AI Technical Summary
Branched polypropylene obtained by existing methods has high melt tension but poor spreadability during melting, and high strain hardening rate at high strain rates leads to non-uniform oriented crystallization and poor moldability.
A branched propylene polymer with a multi-branching index (MBI) of 0.15 to 1.00 and strain hardening degree (SHI@1s) of 0.70 to 3.00 is synthesized by controlling branch chain length and distribution, using metallocene catalysts to introduce a large number of short branches in the high molecular weight region, reducing relaxation time variability.
The polymer maintains high melt tension necessary for molding while improving spreadability and moldability by minimizing non-uniform crystallization, ensuring stable melt tension across varying strain rates.
Smart Images

Figure 2024149581000010 
Figure 2024149581000011 
Figure 2024149581000012
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a branched propylene polymer. [Background technology]
[0002] In recent years, much research has been conducted into introducing a branched structure into polypropylene to improve its suitability for sheet molding, blow molding, thermoforming, foam molding, and other applications that require a material with a relatively high melt tension. Recently, a macromer copolymerization method mainly using a metallocene catalyst has been proposed as a method for introducing a branched structure into polypropylene. Branched polypropylene produced by the macromer copolymerization method has advantages such as less generation of gel due to crosslinking reaction compared to polypropylene in which a branched structure is introduced by irradiation with an electron beam, etc.
[0003] As such a macromer copolymerization method, for example, a method has been proposed in which a propylene macromer having a vinyl structure at its terminal is produced using a specific catalyst under specific polymerization conditions in the first polymerization stage (macromer synthesis step), and then propylene and the propylene macromer are copolymerized using a specific catalyst under specific polymerization conditions in the second polymerization stage (macromer copolymerization step). It has been shown that the resulting branched polypropylene has high melt strength and melt tension (see, for example, Patent Documents 1 and 2). Also, a single-stage polymerization method has been proposed in which a macromer synthesis step and a macromer copolymerization step are carried out simultaneously using a specific metallocene catalyst, and it has been shown that the resulting branched polypropylene exhibits improved melt strength (see, for example, Patent Document 3). In addition, a method for multi-stage polymerization has been proposed using a catalyst that combines a catalyst containing two specific metallocene compounds, specifically, metallocene compounds such as rac-SiMe2[2-Me-4-Ph-lnd]2ZrC12 and rac-SiMe2[2-Me-4-Ph-lnd]2HfC12, with silica supporting methylaluminoxane (MAO). It has been reported that the branched polypropylene obtained exhibits a relatively high melt tension (see Patent Document 4). In addition, a method has been devised that uses a catalyst containing a specific metallocene compound and an ion-exchangeable layered silicate, and it has been reported that the resulting branched polypropylene has a broad molecular weight distribution, a large amount of branching, and good melt tension (see Patent Document 5).
[0004] In addition, a method for producing a propylene-based polymer having a strain hardening factor (λmax) of 2.0 or more in melt tension measurement using a catalyst containing specific multiple metallocene compounds has been devised, and it has been reported that the obtained branched polypropylene has good melt tension (see Patent Document 6).
[0005] Furthermore, Patent Document 7 discloses that by polymerizing propylene using a catalyst in which a single metallocene catalyst is supported on silica having a very low porosity, a branched polypropylene having a better balance between mechanical properties and processability can be obtained by introducing short chain branches with a specific degree of branching and a relatively large amount of amorphous regions. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Special Publication No. 2001-525460 [Patent Document 2] Japanese Patent Application Publication No. 10-338717 [Patent Document 3] Special Publication No. 2002-523575 [Patent Document 4] JP 2001-64314 A [Patent Document 5] JP 2007-154121 A [Patent Document 6] JP 2009-57542 A [Patent Document 7] Special Publication No. 2009-542872 Summary of the Invention [Problem to be solved by the invention]
[0007] However, the branched polypropylenes obtained by the macromer copolymerization methods disclosed in the above Patent Documents 1 to 6 have high melt tension and are highly suitable for sheet molding, blow molding, thermoforming, foam molding, and the like, but have a problem in that the extensibility of the melt is not excellent. In addition, the branched polypropylene obtained by the method disclosed in Patent Document 7 has improved mechanical properties by increasing the content of non-crystalline regions, but the strain hardening at a high strain rate (SHI@1 sec -1 ) is not so high that the moldability during various molding processes is not fully satisfactory.
[0008] An object of the present invention is to provide a branched propylene polymer which has excellent extensibility when molten while maintaining a melt tension necessary for molding. [Means for solving the problem]
[0009] The branched propylene polymer provided by the present invention is characterized by having the following properties (1) and (2). Property (1): Multibranching index (MBI) is 0.15 or more and 1.00 or less. Property (2): Strain hardening at a strain rate (dε / dt) of 1.0 / s (SHI@1s -1 ) is greater than or equal to 0.70 and less than or equal to 3.00. Here, the multibranching index (MBI) is the slope of a plot of the strain hardening index (SHI) at strain rates (dε / dt) of 0.01 / sec to 1.0 / sec, with the logarithm of the strain rate (log(dε / dt)) on the horizontal axis and the strain hardening index (SHI) at strain rates of 0.01 / sec to 1.0 / sec on the vertical axis. In addition, strain hardening index (SHI) is the slope of a plot of the logarithm (log(ε)) of Henky strain (ε) on the horizontal axis and the logarithm (log(ηE)) of extensional viscosity (ηE) on the vertical axis in the Henky strain (ε) range from 1 to 3, when the extensional viscosity is measured at a temperature of 180°C and a predetermined strain rate (dε / dt). Effect of the Invention
[0010] According to the present invention, there is provided a branched propylene polymer which has excellent extensibility when molten while maintaining the melt tension required for molding. [Brief description of the drawings]
[0011] [Figure 1A] FIG. 1A is a schematic diagram illustrating that when a branched propylene polymer has many branches with short branch chain lengths in the high molecular weight region of the molecular weight distribution, entanglement points of molecular chains do not appear so frequently. [Figure 1B] FIG. 1B is a schematic diagram illustrating that when a branched propylene polymer has many branches with long branch chain lengths in the high molecular weight region of the molecular weight distribution, many entanglement points of molecular chains appear. [Diagram 2] FIG. 2 is an example of a plot diagram for determining the strain hardening index (SHI). [Diagram 3] FIG. 3 is an example of a plot diagram for determining the branching index. [Figure 4] FIG. 4 is a diagram illustrating the baseline and intervals of a chromatogram in GPC. [Diagram 5] FIG. 5 is a graph in which the horizontal axis represents MFR (MFR 230° C., 2.16 kg load) and the vertical axis represents multibranching index (MBI), and data on the branched propylene polymers obtained in each of the Examples and Comparative Examples are plotted. [Figure 6] FIG. 6 is a graph in which the horizontal axis represents MFR (MFR 230° C., 2.16 kg load) and the vertical axis represents the maximum winding speed (MaxDraw) at 230° C., and data on the branched propylene polymers obtained in each Example and Comparative Example are plotted. [Figure 7] FIG. 7 is a graph in which the data of the branched propylene polymers obtained in each Example and Comparative Example are plotted, with the melt tension (MT230°C) on the horizontal axis and the maximum winding speed (MaxDraw) at 230°C on the vertical axis. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present inventors synthesized a branched propylene polymer based on a design concept that, in order to improve the extensibility of a branched propylene polymer, a multi-branched molecule having a molecular structure in which a large number of branched chains having a shorter branch chain length than that of a conventional branched propylene polymer are introduced per molecule is contained in a high molecular weight region of the molecular weight distribution of the branched propylene polymer, thereby obtaining a branched propylene polymer having a relaxation time distribution in which many components have a relatively short relaxation time and few components have an extremely long relaxation time. As a result, they succeeded in obtaining a branched propylene polymer with improved extensibility. As shown in FIG. 1A , when a branched propylene-based polymer contains hyperbranched molecules having many branches with short branch chain lengths in the high molecular weight region of the molecular weight distribution, when the branched propylene-based polymer is distorted, an appropriate number of entanglement points of molecular chains appear, and the branched propylene-based polymer exhibits a relaxation time distribution in which there are many components with relatively short relaxation times and few components with extremely long relaxation times. This makes it difficult for local oriented crystallization originating from the entanglement points of molecular chains to occur, making it possible to suppress non-uniformity in oriented crystallization, which is considered to improve extensibility. In contrast, as shown in FIG. 1B , when a branched propylene-based polymer contains hyperbranched molecules having many branches with excessively long branch chain lengths in a high molecular weight region, many entanglement points of molecular chains appear when the branched propylene-based polymer is distorted, resulting in the presence of many components that do not relax or components that take a long relaxation time. As a result, oriented crystallization proceeds locally from the entanglement points of molecular chains at many locations in the polymer, resulting in non-uniform oriented crystallization and poor extensibility. That is, the branched propylene polymer of the present invention is presumed to have a molecular structure based on the design concept of introducing a large number of relatively short long-chain branches into the high molecular weight region of the molecular weight distribution, and has the following characteristic values, and has excellent extensibility when molten while maintaining the melt tension required for molding. The present invention will be described in detail below. In this specification, the use of "to" indicating a range of values means that the values before and after the range include the lower limit and upper limit. In the present invention, logarithms are expressed in the common logarithm sense, ie, with the base 10. In the present invention, the term "stretchability" refers to the property of a resin in a molten state that allows it to be stretched widely and thinly and uniformly, or narrowly and long and uniformly.
[0013] I. Branched propylene polymer of the present invention The branched propylene polymer of the present invention has the following properties (1) and (2), and preferably further has one or more of the following properties (3) to (10). The multi-branching index (MBI) defined in the property (1) can be used as an index for determining the degree of ductility of a molten resin, and the strain hardening index (SHI) defined in the property (2) can be used as an index for determining the degree of melt tension of a molten resin. In the present invention, by specifying the multi-branching index (MBI) and the strain hardening index (SHI) to be within a certain range, a branched propylene polymer having excellent ductility when molten while maintaining a melt tension required for molding is provided.
[0014] Characteristics (1): The branched propylene polymer of the present invention has a multi-branching index (MBI) of 0.15 or more and 1.00 or less. Here, the multibranching index (MBI) is the slope of a plot of the strain hardening index (SHI) of a polymer at strain rates (dε / dt) of 0.01 / sec to 1.0 / sec, with the logarithm of the strain rate (log(dε / dt)) on the horizontal axis and the strain hardening index (SHI) at strain rates of 0.01 / sec to 1.0 / sec on the vertical axis. The strain hardening of a polymer changes with the strain rate (dε / dt). The multi-branching index (MBI) indicates the dependence of the strain hardening index (SHI) on the strain rate (dε / dt). A larger value of the multi-branching index (MBI) means that the strain hardening index (SHI) increases more with an increase in the strain rate (dε / dt).
[0015] In addition, the strain hardening index (SHI) is the slope of a plot of the logarithm (log(ε)) of Henky strain (ε) on the horizontal axis and the logarithm (log(ηE)) of extensional viscosity (ηE) on the vertical axis in the Henky strain (ε) range from 1 to 3, when the extensional viscosity of a polymer is measured at a temperature of 180°C and a predetermined strain rate (dε / dt). Strain hardening index (SHI) indicates the strain hardening of a polymer when strain is applied to the polymer at a given strain rate (dε / dt). When strain is applied to the polymer at a given strain rate (dε / dt), the polymer does not relax and the extensional viscosity increases with the increase in strain.
[0016] (Method of measuring extensional viscosity and calculation of strain hardening index (SHI) and multi-branching index (MBI) at each strain rate (dε / dt)) The strain hardening index (SHI) and multi-branching index (MBI) can be determined by measuring the uniaxial extensional viscosity using the measuring device and measuring method described in, for example, Polymer, Vol. 42, p. 8663 (2001). In the present invention, the strain hardening index (SHI) at each strain rate (dε / dt) can be measured by the following measurement and method. Equipment: Rheometorics Ares Fixture: TA Instruments Extentional Viscosity Fixture ·Measurement temperature: 180℃ ·Strain rate: 1.0 / sec, 0.1 / sec, 0.01 / sec Preparation of test specimen: Press mold a sheet of 18 mm x 10 mm and 0.7 mm thick.
[0017] Figure 2 is an example of a plot diagram for determining the strain hardening index (SHI). Using the above measurement method, data on the time change of the extensional viscosity (ηE) is obtained at a predetermined constant strain rate (dε / dt), the measurement data is plotted on a graph with the logarithm (log(ε)) of the Henky strain (ε) on the horizontal axis and the logarithm (log(ηE)) of the extensional viscosity (ηE) on the vertical axis, and the slope of the extensional viscosity in the Henky strain (ε) range from 1 to 3 is identified from the graph, and the slope is taken as the strain hardening index (SHI) at the strain rate (dε / dt) under the measurement conditions. Fig. 3 is an example of a plot diagram for determining the multi-branching index. Using the above-mentioned measurement method, the strain hardening index (SHI) is measured at multiple strain rates in the range of strain rates (dε / dt) from 0.01 / sec to 1.0 / sec, and the strain hardening index (SHI) at each strain rate is plotted on a graph with the logarithm of the strain rate (log(dε / dt)) on the horizontal axis and the strain hardening index (SHI) on the vertical axis. The slope of the graph in the range of strain rates from 0.01 / sec to 1.0 / sec is identified, and this slope is taken as the multi-branching index (MBI). In the example of Fig. 3, SHI@0.01s -1 , SHI@0.1s -1 , SHI@1.0s -1 The three plots were plotted on a graph, and the slope of the straight line approximating the three plots was taken as the multibranching index (MBI).
[0018] In general, the more components with long relaxation times exist in a polymer, the greater the strain hardening of the polymer will be even at a slow strain rate. The relaxation time of a polymer depends on the structure of the polymer molecule, such as the molecular weight, the presence or absence of branches, the amount of branches, and the length of the branched chains. In particular, in the case of a branched propylene polymer, the relaxation time becomes longer as the branch chain length becomes longer. When the branched chain length of the branched propylene polymer is very long, the relaxation time of the branched propylene polymer is very long, and therefore, even if the strain rate is slow, high strain hardening is exhibited. On the other hand, when the branch chain length is short, the relaxation time of the branched propylene-based polymer is short, so that at a fast strain rate, the branched propylene-based polymer does not relax and exhibits high strain hardening, whereas at a slow strain rate, the branched propylene-based polymer relaxes and the strain hardening decreases. Therefore, the branched propylene polymer as a polymer assembly has different strain hardening dependence on strain rate, i.e., multi-branching index (MBI), depending on the combination of components with long relaxation times and components with short relaxation times and the content ratio of each component. When a branched propylene polymer contains a large amount of components that do not relax or components that have a long relaxation time, oriented crystallization proceeds locally from entanglement points of molecular chains at many locations in the polymer, resulting in non-uniform oriented crystallization and poor extensibility. In contrast, when a branched propylene polymer contains many multi-branched molecules having many branches with short branch chain lengths per molecule in the high molecular weight region of the molecular weight distribution, the polymer exhibits a relaxation time distribution in which there are many components with relatively short relaxation times and few components with extremely long relaxation times. This makes it difficult for local oriented crystallization to occur originating from entanglement points of molecular chains, and makes it possible to suppress non-uniformity in oriented crystallization, which is believed to improve extensibility.
