Conductive resin composition and antistatic agent
A conductive resin composition with an aqueous urethane resin and conductive polymer addresses the need for improved conductivity in antistatic agents, achieving effective antistatic performance.
Patent Information
- Application Number
- JP2023064062
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-11
- Publication Date
- 2024-10-24
AI Technical Summary
Existing antistatic agents do not meet the increasing market demands for improved conductivity.
A conductive resin composition containing an aqueous urethane resin with specific polyol compounds and a conductive polymer, formulated to have an acid value within a specific range, is developed.
The composition achieves excellent conductivity, suitable for use as an antistatic agent.
Smart Images

Figure 2024150979000001 
Figure 2024150979000002 
Figure 2024150979000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an electroconductive resin composition and an antistatic agent. [Background technology]
[0002] Antistatic agents are widely used in films, semiconductors, trays for transporting electronic components, floors, and other applications because they can suppress the generation of static electricity.
[0003] Known antistatic agents include conductive compositions that contain a polymer having a polyester skeleton, a polysiloxane skeleton and / or a fluororesin skeleton, and a conductive polymer, in which the mass ratio of the polymer to the conductive polymer is 85 / 15 to 20 / 80 (see, for example, Patent Document 1). However, these antistatic agents do not satisfy the increasingly high requirements for electrical conductivity, and are insufficient for current market demands.
[0004] Therefore, there has been a demand for a material capable of forming an antistatic agent having excellent electrical conductivity. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2009-270047 A Summary of the Invention [Problem to be solved by the invention]
[0006] An object of the present invention is to provide a conductive resin composition capable of forming an antistatic agent having excellent conductive performance, and an antistatic agent comprising the conductive resin composition. [Means for solving the problem]
[0007] Means for Solving the Problems The present inventors have conducted intensive research to solve the above problems, and as a result have found that the above problems can be solved by using an aqueous urethane resin composition that uses a specific polyol compound as a raw material and includes a urethane resin having an acid value within a specific range, and a conductive resin composition that contains a conductive polymer, and have thus completed the present invention.
[0008] That is, the present invention relates to a conductive resin composition comprising an aqueous urethane resin composition (A) containing a urethane resin (a1) and an aqueous medium (a2), and a conductive polymer (B), wherein the urethane resin (a1) comprises, as essential raw materials, a polyol compound (a1-1) containing a polyether polyol, a polyisocyanate compound (a1-2), and a neutralizing agent (a1-3), and the acid value of the urethane resin (a1) is in the range of 20 to 60 mgKOH / g; and an antistatic agent comprising the conductive resin composition. Effect of the Invention
[0009] Since the conductive resin composition of the present invention has excellent electrical conductivity, it can be suitably used as an antistatic agent. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The conductive resin composition of the present invention is characterized by containing an aqueous urethane resin composition (A) and a conductive polymer (B).
[0011] The aqueous urethane resin composition (A) contains a urethane resin (a1) and an aqueous medium (a2). The urethane resin (a1) contains, as essential raw materials, a polyol compound (a1-1), a polyisocyanate compound (a1-2) and a neutralizing agent (a1-3).
[0012] As the polyol compound (a1-1), a polyether polyol is used as an essential component.
[0013] The polyether polyol may, for example, be one obtained by addition polymerization of an alkylene oxide using one or more compounds having two or more active hydrogen atoms as an initiator.
[0014] Examples of the initiator include ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, trimethylene glycol, 1,3-butanediol, 1,4-butanediol, 1,6-hexanediol, glycerin, trimethylolethane, and trimethylolpropane.
[0015] Examples of the alkylene oxide include ethylene oxide, propylene oxide, butylene oxide, styrene oxide, epichlorohydrin, and tetrahydrofuran.
[0016] Examples of the polyether polyol include polyoxytetramethylene glycol, polypropylene glycol, polyethylene glycol, etc. The number average molecular weight of the polyether polyol is preferably in the range of 1,000 to 3,000, since a conductive resin composition having excellent conductivity can be obtained.
[0017] As the polyol compound (a1-1), polyol compounds other than the polyether polyols can also be used, if necessary.
