High-temperature ultra-high reliability alloys
A lead-free solder alloy with tailored compositions of silver, bismuth, antimony, and copper enhances mechanical and thermal properties, addressing the limitations of 96.5Sn3.0Ag0.5Cu for high-temperature applications by providing superior tensile strength and creep resistance.
Patent Information
- Application Number
- JP2024118696
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2019-09-02
- Filing Date
- 2024-07-24
- Publication Date
- 2024-10-23
AI Technical Summary
Existing lead-free solder alloys, such as 96.5Sn3.0Ag0.5Cu, do not perform well at high temperatures, and existing alternatives lack a favorable combination of high temperature reliability and mechanical properties necessary for applications in automotive, high power electronics, and energy sectors.
A lead-free solder alloy comprising specific weight percentages of silver, bismuth, antimony, copper, and other elements, including optional additives like nickel, titanium, and rare earths, which enhance mechanical properties and high temperature reliability by modifying the alloy's microstructure through solid solution strengthening and precipitation hardening.
The alloy exhibits improved mechanical properties, high temperature creep resistance, and thermomechanical properties, with tensile strength and creep rupture times significantly higher than 96.5Sn3.0Ag0.5Cu, suitable for operating temperatures of at least 150°C and resisting thermal cycling and shock.
Smart Images

Figure 2024150664000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates generally to the field of metallurgy, and more specifically to solder alloys suitable for use in electronic soldering applications such as, but not limited to, wave soldering, surface mount technology, hot air leveling and ball grid arrays, land grid arrays, bottom termination packages, LEDs and chip scale packages. [Background technology]
[0002] Lead-free solders were initially developed due to environmental and health concerns and as an alternative to traditional soft solder alloys. Many traditional lead-free solder alloys are based on a Sn-0.7 wt% Cu eutectic composition. Tin-silver-copper systems have also been accepted by the electronics industry as lead-free alternatives to soldering materials. For example, near-eutectic 96.5Sn3.0Ag0.5Cu exhibits superior fatigue life compared to eutectic Sn-Pb solder while having a melting point in the range of about 217-220°C. Summary of the Invention [Problem to be solved by the invention]
[0003] As the use of lead-free soldering materials becomes more widespread, either due to environmental directives or pressure from end users, the scope of application of such materials will also increase. For example, in some sectors, such as automotive, high-power electronics, including LED lighting, and energy, it is desirable for solder alloys to function at higher temperatures, e.g., 150°C or higher, for relatively long periods of time. However, the 96.5Sn3.0Ag0.5Cu alloy does not perform well at such temperatures.
[0004] Some attempts have been made to find a better performing alternative to 96.5Sn3.0Ag0.5Cu. US Patent Publication No. 10,376,994(B2) relates to soldering materials based on Sn, Ag, and Cu. US Patent Publication No. 2016 / 0325384(A1) relates to high reliability lead-free solder alloys for harsh environments and electronic applications. EP Patent Publication No. 3321025(A1) relates to lead-free solder alloys, flux compositions, solder paste compositions, electronic circuit boards, and electronic control devices. US Patent Publication No. 10,195,698(B2) relates to high reliability lead-free solder alloys. US Patent Publication No. 10,300,562(B2) relates to solder alloys, solder pastes, and electronic circuit boards. WO 2019 / 094242(A1) relates to low silver-tin based alternative solder alloys to standard SAC alloys for high reliability applications. WO 2019 / 094243(A1) relates to high reliability lead-free solder alloys for electronic applications in extreme environments. However, none of these alternatives provide a favorable combination of high temperature reliability and favorable mechanical properties.
[0005] The present invention aims to solve at least some of the problems associated with the prior art, or to provide a commercially acceptable alternative.
[0006] Thus, in a first aspect, the present invention provides a lead-free solder alloy comprising: 2.5 to 5% by weight of silver; 0.01 to 5% by weight of bismuth; 1 to 7 weight percent antimony; 0.01 to 2% by weight of copper; up to 6% by weight indium, Maximum 0.5% by weight titanium, up to 0.5% by weight germanium, Maximum 0.5% by weight rare earths, Maximum 0.5% by weight of cobalt, Maximum 5.0% by weight aluminum, Maximum 5.0% by weight silicon, Maximum 0.5% by weight manganese, Maximum 0.5% by weight chromium, maximum 0.5% by weight iron, maximum 0.5% by weight phosphorus; up to 0.5% gold by weight, up to 1% by weight of gallium, up to 0.5% by weight of tellurium, up to 0.5% by weight of selenium, Maximum 0.5% by weight calcium, maximum 0.5% by weight vanadium, Maximum 0.5% by weight of molybdenum, up to 0.5% by weight of platinum, and one or more of the following: up to 0.5% by weight of magnesium; Optionally, up to 0.5 wt. % nickel; and and a balance of tin along with any unavoidable impurities. [Brief description of the drawings]
[0007] The invention will now be further described with reference to the following drawings: [Figure 1] FIG. 1 shows a micrograph of a solder alloy according to the present invention. [Diagram 2] FIG. 2 shows a plot of solidus and liquidus temperatures for alloys having various Sb contents. [Diagram 3] FIG. 3 shows a plot of the solidus and liquidus temperatures for alloys having various Sb and Bi contents. [Figure 4] FIG. 4 shows a plot of hardness values for alloys having various Sb and Cu contents. [Diagram 5] FIG. 5 shows a plot of hardness values for alloys having various Sb and Bi contents. [Figure 6] FIG. 6 shows photomicrographs of a number of solder alloys according to the present invention. [Figure 7]FIG. 7 shows a plot of the ultimate tensile strengths (UTS) of a number of solder alloys according to the present invention and Sn3Cu0.5Ag. [Figure 8] FIG. 8 shows a plot of yield strengths (YS) for a number of solder alloys according to the present invention and Sn3Cu0.5Ag. [Figure 9] FIG. 9 shows a plot of creep strength at 150° C. and 200 N for a number of solder alloys according to the present invention as well as Sn3Cu0.5Ag. [Figure 10] FIG. 10 shows a plot of creep elongation at 150° C. and 200 N for a number of solder alloys according to the present invention as well as Sn3Cu0.5Ag. [Figure 11] FIG. 11 shows a photomicrograph of a BGA formed using a solder alloy according to the present invention. [Figure 12] FIG. 12 shows a Weibull distribution plot of in situ monitored failures of a BGA228 for a number of solder alloys according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] The present invention will now be further described. In the following passages, different aspects of the invention are defined in more detail. Each aspect so defined can be combined with any other aspect or aspects, unless expressly indicated otherwise. In particular, any feature indicated as being preferred or advantageous may be combined with any other feature or features indicated as being preferred or advantageous.
[0009] As used herein, the term "solder alloy" encompasses fusible metal alloys having a melting point in the range of 90-400° C. The alloys are lead-free, meaning that no lead is intentionally added, and therefore the lead content is either zero or below incidental impurity levels.
[0010] The solder alloy may exhibit improved high temperature reliability and may typically be able to withstand operating temperatures of at least 150° C. The solder alloy may exhibit improved mechanical properties and high temperature creep resistance compared to conventional 96.5SnAg3.0Cu0.5 alloys.
[0011] The solder alloy may have a high melting point, specifically a liquidus temperature greater than 210°C and less than 260°C. The solder alloy preferably has a liquidus temperature greater than 212°C, more preferably greater than 215°C, even more preferably greater than 218°C, and even more preferably greater than 220°C. A higher liquidus temperature may allow the alloy to be used in higher temperature soldering processes. The solder alloy preferably has a liquidus temperature less than 250°C, more preferably less than 240°C, and even more preferably less than 235°C. Such liquidus temperatures may be advantageous because peak reflow temperatures are typically 25-30°C above the liquidus temperature, and reflow temperatures greater than about 260°C may lead to various problems during soldering, such as damage to printed circuit boards and components.
[0012] The solder alloy may exhibit favorable mechanical properties and favorable solderability. The solder alloy may exhibit excellent high temperature creep properties and excellent thermomechanical properties and fatigue life, such as those evaluated in thermal cycle or thermal shock tests covering a wide temperature range and long dwell times. The solder alloy may exhibit excellent thermal cycle and / or thermal shock performance under harsh environmental conditions, such as, for example, from -40 to 150°C, with dwell times of 30 minutes at each temperature.
[0013] Alloying additions are used to modify the alloy's microstructure and therefore its properties due to physical metallurgical mechanisms such as precipitation strengthening, solid solution strengthening, grain refinement, and diffusion control.
[0014] Advantageously, the mechanical properties of the solder alloy, such as hardness, tensile strength, and high temperature creep, can be at least twice as large as those of 96.5SnAg3.0Cu0.5. Bismuth, antimony, and indium, for example, affect the solidus and / or liquidus temperature of the solder alloy. These elements also have high solid solubility in tin and therefore can contribute significantly to solid solution strengthening of the matrix. Changes in solidus or liquidus temperature do not appear to adversely affect the mechanical properties of the alloy.
[0015] The diffusion-dependent creep deformation depends on the homogeneous temperature, i.e., the ratio of the test temperature of the material to its melting temperature on an absolute scale. The homogeneous temperature of a solder alloy can be in the range of 0.84 to 0.86. Therefore, the melting temperature of a solder alloy does not have a significant effect on the mechanical properties.
[0016] An optimal combination of solid solution and precipitation strengthening can result in a distributed network of precipitation particles in a strong matrix. The precipitation particles can include, for example, Ag3Sn and (Cu,Ni)6Sn5. The precipitation network resists grain boundary migration during creep deformation, thus enhancing creep strength.
[0017] The solder alloy comprises 2.5-5.0 wt% silver. The solder alloy preferably comprises 2.8-4.5 wt% silver, more preferably 3-4 wt% silver. The presence of certain amounts of silver can serve to improve mechanical properties, such as strength, by the formation of network-like intermetallic compounds, such as Ag3Sn. In addition, the presence of silver can improve wetting and spreading. Higher levels of silver, especially levels above 4.5 wt%, can increase the liquidus temperature, and larger precipitates of Ag3Sn formed in the solder matrix act as sites for crack initiation and subsequent failure. Lower silver contents may not form sufficient Ag3Sn precipitates that can help improve strength.
[0018] The solder alloy comprises 0.01-5 wt% bismuth. The solder alloy preferably comprises 1.0-4.0 wt% bismuth, more preferably 2.0-4.0 wt% bismuth, even more preferably 2.5-4 wt% bismuth, even more preferably 2.8-4 wt% bismuth, even more preferably 3-4 wt% bismuth. In a preferred embodiment, then, the alloy comprises at least 2.8 wt% bismuth, preferably at least 3 wt% bismuth. The presence of a certain amount of bismuth can act to improve mechanical properties by solid solution strengthening. Bismuth can also act to improve creep resistance. Bismuth can also improve wetting and diffusion. However, bismuth additions beyond a certain amount can result in precipitation of bismuth in the tin, resulting in a more brittle alloy.
[0019] The solder alloy comprises 1-7 wt% antimony. The solder alloy preferably comprises 1.0-6.5 wt% antimony, more preferably 2-6 wt% antimony, even more preferably 3-6 wt% antimony, even more preferably 3.1-6 wt% antimony, even more preferably 3.2-6 wt% antimony. In a preferred embodiment, the alloy comprises at least 3 wt% antimony, preferably at least 3.1 wt% antimony, even more preferably at least 3.2 wt% antimony. The presence of a certain amount of antimony can act to improve mechanical properties by solid solution strengthening. Antimony can also act to improve creep resistance and thermal fatigue resistance. Antimony can also increase the liquidus temperature of the alloy. Antimony additions below the specified range may not have the required improvement in mechanical strength and thermal fatigue resistance. Antimony additions above the specified range can increase the liquidus temperature and thereby the required reflow temperature. Reflow temperatures higher than 260° C. can lead to various problems during soldering, including damaging the printed circuit board and components.
