Cationic electrodeposition coating composition

The cationic electrodeposition coating composition, utilizing aminated epoxy resin with controlled functional groups and solubility parameters, addresses adhesion and barrier challenges, enhancing rust prevention and reducing VOCs in cationic electrodeposition paints.

JP2024149621AInactive Publication Date: 2024-10-18NIPPON PAINT AUTOMOTIVE COATINGS
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2024125616
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-10-18
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing cationic electrodeposition paints face challenges in achieving improved adhesion and barrier properties while reducing volatile organic compound (VOC) content, with existing methods struggling to further reduce solvent amounts and enhance rust prevention.

Method used

A cationic electrodeposition coating composition is formulated using an aminated epoxy resin with specific adhesion functional groups and solubility parameters, combined with a blocked polyisocyanate curing agent, to enhance adhesion and barrier properties, while minimizing VOCs by reducing the use of ketimine compounds like diketimine.

Benefits of technology

The composition achieves improved adhesion and barrier properties, resulting in enhanced rust prevention with reduced VOC emissions, demonstrating superior performance in corrosion resistance tests.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024149621000001
    Figure 2024149621000001
Patent Text Reader

Abstract

To provide a cationic electrodeposition coating composition which makes it possible to further improve the adhesive and blocking properties of a coating film produced therefrom, compared with those of the conventional coating films, thereby improving the anticorrosive properties and also achieving further reduction in VOC content.SOLUTION: The present invention discloses a cationic electrodeposition coating composition comprising an aminated epoxy resin and a blocked polyisocyanate curing agent. The number of adhesive functional groups in the aminated epoxy resin is 2.9 to 3.9 meq / solid g and the aminated epoxy resin has a solubility parameter (SP) of 10.2 to 11.6.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cationic electrodeposition coating composition, and more particularly to a cationic electrodeposition coating composition using a new aminated epoxy resin. [Background technology]

[0002] Cationic electrocoating paints are widely used as undercoats to impart corrosion resistance to industrial products such as automobiles, and contain aminated epoxy resins and blocked polyisocyanate curing agents. In addition to high rust resistance, cationic electrocoating paints require low VOC (volatile organic compounds) content, high adhesion, and high hydrophobicity (blocking properties).

[0003] The adhesion and hydrophobicity (blocking property) of cationic electrocoatings are important properties that contribute to rust prevention, and there is a constant demand for improvements. For example, JP-T-2000-501448 (Patent Document 1) discloses a cationic electrocoating composition that uses a diamine compound having a primary amino group and a tertiary amino group reacted with an epoxy resin, but further improvements are required in adhesion and blocking property.

[0004] On the other hand, focusing on low VOC, for example, JP 2011-256306 A (Patent Document 2) describes reducing the amount of organic solvent added to a coating composition by mixing or reacting a specific aromatic compound. Also, JP 2009-1781 A (Patent Document 3) proposes reducing the amount of organic solvent required in a cationic electrodeposition coating composition by using a specific xylene formaldehyde resin.

[0005] These documents aim to reduce the amount of organic solvent added to the cationic electrodeposition coating composition, but the amount of organic solvent added to the cationic electrodeposition coating composition is already very small, making it difficult to reduce this amount. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Special Publication No. 2000-501448 [Patent Document 2] JP 2011-256306 A [Patent Document 3] JP 2009-1781 A Summary of the Invention [Problem to be solved by the invention]

[0007] The present invention provides a cationic electrodeposition coating composition which has improved adhesion and barrier properties of the coating film obtained from the cationic electrodeposition coating composition, and which can enhance rust prevention and further reduce VOC. In order to achieve the above object, the present invention focuses on and controls the amount of adhesion functional groups and the solubility parameter (SP value) which contributes to barrier properties. [Means for solving the problem]

[0008] That is, the present invention provides the following aspects: [1] A cationic electrodeposition coating composition containing an aminated epoxy resin and a blocked polyisocyanate curing agent, A cationic electrodeposition coating composition, characterized in that the aminated epoxy resin has an adhesion functional group number of 2.9 to 3.9 meq / solid g and a solubility parameter (SP) of 10.2 to 11.6. [2] A cationic electrodeposition coating composition comprising an aminated epoxy resin and a blocked polyisocyanate curing agent, a solubility parameter (SP) of a mixture of the aminated epoxy resin and the blocked polyisocyanate curing agent is 9.9 to 11.3; and, The cationic electrodeposition coating composition according to [1], characterized in that after the cationic electrodeposition coating composition is applied to a steel plate so as to have a dry film thickness of 15 μm and baked at 170° C. for 20 minutes, the remaining adhesion functional group is 1.4 to 2.4 meq / solid g. [3] The cationic electrodeposition coating composition according to [1] or [2], wherein the aminated epoxy resin is obtained by amminating an epoxy resin with a diamine having a primary amino group and a secondary or tertiary amino group. [4] The cationic electrodeposition coating composition according to [3], wherein the epoxy resin is a reaction product of epichlorohydrin and a polycyclic phenol compound, and the oxirane ring in the reaction product is chain-extended with a chain extender. [5] The cationic electrodeposition coating composition according to any one of [2] to [4], wherein the diamine having a primary amino group and a secondary or tertiary amino group is N,N-dimethyl-1,3-propanediamine, N-(3-aminopropyl)diethanolamine, dimethylaminoethylamine, or a mixture thereof. Effect of the Invention

[0009] In the present invention, it has been found that by controlling the number of adhesive functional groups of the aminated epoxy resin in a cationic electrodeposition coating composition containing an aminated epoxy resin and a blocked polyisocyanate curing agent to 2.9-3.9 meq / solid g and the solubility parameter (SP) to 10.2-11.6, adhesion and barrier properties are improved and a coating film with even higher rust prevention properties can be obtained. In addition, in the present invention, when producing an aminated epoxy resin, the ketimine compounds that have been commonly used up until now, particularly diketimine compounds having two ketimine groups, are used as little as possible, or not at all, and instead, the resin is aminated with a diamine having a primary amino group and a secondary or tertiary amino group that is not blocked with another ketimine, thereby ensuring a high number of functional groups and achieving hydrophobization, thereby enabling the resin to exhibit performance similar to that of the past. As already mentioned, since no or very little ketimine compounds are used, no blocking agent (e.g., methyl isobutyl ketone (MIBK)) is produced when the primary amino group blocked by ketimine is deblocked, suppressing the generation of VOCs. In this case, the primary amino group in the diamine having a primary amino group not blocked by ketimine and a secondary or tertiary amino group is consumed in the reaction with the epoxy resin, so that the primary amino group does not exist in the obtained aminated epoxy resin, and the remaining secondary or tertiary amino group achieves high basicity, increases the number of neutralization points, and contributes to emulsification and adhesion.

