Metal powder for projection
A cost-effective metal powder with specific alloy composition and circularity addresses the high cost of existing shot peening materials by achieving high hardness and durability for efficient shot peening and blasting without expensive elements or heat treatment.
Patent Information
- Application Number
- JP2023063712
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-10
- Publication Date
- 2024-10-23
AI Technical Summary
Existing shot peening materials for treating high-hardness materials are expensive due to the use of elements like hafnium and zirconium, and there is a need for a cost-effective alternative with high hardness.
A metal powder composition comprising specific amounts of C, Si, Mn, Cr, B, Ni, Mo, W, and V, with a hardness of 950 to 1300 HV, produced without expensive elements and through atomization, ensuring a circularity of 0.7 to 0.95, which enhances manufacturability and resistance to cracking.
The metal powder achieves high hardness and durability while maintaining cost-effectiveness, suitable for shot peening and blasting applications without requiring separate heat treatment, with improved circularity reducing breakage during projection.
Smart Images

Figure 2024150339000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a metal powder for blasting, and more particularly to a metal powder for blasting that is suitably used as a blasting material for shot peening or shot blasting. [Background technology]
[0002] Shot peening is a surface treatment method in which a large number of particles of projection material are projected at high speed onto the surface of a workpiece to impart compressive residual stress near the surface of the workpiece and improve its fatigue strength. Shot peening is used for automobile parts such as gears, molds, etc.
[0003] The blasting material used in shot peening should be hard enough to compress the surface of the material being treated, and in recent years, the blasting material itself is required to have even higher hardness (for example, HV1000 or higher) due to the increased strength of the material being treated as a result of lighter weight materials. Even when the purpose is surface polishing or scale removal, the higher the hardness, the more efficient the effect of being able to reduce the processing time and number of times it can be treated.
[0004] Known methods for producing high-hardness shot materials include using expensive elements such as hafnium or zirconium in the material, or adding a separate heat treatment, but all of these methods increase the production cost of the shot material, and therefore there has been a demand for low-cost shot materials with high hardness.
[0005] Incidentally, the following Patent Document 1 discloses a technology related to the present invention. Patent Document 1 discloses a high-hardness shot material made of an Fe-based alloy containing a specified amount of B and Al. However, while the material described in Patent Document 1 contains Al as an essential element, it does not contain C, and does not specifically disclose the chemical composition of the metal powder for blasting of the present invention. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2009-263756 A Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention has been made against the background described above, and aims to provide a metal powder for blasting that is high in hardness and inexpensive. [Means for solving the problem]
[0008] The metal powder for projection according to the first aspect of the present invention is defined as follows: It contains, by mass%, C: 2.0-5.0%, Si: 3.5% or less, Mn: 3.0% or less, Cr: 25.0-37.0%, B: 0.5-3.0%, Ni: 3.0% or less, with the balance being Fe and unavoidable impurities, and has a hardness of 950-1300HV.
[0009] Here, the average circularity can be set to 0.7 or more and less than 0.95 (second aspect).
[0010] In addition, the metal powder for projection according to a third aspect of the present invention comprises: In the first or second aspect, the steel sheet further contains, by mass%, one or more of Mo: 3.0% or less, W: 3.0% or less, and V: 3.0% or less.
[0011] The metal powder for projection defined in this manner is made of an alloy composition that does not use expensive elements such as hafnium or zirconium, and has high hardness (950 to 1300 HV) even though it is an atomized powder that does not require separate heat treatment, so it can be provided as a high-hardness, inexpensive metal powder for projection. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Next, the metal powder for projection according to one embodiment of the present invention will be specifically described.
[0013] The metal powder for blasting according to the present embodiment is composed of a large number of particles and is used as a blasting material for shot peening and shot blasting. The powder hardness is 950 to 1300 HV, and the average circularity is 0.7 or more and less than 0.95. The metal powder for projection is an Fe-based alloy containing predetermined amounts of C, Cr, and B, with the balance being Fe and unavoidable impurities. It may further contain Si, Mn, Ni, Mo, W, and V.
[0014] The reasons for limiting the chemical components of the metal powder for blasting are described in detail below. In the following description, "%" means "mass %" unless otherwise specified.
[0015] C: 2.0-5.0% C is an element that increases powder hardness. To obtain this effect, in this embodiment, C is contained in an amount of 2.0% or more, preferably 3.0% or more, and more preferably 3.5% or more. However, if an excessive amount of C is added, the nozzle of the melt is clogged with Cr carbide during atomization, which leads to deterioration of powder manufacturability. Therefore, the C content is set to 5.0% or less, preferably 4.6% or less, and more preferably 4.3% or less.
[0016] Si:3.5% or less Silicon is an element that increases the powder hardness. In addition, silicon acts as a deoxidizing element to prevent clogging of the discharge nozzle, improving powder manufacturability. Although silicon does not have to be contained, in order to obtain these effects, the silicon content is preferably 0.5% or more, and more preferably 1.0% or more. However, excessive addition of Si leads to a decrease in toughness and circularity, making the material more susceptible to cracking during shooting and shortening its life as a shooting material. For this reason, the Si content is set to 3.5% or less, preferably 3.0% or less, and more preferably 2.5% or less.