[0020] The solder alloy comprises 0.01-2 wt.% copper. The solder alloy preferably comprises 0.3-1.2 wt.% copper, preferably 0.4-0.8 wt.% copper. The presence of certain amounts of copper can serve to improve mechanical properties, e.g., strength, through the formation of Cu-Sn intermetallic compounds. Copper additions within certain ranges provide the optimum amount of intermetallic compound precipitates required to strengthen the alloy.
[0021] The solder alloy optionally includes up to 0.5 wt. % nickel, for example 0.001-0.5 wt. %. The solder alloy preferably includes nickel. The solder alloy preferably includes 0.001-0.4 wt. % nickel, more preferably 0.01-0.3 wt. % nickel, and even more preferably 0.02-0.2 wt. % nickel. The presence of a certain amount of nickel can act to improve mechanical properties by forming intermetallic compounds with tin and copper, which can result in precipitation strengthening. In addition, the presence of nickel can act to reduce the dissolution rate of copper. Nickel can also increase thermal reliability by reducing IMC growth at the substrate / solder interface.
[0022] The solder alloy optionally comprises up to 6% indium by weight, for example 0.001-6% indium by weight. The solder alloy preferably comprises indium. The solder alloy preferably comprises 0.001-5.5% indium by weight, more preferably 0.02-4% indium by weight, even more preferably 0.5-3% indium by weight. The presence of a certain amount of indium can serve to improve mechanical properties by solid solution strengthening and / or precipitation strengthening. The addition of indium can also lower the solidus and liquidus temperatures, with a greater impact on lowering the solidus temperature. Higher levels of indium can result in the formation of low temperature phases that adversely affect the long-term reliability of the alloy.
[0023] The solder alloy optionally comprises up to 0.5 wt.% titanium, for example 0.01-0.5 wt.% titanium. The solder alloy preferably comprises titanium. The solder alloy preferably comprises 0.001-0.3 wt.% titanium, more preferably 0.005-0.2 wt.% titanium, even more preferably 0.007-0.05 wt.% titanium. The presence of the specified amount of titanium can improve one or more of strength, solid state interfacial reaction, and thermo-mechanical reliability.
[0024] The solder alloy optionally comprises up to 0.5 wt. % germanium, for example 0.01-0.5 wt. % germanium. The solder alloy preferably comprises germanium.
[0025] The solder alloy preferably comprises 0.001-0.3 wt.% germanium, more preferably 0.001-0.1 wt.% germanium, and even more preferably 0.001-0.02 wt.% germanium. The presence of germanium may act to improve mechanical properties by particle dispersion. Germanium may also aid in deoxidation and improve wettability and solder joint strength, as well as appearance. In addition, germanium in combination with nickel and / or titanium may improve thermomechanical fatigue properties.
[0026] The solder alloy optionally includes up to 0.5 wt. % rare earth, for example 0.001-0.5 wt. % rare earth. The solder alloy preferably includes rare earth. As used herein, the term rare earth element refers to one or more elements selected from Sc, Y, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu.
[0027] The solder alloy preferably contains 0.002-0.3 wt.% rare earth, more preferably 0.003-0.05 wt.% rare earth. Preferred rare earths include cerium, neodymium, and lanthanum. The presence of rare earths may act to improve mechanical properties by particle dispersion and / or microstructural modification. Rare earths may act to improve diffusion and wettability.
[0028] The solder alloy optionally comprises up to 0.5 wt. % cobalt, for example 0.001-0.5 wt. % cobalt. The solder alloy preferably comprises cobalt. The solder alloy preferably comprises 0.01-0.2 wt. % cobalt, preferably from 0.01-0.2 wt. % cobalt, even more preferably 0.02-0.1 wt. % cobalt. The presence of a certain amount of cobalt can improve the strength and / or high temperature properties of the solder. In a preferred embodiment, the alloy is "cobalt-free". This can be advantageous in view of the high cost of cobalt and the toxicity of cobalt.
[0029] The solder alloy optionally comprises up to 5% by weight of aluminum, for example 0.001-5% by weight of aluminum. The solder alloy preferably comprises aluminum. The solder preferably comprises 0.001-3% by weight, more preferably 0.005-2% by weight of aluminum, even more preferably 0.01-1.5% by weight of aluminum, even more preferably 0.015-1% by weight of aluminum, even more preferably 0.02-0.08% by weight of aluminum. The presence of aluminum in the recited amounts can improve the fatigue life of the solder.
[0030] The solder alloy optionally contains up to 5% by weight of silicon, for example 0.001-5% by weight of silicon. The solder alloy preferably contains silicon. The solder alloy preferably contains 0.001-3% by weight of silicon, more preferably 0.005-2% by weight of silicon, even more preferably 0.01-1.5% by weight of silicon, even more preferably 0.015-1% by weight of silicon, even more preferably 0.02-0.08% by weight of silicon. The presence of silicon in the listed amounts can improve the mechanical properties, fatigue life, and thermal and electrical conductivity of the solder.
[0031] The solder alloy optionally contains up to 0.5 wt. % chromium, preferably 0.001-0.5 wt. % chromium, up to 0.5 wt. % manganese, preferably 0.001-0.5 wt. % manganese, more preferably 0.003-0.015 wt. % manganese, even more preferably 0.005-0.01 wt. % manganese, up to 0.5 wt. % iron, preferably 0.01-0.5 wt. % iron, more preferably 0.01-0.1 wt. % iron, even more preferably 0.015-0.035 wt. % iron. or 0.85-0.95% by weight iron, maximum 0.5% by weight phosphorus, preferably 0.001-0.5% by weight phosphorus, maximum 0.5% by weight gold, preferably 0.001-0.5% by weight gold, maximum 1% by weight gallium, preferably 0.01-0.9% by weight gallium, more preferably 0.2-0.8% by weight gallium, even more preferably 0.4-0.6% by weight gallium, maximum 0.5% by weight tellurium, preferably 0.001-0.5% by weight tellurium, maximum 0.5% by weight selenium, preferably 0. The alloys contain one or more of the following: 0.001-0.5% by weight selenium, up to 0.5% by weight calcium, preferably 0.001-0.5% by weight calcium, up to 0.5% by weight vanadium, preferably 0.001-0.5% by weight vanadium, up to 0.5% by weight molybdenum, preferably 0.001-0.5% by weight molybdenum, up to 0.5% by weight platinum, preferably 0.001-0.5% by weight platinum, and up to 0.5% by weight magnesium, preferably 0.001-0.5% by weight magnesium. Aluminum, calcium, gallium, germanium, magnesium, phosphorus, and vanadium can act as deoxidizers and can also improve wettability and solder joint strength. Other elemental additions such as gold, chromium, iron, manganese, molybdenum, platinum, selenium, and tellurium can act to improve strength and interface reactions. Aluminum in combination with silicon can act to improve the strength and reliability performance of the alloy. Germanium in combination with silicon can also improve the strength and reliability performance of the alloy.
[0032] The solder alloy is preferably selected from nickel, titanium, germanium, indium, manganese, rare earths, cobalt, aluminum, silicon, chromium, iron, phosphorus, gold, gallium, tellurium, selenium, calcium, vanadium, molybdenum, platinum, and magnesium, and preferably contains 1 to 3 elements, preferably 1 or 2 elements, more preferably 2 elements selected from nickel, titanium, germanium, indium, manganese, rare earths, cobalt, silicon, iron, and gallium. The solder alloy preferably comprises nickel and indium, or nickel and manganese, or nickel and germanium, or nickel, indium, and neodymium, or nickel and titanium, or nickel and cerium, or indium, or indium, titanium, and germanium, or nickel, or neodymium, or germanium, or silicon, or nickel and iron, or nickel and silicon, or nickel and cobalt, or cobalt and manganese, or manganese, or manganese and iron, or cobalt and germanium, or cobalt and titanium, or nickel and gallium, or indium and cobalt. Such alloys may exhibit favorable mechanical properties.
[0033] The solder alloy is preferably selected from nickel, titanium, germanium, indium, manganese, rare earths, cobalt, silicon, iron, and gallium, preferably comprising nickel and one of titanium, germanium, indium, manganese, rare earths, cobalt, aluminum, silicon, chromium, iron, phosphorus, gold, gallium, tellurium, selenium, calcium, vanadium, molybdenum, platinum, and magnesium, preferably one of titanium, germanium, manganese, cobalt, and indium, more preferably one of titanium, germanium, and manganese. Such alloys may exhibit favorable mechanical properties.
[0034] The weight percent of antimony is preferably greater than the weight percent of bismuth. Such alloys may exhibit favorable mechanical properties, particularly high strength. If the bismuth content is also controlled to not exceed about 4 weight percent, high strength may be combined with low brittleness.
[0035] The sum of the weight percent of antimony and the weight percent of bismuth is preferably 6.5 or more, more preferably 7.5 or more. This can increase the strength of the alloy. The sum of the weight percent of antimony and the weight percent of bismuth is preferably 12 or less, more preferably 11 or less. This can provide a low solidus-liquidus gap, typically about 14°C or less. This can also avoid the occurrence of undesirable high liquidus temperatures. For example, the sum of the weight percent of antimony and the weight percent of bismuth is preferably 6.5 to 12, more preferably 6.5 to 11, and even more preferably 7.5 to 10. Such an alloy can exhibit favorable mechanical properties. In particular, such an alloy can exhibit a favorable combination of high strength and a low solidus-liquidus temperature gap, typically less than about 14°C, and a desirable liquidus temperature. When the sum of the weight percent of antimony and the weight percent of bismuth is controlled to be the above amount, and at the same time the bismuth content is controlled not to exceed 4 wt%, particularly favorable mechanical properties can be obtained. The reasons are as follows. At room temperature, bismuth has a maximum solubility of about 4 wt.% in Sn, while antimony has a maximum solubility of 3 wt.%. Antimony contributes significant solid solution strengthening at least up to 150°C. If the maximum solubility of bismuth is not exceeded, a greater strength enhancing effect of antimony is obtained. A bismuth content of more than about 4 wt.% may not lead to a further increase in strength due to excess bismuth precipitates, and may also be detrimental to the mechanical behavior by increasing the brittleness of the alloy.
[0036] In a particularly preferred embodiment, the alloy comprises 2.5 to 4% by weight of silver; 2.8 to 4.2% by weight of bismuth, preferably 2.8 to 4% by weight of bismuth; 3.2 to 6.2 weight percent antimony; 0.4 to 0.8 weight percent copper; 0.04 to 0.18 weight percent nickel; 0.007 to 0.05 weight percent titanium, 0.001 to 0.02 weight percent germanium, and 0.005 to 0.01 weight percent manganese; the balance being tin, together with any unavoidable impurities; the weight percent of antimony is greater than the weight percent of bismuth; The sum of the weight percent of antimony and the weight percent of bismuth is 6.5 or more.
[0037] Such alloys may exhibit a particularly favorable combination of favorable mechanical properties, favorable solderability, excellent high temperature creep properties and excellent thermomechanical properties, and fatigue life, including those evaluated in thermal cycle or thermal shock tests covering a wide temperature range and long dwell times. In addition, such alloys are "cobalt-free," which may be advantageous in view of the high cost of cobalt and its toxicity.
[0038] In another particularly preferred embodiment, the solder alloy comprises 3 to 5% by weight of silver; 0.01 to 0.2 weight percent bismuth; 4 to 6 weight percent antimony; 0.3 to 1 weight percent copper; up to 6% by weight indium, Maximum 0.5% by weight titanium, up to 0.5% by weight germanium, Maximum 0.5% by weight rare earths, Maximum 0.5% by weight of cobalt, Maximum 5.0% by weight aluminum, Maximum 5.0% by weight silicon, Maximum 0.5% by weight manganese, Maximum 0.5% by weight chromium, maximum 0.5% by weight iron, maximum 0.5% by weight phosphorus; up to 0.5% gold by weight, up to 1% by weight of gallium, up to 0.5% by weight of tellurium, up to 0.5% by weight of selenium, Maximum 0.5% by weight calcium, maximum 0.5% by weight vanadium, Maximum 0.5% by weight of molybdenum, up to 0.5% by weight platinum, one or more of the following: manganese, up to 0.5% by weight; The balance being tin along with any unavoidable impurities.
