Multi-layered structure and liquid paper container
The multilayer structure with a paper layer, inorganic vapor deposition, and ethylene-vinyl alcohol copolymer barrier resin addresses gas barrier and strength issues in paper containers, ensuring effective performance and recyclability.
Patent Information
- Application Number
- JP2024125472
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-12-05
- Filing Date
- 2024-07-31
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-12-05
AI Technical Summary
Paper containers for beverages and liquids face challenges in maintaining high gas barrier properties, especially in bent portions, and require sufficient strength to prevent leakage in low-temperature environments, while also being recyclable without defects.
A multilayer structure comprising a paper layer, an inorganic vapor deposition layer, a barrier resin layer made of ethylene-vinyl alcohol copolymer, an adhesive resin layer, and a moisture-proof resin layer, with specific thickness and composition ranges, ensuring high gas barrier properties and strength even after bending, and minimizing defects during recycling.
The multilayer structure maintains high gas barrier properties and sufficient strength in both unfolded and folded states, particularly in low-temperature conditions, and reduces defects during recycling, enhancing the recyclability of paper containers.
Smart Images

Figure 2024149613000001 
Figure 2024149613000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a multi-layer structure and a liquid paper container. [Background technology]
[0002] Paper containers are widely used as containers for containing beverages such as milk and juice, liquid foods such as soup, alcoholic beverages such as sake and shochu, and various other non-food liquids. From the viewpoints of barrier properties, heat sealability, and the like, multilayer structures in which a resin layer, a vapor deposition layer, a metal foil, and the like are laminated on a paper layer are widely used as materials for paper containers. Patent Document 1 describes a paper container formed from a multilayer structure in which a synthetic resin layer, etc. is laminated on one side of a base material mainly made of a paper layer, and an intermediate layer made of a linear low-density polyethylene resin, a barrier layer, and a sealant layer are laminated in this order on the other side of the base material. For the barrier layer of the multilayer structure in Patent Document 1, a vapor deposition film in which an inorganic substance is vapor-deposited on a polyethylene terephthalate resin film is used. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2004-250025 A Summary of the Invention [Problem to be solved by the invention]
[0004] Paper containers for storing beverages and the like are required to have high gas barrier properties from the viewpoint of maintaining quality. In particular, because paper containers are formed by folding a multilayer structure including a paper layer and heat sealing it, etc., the gas barrier properties are easily reduced due to pinholes occurring at the bent parts. In addition, when beverages and the like stored in the paper containers are transported in a low-temperature environment, the paper containers are required to have sufficient strength to withstand vibrations, drops, etc., so that leakage does not occur from heat-sealed parts, etc.
[0005] Furthermore, packaging materials such as paper containers are desired to be materials that are easy to collect and reuse (high recyclability). However, in a multilayer structure in which various resin layers and the like are provided in addition to a paper layer, when the resin layers from which the paper layers have been removed are melt-molded, defects may occur in the resulting recycled product (melt-molded product) due to differences in the melting temperatures of the resins, cross-linking reactions of the resins, and the like, resulting in a deterioration in appearance and quality.
[0006] The present invention has been made based on the above circumstances, and its object is to provide a multilayer structure that has high gas barrier properties both before and after folding, can be used to form a paper container with sufficient strength even in a low-temperature environment, and suppresses the occurrence of defects during recycling, and a liquid paper container using such a multilayer structure. [Means for solving the problem]
[0007] The above objectives are: [1] A multilayer structure having a paper layer (A), an inorganic vapor deposition layer (B), a barrier resin layer (C), an adhesive resin layer (D) and a moisture-proof resin layer (E), in which the inorganic vapor deposition layer (B), the barrier resin layer (C), the adhesive resin layer (D) and the moisture-proof resin layer (E) are all directly laminated in this order, the inorganic vapor deposition layer (B) has an average thickness of 5 nm to 200 nm, the barrier resin layer (C) contains as a main component an ethylene-vinyl alcohol copolymer (c) having an ethylene unit content of 20 mol % to 50 mol % and a saponification degree of 90 mol % or more, the adhesive resin layer (D) contains as a main component an adhesive resin (d), and the moisture-proof resin layer (E) contains as a main component polyethylene (e), and does not contain a layer containing as a main component a resin having a melting point of 200°C or more and a metal layer having an average thickness of 1 μm or more; [2] The multilayer structure of [1], further comprising a thermoplastic resin layer (X) interposed between the paper layer (A) and the inorganic vapor deposition layer (B) or the moisture-proof resin layer (E); [3] A multilayer structure according to [1] or [2], having a paper layer (A), an inorganic vapor deposition layer (B), a barrier resin layer (C), an adhesive resin layer (D) and a moisture-proof resin layer (E) in this order; [4] The multilayer structure of any one of [1] to [3], wherein the adhesive resin (d) is an acid-modified polyethylene; [5] The multilayer structure according to any one of [1] to [4], wherein the inorganic vapor-deposited layer (B) is a metal vapor-deposited layer mainly composed of aluminum or an inorganic oxide vapor-deposited layer mainly composed of alumina or silica; [6] The multilayer structure of any of [1] to [5], wherein the barrier resin layer (C) contains 10 ppm or more and 200 ppm or less of at least one polyvalent metal ion selected from the group consisting of magnesium ions, calcium ions, and zinc ions; [7] The multilayer structure of any one of [1] to [6], wherein the ethylene-vinyl alcohol copolymer (c) contains two or more ethylene-vinyl alcohol copolymers having different ethylene unit contents; [8] The density of polyethylene (e) is 0.880 g / cm 3 More than 0.940g / cm 3 The multilayer structure of any of [1] to [7], wherein the polyethylene (e) is a linear low-density polyethylene, a low-density polyethylene, or a mixture thereof; [9] The multilayer structure of any of [1] to [8], wherein a laminate of the barrier resin layer (C), the adhesive resin layer (D) and the moisture-proof resin layer (E) is a coextruded film, the average thickness of the coextruded film is 8 μm or more and 120 μm or less, and an inorganic vapor deposition layer (B) is provided on the surface of the coextruded film on the barrier resin layer (C) side;
[10] The multilayer structure of [9], wherein the average thickness of the barrier resin layer (C) is 0.2 μm or more and less than 30 μm, and the ratio of the average thickness of the barrier resin layer (C) to the average thickness of the coextruded film is less than 25%;
[11] The multilayer structure of [9] or
[10] , wherein the coextruded film is substantially unstretched;
[12] The multilayer structure of [9] or
[10] , wherein the coextruded film is stretched at least uniaxially by a factor of 3 or more but less than 12;
[13] The multilayer structure of [9] or
[10] , wherein the coextruded film is biaxially stretched by at least 3 times but less than 12 times;
[14] The multilayer structure of any one of [9] to
[13] , further comprising a moisture-proof resin layer (F) containing polyethylene (f) as a main component;
[15] The density of polyethylene (f) is 0.880 g / cm 3 More than 0.940g / cm 3 The multilayer structure of
[14] , wherein the polyethylene (f) is a linear low density polyethylene, a low density polyethylene, or a mixture thereof;
[16] The multilayer structure of
[14] or
[15] , in which a moisture-proof resin layer (F) is directly laminated on the coextruded film;
[17] Any of the multilayer structures of [1] to
[16] , which does not have an adhesive layer made of a curable adhesive;
[18] The basis weight of the paper layer (A) is 200 g / m 2 More than 400g / m 2 any of the multilayer structures of [1] to
[17] , wherein the multilayer structure is less than
[19] Any of the multilayer structures of [1] to
[18] , in which the mass ratio of the paper layer (A) to the entire multilayer structure is 0.60 or more;
[20] The multilayer structure of any one of [1] to
[19] , wherein the total average thickness ratio of layers containing a polyethylene resin as a main component in the portion other than the paper layer (A) is 0.75 or more;
[21] The multilayer structure of any of [1] to
[20] , wherein the total average thickness ratio of layers mainly composed of a resin having ethylene units in a portion other than the paper layer (A) is 0.95 or more;
[22] The multilayer structure of any one of [1] to
[21] , having a paper layer (A) on a surface thereof;
[23] The oxygen transmission rate measured according to the method described in JIS K 7126-2:2006 under conditions of 20°C and 65% RH is 0.5 cc / (m 2 A multilayer structure of any one of [1] to
[22] , in which the thermal conductivity is less than 100% (day·atm);
[24] The sheet is folded in four so that the paper layer (A) faces outward from the moisture-proof resin layer (E), and then a 5 kg load is applied from above and left to stand for one minute to perform a folding process. The oxygen transmission rate measured under conditions of 20°C and 65% RH according to the method described in JIS K 7126-2:2006 is 1.0 cc / (m 2A multilayer structure of any one of [1] to
[23] , in which the thermal conductivity is less than 100% (day·atm);
[25] A liquid paper container formed from any one of the multilayer structures of [1] to
[24] ; This is achieved by providing Effect of the Invention
[0008] According to the present invention, it is possible to provide a multilayer structure that has high gas barrier properties both before and after folding, can be used to form a paper container with sufficient strength even in a low-temperature environment, and suppresses the occurrence of defects when recycled, and a liquid paper container using such a multilayer structure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] <Multilayer structure> The multilayer structure of the present invention has a paper layer (A), an inorganic vapor deposition layer (B), a barrier resin layer (C), an adhesive resin layer (D) and a moisture-proof resin layer (E), the inorganic vapor deposition layer (B), the barrier resin layer (C), the adhesive resin layer (D) and the moisture-proof resin layer (E) are all directly laminated in this order, the inorganic vapor deposition layer (B) has an average thickness of 5 nm to 200 nm, the barrier resin layer (C) contains as a main component an ethylene-vinyl alcohol copolymer (c) having an ethylene unit content of 20 mol % to 50 mol % and a saponification degree of 90 mol % or more, the adhesive resin layer (D) contains as a main component an adhesive resin (d), the moisture-proof resin layer (E) contains as a main component polyethylene (e), and does not contain a layer containing as a main component a resin having a melting point of 200° C. or more and a metal layer having an average thickness of 1 μm or more. Hereinafter, the ethylene-vinyl alcohol copolymer will also be referred to as "EVOH".
[0010] The multilayer structure of the present invention has high gas barrier properties both before and after folding, and can form a paper container having sufficient strength even in a low-temperature environment, and the occurrence of defects during recycling is suppressed. The reason for this is unclear, but the following reason is presumed. The multilayer structure has a structure in which an inorganic vapor deposition layer (B) having a predetermined thickness and a barrier resin layer (C) mainly composed of EVOH, which has excellent gas barrier properties, are directly laminated, and therefore has high gas barrier properties both before and after folding. In addition, the multilayer structure has a moisture-proof resin layer (E) mainly composed of polyethylene (e). Therefore, a paper container having sufficient strength even in a low-temperature environment can be formed by, for example, heat-sealing this moisture-proof resin layer (E) to form a paper container. Furthermore, the occurrence of defects during recycling of the multilayer structure is suppressed because the thickness of the inorganic vapor deposition layer (B) is relatively thin, the barrier resin layer (C) and the moisture-proof resin layer (E) are composed mainly of specified resins, and the multilayer structure does not have a layer containing as its main component a resin having a melting point of 200°C or higher and a metal layer with an average thickness of 1 μm or more.
[0011] In this specification, the term "main component" refers to the component that is contained in the greatest amount by mass. The "average thickness" of each layer, etc. refers to the average value of thicknesses measured at any five points. "ppm" means the content by mass (ppm by mass). "Polyethylene" means a homopolymer of ethylene, a copolymer of 80 mol % or more ethylene and 20 mol % or less α-olefin monomer, and a copolymer of 90 mol % or more ethylene and less than 10 mol % of non-olefin monomers whose functional groups contain atoms other than carbon, oxygen, and hydrogen atoms. The term "acid-modified polyethylene" refers to a polymer obtained by modifying polyethylene with an acid. The acid-modified polyethylene may be a polymer in which at least one of an acid group and an acid anhydride group is introduced into polyethylene. "Polyethylene resin" refers to polyethylene and modified polyethylene (acid-modified polyethylene, etc.). Modified polyethylene refers to a polymer obtained by modifying polyethylene. In addition, the "surface" of the multilayer structure does not mean to distinguish between the front and back, but refers to the exposed surface. In other words, the multilayer structure has two surfaces. Similarly, the multilayer structure has two outermost layers.
