Laminated film

A laminated film with a polypropylene base and optimized inorganic and organic layers addresses the challenges of recyclability and environmental impact, achieving superior gas barrier and adhesive properties.

JP2024149587AInactive Publication Date: 2024-10-18TOYOBO CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2024124409
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-10-18
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing gas barrier coated films made from polypropylene films do not adequately address the requirements of being recyclable, having sufficient gas barrier properties, and minimizing environmental impact, particularly due to issues with humidity dependence, adhesion, and thick coating layers that hinder recycling and increase environmental burden.

Method used

A laminated film structure comprising a polypropylene base film with an inorganic thin film layer and an organic resin layer, optimized for thickness, adhesion, and roughness, to achieve improved gas barrier properties and adhesive strength while maintaining recyclability and reducing environmental impact.

Benefits of technology

The laminated film provides excellent gas barrier performance, adhesive strength, and processability, enabling easy recycling and reducing environmental impact by minimizing the thickness of adhesive layers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024149587000001
    Figure 2024149587000001
  • Figure 2024149587000002
    Figure 2024149587000002
  • Figure 2024149587000003
    Figure 2024149587000003
Patent Text Reader

Abstract

To provide a laminated film that can form a laminate structure composed of almost a single resin type mainly comprising a polypropylene film and having a low environmental load, and has necessary performance, such as gas barrier properties, adhesiveness, and processing suitability, required for a packaging material.SOLUTION: In a laminated film, a surface layer (B) is provided on one surface of a substrate layer (A) mainly composed of a polypropylene-based resin, a surface layer (C) is provided on the other surface of the substrate layer (A), and an inorganic thin film layer (D) is laminated on the surface layer (B) and an organic resin layer (E) is further laminated on the inorganic thin film layer (D). The laminated film satisfies the following requirements (a) to (d): (a) the adhesion amount of the organic resin layer (E) is 0.10 g / m2 or more and 0.50 g / m2 or less; (b) the Martens hardness of the organic resin layer side surface of the laminated film is 248 N / mm2 or less when measured with a test force of 0.1 mN; (c) the haze of the laminated film is 6% or less; and (d) the oxygen permeability of the laminated film in a 23°C×65% RH environment is 10 mL / m2 d MPa or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a gas barrier laminate film, more specifically to a gas barrier coated film that imposes a small environmental load during production and disposal, and that combines excellent gas barrier performance with sufficient adhesive strength for use as a packaging material. [Background technology]

[0002] In recent years, regulations aimed at reducing the use of disposable plastics have been strengthened in Europe and other countries around the world. Behind this lies the growing international awareness of resource circulation and the worsening waste problems in emerging countries. For this reason, there is a demand for environmentally friendly products from the perspective of the 3Rs (recycle, reuse, reduce) for plastic packaging materials required for food, medicines, etc.

[0003] The performance required for the aforementioned environmentally friendly packaging materials includes (1) being made from recyclable materials, (2) having gas barrier performance that can block various gases and extend the shelf life, and (3) having a laminate structure that has a low environmental impact (for example, not using organic solvents, using only small amounts of materials, and being recyclable by converting them into mono-materials).

[0004] In recent years, the use of polypropylene films has been attracting attention in order to make the above (2) and (3) possible. Polypropylene films are used for a wide range of purposes, such as packaging for food and various other products, electrical insulation, and surface protection films. Polypropylene films are capable of exhibiting high water vapor barrier properties due to their molecular structure. Furthermore, since polypropylene- or polyethylene-based heat seal resins are generally used as sealants to be bonded to the surface substrate film, for example, by using a polypropylene film for the surface substrate and an unstretched polypropylene sheet for the sealant, it is possible to achieve mono-materialization of the entire packaging material while maintaining gas barrier properties, and to design packaging materials that are easy to recycle and are environmentally friendly.

[0005] However, with regard to the gas barrier property of (2) above, although polypropylene film has water vapor barrier property, the water vapor barrier property is not sufficient compared to, for example, transparent inorganic vapor-deposited polyester film, which is generally considered to have excellent water vapor barrier property, and there is a problem that the oxygen barrier property is very poor. In response to this, films have been used in which a polymer resin composition, which is generally considered to have a relatively high oxygen barrier property, such as polyvinyl alcohol, ethylene-vinyl alcohol copolymer, polyvinylidene chloride resin, polyacrylonitrile, etc., is laminated on a polypropylene film (for example, see Patent Documents 1 to 3).

[0006] However, the gas barrier coating film made of the above-mentioned polyvinyl alcohol or ethylene vinyl alcohol copolymer polymer resin composition has a high humidity dependency, and therefore the gas barrier property is deteriorated under high humidity conditions. Also, polyvinylidene chloride resin and polyacrylonitrile have low humidity dependency, but the barrier value as an absolute value is insufficient, and there is a problem that there is a high risk of hazardous substances being generated during disposal and incineration.

[0007] As a method for improving the humidity dependency of vinyl alcohol-based resins, a gas barrier coated film has been proposed in which a coating layer in which a silane-based crosslinking agent is mixed with vinyl alcohol-based resin is laminated. In this case, since the vinyl alcohol-based resin is crosslinked by silanol groups, the film has low humidity dependency and shows good gas barrier properties (see, for example, Patent Documents 4 and 5).

[0008] However, these gas barrier coated films require sufficient heat treatment to crosslink them, and when the substrate is a polypropylene film, the mechanical properties deteriorate and the film is thermally wrinkled during processing, which means that the film does not have sufficient properties as a packaging material. In addition, the film requires a lot of heat energy during the heat treatment during processing, which is undesirable from the viewpoint of environmental load. Furthermore, the water vapor barrier performance is still insufficient.

[0009] On the other hand, as a means for further improving the barrier performance, a gas barrier coated film has been proposed in which a resin layer containing inorganic layered particles of a specific particle size and aspect ratio is laminated to a vinyl alcohol resin. In this case, the inorganic layered particles dispersed in the resin layer cause a detouring effect of gas molecules, resulting in good gas barrier properties (see, for example, Patent Documents 6 and 7).

[0010] However, in these gas barrier coated films, the inorganic layered particles are often not uniformly dispersed in the coating film, which results in impaired adhesion to the substrate film and reduced laminate strength.Furthermore, sufficient performance has not been achieved in terms of improving both the oxygen barrier property and the water vapor barrier property.

