Paper, gas barrier laminate, and package

The paper-based gas barrier laminate addresses poor interlayer adhesion in conventional laminates by using a polyfunctional vinyl resin in the clay coat layer and a matching binder in the anchor coat layer, ensuring robust gas barrier performance and recyclability.

JP2024151087APending Publication Date: 2024-10-24TOPPAN HOLDINGS INC
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023064220
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-11
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Conventional gas barrier laminates using paper face issues with poor adhesion at the interface between the clay coat layer and the anchor coat layer, leading to peeling and deterioration of barrier properties.

Method used

A paper-based gas barrier laminate structure comprising a paper base material, a clay coat layer with a polyfunctional vinyl resin containing divinylbenzene, an anchor coat layer, and a vapor deposition layer, optionally with an overcoat layer, where the binder resin of the clay coat and anchor coat layers are the same, enhancing interlayer adhesion.

Benefits of technology

The laminate structure improves adhesion between layers, thereby maintaining and enhancing gas barrier properties, allowing for reduced plastic use and improved recyclability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024151087000001_ABST
    Figure 2024151087000001_ABST
Patent Text Reader

Abstract

To provide paper, a gas barrier laminate and a package which can achieve improved barrier properties.SOLUTION: The barrier properties of a gas barrier laminate are improved by incorporating a component for improving the interlayer barrier between a clay coat layer and an anchor coat layer into a resin in the clay coat layer on a paper base material. The component contains a polyfunctional vinyl-based resin whose repeating units contain a polyfunctional vinyl monomer.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to paper, a gas barrier laminate, and a packaging material. [Background technology]

[0002] In many fields, such as food, beverages, pharmaceuticals, and chemicals, packaging materials are used according to the contents. Packaging materials are required to have gas barrier properties that prevent the permeation of oxygen and water vapor, which can cause deterioration of the contents.

[0003] In recent years, the momentum for eliminating plastic has been increasing due to growing environmental awareness triggered by the problem of marine plastic waste. From the viewpoint of reducing the amount of plastic materials used, the use of paper instead of plastic materials has been considered in various fields. For example, Patent Document 1 below discloses a gas barrier laminate in which a barrier layer is laminated on a paper support. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 6668576 Summary of the Invention [Problem to be solved by the invention]

[0005] Conventional materials using paper have a gas barrier laminate formed by using an adhesive with barrier properties in the deposition layer or anchor coat on the clay coat layer covering the paper base material, and thus exhibit barrier properties. However, in conventional gas barrier laminates, the adhesion at the interface between the clay coat layer and the anchor coat layer is poor, and peeling occurs at the interface. This causes a problem of deterioration of the barrier properties, and there is room for improvement.

[0006] The present invention has been made in consideration of the above-mentioned circumstances, and has an object to provide paper, a gas barrier laminate, and a package that can improve the barrier properties of packaging materials. [Means for solving the problem]

[0007] According to one aspect of the present invention, there is provided a paper comprising a paper base material and a clay coating layer present on the paper base material and containing a binder resin including a polyfunctional vinyl resin whose repeating units include a polyfunctional vinyl monomer.

[0008] According to another aspect of the invention, there is provided the paper according to the above aspect, wherein the polyfunctional vinyl monomer is divinylbenzene.

[0009] According to yet another aspect of the present invention, there is provided a gas barrier laminate comprising the paper according to any of the above aspects, and including the paper base material, the clay coating layer, the anchor coating layer, and a deposition layer laminated in this order.

[0010] According to yet another aspect of the present invention, there is provided a gas barrier laminate according to the above aspect, further comprising an overcoat layer on the vapor deposition layer.

[0011] According to yet another aspect of the present invention, there is provided the gas barrier laminate according to any one of the above aspects, wherein the binder resin of the clay coating layer and the material of the anchor coating layer are the same.

[0012] According to yet another aspect of the present invention, there is provided a package including the gas barrier laminate according to any one of the above aspects. Effect of the Invention

[0013] According to the present invention, by incorporating a component that improves the adhesion between the clay coat layer and the anchor coat layer into the resin in the clay coat layer of the paper, it is possible to provide paper, a gas barrier laminate, and a packaging material that can suppress the deterioration of barrier properties caused by poor adhesion. [Brief description of the drawings]

[0014] [Figure 1] 1 is a schematic cross-sectional view showing a gas barrier laminate according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings as needed. However, the present invention is not limited to the following embodiments.