[0018] Examples of the other polyol compounds include polyester polyols, polyester ether polyols, polycarbonate polyols, etc. These polyol compounds can be used alone or in combination of two or more kinds.
[0019] Examples of the polyester polyol include those obtained by subjecting a polyvalent carboxylic acid and a polyhydric alcohol to an esterification reaction.
[0020] Examples of the polycarboxylic acid include aromatic dicarboxylic acids such as phthalic acid, terephthalic acid, isophthalic acid, and naphthalenedicarboxylic acid, and esters thereof, and aliphatic dicarboxylic acids such as succinic acid, glutaric acid, adipic acid, maleic acid, pimelic acid, suberic acid, azelaic acid, itaconic acid, sebacic acid, chlorendic acid, 1,2,4-butane-tricarboxylic acid, decanedicarboxylic acid, cyclohexanedicarboxylic acid, dimer acid, and fumaric acid, and esters thereof. These polycarboxylic acids and esters thereof can be used alone or in combination of two or more.
[0021] Examples of the polyhydric alcohol include aromatic diols such as benzene dimethanol, toluene dimethanol, and xylene dimethanol, and aliphatic polyols such as ethylene glycol, propylene glycol, 1,3-propylene diol, 1,4-butanediol, 1,6-hexanediol, 1,8-octanediol, diethylene glycol, triethylene glycol, cyclohexane-1,4-diol, cyclohexane-1,4-dimethanol, and neopentyl glycol ethylene glycol. These polyhydric alcohols can be used alone or in combination of two or more.
[0022] The polyester ether polyol may be, for example, a polyether polyol obtained by adding an alkylene oxide to an initiator and reacting with a polycarboxylic acid. The initiator may be the same as the initiator exemplified above, and the alkylene oxide may be the same as the alkylene oxide exemplified above. The polycarboxylic acid may be the same as the polycarboxylic acid exemplified above.
[0023] Examples of the polycarbonate polyol include those obtained by reacting a carbonate ester with a polyol, those obtained by reacting phosgene with bisphenol A, and the like. Examples of the carbonate ester include methyl carbonate, dimethyl carbonate, ethyl carbonate, diethyl carbonate, cyclocarbonate, and diphenyl carbonate. Examples of the polyol that can react with the carbonate ester include ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, dipropylene glycol, 1,4-butanediol, 1,3-butanediol, 1,2-butanediol, 2,3-butanediol, 1,5-pentanediol, 1,5-hexanediol, 2,5-hexanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, and 1,11-undecanediol. Examples of the polyether polyol include relatively low molecular weight dihydroxy compounds such as butyl ether, 1,12-dodecanediol, 3-methyl-1,5-pentanediol, 2-ethyl-1,3-hexanediol, 2-methyl-1,3-propanediol, 2-methyl-1,8-octanediol, 2-butyl-2-ethylpropanediol, 2-methyl-1,8-octanediol, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, hydroquinone, resorcin, bisphenol-A, bisphenol-F, and 4,4'-biphenol; polyether polyols such as polyethylene glycol, polypropylene glycol, and polytetramethylene glycol; and polyester polyols such as polyhexamethylene adipate, polyhexamethylene succinate, and polycaprolactone.
[0024] The content of the polyol compound (a1-1) in the raw material of the urethane resin (a1) is preferably in the range of 5 to 80 mass %, more preferably in the range of 10 to 70 mass %, since a conductive resin composition having excellent conductivity can be obtained.
[0025] Examples of the polyisocyanate compound (a1-2) include aromatic polyisocyanates such as phenylene diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, xylylene diisocyanate, naphthalene diisocyanate, polymethylene polyphenyl polyisocyanate, and carbodiimidized diphenylmethane polyisocyanate; aliphatic polyisocyanates such as hexamethylene diisocyanate, lysine diisocyanate, cyclohexane diisocyanate, isophorone diisocyanate, dicyclohexylmethane diisocyanate, xylylene diisocyanate, tetramethylxylylene diisocyanate, dimer acid diisocyanate, and norbornene diisocyanate; and alicyclic diisocyanates such as norbornane diisocyanate, isophorone diisocyanate, hydrogenated xylylene diisocyanate, and hydrogenated diphenylmethane diisocyanate. These polyisocyanate compounds can be used alone or in combination of two or more kinds.
