Polyamide resin composition
The polyamide resin composition, combining aliphatic polyamide resin, acid-modified polyolefin, and glass fibers with a specific sizing agent, addresses wear and mechanical issues in sliding parts, offering improved durability and low friction.
Patent Information
- Application Number
- JP2024114613
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-12-22
- Filing Date
- 2024-07-18
- Publication Date
- 2024-10-23
AI Technical Summary
Existing polyamide resin compositions for sliding parts do not adequately address wear resistance and mechanical properties, particularly when used under friction conditions.
A polyamide resin composition comprising aliphatic polyamide resin, acid-modified polyolefin, and glass fibers coated with a sizing agent containing a polyurethane resin and a copolymer with an acidic group, along with higher fatty acid compounds, to enhance mechanical properties and sliding performance.
The composition exhibits excellent mechanical properties, sliding properties, and reduced wear resistance, making it suitable for applications requiring durability and low friction.
Smart Images

Figure 2024150581000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyamide resin composition. [Background technology]
[0002] Polyamide resins have excellent properties as engineering plastics and are widely used in various industrial fields such as automobiles, machinery, electricity, and electronics. In particular, because polyamide resins have excellent rigidity and toughness, they are used in sliding parts used under frictional conditions such as gears, cams, pulleys, bearings, bearing retainers, door checkers, and timing chain guide parts.
[0003] In order to improve the sliding properties, particularly the wear resistance, of such sliding parts, polyamide resins containing polyolefin components have been developed. Patent Documents 1 and 3 describe that a polyamide resin composition using an ultra-high molecular weight polyolefin component has excellent sliding properties. Patent Documents 1 and 2 use an acid-modified polyolefin component. Patent Document 4 discloses a glass fiber reinforced polyamide resin obtained by combining glass fibers treated with a glass fiber bundling agent containing a copolymer compound, aminosilane, and a polyurethane resin, and a polyamide resin. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2018-199789 A [Patent Document 2] JP 2018-119018 A [Patent Document 3] Japanese Patent Application Publication No. 10-60269 [Patent Document 4] JP 2014-231452 A Summary of the Invention [Problem to be solved by the invention]
[0005] Sliding parts are required not only to not wear out through repeated use, but also to not deteriorate the objects they come into contact with. Although the polyamide resin compositions of Patent Documents 1 to 3 have been confirmed to have good sliding properties, further improvements have been required to obtain compositions that satisfy the above requirements. With respect to the polyamide resin of Patent Document 4, merely the mechanical strength has been confirmed.
[0006] An object of the present invention is to provide a polyamide resin composition having excellent mechanical properties, sliding properties and abrasion resistance. [Means for solving the problem]
[0007] The present invention relates to, for example, the following [1] to [6]. [1] A polyamide resin composition comprising an aliphatic polyamide resin (A), an acid-modified polyolefin (B), and glass fibers (C) coated with a sizing agent, The polyamide resin composition comprises 100 parts by mass of a polyamide resin composition, and the polyamide resin composition comprises 50.00 to 90.00 parts by mass of an aliphatic polyamide resin (A), 2.00 to 15.00 parts by mass of an acid-modified polyolefin (B), and 6.00 to 14.00 parts by mass of glass fibers (C) coated with a sizing agent. The intrinsic viscosity [η] of the acid-modified polyolefin (B) measured in a decalin solvent at 135° C. is 10 to 40 dl / g; The average fiber diameter of the glass fibers is 10.0 μm or less, The sizing agent contains a polyurethane resin and a copolymer having an acidic group. Polyamide resin composition. [2] The polyamide resin composition according to [1], further comprising 0.05 to 0.50 parts by mass of at least one higher fatty acid compound (D) selected from the group consisting of higher fatty acid amides (D1) and higher fatty acid salts (D2) per 100 parts by mass of the polyamide resin composition. [3] The polyamide resin composition according to [1] or [2], wherein the aliphatic polyamide resin (A) has a structural unit derived from an aminocarboxylic acid or a lactam. [4] The polyamide resin composition according to any one of [1] to [3], wherein the aliphatic polyamide resin (A) has a number average molecular weight of 10,000 to 35,000. [5] A molded article made from the polyamide resin composition of any one of [1] to [4]. [6] A molded product of [5] used in applications where sliding properties are required. Effect of the Invention
[0008] The polyamide resin composition of the present invention is excellent in mechanical properties, sliding properties and abrasion resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The present invention relates to a polyamide resin composition comprising an aliphatic polyamide resin (A), an acid-modified polyolefin (B), and glass fibers (C) coated with a sizing agent, The polyamide resin composition comprises 100 parts by mass of a polyamide resin composition, and the polyamide resin composition comprises 50.00 to 90.00 parts by mass of an aliphatic polyamide resin (A), 2.00 to 15.00 parts by mass of an acid-modified polyolefin (B), and 6.00 to 14.00 parts by mass of glass fibers (C) coated with a sizing agent. The intrinsic viscosity [η] of the acid-modified polyolefin (B) measured in a decalin solvent at 135° C. is 10 to 40 dl / g; The average fiber diameter of the glass fibers is less than 10.0 μm, The sizing agent contains a polyurethane resin and a copolymer having an acidic group. The present invention relates to a polyamide resin composition.
[0010] <Aliphatic polyamide resin (A)> The polyamide resin composition contains an aliphatic polyamide resin (A). The aliphatic polyamide resin (A) may be an aliphatic homopolyamide resin (A-1) or an aliphatic copolyamide resin (A-2). These may be used alone or in combination of two or more.
[0011] (A-1) Aliphatic homopolyamide resin The aliphatic homopolyamide resin (A-1) means a polyamide resin having one type of monomer component constituting the aliphatic polyamide resin. Here, the monomer component constituting the aliphatic polyamide resin includes a combination of an aliphatic diamine and an aliphatic dicarboxylic acid, a lactam or an aminocarboxylic acid. The combination of an aliphatic diamine and an aliphatic dicarboxylic acid is a monomer component consisting of a condensation product of an aliphatic diamine and an aliphatic dicarboxylic acid. When the monomer components constituting the aliphatic polyamide resin are a combination of an aliphatic diamine and an aliphatic dicarboxylic acid, the combination of one type of aliphatic diamine and one type of aliphatic dicarboxylic acid is regarded as one type of monomer component.
[0012] The number of carbon atoms in the aliphatic diamine is preferably 2 to 20, and more preferably 4 to 12. The number of carbon atoms in the aliphatic dicarboxylic acid is preferably 2 to 20, and more preferably 6 to 12. The number of carbon atoms in the lactam is preferably 4 to 12. The number of carbon atoms in the aminocarboxylic acid is preferably 4 to 12.
[0013] Examples of lactams include ε-caprolactam, enantholactam, undecane lactam, α-pyrrolidone, α-piperidone, and lauryllactam. Among these, from the viewpoint of polymerization productivity, one selected from the group consisting of ε-caprolactam, undecanelactam and lauryllactam is preferred. Furthermore, examples of the aminocarboxylic acid include 6-aminocaproic acid, 7-aminoheptanoic acid, 9-aminononanoic acid, 11-aminoundecanoic acid, and 12-aminododecanoic acid. Among these, from the viewpoint of polymerization production, one selected from the group consisting of 6-aminocaproic acid, 11-aminoundecanoic acid, and 12-aminododecanoic acid is preferred.
