Cleaning composition, cleaning sheet and method for producing cleaning sheet

A cleaning composition and sheet with glycol ether, abrasive, and polyhydric alcohol efficiently remove water repellents and oil films from glass and mirrors, ensuring effective cleaning and abrasive retention.

JP2024150101APending Publication Date: 2024-10-23CAR MATE MFG
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
JP2023063350
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-10
Publication Date
2024-10-23

AI Technical Summary

Technical Problem

Existing cleaning methods, such as those described in Patent Documents 1 and 2, are ineffective in removing water repellents and oil films from surfaces like automobile glass and mirrors.

Method used

A cleaning composition and sheet containing glycol ether, an abrasive, and a polyhydric alcohol, preferably with alumina or cerium oxide, are used in a dry state, with the sheet being impregnated and dried to enhance cleaning efficacy.

Benefits of technology

The composition and sheet effectively remove oil films and other stains from glass and mirror surfaces, maintaining abrasive integrity and providing convenient, effective cleaning.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024150101000001
    Figure 2024150101000001
  • Figure 2024150101000002
    Figure 2024150101000002
  • Figure 2024150101000003
    Figure 2024150101000003
Patent Text Reader

Abstract

To provide a cleaning composition and a cleaning sheet that enable the removal of oil films and other stains from the glass surfaces of vehicles and automobiles contaminated with the dirt.SOLUTION: A cleaning composition at least contains glycol ether and / or glycol, an abrasive, and a polyhydric alcohol. The cleaning composition may be a dried cleaning liquid. A cleaning sheet comprises a cleaning composition that at least contains glycol ether and / or glycol, an abrasive, and a polyhydric alcohol, the cleaning composition incorporated within the sheet. The cleaning sheet may be in dry conditions.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cleaning composition, a cleaning sheet, and a method for producing a cleaning sheet, and in particular to a cleaning composition, a cleaning sheet, and a method for producing a cleaning sheet for cleaning the surfaces of glass and the like of automobiles, railway cars, and the like, and mirrors and the like of motorcycles, automobiles, and the like. [Background technology]

[0002] The window glass of automobiles and railroad cars, and the mirrors of automobiles and motorcycles, etc., are prone to adhesion of dirt and often have an oil film attached thereto. In addition, water repellent agents and coating agents are sometimes applied to the window glass and mirrors of automobiles, etc., and in this case, old water repellent agents attached to the glass or mirrors, etc. must be removed before applying new water repellent agents. In addition, when applying a coating to glass, etc., a cleaning operation is indispensable for cleaning the surface of the glass or mirror, etc., in order to prepare the coating. However, for example, Patent Document 1 discloses a water stain cloth in which a cloth is impregnated with a liquid cleaning agent containing an alkaline component, an abrasive, a thickener, silicone oil and / or wax powder in order to remove stains such as water stains on automobiles, etc., but it is unable to remove stains such as water repellents, oil films, etc. Patent Document 2 discloses an abrasive cleaning cloth in which a cloth is impregnated with an abrasive particle dispersion containing abrasive particles, a surfactant, diorganopolysiloxane oil and a solvent and dried in order to remove stains from the painted surfaces of automobiles, motorcycles, etc., and hard surfaces such as glass and metal, but it is unable to remove stains such as water repellents, oil films, etc.

[0003] [Patent Document 1] JP 2005-87487 A [Patent Document 2] JP 2008-284102 A DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]

[0004] In view of the above problems, the present inventors have conducted extensive research and have completed the present invention. That is, the object of the present invention is to provide a cleaning composition and a cleaning sheet capable of removing dirt from the surfaces of objects, such as the mirror surfaces of automobiles and motorcycles, and the glass surfaces of automobiles, etc., to which dirt such as water repellents and oil films has adhered, and a method for producing the cleaning sheet. [Means for solving the problem]