[0016] <Gas barrier laminate> 1 is a schematic cross-sectional view showing a gas barrier laminate according to one embodiment. The gas barrier laminate 10 according to one embodiment comprises a paper substrate 1, a clay coat layer 2, an anchor coat layer 3, a deposition layer 4, and an overcoat layer 5. These members are laminated in this order to form the gas barrier laminate 10.

[0017] [Paper base material] The paper base material 1 is not particularly limited, and may be appropriately selected depending on the application of the packaging material to which the gas barrier laminate 10 is applied. There are no particular limitations on the paper as long as it is made mainly of plant-derived pulp. Specific examples of the paper base material 1 include bleached kraft paper, unbleached kraft paper, wood-free paper, paperboard, liner paper, coated paper, one-sided glazed paper, glassine paper, and Graphan (registered trademark) paper. The basis weight of the paper base material 1 is, for example, 20 g / m 2 ~500g / m 2 , 30g / m 2 ~100g / m 2 It may be.

[0018] [Clay court layer] By providing the clay coat layer 2 on the paper substrate 1, it is possible to prevent the diffusion of moisture and oil from the back side of the paper substrate and the penetration of the anchor coat layer into the paper substrate. In addition, the clay coat layer 2 can also play a role of filling the unevenness of the paper, and the provision of the clay coat layer 2 allows the anchor coat layer to be formed uniformly without defects. For example, various copolymers such as styrene-butadiene, styrene-acrylic, and ethylene-vinyl acetate, polyvinyl alcohol resins, etc. can be used as binder resins in the clay coat layer. In addition, the clay coat layer may contain clay, kaolin, calcium carbonate, talc, mica, etc. as fillers. The filler in the clay coat is preferably 50% by mass to 98% by mass.

[0019] In the present invention, in order to improve the barrier properties of the laminate of the paper base material and the clay coat layer thereon, at least a vinyl resin is used as the clay coat binder resin, and a polyfunctional vinyl resin containing a polyfunctional vinyl monomer such as divinylbenzene as a repeating unit is contained. The polyfunctional vinyl resin can improve the adhesion between the clay coat layer and the anchor coat layer provided thereon by the action of hydrogen bonding, high crosslinking, molecular rotation inhibition, stacking, etc. In addition, the mixing amount should be kept at 10 mol% or less because if the ratio of the monomer unit of the polyfunctional vinyl resin in the binder resin exceeds 10 mol%, the binder resin crosslinking proceeds and the viscosity becomes high, and it is preferable that the ratio is 0.1 mol% to 10 mol%. In addition, from the viewpoint of blocking effect on the paper surface, gloss, and printability, it is preferable to contain styrene monomer units at a ratio of 50 mol% to 95 mol%, and monomer units other than styrene and polyfunctional vinyl at a ratio of 5 mol% to 50 mol%, respectively.

[0020] The thickness of the clay coating layer is not particularly limited, but may be, for example, 1 μm to 10 μm, or 3 μm to 8 μm.

[0021] The mass proportion of paper is preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 80% by mass or more, based on the entire gas barrier laminate. If the mass proportion of paper is 50% by mass or more based on the entire gas barrier laminate, the amount of plastic material used can be sufficiently reduced, the gas barrier laminate as a whole can be said to be made of paper, and recyclability is excellent.

[0022] [Anchor coat layer] The anchor coat layer 3 is provided on the surface of the paper substrate to improve the adhesion between the paper substrate 1 and the deposition layer 4 described later, and to improve the gas barrier properties of the gas barrier laminate. The anchor coat layer 3 contains, for example, a first polyurethane having at least one selected from polyurethanes made of a polyol component and a polyisocyanate. Such an anchor coat layer 3 has excellent flexibility, and can suppress cracking of the deposition layer described later after bending (folding), and can improve the adhesion between the anchor coat layer and the deposition layer. Furthermore, by containing the above-mentioned polyurethane, it is possible to form a dense film due to the crystallinity and crosslinking of polyurethane. In addition, polyurethane is expected to form hydrogen bonds and couplings. Therefore, by containing polyurethane, a gas barrier laminate with excellent water vapor barrier properties can be obtained.

