Polylactic acid film and laminate film

By stretching polylactic acid films multiple times at high temperatures, the elastic modulus and heat resistance are improved, addressing dimensional and appearance issues, making the film suitable for industrial use with biodegradability.

JP2024149821APending Publication Date: 2024-10-18TOYOBO CO LTD

Patent Information

Application Number
JP2024137777
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-07
Filing Date
2024-08-19
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Polylactic acid films exhibit low elastic modulus and heat resistance, leading to issues like dimensional changes and appearance defects during industrial processing, despite improvements in heat resistance methods.

Method used

The polylactic acid film is stretched multiple times at high temperatures near its melting point to suppress internal molecular chains, achieving a total stretching ratio that enhances elastic modulus and heat resistance, with specific tensile modulus, crystallinity, and heat shrinkage rates within defined ranges.

Benefits of technology

The resulting film demonstrates excellent elastic modulus and heat resistance, ensuring good dimensional stability during high-temperature processing, suitable for industrial applications such as release films and optical applications, while being biodegradable.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024149821000001
    Figure 2024149821000001
  • Figure 2024149821000002
    Figure 2024149821000002
Patent Text Reader

Abstract

To provide a polylactic acid film having excellent elasticity modulus and heat resistance regarding polylactic acid which is derived from a biomass material and has biodegradability.SOLUTION: A polylactic acid film is made of a resin composition containing polylactic acid. In the polylactic acid film, a tensile modulus of elasticity Ea in a longer direction and a tensile modulus of elasticity Eb in a width direction satisfy a formula of Ea+Eb>8.0 GPa, the degree of crystallinity is 40% or more and 90% or less, and thermal shrinkage in the longer direction and thermal shrinkage in the width direction are 10.0% or less respectively when the film is heated at 150°C for 30 minutes. In the polylactic acid film, it is preferable that the weight ratio of L-lactic acid / D-lactic acid be 100 / 0 to 85 / 15.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polylactic acid film made of a resin composition containing polylactic acid, and a laminate film containing the same. [Background technology]

[0002] Films made of polylactic acid (hereinafter sometimes referred to as "PLA") resin are derived from biomass raw materials and are biodegradable, so they are being developed as an alternative to conventional fossil raw materials. However, compared to polyethylene terephthalate, nylon, polyolefin, and other materials commonly used in industry, polylactic acid films made of polylactic acid resin have a low elastic modulus and low heat resistance. Therefore, when used for industrial purposes, PLA films have problems such as dimensional changes and wrinkles during processing.

[0003] In order to solve such problems, methods have been proposed that improve the film-forming conditions of the PLA film. For example, Patent Document 1 discloses a method of improving heat resistance without impairing moldability by performing longitudinal stretching in two or more separate steps, followed by transverse stretching, and performing the second longitudinal stretching at a temperature lower than the first stretching. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2004-359948 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, although the polylactic acid film produced by the method of Patent Document 1 has improved heat resistance, the second longitudinal stretching temperature is low, so the subsequent widthwise stretching ratio cannot be set high, resulting in a problem of low elastic modulus.

[0006] The above-mentioned conventional techniques have been unable to improve the tensile modulus in the longitudinal and transverse directions and at the same time obtain good heat resistance. An object of the present invention is to provide a polylactic acid film having excellent elastic modulus and heat resistance, which is produced by using polylactic acid derived from a biomass raw material and has biodegradability, and a laminate film containing the same. [Means for solving the problem]

[0007] As a result of extensive research by the present inventors on polylactic acid films, the present inventors have found that by stretching the polylactic acid film multiple times in multiple stages at a high temperature near the melting point of polylactic acid, it is possible to suppress the stretching stress of the internal molecular chains and improve the total stretching ratio, thereby achieving a crystallinity within a predetermined range and successfully improving the elastic modulus and heat resistance of the polylactic acid film of the present invention. That is, in order to solve the above problems, the present invention has the following configuration.

[0008] 1. A polylactic acid film made of a resin composition containing polylactic acid, A polylactic acid film having a longitudinal tensile modulus Ea and a transverse tensile modulus Eb that satisfy the formula Ea+Eb>8.0 GPa, a crystallinity of 40% or more and 90% or less, and a longitudinal heat shrinkage rate and a transverse heat shrinkage rate each of which is 10.0% or less when heated at 150°C for 30 minutes. 2. The polylactic acid film according to 1 above, which has a thermal shrinkage rate of 3.0% or less in both the longitudinal direction and the transverse direction when heated at 120° C. for 30 minutes. 3. The polylactic acid film according to 1 or 2 above, wherein the weight ratio of L-lactic acid / D-lactic acid is 100 / 0 to 85 / 15. 4. The polylactic acid film according to any one of 1. to 3. above, which has a total light transmittance of 75% or more and a haze of 3% or less. 5. A laminated film having a base layer and a release layer, the base layer comprising the polylactic acid film according to any one of 1. to 4. above. 6. The laminated film according to 5 above, which is a release film for use in producing a ceramic green sheet, and the release layer is made of a composition containing a silicone release component. 7. A laminate film according to 5. or 6. above, wherein the maximum protrusion height (P) of the surface of the release layer is 200 nm or less, and the arithmetic mean roughness (Sa) of the surface of the release layer is 10 nm or less. Effect of the Invention