[0010] In the present invention, as described above, the aminated epoxy resin is characterized by having an adhesion functional group number of 2.9 to 3.9 meq / solid g and a solubility parameter (SP) of 10.2 to 11.6. By controlling the adhesion functional group number and the solubility parameter (SP) within a specific numerical range, the corrosion resistance of the finally obtained multi-layer coating film can be improved. To control these numerical values, the diamine having a primary amino group and a secondary or tertiary amino group that is not blocked with ketimine may need to have a hydroxyl group. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The cationic electrodeposition coating composition of the present invention contains an aminated epoxy resin and a blocked polyisocyanate curing agent, and is characterized in that the aminated epoxy resin has an adhesion functional group number of 2.9 to 3.9 meq / solid g and a solubility parameter (SP) of 10.2 to 11.6. In this specification, when a numerical range is expressed as "a to b" (a and b both represent numerical values), it means a or more and b or less.

[0012] <Aminified epoxy resin> Aminated epoxy resins are film-forming resins that form electrodeposition coatings. Aminated epoxy resins are obtained by modifying the oxirane rings (also called "epoxy groups") of epoxy resins with amine compounds, i.e., by aminating them.

[0013] The starting epoxy resin is a polyphenol polyglycidyl ether type epoxy resin, which is a reaction product of a polycyclic phenol compound such as bisphenol A, bisphenol F, bisphenol S, phenol novolac, or cresol novolac with epichlorohydrin. In this specification, the term "polyphenol polyglycidyl ether type epoxy resin" includes a state in which a polyphenol polyglycidyl ether type epoxy resin and a polycyclic phenol compound have reacted (chain extension reaction). In this amine modification step, it is preferable to use an epoxy resin in which a polyphenol polyglycidyl ether type epoxy resin and a polycyclic phenol compound have reacted (chain extension reaction). The reaction conditions for the chain extension reaction of the polyphenol polyglycidyl ether type epoxy resin and the polycyclic phenol compound can be appropriately selected depending on the stirring device and reaction scale used. Examples of reaction conditions include conditions in which the reaction is performed at 85 to 180°C for 0.1 to 8 hours, and more preferably at 100 to 150°C for 2 to 8 hours. As the stirring device used, a stirring device generally used in the paint field can be used.

[0014] Other examples of starting resins include the oxazolidone ring-containing epoxy resins described in JP-A-5-306327. These epoxy resins can be prepared by reacting epichlorohydrin with a diisocyanate compound or a bis-urethane compound obtained by blocking the isocyanate group of a diisocyanate compound with a lower alcohol such as methanol or ethanol.

[0015] Before the amine modification, a part of the epoxy resin may be chain-extended with a bifunctional polyester polyol, polyether polyol (e.g., a polyol having a polyethylene oxide group, a polyol having a polypropylene oxide group, etc.), a dibasic carboxylic acid, or the like. For example, when a polyol having a polypropylene oxide group is used for the chain-extension reaction, a polypropylene oxide group-containing epoxy resin is obtained. An example of this embodiment is a state in which a polyphenol polyglycidyl ether type epoxy resin, a polycyclic phenol compound, and a polypropylene oxide group-containing epoxy resin are reacted (chain-extension reaction). When the epoxy resin to be reacted with the amine compound in the amine modification step contains a polypropylene oxide group-containing epoxy resin, the content of the polypropylene oxide group-containing epoxy resin is preferably 1 to 40 parts by mass, more preferably 15 to 25 parts by mass, relative to 100 parts by mass of the epoxy resin.

[0016] In general, the oxirane ring of the epoxy resin is reacted with an amine compound to obtain an aminated epoxy resin. Conventionally, the amine compound used to form the aminated epoxy resin is prepared by blocking a ketimine compound, particularly an amino compound having two primary amino groups in one molecule, with a ketone to obtain a diketimine, which is then introduced into an epoxy resin and then deblocked. However, in the present invention, it is necessary to amine the epoxy resin without using a ketimine compound as much as possible. The formation of a ketimine group requires blocking with a ketone compound (generally, methyl isobutyl ketone), which regenerates the ketone compound during deblocking and becomes a volatile organic compound (VOC), so it is preferable to avoid using a ketimine compound, particularly a diketimine compound, as much as possible in order to achieve low VOC.

[0017] In the present invention, as described above, it is preferable to avoid using ketimine compounds as much as possible, so a diamine having a primary amino group not blocked with ketimine and a secondary or tertiary amino group is used as an amine compound. In this case, the primary amino group is not blocked with a ketimine compound as in the past, but is consumed in the amination reaction of the epoxy resin and is used to form a branched chain of the aminated epoxy resin. As a diamine having a primary amino group not blocked with ketimine and a secondary or tertiary amino group, it is preferable to use a diamine having a primary amino group and a tertiary amino group such as N,N-dimethyl-1,3-propanediamine or dimethylaminoethylamine, or a diamine having an extra hydroxyl group in addition to a primary amino group and a tertiary amino group such as N-(3-aminopropyl)diethanolamine for amination. The presence of a hydroxyl group compensates for the lack of functional groups that contribute to adhesion and curability due to the absence of a ketimine compound, and is used to control the amount of adhesive functional groups described later. In the present invention, it is necessary to use a diamine having a primary amino group and a secondary or tertiary amino group that are not blocked with these ketimines, or an amino compound having an extra hydroxyl group in addition to a primary amino group (particularly referred to as a "high amine strength diamine" in this specification). The number of primary amino groups is one in the above example, but it may have multiple groups. However, since primary amino groups are highly reactive, one group is better in terms of controlling the reaction. The number of hydroxyl groups is two in the above example, but it is not limited to two in terms of contributing to adhesion and curability as described above, and may be one or more.

[0018] As the amine compound, only the diamine having high amine strength as mentioned above can be used, but a mixture of the amine compound generally used in producing aminated epoxy resin and the diamine having high amine strength as mentioned above is often used. Examples of commonly used amine compounds include primary amines such as butylamine, octylamine, and monoethanolamine; secondary amines such as diethylamine, dibutylamine, methylbutylamine, diethanolamine, and N-methylethanolamine; and complex amines such as diethylenetriamine. In the present invention, it is better not to use amine compounds having ketimine groups or diketimine groups, but this does not mean that they cannot be used, and they can be used as long as they satisfy the above-mentioned number of adhesion functional groups and solubility parameter (SP). Examples of amine compounds having ketimine groups or diketimine groups that can be used include ketimine of aminoethylethanolamine and diketimine of diethylenetriamine. In addition, tertiary amines that may be used as necessary may be used, and specific examples thereof include, for example, triethylamine, N,N-dimethylbenzylamine, and N,N-dimethylethanolamine. These amines may be used alone or in combination of two or more kinds.

[0019] In the amine modification step, the amount of the amine compound reacted with the epoxy resin is preferably 0.9 to 1.2 equivalents per equivalent of the epoxy group in the epoxy resin.

[0020] The reaction conditions for reacting the epoxy resin with the amine compound to modify it with an amine can be appropriately selected depending on the reaction scale, etc. Examples of the reaction conditions include reaction at 80 to 150° C. for 0.1 to 5 hours, and more preferably reaction at 120 to 150° C. for 0.5 to 3 hours.