[0019] In order to provide the branched propylene polymer of the present invention with excellent extensibility when melted, the lower limit of the multi-branching index (MBI) of the branched propylene polymer is set to 0.15 or more, preferably 0.16 or more, and more preferably 0.17 or more. In order to provide stability in melt tension by suppressing the strain rate dependency of strain hardening, the upper limit of the multi-branching index (MBI) of the branched propylene polymer of the present invention is set to 1.00 or less, preferably 0.80 or less, and more preferably 0.50 or less. By setting the multi-branching index (MBI) of the branched propylene polymer to 0.15 or more and 1.0 or less, the polymer does not relax at a fast strain rate (1.0 / sec) and has a large strain hardening degree (SHI@0.1 / sec), but relaxes at a slow strain rate (0.01 / sec) and has a small strain hardening degree (SHI@0.01 / sec). Therefore, the branched propylene polymer of the present invention exhibits a relaxation time distribution in which many components have a relatively short relaxation time and few components have an extremely long relaxation time, and therefore has excellent extensibility. The branched propylene polymer has a strain hardening index (SHI@1s) in a specific range as specified in the following property (2). -1 ), if the multibranching index (MBI) is less than 0.15, the strain rate dependency of the strain hardening index (SHI) is too small, so that even at a slow strain rate such as 0.01 s or 0.1 s, the strain hardening at a strain rate of 1 s (SHI@1s -1 ) shows a large strain hardening degree that is not so different from that of the branched propylene polymer. Therefore, in this case, the branched propylene polymer contains many components having a long relaxation time, and has poor ductility. On the other hand, the branched propylene polymer has a strain hardening index (SHI@1s -1 ), if the multi-branching index (MBI) is more than 1.0, the strain rate dependency of the strain hardening (SHI) is too high, so that even a slight change in the strain rate changes the strain hardening, and the melt tension is likely to become unstable. Therefore, in this case, when the branched propylene polymer is molded, problems such as molding defects occurring and difficulty in controlling the conditions of the molding process occur.
[0020] The strain hardening and the multi-branching index (MBI), which is indicated by the strain rate dependency of the strain hardening, can be adjusted by controlling the amount and length of the branched chains in the branched propylene-based polymer. For example, the molecular weight of the macromer in the macromer synthesis step correlates with the length of the branched chain. Therefore, in the combination of a metallocene complex that mainly contributes to the synthesis of the macromer and a metallocene complex that mainly contributes to the copolymerization of propylene and the macromer, the molecular weight of the macromer can be adjusted by selecting the metallocene complex that contributes to the synthesis of the macromer. Specifically, the molecular weight of the macromer can be adjusted by selecting a combination of bulkier substituents at the 2- and 4-positions of the indene skeleton of the metallocene. In addition, macromers are produced through β-hydrogen elimination from the ends of growing chains. By increasing the polymerization temperature, the β-hydrogen elimination reaction can be made faster relative to the propylene insertion growth reaction, thereby reducing the molecular weight of the macromer. Regarding the amount of branching, the ratio of propylene to macromer in the macromer copolymerization step correlates with the amount of branching. Specifically, the amount of macromer incorporation can be adjusted by selecting the activity of the metallocene complex that contributes to the synthesis of the macromer and the activity of the metallocene complex that mainly contributes to the copolymerization of propylene and macromer. As another method, the amount of the macromer incorporated can be adjusted by selecting the amount of the metallocene complex used that contributes to the synthesis of the macromer and the amount of the metallocene complex used that mainly contributes to the copolymerization of propylene and the macromer.
[0021] Characteristics (2): The branched propylene polymer of the present invention has a strain hardening coefficient (SHI@1s -1 ) is preferably 0.70 or more and 3.00 or less. Here, the strain hardening rate at 1.0 / s (SHI@1s -1 ) is the slope of a plot of the logarithm of Henky strain (ε) (log(ε)) on the horizontal axis and the logarithm of extensional viscosity (ηE) (log(ηE)) on the vertical axis in the Henky strain (ε) range from 1 to 3, when measuring the extensional viscosity at a temperature of 180°C and a strain rate (dε / dt) of 1.0 / sec. From the viewpoint of increasing the melt tension to improve moldability and improving extensibility, the branched propylene polymer of the present invention has a strain hardening index (SHI@1s -1 ) is preferably 0.70 or more, more preferably 0.80 or more, and even more preferably 1.0 or more. -1 ) is preferably 3.00 or less, more preferably 2.00 or less, and even more preferably 1.70 or less. Branched propylene polymers have a high strain rate and a high strain hardening rate (SHI@1s -1When the strain hardening coefficient (SHI@1s) is relatively large, the polymer contains components that do not relax at high strain rates, which increases the elongational viscosity. -1 ) compared to polymers with a smaller elongational viscosity, the melt tension is increased due to the higher elongational viscosity, which improves moldability in sheet molding, blow molding, thermoforming, and foam molding. From this viewpoint, the branched propylene polymer of the present invention has a strain hardening index (SHI@1s -1 ) is preferably 0.70 or more. On the other hand, the branched propylene polymer exhibits a high strain rate and a high strain hardening rate (SHI@1s -1 If the strain hardening index (SHI@1s) is too large, the number of components that do not relax or components that relax for a long period of time is large, so that oriented crystallization proceeds locally from the entanglement points of molecular chains, resulting in a problem of deterioration in ductility. From this viewpoint, the branched propylene polymer of the present invention has a strain hardening index (SHI@1s -1 ) is preferably 3.00 or less.
[0022] Characteristics (3): In the branched propylene polymer of the present invention, the proportion of components soluble in p-xylene at 25° C. (CXS) is less than 0.5% by mass. CXS is used as an index of the proportion of low molecular weight and low regular components in branched propylene polymers. If CXS is too high, the amount of low molecular weight and low stereoregular components increases, which affects various physical properties. The CXS is preferably 0.4 mass % or less, and more preferably 0.3 mass % or less. There is no lower limit for CXS, but from the viewpoint of the feel of the molded article, it is preferably 0.1% by mass or more, and more preferably 0.2% by mass or more.
[0023] In the present invention, the method for measuring CXS is as follows. 2 g of the sample is dissolved in 300 ml of p-xylene (containing 0.5 mg / ml BHT) at 130°C to form a solution, which is then left to stand at 25°C for 48 hours. The precipitate and filtrate are then separated by filtration. The p-xylene is evaporated from the filtrate, which is then dried under reduced pressure at 100°C for 12 hours to recover the components dissolved in the p-xylene at 25°C. The percentage value of the mass of the recovered components relative to the mass of the sample is defined as CXS.
[0024] In order to control the amount of CXS, it is good to select a bridged indene complex or azulene complex as the metallocene complex of the catalyst component so that the amount of low molecular weight components is relatively small and the stereoregularity is high, and in particular, it is possible to control the amount of CXS by adjusting the bulkiness of the substituent at the 2nd or 4th position. In addition, when two complexes are combined, the overall amount of CXS can be controlled by selecting a complex with high stereoregularity and adjusting the ratio of the complexes. In addition, if the amount of the organoaluminum compound, which is a catalyst component, is increased, it coordinates with part of the complex, causing it to change, resulting in an increase in low molecular weight components and a decrease in stereoregularity. Therefore, the amount of CXS can be controlled by optimizing the amount of the organoaluminum compound.
[0025] Characteristics (4): In the branched propylene polymer of the present invention, the molecular weight Mn of the branched side chain of the branched propylene polymer is preferably 11,000 or more and 53,000 or less. Reference: Macromolecules, Vol. 31, p. 1335 (1998) states that the entanglement molecular weight of isotactic polypropylene was found to be 6900 g / mol. Also, in the reference, Macromolecules, Vol. 35, p. 10062 (2002), it is stated that when the branch length of a propylene polymer is 7000 g / mol or less, the effect on viscoelasticity is small. In light of these documents, in order to exhibit viscoelastic behavior such as strain hardening, the length of the branched chain must be 6,900 to 7,000 g / mol or more in terms of the entanglement molecular weight of polypropylene. This corresponds to a skeleton carbon number of about 400 or more. The skeleton carbon here means all carbons other than methyl carbons in the case of propylene alone or copolymerization of propylene and ethylene. In addition, when butene is used in addition to the above monomers, it means all carbon atoms other than methyl carbons and ethyl carbons. Therefore, at a high strain rate, the degree of strain hardening increases and, in order to obtain the melt tension required for molding, the length of the branched chain of the branched propylene polymer of the present invention, in terms of the number of carbon atoms in the backbone, is preferably 500 or more (11,000 or more in terms of the molecular weight of polypropylene), more preferably 700 or more (15,000 or more in terms of the molecular weight of polypropylene), and even more preferably 1000 or more (21,000 or more in terms of the molecular weight of polypropylene). Regarding the branch length of the branched propylene polymer of the present invention, at a fast strain rate, the degree of strain hardening is large and a melt tension required for molding can be obtained, but at a slow strain rate, the strain is sufficiently relaxed and the strain hardening becomes small, so that the number of carbon atoms in the skeleton is preferably 2500 or less (polypropylene molecular weight equivalent: 53,000 or less), more preferably 2200 or less (polypropylene molecular weight equivalent: 46,000 or less), and even more preferably 2000 or less (polypropylene molecular weight equivalent: 42,000 or less).
[0026] The polypropylene molecular weight conversion value here is, strictly speaking, different from the molecular weight value measured by GPC, but is close to the number average molecular weight (Mn) measured by GPC. In addition, the length of the branch on the branched propylene-based polymer cannot be measured directly, but by polymerizing propylene under the same conditions as those for producing the branched propylene-based polymer of the present invention, a macromer corresponding to the branch portion is synthesized, and the number average molecular weight (Mn) of the macromer measured by GPC according to the method shown in the Examples can be assumed to be the length of the branch. Therefore, the lower limit of the branched chain length of the branched propylene polymer of the present invention is preferably 11,000 or more, more preferably 15,000 or more, and even more preferably 21,000 or more, in terms of the number average molecular weight (Mn) measured by GPC. On the other hand, the upper limit of the branched chain length of the branched propylene polymer of the present invention is preferably 53,000 or less, more preferably 46,000 or less, and even more preferably 42,000 or less, in terms of the number average molecular weight (Mn) measured by GPC.
[0027] (Method of measuring molecular weight) The molecular weight is obtained as the number average molecular weight (Mn), weight average molecular weight (Mw), and Q value (Mw / Mn) by gel permeation chromatography (GPC). Details of the measurement method and measuring equipment are as follows. Apparatus: Waters GPC (ALC / GPC, 150C) Detector: FOXBORO MIRAN, 1A, IR detector (measurement wavelength: 3.42 μm) Column: Showa Denko AD806M / S (3 columns) Mobile phase solvent: o-dichlorobenzene (ODCB) ·Measurement temperature: 140℃ ·Flow rate; 1.0mL / min ·Injection volume; 0.2mL The sample is prepared by mixing the sample with ODCB (containing 0.5 mg / mL dibutylhydroxytoluene (BHT)) at a sample concentration of 1 mg / mL and dissolving at 140° C. for about 1 hour. The baseline and intervals of the obtained chromatogram are as shown in Figure 4. The retention volume obtained by GPC measurement is converted to molecular weight using a calibration curve prepared in advance using standard polystyrenes. The standard polystyrenes used are all the following brands manufactured by Tosoh Corporation. Brand Name: F380, F288, F128, F80, F40, F20, F10, F4, F1, A5000, A2500, A1000 A calibration curve is created by injecting 0.2 mL of a solution of each standard dissolved in ODCB (containing 0.5 mg / mL BHT) so that the concentration of each standard is 0.5 mg / mL. The calibration curve is a cubic equation obtained by approximating the curve using the least squares method. Viscosity formula used for conversion to molecular weight: [η] = K × M α The following numerical values are used: PS:K=1.38×10 -4 , α=0.7 PP:K=1.03×10 -4 , α=0.78
[0028] Characteristics (5): The branched propylene polymer of the present invention preferably has a melt flow rate (MFR) measured at a temperature of 230° C. under a load of 2.16 kg of 1 to 10 g / 10 min. MFR is an index of fluidity when melted. As the molecular weight of a polymer increases, the MFR decreases. If the MFR is too small, the fluidity when melted decreases, making hot molding difficult. On the other hand, as the molecular weight of a polymer decreases, the MFR increases. If the MFR is too large, it causes a decrease in melt tension. Also, if the MFR is large, the fluidity when melted improves, but the impact strength may decrease. From the viewpoint of heat moldability, the MFR of the propylene polymer of the present invention is preferably 1 g / 10 min or more, more preferably 2 g / 10 min or more, and even more preferably 3 g / 10 min or more. On the other hand, from the viewpoints of melt tension and impact strength, the MFR of the propylene polymer of the present invention is preferably 10 g / 10 min or less, more preferably 8 g / 10 min or less, and even more preferably 6 g / 10 min or less. Among these, a particularly preferred range of MFR is 1 g / 10 min or more and 6 g / 10 min or less. In the present invention, the melt flow rate (MFR) is a value measured in accordance with JIS K6921-2 "Plastics - Polypropylene (PP) molding and extrusion materials - Part 2: Preparation of test pieces and determination of properties" under test conditions of 230°C and a load of 2.16 kgf. The melt flow rate (MFR) can be easily adjusted by changing the polymerization temperature or pressure or, as a general method, by adding a chain transfer agent such as hydrogen during polymerization.
[0029] Characteristics (6): Regarding the branching amount of the branched propylene polymer of the present invention, 13 It can be measured as an average value for the entire polymer using C-NMR, and a relative outline of the degree of branching at each absolute molecular weight can be obtained as an index from the relationship between the absolute molecular weight (Mabs) and the branching index (g') using 3D-GPC. In the branched propylene polymer of the present invention, the ratio of components having a molecular weight M of 1 million or more to the total amount of the polymer (W1 million) is preferably 0.070 or more and 0.100 or less in a molecular weight distribution curve measured by GPC. W1 million is an index showing the ratio of high molecular weight components contained in a polymer. W1 million is defined as the value obtained by subtracting from 1 the integral value up to a molecular weight M of 1 million or less (Log(M)=6.0) in an integrated molecular weight distribution curve (total amount normalized to 1 on a mass basis) measured by GPC. The branched propylene polymer of the present invention preferably has a branching index g' (1 million) of 0.80 or more and 0.90 or less when the absolute molecular weight Mabs measured by 3D-GPC is 1 million.