[0009] The polylactic acid film of the present invention has excellent elastic modulus and heat resistance. Therefore, it has good dimensional stability during processing at high temperatures and high rigidity, making it suitable for industrial applications such as release film applications and optical applications. Furthermore, since it is made from biomass-derived raw materials and is biodegradable, it is possible to provide an excellent polylactic acid film and a laminated film containing the same that take into consideration the recent SDGs. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The polylactic acid film of the present invention is a polylactic acid film made of a resin composition containing polylactic acid. In this polylactic acid film, the tensile modulus Ea in the longitudinal direction and the tensile modulus Eb in the transverse direction satisfy the formula "Ea + Eb > 8.0 GPa", the crystallinity is 40% or more and 90% or less, and when heated at 150 ° C. for 30 minutes, the thermal shrinkage rate in the longitudinal direction and the thermal shrinkage rate in the transverse direction are each 10.0% or less. In addition, the laminated film of the present invention is a laminated film containing this polylactic acid film, and is preferably a laminated film containing the polylactic acid film in the base layer and further having a release layer on one or both sides of the base layer.

[0011] (Polylactic acid) The polylactic acid preferably used in the present invention is obtained by ring-opening polymerization of lactide using a compound having a hydroxyl group as an initiator in the presence of a specific catalyst. The specific catalyst is, for example, tin, aluminum, etc. The polylactic acid can contain an L-lactic acid component and a D-lactic acid component as a copolymer component or a blend component. In the polylactic acid film and resin composition, the weight ratio of L-lactic acid (hereinafter L-form) / D-lactic acid (hereinafter D-form) is preferably 100 / 0 to 85 / 15, more preferably 100 / 0 to 90 / 10, further preferably 100 / 0 to 90 / 10, and particularly preferably 100 / 0 to 95 / 5. When the ratio of L-lactic acid (hereinafter L-form) / D-lactic acid (hereinafter D-form) is 100 / 0 to 85 / 15, high crystallinity is obtained, which is preferable. In the present invention, the preferred glass transition point is 40 to 70°C, the preferred melting point is 150 to 180°C, and it is also preferable that oriented crystallization is possible. The glass transition point and melting point can be obtained by a differential scanning calorimeter (DSC), etc. The presence or absence of crystallinity can be confirmed by the presence or absence of a crystallization peak during the heating process or the cooling process after melting in DSC.

[0012] The reduced viscosity (ηsp / c) of the resin composition used in the present invention is preferably in the range of 1.0 dl / g or more and 3.0 dl / g or less. When the reduced viscosity is 1.0 dl / g or more, the polylactic acid film can be prevented from tearing. When the reduced viscosity is 3.0 dl / g or less, the increase in filtration pressure is small, making it easy to perform high-precision filtration.

[0013] The reduced viscosity (ηsp / c) of the polylactic acid film of the present invention is preferably in the range of 1.0 dl / g to 2.5 dl / g. When the reduced viscosity is 1.0 dl / g or more, breakage does not occur frequently during the stretching process, which is preferable. When the reduced viscosity is 2.5 dl / g or less, cuttability is good when cutting to a predetermined product width, and dimensional defects do not occur, which is preferable.

[0014] The resin composition used in the present invention may contain one or more additives such as inactive particles such as inorganic particles, heat-resistant polymer particles, crosslinked polymer particles, fluorescent whitening agents, ultraviolet inhibitors, infrared absorbing dyes, heat stabilizers, surfactants, and antioxidants, depending on the purpose of use. As the antioxidant, an aromatic amine-based or phenol-based antioxidant may be used. As the stabilizer, a phosphorus-based stabilizer such as phosphoric acid or a phosphoric acid ester-based stabilizer, a sulfur-based stabilizer, or an amine-based stabilizer may be used.

[0015] (Production method of polylactic acid film) The polylactic acid film of the present invention is preferably an oriented film, more preferably a biaxially oriented film, from the standpoints of mechanical strength, chemical resistance, heat resistance, and the like.

[0016] The resin composition of the present invention can be processed into an unstretched sheet by various methods, and then biaxially stretched to obtain a polylactic acid film. As a method for producing the unstretched sheet, a melt extrusion method can be used in addition to a solution casting method. The melt extrusion method is preferred in the present invention.

[0017] The melting temperature of the resin composition is preferably in the range of 150 to 250° C., more preferably 180 to 240° C. A temperature of 150° C. or higher is preferable because it provides an appropriate melt viscosity and increases productivity, and a temperature of 250° C. or lower is preferable because it suppresses thermal degradation of the polylactic acid resin.

[0018] The die temperature during melt extrusion is the same as described above, but is preferably 150 to 300° C., more preferably 170 to 290° C., and even more preferably 180 to 240° C. When the die temperature during melt extrusion is 150° C. or higher, the melt viscosity falls within a suitable range, allowing stable extrusion. When the temperature is 300° C. or lower, thermal decomposition of the resin can be suppressed.

[0019] The polylactic acid film of the present invention can be produced according to a general polyester film production method. For example, a method can be mentioned in which a polyester resin is melted, and the non-oriented polyester extruded into a sheet is stretched in the longitudinal direction at a temperature equal to or higher than the glass transition temperature by utilizing the speed difference between rolls, and then stretched in the transverse direction by a tenter and heat-treated. Specifically, for example, in the longitudinal stretching step in the longitudinal direction, the film is heated and stretched 1.1 to 6 times between two or many rolls having different peripheral speeds. The heating means at this time may be a method using a heating roll or a method using a non-contact heating medium, or these may be used in combination. At this time, it is preferable that the temperature of the film is in the range of (Tg-10°C) to (Tg+50°C). Next, it is preferable that the uniaxially stretched film is introduced into a tenter and stretched 1.1 to 10 times in the width direction at a temperature of (Tg-10°C) to Tm or lower.