[0005] The cleaning composition of the present invention is characterized by containing at least a glycol ether and / or glycol, an abrasive, and a polyhydric alcohol. In the present invention, the cleaning composition is preferably in a dried state. The cleaning sheet of the present invention is characterized by having a cleaning composition containing at least a glycol ether and / or glycol, an abrasive, and a polyhydric alcohol. In the present invention, the cleaning sheet is preferably in a dry state. In the present invention, the polyhydric alcohol constituting the cleaning composition is preferably at least one selected from the group consisting of glycerin, 1,3-butanediol, ethylene glycol, propylene glycol, and diethylene glycol. The abrasive constituting the cleaning composition is preferably at least one selected from the group consisting of alumina, cerium oxide, and zirconium oxide. In the present invention, it is preferred that the glycol ether constituting the cleaning composition is a glycol ether, and the glycol is a glycol. The method for producing a cleaning sheet of the present invention is characterized by comprising a step of impregnating a sheet with a cleaning composition containing at least a glycol ether and / or glycol, an abrasive, and a polyhydric alcohol, and then a drying step of drying the sheet. Here, the drying step is preferably carried out at a temperature of 70 to 150° C. for a time period of 3 to 60 minutes. Effect of the Invention

[0006] According to the present invention, it is possible to provide a cleaning composition, a cleaning sheet, and the like that can clean glass surfaces, mirror surfaces, and the like having dirt such as an oil film attached thereto. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] The cleaning composition of the present invention contains at least a glycol ether and / or a glycol, an abrasive, and a polyhydric alcohol. Such a cleaning composition is in a liquid form, and may be referred to as a cleaning liquid in the present invention.

[0008] Examples of the abrasives used in the present invention include aluminum oxide (alumina), silica, kaolin, aluminum silicate, zeolite, bentonite, talc, montmorillonite, diatomaceous earth, cerium oxide, zirconium oxide, zirconium silicate, silicon carbide, titanium oxide, aluminum tripolyphosphate, aluminum hydroxide, barium sulfate, calcium silicate, and calcined products thereof. These abrasives may be used alone or in combination of two or more, and two or more abrasives with different particle sizes may be used.

[0009] The abrasive used in the present invention has an average particle size of 0.05 to 50 μm, preferably 0.1 to 20 μm, and more preferably 0.5 to 10 μm. When the average particle size of the abrasive is within the range of 0.05 to 50 μm, dirt can be efficiently scraped off, and the dirt scraped off in this manner can be adsorbed on the surface of the abrasive, thereby preventing the dirt from reattaching. In the present invention, it is preferable to use two or more types of abrasives having different average particle diameters. For example, it is preferable to select two or more types from abrasives having an average particle diameter of preferably 0.05 μm to 50 μm, and more preferably from abrasives having an average particle diameter of 0.5 μm to 10 μm.

[0010] The abrasive is preferably blended in the cleaning composition (cleaning liquid) at 10 to 60% by weight, more preferably 15 to 40% by weight, and particularly preferably 20 to 25% by weight. When the blending amount of the abrasive is within the range of 10 to 60% by weight, dirt can be efficiently rubbed off, and the dirt thus rubbed off can be adsorbed on the surface of the abrasive, thereby preventing the dirt from reattaching.

[0011] The cleaning composition (cleaning liquid) of the present invention contains a glycol ether and / or a glycol. Glycol ethers are compounds in which the OH groups at one or both ends of ethylene glycol or propylene glycol are substituted with alkyl or aryl groups. Examples of glycol ethers that can be used in the present invention include so-called glycol ethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, ethylene glycol monoethyl ether acetate, diethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether, diethylene glycol monobutyl ether, ethylene glycol monobutyl ether acetate, diethylene glycol monobutyl ether acetate, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, dipropylene glycol dimethyl ether, propylene glycol monomethyl ether propionate, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, ethylene glycol diethyl ether, diethylene glycol diethyl ether, diethylene glycol methyl ethyl ether, diethylene glycol dibutyl ether, diethylene glycol monohexyl ether, ethylene glycol isopropyl ether, ethylene glycol monohexyl ether, and ethylene glycol phenyl ether. In the present invention, diethylene glycol diethyl ether and the like are preferably used.