[0026] The content of the polyisocyanate compound (a1-2) in the raw material of the urethane resin (a1) is preferably in the range of 10 to 60 mass %, more preferably in the range of 20 to 50 mass %, since a conductive resin composition having excellent conductivity can be obtained.
[0027] Examples of the neutralizing agent (a1-3) include alkali metal hydroxides such as sodium hydroxide and potassium hydroxide, and amine compounds such as triethylamine, ammonia, morpholine, monoethanolamine, diethylethanolamine, etc. These neutralizing agents can be used alone or in combination of two or more kinds.
[0028] The amount of the neutralizer (a1-3) used is preferably in the range of 0.5 to 15 mass % in the raw material of the urethane resin (A), and more preferably in the range of 1 to 10 mass %, since a conductive resin composition having excellent conductivity can be obtained.
[0029] As the urethane resin (a1), an acidic diol compound (a1-4) can also be used, if necessary.
[0030] Examples of the acidic diol compound (a1-4) include dimethylolalkanoic acids such as dimethylolpropionic acid and dimethylolbutanoic acid, N,N-bishydroxyethylglycine, N,N-bishydroxyethylalanine, 3,4-dihydroxybutanesulfonic acid, 3,6-dihydroxy-2-toluenesulfonic acid, etc. These acidic diol compounds can be used alone or in combination of two or more kinds.
[0031] The amount of the acidic diol compound (a1-4) used is preferably in the range of 1 to 20 mass % in the raw material of the urethane resin (A), and more preferably in the range of 3 to 15 mass %, since a conductive resin composition having excellent conductivity can be obtained.
[0032] In addition, a chain extender (a1-5) can also be used for the urethane resin (a1) as needed.
[0033] Examples of the chain extender (a1-5) include diamines such as ethylenediamine, 1,2-propanediamine, 1,6-hexamethylenediamine, piperazine, 2,5-dimethylpiperazine, isophoronediamine, 4,4'-dicyclohexylmethanediamine, 3,3'-dimethyl-4,4'-dicyclohexylmethanediamine, and 1,4-cyclohexanediamine; and amines having one primary amino group and one secondary amino group, such as N-hydroxymethylaminoethylamine, N-hydroxyethylaminoethylamine, N-hydroxypropylaminopropylamine, N-ethylaminoethylamine, and N-methylaminopropylamine. diamines containing the above; polyamines such as diethylenetriamine, dipropylenetriamine, and triethylenetetramine; hydrazines such as hydrazine, N,N'-dimethylhydrazine, and 1,6-hexamethylenebishydrazine; dihydrazides such as succinic acid dihydrazide, adipic acid dihydrazide, glutaric acid dihydrazide, sebacic acid dihydrazide, and isophthalic acid dihydrazide; semicarbazides such as β-semicarbazide propionic acid hydrazide, 3-semicarbazide-propyl-carbazic acid ester, and semicarbazide-3-semicarbazide methyl-3,5,5-trimethylcyclohexane. These chain extenders can be used alone or in combination of two or more.
[0034] The amount of the chain extender (a1-5) used is preferably in the range of 0.1 to 10 mass % in the raw material of the urethane resin (A), and more preferably in the range of 1 to 5 mass %, since a conductive resin composition having excellent conductivity can be obtained.
[0035] The acid value of the urethane resin (a1) is in the range of 20 to 60 mgKOH / g, and since a conductive resin composition having excellent conductivity can be obtained, the acid value is preferably in the range of 25 to 50 mgKOH / g, and more preferably in the range of 25 to 40 mgKOH / g.
[0036] The method for producing the urethane resin (a1) is not particularly limited, and any method may be used. For example, the urethane resin (a1) may be produced by reacting all of the reaction raw materials including the polyol compound (a1-1), the polyisocyanate compound (a1-2), and the neutralizing agent (a1-3) at once, or by reacting the reaction raw materials in sequence.
[0037] Examples of the aqueous medium (a2) include ion-exchanged water, distilled water, etc. These aqueous media can be used alone or in combination of two or more kinds.
[0038] The method for producing the aqueous urethane resin composition is not particularly limited, and any method may be used for producing the aqueous urethane resin composition, for example, a method of mixing the urethane resin (a1) and the aqueous medium (a2) to obtain the aqueous urethane resin composition.