[0011] All of the above-mentioned barrier coat layers needed to be laminated to a thickness of at least 0.5 μm to achieve sufficient barrier performance. If the coat layer was too thick, recycling could be difficult, and it was also not suitable from the perspective of mono-materialization using a single material. Furthermore, there was an issue of printing defects due to unevenness and irregularities in the coat during processing such as printing. [Prior art documents] [Patent documents]

[0012] [Patent Document 1] JP 2000-52501 A [Patent Document 2] Japanese Patent Application Publication No. 4-359033 [Patent Document 3] JP 2003-231221 A [Patent Document 4] Japanese Patent Application Publication No. 4-345841 [Patent Document 5] JP 2006-95782 A [Patent Document 6] Japanese Patent Application Publication No. 9-111017 [Patent Document 7] JP 2005-35167 A Summary of the Invention [Problem to be solved by the invention]

[0013] In the above Patent Documents 1 to 3, in addition to insufficient barrier performance, no consideration was given to environmentally friendly design. Patent Documents 4 and 5 did not consider appropriate coating processing of polypropylene film, and water vapor barrier properties were not fully discussed. Patent Document 6 did not consider improvement of adhesiveness or water vapor barrier properties. Patent Document 7 did not consider oxygen barrier properties. Furthermore, none of the documents considered improvement of processability or environmental friendliness by thinning the coating layer, nor did they consider environmental friendliness by thinning the adhesive layer when forming a laminate structure. In other words, until now, there has not been a material that satisfies all three of the performance requirements for an environmentally friendly packaging material: (1) containing recyclable materials as constituent materials, (2) having gas barrier performance that can block various gases and extend the shelf life, and (3) having a laminate structure that is easy to recycle and has a low environmental impact (mono-material).

[0014] The present invention has been made in view of the above problems in the prior art. In other words, the object of the present invention is to provide a laminate film that can form a laminate structure composed of almost a single resin type that has a low environmental impact, mainly consisting of a polypropylene film, and that has the necessary performance properties required for packaging materials, such as gas barrier properties, adhesion, transparency, and processability. [Means for solving the problem]

[0015] The present inventors discovered that by laminating a specific inorganic thin film layer and a coating layer tailored to the required performance on a polypropylene film, it is possible to greatly improve the gas barrier performance, and further provide a high-quality film with improved adhesive strength and low environmental impact, thereby completing the present invention.

[0016] That is, the present invention comprises the following: 1. A laminate film comprising a substrate layer (A) mainly composed of a polypropylene resin, a surface layer (B) on one surface thereof, a surface layer (C) on the other surface thereof, an inorganic thin film layer (D) laminated on the surface layer (B), and an organic resin layer (E) laminated on the inorganic thin film layer (D), the laminate film being characterized by satisfying the following requirements (a) to (d): (a) The coating weight of the organic resin layer (E) is 0.10 g / m 2 More than 0.50g / m 2 It is less than or equal to. (b) The Martens hardness of the organic resin layer side surface of the laminated film is 248 N / mm when measured with a test force of 0.1 mN. 2 It is less than or equal to. (c) The haze of the laminated film is 6% or less. (d) The oxygen permeability of the laminated film in a 23°C x 65% RH environment is 10 mL / m 2 ·d·MPa or less. 2.Water vapor permeability at 40℃ × 90%RH is 1g / m 2 2. The laminate film according to claim 1, wherein the thickness of the laminate film is 1.0 mm or less. 3. The oxygen permeability of the laminated film in an environment of 23°C x 80% RH is 15 mL / m 2 3. The laminate film according to 1 or 2, characterized in that the compressive strength is 1.0 MPa or less. 4. The laminate film according to any one of 1 to 3, wherein the organic resin layer on the laminate film has an arithmetic mean roughness in a 2 μm square range of 2.0 to 8.0 nm. 5. The laminate film according to any one of 1 to 4, wherein the thickness of the laminate film is 9 μm to 200 μm. 6. A packaging material comprising the laminate film according to any one of 1 to 5 above and an olefin-based sealant layer laminated on one side thereof. Effect of the Invention

[0017] With this technology, the inventors have been able to provide a laminated film that is environmentally friendly and has the necessary performance required for packaging materials, such as barrier properties, adhesive properties, and processability. In particular, the adhesive strength of laminated products can be improved, and sufficient adhesive strength can be achieved even when the thickness of the adhesive layer is reduced, which reduces the consumption of adhesive used and leads to further reduction in the environmental load. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] The present invention will be described in detail below. [Base film layer] The propylene-based resin stretched film used as the base film in the present invention is preferably a biaxially stretched film. As the biaxially stretched polypropylene-based resin film, a known biaxially stretched polypropylene-based resin film can be used, and the raw materials, mixing ratio, etc. are not particularly limited. For example, in addition to polypropylene homopolymer (propylene homopolymer), it may be a random copolymer or block copolymer with propylene as the main component and one or more α-olefins selected from ethylene, butene, pentene, hexene, etc., or a mixture of two or more of these polymers. In addition, known additives such as antioxidants, antistatic agents, and plasticizers may be added for the purpose of improving physical properties, and for example, petroleum resins and terpene resins may be added.

[0019] The biaxially oriented polypropylene resin film used in the present invention may be a single layer film, or may be a laminated film in which a plurality of resin films including a biaxially oriented polypropylene resin film are laminated. When a laminated film is used, the type of laminate, the number of layers, the lamination method, etc. are not particularly limited, and can be arbitrarily selected from known methods according to the purpose.

[0020] In the present invention, the polypropylene resin constituting the base film is preferably a propylene homopolymer that does not substantially contain a comonomer, and even if it contains a comonomer, the amount of the comonomer is preferably 0.5 mol% or less. The upper limit of the amount of the comonomer is more preferably 0.3 mol%, and even more preferably 0.1 mol%. When it is in the above range, the crystallinity is improved, the heat shrinkage rate at high temperatures is small, and the heat resistance is improved. Note that a small amount of comonomer may be contained within a range that does not significantly reduce the crystallinity.

[0021] The polypropylene resin constituting the base film preferably contains a propylene homopolymer obtained only from propylene monomers, and even if it is a propylene homopolymer, it is most preferable that it does not contain a heterogeneous bond such as a head-to-head bond.

[0022] The lower limit of the xylene soluble content of the polypropylene resin constituting the base film is preferably 0.1% by mass from a practical standpoint. The upper limit of the xylene soluble content is preferably 7% by mass, more preferably 6% by mass, and even more preferably 5% by mass. When it is in the above range, the crystallinity is improved, the heat shrinkage rate at high temperatures is smaller, and the heat resistance is improved.

[0023] In the present invention, the lower limit of the melt flow rate (MFR) (230°C, 2.16 kgf) of the polypropylene resin is preferably 0.5 g / 10 min. The lower limit of the MFR is more preferably 1.0 g / 10 min, even more preferably 2.0 g / 10 min, particularly preferably 4.0 g / 10 min, and most preferably 6.0 g / 10 min. Within the above range, the mechanical load is small, and extrusion and stretching are easy. The upper limit of the MFR is preferably 20 g / 10 min. The upper limit of the MFR is more preferably 17 g / 10 min, even more preferably 16 g / 10 min, and particularly preferably 15 g / 10 min. Within the above range, stretching is easy, thickness unevenness is small, the stretching temperature and heat setting temperature are easily increased, the heat shrinkage rate is smaller, and heat resistance is improved.

[0024] From the viewpoint of heat resistance, the base film may be a uniaxially stretched film in the longitudinal direction (MD) or transverse direction (TD), but is preferably a biaxially stretched film. In the present invention, by stretching at least uniaxially, a film having a low thermal shrinkage rate at high temperatures and high heat resistance, which was not expected for conventional polypropylene films, can be obtained. Examples of the stretching method include simultaneous biaxial stretching and sequential biaxial stretching, but sequential biaxial stretching is preferred from the viewpoint of improving flatness, dimensional stability, thickness unevenness, etc.