[0039] Such alloys may exhibit a particularly favorable combination of favorable mechanical properties, favorable solderability, excellent high temperature creep properties and excellent thermomechanical properties, and fatigue life, including those evaluated in thermal cycle or thermal shock tests covering a wide temperature range and long dwell times. Such alloys may be "nickel-free," i.e., containing nickel at or below incidental impurity levels. This may be advantageous since nickel is toxic and prohibited in certain jurisdictions from use in consumer contact articles. The alloys may consist of the listed elements.
[0040] The solder alloy preferably exhibits a solidus-liquidus temperature gap of less than 16° C., preferably less than or equal to 14° C., and more preferably less than or equal to 12° C. A solidus-liquidus temperature gap that is too large can lead to soldering defects due to a mushy zone formed prior to complete solidification of the solder.
[0041] The solder alloy is preferably in the form of a bar, stick, solid or flux cored wire, foil or strip, film, preform, powder or paste (a blend of powder and flux), solder spheres for use in ball grid array joints, preformed solder pieces or reflowed or solidified solder joints, pre-applied to any solderable material such as copper ribbon for photovoltaic applications, or any type of printed circuit board.
[0042] The alloy typically contains at least 70% by weight tin, more typically at least 80% by weight tin, and even more typically at least 84% by weight tin.
[0043] It will be understood that the alloys described herein may contain unavoidable impurities, but that in total these are unlikely to exceed 1% by weight of the composition. Preferably, the solder alloy contains unavoidable impurities in an amount of 0.5% by weight or less of the composition, more preferably 0.3% by weight or less of the composition, even more preferably 0.1% by weight or less of the composition, even more preferably 0.05% by weight or less of the composition, and most preferably 0.02% by weight or less of the composition.
[0044] The solder alloys described herein may consist of the recited elements. Alternatively, the solder alloys described herein may consist essentially of the recited elements. Thus, in addition to those elements which are essential (i.e., tin, bismuth, antimony, and copper), it will be understood that other unspecified elements may be present in the composition, so long as the essential properties of the composition are not substantially affected by their presence in the composition.
[0045] The alloys of the present invention may be produced by mixing the corresponding pure elements or by mixing prefabricated alloys in any form factor and by using any manufacturing method, provided their final composition is covered by the specifications set forth herein.
[0046] In a preferred embodiment, the alloy consists of 2.8-3.2 wt.% silver, 2.8-3.2 wt.% bismuth, 4.5-5.5 wt.% antimony, 0.3-0.8 wt.% copper, 0.08-0.2 wt.% nickel, 0.001-0.01 wt.% germanium, and the balance tin along with unavoidable impurities. Such alloys may exhibit a particularly favorable combination of favorable mechanical properties, favorable solderability, excellent high temperature creep properties and excellent thermomechanical properties, and fatigue life, including those evaluated in thermal cycle or thermal shock tests covering a wide temperature range and long dwell times.
[0047] In a preferred embodiment, the solder alloy consists of 2.8-3.2 wt.% silver, 2.8-3.2 wt.% bismuth, 5.5-6.5 wt.% antimony, 0.3-0.8 wt.% copper, 0.08-0.2 wt.% nickel, 0.005-0.02 wt.% titanium, and the balance tin along with unavoidable impurities. Such alloys may exhibit a particularly favorable combination of favorable mechanical properties, favorable solderability, excellent high temperature creep properties and excellent thermomechanical properties, and fatigue life, including those evaluated in thermal cycle or thermal shock tests covering a wide temperature range and long dwell times.
[0048] In a preferred embodiment, the alloy consists of 3.1-3.7 wt.% silver, 3-3.5 wt.% bismuth, 3-3.8 wt.% antimony, 0.4-0.9 wt.% copper, 0.01-0.9 wt.% nickel, 0.001-0.01 wt.% germanium, and the balance tin together with unavoidable impurities.
[0049] In a preferred embodiment, the alloy consists of 3.2-3.9 wt.% silver, 3.5-4.5 wt.% bismuth, 5.5-6.5 wt.% antimony, 0.3-0.9 wt.% copper, 0.05-0.12 wt.% nickel, 0.001-0.01 wt.% manganese, and the balance tin along with unavoidable impurities. Such alloys may exhibit a particularly favorable combination of favorable mechanical properties, favorable solderability, excellent high temperature creep properties and excellent thermomechanical properties, and fatigue life, including those evaluated in thermal cycle or thermal shock tests covering a wide temperature range and long dwell times.
[0050] In a preferred embodiment, the alloy consists of 3.5-4.2 wt.% silver, 0.01-0.1 wt.% bismuth, 5-6 wt.% antimony, 0.4-0.9 wt.% copper, 0.001-0.01 wt.% germanium, 0.2-0.8 wt.% indium, 0.02-0.08 wt.% cobalt, and the balance tin along with unavoidable impurities. Such alloys may exhibit a particularly favorable combination of favorable mechanical properties, favorable solderability, excellent high temperature creep properties and excellent thermomechanical properties, and fatigue life, including those evaluated in thermal cycle or thermal shock tests covering a wide temperature range and long dwell times.
[0051] In a preferred embodiment, the alloy comprises 3-4 wt.% silver, 1-3 wt.% antimony, 2-4 wt.% bismuth, 0.3-1 wt.% copper, 0.1-0.25 wt.% nickel, 0.5-3.5 wt.% indium, and the balance tin along with unavoidable impurities. Such alloy has a melting temperature range of 202.8-217.9°C, which is lower than the near eutectic temperature of the conventional 96.5Sn3.0Ag0.5Cu alloy. Such alloy has a hardness and tensile strength that is approximately twice the order of magnitude of the hardness of 96.5Sn3.0Ag0.5Cu. The creep rupture time is 2.5 times that of 96.5Sn3.0Ag0.5Cu. In one specific example of this embodiment, the alloy comprises about 3% by weight silver, about 3.1% by weight bismuth, about 2.1% by weight antimony, about 0.8% by weight copper, about 0.25% by weight nickel, about 3.3% by weight indium, and the balance tin along with incidental impurities.
[0052] In a preferred embodiment, the alloy comprises 3-4.5% by weight silver, 1-3% by weight antimony, 2.5-4% by weight bismuth, 0.5-1.5% by weight copper, 0.1-0.25% by weight nickel, 0.5-1.5% by weight indium, and the balance tin along with incidental impurities. Such alloy has a melting temperature range of 209.7-223.5°C and a hardness that is approximately twice the magnitude of that of 96.5SnAg3.0Cu0.5. The creep rupture time of this alloy is 2.5 times that of 96.5Sn3.0Ag0.5Cu. In one specific example of this embodiment, the alloy comprises approximately 3% by weight silver, 3.1% by weight bismuth, 2.1% by weight antimony, 0.75% by weight copper, 0.2% by weight nickel, 1.2% by weight indium, and the balance tin along with incidental impurities.
[0053] In a preferred embodiment, the alloy comprises 3-4.5 wt.% silver, 2-4 wt.% bismuth, 3.5-6.5 wt.% antimony, 0.5-1.5 wt.% copper, 0.05-0.2 wt.% nickel, and the balance tin along with incidental impurities. Such alloy has a melting temperature range of 203.3-236.1°C, and a tensile strength and creep rupture time that are more than twice that of 96.5Sn3.0Ag0.5Cu. In one specific example of this embodiment, the alloy comprises approximately 3.6 wt.% silver, 3.9 wt.% bismuth, 4 wt.% antimony, 0.7 wt.% copper, 0.1 wt.% nickel, and the balance tin along with incidental impurities.
[0054] In a preferred embodiment, the alloy comprises 3-4% by weight silver, 3-4.5% by weight bismuth, 5-6.5% by weight antimony, 0.5-1% by weight copper, 0.05-0.2% by weight nickel, 0.001-0.01% by weight manganese, and the balance tin together with unavoidable impurities. In this preferred embodiment, the alloy preferably consists of 3.2-4% by weight silver, 3.5-4.5% by weight bismuth, 5.5-6.5% by weight antimony, 0.3-0.09% by weight copper, 0.05-0.12% by weight nickel, 0.001-0.01% by weight manganese, and the balance tin together with unavoidable impurities. Such alloys have a melting temperature range of 197.4-231.6°C. In one specific example of this embodiment, the alloy comprises about 3.5% by weight silver, 4.2% by weight bismuth, 6.1% by weight antimony, 0.7% by weight copper, 0.1% by weight nickel, 0.005% by weight manganese, and the balance tin along with incidental impurities.
[0055] In a preferred embodiment, the alloy comprises 3-4 wt.% silver, 3-4 wt.% bismuth, 3.5-4.5 wt.% antimony, 0.3-0.8 wt.% copper, 0.02-0.3 wt.% nickel, 0.001-0.002 wt.% germanium, and the balance tin along with incidental impurities. Such alloys have a melting temperature range of 211.4-225.5°C. Such alloys have more than twice the tensile strength and creep rupture time of 96.5Sn3.0Ag0.5Cu. In one specific example of this embodiment, the alloy comprises 3.2 wt.% silver, 3.4 wt.% bismuth, 0.5 wt.% copper, 3.9 wt.% antimony, 0.15 wt.% nickel, 0.001 wt.% germanium, and the balance tin along with incidental impurities.
[0056] In a preferred embodiment, the alloy comprises 3-4 wt.% silver, 2.5-3.5 wt.% bismuth, 4-5.5 wt.% antimony, 0.3-0.8 wt.% copper, 0.1-0.2 wt.% nickel, 0.001-0.002 wt.% germanium, and the balance tin along with unavoidable impurities. Such alloys have a melting temperature range of 215.2-228.3°C. Such alloys have tensile strengths more than twice that of 96.5Sn3.0Ag0.5Cu. The creep rupture time of such alloys is four times that of 96.5Sn3.0Ag0.5Cu. In one specific example of this embodiment, the alloy comprises, by weight, about 3.2% silver, 3% bismuth, 0.5% copper, 4.9% antimony, 0.15% nickel, 0.001% germanium, and the balance tin along with incidental impurities.
[0057] In a preferred embodiment, the alloy comprises 3-4% by weight silver, 3-4% by weight bismuth, 0.3-0.8% by weight copper, 3-4% by weight indium, 5.5-6.5% by weight antimony, 0.03-0.1% by weight nickel, 0-0.005% by weight of some rare earth element (preferably neodymium), and the balance tin along with unavoidable impurities. Such alloy has a melting temperature range of 186.9-232.9°C. Such alloy has more than three times the tensile strength and four times the creep strength of 96.5Sn3.0Ag0.5Cu. In one specific example of this embodiment, the alloy comprises 3.5% by weight silver, 3.7% by weight bismuth, 0.55% by weight copper, 3.4% by weight indium, 6.1% by weight antimony, 0.06% by weight nickel, 0.002% by weight neodymium, and the balance tin along with incidental impurities.
[0058] In a preferred embodiment, the alloy comprises 3-4 wt.% silver, 2.5-4 wt.% bismuth, 0.3-0.8 wt.% copper, 5-6.5 wt.% antimony, 0.1-0.2 wt.% nickel, 0.001-0.01 wt.% titanium, and the balance tin along with incidental impurities. Such alloys have a melting temperature range of 202.5-234.5°C. Such alloys have more than twice the tensile strength and more than six times the creep rupture time of 96.5Sn3.0Ag0.5Cu. In one specific example of this embodiment, the alloy comprises 3.2 silver, 3 bismuth, 0.5 wt.% copper, 5.9 antimony, 0.15 wt.% nickel, 0.006 wt.% titanium, and the balance tin along with incidental impurities.