[0012] Glycol is a compound having a structure in which hydrogen atoms bonded to two or more carbon atoms of an aliphatic hydrocarbon having two or more carbon atoms or a cyclic aliphatic hydrocarbon are each replaced with a hydroxyl group, and representative examples include so-called glycols such as ethylene glycol, propylene glycol, and diethylene glycol. An example of the glycol preferably used in the present invention is propylene glycol.

[0013] In the present invention, the glycol ether and / or glycol is preferably blended in an amount of 1 to 40% by weight, more preferably 1 to 20% by weight, and particularly preferably 3 to 10% by weight, based on 100% by weight of the cleaning liquid.

[0014] The cleaning composition (cleaning liquid) in the present invention preferably contains a polyhydric alcohol, such as glycerin, propylene glycol, 1,3-butanediol, ethylene glycol, and diethylene glycol. In the present invention, it is preferable that glycerin, propylene glycol, 1,3-butanediol, and the like are blended as the polyhydric alcohol. Note that two or more kinds of polyhydric alcohols may be used in combination. In the present invention, the polyhydric alcohol functions as a binder and has the function of fixing the abrasive particles.

[0015] The cleaning composition (cleaning liquid) in the present invention may contain a solvent. Examples of the solvent include isopropyl alcohol, methanol, ethanol, butanol, etc. In the present invention, it is preferable to use isopropyl alcohol or the like as the solvent.

[0016] In the present invention, known binders, additives, etc. can be appropriately blended depending on the purpose and application.

[0017] The cleaning composition (cleaning liquid) of the present invention can be obtained by mixing at least glycol ether and / or glycol, an abrasive, and a polyhydric alcohol, optionally using a solvent or the like.

[0018] In the present invention, it is preferable to dry a cleaning composition (cleaning liquid) containing at least glycol ether and / or glycol, an abrasive, and a polyhydric alcohol. The cleaning composition dried in this way can exhibit a very excellent cleaning effect in removing dirt such as oil film attached to glass or mirror surfaces. In addition, since it is in a dry state, it is convenient to carry and can be used for cleaning work easily.

[0019] In the present invention, the cleaning composition (cleaning liquid) can be impregnated into a sheet to form a cleaning sheet. Here, the method of impregnating the sheet with the cleaning liquid may be to impregnate the sheet with the cleaning liquid, or to spray the cleaning liquid onto the sheet. Examples of the impregnation method include a dip method, a dip roll coater method, a gravure roll coater method, a spray coat method, a reverse roll coater method, a direct roll coater method, a kiss roll coater method, an inverse knife coater method, an air knife coater method, an opposite knife coater method, and a brush coating method.

[0020] The sheet may be a nonwoven fabric, etc. Examples of the material of the fiber of the nonwoven fabric etc. used in the present invention include cotton, rayon, nylon, polyester, polypropylene, polyethylene, acrylic, polylactic acid, etc. The sheet has a basis weight of 30g / m 2 More preferably, the content is 40 to 200 g / m 2 and particularly preferably 150 to 200 g / m 2 It is. The sheet used in the present invention preferably has a thickness of 0.1 to 5.0 mm, and more preferably 0.5 to 2.0 mm.

[0021] In the present invention, it is preferable to dry the cleaning sheet containing the cleaning liquid to obtain a dry cleaning sheet. The drying conditions are preferably such that the liquid of the cleaning composition (cleaning liquid) impregnated in the cleaning sheet is appropriately evaporated, and for example, the drying temperature is preferably 70 to 150° C., more preferably 100 to 120° C. The drying time is preferably 3 to 60 minutes, more preferably 10 to 20 minutes. Dry cleaning sheets have the advantage that they are easy to carry and store, and can be easily taken out and used immediately when it is desired to clean surfaces such as automobile windows and mirrors, etc. Moreover, dry cleaning sheets can provide an extremely excellent cleaning effect that has not existed in the past. The preferred method of using the dry cleaning sheet is to drip a small amount of water onto the surface of the object to be cleaned, such as glass or a mirror, and then bring the cleaning sheet into contact with the surface and rub to remove dirt such as oily film.

