Sealing layers comprising conductive filler for sealing microcells of electrophoretic displays

Aqueous polymeric compositions with specific ratios of poly(vinyl alcohol), polyurethane, and conductive fillers form a sealing layer that addresses the challenges of barrier properties, moisture absorption, and electrical resistivity in electrophoretic displays, improving electro-optical performance.

JP2024149723AInactive Publication Date: 2024-10-18E INK CORP
View PDF 34 Cites 0 Cited by

Patent Information

Application Number
JP2024132040
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-02-04
Filing Date
2024-08-08
Publication Date
2024-10-18
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing sealing layers for electrophoretic displays face challenges in providing optimal barrier properties against non-polar fluids, moisture absorption, and electrical resistivity, leading to degraded electro-optical performance.

Method used

Aqueous polymeric compositions comprising 30 to 70% poly(vinyl alcohol) homopolymer or poly(vinyl alcohol-co-ethylene) copolymer, 7 to 29% polyurethane, and 1 to 45% conductive filler, such as carbon black, with a total surface energy greater than 55 mN/m, are used to form a sealing layer that balances barrier, moisture resistance, and electrical conductivity.

Benefits of technology

The sealing layer achieves improved electro-optical performance by preventing non-polar fluid efflux, reducing moisture absorption, and maintaining low power consumption, thereby enhancing image quality and resolution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024149723000024
    Figure 2024149723000024
  • Figure 2024149723000025
    Figure 2024149723000025
  • Figure 2024149723000026
    Figure 2024149723000026
Patent Text Reader

Abstract

To provide sealing layers comprising a conductive filler for sealing microcells of electrophoretic displays.SOLUTION: The present invention is directed to a sealing layer that comprises a poly(vinyl alcohol) homopolymer or a poly(vinyl alcohol-co-ethylene) copolymer, a polyurethane, and a conductive filler. The sealing layer shows good barrier properties to a non-polar fluid. The sealing layer can be used to seal microcells of electro-optic devices, contributing to improved good electro-optic performance of the device, especially at low temperatures. This invention relates to aqueous polymer compositions and sealing layers both comprising a conductive filler. The aqueous polymer compositions can be used to form sealing layers for sealing microcells of electro-optic devices, such as electrophoretic displays.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] Related Applications This application claims priority to U.S. Provisional Patent Application No. 63 / 145,582, filed February 4, 2021. Any patents, published applications or other published documents referenced herein are incorporated by reference in their entirety.

[0002] FIELD OF THEINVENTION The present invention relates to a water-based polymer composition containing conductive fillers and a sealing layer. The water-based polymer composition can be used to form a sealing layer for sealing microcells in electro-optical devices, such as electrophoretic displays. [Background technology]

[0003] 2. Background of the Invention The term "electro-optical," as applied to a material or display, is used herein in its conventional sense in the imaging arts to refer to a material having first and second display states that differ in at least one optical property, and that changes from its first display state to its second display state upon application of an electric field to the material. The optical property is typically color as perceived by the human eye, but may also be another optical property, such as light transmission, reflectance, emission, or, in the case of displays intended to be machine-readable, pseudocolor in the sense of a change in reflectance of electromagnetic wavelengths outside the visible range.

[0004] The terms "bistable" and "bi-stable" are used herein in their conventional sense in the art to refer to displays containing display elements having first and second display states differing in at least one optical property, such that any given element is driven to assume either its first or second display state with an addressing pulse of finite duration, and the state persists after the addressing pulse has ended for at least several times, e.g., at least four times, the minimum duration of the addressing pulse required to change the state of the display element. In U.S. Pat. No. 7,170,670 it is shown that some particle-based electrophoretic displays capable of gray scale are stable not only in their extreme black and white states, but also in their intermediate gray states, and the same is true for some other types of electro-optical devices. Displays of this type are properly referred to as "multi-stable" rather than bistable, but for convenience the term "bistable" may be used herein to cover both bistable and multi-stable displays.

[0005] One type of electro-optical device that has been the subject of intense research and development over the years is the particle-based electrophoretic display, in which a plurality of charged particles move through a fluid under the influence of an electric field. Electrophoretic displays can have attributes of good brightness and contrast, wide viewing angles, state bistability, and low power consumption when compared to liquid crystal displays.

[0006] Numerous patents and applications assigned to or in the name of Massachusetts Institute of Technology (MIT), E Ink Corporation, E Ink California, LLC and affiliates describe various techniques used in encapsulated and microcell electrophoretic media, as well as other electro-optic media. Capsule electrophoretic media contain a multitude of small capsules, each of which itself contains an internal phase containing electrophoretically mobile particles in a fluid medium, and a capsule wall surrounding the internal phase. Typically, the capsules are themselves held in a polymer binder to form a coherent layer located between two electrodes. In microcell electrophoretic displays, the charged particles and fluid are not encapsulated in microcapsules, but instead are held in a plurality of cavities formed in a carrier medium, typically a polymer film.

[0007] The technologies described in these patents and applications include:

[0008] (a) Electrophoretic particles, fluids and fluid additives, see, e.g., U.S. Pat. Nos. 7,002,728 and 7,679,814.

[0009] (b) Capsules, binders and encapsulation processes, see, e.g., U.S. Pat. Nos. 6,922,276 and 7,411,719.

[0010] (c) Microcell structures, wall materials, and methods of forming the microcells, see, for example, US Pat. Nos. 7,072,095 and 9,279,906.

[0011] (d) Methods for filling and sealing microcells, see, e.g., U.S. Pat. Nos. 7,144,942, 7,005.468, and 7,715,088, and U.S. Patent Application Publication Nos. 2004-0120024 and 2004-0219306.

[0012] (e) Films and subassemblies containing electro-optical materials, see, for example, US Pat. Nos. 6,982,178 and 7,839,564.

[0013] (f) Backplanes, adhesive layers and other auxiliary layers and methods used in displays, see, for example, US Pat. Nos. 7,116,318 and 7,535,624.

[0014] (g) Color formation and color adjustment, see, for example, U.S. Pat. Nos. 7,075,502 and 7,839,564.

[0015] (h) Methods for driving displays, see, for example, US Pat. Nos. 7,012,600 and 7,453,445.

[0016] (i) Display applications, see, for example, US Pat. Nos. 7,312,784 and 8,009,348.

[0017] (j) Non-electrophoretic displays and non-display applications of encapsulation and microcell technology as described in U.S. Pat. No. 6,241,921 and U.S. Patent Application Publication No. 2015 / 0277160, see, e.g., U.S. Pat. No. 7,615,325, and U.S. Patent Application Publication Nos. 2015 / 0005720 and 2016 / 0012710.

[0018] The contents of all of the above references are incorporated herein by reference in their entirety.

[0019] Structures having a plurality of sealed microcells containing a dispersion of charged pigment particles in a non-polar fluid are used commercially in electrophoretic displays. A microcell is also known in the literature as a microcavity or microcup. A typical method for making a sealed microcell structure for an electrophoretic display includes (a) fabricating a polymer sheet with a plurality of microcavities by microembossing, each microcavity having an opening; (b) filling the microcavities with an electrophoretic medium, which is a dispersion containing charged pigment particles in a non-polar fluid; and (c) sealing the microcavities with an aqueous polymer composition to form a sealing layer. The sealed microcavities containing the electrophoretic medium form the electro-optical material layer of the device. The electro-optical material layer is disposed between a front electrode and a rear electrode. Application of an electric field across the electrophoretic medium by these electrodes causes the pigment particles to migrate through the electrophoretic medium to produce an image. The sealing layer plays an important role for the function and performance of the device.

[0020] First, since the sealing layer contacts the electrophoretic medium and seals it inside the microcavity, (1) the sealing layer must be practically insoluble in the non-polar fluid of the electrophoretic medium, and (2) the sealing layer must be a good barrier to the non-polar fluid so that it does not diffuse out of the microcell during the device lifetime.

[0021] Second, the sealing layer must not absorb significant amounts of moisture from the environment, i.e., must not allow environmental moisture to enter the electrophoretic medium of the device, which could negatively affect the electro-optical performance of the device. Finally, it is very important that the sealing layer in an electrophoretic display has good electrical properties: the electric field applied across the electrophoretic medium for display operation is transmitted through the sealing layer.

[0022] Therefore, the barrier, moisture absorption, and electrical properties of the sealing layer have a significant impact on the electro-optical performance of the display. Poor properties result in performance degradation. The technical problem of providing a sealing layer with properties that result in good electro-optical performance is difficult because different formulation strategies may be required for different purposes. For example, barrier properties against non-polar fluids typically require more hydrophilic components, while such components absorb more moisture from the environment. Furthermore, sealing layers with high electrical resistivity require higher power consumption for the operation of the display, while sealing layers with low resistivity result in poor image resolution. Thus, there is a need for polymer compositions that form sealing layers optimized for improved barrier against non-polar fluids, reduced moisture absorption, and optimal electrical resistivity. The present inventors have found that aqueous polymer compositions including poly(vinyl alcohol) homopolymer or poly(vinyl alcohol-co-ethylene) copolymer, polyurethane, and conductive filler that form sealing layers with a specific range of surface energy result in excellent electro-optical performance. [Prior art documents] [Patent documents]

[0023] [Patent Document 1] U.S. Patent No. 7,170,670 [Patent Document 2] U.S. Patent No. 7,002,728 [Patent Document 3] U.S. Pat. No. 7,679,814 [Patent Document 4] U.S. Patent No. 6,922,276 [Patent Document 5] U.S. Pat. No. 7,411,719 [Patent Document 6] U.S. Patent No. 7,072,095 [Patent Document 7] U.S. Pat. No. 9,279,906 [Patent Document 8] U.S. Patent No. 7,144,942 [Patent Document 9] U.S. Patent No. 7,005,468 [Patent Document 10] U.S. Patent No. 7,715,088 [Patent Document 11] US Patent Application Publication No. 2004-0120024 [Patent Document 12] US Patent Application Publication No. 2004-0219306 [Patent Document 13] U.S. Patent No. 6,982,178 [Patent Document 14] U.S. Pat. No. 7,839,564 [Patent Document 15] U.S. Patent No. 7,116,318 [Patent Document 16] U.S. Patent No. 7,535,624 [Patent Document 17] U.S. Patent No. 7,075,502 [Patent Document 18] U.S. Patent No. 7,012,600 [Patent Document 19] U.S. Patent No. 7,453,445 [Patent Document 20] U.S. Patent No. 7,312,784 [Patent Document 21] U.S. Pat. No. 8,009,348 [Patent Document 22] U.S. Patent No. 6,241,921 [Patent Document 23] US Patent Application Publication No. 2015 / 0277160 [Patent Document 24] U.S. Patent No. 7,615,325 [Patent Document 25] US Patent Application Publication No. 2015 / 0005720 [Patent Document 26] US Patent Application Publication No. 2016 / 0012710 Summary of the Invention [Means for solving the problem]

[0024] Summary of the Invention In one aspect, the invention is directed to a sealing layer comprising: (i) 30-70 wt. % of a water soluble poly(vinyl alcohol) homopolymer or poly(vinyl alcohol-co-ethylene) copolymer, based on the weight of the sealing layer excluding solvent, the poly(vinyl alcohol) having a degree of hydrolysis of 90-99.9%, the poly(vinyl alcohol-co-ethylene) copolymer having a degree of hydrolysis of 90-99.9% and an ethylene content of less than 10%; (ii) 7-29 wt. % of a polyurethane, based on the weight of the sealing layer excluding solvent; and (iii) 1-45 wt. % of a conductive filler, based on the weight of the sealing layer excluding solvent, the conductive filler being selected from the group consisting of carbon black, graphene, graphite, and carbon nanotubes, the conductive filler having a total surface energy greater than 40 mN / m, as determined by the Washburn method using hexane as the test liquid. The conductive filler has a dispersive component of surface energy. The dispersive component of surface energy of the conductive filler may be greater than 15 mN / m as determined by the Washburn method using hexane as the test liquid.

[0025] The sealing layer has a total surface energy, and the total surface energy of the sealing layer is greater than 55 mN / m. The total surface energy of the sealing layer is determined using a contact angle method by (a) forming a sealing layer by coating the aqueous polymer composition onto a substrate at a dry thickness of 30 mm, heating at 100° C. for 15 minutes, and conditioning the sealing layer at 25° C. and 55% relative humidity for 24 hours, (b) measuring the contact angles of a water droplet and a diiodomethane droplet on the formed sealing layer, and (c) calculating the total surface energy using the OWRK model.

[0026] The sealing layer can have a dispersion component of surface energy, and said dispersion component of surface energy may be higher than 40 mN / m. The dispersion component of surface energy of the sealing layer can be measured using a contact angle method by: (a) forming a sealing layer by coating the aqueous polymer composition on a substrate at a dry thickness of 30 mm, heating at 100° C. for 15 minutes, and conditioning the sealing layer at 25° C. and 55% relative humidity for 24 hours; (b) measuring the contact angles of a water droplet and a diiodomethane droplet on the formed sealing layer; and (c) calculating the contact angle using the OWRK model. It is determined by calculating the dispersion component of the surface energy.

[0027] The sealing layer is formed by an aqueous polymer composition comprising: (i) 30-70 wt. % of a water-soluble poly(vinyl alcohol) homopolymer or poly(vinyl alcohol-co-ethylene) copolymer, based on the weight of the sealing layer excluding the solvent, the poly(vinyl alcohol) having a degree of hydrolysis of 90-99.9%, the poly(vinyl alcohol-co-ethylene) copolymer having a degree of hydrolysis of 90-99.9% and an ethylene content of less than 10%, (ii) 7-29 wt. % of a polyurethane, based on the weight of the sealing layer excluding the solvent, and (iii) 1-45 wt. % of a conductive filler, based on the weight of the sealing layer excluding the solvent, the conductive filler being selected from the group consisting of carbon black, graphene, graphite, and carbon nanotubes, the conductive filler having a total surface energy greater than 40 mN / m, as determined by the Washburn method using hexane as the test liquid. The conductive filler has a dispersive component of surface energy. The dispersive component of surface energy of the conductive filler may be greater than 15 mN / m as determined by the Washburn method using hexane as the test liquid. The sealing layer has a total surface energy, and the total surface energy of the sealing layer is greater than 55 mN / m. The total surface energy of the sealing layer is determined using a contact angle method by (a) forming a sealing layer by coating the aqueous polymer composition on a substrate at a dry thickness of 30 mm, heating at 100° C. for 15 minutes, and conditioning the sealing layer at 25° C. and 55% relative humidity for 24 hours, (b) measuring the contact angles of a water droplet and a diiodomethane droplet on the formed sealing layer, and (c) calculating the total surface energy using the OWRK model. The sealing layer has a dispersive component of surface energy, and the dispersive component of surface energy may be greater than 40 mN / m. The dispersive component of surface energy of the sealing layer is determined on the sealing layer using a contact angle method.