[0059] In a preferred embodiment, the alloy comprises 3-4 wt.% silver, 3-4 wt.% bismuth, 0.5-1 wt.% copper, 1-2 wt.% indium, 5.5-6.5 wt.% antimony, 0.18-0.25 wt.% nickel, and the balance tin along with incidental impurities. Such alloys have a melting temperature range of 214.3-228.4°C. Such alloys have twice the tensile strength and four times the creep rupture time of 96.5Sn3.0Ag0.5Cu. In one specific example of such an embodiment, the alloy comprises approximately 3.1 wt.% silver, 3.1 wt.% bismuth, 0.7 wt.% copper, 1.15 wt.% indium, 6.1 wt.% antimony, 0.25 wt.% nickel, and the balance tin along with incidental impurities.
[0060] In a preferred embodiment, the alloy comprises 3-4 wt.% silver, 3-4 wt.% bismuth, 0.5-1 wt.% copper, 5.5-6.5 wt.% antimony, 0.2-0.3 wt.% nickel, and the balance tin along with incidental impurities. Such alloys have a melting temperature range of 214-230.4°C. Such alloys have twice the tensile strength and more than three times the creep strength of 96.5Sn3.0Ag0.5Cu. In one specific example of this embodiment, the alloy comprises approximately 3.5 wt.% silver, 3.5 wt.% bismuth, 0.7 wt.% copper, 6.2 wt.% antimony, 0.3 wt.% nickel, and the balance tin along with incidental impurities.
[0061] In a preferred embodiment, the alloy comprises 3-4 wt.% silver, 3-4 wt.% bismuth, 0.4-0.7 wt.% copper, 2.5-3.5 wt.% indium, 5.5-6.5 wt.% antimony, and the balance tin along with incidental impurities. Such alloys have a melting temperature range of 195.3-229.3°C. Such alloys have more than three times the tensile strength and more than four times the creep rupture time of 96.5Sn3.0Ag0.5Cu. In one specific example of this embodiment, the alloy comprises approximately 3.5 wt.% silver, 3.7 wt.% bismuth, 0.5 wt.% copper, 3.4 wt.% indium, 6.1 wt.% antimony, and the balance tin along with incidental impurities.
[0062] In a preferred embodiment, the alloy comprises 3-4 wt.% silver, 3-4 wt.% bismuth, 0.4-0.6 wt.% copper, 2.5-3.5 wt.% indium, 5.5-6.5 wt.% antimony, 0.001-0.01 wt.% titanium, 0.0008-0.002 wt.% germanium, and the balance tin along with unavoidable impurities. Such alloy has a melting temperature range of 186.5-232.5°C. Such alloy has three times the tensile strength and three times the creep rupture time of 96.5Sn3.0Ag0.5Cu. In one specific example of this embodiment, the alloy comprises approximately 3.5% by weight silver, 3.8% by weight bismuth, 0.5% by weight copper, 3.4% by weight indium, 6.1% by weight antimony, 0.006% by weight titanium, 0.001% by weight germanium, and the balance tin along with incidental impurities.
[0063] In a preferred embodiment, the alloy comprises 3-4 wt.% silver, 3-4 wt.% bismuth, 0.5-0.8 wt.% copper, 3-4 wt.% antimony, 0.05-0.1 wt.% nickel, 0.001-0.002 wt.% germanium, and the balance together with incidental impurities. Such alloys have a melting temperature range of 198.9-230.9°C. Such alloys have more than twice the tensile strength and three times the creep rupture strength of 96.5Sn3.0Ag0.5Cu. In one specific example of this embodiment, the alloy comprises approximately 3.6 wt.% silver, 3.9 wt.% bismuth, 0.7 wt.% copper, 3.9 wt.% antimony, 0.09 wt.% nickel, 0.001 wt.% germanium, and the balance together with incidental impurities, tin.
[0064] In a preferred embodiment, the alloy comprises 3-4 wt.% silver, 3-4 wt.% bismuth, 0.5-0.8 wt.% copper, 3-4 wt.% antimony, 0.03-0.08 wt.% nickel, 0.01-0.03 wt.% titanium, and the balance tin along with incidental impurities. Such alloys have a melting temperature range of 198.9-227.6°C. Such alloys have twice the tensile strength and more than three times the creep rupture time of 96.5Sn3.0Ag0.5Cu. In one specific example of this embodiment, the alloy comprises approximately 3 wt.% silver, 3.2 wt.% bismuth, 0.7 wt.% copper, 3.5 wt.% antimony, 0.06 wt.% nickel, 0.02 wt.% titanium, and the balance tin along with incidental impurities.
[0065] In a preferred embodiment, the alloy comprises 2.5-3.5% by weight silver, 2.5-3.5% by weight bismuth, 0.3-0.6% by weight copper, 5.5-6.5% by weight antimony, 0.01-0.04% by weight nickel, 0.01-0.03% by weight titanium, and the balance tin along with incidental impurities. Such alloys have a melting temperature range of 202.6-229.2°C. Such alloys have more than three times the tensile strength and more than six times the creep rupture strength of 96.5Sn3.0Ag0.5Cu. In one specific example of this embodiment, the alloy comprises approximately 3% by weight silver, 3.2% by weight bismuth, 0.5% by weight copper, 6.1% by weight antimony, 0.03% by weight nickel, 0.02% by weight titanium, and the balance tin along with incidental impurities.
[0066] In a preferred embodiment, the alloy comprises 2.5-3.5% by weight silver, 2.5-3.5% by weight bismuth, 0.3-0.6% by weight copper, 5.5-6.5% by weight antimony, 0.001-0.015% by weight nickel, 0.015-0.035% by weight titanium, and the balance tin along with incidental impurities. Such alloys have a melting temperature range of 203.3-229.7°C. Such alloys have more than three times the tensile strength and more than six times the creep rupture strength of 96.5Sn3.0Ag0.5Cu. In one specific example of this embodiment, the alloy comprises approximately 3% by weight silver, 3.2% by weight bismuth, 0.5% by weight copper, 6.1% by weight antimony, 0.01% by weight nickel, 0.03% by weight titanium, and the balance tin along with incidental impurities.
[0067] In a preferred embodiment, the alloy comprises 3-4% by weight silver, 3-4% by weight bismuth, 0.4-0.8% by weight copper, 3-4% by weight antimony, 0.03-0.05% by weight titanium, 0.005-0.01% by weight germanium, and the balance tin along with incidental impurities. Such alloys have a melting temperature range of 203.8-226.5°C. Such alloys have more than twice the tensile strength and four times the creep rupture strength of 96.5Sn3.0Ag0.5Cu. In one specific example of this embodiment, the alloy comprises approximately 3.4% by weight silver, 3.5% by weight bismuth, 0.7% by weight copper, 3.4% by weight antimony, 0.002% titanium, 0.007% germanium, and the balance tin along with incidental impurities.
[0068] In a preferred embodiment, the alloy comprises 3-4 wt% silver, 3-4 wt% bismuth, 0.5-0.8 wt% copper, 4.5-5.5 wt% antimony, 0.09-0.15 wt% nickel, 0.02-0.05 wt% titanium, 0.0008-0.0014 wt% germanium, and the balance tin along with incidental impurities. In one specific example of this embodiment, the alloy comprises approximately 3 wt% silver, 3.1 wt% bismuth, 0.7 wt% copper, 5.1 wt% antimony, 0.14 wt% nickel, 0.04 wt% titanium, 0.001 wt% germanium, and the balance tin along with incidental impurities.
[0069] In a preferred embodiment, the alloy comprises 3-4% by weight silver, 3-4% by weight bismuth, 0.5-0.8% by weight copper, 3-4% by weight antimony, 0.001-0.012% by weight neodymium, and the balance tin along with incidental impurities. Such alloys have a melting temperature range of 210.8-224.5°C. Such alloys have approximately four times the creep strength of 96.5Sn3.0Ag0.5Cu. In one specific example of this embodiment, the alloy comprises approximately 3.5% by weight silver, 3.1% by weight bismuth, 0.7% by weight copper, 3.8% by weight antimony, 0.005% by weight neodymium, and the balance tin along with incidental impurities.
[0070] In a preferred embodiment, the alloy comprises 3-4 wt.% silver, 3-4 wt.% bismuth, 3-4 wt.% antimony, 0.4-0.7 wt.% copper, 0.02-0.07 wt.% nickel, 0.001-0.005 wt.% germanium, and the balance tin along with incidental impurities. Such alloys have a melting temperature range of 202.9-224.6°C. Such alloys have 2.5 times the creep strength of 96.5Sn3.0Ag0.5Cu. In one such specific example of this embodiment, the alloy comprises approximately 3.5 wt.% silver, 4.16 wt.% bismuth, 3.9 wt.% antimony, 0.5 wt.% copper, 0.06 wt.% nickel, 0.001 wt.% germanium, and the balance tin along with incidental impurities.
[0071] In a preferred embodiment, the alloy comprises 3-4 wt.% silver, 3-4 wt.% bismuth, 4-6 wt.% antimony, 0.4-0.7 wt.% copper, 2.5-3.5 wt.% indium, and the balance tin along with incidental impurities. Such alloys have a melting temperature range of 195.8-228.6°C. Such alloys have twice the creep strength of 96.5Sn3.0Ag0.5Cu. In one specific example of this embodiment, the alloy comprises approximately 3.8 wt.% silver, 4.2 wt.% bismuth, 4.7 wt.% antimony, 0.5 wt.% copper, 3.2 wt.% indium, and the balance tin along with incidental impurities.
[0072] In a preferred embodiment, the alloy comprises 3-4 wt.% silver, 1-2 wt.% bismuth, 1-2 wt.% copper, 3-4 wt.% antimony, 0.008-0.02 wt.% aluminum, 0.005-0.01 wt.% silicon, and the balance tin along with incidental impurities. Such alloys have a melting temperature range of 217.52-227.05° C. In one specific example of this embodiment, the alloy comprises approximately 3.8 wt.% silver, 1.6 wt.% bismuth, 1.3 wt.% copper, 4 wt.% antimony, 0.015 wt.% aluminum, 0.007 wt.% silicon, and the balance tin along with incidental impurities.
[0073] In a preferred embodiment, the alloy comprises 3-4 wt.% silver, 3-4 wt.% bismuth, 3-4 wt.% antimony, 0.5-0.8 wt.% copper, 0.03-0.06 wt.% nickel, 0.001-0.008 wt.% germanium, and the balance tin along with incidental impurities. Such alloy has a melting temperature range of 212.8-224.5° C. In one specific example of this embodiment, the alloy comprises approximately 3.4 wt.% silver, 3.3 wt.% bismuth, 0.6 wt.% copper, 3.4 wt.% antimony, 0.05 wt.% nickel, and 0.001 wt.% germanium.
[0074] In a preferred embodiment, the alloy comprises 3-4 wt.% silver, 3.5-5 wt.% bismuth, 0.5-0.8 wt.% copper, 1-3 wt.% antimony, 0.1-0.2 wt.% nickel, 0.01-0.02 wt.% iron, and the balance tin along with any unavoidable impurities. Such alloys have a melting temperature range of 209.9-221.2°C. Such alloys have three times the creep strength of 96.5Sn3.0Ag0.5Cu. In one specific example of this embodiment, the alloy comprises approximately 3.4 wt.% silver, 4.1 wt.% bismuth, 0.7 wt.% copper, 2.1 wt.% antimony, 0.2 wt.% nickel, 0.02 wt.% iron, and the balance tin along with any unavoidable impurities.
[0075] In a preferred embodiment, the alloy comprises 3.5-4 wt.% silver, 0.02-1 wt.% bismuth, 0.5-0.7 wt.% copper, 0.1-1 wt.% indium, 4.5-6 wt.% antimony, 0.03-0.1 wt.% nickel, and the balance tin along with incidental impurities. Such alloys have a melting temperature range of 222.6-232.3°C. Such alloys have creep rupture strengths more than seven times that of 96.5Sn3.0Ag0.5Cu. In one specific example of this embodiment, the alloy comprises approximately 3.8 wt.% silver, 0.06 wt.% bismuth, 0.6 wt.% copper, 0.6 wt.% indium, 5.3 wt.% antimony, 0.06 wt.% nickel, and the balance tin along with incidental impurities.