[0022] The cleaning composition of the present invention can be a dry cleaning composition. That is, the liquid cleaning composition (cleaning liquid) of the present invention can be dried to form a solid cleaning composition. As a method of using the liquid cleaning composition, for example, it can be impregnated into a sponge or the like, and the surface of glass or the like can be rubbed with the sponge to clean. In addition, the solid cleaning composition can be cleaned by dropping water on the surface of the object to be cleaned such as glass, placing the cleaning composition thereon, and rubbing the surface with a sponge or the like.

[0023] The cleaning composition of the present invention can be used to sufficiently remove oily stains and the like adhering to the glass of automobiles and railroad cars, and the mirror surfaces of automobiles, motorcycles, etc. Furthermore, the cleaning sheet of the present invention can be used to easily, conveniently, and sufficiently remove stains such as oily films adhering to the glass and mirrors of automobiles, etc., anytime, anywhere. EXAMPLES

[0024] The present invention will be specifically described below by showing examples, but the present invention is not limited to these examples.

[0025] (Preparation of cleaning composition) Preparation of cleaning solution 1: Two types of alumina were prepared, namely, alumina with an average particle size of 2 μm and alumina with an average particle size of 1 μm. Cleaning solution 1 was prepared by mixing 15 weight % of alumina with an average particle size of 2 μm, 10 weight % of alumina with an average particle size of 1 μm, 10 weight % of glycerin, 5 weight % of propylene glycol, and 60 weight % of isopropyl alcohol.

[0026] Preparation of cleaning solution 2: Cleaning liquid 2 was prepared by mixing 15 wt % alumina with an average particle size of 2 μm, 10 wt % alumina with an average particle size of 1 μm, 5 wt % propylene glycol, and 70 wt % isopropyl alcohol.

[0027] Preparation of cleaning solution 3: Cleaning solution 3 was prepared by mixing 15 wt % alumina with an average particle size of 2 μm, 10 wt % alumina with an average particle size of 1 μm, 10 wt % glycerin, 5 wt % diethylene glycol diethyl ether, and 60 wt % isopropyl alcohol.

[0028] Preparation of washing solution 4: Cleaning liquid 4 was prepared by mixing 15 wt % alumina with an average particle size of 2 μm, 10 wt % alumina with an average particle size of 1 μm, 5 wt % diethylene glycol diethyl ether, and 70 wt % isopropyl alcohol.

[0029] Preparation of washing solution 5: Cleaning liquid 5 was prepared by mixing 15 wt % alumina having an average particle size of 2 μm, 10 wt % alumina having an average particle size of 1 μm, 10 wt % glycerin, and 65 wt % isopropyl alcohol.

[0030] Preparation of cleaning solution 6: Cleaning liquid 6 was prepared by mixing 15 wt % alumina having an average particle size of 2 μm, 10 wt % alumina having an average particle size of 1 μm, and 75 wt % isopropyl alcohol.

[0031] Example 1 As a test material, the surface of a glass plate was polished, and then an oil film was formed on the glass surface by applying an oil film forming liquid (fluorine-based water repellent, product number C112 manufactured by Carmate Co., Ltd.) to the polished glass surface and curing the liquid to prepare a test glass plate. The contact angle of the test surface of the obtained glass plate was measured. The contact angle measurements in the examples were all performed by the method described below. 0.69 g of the obtained cleaning solution 1 was added to 0.33 g of a spunbond nonwoven fabric (ESE-545, manufactured by Mitsui Chemicals, Inc.: basis weight 140 g / m 2 , thickness 1.9mm, ventilation volume 155cc / cm 2 / sec) and then dried at 95°C for 15 minutes to prepare a dry cleaning sheet 1. The obtained cleaning sheet 1 was wrapped around a sponge (2 cm x 5 cm). After 0.5 g of water was dropped onto the surface of a glass plate to be tested, the cleaning sheet 1 wrapped around the sponge was placed in contact with the surface, and a load of 2 kg was applied from above the cleaning sheet 1 to rub the surface to be tested a predetermined number of times. When the number of rubbings reached 20, the contact angle of the test surface was measured. In the same manner, the contact angle was measured when the surface had been rubbed 40 times, and when the surface had been rubbed 60 times. The results are shown in Table 1.