[0014] Examples of the aliphatic diamine include aliphatic diamines other than alicyclic ones, such as ethylenediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine, decamethylenediamine, undecamethylenediamine, dodecamethylenediamine, tridecanediamine, tetradecanediamine, pentadecanediamine, hexadecanediamine, heptadecanediamine, octadecanediamine, nonadecanediamine, eicosanediamine, 2-methyl-1,8-octanediamine, and 2,2,4 / 2,4,4-trimethylhexamethylenediamine. Diamines: alicyclic diamines such as 1,3- / 1,4-cyclohexyldiamine, bis(4-aminocyclohexyl)methane, bis(4-aminocyclohexyl)propane, bis(3-methyl-4-aminocyclohexyl)methane, (3-methyl-4-aminocyclohexyl)propane, 1,3- / 1,4-bisaminomethylcyclohexane, 5-amino-2,2,4-trimethyl-1-cyclopentanemethylamine, 5-amino-1,3,3-trimethylcyclohexanemethylamine, bis(aminopropyl)piperazine, bis(aminoethyl)piperazine, and norbornanedimethyleneamine. Among these, from the viewpoint of polymerization productivity, aliphatic diamines other than alicyclic diamines are preferred, and hexamethylenediamine is more preferred.
[0015] Examples of the aliphatic dicarboxylic acid include non-alicyclic aliphatic dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecanedioic acid, tridecanedioic acid, tetradecanedioic acid, pentadecanedioic acid, hexadecanedioic acid, octadecanedioic acid, and eicosanedioic acid; and alicyclic dicarboxylic acids such as 1,3- / 1,4-cyclohexanedicarboxylic acid, dicyclohexanemethane-4,4'-dicarboxylic acid, and norbornanedicarboxylic acid. Among these, aliphatic dicarboxylic acids other than alicyclic ones are preferred, one selected from the group consisting of adipic acid, sebacic acid and dodecanedioic acid is more preferred, and adipic acid or dodecanedioic acid is even more preferred.
[0016] Combinations of aliphatic diamines and aliphatic dicarboxylic acids include a combination of hexamethylenediamine and adipic acid, a combination of hexamethylenediamine and sebacic acid, and a combination of hexamethylenediamine and dodecanedioic acid, and equimolar salts of these combinations are preferably used.
[0017] Specific examples of the aliphatic homopolyamide resin (A-1) include polybutyrolactam (polyamide 4), polytetramethylene adipamide (polyamide 46), polytetramethylene azelamide (polyamide 49), polytetramethylene sebacamide (polyamide 410), polyvalerolactam, (Polyamide 5), Polycaprolactam (Polyamide 6), Polyenantholactam (Polyamide 7), Polyundecanelactam (Polyamide 11), Polylauryllactam (Polyamide 12), Polypentamethylene adipamide (Polyamide 56), Polyhexamethylene adipamide (Polyamide 66), Polytetramethylene dodecamide (Polyamide 412), Polypentamethylene azelamide (Polyamide 59), Polypentamethylene sebacamide (Polyamide 510), Polypentamethylene dodecamide (Polyamide 512), Polypentamethylene tridecamide (Polyamide 513), Polyhexamethylene azelamide (Polyamide 69), Polyhexamethylene sebacamide (Polyamide 610), Polyhexamethylene dodecamide (Polyamide 612), polynonamethylene adipamide (polyamide 96), polynonamethylene azelamide (polyamide 99), polynonamethylene sebacamide (polyamide 910), polynonamethylene dodecamide (polyamide 912), polydecamethylene adipamide (polyamide 106), polydecamethylene azelamide (polyamide 109), polydecamethylene decamamide (polyamide 1010), polydecamethylene dodecamide (polyamide 1012), polydodecamethylene adipamide (polyamide 126), polydodecamethylene azelamide (polyamide 129), polydodecamethylene sebacamide (polyamide 1210), polydodecamethylene dodecamide (polyamide 1212), polydodecamethylene oxamide (polyamide 122), and the like. The aliphatic homopolyamide resin (A-1) may be used alone or in combination of two or more kinds.
[0018] Among these, from the viewpoint of polymerization productivity, the aliphatic homopolyamide resin (A-1) is preferably at least one selected from the group consisting of polyamide 6, polyamide 11, polyamide 12, polyamide 66, polyamide 610, and polyamide 612, more preferably at least one selected from polyamide 6, polyamide 11, polyamide 12, polyamide 610, and polyamide 612, and even more preferably polyamide 6.
[0019] (A-2) Aliphatic copolyamide resin The aliphatic copolyamide resin (A-2) is an aliphatic polyamide resin that has two or more kinds of monomer components constituting the aliphatic polyamide resin and does not have an aromatic ring. Therefore, the aliphatic copolyamide resin (A-2) includes a combination of an aliphatic diamine and an aliphatic dicarboxylic acid, and an aliphatic copolyamide resin that is a copolymer of two or more kinds of monomers selected from the group consisting of lactam and aminocarboxylic acid. Here, the combination of an aliphatic diamine and an aliphatic dicarboxylic acid is a monomer component consisting of a condensate of an aliphatic diamine and an aliphatic dicarboxylic acid. The combination of an aliphatic diamine and an aliphatic dicarboxylic acid is regarded as one type of monomer component by combining one type of diamine and one type of dicarboxylic acid.
[0020] Examples of the aliphatic diamine include the same as those exemplified as the raw material of the aliphatic homopolyamide resin (A-1). The diamine may be used alone or in combination of two or more. Among these, from the viewpoint of polymerization productivity, at least one selected from the group consisting of aliphatic diamines other than alicyclic is preferred, at least one selected from the group consisting of linear aliphatic diamines is more preferred, and hexamethylenediamine is even more preferred.
[0021] Examples of the aliphatic dicarboxylic acid include the same as those exemplified as the raw material of the aliphatic homopolyamide resin (A-1). The dicarboxylic acid may be used alone or in combination of two or more. Among these, aliphatic dicarboxylic acids other than alicyclic ones are preferred, at least one selected from the group consisting of adipic acid, sebacic acid, and dodecanedioic acid is more preferred, and at least one selected from the group consisting of adipic acid and dodecanedioic acid is even more preferred.
[0022] Examples of lactams include those exemplified as raw materials for the aliphatic homopolyamide resin (A-1). One type of lactam may be used alone, or two or more types may be used in appropriate combination. Among these, from the viewpoint of polymerization productivity, at least one selected from the group consisting of ε-caprolactam, undecanelactam and lauryllactam is preferred.
[0023] Examples of aminocarboxylic acids include those exemplified as raw materials for the aliphatic homopolyamide resin (A-1). The aminocarboxylic acids may be used alone or in combination of two or more. Among these, from the viewpoint of polymerization production, at least one selected from the group consisting of 6-aminocaproic acid, 11-aminoundecanoic acid, and 12-aminododecanoic acid is preferred.
[0024] Specific examples of the aliphatic copolymer polyamide resin (A-2) include caprolactam / hexamethylenediaminoadipic acid copolymer (polyamide 6 / 66), caprolactam / hexamethylenediaminoazelaic acid copolymer (polyamide 6 / 69), caprolactam / hexamethylenediaminosebacic acid copolymer (polyamide 6 / 610), caprolactam / hexamethylenediaminoundecanoic acid copolymer (polyamide 6 / 611), caprolactam / hexamethylenediaminododecanoic acid copolymer (polyamide 6 / 612), caprolactam / aminoundecanoic acid copolymer (polyamide 6 / 11), Examples of the aliphatic copolymer polyamides include caprolactam / lauryllactam copolymer (polyamide 6 / 12), caprolactam / hexamethylenediaminoadipic acid / lauryllactam copolymer (polyamide 6 / 66 / 12), caprolactam / hexamethylenediaminoadipic acid / hexamethylenediaminosebacic acid copolymer (polyamide 6 / 66 / 610), caprolactam / hexamethylenediaminoadipic acid / hexamethylenediaminododecanedicarboxylic acid copolymer (polyamide 6 / 66 / 612), and hexamethylenediaminoadipic acid / caprolactam copolymer (polyamide 66 / 6). The aliphatic copolymer polyamide resin (A-2) may be used alone or in the form of a mixture of two or more kinds.