[0017] Mn:3.0% or less Mn is an element that increases powder hardness. Mn does not have to be contained, but in order to obtain the above effects, the Mn content is preferably 0.3% or more, and more preferably 0.6% or more. However, if an excessive amount of Mn is added, the nozzle may be clogged with Mn oxide during atomization, leading to deterioration in powder manufacturability. For this reason, the Mn content is set to 3.0% or less, preferably 2.5% or less, and more preferably 2.0% or less.
[0018] Cr: 25.0~37.0% Cr is an element that increases the powder hardness. In addition, it forms a passivation film with excellent corrosion resistance, which can increase the wear resistance and corrosion resistance of the powder. For this reason, in this embodiment, Cr is contained at 25.0% or more. The Cr content is preferably 27.0% or more, and more preferably 28.0% or more. However, from the viewpoint of material costs, the Cr content is set to 37.0% or less, preferably 35.0% or less, and more preferably 33.0% or less.
[0019] B: 0.5-3.0% If the B content is low, sufficient hardness cannot be obtained. In addition, the shape of the powder particles becomes irregular, making them more susceptible to cracking during projection. For this reason, in this embodiment, B is contained in an amount of 0.5% or more. It is preferably 0.7% or more, and more preferably 0.9% or more. However, if an excessive amount of B is added, the amount of boride increases too much, which reduces toughness and makes it easier for cracks to occur during blasting. For this reason, the B content is set to 3.0% or less, preferably 2.4% or less, and more preferably 2.0% or less.
[0020] Ni: 3.0% or less Ni is an element that contributes to improving corrosion resistance and can be contained as necessary. However, since Ni reduces the hardness of the powder particles, the Ni content is set to 3.0% or less, preferably 2.0% or less, and more preferably 1.0% or less.
[0021] Mo: 3.0% or less, W: 3.0% or less, V: 3.0% or less Mo, W, and V are elements that increase the hardness of powder particles and can be contained as necessary. However, if they are added in excess, the toughness decreases, the powder becomes more likely to crack during blasting, and the powder lifespan decreases. For this reason, the content of each of these elements is set to 3.0% or less, preferably 2.0% or less, and more preferably 1.0% or less.
[0022] Powder hardness: 950~1300HV In order to meet the increasing strength of the treated material, it is desirable to make the metal powder harder, but if the powder hardness is too high, cracks will easily occur during blasting, and the life of the blasting material (the number of times it can be used repeatedly) will be shortened. For this reason, in this embodiment, the powder hardness is set to 950 to 1300 HV.
[0023] Average circularity: 0.7 or more, less than 0.95 Circularity is 4πA / P, where A is the projected area of a powder particle and P is the perimeter. 2 The circularity of a powder particle with a perfectly circular shape is 1, and the more complex the shape, the smaller the circularity becomes. When used as a projection material, increasing the circularity of the powder particles (closer to 1) has the advantage of making them less likely to break when projected. However, if the circularity is excessively high (closer to a perfect circle), the ability to cut the target object is reduced, so in this embodiment, the average circularity is set to be 0.7 or more and less than 0.95.
[0024] (Method of manufacturing metal powder for blasting) The metal powder for projection can be produced by converting a molten alloy having a predetermined chemical composition into a powder form using a method such as atomization.
[0025] In the above manufacturing method, the molten alloy can be obtained by weighing out each raw material so as to have a predetermined chemical composition, and melting the weighed raw materials using melting means such as an arc furnace, a high-frequency induction furnace, or a heating furnace.
[0026] Examples of methods for obtaining powder from a molten alloy include the atomization method (gas atomization method, water atomization method, etc.). A gas such as N2, Ar, He, or the like or water is sprayed at high pressure onto the molten alloy that is discharged from the tip of a discharge nozzle into a spray chamber and flows downward continuously (in a rod shape), and the molten alloy is crushed and cooled to obtain powder. In order to obtain the above-specified circularity (0.7 or more and less than 0.95), the water atomization method is preferable because the gas atomization method results in an excessively high circularity. The water atomization method is also superior to the gas atomization method in terms of manufacturing costs.
[0027] The circularity of powder particles produced by the atomization method also varies based on the content of elements in the molten metal. For example, increasing the amount of B increases the surface tension of the molten metal, which increases the circularity of the powder particles. Conversely, if the amount of Si increases, the particles become more likely to deform (the circularity decreases). For this reason, it is possible to ensure the desired circularity by taking into account the effect of each alloy element on the circularity and properly balancing the amount of each alloy element added.
[0028] The blast metal powder thus produced has Cr-based carboborides dispersed and precipitated in a matrix of a mainly martensite structure, and can achieve a specified hardness (950 to 1300 HV) as-atomized. EXAMPLES
[0029] Next, examples of the present invention will be described in detail. Various evaluations were carried out using metal powders of examples and comparative examples (total of 25 types) shown in Table 1 below.