[0028] The polyurethane of the sealing layer may be crosslinked by a crosslinking agent. The crosslinking agent may be a polyisocyanate, a polyfunctional polycarbodiimide, a polyfunctional aziridine, a silane coupling agent, a boron / titanium / zirconium-based crosslinking agent, or melamine formaldehyde. The polyurethane of the sealing layer may have a number average molecular weight of 1,000 to 2,000,000 Daltons.

[0029] The polyurethane of the sealing layer has a polar component of surface energy. The polar component of the surface energy of the polyurethane can be between 10 mN / m and 20 mN / m. The polar component of the surface energy of the polyurethane is determined on the polyurethane film using a contact angle method. The contact angle method includes the steps of (a) forming a polyurethane film by coating an aqueous polyurethane composition on a substrate at a dry thickness of 30 mm, heating at 100°C for 15 minutes, and conditioning the polyurethane film at 25°C and 55% relative humidity for 24 hours, (b) measuring the contact angles of water droplets and diiodomethane droplets on the formed polyurethane film, and (c) calculating the polar component of the surface energy of the polyurethane using the OWRK model.

[0030] The sealing layer may include a wetting agent, which may be an organosilicone surface tension reducing agent.

[0031] The conductive filler of the sealing layer can be carbon black. The carbon black can have an oil absorption of less than 100 mL per 100 mg of carbon black as measured by the oil absorption method according to ASTM 2414. The carbon black can have an average particle size of more than 20 nm as measured by electron microscopy according to ASTM D3849. Carbon black has a viscosity of 90 mg / L as measured by nitrogen adsorption according to ASTM D6556. 2 The carbon black may have a specific surface area of ​​less than 200 m / g as measured by nitrogen adsorption according to ASTM D6556. 2 / g and a volatile matter content, measured using the method according to DIN 53552, higher than 5%.

[0032] The poly(vinyl alcohol) homopolymer or poly(vinyl alcohol-co-ethylene) copolymer of the sealing layer may have a number average molecular weight of 1,000 to 1,000,000 Daltons. The poly(vinyl alcohol) homopolymer or poly(vinyl alcohol-co-ethylene) copolymer of the sealing layer may have a degree of hydrolysis of 92% to 99%. The poly(vinyl alcohol-co-ethylene) copolymer of the sealing layer may have an ethylene content of less than 9%.

[0033] The sealing layer may be used to seal the microcells of an electrophoretic display. The electrophoretic display may include an electro-optic material layer including a first light-transmissive electrode layer; a plurality of microcells and a sealing layer, each of the plurality of microcells including a bottom, a wall and an opening and containing an electrophoretic medium, the electrophoretic medium including at least one type of charged pigment particles dispersed in a non-polar fluid, the sealing layer spanning the openings of the plurality of microcells; a second electrode layer, the electro-optic material layer being disposed between the first light-transmissive electrode layer and the second electrode layer. The sealing layer may be formed from an aqueous polymer composition.

[0034] In another aspect, the invention provides a sealing layer comprising: (i) 30-70 wt. % of a water soluble poly(vinyl alcohol) homopolymer or poly(vinyl alcohol-co-ethylene) copolymer, based on the weight of the sealing layer excluding the solvent, the poly(vinyl alcohol) having a degree of hydrolysis of 90-99.9%, the poly(vinyl alcohol-co-ethylene) copolymer having a degree of hydrolysis of 90-99.9% and an ethylene content of less than 10%; and (ii) 7-29 wt. % of a polyurethane, based on the weight of the sealing layer excluding the solvent, the polyurethane having a total surface energy of (iii) a conductive filler, 1-45 wt % based on the weight of the sealing layer excluding solvent, the conductive filler being selected from the group consisting of carbon black, graphene, graphite, and carbon nanotubes, the conductive filler having a total surface energy, the total surface energy of the conductive filler being greater than 40 mN / m, the total surface energy being determined by the Washburn method using hexane as a test liquid. The sealing layer has a total surface energy. The total surface energy of the sealing layer may be greater than 55 mN / m. The total surface energy of the sealing layer is determined using a contact angle method. The contact angle method includes the steps of (a) forming a polyurethane film by coating the aqueous polyurethane composition on a substrate at a dry thickness of 30 mm, heating at 100° C. for 15 minutes, and conditioning the sealing layer at 25° C. and 55% relative humidity for 24 hours, (b) measuring the contact angles of a water droplet and a diiodomethane droplet on the formed polyurethane film, and (c) calculating the total surface energy of the polyurethane using the OWRK model. The sealing layer can have a dispersive component of surface energy, the dispersive component of surface energy being higher than 40 mN / m. The dispersive component of surface energy of the sealing layer is determined using the contact angle method.

[0035] The sealing layer may also be used to seal the microcells of the front plane laminate. The front plane laminate may include a first light transmissive electrode layer, an electro-optic material layer, an adhesive layer, and a sealing layer. and a release sheet. The electrophoretic display may include a first light-transmissive electrode layer, an electro-optic material layer, and a second electrode layer. The electro-optic material layer is disposed between the first light-transmissive electrode layer and the second electrode layer. The electro-optic material layer includes a plurality of microcells and a sealing layer. The sealing layer may be formed by an aqueous polymer composition. Each of the plurality of microcells includes a bottom, a wall, and an opening and contains an electrophoretic medium, the electrophoretic medium including at least one type of charged pigment particles dispersed in a non-polar fluid. The sealing layer spans the openings of the plurality of microcells.

[0036] A sealing layer may also be used to seal the microcells of the dual release sheet. The dual release sheet may include a first release sheet, a first adhesive layer, an electro-optic material layer, a second adhesive layer, and a second release sheet. The electro-optic material layer may include a plurality of microcells and a sealing layer. The sealing layer may be formed from an aqueous polymer composition. Each of the plurality of microcells includes a base, a wall, and an opening and contains an electrophoretic medium, the electrophoretic medium including at least one type of charged pigment particles dispersed in a non-polar fluid. The sealing layer spans the openings of the plurality of microcells. [Brief description of the drawings]

[0037] [Figure 1] FIG. 1 shows the structure of multiple microcells before they are filled and sealed.

[0038] [Diagram 2] FIG. 2 shows an example of an electro-optical device that includes a microcell structure.

[0039] [Diagram 3]FIG. 3 shows an example of a front plane laminate assembly that can be used to form an electro-optical device that includes a microcell structure.

[0040] [Figure 4] FIG. 4 shows an example of a dual release sheet that can be used to form an electro-optical device containing a microcell structure.

[0041] [Diagram 5] FIG. 5 illustrates a method for fabricating a microcell using a roll-to-roll process.

[0042] [Figure 6-1] 6A and 6B detail the creation of a microcell using photolithographic exposure through a photomask of a conductor film coated with a thermoset precursor.

[0043] [Figure 6-2] Figures 6C and 6D detail an alternative embodiment fabricated using photolithography, in which a combination of top and bottom exposures is used to allow one lateral wall to be hardened by a top photomask exposure and another lateral wall to be hardened by a bottom exposure through an opaque base conductor film.

[0044] [Figure 7A] 7A-7D show the steps of filling and sealing the array of microcells. [Figure 7B] 7A-7D show the steps of filling and sealing the array of microcells. [Figure 7C] 7A-7D show the steps of filling and sealing the array of microcells. [Figure 7D] 7A-7D show the steps of filling and sealing the array of microcells.

[0045] [Figure 8]8A and 8B show electro-optical device structures used to evaluate example sealing layers for their barrier properties and electro-optical performance, respectively.

[0046] [Figure 9A] 9A-9F show the waveforms used to evaluate the electro-optical performance of the example devices. [Figure 9B] 9A-9F show the waveforms used to evaluate the electro-optical performance of the example devices. [Figure 9C] 9A-9F show the waveforms used to evaluate the electro-optical performance of the example devices. [Figure 9D] 9A-9F show the waveforms used to evaluate the electro-optical performance of the example devices. [Figure 9E] 9A-9F show the waveforms used to evaluate the electro-optical performance of the example devices. [Figure 9F] 9A-9F show the waveforms used to evaluate the electro-optical performance of the example devices.

[0047] [Figure 10A] 10A-10D show microscopic images of the microcells evaluated for barrier properties. [Figure 10B] 10A-10D show microscopic images of the microcells evaluated for barrier properties. [Figure 10C] 10A-10D show microscopic images of the microcells evaluated for barrier properties. [Figure 10D] 10A-10D show microscopic images of the microcells evaluated for barrier properties.

[0048] [Figure 11] FIG. 11 shows the viscosity profile of the aqueous polymer composition at various shear rates.

[0049] [Figure 12]FIG. 12 shows microscopic images of polymer films containing combinations of poly(vinyl alcohol-co-ethylene) copolymer and polyurethane having various interfacial tensions. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0050] Detailed Description of the Invention The term "excluding solvent" referring to the weight of the sealing layer or the weight of the aqueous polymer composition of the present invention means that the weight of the sealing layer or the weight of the aqueous polymer composition referred to does not include water and other solvents that may be present in the sealing layer or the aqueous polymer composition.

[0051] The term "molecular weight" or "MW" as used herein, unless otherwise stated, refers to number average molecular weight. Number average molecular weight may be measured by gel permeation chromatography.

[0052] A. Microcell Structure

[0053] 1 shows the structure of a number of microcells 100 before being filled and sealed. Each microcell includes a base 101, a wall 102, and an opening 103.

[0054] B. Structure of an electro-optical device including a microcell structure

[0055] FIG. 2 shows an example of an electro-optical device 200 including a microcell structure 220. The example electro-optical device 200 includes a first light-transmissive electrode layer 210, a microcell layer 220, a sealing layer 230, an adhesive layer 240, and a second electrode layer 250. The microcell layer includes a plurality of microcells defined by a bottom 221 and a wall 222. Each of the plurality of microcells contains an electrophoretic medium 225, the medium including charged particles in a non-polar fluid. The microcells are sealed with a sealing layer 230, which spans the openings of the plurality of microcells. The second electrode layer 250 is connected to the sealing layer 230 using an adhesive layer 240. The plurality of microcells and the sealing layer constitute an electro-optical material layer of the electro-optical device 200. A source of an electric field (not shown) can connect the first light-transmissive electrode layer 210 with the second electrode layer 250. Application of an electric field across the electro-optic material layer causes charged particles to move through the electrophoretic medium to create an image that can be viewed by an observer looking at the viewing side 210 of the electro-optic device 200. An optional primer layer (not shown in FIG. 2) can be disposed between the first light-transmissive electrode layer 210 and the plurality of microcells 230.

[0056] The example electro-optical device shown in FIG. 2 may be constructed by a front plane laminate 300 shown in FIG. 3. The front plane laminate 300 includes a first light-transmitting electrode layer 310, a plurality of microcells 320, a sealing layer 330, an adhesive layer 340, and a release sheet 360. Each of the plurality of microcells contains an electrophoretic medium 325, which includes charged particles in a non-polar fluid. The microcells are sealed with a sealing layer 330, which spans the openings of the plurality of microcells. The release sheet 360 is connected to the sealing layer 330 using an adhesive layer 340. Removal of the release sheet 360 exposes a surface of the adhesive layer 340, which may be connected onto a second electrode layer to form an electro-optical device. An optional primer layer (not shown in FIG. 3) may be disposed between the first light-transmitting electrode layer 310 and the plurality of microcells 330.

[0057] The example electro-optical device shown in FIG. 2 may also be constructed with a dual release sheet 400 shown in FIG. 4. The dual release sheet 400 includes a first release sheet 480, a first adhesive layer 470, a plurality of microcells 420, a sealing layer 430, a second adhesive layer 440, and a second release sheet 460. Each of the plurality of microcells contains an electrophoretic medium 425, which includes charged particles in a non-polar fluid. The microcells are sealed with a sealing layer 430, which spans the openings of the plurality of microcells. The first release sheet 480 is connected to the plurality of microcells 420 with a first adhesive layer 470. The second release sheet is connected to the sealing layer 430 with a second adhesive layer 440. Removal of the first release sheet 460 exposes the surface of the first adhesive layer 470, which may be connected onto a first light-transmitting electrode layer. Removal of the second release sheet 460 exposes a surface of the second adhesive layer 440, which may be connected onto a second electrode layer to form an electro-optical device. An optional primer layer (not shown in FIG. 4) may be disposed between the first adhesive layer 470 and the plurality of microcells 430.

[0058] C. Formation of Microcell Structure

[0059] Techniques for constructing microcells. Microcells can be formed in either a batch-wise process or a continuous roll-to-roll process as disclosed in U.S. Pat. No. 6,933,098. The latter provides a continuous, low-cost, high-throughput manufacturing technique for generating compartments for use in a variety of applications, including delivery of beneficial agents and electrophoretic displays. Microcell arrays suitable for use with the present invention can be created using microembossing, as shown in FIG. The male mold 500 may be placed either above the web 504 or below the web 504 (not shown). However, alternative arrangements are possible. See, for example, U.S. Pat. No. 7,715,088, which is incorporated herein by reference in its entirety. The conductive substrate may be constructed by forming a conductor film 501 on a polymer substrate that will become the backing layer for the device. A composition 502 containing a thermoplastic, thermoset, or precursors thereof is then coated onto the conductor film. The thermoplastic or thermoset precursor layer is embossed by a male mold in the form of a roller, plate, or belt at a temperature above the glass transition temperature of the thermoplastic or thermoset precursor layer.