[0030] The branching index g' is the intrinsic viscosity [η] of a polymer with a long chain branching structure. br Intrinsic viscosity [η] of a linear polymer with the same molecular weight lin Ratio of ([η] br / [η] lin ) and takes a value less than 1.0 when long chain branches are present. The definitions are described, for example, in "Developments in Polymer Characterization-4" (JV Dawkins ed. Applied Science Publishers, 1983), and are known guidelines for those skilled in the art. The branching index g' can be calculated by, for example, measuring the absolute molecular weight M abs can be obtained as a function of In the present invention, 3D-GPC refers to a GPC apparatus connected with three detectors, which are a differential refractometer (RI), a viscometer, and a multi-angle laser light scattering detector (MALLS). The GPC apparatus used is Alliance GPCV2000 manufactured by Waters Corporation, equipped with a differential refractometer (RI) and a viscometer. The light scattering detector used is a multi-angle laser light scattering detector (MALLS) manufactured by Wyatt Technology Corporation, DAWN-E. The detectors are connected in the following order: MALLS, RI, and Viscometer. The mobile phase solvent was 1,2,4-trichlorobenzene (containing the antioxidant Irganox 1076 manufactured by BASF Japan at a concentration of 0.5 mg / mL). The flow rate is 1 mL / min, and two Tosoh GMHHR-H(S)HT columns are connected in series. The temperatures of the column, the sample injection part and each detector were 140°C. The sample concentration was 1 mg / mL, and the injection volume (sample loop volume) was 0.2175 mL. Absolute molecular weight obtained from MALLS (M abs ), the root mean square radius of gyration (Rg), and the intrinsic viscosity ([η]) obtained from the Viscometer are calculated using the data processing software ASTRA (version 4.73.04) attached to MALLS, with reference to the following literature. References: 1.Developments in Polymer Characterization, vol.4. Essex: Applied Science; 1984. Chapter1. 2.Polymer, 45, 6495-6505(2004) 3.Macromolecules, 33, 2424-2436(2000) 4.Macromolecules, 33, 6945-6952(2000) The branching index g' is the intrinsic viscosity ([η] br ) and the intrinsic viscosity ([η] obtained by separately measuring a linear polymer lin ) and the ratio ([η] br / [η] lin ) is calculated as follows.
[0031] When a long chain branch structure is introduced into a polymer molecule, the radius of gyration becomes smaller compared to a linear polymer molecule of the same molecular weight. Since a smaller radius of gyration results in a smaller intrinsic viscosity, the intrinsic viscosity ([η]) of a linear polymer of the same molecular weight increases with the introduction of a long chain branch structure. lin ) versus the intrinsic viscosity of branched polymers ([η] br ) ratio ([η] br / [η] lin ) becomes smaller. Therefore, for polymers with long chain branching, the branching index g'([η] br / [η] lin ) is less than 1.0, and linear polymers, by definition, have a branching index g' of 1.0. Here, a commercially available homopolypropylene (Novatec PP (registered trademark) manufactured by Japan Polypropylene Corporation, grade name: FY6) was used as the linear polymer, and [η] lin [η] of linear polymer lin The logarithm of [η] has a linear relationship with the logarithm of the molecular weight, as known from the Mark-Houwink-Sakurada equation. lin can be obtained by extrapolating to the low molecular weight side or the high molecular weight side as appropriate. A branching index g' of less than 1.0 can be achieved by introducing a large amount of long chain branches, or by increasing the branch chain length when the number of branches is the same. This can be achieved by controlling the selection of catalysts, their combination and amount ratio, and the prepolymerization conditions. Each branching index g' can be set within the above-mentioned specific range by appropriately adjusting the amount of hydrogen during polymerization in addition to the selection of catalysts, their combination and amount ratio, as described below.
[0032] Characteristics (7): The branched propylene polymer has a melting point (Tm) of 150° C. or higher and 157° C. or lower, as measured by differential scanning calorimetry (DSC). The higher the Tm of the branched propylene polymer, the more improved its heat resistance and rigidity are. Therefore, the Tm is preferably 150° C. or higher, and more preferably 151° C. or higher. On the other hand, if the branched propylene polymer has too high a Tm, the rigidity may become too high, resulting in poor feel to the touch, etc. Therefore, the Tm is preferably 157° C. or less, and more preferably 155° C. or less. In the case of polypropylene, Tm is decreased by the insertion of ethylene units or regioregular defects. The Tm of the branched propylene polymer of the present invention can be controlled by selecting an optimal complex for regioregular defects as a polymerization catalyst, selecting a combination of multiple complexes, and further controlling the polymerization temperature and polymerization pressure. The melting point (Tm) of the branched propylene polymer can be measured by the following method: Using a Seiko Instruments Inc. DSC6200, 5 mg of a sheet-shaped sample piece is packed in an aluminum pan, heated from room temperature to 200°C at a heating rate of 100°C / min, held for 5 minutes, and then cooled to 20°C at 10°C / min to crystallize, and the crystallization temperature (Tc) is determined as the maximum crystallization peak temperature (°C), and then heated to 200°C at 10°C / min to determine the melting point (Tm) as the maximum melting peak temperature (°C). The sheet-like sample can be obtained by sandwiching the branched propylene polymer powder between press plates, preheating it at 190°C for 2 minutes, pressing it at 5 MPa for 2 minutes, and then cooling it at 0°C and 10 MPa for 2 minutes.
[0033] Characteristics (8): The branched propylene polymer of the present invention may have a long chain branched (LCB) structural portion represented by the following structural formula (A).
[0034] [ka]
[0035] [In the structural formula (A), P1, P2, and P3 are residues generated at the ends of the branched propylene polymer, each having one or more propylene units, Cbr represents a methine carbon at the root of a branched chain having 7 or more carbon atoms, and Ca, Cb, and Cc represent methylene carbons adjacent to the methine carbon (Cbr).] In the structural formula (A), the main chain of the branched propylene polymer is P 1 -Cbr-P 2 Line, P 1 -Cbr-P 3 Line or P 2 -Cbr-P 3 There are three types of lines. 3 Line, CBR-P 2 Line or Cbr-P 1 The line can be the branched chain. 1 , P 2 , P 3 may itself contain a branched carbon (Cbr) other than the Cbr depicted in structural formula (A). Here, the assignment of the LCB structure is 13 By C-NMR, three methylene carbons (Ca, Cb, Cc) are observed at 44.0-44.1 ppm, 44.7-44.8 ppm, and 44.8-44.9 ppm, and a methine carbon (Cbr) is observed at 31.6-31.8 ppm. It is characterized in that the three methylene carbons adjacent to Cbr are observed as three diastereotopic unequal carbons. Also, the LCB number is: 13 It is the number of branched chains having 7 or more carbon atoms per 1000 monomer units (1000p) calculated by C-NMR. Branched chains with more than six carbon atoms can be distinguished from branched chains with six or fewer carbon atoms by the difference in the peak position of the methine carbon at the base of the branch (Macromolecules, Vol. 35, No. 10, 2002). In the present invention, the LCB number is not particularly limited, but is preferably 1.0 or less per 1000 p.
[0036] 13 Details of the method for measuring the long chain branching (LCB) structure calculated by C-NMR are as follows. [Sample preparation] Approximately 200 mg of sample is placed in an NMR sample tube with an inner diameter of 10 mm together with 2.4 ml of o-dichlorobenzene / deuterated bromide benzene (C6D5Br) = 2 / 1 (volume ratio) and hexamethyldisiloxane, a chemical shift standard substance, and the tube is purged with nitrogen, sealed, and heated to dissolve to make a homogeneous solution. [Apparatus and measurement method] NMR measurements were performed using an AVANCE400 NMR instrument manufactured by Bruker Biospin Corporation equipped with a 10 mm diameter cryoprobe. Probe temperature 120°C, pulse angle 45°, pulse interval 4.2 seconds, cumulative count 20,000 or more, proton broadband decoupling method 13 Perform C-NMR measurement. The chemical shifts are those of hexamethyldisiloxane. 13 The C signal was set to 1.98 ppm, and the other 13 The chemical shifts of the C signals were referenced to this. [How to calculate the number of long chain branches (LCB number)] When the intensity of methylene carbon in the propylene main chain from 44.4 to 49.0 ppm is standardized to 1000, the average of the methylene carbon intensity from 44.0 to 44.1 ppm and the methine carbon (Cbr) intensity from 31.6 to 31.8 ppm is defined as the number of long chain branches per 1000 propylene monomer units.
[0037] Characteristics (9): In order to obtain a propylene-based polymer excellent in extensibility while maintaining a melt tension necessary for molding, the propylene-based polymer produced by the present invention has a melt tension at 230°C (MT230°C) of preferably 4.0 g or more, more preferably 5.0 g or more, and particularly preferably 6.0 g or more, and an upper limit of MT230°C is preferably 19.0 g or less, more preferably 18.0 g or less, and particularly preferably 17.0 g or less. The melt tension at 230°C (MT230°C) is measured using a melt tension tester (e.g., Capilograph 1B manufactured by Toyo Seiki Seisakusho). At a resin temperature of 230°C, resin is extruded into a string shape under the following conditions, and the tension detected at the pulley when the resin is wound up around a roller is taken up as the melt tension (MT230°C). Capillary: diameter 2.0mm, length 40mm Cylinder diameter: 9.55mm Cylinder extrusion speed: 20mm / min · Winding speed: 4.0m / min In addition, if breakage occurs at a winding speed of 4.0 m / min, it is considered that "melt tension cannot be evaluated."
[0038] Characteristics (10): The branched propylene polymer produced by the present invention has a controlled branched structure (amount of branches, branch length, branch distribution), and therefore has high melt tension and improved melt extensibility. The melt extensibility was measured by the above-mentioned melt tension measurement method, in which the resin was extruded into a string shape under the following conditions and wound around a roller while gradually increasing the winding speed from 4.0 m / min (acceleration: 5.4 cm / s 2 ) The winding speed just before the string-like material breaks is measured, and the maximum winding speed (MaxDraw) thus measured can be used as an index for evaluation. Note that a larger MaxDraw means better extensibility.
[0039] The maximum winding speed can be measured using a Capillograph 1B manufactured by Toyo Seiki Seisakusho Co., Ltd. under the following conditions: The initial winding speed is 4.0 m / min, and the speed is increased at a constant acceleration rate. The winding speed at which the strand breaks is measured. Capillary: diameter 2.0mm, length 40mm Cylinder diameter: 9.55mm Cylinder extrusion speed: 20mm / min · Winding speed: 4.0m / min-200.0m / min ·Temperature: 230℃
[0040] The branched propylene polymer produced by the present invention can have a large MaxDraw while maintaining a high melt tension by controlling the branching components and the branch chain length, and has an improved balance between melt tension and melt extensibility. In the branched propylene polymer produced by the present invention, the maximum draw speed (MaxDraw) is preferably 55 m / min or more, more preferably 65 m / min or more, and further preferably 75 m / min or more.
[0041] In terms of durability, it is preferable that the branched propylene polymer produced by the present invention has a relationship between the maximum draw-up speed (MaxDraw) (unit: m / min) and the MFR (unit: g / 10 min) satisfying the relationship represented by the following formula (1). (MaxDraw) ≧ 62 × log(MFR) + 7 Equation (1) Generally, increasing the fluidity leads to excellent extensibility, but the melt tension decreases, and increasing the fluidity to provide excellent extensibility leads to the problem that the melt tension becomes insufficient, so it is desirable for the propylene polymer to have both the melt tension required for molding and excellent extensibility. The above formula (1) shows that the branched propylene polymer produced by the present invention has excellent extensibility commensurate with the fluidity, as compared with conventional propylene polymers. That is, in order to distinguish the branched propylene polymer of the present invention from the conventional ones, the maximum winding speed (MaxDraw) is considered to be a function positively correlated with an increase in fluidity (MFR), the parameters of the function are set, and the maximum winding speed (MaxDraw) of the branched propylene polymer produced by the present invention is shown to be greater in proportion to the fluidity than the maximum winding speed (MaxDraw) of the conventional propylene polymer defined by the function. Specifically, based on the data of the examples and comparative examples, the values of the maximum winding speed (MaxDraw) and fluidity (MFR) that distinguish the examples from the comparative examples of the prior art are assumed, and the parameters of the relational equation that holds between the maximum winding speed (MaxDraw) and the fluidity (MFR) are determined by the least squares method. The branched propylene polymer produced by the present invention has excellent extensibility commensurate with its fluidity, and therefore retains the melt tension necessary for molding and exhibits excellent extensibility even if its fluidity is low.
[0042] II. Method for producing branched propylene polymer The method for producing the branched propylene polymer of the present invention is not particularly limited as long as it is a method that can produce a branched propylene polymer that satisfies the above-mentioned physical properties that are the characteristics of the present invention. For example, a macromer copolymerization method using a metallocene catalyst is included, and preferably, a method using a catalyst containing multiple metallocene compounds as described below that can produce a long-chain branched propylene polymer is included. As a method for producing the branched propylene polymer of the present invention, a method for producing a branched propylene polymer using the following catalyst components (A), (B) and (C) as a propylene polymerization catalyst can be mentioned as a suitable method. (A): At least one of the components [A-1], which is a compound represented by the following general formula (a1), and at least one of the components [A-2], which is a compound represented by the following general formula (a2), are selected as two or more transition metal compounds of Group 4 of the periodic table. Component [A-1]: A compound represented by general formula (a1) Component [A-2]: a compound represented by general formula (a2) (B): A compound or ion-exchangeable layered silicate that reacts with component (A) to form an ion pair. (C): Organoaluminum compounds
[0043] The catalyst components (A), (B) and (C) will be described in detail below. 1. Catalyst component (A) 1-1. Component [A-1]: Compound represented by general formula (a1) As the component [A-1], a metallocene compound represented by the following general formula (a1) is preferably used from the viewpoint of producing a propylene-based polymer having a high terminal vinyl ratio.
[0044] [ka]
[0045] [In general formula (a1), R 11 and R 12 R each independently represents a heterocyclic group containing nitrogen, oxygen or sulfur and having 4 to 16 carbon atoms. 13 and R 14 Q each independently represents an aryl group having 6 to 30 carbon atoms which may contain halogen, silicon, oxygen, sulfur, nitrogen, boron, phosphorus, or a plurality of hetero elements selected from these, or a heterocyclic group having 6 to 16 carbon atoms which contains nitrogen, oxygen, or sulfur. 11 represents a divalent hydrocarbon group having 1 to 20 carbon atoms, or a silylene group or germylene group which may have a hydrocarbon group having 1 to 20 carbon atoms; M 11 represents zirconium or hafnium, and X 11 and Y 11 each independently represents a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a silyl group having a hydrocarbon group having 1 to 20 carbon atoms, a halogenated hydrocarbon group having 1 to 20 carbon atoms, an amino group, or an alkylamino group having 1 to 20 carbon atoms.]