[0039] Examples of the method for mixing the urethane resin (a1) and the aqueous medium (a2) include a method using a reaction vessel equipped with an agitating blade; a kneading machine such as a kneader, a continuous kneader, a taper roll, a single-screw extruder, a twin-screw extruder, a triple-screw extruder, a universal mixer, a plastomill, or a Bodeta-type kneader; a rotary dispersion mixer such as a homomixer, a static mixer, FILMICS, an Ebara Milder, a Clearmix, an Ultra-Turrax, a Cavitron, or a Biomixer; an ultrasonic dispersion device; or a device that has no moving parts and can mix by the flow of the fluid itself, such as an in-line mixer.
[0040] The mass ratio of the urethane resin (a1) to the aqueous medium (a2) [(a1) / (a2)] is preferably in the range of 50 / 50 to 80 / 20, and more preferably in the range of 50 / 50 to 70 / 30, since a conductive resin composition having excellent conductivity can be obtained.
[0041] The aqueous urethane resin composition (A) may contain other additives as required.
[0042] Examples of the other additives include surfactants, emulsifiers, thickeners, urethane catalysts, fillers, flame retardants, leveling agents, antiblocking agents, etc. These additives can be used alone or in combination of two or more kinds.
[0043] Examples of the surfactant include nonionic surfactants such as polyoxyethylene nonylphenyl ether, polyoxyethylene lauryl ether, polyoxyethylene styryl phenyl ether, polyoxyethylene sorbitol tetraoleate, and polyethylene-polypropylene copolymer; anionic surfactants such as fatty acid salts such as sodium oleate, alkyl sulfate ester salts, alkylbenzene sulfonates, alkyl sulfosuccinates, naphthalene sulfonates, polyoxyethylene alkyl sulfates, sodium alkanesulfonates, and sodium alkyl diphenyl ether sulfonates; and cationic surfactants such as alkylamine salts, alkyltrimethylammonium salts, and alkyldimethylbenzylammonium salts.
[0044] Examples of the emulsifier include nonionic emulsifiers such as polyoxyethylene nonylphenyl ether, polyoxyethylene lauryl ether, polyoxyethylene styrylphenyl ether, polyoxyethylene sorbitol tetraoleate, and polyethylene-polypropylene copolymer; anionic emulsifiers such as fatty acid salts such as sodium oleate, alkyl sulfate ester salts, alkylbenzene sulfonates, alkyl sulfosuccinates, naphthalene sulfonates, polyoxyethylene alkyl sulfates, sodium alkanesulfonates, and sodium alkyldiphenyl ether sulfonates; and cationic emulsifiers such as alkylamine salts, alkyltrimethylammonium salts, and alkyldimethylbenzylammonium salts. These emulsifiers can be used alone or in combination of two or more.
[0045] Examples of the thickener include association type and acid type thickeners.
[0046] Examples of the urethane-forming catalyst include organotin-based and bismuth-based catalysts.
[0047] Examples of the filler include calcium carbonate and silica.
[0048] Examples of the flame retardant include phosphorus-based flame retardants.
[0049] The leveling agent may be, for example, a silicon-based leveling agent.
[0050] Examples of the anti-blocking agent include acrylic agents and cellulose ester agents.
[0051] Examples of the conductive polymer (B) include poly(3,4-ethylenedioxythiophene):poly(styrenesulfonic acid) (hereinafter, sometimes referred to as "PEDOT:PSS"), carbon nanotubes, polyacetylene, polyaniline, polypyrrole, polythiophene, and ionic liquids.
[0052] The mass ratio [(A) / (B)] of the aqueous urethane resin composition (A) to the conductive polymer (B) per solid content is preferably in the range of 5 / 95 to 95 / 5, since a conductive resin composition having excellent conductivity can be obtained.
[0053] The method for producing the conductive resin composition of the present invention is not particularly limited, and any method may be used for producing the conductive resin composition. For example, a method of mixing the aqueous urethane resin composition (A) and the conductive polymer (B) may be used.