[0060] The thermoplastic or thermosetting precursors for the preparation of the microcells can be multifunctional acrylates or methacrylates, vinyl ethers, epoxides, and their oligomers or polymers, etc. The combination of multifunctional epoxides and multifunctional acrylates is also very useful for achieving desirable physical-mechanical properties. Crosslinkable oligomers that impart flexibility, such as urethane acrylates or polyester acrylates, can be added to improve the bending resistance of the embossed microcells. The composition may contain polymers, oligomers, monomers and additives, or may contain only oligomers, monomers and additives. The glass transition temperature (i.e., T g ) is typically in the range of about -70°C to about 150°C, or about -20°C to about 50°C. The microembossing process typically g A heated male mold, or a heated housing substrate against which the mold exerts pressure, can be used to control the temperature and pressure of the microembossing process.

[0061] As shown in FIG. 5, the mold is demolded while or after the precursor layer is cured to reveal an array of microcells 503. The curing of the precursor layer can be achieved by cooling, solvent evaporation, cross-linking by radiation, heat or moisture. If the curing of the thermosetting material precursor is achieved by UV radiation, the UV can be emitted from the bottom or top of the web onto the transparent conductor film as shown in the two figures. Alternatively, a UV lamp can be placed inside the mold. In this case, the mold must be transparent to allow the UV light to be emitted through the pre-patterned male mold onto the thermosetting material precursor layer. The male mold can be prepared by any suitable method, for example a diamond turning process or a photoresist process followed by either etching or electroplating. A master template for the male mold can be manufactured by any suitable method, for example electroplating. In electroplating, a thin layer of a seed metal, such as chrome inconel, is sputtered onto a glass base. (typically 3000 Å). The mold is then coated with a layer of photoresist and exposed to UV. A mask is placed between the UV and the layer of photoresist. The exposed areas of the photoresist are hardened. The unexposed areas are then removed by washing with a suitable solvent. The remaining hardened photoresist is dried and a thin layer of seed metal is sputtered again. The master is then ready for electroforming. A typical material used for electroforming is nickel cobalt. Alternatively, the master can be made from nickel by electroforming or electroless nickel deposition. The floor of the mold is typically between about 50 and 400 microns. The master is then fabricated as described in "Replication techniques for micro-optics", SPIE Proc. Vol. 3099, pp. 76-82 (1997) Other microengineering techniques can also be used, including e-beam writing, dry etching, chemical etching, laser writing or laser interference. Alternatively, the mold can be made using plastics, ceramics or metals by photomachining.

[0062] Prior to application of the UV-curable resin composition, the mold may be treated with a release agent to aid in the demolding process. The UV-curable resin may be degassed prior to dispensing and may contain a solvent, if desired. Solvent, if present, evaporates easily. The UV-curable resin is dispensed over the male mold by any suitable method, such as coating, dipping, pouring, etc. The dispensing device may be moving or stationary. The conductor film is superimposed on the UV-curable resin. If necessary, pressure may be applied to ensure proper bonding between the resin and the plastic and to control the thickness of the floor of the microcell. Pressure may be applied using laminating rollers, vacuum forming, compression devices, or any other similar means. If the male mold is metallic and opaque, the plastic substrate is typically transparent to the actinic radiation used to cure the resin. Conversely, the male mold may be transparent and the plastic substrate may not be transparent to the actinic radiation. To ensure good transfer of the molded features onto the transfer sheet, the conductor film must have good adhesion to the UV-curable resin, which should have good release properties for the mold surface.

[0063] Microcell arrays for the present invention typically include a preformed conductor film, such as indium tin oxide (ITO) conductor lines, although other conductive materials, such as silver or aluminum, may be used. The conductive layer may be backed by or integrated into a substrate, such as polyethylene terephthalate, polyethylene naphthalate, polyaramid, polyimide, polycycloolefin, polysulfone, epoxy, and composites thereof. The conductor film may be coated with a radiation-curable polymer precursor layer. The film and precursor layer are then imagewise exposed to radiation to form the microcell wall structure. After exposure, the precursor material is removed from the non-exposed areas, leaving the hardened microcell walls bonded to the conductor film / support web. Imagewise exposure may be accomplished by passing UV or other forms of radiation through a photomask to generate an exposure image or predetermined exposure pattern of the radiation-curable material coated on the conductor film. Although not generally necessary, the mask can be positioned and aligned relative to the conductor film, i.e., the ITO lines, such that the transparent mask portions align with the spaces between the ITO lines and the opaque mask portions align with the ITO material (intended for the cell floor areas of the microcells).

[0064] Photolithography. Microcells can also be produced using photolithography. A photolithography process for fabricating a microcell array is shown in Figures 6A and 5B. As shown in Figures 6A and 6B, a microcell array 600 can be prepared by exposing a radiation curable material 601a, coated on a conductor electrode film 602 by known methods, to UV light (or alternatively other forms of radiation, e-beam, etc.) through a mask 606 to form walls 601b corresponding to the image projected through the mask 606. The base conductor film 602 is preferably mounted on a supporting substrate base web (603), which may include a plastic material.

[0065] In the photomask 606 of Figure 6A, the dark squares 604 represent the opaque areas and the spaces between the dark squares represent the transparent areas 605 of the mask 606. UV is emitted through the transparent areas 605 onto the radiation curable material 601a. ​​The exposure is preferably performed directly on the radiation curable material 601a, i.e., UV does not pass through to the substrate 603 or to the base conductors 602 (top exposure). For this reason, neither the substrate 603 nor the conductors 602 need to be transparent to the UV or other wavelengths of radiation used.

[0066] As shown in Figure 6B, the exposed areas 601b are cured. The unexposed areas (protected by the opaque areas 604 of the mask 606) are then removed by a suitable solvent or developer to form the microcells 607. The solvent or developer is selected from those commonly used to dissolve or reduce the viscosity of radiation curable materials, such as methyl ethyl ketone (MEK), toluene, acetone, isopropanol, etc. The preparation of the microcells begins with placing a photoresist under a conductor film / substrate support web. This can also be achieved by placing a mask, where UV light is emitted from the bottom through a photomask and the substrate needs to be transparent to the radiation.

[0067] Image-wise exposure. Yet another alternative method for the preparation of the microcell array of the present invention by image-wise exposure is shown in Figures 6C and 6D. If opaque conductor lines are used, the conductor lines can be used as a photomask for exposure from the bottom. Durable microcell walls are formed by further exposure from the top through a second photomask having opaque lines perpendicular to the conductor lines. Figure 6C shows the use of both top and bottom exposure principles to produce the microcell array 610 of the present invention. The base conductor film 612 is opaque and patterned with lines. The radiation curable material 611a coated on the base conductor 612 and substrate 613 is exposed from the bottom through the conductor line pattern 612, which acts as the first photomask. The second exposure is performed from the "top" side through a second photomask 616 having a line pattern perpendicular to the conductor lines 612. The spaces 615 between the lines 614 are substantially transparent to UV light. In this process, the wall material 611b cures laterally from the bottom up and then cures vertically from the top down, together forming a complete microcell 617. The unexposed areas are then removed by a solvent or developer as previously described to reveal the microcell 617, as shown in Figure 6D.

[0068] The microcells may be constructed from thermoplastic elastomers that have good compatibility with the microcell and do not interact with the medium. Examples of useful thermoplastic elastomers include diblock, triblock, and multiblock copolymers of the ABA and (AB)n type, where A is styrene, α-methylstyrene, ethylene, propylene, or norbornene, and B is butadiene, isoprene, ethylene, propylene, butylene, dimethylsiloxane, or propylene sulfide, and A and B must not be the same in the formula. The number n is ≧1, preferably 1 to 10. Particularly useful are diblock or triblock copolymers of styrene or ox-methylstyrene, such as SB (poly(styrene-b-butadiene)), SBS (poly(styrene-b-butadiene-b-styrene)), SIS (poly(styrene-b-isoprene-b-styrene)), SEBS (poly(styrene-b-ethylene / butylene-b-styrene (stylene))) poly(styrene-b-ethylene / butylene-b-styrene (stylene)). Examples of suitable block copolymers include poly(styrene-b-dimethylsiloxane-b-styrene), poly((α-methylstyrene-b-isoprene), poly(α-methylstyrene-b-isoprene-b-α-methylstyrene), poly(α-methylstyrene-b-propylene sulfide-b-α-methylstyrene), and poly(α-methylstyrene-b-dimethylsiloxane-b-α-methylstyrene). Commercially available styrene block copolymers, such as the Kraton D and G series (Kraton Polymer, Houston, Tex.), are particularly useful. Crystalline rubbers, such as poly(ethylene-co-propylene-co-5-methylene-2-norbomene) or EPDM (ethylene-propylene-diene terpolymer) rubbers, such as Vistalon 6505 (Exxon Mobil, Houston, Tex.) and their grafted copolymers have also been found to be very useful.

[0069] The thermoplastic elastomer may be dissolved in a solvent or solvent mixture that is immiscible with the carrier in the microcell and exhibits a specific gravity lower than that of the carrier. Low surface tension solvents are preferred for the overcoating composition since they have better wetting properties than the microcell walls and the fluid. Solvents or solvent mixtures having a surface tension lower than 35 dynes / cm are preferred. Surface tensions lower than 30 dynes / cm are more preferred. Suitable solvents include alkanes (preferably C 6~12 Alkanes, such as heptane, octane or Exxon Chemical Comp any of the Isopar solvents, nonane, decane and their isomers), cycloalkanes (preferably C 6~12 Cycloalkanes, such as cyclohexane and decalin, alkylbenzenes (preferably mono- or di-C 1~6 Alkylbenzenes, such as toluene, xylene, etc.), alkyl esters (preferably C 2~5 Alkyl esters, such as ethyl acetate, isobutyl acetate, etc.) and C 3~5 Included are alkyl alcohols (e.g., isopropanol, etc. and their isomers). Mixtures of alkyl benzenes and alkanes are particularly useful.

[0070] In addition to the polymer additive, the polymer mixture may contain a wetting agent (surfactant). Also, in order to improve the adhesion of the sealant to the microcell and provide a more flexible coating process, wetting agents (e.g., FC surfactants from 3M Company, Zonyl fluorosurfactants from DuPont, fluoroacrylates, fluoromethacrylates, fluoro-substituted long-chain alcohols, perfluoro-substituted long-chain carboxylic acids and their derivatives, and Silwet silicone surfactants from OSi, Greenwich, Conn.) may be included in the composition. Other ingredients are also very useful to enhance the physical mechanical properties of the seal layer by crosslinking or polymerization reactions during or after the overcoating process, including crosslinking agents (e.g., bisazides, such as 4,4'-diazidodiphenylmethane and 2,6-di-(4'-azidobenzal)-4-methylcyclohexanone), vulcanizing agents (e.g., 2-benzothiazolyl disulfide and tetramethylthiuram disulfide), multifunctional monomers or oligomers (e.g., hexanediol, diacrylates, trimethylolpropane, triacrylates, divinylbenzene, diallylphthalene), thermal initiators (e.g., dilauroyl peroxide, benzoyl peroxide) and photoinitiators (e.g., isopropylthioxanthone (ITX), Irgacure 651 and Irgacure 369 from Ciba-Geigy).

[0071] The microcell array 700 may be prepared by any of the methods previously described. As shown in the cross-sectional views of Figures 7A-7D, the microcell walls 702 extend upward from the backing layer 701 and the conductive layer 710 to form open microcells. In one embodiment, the conductive layer 710 is formed on or in the backing layer 701. Although Figures 7A-7D show the conductive layer 710 extending continuously onto the backing layer 701, it is also possible for the conductive layer 710 to extend continuously below or within the backing layer 701 or to be interrupted by the microcell walls 702. The microcell array 700 may be cleaned and sterilized prior to filling to ensure that the beneficial agent is not compromised prior to use.

[0072] The microcells are then filled with an electrophoretic medium 725, which includes charged particles in a non-polar fluid, to form a plurality of filled microcells 770. The microcells may be filled using a variety of techniques. In some embodiments, blade coating may be used to fill the microcells to the depth of the microcell walls 702. In other embodiments, inkjet-type microinjection may be used to fill the microcells. In yet other embodiments, a microneedle array may be used to fill the array of microcells with the electrophoretic medium 725.

[0073] 7C, after filling, the microcells are sealed by applying a water-based polymer composition to form sealed microcells 780 that include a sealing layer 730. In some embodiments, the sealing process may include exposure to heat, dry hot air, or UV radiation. The sealing layer should have good barrier properties to the non-polar fluids of the electrophoretic medium 725.

[0074] In an alternative embodiment, various individual microcells can be filled with the desired mixture by using repeated photolithography. This process typically involves coating an array of empty microcells with a layer of photoresist acting as a positive type, selectively opening a certain number of microcells by imagewise exposing the positive type photoresist, subsequently developing the photoresist, filling the open microcells with the desired mixture, and sealing the filled microcells by a sealing process. These steps can be repeated to create sealed microcells filled with other mixtures. This procedure allows the formation of large sheets of microcells having the desired ratios or concentrations of mixtures.

[0075] Sealing of the filled microcells can be accomplished in several ways. One approach involves mixing the aqueous polymer composition with the electrophoretic medium composition. The aqueous polymer composition can be immiscible with the electrophoretic medium composition, preferably having a specific gravity lower than that of the electrophoretic medium composition. The two compositions, the aqueous polymer composition and the electrophoretic medium composition, are thoroughly mixed and immediately coated onto a number of microcells using a precise coating mechanism, such as a Mayer bar, gravure, doctor blade, slot coating or slit coating. Excess fluid is scraped off by a wiper blade or similar device. A small amount of a weak solvent or solvent mixture, such as isopropanol, methanol or an aqueous solution thereof, can be used to clean the fluid remaining on the top surface of the partition wall of the microcell. The aqueous polymer composition is then separated from the electrophoretic medium composition and floats on top of the electrophoretic medium composition. Alternatively, after the mixture of electrophoretic medium composition and aqueous polymer composition is filled into the microcell, a substrate can be laminated on top to control the metering of the mixture of compositions and promote phase separation of the aqueous polymer composition from the electrophoretic medium composition to form a uniform seal layer. The substrate used can be a functional substrate in the final structure or a sacrifice substrate, such as a release substrate, that can be removed later. The seal layer is then formed by curing the aqueous polymer composition in situ (i.e., when in contact with the electrophoretic medium composition). Curing of the aqueous polymer composition can be accomplished by UV or other forms of radiation, such as visible light, IR, or electron beam. Alternatively, heat or moisture can also be used to cure the aqueous polymer composition in place when a heat or moisture curable composition is used.