[0025] In the sequential biaxial stretching method, polypropylene resin is heated and melted in a single-screw or twin-screw extruder so that the resin temperature is 200°C to 280°C, formed into a sheet from a T-die, and extruded onto a chill roll at a temperature of 10°C to 100°C to obtain an unstretched sheet. Next, the sheet is roll-stretched 3.0 to 8.0 times in the longitudinal direction (MD direction) at 120°C to 165°C, and then, after preheating with a tenter, can be stretched 4.0 to 20.0 times in the transverse direction (TD direction) at a temperature of 155°C to 175°C. Furthermore, after the biaxial stretching, a heat setting treatment can be performed while allowing relaxation of 1% to 15% at a temperature of 165°C to 175°C.

[0026] In order to impart handling properties (for example, winding properties after lamination), it is preferable that the substrate film used in the present invention contains particles in the film to form protrusions on the film surface. Examples of particles contained in the film include inorganic particles such as silica, kaolinite, talc, calcium carbonate, zeolite, and alumina, and heat-resistant polymer particles such as acrylic, PMMA, nylon, polystyrene, polyester, and benzoguanamine-formaldehyde condensate. From the viewpoint of transparency, it is preferable that the content of particles in the film is low, for example, 1 ppm or more and 1000 ppm or less. Furthermore, from the viewpoint of transparency, it is preferable to select particles having a refractive index close to that of the resin used. In addition, the film may contain antioxidants, ultraviolet absorbers, antistatic agents, dyes, lubricants, nucleating agents, adhesives, antifogging agents, flame retardants, antiblocking agents, inorganic or organic fillers, etc., in order to impart various functions as necessary.

[0027] Other than the polypropylene resin used in the present invention, the film may contain a resin for improving the mechanical properties of the base film and the adhesion to the ink layer or adhesive layer laminated on the gas barrier coating layer, within the scope of the present invention. Examples of such resins include polypropylene resins other than those mentioned above, random copolymers which are copolymers of propylene and ethylene and / or α-olefins having 4 or more carbon atoms, and various elastomers.

[0028] In the present invention, the thickness of the base film is arbitrarily set according to each application, but the lower limit is preferably 2 μm or more, more preferably 3 μm or more, and even more preferably 4 μm or more. On the other hand, the upper limit of the thickness is preferably 300 μm or less, more preferably 250 μm or less, even more preferably 200 μm or less, and particularly preferably 100 μm or less. If the thickness is thin, the handling property is likely to be poor. On the other hand, if the thickness is thick, not only is there a problem in terms of cost, but also when it is wound into a roll and stored, poor flatness is likely to occur due to a rolling tendency.

[0029] The haze of the polypropylene film used as the substrate of the present invention is preferably transparent from the viewpoint of visibility of the contents, specifically, 6% or less, more preferably 5% or less, and even more preferably 4% or less. Haze tends to deteriorate, for example, when the stretching temperature or heat setting temperature is too high, when the cooling roll (CR) temperature is high and the cooling speed of the stretched raw sheet is slow, or when there is too much low molecular weight, so it can be controlled within the above range by adjusting these. Here, the haze was evaluated in accordance with JIS K7136, using a turbidity meter (Nippon Denshoku, NDH2000).

[0030] Furthermore, the base film layer in the present invention may be subjected to corona discharge treatment, glow discharge treatment, flame treatment, surface roughening treatment, or known anchor coat treatment, printing, decoration, etc., as long as the object of the present invention is not impaired. It is preferable to perform anchor coat treatment in order to stabilize the barrier property. However, since a resin other than polyolefin, such as polyurethane or polyester, is generally used for the anchor coat layer, it is preferable to control the adhesion amount to be small from the viewpoint of mono-material when performing anchor coat treatment. The adhesion weight of the anchor coat layer is 0.01 to 0.50 g / m 2 This allows the anchor coat layer to be uniformly controlled during coating, resulting in a film with fewer coating irregularities and defects. The amount of the anchor coat layer is preferably 0.05 g / m 2 More preferably, 0.10 g / m 2 or more, preferably 0.47 g / m 2 Less than or equal to 0.45 g / m 2 The adhesion weight of the anchor coat layer is 0.50 g / m or less. 2 If the thickness exceeds 100 mm, the gas barrier property is improved, but the moisture content in the laminated film increases due to the thickness. In terms of processability, the thickness may cause blocking. Furthermore, there is a concern that the recyclability and manufacturing cost of the film may be adversely affected.

[0031] [Inorganic thin film layer] The gas barrier laminated film of the present invention has an inorganic thin film layer on the surface of the base film layer. The inorganic thin film layer is a thin film made of a metal or an inorganic oxide. There are no particular limitations on the material forming the inorganic thin film layer as long as it can be made into a thin film, but from the viewpoint of gas barrier properties, preferred examples include inorganic oxides such as silicon oxide (silica), aluminum oxide (alumina), and a mixture of silicon oxide and aluminum oxide. In this composite oxide, the mixing ratio of silicon oxide and aluminum oxide is preferably in the range of 20 to 70 mass% Al in terms of the mass ratio of the metal content. If the Al concentration is less than 20 mass%, the water vapor barrier properties may be reduced. On the other hand, if it exceeds 70 mass%, the inorganic thin film layer tends to become hard, and there is a risk that the film will be destroyed during secondary processing such as printing and lamination, resulting in a decrease in gas barrier properties. In addition, when the Al concentration is 100 mass%, the water vapor barrier performance is good, but since it is a single material, the surface tends to be smooth, and the slipperiness is poor and processing defects (wrinkles, acne, etc.) are likely to occur. Note that silicon oxide here refers to SiO or SiO 2 Aluminum oxide is AlO or Al 2 O 3 and mixtures thereof.

[0032] The inorganic thin film layer has a thickness of usually 1 to 100 nm, preferably 5 to 50 nm. If the inorganic thin film layer has a thickness of less than 1 nm, it may be difficult to obtain satisfactory gas barrier properties, while if the inorganic thin film layer has a thickness exceeding 100 nm, the corresponding improvement in gas barrier properties cannot be obtained, and it is rather disadvantageous in terms of flex resistance and production costs.

[0033] The method for forming the inorganic thin film layer is not particularly limited, and any known deposition method may be appropriately used, for example, a physical deposition method (PVD method) such as a vacuum deposition method, a sputtering method, or an ion plating method, or a chemical deposition method (CVD method). A typical method for forming an inorganic thin film layer will be described below using a silicon oxide / aluminum oxide thin film as an example. For example, when the vacuum deposition method is used, SiO 2 and Al 2 O3 or a mixture of SiO 2 A mixture of ZnO and Al is preferably used. Particles are usually used as the deposition raw materials, and in this case, the size of each particle is desirably large enough that the pressure during deposition does not change, and the preferred particle diameter is 1 mm to 5 mm. Heating can be performed by resistance heating, high-frequency induction heating, electron beam heating, laser heating, or other methods. It is also possible to introduce oxygen, nitrogen, hydrogen, argon, carbon dioxide, water vapor, or other reactive gases as reactive gases, or to employ reactive deposition using ozone addition, ion assist, or other means. Furthermore, the film formation conditions can be changed arbitrarily, such as by applying a bias to the deposition target (laminated film to be subjected to deposition), or by heating or cooling the deposition target. Such deposition materials, reactive gases, bias, heating and cooling of the deposition target, etc. can be changed in the same way when the sputtering method or CVD method is used.