[0046] Above R 11 and R 12The nitrogen-, oxygen- or sulfur-containing heterocyclic group having 4 to 16 carbon atoms is preferably a 2-furyl group, a substituted 2-furyl group, a substituted 2-thienyl group or a substituted 2-furfuryl group, and more preferably a substituted 2-furyl group. R 11 and R 12 is a group selected from heterocyclic groups containing nitrogen, oxygen, or sulfur and having 4 to 16 carbon atoms, the terminal vinyl ratio (Rv) can be increased. In particular, by introducing a substituent of an appropriate size onto the heterocyclic group, the relative positional relationship between the heterocycle and the coordination field on the transition metal and the growing polymer chain can be made appropriate, thereby making it possible to further increase the terminal vinyl ratio (Rv) and reduce the molecular weight of the polymer. Examples of the substituent of the substituted 2-furyl group, substituted 2-thienyl group, and substituted 2-furfuryl group include alkyl groups having 1 to 6 carbon atoms, such as methyl, ethyl, n-propyl, i-propyl, n-butyl, i-butyl, and t-butyl groups, halogen atoms such as fluorine and chlorine atoms, alkoxy groups having 1 to 6 carbon atoms, such as methoxy and ethoxy groups, and trialkylsilyl groups. Among these, methyl, trimethylsilyl, and t-butyl groups are preferred, and methyl and t-butyl groups are particularly preferred. In addition, R 11 and R 12 Particularly preferred as R are 5-t-butyl-2-furyl and 5-methyl-2-furyl groups. 11 and R 12 are preferably identical to each other.
[0047] Above R 13 and R 14 are each independently an aryl group having 6 to 30 carbon atoms which may contain halogen, silicon, oxygen, sulfur, nitrogen, boron, phosphorus, or a plurality of hetero elements selected from these, or a heterocyclic group having 6 to 16 carbon atoms which contains nitrogen, oxygen, or sulfur. In particular, R 13 and R 14By making the copolymer bulkier, it is possible to obtain a propylene polymer having higher stereoregularity, fewer heterogeneous bonds, and a higher terminal vinyl ratio. So, R 13 and R 14 is preferably an aryl group having one or more hydrocarbon groups having 1 to 6 carbon atoms, silyl groups having a hydrocarbon group having 1 to 6 carbon atoms, halogen-containing hydrocarbon groups having 1 to 6 carbon atoms, or aryl groups which may have a halogen atom as a substituent on an aryl ring skeleton, in the range of 6 to 16 carbon atoms, and such R 13 and R 14 Specific examples of the aryl group include a 4-t-butylphenyl group, a 2,3-dimethylphenyl group, a 3,5-di-t-butylphenyl group, a 4-chlorophenyl group, a 4-trimethylsilylphenyl group, a 1-naphthyl group, and a 2-naphthyl group. Also, R 13 and R 14 More preferably, R is a phenyl group having one or more hydrocarbon groups having 1 to 6 carbon atoms, silyl groups having a hydrocarbon group having 1 to 6 carbon atoms, halogen-containing hydrocarbon groups having 1 to 6 carbon atoms, or halogen atoms as substituents, with the carbon number being in the range of 6 to 16. The position of substitution is preferably the 4-position on the phenyl group. 13 and R 14 Specific examples of R include a 4-t-butylphenyl group, a 4-biphenylyl group, a 4-chlorophenyl group, and a 4-trimethylsilylphenyl group. 13 and R 14 are preferably identical to each other.
[0048] Above X 11 and Y 11 is an auxiliary ligand, and reacts with component (B) to produce an active metallocene having olefin polymerization ability. Therefore, as long as this purpose is achieved, X 11 and Y 11There are no limitations on the type of ligand, and each independently represents a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a silyl group having a hydrocarbon group having 1 to 20 carbon atoms, a halogenated hydrocarbon group having 1 to 20 carbon atoms, an oxygen-containing hydrocarbon group having 1 to 20 carbon atoms, an amino group, or an alkylamino group having 1 to 20 carbon atoms.
[0049] Above Q 11 represents a divalent hydrocarbon group having 1 to 20 carbon atoms linking two five-membered rings, or a silylene group or germylene group which may have a hydrocarbon group having 1 to 20 carbon atoms. When two hydrocarbon groups are present on the above-mentioned silylene group or germylene group, they may be linked to each other to form a ring structure. Above Q 11 Specific examples of the alkylene group include alkylene groups such as methylene, methylmethylene, dimethylmethylene, and 1,2-ethylene; aryl alkylene groups such as diphenylmethylene; silylene groups; alkylsilylene groups such as methylsilylene, dimethylsilylene, diethylsilylene, di(n-propyl)silylene, di(i-propyl)silylene, and di(cyclohexyl)silylene; (alkyl)(aryl)silylene groups such as methyl(phenyl)silylene; arylsilylene groups such as diphenylsilylene; alkyloligosilylene groups such as tetramethyldisilylene; germylene groups; alkylgermylene groups in which the silicon of the silylene group having the above-mentioned divalent hydrocarbon group having 1 to 20 carbon atoms is replaced with germanium; (alkyl)(aryl)germylene groups; and arylgermylene groups. Among these, a silylene group having a hydrocarbon group of 1 to 20 carbon atoms or a germylene group having a hydrocarbon group of 1 to 20 carbon atoms is preferred, with an alkylsilylene group and an alkylgermylene group being particularly preferred.
[0050] Among the compounds represented by the above general formula (a1), preferred compounds are specifically exemplified below. (1) dichloro[1,1'-dimethylsilylenebis{2-(2-furyl)-4-phenyl-indenyl}]hafnium, (2) dichloro[1,1'-dimethylsilylenebis{2-(2-thienyl)-4-phenyl-indenyl}]hafnium, (3) dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-phenyl-indenyl}]hafnium, (4) dichloro[1,1'-diphenylsilylenebis{2-(5-methyl-2-furyl)-4-phenyl-indenyl}]hafnium, (5) dichloro[1,1'-dimethylgermylenebis{2-(5-methyl-2-furyl)-4-phenyl-indenyl}]hafnium, (6) dichloro[1,1'-dimethylgermylenebis{2-(5-methyl-2-thienyl)-4-phenyl-indenyl}]hafnium, (7) dichloro[1,1'-dimethylsilylenebis{2-(5-t-butyl-2-furyl)-4-phenyl-indenyl}]hafnium, (8) dichloro[1,1'-dimethylsilylenebis{2-(5-trimethylsilyl-2-furyl)-4-phenyl-indenyl}]hafnium, (9) dichloro[1,1'-dimethylsilylenebis{2-(5-phenyl-2-furyl)-4-phenyl-indenyl}]hafnium, (10) dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-(4-chlorophenyl)-indenyl}]hafnium, (11) dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-(4-isopropyl-phenyl)-indenyl}]hafnium, (12) dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-(4-t-butylphenyl)-indenyl}]hafnium, (13) dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-(4-trimethylsilylphenyl)-indenyl}]hafnium, (14) dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-(4-biphenylyl)-indenyl}]hafnium, (15) dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-(1-naphthyl)-indenyl}]hafnium, (16) dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-(2-naphthyl)-indenyl}]hafnium, (17) dichloro[1,1'-dimethylsilylenebis{2-(5-t-butyl-2-furyl)-4-(1-naphthyl)-indenyl}]hafnium, (18) dichloro[1,1'-dimethylsilylenebis{2-(5-t-butyl-2-furyl)-4-(2-naphthyl)-indenyl}]hafnium, (19) dichloro[1,1'-dimethylsilylenebis{2-(5-t-butyl-2-furyl)-4-(4-isopropyl-phenyl)-indenyl}]hafnium, (20) dichloro[1,1'-dimethylsilylenebis{2-(5-t-butyl-2-furyl)-4-(4-t-butylphenyl)-indenyl}]hafnium, (21) dichloro[1,1'-dimethylsilylenebis{2-(5-t-butyl-2-furyl)-4-(4-trimethylsilylphenyl)-indenyl}]hafnium,
[0051] Of these, more preferred are: (3) dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-phenyl-indenyl}]hafnium, (7) dichloro[1,1'-dimethylsilylenebis{2-(5-t-butyl-2-furyl)-4-phenyl-indenyl}]hafnium, (11) dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-(4-isopropyl-phenyl)-indenyl}]hafnium, (12) dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-(4-t-butylphenyl)-indenyl}]hafnium, (13) dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-(4-trimethylsilylphenyl)-indenyl}]hafnium, (19) dichloro[1,1'-dimethylsilylenebis{2-(5-t-butyl-2-furyl)-4-(4-isopropyl-phenyl)-indenyl}]hafnium, (20) dichloro[1,1'-dimethylsilylenebis{2-(5-t-butyl-2-furyl)-4-(4-t-butylphenyl)-indenyl}]hafnium, (21) dichloro[1,1'-dimethylsilylenebis{2-(5-t-butyl-2-furyl)-4-(4-trimethylsilylphenyl)-indenyl}]hafnium, It is.
[0052] Also particularly preferred are (11) dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-(4-isopropyl-phenyl)-indenyl}]hafnium, (12) dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-(4-t-butylphenyl)-indenyl}]hafnium, (13) dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-(4-trimethylsilylphenyl)-indenyl}]hafnium, (19) dichloro[1,1'-dimethylsilylenebis{2-(5-t-butyl-2-furyl)-4-(4-isopropyl-phenyl)-indenyl}]hafnium, (20) dichloro[1,1'-dimethylsilylenebis{2-(5-t-butyl-2-furyl)-4-(4-t-butylphenyl)-indenyl}]hafnium, (21) dichloro[1,1'-dimethylsilylenebis{2-(5-t-butyl-2-furyl)-4-(4-trimethylsilylphenyl)-indenyl}]hafnium, It is.
[0053] 1-2. Ingredient [A-2] As the component [A-2], a metallocene compound represented by the following general formula (a2) is preferably used from the viewpoint of efficiently copolymerizing the macromer with propylene.
[0054] [ka]
[0055] [In general formula (a2), R 21 and R 22 R is each independently a hydrocarbon group having 1 to 6 carbon atoms. 23 and R 24 Q each independently represents an aryl group having 6 to 30 carbon atoms which may contain halogen, silicon, oxygen, sulfur, nitrogen, boron, phosphorus, or a plurality of hetero elements selected therefrom. 21 represents a divalent hydrocarbon group having 1 to 20 carbon atoms, or a silylene group or germylene group which may have a hydrocarbon group having 1 to 20 carbon atoms; M 21 represents zirconium or hafnium, and X 21 and Y 21 each independently represents a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a silyl group having a hydrocarbon group having 1 to 20 carbon atoms, a halogenated hydrocarbon group having 1 to 20 carbon atoms, an amino group, or an alkylamino group having 1 to 20 carbon atoms.]
[0056] Above R 21 and R 22 are each independently a hydrocarbon group having 1 to 6 carbon atoms, preferably an alkyl group, and more preferably an alkyl group having 1 to 4 carbon atoms. Specific examples include methyl, ethyl, n-propyl, i-propyl, n-butyl, i-butyl, sec-butyl, n-pentyl, i-pentyl, n-hexyl, and the like, and are preferably methyl, ethyl, or n-propyl.
[0057] In addition, the above R 23 and R 24are each independently an aryl group having 6 to 30 carbon atoms, preferably 6 to 24 carbon atoms, which may contain halogen, silicon, oxygen, sulfur, nitrogen, boron, phosphorus, or a plurality of hetero elements selected from these. Such aryl groups are phenyl groups, biphenylyl groups, and naphthyl groups, which may have a substituent. Preferred examples include phenyl, 3-chlorophenyl, 4-chlorophenyl, 3-fluorophenyl, 4-fluorophenyl, 4-methylphenyl, 4-i-propylphenyl, 4-t-butylphenyl, 4-trimethylsilylphenyl, 4-(2-fluoro-4-biphenylyl), 4-(2-chloro-4-biphenylyl), 1-naphthyl, 2-naphthyl, 4-chloro-2-naphthyl, 3-methyl-4-trimethylsilylphenyl, 3,5-dimethyl-4-t-butylphenyl, 3,5-dimethyl-4-trimethylsilylphenyl, and 3,5-dichloro-4-trimethylsilylphenyl.
[0058] Q 21 represents either a divalent hydrocarbon group having 1 to 20 carbon atoms that links two five-membered rings or bridges two conjugated five-membered ring ligands via a carbon having 1 or 2 carbon atoms, or a silylene group or germylene group that may have a hydrocarbon group having 1 to 20 carbon atoms. When two hydrocarbon groups are present on the above-mentioned silylene group or germylene group, they may be bonded to each other to form a ring structure. The above Q 21Specific examples of the alkylene group include alkylene groups such as methylene, methylmethylene, dimethylmethylene, and 1,2-ethylene; aryl alkylene groups such as diphenylmethylene; silylene groups; alkylsilylene groups such as methylsilylene, dimethylsilylene, diethylsilylene, di(n-propyl)silylene, di(i-propyl)silylene, and di(cyclohexyl)silylene; (alkyl)(aryl)silylene groups such as methyl(phenyl)silylene; arylsilylene groups such as diphenylsilylene; alkyloligosilylene groups such as tetramethyldisilylene; germylene groups; alkylgermylene groups in which the silicon of the silylene group having the above-mentioned divalent hydrocarbon group having 1 to 20 carbon atoms is replaced with germanium; (alkyl)(aryl)germylene groups; and arylgermylene groups. Among these, a silylene group having a hydrocarbon group of 1 to 20 carbon atoms or a germylene group having a hydrocarbon group of 1 to 20 carbon atoms is preferred, with an alkylsilylene group and an alkylgermylene group being particularly preferred. Furthermore, the above M 21 is zirconium or hafnium, preferably hafnium.
[0059] Above X 21 and Y 21 is an auxiliary ligand, and reacts with component (B) as a cocatalyst to produce an active metallocene having olefin polymerization ability. Therefore, as long as this purpose is achieved, X 21 and Y 21 There are no limitations on the type of ligand, and each independently represents a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a silyl group having a hydrocarbon group having 1 to 20 carbon atoms, a halogenated hydrocarbon group having 1 to 20 carbon atoms, an oxygen-containing hydrocarbon group having 1 to 20 carbon atoms, an amino group, or an alkylamino group having 1 to 20 carbon atoms.