[0032] Example 2 In Example 1, cleaning liquid 1 was changed to cleaning liquid 2, and 1.02 g of cleaning liquid 2 was impregnated into 0.33 g of spunbond nonwoven fabric (ESE-545), and then dried at 95°C for 15 minutes in the same manner as in Example 1 to prepare a dry cleaning sheet 2. In the same manner as in Example 1, a sponge was wrapped with cleaning sheet 2 to prepare a sponge. In the same manner as in Example 1, an oil film forming liquid (C112) was applied to a polished glass surface and cured to prepare a glass plate as a test subject, and the contact angle of the test subject surface of the glass plate was measured. The cleaning sheet 2 wrapped around the prepared sponge was placed on the surface of the glass plate to be tested after 0.5 g of water was dropped onto it, and a force of 2 kg was applied from above the cleaning sheet 2, and the test surface was rubbed a predetermined number of times in the same manner as in Example 1. That is, the contact angle was measured after 20 reciprocal rubs, after 40 reciprocal rubs, and after 60 reciprocal rubs. The results are shown in Table 1.

[0033] Example 3 In Example 1, cleaning liquid 1 was changed to cleaning liquid 3, and 0.67 g of cleaning liquid 3 was impregnated into 0.33 g of spunbond nonwoven fabric (ESE-545), and then dried at 95° C. for 15 minutes in the same manner as in Example 1 to produce a dry cleaning sheet 3. In the same manner as in Example 1, the obtained cleaning sheet 3 was wrapped around a sponge to produce a sponge. In the same manner as in Example 1, an oil film forming liquid (C112) was applied to a polished glass surface and cured to prepare a glass plate as a test subject, and the contact angle of the test subject surface of the glass plate was measured. After 0.5 g of water was dropped onto the surface of the glass plate to be tested, the cleaning sheet 3 wrapped around the sponge was placed in contact with the surface, and a force of 2 kg was applied from above the cleaning sheet 3 to rub the surface to be tested a predetermined number of times in the same manner as in Example 1. When the number of times of rubbing reached 20, the contact angle of the surface to be tested was measured. In the same manner, the contact angle was measured when the surface had been rubbed 40 times, and when the surface had been rubbed 60 times. The results are shown in Table 1.

[0034] Example 4 In Example 1, cleaning liquid 1 was changed to cleaning liquid 4, and 1.02 g of cleaning liquid 4 was impregnated into 0.33 g of spunbond nonwoven fabric (ESE-545), and then dried at 95° C. for 15 minutes in the same manner as in Example 1 to produce a dry cleaning sheet 4. In the same manner as in Example 1, the obtained cleaning sheet 4 was wrapped around a sponge to produce a sponge. In the same manner as in Example 1, an oil film forming liquid (C112) was applied to a polished glass surface and cured to prepare a glass plate as a test subject, and the contact angle of the test subject surface of the glass plate was measured. After 0.5 g of water was dropped onto the surface of the glass plate to be tested, the cleaning sheet 4 wrapped around the sponge was placed in contact with the surface, and a load of 2 kg was applied from above the cleaning sheet 4, and the test surface was rubbed a predetermined number of times in the same manner as in Example 1. When the number of rubbings reached 20, the contact angle of the test surface was measured. In the same manner, the contact angle was measured when the surface had been rubbed 40 times, and when the surface had been rubbed 60 times. The results are shown in Table 1.

[0035] Comparative Example 1 In Example 1, cleaning liquid 1 was changed to cleaning liquid 5, and 0.72 g of cleaning liquid 5 was impregnated into 0.33 g of spunbond nonwoven fabric (ESE-545), and then dried at 95° C. for 15 minutes in the same manner as in Example 1 to produce cleaning sheet 5. In the same manner as in Example 1, the obtained cleaning sheet 5 was wrapped around a sponge to produce a sponge. In the same manner as in Example 1, an oil film forming liquid (C112) was applied to a polished glass surface and cured to prepare a glass plate as a test subject, and the contact angle of the test subject surface of the glass plate was measured. After 0.5 g of water was dropped onto the surface of the glass plate to be tested, the cleaning sheet 5 wrapped around the sponge was placed in contact with the surface, and a load of 2 kg was applied from above the cleaning sheet 5, and the surface to be tested was rubbed a predetermined number of times in the same manner as in Example 1. Similarly, the contact angle was measured after 20 reciprocal rubs, after 40 reciprocal rubs, and after 60 reciprocal rubs. The results are shown in Table 1.