[0034] [Organic resin layer] In the present invention, the organic resin layer is provided for the purpose of improving the gas barrier performance and adhesiveness of the base film, but in the present invention, the provision of the organic resin layer increases the number of steps, leading to increased costs, and depending on the film thickness, may make recycling difficult, which may impose a burden on the environment. This must be taken into consideration when designing the present invention.

[0035] The adhesion weight of the organic resin layer is 0.10 to 0.50 (g / m 2 Since the organic resin layer is thin, it can contribute to reducing foreign matter during recycling. The lower limit of the amount of adhesion of the organic resin layer is preferably 0.15 (g / m 2 ) or more, more preferably 0.20 (g / m 2 ) or more, more preferably 0.25 (g / m 2 ) or more, and the upper limit is preferably 0.45 (g / m 2 ) or less, more preferably 0.40 (g / m 2 ) or less, more preferably 0.35 (g / m 2 The adhesion weight of the organic resin layer is 0.50 (g / m 2), the gas barrier properties improve, but the cohesive force inside the organic resin layer becomes insufficient and the uniformity of the organic resin layer also decreases, resulting in unevenness (increased haze, whitening) and defects in the appearance of the coat, and in some cases the gas barrier properties and adhesive properties may not be fully realized. In terms of processability, a thick film thickness may cause blocking. Furthermore, there is a concern that it may have a negative effect on the recyclability of the film. On the other hand, if the film thickness of the organic resin layer is more than 0.10 (g / m 2 ) there is a risk that sufficient gas barrier properties and interlayer adhesion cannot be obtained.

[0036] As the resin composition used for the organic resin layer formed on the surface of the laminated film of the present invention, a polymer resin composition generally said to have a relatively high oxygen barrier property can be used. Examples include polyvinyl alcohol, ethylene-vinyl alcohol copolymer, polyvinylidene chloride resin, polyacrylonitrile, etc. Polyvinyl alcohol-based polymers are mainly composed of polyvinyl alcohol units, and a significant improvement in barrier performance due to high cohesiveness caused by a hydrogen bond structure can be expected. The polymerization degree and saponification degree of the polyvinyl alcohol-based polymer are determined based on the target gas barrier property and the viscosity of the coating aqueous solution. The polymerization degree is preferably 2600 or less from the viewpoint of coating workability, since the aqueous solution has a high viscosity and is prone to gelation, making coating difficult. With regard to the saponification degree, if it is less than 90%, sufficient oxygen gas barrier property cannot be obtained under high humidity, and if it exceeds 99.7%, it is difficult to adjust the aqueous solution, it is prone to gelation, and it is not suitable for industrial production. Therefore, the saponification degree is preferably 90 to 99.7%, and more preferably 93 to 99%. In the present invention, various copolymerized or modified polyvinyl alcohol polymers, such as polyvinyl alcohol polymers copolymerized with ethylene and silanol-modified polyvinyl alcohol polymers, can also be used within the scope of not impairing processability or productivity.

[0037] The organic resin layer of the present invention preferably contains an inorganic layered compound. The presence of the inorganic layered compound is expected to provide a labyrinth effect for gas, improving the gas barrier properties. Examples of the material include clay minerals (including synthetic products thereof) such as smectite, kaolin, mica, hydrotalcite, and chlorite. Specific examples include montmorillonite, beidellite, saponite, hectorite, sauconite, stevensite, kaolinite, nacrite, dickite, halloysite, hydrated halloysite, tetrasilylic mica, sodium teniolite, muscovite, margarite, phlogopite, talc, antigorite, chrysotile, pyrophyllite, vermiculite, xanthophyllite, and chlorite. Furthermore, scaly silica and the like can also be used as the inorganic layered compound. These may be used alone or in combination of two or more. Among these, smectite (including synthetic products thereof) is particularly preferred because it has a high effect of improving water vapor barrier properties.

[0038] In addition, the inorganic layered compound is preferably one that contains a metal ion, particularly an iron ion, having redox properties. Among these, montmorillonite, a type of smectite, is preferable from the viewpoint of coating suitability and gas barrier properties. As the montmorillonite, a known compound that has been used in gas barrier agents can be used. For example, the following general formula: (X,Y)2~3Z4O10(OH)2·mH2O·(Wω) (In the formula, X represents Al, Fe(III), or Cr(III). Y represents Mg, Fe(II), Mn(II), Ni, Zn, or Li. Z represents Si or Al. W represents K, Na, or Ca. HO represents interlayer water. m and ω represent positive real numbers.) Among these, those in which W in the formula is Na are preferred because they cleave in an aqueous medium.

[0039] The size and shape of the inorganic layered compound are not particularly limited, but the particle size (major axis) is preferably 5 μm or less, more preferably 4 μm or less, and even more preferably 3 μm or less. If the particle size is larger than 5 μm, the dispersibility is poor, and as a result, the coatability of the organic resin layer and the coat appearance may be deteriorated. On the other hand, the aspect ratio is 50 to 5000, more preferably 100 to 4000, and even more preferably 200 to 3000.

[0040] In the present invention, the arithmetic mean roughness of the organic resin layer in a 2 μm square field of view using an atomic force microscope is preferably 2.0 to 8.0 nm. This allows the uniformity of the organic resin layer to be maintained and stable barrier performance to be expressed, while the formation of surface irregularities mainly derived from the coordination of inorganic layered particles can improve adhesion and blocking resistance. The arithmetic mean roughness is preferably 2.5 nm or more, more preferably 3.0 nm or more, and even more preferably 3.5 nm or more, and is preferably 7.5 nm or less, more preferably 7.0 nm or less, and even more preferably 6.5 nm or less. If the arithmetic mean roughness exceeds 8.0 nm, the surface becomes too rough and the uniformity of the organic resin layer also decreases, so that unevenness and defects occur in the coat appearance, which may decrease the printability, adhesion, and barrier properties. On the other hand, if the arithmetic mean roughness is less than 2.0 nm, the surface is too flat, which may decrease adhesion, ink transfer during printing, and the like. In addition, the blocking resistance described later also deteriorates, and blocking may occur when the film is wound into a roll. In order to achieve an arithmetic mean roughness value within the specified numerical range, it is necessary to use the materials described above in the specified deposition amount, and further to set the compounding ratio of the materials within the appropriate range described above in combination with the dilution conditions of the coating liquid and the drying and heat treatment conditions described below.

[0041] In the present invention, the Martens hardness when the organic resin layer side surface of the laminated film is measured with a test force of 0.1 mN is 248 N / mm 2 It is preferable that the resistance is less than or equal to 245 N / mm 2 or less, and more preferably 240 N / mm 2 or less, and particularly preferably 235 N / mm2 or less, most preferably 230N / mm 2 However, to prevent problems such as winding around the roll during processing and blocking of the roll itself, the maximum allowable load is 160N / mm 2 It is preferable that the value does not fall below this. Martens hardness is 248N / mm 2 If it exceeds this value, the surface becomes hard, the conformability of the resin surface during processing becomes poor, the adhesive strength decreases, and there is a high possibility that defects such as delamination of the laminate film will occur. In order to set the Martens hardness value within the above-mentioned predetermined range, it is necessary to use the above-mentioned materials and set the above-mentioned coating amount within the above-mentioned predetermined range.