[0076] In a preferred embodiment, the alloy comprises 3-4 wt.% silver, 2.8-3.8 wt.% bismuth, 0.5-0.8 wt.% copper, 3.5-4.5 wt.% antimony, 0.02-0.1 wt.% nickel, 0.01-0.025 wt.% silicon, and the balance tin along with incidental impurities. Such alloy has a melting temperature range of 214.4-225.6° C. In one specific example of this embodiment, the alloy comprises approximately 3.5 wt.% silver, 3.1 wt.% bismuth, 0.6 wt.% copper, 4.1 wt.% antimony, 0.03 wt.% nickel, 0.006 wt.% silicon, and the balance tin along with incidental impurities.
[0077] In a preferred embodiment, the alloy comprises 3-4 wt.% silver, 2.5-3.5 wt.% bismuth, 0.5-0.8 wt.% copper, 0.02-0.1 wt.% nickel, 0.01-0.03 wt.% iron, and the balance tin along with incidental impurities. Such alloy has a melting temperature range of 214.4-226.7° C. In one specific example of this embodiment, the alloy comprises approximately 3.6 wt.% silver, 3 wt.% bismuth, 0.6 wt.% copper, 3.9 wt.% antimony, 0.05 wt.% nickel, 0.03 wt.% iron, and the balance tin along with incidental impurities.
[0078] In a preferred embodiment, the alloy comprises 2.5-3.5% by weight silver, 2.5-3.5% by weight bismuth, 0.4-0.6% by weight copper, 5-6% by weight indium, 1-2% by weight antimony, 0.02-0.08% by weight nickel, and the balance tin along with incidental impurities. Such alloys have a melting temperature range of 195.1-211.8° C. In one specific example of this embodiment, the alloy comprises approximately 3% by weight silver, 3.2% by weight bismuth, 0.5% by weight copper, 6% by weight indium, 1.6% by weight antimony, 0.06% by weight nickel, and the balance tin along with incidental impurities.
[0079] In a preferred embodiment, the alloy comprises 3-4 wt.% silver, 3-4 wt.% bismuth, 0.5-0.7 wt.% copper, 3-4 wt.% antimony, 0.02-0.1 wt.% nickel, 0.02-0.08 wt.% cobalt, and the balance tin along with incidental impurities. Such alloys have a melting temperature range of 209.6-224.9° C. In one specific example of this embodiment, the alloy comprises approximately 3.4 wt.% silver, 3.6 wt.% bismuth, 0.6 wt.% copper, 3.6 wt.% antimony, 0.05 wt.% nickel, 0.06 wt.% cobalt, and the balance tin along with incidental impurities.
[0080] In a preferred embodiment, the alloy comprises 2.5-3.5% by weight silver, 3-4% by weight bismuth, 0.5-0.7% by weight copper, 3-4% by weight antimony, 0.03-0.1% by weight cobalt, 0.001-0.005% by weight manganese, and the balance tin along with incidental impurities. Such alloys have a melting temperature range of 210-225.3° C. In one specific example of this embodiment, the alloy comprises approximately 3% by weight silver, 3.6% by weight bismuth, 0.7% by weight copper, 3.9% by weight antimony, 0.05% by weight cobalt, 0.002% by weight manganese, and the balance tin along with incidental impurities.
[0081] In a preferred embodiment, the alloy comprises 3-4 wt.% silver, 3-4 wt.% bismuth, 0.5-0.7 wt.% copper, 3.5-4.5 wt.% antimony, and 0.002-0.01 wt.% manganese. Such alloy has a melting temperature range of 213.9-224.6° C. In one specific example of this embodiment, the alloy comprises approximately 3.5 wt.% silver, 3.1 wt.% bismuth, 0.7 wt.% copper, 4 wt.% antimony, 0.006 wt.% manganese, and the balance tin along with incidental impurities.
[0082] In a preferred embodiment, the alloy comprises 3-4 wt.% silver, 3-4 wt.% bismuth, 0.5-0.7 wt.% copper, 3.5-4.5 wt.% antimony, 0.001-0.005 wt.% manganese, 0.01-0.1 wt.% iron, and the balance tin along with incidental impurities. Such alloy has a melting temperature range of 214.7-224.6° C. In one specific example of this embodiment, the alloy comprises approximately 3.5 wt.% silver, 3.1 wt.% bismuth, 0.7 wt.% copper, 4 wt.% antimony, 0.003 wt.% manganese, 0.09 wt.% iron, and the balance tin along with incidental impurities.
[0083] In a preferred embodiment, the alloy comprises 3-4 wt.% silver, 3-4 wt.% bismuth, 0.5-0.7 wt.% copper, 3.5-4.5 wt.% antimony, 0.01-0.1 wt.% nickel, 0.01-0.1 wt.% cobalt, 0.005-0.015 wt.% germanium, and the balance tin along with incidental impurities. Such alloys have a melting temperature range of 215-225.7° C. In one specific example of this embodiment, the alloy comprises approximately 3.5 wt.% silver, 3.1 wt.% bismuth, 0.7 wt.% copper, 4 wt.% antimony, 0.05 wt.% nickel, 0.05 wt.% cobalt, 0.01 wt.% germanium, and the balance tin along with incidental impurities.
[0084] In a preferred embodiment, the alloy comprises 2.5-3.5% by weight silver, 3-4% by weight bismuth, 0.5-0.7% by weight copper, 4.5-5.5% by weight antimony, 0.02-0.07% by weight cobalt, 0.01-0.05% by weight titanium, and the balance tin along with incidental impurities. Such alloys have a melting temperature range of 213.8-228.5° C. In one specific example of this embodiment, the alloy comprises approximately 3% by weight silver, 3.1% by weight bismuth, 0.6% by weight copper, 5% by weight antimony, 0.06% by weight cobalt, 0.04% by weight titanium, and the balance tin along with incidental impurities.
[0085] In a preferred embodiment, the alloy comprises 3-4 wt.% silver, 0.02-0.1 wt.% bismuth, 0.5-0.7 wt.% copper, 4.5-5.5 wt.% antimony, 0.1-1 wt.% gallium, and the balance tin along with incidental impurities. Such alloy has a melting temperature range of 221.9-229.3° C. In one specific example of this embodiment, the alloy comprises approximately 3.7 wt.% silver, 0.08 wt.% bismuth, 0.6 wt.% copper, 5.2 wt.% antimony, 0.05 wt.% nickel, 0.5 wt.% gallium, and the balance tin along with incidental impurities.
[0086] In a preferred embodiment, the alloy comprises 3-4 wt.% silver, 0.01-0.1 wt.% bismuth, 0.5-0.7 wt.% copper, 0.4-0.7 wt.% indium, 4.5-5.5 wt.% antimony, 0.02-0.08 wt.% cobalt, and the balance tin along with incidental impurities. Such alloys have a melting temperature range of 221.6-229.7° C. In one specific example of this embodiment, the alloy comprises approximately 3.7 wt.% silver, 0.07 wt.% bismuth, 0.6 wt.% copper, 0.6 wt.% indium, 5.2 wt.% antimony, 0.06 wt.% cobalt, and the balance tin along with incidental impurities.
[0087] In a preferred embodiment, the alloy comprises 3-4 wt.% silver, 0.5-2 wt.% bismuth, 0.5-0.7 wt.% copper, 3.5-4.5 wt.% antimony, and the balance tin along with incidental impurities. Such alloys have a melting temperature range of 219.1-227.5° C. In one specific example of this embodiment, the alloy comprises approximately 3.7 wt.% silver, 1.1 wt.% bismuth, 0.6 wt.% copper, 4 wt.% antimony, and the balance tin along with incidental impurities.
[0088] In a preferred embodiment, the alloy comprises 3-4 wt.% silver, 2.5-3.5 wt.% bismuth, 0.5-0.7 wt.% copper, 3-4 wt.% antimony, and the balance tin along with incidental impurities. Such alloy has a melting temperature range of 216.2-226.9° C. In one specific example of this embodiment, the alloy comprises approximately 3.7 wt.% silver, 2.1 wt.% bismuth, 0.6 wt.% copper, 3.9 wt.% antimony, and the balance tin along with incidental impurities.
[0089] In a preferred embodiment, the alloy comprises 3-4% by weight silver, 3-4% by weight bismuth, 0.5-0.7% by weight copper, 3-4% by weight antimony, and the balance tin along with incidental impurities. Such alloy has a melting temperature range of 212.5-224.8° C. In one specific example of this embodiment, the alloy comprises approximately 3.8% by weight silver, 3.2% by weight bismuth, 0.7% by weight copper, 3.6% by weight antimony, and the balance tin along with incidental impurities.
[0090] In a preferred embodiment, the alloy comprises 3-4 wt.% silver, 3.5-4.5 wt.% bismuth, 0.5-0.7 wt.% copper, 3-4 wt.% antimony, and the balance tin along with incidental impurities. Such alloys have a melting temperature range of 210.7-223.9° C. In one specific example of this embodiment, the alloy comprises approximately 3.5 wt.% silver, 4 wt.% bismuth, 0.6 wt.% copper, 3.6 wt.% antimony, and the balance tin along with incidental impurities.
[0091] In a preferred embodiment, the alloy comprises 3-4 wt.% silver, 4.5-5.5 wt.% bismuth, 0.4-0.6 wt.% copper, 3-4 wt.% antimony, and the balance tin along with incidental impurities. Such alloys have a melting temperature range of 209.5-222.7° C. In one specific example of this embodiment, the alloy comprises approximately 3.1 wt.% silver, 5.1 wt.% bismuth, 0.5 wt.% copper, 3.7 wt.% antimony, and the balance tin along with incidental impurities.
[0092] In a preferred embodiment, the alloy comprises 3-4 wt.% silver, 5.5-6.5 wt.% bismuth, 0.4-0.7 wt.% copper, 3-4 wt.% antimony, and the balance tin along with incidental impurities. Such alloys have a melting temperature range of 206.2-220.8° C. In one specific example of this embodiment, the alloy comprises approximately 3.2 wt.% silver, 6 wt.% bismuth, 0.5 wt.% copper, 3.2 wt.% antimony, and the balance tin along with incidental impurities.
[0093] In a further aspect, the present invention provides a lead-free solder alloy comprising: (a) 2.5 to 5% by weight silver (b) 0.01 to 5% by weight of bismuth (c) 1.0 to 7.0% by weight of antimony (d) 0.01 to 2.0% by weight copper (e) At least one of the following elements: Maximum 0.5% nickel by weight Maximum 0.5% titanium by weight Up to 0.5% germanium by weight Maximum 5.0% indium by weight Maximum 0.5% manganese by weight Up to 0.5% by weight of rare earths such as neodymium, cerium, and lanthanum.
[0094] Maximum 5.0% aluminum by weight Maximum 5.0% silicon by weight (f) optionally, one or more of the following elements: 0-0.5% by weight chromium 0-0.5% by weight iron 0-0.5% by weight phosphorus 0-0.5% gold by weight 0-0.5% gallium by weight 0-0.5% by weight tellurium 0-0.5% by weight selenium 0-0.5% by weight calcium 0-0.5% vanadium by weight 0-0.5% by weight molybdenum 0-0.5% by weight platinum 0-0.5% by weight magnesium (g) providing a solder alloy comprising: a balance of tin, together with any incidental impurities.
[0095] The advantages and preferred features of the first aspect apply equally to this aspect.
[0096] In a further aspect, the present invention provides a soldered joint comprising the solder alloy described herein.
[0097] In a further aspect, the present invention provides a method for producing a composition comprising the steps of: A solder alloy as described herein; and a solder flux.