[0036] Comparative Example 2 In Example 1, cleaning liquid 1 was changed to cleaning liquid 6, and 0.98 g of cleaning liquid 6 was impregnated into 0.33 g of spunbond nonwoven fabric (ESE-545), and then dried at 95° C. for 15 minutes in the same manner as in Example 1 to produce cleaning sheet 6. The obtained dry cleaning sheet 6 was wrapped around a sponge similar to that described above to produce a cleaning sheet. In the same manner as in Example 1, an oil film forming liquid (C112) was applied to a polished glass surface and cured to prepare a glass plate as a test subject, and the contact angle of the test surface of the glass plate was measured. After 0.5 g of water was dropped onto the surface of the glass plate to be tested, the cleaning sheet 6 wrapped around the sponge was placed in contact with the surface, and a force was applied so that a load of 2 kg was applied from above the cleaning sheet 6, and the test surface was rubbed a predetermined number of times in the same manner as in Example 1. When the number of rubs reached 20, the contact angle of the test surface was measured. When the number of rubs reached 20, the contact angle of the test surface was measured. In the same manner, the contact angle was measured when the test surface had been rubbed 40 times, and when the test surface had been rubbed 60 times. The results are shown in Table 1.

[0037] Contact angle measurement: The contact angles were measured at three random points on the surface of the test subject using a measuring instrument (model CA-DT) manufactured by Kyowa Interface Science Co., Ltd., and the average value was calculated.

[0038] Example 5 20 g of cleaning solution 2 was placed in a petri dish and heated overnight in a thermostatic chamber at 70° C. to prepare cleaning composition 1 in a dry state. In the same manner as in Example 1, the surface of a glass plate as a test material was polished, and then an oil film-forming liquid (C112) was applied to the polished glass surface and cured to form an oil film on the glass surface, to prepare a glass plate as a test subject. The contact angle of the test surface of the obtained glass plate was measured. 0.1g of the obtained cleaning composition 1 was placed on the surface of the glass plate to be tested, 0.5g of water was dropped on it, and a sponge (2cm x 5cm) similar to that in Example 1 was placed on the surface of the glass plate to be tested so that the sponge was in contact with the surface of the glass plate to be tested, and a force was applied so that a load of 2kg was applied from above the sponge to rub the surface to be tested. When the number of times of rubbing reached 20 times, the contact angle of the surface to be tested was measured. In the same manner, the contact angle was also measured at the time of 40 times of rubbing and at the time of 60 times of rubbing. The results are shown in Table 2.

[0039] Example 6 A dry cleaning composition 2 was prepared in the same manner as in Example 5, except that cleaning liquid 2 in Example 5 was changed to cleaning liquid 4. In the same manner as in Example 1, the surface of a glass plate as a test material was polished, and then an oil film-forming liquid (C112) was applied to the polished glass surface and cured to form an oil film on the glass surface, to prepare a glass plate as a test subject. The contact angle of the test surface of the obtained glass plate was measured. 0.1g of the obtained cleaning composition 2 was placed on the surface of the glass plate to be tested, 0.5g of water was dropped on it, and a sponge (2cm x 5cm) similar to that in Example 1 was placed on the surface of the glass plate to be tested so that the sponge was in contact with the surface of the glass plate to be tested, and a force was applied so that a load of 2kg was applied from above the sponge to rub the surface to be tested. When the number of times of rubbing reached 20 times, the contact angle of the surface to be tested was measured. In the same manner, the contact angle was also measured at the time of 40 times of rubbing and at the time of 60 times of rubbing. The results are shown in Table 2.