[0025] Among these, from the viewpoint of suppressing the water absorption rate of the molded product and maintaining the mechanical strength, at least one selected from the group consisting of polyamide 6 / 66, polyamide 6 / 12 and polyamide 6 / 66 / 12 is preferred, at least one selected from the group consisting of polyamide 6 / 66 and polyamide 6 / 66 / 12 is more preferred, and polyamide 6 / 66 is particularly preferred.
[0026] From the viewpoint of productivity, the aliphatic polyamide resin (A) preferably has a structural unit derived from an aminocarboxylic acid or a lactam, is preferably an aliphatic homopolyamide resin (A-1), is more preferably one or more selected from the group consisting of polyamide 6, polyamide 46, polyamide 66, polyamide 610, polyamide 612, polyamide 11 and polyamide 12, and is particularly preferably polyamide 6, polyamide 46 and / or polyamide 66.
[0027] From the viewpoint of sliding property, the number average molecular weight of the aliphatic polyamide resin (A) is preferably 10,000 to 35,000, more preferably 10,000 to 32,000, and even more preferably 11,000 to 30,000. The number average molecular weight is a value calculated from the relative viscosity. The relative viscosity is a value measured at 25°C according to JIS K6920-2 by dissolving 1g of polyamide in 100ml of 96% concentrated sulfuric acid.
[0028] The terminal amino group concentration of the aliphatic polyamide resin (A), as determined by dissolving the resin in a mixed solvent of phenol and methanol and performing neutralization titration, is preferably in the range of 30 μmol / g or more, more preferably in the range of 30 μmol / g or more and 50 μmol / g or less. If the terminal amino group concentration is within the above range, sufficient moldability and mechanical properties can be obtained.
[0029] When the aliphatic polyamide resin (A) contains two or more polyamide resins with different terminal amino group concentrations (for example, at least one aliphatic homopolyamide resin (A-1) and at least one aliphatic copolymer polyamide resin (A-2)), the terminal amino group concentration in the aliphatic polyamide resin (A) is preferably measured by the above-mentioned neutralization titration. However, when the terminal amino group concentration of each polyamide resin and its mixing ratio are known, the terminal amino group concentration of the aliphatic polyamide resin (A) may be determined by multiplying each terminal amino group concentration by the mixing ratio and adding up the average value. In the present invention, the value measured by neutralization titration is used. The aliphatic polyamide resin (A) may be one type of component or a combination of two or more types of components.
[0030] The amount of the aliphatic polyamide resin (A) is 50.00 to 90.00 parts by mass, preferably 65.00 to 87.00 parts by mass, and more preferably 75.00 to 85.00 parts by mass, per 100 parts by mass of the polyamide resin composition. When the amount of the aliphatic polyamide resin (A) is within the above range, the mechanical properties and moldability are good.
[0031] <Acid-modified polyolefin (B)> The polyamide resin composition contains an acid-modified polyolefin (B). The acid-modified polyolefin (B) is a polyolefin modified with a compound containing an acid-modifying group. The acid-modified polyolefin (B) may be modified with a compound containing a modifying group other than the acid-modifying group in addition to being modified with a compound containing an acid-modifying group. By modifying the polyolefin with a compound containing an acid-modifying group, the affinity for the aliphatic polyamide resin (A) is improved.
[0032] Polyolefins are homopolymers or copolymers of olefins. Examples of the olefin include ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, 1-tridecene, 1-tetradecene, 1-pentadecene, 1-hexadecene, 1-heptadecene, 1-octadecene, 1-nonadecene, 1-eicosene, 3-methyl-1-butene, 3-methyl-1-pentene, 3-ethyl-1-pentene, 4-methyl-1-pentene, 4-methyl-1-hexene, 4,4-dimethyl-1-hexene, 4,4-dimethyl-1-pentene, 4-ethyl-1-hexene, 3-ethyl-1-hexene, 9-methyl-1-decene, 11-methyl-1-dodecene, and 12-ethyl-1-tetradecene. These may be used alone or in combination of two or more.
[0033] The copolymer may also be one obtained by copolymerizing a polyene such as a non-conjugated diene. Examples of the non-conjugated diene include 1,4-pentadiene, 1,4-hexadiene, 1,5-hexadiene, 1,4-octadiene, 1,5-octadiene, 1,6-octadiene, 1,7-octadiene, 2-methyl-1,5-hexadiene, 6-methyl-1,5-heptadiene, 7-methyl-1,6-octadiene, 4-ethylidene-8-methyl-1,7-nonadiene, 4,8-dimethyl-1,4,8-decatriene (DMDT), dicyclopentadiene, ... Examples of the aryl group include butyl ether, cyclohexadiene, cyclooctadiene, 5-vinylnorbornene, 5-ethylidene-2-norbornene, 5-methylene-2-norbornene, 5-isopropylidene-2-norbornene, 6-chloromethyl-5-isopropenyl-2-norbornene, 2,3-diisopropylidene-5-norbornene, 2-ethylidene-3-isopropylidene-5-norbornene, 2-propenyl-2,5-norbornadiene, etc. These may be used alone or in combination of two or more. The polyolefin is preferably a homopolymer of ethylene or a copolymer of ethylene and an α-olefin other than ethylene. Commercially available polyolefins include those sold as ultra-high molecular weight polyolefins.
[0034] Examples of the acid-modified group of the polyolefin include a carboxyl group, a carboxyl metal salt, an acid anhydride group, and a sulfonic acid group. The acid-modified group is preferably a carboxyl group or an acid anhydride group. Examples of the modified group other than the acid-modified group include an amino group, a hydroxyl group, a silanol group, an alkoxy group, a hydroxyl group, an epoxy group, an isocyanate group, a mercapto group, and an oxazoline group.
[0035] The acid-modified polyolefin (B) can be obtained by melt-kneading a polyolefin and a compound containing an acid-modified group, and graft-modifying the polyolefin to introduce an acid-modified group. The acid-modified polyolefin (B) can also be obtained by reacting a polyolefin with a compound containing an acid-modified group in the absence of a solvent using an extruder, a twin-screw kneader, or the like.
[0036] Examples of the compound containing an acid-modified group include unsaturated carboxylic acid or its derivative, hydroxyl group-containing ethylenically unsaturated compound, amino group-containing ethylenically unsaturated compound, vinyl group-containing organosilicon compound, etc. Examples of the unsaturated carboxylic acid or its derivative include unsaturated compound having one or more carboxyl groups, ester of a compound having a carboxyl group and an alkyl alcohol, unsaturated compound having one or more anhydrous carboxyl groups, etc. Examples of the unsaturated group include vinyl group, vinylene group, unsaturated cyclic hydrocarbon group, etc. From the viewpoint of reactivity, the compound containing an acid-modified group is preferably unsaturated carboxylic acid or its derivative.
[0037] Specific examples of the unsaturated carboxylic acid include unsaturated dicarboxylic acids such as acrylic acid, maleic acid, fumaric acid, tetrahydrophthalic acid, itaconic acid, mesaconic acid, citraconic acid, crotonic acid, isocrotonic acid, and endo-cis-bicyclo[2,2,1]hept-5-ene-2,3-dicarboxylic acid. In addition, examples of the derivatives of the unsaturated carboxylic acid include acid halides, amides, imides, anhydrides, and esters of the unsaturated carboxylic acids, and malenyl chloride, maleimide, maleic anhydride, citraconic anhydride, monomethyl maleate, dimethyl maleate, and glycidyl maleate are preferred. From the viewpoint of reactivity, the unsaturated carboxylic acid or its derivative is more preferably maleic anhydride and / or acrylic acid, and particularly preferably maleic anhydride. The compound containing an acid-modifiable group may be one component or two or more components.
[0038] The compound containing a modifying group other than the acid-modified group can be appropriately selected from the compounds containing a modifying group other than the acid-modified group described above.