[0098] In a further aspect, the present invention provides a method of forming a solder joint, the method comprising: (i) providing two or more workpieces to be joined; (ii) providing a solder alloy as described herein or a solder paste as described herein; (iii) heating the solder alloy or solder paste adjacent the workpieces to be joined.
[0099] The workpieces may be components of printed circuit boards, such as substrates and dies.
[0100] In a further aspect, the present invention provides the use of a solder alloy as described herein or a solder paste as described herein in a soldering method.
[0101] The soldering method is preferably selected from wave soldering, Surface Mount Technology (SMT) soldering, die attach soldering, thermal interface soldering, hand soldering, laser and RF induction soldering, soldering to solar modules, soldering to level 2 LED package substrates, solder dip, and rework soldering.
[0102] In a further aspect, the present invention provides a method of making a solder alloy as described herein, comprising the steps of: Providing a list of elements; and melting the recited elements; The recited elements may be provided in the form of individual elements and / or in the form of one or more alloys containing one or more of the recited elements.
[0103] The invention will now be further described with reference to the following non-limiting examples.
[0104] Example 1 - Alloy 1 Alloy 1 contains 3 wt% silver, 3.1 wt% bismuth, 2.1 wt% antimony, 0.8 wt% copper, 3.3 wt% indium, 0.2 wt% nickel, and the balance tin along with unavoidable impurities. Alloy 1 has a melting temperature range of 202.8-217.9°C and a Vickers hardness of 28.6 Hv.
[0105] Example 1a - Alloy 1a (Reference Example) Alloy 1a contains, by weight, 3.8% silver, 3% bismuth, 1.4% antimony, 0.7% copper, 0.15% nickel, and the balance tin along with incidental impurities.
[0106] Example 1b - Alloy 1b (Reference Example) Alloy 1b contains 3.3% by weight silver, 3.2% by weight bismuth, 3% by weight antimony, 0.7% by weight copper, 0.04% by weight nickel, 0.01% by weight cobalt, and the balance tin along with incidental impurities.
[0107] Example 2 - Alloy 2 Alloy 2 contains 3 wt% silver, 3.1 wt% bismuth, 2.1 wt% antimony, 0.7 wt% copper, 0.2 wt% nickel, 1.2 wt% indium, and the balance tin along with unavoidable impurities. Alloy 2 has a melting temperature range of 209.7 to 223.5°C and a Vickers hardness of 27.2 Hv.
[0108] Example 3 - Alloy 3 Alloy 3 contains 3.6% by weight silver, 3.9% by weight bismuth, 0.7% by weight copper, 4% by weight antimony, 0.09% by weight nickel, 0.001% by weight manganese, and the balance tin along with incidental impurities. Alloy 3 has a melting temperature range of 203.3 to 236.1°C.
[0109] Example 4 - Alloy 4 Alloy 4 contains 3.5% by weight silver, 4.1% by weight bismuth, 6.1% by weight antimony, 0.7% by weight copper, 0.1% by weight nickel, 0.004% by weight manganese, and the balance tin along with incidental impurities. Alloy 4 has a melting temperature range of 197.4 to 231.6°C. A cross section of the as-cast microstructure of this alloy, shown in Figure 6, reveals the dispersion of Ag3Sn in the tin matrix. Larger precipitates of (Cu,Ni)6Sn5, and some fine precipitates of tin-bismuth intermetallic compounds are also observed. Such a microstructure is an example of solid solution strengthening and precipitation strengthening, which contributes to the alloy strengthening and its improved mechanical properties.
[0110] Example 7 - Alloy 7 Alloy 7 contains 3.2% by weight silver, 3.4% by weight bismuth, 0.5% by weight copper, 3.9% by weight antimony, 0.16% by weight nickel, 0.001% by weight germanium, and the balance tin along with any incidental impurities. The melting temperature range of this alloy is 211.4 to 225.5°C.
[0111] Example 8 - Alloy 8 Alloy 8 contains 3.2 wt% silver, 3 wt% bismuth, 0.5 wt% copper, 4.9 wt% antimony, 0.16 wt% nickel, 0.001 wt% germanium, and the balance tin along with any unavoidable impurities. The melting temperature range of this alloy is 215.2-228.3°C. The bulk microstructure of this alloy, shown in Figure 6, consists of a eutectic network of Ag3Sn along with Bi-Sn (white) and (Cu,Ni)6Sn5 precipitates (dark particles). Some of the (Cu,Ni)6Sn5 precipitates tend to form a petal-like structure. Such a morphology of the precipitates suggests that the alloy has improved mechanical properties, as shown in Figures 7, 8, and 9.
[0112] Example 9 - Alloy 9 Alloy 9 contains 3.5% by weight silver, 3.7% by weight bismuth, 0.5% by weight copper, 3.4% by weight indium, 6.1% by weight antimony, 0.06% by weight nickel, 0.002% by weight neodymium, and the balance tin along with incidental impurities. The melting temperature range of this alloy is 186.9 to 232.9°C.
[0113] Example 10 - Alloy 10 Alloy 10 contains 3.2 wt.% silver, 3 wt.% bismuth, 0.5 wt.% copper, 5.9 wt.% antimony, 0.16 wt.% nickel, 0.006 wt.% titanium, and the balance tin along with any unavoidable impurities. The bulk microstructure of this alloy consists of a well-dispersed eutectic network of Ag3Sn, Bi-Sn, and Cu6Sn5 precipitates. This alloy has a melting temperature range of 202.5-234.5°C.
[0114] Example 11 - Alloy 11 Alloy 11 contains 3.1% by weight silver, 3.1% by weight bismuth, 0.7% by weight copper, 1.1% by weight indium, 6.1% by weight antimony, 0.25% by weight nickel, and the balance tin along with any incidental impurities. Alloy 11 has a melting temperature range of 214.3 to 228.4°C. The hardness of this alloy is 32.4 Hv.
[0115] Example 12 - Alloy 12 Alloy 12 contains 3.5% by weight silver, 3.5% by weight bismuth, 0.7% by weight copper, 6.2% by weight antimony, 0.3% by weight nickel, 0.001% by weight cerium, and the balance tin along with incidental impurities. The melting temperature range of this alloy is 213.9-230.4°C. The hardness of this alloy is 28Hv.
[0116] Example 13 - Alloy 13 Alloy 13 contains 3.5% by weight silver, 3.7% by weight bismuth, 0.5% by weight copper, 3.4% by weight indium, 6.1% by weight antimony, and the balance tin along with incidental impurities. This alloy has a melting temperature range of 195.3 to 229.3°C.
[0117] Example 14 - Alloy 14 Alloy 14 contains 3.5% by weight silver, 3.8% by weight bismuth, 0.5% by weight copper, 3.4% by weight indium, 6.18% by weight antimony, 0.006% by weight titanium, 0.001% by weight germanium, and the balance tin along with any incidental impurities. The melting temperature range of this alloy is 186.5 to 232.5°C.
[0118] Example 15 - Alloy 15 Alloy 15 contains 3.6% by weight silver, 3.9% by weight bismuth, 0.7% by weight copper, 3.9% by weight antimony, 0.09% by weight nickel, 0.001% by weight germanium, and the balance tin along with any incidental impurities. The alloy has a melting temperature range of 198.9 to 230.9°C.
[0119] Example 16 - Alloy 16 (Reference Example) Alloy 16 contains, by weight, 3.5% silver, 3.2% bismuth, 0.7% copper, 3.2% antimony, 0.05% nickel, and the balance tin along with any incidental impurities.
[0120] Example 17 - Alloy 17 Alloy 17 contains 3 wt% silver, 3.2 wt% bismuth, 0.7 wt% copper, 3.5 wt% antimony, 0.06 wt% nickel, 0.02 wt% titanium, and the balance tin along with any unavoidable impurities. Alloy 17 has a melting temperature range of 198.9-227.6°C. The bulk microstructure of this alloy is shown in Figure 6. A fine network of Ag3Sn with well-dispersed (Cu,Ni)6Sn5 and bismuth-tin precipitates is clearly visible.
[0121] Example 18 - Alloy 18 Alloy 18 contains, by weight, 3% silver, 3.2% bismuth, 0.5% copper, 6.1% antimony, 0.03% nickel, 0.02% titanium, and the balance tin along with any incidental impurities.
[0122] Example 19 - Alloy 19 Alloy 19 contains 3 wt.% silver, 3.2 wt.% bismuth, 0.5 wt.% copper, 6.1 wt.% antimony, 0.01 wt.% nickel, 0.03 wt.% titanium, and the balance tin along with incidental impurities. The melting temperature range of Alloy 19 is 203.3-229.7°C.
[0123] Example 20 - Alloy 20 Alloy 20 contains 3.4% by weight silver, 3.4% by weight bismuth, 0.7% by weight copper, 3.4% by weight antimony, 0.002% by weight titanium, 0.007% by weight germanium, and the balance tin along with any incidental impurities. Alloy 20 has a melting temperature range of 203.8 to 226.5°C.
[0124] Example 21 - Alloy 21 Alloy 21 contains, by weight, 3% silver, 3.1% bismuth, 0.7% copper, 5.1% antimony, 0.14% nickel, 0.04% titanium, 0.001% germanium, and the balance tin along with any incidental impurities.
[0125] Example 22 - Alloy 22 Alloy 22 contains 3.5% by weight silver, 3.1% by weight bismuth, 0.7% by weight copper, 3.8% by weight antimony, 0.005% by weight neodymium, and the balance tin along with any incidental impurities. Alloy 22 has a melting temperature range of 210.8 to 224.5°C.
[0126] Example 23 - Alloy 23 Alloy 23 contains, by weight, 3.5% silver, 4.2% bismuth, 0.5% copper, 3.9% antimony, 0.06% nickel, 0.001% germanium, and the balance tin along with any incidental impurities.
[0127] Example 24 - Alloy 24 Alloy 24 contains 3.8% by weight silver, 4.2% by weight bismuth, 0.5% by weight copper, 3.2% by weight indium, 4.7% by weight antimony, and the balance tin along with any incidental impurities. Alloy 24 has a melting temperature range of 195.8 to 228.6°C.
[0128] Example 25 - Alloy 25 Alloy 25 contains 3.8% by weight silver, 4.2% by weight bismuth, 0.5% by weight copper, 3.3% by weight indium, 4.6% by weight antimony, 0.001% by weight germanium, and the balance tin along with optional incidental impurities. The melting temperature range of Alloy 25 is 194.5°C to 220.3°C.
[0129] Example 26 - Alloy 26 Alloy 26 contains 3.8% by weight silver, 1.6% by weight bismuth, 1.3% by weight copper, 4% by weight antimony, 0.015% by weight aluminum, 0.007% by weight silicon, and the balance tin along with any incidental impurities. The melting temperature range of Alloy 26 is 217.5-227.1°C.
[0130] Example 27 - Alloy 27 Alloy 27 contains 3.4% by weight silver, 3.3% by weight bismuth, 0.6% by weight copper, 3.4% by weight antimony, 0.05% by weight nickel, 0.001% by weight neodymium, and the balance tin along with any incidental impurities. The melting temperature range of this alloy is 212.8-224.5°C.
[0131] Example 28 - Alloy 29 Alloy 29 contains, by weight, 3.4% silver, 4.1% bismuth, 0.7% copper, 2.1% antimony, 0.2% nickel, 0.02% iron, and the balance tin along with incidental impurities.
[0132] Example 29 - Alloy 31 Alloy 31 contains 3.8% by weight silver, 0.06% by weight bismuth, 0.6% by weight copper, 0.6% by weight indium, 5.3% by weight antimony, 0.06% by weight nickel, and the balance tin along with incidental impurities. The alloy has a melting temperature range of 222.6 to 232.3°C. The creep strength of Alloy 31 is seven times that of 96.5Sn3.0Ag0.5Cu.