[0021] The aminated epoxy resin of the present invention is required to have an adhesion functional group number of 2.9 to 3.9 meq / solid g and a solubility parameter (SP) of 10.2 to 11.6. The adhesion functional group number is the number of adhesion functional groups present in the aminated epoxy resin, and can be determined by theoretical calculation from the number of functional groups contained in each raw material and the amount of each raw material. The adhesion functional group number is preferably 3.2 to 3.9 meq / solid g, and more preferably 3.6 to 3.9 meq / solid g. If the adhesion functional group number is less than 2.9 meq / solid g, the adhesion of the coating film is insufficient. On the other hand, if the adhesion functional group number is more than 3.9 meq / solid g, the hydrophobicity of the resin is insufficient. The solubility parameter (SP) is an index that indicates the solubility of the resin, and can be determined by a turbidity point titration method using water, which is a poor solvent with a high SP value, and n-hexane, which is a poor solvent with a low SP value. Details of the solubility parameter (SP) are described in the examples of this specification. The solubility parameter (SP) value is preferably 10.2 to 11.3, and more preferably 10.2 to 10.9. It is difficult to make the solubility parameter (SP) of the aminated epoxy resin of the present invention smaller than 10.2 from the viewpoint of compatibility with the number of adhesive functional groups, and if the solubility parameter (SP) is higher than 11.6, the hydrophobicity of the resin is insufficient.

[0022] The number average molecular weight of the aminated epoxy resin is preferably in the range of 1,000 to 7,000. By having a number average molecular weight of 1,000 or more, the physical properties such as solvent resistance and corrosion resistance of the obtained cured electrodeposition coating film become good. On the other hand, by having a number average molecular weight of 7,000 or less, the viscosity of the aminated epoxy resin can be easily adjusted, making smooth synthesis possible, and the emulsion dispersion of the obtained aminated epoxy resin can be easily handled. The number average molecular weight of the aminated epoxy resin is more preferably in the range of 1,500 to 4,000.

[0023] The amine value of the aminated epoxy resin is preferably within the range of 20 to 100 mgKOH / g. When the amine value of the aminated epoxy resin is 20 mgKOH / g or more, the emulsion dispersion stability of the aminated epoxy resin in the electrodeposition coating composition is good. On the other hand, when the amine value is 100 mgKOH / g or less, the amount of amino groups in the cured electrodeposition coating film becomes appropriate, and there is no risk of reducing the water resistance of the coating film. The amine value of the aminated epoxy resin is more preferably within the range of 20 to 80 mgKOH / g.

[0024] The hydroxyl value of the aminated epoxy resin is preferably within the range of 150 to 650 mgKOH / g. When the hydroxyl value is 150 mgKOH / g or more, the cured electrodeposition coating film is cured well, and the coating film appearance is improved. On the other hand, when the hydroxyl value is 650 mgKOH / g or less, the amount of hydroxyl groups remaining in the cured electrodeposition coating film becomes appropriate, and there is no risk of reducing the water resistance of the coating film. The hydroxyl value of the aminated epoxy resin is more preferably within the range of 150 to 400 mgKOH / g.

[0025] In the electrodeposition coating composition of the present invention, by using an aminated epoxy resin (A) having a number average molecular weight in the range of 1,000 to 7,000, an amine value of 20 to 100 mgKOH / g, and a hydroxyl value of 150 to 650 mgKOH / g, more preferably 150 to 400 mgKOH / g, there is an advantage in that excellent corrosion resistance can be imparted to the substrate.

[0026] As the aminated epoxy resin, aminated epoxy resins having different amine values ​​and / or hydroxyl values ​​may be used in combination as necessary. When two or more aminated epoxy resins having different amine values ​​and hydroxyl values ​​are used in combination, the average amine value and average hydroxyl value calculated based on the mass ratio of the aminated epoxy resins used are preferably in the above-mentioned numerical range. As the aminated epoxy resins to be used in combination, it is preferable to use an aminated epoxy resin having an amine value of 20 to 50 mgKOH / g and a hydroxyl value of 50 to 300 mgKOH / g in combination with an aminated epoxy resin having an amine value of 50 to 200 mgKOH / g and a hydroxyl value of 200 to 500 mgKOH / g in combination. When such a combination is used, there is an advantage that the core part of the emulsion becomes more hydrophobic and the shell part becomes hydrophilic, thereby imparting excellent corrosion resistance.

[0027] The aminated epoxy resin may contain an amino group-containing acrylic resin, an amino group-containing polyester resin, or the like, as necessary.

[0028] <Blocked polyisocyanate curing agent> A blocked polyisocyanate curing agent (hereinafter, sometimes simply referred to as a "curing agent") is a coating film-forming resin that constitutes an electrodeposition coating film. The blocked polyisocyanate curing agent can be prepared by blocking a polyisocyanate with a sealing agent.

[0029] Examples of polyisocyanates include aliphatic diisocyanates such as hexamethylene diisocyanate (including trimer), tetramethylene diisocyanate, and trimethylhexamethylene diisocyanate; alicyclic polyisocyanates such as isophorone diisocyanate and 4,4'-methylenebis(cyclohexylisocyanate); and aromatic diisocyanates such as 4,4'-diphenylmethane diisocyanate, tolylene diisocyanate, and xylylene diisocyanate.

[0030] Examples of the sealing agent that can be preferably used include monovalent alkyl (or aromatic) alcohols such as n-butanol, n-hexyl alcohol, 2-ethylhexanol, lauryl alcohol, phenol carbinol, and methylphenyl carbinol; cellosolves such as ethylene glycol monohexyl ether and ethylene glycol mono 2-ethylhexyl ether; polyether-type both-terminal diols such as polyethylene glycol, polypropylene glycol, and polytetramethylene ether glycol phenol; polyester-type both-terminal polyols obtained from diols such as ethylene glycol, propylene glycol, and 1,4-butanediol and dicarboxylic acids such as oxalic acid, succinic acid, adipic acid, suberic acid, and sebacic acid; phenols such as para-t-butylphenol and cresol; oximes such as dimethyl ketoxime, methyl ethyl ketoxime, methyl isobutyl ketoxime, methyl amyl ketoxime, and cyclohexanone oxime; and lactams represented by ε-caprolactam and γ-butyrolactam.

[0031] The blocking rate of the blocked polyisocyanate curing agent is preferably 100%, which has the advantage of improving the storage stability of the electrodeposition coating composition.

[0032] As the blocked polyisocyanate curing agent, it is preferable to use in combination a curing agent prepared by blocking an aliphatic diisocyanate with a blocking agent and a curing agent prepared by blocking an aromatic diisocyanate with a blocking agent.

[0033] The blocked polyisocyanate curing agent reacts preferentially with the primary amine of the aminated epoxy resin, and then reacts with the hydroxyl group to cure. As the curing agent, at least one curing agent selected from the group consisting of organic curing agents such as melamine resins or phenolic resins, silane coupling agents, and metal curing agents may be used in combination with the blocked isocyanate curing agent.