[0042] In the organic resin layer of the present invention, various crosslinking agents may be blended in order to improve the cohesive strength and the moisture-heat-resistant adhesion of the film, as long as the gas barrier properties and productivity are not impaired. Examples of crosslinking agents include silicon-based crosslinking agents, oxazoline compounds, carbodiimide compounds, epoxy compounds, isocyanate compounds, and the like. Among them, silicon-based crosslinking agents are particularly preferred from the viewpoint of improving the water-resistant adhesion to the inorganic thin film layer by blending the silicon-based crosslinking agent. In addition, oxazoline compounds, carbodiimide compounds, epoxy compounds, and the like may be used in combination as crosslinking agents. However, when recycling is important, it is preferable not to blend a crosslinking agent.

[0043] In the present invention, the film haze after lamination of the organic resin layer is preferably 10% or less, more preferably 8% or less, and even more preferably 6% or less, from the viewpoint of visibility of the contents. If the haze is more than 10%, the transparency is significantly deteriorated, and there is a concern that it may affect the unevenness of the surface, which may lead to poor appearance in the subsequent printing process. The haze can be adjusted by the composition ratio of the organic resin layer, the solvent conditions, the film thickness, etc. Here, the haze was evaluated in accordance with JIS K7136 using a turbidity meter (manufactured by Nippon Denshoku, NDH2000).

[0044] The method of coating the resin composition for the organic resin layer is not particularly limited as long as it is a method for forming a layer by coating the resin composition on the film surface. For example, a typical coating method such as gravure coating, reverse roll coating, wire bar coating, or die coating can be used.

[0045] When forming an organic resin layer, it is preferable to apply a resin composition for an organic resin layer, pre-dry it at a relatively low temperature to evaporate the solvent, and then dry it at a high temperature, since this will give a uniform film. The pre-drying temperature is preferably 80 to 110°C, more preferably 85 to 105°C, and even more preferably 90 to 100°C. If the pre-drying temperature is less than 80°C, the organic resin layer may not be sufficiently dried. If the pre-drying temperature is higher than 110°C, the organic resin layer may dry before it spreads, resulting in poor appearance.

[0046] On the other hand, the main drying temperature is preferably 110 to 140°C, more preferably 115 to 135°C, and even more preferably 120 to 130°C. If the main drying temperature is less than 110°C, the film formation of the organic resin layer does not proceed, and the cohesive strength and adhesiveness decrease, which may result in a negative effect on the barrier properties. If the temperature exceeds 140°C, the film may become too hot, making it brittle, or wrinkles due to heat shrinkage may become large.

[0047] The drying time for the preliminary drying is preferably 3.0 to 10.0 seconds, more preferably 3.5 to 9.5 seconds, and even more preferably 4.0 to 9.0 seconds. The drying time for the main drying is preferably 3.0 to 10.0 seconds, more preferably 3.5 to 9.5 seconds, and even more preferably 4.0 to 9.0 seconds. However, care must be taken because the drying conditions vary depending on the type of heat medium and the intake and exhaust conditions of the drying furnace. In addition to the drying, it is also more effective to perform an additional heat treatment for 1 to 4 days in a temperature range as low as possible, specifically, in a temperature range of 40 to 60°C, in order to advance the film formation of the organic resin layer.

[0048] [Packaging materials] When the laminated film of the present invention is used as a packaging material, it is preferable to form a laminate having a heat-sealable resin layer called a sealant. The heat-sealable resin layer is usually provided on an organic resin layer, but may also be provided on the outside of the base film layer (the surface opposite to the surface on which the organic resin layer is formed). The heat-sealable resin layer is usually formed by extrusion lamination or dry lamination. The thermoplastic polymer forming the heat-sealable resin layer may be any polymer capable of sufficiently exhibiting sealant adhesion, and may be, for example, polyethylene resins such as olefin-based HDPE, LDPE, and LLDPE, polypropylene resins, ethylene-vinyl acetate copolymers, ethylene-α-olefin random copolymers, and ionomer resins. Among these, LLDPE or polypropylene resins, which are highly versatile in terms of durability, seal strength, cost, and mono-materialization, are particularly preferable. The thickness of the sealant layer is preferably 20 to 100 μm, more preferably 30 to 90 μm, and even more preferably 40 to 80 μm. If the thickness is less than 20 μm, sufficient seal strength may not be obtained, or the sealant may lack stiffness and be difficult to handle. On the other hand, if the thickness exceeds 100 μm, the bag will feel stiff and will be difficult to handle, and the price may also become high.

[0049] [Adhesive layer] The adhesive layer used in the present invention can be a general-purpose adhesive for lamination. For example, (non-)solvent, water-based, or hot melt adhesives mainly composed of poly(ester)urethane, polyester, polyamide, epoxy, poly(meth)acrylic, polyethyleneimine, ethylene-(meth)acrylic acid, polyvinyl acetate, (modified) polyolefin, polybutadiene, wax, or casein can be used. Among these, urethane or polyester adhesives are preferred in consideration of heat resistance and flexibility that can follow the dimensional changes of each substrate. The adhesive layer can be laminated by, for example, direct gravure coating, reverse gravure coating, kiss coating, die coating, roll coating, dip coating, knife coating, spray coating, fountain coating, or other methods, and the coating amount after drying is preferably 1 to 8 g / m2 in order to develop sufficient adhesiveness. More preferably, it is 2 to 7 g / m2. 2 , and more preferably 3 to 6 g / m 2 The coating amount is 1g / m 2 If it is less than 8g / m, it becomes difficult to bond the entire surface, and the adhesive strength decreases. 2 If the thickness exceeds the above range, it takes a long time for the film to completely harden, unreacted materials are likely to remain, and the adhesive strength decreases. When using a conventional general polypropylene film, an adhesive layer with a thickness of about 2 to 3 μm is required to exhibit sufficient adhesive strength, but the product of the present invention can exhibit the same or higher adhesive strength even with an adhesive layer thickness of 1 / 3 to 1 / 2 of this. In other words, by using the product of the present invention, it is possible to reduce the amount of adhesive used.

[0050] Furthermore, in the laminate film of the present invention, at least one printed layer or other plastic substrate and / or paper substrate may be laminated between the substrate film layer and the heat-sealable resin layer or on the outer side thereof.

[0051] As the printing ink for forming the printing layer, water-based and solvent-based resin-containing printing inks can be preferably used. Examples of the resin used in the printing ink include acrylic resins, urethane resins, polyester resins, vinyl chloride resins, vinyl acetate copolymer resins, and mixtures thereof. The printing ink may contain known additives such as antistatic agents, light blocking agents, ultraviolet absorbers, plasticizers, lubricants, fillers, colorants, stabilizers, lubricants, defoamers, crosslinking agents, anti-blocking agents, and antioxidants. The printing method for providing the printing layer is not particularly limited, and known printing methods such as offset printing, gravure printing, and screen printing can be used. To dry the solvent after printing, known drying methods such as hot air drying, hot roll drying, and infrared drying can be used.