[0076] In the second approach, the electrophoretic medium composition may be filled into the microcells first, and then the aqueous polymer composition is overcoated onto the filled microcells. Overcoating may be accomplished by conventional coating and printing processes, such as blanket coating, inkjet printing, or other printing processes. In this approach, the sealing layer is formed in situ by curing the aqueous polymer composition by solvent evaporation, radiation, heat, moisture, or interfacial reaction. Interfacial polymerization followed by UV curing is beneficial to the sealing process. Intermixing of the electrophoretic medium composition with the sealing overcoat is significantly suppressed by the formation of a thin barrier layer at the interface by interfacial polymerization. The sealing is then completed by a post-curing step, for example by UV radiation. The degree of intermixing may be further reduced if the specific gravity of the aqueous polymer composition is lower than that of the electrophoretic medium composition. Volatile organic solvents may be used to adjust the viscosity and thickness of the sealing overcoat. The rheology of the aqueous polymer composition may be tailored for optimal sealability and coatability. If a volatile solvent is used in the overcoat, it is preferred that the volatile solvent be immiscible with the solvent in the electrophoretic medium composition.

[0077] After the microcells are filled and sealed, the sealed array can be laminated with a second electrode layer 750 containing multiple electrodes. The second electrode layer 750 is shown in FIG. 7D. 7D , the second electrode layer 750 is bonded onto the sealing layer 730 to form the electro-optical device 790. An adhesive may be used to bond the second electrode layer 750 onto the sealing layer 730 (adhesive layer not shown in FIG. 7D ). The adhesive may be conductive. The adhesive of the adhesive layer may be a pressure sensitive adhesive, a hot melt adhesive, or a heat, moisture or radiation curable adhesive. The lamination adhesive may be post cured by radiation, e.g., UV, through the top conductive layer if the top conductive layer is radiation transparent. In other embodiments, multiple electrodes may be bonded directly to the sealed array of microcells.

[0078] In general, the microcells may be of any shape, and their size and shape may vary. The microcells may be of substantially uniform size and shape in a system. However, it is possible to have microcells of a mixture of shapes and sizes. The openings of the microcells may be circular, square, rectangular, hexagonal, or any other shape. The size of the partition area between the openings may also vary. The dimensions of each individual microcell are approximately 1×10 1 ~Approx. 1×10 6 μm 2 , or approximately 1 × 10 2 ~Approx. 1×10 6 μm 2 , or approximately 1 × 10 3 ~Approx. 1×10 5 μm 2 The range may be:

[0079] The depth of the microcells can range from about 5 to about 200 μm, or from about 10 to about 100 μm. The ratio of opening to total area ranges from about 0.05 to about 0.95, or from about 0.4 to about 0.9.

[0080] An electrophoretic display usually includes a layer of electro-optical material and at least two other layers disposed on either side of the electro-optical material layer, one of these two layers being an electrode layer. In most such displays, both layers are electrode layers, and one or both of the electrode layers are patterned to define the pixels of the display. For example, one electrode layer may be patterned into elongated row electrodes and the other into elongated column electrodes extending at right angles to the row electrodes, the pixels being defined by the intersections of the row and column electrodes. Alternatively, and more commonly, one electrode layer has the form of a single continuous electrode and the other electrode layer is patterned into a matrix of pixel electrodes, each of which defines one pixel of the display. In another type of electrophoretic display, intended for use with a stylus, printhead or similar movable electrode that is separate from the display, only one of the layers adjacent to the electro-optic material layer contains electrodes; the layer on the opposite side of the electro-optic material layer is typically a protective layer intended to prevent the movable electrode from damaging the electro-optic material layer.

[0081] The manufacture of a three-layer electrophoretic display usually involves at least one lamination operation. For example, some of the aforementioned MIT and E Ink patents and applications describe methods for producing encapsulated electrophoretic displays in which an encapsulated electrophoretic medium, including capsules in a binder, is coated onto a flexible substrate including indium tin oxide (ITO) or a similar conductive coating coated onto a plastic film. Separately, a backplane is prepared that includes an array of pixel electrodes and conductors in a suitable arrangement to connect the pixel electrodes and drive the circuitry. To form the final display, the substrate having the electro-optical material layer is laminated to the backplane using a lamination adhesive.

[0082] The aforementioned U.S. Patent No. 6,982,178 describes a method of assembling a solid-state electrophoretic display that is well suited for mass production. Essentially, this patent describes a so-called "front plane laminate" ("FPL") that includes, in order, a light-transmissive electrode layer, a layer of electro-optic material in electrical contact with the light-transmissive electrode layer, an adhesive layer, and a release sheet. Typically, the light-transmissive electrode layer is supported on a light-transmissive substrate that can be mounted on a substrate that is capable of being folded or shrunk to the size of a 10 inch (254 mm) diameter drum (for example) without undergoing permanent deformation. It is preferably flexible in the sense that it can be manually wrapped around a substrate. The term "light-transmitting" is used in this patent and herein to mean that the layer so designated transmits sufficient light to enable an observer looking through the layer to observe a change in the display state of the electrophoretic medium, which change is normally seen through the light-transmitting electrode layer and the adjacent substrate (if present). If the electrophoretic medium exhibits a change in reflectivity of non-visible wavelengths, the term "light-transmitting" should of course be interpreted as referring to the transmission of the relevant non-visible wavelengths. The substrate is typically a polymer film, usually having a thickness in the range of about 1 to about 25 mils (25 to 634 μm), preferably about 2 to about 10 mils (51 to 254 μm). The light-transmitting electrode layer may conveniently be a thin metal or metal oxide layer, for example, aluminum or ITO, or a conductive polymer. Aluminum or ITO-coated poly(ethylene terephthalate) (PET) films are suitable for use with, for example, EIdu Commercially available as "aluminized Mylar" ("Mylar" is a registered trademark) from Pont de Nemours & Company, Wilmington, Del., such commercially available materials may be used with good results in the front plane laminate. Assembly of an electrophoretic display using such a front plane laminate may be performed by removing the release sheet from the front plane laminate and contacting the adhesive layer with the backplane under conditions effective to adhere the adhesive layer to the backplane, thereby securing the adhesive layer, electro-optic material layer, and light-transmitting electrode layer to the backplane. This process is well suited to mass production, as the front plane laminate can be mass-produced, typically using roll-to-roll coating techniques, and then cut into pieces of any size required for use with a particular backplane.

[0083] No. 7,561,324 describes a so-called "dual release sheet," which is essentially a simplification of the front plane laminate of the aforementioned U.S. Pat. No. 6,982,178. One form of dual release sheet includes a layer of electro-optic material sandwiched between two adhesive layers, one or both of which are covered by a release sheet. Another form of dual release sheet includes a layer of solid electro-optic material sandwiched between two release sheets. Both forms of dual release film are intended for use in processes generally similar to the processes for assembling electrophoretic displays from front plane laminates already described, but involving two separate laminates. Typically, in a first laminate, the dual release sheet is laminated to a front electrode to form a front subassembly, and then in a second laminate, the front subassembly is laminated to a backplane to form the final display, although these two stacking orders can be reversed if desired. No. 7,839,564 describes a so-called "inverted front plane laminate," which is a variation of the front plane laminate described in the aforementioned U.S. Pat. No. 6,982,178. The inverted front plane laminate may include, in order, at least one of a light-transmissive protective layer and a light-transmissive electrode layer, an adhesive layer, an electro-optic material layer, and a release sheet. The inverted front plane laminate is used to form an electrophoretic display having a layer of laminating adhesive between the electro-optic material layer and the light-transmissive electrode layer, with or without a typically thin second adhesive layer between the electro-optic material layer and the backplane. Such an electrophoretic display may combine good resolution with good low temperature performance.

[0084] Electrophoretic medium.

[0085] Electrophoretic medium, in the context of the present invention, refers to a composition in a microcell. The microcell can be filled with at least one type of charged pigment particles in a non-polar fluid for display applications. The electrophoretic medium is a mixture of one type of charged type particles, or one or more types of particles having different colors, charges and charge polarities. The charged particles move in the electrophoretic medium under the influence of an electric field applied across the electro-optical material layer. The charged particles can be inorganic or organic pigments with a polymer surface treatment to improve their stability. The electrophoretic medium can include pigments having white, black, cyan, magenta, yellow, blue, green, red, and other colors. The electrophoretic medium can also include charge control agents, charge adjuvants, rheology modifiers, and other additives. Examples of non-polar fluids include hydrocarbons such as Isopar, decahydronaphthalene (decalin), 5-ethylidene-2-norbornene, fatty oils, paraffin oil, silicon liquid, aromatic hydrocarbons such as toluene, xylene, Phenylxylylethane, dodecylbenzene or alkylnaphthalenes, halogenated solvents such as perfluorodecalin, perfluorotoluene, perfluoroxylene, dichlorobenzotrifluoride, 3,4,5-trichlorobenzotrifluoride, chloropentafluoro-benzene, dichlorononane or pentachlorobenzene, and perfluorinated solvents such as FC-43, FC-70 or FC-5060 from 3M Company, St. Paul MN, low molecular weight halogen-containing polymers such as poly(perfluoropropylene oxide) from TCI America, Portland, Oregon, poly(chlorotrifluoro-ethylene) such as halocarbon oils from Halocarbon Product Corp., River Edge, NJ, perfluoropolyalkyl ethers such as Galden from Ausimont, or Krytox oils and Greases K-Fluid series from DuPont, Delaware, polydimethylsiloxane-based silicone oils (DC-200) from Dow-corning.

[0086] Sealing layer

[0087] The sealing layer must provide a barrier to the electrophoretic medium so that the non-polar fluid is not removed from the microcells, and must not negatively affect the electro-optical performance of the device.

[0088] One important property of the sealing layer is its electrical volume resistivity. If the resistivity of the sealing layer is too high, a significant voltage drop occurs within the sealing layer, necessitating a voltage boost across the electrodes to operate the device. Boosting the voltage across the electrodes in this manner is undesirable, as it increases the power consumption of the display and may require the use of more complex and expensive control circuitry to handle the boosted voltage. On the other hand, if there is too little sealing, undesirable crosstalk between adjacent pixel electrodes is observed, degrading image quality. In addition, since volume resistivity typically increases rapidly with decreasing temperature, too high a volume resistivity of the sealing layer negatively impacts the electro-optical performance of the display at low temperatures. The sealing layer should have a resistivity of 4×10 7 The sealing layer may have a volume resistivity of 5×10 ohm.cm or higher. 7 The sealing layer may have a volume resistivity of 10 ohm.cm or higher. 8 The sealing layer may have a volume resistivity of 5×10 ohm.cm or higher. 7 ~10 12 ohms.cm, or 10 8 ~10 10 The sealing layer may have a volume resistivity of 10 ohms.cm. 10 or less.

[0089] Another important property of the sealing layer besides the barrier properties and volume resistivity is its moisture absorption: if the sealing layer absorbs significant amounts of moisture from the environment over time, the electro-optical performance of the device will be poor.

[0090] The inventors have demonstrated that a combination of water-soluble poly(vinyl alcohol) homopolymer or poly(vinyl alcohol-co-ethylene) copolymer and polyurethane has a strength of more than 40 mN / m. It has been found that a sealing layer having a total surface energy greater than 55 mN / m formed by an aqueous polymer composition containing a conductive filler having a high total surface energy and an aqueous carrier provides excellent barrier properties.

[0091] The inventors have also found that a sealing layer comprising a combination of a water-soluble poly(vinyl alcohol) homopolymer or poly(vinyl alcohol-co-ethylene) copolymer, polyurethane, and a conductive filler forms a sealing layer for electro-optic displays that has excellent electro-optic performance, especially at low temperatures.

[0092] The sealing layer may include (i) 30-70 wt % of a water soluble poly(vinyl alcohol) homopolymer or poly(vinyl alcohol-co-ethylene) copolymer, based on the weight of the sealing layer excluding the solvent, (ii) 7-29 wt % of a polyurethane, based on the weight of the sealing layer excluding the solvent, and (iii) 1-45 wt % of a conductive filler, based on the weight of the sealing layer excluding the solvent. The poly(vinyl alcohol) homopolymer may have a degree of hydrolysis of 90-99.5% and the poly(vinyl alcohol-co-ethylene) copolymer may have a degree of hydrolysis of 90-99.5% and an ethylene content of less than 10. The degree of hydrolysis of the poly(vinyl alcohol) homopolymer and poly(vinyl alcohol-co-ethylene) copolymer may be 92-99%, or 93-99%, or 92-98%, or 92-96%, or 95-99%, or 92-95%. The ethylene content of poly(vinyl alcohol-co-ethylene) copolymers may be less than 9%, or less than 8.5%, or less than 8%. The ethylene content of poly(vinyl alcohol-co-ethylene) copolymers may be 7-11%, or 8-10%, or 8-9%, or 9-11%, or 10-11%. The degree of hydrolysis of polyvinyl alcohol homopolymers and copolymers is conventionally reported by the manufacturers of such polymers and indicates the ratio of moles of vinyl alcohol units in the polymer to total vinyl units. The other units are typically vinyl acetate (esters). The ethylene content of poly(vinyl alcohol-co-ethylene) copolymers is also reported by the manufacturers and indicates the ratio of moles of ethylene units in the polymer to other units. In this case, the other units are vinyl alcohol.