[0034] Preparation of resin emulsion The resin emulsion can be prepared by dissolving the aminated epoxy resin and the blocked polyisocyanate curing agent in an organic solvent to prepare a solution, mixing these solutions, and then neutralizing the mixture with a neutralizing acid. Examples of the neutralizing acid include organic acids such as methanesulfonic acid, sulfamic acid, lactic acid, dimethylolpropionic acid, formic acid, and acetic acid. In the present invention, it is more preferable to neutralize the resin emulsion containing the aminated epoxy resin and the curing agent with one or more acids selected from the group consisting of formic acid, acetic acid, and lactic acid.

[0035] The content of the blocked polyisocyanate curing agent is required to be sufficient to react with active hydrogen-containing functional groups such as primary amino groups, secondary amino groups, or hydroxyl groups in the aminated epoxy resin during curing to give a good cured coating film. The preferred content of the curing agent is in the range of 90 / 10 to 50 / 50, more preferably 80 / 20 to 65 / 35, expressed as the solid content mass ratio of the aminated epoxy resin to the curing agent (aminated epoxy resin / curing agent). By adjusting the solid content mass ratio of the aminated epoxy resin to the blocked polyisocyanate curing agent, the fluidity and curing speed of the coating film (deposited film) during film formation are improved, and the coating appearance is improved.

[0036] The solid content of the resin emulsion is usually 25 to 50 mass %, and preferably 35 to 45 mass %, based on the total amount of the resin emulsion. Here, the "solid content of the resin emulsion" refers to the mass of all components contained in the resin emulsion that remain in a solid form even after removal of the solvent. Specifically, it refers to the total mass of the aminated epoxy resin, the curing agent, and other solid components added as necessary, contained in the resin emulsion.

[0037] The neutralizing acid is preferably used in an amount such that the equivalent ratio of the neutralizing acid to the equivalent of the amino group in the aminated epoxy resin is 10 to 100%, and more preferably 20 to 70%. In this specification, the equivalent ratio of the neutralizing acid to the equivalent of the amino group in the aminated epoxy resin is referred to as the neutralization rate. When the neutralization rate is 10% or more, affinity for water is ensured, and water dispersibility is improved.

[0038] <Pigment dispersion paste> The cationic electrodeposition coating composition of the present invention may contain a pigment dispersion paste as necessary. The pigment dispersion paste is a component optionally contained in the electrodeposition coating composition, and generally contains a pigment dispersing resin and a pigment.

[0039] Pigment Dispersion Resin The pigment dispersion resin is a resin for dispersing pigments, and is used by dispersing it in an aqueous medium. As the pigment dispersion resin, a pigment dispersion resin having a cationic group, such as a modified epoxy resin having at least one or more groups selected from a quaternary ammonium group, a tertiary sulfonium group, and a primary amino group, can be used. Specific examples of the pigment dispersion resin include a quaternary ammonium group-containing epoxy resin and a tertiary sulfonium group-containing epoxy resin. As the aqueous solvent, ion-exchanged water or water containing a small amount of alcohols is used.

[0040] Pigments Pigment is the pigment generally used in electrodeposition coating composition.Pigment can be, for example, commonly used inorganic pigment and organic pigment, for example, color pigment such as titanium white (titanium dioxide), carbon black and red iron oxide; extender pigment such as kaolin, talc, aluminum silicate, calcium carbonate, mica and clay; rust-preventive pigment such as iron phosphate, aluminum phosphate, calcium phosphate, aluminum tripolyphosphate, aluminum phosphomolybdate and aluminum zinc phosphomolybdate.

[0041] Manufacturing of pigment dispersion paste The pigment dispersion paste is prepared by mixing a pigment dispersion resin and a pigment. The content of the pigment dispersion resin in the pigment dispersion paste is not particularly limited, but for example, it can be used in an amount of 20 to 100 parts by mass in terms of the resin solid content ratio per 100 parts by mass of the pigment.

[0042] The solid content of the pigment dispersion paste is usually 40 to 70% by mass, and particularly preferably 50 to 60% by mass, based on the total amount of the pigment dispersion paste.

[0043] In this specification, the "solid content of the pigment dispersion paste" means the mass of all components contained in the pigment dispersion paste that remain in a solid state even after removal of the solvent, specifically, the total mass of the pigment dispersion resin, pigment, and other solid components added as necessary contained in the pigment dispersion paste.

[0044] <Other ingredients, etc.> The cationic electrodeposition coating composition of the present invention may further contain a metal nitrite salt in addition to the above components. As the metal nitrite salt, a nitrite salt of an alkali metal or a nitrite salt of an alkaline earth metal is preferable, and a nitrite salt of an alkaline earth metal is more preferable. As the metal nitrite salt, for example, calcium nitrite, sodium nitrite, potassium nitrite, magnesium nitrite, strontium nitrite, barium nitrite, zinc nitrite, etc. can be mentioned.

[0045] The cationic electrodeposition coating composition contains a metal nitrite, which has the advantage of improving corrosion resistance, particularly the corrosion resistance of edges (edge ​​rust prevention). When the cationic electrodeposition coating composition contains a metal nitrite, the content is preferably 0.001 to 0.2 mass% of the metal component calculated as the metal element relative to the total mass of the coating film-forming resin.

[0046] The metal nitrite can be added to the cationic electrodeposition coating composition by any method. For example, an aqueous solution of the metal nitrite may be prepared in advance and added to the cationic electrodeposition coating composition. Alternatively, the metal nitrite may be mixed with the pigment in advance and dispersed in the same manner as the pigment.

[0047] <Production of cationic electrodeposition coating composition> The cationic electrodeposition coating composition of the present invention can be prepared by mixing a resin emulsion containing an aminated epoxy resin and a blocked polyisocyanate curing agent, a pigment dispersion paste, additives, etc., by a commonly used method.

[0048] In this specification, the "solid content of the electrodeposition coating composition" means the mass of all components contained in the electrodeposition coating composition that remain in the form of a solid even after removal of the solvent, specifically, the total mass of the solid content of the aminated epoxy resin, blocked polyisocyanate curing agent, and optionally the pigment dispersing resin, pigment, and other solid components contained in the electrodeposition coating composition.

[0049] The solid content of the cationic electrodeposition coating composition of the present invention is preferably 1-30% by mass based on the total amount of the electrodeposition coating composition. If the solid content of the cationic electrodeposition coating composition is less than 1% by mass, the amount of deposition of the electrodeposition coating film is small, and it may be difficult to ensure sufficient corrosion resistance. If the solid content of the cationic electrodeposition coating composition is more than 30% by mass, the throwing power or coating appearance may be deteriorated.

[0050] The cationic electrodeposition coating composition of the present invention preferably has a pH of 4.5 to 7. If the pH of the cationic electrodeposition coating composition is less than 4.5, the amount of acid present in the cationic electrodeposition coating composition becomes excessive, which may result in poor coating film appearance or coating workability. On the other hand, if the pH exceeds 7, the filterability of the cationic electrodeposition coating composition may decrease, and the horizontal appearance of the cured electrodeposition coating film may decrease. The pH of the cationic electrodeposition coating composition can be set within the above range by adjusting the amount of neutralizing acid used, the amount of free acid added, etc. The pH is more preferably 5 to 7.