[0039] When the polyolefin is modified with an acid, the amounts of the compound containing the acid-modifying group and the compound containing any modifying group other than the acid-modifying group to be added can be appropriately set depending on the desired degree of modification of the polyolefin.
[0040] When the acid-modified polyolefin (B) is obtained by melt-kneading a polyolefin and a compound containing an acid-modified group, and graft-modifying the polyolefin to introduce an acid-modified group, the graft-modification of the polyolefin can be carried out, for example, by dissolving the polyolefin in an organic solvent, then adding the compound containing an acid-modified group and a radical initiator to the solution, and reacting them. The reaction temperature is preferably 70°C to 200°C, and particularly preferably 80°C to 190°C. The reaction time is preferably 0.5 hours to 15 hours, and particularly preferably 1 to 10 hours.
[0041] When the acid-modified polyolefin (B) is obtained by reacting a polyolefin with a compound containing an acid-modified group without using a solvent, such as an extruder or a twin-screw kneader, the reaction is preferably carried out at a temperature equal to or higher than the melting point of the polyolefin, particularly preferably from 160° C. to 330° C. The reaction is preferably carried out by melt kneading for 0.5 to 10 minutes.
[0042] The acid-modified polyolefin (B) has an intrinsic viscosity [η] of 10 to 40 dl / g, preferably 15 to 35 dl / g, and more preferably 20 to 30 dl / g, measured in decalin solvent at 135°C. When the intrinsic viscosity [η] is 10 or more, the dynamic friction coefficient of the polyamide resin composition tends to be low and the sliding properties tend to be improved. The intrinsic viscosity [η] of the acid-modified polyolefin (B) can be adjusted by the polymerization conditions.
[0043] In addition to the above, examples of the acid-modified polyolefin (B) include the components described in JP-A-2018-199789 and JP-A-2006-28231. The acid-modified polyolefin (B) may be one type of component or a combination of two or more types of components.
[0044] The amount of the acid-modified polyolefin (B) is 2.00 to 15.00 parts by mass, preferably 2.00 to 13.00 parts by mass, and more preferably 4.00 to 11.00 parts by mass, per 100 parts by mass of the polyamide resin composition. When the amount of the acid-modified polyolefin (B) is within the above range, the sliding property and mechanical strength are good.
[0045] <Glass fiber coated with a sizing agent containing a polyurethane resin and a copolymer having an acidic group (C)> The polyamide resin composition contains glass fiber (C) coated with a sizing agent containing a polyurethane resin and a copolymer having an acidic group. The glass fiber (C) coated with a sizing agent containing a polyurethane resin and a copolymer having an acidic group (hereinafter also referred to as "glass fiber (C) coated with a sizing agent") is a component that imparts excellent sliding properties and mechanical properties to the polyamide resin composition.
[0046] [Glass fiber] Examples of the glass constituting the glass fiber include those having compositions such as A glass, AR glass, C glass, D glass, E glass, H glass, S glass, T glass, M glass, and NE glass.
[0047] A fiber has an aspect ratio (ratio of long diameter to short diameter) of 10 or more. Glass fibers may break when melt-kneaded with other components, and therefore, as long as the glass fibers meet the definition of "fiber" in this specification when blended, they may also be broken during melt-kneading and, as a result, may no longer meet the definition of "fiber" in this specification in the polyamide composition.
[0048] The shape of the glass fiber is not particularly limited, and examples thereof include flat fiber, chopped strand, etc. The cross-sectional shape of the glass fiber is not particularly limited, and examples thereof include a perfect circle, a cocoon, an oval, a rectangle, or shapes similar thereto.
[0049] The average fiber diameter of the glass fibers is 10.0 μm or less, preferably 5.0 μm to 10.0 μm, and more preferably 5.0 μm to 8.0 μm. When the average fiber diameter of the glass fibers is within the above range, the sliding properties are excellent and the amount of wear is suppressed. The average fiber diameter of the glass fibers is a value measured by an optical microscope, and when a commercially available product is used, it may be a catalog value. The average fiber diameter of the glass fibers (C) coated with a sizing agent is also preferably within the same range.
[0050] When the cross section of the glass fiber is rectangular or a similar shape, the length of one side of the cross section is preferably 0.5 μm to 50 μm, and particularly preferably 1 to 40 μm. The number average fiber length of the glass fiber is preferably 250 μm to 400 μm, and particularly preferably 300 μm to 360 μm. The weight average fiber length of the glass fiber is preferably 350 μm to 550 μm, and particularly preferably 380 μm to 500 μm. The number average fiber length and weight average fiber length of the glass fiber can be determined by using image analysis software from an image taken with a transmission microscope. The aspect ratio obtained by dividing the number average fiber length by the average fiber diameter of the glass fiber is preferably 10 or more, and particularly preferably 15 to 100, from the viewpoints of rigidity, mechanical strength, and fluidity.
[0051] [Polyurethane resin] The polyurethane resin is a resin obtained by subjecting a polyol component and a polyisocyanate component to a urethane reaction.
[0052] <Polyol component> Examples of the polyol component include polyester polyols (condensation polyester polyols, lactone polyester polyols), polycarbonate polyols, and polyether polyols.
[0053] Condensation polyester polyols include those obtained by reacting dicarboxylic acids or lower alkyl esters thereof with aliphatic diols. Examples of dicarboxylic acids or lower alkyl esters thereof include adipic acid, succinic acid, azelaic acid, pimelic acid, sebacic acid, and phthalic acid. Examples of aliphatic diols include aliphatic diols without side chains such as ethylene glycol, 1,4-butanediol, 1,6-hexanediol, and 1,10-decamethylene glycol, and aliphatic diols with side chains such as 1,2-propylene glycol, 1,3-butanediol, 2,5-dimethyl-2,5-hexanediol, 2,2-diethyl-1,3-propanediol, and neopentyl glycol.
[0054] Examples of lactone-based polyester polyols include those obtained by reacting a lactone compound such as β-propiolactone, pivalolactone, δ-valerolactone, ε-caprolactone, methyl-ε-caprolactone, dimethyl-ε-caprolactone, or trimethyl-ε-caprolactone with a hydroxy compound such as a short-chain polyol.
[0055] The polycarbonate polyol is obtained by transesterification of a hydroxy compound such as a short-chain polyol with diallyl carbonate, dialkyl carbonate, or ethylene carbonate. For example, poly-1,6-hexamethylene carbonate, poly-2,2'-bis(4-hydroxyhexyl)propane carbonate, etc. are industrially produced and easily available. Another method for obtaining polycarbonate polyol is the so-called phosgene method (or solvent method).
[0056] Examples of polyether polyols include polyethylene glycol, polypropylene glycol, polytetramethylene glycol, polyoxypropylene glycol, and glycerin-based polyalkylene ether glycol.
[0057] <Polyisocyanate component> Examples of the polyisocyanate include aliphatic polyisocyanates, alicyclic polyisocyanates, and aromatic polyisocyanates.
[0058] Examples of aliphatic polyisocyanates include ethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate (HDI), dodecamethylene diisocyanate, 1,6,11-undecane triisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, lysine diisocyanate, 2,6-diisocyanatomethyl caproate, bis(2-isocyanatoethyl) fumarate, bis(2-isocyanatoethyl) carbonate, and 2-isocyanatoethyl-2,6-diisocyanatohexanoate.
[0059] Examples of alicyclic polyisocyanates include isophorone diisocyanate (IPDI), 4,4'-dicyclohexylmethane diisocyanate (hydrogenated MDI), cyclohexylene diisocyanate, methylcyclohexylene diisocyanate (hydrogenated TDI), bis(2-isocyanatoethyl)-4-cyclohexene-1,2-dicarboxylate, 2,5-norbornane diisocyanate, and 2,6-norbornane diisocyanate.