[0040] Comparative Example 3 Dry cleaning composition 3 was prepared in the same manner as in Example 5, except that cleaning liquid 2 in Example 5 was changed to cleaning liquid 6. In the same manner as in Example 1, the surface of a glass plate as a test material was polished, and then an oil film-forming liquid (C112) was applied to the polished glass surface and cured to form an oil film on the glass surface, to prepare a glass plate as a test subject. The contact angle of the test surface of the obtained glass plate was measured. 0.1g of the obtained cleaning composition 3 was placed on the surface of the glass plate to be tested, 0.5g of water was dropped on it, and a sponge (2cm x 5cm) similar to that in Example 1 was placed on the surface of the glass plate to be tested so that the sponge was in contact with the surface of the glass plate to be tested, and a force was applied so that a load of 2kg was applied from above the sponge to rub the surface to be tested. When the number of times of rubbing reached 20 times, the contact angle of the test surface was measured. In the same manner, the contact angle was also measured at the time of 40 times of rubbing and at the time of 60 times of rubbing. The results are shown in Table 2.

[0041] Example 7 As a test material, a glass plate was prepared as a test subject by polishing the surface of the glass plate in the same manner as in Example 1, and then applying an oil film-forming liquid (C112) to the polished glass surface and curing the liquid to form an oil film on the glass surface. The contact angle of the test surface of the obtained glass plate was measured. A sponge (2 cm x 5 cm) was soaked with 0.5 g of the obtained cleaning solution 1, and the sponge was placed on the surface of the glass plate to be tested so that it was in contact with the surface. A force of 2 kg was applied to the sponge so that the test surface was rubbed. When the number of times of rubbing reached 10 times, the contact angle of the test surface was measured. In the same manner, the contact angle was also measured after 20 and 30 times of rubbing. The results are shown in Table 3.

[0042] Example 8 As a test material, a glass plate was prepared as a test subject by polishing the surface of the glass plate in the same manner as in Example 1, and then applying an oil film-forming liquid (C112) to the polished glass surface and curing the liquid to form an oil film on the glass surface. The contact angle of the test surface of the obtained glass plate was measured. In Example 7, the cleaning liquid 2 was impregnated into a sponge and tested in the same manner as in Example 7, except that the cleaning liquid 1 was changed to cleaning liquid 2. That is, 0.5 g of cleaning liquid 2 was impregnated into a sponge, and the sponge was placed on the test surface of the glass plate to be tested so that the sponge was in contact with the test surface, and a force was applied so that a load of 2 kg was applied from above the sponge to rub the test surface. When the number of rubbings reached 10, the contact angle of the test surface was measured, and when the number of rubbings reached 20, the contact angle was also measured, and when the number of rubbings reached 30. The results are shown in Table 3.

[0043] Example 9 As a test material, a glass plate was prepared as a test subject by polishing the surface of the glass plate in the same manner as in Example 1, and then applying an oil film-forming liquid (C112) to the polished glass surface and curing the liquid to form an oil film on the glass surface. The contact angle of the test surface of the obtained glass plate was measured. In Example 7, the cleaning liquid 3 was impregnated into a sponge and tested in the same manner as in Example 7, except that the cleaning liquid 1 was changed to cleaning liquid 3. That is, 0.5 g of cleaning liquid 3 was impregnated into a sponge, and the sponge was placed on the test surface of the glass plate to be tested so that the sponge was in contact with the test surface, and a force was applied so that a load of 2 kg was applied from above the sponge to rub the test surface. When the number of rubbings reached 10, the contact angle of the test surface was measured, and when the number of rubbings reached 20, the contact angle was also measured, and when the number of rubbings reached 30. The results are shown in Table 3.