[0012] Each layer and layer configuration of the multilayer structure according to one embodiment of the present invention will be described in detail below.
[0013] (Paper layer (A)) The paper layer (A) is usually a base layer in the multilayer structure of the present invention. The paper layer (A) can be a general paper mainly composed of plant-derived pulp. The paper layer (A) may contain pulp, as well as sizing agents, fillers, paper strength agents, retention aids, pH adjusters, drainage aids, water resistance agents, softeners, antistatic agents, defoamers, slime control agents, dyes, pigments, etc.
[0014] Examples of the paper constituting the paper layer (A) include kraft paper, fine paper, medium quality paper, alkaline paper, paperboard, glassine paper, semi-glassine paper, parchment paper, etc., with kraft paper or paperboard being preferred, and paperboard being more preferred.
[0015] The basis weight (mass per unit area) of the paper layer (A) is not particularly limited, and is, for example, 50 g / m 2 More than 500g / m 2 It can be less than 100 g / m 2 More than 450g / m 2 Less than 200 g / m is preferable. 2 More than 400g / m 2 Less than 220 g / m is more preferable. 2 More than 350g / m 2 More preferably less than 240 g / m 2 More than 300g / m 2When the basis weight of the paper layer (A) is equal to or more than the lower limit, the strength of the resulting paper container in a low-temperature environment can be further increased. On the other hand, when the basis weight of the paper layer (A) is less than the upper limit, the moldability can be improved.
[0016] The density of the paper layer (A) is, for example, 0.5 g / cm 3 More than 1.5g / cm 3 Less than 0.7 g / cm is preferred. 3 More than 1.3g / cm 3 The following is more preferred:
[0017] The paper used for the paper layer (A) can be produced by a known method, and commercially available paper can be used for the paper layer (A).
[0018] (Inorganic vapor deposited layer (B)) The inorganic vapor deposition layer (B) mainly ensures the gas barrier property in the multilayer structure of the present invention.
[0019] The inorganic vapor deposition layer (B) can be formed by vapor deposition of an inorganic material. Usually, the inorganic vapor deposition layer (B) is formed by vapor deposition of an inorganic material on the surface of the barrier resin layer (C). Examples of inorganic materials include metals (e.g., aluminum, copper, etc.), oxides (e.g., alumina, silica, etc.), nitrides (e.g., silicon nitride, etc.), nitride oxides (e.g., silicon oxynitride, etc.), and carbonitrides (e.g., silicon carbonitride, etc.).
[0020] The inorganic vapor deposition layer (B) is preferably a metal vapor deposition layer or an inorganic oxide vapor deposition layer. When light blocking properties and barrier properties after folding are important, the inorganic vapor deposition layer (B) is more preferably a metal vapor deposition layer, preferably a metal vapor deposition layer mainly composed of aluminum, and may be an aluminum vapor deposition layer. On the other hand, when prevention of coloring during recycling is important, the inorganic vapor deposition layer (B) is preferably an inorganic oxide vapor deposition layer, and preferably an inorganic oxide vapor deposition layer mainly composed of alumina (aluminum oxide) or silica (silicon oxide).
[0021] In the case of a metal deposition layer mainly composed of aluminum (inorganic deposition layer (B)), oxidation occurs irreversibly and aluminum oxide may be partially contained. In the case of a metal deposition layer mainly composed of aluminum (inorganic deposition layer (B)), the molar ratio of the content of oxygen atoms to the content of aluminum atoms (O mol / Al mol ) is preferably 0.5 or less, more preferably 0.3 or less, and even more preferably 0.1 or less.
[0022] The lower limit of the average thickness of the inorganic vapor deposition layer (B) is 5 nm, preferably 10 nm, more preferably 20 nm, and even more preferably 30 nm. When the average thickness of the inorganic vapor deposition layer (B) is equal to or greater than the lower limit, the gas barrier property can be further improved. The upper limit of the average thickness of the inorganic vapor deposition layer (B) is 200 nm, preferably 150 nm, more preferably 120 nm, and even more preferably 80 nm. When the average thickness of the inorganic vapor deposition layer (B) is equal to or less than the upper limit, the occurrence of defects, coloring, and the like during recycling can be suppressed. A recycled product (melt-molded product) with suppressed defects, coloring, and the like is preferable because of its good appearance, etc.
[0023] The inorganic vapor deposition layer (B) can be provided by a known physical vapor deposition method or chemical vapor deposition method, specifically, a vacuum vapor deposition method, a sputtering method, an ion plating method, an ion beam mixing method, a plasma CVD method, a laser CVD method, an MO-CVD method, a thermal CVD method, etc., and the physical vapor deposition method is preferable, and the vacuum vapor deposition method is more preferable.
[0024] Prior to deposition, the surface of the layer to be deposited (e.g., the barrier resin layer (C)) may be plasma-treated. The plasma treatment may be performed by a known method, and atmospheric pressure plasma treatment is preferred. Examples of the discharge gas in the atmospheric pressure plasma treatment include nitrogen gas, helium, neon, argon, krypton, xenon, and radon. Among these, nitrogen, helium, and argon are preferred, and nitrogen is more preferred from the viewpoint of cost reduction.
[0025] The inorganic vapor deposition layer (B) may consist of a single layer or multiple layers.
[0026] (Barrier resin layer (C)) The barrier resin layer (C) contains, as a main component, EVOH (c) having an ethylene unit content of 20 mol% to 50 mol% and a saponification degree of 90 mol% or more. Since the multilayer structure of the present invention has such a barrier resin layer (C), it can exhibit high gas barrier properties both in the state before and after bending.
[0027] EVOH (c) is a copolymer having ethylene units and vinyl alcohol units. EVOH (c) is usually obtained by saponification of an ethylene-vinyl ester copolymer. EVOH (c) may have residual vinyl ester units. The production and saponification of the ethylene-vinyl ester copolymer can be carried out by a known method. Examples of vinyl esters include vinyl acetate, vinyl formate, vinyl propionate, vinyl valerate, vinyl caprate, vinyl laurate, vinyl stearate, vinyl pivalate, vinyl versatate, and other aliphatic carboxylic acid vinyl esters, with vinyl acetate being preferred.
[0028] The lower limit of the ethylene unit content of EVOH (c) is 20 mol%, preferably 24 mol%, and more preferably 28 mol% or 30 mol% in some cases. By having the ethylene unit content of EVOH (c) be equal to or greater than the lower limit, it is possible to increase the strength in a low-temperature environment and suppress defects and coloration during recycling. The upper limit of the ethylene unit content of EVOH (c) is 50 mol%, preferably 46 mol%, and more preferably 42 mol% or 38 mol% in some cases. By having the ethylene unit content of EVOH (c) be equal to or less than the upper limit, it is possible to increase the gas barrier properties after bending treatment.
[0029] The lower limit of the saponification degree of EVOH (c) is 90 mol%, preferably 95 mol%, more preferably 99 mol%, and even more preferably 99.9 mol%. When the saponification degree of EVOH (c) is equal to or higher than the lower limit, the gas barrier properties tend to be improved. The upper limit of the saponification degree of EVOH (c) may be 100 mol%.
[0030] EVOH (c) may have structural units other than ethylene units, vinyl alcohol units, and vinyl ester units, to the extent that the object of the present invention is not hindered. In particular, by introducing a modifying group containing a primary hydroxyl group having a specific structure, it may be possible to achieve a high level of both gas barrier properties and moldability of EVOH (c). The content of other monomer units is preferably 5% by mass or less, more preferably 3% by mass or less, even more preferably 1% by mass or less, and particularly preferably substantially none. Examples of such other monomers include α-olefins such as propylene, n-butene, isobutylene, and 1-hexene; acrylic acid and its salts; unsaturated monomers having an acrylic acid ester group; methacrylic acid and its salts; unsaturated monomers having a methacrylic acid ester group; acrylamide, N-methylacrylamide, N-ethylacrylamide, N,N-dimethylacrylamide, diacetoneacrylamide, acrylamidopropanesulfonic acid and its salts, acrylamidopropyldimethylamine and its salts (e.g., quaternary salts); methacrylamide, N-methylmethacrylamide, N-ethylmethacrylamide, methacrylamidopropanesulfonic acid and its salts, methacrylamidopropyldimethylamine and its salts (e.g., quaternary salts); methyl vinyl ether, ethyl vinyl ether, n-propyl vinyl ether, i-propyl vinyl ether, vinyl ethers such as acrylonitrile, n-butyl vinyl ether, i-butyl vinyl ether, t-butyl vinyl ether, dodecyl vinyl ether, stearyl vinyl ether, 2,3-diacetoxy-1-vinyloxypropane, and the like; vinyl cyanides such as acrylonitrile, methacrylonitrile, and the like; vinyl halides such as vinyl chloride, vinyl fluoride, and the like; vinylidene halides such as vinylidene chloride, vinylidene fluoride, and the like; allyl compounds such as allyl acetate, 2,3-diacetoxy-1-allyloxypropane, and allyl chloride, and the like; unsaturated dicarboxylic acids and salts or esters thereof such as maleic acid, itaconic acid, and fumaric acid, and the like; vinyl silane compounds such as vinyltrimethoxysilane, and the like; isopropenyl acetate, 1,3-diacetoxy-2-methylenepropane, 1,3-dipropionyloxy-2-methylenepropane, and 1,3-dibutyronyloxy-2-methylenepropane, and the like.
[0031] The MFR of EVOH (c) (190° C., 2.16 kg load) is preferably 0.5 g / 10 min or more and 12 g / 10 min or less, more preferably 0.8 g / 10 min or more and 8.0 g / min or less, and more preferably 1.2 g / 10 min or more and 4.0 g / min or less.
[0032] The EVOH (c) may be used alone or in combination of two or more kinds.
[0033] EVOH (c) may contain two or more kinds of EVOH with different ethylene unit contents. In such a case, it is possible to improve the gas barrier property after bending treatment and the strength in a low-temperature environment in a well-balanced manner. The two kinds of EVOH with different ethylene unit contents may be two kinds of EVOH with different melting points. For example, when the melting point is measured by DSC, a peak temperature corresponding to each EVOH may be confirmed. In the measurement of the melting point by DSC, the temperature is raised from 30°C to 250°C at a rate of 10°C / min, cooled at 50°C / min, and the melting point is determined from the peak temperature measured in the second heating.
[0034] Of the two EVOHs (c), the EVOH (c1) having the lower ethylene unit content has an ethylene unit content of preferably 20 mol% to 40 mol%, more preferably 24 mol% to 32 mol%. Of the two EVOHs (c), the EVOH (c2) having the higher ethylene unit content has an ethylene unit content of preferably 32 mol% to 50 mol%, more preferably 38 mol% to 48 mol%.
[0035] The difference (c2-c1) in the ethylene unit content between EVOH (c2) and EVOH (c1), i.e., the value obtained by subtracting the ethylene unit content of EVOH (c1) from the ethylene unit content of EVOH (c2), is preferably from 4 mol% to 40 mol%, more preferably from 8 mol% to 30 mol%, even more preferably from 12 mol% to 25 mol%, and still more preferably from 15 mol% to 20 mol%.
[0036] The mass ratio (c1 / c2) of EVOH (c1) to EVOH (c2), i.e., the mass ratio of the content of EVOH (c1) to the content of EVOH (c2), is preferably 50 / 50 or more and 95 / 5 or less, more preferably 60 / 40 or more and 90 / 10 or less, and more preferably 70 / 30 or more and 85 / 15 or less.
[0037] The lower limit of the content of EVOH (c) in the barrier resin layer (C) is preferably 70 mass%, more preferably 80 mass%, and further preferably 90 mass%, and may be 95 mass%, 99 mass%, or 99.9 mass%, from the viewpoint of gas barrier properties, etc. The upper limit of the content of EVOH (c) in the barrier resin layer (C) may be 100 mass% or 99.99 mass%.