[0060] Examples of aromatic polyisocyanates include 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, 2,4-tolylene diisocyanate (TDI), 2,6-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate (MDI), 2,4-diphenylmethane diisocyanate, 4,4'-diisocyanatobiphenyl, 3,3'-dimethyl-4,4'-diisocyanatobiphenyl, 3,3'-dimethyl-4,4'-diisocyanatodi ... Phenylmethane, 1,5-naphthylene diisocyanate, 4,4',4''-triphenylmethane triisocyanate, m-isocyanatophenylsulfonyl isocyanate, p-isocyanatophenylsulfonyl isocyanate, 1-methyl-2,6-phenylene diisocyanate, 1-methyl-2,5-phenylene diisocyanate, 1-methyl-2,6-phenylene diisocyanate, 1-methyl-3,5-phenylene diisocyanate, 1-ethyl-2,4-phenylene Diisocyanate, 1-isopropyl-2,4-phenylene diisocyanate, 1,3-dimethyl-2,4-phenylene diisocyanate, 1,3-dimethyl-4,6-phenylene diisocyanate, 1,4-dimethyl-2,5-phenylene diisocyanate, diethylbenzene diisocyanate, diisopropylbenzene diisocyanate, 1-methyl-3,5-diethylbenzene diisocyanate, 3-methyl-1,5-diethylbenzene-2,4-diisocyanate , 1,3,5-triethylbenzene-2,4-diisocyanate, naphthalene-1,4-diisocyanate, 1-methyl-naphthalene-1,5-diisocyanate, naphthalene-2,6-diisocyanate, naphthalene-2,7-diisocyanate, 1,1-dinaphthyl-2,2'-diisocyanate, biphenyl-2,4'-diisocyanate, 3,3'-dimethylbiphenyl-4,4'-diisocyanate, 2,2'-diphenylmethane diisocyanate, and the like.
[0061] The polyisocyanate is preferably a diisocyanate having two isocyanato groups per molecule.
[0062] In the urethanization reaction, a chain extender such as a polyhydric alcohol or a polyhydric amine can also be used.
[0063] [Copolymers with acidic groups] Examples of the copolymer having an acidic group include a copolymer of a monomer having an acidic group, and a copolymer of a monomer having an acidic group and a monomer not having an acidic group.
[0064] Examples of monomers having an acidic group include unsaturated carboxylic acids and carboxylic anhydrides. Examples of unsaturated carboxylic acids include acrylic acid, maleic acid, fumaric acid, tetrahydrophthalic acid, itaconic acid, mesaconic acid, citraconic acid, crotonic acid, isocrotonic acid, and endo-cis-bicyclo[2,2,1]hept-5-ene-2,3-dicarboxylic acid. Examples of carboxylic anhydrides include dicarboxylic anhydrides such as maleic anhydride, itaconic anhydride, succinic anhydride, phthalic anhydride, glutaric anhydride, dodecenylsuccinic anhydride, chlorendic anhydride, and citraconic anhydride. Examples of carboxylic anhydrides include dicarboxylic anhydrides such as maleic anhydride, itaconic anhydride, succinic anhydride, phthalic anhydride, glutaric anhydride, dodecenylsuccinic anhydride, and chlorendic anhydride. The carboxylic anhydride is preferably maleic anhydride, since it has little steric hindrance during copolymerization and has a small polarity of the compound. The monomer having an acidic group may also be a monomer having a functional group having the same function as the acidic group, and examples of such functional groups include acid halides, amides, imides, and esters of the unsaturated carboxylic acids, and examples of monomers having a functional group having the same function as the acidic group include malenyl chloride, maleimide, monomethyl maleate, dimethyl maleate, glycidyl maleate, etc. These may be used alone or in combination of two or more.
[0065] Examples of monomers that do not have an acidic group include styrene, ethylene, and acetylene.
[0066] The copolymer having an acidic group is preferably a copolymer compound in which an unsaturated dicarboxylic acid and / or a carboxylic acid anhydride, methyl acrylate, and methyl methacrylate are copolymerized.
[0067] The copolymerization ratio of the unsaturated dicarboxylic acid and / or carboxylic anhydride is preferably 20 to 60 mass%, and more preferably 25 to 55 mass%, from the viewpoints of reactivity and mechanical properties when producing the copolymer. The copolymerization ratio of methyl acrylate is preferably 20 to 75 mass%, and more preferably 30 to 65 mass%, from the viewpoints of reactivity and mechanical properties when producing the copolymer. The copolymerization ratio of methyl methacrylate is preferably 5 to 20 mass%, and more preferably 7 to 17 mass%, from the viewpoints of reactivity and mechanical properties when producing the copolymer. The copolymerization ratio of the monomer not having an acidic group is preferably 10 mass% or less, and more preferably 1 mass% or less.
[0068] From the viewpoints of reactivity during production of the copolymer and mechanical properties, the weight-average molecular weight of the copolymer compound is preferably 10,000 to 60,000, and particularly preferably 20,000 to 50,000. The weight-average molecular weight of the copolymer compound is a molecular weight measured by gel permeation chromatography (GPC).
[0069] [Other ingredients in sizing agents] The sizing agent may contain further components in addition to the polyurethane resin and the copolymer having an acidic group. Examples of the further components include coupling agents, lubricants, nonionic surfactants, antistatic agents, water, organic solvents, etc. Examples of the lubricants include fatty acid amides and quaternary ammonium salts. Examples of the nonionic surfactants include synthetic alcohols, natural alcohols, and fatty acid esters. The water and organic solvents are components that dissolve the lubricants, nonionic surfactants, antistatic agents, etc. Examples of the organic solvents include ethanol, etc.
[0070] The content of each component in the sizing agent can be appropriately set depending on the properties of the resulting glass fibers.
[0071] [Coating] The glass fibers are coated with a sizing agent containing a polyurethane resin and a copolymer having an acidic group. The term "coated" means that the sizing agent is attached to at least a part of the surface of the glass fibers. The glass fibers are surface-treated by coating with the sizing agent. The glass fibers may also be subjected to a bundling process in which two or more glass fibers are bundled into one by coating with the sizing agent. The bundling process can also be performed by coating a plurality of glass fiber monofilaments formed by drawing molten glass from a plurality of nozzles with the sizing agent, bundling the monofilaments into one glass fiber strand, and then winding the monofilaments into a cake.
[0072] The glass fibers (C) coated with the sizing agent may be surface-treated with a further component, such as the further component contained in the sizing agent.
[0073] In addition to the above, the glass fibers (C) coated with a sizing agent containing a polyurethane resin and a copolymer having an acidic group may contain the components described in JP-A-2014-231452. The glass fibers (C) coated with a sizing agent containing a polyurethane resin and a copolymer having an acidic group may be one type of component or a combination of two or more types of components.
[0074] The blending amount of the glass fiber (C) coated with a sizing agent is 6.00 to 14.00 parts by mass. If the blending amount of the glass fiber (C) is outside the above range, the mechanical properties tend to be inferior. If the blending amount of the glass fiber (C) exceeds 14.00 parts by mass, the wear amount of the sliding parts and objects in contact with the sliding parts increases. From the viewpoint of moldability and mechanical strength, the blending amount of the glass fiber (C) coated with a sizing agent is preferably 7.00 to 13.00 parts by mass, and particularly preferably 8.00 to 12.00 parts by mass.
[0075] <Higher fatty acid compound (D)> The polyamide resin composition is preferably blended with at least one higher fatty acid compound (D) selected from the group consisting of higher fatty acid amides (D1) and higher fatty acid salts (D2). Among the higher fatty acid compounds (D), higher fatty acid amides are preferred. In addition, from the viewpoint of suppressing the amount of wear, it is preferred to use a combination of higher fatty acid amides and higher fatty acid salts.