[0060] Non-limiting examples of the metallocene compound represented by the above general formula (a2) include the following. However, to avoid a large number of complicated examples, only representative example compounds are described. Also, although compounds having hafnium as a central metal are described, similar zirconium compounds can also be used, and it is self-evident that various ligands, bridging groups, or auxiliary ligands can be used as desired. (1) dichloro{1,1'-dimethylsilylenebis(2-methyl-4-phenyl-4-hydroazulenyl)}hafnium, (2) dichloro[1,1'-dimethylsilylenebis{2-methyl-4-(4-chlorophenyl)-4-hydroazulenyl}]hafnium, (3) dichloro[1,1'-dimethylsilylenebis{2-methyl-4-(4-t-butylphenyl)-4-hydroazulenyl}]hafnium, (4) dichloro[1,1'-dimethylsilylenebis{2-methyl-4-(4-trimethylsilylphenyl)-4-hydroazulenyl}]hafnium, (5) dichloro[1,1'-dimethylsilylenebis{2-methyl-4-(3-chloro-4-t-butylphenyl)-4-hydroazulenyl}]hafnium, (6) dichloro[1,1'-dimethylsilylenebis{2-methyl-4-(3-methyl-4-t-butylphenyl)-4-hydroazulenyl}]hafnium, (7) dichloro[1,1'-dimethylsilylenebis{2-methyl-4-(3-chloro-4-trimethylsilylphenyl)-4-hydroazulenyl}]hafnium, (8) dichloro[1,1'-dimethylsilylenebis{2-methyl-4-(3-methyl-4-trimethylsilylphenyl)-4-hydroazulenyl}]hafnium, (9) dichloro[1,1'-dimethylsilylenebis{2-methyl-4-(1-naphthyl)-4-hydroazulenyl}]hafnium, (10) dichloro[1,1'-dimethylsilylenebis{2-methyl-4-(2-naphthyl)-4-hydroazulenyl}]hafnium, (11) dichloro[1,1'-dimethylsilylenebis{2-methyl-4-(4-chloro-2-naphthyl)-4-hydroazulenyl}]hafnium, (12) dichloro[1,1'-dimethylsilylenebis{2-methyl-4-(2-fluoro-4-biphenylyl)-4-hydroazulenyl}]hafnium, (13) dichloro[1,1'-dimethylsilylenebis{2-methyl-4-(2-chloro-4-biphenylyl)-4-hydroazulenyl}]hafnium, (14) dichloro[1,1'-dimethylsilylenebis{2-methyl-4-(9-phenanthryl)-4-hydroazulenyl}]hafnium, (15) dichloro[1,1'-dimethylsilylenebis{2-ethyl-4-(4-chlorophenyl)-4-hydroazulenyl}]hafnium, (16) dichloro[1,1'-dimethylsilylenebis{2-n-propyl-4-(3-chloro-4-trimethylsilylphenyl)-4-hydroazulenyl}]hafnium, (17) dichloro[1,1'-dimethylsilylenebis{2-ethyl-4-(3-chloro-4-t-butylphenyl)-4-hydroazulenyl}]hafnium, (18) dichloro[1,1'-dimethylsilylenebis{2-ethyl-4-(3-methyl-4-trimethylsilylphenyl)-4-hydroazulenyl}]hafnium, (19) dichloro[1,1'-dimethylgermylenebis{2-methyl-4-(2-fluoro-4-biphenylyl)-4-hydroazulenyl}]hafnium, (20) dichloro[1,1'-dimethylgermylenebis{2-methyl-4-(4-t-butylphenyl)-4-hydroazulenyl}]hafnium, (21) dichloro[1,1'-(9-silafluorene-9,9-diyl)bis{2-ethyl-4-(4-chlorophenyl)-4-hydroazulenyl}]hafnium, (22) dichloro[1,1'-dimethylsilylenebis{2-ethyl-4-(4-chloro-2-naphthyl)-4-hydroazulenyl}]hafnium, (23) dichloro[1,1'-dimethylsilylenebis{2-ethyl-4-(2-fluoro-4-biphenylyl)-4-hydroazulenyl}]hafnium, (24) Dichloro[1,1'-(9-silafluorene-9,9-diyl)bis{2-ethyl-4-(3,5-dichloro-4-trimethylsilylphenyl)-4-hydroazulenyl}]hafnium, and the like.
[0061] Among these, preferred are (2) dichloro[1,1'-dimethylsilylenebis{2-methyl-4-(4-chlorophenyl)-4-hydroazulenyl}]hafnium, (7) dichloro[1,1'-dimethylsilylenebis{2-methyl-4-(3-chloro-4-trimethylsilylphenyl)-4-hydroazulenyl}]hafnium, (18) dichloro[1,1'-dimethylsilylenebis{2-ethyl-4-(3-methyl-4-trimethylsilylphenyl)-4-hydroazulenyl}]hafnium, (22) dichloro[1,1'-dimethylsilylenebis{2-ethyl-4-(4-chloro-2-naphthyl)-4-hydroazulenyl}]hafnium, (23) dichloro[1,1'-dimethylsilylenebis{2-ethyl-4-(2-fluoro-4-biphenylyl)-4-hydroazulenyl}]hafnium, (24) dichloro[1,1'-(9-silafluorene-9,9-diyl)bis{2-ethyl-4-(3,5-dichloro-4-trimethylsilylphenyl)-4-hydroazulenyl}]hafnium, It is.
[0062] Also particularly preferably, (2) dichloro[1,1'-dimethylsilylenebis{2-methyl-4-(4-chlorophenyl)-4-hydroazulenyl}]hafnium, (18) dichloro[1,1'-dimethylsilylenebis{2-ethyl-4-(3-methyl-4-trimethylsilylphenyl)-4-hydroazulenyl}]hafnium, (22) dichloro[1,1'-dimethylsilylenebis{2-ethyl-4-(2-fluoro-4-biphenylyl)-4-hydroazulenyl}]hafnium, (24) dichloro[1,1'-(9-silafluorene-9,9-diyl)bis{2-ethyl-4-(3,5-dichloro-4-trimethylsilylphenyl)-4-hydroazulenyl}]hafnium, It is.
[0063] 2. Catalyst component (B) The catalyst component (B) used in the present invention is a compound or an ion-exchangeable layered silicate which reacts with the catalyst component (A) to form an ion pair. The catalyst component (B) may be used alone or in combination of two or more thereof, and is preferably an ion-exchangeable layered silicate.
[0064] 2-1. Compound that forms an ion pair with catalyst component (A) Examples of the compound that reacts with the catalyst component (A) to form an ion pair include aluminum oxy compounds and boron compounds. Specific examples of the aluminum oxy compounds include compounds represented by the following general formulas (I) to (III).
[0065] [ka]
[0066] In the above general formulas (I), (II) and (III), R 91 , R 101 and R 111 represents a hydrogen atom or a hydrocarbon group, preferably a hydrocarbon group having 1 to 10 carbon atoms, and particularly preferably a hydrocarbon group having 1 to 6 carbon atoms. 91 , R 101 and R 111 may be the same or different, and p represents an integer of 0 to 40, preferably 2 to 30. The compounds represented by the general formulas (I) and (II) are also called aluminoxanes, and among them, methylaluminoxane or methylisobutylaluminoxane is preferred. The above aluminoxanes can be used in combination of multiple types within each group or between each group. The above aluminoxanes can be prepared under various known conditions. In general formula (III), R 112 represents a hydrocarbon group having 1 to 10 carbon atoms, preferably 1 to 6 carbon atoms. The compound represented by the general formula (III) is a compound represented by the general formula R 112 It can be obtained by reacting with an alkylboronic acid represented by B(OH)2 in a molar ratio of 10:1 to 1:1. Examples of the boron compound include complexes of cations such as carbonium cation and ammonium cation with organic boron compounds such as triphenyl boron, tris(3,5-difluorophenyl) boron and tris(pentafluorophenyl) boron, and various organic boron compounds such as tris(pentafluorophenyl) boron.
[0067] 2-2. Ion-exchangeable layered silicate In the present invention, the ion-exchangeable layered silicate (hereinafter, sometimes simply referred to as silicate) used as a raw material refers to a silicate compound having a crystal structure in which layers formed by ionic bonds or the like are stacked in parallel with each other through bonding forces, having interlayer ions between the layers, and in which the contained interlayer ions are exchangeable. Most silicates are naturally produced as the main component of clay minerals. They are generally purified by dispersing / swelling them in water and measuring the difference in sedimentation rate, but it is not necessary to completely remove impurities, and they may contain impurities other than ion-exchangeable layered silicates (quartz, cristobalite, etc.). Depending on the type, amount, particle size, crystallinity, and dispersion state of these impurities, they may be more preferable than pure silicates, and such complexes are also included in the ion-exchangeable layered silicates of catalyst component (B). Moreover, the silicate used in the present invention is not limited to naturally occurring silicates, but may be synthetically produced silicates.
[0068] Specific examples of ion-exchangeable layered silicates include layered silicates having a 1:1 structure or a 2:1 structure, as described in, for example, "Clay Mineralogy" by Shiramizu Haruo, Asakura Publishing (1988). The 1:1 type structure refers to a structure based on stacking of one layer of tetrahedral sheet and one layer of octahedral sheet, as described in the above-mentioned "Clay Mineralogy" and the like. The 2:1 type structure refers to a structure based on stacking two layers of tetrahedral sheets sandwiching one layer of octahedral sheet. Specific examples of ion-exchangeable layered silicates having a 1:1 type structure include kaolin group silicates such as dickite, nacrite, kaolinite, metahalloysite, and halloysite, and serpentine group silicates such as chrysotile, lisardite, and antigorite. Specific examples of ion-exchangeable layered silicates having a 2:1 type structure include smectite group silicates such as montmorillonite, beidellite, nontronite, saponite, hectorite, stevensite, etc., vermiculite group silicates such as vermiculite, mica group silicates such as mica, illite, sericite, glauconite, etc., attapulgite, sepiolite, palygorskite, bentonite, pyrophyllite, talc, chlorite group, etc. These may form mixed layers. Among these, it is preferable that the main component is an ion-exchangeable layered silicate having a 2:1 type structure, more preferably that the main component is a smectite group silicate, and even more preferably that the main component is montmorillonite. The type of interlayer cation (the positive ion contained between the layers of the ion-exchangeable layered silicate) is not particularly limited, but preferred main components are alkali metals of Group 1 of the periodic table, such as lithium and sodium, alkaline earth metals of Group 2 of the periodic table, such as calcium and magnesium, and transition metals, such as iron, cobalt, copper, nickel, zinc, ruthenium, rhodium, palladium, silver, iridium, platinum, and gold, which are relatively easily available.
[0069] The ion-exchangeable layered silicate may be used in a dry state or in a slurried state in a liquid. The shape of the ion-exchangeable layered silicate is not particularly limited, and may be a naturally occurring shape or a shape at the time of artificial synthesis, or may be an ion-exchangeable layered silicate whose shape has been processed by operations such as pulverization, granulation, and classification. Among these, the use of granulated ion-exchange layered silicate is particularly preferred because it gives good polymer particle properties when the ion-exchange layered silicate is used as a catalyst component. The ion-exchanged layered silicate can be used as it is without any particular treatment, but is preferably subjected to a chemical treatment. For the chemical treatment method of the ion-exchanged layered silicate, see paragraphs 0042 to 0071 of JP2009-299046A.
[0070] The catalyst component (B) preferably used in the present invention is a chemically treated ion-exchangeable layered silicate, and has an Al / Si atomic ratio of 0.01 to 0.25, preferably 0.03 to 0.24, and more preferably 0.05 to 0.23. The Al / Si atomic ratio is considered to be an index of the acid treatment strength of the clay portion. The aluminum and silicon in the ion-exchange layered silicate are measured by creating a calibration curve according to the JIS method of chemical analysis and quantifying the amounts by fluorescent X-rays.
[0071] 3.Component (C) The catalyst component (C) used in the present invention is an organoaluminum compound, and preferably an organoaluminum compound represented by the following general formula (IV) is used. (AlR n X 3-n ) m ...General formula (IV) [In the above general formula (IV), R represents an alkyl group having 1 to 20 carbon atoms, X represents a halogen, a hydrogen, an alkoxy group or an amino group, n represents an integer of 1 to 3, and m represents an integer of 1 to 2.] When X is a halogen, it is preferably chlorine; when X is an alkoxy group, it is preferably an alkoxy group having 1 to 8 carbon atoms; and when X is an amino group, it is preferably an amino group having 1 to 8 carbon atoms. The organoaluminum compounds may be used alone or in combination of two or more kinds. Specific examples of the organic aluminum compound include trimethylaluminum, triethylaluminum, tri-normal propylaluminum, tri-normal butylaluminum, triisobutylaluminum, tri-normal hexylaluminum, tri-normal octylaluminum, tri-normal decylaluminum, diethylaluminum chloride, diethylaluminum sesquichloride, diethylaluminum hydride, diethylaluminum ethoxide, diethylaluminum dimethylamide, diisobutylaluminum hydride, diisobutylaluminum chloride, etc. Among these, preferred are trialkylaluminum and alkylaluminum hydrides with m=1 and n=3. More preferred are trialkylaluminums with R having 1 to 8 carbon atoms.
[0072] 4. Catalyst Preparation The olefin polymerization catalyst used in the present invention contains the above-mentioned catalyst components. These can be obtained by contacting them in or outside a polymerization vessel. The olefin polymerization catalyst may be prepolymerized in the presence of an olefin. The contact of the catalyst components is usually carried out in an aliphatic or aromatic hydrocarbon solvent. The contact temperature is not particularly limited, but is preferably between -20°C and 150°C. The contact order may be any combination suitable for the purpose, but the particularly preferred orders for each catalyst component are as follows: When using catalyst component (C), it is possible to contact catalyst component (C) with catalyst component (A), or with catalyst component (B), or with both catalyst component (A) and catalyst component (B) before contacting catalyst component (A) with catalyst component (B), or to contact catalyst component (C) with catalyst component (A) and catalyst component (B) at the same time as contacting catalyst component (A) with catalyst component (B), or to contact catalyst component (C) after contacting catalyst component (A) with catalyst component (B). However, it is preferable to contact catalyst component (C) with either catalyst component before contacting catalyst component (A) with catalyst component (B). After contacting the catalyst components, they can be washed with an aliphatic hydrocarbon or aromatic hydrocarbon solvent.
[0073] The amounts of the catalyst components (A), (B) and (C) used in the present invention are arbitrary. For example, the amount of the catalyst component (A) used relative to the catalyst component (B) is preferably in the range of 0.1 μmol to 1000 μmol, more preferably 0.5 μmol to 500 μmol, per 1 g of the catalyst component (B). The amount of catalyst component (C) used relative to catalyst component (A) is preferably 0.01 to 5×10 in terms of the molar ratio of aluminum of catalyst component (C) to the transition metal of catalyst component (A). 6 , more preferably 0.1 to 1×10 4 The range is.
[0074] The branched propylene polymer of the present invention can be produced by using a catalyst component capable of producing a macromer and a catalyst component capable of copolymerizing the macromer with propylene. Although it is possible to produce the polymer by using a single catalyst component having both the ability to produce the macromer and the ability to copolymerize the macromer with propylene, a method using separate catalyst components having each ability can be selected to efficiently produce the branched propylene polymer of the present invention. That is, the method using a component [A-1] capable of producing a macromer and a component [A-2] capable of copolymerizing the macromer with propylene makes it easy to produce a branched propylene polymer satisfying the requirements of the present invention. The ratio of the component [A-1] and the component [A-2] to be used may be any ratio within a range that satisfies the properties of the branched propylene polymer of the present invention, but the molar ratio of the transition metal in [A-1] to the total amount of the components [A-1] and [A-2] is preferably 0.30 or more and 0.99 or less. By changing this ratio, it is possible to adjust the balance between melt properties and catalytic activity. In other words, component [A-1] produces low molecular weight vinyl-terminated macromers, and component [A-2] produces high molecular weight polymers in which some macromers are copolymerized. Therefore, by changing the ratio of component [A-1], it is possible to control the average molecular weight, molecular weight distribution, the bias of the molecular weight distribution toward the low molecular weight side, the very high molecular weight components, and the branching (amount, length, distribution) of the produced polymer, and thereby to control melt properties such as strain hardening and melt tension. The molar ratio of the transition metal in component [A-1] to the total amount of components [A-1] and [A-2] is preferably 0.30 or more, more preferably 0.40 or more, and even more preferably 0.50 or more. The upper limit is preferably 0.99 or less, more preferably 0.90 or less, and in order to efficiently obtain the polymer of the present invention with high catalytic activity, it is preferably 0.80 or less, and even more preferably 0.70 or less. Furthermore, by using the component [A-1] within the above range, it is possible to adjust the balance between the average molecular weight and the catalytic activity.