[0052] The laminate of the present invention has an oxygen permeability of 10 mL / m under conditions of 23°C x 65% RH. 2 In order to achieve good gas barrier properties, it is preferable that the gas barrier pressure is 5 mL / m or less by controlling the organic resin layer components and the deposition amount. 2 d MPa or less, preferably 3mL / m 2 ·d·MPa or less. Oxygen permeability is 10mL / m 2 If it exceeds 1.5 MPa, it becomes difficult to meet the requirements for applications that require high gas barrier properties.

[0053] The laminate of the present invention has a water vapor permeability of 3 g / m2 under conditions of 40°C x 90% RH. 2 In terms of exhibiting good gas barrier properties, it is preferable that the thickness is 2 g / m or less. Furthermore, by controlling the amount of the organic resin layer component attached, it is possible to obtain a thickness of 2 g / m or less. 2 d or less, preferably 1 g / m 2 d or less. The water vapor permeability is 3g / m 2 If it exceeds ·d, it becomes difficult to meet the requirements for applications that require high gas barrier properties. The laminate of the present invention has an oxygen permeability of 15 mL / m under conditions of 23°C x 80% RH. 2In order to achieve good gas barrier properties, it is preferable that the gas barrier pressure is 10 mL / m or less by controlling the amount of the organic resin layer component and ... 2 ·d·MPa or less, preferably 5mL / m 2 ·d·MPa or less. Oxygen permeability is 15mL / m 2 If it exceeds 1.5 MPa, it becomes difficult to meet the requirements for applications that require high gas barrier properties.

[0054] The laminate of the present invention preferably has a laminate strength of 1.0 N / 15 mm or more under conditions of 23°C x 65% RH, more preferably 1.5 N / 15 mm or more, and even more preferably 2.0 N / 15 mm or more. If the laminate strength is less than 1.0 N / 15 mm, peeling may occur due to bending load or heat during sealing, resulting in deterioration of barrier properties or leakage of contents. Furthermore, there is a risk of deterioration in hand tearability. EXAMPLES

[0055] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to the following examples. The films were evaluated by the following measurement methods.

[0056] (1) Thickness of laminated film The measurement was performed using a dial gauge in accordance with JIS K7130-1999 Method A.

[0057] (2) Haze of laminated film The measurement was performed using a haze meter NDH-2000 (manufactured by Nippon Denshoku Industries Co., Ltd.) in accordance with JIS K7136.

[0058] (3) Adhesion amount of organic resin layer In each of the Examples and Comparative Examples, each laminate film obtained at the stage of laminating an organic resin layer onto a base film was used as a sample, and a test piece of 100 mm × 100 mm was cut out from this sample, and the organic resin layer was wiped off with ethanol. The amount of adhesion was calculated from the change in mass of the film before and after wiping.

[0059] (1) Measurement method for Martens hardness (N / mm2) The obtained laminated film was cut into approximately 2 cm squares, and the surface opposite to the organic resin layer side (measurement surface) was fixed with an adhesive on a glass plate with a thickness of approximately 1 mm, and then left in an atmosphere of 23°C and 50% RH for 12 hours to condition the humidity. This sample was measured using a dynamic ultra-microhardness tester (Shimadzu Corporation's "DUH-211") under the following measurement conditions according to the method of ISO14577-1 (2002). The measurement was performed 10 times by changing the position of the film, and the average value of 8 points excluding the maximum and minimum was calculated. <Measurement conditions> (setting) Measurement environment: Temperature 23°C, relative humidity 50% Test mode: Load-unload test ·Indenter used: ridge angle 115 degrees, triangular pyramid indenter Indentation modulus: 1.140×106N / mm 2 Indenter Poisson's ratio: 0.07 Cf-Ap,As correction: Yes Test force: 0.10mN ·Load speed: 0.0050mN / sec ·Load holding time: 5sec ·Unloading holding time: 0sec The Martens hardness was calculated from the slope (m) of the test force vs. indentation depth curve, where the depth between 50% F and 90% F (F = 0.10 mN) of the test force is proportional to the square root of the test force, using the following formula (1). Martens hardness HMs=1 / (26.43×m 2 ) ····(1)

[0060] (6) Measurement method for arithmetic mean roughness of organic resin layer The surface roughness of the laminated film was measured using a scanning probe microscope (SPM) (Shimadzu Corporation "SPM9700") (cantilever: OMCL-AC200TS provided by Olympus Corporation, observation mode: phase mode). In detail, an SPM image was obtained with a viewing angle of 2 μm square on the film surface. The obtained image was used to correct the tilt in the X, Y, and Z directions using the tilt correction function of the software attached to the SPM, and the arithmetic mean roughness value was calculated. The arithmetic mean roughness was calculated by extracting only a reference length in the direction of the average line from the roughness curve obtained by removing surface waviness components longer than a specified wavelength from the cross-sectional curve using a high-pass filter, taking the X axis in the direction of the average line of the extracted part and the Y axis in the direction of the longitudinal magnification, and expressing the roughness curve as y = f(X), and expanding the value obtained by the following formula into two dimensions. Ra=1 / L∫L0 |f(x)|dx L: Reference length

[0061] (7) Evaluation method for oxygen permeability In each of the Examples and Comparative Examples, the laminated films obtained at the stage of laminating the organic resin layer on the substrate film were used as samples, and oxygen permeability was measured under two atmospheric conditions of temperature 23°C, humidity 65% ​​RH and temperature 23°C, humidity 80% RH using an oxygen permeability measuring device ("OX-TRAN (registered trademark) 1 / 50" manufactured by MOCON) in accordance with JIS-K7126 Method B. The oxygen permeability was measured in the direction in which oxygen permeates from the substrate film side to the organic resin layer side.

[0062] (8) Method for evaluating water vapor permeability In each of the Examples and Comparative Examples, the laminated films obtained at the stage of laminating the organic resin layer on the substrate film were used as samples, and the water vapor permeability was measured in an atmosphere at a temperature of 40° C. and a humidity of 90% RH using a water vapor permeability measuring device ("PERMATRAN-W 3 / 33MG" manufactured by MOCON) in accordance with JIS-K7129 Method B. The water vapor permeability was measured in the direction in which water vapor permeates from the substrate film side to the organic resin layer side.

[0063] (9) Evaluation of blocking resistance of laminated film In each Example and Comparative Example, each laminated film obtained at the stage of laminating an organic resin layer on a base film was used as a sample, and two sets of samples cut into strips 15 mm wide and 200 mm long were prepared, and one drop of water (about 0.02 g) was dropped onto the organic resin layer surface of one sample, and then the organic resin layer surface of the other sample was placed on top of the other sample, sandwiched between glass plates, and dried at 40°C for 24 hours to evaporate the water, and the two strips were peeled off to check the adhesion state of the film. Those that were so adhered that the film was torn when peeled off were judged as ×, and those that could be peeled off smoothly without tearing were judged as ◯.