[0076] Examples of higher fatty acids include fatty acids having 12 or more carbon atoms, such as lauric acid, stearic acid, myristic acid, erucic acid, palmitic acid, behenic acid, oleic acid, arachidic acid, ricinoleic acid, and behenic acid. Examples of the higher fatty acid salt (D2) include metal salts of higher fatty acids. Examples of metals include Group 1 elements (alkali metals), Group 2 elements (alkaline earth metals), Group 12 elements, and Group 13 elements. Specific examples include magnesium stearate, zinc stearate, lithium stearate, calcium stearate, aluminum palmitate, lithium behenate, and calcium behenate.
[0077] Examples of the higher fatty acid amide (D1) include aliphatic mono higher fatty acid amides such as lauric acid amide, palmitic acid amide, oleic acid amide, stearic acid amide, erucic acid amide, behenic acid amide, ricinoleic acid amide, and 12-hydroxystearic acid amide, N-lauryl lauric acid amide, N-palmityl palmitic acid amide, N-oleyl palmitic acid amide, N-oleyl oleic acid amide, N-oleyl stearic acid amide, N-stearyl stearic acid amide, N-stearyl oleic acid amide, and N-stearyl erucic acid amide. , N-substituted aliphatic monocarboxylic acid amides such as N-stearyl-12-hydroxystearic acid amide, N-oleyl-12-hydroxystearic acid amide, methylol stearic acid amide, methylol behenic acid amide, and 12-hydroxystearic acid monoethanolamide, methylene bisstearic acid amide, methylene bislauric acid amide, methylene bis-12-hydroxystearic acid amide, ethylene biscapric acid amide, ethylene bislauric acid amide, ethylene bisoleic acid amide, ethylene bisstearic acid amide, ethylene N,N'-dioleyl sebacic acid amide, N,N'-dioleyl adipic acid amide, N,N'-distearyl adipic acid amide, N,N'-distearyl sebacic acid amide, etc. aliphatic biscarboxylic acid amides such as N,N'-dicyclohexanecarbonyl-1,4-diaminocyclohexane, 1,4-cyclohexanedicarboxamide, 1,4-cyclohexanedicarboxylic acid diaminocyclohexane, 1,2,3,4-butanetetracarboxylic acid tetracyclohexylamide, N,N'-bis(3-hydroxypropyl)-1,4-cubanedicarboxamide, N,N'-(1,4-cyclohexanediyl)bis(acetamide), tris(methylcyclohexyl)propanetricarboxamide, and the like;Examples of aromatic carboxylic acid amides include 4-cyclohexanedicarboxylic acid dianilide, 1,4-cyclohexanedicarboxylic acid dibenzylamide, trimesic acid tris(t-butylamide), trimesic acid tricyclohexylamide, trimesic acid tri(2-methylcyclohexylamide), trimesic acid tri(4-cyclohexylamide), 2,6-naphthalene acid dicarboxylic acid dicyclohexylamide, N,N'-dibenzylcyclohexane-1,4-dicarboxamide, N,N'-distearylisophthalic acid amide, N,N'-distearylterephthalic acid amide, m-xylylenebisstearic acid amide, and m-xylylenebis-12-hydroxystearic acid amide. Among these, preferred are aliphatic carboxylic acid amides selected from the group consisting of aliphatic monocarboxylic acid amides, N-substituted aliphatic monocarboxylic acid amides, and aliphatic biscarboxylic acid amides, and more preferred are aliphatic biscarboxylic acid amides. The higher fatty acid compound (D) may be one type of component or a combination of two or more types of components.
[0078] The amount of the higher fatty acid compound (D) is preferably 0.05 to 0.50 parts by mass, more preferably 0.10 to 0.50 parts by mass, and further preferably 0.15 to 0.45 parts by mass, per 100 parts by mass of the polyamide resin composition. When the amount of the higher fatty acid compound (D) is within the above range, the compound does not bleed out from the molded product, improves releasability, and contributes favorably to crystallization.
[0079] <Ingredients other than (A) to (D)> The polyamide resin composition may contain components other than (A) to (D) as long as the effects of the present invention are not impaired. The components other than (A) to (D) include resins other than the components (A) and (B) and functionality-imparting agents.
[0080] Examples of resins other than component (A) and component (B) include semi-aromatic polyamide resins, aromatic polyamide resins, unmodified polyolefin resins such as low-, medium-, and high-density polyethylene, polypropylene, and polybutene, polyester resins such as polyethylene terephthalate, polybutylene terephthalate, and polyester-based elastomers, vinyl aromatic resins such as polystyrene, ABS resin, and AS resin, polyether resins, polyurethane resins, acrylic resins, polyimide resins, polycarbonate resins, polyacetal, polyvinyl alcohol, and rosin resins.
[0081] Examples of the functionality-imparting agent include various additives that are usually blended into polyamide resin compositions, such as plasticizers, heat resistance agents, foaming agents, weather resistance agents, crystal nucleating agents, antioxidants, crystallization accelerators, release agents, lubricants, antistatic agents, dispersants, flame retardants, flame retardant assistants, pigments, and dyes.
[0082] Here, when the functionality-imparting agent is a heat resistance agent, an organic or inorganic heat resistance agent can be used depending on the purpose, and these may be used alone or in combination of two or more kinds. Examples of the organic heat-resistant agent include phenol-based compounds, phosphorus-based compounds, sulfur-based compounds, nitrogen-based compounds, etc. These may be used alone or in combination of two or more. Preferred examples of the phenolic compound include hindered phenolic organic compounds. In this specification, the term "hindered phenol" refers to a compound having a substituent at the ortho position of the phenolic hydroxyl group. Preferred examples of the phosphorus-based compound include hindered phenol phosphite compounds and hindered phenol hypophosphite compounds.
[0083] The heat resistance agent is preferably an inorganic compound or a combination of an inorganic compound and a nitrogen-containing compound. The inorganic compounds include metal halides and inorganic compounds other than metal halides.
[0084] Metal halides are compounds of halogens and metals. Examples of halogens include fluorine, chlorine, bromine, and iodine. Examples of metals include Group 1 elements (alkali metals), Group 2 elements (alkaline earth metals), and Group 3 to Group 12 elements (e.g., transition metals). The metal in the metal halide is preferably a Group 1 element (alkali metal) or Group 11 element (copper group). Examples of metal halides when the metal is a Group 1 element (alkali metal) include potassium iodide, potassium bromide, potassium chloride, sodium iodide, and sodium chloride. Examples of metal halides when the metal is a Group 11 element (copper group) include cuprous chloride, cupric chloride, cuprous bromide, cupric bromide, cuprous iodide, and cupric iodide. It is particularly preferable that the metal halide is potassium iodide and / or cuprous iodide.
[0085] Examples of inorganic compounds other than metal halides include metals, metal oxides, metal hydroxides, metal nitrides, metal phosphates, metal phosphites, metal carbonates, metal silicates, metal titanates, metal borates, metal sulfates, metal nitrates, etc. Specific examples of inorganic compounds other than metal halides include talc, mica, synthetic mica, glass flakes, non-swelling mica, fullerenes, carbon nanotubes, carbon black, graphite, metal foil, ceramic beads, clay, sericite, zeolite, bentonite, aluminum hydroxide, dolomite, kaolin, silica, finely powdered silicic acid, feldspar powder, potassium titanate, shirasu balloons, calcium carbonate, magnesium carbonate, barium sulfate, calcium oxide, aluminum oxide, titanium oxide, acid Examples of such fibers include magnesium nitride, aluminum silicate, silicon oxide, magnesium hydroxide, gypsum, novaculite, dawsonite, clay, glass fiber, carbon fiber, graphite fiber, metal fiber, potassium titanate whisker, aluminum borate whisker, magnesium-based whiskers, silicon-based whiskers, wollastonite, sepiolite, slag fiber, zonolite, elestadite, gypsum fiber, silica fiber, silica-alumina fiber, zirconia fiber, boron nitride fiber, silicon nitride fiber, and boron fiber.