[0020] Furthermore, after the stretching is completed, in order to reduce the thermal shrinkage rate of the film, it is preferable to carry out a heat setting treatment within 30 seconds, preferably within 10 seconds, in the heat setting step, and to carry out a longitudinal relaxation treatment, a transverse relaxation treatment, etc. of 0.5 to 10%.

[0021] The heat setting temperature is preferably in the range of 90 to 180° C. When the heat setting temperature is 90° C. or higher, sufficient dimensional stability due to heat of the film can be obtained, which is preferable, and when the heat setting temperature is 180° C. or lower, the phenomenon of the film being punctured due to heat can be suppressed, which is preferable.

[0022] (Physical properties of polylactic acid film) The thickness of the polylactic acid film of the present invention is preferably 2 μm or more and 500 μm or less, more preferably 15 μm or more and 400 μm or less, and even more preferably 20 μm or more and 250 μm or less. When the thickness of the polylactic acid film is 2 μm or more, the polylactic acid film has a minimum rigidity and is easy to handle. When the thickness of the polylactic acid film is 500 μm or less, the transportability of the film when transporting the film with multiple rolls and the handleability of the produced film are improved, making it easy to handle.

[0023] The sum of the tensile modulus Ea in the MD direction and the tensile modulus Eb in the TD direction of the polylactic acid film is preferably 8.0 GPa or more. The preferred lower limit of the sum of the tensile modulus is 8.2 GPa, more preferably 8.4 GPa, even more preferably 8.6 GPa, even more preferably 8.8 GPa, even more preferably 9.0 GPa, particularly preferably 9.5 GPa, and most preferably 10.0 GPa or more. When the sum of the tensile modulus is 8.0 GPa or more, the rigidity of the film is sufficient, and the occurrence of wrinkles and warping of the film can be suppressed, which is preferable. Considering the manufacturing point of view, the upper limit of the sum of the tensile modulus is considered to be 15.0 GPa.

[0024] The breaking strength of the polylactic acid film is preferably 75 MPa or more in both the MD and TD directions. The lower limit of the breaking strength is preferably 100 MPa, more preferably 150 MPa, even more preferably 200 MPa, and even more preferably 220 MPa. A breaking strength of 75 MPa or more is preferable because the mechanical strength of the film is sufficient and the occurrence of problems such as elongation and displacement during the film processing step can be suppressed. Considering the manufacturing point of view, the upper limit of the breaking strength is considered to be 1000 MPa.

[0025] The breaking elongation of the polylactic acid film is preferably 5% or more in both the MD and TD directions. A breaking elongation of 5% or more is preferable because the mechanical elongation of the film is sufficient, and the occurrence of defects such as cracking and tearing during the film processing step can be suppressed. Considering the manufacturing point of view, the upper limit of the breaking elongation is considered to be 300%. The upper limit of the breaking elongation is more preferably 150%, even more preferably 100%, and even more preferably 80%.

[0026] In the polylactic acid film, when heated at 150°C for 30 minutes, the heat shrinkage in the MD direction and the heat shrinkage in the TD direction are each preferably 10.0% or less. When heated at 150°C for 30 minutes, the upper limit of each of the heat shrinkage in the MD direction and the heat shrinkage in the TD direction is more preferably 8.0% or less, even more preferably 6.0% or less, even more preferably 4.0% or less, particularly preferably 3.0% or less, and most preferably 2.0% or less. If the heat shrinkage is small, processing such as coating can be easily performed, and poor appearance due to deformation of the film under high heat can be suppressed. Although it is preferable that the heat shrinkage is low, the lower limit is considered to be 0.01% from the viewpoint of production.

[0027] In the polylactic acid film, when heated at 120°C for 30 minutes, the heat shrinkage in the MD direction and the heat shrinkage in the TD direction are each preferably 3.0% or less. When heated at 120°C for 30 minutes, the upper limit of each of the heat shrinkage in the MD direction and the heat shrinkage in the TD direction is more preferably 2.0% or less, even more preferably 1.6% or less, even more preferably 1.4% or less, particularly preferably 1.2% or less, and most preferably 1.0% or less. If the heat shrinkage is small, processing such as coating can be easily performed, and poor appearance due to deformation of the film under high heat can be suppressed. Although it is preferable that the heat shrinkage is low, the lower limit is considered to be 0.01% from the viewpoint of production.

[0028] The total light transmittance of the polylactic acid film is preferably 75% or more. In order to improve the accuracy of detection of internal foreign bodies that are defects of the film, it is preferable that the transparency is high. Therefore, the total light transmittance of the film of the present invention is preferably 75% or more, more preferably 80% or more, even more preferably 85% or more, even more preferably 88% or more, particularly preferably 91% or more, and most preferably 93% or more. In order to improve the accuracy of detection of internal foreign bodies that are defects of the film, the higher the total light transmittance, the better, but it is technically difficult to achieve a total light transmittance of 100%. From the viewpoint of production, the total light transmittance is preferably less than 100%.