[0038] The barrier resin layer (C) preferably contains at least one polyvalent metal ion selected from the group consisting of magnesium ions, calcium ions, and zinc ions. The lower limit of the content of the polyvalent metal ions in the barrier resin layer (C) is preferably 10 ppm, more preferably 30 ppm, and even more preferably 50 ppm, and may even be more preferably 80 ppm when emphasis is placed on suppressing defects in the recycled resin. When the barrier resin layer (C) contains the polyvalent metal ions at or above the lower limit, the occurrence of defects during recycling is further suppressed. On the other hand, the upper limit of the content of the polyvalent metal ions in the barrier resin layer (C) may be, for example, 300 ppm, but is preferably 200 ppm, more preferably 150 ppm, and even more preferably 120 ppm, and may even be more preferably 80 ppm when emphasis is placed on suppressing coloration of the recycled resin. When the content of the polyvalent metal ions in the barrier resin layer (C) is equal to or less than the upper limit, the occurrence of coloration during recycling is suppressed.
[0039] The polyvalent metal ion preferably contains magnesium ion, and more preferably is magnesium ion, which can further suppress the occurrence of defects during recycling.
[0040] The polyvalent metal ion is preferably present in the barrier resin layer (C) as a cation constituting a salt, and more preferably as a cation constituting a carboxylate in the barrier resin layer (C). In a salt such as a carboxylate, the polyvalent metal ion and an anion may be bonded or free.
[0041] The carboxylate containing the polyvalent metal ion is preferably a higher fatty acid salt. Specifically, it is preferably a salt of a carboxylic acid having 12 or more carbon atoms. When the polyvalent metal ion is present in the form of such a higher fatty acid salt, the occurrence of coloring during recycling is further suppressed. Examples of the carboxylic acid having 12 or more carbon atoms include lauric acid, lauric acid, tridecylic acid, myristic acid, pentadecylic acid, palmitic acid, heptadecylic acid, stearic acid, basic stearic acid, hydroxystearic acid, basic hydroxystearic acid, nonadecanoic acid, oleic acid, behenic acid, montanic acid, and linoleic acid. The number of carbon atoms of the carboxylic acid may be 12 or more and 30 or less, 14 or more and 26 or less, or 16 or more and 22 or less.
[0042] The polyvalent metal ions may be present in the barrier resin layer (C) as cations constituting fatty acid salts having 11 or less carbon atoms (acetates, propionates, etc.), salts other than fatty acid salts (nitrates, sulfates, etc.), etc. A part or all of the polyvalent metal ions may be present in a state coordinated to, for example, hydroxyl groups of EVOH (c).
[0043] The barrier resin layer (C) may contain, as optional components other than EVOH (c) and the polyvalent metal ions or salts containing the polyvalent metal ions, boron compounds, carboxylic acids, phosphorus compounds, metal ions other than the polyvalent metal ions, antioxidants, ultraviolet absorbers, plasticizers, antistatic agents, lubricants, colorants, fillers, heat stabilizers, resins other than EVOH (c), etc. The barrier resin layer (C) may contain two or more of these optional components.
[0044] Examples of the boron compound include boric acids such as orthoboric acid, metaboric acid, and tetraboric acid; boric acid esters such as triethyl borate and trimethyl borate; alkali metal salts or alkaline earth metal salts of the boric acids, borate salts such as borax; and boron hydrides. The content of the boron compound in the barrier resin layer (C) is preferably 10 ppm or more and 1,000 ppm or less, and more preferably 50 ppm or more and 400 ppm or less. By setting the content of the boron compound within the above range, melt moldability, appearance, and the like are improved. The content of the boron compound is the content calculated as elemental boron.
[0045] Examples of the carboxylic acids include formic acid, acetic acid, propionic acid, butyric acid, lactic acid, and salts thereof. The carboxylic acids are preferably carboxylic acids having 4 or less carbon atoms or saturated carboxylic acids, and more preferably acetic acid. The carboxylic acids may also include the carboxylates containing the polyvalent metal ions described above.
[0046] Examples of the phosphorus compound include phosphates such as phosphoric acid and phosphorous acid. The phosphate may be in the form of any of primary phosphate, secondary phosphate, and tertiary phosphate. The cationic species of the phosphate is not particularly limited, but is preferably an alkali metal salt or an alkaline earth metal salt, and among these, sodium dihydrogen phosphate, potassium dihydrogen phosphate, disodium hydrogen phosphate, and dipotassium hydrogen phosphate are more preferable. The content of the phosphorus compound in the barrier resin layer (C) is preferably 1 ppm or more and 200 ppm or less, and more preferably 10 ppm or more and 100 ppm or less. By setting the content of the phosphorus compound within the above range, the thermal stability is improved and defects and coloring during recycling are suppressed. The content of the phosphorus compound is the content calculated as a phosphate radical.
[0047] Examples of the metal ions other than the polyvalent metal ions include monovalent metal ions and polyvalent metal ions other than the polyvalent metal ions described above, and the monovalent metal ions are preferred. As the monovalent metal ions, alkali metal ions are preferred.
[0048] Examples of the alkali metal ion include lithium ion, sodium ion, potassium ion, etc., and sodium ion or potassium ion is preferred from the viewpoint of industrial availability. Examples of the alkali metal salt containing an alkali metal ion include aliphatic carboxylate, aromatic carboxylate, carbonate, hydrochloride, nitrate, sulfate, phosphate, and metal complex. Among them, aliphatic carboxylate or phosphate is preferred from the viewpoint of availability, specifically, sodium acetate, potassium acetate, sodium phosphate, or potassium phosphate is preferred. The content of the alkali metal ion in the barrier resin layer (C) is preferably 10 ppm or more and 1,000 ppm or less, more preferably 100 ppm or more and 400 ppm or less. By setting the content of the alkali metal ion within the above range, interlayer adhesion and the like are improved, and coloring during recycling is suppressed.
[0049] Examples of antioxidants include 2,5-di-t-butylhydroquinone, 2,6-di-t-butyl-p-cresol, 4,4'-thiobis(6-t-butylphenol), 2,2'-methylene-bis(4-methyl-6-t-butylphenol), and octadecyl-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate.
[0050] Examples of ultraviolet absorbers include ethylene-2-cyano-3,3'-diphenylacrylate, 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-3'-t-butyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-hydroxy-4-methoxybenzophenone, 2,2'-dihydroxy-4-methoxybenzophenone, and 2-hydroxy-4-oxybenzophenone.
[0051] Examples of the plasticizer include dimethyl phthalate, diethyl phthalate, dioctyl phthalate, wax, liquid paraffin, and phosphoric ester.
[0052] Examples of the antistatic agent include pentaerythritol monostearate, sorbitan monopalmitate, sulfated polyolefins, polyethylene oxide, and polyethylene glycol (trade name: Carbowax).
[0053] Examples of the lubricant include ethylene bis stearamide and butyl stearate.
[0054] Examples of the colorant include carbon black, phthalocyanine, quinacridone, indoline, azo pigments, and red iron oxide.
[0055] Examples of the filler include glass fiber, wollastonite, calcium silicate, talc, and montmorillonite.
[0056] Examples of the heat stabilizer include hindered phenol compounds and hindered amine compounds.
[0057] Examples of the resin other than EVOH (c) include polyamide and polyolefin.
[0058] The barrier resin layer (C) may be a non-stretched layer or a stretched layer. When the barrier resin layer (C) is a stretched layer, it can exhibit good gas barrier properties even when the barrier resin layer (C) is relatively thin.
[0059] The lower limit of the average thickness of the barrier resin layer (C) is preferably 0.1 μm, more preferably 0.2 μm, even more preferably 0.4 μm, even more preferably 0.5 μm, 0.6 μm, 0.8 μm or 1 μm, and may be 2 μm. When the average thickness of the barrier resin layer (C) is equal to or greater than the lower limit, the gas barrier property can be further improved. The upper limit of the average thickness of the barrier resin layer (C) is preferably 30 μm, more preferably 20 μm, even more preferably 15 μm, even more preferably 10 μm or 5 μm, and may be 3 μm. When the average thickness of the barrier resin layer (C) is equal to or less than the upper limit, the occurrence of coloring during recycling can be suppressed.
[0060] The barrier resin layer (C) may consist of a single layer or multiple layers.
[0061] (Adhesive resin layer (D)) The adhesive resin layer (D) contains an adhesive resin (d) as a main component, and adheres the barrier resin layer (C) and the moisture-proof resin layer (E) to each other.
[0062] The adhesive resin (d) is not particularly limited as long as it is a resin having adhesive properties, and examples thereof include acid-modified polyolefins (such as carboxylic acid-modified polyolefins and sulfonic acid-modified polyolefins), and epoxy-modified polyolefins. The adhesive resin (d) is preferably a thermoplastic resin. The adhesive resin (d) is preferably an acid-modified polyolefin (such as acid-modified polyethylene and acid-modified polypropylene), and more preferably an acid-modified polyethylene. The adhesive resin (d) is also preferably a carboxylic acid-modified polyolefin, and more preferably a carboxylic acid-modified polyethylene.
[0063] The carboxylic acid-modified polyolefin may be a polyolefin having a carboxy group or an anhydride group thereof. The carboxylic acid-modified polyolefin (polyolefin having a carboxy group or an anhydride group thereof) can be obtained, for example, by chemically bonding an ethylenically unsaturated carboxylic acid or an anhydride thereof to an unmodified polyolefin by an addition reaction, a graft reaction, or the like.
[0064] As the unmodified polyolefin used in the production of the carboxylic acid modified polyolefin, polyethylene is preferred.
[0065] Examples of ethylenically unsaturated carboxylic acids and their anhydrides include monocarboxylic acids, monocarboxylic acid esters, dicarboxylic acids, dicarboxylic acid monoesters, dicarboxylic acid diesters, and dicarboxylic acid anhydrides.Specific examples include maleic acid, fumaric acid, itaconic acid, maleic anhydride, itaconic anhydride, maleic acid monomethyl ester, maleic acid monoethyl ester, maleic acid diethyl ester, and fumaric acid monomethyl ester.Of these, dicarboxylic acid anhydrides such as maleic anhydride and itaconic anhydride are preferred, and maleic anhydride is more preferred.That is, the adhesive resin (d) is also preferably a maleic anhydride-modified polyolefin, and more preferably a maleic anhydride-modified polyethylene.
[0066] Carboxylic acid-modified polyolefins are obtained by introducing ethylenically unsaturated carboxylic acid or its anhydride into unmodified polyolefins by addition reaction or graft reaction in the presence of a solvent such as xylene and a catalyst such as peroxide. The lower limit of the amount of addition or grafting (degree of modification) of carboxylic acid or its anhydride to the unmodified polyolefin is preferably 0.01% by mass, more preferably 0.02% by mass, based on the unmodified polyolefin. On the other hand, the upper limit of the amount of addition or grafting (degree of modification) is preferably 15% by mass, more preferably 10% by mass, based on the unmodified polyolefin.
[0067] The acid value of the acid-modified polyolefin such as the carboxylic acid-modified polyolefin is preferably from 0.3 mgKOH / g to 5.0 mgKOH / g, more preferably from 1.0 mgKOH / g to 3.0 mgKOH / g.
[0068] The MFR (190° C., 2.16 kg load) of the adhesive resin (d) is preferably 0.5 g / 10 min or more and 12 g / 10 min or less, and more preferably 1.0 g / 10 min or more and 8.0 g / min or less.
[0069] The adhesive resin (d) may be used alone or in combination of two or more kinds.
[0070] The content of the adhesive resin (d) in the adhesive resin layer (D) is preferably 80% by mass or more and 100% by mass or less, more preferably 90% by mass or more and 100% by mass or less, and even more preferably 97% by mass or more and 100% by mass or less. The adhesive resin layer (D) may contain, as a component other than the adhesive resin (d), an antioxidant, an ultraviolet absorber, a plasticizer, an antistatic agent, a lubricant, a colorant, a filler, a heat stabilizer, a resin other than the adhesive resin (d), and the like.
[0071] The adhesive resin layer (D) may be a non-oriented layer or a oriented layer.