[0051] The pH of the cationic electrodeposition coating composition can be measured using a commercially available pH meter having a temperature compensation function.

[0052] The milligram equivalent of acid (MEQ(A)) per 100 g of solid content of the cationic electrodeposition coating composition is preferably 10 to 50. The milligram equivalent of acid (MEQ(A)) per 100 g of resin solid content of the cationic electrodeposition coating composition can be adjusted by the amount of neutralizing acid and the amount of free acid.

[0053] Here, MEQ(A) is an abbreviation for mg equivalent(acid), and is the total mg equivalent of all acids per 100 g of solid content of the paint. This MEQ(A) can be measured by quantitatively determining the amount of acid contained in the cationic electrodeposition coating composition by precisely weighing out about 10 g of the solid content of the electrodeposition coating composition, dissolving it in about 50 ml of a solvent (THF: tetrahydrofuran), and then performing potentiometric titration using a 1 / 10 N NaOH solution.

[0054] The cationic electrodeposition coating composition of the present invention may contain additives generally used in the coating field, such as organic solvents such as ethylene glycol monobutyl ether, ethylene glycol monohexyl ether, ethylene glycol monoethylhexyl ether, propylene glycol monobutyl ether, dipropylene glycol monobutyl ether, and propylene glycol monophenyl ether, surfactants such as drying inhibitors and defoamers, viscosity modifiers such as acrylic resin fine particles, anti-repellent agents, and inorganic rust inhibitors such as vanadium salts, copper, iron, manganese, magnesium, and calcium salts, as necessary. In addition to these, known auxiliary complexing agents, buffers, smoothing agents, stress relaxation agents, gloss agents, semi-gloss agents, antioxidants, and ultraviolet absorbers may be blended according to the purpose. These additives may be added during the production of the resin emulsion, during the production of the pigment dispersion paste, or during or after the mixing of the resin emulsion and the pigment dispersion paste.

[0055] The cationic electrodeposition coating composition of the present invention may contain other film-forming resin components in addition to the above-mentioned aminated epoxy resin. Examples of other film-forming resin components include acrylic resins, polyester resins, urethane resins, butadiene resins, phenolic resins, and xylene resins. Other film-forming resin components that can be contained in the electrodeposition coating composition are preferably phenolic resins and xylene resins. Examples of phenolic resins and xylene resins include xylene resins having 2 to 10 aromatic rings.

[0056] In the cationic electrodeposition coating composition of the present invention, the solubility parameter (SP) of the mixture of the aminated epoxy resin and the blocked polyisocyanate curing agent is also an index for observing the performance of the electrodeposition coating. In the present invention, the solubility parameter (SP) of the mixture of the aminated epoxy resin and the blocked polyisocyanate curing agent must be 9.9 to 11.3, preferably 9.9 to 11.2, and more preferably 9.9 to 11.1. If the solubility parameter (SP) of the mixture of the aminated epoxy resin and the blocked polyisocyanate curing agent is less than 9.9, the adhesion decreases, and conversely, if it is more than 11.3, the hydrophilicity increases and the barrier properties of the coating film decrease.

[0057] The cationic electrodeposition coating composition of the present invention is also required to have a residual adhesion functional group number of 1.4 to 2.4 meq / solid g after the cationic electrodeposition coating composition of the present invention is applied to a steel plate so as to have a dry film thickness of 15 μm and baked at 170° C. for 20 minutes. This defines the performance of the coating film after the coating composition is obtained, and the residual adhesion functional group number is a theoretical value and can be calculated by subtracting the amount of isocyanate groups (meq / solid g) of the blocked polyisocyanate curing agent from the amount of functional groups of the aminated epoxy resin, specifically the total amount of hydroxyl groups (meq / solid g) and the amount of primary amines (meq / solid g). The residual adhesion functional group number is preferably 1.6 to 2.2 meq / solid g, more preferably 1.7 to 2.1 meq / solid g. If the number of remaining adhesion functional groups in the coating film applied under these conditions is less than 1.4 meq / solid g, the coating film will not be able to have sufficient adhesion performance, and if it is more than 2.4 meq / solid g, the coating film will become too hydrophilic, resulting in a decrease in its barrier properties.

[0058] <Electrodeposition painting and electrocoating film formation> An electrodeposition coating film can be formed by electrodeposition coating of a substrate using the cationic electrodeposition coating composition of the present invention. In the electrodeposition coating using the cationic electrodeposition coating composition of the present invention, the substrate is used as a cathode, and a voltage is applied between the cathode and the anode. This causes an electrodeposition coating film to be deposited on the substrate.

[0059] As the substrate to which the cationic electrodeposition coating composition of the present invention is applied, various substrates to which electricity can be applied can be used. Examples of substrates that can be used include cold-rolled steel sheets, hot-rolled steel sheets, stainless steel, electrogalvanized steel sheets, hot-dip galvanized steel sheets, zinc-aluminum alloy-plated steel sheets, zinc-iron alloy-plated steel sheets, zinc-magnesium alloy-plated steel sheets, zinc-aluminum-magnesium alloy-plated steel sheets, aluminum-plated steel sheets, aluminum-silicon alloy-plated steel sheets, and tin-plated steel sheets.

[0060] In the electrodeposition coating process, the object to be coated is immersed in the electrodeposition coating composition, and then electrodeposition coating is performed by applying a voltage of 50 to 450 V. If the applied voltage is less than 50 V, the electrodeposition may be insufficient, and if it exceeds 450 V, the appearance of the coating film may be poor. During electrodeposition coating, the bath temperature of the coating composition is usually adjusted to 10 to 45°C.

[0061] The time for applying the voltage varies depending on the electrodeposition conditions, but can generally be set to 2 to 5 minutes.

[0062] In the electrodeposition coating using the cationic electrodeposition coating composition of the present invention, the thickness of the electrodeposition coating film to be deposited is preferably such that the thickness of the electrodeposition coating film finally obtained by heat curing is preferably 5 to 60 μm, more preferably 10 to 25 μm. If the thickness of the electrodeposition coating film is less than 5 μm, the rust prevention properties may be insufficient.

[0063] The electrodeposition coating film deposited as described above can be cured by, if necessary, rinsing with water and then heating for 10 to 30 minutes at, for example, 120 to 260° C., preferably 140 to 220° C. This forms a cured electrodeposition coating film.

[0064] The cationic electrodeposition coating composition of the present invention has the advantage that, even when a cured electrodeposition coating film is provided on a substrate having edges, a cured electrodeposition coating film having excellent edge rust prevention properties can be provided. The cationic electrodeposition coating composition of the present invention has a function of retaining the deposited electrodeposition coating film, and therefore can be suitably used in cases where a cured electrodeposition coating film is provided on a substrate having edges.