[0029] The surface of the polylactic acid film of the present invention is preferably smooth, and when used as a release film for producing ceramic green sheets, it is preferable that the haze is small. The haze is preferably 3% or less, more preferably 2% or less, and most preferably 1% or less. The lower limit of the haze is the lower the better, but it may be 0.1% or more, or 0.3% or more. In order to reduce the haze, it is better that the film surface does not have too much unevenness, but in order to provide a certain degree of slipperiness from the viewpoint of handling properties against a rotating roll, it is preferable to form a certain amount of unevenness on at least one surface.

[0030] The crystallinity of the polylactic acid film is preferably 40% to 90%, more preferably 50% to 85%, and even more preferably 55% to 80%. A crystallinity in the range of 40% to 90% is preferable because it improves strength and provides a high elastic modulus.

[0031] In addition, when a smooth release layer or the like is formed on the surface of the polylactic acid film, it is preferable that at least one surface of the polylactic acid film is also smooth. The smooth surface of the polylactic acid film is preferably one having an arithmetic mean roughness (Sa) of 10 nm or less and a maximum projection height (P) of 200 nm or less. More preferably, the arithmetic mean roughness of the surface is 10 nm or less and a maximum projection height of 150 nm or less, more preferably, the arithmetic mean roughness of the surface is 10 nm or less and a maximum projection height of 120 nm or less, and even more preferably, the arithmetic mean roughness of the surface is 8 nm or less and a maximum projection height of 120 nm or less. If the arithmetic mean roughness of the surface is 10 nm or less and the maximum projection height is 200 nm or less, the surface of the release layer or the like formed on the surface can be smoothed to the same degree. The arithmetic mean roughness (Sa) of the surface of the polylactic acid film may be 0.1 nm or more, or may be 0.3 nm or more. The maximum projection height (P) of the surface may be 1 nm or more, or may be 3 nm or more.

[0032] (Laminated film) The laminated film of the present invention is a laminated film having a base layer and a release layer, and the base layer contains the polylactic acid film as described above. The release layer can be provided on one or both sides of the base layer, and is preferably provided on the outermost surface. The substrate layer may be made of a polylactic acid film, but may further include other layers such as other polyester layers, an easy-adhesion layer, an antistatic layer, and an easy-slip layer. The laminated film of the present invention can be used as a release film for the production or transfer of ceramic green sheets, various resin sheets, and optical films, as pressure sensitive adhesive sheets, and adhesive sheets. (Release layer) The resin constituting the release layer is not particularly limited, and may be a silicone resin, a fluororesin, an alkyd resin, various waxes, an aliphatic olefin, etc., and each resin may be used alone or in combination of two or more kinds. The release layer preferably contains a silicone release component such as a silicone resin or a silicone oil.

[0033] For example, a silicone resin is a resin having a silicone structure in the molecule, and examples thereof include cured silicone, silicone graft resin, and modified silicone resin such as alkyl modification. From the viewpoint of migration, it is preferable to use a reactive cured silicone resin. Examples of reactive cured silicone resins include those of addition reaction system, condensation reaction system, and ultraviolet or electron beam curing system. More preferably, low-temperature curing addition reaction system and ultraviolet or electron beam curing system that can be processed at low temperature are preferable. By using these silicone resins, the polyester film can be processed at low temperature during coating processing. Therefore, the polyester film is less thermally damaged during processing, and a polyester film with high flatness can be obtained, and defects such as pinholes can be reduced even when manufacturing thin sheets such as ceramic green sheets.

[0034] An example of an addition reaction silicone resin is one in which polydimethylsiloxane with vinyl groups introduced at the end or side chain is reacted with hydrogen siloxane using a platinum catalyst to harden it. In this case, it is more preferable to use a resin that can be hardened within 30 seconds at 120°C, as this allows processing at low temperatures. Examples include low-temperature addition cure types (LTC1006L, LTC1056L, LTC300B, LTC303E, LTC310, LTC314, LTC350G, LTC450A, LTC371G, LTC750A, LTC755, LTC760A, etc.) and thermal UV cure types (LTC851, BY24-510, BY24-561, BY24-562, etc.) manufactured by Dow-Toray, and solvent addition + UV cure types (X62-5040, X62-5065, X62-5072T, KS5508, etc.) and dual cure types (X62-2835, X62-2834, X62-1980, etc.) manufactured by Shin-Etsu Chemical.

[0035] An example of a condensation reaction silicone resin is one in which a polydimethylsiloxane having an OH group at its terminal and a polydimethylsiloxane having an H group at its terminal are subjected to a condensation reaction using an organotin catalyst to create a three-dimensional crosslinked structure.

[0036] Examples of UV-curable silicone resins include, as the most basic type, those that utilize the same radical reaction as normal silicone rubber crosslinking, those that introduce unsaturated groups to cause photocuring, those that use UV to decompose onium salts to generate strong acids that cleave epoxy groups to cause crosslinking, and those that crosslink by addition reaction of thiols to vinyl siloxanes. Electron beams can also be used instead of the UV rays. Electron beams have stronger energy than UV rays, and it is possible to carry out a radical crosslinking reaction without using an initiator as in the case of UV curing. Examples of resins that can be used include UV-curable silicones manufactured by Shin-Etsu Chemical Co., Ltd. (X62-7028A / B, X62-7052, X62-7205, X62-7622, ​​X62-7629, X62-7660, etc.), UV-curable silicones manufactured by Momentive Performance Materials, Inc. (TPR6502, TPR6501, TPR6500, UV9300, UV9315, XS56-A2982, UV9430, etc.), and UV-curable silicones manufactured by Arakawa Chemical Co., Ltd. (Silicolise UV POLY200, POLY215, POLY201, KF-UV265AM, etc.).