[0072] The lower limit of the average thickness of the adhesive resin layer (D) is preferably 0.1 μm, more preferably 0.5 μm, further preferably 1 μm, and may be 2 μm. When the average thickness of the adhesive resin layer (D) is equal to or greater than the lower limit, sufficient adhesiveness can be exhibited. In addition, defects and coloring during recycling can be further suppressed. The upper limit of the average thickness of the adhesive resin layer (D) is preferably 20 μm, more preferably 10 μm, further preferably 5 μm, and may be 3 μm. When the average thickness of the adhesive resin layer (D) is equal to or less than the upper limit, defects and coloring during recycling can be further suppressed.
[0073] The adhesive resin layer (D) may consist of a single layer or may consist of multiple layers.
[0074] (Moisture-proof resin layer (E)) The moisture-proof resin layer (E) contains polyethylene (e) as a main component. The moisture-proof resin layer (E) contains polyethylene (e) as a main component, so that the multilayer structure of the present invention can exhibit sufficient moisture-proof properties. In addition, the moisture-proof resin layer (E) contains polyethylene (e) as a main component, so that the multilayer structure of the present invention can be formed into a paper container having sufficient strength even in a low-temperature environment, and the occurrence of defects during recycling is also suppressed. The moisture-proof resin layer (E) may be a heat-sealing layer for bonding the moisture-proof resin layers (E) to each other or to the moisture-proof resin layer (E) and another layer by heat sealing. From the viewpoint of further increasing the strength of the obtained paper container in a low-temperature environment, the moisture-proof resin layer (E) may be the outermost layer in the multilayer structure.
[0075] The type of polyethylene (e) is not particularly limited, and examples thereof include high-density polyethylene, low-density polyethylene, and linear low-density polyethylene. Among these, linear low-density polyethylene, low-density polyethylene, or a mixture thereof is preferred. Linear low-density polyethylene is a resin obtained by polymerizing ethylene with an α-olefin having 3 or more carbon atoms. Examples of α-olefins having 3 or more carbon atoms include propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-decene, 1-dodecene, and 4-methyl-1-pentene. Among these, linear low-density polyethylene is preferably linear low-density polyethylene obtained by polymerizing ethylene with an α-olefin having 6 or more carbon atoms, and more preferably linear low-density polyethylene obtained by polymerizing ethylene with an α-olefin having 8 or more carbon atoms. When the carbon number of the α-olefin copolymerized with ethylene is relatively large, various mechanical strengths such as puncture strength and tensile strength may be particularly improved. In addition, it is preferable to use a metallocene catalyst as the polymerization catalyst. The linear low-density polyethylene polymerized using a metallocene catalyst is produced by copolymerizing ethylene and an α-olefin in the presence of a catalyst formed from a compound having at least one ligand having a cyclopentadienyl skeleton and having a transition metal of Group 4 of the periodic table as the central metal atom (preferably a compound having zirconium as the central metal atom), an organoaluminum oxy compound, and various components added as necessary. The linear low-density polyethylene polymerized using a metallocene catalyst has excellent melt moldability, and the multilayer film obtained has an excellent balance of heat resistance, flexibility, and mechanical strength. By using such a polyethylene, it is possible to further increase the strength of the molded paper container in a low-temperature environment. One or more types of polyethylene (e) can be used.
[0076] The upper limit of the density of polyethylene (e) is, for example, 0.96 g / cm 3 0.940g / cm 3 is preferred, and 0.930 g / cm 3The lower limit of the density of the polyethylene (e) is 0.880 g / cm 3 is preferred, and 0.890 g / cm 3 More preferably, 0.900 g / cm 3 or 0.910 g / cm 3 By using a polyethylene having a relatively low density as the polyethylene (e) in this way, it is possible to further increase the strength of the molded paper container in a low-temperature environment.
[0077] The MFR (190° C., 2.16 kg load) of the polyethylene (e) is preferably 0.4 g / 10 min or more and 4.0 g / 10 min or less, and more preferably 0.8 g / 10 min or more and 2.0 g / min or less.
[0078] The content of polyethylene (e) in the moisture-proof resin layer (E) is preferably from 80% by mass to 100% by mass, more preferably from 90% by mass to 100% by mass, and even more preferably from 97% by mass to 100% by mass. The moisture-proof resin layer (E) may contain, as components other than the polyethylene (e), antioxidants, ultraviolet absorbers, plasticizers, antistatic agents, lubricants, colorants, fillers, heat stabilizers, resins other than the polyethylene (e), and the like.
[0079] The moisture-proof resin layer (E) may be a non-stretched layer or a stretched layer.
[0080] The lower limit of the average thickness of the moisture-proof resin layer (E) is preferably 1 μm, more preferably 5 μm, even more preferably 10 μm, even more preferably 20 μm, and may be 30 μm, 40 μm, or 45 μm. When the average thickness of the moisture-proof resin layer (E) is equal to or greater than the lower limit, sufficient heat sealing can be performed, and a paper container having higher strength in a low-temperature environment can be formed. Furthermore, when the average thickness of the moisture-proof resin layer (E) is equal to or greater than the lower limit, sufficient moisture resistance can be exhibited. The upper limit of the average thickness of the moisture-proof resin layer (E) is preferably 200 μm, more preferably 100 μm, and may be 50 μm.
[0081] The moisture-proof resin layer (E) may consist of a single layer or multiple layers.
[0082] (Thermoplastic resin layer (X)) The multilayer structure of the present invention preferably further has a thermoplastic resin layer (X) interposed between the paper layer (A) and the inorganic vapor deposition layer (B) or the moisture-proof resin layer (E). In other words, the multilayer structure of the present invention preferably has a layer structure in which the paper layer (A) and the inorganic vapor deposition layer (B) or the moisture-proof resin layer (E) are laminated via the thermoplastic resin layer (X). It may be said that the paper layer (A) is laminated via the thermoplastic resin layer (X) on one side of a laminate (composite film) of the inorganic vapor deposition layer (B), the barrier resin layer (C), the adhesive resin layer (D) and the moisture-proof resin layer (E). By having such a thermoplastic resin layer (X) in the multilayer structure, it is possible to increase the adhesion between the paper layer (A) and the inorganic vapor deposition layer (B) or the moisture-proof resin layer (E). In addition, by bonding the paper layer (A) and the inorganic vapor deposition layer (B) or the moisture-proof resin layer (E) with the thermoplastic resin layer (X), defects and coloring during recycling can be further suppressed.
[0083] The thermoplastic resin layer (X) is mainly composed of a thermoplastic resin. The thermoplastic resin is not particularly limited as long as it is a thermoplastic resin having a melting point of less than 200°C, and examples thereof include polyolefin, polystyrene, polycarbonate, acrylic resin, and the above-mentioned adhesive resin (acid-modified polyolefin, etc.). Among these, polyolefin or acid-modified polyolefin is preferred, polyolefin is more preferred, and polyethylene is even more preferred. By making the thermoplastic resin layer (X) mainly composed of such a thermoplastic resin, it is possible to suppress the occurrence of coloring during recycling.
[0084] The content of the thermoplastic resin in the thermoplastic resin layer (X) is preferably 80% by mass or more and 100% by mass or less, more preferably 90% by mass or more and 100% by mass or less, and even more preferably 97% by mass or more and 100% by mass or less. The thermoplastic resin layer (X) may contain, as components other than the thermoplastic resin, antioxidants, ultraviolet absorbers, plasticizers, antistatic agents, lubricants, colorants, fillers, heat stabilizers, resins other than the thermoplastic resins, and the like.
[0085] The lower limit of the average thickness of the thermoplastic resin layer (X) is preferably 1 μm, more preferably 3 μm, even more preferably 5 μm, and even more preferably 10 μm. When the average thickness of the thermoplastic resin layer (X) is equal to or greater than the lower limit, the adhesion between the paper layer (A) and the inorganic vapor deposition layer (B) can be improved. The upper limit of the average thickness of the thermoplastic resin layer (X) is preferably 100 μm, more preferably 50 μm, and may be 30 μm.
[0086] The thermoplastic resin layer (X) is preferably an extruded resin layer. That is, the paper layer (A) and the inorganic vapor deposition layer (B) (or a coextruded film having an inorganic vapor deposition layer (B) described later on one side) or the moisture-proof resin layer (E) (or a coextruded film having an inorganic vapor deposition layer (E) described later on one side) are preferably laminated by sandwich lamination. However, the paper layer (A) and the inorganic vapor deposition layer (B) (or a coextruded film having an inorganic vapor deposition layer (B) described later on one side) or the moisture-proof resin layer (E) (or a coextruded film having an inorganic vapor deposition layer (E) described later on one side) may be laminated by other methods, such as dry lamination. In this case, the layer interposed between the paper layer (A) and the inorganic vapor deposition layer (B) or the moisture-proof resin layer (E) may be an adhesive layer other than the thermoplastic resin layer (X).
[0087] (Co-extruded film) In the multilayer structure of the present invention, the laminate of the barrier resin layer (C), the adhesive resin layer (D) and the moisture-proof resin layer (E) is preferably a coextruded film. That is, the barrier resin layer (C), the adhesive resin layer (D) and the moisture-proof resin layer (E) are preferably formed by coextrusion. This makes it possible to achieve a high level of balance between film properties such as barrier properties and flexibility, and processability and economic efficiency. Furthermore, it is preferable that an inorganic vapor deposition layer (B) is provided on the surface of the barrier resin layer (C) side of the coextruded film. In this embodiment, the inorganic vapor deposition layer (B) may be provided by vapor deposition on the surface of the barrier resin layer (C) side of the coextruded film. By using such a coextruded film, the productivity, gas barrier properties, etc. of the multilayer structure can be improved.
[0088] The lower limit of the average thickness of the coextruded film is preferably 8 μm, more preferably 15 μm, and even more preferably 25 μm. By making the average thickness of the coextruded film equal to or greater than the lower limit, the gas barrier property and the strength of the resulting paper container in a low-temperature environment can be further improved. The upper limit of the average thickness of the coextruded film is preferably 120 μm, more preferably 80 μm, and even more preferably 60 μm. By making the average thickness of the coextruded film equal to or less than the upper limit, the multilayer structure can be made thinner. The average thickness of the coextruded film is equal to the sum of the average thicknesses of all layers of the coextruded film.
[0089] From the viewpoints of gas barrier properties, recyclability, and economic efficiency, the average thickness of the barrier resin layer (C) of the coextruded film is preferably 0.2 μm or more and less than 30 μm. It is also preferable that the ratio of the average thickness of the barrier resin layer (C) to the average thickness of the coextruded film is less than 25%. The average thickness of the barrier resin layer (C) is more preferably 0.4 μm or more and less than 15 μm, even more preferably 0.6 μm or more and less than 10 μm, and even more preferably 0.8 μm or more and less than 5 μm. The ratio of the average thickness of the barrier resin layer (C) to the average thickness of the coextruded film is more preferably less than 20%, even more preferably less than 15%.
[0090] The coextruded film may be a non-stretched film that is not substantially stretched, or may be a uniaxially or biaxially stretched film. When the coextruded film is a non-stretched film, the strength of the resulting paper container in a low-temperature environment tends to be increased. When the coextruded film is a stretched film, the gas barrier property tends to be further increased.
[0091] The coextruded film is preferably stretched at least uniaxially by 3 times or more and less than 12 times, and more preferably stretched at least uniaxially by 4 times or more and less than 10 times. The coextruded film is also preferably stretched biaxially by 3 times or more and less than 12 times, and more preferably stretched biaxially by 3.5 times or more and less than 10 times. By stretching the coextruded film at such a stretch ratio, the gas barrier property of the multilayer structure can be further improved.