[0086] Examples of the nitrogen-containing compound include melamine, benguanamine, dimethylol urea, and cyanuric acid.
[0087] When a heat resistant agent is added, the amount of the heat resistant agent added is preferably 0.01 to 2.00 parts by mass, more preferably 0.05 to 1.00 parts by mass, and more preferably 0.10 to 0.50 parts by mass, per 100 parts by mass of the polyamide resin composition.
[0088] Examples of functionality-imparting agents other than those mentioned above include the components described in JP-A-2002-370551. Each of the components other than (A) to (D) may be one type of component or a combination of two or more types of components.
[0089] <Method of producing polyamide resin composition> The method for producing the polyamide resin composition is not particularly limited as long as it is a method that can knead each component, and examples thereof include a production method using a twin-screw kneader, a twin-screw extruder, a single-screw extruder, a multi-screw extruder, etc. For example, any method may be used, such as a method in which all raw materials are blended using a twin-screw extruder and then melt-kneaded, a method in which a portion of the raw materials are blended and then melt-kneaded, and the remaining raw materials are further blended and melt-kneaded, or a method in which a portion of the raw materials are blended and then the remaining raw materials are mixed using a side feeder during melt-kneading.
[0090] In the polyamide resin composition, the aliphatic polyamide resin (A) and the acid-modified polyolefin (B) may be partially reacted. The reaction may be carried out in such a manner that the terminal amino group of the aliphatic polyamide resin (A) reacts with the acid-modified group of the acid-modified polyolefin (B). Therefore, the amount of each component when producing the polyamide resin composition may not be equal to the amount of each component in the polyamide resin composition after production.
[0091] [Uses of polyamide resin compositions, etc.] The polyamide resin composition is not particularly limited, and can be used to manufacture molded articles using known methods such as injection molding, extrusion molding, blow molding, rotational molding, vacuum molding, and compressed air molding. In addition, molded articles containing the polyamide resin composition can be used for parts that require sliding properties. Examples of parts that require sliding properties include gears, cams, pulleys, bearings, bearing retainers, door checks, timing chain guides, cable / hose support / guiding device products, and other dynamic applications. There is no problem with using the composition for other components that require similar functions. EXAMPLES
[0092] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.
[0093] <<Measurement method and evaluation>> [Mechanical properties] (1) Tensile stress, tensile breaking strain Type A test pieces were prepared based on ISO294-1, and tensile tests were carried out at 23°C and 50% RH based on ISO527-1,2.
[0094] (2) Flexural strength and flexural modulus Type B test pieces were prepared based on ISO294-1, and bending tests were carried out at 23°C and 50% RH based on ISO178 (Method A).
[0095] (3) Charpy impact strength Type B test pieces were prepared based on ISO294-1, and V-notched based on ISO 179 / 1eA. Charpy impact tests were performed with a hammer capacity of 1J at 23℃ and 50%RH.
[0096] The tensile stress is 110 to 130 MPa, the tensile breaking strain is 3.0 to 5.0%, the bending strength is 160 to 200 MPa, the bending modulus is 4,500 to 5,000 MPa, and the Charpy impact strength is 4.0 KJ / m 2If the value was equal to or greater than the above, the specimen was determined to have excellent "mechanical properties."
[0097] [Hardness] (1) Rockwell hardness (M scale) The measurements were made at 23°C and 50% RH using an electric digital Rockwell hardness tester (ARD-P) manufactured by Akashi Seisakusho Co., Ltd. in accordance with ISO 6508-1. In addition, when the Rockwell hardness is 80 to 92, the "hardness" is determined to be appropriate for a material for sliding parts.
[0098] [Sliding properties] The sliding properties between the polyamide resin composition and carbon steel were measured as follows. (1) Limit PV value Using an SE100D-C160S injection molding machine manufactured by Sumitomo Heavy Industries, Ltd., 60 mm x 40 mm x 3 mm test pieces of the polyamide resin composition of the examples and comparative examples were prepared. In accordance with the JISK7218A method, a Suzuki-type friction and wear tester (manufactured by Orientec Co., Ltd., EFM-III-EN) was used, and a ring with an outer diameter of 25.6 mm, an inner diameter of 20 mm, and a height of 15 mm, made of carbon steel S45C as described in JIS standard G4051, was used in a ring-on-disk method, with a test speed (circumferential speed) of 500 mm / s, a test load of 25 kgf (245 N) was applied at the start of the test, and the load was increased by 25 kgf (245 N) every 5 minutes, to measure the limit PV value of the prepared test piece. The limit PV test value was calculated from the load just before the load at which the test piece melted and a test speed (circumferential speed) of 500 mm / s using the following formula (I). Formula (I) Limit PV value = Pressure applied to the test piece just before it melts × Test speed (circumferential speed)
[0099] (2) Coefficient of kinetic friction Using an SE100D-C160S injection molding machine manufactured by Sumitomo Heavy Industries, Ltd., 60 mm x 40 mm x 3 mm test pieces of the polyamide resin composition of the examples and comparative examples were prepared. In accordance with the JISK7218A method, a Suzuki-type friction and wear tester (manufactured by Orientec Co., Ltd., EFM-III-EN) was used, and a ring with an outer diameter of 25.6 mm, an inner diameter of 20 mm, and a height of 15 mm, made of carbon steel S45C as described in the JIS standard G4051, was used in a ring-on-disk method, with a test speed (circumferential speed) of 500 mm / s, a test load of 25 kgf (245 N) was applied at the start of the test, and the load was increased by 25 kgf (245 N) every 5 minutes. The friction resistance of the prepared test piece was measured just before the limit PV value. The dynamic friction coefficient is a value calculated from the following formula (II). Formula (II) Coefficient of dynamic friction = (friction resistance just before the limit PV value is reached) / (normal load applied to the test piece)
[0100] In addition, a material was deemed to have excellent "slidability" when its limiting PV value was 400 MPa·cm / sec or more and its dynamic friction coefficient (polyamide vs. carbon steel) was 0.10 or less.