[0023] The anchor coat layer 3 also contains, for example, a first polyolefin having at least one selected from a carboxyl group, a salt of a carboxyl group, a carboxylic anhydride group, and a carboxylic acid ester. Such an anchor coat layer 3 has excellent flexibility, and can suppress cracking of the deposition layer described below after bending (folding), and can improve the adhesion between the anchor coat layer and the deposition layer. Furthermore, by containing the above-mentioned polyolefin, it is possible to form a dense film due to the crystallinity of the polyolefin. In addition, polyolefins also have few polar groups. Therefore, by containing polyolefins, a gas barrier laminate with excellent water vapor barrier properties can be obtained.

[0024] The anchor coat layer 3 may contain other components in addition to the first polyurethane or the first polyolefin, such as polyolefin, silane coupling agent, organic titanate, acrylic resin, polyester, polyurethane, polycarbonate, polyurea, polyamide, polyimide, melamine resin, and phenol resin.

[0025] The content of the first polyurethane or the first polyolefin in the anchor coat layer 3 may be, for example, 50% by mass or more, 70% by mass or more, 90% by mass or more, or 100% by mass.

[0026] Alternatively, the anchor coat layer 3 can be formed from the same material as the binder resin of the clay coat layer 2. By using the same material for the anchor coat layer 3 as the binder resin of the clay coat layer 2, the adhesion between the layers is further improved, and better gas barrier performance can be obtained.

[0027] The thickness of the anchor coat layer 3 may be, for example, 1 μm or more, 2 μm or more, 20 μm or less, 10 μm or less, or 5 μm or less. If the thickness of the anchor coat layer 3 is 1 μm or more, the unevenness of the paper base material described above can be efficiently filled, and the deposition layer described below can be laminated uniformly. Also, if the thickness of the anchor coat layer 3 is 20 μm or less, the deposition layer can be laminated uniformly while suppressing costs.

[0028] Examples of the solvent contained in the coating liquid of the anchor coat layer 3 include water, methyl alcohol, ethyl alcohol, isopropyl alcohol, n-propyl alcohol, n-butyl alcohol, n-pentyl alcohol, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, toluene, hexane, heptane, cyclohexane, acetone, methyl ethyl ketone, diethyl ether, dioxane, tetrahydrofuran, ethyl acetate, and butyl acetate. These solvents may be used alone or in combination of two or more. Among these, from the viewpoint of characteristics, methyl alcohol, ethyl alcohol, isopropyl alcohol, toluene, ethyl acetate, methyl ethyl ketone, and water are preferred. Furthermore, from the viewpoint of environmental load, methyl alcohol, ethyl alcohol, isopropyl alcohol, and water are preferred.

[0029] The anchor coat layer 3 can be provided by applying a coating liquid containing at least the first polyurethane, the first polyolefin, or the same binder resin and solvent as the clay coat layer 2 onto paper containing a paper substrate and a clay coat layer, and then drying the coating liquid. The smaller the average particle size of the first polyolefin in the coating liquid, the better from the viewpoint of smoothing the coating surface after drying, uniformly laminating the deposition layer, and improving the barrier properties. Specifically, it may be 1 μm or less, 0.7 μm or less, or 0.5 μm or less. The lower limit of the average particle size of the first polyolefin is not particularly limited, but may be, for example, 1 nm or more.

[0030] [Vapour-deposited layer] The deposition layer 4 is a layer formed by depositing a metal or an inorganic compound. The deposition layer may be one obtained by depositing aluminum, or aluminum oxide (AlO x ), silicon oxide (SiO x The subscript "x" indicates that the atomic ratio of Al or Si to O may deviate from the stoichiometric ratio.

[0031] The thickness of the deposited layer 4 may be appropriately set depending on the application, but is preferably 10 nm to 300 nm, and more preferably 30 nm to 100 nm. By setting the thickness of the deposited layer 4 to 10 nm or more, the continuity of the deposited layer 4 can be easily ensured, and by setting the thickness to 300 nm or less, the occurrence of curling or cracking can be sufficiently suppressed, and sufficient gas barrier performance and flexibility can be easily achieved.

[0032] From the viewpoint of oxygen gas barrier performance and film uniformity, it is preferable to form the deposition layer 4 by a vacuum deposition method. There are known deposition methods such as vacuum deposition, sputtering, and chemical vapor deposition (CVD), but vacuum deposition is preferred because of its fast deposition rate and high productivity. Among the vacuum deposition methods, deposition by electron beam heating is particularly effective because the deposition rate can be easily controlled by the irradiation area and electron beam current, and the temperature of the deposition material can be raised and lowered in a short time.