[0075] 5. Prepolymerization The olefin polymerization catalyst is preferably subjected to a preliminary polymerization in which an olefin is brought into contact with the catalyst and polymerized in a small amount. By carrying out the preliminary polymerization treatment, it is possible to prevent the formation of gel when the main polymerization is carried out. This is believed to be because the long chain branches can be uniformly distributed among the polymer particles when the main polymerization is carried out. The olefin used in the prepolymerization is not particularly limited, but examples thereof include ethylene, propylene, 1-butene, 1-hexene, 1-octene, 4-methyl-1-pentene, 3-methyl-1-butene, vinylcycloalkane, and styrene, and is preferably propylene. The olefin may be fed to the prepolymerization reactor at a constant rate or at a constant pressure, or any combination thereof, or in a stepwise manner. The prepolymerization temperature and prepolymerization time are not particularly limited, but are preferably in the range of −20° C. to 100° C. and 5 minutes to 24 hours, respectively. The amount of prepolymerization is preferably 0.01-100, more preferably 0.1-50, in terms of the mass ratio of the prepolymerized polymer to the catalyst component (B). In addition, the catalyst component (C) can be added during the prepolymerization, and washing can also be carried out at the end of the prepolymerization. It is also possible to use a method in which a polymer such as polyethylene or polypropylene or a solid inorganic oxide such as silica or titania is made to coexist during or after the contact of the above catalyst components. After the preliminary polymerization, the catalyst may be dried. The drying method is not particularly limited, and examples thereof include drying under reduced pressure, drying by heating, and drying by passing a dry gas through the catalyst. These methods may be used alone or in combination of two or more methods. In the drying step, the catalyst may be stirred, vibrated, or fluidized.
[0076] 6. Propylene Polymerization The polymerization mode may be any mode that allows efficient contact between the olefin polymerization catalyst and the monomer. Specifically, a slurry polymerization method using an inert solvent, a bulk polymerization method using propylene as a solvent without substantially using an inert solvent, a solution polymerization method, or a gas phase polymerization method in which each monomer is kept in a gaseous state without substantially using a liquid solvent can be used. Furthermore, a method of carrying out continuous polymerization or batch polymerization can also be applied. Although multi-stage polymerization having two or more stages can also be carried out, it is preferable to carry out single-stage polymerization. Among these, it is preferable to carry out the bulk polymerization method, in which case the polymerization temperature can be from 50° C. to the temperature at which propylene becomes critical.
[0077] Furthermore, in order to produce the branched propylene polymer of the present invention, the polymerization temperature is preferably 65° C. or higher. In the polymerization reaction mediated by the above-mentioned component [A-1], a vinyl group is formed at the end by the β-methyl elimination reaction as a termination reaction, and a macromer that can be copolymerized with propylene is produced. The rate of the β-methyl elimination reaction is affected by the polymerization temperature, and generally, the higher the polymerization temperature, the higher the β-methyl elimination rate becomes, and as a result, the ratio with the propagation reaction rate becomes larger, and the molecular weight of the macromer decreases. Therefore, in the method for producing the branched propylene polymer of the present invention, the polymerization temperature is preferably 65° C. or higher. By setting the polymerization temperature at 65° C. or higher, the average molecular weight of the macromer falls within the range that is preferred in the present invention, making it possible to introduce branches having short branch chain lengths into the branched propylene polymer. For the above reasons, the polymerization temperature is preferably 65° C. or higher, more preferably 70° C. or higher, and even more preferably 75° C. or higher. On the other hand, the upper limit must be equal to or lower than the critical temperature of propylene in order to carry out bulk polymerization, and is preferably 85° C. or lower, and even more preferably 83° C. or lower. In particular, when a compound represented by general formula (a1) is selected as component [A-1], if the substituent at the 2-position of the indenyl group is, for example, a methylfuryl group, the polymer of the present invention can be obtained by polymerization at preferably 80°C or higher. However, if the substituent at the 2-position of the indenyl group is a bulkier substituent such as a t-butylfuryl group, the polymer of the present invention can be obtained at a lower polymerization temperature, such as 70°C. In this case, the pressure is more preferably 1.5 MPa or more, further preferably 2.5 MPa or more, and preferably 3.5 MPa or more. The upper limit is preferably 4.4 MPa or less, and further preferably 4.0 MPa or less. The polymerization may be a homopolymerization of propylene, or a copolymerization using, in addition to the propylene monomer, one or more α-olefin comonomers having 2 to 20 carbon atoms other than propylene, such as ethylene, 1-butene, 1-hexene, 1-octene, 4-methyl-1-pentene, etc., as comonomers. The amount of the comonomer is preferably 10 mol % or less, more preferably 5 mol % or less, as a copolymerization ratio in the branched propylene polymer, and is preferably 15 mol % or less, more preferably 7.5 mol % or less, as a charge amount during polymerization.
[0078] Furthermore, in order to produce the branched propylene polymer of the present invention, hydrogen is used as a molecular weight modifier. The range of hydrogen in terms of molar ratio to propylene is 1.0×10 -5 More than 1.0×10 is preferable. -4 More preferably, 0.5×10 -3 The above is even more preferable. In addition, the upper limit is 1.0×10 -2 Less than 0.5×10 is preferable. -2 Less than 0.2×10 is more preferable. -2 The following is even more preferred: The polymer produced by the above-mentioned component [A-1] has a very slow chain transfer by hydrogen, whereas the polymer produced by the component [A-2] has a relatively fast chain transfer by hydrogen, so that when there is a small amount of hydrogen, a high molecular weight polymer can be produced. Therefore, when the amount of hydrogen used is small, the polymer produced by the component [A-2] (i.e., a copolymer of polypropylene and vinyl-terminated macromer, a polymer equivalent to a branched propylene-based polymer) is on the higher molecular weight side than the polymer produced by the component [A-1] (i.e., a vinyl-terminated macromer, a polymer forming a branched chain). Therefore, when propylene is polymerized using a combination of the components [A-1] and [A-2] under conditions in which a small amount of hydrogen is used, the molecular weight distribution of the branched propylene polymer can be expanded toward the high molecular weight side, and the branch chain length can be shortened.
[0079] In addition, component [A-1] produces vinyl-terminated macromers, which in turn mediate copolymerization of propylene with the macromer to produce branched macromers with vinyl terminal groups. On the other hand, component [A-2] does not produce macromers by itself, but only when the macromer produced by component [A-1] approaches component [A-2] does it mediate copolymerization of propylene with the macromer to produce a branched polymer.
[0080] As described above, when a branched propylene polymer is produced by a macromer copolymerization method by combining components [A-1] and [A-2], (1) a branch having a short branch chain length can be introduced by setting the polymerization temperature at 65°C or higher, and further, (2) the amount of hydrogen used as a molecular weight regulator can be reduced to broaden the molecular weight distribution of the branched propylene polymer to the high molecular weight side, and further, (3) due to the difference in contact efficiency between components [A-1] and [A-2] and the terminal vinyl macromer, macromers having many branched structures generated by component [A-1], which has a high contact efficiency with the macromer, are introduced into the high molecular weight branched polymer generated by component [A-2], and therefore, due to the combined effects of the above (1), (2) and (3), a large number of branches having a short branch chain length can be introduced into the high molecular weight region of the molecular weight distribution of the branched propylene polymer. Specifically, the branching index g' at the component with a molecular weight M of 1 million or more in the molecular weight distribution and the absolute molecular weight Mabs of 1 million can be set to the preferred range as described above. Therefore, the obtained branched propylene polymer can have a relaxation time distribution in which many components have a relatively short relaxation time and few components have an extremely long relaxation time.
[0081] III. Uses of branched propylene polymers The branched propylene polymer of the present invention can be used as a molding material after being heated, melted and kneaded using a melt kneader and then cut into pellets. The branched propylene polymer of the present invention can be blended with various additives such as known antioxidants, ultraviolet absorbers, antistatic agents, nucleating agents, lubricants, flame retardants, antiblocking agents, colorants, inorganic or organic fillers, and further with various synthetic resins and natural resins, as necessary. These pellet-like molding materials can be molded by various known polypropylene molding methods, such as injection molding, extrusion molding, foam molding, and blow molding, to produce various molded products such as industrial injection molded parts, containers, non-oriented films, uniaxially oriented films, biaxially oriented films, sheets, pipes, and fibers. In addition, the branched propylene polymer of the present invention has an excellent balance between melt fluidity and melt tension, and therefore can be suitably used in fields requiring uniform wall thickness in sheet molding, blow molding, etc., uniform foam cell diameter in foam molding, etc., and fine fiber diameter in melt spinning, etc. The branched propylene polymer of the present invention can also be used by blending with other resins. EXAMPLES
[0082] Next, the present invention will be described more specifically with reference to examples. However, the present invention is not limited to the following examples as long as it does not depart from the gist of the present invention. (1) Synthesis of component (A) (1-1) Synthesis example of component [A-1] (Complex 1) Synthesis of rac-dichloro[1,1'-dimethylsilylenebis{2-(5-t-butyl-2-furyl)-4-(4-isopropylphenyl)indenyl}]hafnium: rac-Dichloro[1,1'-dimethylsilylenebis{2-(5-t-butyl-2-furyl)-4-(4-isopropylphenyl)indenyl}]hafnium was synthesized according to the methods described in Example 13 of JP-A-2009-299046 and Example 1 of JP-A-2009-91512. (Complex 2) Synthesis of rac-dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-(4-isopropylphenyl)indenyl}]hafnium: rac-Dichloro[1,1′-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-(4-isopropylphenyl)indenyl}]hafnium was synthesized according to the method of Synthesis Example 1 in JP2012-149160A. (1-2) Synthesis example of component [A-2] (Complex 3) Synthesis of rac-dichloro[1,1'-dimethylsilylenebis{2-methyl-4-(4-chlorophenyl)-4-hydroazulenyl}]hafnium: rac-Dichloro[1,1'-dimethylsilylenebis{2-methyl-4-(4-chlorophenyl)-4-hydroazulenyl}]hafnium was synthesized according to the method of Example 7 of JP-A-11-240909.
[0083] (2) Synthesis example of component (B): Chemical treatment of ion-exchangeable layered silicate Into a 1 L three-neck flask equipped with a stirring blade and a reflux device, 645.1 g of distilled water and 82.6 g of 98% sulfuric acid were added and heated to 95°C. 100 g of commercially available montmorillonite (Benclay KK manufactured by Mizusawa Chemical Industry Co., Ltd., Al=9.78% by mass, Si=31.79% by mass, Mg=3.18% by mass, Al / Si (molar ratio)=0.320, average particle size 14 μm) was added thereto, and the mixture was reacted for 320 minutes at 95° C. After 320 minutes, 0.5 L of distilled water was added to stop the reaction, and 255 g of a cake-like solid was obtained by filtration. This cake (1 g) contained 0.31 g of the chemically treated montmorillonite (intermediate). The chemical composition of the chemically treated montmorillonite (intermediate) was Al = 7.68 mass%, Si = 36.05 mass%, Mg = 2.13 mass%, and the Al / Si (molar ratio) = 0.222. 1545g of distilled water was added to the cake to make a slurry, and the temperature was raised to 40℃. 5.734g of lithium hydroxide hydrate was added as a solid, and the reaction was carried out at 40℃ for 1 hour. After 1 hour, the reaction slurry was filtered and washed with 1L of distilled water three times, and a cake-like solid was obtained again. The collected cake was dried to obtain 80 g of chemically treated montmorillonite, which had a chemical composition of Al=7.68% by mass, Si=36.05% by mass, Mg=2.13% by mass, Al / Si (molar ratio)=0.222, and Li=0.53% by mass.
[0084] (3) Preparation of catalyst (3-1) Synthesis example of catalyst 1 10 g of the chemically treated montmorillonite obtained above was placed in a three-neck flask (volume 1 L), and heptane (66 mL) was added to make a slurry. Triisobutylaluminum (25 mmol: 34.0 mL of a heptane solution with a concentration of 143 mg / mL) was added to this and stirred for 1 hour, and then the mixture was washed with heptane until the residual liquid ratio became 1 / 100, and the total volume was made up to 50 mL. In another flask (volume 200 mL), rac-dichloro[1,1'-dimethylsilylenebis{2-(5-t-butyl-2-furyl)-4-(4-isopropylphenyl)indenyl}]hafnium (complex 1) (105 μmol) prepared in Synthesis Example 1 of the catalyst component [A-1] was dissolved in toluene (21 mL) to prepare solution 1. Furthermore, in another flask (volume 200 mL), rac-dichloro[1,1'-dimethylsilylenebis{2-methyl-4-(4-chlorophenyl)-4-hydroazulenyl}]hafnium (complex 3) (45 μmol) prepared in Synthesis Example of the catalyst component [A-2] was dissolved in toluene (9 mL) to prepare solution 2.
[0085] Triisobutylaluminum (0.42 mmol: 0.6 mL of a heptane solution with a concentration of 143 mg / mL) was added to a 1 L flask containing the above-mentioned chemically treated montmorillonite, and then the above-mentioned solution 1 (21 mL) was added and stirred at room temperature for 20 minutes. Thereafter, triisobutylaluminum (0.18 mmol: 0.25 mL of a heptane solution with a concentration of 143 mg / mL) was further added, and then the above solution 2 was added, followed by stirring at room temperature for 1 hour. Then, 170 mL of heptane was added, and the slurry was introduced into a 1 L autoclave. After the internal temperature of the autoclave was brought to 40°C, propylene was fed at a rate of 5g / hour, and prepolymerization was carried out while maintaining 40°C for 4 hours. Thereafter, the propylene feed was stopped, and residual polymerization was carried out for 1 hour. After removing the supernatant of the obtained catalyst slurry by decantation, triisobutylaluminum (6mmol: 8.5mL of heptane solution with a concentration of 143mg / mL) was added to the remaining portion and stirred for 5 minutes. The solid was dried under reduced pressure for 1 hour to obtain 29.9 g of a dry prepolymerized catalyst. The prepolymerization ratio (the value obtained by dividing the amount of the prepolymerized polymer by the amount of the solid catalyst) was 1.99. This prepolymerized catalyst was designated as Catalyst 1.