[0093] The sealing layer may be formed by an aqueous polymer composition. The aqueous polymer composition may include (i) 30-70 wt. % of a water-soluble poly(vinyl alcohol) homopolymer or poly(vinyl alcohol-co-ethylene) copolymer, based on the weight of the aqueous polymer composition excluding the solvent, (ii) 7-29 wt. % of a polyurethane, based on the weight of the aqueous polymer composition excluding the solvent, and (iii) 1-45 wt. % of a conductive filler, based on the weight of the aqueous polymer composition excluding the solvent, and (iv) an aqueous carrier. The poly(vinyl alcohol) homopolymer may have a degree of hydrolysis of 90-99.5%, and the poly(vinyl alcohol-co-ethylene) copolymer may have a degree of hydrolysis of 90-99.5% and an ethylene content of less than 10%. The degree of hydrolysis of the poly(vinyl alcohol) homopolymer and the poly(vinyl alcohol-co-ethylene) copolymer may be 92-99%, or 92-95%. The ethylene content of the poly(vinyl alcohol-co-ethylene) copolymer may be less than 9%, or less than 8.5%, or less than 8%. The degree of hydrolysis of polyvinyl alcohol homopolymers and copolymers is conventionally reported by the manufacturers of such polymers and indicates the ratio by mole of vinyl alcohol units in the polymer to the total vinyl units. The other units are typically vinyl acetate (ester). The ethylene content of poly(vinyl alcohol-co-ethylene) copolymers is also reported by the manufacturers and indicates the ratio by mole of ethylene units in the polymer to the other units. In this case, the other units are vinyl alcohol. The application, drying or curing of the aqueous polymer composition is carried out by applying (i) 30 to 70 weight percent of a water-soluble poly(vinyl alcohol) homopolymer or poly(vinyl alcohol-co-ethylene) copolymer based on the weight of the sealing layer excluding the solvent. and (ii) from 7 to 29 weight percent polyurethane, based on the weight of the sealing layer excluding the solvent. The sealing layer may have some residual water and other solvents remaining in the layer after drying or curing.

[0094] The sealing layer may comprise 30-70% by weight, or 30-65% by weight, or 30-60% by weight, or 30-55% by weight, or 30-50% by weight, or 35-70% by weight, or 35-65% by weight, or 35-60% by weight, or 35-55% by weight, or 35-50% by weight, or 40-70% by weight, or 40-65% by weight, or 40-60% by weight, or 40-55% by weight of a water soluble poly(vinyl alcohol) homopolymer or poly(vinyl alcohol-co-ethylene) copolymer, based on the weight of the aqueous polymer composition excluding the solvent.

[0095] The sealing layer may comprise 7-29% by weight, or 10-29% by weight, or 15-29% by weight, or 17-29% by weight, or 18-29% by weight, or 20-29% by weight, or 10-25% by weight, or 15-25% by weight, or 17-25% by weight, or 18-25% by weight, or 20-25% by weight, or 10-21% by weight, or 15-21% by weight, or 17-21% by weight of polyurethane based on the weight of the aqueous polymer composition excluding the solvent.

[0096] The sealing layer may comprise a water soluble poly(vinyl alcohol) homopolymer or poly(vinyl alcohol-co-ethylene) copolymer in a weight ratio to polyurethane of 4.0 to 1.2, or 3.5 to 1.2, or 3.3 to 1.2, or 3.0 to 1.2, or 2.5 to 1.2, or 4.0 to 1.5, or 3.5 to 1.5, or 3.3 to 1.5, or 3.0 to 1.5, or 2.5 to 1.5, or 4.0 to 1.8, or 3.5 to 1.8, or 3.3 to 1.8, or 3.0 to 1.8, or 2.5 to 1.8, or 4.0 to 2.2, or 3.5 to 2.2, or 3.3 to 2.2, or 3.0 to 2.2, or 2.5 to 2.2.

[0097] The poly(vinyl alcohol) homopolymers and poly(vinyl alcohol-co-ethylene) copolymers of the sealing layer can have a weight average molecular weight (MW) of 1,000 to 1,000,000 Daltons, or 10,000 to 500,000 Daltons, or 20,000 to 400,000 Daltons.

[0098] Polyurethanes are typically prepared by polyaddition processes involving diisocyanates. Non-limiting examples of polyurethanes include polyether polyurethanes, polyester polyurethanes, polycarbonate polyurethanes, polyether polyureas, polyureas, polyester polyureas, polyester polyureas, polyisocyanates (e.g., polyurethanes containing isocyanate bonds), and polycarbodiimides (e.g., polyurethanes containing carbodiimide bonds). Generally, polyurethanes contain urethane groups. The polyurethanes utilized in the aqueous polymer compositions and sealing layers described herein can be prepared using methods known in the art. Preferably, the polyurethanes of the aqueous polymer compositions of the present invention are polyester polyurethanes, polycarbonate polyurethanes, and mixtures thereof.

[0099] The polyurethane of the sealing layer may have a weight average molecular weight (MW) of 1,000 to 2,000,000 daltons, or 10,000 to 300,000 daltons, or 15,000 to 200,000 daltons.

[0100] Good barrier properties were observed for sealing layers containing polyurethanes with a polar component of surface energy between 10 and 20 mN / m. The component may be 10-25mN / m, or 10-20mN / m, or 11-20mN / m, or 12-20mN / m, or 13-20mN / m, or 14-20mN / m, or 15-20mN / m, or 10-18mN / m, or 11-18mN / m, or 12-18mN / m, or 13-18mN / m, or 14-18mN / m, or 15-18mN / m, or 10-16mN / m, or 11-16mN / m, or 12-16mN / m, or 13-16mN / m, or 14-16mN / m.

[0101] The polyurethane of the sealing layer formed by the water-based polymer composition may be added to the water-based polymer composition as an aqueous solution or dispersion or emulsion, or as a latex.

[0102] The interfacial tension between the water-soluble poly(vinyl alcohol) polymer or poly(vinyl alcohol-co-ethylene) copolymer and polyurethane can be less than 2 mN / m. The interfacial tension between the water-soluble poly(vinyl alcohol) polymer or poly(vinyl alcohol-co-ethylene) copolymer and polyurethane can be less than 1.9 mN / m, or less than 1.8 mN / m, or less than 1 mN / m, or less than 0.8 mN / m, or less than 0.6 mN / m, or less than 0.7 mN / m.The interfacial tension between the water-soluble poly(vinyl alcohol) polymer or poly(vinyl alcohol-co-ethylene) copolymer and the polyurethane is 0-2.0 mN / m, or 0.1-2.0 mN / m, or 0.2-2.0 mN / m, or 0.3-2.0 mN / m, or 0.4-2.0 mN / m, or 0.5-2.0 mN / m, or 0.6-2.0 mN / m, or 0.7-2.0 mN / m, or 0.8-2.0 mN / m, or 1.0-2.0 mN / m, or 1.5-2.0 mN / m, or 0-1.8 mN / m, or 0.1- 1.8mN / m, or 0.2-1.8mN / m, or 0.3-1.8mN / m, or 0.4-1.8mN / m, or 0.5-1.8mN / m, or 0.6-1.8mN / m, or 0.7-1.8mN / m, or 0.8-1.8mN / m, or 1.0-1.8mN / m, or 0-1.5mN / m, or 0.2-1.5mN / m, or 0.3-1.5mN / m, or 0.4-1.5mN / m, or 0.5-1.5mN / m, or 0.6-1.5mN / m, or 0.7-1.5mN / m, or 0.8-1.5mN / m m, or 1.0-1.5mN / m, or 0-1.0mN / m, or 0.1-1.0mN / m, or 0.2-1.0mN / m, or 0.3-1.0mN / m, or 0.4-1.0mN / m, or 0.5-1.0mN / m, or 0.6-1.0mN / m, or 0.7-1.0mN / m, or 0.8-1.0mN / m, or 0-0.8mN / m, or 0.1-0.8mN / m, or 0.2-0.8mN / m, or 0.3-0.8mN / m, or 0.4-0.8mN / m, or 0.5-0.8mN / m, or 0-0 .7mN / m, or 0.1-0.7mN / m, or 0.2-0.7mN / m, or 0.3-0.7mN / m, or 0.4-0.7mN / m, or 0-0.6mN / m, or 0.1-0.6mN / m, or 0.2-0.7mN / m, or 0.3-0.7mN / m, or 0-0.6mN / m, or 0.1-0.6mN / m, or 0.2-0.6mN / m, or 0.3-0.6mN / m, or 0.4-0.6mN / m, or 0-0.5mN / m, or 0.1-0.5mN / m, or 0.2-0.5mN / m.

[0103] The aqueous polymer composition may comprise 40 to 96 wt. %, or 60 to 95 wt. %, or 70 to 92 wt. %, or 80 to 90 wt. % of the aqueous carrier, based on the weight of the aqueous polymer composition.

[0104] The sealing layer may include a crosslinked polyurethane.

[0105] The polyurethane may be crosslinked by a crosslinking agent, which may be a polyisocyanate, a polyfunctional polycarbodiimide, a polyfunctional aziridine, a silane coupling agent, a boron / titanium / The crosslinking agent is preferably a zirconium-based crosslinking agent, or melamine formaldehyde. Since the sealing layer is formed by the aqueous polymer composition, the aqueous polymer composition may contain 0.5 to 10% by weight of the crosslinking agent based on the weight of the aqueous polymer composition excluding the solvent. The crosslinking agent forms chemical bonds between polyurethane molecules. Crosslinking of the polyurethane of the sealing layer may increase the adhesion between the sealing layer and the microcell. The crosslinking agent is preferably soluble or dispersible in the aqueous carrier of the aqueous polymer composition. The crosslinking agent may be a monomer, oligomer or polymer. Examples of the crosslinking agent include polyisocyanates, polyfunctional polycarbodiimides, polyfunctional aziridines, silane coupling agents, boron / titanium / zirconium-based crosslinking agents, or melamine formaldehyde. The polycarbodiimide crosslinking agent is reactive at acidic pH conditions. Preferably, the crosslinking agent does not include a sulfosuccinate surfactant.

[0106] The aqueous polymer composition forming the sealing layer may also include a pH adjuster. The pH adjuster is added to the aqueous polymer composition to adjust its pH to a value between 6.5 and 8.5. One example of a pH adjuster is ammonium hydroxide, but various acids and bases can be used. The pH adjuster can increase the pH of the aqueous polymer composition, thereby reducing the crosslinking rate of the aqueous polymer composition before use, and provide optimal pH conditions for the rheology modifier to interact with the particles of the aqueous polymer composition, improving its effectiveness. The pH adjuster can be used in a content of 0.2% by weight to 1% by weight based on the weight of the aqueous polymer composition excluding the solvent.

[0107] The sealing layer may also include 0.05-10 wt. %, or 0.1-5 wt. %, or 0.5-2 wt. % of a rheology modifier, based on the weight of the sealing layer excluding the solvent. The rheology modifier increases the storage stability of the aqueous polymer composition used to form the sealing layer. The rheology modifier also promotes film formation, improves seal stability, and provides other functions. Non-limiting examples of rheology modifiers include associative thickeners, alkali swellable acrylic emulsions, and other polymeric thickeners. The aqueous polymer composition may be shear thinning, i.e., its viscosity is reduced at higher shear. For example, the rheology profile of the aqueous polymer composition may be 10 -4 Viscosity at a shear rate of 1 / sec and 10 2 Between the viscosity at a shear rate of 1 / sec, a decrease in viscosity of 5 to 10,000 times can be observed.

[0108] The sealing layer may also include a wetting agent, also called a surfactant. Examples of wetting agents include 3M Examples of wetting agents include FC surfactants from Company, Zonyl fluorosurfactants, fluoroacrylates, fluoromethacrylates, fluoro-substituted long chain alcohols, perfluoro-substituted long chain carboxylic acids and their derivatives from DuPont, and Silwet silicone surfactants from OSi, Greenwich, Conn. The wetting agents can increase the affinity between the sealing layer and the microcell, enhance the interfacial area between them, improve adhesion of the sealing layer to the microcell, and provide a more flexible coating process.

[0109] The sealing layer may also include 1-45% by weight of a filler, based on the weight of the sealing layer excluding the solvent. The filler may be a conductive filler. The filler of the sealing layer may be selected from the group consisting of carbon black, graphene, graphite, and carbon nanotubes. The filler reduces the volume resistivity of the sealing layer, but may also affect other properties of the layer, such as its surface energy. To be useful as a filler, carbon black must have good dispersibility in the aqueous polymer composition. The aqueous polymer composition and corresponding sealing layer may include 1-45% by weight, or 5-45% by weight, or 10-45% by weight, or 15-40% by weight, or 17-38% by weight, or 18-36% by weight, or 15-36% by weight, or 18-36% by weight, or 20-36% by weight of a filler, based on the weight of the aqueous polymer composition excluding the solvent.

[0110] It has been observed by the inventors that a key aspect enabling good electro-optical performance, especially at low temperatures, is the surface energy of the sealing layer. The total surface energy of the sealing layer must be greater than 55 mN / m. The total surface energy of the sealing layer may be 55-80 mN / m, or 55-70 mN / m. The dispersive component of the surface energy may be higher than 40 mN / m. The dispersive component of the surface energy of the sealing layer may be higher than 41 mN / m, or higher than 43 mN / m. The dispersive component of the surface energy of the sealing layer may be 40-60 mN / m, or 40-50 mN / m, or 40-45 mN / m.

[0111] The high surface energy of the sealing layer can be achieved by the selection of the components of the aqueous polymer composition forming the sealing layer. For example, the conductive filler can have a total surface energy of more than 40 mN / m, or more than 45 mN / m, or more than 50 mN / m. The dispersed component of the conductive filler can be more than 15 mN / m, or more than 20 mN / m. The conductive filler can have a total surface energy of 40-80 mN / m, or 40-70 mN / m, or 40-65 mN / m, or 40-60 mN / m. The dispersed component of the conductive filler can be 15-40 mN / m, or 15-30 mN / m, or 15-25 mN / m. The high surface energy of the sealing layer can also be achieved by selecting a polyurethane having a high surface energy. For example, the polyurethane of the sealing layer can have a total surface energy of more than 50 mN / m. The dispersed component of the polyurethane can be more than 40 mN / m. The polyurethane may have a total surface energy of greater than 45 mN / m, or greater than 50 mN / m, or greater than 55 mN / m. The polyurethane may have a total surface energy of 45-75 mN / m, or 45-70 mN / m, or 45-65 mN / m, or 50-75 mN / m, or 50-70 mN / m, or 50-65 mN / m. The dispersion component of the polyurethane may be 40-70 mN / m, or 40-50 mN / m.