[0064] (10) Evaluation of solvent volatility in organic resin layers In each of the Examples and Comparative Examples, each laminate film obtained at the stage of laminating an organic resin layer onto a base film was used as a sample, and when the organic resin layer was lightly pressed with a paper towel, if the organic resin layer adhered to the paper towel, it was judged as X, indicating insufficient solvent evaporation, and if the organic resin layer did not adhere to the paper towel, it was judged as O, indicating sufficient solvent evaporation.

[0065] (11) Appearance evaluation of organic resin layer In each example and comparative example, each laminate film obtained at the stage of laminating an organic resin layer on a base film was used as a sample. Films in which missing parts, streaks, unevenness, etc. in the organic resin layer were visually observed were judged to have a poor appearance and rated as ×, and films in which there were no such defects were judged to have a good appearance and rated as ◯.

[0066] [Preparation of laminated body] An ester-based adhesive (TM569 / CAT10L manufactured by Toyo-Morton Co., Ltd.) was applied onto the laminates obtained in the Examples and Comparative Examples, and then an unstretched polypropylene film (P1128 manufactured by Toyobo Co., Ltd.; thickness 30 μm; referred to as CPP) was dry laminated on a metal roll heated to 60°C. The laminate was then aged at 40°C for 4 days to obtain a laminate gas barrier laminate for evaluation. The laminate A was coated so that the thickness of the adhesive after drying would be 3 μm, the laminate B was coated so that the thickness of the adhesive after drying would be 1.5 μm, and the laminate C was coated so that the thickness of the adhesive after drying would be 0.8 μm.

[0067] (12) Evaluation method for laminate strength The laminated laminates A to C prepared above were cut into test pieces with a width of 15 mm and a length of 200 mm, and the laminate strength (normal state) was measured using a Tensilon universal material testing machine (Tensilon UMT-II-500 type, manufactured by Toyo Baldwin Co., Ltd.) under conditions of a temperature of 23° C. and a relative humidity of 65%. The laminate strength was measured at a tensile speed of 200 mm / min, and the strength was measured when the laminated film layer and the heat-sealable resin layer of each laminated film obtained in the examples and comparative examples were peeled off at a peel angle of 90 degrees.

[0068] [Inorganic thin film layer] The method for producing the inorganic thin film layer used in each of the Examples and Comparative Examples is described below. The method was used in Examples 1 to 7 and Comparative Examples 1 to 4 and 8, and is shown in Table 2. In Comparative Examples 5 to 7, no inorganic thin film layer was laminated.

[0069] (Formation of inorganic thin film layer M-1) Aluminum oxide was vapor-deposited on the base film layer as the inorganic thin film layer M-1. The method of vapor-depositing aluminum oxide on the base film layer was to set the film on the unwinding side of a continuous vacuum deposition machine, run it over a cooled metal drum, and wind the film. At this time, the continuous vacuum deposition machine was depressurized to 10-4 Torr or less, and 99.99% pure aluminum metal was loaded into an alumina crucible from the bottom of the cooling drum, and the aluminum metal was heated and evaporated. Oxygen was supplied to the vapor to cause an oxidation reaction, which was then deposited on the film, forming an aluminum oxide film with a thickness of 10 nm.

[0070] (Formation of inorganic thin film layer M-2) As the inorganic thin film layer M-2, a composite oxide layer of silicon dioxide and aluminum oxide was formed on the substrate film layer by electron beam deposition. 2 (99.9% purity) and A1 2 O 3 (99.9% purity) was used. The inorganic thin film layer (SiO 2 / A1 2 O 3 The thickness of the composite oxide layer was 13 nm. The composition of this composite oxide layer was SiO 2 / A1 2 O 3 The mass ratio was 60 / 40.

[0071] The coating fluids used in the present examples and comparative examples are described in detail below. The coating fluids used in the present examples and comparative examples are shown in Table 2.

[0072] [Polyvinyl alcohol resin solution (A)] To 90 parts by mass of purified water, 10 parts by mass of fully saponified polyvinyl alcohol resin (manufactured by Nippon Synthetic Chemical Industry Co., Ltd., product name: G Polymer OKS8049Q, (saponification degree 99.0% or more, average polymerization degree 450) was added, and the mixture was heated to 80°C with stirring, and then stirred for about 1 hour. The mixture was then cooled to room temperature, and a nearly transparent polyvinyl alcohol solution (PVA solution) with a solids content of 10% was obtained.

[0073] [Inorganic layered compound dispersion (B)] 5 parts by mass of montmorillonite (trade name: Kunipia F, manufactured by Kunimine Industries Co., Ltd.), which is an inorganic layered compound, was added to 95 parts by mass of purified water while stirring, and thoroughly dispersed with a homogenizer set at 1500 rpm. After that, the mixture was kept at 23°C for 1 day to obtain an inorganic layered compound dispersion liquid with a solid content of 5%. [EVOH resin solution (C)] 10 parts by mass of ethylene-vinyl alcohol copolymer (EVOH) resin (manufactured by Kuraray Co., Ltd., product name: L171B, (ethylene content 27 mol%)) was added to a mixed solution of 40 parts by mass of purified water and 50 parts by mass of isopropyl alcohol, and the mixture was heated to 80°C with stirring and then stirred for about 1 hour. The mixture was then cooled to room temperature, thereby obtaining an EVOH solution with a solid content of 10%.

[0074] [Coating Solution 1 Used for Organic Resin Layer in Example 1] The materials were mixed in the following mixing ratio to prepare a coating liquid (resin composition for organic resin layer). Ion-exchanged water 20.00% by mass Isopropyl alcohol 15.00% by mass Polyvinyl alcohol resin solution (A) 35.00% by mass Inorganic layered compound separation liquid (B) 30.00% by mass

[0075] [Coating Solution 2 used for organic resin layer in Examples 2, 3, 6, 7 and Comparative Examples 3 to 5 and 8] The materials were mixed in the following mixing ratio to prepare a coating liquid (resin composition for organic resin layer). Ion-exchanged water 15.00% by mass Isopropyl alcohol 15.00% by mass Polyvinyl alcohol resin solution (A) 30.00% by mass Inorganic layered compound separation liquid (B) 40.00% by mass

[0076] [Coating Solution 3 Used for Organic Resin Layer in Example 4] The materials were mixed in the following ratio to prepare a coating liquid (resin composition for organic resin layer). Ion-exchanged water 10.00% by mass Isopropyl alcohol 15.00% by mass Polyvinyl alcohol resin solution (A) 25.00% by mass Inorganic layered compound separation liquid (B) 50.00% by mass

[0077] [Coating Solution 4 used for organic resin layer in Example 5 and Comparative Example 7] The materials were mixed in the following ratio to prepare a coating liquid (resin composition for organic resin layer). Ion-exchanged water 27.50% by mass Isopropyl alcohol 15.00% by mass EVOH resin solution (C) 42.50% by mass Inorganic layered compound separation liquid (B) 15.00% by mass

[0078] [Coating Solution 5 used for Organic Resin Layer in Comparative Example 1] The materials were mixed in the following ratio to prepare a coating liquid (resin composition for organic resin layer). Ion-exchanged water 35.00% by mass Isopropyl alcohol 15.00% by mass Polyvinyl alcohol resin solution (A) 50.00% by mass

