDX mapping images of In, and in the bright areas (Ga-rich areas) and dark areas (Ga-poor areas) in the EDX mapping images of Ga. Quantitative analysis was performed for five points each.
[0524] 43A to 43D show the results of quantitative analysis of Sample C1. Fig. 43A shows the analysis results for the In-rich region, Fig. 43B shows the In-poor region, Fig. 43C shows the Ga-rich region, and Fig. 43D shows the Ga-poor region. In each figure, the horizontal axis shows the ratio of each element when the sum of the compositions of In, Ga, and Zn is 100%, and five measurement points are shown in bar graphs.
[0525] 43B and 43C, it can be seen that Ga is detected more than In, and that there are regions with a higher proportion of Ga compared to the target composition (In:Ga:Zn=4:2:4.1). The fact that In is detected in the In-poor region in FIG. 43B is believed to be the result of the thickness of the measurement sample being about 30 nm, and the In present in the depth direction being detected.
[0526] 43A and 43D, there are also areas where the Ga composition is extremely small or where Ga is not detected. It is presumed that indium oxide or indium zinc oxide exists in the areas where Ga is not detected.
[0527] From the above results, it was confirmed that the metal oxide film actually formed was not a uniform film reflecting the composition of the target, but a film in which regions of different compositions were distributed.
[0528] Although only the results for Sample C1 are shown here, similar trends were observed for Sample C2 and Sample C3.
[0529] [Histogram analysis] Next, a quantitative analysis was performed on the entirety of each EDX mapping image shown in FIG. 42, and the obtained compositions of In, Ga, and Zn were analyzed using histograms.
[0530] Figures 44A, 44B, and 44C show histograms for Sample C1, Sample C2, and Sample C3, respectively. In each figure, the horizontal axis indicates composition, and the vertical axis indicates frequency. In addition, in order to make each element easier to see, the element name is clearly indicated near the apex of the peak in each figure.
[0531] 44A to 44C, it was confirmed that there was no significant difference in the composition distribution in any of the samples. It was also confirmed that there was a region in which Ga was not detected (a region in which the Ga composition was 0) in any of the samples. From the above, it was confirmed that there was no significant difference in the composition distribution in multiple metal oxide films with different crystallinity formed by changing the oxygen flow rate ratio.
[0532] From the above results, it was confirmed that the metal oxide film of one embodiment of the present invention is not a uniform film, but a film in which the metal elements constituting the metal oxide film are distributed non-uniformly, and is observed as a composite film. [Explanation of symbols]
[0533] 10: substrate, 11: metal oxide film, 12a, 12b: region, 20: direct spot, 20a, 20b, 20c, 20d: electron beam diffraction pattern, 21: first spot, 22: second spot, 30, 30a, 30b, 30c, 30r: histogram, 31: first region, 32: second region, 41, 42: peak, 300, 300A: transistor, 302: substrate, 304: conductive layer, 306: insulating layer, 308: semiconductor layer, 312a, 312b, 313a, 313b: conductive layer, 314, 316: insulating layer, 320: conductive layer, 342: opening, 350, 350A, 350B, 350C: transistor, 352: substrate, 353, 353a, 353b: insulating layer, 356: conductive layer, 358: semiconductor layer, 358n: low resistance region, 360: insulating layer, 362: conductive layer, 364: metal oxide layer, 366, 368: insulating layer, 370a, 370b: conductive layer, 391a, 391b, 392: opening
Claims
[Claim 1] A metal oxide film containing indium, M (M is aluminum, gallium, yttrium, or tin), and zinc, a distribution of lattice spacing d determined by electron beam diffraction in which an electron beam is irradiated from a direction perpendicular to a film surface of the metal oxide film has a first peak and a second peak; The apex of the first peak is located at 0.25 nm or more and 0.30 nm or less, The apex of the second peak is located at 0.15 nm or more and 0.20 nm or less, the distribution of the lattice spacing d is obtained from a plurality of electron beam diffraction patterns in a plurality of regions of the metal oxide film, The electron beam diffraction is performed using an electron beam having a beam diameter of 0.3 nm or more and 10 nm or less. Metal oxide film.
Citation Information
Patent Citations
Transistor, semiconductor device, and electronic apparatus
JP2017183718A
Metal oxide film and semiconductor device
JP2018006728A
Semiconductor device
JP2014007399A