[0037] The above-mentioned UV-curable silicone resin may be an acrylate-modified or glycidoxy-modified polydimethylsiloxane, etc. Good release performance can also be achieved by mixing such modified polydimethylsiloxane with a multifunctional acrylate resin or epoxy resin, etc., and using the mixture in the presence of an initiator.

[0038] Other examples of resins that can be used include alkyd resins and acrylic resins having long-chain alkyl groups, such as stearyl-modified and lauryl-modified resins, and alkyd-based resins, acrylic-based resins, and olefin-based resins obtained by reactions such as methylated melamine. When forming sheets for use in electronic parts, etc., release agents that do not contain silicone are also preferred.

[0039] Examples of the amino alkyd resins and amino acrylic resins obtained by the reaction of methylated melamine include the Tesfine series manufactured by Showa Denko Materials Co., Ltd.

[0040] When the above resin is used in the release layer of the present invention, one type may be used, or two or more types may be mixed. When two or more types are mixed, two or more types of silicone-based resins may be used, and it is also preferable to mix a plurality of different resin types, such as a binder resin and a silicone-based resin.

[0041] In particular, when forming a thin film sheet such as a ceramic green sheet, it is preferable that the release layer does not deform when peeled off, so it is preferable that the release layer is crosslinked and cured. Therefore, it is also preferable that the release layer contains a binder component, a crosslinking agent, etc. in addition to the silicone-based release agent.

[0042] The binder component contained in the release layer of the present invention is preferably, for example, a component capable of crosslinking in order to increase the crosslinking density of the release layer and improve the durability and solvent resistance of the release layer. Therefore, the binder component is preferably formed by reacting a resin having a reactive functional group with a crosslinking agent. It is also preferable that either the reactive functional group or the crosslinking agent is self-crosslinked alone. However, in the present invention, the binder component does not exclude an embodiment in which only the resin having a reactive functional group or the crosslinking agent is used as the binder component.

[0043] Suitable examples of resins having reactive functional groups include polyester resins, polyacrylic resins, polyurethane resins, polyolefin resins, etc. These resins preferably have at least one reactive functional group selected from the group consisting of carboxyl groups, hydroxyl groups, epoxy groups, amino groups, etc.

[0044] It is also preferable that the release layer of the present invention contains a crosslinking agent. Examples of crosslinking agents are melamine-based, isocyanate-based, carbodiimide-based, oxazoline-based, and epoxy-based. The crosslinking agent may be used alone or in combination of two or more. Particularly preferable is a crosslinking agent that reacts with the reactive functional group introduced into the binder component.

[0045] The release layer of the present invention may contain particles having a particle size of 1 μm or less, but from the viewpoint of preventing the occurrence of pinholes, it is preferable that the layer does not substantially contain any particles that form protrusions.

[0046] In order to adjust the release force, the release layer of the present invention may contain additives such as a light release additive or a heavy release additive, or additives such as an adhesion improver and an antistatic agent. In order to improve the adhesion to the base layer, it is also preferable to perform a pretreatment such as an anchor coat, a corona treatment, a plasma treatment, or an atmospheric pressure plasma treatment on the surface of the polylactic acid film before providing the release coating layer.

[0047] In the present invention, the thickness of the release layer may be set according to the purpose of use, and is not particularly limited, but is preferably in the range of 0.005 to 2.0 μm after curing. When the thickness of the release layer is 0.005 μm or more, the peeling performance is maintained, which is preferable. In addition, when the thickness of the release layer is 2.0 μm or less, the curing time is not too long, and there is no risk of uneven thickness of the sheet due to a decrease in the flatness of the release film, which is preferable. In addition, since the curing time is not too long, there is no risk of the resin constituting the release layer agglomerating, and there is no risk of forming protrusions, which is preferable, and pinhole defects of the sheet are unlikely to occur.

[0048] The outer surface of the film on which the release layer is formed (i.e., the outer surface of the release layer) is preferably flat so as not to cause defects in the sheet to be coated and molded on the outer surface of the film. The arithmetic mean roughness (Sa) of the release layer surface is preferably 10 nm or less and the maximum protrusion height (P) is preferably 200 nm or less. Furthermore, the arithmetic mean roughness of the release layer surface is more preferably 10 nm or less and the maximum protrusion height is 100 nm or less, and the arithmetic mean roughness of the release layer surface is even more preferably 10 nm or less and the maximum protrusion height is 30 nm or less. If the arithmetic mean roughness of the release layer surface is 10 nm or less and the maximum protrusion height is 200 nm or less, defects such as pinholes do not occur during sheet formation, and the yield is good, which is preferable. It can be said that the smaller the arithmetic mean roughness (Sa) of the release layer surface, the more preferable it is, but it may be 0.1 nm or more, or it may be 0.3 nm or more. It can be said that the smaller the maximum protrusion height (P) is, the more preferable it is, but it may be 1 nm or more, or it may be 3 nm or more.

[0049] The lower limit of the surface free energy of the release layer provided in the release film of the present invention is 8 mJ / m 2 More preferably, it is 10 mJ / m or more. 2 More than 12 mJ / m 2 More preferably, 8 mJ / m 2 If the thickness is more than this, then repelling or the like is unlikely to occur when the sheet dissolving solution is applied, which is preferable.