[0065] In this specification, the corrosion resistance of a cured electrodeposition coating formed on a substrate having edges is evaluated by a salt spray test (35°C x 72 hours) in accordance with JIS Z 2371 (2000). When a high-thickness cured electrodeposition coating, for example, a thickness of 25 to 50 μm, is subjected to a salt spray test, the number of rust spots occurring in the edge coating of the cured electrodeposition coating formed on a substrate having edges is 1 cm or less. 2 For example, 3 pieces / cm 2 If the number of rust spots is less than 1 cm, the coating has excellent corrosion resistance (rust prevention) at the edge. 2 1 piece per cm 2 If it is less than this, it can be said that the coating film has extremely excellent edge corrosion resistance. EXAMPLES

[0066] The present invention will be described in more detail with reference to the following examples, but the present invention is not limited thereto. In the examples, "parts" and "%" are by weight unless otherwise specified.

[0067] Production Example 1-A Production of aminated epoxy resin (resin A) 12 parts of butyl cellosolve, 940 parts of bisphenol A type epoxy resin (trade name DER-331J, manufactured by Dow Chemical Company), 254 parts of bisphenol A, 80 parts of phenol, and 2 parts of dimethylbenzylamine were added, and the temperature inside the reaction vessel was kept at 120° C. and the reaction was allowed to proceed until the epoxy equivalent reached 700 g / eq, after which the temperature inside the reaction vessel was cooled to 110° C. Then, a mixture of 90 parts of diethanolamine and 44 parts of N,N-dimethyl-1,3-propanediamine was added, and the reaction was allowed to proceed at 110° C. for 1 hour to obtain an aminated epoxy resin (cation-modified epoxy resin: resin A).

[0068] Production Example 1-B Production of aminated epoxy resin (resin B) 12 parts of butyl cellosolve, 940 parts of bisphenol A type epoxy resin (trade name DER-331J, manufactured by Dow Chemical Company), 228 parts of bisphenol A, and 2 parts of dimethylbenzylamine were added, and the temperature inside the reaction vessel was kept at 120° C. and the reaction was allowed to proceed until the epoxy equivalent reached 400 g / eq, after which the temperature inside the reaction vessel was cooled to 110° C. Next, a mixture of 212 parts of diethanolamine and 44 parts of N,N-dimethyl-1,3-propanediamine was added, and the reaction was allowed to proceed at 110° C. for 1 hour to obtain an aminated epoxy resin (cation-modified epoxy resin: resin B).

[0069] Production Example 1-C Production of aminated epoxy resin (resin C) 12 parts of butyl cellosolve, 940 parts of bisphenol A type epoxy resin (trade name DER-331J, manufactured by Dow Chemical Company), 254 parts of bisphenol A, 70 parts of phenol, and 2 parts of dimethylbenzylamine were added, and the temperature inside the reaction vessel was kept at 120°C. The reaction was continued until the epoxy equivalent reached 650 g / eq, and then the temperature inside the reaction vessel was cooled to 110°C. Next, a mixture of 100 parts of diethanolamine and 49 parts of N,N-dimethyl-1,3-propanediamine was added, and the reaction was continued for 1 hour at 110°C to obtain an aminated epoxy resin (cation-modified epoxy resin: resin C).

[0070] Production Example 1-D Production of aminated epoxy resin (resin D) 28 parts of butyl cellosolve, 940 parts of bisphenol A type epoxy resin (trade name DER-331J, manufactured by Dow Chemical Company), 342 parts of bisphenol A, 104 parts of phenol, and 2 parts of dimethylbenzylamine were added, and the temperature inside the reaction vessel was kept at 120° C. and reacted until the epoxy equivalent reached 1500 g / eq, and then cooled until the temperature inside the reaction vessel reached 110° C. Next, a mixture of 116 parts of diethylenetriamine diketimine (a methyl isobutyl ketone solution with a solid content of 73%), 30 parts of N-methylethanolamine, and 9 parts of diethanolamine was added, and reacted at 110° C. for 1 hour to obtain an aminated epoxy resin (cation-modified epoxy resin: resin D).

[0071] Production Example 1-E Production of aminated epoxy resin (resin E) 27 parts of butyl cellosolve, 940 parts of bisphenol A type epoxy resin (trade name DER-331J, manufactured by Dow Chemical Company), 254 parts of bisphenol A, 47 parts of phenol, and 2 parts of dimethylbenzylamine were added, and the temperature inside the reaction vessel was kept at 120° C. and the reaction was allowed to proceed until the epoxy equivalent reached 570 g / eq, after which the temperature inside the reaction vessel was cooled to 110° C. 214 parts of diethanolamine were added and the reaction was allowed to proceed at 110° C. for 1 hour to obtain an aminated epoxy resin (cationically modified epoxy resin: resin F).

[0072] Production Example 1-F Production of aminated epoxy resin (Resin F) 27 parts of butyl cellosolve, 940 parts of bisphenol A type epoxy resin (trade name DER-331J, manufactured by Dow Chemical Company), 254 parts of bisphenol A, 19 parts of phenol, and 2 parts of dimethylbenzylamine were added, and the temperature inside the reaction vessel was kept at 120°C. The reaction was continued until the epoxy equivalent reached 490 g / eq, and then the temperature inside the reaction vessel was cooled to 110°C. 242 parts of diethanolamine were added, and the reaction was continued at 110°C for 1 hour, to obtain an aminated epoxy resin (cationically modified epoxy resin: resin F).

[0073] Production Example 1-G Production of aminated epoxy resin (resin G) 28 parts of butyl cellosolve, 940 parts of bisphenol A type epoxy resin (trade name DER-331J, manufactured by Dow Chemical Company), 228 parts of bisphenol A, 188 parts of phenol, and 2 parts of dimethylbenzylamine were added, and the temperature inside the reaction vessel was kept at 120°C. The reaction was continued until the epoxy equivalent reached 1400 g / eq, and then the temperature inside the reaction vessel was cooled to 110°C. A mixture of 212 parts of diethylenetriamine diketimine (a methyl isobutyl ketone solution with a solid content of 73%) and 5 parts of N-methylethanolamine was added, and the reaction was continued for 1 hour at 110°C, yielding an aminated epoxy resin (cationically modified epoxy resin: resin G).

[0074] Production Example 2-1 Production of blocked polyisocyanate curing agent (1) 1370 parts of polymethylene polyphenyl polyisocyanate (MDI) and 732 parts of MIBK were charged into a reaction vessel and heated to 60° C. 300 parts of butyl diglycol ether and 1330 parts of butyl cellosolve were added dropwise to the vessel over 2 hours at 60° C. After further heating at 75° C. for 4 hours, it was confirmed that the absorption due to the isocyanate group had disappeared in the measurement of the IR spectrum, and after cooling, 27 parts of MIBK were added to obtain a blocked polyisocyanate curing agent (1).