[0033] [Overcoat layer] The overcoat layer 5 is provided on the surface of the vapor-deposited layer 4 so as to be in contact with the vapor-deposited layer 4, and contains a second polyolefin having at least one selected from a carboxyl group, a salt of a carboxyl group, a carboxylic anhydride group, and a carboxylate ester. The overcoat layer 5 may be omitted.

[0034] Such an overcoat layer 5 has excellent flexibility, can suppress cracking of the deposition layer after bending (folding), and has excellent adhesion to the deposition layer. Furthermore, by including the above-mentioned second polyolefin, it is possible to form a dense film due to the crystallinity of the polyolefin. Furthermore, polyolefins also have few polar groups. Therefore, by including polyolefin, it is possible to obtain a gas barrier laminate with excellent water vapor barrier properties. Furthermore, by including the above-mentioned second polyolefin, the overcoat layer 5 can also function as a heat seal layer, so there is no need to provide a separate heat seal layer.

[0035] The overcoat layer 5 may contain other components in addition to the second polyolefin, such as a silane coupling agent, an organic titanate, an acrylic resin, a polyester, a polyurethane, a polycarbonate, a polyurea, a polyamide, a polyolefin emulsion, a polyimide, a melamine resin, a phenolic resin, and the like.

[0036] The content of the second polyolefin in the overcoat layer 5 may be, for example, 50% by mass or more, 70% by mass or more, 90% by mass or more, or 100% by mass.

[0037] The thickness of the overcoat layer 5 may be, for example, 0.05 μm or more, 0.5 μm or more, 1 μm or more, 20 μm or less, 10 μm or less, or 5 μm or less. If the thickness of the overcoat layer 5 is 0.05 μm or more, it can fully fulfill the role of the heat seal layer described above. Also, if the thickness of the overcoat layer 5 is 20 μm or less, it can fully fulfill the adhesiveness to the deposition layer and the barrier property while suppressing the cost.

[0038] Examples of the solvent contained in the coating liquid for the overcoat layer 5 include water, methyl alcohol, ethyl alcohol, isopropyl alcohol, n-propyl alcohol, n-butyl alcohol, n-pentyl alcohol, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, toluene, hexane, heptane, cyclohexane, acetone, methyl ethyl ketone, diethyl ether, dioxane, tetrahydrofuran, ethyl acetate, and butyl acetate. These solvents may be used alone or in combination of two or more. Among these, from the viewpoint of characteristics, methyl alcohol, ethyl alcohol, isopropyl alcohol, toluene, ethyl acetate, methyl ethyl ketone, and water are preferred. Also, from the viewpoint of environmental load, methyl alcohol, ethyl alcohol, isopropyl alcohol, and water are preferred. The overcoat layer 5 can be provided by applying a coating liquid containing the above-mentioned second polyolefin and a solvent on the deposition layer and drying it. The average particle size of the second polyolefin in the coating liquid is preferably as small as possible from the viewpoint of increasing the start-up temperature during heat sealing and preventing blocking during transport of the package. Although there are no particular limitations, specifically, it may be 1 μm or less, 0.7 μm or less, or 0.5 μm or less.

[0039] The first polyolefin and the second polyolefin contained in the anchor coat layer 3 and the overcoat layer 5, respectively, may be the same or different. Considering ease of production, it is preferable that the polyolefins in each layer are the same.

[0040] <Package> The gas barrier laminate according to the present embodiment can be used to produce a package in the form of a packaging bag, such as a gusset bag, a pillow bag, a three-side sealed bag, a standing pouch, etc. Alternatively, the gas barrier laminate can be used to produce a package in another form, such as a package including a container body and a lid.

[0041] The packaging body can be used as a packaging article that contains food, medicine, and the like. It is particularly suitable for containing food such as sweets. The packaging body according to the present embodiment can maintain high gas barrier properties. EXAMPLES

[0042] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0043] <Preparation of coated paper> A clay coating solution B was prepared using 20 parts by mass of dispersion A, which was prepared by adjusting the solid content to 40% by mass using a copolymer consisting of 82% by mass of styrene, 6% by mass of divinylbenzene, and 12% by mass of acrylic acid, water, and ammonia water, and 80 parts by mass of a dispersion prepared by dispersing kaolin in water so that the solid content was 80% by mass. Next, a non-coated paper (Conflex Glaze: 40 g / m 2 ) was coated with clay coating solution B on one side and dried to prepare coated paper C (55 g / m 2 ).