[0086] (3-2) Synthesis example of catalyst 2 Internal volume 1m 3 150 kg of the chemically treated montmorillonite obtained above was placed in a reactor, 2832 L of hexane was added to make a slurry, 74.4 kg (375 mol) of triisobutylaluminum was added over 85 minutes, and the mixture was stirred for 60 minutes. After that, the mixture was washed with hexane until the residual liquid ratio was 1 / 32, and the total volume was made 900 L. The slurry solution containing this chemically treated montmorillonite was kept at 50° C., and 0.65 kg of triisobutylaluminum (4.257 kg, 3.28 mol of a hexane solution with a concentration of 15.3% by mass) was added thereto. After stirring for 5 minutes, 0.657 kg (0.81 mol) of rac-dichloro[1,1'-dimethylsilylenebis{2-methyl-4-(4-chlorophenyl)-4-hydroazulenyl}]hafnium (complex 3) and 96 L of toluene were added, and stirring was continued for 60 minutes. Thereafter, 9.758 kg (26.61 mol) of tri-normal octylaluminum was added and stirred for 6 minutes, and then, in a separate vessel equipped with a stirrer, 240 L of toluene was added to 0.064 kg of triisobutylaluminum (9.88 kg, 0.32 mol of a toluene solution with a concentration of 0.648 mass%), to which was added 1.768 kg (1.89 mol) of rac-dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-(4-isopropylphenyl)indenyl}]hafnium (complex 2) to prepare a solution, and 100 L of toluene was added, followed by further stirring for 20 minutes. Thereafter, 2387 L of hexane was added, the internal temperature of the reactor was raised to 40°C, and then 328.1 kg of propylene was fed over 240 minutes to carry out prepolymerization while maintaining the temperature at 40°C. Thereafter, the propylene feed was stopped, and the residual polymerization was carried out at 40° C. for 80 minutes. After the completion of the residual polymerization, the stirring was stopped, and the contents were allowed to settle and settle. The supernatant was removed so that the solution volume was 1500 L, 12.7 kg of triisobutylaluminum was added, 3974 L of hexane was added again, and the mixture was stirred, then allowed to settle and settle, and the supernatant was removed so that the solution volume was 1500 L. To this solution, 8.9 kg of triisobutylaluminum (42.9 kg of a hexane solution with a concentration of 20.8% by mass) and 205 L of hexane were added. Thereafter, the reaction solution was transferred to a dryer and dried at 40° C. for 9 hours. As a result, 465 kg of a dry prepolymerized catalyst was obtained. The prepolymerization ratio (amount of prepolymerized polymer divided by amount of solid catalyst) was 2.10. This prepolymerized catalyst was designated as catalyst 2.
[0087] (4) Examples [Example 1] (polymerization) A 3 L autoclave was thoroughly dried in advance by passing nitrogen through it under heating, and then the inside of the autoclave was replaced with propylene and cooled to room temperature. 2.86 mL of a heptane solution of triisobutylaluminum (143 mg / mL) was added, and then 60 NmL of hydrogen was introduced. Next, 750 g of liquid propylene was introduced, and the temperature was then raised to 70°C. Then, 120 mg of the catalyst 1 (excluding the prepolymerized polymer) was pumped into the polymerization tank with high-pressure argon to initiate polymerization. After maintaining at 70° C. for 1 hour, 5 ml of ethanol was pumped in to terminate the polymerization. As a result, 216 g of polymer was obtained. (granulation) 100 parts by mass of the obtained branched propylene polymer were blended with 0.125 parts by mass of a phenol-based antioxidant IRGANOX1010 (trade name, manufactured by BASF Japan, tetrakis[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]methane) and 0.125 parts by mass of a phosphite-based antioxidant IRGAFOS168 (trade name, manufactured by BASF Japan, tris(2,4-di-t-butylphenyl)phosphite) and mixed for 3 minutes at room temperature using a high-speed stirring mixer Henschel Mixer (trade name, manufactured by Nippon Coke & Engineering Co., Ltd.). Then, the mixture was melt-kneaded using a twin-screw extruder KZW-15 (manufactured by Technobel Co., Ltd.) at a screw rotation speed of 400 rpm and a kneading temperature of 80, 120, and 230 ° C. from the bottom of the hopper (the same temperature from then until the die outlet). The molten resin extruded from the strand die was taken up while being cooled and fixed in a cooling water tank, and the strands were cut and pelletized using a strand cutter. The MFR of the obtained pellets (MFR pellet )=1.4 g / 10 min. Other results are shown in Table 1.
[0088] [Example 2] The same polymerization as in Example 1 was carried out, except that 130 mg of catalyst 1 (excluding the prepolymerized polymer) and 70 Nml of hydrogen were introduced, and 255 g of polymer was obtained. Granulation was carried out in the same manner as in Example 1. The MFR of the resulting pellets (MFR pellet )=1.8g / 10min. Other results are shown in Table 1.
[0089] [Example 3] The same polymerization as in Example 1 was carried out, except that 90 mg of catalyst 1 (excluding the prepolymerized polymer) and 80 Nml of hydrogen were introduced, and 230 g of polymer was obtained. Granulation was carried out in the same manner as in Example 1. The MFR of the resulting pellets (MFR pellet )=3.2 g / 10 min. Other results are shown in Table 1.
[0090] [Example 4] The same polymerization as in Example 1 was carried out, except that 80 mg of catalyst 1 (excluding the prepolymerized polymer) and 90 Nml of hydrogen were introduced, and 250 g of polymer was obtained. Granulation was carried out in the same manner as in Example 1. The MFR of the resulting pellets (MFR pellet )=4.1 g / 10 min. Other results are shown in Table 1.
[0091] [Reference Example 1]: Example of side chain homopolymerization method (Catalyst Preparation) 20 g of the chemically treated montmorillonite obtained above was placed in a 1 L three-neck flask, and 131 mL of heptane was added to form a slurry. 50 mmol of triisobutylaluminum (69 mL of a heptane solution with a concentration of 143.4 mg / mL) was added thereto, and the mixture was stirred for 60 minutes. Then, the mixture was washed with heptane up to 1 / 100, and the total volume was adjusted to 100 mL. The slurry solution containing this chemically treated montmorillonite was kept at 50° C., and 4.2 mmol of tri-normal octylaluminum (10.7 mL of a heptane solution with a concentration of 143.4 mg / mL) was added thereto, followed by stirring for 20 minutes. To this was added 0.3 mmol of rac-dichloro[1,1'-dimethylsilylenebis{2-(5-t-butyl-2-furyl)-4-(4-isopropylphenyl)indenyl}]hafnium (complex 1) (prepared as a slurry with 50 mL of toluene), and the mixture was stirred for 20 minutes while maintaining the temperature at 50°C. Then, 350 mL of heptane was added and the slurry was introduced into a 1 L autoclave. After the internal temperature of the autoclave was raised to 40° C., propylene was fed at a rate of 10 g / hour, and prepolymerization was carried out for 4 hours while maintaining the temperature at 40° C. Thereafter, the propylene feed was stopped, and residual polymerization was carried out for 1 hour while maintaining the temperature at 40° C. The supernatant of the obtained catalyst slurry was removed by decantation, and then heptane was added again and decanted to wash the prepolymerized catalyst. 12 mmol of triisobutylaluminum (16.6 mL of a heptane solution with a concentration of 143.4 mg / mL) was added to the portion remaining after the decantation and stirred for 10 minutes. This solid was dried under reduced pressure at 40°C for 2 hours to obtain 57.6 g of a dried prepolymerized catalyst. The prepolymerization ratio (the value obtained by dividing the amount of prepolymerized polymer by the amount of solid catalyst) was 1.88. This prepolymerized catalyst was designated as catalyst 3. (4) Polymerization A 3L autoclave was thoroughly dried in advance by passing nitrogen through it under heating, and then the inside of the vessel was replaced with propylene and cooled to room temperature. 2.86 mL of a heptane solution of triisobutylaluminum (140 mg / mL) was added, and then 60 Nml of hydrogen was introduced. Next, 750 g of liquid propylene was introduced, and the temperature was raised to 70°C. Then, 150 mg of the above catalyst 3, excluding the prepolymerized polymer, was pumped into the polymerization vessel and polymerized at 70°C for 1 hour. Finally, the unreacted propylene was quickly purged to stop the polymerization. As a result, about 195 g of propylene homopolymer was obtained. MFR=620 g / 10 min. Mn was calculated by GPC and found to be 33,000. This can be estimated as 1,571 skeletal carbons. The results are shown in Table 2.
[0092] [Reference Example 2]: Example of side chain homopolymerization method The same polymerization as in Reference Example 1 was carried out, except that 120 mg of catalyst 3 (excluding the prepolymerized polymer) and 90 Nml of hydrogen were introduced. As a result, 210 g of polymer was obtained. MFR=680 / 10 min. Mn was calculated by GPC and found to be 32,000. This can be estimated as 1,524 skeletal carbons. The results are shown in Table 2.
[0093] [Example 5] A 3 L autoclave was thoroughly dried in advance by passing nitrogen through it under heating, and then the inside of the autoclave was replaced with propylene and cooled to room temperature. 2.86 mL of a heptane solution of triisobutylaluminum (143 mg / mL) was added, and then 120 NmL of hydrogen was introduced. Next, 750 g of liquid propylene was introduced, and the temperature was then raised to 80°C. Then, 50 mg of catalyst 2 (excluding the prepolymerized polymer) was pumped into the polymerization tank with high-pressure argon to initiate polymerization. After maintaining the temperature at 80° C. for 1 hour, 5 ml of ethanol was pumped in to terminate the polymerization. As a result, 250 g of polymer was obtained. Granulation was carried out in the same manner as in Example 1, and the MFR of the resulting pellets (MFRpellet) was 3.0 g / 10 min. Other results are shown in Table 1.
[0094] [Reference Example 3]: Example of homopolymerization method of side chain (Catalyst Preparation) 20 g of the chemically treated montmorillonite obtained above was placed in a 1 L three-neck flask, and 131 mL of heptane was added to form a slurry. 50 mmol of triisobutylaluminum (69 mL of a heptane solution with a concentration of 143.4 mg / mL) was added thereto, and the mixture was stirred for 60 minutes. Then, the mixture was washed with heptane up to 1 / 100, and the total volume was adjusted to 100 mL. The slurry solution containing this chemically treated montmorillonite was kept at 50° C., and 4.2 mmol of tri-normal octylaluminum (10.7 mL of a heptane solution with a concentration of 143.4 mg / mL) was added thereto, followed by stirring for 20 minutes. To this was added 0.3 mmol of rac-dichloro[1,1'-dimethylsilylenebis{2-(5-methyl-2-furyl)-4-(4-isopropylphenyl)indenyl}]hafnium (complex 2) (prepared as a slurry with 50 mL of toluene), and the mixture was stirred for 20 minutes while maintaining the temperature at 50°C. Then, 350 mL of heptane was added and the slurry was introduced into a 1 L autoclave. After the internal temperature of the autoclave was raised to 40° C., propylene was fed at a rate of 10 g / hour, and prepolymerization was carried out for 4 hours while maintaining the temperature at 40° C. Thereafter, the propylene feed was stopped, and residual polymerization was carried out for 1 hour while maintaining the temperature at 40° C. The supernatant of the obtained catalyst slurry was removed by decantation, and then heptane was added again and decanted to wash the prepolymerized catalyst. 12 mmol of triisobutylaluminum (16.6 mL of a heptane solution with a concentration of 143.4 mg / mL) was added to the portion remaining after the decantation and stirred for 10 minutes. The solid was dried under reduced pressure at 40°C for 2 hours to obtain 54.0 g of a dried prepolymerized catalyst. The prepolymerization ratio (the value obtained by dividing the amount of prepolymerized polymer by the amount of solid catalyst) was 1.7. This prepolymerized catalyst was designated as catalyst 4. (polymerization) A 3L autoclave was thoroughly dried in advance by passing nitrogen through it under heating, and then the inside of the vessel was replaced with propylene and cooled to room temperature. 2.86 mL of a heptane solution of triisobutylaluminum (140 mg / mL) was added, and then 80 Nml of hydrogen was introduced. Then, 750 g of liquid propylene was introduced, and the temperature was raised to 80°C. Then, 165 mg of the above catalyst 4, excluding the prepolymerized polymer, was pumped into the polymerization vessel and polymerized at 80°C for 1 hour. Finally, the unreacted propylene was quickly purged to stop the polymerization. As a result, about 220 g of propylene homopolymer was obtained. MFR=520 g / 10 min. Mn was calculated by GPC and found to be 36,000. This can be estimated as 1,714 skeletal carbons. The results are shown in Table 2.
[0095] [Reference Example 4]: Example of side chain homopolymerization method The same polymerization as in Reference Example 3 was carried out, except that 150 mg of catalyst 4 (excluding the prepolymerized polymer) and 120 Nml of hydrogen were introduced. As a result, 240 g of polymer was obtained. MFR=570 / 10 min. Mn was calculated by GPC and found to be 35,000. This can be estimated as 1,667 skeletal carbons. The results are shown in Table 2.
[0096] [Comparative Example 1] A 3 L autoclave was thoroughly dried in advance by passing nitrogen through it under heating, and then the inside of the autoclave was replaced with propylene and cooled to room temperature. 2.86 mL of a heptane solution of triisobutylaluminum (143 mg / mL) was added, and then 210 NmL of hydrogen was introduced. Next, 750 g of liquid propylene was introduced, and the temperature was raised to 70° C. Then, 60 mg of the catalyst 2, excluding the prepolymerized polymer, was pumped into the polymerization tank with high-pressure argon to initiate polymerization. After maintaining at 70° C. for 1 hour, 5 ml of ethanol was pumped in to terminate the polymerization. As a result, 225 g of polymer was obtained. Granulation was carried out in the same manner as in Example 1. The MFR of the obtained pellets (MFR pellet )=1.4g / 10min.
[0097] [Comparative Example 2] The same polymerization as in Comparative Example 1 was carried out, except that 45 mg of catalyst 2 (excluding the prepolymerized polymer) and 230 Nml of hydrogen were introduced. As a result, 240 g of polymer was obtained. Granulation was carried out in the same manner as in Example 1. The MFR of the obtained pellets (MFR pellet )=2.8g / 10min.
[0098] [Reference Example 5]: Example of homopolymerization method of side chain A 3 L autoclave was thoroughly dried in advance by passing nitrogen through it under heating, and then the inside of the autoclave was replaced with propylene and cooled to room temperature. 2.86 mL of a heptane solution of triisobutylaluminum (140 mg / mL) was added, and then 210 NmL of hydrogen was introduced. Next, 750 g of liquid propylene was introduced, and the temperature was raised to 70° C. Then, 150 mg of the above catalyst 4, excluding the prepolymerized polymer, was pumped into the polymerization tank and polymerized at 70° C. for 1 hour. Finally, the unreacted propylene was quickly purged to terminate the polymerization. As a result, about 225 g of propylene homopolymer was obtained. MFR=38 g / 10 min. Mn was calculated by GPC and found to be 63,000. This can be estimated as 3,000 skeletal carbons. The results are shown in Table 2.