[0112] The inventors have found that the oil absorption value of the carbon black used in the sealing layer is preferably 100 mL / 100 mg of carbon black or less. Electro-optic displays having a sealing layer containing a carbon black filler with an OAN of less than 100 mL / 100 mg of carbon black exhibit improved resolution, as shown in Table 10 below. The oil absorption of the carbon black in the sealing layer can be less than 95 mL / 100 mg of carbon black, or less than 90 mL / 100 mg of carbon black, or less than 85 mL / 100 mg of carbon black, or less than 80 mL / 100 mg of carbon black, or less than 70 mL / 100 mg of carbon black, or less than 60 mL / 100 mg of carbon black, or less than 50 mL / 100 mg of carbon black.

[0113] The oil absorption of the carbon black in the sealing layer is 30mL to 100mL per 100mg of carbon black, or 40mL to 100mL per 100mg of carbon black, or 45mL to 100mL per 100mg of carbon black, or 50mL to 100mL per 100mg of carbon black, or 40mL to 95mL per 100mg of carbon black, or 45mL to 95mL per 100mg of carbon black, or 50mL to 95mL per 100mg of carbon black, or It may be 55mL to 95mL per 100mg of carbon black, or 40mL to 90mL per 100mg of carbon black, or 45mL to 90mL per 100mg of carbon black, or 50mL to 90mL per 100mg of carbon black, or 40mL to 80mL per 100mg of carbon black, or 45mL to 80mL per 100mg of carbon black, or 50mL to 80mL per 100mg of carbon black, or 55mL to 80mL per 100mg of carbon black.

[0114] Oil absorption is typically reported by carbon black manufacturers as OAN, measured using a method according to ASTM 2414. Oil absorption represents the degree of structure and agglomeration of carbon black particles. That is, the higher the OAN, the more structured (bonded together and having a branched structure) and / or the more agglomerated the particles are. Carbon black with more structure / agglomeration can generally provide higher electrical conductivity to the sealing layer.

[0115] Another conclusion of the experimental work disclosed herein is that the carbon black filler in the sealing layer preferably has an average particle size greater than 20 nm. Thus, carbon black having a very small average particle size is difficult to disperse, resulting in a sealing layer with inferior properties. The average particle size of the carbon black filler in the sealing layer may be greater than 30 nm, or greater than 40 nm, or greater than 50 nm, or greater than 60 nm, or greater than 80 nm, or greater than 100 nm. The average particle size of the carbon black filler in the sealing layer may be 31-150 nm, or 40-150 nm, or 50-150 nm, or 60-150 nm, or 80-150 nm, or 100-150 nm, or 31-100 nm, or 40-100 nm, or 50-100 nm. The average particle size is another physical property of the carbon black grade, reported by the carbon black manufacturer. The average particle size typically corresponds to the average diameter of the particles as determined by transmission electron microscopy (TEM) using ASTM method D3849.

[0116] As can be seen from Table 7 in the Examples section, improved results in terms of carbon black dispersion quality were observed at 90 m 2 This was achieved by using a carbon black filler having a specific surface area of ​​less than 85 m / g. 2 / g or less than 80m 2 / g or less than 75m 2 / g or less than 70m 2 / g or less than 60m 2 / g or less than 50m 2 / g or less than 40m 2 The carbon black in the sealing layer may have a specific surface area of ​​20 to 89 m / g. 2 / g, or 30-89m 2 / g, or 35-89m 2 / g, or 40-89m 2 / g, or 50-89m 2 / g, or 20-88m 2 / g, or 30-88m 2 / g, or 35-88m 2 / g, or 40-88m 2 / g, or 50-88m 2 / g, or 20-85m 2 / g, or 30-85m 2 / g, or 35-85m 2 / g, or 40-85m 2 / g, or 50-85m 2 / g, or 20-80m 2 / g, or 30-80m 2 / g, or 35-80m 2 / g, or 40-80m 2 / g, or 50-80m 2 / g, or 20-70m 2 / g, or 30-70m 2 / g, or 35-70m 2 / g, or 40-70m 2 / g, or 50-70m 2 / g, or 20-65m 2 / g, or 30-65m 2 / g, or 35-65m 2 / g, or 40-65m 2 / g, or 50-65m 2 / g. 2Carbon blacks having a specific surface area of ​​200 m / g and higher exhibit poor dispersion quality, which results in poor aqueous polymer compositions and sealing layers with poor properties. However, the inventors have also found that carbon black products having a higher volatile content can be dispersed more easily than carbon black products having a lower volatile content, even if they have a high specific surface area. The relevant results are shown in Table 7. That is, the carbon black of the sealing composition of the present invention has a low dispersion quality at 200 m 2 The carbon black of the sealing composition of the present invention may have a specific surface area of ​​less than 200 m / g and a volatile content of greater than 4.5%. 2 The carbon black of the sealing composition of the present invention may have a specific surface area of ​​less than 190 m / g and a volatile content of greater than 5%. 2 / g or less than 180m 2 / g or less than 170m 2 The seal composition of the present invention may have a specific surface area of ​​less than 100 nm / g and a volatile content of greater than 5%, or greater than 7%, or greater than 8%, or greater than 9%, or greater than 10%, or greater than 12%. The carbon black of the product is 30 to 195 mm 2 / g, or 40-195m 2 / g, or 50-195m 2 / g, or 60-195m 2 / g, or 30-190m 2 / g, or 40-190m 2 / g, or 50-190m 2 / g, or 60-190m 2 / g, or 30-180m 2 / g, or 40-180m 2 / g, or 50-180m 2 / g, or 60-180m 2 / g, or 100-195m 2 / g, or 100-190m 2 / g, or 150-195m 2The carbon black may have a specific surface area of ​​1000 nm / g, or 5.1-25%, or 5.1-20%, or 5.1-15%, or 7-25%, or 7-10%, or 7-15%, or 10-25%, or 10-20%, or 10-15% volatile content. Specific surface area is a physical property that is conventionally reported by carbon black manufacturers. Specific surface area is measured using a nitrogen adsorption method according to ASTM D6556. Specific surface area represents the surface area of ​​the carbon black particles per unit of weight (per gram). The volatile content of carbon black is a property that is typically reported by carbon black manufacturers. The volatile content corresponds to the content of the product in species containing oxygen-containing species, such as carbonyls, carboxylic acids, pyrones, phenols, quinones, lactols, ethers, lactones, etc. These species are bound to the surface of the carbon black particles and typically cannot be removed by common extraction techniques. These species are formed by certain conditions during the formation of the carbon black material or by oxidative post-treatment, such as ozone treatment. The volatile content of carbon black is measured as the weight percent of material removed from the product after heating at 950° C. A paper entitled "Testing of Carbon Black; Determination of the Amount of Components Volatilized on Heating" is available at: The method for "Deposition of Carbon Black that are Volatile on Heating" is DIN535 52. The volatile content does not include moisture or solvent content that may be present in the particles.

[0117] In general, the sealing layer of an electrophoretic display plays an important role in the display performance. Poor barrier properties of the sealing layer result in the outflow of non-polar fluid of the electrophoretic medium from the electro-optical material layer over time, thereby resulting in serious degradation of the electro-optical performance of the display. It has been observed that increasing the content of poly(vinyl alcohol) homopolymer or poly(vinyl alcohol-co-ethylene) copolymer in the sealing layer improves its barrier properties. However, a sealing layer having a high content of poly(vinyl alcohol) homopolymer or poly(vinyl alcohol-co-ethylene) copolymer increases the moisture absorption of the layer, which is also undesirable. The interfacial tension between the poly(vinyl alcohol) polymer or poly(vinyl alcohol-co-ethylene) copolymer and polyurethane can be less than 2 mN / m.

[0118] These and other aspects of the present invention will be further understood in light of the following examples, which are intended to illustrate certain embodiments of the invention but are not intended to limit its scope, as defined by the claims. EXAMPLES

[0119] Sealing layer evaluation method

[0120] A. Example of preparation of water-based polymer composition forming a sealing layer.

[0121] A1. Example of Preparation of Carbon Black Dispersion. Carbon black powder is mixed with 1.6 liters of an aqueous solution of poly(vinyl alcohol) homopolymer or poly(vinyl alcohol-co-ethylene) copolymer. In one example, 162 g of carbon black and 105.6 g of polymer were used. The dispersion was mixed in an overhead mixer (Hei-Torque Value 200) at 300 rpm for 30 minutes. The dispersion was then mixed in a Gen The dispersion was recirculated through a 1 Q1375 Flocell sonicator and the sonicator jacket was cooled with cold water at 10° C. for 3 hours and 23 minutes at 100% amplitude. The dispersion was stirred continuously until it was used to prepare the aqueous polymer composition.

[0122] A2. Example of Preparation of Waterborne Polymer Composition. In a vessel, an aqueous polyurethane dispersion was combined with a wetting agent and an aqueous solution of a poly(vinyl alcohol) homopolymer or poly(vinyl alcohol-co-ethylene) copolymer, containing approximately 20% by weight of the homopolymer or copolymer. In one example, 194 g of a 35% by weight aqueous polyurethane dispersion and 372 g of a 20% by weight poly(vinyl alcohol) homopolymer or poly(vinyl alcohol-co-ethylene) copolymer were used. The dispersion was mixed for 10 minutes at 90 rpm using a Hei-torque Value 200 overhead mixer. The appropriate amount of crosslinker was then added and the dispersion was mixed for an additional 60 minutes at 90 rpm. The appropriate amount of carbon black dispersion prepared in A1 was added (1.39 L in one example) and the mixture was mixed for 60 minutes at 500 rpm. The pH was then adjusted to 6.5-8.5 using ammonium hydroxide and the dispersion was mixed for an additional 30 minutes. The appropriate amount of rheology modifier was added dropwise to the dispersion and mixing was continued for an additional 60 minutes. The dispersion was then degassed under reduced pressure (25 mmHg) for 5 days. The resulting aqueous polymer composition was used for the preparation of the sealing layer of the corresponding device within 7 days after the aqueous polymer composition was prepared.

[0123] B. Example of preparation of sealing layer using drawdown method.

[0124] The water-based polymer composition prepared in A2 above was coated onto the indium tin oxide (ITO) side of the ITO-PET film using a Gradco drawdown coater. A square applicator with a 15 mil gap and 8 passes was used. The drawdown speed was set at 2 m / min to target a dry film thickness of 30 + / - 2 μm. The coating was dried in an oven at 100° C. for 15 minutes. The dried film was conditioned at 25° C. and 55% relative humidity for 24 hours.

[0125] C. Evaluation of the barrier properties of the sealing layer against non-polar fluids.

[0126] An aqueous dispersion was prepared by mixing 10 grams of poly(vinyl alcohol) homopolymer or 10 grams of poly(vinyl alcohol-co-ethylene) copolymer and 10 grams of polyurethane in 100 mL of water. The dispersion was used as the aqueous polymer composition to form the sealing layer of device 800 shown in FIG. 8A. The sealing layer was formed by the method described in B above. Device 800 included, in order, substrate 803, light-transmitting conductive layer 804, primer layer 805, microcell layer 806, and sealing layer 807. The microcell contained an electrophoretic medium comprising white, black, and red pigment particles in Isopar E. Device 800 was stored at 70° C. for at least 24 hours. After this period, the electro-optical device was inspected using an optical microscope for sagging of the sealing layer caused by loss of the non-polar fluid of the electrophoretic medium. If the distance between the bottom of the inspected microcavity and the lowest point of the bottom surface of the sealing layer is less than 85% of the distance between the bottom of the microcavity and the highest point of the bottom surface of the sealing layer in the same microcell, the sealing layer is classified as failing for its barrier properties. Otherwise, i.e., if the distance between the bottom of the inspected microcell and the lowest point of the sealing layer is 85% or greater than the distance between the bottom of the microcell and the highest point of the bottom surface of the sealing layer in the inspected microcell, the sealing layer is classified as passing for its barrier properties. For example, the sealing layer used to prepare the electro-optical device shown in FIG. 10C was classified as passing because the ratio of h2:h1 was 1 (no sagging), while the sealing layer used to prepare the electro-optical device shown in FIG. 10D was classified as failing because the ratio of h2:h1 was 35% (sagging level above 85%). Barrier The evaluation of the properties can also be performed qualitatively by observing the prepared electro-optical devices from the observation side of the device by optical microscopy. A device containing a severely sagging sealing layer has a significantly different appearance (uniform surface vs. non-uniform surface) than a device containing a sealing layer that has good barrier properties against non-polar fluids. For example, a microcell having a sealing layer of FIG. 10C (passing) appears uniform as shown in FIG. 10A in contrast to a microcell having a sealing layer of FIG. 10D (failed), which appears non-uniform as shown in FIG. 10B. The evaluation of various combinations of (1) poly(vinyl alcohol) homopolymer or poly(vinyl alcohol-co-ethylene) copolymer and (2) polyurethane is shown in Table 1. Polymer 1 is a poly(vinyl alcohol) homopolymer or poly(vinyl alcohol-co-ethylene) copolymer, and polymer 2 is a polyurethane. Details regarding the commercial materials of polymer 1 and polymer 2 can be found in Table 2.

[0127] D. Determination of the surface energy of the sealing layer using the contact angle method.