[0044] <Preparation of gas barrier laminate> Example 1 A urethane dispersion D consisting of a polyester polyol base agent (Kuraray Polyol P-530) and an isocyanate curing agent obtained by treating Takenate D-110NB with polyethylene glycol (PEG) was applied to the coated surface of the coated paper C using a bar coater, and dried in an oven to form an anchor coat layer. The thickness of the anchor coat layer was 1 μm. Subsequently, Al was vapor-deposited on the anchor coat layer. The thickness of the Al vapor-deposited layer was 50 nm. Then, a dispersion E containing a salt of a carboxyl group (product name: Chemipearl S100, ionomer type, particle size: <0.1 μm, solvent: water, isopropanol (IPA), manufactured by Mitsui Chemicals) was applied to the vapor-deposited layer using a bar coater, and dried in an oven to form an overcoat layer, thereby obtaining a gas barrier laminate. The thickness of the overcoat layer was 3 μm. The mass ratio of paper in the gas barrier laminate was about 85 mass%.

[0045] Example 2 A gas barrier laminate was obtained in the same manner as in Example 1, except that the anchor coat layer was formed using Dispersion E. The mass proportion of paper in the gas barrier laminate was approximately 85 mass %.

[0046] Example 3 A gas barrier laminate was obtained in the same manner as in Example 1, except that the anchor coat layer was formed using Dispersion A. The mass proportion of paper in the gas barrier laminate was approximately 85 mass %.

[0047] Comparative Example 1 The coated paper C used was clay coated paper (CanCoat: 60 g / m 2 A gas barrier laminate was obtained in the same manner as in Example 1, except that the clay coat binder was used (no polyfunctional vinyl monomer was used for the clay coat binder). The mass ratio of paper in the gas barrier laminate was about 85 mass %.

[0048] Comparative Example 2 The coated paper C used was clay coated paper (CanCoat: 60 g / m 2 A gas barrier laminate was obtained in the same manner as in Example 2, except that the clay coat binder was used (no polyfunctional vinyl monomer was used for the clay coat binder). The mass ratio of paper in the gas barrier laminate was about 85 mass %.

[0049] Comparative Example 3 Coated paper G was produced using dispersion F, which was prepared to a solid content of 40 mass% using a copolymer consisting of 88 mass% styrene and 12 mass% acrylic acid, water, and aqueous ammonia, instead of dispersion A, and a gas barrier laminate was obtained in the same manner as in Example 1, except that this coated paper G was used instead of coated paper C. The mass proportion of paper in the gas barrier laminate was approximately 85 mass%.

[0050] <Measurement of water vapor permeability> The water vapor permeability of the gas barrier laminates according to the examples and comparative examples was measured by the MOCON method. The measurement conditions were a temperature of 40° C. and a relative humidity of 90%. The results are shown in Table 1 in units of [g / m 2 ·day].

[0051] <Oxygen permeability measurement> The oxygen permeability of the gas barrier laminates according to the examples and comparative examples was measured according to JIS K7126:2006, Method B (isobaric method). The measurement was performed using an OX-TRAN 2 / 20 made by Modern Control at a temperature of 30°C and a relative humidity of 70%. The results are shown in Table 1 in units of [cc / m 2 / d / atm].

[0052] [Table 1] [Explanation of symbols]

[0053] Reference Signs List 1: paper substrate, 2: clay coating layer, 3: anchor coating layer, 4: vapor deposition layer, 5: overcoat layer, 10: gas barrier laminate.

Claims

1. Paper base material a clay coating layer on the paper base material, the clay coating layer including a binder resin including a vinyl resin having a repeating unit including a polyfunctional vinyl monomer; Paper containing.

2. The paper of claim 1 , wherein the multifunctional vinyl monomer is divinylbenzene.

3. The paper according to claim 1 or 2, A gas barrier laminate in which the paper base material, the clay coating layer, the anchor coating layer, and the vapor deposition layer are laminated in this order.

4. The gas barrier laminate according to claim 3 , further comprising an overcoat layer on the deposition layer.

5. The gas barrier laminate according to claim 3 , wherein the binder resin of the clay coating layer and the material of the anchor coating layer are the same.

6. A package comprising the gas barrier laminate according to claim 3.

Citation Information

Patent Citations

  • Gas barrier laminate

    JP6668576B1