[0075] Production Example 3 - Production of pigment dispersing resin In a reaction vessel equipped with a stirrer, a cooling tube, a nitrogen inlet tube, and a thermometer, 385 parts of bisphenol A type epoxy resin, 120 parts of bisphenol A, 95 parts of octylic acid, and 1 part of 1% 2-ethyl-4-methylimidazole solution were charged, and reacted at 160-170°C under a nitrogen atmosphere for 1 hour. Then, after cooling to 120°C, 198 parts of a methyl isobutyl ketone solution of 2-ethylhexanolic half-blocked tolylene diisocyanate (solid content 95%) was added. The reaction mixture was kept at 120-130°C for 1 hour, and 157 parts of ethylene glycol mono n-butyl ether was added. Then, the mixture was cooled to 85-95°C and homogenized. Next, 277 parts of diethylenetriamine diketimine (methyl isobutyl ketone solution with a solid content of 73%) was added, and the mixture was stirred at 120°C for 1 hour, followed by adding 13 parts of ethylene glycol mono n-butyl ether to produce an aminated resin. Next, 18 parts of ion-exchanged water and 8 parts of formic acid were charged, the above-mentioned aminated resin was mixed, and the mixture was stirred for 15 minutes. 200 parts of ion-exchanged water was then added to obtain a resin solution (resin solids content 25%) of a pigment dispersion resin (average molecular weight 2,200).

[0076] Production Example 4-A: Production of electrocoating resin emulsion (EmA) 400g (solid content) of the resin (Resin A) obtained in Production Example 1-A and 160g (solid content) of the blocked polyisocyanate curing agent (1) obtained in Production Example 2-1 were mixed, and ethylene glycol mono-2-ethylhexyl ether was added so that the amount was 3% (15g) based on the solid content. Next, formic acid was added to achieve a neutralization rate of 40% for neutralization, and ion-exchanged water was added to slowly dilute the mixture to obtain an electrodeposition paint resin emulsion (EmA).

[0077] Production Example 5-B~G Production of electrodeposition paint resin emulsion (EmB~G) The aminated epoxy resins (Resins B to G) obtained in Production Examples 1-B to 1-G were also used to obtain electrodeposition paint resin emulsions (EmB to EmG) in the same manner as in Production Example 4-A.

[0078] Production Example 6: Production of pigment dispersion paste for electrodeposition paint Using a sand mill, the mixture obtained was dispersed at 40° C. based on the formulation shown in Table 1 below, including the pigment dispersion resin obtained in Production Example 3, until the volume average particle diameter D50 was 0.6 μm, and prepared to obtain a pigment dispersion paste (solid content 49%). The volume average particle diameter D50 was measured using a laser Doppler particle size analyzer (manufactured by Nikkiso Co., Ltd., "Microtrac UPA150"), by diluting the dispersion with ion-exchanged water so that the signal level was appropriate, and the volume average particle diameter D50 was measured.

[0079] Example 1 Into a stainless steel container were added 1,394 g of ion-exchanged water, 560 g of resin emulsion (EmA), and 41 g of the pigment dispersion paste obtained in Production Example 6, followed by aging at 40° C. for 16 hours to form an electrodeposition coating composition.

[0080] Examples 2 and 3 and Comparative Examples 1 to 4 In the same manner as in Example 1, electrodeposition coating compositions were obtained for Examples 2 and 3 (EmB and EmC) and Comparative Examples 1, 2, 3 and 4 (EmD, EmE, EmF and EmG).

[0081] A cold-rolled steel sheet (JISG3141, SPCC-SD) was degreased by immersing in Surf Cleaner EC90 (manufactured by Nippon Paint Co., Ltd.) at 50°C for 2 minutes. Then, the sheet was immersed in a zirconium conversion treatment solution containing 0.005% ZrF and adjusted to pH 4 with NaOH at 40°C for 90 seconds to perform zirconium conversion treatment. Next, the electrodeposition coating composition obtained in the Examples or Comparative Examples was added with a required amount of 2-ethylhexyl glycol so that the film thickness of the electrodeposition coating film after curing was 15 μm, and then the steel sheet was immersed, and a voltage was applied under the conditions of increasing the voltage for 30 seconds to 180 V and then maintaining the voltage for 150 seconds to deposit an uncured electrodeposition coating film on the substrate.

[0082] The uncured electrodeposition coating film thus obtained was baked and cured at 170°C for 15 minutes to obtain an electrodeposition-coated plate having a cured electrodeposition coating film. The resulting cured electrodeposition coating film was subjected to the following evaluations. The results are shown in Table 1. Table 1 also shows the characteristics of each electrodeposition coating composition (amount of adhesion functional groups, amount of remaining adhesion functional groups in the baked coating film, solubility parameter (SP) of the aminated epoxy resin, and SP of a coating in which BI (blocked polyisocyanate curing agent) was mixed with the aminated epoxy resin).

[0083] <Amount of Adhesion Functional Groups in Amine Epoxy Resin> Adhesive functional group amount (m eq / solid g) = equivalent weight (eq) / solid content amount (g) x 1000

[0084] <Residual adhesion functional group content of baked coating> It was calculated by subtracting the amount of isocyanate groups (meq / solid g) of the blocked polyisocyanate curing agent from the sum of the amount of hydroxyl groups (meq / solid g) and the amount of primary amine (meq / solid g) of the aminated epoxy resin.

[0085] <Solubility parameter (SP) of aminated epoxy resin> and <Solubility parameter (SP) when aminated epoxy resin is mixed with blocked polyisocyanate curing agent (BI)> The solubility parameter (SP value) can be actually measured by the following method. Reference SUH, CLARKE [JPSA-1, 5, 1671-1681(1967)] ·Measurement temperature: 20℃ Sample: Weigh out 0.5 g of resin into a 100 ml beaker, add 10 ml of a good solvent using a volumetric pipette, and dissolve using a magnetic stirrer. Solvent: Good solvent: dioxane, acetone Poor solvent: n-hexane, ion-exchanged water Turbidity measurement: Drop a poor solvent using a 50 ml burette, and measure the amount dropped at which turbidity appears. · Calculation: The SP value δ of the resin is given by the following formula. δ = (V ml1 / 2 δ ml +V mh 1 / 2 δ mh ) / (V ml 1 / 2 +V mh 1 / 2 ) Vm = V1V2 / (φ1V2 + φ2V1) δm = φ1δ1 + φ2δ2 V i : Molecular volume of solvent (ml / mol) φ i : Volume fraction of each solvent at cloud point δ i : SP value of solvent ml: Low SP poor solvent mixture system mh: High SP poor solvent mixture system

[0086] <VOC content> {Amount of solvent formulation (g) × Specific gravity of Em (1.05 (g / cm3)) / Total weight of Em (g)} × 1000 = VOC content (g / L) Evaluation criteria ○: 30 g / L or less △: 30 - 40 g / L or less ×: Exceeds 40 g / L

[0087] Using the electrodeposition coating composition and coated board obtained by the above examples, the following evaluation tests were conducted.