[0128] The surface energy of the prepared sealing layer (as described in B above) was measured using the Kruss The contact angles were measured using a drop shape analyzer supplied by Sigma-Aldrich GmbH. Using a syringe equipped with a needle, a drop of deionized water with a size of 2.6 μL was placed on the top surface of the sealing layer and the contact angle between the liquid (water) and the sealing layer was measured. The measurement was repeated by replacing the water drop with a diiodomethane drop. The surface energy of the film was calculated by performing contact measurements using these two liquids of known surface energy. The contact angle measurements were repeated three times for each liquid (water and diiodomethane). The contact angles between the liquid and the top surface of the sealing layer were measured using a high-resolution camera 5 seconds, 30 seconds, and 55 seconds after the drop was placed on the sample film. The total surface energy, as well as its polar and dispersive components, were then calculated for each data point using the method of Owens, Wendt, Rabel, and Kaelble (OWRK). The reported surface energy was the average of nine data points (three drops × three measurements).

[0129] E. Determination of surface energy of polyurethane films using contact angle method.

[0130] The surface energy of polyurethane was determined by first preparing a polymer film on a substrate. The polymer film was prepared by coating the aqueous polyurethane dispersion onto the substrate using a Gradco drawdown coating machine. A square applicator with a gap of 15 mils and 8 passes was used. The drawdown speed was set at 2 m / min to target a dry film thickness of 30 + / - 2 μm. The coating was dried in an oven at 100°C for 15 minutes. The dried film was conditioned at 25°C and 55% relative humidity for 24 hours. The contact angles of two different liquids (water and diiodomethane) were then determined using the method described in D above, and the total surface energy of the polymer film, as well as its polar and dispersive components, were calculated using the OWRK model.

[0131] F. Preparation of electro-optical devices.

[0132] An electro-optical device was prepared by filling a plurality of microcells with a mixture of electrically charged pigment particles (white, black, and red) in Isopar E, followed by coating with an aqueous polymer composition as described above in B. The device shown in FIG. 8B was constructed. The electro-optical device 850 included, in order, a protective film 851, an optically clear first adhesive layer 852, a substrate 853, an optically transparent conductive layer 854, a primer layer 855, a microcell layer 856, a sealing layer 857, a second adhesive layer 858, an ITO electrode layer 859, and a glass layer 860. A source of electric field 861 drives the optically transparent conductive layer 854. The first light transmitting layer 852 had a thickness of approximately 25 μm. The substrate 853 had a thickness of approximately 100 μm. The primer layer 855 was The second adhesive layer 857 had a thickness of approximately 10 μm and a thickness of approximately 6 μm. The microcell layer 856 included a plurality of microcells. Each microcell had a bottom thickness of approximately 0.4 μm and a height of approximately 14 μm. The sealing layer 857 had a thickness of approximately 10 μm and the second adhesive layer had a thickness of approximately 6 μm.

[0133] G. Red Ra * measurement.

[0134] The electro-optical performance of the sample device prepared in E above was evaluated by collecting color data. Color data was collected by applying two different waveforms, a short waveform PD and a long waveform PP, to drive the desired red color state at two different temperatures. Additionally, waveforms were applied to drive the white state at two different temperatures. The applied waveforms are shown in Figures 9A-9F. Figure 9A corresponds to a PD waveform driving the red state at 25°C. Figure 9B corresponds to a PD waveform driving the red state at 0°C. Figure 9C corresponds to a PP waveform driving the red state at 25°C. Figure 9D corresponds to a PP waveform driving the red state at 0°C. Figure 9E corresponds to a waveform driving the white state at 25°C. Figure 9F corresponds to a waveform driving the white state at 0°C. The waveforms were applied over a wide range of voltages to obtain the red a as a function of the applied waveform. * The spectrophotometer i1 supplied by X-Rite was used to measure the color state of the image induced on the device sample, red a * The color performance was reported as red a * Evaluate as a value. * A higher value means a better red color (a more saturated red).

[0135] H. Maximum a in red state * Determining the voltage required.

[0136] In addition to the color values ​​of each display, up to a * A series of experiments were carried out to determine the voltages required to generate a. Specifically, the applied voltage for each waveform was varied and the a for each voltage value was * The values ​​were determined using Method F above. * The voltage that produced the values ​​is reported for each waveform. Typically, higher applied voltages increase power consumption, so smaller voltages are desirable.

[0137] I. Determination of Interfacial Tension

[0138] For a particular combination of polymers, the interfacial tension between polymer 1 and polymer 2 was calculated from the surface energy values ​​(determined by the method described in D above). Calculation of the interfacial tension between two components was performed by using the surface energy values ​​of each component and the following geometric equation:

number

[0139] J. Evaluation method for carbon black dispersibility

[0140] Carbon black dispersions using various carbon black samples were prepared using the method described in A1 above. The polymer used in the dispersions was poly(vinyl alcohol-co-ethylene) copolymer (Exceval (trade name) supplied by Kuraray). The carbon black dispersion was prepared using a 100% cellulose acetate syrup (RS-1717). After preparation of the carbon black dispersion, a drop of the carbon black dispersion was placed between a microscope glass slide and a cover plate. The samples were examined under a light microscope at 20x magnification. Images corresponding to an area of ​​140 μm×140 μm were visually analyzed for the number of agglomerates having a diameter size of 7 μm and greater. If the sample showed 10 or more agglomerated particles having a diameter size of 7 μm and greater, the sample was classified as failing for dispersibility. Otherwise, it was classified as passing for dispersibility.

[0141] L. Method for evaluating the volume resistivity of the sealing layer.

[0142] The volume resistivity of the sealing layer prepared using the method described in B above was determined using a Model 8009 Resistivity Fixture and Model 6571 Electrometer supplied by Keithley. This device allows the user to determine the volume resistivity of the free-standing film by applying an AC voltage to the substrate and measuring the output current. From the voltage and current, the electrical resistance of the sample was calculated. The method involves cutting a 4" x 4" square section of the sealing layer and peeling the section from the ITO-PET substrate to obtain a free-standing sealing film. The thickness was measured using a thickness gauge and then the film was placed in an environmental chamber at 25°C and 55% relative humidity for 4 days to condition. The film was then placed in a resistivity fixture Model 8009 and tested at a setting of 15 volts for 15 seconds. The electrometer provides the volume resistivity value.

[0143] M. Methods for assessing display image resolution.

[0144] The resolution of electrophoretic displays prepared by the method described in E above was evaluated by measuring the thickness of actual lines of color on the display, which were the result of a pixel controller command to form (at 50° C.) a line having a width of one pixel. The measured thickness was then compared to the thickness of a standard one-pixel line without blooming. 100% resolution corresponds to the highest resolution with no blooming, and 0% resolution corresponds to an actual line that is twice as thick as a standard line.

[0145] K. Method for evaluating the viscosity profile of an aqueous polymer composition.

[0146] The viscosity profile of the aqueous polymer composition prepared as described in A2 above was performed with a rotational TA Instruments rheometer equipped with parallel plates having a diameter of 40 mm and a gap of 50 μm. A sample of the aqueous polymer composition was placed between the parallel plates and the viscosity was measured at 10 -3 1 / s~10 2 The viscosity profiles of examples of the aqueous polymer compositions of the present invention are shown in Figure 11. Figure 11 shows that the aqueous polymer compositions evaluated are shear thinning, exhibiting a reduction in viscosity at higher shear rates compared to the viscosity at lower shear rates. Specifically, Figure 11 shows that the aqueous polymer compositions evaluated at 10 -3 The viscosity of the aqueous polymer composition evaluated at a shear rate of 1 / sec was 10 2 More than 10 times greater than the viscosity at a shear rate of 1 / sec.

[0147] O. Methods for evaluating the total surface energy and dispersive components of the surface energy of conductive fillers.

[0148] A porous based glass tube was filled with powdered conductive filler. The glass tube was placed on top of a container containing hexane as the test liquid. The hexane was drawn into the glass tube by capillary action. The glass tube was attached to a force sensor that measured the mass change over time as the liquid traveled up the glass tube and wetted the filler surface. By taking the slope of this measurement and with the known properties of the hexane test liquid, the following equation was ultimately used to determine the mass of the filler: The contact angle of the conductive filler can be calculated.

number

[0149] Evaluation results

[0150] Unless otherwise stated, the amount of components in the disclosed compositions is based on dry matter (without solvent).To express the content of carrier, the term QS (quantity) is used in some compositions.This term means that the content of this component in the composition is the amount required to achieve and not exceed the total of 100% of the composition.

[0151] Several aqueous polymer compositions were prepared by the general method described in A1 and A2 above. The weight ratio of poly(vinyl alcohol) homopolymer or poly(vinyl alcohol-co-ethylene) copolymer to polyurethane was 2.3, and the amount of aqueous carrier in the aqueous polymer composition was 80-83 wt%. Based on the weight of the aqueous polymer composition excluding the solvent, the content of crosslinker was 0.90 wt%, while the content of wetting agent (Silwet L-7607) was 0.19 wt%. In addition, the aqueous polymer composition also contained 0.22 wt% of a rheology modifier (modified alkali swellable acrylic emulsion (Solthix A100 supplied by Lubrizol)) based on the weight of the aqueous polymer composition excluding the solvent. The content of carbon black in the aqueous polymer was 10. 8 ~10 10The amount of the aqueous polymer composition was adjusted to achieve a sealing layer having a volume resistivity in the range of ohm.cm, typically 3.6-6% by weight based on the weight of the aqueous polymer composition excluding the solvent.

[0152] The sealing layer compositions are summarized in Table 1. The sealing layers were prepared from these aqueous polymer compositions using the method described in B above. The sealing layers were then evaluated for total surface energy and dispersive component of surface energy by the method described in D above. Separately, the total surface energy and dispersive component of corresponding control films prepared from each polyurethane used in the aqueous polymer composition using the method described in E above. These polyurethane control films contain neither poly(vinyl alcohol) homopolymer nor poly(vinyl alcohol-co-ethylene) copolymer, nor carbon black. Finally, the total surface energy and dispersive component of surface energy of two of the carbon black grades were measured using the method described in O above.

[0153] Electrophoretic displays were constructed from various compositions using the method described in F above. The electrophoretic displays were driven to the red state at 0° C. using two different waveforms as described in G above. Finally, the maximum a of the red state for each waveform was calculated. * The voltages required to generate the values ​​were determined using the method described in H above.

[0154] [Table 1-1] [Table 1-2] [Table 1-3]

[0155] Information on materials in Table 1: [1] Poly(vinyl alcohol-co-ethylene) copolymer; Exceval® RS-1717 supplied by Kuraray; [2] Polyurethane aqueous dispersion; L3838 aqueous dispersion supplied by Hauthaway as a 35% dispersion in water; [3] Polyurethane aqueous dispersion; HD2125 aqueous dispersion supplied by Hauthaway as a 35% dispersion in water; [4] Polyurethane aqueous dispersion (polyester); Witcobond® 386-03 supplied by Chemtura Corp.; [5] Carbon black; Raven® 1060 UP supplied by Columbia; [6] Carbon black; Nerox® 3500 supplied by Orion Engineered Carbons; [7] Carbon black; Nerox® 2500 supplied by Orion Engineered Carbons; [8] Carbon black; Cabot TPK1227R, supplied by Corporation; [9] carbon black; Raven® 14, supplied by Columbia.

[0156] The evaluation results in Table 1 show that improved electro-optical performance was observed in Examples 1 to 5 of the present invention compared to Comparative Example 6. The low temperature (0° C.) red state of the electro-optical device formed by the examples of the composition of the present invention, when driven by a PP waveform, was measured spectrophotometrically as a * The same is true for the red state driven by the PD waveform, which shows better (more saturated) color than the comparative example, as can be seen by the higher value of the value. The colors of the display of the present invention are not only more saturated, but also have a maximum *This is achieved at a lower voltage, as can be seen from the lower value of the voltage at . This means that the display of the present invention consumes less power than the display using the comparative composition example. This is achieved because the total surface energy of the sealing layer of the example of the present invention is approximately 66 mN / m, which is higher than 55 mN / m, in contrast to the total surface energy of 53 mN / m of the sealing layer formed by the comparative example. Similarly, the improved performance of the display of the present invention is achieved because the high dispersion surface energy of the sealing layer is higher than 40 mN / m, in contrast to the 38 mN / m of the sealing layer of the display of the present invention. The total surface energy of the components of the composition has a positive effect on the surface energy of the sealing layer. In particular, polyurethanes that form films with a total surface energy higher than 50 mN / m (e.g., polyurethane dispersions L3838 and HD2125) perform better than polyurethanes that form films with a lower total surface energy (Witcobond® 386-03).

[0157] The effect of the surface energy of the conductive filler also plays a role in the improved performance. Carbon blacks with a total surface energy higher than 40 mN / m, such as carbon black Raven® 1060 UP, outperform carbon blacks with a total surface energy lower than 40 mN / m, such as carbon black Raven® 14. In addition, carbon blacks with a dispersive component of surface energy higher than 15 mN / m show good performance. Without being bound by theory, the improved electro-optical performance (especially at low temperatures) of the sealing layer with high surface energy may enable the sealing layer to transfer charge through the interlayer with lower interfacial resistance and capacitance. Lower resistance and capacitance at the sealing layer / electrophoretic medium interface results in significantly less electro-optical bias (kickback), especially at low temperatures. Higher surface energy of the sealing layer may also result in lower contact resistance and capacitance at the seal interface with an adhesive layer that may be adjacent to the sealing layer. High surface energy of the sealing layer may increase the work of adhesion between the sealing layer and the adhesive layer, reducing the contact resistance between the layers. Furthermore, lower contact resistance at the seal / adhesive interface results in lower voltage drop, lower power consumption, and improved electro-optical performance over a range of temperatures.The effect of the surface energy of the seal layer on the electro-optical performance in electrophoretic displays has not been disclosed in the literature.

[0158] Table 2 provides surface energy data for various polymer 1 and polymer 2 species. Table 2 also includes the barrier properties of the various layers and the calculated interfacial evaluation of the various polymer combinations. The methods for preparing the corresponding polymer layers used to evaluate the barrier properties are described in C above. The surface energy determination (following the method described in D above) was performed by first preparing and conditioning the sealing layer from the corresponding aqueous polymer composition containing only one of the polymers. The interfacial tension for each polymer combination was calculated from the surface energy data and the calculation method described in I above.