[0099] [Reference Example 6]: Example of side chain homopolymerization method The same polymerization as in Reference Example 3 was carried out, except that 130 mg of catalyst 4 (excluding the prepolymerized polymer) and 245 Nml of hydrogen were introduced. As a result, 230 g of polymer was obtained. MFR=53 / 10 min. Mn was calculated by GPC and found to be 62,000. This can be estimated as 2,952 skeletal carbons. The results are shown in Table 2.
[0100] (5) Measurement and evaluation methods The physical properties and extensibility of the branched propylene polymers obtained in Examples 1 to 5 and Comparative Examples 1 and 2 were measured or evaluated by the following methods. (5-1) Elongational viscosity (ηE), strain hardening index (SHI) and multi-branching index (MBI) The extensional viscosity was measured at each strain rate (1.0 / sec, 0.1 / sec, 0.01 / sec) by the method described above in the description of properties (1) and (2), and the strain hardening index (SHI) at each strain rate (dε / dt) was calculated using the measured values of the extensional viscosity. In addition, the multi-branching index (MBI) was calculated using the calculated values of the strain hardening index (SHI) at each strain rate (dε / dt). The apparatus and conditions used for measuring the extensional viscosity are as follows. <Measurement equipment and conditions> Equipment: Rheometorics Ares Fixture: TA Instruments Extentional Viscosity Fixture ·Measurement temperature: 180℃ ·Strain rate: 1.0 / sec, 0.1 / sec, 0.01 / sec Preparation of test specimen: Press mold a sheet of 18 mm x 10 mm and 0.7 mm thick.
[0101] (5-2) Proportion of components soluble in p-xylene at 25°C (CXS) The proportion of p-xylene soluble matter (CXS) contained in the branched propylene polymer was measured by the method described above in the description of the property (3).
[0102] (5-3) Molecular weight of branched side chains The catalysts (catalysts 1 and 2) used in the examples and comparative examples were a combination of complex 1 or complex 2, which is a component [A-1] capable of synthesizing a macromer, and complex 3, which is a component [A-2] capable of copolymerizing propylene with a macromer. In order to measure or estimate the molecular weight of the branched side chain, Reference Examples 1 to 6 were carried out using only complex 1 (catalyst 3) or complex 2 (catalyst 4), which is capable of synthesizing a macromer, and the molecular weight (Mn) of the resulting macromer was measured. The molecular weight (Mn) of the macromer was measured by gel permeation chromatography (GPC) using the method described above in the description of property (4). The apparatus and conditions used for measuring the macromer molecular weight (Mn) are as follows: <Measurement equipment and conditions> Apparatus: Waters GPC (ALC / GPC, 150C) Detector: FOXBORO MIRAN, 1A, IR detector (measurement wavelength: 3.42 μm) Column: Showa Denko AD806M / S (3 columns) Mobile phase solvent: o-dichlorobenzene (ODCB) ·Measurement temperature: 140℃ ·Flow rate; 1.0mL / min ·Injection volume; 0.2mL
[0103] (5-4) Melt flow rate (MFR) at 230℃ and 2.16kg load The MFR of the branched propylene polymer in a powder state and the MFR of the branched propylene polymer in a pelletized state were measured. Also, the MFR of the macromers obtained in Reference Examples 1 to 6 were measured. As described above in the description of the characteristic (5), the MFR was measured in accordance with JIS K6921-2 "Plastics-Polypropylene (PP) molding and extrusion materials-Part 2: Preparation of test pieces and determination of properties" under test conditions of 230°C and a load of 2.16 kgf.
[0104] (5-5) Branching index g' (1 million) for components with molecular weight M of 1 million or more (W1 million) and absolute molecular weight Mabs of 1 million By the method described above in the description of the characteristic (6), the branched propylene polymer was measured for the components (W1 million) having a weight average molecular weight Mw of 1 million or more and the branching index g' (1 million) having an absolute molecular weight Mabs of 1 million.
[0105] (5-6) Melting point (Tm) The melting point (Tm) of the branched propylene polymer was measured by the method described above in the description of the property (7).
[0106] (5-7) Number of long chain branches (LCB) The number of long chain branches (LCB) having 7 or more carbon atoms per 1,000 monomer units was measured by the method described above in the description of property (8).
[0107] (5-8) Melt tension The melt tension MT230°C (unit: g / 10 min) of the branched propylene polymer at 230°C was measured by the method described above in the description of the property (9).
[0108] (5-9) Spreadability The maximum take-up speed MaxDraw (unit: m / min) of the branched propylene polymer at 170° C. was measured by the method described above in the description of the property (10).
[0109] (6) Evaluation results The results of each of the Examples and Comparative Examples are shown in Tables 1 to 4. Table 1 shows the polymerization conditions of the examples and comparative examples in which branched propylene polymers were synthesized, and the MFR, the proportion of xylene soluble components, the components with a molecular weight M of 1 million or more (W1 million), the branching index g' (1 million) at an absolute molecular weight Mabs of 1 million, the number of long chain branches (LCB) having 7 or more carbon atoms per 1,000 monomer units, the melting point (Tm), and the macromers of the reference examples corresponding to the branched chains of the branched propylene polymers. Table 2 shows the polymerization conditions of Reference Examples in which macromers corresponding to the branched chains of the branched propylene polymers obtained in the Examples and Comparative Examples were synthesized, and the MFR, number average molecular weight (Mn), and carbon number of the skeleton of the obtained macromers. Table 3 shows the MFR, the elongational viscosity ηE at each strain rate (0.01 / sec, 0.1 / sec, 1.0 / sec), the strain hardening index (SHI) at each strain rate (0.01 / sec, 0.1 / sec, 1.0 / sec), and the multi-branching index (MBI) calculated from the strain hardening index (SHI) at strain rates from 0.01 / sec to 1.0 / sec for the branched propylene polymers obtained under the polymerization conditions of each Example and Comparative Example. The graph in FIG. 5 is a graph in which the horizontal axis represents MFR (MFR 230° C., 2.16 kg load) and the vertical axis represents multibranching index (MBI), and data on the branched propylene polymers obtained in each of the Examples and Comparative Examples are plotted. Table 4 shows the MFR, melt tension at 230°C (MT230°C), and maximum draw-up speed at 230°C (MaxDraw) for the branched propylene polymers obtained under the polymerization conditions of each of the Examples and Comparative Examples. The graph in FIG. 6 is a graph in which the data of the branched propylene polymers obtained in each Example and Comparative Example are plotted, with MFR (MFR 230° C., 2.16 kg load) on the horizontal axis and maximum winding speed (MaxDraw) at 170° C. on the vertical axis. The graph in FIG. 7 is a graph in which the data of the branched propylene polymers obtained in each Example and Comparative Example are plotted, with the melt tension (MT230°C) on the horizontal axis and the maximum winding speed (MaxDraw) at 230°C on the vertical axis.
[0110] [Table 1]
[0111] [Table 2]
[0112] [Table 3]
[0113] [Table 4]
[0114] As shown in Table 3, the branched propylene polymers of Examples 1 to 5 have a multi-branching index (MBI) of 0.15 to 0.43, which is within the range of property (1), and a strain hardening index (SHI@1.0 -1 ) was 1.14 to 1.75, which was within the range of property (2). As shown in Table 4, the branched propylene polymers of Examples 1 to 5 had a melt tension@230°C of 6.0 to 16.6 g, and while maintaining the melt tension necessary for molding, the maximum winding speed (230°C) was 66 to 119 m / s, and they also had excellent extensibility when molten. In contrast, as shown in Table 3, the branched propylene polymers of Comparative Examples 1 and 2 had a strain hardening index (SHI@1.0 -1 ) was 1.75 to 1.88, which was within the range of property (2), but the multi-branching index (MBI) was 0.05 to 0.08, which was smaller than the lower limit of the range of property (1). As shown in Table 4, the branched propylene polymers of Comparative Examples 1 and 2 had a melt tension@230°C of 8.6 to 16.6 g, which was sufficient for molding, but had a maximum winding speed (230°C) of 31 to 53 m / s, which was inferior in extensibility when molten. As shown in FIG. 5, when a graph was prepared by plotting data of the branched propylene polymers obtained in each of the Examples and Comparative Examples, with MFR on the horizontal axis and multi-branching index (MBI) on the vertical axis, it was confirmed that the branched propylene polymers of the Examples had a larger MBI than the branched propylene polymers of the Comparative Examples. As shown in FIG. 6, a graph was prepared by plotting data of the branched propylene polymers obtained in each of the Examples and Comparative Examples, with MFR (MFR 230° C., 2.16 kg load) on the horizontal axis and maximum winding speed (MaxDraw) at 230° C. on the vertical axis. It was confirmed that the branched propylene polymers of the Examples were superior in extensibility to the branched propylene polymers of the Comparative Examples. As shown in FIG. 7, a graph was prepared by plotting data of the branched propylene polymers obtained in each Example and Comparative Example, with melt tension (MT230°C) on the horizontal axis and maximum take-up speed (MaxDraw) at 230°C on the vertical axis. It was confirmed that the branched propylene polymers of the Examples were superior in extensibility to the branched propylene polymers of the Comparative Examples.
[0115] As shown in Table 1, in the branched propylene polymers of Examples 1 to 5, the component with a molecular weight M of 1 million or more (W1 million) in the molecular weight distribution curve was 0.070 to 0.100. In contrast, in the branched propylene polymers of Comparative Examples 1 and 2, the content of components having a molecular weight Mw of 1 million or more (W1 million) was 0.067 to 0.068. Therefore, the branched propylene polymers of Examples 1 to 5 have a larger high molecular weight region than the branched propylene polymers of Comparative Examples.
[0116] Furthermore, as shown in Table 1, the branched propylene polymers of Examples 1 to 5 had a branching index g' (1 million) of 0.88 to 0.89 when the absolute molecular weight Mabs was 1 million. In contrast, the branching index g' (1 million) of Comparative Examples 1 and 2 was 0.89. The branched propylene polymers of Examples 1 to 5 are equivalent to those of Comparative Examples 1 and 2 in terms of the branching index g' (million). However, as described above, the high molecular weight region represented by the component having a weight average molecular weight Mw of 1 million or more (W million) is greater than those of Comparative Examples 1 and 2. Therefore, the amount of branched chains introduced into the high molecular weight region is greater than those of Comparative Examples 1 and 2.
[0117] Furthermore, as shown in Tables 1 and 2, the length of the side chain introduced into the branched propylene polymers of Examples 1 to 5 is estimated to be a molecular weight Mn of 33,000 (1,571 in terms of the number of skeleton carbon atoms) to 36,000 (1,714 in terms of the number of skeleton carbon atoms) from the results of Reference Examples 1 to 4. In contrast, the length of the side chain introduced into the branched propylene polymers of Comparative Examples 1 to 3 is estimated to be a molecular weight Mn of 62,000 to 63,000 from the results of Reference Examples 5 and 6. Therefore, the branched propylene polymers of Examples 1 to 5 have shorter side chains than the branched propylene polymers of Comparative Examples.
[0118] As shown in Table 1, the branched propylene polymers of Examples 1 to 5 have a small number of long chain branches (LCB) having 7 or more carbon atoms per 1000 monomer units of 1.0 or less. The branched propylene polymers of Comparative Examples 1 and 2 also have a small number of long chain branches (LCB) of 1.0 or less.
[0119] From the above-described molecular structure analysis, it was confirmed that the branched propylene polymers obtained in Examples 1 to 5 have a molecular structure in which, in the high molecular weight region, there are many multi-branched molecules having many branches with short branch chain lengths per molecule, and the polymers have a relaxation time distribution in which there are many components having a relatively short relaxation time and few components having an extremely long relaxation time.
Claims
1. A branched propylene polymer having the following properties (1) and (2): Property (1): The multi-branching index (MBI) is 0.15 or more and 1.00 or less. Property (2): Strain hardening index (SHI@1s) at a strain rate (dε / dt) of 1.0 / s -1 ) is 0.70 or more and 3.00 or less. Here, the multibranching index (MBI) is the slope of a plot of the strain hardening index (SHI) at strain rates (dε / dt) of 0.01 / sec to 1.0 / sec, with the logarithm of the strain rate (log(dε / dt)) on the horizontal axis and the strain hardening index (SHI) at strain rates of 0.01 / sec to 1.0 / sec on the vertical axis. The strain hardening index (SHI) is the slope of a plot of the logarithm (log(ε)) of the Henky strain (ε) on the horizontal axis and the logarithm (log(η)) of the extensional viscosity (η) on the vertical axis in the Henky strain (ε) range of 1 to 3, in the measurement of the extensional viscosity at a temperature of 180° C. and a predetermined strain rate (dε / dt).
2. The branched propylene polymer according to claim 1 , further satisfying the following characteristic (3): Property (3): The proportion of components soluble in p-xylene at 25° C. (CXS) is less than 0.5 mass %.
3. The branched propylene polymer according to claim 1 or 2, further satisfying the following characteristic (4): Property (4): The molecular weight Mn of the branched side chain is 11,000 or more and 53,000 or less.
4. The branched propylene polymer according to any one of claims 1 to 3, further satisfying the following characteristic (5). Property (5): The melt flow rate (MFR) measured at a temperature of 230° C. under a load of 2.16 kg is 1 to 10 g / 10 min.
5. The branched propylene polymer according to any one of claims 1 to 4, further satisfying the following property (6-1). Property (6-1): In a molecular weight distribution curve measured by GPC, the component having a molecular weight M of 1 million or more (W1 million) is 0.070 or more and 0.100 or less.
6. The branched propylene polymer according to any one of claims 1 to 5, further satisfying the following property (6-2). Property (6-2): The branching index g' (1 million) at an absolute molecular weight Mabs of 1 million as measured by 3D-GPC is 0.80 or more and 0.90 or less.
7. The branched propylene polymer according to any one of claims 1 to 6, further satisfying the following characteristic (7): Property (7): The melting point (Tm) measured by differential scanning calorimetry (DSC) is 150° C. or higher and 157° C. or lower.
8. The branched propylene polymer according to any one of claims 1 to 7, further satisfying the following characteristic (8). Property (8): The branched propylene polymer has a long chain branched structure portion represented by the following structural formula (A). 【Chemistry 1】 [In the structural formula (A), P 1 , P 2 , P 3 are residues generated at the ends of branched propylene polymers, each of which has one or more propylene units, Cbr represents a methine carbon at the root of a branched chain having 7 or more carbon atoms, and Ca, Cb, and Cc represent methylene carbons adjacent to the methine carbon (Cbr).
Citation Information
Patent Citations
Propylene-based polymer
JP2009275207A
Polymerization catalyst for propylene / ethylene-alpha-olefin block copolymer and method for producing propylene-based block copolymer by using the same
JP2010150497A
Olefin polymerization catalyst and method for producing the same
JP2010196037A
Polyethylene resin composition for container and molded body comprising the same
JP2014208749A
Method for producing propylene polymer
JP2018162391A