[0054] Examples of the method for mixing the aqueous urethane resin composition (A) and the conductive polymer (B) include a method using a reaction vessel equipped with an agitator; a kneader, a continuous kneader, a taper roll, a single-screw extruder, a twin-screw extruder, a triple-screw extruder, a universal mixer, a plastomill, a Bodeta-type kneader, or the like; a rotary dispersion mixer such as a homomixer, a static mixer, FILMICS, an Ebara Milder, a Clearmix, an Ultra-Turrax, a Cavitron, or a Biomixer; an ultrasonic dispersion device; or a device that has no moving parts and can mix by the flow of the fluid itself, such as an in-line mixer.
[0055] The conductive resin composition of the present invention may contain other additives as necessary.
[0056] Examples of the other additives include antioxidants, fillers, antioxidants, pigments, plasticizers, crosslinking agents, and surfactants.
[0057] Examples of the antioxidant include butylhydroxytoluene (BHT), butylhydroxyanisole (BHA), etc. These antioxidants can be used alone or in combination of two or more kinds.
[0058] The filler may be an organic or inorganic filler of various shapes. Specific examples include calcium carbonate, silica, etc. These fillers may be used alone or in combination of two or more.
[0059] Examples of the anti-aging agent include hindered phenol compounds.
[0060] Examples of the pigment include inorganic pigments such as titanium oxide, zinc oxide, ultramarine, red iron oxide, lithopone, lead, cadmium, iron, cobalt, aluminum, hydrochloride, and sulfate; and organic pigments such as azo pigments, phthalocyanine pigments, quinacridone pigments, quinacridonequinone pigments, dioxazine pigments, anthrapyrimidine pigments, anthanthrone pigments, indanthrone pigments, flavanthrone pigments, perylene pigments, perinone pigments, diketopyrrolopyrrole pigments, quinonaphthalone pigments, anthraquinone pigments, thioindigo pigments, benzimidazolone pigments, isoindoline pigments, and carbon black. These pigments can be used alone or in combination of two or more.
[0061] Examples of the plasticizer include dioctyl phthalate (DOP), dibutyl phthalate (DBP), dioctyl adipate, isodecyl succinate, diethylene glycol dibenzoate, pentaerythritol ester, butyl oleate, methyl acetylricinoleate, tricresyl phosphate, trioctyl phosphate, propylene glycol polyester adipate, butylene glycol polyester adipate, etc. These plasticizers can be used alone or in combination of two or more.
[0062] Examples of the crosslinking agent include melamine-based, oxazoline-based, epoxy-based, alkoxysilane-based compounds, etc. These crosslinking agents can be used alone or in combination of two or more kinds.
[0063] Examples of the surfactant include carboxylic acids such as coconut oil fatty acid amine salts and gum rosin, ester compounds such as castor oil sulfates, phosphate esters, alkyl ether sulfates, sorbitan fatty acid esters, sulfonates, and succinates, sulfonate compounds such as alkylarylsulfonate amine salts and dioctyl sodium sulfosuccinate, phosphate compounds such as sodium lauryl phosphate, and amide compounds such as coconut oil fatty acid ethanolamide. These surfactants can be used alone or in combination of two or more.
[0064] The antistatic agent of the present invention comprises the conductive resin composition. EXAMPLES
[0065] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to the examples given below.
[0066] (Synthesis Example 1: Synthesis of polyester polyol (1)) In a reaction vessel equipped with a thermometer, a nitrogen gas inlet tube, and a stirrer, 15 parts by mass of ethylene glycol, 25 parts by mass of neopentyl glycol, 25 parts by mass of terephthalic acid, 25 parts by mass of isophthalic acid, 10 parts by mass of adipic acid, and 0.1 parts by mass of dibutyltin oxide were charged while introducing nitrogen gas, and a polycondensation reaction was carried out at 230° C. until the acid value became 0.1 or less, to obtain a polyester polyol (1).
[0067] (Synthesis Example 2: Synthesis of polyester polyol (2)) Using the formulation shown in Table 1, a polyester polyol (2) was obtained in the same manner as in Synthesis Example 1.
[0068] The compositions of the polyester polyols (1) and (2) obtained in Synthesis Examples 1 and 2 are shown in Table 1.