[0159] [Table 2-1] [Table 2-2] [Table 2-3]

[0160] [Table 3-1] [Table 3-2]

[0161] The data in Table 2 show that a sealing layer formed using an aqueous polymer composition containing a combination of Polymer 1 and Polymer 2 having low interfacial tension exhibits good barrier properties against non-polar fluids. The sealing layer includes (a) a poly(vinyl alcohol) polymer or poly(vinyl alcohol-co-ethylene) copolymer having a degree of hydrolysis of 90-99.5% and an ethylene content of less than 10%, and (b) a polyurethane.

[0162] The data in Table 2 also show that sealing layers comprising (a) poly(vinyl alcohol) polymers or poly(vinyl alcohol-co-ethylene) copolymers having a degree of hydrolysis of 90-99.5% and an ethylene content of less than 10%, and (b) polyurethanes, exhibit good barrier properties against non-polar fluids, with the polyurethanes having a polar component of surface energy between 10-20 mN / m.

[0163] Microscopic evaluation of the polymer films prepared by the four aqueous polymer compositions prepared by the method described in B above showed a correlation between the uniformity of the film and the interfacial tension between the two polymers. The weight ratio of polymer 1:polymer 2 in the prepared films was 1:1. Table 4 and the microscopic images in FIG. 12 show that lower interfacial tension provides a more uniform polymer film. The improved compatibility achieved by the combination of polymers having lower interfacial tension may explain the improved barrier properties of the corresponding layers.

[0164] [Table 4-1] [Table 4-2]

[0165] Further sealing layers were prepared from aqueous polymer compositions containing various contents of combinations of polymer 1 and polymer 2. These aqueous polymer compositions contained, in addition to the polymer combinations, carbon black filler, crosslinker, wetting agent, rheology modifier, and aqueous carrier. The aqueous polymer compositions showing the aqueous carrier content are provided in Table 5. Table 6 corresponds to the same compositions as Table 5, but the compositions in Table 6 have been adjusted to show the weight percent of each component relative to the weight of the aqueous polymer composition excluding the solvent. The aqueous polymer compositions were prepared using the methods described in A1 and A2 above. The corresponding sealing layers were prepared using the method described in B above.

[0166] [Table 5-1] [Table 5-2]

[0167] [Table 6-1] [Table 6-2]

[0168] Ingredient information for Tables 5 and 6: [1] Exceval® RS-1717 supplied by Kuraray; [2] Dispercoll® U XP2815 supplied by Covestro; 35% dispersion in water; [3] Hauthane HD-2125 supplied by Hauthaway; 35% dispersion in water; [4] Hauthane L3838 supplied by Hauthaway; 35% dispersion in water; [5] CARBODILITE® supplied by Nisshimbo Chemical. V-02-L2; 40% solution in water, [6] Picassian® XL-701 supplied by Stahl, [7] Silwet® L-7607 copolymer supplied by Momentive, [8] Solthix™ A-100 supplied by Lubrizol.

[0169] A series of carbon black products were evaluated for their dispersibility in polymer compositions. Carbon blacks that exhibit good dispersibility allow for aqueous polymer compositions with good dispersion quality. The dispersion quality of the aqueous polymer composition is an important parameter that affects the properties of the resulting sealing layer. Poor dispersion quality of the aqueous polymer composition results in a sealing layer with very low volume conductivity, thereby reducing the electro-optical performance and electrical efficiency of the device. Table 7 provides the results of the study. The dispersion quality of the carbon black dispersions was determined by the method described in H above.

[0170] [Table 7]

[0171] The results of the evaluation of the dispersibility of carbon black in Table 7 are shown in Table 7. 2Carbon black grades with a specific surface area of ​​less than 85 to 200 m / g show good dispersibility in aqueous polymer dispersions. 2 Carbon blacks having a specific surface area between 200 m / g and a volatile matter content of more than 5% also have good dispersibility in aqueous polymer dispersions. Carbon blacks having a specific surface area higher than 85 and a volatile matter content of less than 5% do not have good dispersibility in aqueous polymer dispersions. Finally, 2 Carbon black with a specific surface area higher than 1 / g is preferred for its good incorporation into aqueous polymer dispersions. It does not indicate dispersibility. The volatile content of carbon black is measured as the weight percent of material removed from the product after heating at 950°C. The method entitled "Test for Carbon Black; Determination of the Amount of Components of Carbon Black Volatilized on Heating" is described in DIN 53552. The volatile content does not include any moisture or solvent content that may be present in the particles.

[0172] A series of carbon black products, whose average particle size was reported by the supplier using transmission electron microscopy (TEM), were also evaluated for their dispersibility in the polymer compositions. Table 8 provides the results of the investigation. The dispersion quality of the carbon black dispersions was determined by the method described in H above.

[0173] [Table 8-1] [Table 8-2]

[0174] The results of the carbon black dispersibility evaluation in Table 8 show that carbon black products having an average particle size greater than 20 nm have good dispersibility in aqueous polymer dispersions. Carbon black supplier Orion Engineered Carbon determined the average particle size of the products using ASTM D3849 (Standard Method for Carbon Black--Morphological Characterization of Carbon Black Using Electron Microscopy).

[0175] A series of sealing layers formed with aqueous polymer compositions containing various commercially available carbon black products were evaluated for volume resistivity of the sealing layer using the method previously described ( I. Method for Evaluating Volume Resistivity of Sealing Layer). Electro-optic displays were prepared using the methods described above (E. Preparation of Electro-optic Devices). The prepared electro-optic displays were evaluated for resolution by the methods described above (J. Method for Evaluating Resolution of Display Images). Tables 9 and 10 provide the aqueous polymer compositions prepared for this study. The aqueous polymer compositions showing the content of all components of the aqueous polymer composition, including the content of the aqueous carrier content, are provided in Table 9. Table 10 provides the sealing layer compositions (excluding potential water content), which were prepared by the aqueous polymer compositions of Table 9. The compositions of Table 9 provide the weight percent of each component by weight of the aqueous polymer composition including water. Various aqueous polymer compositions were prepared by the methods described in A1 and A2 above. The corresponding sealing layers were prepared by the methods described in B above.

[0176] [Table 9-1] [Table 9-2]

[0177] [Table 10-1] [Table 10-2]

[0178] The data in Table 10 show that optimal volume resistivity of the sealing layer and device resolution was achieved with carbon black having an oil absorption value of less than 100 mL / 100 g.

[0179] During further investigation, it was observed that aqueous polymer compositions containing more than 70% by weight of poly(vinyl alcohol) homopolymer or poly(vinyl alcohol-co-ethylene) copolymer, based on the weight of the aqueous polymer composition excluding the solvent, formed sealing layers that absorbed significant amounts of moisture from the environment, with this high moisture absorption negatively impacting the electro-optical performance of the display. For example, the present invention provides the following: (Item 1) (i) a water-soluble poly(vinyl alcohol) homopolymer or poly(vinyl alcohol-co-ethylene) copolymer, 30-70% by weight based on the weight of the sealing layer excluding solvent, said poly(vinyl alcohol) having a degree of hydrolysis of 90-99.9%, said poly(vinyl alcohol-co-ethylene) copolymer having a degree of hydrolysis of 90-99.9% and an ethylene content of less than 10%; (ii) 7 to 29% by weight of polyurethane, based on the weight of the sealing layer excluding the solvent; (iii) A conductive filler, 1 to 45 wt. % based on the weight of the sealing layer excluding the solvent, the conductive filler being selected from the group consisting of carbon black, graphene, graphite, and carbon nanotubes, the conductive filler having a total surface energy greater than 40 mN / m, the total surface energy of the conductive filler being determined by the Washburn method using hexane as a test liquid. A sealing layer comprising: 1. A sealing layer having a total surface energy, the total surface energy of the sealing layer being greater than 55 mN / m, the total surface energy of the sealing layer being determined using a contact angle method by: (a) forming the sealing layer by coating an aqueous polymer composition onto a substrate at a dry thickness of 30 mm, heating at 100° C. for 15 minutes, and conditioning the sealing layer at 25° C. and 55% relative humidity for 24 hours; (b) measuring the contact angles of a water droplet and a diiodomethane droplet on the formed sealing layer; and (c) calculating the total surface energy using an OWRK model. (Item 2) Item 2. The sealing layer according to item 1, wherein the sealing layer has a dispersive component of surface energy, the dispersive component of the surface energy being greater than 40 mN / m, and the dispersive component of the surface energy of the sealing layer is determined using a contact angle method. (Item 3) Item 2. The sealing layer of item 1, wherein the conductive filler has a dispersive component of surface energy, and the dispersive component of the surface energy of the conductive filler is greater than 15 mN / m as determined by the Washburn method using hexane as the test liquid. (Item 4) 2. The sealing layer according to item 1, wherein the polyurethane is crosslinked by a crosslinking agent, the crosslinking agent being a polyisocyanate, a multifunctional polycarbodiimide, a multifunctional aziridine, a silane coupling agent, a boron / titanium / zirconium based crosslinking agent, or a melamine formaldehyde. (Item 5) 2. The sealing layer of claim 1, further comprising a wetting agent, said wetting agent being an organosilicone surface tension reducing agent. (Item 6) 2. The sealing layer according to item 1, wherein the conductive filler is carbon black. (Item 7) 7. The sealing layer according to item 6, wherein the carbon black has an oil absorption of less than 100 mL per 100 mg of carbon black as measured by the oil absorption method according to ASTM 2414. (Item 8) 7. The sealing layer according to item 6, wherein the carbon black has an average particle size of more than 20 nm as measured by electron microscopy according to ASTM D3849. (Item 9) The carbon black has a viscosity of 90 mm as measured by nitrogen adsorption according to ASTM D6556. 2 7. The sealing layer according to item 6, having a specific surface area of ​​less than 1 / g. (Item 10) The carbon black has a viscosity of 200 mm as measured by nitrogen adsorption according to ASTM D6556. 2 / g and a volatile matter content, measured by the method according to DIN 53552, higher than 5%. (Item 11) 2. The sealing layer according to item 1, wherein the polyurethane has a number average molecular weight of 1,000 to 2,000,000 Daltons. (Item 12) Item 2. The sealing layer according to item 1, wherein the polyurethane has a polar component of surface energy, the polar component of the surface energy of the polyurethane being between 10 mN / m and 20 mN / m, and the polar component of the surface energy of the polyurethane being determined using a contact angle method. (Item 13) 2. The sealing layer according to item 1, wherein the poly(vinyl alcohol) homopolymer or poly(vinyl alcohol-co-ethylene) copolymer has a number average molecular weight of 1,000 to 1,000,000 Daltons. (Item 14) 2. The sealing layer according to item 1, wherein the poly(vinyl alcohol) homopolymer or poly(vinyl alcohol-co-ethylene) copolymer has a degree of hydrolysis of 92% to 99%. (Item 15) 2. The sealing layer of claim 1, wherein the poly(vinyl alcohol-co-ethylene) copolymer has an ethylene content of less than 9%. (Item 16) (i) a water-soluble poly(vinyl alcohol) homopolymer or poly(vinyl alcohol-co-ethylene) copolymer, 30-70% by weight based on the weight of the sealing layer excluding solvent, said poly(vinyl alcohol) having a degree of hydrolysis of 90-99.9%, said poly(vinyl alcohol-co-ethylene) copolymer having a degree of hydrolysis of 90-99.9% and an ethylene content of less than 10%; (ii) a polyurethane of 7-29 wt. % based on the weight of the sealing layer excluding solvent, the polyurethane having a total surface energy greater than 50 mN / m, the total surface energy of the polyurethane being determined using a contact angle method by: (a) coating an aqueous polyurethane composition onto a substrate at a dry thickness of 30 mm, heating at 100° C. for 15 minutes, and conditioning the polyurethane film at 25° C. and 55% relative humidity for 24 hours to form a polyurethane film; (b) measuring the contact angles of a water droplet and a diiodomethane droplet on the formed polyurethane film; and (c) calculating the total surface energy using the OWRK model. (iii) A conductive filler, 1 to 45 wt. % based on the weight of the sealing layer excluding the solvent, the conductive filler being selected from the group consisting of carbon black, graphene, graphite, and carbon nanotubes, the conductive filler having a total surface energy, the total surface energy of the conductive filler being greater than 40 mN / m, the total surface energy being determined by the Washburn method using hexane as a test liquid. A sealing layer comprising: A sealing layer, the sealing layer having a total surface energy, the total surface energy of the sealing layer being greater than 55 mN / m, the total surface energy of the sealing layer being determined using a contact angle method. (Item 17) Item 17. The sealing layer according to item 16, wherein the sealing layer has a dispersive component of surface energy, the dispersive component of the surface energy being higher than 40 mN / m, and the dispersive component of the surface energy of the sealing layer is determined using a contact angle method. (Item 18) Item 17. The sealing layer according to item 16, wherein the polyurethane has a dispersive component of surface energy, the dispersive component of the surface energy of the polyurethane being greater than 40 mN / m, and the dispersive component of the surface energy of the polyurethane being determined using a contact angle method. (Item 19) a first light transmissive electrode layer; 2. An electro-optic material layer including a sealing layer according to item 1 and a plurality of microcells, each of the plurality of microcells including a bottom, a wall and an opening, containing an electrophoretic medium, the electrophoretic medium including at least one type of charged pigment particles dispersed in a non-polar fluid, the sealing layer spanning the openings of the plurality of microcells. Second electrode layer 1. An electrophoretic display comprising: An electrophoretic display, wherein the electro-optic material layer is disposed between the first light-transmissive electrode layer and the second electrode layer. (Item 20) 20. The electrophoretic display of item 19, wherein the electrophoretic medium comprises four types of charged pigment particles, the colors of the four or more pigment particles being selected from the group consisting of white, magenta, yellow, cyan, blue, red, green, and black.

Claims

[Claim 1] The invention described in the specification.

Citation Information

Patent Citations

  • Long-wearing nail polish with specific surface properties

    JP2002513735A

  • Manufacturing method of display element

    JP2004138959A

  • Adhesive layer and sealing layer for electrophoretic displays

    JP2006517038A

  • liquid containing film structure

    JP2009544060A

  • Electrophoretic display device and electronic apparatus

    JP2017049552A