[0079] [Coating Solution 6 used for Organic Resin Layer in Comparative Example 2] The materials were mixed in the following ratio to prepare a coating liquid (resin composition for organic resin layer). Ion-exchanged water 30.00% by mass Isopropyl alcohol 15.00% by mass Polyvinyl alcohol resin solution (A) 45.00% by mass Inorganic layered compound separation liquid (B) 10.00% by mass

[0080] [Coating Solution 7 Used for Organic Resin Layer in Comparative Example 6] The materials were mixed in the following ratio to prepare a coating liquid (resin composition for organic resin layer). Ion-exchanged water 35.00% by mass Isopropyl alcohol 15.00% by mass EVOH resin solution (C) 50.00% by mass

[0081] (Coating a coating liquid onto a film (laminating an organic resin layer)) The coating liquid prepared above was applied by gravure roll coating to the surface on which the inorganic thin film layer was laminated or to the corona-treated surface of the substrate film on which the inorganic thin film layer was not laminated, and the coating was pre-dried at 90°C for 4 seconds, and then dried at 130°C for 4 seconds to obtain an organic resin layer. The adhesion amount of the organic resin layer E after drying was as shown in Table 2. Then, a post-heat treatment was performed at 40°C for 2 days. The coating liquid constituting the organic resin layer, and the temperature of the main drying and the post-heat treatment conditions were changed as shown in Table 2 in each Example and Comparative Example.

[0082] In this manner, a laminate film having an organic resin layer on a substrate film was produced. In the substrates of Examples 1 to 6 and Comparative Examples 1 to 7, the substrate layer (A) was made of polypropylene homopolymer PP-1 shown in Table 1. The surface layer (B) was made of a blend of 43.2% by weight of polypropylene homopolymer PP-2 shown in Table 1, 52.0% by weight of ethylene copolymerized polypropylene polymer PP-4 shown in Table 1, and 4.8% by weight of antiblocking agent-containing master batch FTX0627G. In this case, the melt flow rate (g / 10 min) of the polypropylene resin composition constituting the surface layer (B) was 5.1. For the surface layer (C), a mixture of 93.6% by weight of polypropylene homopolymer PP-1 shown in Table 1 and 6.4% by weight of antiblocking agent-containing master batch FTX0627G was used. The base layer (A) was extruded with a 45 mm extruder, the surface layer (B) with a 25 mm extruder, and the surface layer (C) with a 20 mm extruder. The raw resins were melted at 250 ° C. and co-extruded from a T-die into a sheet shape, and the surface layer (B) was cooled and solidified so that it contacted a cooling roll at 30 ° C., and then stretched 4.5 times in the machine direction (MD) at 135 ° C. Next, in a tenter, both ends of the film in the transverse direction (TD) were clamped with clips, preheated at 173 ° C., stretched 8.2 times in the transverse direction (TD) at 164 ° C., and heat-set at 171 ° C. while relaxing 6.7% in the transverse direction (TD). In this way, a biaxially oriented polypropylene film having a structure of surface layer (B) / base layer (A) / surface layer (C) was obtained.

[0083] The surface of the surface layer (B) of the biaxially oriented polypropylene film was corona-treated using a corona treatment machine manufactured by Softal Corona & Plasma GmbH at an applied current value of 0.75 A, and then wound up with a winder. The thickness of the obtained film was 20 μm (thicknesses of surface layer (B) / base layer (A) / surface layer (C) were 1.3 μm / 17.7 μm / 1.0 μm). The Martens hardness of the surface layer (B) was 248 N / mm 2 The following biaxially oriented polypropylene film was used. The obtained laminated film was evaluated. The results are shown in Table 2. In Example 7, the anchor coat layer was formed on the surface layer (B) of the substrate of Example 1 by gravure roll coating using Coating Solution 1 shown below, and then dried at 130° C. for 10 seconds. The adhesion amount of the anchor coat layer was 0.40 g / m 2 It was.

[0084] [Coating fluid 1] Silane coupling agent; N-2-(aminoethyl)-3-aminopropyltrimethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., "KBM-603") 0.25 parts by mass was dissolved in 1.48 parts by mass of acetone, and 4.07 parts by mass of isocyanate; trimethylolpropane adduct of meta-xylylene diisocyanate (manufactured by Mitsui Chemicals, Inc., "Takenate D-110N": solid content 75%) was mixed and stirred for 10 minutes using a magnetic stirrer. The obtained mixed solution was diluted with 69.55 parts by mass of methyl ethyl ketone and 14.03 parts by mass of 1-methoxy-2-propanol (hereinafter referred to as PGM), and 10.62 parts by mass of polyester resin (manufactured by DIC Corporation, DF-COAT GEC-004C: solid content 30%) was added to obtain the target coating solution 1. In Comparative Example 8, Pylen Film P2102 manufactured by Toyobo Co., Ltd., a film having a thickness of 20 μm was used.

[0085] [Table 1]

[0086] [Table 2A]

[0087] [Table 2B] [Industrial Applicability]

[0088] According to the present invention, it is possible to provide a laminate film that can form a laminate structure composed of almost a single resin type, mainly polypropylene film, which has a low environmental impact, and that has the necessary performance of gas barrier properties and adhesiveness required for packaging materials. Moreover, since the laminate film of the present invention has few processing steps and is excellent in processability and can be easily produced, it is excellent in both economy and production stability, and a gas barrier film with uniform properties can be provided.

Claims

1. A surface layer (B) is provided on one surface of a substrate layer (A) mainly composed of a polypropylene resin. A surface layer (C) is provided on the other surface of the layer (A), and an inorganic thin film layer (D) is provided on the surface layer (B). The laminated film is formed by laminating an inorganic thin film layer (D) on which an organic resin layer (E) is further laminated. and satisfying the following requirements (a) to (d): (a) The coating amount of the organic resin layer (E) is 0.10 g / m 2 0.50g / m or more 2 The following is and. (b) The martensite when the organic resin layer side surface of the laminated film is measured with a test force of 0.1 mN The hardness is 248N / mm 2 It is less than or equal to. (c) the haze of the laminated film is 6% or less. (d) The oxygen permeability of the laminated film in an environment of 23°C x 65% RH is 10 mL / m 2 - d - MPa or less.

2. Water vapor permeability at 40°C x 90% RH is 1g / m 2 ・Characterized as being d or less The packaging laminate film according to claim 1 .

3. The oxygen permeability of the laminated film in an environment of 23°C x 80% RH is 15 mL / m 2 3. The packaging laminate film according to claim 1, wherein the compressive strength is 0.05 -d-MPa or less.

4. 4. The packaging laminate film according to claim 1, wherein the organic resin layer on the laminate film has an arithmetic mean roughness in a 2 μm square range of 2.0 to 8.0 nm.

5. 5. The packaging laminate film according to claim 1, wherein the thickness of the laminate film is from 9 μm to 200 μm.

Citation Information

Patent Citations

  • Gas barrier film and its production

    JP1997111017A

  • Gas barrier polypropylene based laminate film

    JP2008230153A

  • Laminated film

    JP2017226776A

  • Laminate film of barrier properties and its manufacture

    JP1992345841A

  • Composite film and production thereof

    JP1992359033A