[0133] Example 30 - Alloy 32 Alloy 32 contains 3.5% by weight silver, 3.1% by weight bismuth, 0.6% by weight copper, 4.1% by weight antimony, 0.03% by weight nickel, 0.006% by weight silicon, and the balance tin along with incidental impurities. This alloy has a melting temperature range of 214.4 to 225.6°C.
[0134] Example 31 - Alloy 33 Alloy 33 contains 3.6% silver, 3% bismuth, 0.6% copper, 3.9% antimony, 0.05% nickel, 0.03% iron, and the balance tin along with incidental impurities. This alloy has a melting temperature range of 214.4 to 226.7°C.
[0135] Example 32 - Alloy 34 Alloy 34 contains 3% by weight silver, 3.2% by weight bismuth, 0.5% by weight copper, 6.3% by weight indium, 1.6% by weight antimony, 0.06% by weight nickel, and the balance tin along with incidental impurities. This alloy has a melting temperature range of 195.1 to 211.8°C.
[0136] Example 33 - Alloy 36 (Reference Example) Alloy 36 contains 3.8% by weight silver, 4% by weight bismuth, 0.7% by weight copper, 2% by weight antimony, 0.03% by weight nickel, and the balance tin along with incidental impurities. Alloy 36 has a melting temperature range of 208.9 to 221.9°C.
[0137] Example 34 - Alloy 37 Alloy 37 contains 3.4% silver, 3.6% bismuth, 0.6% copper, 3.6% antimony, 0.05% nickel, 0.06% cobalt, and the balance tin along with incidental impurities. The melting temperature range of this alloy is 209.6°C to 224.9°C.
[0138] Example 35 - Alloy 38 Alloy 38 contains 3% by weight silver, 3.6% by weight bismuth, 0.7% by weight copper, 3.9% by weight antimony, 0.05% by weight cobalt, 0.002% by weight manganese, and the balance tin along with incidental impurities. This alloy has a melting temperature range of 210-225.3°C.
[0139] Example 36 - Alloy 39 Alloy 39 contains 3.5% by weight silver, 3.1% by weight bismuth, 0.7% by weight copper, 4% by weight antimony, 0.006% by weight manganese, and the balance tin along with incidental impurities. Alloy 39 has a melting temperature range of 213.9 to 224.6°C.
[0140] Example 37 - Alloy 40 Alloy 40 contains 3.5% by weight silver, 3.1% by weight bismuth, 0.7% by weight copper, 4% by weight antimony, 0.003% by weight manganese, 0.09% by weight iron, and the balance tin along with incidental impurities. This alloy has a melting temperature range of 214.7 to 224.6°C.
[0141] Example 38 - Alloy 41 Alloy 41 contains 3.5% by weight silver, 3.1% by weight bismuth, 0.7% by weight copper, 4% by weight antimony, 0.05% by weight nickel, 0.05% by weight cobalt, 0.01% by weight germanium, and the balance tin along with incidental impurities. The melting temperature range of Alloy 41 is 215.0-225.7°C.
[0142] Example 39 - Alloy 42 Alloy 42 contains 3% by weight silver, 3.1% by weight bismuth, 0.6% by weight copper, 5% by weight antimony, 0.06% by weight cobalt, 0.04% by weight titanium, and the balance tin along with incidental impurities. This alloy has a melting temperature range of 213.8 to 228.5°C.
[0143] Example 40 - Alloy 43 Alloy 43 contains 3.7% by weight silver, 0.08% by weight bismuth, 0.6% by weight copper, 5.2% by weight antimony, 0.05% by weight nickel, 0.5% by weight gallium, and the balance tin along with incidental impurities. Alloy 43 has a melting temperature range of 221.9 to 229.3°C.
[0144] Example 41 - Alloy 45 Alloy 45 contains 3.7% by weight silver, 0.07% by weight bismuth, 0.6% by weight copper, 0.6% by weight indium, 5.2% by weight antimony, 0.06% by weight cobalt, and the balance tin along with incidental impurities. The melting temperature range of this alloy is 221.6 to 229.7°C.
[0145] Example 42 - Alloy 56 (Reference Example) Alloy 56 contains 3.7% by weight silver, 1.1% by weight bismuth, 0.6% by weight copper, 4% by weight antimony, and the balance tin along with incidental impurities. This alloy has a melting temperature range of 219.1 to 227.5° C. This alloy has a hardness of 27.7 Hv.
[0146] Example 43 - Alloy 57 (Reference Example) Alloy 57 contains 3.7% by weight silver, 2.1% by weight bismuth, 0.6% by weight copper, 3.9% by weight antimony, and the balance tin along with incidental impurities. The melting temperature range of this alloy is 216.2-226.9°C. The alloy has a hardness of 28.6 Hv.
[0147] Example 44 - Alloy 58 (Reference Example) Alloy 58 contains 3.8% by weight silver, 3.2% by weight bismuth, 0.7% by weight copper, 3.6% by weight antimony, and the balance tin along with incidental impurities. The alloy has a melting temperature range of 212.5 to 224.8°C. The hardness of the alloy is 30.8 Hv.
[0148] Example 45 - Alloy 59 (Reference Example) Alloy 59 contains, by weight, 3.5% silver, 4% bismuth, 0.6% copper, 3.6% antimony, and the balance tin along with incidental impurities. The alloy has a melting temperature range of 210.7-223.9°C and a hardness of 30.8 Hv.
[0149] Example 46 - Alloy 60 (Reference Example) Alloy 60 contains 3.1% by weight silver, 5.1% by weight bismuth, 0.5% by weight copper, 3.7% by weight antimony, and the balance tin along with incidental impurities. The melting temperature range of this alloy is 209.5-222.7°C, and the alloy has a hardness of 32.2 Hv.
[0150] Example 47 - Alloy 61 (Reference Example) Alloy 61 contains 3.2% by weight silver, 6% by weight bismuth, 0.5% by weight copper, 3.2% by weight antimony, and the balance tin along with incidental impurities. This alloy has a melting temperature range of 206.2 to 220.8°C and a hardness of 32.2 Hv.
[0151] A summary of the melting temperature ranges of all alloys is tabulated in Table 1.
[0152] [Table 1]
[0153] A micrograph of a solder alloy according to the present invention (Sn-5.3Sb-3.8Ag-0.06Bi-0.6Cu-0.6In-0.06Ni) is shown in Figure 1. As can be seen, the solder alloy exhibits a microstructure indicative of an extensive Ag3Sn network. As discussed above, such a distributed network of precipitate particles can enhance creep strength by resisting grain boundary migration during creep deformation.
[0154] As discussed above, reflow temperatures higher than 260°C may lead to various problems during soldering, such as damaging printed circuit boards and components. Figures 2 and 3 show the negative effect on the melting behavior of Sn-Ag-Cu alloys when excess antimony or bismuth is added. As shown in Figure 2, increasing the antimony content by 1-8 wt% increases the liquidus temperature significantly, while the solidus temperature increases gradually. In this example, if antimony is 7 wt% or less, the required reflow temperature would be 260°C or less, considering that the peak reflow temperature is 25-30°C above the liquidus temperature. The alloys covered by Figure 2 contain 3.2-3.8 wt% Ag, 1-8 wt% Sb, 0.5-0.9 wt% Cu, and the balance Sn. In Figure 3, antimony is kept at 3-4 wt% while increasing the bismuth content. The alloy of interest in FIG. 3 contains 3.2-3.8 wt.% Ag, 3-4 wt.% Sb, 1-6 wt.% Bi, 0.5-0.7 wt.% Cu, balance Sn. In this example, with 5 wt.% bismuth or less, its solidus temperature remains above 210°C and the solidus-liquidus temperature gap is less than 10°C. This is also important because a low solidus temperature may limit the operating temperature of the solder, and a too large solidus-liquidus temperature gap can lead to solder defects due to a semi-molten zone formed before the solder is fully solidified. As can be seen from FIG. 2 and FIG. 3, increasing antimony has a greater effect on increasing the liquidus temperature than the solidus temperature (FIG. 2). Reducing antimony and increasing bismuth reduces both the solidus and liquidus temperatures of the alloy (FIG. 3).
[0155] The solid solution strengthening and precipitation hardening caused by various alloying additions leads to an increase in hardness. For example, copper, which has a very limited solubility in tin, forms a Cu-Sn intermetallic compound that also increases the hardness of the alloy, whereas antimony contributes significantly to the solid solution strengthening. This effect is shown in Figure 4. Bismuth is also a known solid solution strengthening element of tin. The effect of increasing bismuth and slightly decreasing antimony on the hardness of the alloy is shown in Figure 5. Although increased hardness is often perceived as a negative and undesirable property of solder alloys due to the risk of increased brittleness, hardness can be turned into a desirable property by a balanced alloy design. In this way, hardness can contribute to the improved high thermomechanical properties of the alloys described herein.
[0156] Figure 6 shows, from left to right, the as-cast microstructures of alloys 4, 8, and 17. (Cu,Ni)6Sn5 precipitates are uniformly distributed in a matrix of Ag3Sn and Sn grains (containing Bi and Sb). The white precipitates are Bi-Sn intermetallic particles that form when the solubility limit of bismuth in tin is exceeded.
[0157] 7 and 8 compare the room temperature tensile properties of a number of exemplary alloys with that of 96.5Sn3.0Ag0.5Cu. There is a significant increase in tensile strength compared to 96.5Sn3.0Ag0.5Cu from 66% to 144%.
[0158] The results from the creep tests provide important insights into the resistance to creep and creep deformation (elastic and plastic) over relatively long periods of time. In the case of high temperature creep, the phenomenon of microstructural strengthening alternates with stress relaxation caused by annealing of the microstructure. The high temperature creep properties of the alloys are presented graphically and compared with those of 96.5Sn3.0Ag0.5Cu in Figures 9 and 10. The alloys of the present invention have significantly higher creep strength given by creep rupture time and total creep plastic strain. A higher creep rupture time indicates a higher resistance to creep. For example, at 150°C, the creep rupture time of alloy 8 is 255% higher than that of 96.5Sn3.0Ag0.5Cu.
[0159] The diffusion-dependent creep deformation depends on the homogeneous temperature, i.e., the ratio of the test temperature of the material to its melting temperature on an absolute scale. The homogeneous temperature of a solder alloy can be in the range of 0.84 to 0.86. Therefore, the melting temperature of a solder alloy does not have a significant effect on the mechanical properties.
[0160] Table 2 compares the zero wetting time (T0) of some of the exemplary alloys with 96.5Sn3.0Ag0.5Cu, which can be used as a measure of solderability and wettability. The wetting properties of the alloys according to the invention are comparable to those of the 96.5Sn3.0Ag0.5Cu alloy. This is important because the wetting properties of alloys with many alloying additions are quite often degraded. The wetting tests were performed at 250°C according to the JIS Z3198-4 standard.
[0161] [Table 2]
[0162] As discussed above, intermetallic compound formation due to alloying additions in these exemplary alloys provided additional strength to the bulk alloy and solder joints. Figures 11 and 12 show the results of thermal cycling performance testing. Thermal cycling was performed from -40 to 150°C with a 30 minute dwell time at each of these temperatures in tests conducted according to the IPC 9701A standard. Three important aspects of thermal cycling testing after soldering are the in situ characteristic life, the crack propagation in the solder joints, and the percentage of shear strength retained after thermal cycling testing. The thermal cycling characteristic life is given at 63.2% cumulative failure of BGA228 packages when their electrical resistance was monitored in situ using a high speed data logger. According to the IPC 9701A standard, failure is defined when there is a 20% increase in electrical resistance measured over five consecutive readings. Figure 11 shows an example of how the overall length of a solder joint is measured to calculate crack propagation for a BGA. Crack extension is measured as a percentage of the total length of the solder joint. For illustrative purposes, the crack shown here starts near the solder-IMC interface and extends the equivalent of 23% of the total length of the solder joint. Crack extension within each ball along the outermost row of solder joints in a BGA package is measured at the end of 2500 cycles. The average crack extension was measured for each alloy and is summarized in Table 3.