[0092] (Moisture-proof resin layer (F)) The multilayer structure of the present invention preferably further comprises a moisture-proof resin layer (F) other than the moisture-proof resin layer (E). The moisture-proof resin layer (F) contains polyethylene (f) as a main component. When the multilayer structure further comprises such a moisture-proof resin layer (F), the moisture-proof property and the strength of the obtained paper container in a low-temperature environment can be further improved. The moisture-proof resin layer (F) may be a heat-sealing layer for bonding the moisture-proof resin layers (F) to each other or to the moisture-proof resin layer (F) and another layer by heat sealing. From the viewpoint of further increasing the strength of the obtained paper container in a low-temperature environment, the moisture-proof resin layer (F) may be the outermost layer in the multilayer structure. In addition, when the moisture-proof resin layer (F) contains polyethylene (f) as a main component, defects and coloring during recycling are suppressed. In this specification, the moisture-proof resin layer provided on the side opposite to the side of the paper layer (A) on which the inorganic vapor deposition layer (B) and the like are provided (hereinafter also referred to as the "exposed surface side") is deemed to be the moisture-proof resin layer (F). Also, the moisture-proof resin layer different from the moisture-proof resin layer (E) constituting the coextruded film is deemed to be the moisture-proof resin layer (F). On the other hand, when there are multiple moisture-proof resin layers constituting the coextruded film, all of these moisture-proof resin layers are deemed to be the moisture-proof resin layer (E). When the multilayer structure does not have the coextruded film and has multiple moisture-proof resin layers (excluding the case where the moisture-proof resin layer is on the exposed surface side of the paper layer (A)), all of these moisture-proof resin layers are deemed to be the moisture-proof resin layer (E).
[0093] The type, physical properties, specific form and preferred form of the polyethylene (f) are the same as those of the polyethylene (e) described above, except for the MFR. For example, the density of the polyethylene (f) is 0.880 g / cm 3 More than 0.940g / cm 3Preferably, the polyethylene (f) is a linear low-density polyethylene, a low-density polyethylene, or a mixture thereof. The MFR (190°C, 2.16 kg load) of the polyethylene (f) is preferably 0.4 g / 10 min or more and 30.0 g / 10 min or less, more preferably 0.8 g / 10 min or more and 20.0 g / min or less, and even more preferably 1.0 g / 10 min or more and 10.0 g / min or less.
[0094] The composition, average thickness, and specific and preferred forms of the moisture-proof resin layer (F) are the same as those of the moisture-proof resin layer (E) described above. In one embodiment of the multilayer structure of the present invention, the moisture-proof resin layer (F) is preferably a non-stretched layer. The moisture-proof resin layer (F) may be a stretched layer.
[0095] In the multilayer structure of the present invention, the position of the moisture-proof resin layer (F) is not particularly limited. However, it is preferable that the moisture-proof resin layer (F) is directly laminated to the coextruded film. In the case of such a multilayer structure, the strength in a low-temperature environment can be further increased, and the occurrence of defects and coloring during recycling tends to be further reduced due to the increased usage ratio of polyethylene-based resin. In the multilayer structure of this embodiment, for example, the moisture-proof resin layer (F) can be laminated by melt-extruding polyethylene (f) directly onto the surface of the moisture-proof resin layer (E) of the coextruded film.
[0096] In addition, the moisture-proof resin layer (F) may be laminated on the surface of the moisture-proof resin layer (E) of the coextruded film via another layer (e.g., an adhesive resin layer, another adhesive layer, etc.) In such a multilayer structure, the moisture-proof resin layer (F) can be laminated by dry lamination, sandwich lamination, etc. of the coextruded film and the single-layer film of the moisture-proof resin layer (F).
[0097] The moisture-proof resin layer (F) may be laminated directly or via another layer on the surface of the paper layer (A) opposite to the inorganic vapor deposition layer (B). In such a multilayer structure, the moisture-proof resin layer (F) can be laminated by melt extrusion of polyethylene (f) onto the surface of the paper layer (A), dry lamination or sandwich lamination of the paper layer (A) or a multilayer structure including the paper layer (A) with a monolayer film of the moisture-proof resin layer (F), or the like.
[0098] (Other layers) The multilayer structure of the present invention may have layers other than the paper layer (A), inorganic vapor deposition layer (B), barrier resin layer (C), adhesive resin layer (D), moisture-proof resin layer (E), moisture-proof resin layer (F) and thermoplastic resin layer (X). Examples of other layers that the multilayer structure of the present invention may have include other thermoplastic resin layers, adhesive layers, printed layers, etc. However, the multilayer structure does not have a layer containing a resin having a melting point of 200°C or more as a main component and a metal layer having an average thickness of 1 μm or more. When the multilayer structure contains a layer containing a resin having a melting point of 200°C or more as a main component (for example, a layer containing polyethylene terephthalate as a main component) and a metal layer having an average thickness of 1 μm or more (for example, a metal foil layer having an average thickness of 1 μm or more), defects are likely to occur in the recycled product during melt molding for recycling. Since the multilayer structure does not have such layers, defects are unlikely to occur in the recycled product and the recyclability is excellent.
[0099] Furthermore, the multilayer structure of the present invention preferably does not have an adhesive layer made of a curing adhesive, since the absence of such an adhesive layer can further suppress defects during recycling.
[0100] (Layer composition, etc.) The multilayer structure of the present invention has a paper layer (A), an inorganic vapor deposition layer (B), a barrier resin layer (C), an adhesive resin layer (D), and a moisture-proof resin layer (E). The inorganic vapor deposition layer (B), the barrier resin layer (C), the adhesive resin layer (D), and the moisture-proof resin layer (E) are all directly laminated in this order. The multilayer structure preferably has the paper layer (A), the inorganic vapor deposition layer (B), the barrier resin layer (C), the adhesive resin layer (D), and the moisture-proof resin layer (E) in this order, particularly in terms of increasing strength in a low-temperature environment. The multilayer structure may have the paper layer (A), the moisture-proof resin layer (E), the adhesive resin layer (D), the barrier resin layer (C), and the inorganic vapor deposition layer (B) in this order. The paper layer (A) and the inorganic vapor deposition layer (B) or the moisture-proof resin layer (E) may be directly laminated, but are usually laminated via another layer. The layer interposed between the paper layer (A) and the inorganic vapor deposition layer (B) or the moisture-proof resin layer (E) may be a thermoplastic resin layer (X) or another adhesive layer. The multilayer structure may further have a moisture-proof resin layer (F).
[0101] The multilayer structure of the present invention preferably has a paper layer (A) on one surface. That is, in the multilayer structure, it is preferable that one of the outermost layers is the paper layer (A). However, when a paper container is formed from the multilayer structure, it is preferable that the surface on which the paper layer (A) is exposed is the outer surface. When the multilayer structure has the paper layer (A) on the surface, it becomes easy to detect the paper, specifically, to detect the paper by measuring the infrared spectrum using, for example, a total reflection measurement method. Therefore, in such a multilayer structure, the paper recycling rate can be increased.
[0102] The multilayer structure of the present invention also preferably has a moisture-proof resin layer (E) or a moisture-proof resin layer (F) on one surface. That is, in the multilayer structure, one of the outermost layers is preferably the moisture-proof resin layer (E) or the moisture-proof resin layer (F). When a paper container is formed from the multilayer structure, it is preferable that the surface on which the moisture-proof resin layer (E) or the moisture-proof resin layer (F) is exposed becomes the inner surface. When the multilayer structure has a moisture-proof resin layer (E) or a moisture-proof resin layer (F) on the surface, these layers are bonded by heat sealing, and a paper container having higher strength in a low-temperature environment can be formed. In addition, when the multilayer structure has a moisture-proof resin layer (E) or a moisture-proof resin layer (F) on the surface, detection of polyethylene, specifically, detection of polyethylene by, for example, infrared spectrum measurement using a total reflection measurement method, becomes easy. Therefore, in such a multilayer structure, the recycling rate of polyethylene can be increased.
[0103] The multilayer structure of the present invention preferably has a paper layer (A) on one surface and a moisture-proof resin layer (E) or (F) on the other surface. When the multilayer structure is molded into a paper container, it is preferable that the surface on which the paper layer (A) is exposed becomes the outer surface, and the surface on which the moisture-proof resin layer (E) or (F) is exposed becomes the inner surface.
[0104] Specific layer configurations of the multilayer structure of the present invention are exemplified below. However, the layer configuration of the multilayer structure is not limited to the following configuration. In the following examples of each layer configuration, " / " indicates that the layers are directly laminated. Also, "Ad" indicates an optional adhesive layer. The adhesive layer represented by Ad may be a layer mainly composed of an adhesive resin (a layer made of the same material as the adhesive resin layer (D)). (1) A / X / B / C / D / E (2) A / Ad / B / C / D / E (3) A / X / B / C / D / E / F (4) A / X / B / C / D / E / Ad / F (5) F / A / X / B / C / D / E (6) F / A / Ad / B / C / D / E (7) F / A / X / B / C / D / E / F (8) F / A / X / B / C / D / E / Ad / F (9) F / Ad / A / X / B / C / D / E (10) F / Ad / A / Ad / B / C / D / E (11) F / Ad / A / X / B / C / D / E / F (12) F / Ad / A / X / B / C / D / E / Ad / F (13) A / X / E / D / C / B / F (14) A / X / E / D / C / B / Ad / F (15) A / Ad / E / D / C / B / F (16) A / Ad / E / D / C / B / Ad / F (17) F / A / X / E / D / C / B / F (18) F / A / X / E / D / C / B / Ad / F (19) F / Ad / A / X / E / D / C / B / F (20) F / Ad / A / X / E / D / C / B / Ad / F (21) F / A / Ad / E / D / C / B / F (22) F / A / Ad / E / D / C / B / Ad / F (23)F / Ad / A / Ad / E / D / C / B / F (24)F / Ad / A / Ad / E / D / C / B / Ad / F
[0105] The lower limit of the mass ratio of the paper layer (A) in the multilayer structure of the present invention may be, for example, 0.40 or 0.50 of the entire multilayer structure, but is preferably 0.60, more preferably 0.70, and even more preferably 0.75. By having the mass ratio of the paper layer (A) be equal to or greater than the lower limit, the strength of the molded paper container in a low-temperature environment can be further increased. On the other hand, the upper limit of the mass ratio of the paper layer (A) is preferably 0.95, more preferably 0.90, and even more preferably 0.86. By having the mass ratio of the paper layer (A) be equal to or greater than the lower limit, the gas barrier properties and the strength of the molded paper container in a low-temperature environment can be further increased.
[0106] The lower limit of the total average thickness ratio of the layers mainly composed of polyethylene resin in the part other than the paper layer (A) of the multilayer structure of the present invention is preferably 0.75, more preferably 0.80, even more preferably 0.85, and even more preferably 0.90. By increasing the total average thickness ratio of the layers mainly composed of polyethylene resin in the part other than the paper layer (A), it is possible to further suppress the occurrence of coloring during recycling. The upper limit of the total average thickness ratio of the layers mainly composed of polyethylene resin in the part other than the paper layer (A) is preferably 0.995, more preferably 0.99, and may be 0.98. Examples of layers mainly composed of polyethylene resin include a moisture-proof resin layer (E), a moisture-proof resin layer (F), an adhesive resin layer (D) when the adhesive resin (d) is, for example, acid-modified polyethylene, and a thermoplastic resin layer (X) when the main component is a polyethylene resin (polyethylene or modified polyethylene).
[0107] The lower limit of the total average thickness ratio of the layers mainly composed of a resin having an ethylene unit in the portion other than the paper layer (A) of the multilayer structure of the present invention is preferably 0.95, more preferably 0.98, and even more preferably 0.99. By increasing the total average thickness ratio of the layers mainly composed of a resin having an ethylene unit in the portion other than the paper layer (A), the compatibility during recycling is improved, and the occurrence of defects and coloring can be further suppressed. The upper limit of the total average thickness ratio of the layers mainly composed of a resin having an ethylene unit in the portion other than the paper layer (A) may be, for example, 0.9999. Examples of layers mainly composed of a resin having an ethylene unit include the above-mentioned layer mainly composed of a polyethylene-based resin and the barrier resin layer (C).