[0101] [Wear amount] (1) Abrasion of polyamide In order to confirm the amount of wear of the sliding parts, the amount of wear of the polyamide resin composition against carbon steel was measured as follows. Using an SE100D-C160S injection molding machine manufactured by Sumitomo Heavy Industries, Ltd., 60 mm x 40 mm x 3 mm test pieces of the polyamide resin composition of the examples and comparative examples were prepared. In accordance with the JISK7218A method, a Suzuki-type friction and wear tester (manufactured by Orientec Co., Ltd., EFM-III-EN) was used to measure the wear depth of the polyamide sliding surface of the test piece using a ring with an outer diameter of 25.6 mm, an inner diameter of 20 mm, and a height of 15 mm, made of carbon steel S45C as described in the JIS standard G4051, at a test speed (circumferential speed) of 300 mm / s, a sliding surface pressure of 4.4 MPa, and a sliding distance of 3.24 km, using a ring-on-disk method. The wear amount is a value calculated from the following formula (III). Formula (III) Polyamide wear amount=(sliding area×wear depth of test piece of polyamide resin composition) / (sliding surface pressure×sliding distance)
[0102] (2) Abrasion of polyacetal In order to confirm the amount of wear of an object with which the sliding parts come into contact, a polyacetal resin was used as the object with which the sliding parts come into contact, and the amount of wear of the polyacetal resin against the polyamide resin composition was measured as follows. Using a SE100D-C160S injection molding machine manufactured by Sumitomo Heavy Industries, Ltd., 60 mm x 40 mm x 3 mm test pieces of the polyamide resin composition of the examples and comparative examples were prepared. Similarly, a ring test piece of polyacetal resin with an outer diameter of 25.6 mm, an inner diameter of 20 mm, and a height of 15 mm was prepared. In accordance with the JISK7218A method, a Suzuki-type friction and wear tester (manufactured by Orientec Co., Ltd., EFM-III-EN) was used to measure the sliding surface wear depth of the polyacetal resin test piece using the test piece of the polyamide resin composition and the ring test piece of the polyacetal resin under the conditions of a ring-on-disk method, a test speed (circumferential speed) of 100 mm / s, a sliding surface pressure of 1.25 MPa, and a sliding distance of 1.08 km. The polyacetal wear amount is a value calculated from the following formula (IV). Formula (IV) Amount of polyacetal wear = (sliding area x wear depth of polyacetal resin test piece) / (sliding surface pressure x sliding distance)
[0103] (3) Coefficient of kinetic friction The dynamic friction coefficient between the polyamide resin composition and the polyacetal resin was measured as follows. Using a SE100D-C160S injection molding machine manufactured by Sumitomo Heavy Industries, Ltd., 60 mm x 40 mm x 3 mm test pieces of the polyamide resin composition of the examples and comparative examples were prepared. Similarly, a ring test piece of polyacetal resin with an outer diameter of 25.6 mm, an inner diameter of 20 mm, and a height of 15 mm was prepared. In accordance with the JISK7218A method, a test piece of the polyamide resin composition and a ring test piece of the polyacetal resin were used in a Suzuki-type friction and wear tester (manufactured by Orientec Co., Ltd., EFM-III-EN) to measure friction resistance force under the conditions of a ring-on-disk method, a test speed (circumferential speed) of 100 mm / s, a sliding surface pressure of 1.25 MPa, a sliding distance of 1.08 km, and a sliding surface test load of 25 kg. The dynamic friction coefficient is a value calculated from the following formula (V). Dynamic friction coefficient = (friction resistance force) / (sliding surface test load) (V)
[0104] The polyamide wear amount was 5.0 mm 3 / MPa·km or less, and the polyacetal wear amount was 1.7 mm 3 / MPa·km or less and the dynamic friction coefficient (polyamide vs. polyacetal) was 0.018 or less, the "amount of wear" was judged to be small.
[0105] [comprehensive evaluation] Examples that were judged to have excellent "mechanical properties," excellent "sliding properties," and little "wear" were rated as ◯ (pass), and examples that did not satisfy even one of the criteria were rated × (fail).
[0106] The components used in the examples and comparative examples are as follows. Polyamide 6: UBE Corporation, number average molecular weight 15,000, terminal amino group concentration 40 μmol / g LY1040: Maleic anhydride modified ultra-high molecular weight polyethylene, product name "LUBMER (registered trademark) LY1040", manufactured by Mitsui Chemicals, Inc., intrinsic viscosity [η] = 25 dl / g Glass fiber (1): Round chopped NEG T-211DE Φ6.5 microns (manufactured by Nippon Electric Glass Co., Ltd., average fiber diameter 6.5 μm, coated with a sizing agent containing polyurethane resin and a copolymer with an acidic group) Glass fiber (2): Round chop NEG T-211H Φ10.5 microns (manufactured by Nippon Electric Glass Co., Ltd., average fiber diameter 10.5 μm, coated with a sizing agent containing polyurethane resin and a copolymer with an acidic group) Glass fiber (3): Round chop 456S Φ6.5 microns (manufactured by Nitto Boseki Co., Ltd. Average fiber diameter 6.5 μm, coated with a bundling agent containing polyurethane resin) Ethylenebisstearic acid amide: Product name "Lightamide WH-255", manufactured by Kyoeisha Chemical Co., Ltd. Calcium stearate: NOF Corporation Calcium Stearate U Magnesium stearate: NOF Corporation Magnesium stearate Carbon black: Cabot Corporation VALCAN P CuI / KI: Cuprous iodide / potassium iodide = 1 / 6 (mixture) Dispersant: Nonionic surfactant, product name "Bal-7220", manufactured by Marubishi Kogyosha Co., Ltd. Polyacetal resin used in the measurement: Product name "Duracon M90-40" manufactured by Polyplastics Co., Ltd. The number average molecular weight of polyamide 6 is a value determined by relative viscosity. The relative viscosity is a value measured at 25° C. in accordance with JIS K6920-2 by dissolving 1 g of polyamide in 100 ml of 96% concentrated sulfuric acid. The terminal amino group concentration of polyamide 6 was determined by dissolving it in a mixed solvent of phenol and methanol and subjecting it to neutralization titration. The intrinsic viscosity [η] of the acid-modified polyolefin is a value measured in decalin solvent at 135°C. The average fiber diameter of the glass fibers is a catalog value.
[0107] [Examples 1 to 4, Comparative Examples 1 to 4] The components shown in Table 1 were melt-kneaded in a Coperion ZSK32Mc twin-screw kneader to prepare the desired polyamide resin composition pellets. Unless otherwise specified in the evaluation method, the obtained pellets were injection molded at a cylinder temperature of 290°C and a mold temperature of 80°C to prepare various test pieces, and various physical properties were evaluated.
[0108] [Table 1]
[0109] As is clear from the results in Table 1, the polyamide resin compositions of the examples are excellent in mechanical properties and sliding properties, and have a small amount of wear. In Comparative Example 1, in which the amount of bundled glass fibers (C) was less than the range of the present invention, the mechanical properties were inferior. In Comparative Example 2, in which the average fiber diameter of the glass fibers was longer than the range of the present invention, the sliding properties were poor and the amount of wear of the sliding parts was large. In Comparative Example 3, in which the glass fiber sizing agent did not contain a copolymer having an acidic group, the mechanical properties were poor and the wear amount of the sliding parts was large. In Comparative Example 4, in which the amount of bundled glass fibers (C) was greater than the range of the present invention, the mechanical properties and sliding properties were poor, the hardness was high, and the amount of wear of both the sliding parts and the objects in contact with the sliding parts was large. [Industrial Applicability]
[0110] The polyamide resin composition of the present invention is suitably used for molded articles in which sliding properties are required.
Claims
1. A polyamide resin composition comprising an aliphatic polyamide resin (A), an acid-modified polyolefin (B), and glass fibers (C) coated with a sizing agent, The polyamide resin composition comprises 100 parts by mass of a polyamide resin composition, and the polyamide resin composition comprises 50.00 to 90.00 parts by mass of an aliphatic polyamide resin (A), 2.00 to 15.00 parts by mass of an acid-modified polyolefin (B), and 6.00 to 14.00 parts by mass of glass fibers (C) coated with a sizing agent. The intrinsic viscosity [η] of the acid-modified polyolefin (B) measured in a decalin solvent at 135° C. is 10 to 40 dl / g; The average fiber diameter of the glass fibers is 10.0 μm or less, The sizing agent contains a polyurethane resin and a copolymer having an acidic group. Polyamide resin composition.
2. The polyamide resin composition according to claim 1, further comprising 0.05 to 0.50 parts by mass of at least one higher fatty acid compound (D) selected from the group consisting of higher fatty acid amides (D1) and higher fatty acid salts (D2) per 100 parts by mass of the polyamide resin composition.
3. The polyamide resin composition according to claim 1, wherein the aliphatic polyamide resin (A) has a structural unit derived from an aminocarboxylic acid or a lactam.
4. The polyamide resin composition according to claim 1, wherein the aliphatic polyamide resin (A) has a number average molecular weight of 10,000 to 35,000.
5. A molded article made from the polyamide resin composition according to any one of claims 1 to 4.
6. The molded article according to claim 5, which is used for an application requiring slidability.
Citation Information
Patent Citations
Resin composition excellent in sliding property
JP1998060269A
Glass fiber sizing agent, glass fiber, and glass fiber-reinforced polyamide resin
JP2014231452A
Modified polyethylene resin composition
JP2018119018A
Polyamide resin composition and molding made using the same, and method for producing polyamide resin composition
JP2018199789A