[0050] The upper limit of the surface free energy of the release layer provided on the release film of the present invention is 45 mJ / m 2 It is preferably less than 40 mJ / m 2 Less than or equal to 35 mJ / m 2 More preferably, it is 45 mJ / m 2 It is preferable that the thickness is not more than this because the molded sheet has good releasability.

[0051] In the present invention, the method of forming the release layer is not particularly limited, and a method is used in which a coating liquid in which a release resin is dissolved or dispersed is spread on one side of the base layer by coating or the like, and the solvent is removed by drying, and then the coating is dried by heating, heat curing, or ultraviolet curing. At this time, the drying temperature during solvent drying and heat curing is preferably 180°C or less, more preferably 150°C or less, and most preferably 120°C or less. The heating time is preferably 30 seconds or less, more preferably 20 seconds or less. When the temperature is 180°C or less, the flatness of the film is maintained and there is little risk of causing unevenness in the thickness of the sheet, which is preferable. When the temperature is 120°C or less, the film can be processed without impairing the flatness, and there is a further reduced risk of causing unevenness in the thickness of the sheet, which is particularly preferable.

[0052] In the present invention, the surface tension of the coating liquid when applying the release layer is not particularly limited, but is preferably 30 mN / m or less. By setting the surface tension as described above, the wettability after application can be improved and the unevenness of the coating film surface after drying can be reduced.

[0053] In the present invention, the coating liquid used for coating the release layer is not particularly limited, but it is preferable to add a solvent having a boiling point of 90° C. or higher. By adding a solvent having a boiling point of 90° C. or higher, bumping during drying can be prevented, the coating film can be leveled, and the smoothness of the coating film surface after drying can be improved. The amount of the solvent added is preferably about 10 to 80% by mass based on the entire coating liquid.

[0054] Examples of the method for applying the coating liquid include roll coating methods such as gravure coating and reverse coating, bar coating using a wire bar, die coating, spray coating, and air knife coating.

[0055] (Ceramic green sheets and ceramic capacitors) Generally, a multilayer ceramic capacitor has a rectangular parallelepiped ceramic body. Inside the ceramic body, first internal electrodes and second internal electrodes are alternately provided along the thickness direction. The first internal electrodes are exposed on a first end face of the ceramic body. A first external electrode is provided on the first end face. The first internal electrode is electrically connected to the first external electrode at the first end face. The second internal electrode is exposed on a second end face of the ceramic body. A second external electrode is provided on the second end face. The second internal electrode is electrically connected to the second external electrode at the second end face.

[0056] The release film for producing ceramic green sheets of the present invention is used to produce such a multilayer ceramic capacitor. For example, it is produced as follows. First, the release film of the present invention is used as a carrier film, and a ceramic slurry for forming a ceramic body is applied and dried. A conductive layer for forming a first or second internal electrode is printed on the applied and dried ceramic green sheet. A mother laminate is obtained by appropriately stacking and pressing a ceramic green sheet, a ceramic green sheet on which a conductive layer for forming a first internal electrode is printed, and a ceramic green sheet on which a conductive layer for forming a second internal electrode is printed. The mother laminate is divided into a plurality of pieces to produce a raw ceramic body. The raw ceramic body is fired to obtain a ceramic body. Then, a first and second external electrodes are formed to complete a multilayer ceramic capacitor. EXAMPLES

[0057] Next, the effects of the present invention will be described using examples and comparative examples. First, the evaluation methods of the characteristic values ​​used in the present invention will be described below.

[0058] [Evaluation method]

[0059] (1) Thickness The thickness of the polylactic acid film was measured using a TH-104 made by Tester Sangyo Co., Ltd.

[0060] (2) Crystallinity Measurement was performed using a differential scanning calorimeter (DSC214Polyma) manufactured by Netsch Japan Co., Ltd. Using 10 mg of sample, measurements were performed in the range of 25°C to 250°C at a heating rate of 10°C / min, and the endothermic heat of the melting peak observed during heating was divided by the theoretical heat of fusion of perfect crystals of polylactic acid (93.6 J / g) to determine the crystallinity (%) of the polylactic acid film.

[0061] (3) Tensile modulus The tensile modulus of the polylactic acid film was measured in accordance with JIS K 7127. A sample was cut into a strip of 200 mm in length and 15 mm in width in the MD and TD directions of the film using a single-edged razor, and two parallel marks were made at a distance of 50 mm in the center of the test piece. Next, the strip-shaped sample was clamped with a chuck distance of 100 mm using an autograph AGS-X manufactured by Shimadzu Corporation, and pulled at a speed of 0.5 mm / min, and the tensile modulus (GPa) in each direction was obtained from the obtained load-strain curve of 0.1 to 0.3%. The value of strain was measured using the distance between the marks.

[0062] (4) Breaking strength and elongation The breaking strength and breaking elongation of the polylactic acid film were measured in accordance with JIS C 2318. A sample was cut into a strip of 120 mm in length and 10 mm in width in the MD and TD directions of the film using a single-edged razor. The strip-shaped sample was then clamped with a chuck distance of 100 mm using an Autograph AG-IS manufactured by Shimadzu Corporation and pulled at a speed of 100 mm / min. The breaking strength (MPa) and breaking elongation (%) in each direction were calculated from the obtained load-strain curve.