[0030] 1. Preparation of Metal Powder Each raw material was weighed to obtain the alloy composition shown in Table 1 below. Each weighed raw material was heated and melted using a high-frequency induction furnace to obtain a molten alloy. Then, metal powder was obtained from each obtained molten alloy using a water atomization method.
[0031] [Table 1]
[0032] 2. Characterization of Metal Powders The obtained metal powder was evaluated for (1) powder hardness, (2) manufacturability, (3) cracking during projection, and (4) circularity.
[0033] <Powder hardness> The metal powder was embedded in resin, polished, and measured with a Vickers hardness tester. The hardness was measured according to the JIS Z 2244 Vickers hardness test, and the test force was 0.4903N. The hardness was judged as the average of 10 points (one point for each of 10 powder particles). If the average value was within the range of 950 to 1300 HV, it was judged as pass (◯), and if it was outside the range, it was judged as fail (×).
[0034] <Manufacturability evaluation> The manufacturability was evaluated by observing the state of molten metal being discharged from the discharge nozzle of an atomizing device when the above metal powder was produced using the atomizing device. Manufacturability was judged as pass (◯) when no nozzle clogging was observed during the tapping of 300 kg, and as fail (×) when nozzle clogging was observed.
[0035] <Evaluation of cracks during projection> The above metal powder was projected using a projection device with circulating projection material under the following conditions. Material to be treated: SKD11 (hardness: HRC60) Projection distance: about 100mm Projection angle: 45° Projection time: 8 hours Projection material amount: 20kg Projection pressure: 0.6MPa The average particle size (d50) of the metal powder before and after projection was measured using a laser diffraction particle size distribution measuring device, and cracks were judged as pass (◯) if the average particle size after projection was more than 50% of the average particle size before projection, and fail (×) if it was 50% or less.
[0036] <Evaluation of circularity> The circularity is calculated by the following formula. Circularity = 4πA / P 2 In this formula, A is the projected area of the particle or its cross section, and P is the perimeter of the projected image. An image analyzer is used to measure A and P. For example, CAMSIZER (CAMSIZER is a registered trademark) manufactured by Microtrack Bell can be used. The number of measurement samples (number of measurement particles) was 10,000 or more for each example, and the volume average was taken as the circularity (average circularity). The results of each of these evaluations are shown in Table 1.
[0037] The evaluation results shown in Table 1 reveal the following: In Comparative Example 1, the C content was 1.4%, which was below the lower limit of the range specified in this embodiment, and the target hardness was not obtained.
[0038] In Comparative Example 2, the Si content was 4.0%, which exceeded the upper limit of the specified range, and the powder particles had an irregular shape with low circularity, and the cracking evaluation was "x". In Comparative Example 3, the Cr content was 15.5%, which was below the lower limit of the specified range, and the target hardness was not obtained.
[0039] Comparative Examples 4 and 5 were powders not containing B, and in both cases the target hardness was not achieved, and the cracking evaluation was also "x". In Comparative Example 6, B was 4.5%, which exceeded the upper limit of the specified range, and the hardness was excessively high, resulting in an evaluation of cracking of "x".
[0040] In Comparative Example 7, the Ni content was 4.4%, which exceeded the upper limit of the specified range, and the target hardness was not obtained. In Comparative Example 8, Mo was 4.8%, exceeding the upper limit of the specified range, and the hardness was excessively high, resulting in an evaluation of cracking as "x".
[0041] Comparative Example 9 is an example containing an excessive amount of C, and Comparative Example 10 is an example containing an excessive amount of Mn. In both examples, nozzle clogging occurred, and the manufacturability was evaluated as "x".
[0042] As described above, in all of the comparative examples, at least one of the evaluations of hardness, manufacturability, cracking during projection, and circularity did not achieve the target.
[0043] In contrast, the metal powders of Examples 1 to 15, which had the content of each element within the range specified in this embodiment and were produced as-atomized, obtained good results in the evaluations of hardness, manufacturability, cracking during blasting, and circularity, and were found to be suitable as high-hardness metal powders for blasting.
[0044] Although the embodiment and examples of the present invention have been described in detail above, these are merely examples, and the present invention can be embodied in various modified forms without departing from the spirit and scope of the present invention.
Claims
1. By mass% C: 2.0-5.0% Si: 3.5% or less Mn: 3.0% or less Cr:25.0~37.0% B: 0.5-3.0% Ni: 3.0% or less The balance is Fe and unavoidable impurities. Metal powder for projection, having a hardness of 950 to 1300 HV.
2. 2. The metal powder for projection according to claim 1, wherein the average circularity is 0.7 or more and less than 0.
95.
3. In claim 1 or 2, the Mo: 3.0% or less W: 3.0% or less V: 3.0% or less The metal powder for projection further comprises one or more of the following:
Citation Information
Patent Citations
High hardness shot material