[0108] The lower limit of the total average thickness ratio of layers mainly composed of a thermoplastic resin having a melting point of less than 200° C. in the portion other than the paper layer (A) of the multilayer structure of the present invention is preferably 0.95, more preferably 0.98, and even more preferably 0.99. By increasing the total average thickness ratio of the thermoplastic resin having a melting point of less than 200° C. in the portion other than the paper layer (A), the melt moldability during recycling is improved, and the occurrence of defects and coloring can be further suppressed. The upper limit of the total average thickness ratio of layers mainly composed of a thermoplastic resin having a melting point of less than 200° C. in the portion other than the paper layer (A) may be, for example, 0.9999.
[0109] The lower limit of the average thickness of the multilayer structure of the present invention (average thickness of the entire multilayer structure) is preferably 150 μm, more preferably 200 μm, even more preferably 250 μm, and even more preferably 300 μm. When the average thickness of the multilayer structure is equal to or greater than the lower limit, the strength of the molded paper container in a low-temperature environment can be increased. On the other hand, the upper limit of the average thickness of the multilayer structure is preferably 1,000 μm, and may be 700 μm or 500 μm. When the average thickness of the multilayer structure is equal to or less than the upper limit, the moldability can be increased.
[0110] In the multilayer structure of the present invention, the oxygen transmission rate measured by the method described in JIS K 7126-2:2006 under conditions of 20°C and 65% RH is 0.5 cc / (m 2 ·day·atm), and preferably less than 0.1cc / (m 2 ·day·atm). By having an oxygen transmission rate below the above upper limit, the material can be particularly suitably used as a molding material for paper containers. On the other hand, the lower limit of the oxygen transmission rate is 0.001 cc / (m 2 ·day·atm), and 0.01cc / (m 2 ·day·atm).
[0111] In the multilayer structure of the present invention, the sheet is folded in four so that the paper layer (A) is on the outside of the moisture-proof resin layer (E), and in this state, a load of 5 kg is applied from above and left to stand for one minute to perform a folding treatment. After that, the oxygen transmission rate measured under conditions of 20°C and 65% RH according to the method described in JIS K 7126-2:2006 is 1.0 cc / (m 2 ·day·atm), and preferably less than 0.2cc / (m 2 ·day·atm). Since the oxygen transmission rate after folding is less than the above upper limit, the paper can be particularly suitably used as a molding material for paper containers which are usually folded. On the other hand, the lower limit of the oxygen transmission rate after folding is less than 0.002 cc / (m 2 ·day·atm), and 0.02cc / (m 2 ·day·atm).
[0112] The multilayer structure of the present invention can be crushed for reuse, separated into the paper layer (A) and the portion other than the paper layer (A), and the portion other than the paper layer (A) can be used as a melt molding material. By using the portion of the multilayer structure other than the paper layer (A) as a melt molding material, a melt molded product (recycled product) with few defects can be obtained. The portion of the multilayer structure other than the paper layer (A) can be mixed with other melt molding materials (other recycled resins, unused resins, etc.). The separated paper layer (A) can also be reused.
[0113] The method for producing the multilayer structure of the present invention is not particularly limited. For example, (1) a coextruded film of a barrier resin layer (C), an adhesive resin layer (D) and a moisture-proof resin layer (E) is produced by coextrusion. (2) An inorganic vapor deposition layer (B) is provided on the barrier resin layer (C) side of the coextruded film to produce a composite film. (3) A multilayer structure is obtained by laminating paper, which is the paper layer (A), and a composite film by a known means such as sandwich lamination or dry lamination so that the paper layer (A) faces the inorganic vapor deposition layer (B) or the moisture-proof resin layer (E). When the multilayer structure of the present invention further comprises a moisture-proof resin layer (F), the moisture-proof resin layer (F) can be provided by a known method such as melt extrusion or dry lamination.
[0114] Alternatively, for example, a composite film may be prepared by providing an inorganic vapor deposition layer (B) on a monolayer film of a barrier resin layer (C), and then laminating an adhesive resin layer (D) and a moisture-proof resin layer (E). Also, a two-layer film of an inorganic vapor deposition layer (B) and a barrier resin layer (C) may be laminated with a paper layer, and then an adhesive resin layer (D) and a moisture-proof resin layer (E) may be laminated.
[0115] The multilayer structure of the present invention is preferably used as a molding material for paper containers. The use of the paper container is not particularly limited, and it may be a container for storing solids such as food, but is preferably a container for storing liquids. The multilayer structure may be used for purposes other than as a molding material for paper containers.
[0116] <Liquid paper containers> The paper container for liquids of the present invention is a paper container formed from the multilayer structure of the present invention. The paper container has high gas barrier properties even in the folded portion, has sufficient strength even in a low-temperature environment, and suppresses the occurrence of defects during recycling. The paper container for liquids is suitably used as a container for storing beverages such as milk and juice, liquid foods such as soup, alcoholic beverages such as sake and shochu, and various liquids other than food.
[0117] The paper container for liquids of the present invention is formed by folding the multilayer structure of the present invention into, for example, a box shape and bonding the overlapping parts by heat sealing, etc. In the paper container for liquids, it is preferable that the paper layer (A) is located on the outer surface. Also, it is preferable that the moisture-proof resin layer (E) or the moisture-proof resin layer (F) is located on the inner surface.
[0118] The shape of the paper container for liquid of the present invention is not limited to a box shape, and may be other shapes (e.g., bag shape, etc.). The paper container for liquid may be bonded by a method other than heat sealing, and may have a portion bonded by heat sealing and a portion bonded by another method. In addition, the paper container for liquid may further include a member other than the multilayer structure of the present invention. EXAMPLES
[0119] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples.
[0120] [Example 1] (1) Preparation of EVOH (c)-containing resin composition for barrier resin layer (C) EVOH (c-1) (ethylene unit content 32 mol%, saponification degree 99.99 mol%, MFR (190°C, 2.16 kg load) 1.6 g / 10 min, sodium acetate 220 ppm in terms of sodium ion, phosphate ion 30 ppm in terms of phosphate radical, boric acid 150 ppm in terms of boron element, no polyvalent metal ions) and magnesium stearate (Mg-St) were melt-kneaded so that the magnesium ion content in the resulting resin composition was 50 ppm, to obtain resin composition pellets for the barrier resin layer (C). The extruder used for melt-kneading was a twin-screw extruder with D (mm) = 25, and a unidirectional fully intermeshing screw with L / D = 25 was used. The resin temperature was set to 220°C.
[0121] (2) Resin composition containing adhesive resin (d) for adhesive resin layer (D) Maleic anhydride modified polyethylene "ADMER (trademark) NF518" manufactured by Mitsui Chemicals Inc. (MFR (190°C, 2.16 kg load) 3.1 g / 10 min, density 0.91 g / cm 3 The adhesive resin (d-1) was prepared by subjecting the resin composition to an acid value of 1.8 mgKOH / g and an acid value of 1.8 mgKOH / g. The pellets of the adhesive resin (d-1) were used as they were as the resin composition pellets for the adhesive resin layer (D).
[0122] (3) Polyethylene (e)-containing resin composition for moisture-proof resin layer (E) DOW's low-density polyethylene (LDPE) "INNATE (trademark) TF80" (MFR (190°C, 2.16 kg load) 1.6 g / 10 min, density 0.926 g / cm 3 The pellets of polyethylene (e-1) were used as they were as the resin composition pellets for the moisture-proof resin layer (E).
[0123] (4) Preparation of co-extruded film Using the resin composition pellets of each of (1) to (3), a coextrusion film having a layer thickness and layer structure of C / D / E=4μm / 4μm / 32μm=EVOH4 / tie4 / PE32 was produced by a coextrusion film-forming facility. "Tie" stands for adhesive resin. The average thickness of the layers is also simply called the layer thickness. All extruders were single-screw extruders with D(mm)=30, and full-flight screws with L / D=28 and compression ratio of 3.0 were used. As the die, a 350mm wide feed block lamination type T die was used. The temperature conditions at this time are shown below. Extrusion temperature of barrier resin layer (C): feeding section / compression section / metering section / adapter = 175 / 220 / 220 / 220℃ Extrusion temperature of adhesive resin layer (D): feeding section / compression section / metering section / adapter = 175 / 220 / 220 / 220°C Extrusion temperature of moisture-proof resin layer (E): Feeding section / compression section / metering section / adapter = 175 / 220 / 220 / 220℃ Die temperature: 220℃ Cooling roll temperature: 80℃
[0124] (5) Preparation of composite film A 50 nm-thick aluminum metal vapor deposition layer (inorganic vapor deposition layer (B)) was laminated by a known vacuum deposition method on the surface of the barrier resin layer (C) of the co-extruded film obtained in (4) above, to produce a composite film having layer thicknesses and a layer structure of B / C / D / E=50 nm / 4 μm / 4 μm / 32 μm=Al (50 nm) / EVOH4 / tie4 / PE32.
[0125] (6) Fabrication of multilayer structures Paper layer (A) with a basis weight of 250 g / m 2 A white paperboard having the above composition was prepared. In addition, a linear low-density polyethylene (LLDPE) "LUMITAC (trademark) BL 600K" (MFR (190°C, 2.16 kg load) 21 g / 10 min, density 0.898 g / cm) manufactured by Tosoh Corporation was used as the extrusion lamination resin (thermoplastic resin). 3 ) was prepared. The white paperboard is fed from the first feed section of the extrusion lamination equipment, the composite film obtained in (5) is fed from the second feed section, and the linear low-density polyethylene is extruded between them at 300°C to laminate a linear low-density polyethylene layer (thermoplastic resin layer (X)) having an average thickness of 20 μm therebetween, and the resulting laminate has a thickness of A / X / B / C / D / E=250 g / m 2 A multilayer structure was prepared with layer thicknesses and layer configurations of paper / PE20 / Al(50 nm) / EVOH4 / tie4 / PE32 / 20 μm / 50 nm / 4 μm / 4 μm / 32 μm.
[0126] In addition, the resins constituting the barrier resin layer (C), adhesive resin layer (D), moisture-proof resin layer (E) and thermoplastic resin layer (X) in the obtained multilayer structure all have a predetermined MFR at 190° C. Therefore, it is clear that the melting points of these resins are lower than 200° C. The same applies to the other examples described later.
[0127] (7) Oxygen transmission rate (OTR) of multilayer structure For the multilayer structure obtained in (6) above, the oxygen transmission rate was measured in accordance with the method described in JIS K 7126-2 (isobaric method; 2006) with the paper layer as the oxygen supply side and the composite film as the carrier gas side. Specifically, the oxygen transmission rate (unit: cc / (m)) was measured using an oxygen transmission amount measuring device ("MOCON OX-TRAN2 / 21" manufactured by Modern Control) under conditions of temperature 20°C, humidity 65% RH on the oxygen supply side, humidity 65% RH on the carrier gas side, oxygen pressure 1 atm, and carrier gas pressure 1 atm. 2 The gas barrier properties were measured and judged according to the following criteria. Nitrogen gas containing 2% by volume of hydrogen gas was used as the carrier gas. The results are shown in Table 2. In the cases of A to D, the gas barrier properties were judged to be high even without bending treatment. Judgment criteria A: 0.05cc / (m 2 ·day·atm) B: 0.05cc / (m 2 ·day · atm) or more, 0.1cc / (m 2 ·day·atm) C: 0.1cc / (m 2 ·day · atm) or more, 0.5cc / (m 2 ·day·atm) D: 0.5cc / (m 2 ·day · atm) or more, 2.0cc / (m 2 ·day·atm) E: 2.0cc / (m 2 ·day · atm) or more
[0128] (8) Oxygen transmission rate after bending of multilayer structure (OTR after bending) The multilayer structure obtained in (6) above was cut into a 10 cm square, folded in four so that the paper layer (A) was on the outside of the moisture-proof resin layer (E), and in this state, a 5 kg load was applied from above and left to stand for 1 minute, thereby performing a folding treatment. After folding, the 2 kg load was removed, and the multilayer structure was opened with the folds, and the oxygen transmission rate was measured in accordance with the method described in JIS K 7126-2 (isobaric method; 2006) with the paper layer (A) as the oxygen supply side and the composite film as the carrier gas side. Specifically, the oxygen transmission rate (unit: cc / (m)) was measured using an oxygen transmission amount measuring device ("MOCON OX-TRAN2 / 21" manufactured by Modern Control) under conditions of temperature 20°C, humidity 65% RH on the oxygen supply side, humidity 65% RH on the carrier gas side, oxygen pressure 1 atm, and carrier gas pressure 1 atm. 2 The gas barrier properties after bending were determined to be high. ... Judgment criteria A: 0.1cc / (m 2 ·day·atm) B: 0.1cc / (m 2 ·day · atm) or more, 0.2cc / (m 2 ·day·atm) C: 0.2cc / (m 2 ·day · atm) or more, 1.0cc / (m 2 ·day·atm) D: 1.0cc / (m 2 ·day · atm) or more, 4.0cc / (m 2 ·day·atm) E: 4.0cc / (m 2 ·day · atm) or more
[0129] (9) Drop resistance of multi-layered structure (drop strength (low temperature)) The multilayer structure obtained in (6) above was cut into two pieces measuring 12 cm x 24 cm, which were stacked so that the paper layers (A) were on the outside of each other, and the three sides were heat-sealed at a width of 5 mm. Next, 500 g of water was filled from the opening, and the remaining sides were heat-sealed to create a water-filled paper container. This water-filled paper container was allowed to freely drop three times in an upright position from a height of 1 m at 5°C, and the presence or absence of water leakage was observed. Ten water-filled paper containers were produced by the above method, and the ten containers were evaluated and judged according to the following criteria. The results are shown in Table 2. It was determined that in the cases of A to D, paper containers having sufficient strength could be formed even in a low-temperature environment. Judgment criteria A: Not a single leak was observed. B: One or two water leaks were found. C: 3 to 5 water leaks were found. D: 6 to 8 water leaks were found. E: 9 to 10 water leaks were found.