[0063] (5) Heat shrinkage rate The heat shrinkage of the polylactic acid film was measured in accordance with JIS C 2318. The laminated film was cut to a width of 10 mm and a length of 190 mm in the direction to be measured, and marks were made at 150 mm intervals, and the intervals between the marks (A) were measured. Next, the film was placed in an oven in an atmosphere of 150°C, and heat-treated at 150±3°C for 30 minutes under no load, and the intervals between the marks (B) were measured. The heat shrinkage at 150°C was then calculated using the following formula. In addition, the film cut out in the same manner as above was placed in an oven in an atmosphere of 120°C, and heat-treated at 120±3°C for 30 minutes under no load, and the intervals between the marks (C) were measured, and the heat shrinkage at 120°C was calculated using the following formula. 150℃ heat shrinkage rate (%) = (AB) / A×100 120℃ heat shrinkage rate (%) = (AC) / A x 100

[0064] (6) Hayes The haze (%) of the polylactic acid film was measured using a haze meter NDH-7000 II type manufactured by Nippon Denshoku Industries Co., Ltd. in accordance with JIS K 7136.

[0065] (7) Total light transmittance The total light transmittance (%) of the polylactic acid film was measured using a haze meter NDH-7000 II type manufactured by Nippon Denshoku Industries Co., Ltd. in accordance with JIS K 7136.

[0066] (8) Reduced viscosity (ηsp / c) 0.1 g of polylactic acid was dissolved in 15 mL of a mixed solvent of phenol / 1,1,2,2-tetrachloroethane (75 / 25 (weight ratio)), and the viscosity was measured using an Ostwald viscometer at 30° C. The unit is dl / g.

[0067] (9) Surface roughness Using a non-contact surface shape measurement system (VertScan R550H-M100), the arithmetic mean roughness (Sa) and maximum protrusion height (P) were measured as the average roughness of the area surface under the following conditions. The arithmetic mean roughness (Sa) was calculated by averaging five measurements, and the maximum protrusion height (P) was calculated by measuring seven times and using the maximum of the five measurements excluding the maximum and minimum values. (Measurement conditions) Measurement mode: WAVE mode Objective lens: 10x 0.5×Tube lens ·Measurement area 936μm x 702μm (Analysis conditions) Surface correction: 4th order correction -Interpolation process: Fully interpolated

[0068] Example 1 (1) Preparation of polylactic acid resin As the polylactic acid-based resin, poly-L-lactic acid PLA L175 (weight ratio of L-lactic acid / D-lactic acid is 99 / 1) manufactured by Total Corbion was used.

[0069] (2) Manufacturing of polylactic acid films Poly-L-lactic acid (L175) was dried under reduced pressure (1 Torr) at 120°C for 6 hours, and then fed to an extruder. It was melted at 220°C and extruded from a die into a sheet. A gear pump was used to control the thickness to 400 μm. In addition, a filter medium (initial filtration efficiency: 95%) made of sintered stainless steel with a filtration particle size of 10 μm was used for the filter.

[0070] The extruded resin was cast onto a cooling drum with a surface temperature of 50° C., and adhered to the surface of the cooling drum using an electrostatic application method, followed by cooling and solidification to produce an unstretched film with a thickness of 400 μm.

[0071] The obtained unstretched sheet was heated to a film temperature of 75° C. with a group of heated rolls, and then stretched 3.0 times in the longitudinal direction with a group of rolls having different peripheral speeds.

[0072] The uniaxially stretched film was then held with clips and stretched transversely at a temperature of 75° C. and a transverse stretch ratio of 4.96. Next, a heat treatment was carried out at 150° C. for 15 seconds.

[0073] The biaxially stretched film stretched in the TD direction was again held by clips and stretched transversely. The transverse stretching temperature was 170°C, and the transverse stretching ratio was 1.01 times. Next, heat treatment was performed at 160°C for 15 seconds to obtain a polylactic acid film with a thickness of 40 μm. The physical properties of the obtained film of Example 1 are shown in Table 2. The sum of the crystallinity and tensile modulus of elasticity of the obtained polylactic acid film was high, and the thermal shrinkage rate was low, so that it was shown that a film excellent in modulus of elasticity and heat resistance was obtained in Example 1.

[0074] (Examples 2 and 3) In Examples 2 and 3, polylactic acid films were obtained in the same manner as in Example 1, except that the conditions were changed as shown in Table 1. The physical properties of the obtained films of Examples 2 and 3 are shown in Table 2. In Example 2, a higher elastic modulus was obtained by increasing the second stretching ratio in the TD direction. In Example 3, a relaxation treatment (160°C, relaxation rate 5%) was performed after TD stretching, thereby suppressing heat shrinkage in the TD direction and maintaining a high elastic modulus. The films of Examples 2 and 3 had a high sum of the crystallinity and the tensile elastic modulus, and a low thermal shrinkage rate, and therefore, it was shown that films excellent in elastic modulus and heat resistance were obtained in Examples 2 and 3.

[0075] Example 4 (1) Preparation of polylactic acid resin As the polylactic acid-based resin, poly-L-lactic acid PLA LX175 (weight ratio of L-lactic acid / D-lactic acid: 96 / 4) manufactured by Total Corbion was used.

[0076] (2) Manufacturing of polylactic acid films Poly-L-lactic acid (LX175) was dried under reduced pressure (1 Torr) at 120°C for 6 hours, and then fed to an extruder. It was melted at 220°C and extruded from a die into a sheet. A gear pump was used to control the thickness to 400 μm. In addition, a filter medium made of sintered stainless steel with a filtration particle size of 10 μm (initial filtration efficiency: 95%) was used for the filter.