[0088] Curing property (rubbing property) The coating film was rubbed 50 times with gauze soaked in MIBK, and the curing property was determined based on the surface state of the coating film. The evaluation criteria are as follows. ○: No change in coating film △: Streaks in coating film ×: Coloring on gauze

[0089] Cycle corrosion test (Cycle Corrosion Test (CCT)) A cross-cut was made with a knife on the coating of the electrocoated cold-rolled steel plate after hardening, reaching the base material, and JASOM609-91 "Corrosion Test Method for Automotive Materials" was run for 100 cycles. The cross-cut area was then observed for rust and blisters, and the corrosion resistance was evaluated in accordance with an actual corrosive environment. The evaluation criteria were as follows: Evaluation criteria ◎: The maximum width of rust or blister is less than 5 mm from the cut part (on both sides) ○: The maximum width of rust or swelling is 5mm to less than 7.5mm from the cut part (both sides). No blisters other than the cut part. ○△: The maximum width of rust or blister is 5mm to less than 7.5mm from the cut part (both sides). Blisters are present in areas other than the cut part. △: The maximum width of rust or blister is 7.5mm or more but less than 10mm from the cut part (both sides) △×: The maximum width of rust or blister is 10mm or more and less than 12.5mm from the cut part (both sides) ×: The maximum width of rust or blister is 12.5 mm or more from the cut part (on both sides)

[0090] Edge Corrosion Test For the evaluation of this test, instead of the above cold-rolled steel plate, an L-type dedicated replacement blade (LB10K: manufactured by Olfa Corporation) was used, which was degreased by immersing it in Surf Cleaner EC90 (manufactured by Nippon Paint Surf Chemicals) at 50 ° C for 2 minutes, surface-conditioned with Surf Fine GL-1 (manufactured by Nippon Paint Surf Chemicals), and then immersed in Surf Dyne SD-5000 (manufactured by Nippon Paint Surf Chemicals, zinc phosphate conversion treatment liquid) at 40 ° C for 2 minutes to perform zinc phosphate conversion treatment. The paints of Examples 1 to 3 and Comparative Examples 1 to 4 were electrocoated on this under the same conditions as the above electrocoating to form a cured electrocoated coating film, and the number of rust spots on the tip of the L-type dedicated replacement blade after the salt spray test at 35 ° C x 168 h test was examined. Evaluation criteria ◎: Less than 10 ○: 10 or more but less than 20 ○△: 20 to less than 50 △: 50 to less than 100 ×: 100 or more pieces

[0091] Painting workability (uneven grinding) Steel plates were ground with a grindstone and then electrocoated, and the appearance of the ground area was visually inspected for roughness. ○: The coating film has a uniform appearance. ○△: Some areas are visually recognized as being slightly uneven, but the overall appearance of the coating is almost uniform △: Unevenness is visible ×: Appearance of the coating film is obviously non-uniform

[0092] Stability of electrodeposition coating composition (paint stability) The electrodeposition coating composition was left to stand or stirred, and the state of the coating composition was visually judged to evaluate the coating stability. The evaluation criteria were as follows. Stable here means that the pigment does not settle within 15 minutes after stirring is stopped. Evaluation criteria ○: The electrodeposition coating composition is stable when left standing. ○△: The electrodeposition coating composition is not stable when left to stand, but is quickly stabilized by stirring again. △: The electrodeposition coating composition is stable when it is continuously stirred. ×: The electrodeposition coating composition is not stabilized even when continuously stirred.

[0093] [Table 1]

[0094] As is clear from Table 1 above, the adhesive functional group number and solubility parameter of the aminated epoxy resins A to C (Examples 1 to 3) are within the specified range, so that the performance of the electrodeposition coating film all satisfies the good standard. Moreover, the paints of the Examples have a low VOC amount, rated as ◯, and are excellent in environmental consideration. On the other hand, Comparative Example 1 is a cationic electrodeposition paint using diketimine, and has a high VOC amount of x, and furthermore, the amount of adhesive functional groups is insufficient, so that there are deficiencies in the corrosion test, etc. In Comparative Example 2, the solubility parameter of the aminated epoxy resin is too high, so that there are also deficiencies in the corrosion test, etc. In Comparative Example 3, not only the amount of adhesive functional groups and the solubility parameter (SP) of the aminated epoxy resin, but also the remaining adhesive functional group number of the baked coating film and the solubility parameter (SP) of the mixture of the aminated epoxy resin and the blocked polyisocyanate curing agent are both values ​​that are outside the specified values, so that there are defects in the coating film performance. In Comparative Examples 2 and 3, diketimine is not used as an amine compound in the production of the aminated resin, and diethanolamine is used in large quantities, resulting in low neutralization ability and insufficient paint stability. In Comparative Example 4, not only is diketimine used as in Comparative Example 1, but the amount of adhesion functional groups, the solubility parameter (SP) of the aminated epoxy resin, the number of remaining adhesion functional groups in the baked coating film, and the solubility parameter (SP) of a mixture of aminated epoxy resin and blocked polyisocyanate curing agent are all outside the specified values, resulting in a large VOC amount of x, and poor results in the cycle corrosion test and edge rust prevention.

Claims

1. A cationic electrodeposition coating composition comprising an aminated epoxy resin and a blocked polyisocyanate curing agent, The cationic electrodeposition coating composition is characterized in that the aminated epoxy resin has an adhesion functional group number of 2.9 to 3.9 meq / solid g and a solubility parameter (SP) of 10.2 to 11.

6.

2. A cationic electrodeposition coating composition comprising an aminated epoxy resin and a blocked polyisocyanate curing agent, the solubility parameter (SP) of a mixture of the aminated epoxy resin and the blocked polyisocyanate curing agent is 9.9 to 11.3; and, The cationic electrodeposition coating composition according to claim 1, characterized in that the cationic electrodeposition coating composition is applied to a steel plate so as to have a dry film thickness of 15 μm, and after baking at 170° C. for 20 minutes, the number of remaining adhesion functional groups is 1.4 to 2.4 meq / solid g.

3. 3. The cationic electrodeposition coating composition according to claim 1, wherein the aminated epoxy resin is obtained by amminating an epoxy resin with a diamine having a primary amino group that is not blocked with a ketimine and a secondary or tertiary amino group.

4. 4. A cationic electrodeposition coating composition according to claim 3, wherein said epoxy resin is a reaction product of epichlorohydrin and a polycyclic phenol compound, and the oxirane ring in said reaction product is chain-extended with a chain extender.

5. The cationic electrodeposition coating composition according to claim 3, wherein the diamine having a primary amino group and a secondary or tertiary amino group not blocked with a ketimine is N,N-dimethyl-1,3-propanediamine, N-(3-aminopropyl)diethanolamine, dimethylaminoethylamine or a mixture thereof.

Citation Information

Patent Citations

  • Aqueous binding agent dispersion for cationic electro-dipcoat paint

    EP0961797A1

  • Aqueous binder dispersion for cationic electrodeposition paint

    JP2001509833A

  • Method for forming coating film using cationic electrodeposition coating composition also serving as intermediate coating

    JP2003221546A

  • Cationic electrodeposition coating composition and process for forming multilayer coating

    JP2010095678A

  • Cationic electrodeposition coating material composition and electrodeposition coating method using the same

    JP2010144104A