[0130] (10) Paper detectability The multilayer structure obtained in (6) above was subjected to infrared spectrum measurement on both sides by a total reflection measurement method, and when paper was detected on either side, it was judged as pass (OK), and when paper was not detected on either side, it was judged as fail (NG). The results are shown in Table 2.
[0131] (11) Polyethylene detectability The multilayer structure obtained in (6) above was subjected to infrared spectrum measurement on both sides by a total reflection measurement method, and when polyethylene was detected on either side, it was judged as passing (OK), and when paper was not detected on either side, it was judged as failing (NG). The results are shown in Table 2.
[0132] (12) Recyclability of parts other than the paper layer separated from the multi-layer structure The multilayer structure obtained in (6) above was crushed to a size of 4 mm square or less, and stirred in a 90°C aqueous sodium hydroxide solution (1 mol / L) for 30 minutes to remove the paper layer (A) from the multilayer structure. The parts other than the paper layer (A) floating in the aqueous solution were then collected, washed with water at room temperature, and dried at 60°C for 24 hours. This collected material and a low-density polyethylene resin (LDPE) "Novatec (trademark) LD LJ400" (MFR (190°C, 2.16 kg load) 1.5 g / 10 min, density 0.921 g / cm) manufactured by Japan Polyethylene Corporation were mixed together. 3 ) was blended in a mass ratio (recycled material / low-density polyethylene resin) of 40 / 60, and a monolayer film was formed under the extrusion conditions shown below to obtain a monolayer film having a thickness of 50 μm. As a control, a monolayer film having a thickness of 50 μm was obtained similarly using only the low-density polyethylene resin. The extruder was a single-screw extruder with D (mm) = 20, and a full-flight screw with L / D = 20 and a compression ratio of 3.5 was used. A T-die with a width of 300 mm was used as the die. The thickness of the monolayer film was adjusted by appropriately changing the screw rotation speed and the take-up roll speed. The temperature conditions at this time are shown below. Extrusion temperature: feeding section / compression section / metering section / adapter = 175 / 220 / 220 / 220℃ Die temperature: 220℃ Cooling roll temperature: 80℃ The obtained monolayer films were visually evaluated for coloration and defects and judged according to the following criteria. The results are shown in Table 2. In the cases of A to D, it was determined that the occurrence of coloration or defects during recycling was suppressed. Judging color: Criteria A: The degree of color change was small compared to the control. B: Slight discoloration was observed compared to the control. C: Moderate coloring was observed compared to the control. D: Significant coloring was observed compared to the control. E: Compared to the target, significant coloring and unevenness were observed. Determining defects: criteria A: Compared to the control, the amount of pimples was almost the same. B: The amount of small particles was slightly more than in the control. C: Compared to the control, the amount of small bumps was greater. D: Compared to the control, there was a greater amount of large bumps. E: The amount of large particles was significantly greater than in the control.
[0133] [Example 2] Resin composition pellets, coextruded films, composite films and multilayer structures were produced in the same manner as in Example 1, except that EVOH (c-2) (ethylene unit content 27 mol%, saponification degree 99.99 mol%, MFR (210°C, 2.16 kg load) 4.0 g / 10 min, sodium acetate 220 ppm in terms of sodium ions, phosphate ions 30 ppm in terms of phosphate radicals, boric acid 150 ppm in terms of boron element, no polyvalent metal ions) was used instead of EVOH (c-1), and various measurements and evaluations were performed. The results are shown in Table 2.
[0134] [Example 3] Resin composition pellets, coextruded films, composite films and multilayer structures were produced in the same manner as in Example 1, except that EVOH (c-3) (ethylene unit content 44 mol%, saponification degree 99.99 mol%, MFR (190°C, 2.16 kg load) 5.7 g / 10 min, sodium acetate 220 ppm calculated as sodium ion, phosphate ion 30 ppm calculated as phosphate radical, no polyvalent metal ions) was used instead of EVOH (c-1), and various measurements and evaluations were performed. The results are shown in Table 2.
[0135] [Example 4] Except for using a mixture (dry blend) of EVOH (c-2) and EVOH (c-3) in a mass ratio of 75 / 25 instead of EVOH (c-1), resin composition pellets, coextruded films, composite films, and multilayer structures were produced in the same manner as in Example 1, and various measurements and evaluations were carried out. The results are shown in Table 2.
[0136] [Example 5] Except for changing the average thickness of the aluminum metal vapor deposition layer to 100 nm, resin composition pellets, coextruded films, composite films, and multilayer structures were produced in the same manner as in Example 1, and various measurements and evaluations were carried out. The results are shown in Table 2.
[0137] [Example 6] Except for changing the aluminum metal deposition layer to an alumina (AlOx) deposition layer, resin composition pellets, coextruded films, composite films, and multilayer structures were produced in the same manner as in Example 1, and various measurements and evaluations were carried out. The results are shown in Table 2.
[0138] [Example 7] Except for changing the aluminum metal deposition layer to a silica (SiOx) deposition layer, resin composition pellets, coextruded films, composite films, and multilayer structures were produced in the same manner as in Example 1, and various measurements and evaluations were carried out. The results are shown in Table 2.
[0139] [Example 8] Except for not using magnesium stearate, resin composition pellets, a coextruded film, a composite film and a multilayer structure were produced in the same manner as in Example 1, and various measurements and evaluations were carried out. The results are shown in Table 2.
[0140] [Examples 9 to 10] Except for changing the amount of magnesium stearate kneaded with EVOH (c-1) in terms of magnesium ions as shown in Table 1, resin composition pellets, coextruded films, composite films, and multilayer structures were produced in the same manner as in Example 1, and various measurements and evaluations were carried out. The results are shown in Table 2.
[0141] [Examples 11 to 12] Except for changing the magnesium stearate kneaded with EVOH (c-1) to calcium stearate (Ca-St) (Example 11) or zinc stearate (Zn-St) (Example 12), resin composition pellets, co-extruded films, composite films, and multilayer structures were produced in the same manner as in Example 1, and various measurements and evaluations were carried out. The results are shown in Table 2.
[0142] [Example 13] Instead of polyethylene (e-1), polyethylene (e-2) (linear low-density polyethylene (mLLDPE) "Evolue (trademark) SP1510" (MFR (190 °C, 2.16 kg load) 1.0 g / 10 min, density 0.915 g / cm) manufactured by Prime Polymer Co., Ltd., polymerized with a metallocene catalyst) was used. 3 ) was used, resin composition pellets, a coextruded film, a composite film and a multilayer structure were produced in the same manner as in Example 1, and various measurements and evaluations were carried out. The results are shown in Table 2.
[0143] [Example 14] Instead of polyethylene (e-1), polyethylene (e-3) (high density polyethylene (HDPE) "Novatec (trademark) HD HY540" manufactured by Japan Polyethylene Co., Ltd. (MFR (190°C, 2.16 kg load) 1.0 g / 10 min, density 0.960 g / cm) 3 ) was used, resin composition pellets, a coextruded film, a composite film and a multilayer structure were produced in the same manner as in Example 1, and various measurements and evaluations were carried out. The results are shown in Table 2.
[0144] [Example 15] Except for changing the average thickness of the barrier resin layer (C) to 12 μm, resin composition pellets, coextruded films, composite films, and multilayer structures were produced in the same manner as in Example 1, and various measurements and evaluations were carried out. The results are shown in Table 2.
[0145] [Example 16] Except for changing the average thickness of the moisture-proof resin layer (E) to 52 μm, resin composition pellets, coextruded films, composite films, and multilayer structures were produced in the same manner as in Example 1, and various measurements and evaluations were carried out. The results are shown in Table 2.
[0146] [Example 17] Except for laminating the paper layer and the composite film by a known dry lamination instead of extrusion lamination, resin composition pellets, co-extruded film, composite film, and multilayer structure were produced in the same manner as in Example 1, and various measurements and evaluations were carried out. The results are shown in Table 2. A two-liquid reactive polyurethane adhesive was used as the adhesive for dry lamination, and was used so that the average thickness after drying would be 4 μm.
[0147] [Example 18] A moisture-proof resin layer (F) was applied to the exposed surface of the paper layer (A) of the multilayer structure obtained by the same procedure as in Example 1 using a linear low-density polyethylene (LLDPE) "LUMITAC (trademark) BL 600K" (MFR (190°C, 2.16 kg load) 21 g / 10 min, density 0.898 g / cm) manufactured by Tosoh Corporation. 3 ) was extruded at 300° C. to laminate a linear low-density polyethylene layer having an average thickness of 30 μm, to prepare a multilayer structure, which was then subjected to various measurements and evaluations. The results are shown in Table 2.
[0148] [Example 19] As the preparation of the coextruded film, a coextruded film having a layer thickness and layer structure of C / D / E=5μm / 5μm / 115μm=EVOH5 / tie5 / PE115 was prepared, and stretched 5 times in the longitudinal direction to prepare a coextruded film after stretching of 1μm / 1μm / 23μm=EVOH1 / tie1 / PE23. Except for using this coextruded film, resin composition pellets, coextruded films, composite films and multilayer structures were prepared in the same manner as in Example 1, and various measurements and evaluations were performed. The results are shown in Table 2.
[0149] [Example 20] Instead of EVOH (c-1), EVOH (c-4) (ethylene unit content 44 mol%, saponification degree 99.99 mol%, epoxypropane modification degree 4.6 mol%, MFR (190°C, 2.16 kg load) 5.6 g / 10 min, sodium acetate 220 ppm in sodium ion equivalent, phosphate ion 30 ppm in phosphate radical equivalent, boric acid 150 ppm in boron element equivalent, zinc acetate 30 ppm in zinc ion equivalent) was used. In addition, as the preparation of the coextruded film, a coextruded film having a layer thickness and layer structure of C / D / E=32μm / 32μm / 736μm=EVOH32 / tie32 / PE736 was prepared, and stretched 4 times in the long direction and then 8 times in the short direction to prepare a coextruded film after stretching of 1μm / 1μm / 32μm=EVOH1 / tie1 / PE32, and this coextruded film was used. Except for these points, the resin composition pellets, coextruded film, composite film, and multilayer structure were prepared in the same manner as in Example 1, and various measurements and evaluations were performed. The results are shown in Table 2.