[0077] The extruded resin was cast onto a cooling drum with a surface temperature of 50° C., and adhered to the surface of the cooling drum using an electrostatic application method, followed by cooling and solidification to produce an unstretched film with a thickness of 400 μm.

[0078] The obtained unstretched sheet was heated to a film temperature of 70° C. with a group of heated rolls, and then stretched 3.0 times in the longitudinal direction with a group of rolls having different peripheral speeds.

[0079] The uniaxially stretched film was then held with clips and stretched transversely at a temperature of 75° C. and a transverse stretch ratio of 4.96. Next, a heat treatment was carried out at 150° C. for 15 seconds.

[0080] The biaxially stretched film stretched in the TD direction was again held by clips and stretched transversely. The transverse stretching temperature was 150°C, and the transverse stretching ratio was 1.01 times. Next, a relaxation treatment was performed at 140°C for 15 seconds (relaxation rate 3%) to obtain a polylactic acid film with a thickness of 40 μm. The physical properties of the obtained film of Example 4 are shown in Table 2. The sum of the crystallinity and tensile elastic modulus of the obtained polylactic acid film was high, and the thermal shrinkage rate was low, so that in Example 4, a film excellent in elastic modulus and heat resistance was obtained.

[0081] Example 5 In Example 5, a polylactic acid film was obtained in the same manner as in Example 3, except that an unstretched sheet was introduced into a simultaneous biaxial stretching machine, and while the ends of the film were held with clips, the sheet was stretched 3.0 times in the longitudinal direction and 5.0 times in the width direction in a hot air zone at a temperature of 75°C, and then the sheet was held again with clips and stretched laterally. The physical properties of the film obtained in Example 5 are shown in Table 2. The polylactic acid film obtained had a high sum of the crystallinity and the tensile modulus and a low thermal shrinkage rate, indicating that a film excellent in modulus and heat resistance was obtained in Example 5.

[0082] From the above, the films obtained in Examples 1 to 5 are excellent in elastic modulus and heat resistance, have good dimensional stability during processing at high temperatures, and can obtain high rigidity. Furthermore, the films obtained in Examples 1 to 5 have a maximum projection height (P) of 200 nm or less and an arithmetic mean roughness (Sa) of 10 nm or less, so that when a release layer is formed on the surface of the film, it is possible to make the maximum projection height (P) of the surface 200 nm or less and the arithmetic mean roughness (Sa) of 10 nm or less.

[0083] (Comparative Examples 1 and 2) In Comparative Examples 1 and 2, polylactic acid films were obtained in the same manner as in Examples 1 and 5, except that the conditions were changed as shown in Table 1. The physical properties of the obtained films in Comparative Examples 1 and 2 are shown in Table 2. Comparative Examples 1 and 2 are outside the scope of the present invention because they have a low tensile modulus and a high thermal shrinkage. Comparative Examples 1 and 2 were stretched using the commonly used sequential biaxial stretching or simultaneous biaxial stretching method, and because the stretching ratio was low, the modulus and heat resistance were poor.

[0084] Comparative Example 3 In Comparative Example 3, a biaxially stretched film was obtained in the same manner as in Comparative Example 1, except that the conditions were changed to those shown in Table 1. In Comparative Example 3, the stretch ratio in the TD direction was set high in the commonly used sequential biaxial stretching, but stretching breakage occurred, and a polylactic acid film could not be obtained.

[0085] [Table 1]

[0086] [Table 2] [Industrial Applicability]

[0087] The polylactic acid film and laminate film of the present invention are suitably used, for example, as a release film for producing ceramic green sheets.

Claims

1. A polylactic acid film made of a resin composition containing polylactic acid, A polylactic acid film having a longitudinal tensile modulus Ea and a transverse tensile modulus Eb that satisfy the formula Ea + Eb > 8.0 GPa, a crystallinity of 40% or more and 90% or less, and a longitudinal heat shrinkage rate and a transverse heat shrinkage rate each of which are 10.0% or less when heated at 150°C for 30 minutes.

2. 2. The polylactic acid film according to claim 1, which has a thermal shrinkage rate of 3.0% or less in both the longitudinal direction and the transverse direction when heated at 120° C. for 30 minutes.

3. 2. The polylactic acid film according to claim 1, wherein the weight ratio of L-lactic acid / D-lactic acid is 100 / 0 to 85 / 15.

4. 2. The polylactic acid film according to claim 1, which has a total light transmittance of 75% or more and a haze of 3% or less.

5. A laminated film having a base layer and a release layer, the base layer comprising the polylactic acid film according to any one of claims 1 to 4.

6. 6. The laminated film according to claim 5, which is a release film for use in producing a ceramic green sheet, and the release layer is made of a composition containing a silicone release component.

7. 6. The laminated film according to claim 5, wherein the surface of the release layer has a maximum protrusion height (P) of 200 nm or less and an arithmetic mean roughness (Sa) of the surface of the release layer of 10 nm or less.

Citation Information

Patent Citations

  • Biaxially oriented polylactic acid film for forming and container

    JP2004359948A

Cited By

  • Layered polylactic acid film

    WO2026053853A1

  • Polylactic acid-based film and production method therefor

    WO2026197585A1