[0069] [Table 1]
[0070] (Example 1: Preparation of aqueous urethane resin composition (1)) In a four-neck flask equipped with a thermometer, a stirrer, a reflux condenser and a nitrogen inlet tube, 61.5 parts by mass of polytetramethylene glycol ("PTMG2000" manufactured by Mitsubishi Chemical Corporation; number average molecular weight 2000), 7.3 parts by mass of dimethylolpropionic acid and 2.1 parts by mass of neopentyl glycol were added in the composition shown in Table 1 and thoroughly stirred. Then, 24.9 parts by mass of isophorone diisocyanate (hereinafter abbreviated as "IPDI") and 0.1 parts by mass of dibutyltin dilaurate as a catalyst were added and reacted at 75°C. After the reaction, MEK was added so that the solid concentration was 60% with MEK, and the mixture was stirred for 30 minutes and cooled to 40°C or less to obtain a urethane resin solution. Next, 2.7 parts by mass of potassium hydroxide as a neutralizing agent (1) was added to the obtained urethane resin solution to neutralize the acid group. Next, ion-exchanged water was added under vigorous stirring to a solid content of 20%, and the urethane was emulsified, after which 1.5 parts by mass of a chain extender (ethylenediamine) was added. After completion of the reaction, MEK was distilled off under reduced pressure to obtain an aqueous urethane resin composition (1) with a solid content of 25%.
[0071] (Examples 2 to 5: Preparation of aqueous urethane resin compositions (2) to (5)) Using the formulations shown in Table 2, the same procedures as in Example 1 were carried out to obtain aqueous urethane resin compositions (2) to (5).
[0072] (Comparative Examples 1 to 3: Preparation of Water-Based Urethane Resin Compositions (R1) to (R3)) Using the formulations shown in Table 2, the aqueous urethane resin compositions (R1) to (R3) were obtained in the same manner as in Example 1.
[0073] Table 2 shows the compositions of the aqueous urethane resin compositions (1) to (5) obtained in Examples 1 to 5 and the aqueous urethane resin compositions (R1) to (R3) obtained in Comparative Examples 1 to 3.
[0074] [Table 2]
[0075] In addition, "Excenol2020" in Table 2 refers to "Excenol2020" manufactured by AGC Inc.
[0076] "UH-200" in Table 2 refers to the "UH-200" manufactured by UBE Corporation.
[0077] (Examples 6 to 10: Preparation of conductive resin compositions) To 16.0 parts by mass of each of the aqueous urethane resin compositions obtained in Examples 1 to 5, 147.7 parts by mass of PEDOT:PSS (manufactured by Aldrich, 1.3 wt% dispersion in HO, conductive grade), 20 parts by mass of ethylene glycol, 10 parts by mass of ethanol, and 0.04 parts by mass of a surfactant ("Surfynol 440" manufactured by EVONIK) were added, and the mixture was diluted with 6.26 parts by mass of ion-exchanged water as an aqueous medium and thoroughly stirred to obtain conductive resin compositions (1) to (5).
[0078] (Comparative Examples 4 to 6: Preparation of Conductive Resin Compositions) Conductive resin compositions (R1) to (R3) were obtained in the same manner as in Examples 6 to 10, except that the aqueous urethane resin compositions obtained in Comparative Examples 1 to 3 were used, respectively.
[0079] The conductive resin compositions (1) to (5) and (R1) to (R3) obtained in the above Examples and Comparative Examples were used to carry out the following evaluations.
[0080] [Conductivity evaluation method] In the present invention, the electrical conductivity was evaluated by measuring the surface resistance, stretching resistance and haze.
[0081] [Evaluation method for surface resistance value] The antistatic agents each consisting of the conductive resin compositions (1) to (5) and (R1) to (R3) obtained in the above Examples and Comparative Examples were applied to a PET film (Lumirror 125T60 (manufactured by Toray Industries, Inc.) using a bar coater No. 4, and heat-treated at 120°C for 1 minute to obtain a film coated with the antistatic agent. The film coated with the antistatic agent was allowed to stand for half a day in an environment of 25°C and 50% RHM, and then the surface resistance was measured and evaluated according to the following criteria.