[0150] [Example 21] A moisture-proof resin layer (F) was formed on the exposed surface of the moisture-proof resin layer (E) of the multilayer structure obtained by the same procedure as in Example 20 using a linear low-density polyethylene (LLDPE) "LUMITAC (trademark) BL 600K" (MFR (190°C, 2.16 kg load) 21 g / 10 min, density 0.898 g / cm) manufactured by Tosoh Corporation. 3 ) was extruded at 300° C. to laminate a linear low-density polyethylene layer having an average thickness of 30 μm, to prepare a multilayer structure, which was then subjected to various measurements and evaluations. The results are shown in Table 2.
[0151] [Example 22] Paper layer (A) with a basis weight of 50 g / m 2 Except for using white paper of 1000g, resin composition pellets, a coextruded film, a composite film, and a multilayer structure were produced in the same manner as in Example 1, and various measurements and evaluations were carried out. The results are shown in Table 2.
[0152] [Example 23] Paper layer (A) has a basis weight of 80 g / m 2Except for using white paper of 1000g, resin composition pellets, a coextruded film, a composite film, and a multilayer structure were produced in the same manner as in Example 1, and various measurements and evaluations were carried out. The results are shown in Table 2.
[0153] [Example 24] Paper layer (A) has a basis weight of 150 g / m 2 Except for using white paper of 1000g, resin composition pellets, a coextruded film, a composite film, and a multilayer structure were produced in the same manner as in Example 1, and various measurements and evaluations were carried out. The results are shown in Table 2.
[0154] [Example 25] In producing the multilayer structure, the moisture-proof resin layer (E) and the paper layer (A) of the composite film were laminated via the thermoplastic resin layer (X), and a moisture-proof resin layer (F) was further provided on the exposed inorganic vapor deposition layer (B). Except for this, resin composition pellets, co-extruded film, composite film and multilayer structure were produced in the same manner as in Example 21, and various measurements and evaluations were carried out. The results are shown in Table 2.
[0155] [Comparative Example 1] Resin composition pellets, composite films and multilayer structures were produced in the same manner as in Example 1, except that the following composite films were produced and used instead of the composite film produced in Example 1, and various measurements and evaluations were carried out. Without laminating the barrier resin layer (C) and adhesive resin layer (D), a single-layer film of a moisture-proof resin layer (E) having an average thickness of 40 μm was used, one side of the moisture-proof resin layer (E) was subjected to a corona discharge treatment by a known method, and an aluminum metal vapor deposition layer was laminated on the corona discharge treated side to produce a composite film. The results are shown in Table 2.
[0156] [Comparative Example 2] Except for not laminating the barrier resin layer (C), the adhesive resin layer (D) and the aluminum metal deposition layer, and using a single-layer film of the moisture-proof resin layer (E) having an average thickness of 40 μm instead of the composite film, resin composition pellets and a multilayer structure were prepared in the same manner as in Example 1, and various measurements and evaluations were carried out. The results are shown in Table 2.
[0157] [Comparative Example 3] Except for not laminating an aluminum metal vapor deposition layer, a resin composition pellet, a co-extruded film, and a multilayer structure were produced in the same manner as in Example 1, and various measurements and evaluations were carried out. The results are shown in Table 2.
[0158] [Comparative Example 4] Resin composition pellets, composite films and multilayer structures were produced in the same manner as in Example 21, except that a biaxially oriented polyethylene terephthalate film "Lumirror (trademark) P60" (PET, melting point 256°C, average thickness 12 μm) manufactured by Toray Industries, Inc. was used instead of the coextruded film, both sides of the PET were subjected to corona discharge treatment by a known method, an aluminum metal vapor-deposited layer was laminated on one side of the PET after corona discharge treatment, and a moisture-proof resin layer (F) was laminated on the non-vapor-deposited side of the PET, and various measurements and evaluations were performed. The results are shown in Table 2.
[0159] [Comparative Example 5] Instead of the adhesive resin (d-1), a maleic anhydride modified polypropylene "Admer (trademark) QF551" manufactured by Mitsui Chemicals Inc. (MFR (230°C, 2.16 kg load) 5.7 g / 10 min, density 0.89 g / cm 3 ) was replaced with polypropylene "Novatec (trademark) PP EA7AD" (MFR (230°C, 2.16 kg load) 1.4 g / 10 min, density 0.90 g / cm) manufactured by Japan Polypropylene Corporation instead of polyethylene (e-1). 3 ) was used as the thermoplastic resin layer (X). Instead of linear low-density polyethylene, polypropylene "Novatec (trademark) PP FL03H" (MFR (230°C, 2.16 kg load) 26 g / 10 min, density 0.90 g / cm3) manufactured by Japan Polypropylene Corporation was used. 3 Except for using the above-mentioned 1, resin composition pellets, a coextruded film, a composite film, and a multilayer structure were prepared in the same manner as in Example 1, and various measurements and evaluations were carried out. The results are shown in Table 2.
[0160] [Comparative Example 6] On the exposed surface of the moisture-proof resin layer (E), a moisture-proof resin layer (F) was formed using a linear low-density polyethylene (LLDPE) "LUMITAC (trademark) BL 600K" (MFR (190°C, 2.16 kg load) 21 g / 10 min, density 0.898 g / cm) manufactured by Tosoh Corporation. 3 Except for extruding the copolymer of 1,2-dichloroethylene and 1,2-dichloroethylene at 300° C. to form a linear low-density polyethylene layer having an average thickness of 30 μm, resin composition pellets, a coextruded film, a composite film, and a multilayer structure were prepared in the same manner as in Comparative Example 5, and various measurements and evaluations were carried out. The results are shown in Table 2.
[0161] Table 1 shows the type and basis weight of the paper layer (A) in each multilayer structure, the type and average thickness of the material constituting the inorganic vapor deposition layer (B), the type and ethylene unit content of the resin constituting the barrier resin layer (C), the metal species and content of the polyvalent metal ion, the type and density of the resin constituting the moisture-proof resin layer (E), and the type and density of the resin constituting the moisture-proof resin layer (F) in each multilayer structure. Table 2 also shows the layer configuration and average thickness of each layer in each multilayer structure, the stretch ratio (MD x TD) of the coextruded film, the paper layer ratio (mass ratio of the paper layer to the entire multilayer structure), and the PE ratio other than the paper layer (total average thickness ratio of layers mainly composed of polyethylene resin in parts other than the paper layer), together with the evaluation results.
[0162] [Table 1]
[0163] [Table 2]
[0164] As shown in Table 2, each of the multilayer structures of Examples 1 to 25 had high gas barrier properties both before and after folding, and it was possible to form paper containers with sufficient strength even in low-temperature environments, and it was confirmed that the occurrence of defects during recycling was suppressed. [Industrial Applicability]
[0165] The multilayer structure of the present invention can be suitably used as a molding material for paper containers such as paper containers for liquids.
Claims
1. The sheet has a paper layer (A), an inorganic vapor deposition layer (B), a barrier resin layer (C), an adhesive resin layer (D) and a moisture-proof resin layer (E), the inorganic vapor deposition layer (B), the barrier resin layer (C), the adhesive resin layer (D) and the moisture-proof resin layer (E) are all directly laminated in this order; The average thickness of the inorganic vapor deposition layer (B) is 5 nm or more and 200 nm or less, the barrier resin layer (C) comprises, as a main component, an ethylene-vinyl alcohol copolymer (c) having an ethylene unit content of 20 mol % or more and 50 mol % or less and a saponification degree of 90 mol % or more; The adhesive resin layer (D) contains an adhesive resin (d) as a main component, The moisture-proof resin layer (E) contains polyethylene (e) as a main component, does not have a layer containing as a main component a resin having a melting point of 200° C. or more and does not have a metal layer having an average thickness of 1 μm or more; The sheet was folded in four so that the paper layer (A) was on the outside of the moisture-proof resin layer (E), and in this state, a load of 5 kg was applied from above and left to stand for 1 minute to perform a folding treatment. After that, the oxygen transmission rate measured under conditions of 20°C and 65% RH according to the method described in JIS K 7126-2:2006 was 1.0 cc / (m 2 .day.atm).
2. 2. The multilayer structure according to claim 1, further comprising a thermoplastic resin layer (X) interposed between the paper layer (A) and the inorganic vapor deposition layer (B) or the moisture-proof resin layer (E).
3. 3. The multilayer structure according to claim 1, comprising a paper layer (A), an inorganic vapor deposition layer (B), a barrier resin layer (C), an adhesive resin layer (D) and a moisture-proof resin layer (E) in this order.
4. 3. The multilayer structure according to claim 1, wherein the adhesive resin (d) is an acid-modified polyethylene.
5. 3. The multilayer structure according to claim 1, wherein the inorganic vapor deposition layer (B) is a vapor deposition layer of a metal containing aluminum as a main component, or a vapor deposition layer of an inorganic oxide containing alumina or silica as a main component.
6. 3. The multilayer structure according to claim 1, wherein the ethylene-vinyl alcohol copolymer (c) comprises two or more kinds of ethylene-vinyl alcohol copolymers having different ethylene unit contents.
7. The density of polyethylene (e) is 0.880 g / cm 3 0.940g / cm or more 3 is as follows:
3. The multilayer structure according to claim 1 or 2, wherein the polyethylene (e) is a linear low density polyethylene, a low density polyethylene or a mixture thereof.
8. the laminate of the barrier resin layer (C), the adhesive resin layer (D) and the moisture-proof resin layer (E) is a co-extruded film; The average thickness of the coextruded film is 8 μm or more and 120 μm or less, The multilayer structure according to claim 1 or 2, wherein an inorganic vapor deposition layer (B) is provided on the surface of the coextruded film on the barrier resin layer (C) side.
9. 9. The multilayer structure according to claim 8, wherein the average thickness of the barrier resin layer (C) is 0.2 μm or more and less than 30 μm, and the ratio of the average thickness of the barrier resin layer (C) to the average thickness of the coextruded film is less than 25%.
10. 10. The multilayer structure of claim 8, wherein the coextruded film is substantially unoriented.
11. 9. The multilayer structure of claim 8, wherein the coextruded film is stretched at least uniaxially by a factor of 3 or more but less than 12.
12. 9. The multilayer structure of claim 8, wherein the coextruded film is biaxially stretched by at least 3 times but less than 12 times in each direction.
13. The multilayer structure according to claim 8, further comprising a moisture-proof resin layer (F) containing polyethylene (f) as a main component.
14. The density of polyethylene (f) is 0.880 g / cm 30.940g / cm or more 3 is as follows:
14. The multilayer structure of claim 13, wherein the polyethylene (f) is a linear low density polyethylene, a low density polyethylene or a mixture thereof.
15. 14. The multilayer structure according to claim 13, wherein a moisture-proof resin layer (F) is directly laminated to the coextruded film.
16. 3. The multilayer structure according to claim 1, which does not have an adhesive layer made of a curable adhesive.
17. The basis weight of the paper layer (A) is 200 g / m 2 More than 400g / m 2 3. The multilayer structure of claim 1 or 2, wherein the thickness is less than 100 nm.
18. The multilayer structure according to claim 1 or 2, wherein the mass ratio of the paper layer (A) to the entire multilayer structure is 0.60 or more.
19. 3. The multilayer structure according to claim 1, wherein the total average thickness ratio of layers containing a polyethylene resin as a main component in a portion other than the paper layer (A) is 0.75 or more.
20. 3. The multilayer structure according to claim 1, wherein the total average thickness ratio of layers containing a resin having ethylene units as a main component in a portion other than the paper layer (A) is 0.95 or more.
21. The multilayer structure according to claim 1 or 2, which has a paper layer (A) on a surface thereof.
22. The oxygen transmission rate measured by the method described in JIS K 7126-2:2006 under conditions of 20°C and 65% RH is 0.5 cc / (m 2 3. The multilayer structure according to claim 1, wherein the viscosity is less than 100 MPa (day atm).
23. A paper container for liquids, formed by molding the multilayer structure according to claim 1 or 2.
Citation Information
Patent Citations
Multilayer barrier film, packaging laminate containing the film, packaging container formed from the packaging laminate, and method for manufacturing the film.
JP2014531341A
Laminate and packaging container
JP2021160262A
Vapor-deposited film, packaging material and vacuum insulation body
JP2022007524A
Paper-made container
JP2004250025A