[0163] [Table 3]
[0164] The retained shear strength after 2000 hours of heat aging at 150°C is calculated as a fraction of the initial shear strength obtained from the soldered chip resistor. Table 4 shows the results for several of these alloys, where the remaining shear strength is at least 85% of the original solder joint shear strength.
[0165] [Table 4]
[0166] FIG. 12 shows the Weibull distribution plot of in situ monitored failures of BGA228 for a number of exemplary alloys according to the invention. All of the invented alloys have higher property life and a large number of remaining components. During thermal cycling, the alloys are subjected to thermal stresses that lead to creep deformation. Alloys that can resist creep deformation or accumulate large deformations before fracture are expected to have high thermal fatigue life. The higher creep strength of the invented alloys may result in higher thermal fatigue life.
[0167] The foregoing detailed description has been provided by way of illustration and description and is not intended to limit the scope of the appended claims. Many variations of the presently preferred embodiments described herein will be apparent to those of ordinary skill in the art and remain within the scope of the appended claims and their equivalents.
Claims
1. A lead-free solder alloy, 2.5 to 5 weight percent silver; 0.01 to 5 weight percent bismuth; 1 to 7 weight percent antimony; 0.01 to 2 weight percent copper; up to 6% by weight of indium, maximum 0.5% by weight of titanium, up to 0.5% by weight of germanium, up to 0.5% by weight of rare earths, maximum 0.5% by weight of cobalt, maximum 5.0% by weight of aluminum, up to 5.0 wt.% silicon, maximum 0.5% by weight of manganese, maximum 0.5% by weight of chromium, maximum 0.5% by weight of iron, maximum 0.5% by weight of phosphorus, maximum 0.5% by weight gold, up to 1% by weight of gallium, up to 0.5% by weight of tellurium, maximum 0.5% by weight of selenium, maximum 0.5% by weight of calcium, maximum 0.5% by weight of vanadium, maximum 0.5% by weight of molybdenum, 0.5% by weight maximum of platinum, and up to 0.5 wt.% magnesium; Optionally, up to 0.5 wt. % nickel; and and the balance tin along with any unavoidable impurities.
2. 2. The solder alloy of claim 1, comprising 2.8 to 4.5 wt. % silver, preferably 3 to 4 wt. % silver.
3. 3. A solder alloy according to claim 1 or claim 2 comprising 1.0 to 4.0 wt. % bismuth, preferably 2.0 to 4.0 wt. % bismuth, more preferably 2.5 to 4 wt. % bismuth, even more preferably 2.8 to 4 wt. % bismuth, and even more preferably 3 to 4 wt. % bismuth.
4. 4. A solder alloy according to any one of claims 1 to 3 comprising 1.0 to 6.5 wt.% antimony, preferably 2 to 6 wt.% antimony, more preferably 3 to 6 wt.% antimony, even more preferably 3.1 to 6 wt.% antimony, still even more preferably 3.2 to 6 wt.% antimony.
5. A solder alloy according to any one of the preceding claims, comprising 0.3 to 1.2 wt. % copper, preferably 0.4 to 0.8 wt. % copper.
6. A solder alloy according to any one of the preceding claims, comprising 0.001 to 0.4 wt. % nickel, preferably 0.01 to 0.3 wt. % nickel, more preferably 0.02 to 0.2 wt. % nickel.
7. A solder alloy according to any one of the preceding claims, comprising 0.001 to 5.5% by weight of indium, preferably 0.02 to 4% by weight of indium, more preferably 0.5 to 3% by weight of indium.
8. A solder alloy according to any one of the preceding claims, comprising 0.001 to 0.3 wt% titanium, preferably 0.005 to 0.2 wt% titanium, more preferably 0.007 to 0.05 wt% titanium.
9. A solder alloy according to any one of the preceding claims, comprising 0.001 to 0.3 wt% germanium, preferably 0.001 to 0.1 wt% germanium, more preferably 0.001 to 0.02 wt% germanium.
10. A solder alloy according to any one of the preceding claims, comprising 0.002 to 0.3 wt. % rare earths, preferably 0.003 to 0.05 wt. % rare earths.
11. A solder alloy according to any one of the preceding claims, comprising 0.01 to 0.2 wt. % cobalt, preferably 0.01 to 0.2 wt. % cobalt, more preferably 0.02 to 0.1 wt. % cobalt.
12. 12. A solder alloy according to any one of the preceding claims comprising 0.001 to 3 wt. % Aluminium, preferably 0.005 to 2 wt. % Aluminium, more preferably 0.01 to 1.5 wt. % Aluminium, even more preferably 0.015 to 1 wt. % Aluminium, still even more preferably 0.02 to 0.08 wt. % Aluminium.
13. 13. A solder alloy according to any one of the preceding claims comprising 0.001 to 3 wt.% silicon, preferably 0.005 to 2 wt.% silicon, more preferably 0.01 to 1.5 wt.% silicon, even more preferably 0.015 to 1 wt.% silicon, and even more preferably 0.02 to 0.08 wt.% silicon.
14. 0.001 to 0.5% by weight of chromium, 0.01 to 0.5% by weight of iron, 0.001 to 0.5 wt. % phosphorus, 0.001 to 0.5% by weight of gold, 0.2 to 0.8% by weight of gallium, 0.001 to 0.5 weight percent tellurium, 0.001 to 0.5% by weight of selenium, 0.001 to 0.5% by weight of calcium, 0.001 to 0.5% by weight of vanadium, 0.001 to 0.5% by weight of molybdenum, 0.001 to 0.5 weight percent platinum, and A solder alloy according to any one of the preceding claims, comprising one or more of the following by weight: 0.001 to 0.5% magnesium.
15. 15. The solder alloy according to any one of claims 1 to 14, comprising 1 to 3 elements, preferably 1 or 2 elements, more preferably 2 elements selected from nickel, titanium, germanium, indium, manganese, rare earths, cobalt, aluminium, silicon, chromium, iron, phosphorus, gold, gallium, tellurium, selenium, calcium, vanadium, molybdenum, platinum and magnesium, preferably selected from nickel, titanium, germanium, indium, manganese, rare earths, cobalt, silicon, iron and gallium.
16. 16. The solder alloy according to any one of the preceding claims, comprising nickel, preferably selected from nickel, titanium, germanium, indium, manganese, rare earths, cobalt, silicon, iron and gallium, and one of titanium, germanium, indium, manganese, rare earths, cobalt, aluminium, silicon, chromium, iron, phosphorus, gold, gallium, tellurium, selenium, calcium, vanadium, molybdenum, platinum and magnesium.
17. A solder alloy according to any preceding claim, wherein the weight percentage of antimony is greater than the weight percentage of bismuth.
18. 18. The solder alloy of claim 1, wherein the sum of the weight percent of antimony and the weight percent of bismuth is 6.5 or greater.
19. 2.5 to 4 weight percent silver; 2.8 to 4.2 weight percent bismuth; 3.2 to 6.2 weight percent antimony; 0.4 to 0.8 weight percent copper; 0.04 to 0.18 weight percent nickel; 0.007 to 0.05 weight percent titanium, 0.001 to 0.02 weight percent germanium, and 0.005 to 0.01 wt. % manganese; the balance being tin, together with any unavoidable impurities; the weight percent of said antimony is greater than the weight percent of said bismuth; 19. The solder alloy of claim 1, wherein the sum of the weight percent of antimony and the weight percent of bismuth is 6.5 or greater.
20. The solder alloy is 3-5% by weight silver; 0.01 to 0.2 weight percent bismuth; 4 to 6 weight percent antimony; 0.3 to 1 weight percent copper; up to 6% by weight of indium, maximum 0.5% by weight of titanium, up to 0.5% by weight of germanium, up to 0.5% by weight of rare earths, maximum 0.5% by weight of cobalt, maximum 5.0% by weight of aluminum, up to 5.0 wt.% silicon, maximum 0.5% by weight of manganese, maximum 0.5% by weight of chromium, maximum 0.5% by weight of iron, maximum 0.5% by weight of phosphorus; maximum 0.5% by weight gold, up to 1% by weight of gallium, up to 0.5% by weight of tellurium, maximum 0.5% by weight of selenium, maximum 0.5% by weight of calcium, maximum 0.5% by weight of vanadium, maximum 0.5% by weight of molybdenum, maximum 0.5% by weight of platinum, up to 0.5 wt.% magnesium; 10. The solder alloy of claim 1, comprising: a balance of tin along with any incidental impurities.
21. 2. The solder alloy of claim 1, wherein the alloy consists of 2.8-3.2 wt.% silver, 2.8-3.2 wt.% bismuth, 4.5-5.5 wt.% antimony, 0.3-0.8 wt.% copper, 0.08-0.2 wt.% nickel, 0.001-0.01 wt.% germanium, and the balance tin along with unavoidable impurities.
22. 2. The solder alloy of claim 1, wherein the alloy consists of 2.8-3.2 wt.% silver, 2.8-3.2 wt.% bismuth, 5.5-6.5 wt.% antimony, 0.3-0.8 wt.% copper, 0.08-0.2 wt.% nickel, 0.005-0.02 wt.% titanium, and the balance tin along with unavoidable impurities.
23. 2. The solder alloy of claim 1, wherein the alloy consists of 3.1-3.7 wt.% silver, 3-3.5 wt.% bismuth, 3-3.8 wt.% antimony, 0.4-0.9 wt.% copper, 0.01-0.9 wt.% nickel, 0.001-0.01 wt.% germanium, and the balance tin along with unavoidable impurities.
24. 13. The solder alloy of claim 1, wherein the alloy consists of 3.2-3.9 wt.% silver, 3.5-4.5 wt.% bismuth, 5.5-6.5 wt.% antimony, 0.3-0.9 wt.% copper, 0.05-0.12 wt.% nickel, 0.001-0.01 wt.% manganese, and the balance tin along with incidental impurities. (Alloy 4)
25. 2. The solder alloy of claim 1, wherein the alloy consists of 3.5-4.2 wt.% silver, 0.01-0.1 wt.% bismuth, 5-6 wt.% antimony, 0.4-0.9 wt.% copper, 0.001-0.01 wt.% germanium, 0.2-0.8 wt.% b indium, 0.02-0.08 wt.% cobalt, and the balance tin along with unavoidable impurities.
26. 26. The solder alloy of any one of claims 1 to 25 in the form of a bar, stick, solid wire or flux cored wire, foil or strip, film, preform, powder or paste (powder and flux blend), solder spheres for use in ball grid array joints, preformed solder pieces or reflowed or solidified solder joints, pre-applied to any solderable material such as copper ribbon for photovoltaic applications, or any type of printed circuit board.
27. A soldered joint comprising a solder alloy according to any one of the preceding claims.
28. A solder paste comprising: A solder alloy according to any one of claims 1 to 26, A solder paste comprising a solder flux and
29. 1. A method of forming a solder joint, comprising: (i) providing two or more workpieces to be joined; (ii) providing a solder alloy according to any one of claims 1 to 26 or a solder paste according to claim 28; (iii) heating the solder alloy or the solder paste adjacent the workpieces to be joined.
30. Use of a solder alloy according to any one of claims 1 to 26 or a solder paste according to claim 28 in a soldering process, preferably wherein the soldering process is selected from wave soldering, Surface Mount Technology (SMT) soldering, die attach soldering, thermal interface soldering, hand soldering, laser and RF induction soldering, soldering on solar modules, soldering on level 2 LED package substrates, solder dip and rework soldering.
31. A method for producing a solder alloy according to any one of claims 1 to 26, comprising the steps of: Providing the enumerated elements; and melting said listed elements; The method, wherein the recited elements may be provided in the form of individual elements and / or in the form of one or more alloys containing one or more of the recited elements.
Citation Information
Patent Citations
Lead-free solder alloy, electronic circuit board, and electronic control device
JP2016179498A
High Reliability Lead-Free Solder Alloy for Electronic Equipment Applications in Harsh Environments