[0082] A: Surface resistance is 10 10 It was less than Ω / sq. B: Surface resistance is 10 10 Ω / sq. more than 10Ω 13 / sq. was less than that. C: Surface resistance is 10 13 It was more than Ω / sq.
[0083] [Evaluation method of extension resistance value] 115 parts by mass of each of the conductive resin compositions (1) to (5) and (R1) to (R3) obtained in the above Examples and Comparative Examples were poured into an A5 size mold, dried for 24 hours in an environment of 25° C., and then heat-treated for 1 minute at 120° C. to form a film. The film was then stretched to 300%, and the surface resistance of the film before and after stretching was measured. The change in stretching resistance was calculated using the following formula and evaluated according to the following criteria.
[0084] Stretching resistance value = Surface resistance value after stretching / Surface resistance value before stretching
[0085] A: The stretch resistance value was less than 100. B: The stretch resistance value was 100 or more and less than 1,000. C: The stretch resistance value was 1000 or more.
[0086] [Haze evaluation method] 115 parts by mass of each of the conductive resin compositions (1) to (5) and (R1) to (R3) obtained in the above Examples and Comparative Examples were poured into an A5 size mold, dried for 24 hours in an environment at 25° C., and then heat-treated for 1 minute at 120° C. to prepare a coating. The coating was stretched 300% and visually observed for the presence or absence of haze, and evaluated according to the following criteria.
[0087] A: No haze occurred at all. B: Some haze occurred. C: Haze occurred throughout the area.
[0088] The evaluation results of the conductive resin compositions (1) to (5) obtained in Examples 6 to 10 and the conductive resin compositions (R1) to (R3) obtained in Comparative Examples 4 to 6 are shown in Table 3.
[0089] [Table 3]
[0090] Examples 6 to 10 shown in Table 3 are examples of the conductive resin composition of the present invention. It was confirmed that these conductive resin compositions have excellent electrical conductivity.
[0091] On the other hand, Comparative Example 4 shown in Table 3 is an example of a conductive resin composition in which a urethane resin not using polyether polyol as a polyol compound and the acid value of the urethane resin is outside the range of 20 to 60 mgKOH / g. This conductive resin composition had extremely high surface resistance and stretching resistance, and haze occurred throughout the film, confirming that the conductive resin composition had poor conductivity.
[0092] Comparative Examples 5 and 6 are examples of conductive resin compositions using urethane resins without polyether polyol as the polyol compound. It was confirmed that these conductive resin compositions had significantly high stretch resistance and poor conductivity.
Claims
1. An aqueous urethane resin composition (A) containing a urethane resin (a1) and an aqueous medium (a2); A conductive resin composition comprising a conductive polymer (B), The urethane resin (a1) is made of a polyol compound (a1-1) containing a polyether polyol, a polyisocyanate compound (a1-2), and a neutralizing agent (a1-3) as essential raw materials, The conductive resin composition, wherein the acid value of the urethane resin (a1) is in the range of 20 to 60 mgKOH / g.
2. 2. The conductive resin composition according to claim 1, wherein the polyisocyanate compound (a2) contains an alicyclic diisocyanate.
3. 2. The conductive resin composition according to claim 1, wherein the neutralizing agent (a3) contains a hydroxide of an alkali metal.
4. 2. The conductive resin composition according to claim 1, wherein the urethane resin (a1) further contains an acidic diol compound (a1-4) as a raw material.
5. 2. The conductive resin composition according to claim 1, wherein the urethane resin (a1) further contains a chain extender (a1-5) as a raw material.
6. The conductive resin composition according to claim 1, wherein the conductive polymer (B) is at least one selected from the group consisting of poly(3,4-ethylenedioxythiophene), poly(styrenesulfonic acid), carbon nanotubes, polyacetylene, polyaniline, polypyrrole, polythiophene, and ionic liquids.
7. The conductive resin composition according to claim 1, wherein the mass ratio [(A) / (B)] of the aqueous urethane resin composition (A) to the conductive polymer (B) per solid content is in the range of 5 / 95 to 95 / 5.
8. An antistatic agent comprising the conductive resin composition according to any one of claims 1 to 7.
Citation Information
Patent Citations
Conductive composition, antistatic paint, and protective film using the conductive composition
JP2009270047A