[0044] Example 10 As a test material, a glass plate was prepared as a test subject by polishing the surface of the glass plate in the same manner as in Example 1, and then applying an oil film-forming liquid (C112) to the polished glass surface and curing the liquid to form an oil film on the glass surface. The contact angle of the test surface of the obtained glass plate was measured. In Example 7, the cleaning liquid 4 was impregnated into a sponge and tested in the same manner as in Example 7, except that the cleaning liquid 1 was changed to cleaning liquid 4. That is, 0.5 g of cleaning liquid 4 was impregnated into a sponge, and the sponge was placed on the test surface of the glass plate to be tested so that the sponge was in contact with the test surface, and a force was applied so that a load of 2 kg was applied from above the sponge to rub the test surface. When the number of rubbings reached 10, the contact angle of the test surface was measured, and when the number of rubbings reached 20, the contact angle was also measured, and when the number of rubbings reached 30. The results are shown in Table 3.

[0045] [Table 1]

[0046] [Table 2]

[0047] [Table 3]

[0048] From Table 1, it was found that the cleaning sheets of Examples 1 to 4 were more effective at removing dirt such as oily films on glass surfaces than the cleaning sheets of Comparative Examples 1 and 2. That is, cleaning sheets 1 to 4, which were obtained by impregnating sheets with cleaning solutions 1 to 4 containing the abrasive of the present invention, isopropyl alcohol, and glycol ether or glycol, and then drying, showed a cleaning effect even after 20 back-and-forth rubbings, compared with cleaning sheets 5 and 6, which were obtained by impregnating sheets with comparative cleaning solutions 5 and 6 and then drying, and the difference in cleaning effect was more noticeable after 40 back-and-forth rubbings and 60 back-and-forth rubbings. In addition, normally, when a cleaning sheet is dried, the abrasives and other ingredients tend to peel off, and it is often the case that the cleaning sheet is unable to provide excellent cleaning effects. However, it has been found that with the cleaning sheet of the present invention, the abrasives remain well even when the cleaning sheet is dried, and the cleaning sheet provides excellent cleaning effects.

[0049] From Table 2, it was found that the cleaning compositions of Examples 5 and 6, which were prepared by drying cleaning liquid 2 and cleaning liquid 4, had a better cleaning effect than the cleaning composition of Comparative Example 3, which was prepared by drying comparative cleaning liquid 6. In particular, it was found that Example 6, which was prepared by drying a cleaning liquid containing glycol ether, exhibited a very good cleaning effect, and exhibited a better cleaning effect than Example 5, which was prepared by drying a cleaning liquid containing propylene glycol. From this, it is presumed that the cleaning composition in the dried state of a cleaning liquid containing glycol ether has some effect on the abrasive particles themselves.

[0050] It is clear from Table 3 that the cleaning compositions of the present invention in a liquid state, namely cleaning solutions 1 to 4, have an excellent cleaning effect on stains such as oily films adhering to glass surfaces.

Claims

1. A cleaning composition comprising at least a glycol ether and / or glycol, an abrasive, and a polyhydric alcohol.

2. The cleaning composition of claim 1, wherein the cleaning composition is dried.

3. A cleaning sheet comprising the cleaning composition of claim 1.

4. The cleaning sheet of claim 3, wherein the cleaning sheet is dried.

5. 4. The cleaning sheet according to claim 3, wherein the polyhydric alcohol is at least one selected from the group consisting of glycerin, 1,3-butanediol, ethylene glycol, propylene glycol, and diethylene glycol.

6. 4. The cleaning sheet according to claim 3, wherein the abrasive is at least one selected from the group consisting of alumina, cerium oxide, and zirconium oxide.

7. 4. The cleaning sheet of claim 3, wherein the glycol ether is a glycol ether and the glycol is a glycol.

8. A method for producing a cleaning sheet, comprising the steps of: impregnating a sheet with a cleaning composition containing at least a glycol ether and / or glycol, an abrasive, and a polyhydric alcohol; and then drying the sheet.

9. The method for producing a cleaning sheet according to claim 8, wherein the drying step is carried out at a temperature in the range of 70° C. to 150° C. for a time in the range of 3 minutes to 60 minutes.

Citation Information

Patent Citations

  • JP1980039023U

  • Detergent composition for automobile window glass

    JP1985133100A

  • cleanser

    JP1987151498A

  • Creamy polishing composition

    JP1988146997A

  • cleaner

    JP1989083236A