Nonwoven fabric used for foam molded product reinforcement material, multilayer structure material including nonwoven fabric, foam molded product reinforcement material, and method for manufacturing nonwoven fabric used for foam molded product reinforcement material

A single-layer nonwoven fabric with specific properties, laminated and needle-punched short fibers, addresses the challenges of followability and formability in foamed molded products, ensuring effective foam shielding and noise reduction.

JP2024151528AInactive Publication Date: 2024-10-25AETEC-ALPHA CO LTD +2

Patent Information

Application Number
JP2023064944
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-12
Publication Date
2024-10-25
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing nonwoven fabrics used for reinforcing foamed molded products face issues such as reduced followability, poor formability, and difficulty in processing due to heat welding, leading to foam material seepage and generation of abnormal noise when contacting metal components.

Method used

A nonwoven fabric with a single-layer structure formed by laminating short fibers and bonded through needle punching, having a specific weight, thickness, and interlayer peel strength, which is heat-treated only on the surface to maintain flexibility and suppress foam material passage.

Benefits of technology

The solution provides excellent processability, foam shielding performance, and reduces abnormal noise generation by effectively preventing foam material exposure, while maintaining moldability and economic efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024151528000001_ABST
    Figure 2024151528000001_ABST
Patent Text Reader

Abstract

To provide a nonwoven fabric used for a foam molded product reinforcement material.SOLUTION: A nonwoven fabric used for a foam molded product reinforcement material 10 to be connected to a foam molding material in order to reinforce a foam molded product is a single layer material in which short fibers of webs laminated by folding and stacking webs formed of short fibers are mutually connected by needle-punch. The nonwoven fabric has thickness of 2 to 7.5 mm at load of 7 g / cm2, apparent density of 0.02 to 0.05 g / m2, and delamination strength of 0.05 to 2.45 N / cm. The delamination strength is a value of tensile force required to peel off connected webs from each other.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a nonwoven fabric used in a reinforcing material for a foam-molded product, a multilayer structure containing a nonwoven fabric, a reinforcing material for a foam-molded product, and a method for producing a nonwoven fabric used in a reinforcing material for a foam-molded product. [Background technology]

[0002] One example of a reinforcing material for foam molded products is a nonwoven fabric bonded to a urethane foam molded product (see, for example, Patent Documents 1 and 2). When manufacturing such a foam molded product, for example, a reinforcing material is set in a mold, a urethane foam material is supplied into the mold, and the mold is closed. Then, gas generated by the urethane foam passes through the gaps between the fibers of the nonwoven fabric, and the urethane foam is bonded to the reinforcing material.

[0003] An example of a reinforcing material is a seat pad used in a vehicle seat. The seat pad may be disposed at a position where it comes into contact with a metal part, such as a pipe frame or a spring. The reinforcing material is used to prevent the foam material from being damaged by a local force received from the metal part. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2012-82548 A [Patent Document 2] JP 2013-76179 A Summary of the Invention [Problem to be solved by the invention]

[0005] Patent Document 1 discloses that a nonwoven fabric processed by the needle punch method is partially heat-welded by the air-through method. When such partial heat-welding is performed, the conformability of the welded portion is reduced during molding, and the non-welded portion is stretched and thinned. This causes the foam material to seep out in a patchy manner in the thinned portion. If the seeped foam material is exposed on the surface of the molded product, friction will cause abnormal noise when the foam material comes into contact with a metal member, which is not preferable.

[0006] In order to suppress the generation of such abnormal noise, a multi-layer material in which multiple nonwoven fabric layers are laminated may be used. This is because the passage of the foaming material can be suppressed by including a dense nonwoven fabric, for example, manufactured by the spunbond method, as one of the nonwoven fabric layers. However, a multi-layer material including a dense layer generally has the problem of poor moldability.

[0007] For example, Patent Document 2 discloses a multilayer material in which a short fiber nonwoven fabric layer and a long fiber nonwoven fabric layer are laminated. In this multilayer material, the bulky and dense short fiber nonwoven fabric layer exhibits sound-damping and abrasion resistance as well as ease of deformation, while the long fiber nonwoven fabric layer has a dense part that exhibits a foam shielding function. However, such a multilayer material including a long fiber nonwoven fabric layer is inferior in conformity to a mold when processing such as deep drawing is performed.

[0008] Patent Document 1 discloses that after heat treatment by the air-through method, the nonwoven fabric is sandwiched between heated rollers or a Teflon (registered trademark)-coated net and compressed to a thickness of 2 mm or less. This causes the core-sheath type composite fibers that form the nonwoven fabric to be thermally bonded three-dimensionally. The nonwoven fabric that is thermally bonded in this way becomes hard, making it difficult to stretch and set in a mold. Therefore, such nonwoven fabrics have problems when processed into foam-molded products.

[0009] An object of the present disclosure is to provide a nonwoven fabric used as a reinforcing material for foam molded products, which has excellent processability and sufficient foam shielding performance, a reinforcing material for foam molded products, and a method for manufacturing a nonwoven fabric used as a reinforcing material for foam molded products. [Means for solving the problem]

[0010] According to one embodiment of the present disclosure, a nonwoven fabric used as a reinforcing material for a foam-molded product that is bonded to a foam-molded material in order to reinforce the foam-molded product is a single-layer material in which a web made of staple fibers is folded and laminated, and the staple fibers of the web are bonded to each other by needle punching. 2 The thickness under load is 2 to 7.5 mm, and the apparent density is 0.02 to 0.05 g / m 2 and the interlayer peel strength is 0.05 to 2.45 N / cm, and the interlayer peel strength is the value of the tensile force required to peel the bonded webs from each other. [Brief description of the drawings]

[0011] [Figure 1] FIG. 2 is a perspective view of a reinforcing material according to an embodiment. [Diagram 2] FIG. 2 is a plan view of the nonwoven fabric before it is formed into the reinforcement material of FIG. 1. [Diagram 3] 2 is a cross-sectional view illustrating a method for producing an expansion-molded product using the reinforcing material of FIG. 1. [Figure 4] FIG. 4 is a cross-sectional view of an expansion-molded product produced by the method of FIG. [Diagram 5] 3 is a flow diagram showing a method for producing the nonwoven fabric of FIG. 2. [Figure 6] FIG. 6 is a schematic diagram showing the lamination process of FIG. 5. [Figure 7] 6 is a schematic diagram illustrating the needle punching step and the heat treatment step in FIG. 5. FIG. [Figure 8] FIG. 8 is a side view of a needle used in the needle punching process of FIG. 7. [Figure 9] FIG. 2 is a perspective view of a molding device for molding the reinforcing member of FIG. 1. [Figure 10] 10 is a perspective view showing how a nonwoven fabric is placed on the molding device of FIG. 9. FIG. [Figure 11] 10 is a perspective view showing a state in which a nonwoven fabric is formed using the forming apparatus of FIG. [Figure 12]10 is a perspective view of a first auxiliary cover provided in the molding apparatus of FIG. 9. [Figure 13] FIG. 2 is a plan view of a test piece used to measure interlayer peel strength. [Figure 14] 14 is a schematic diagram showing a state in which the interlayer peel strength is measured using the test piece in FIG. 13. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] As shown in Fig. 1, a reinforcement material 10 for a foam-molded product according to one embodiment of the present disclosure is, for example, a seat pad for reinforcing a cushion material of an automobile seat. The cushion material is an example of a foam-molded product 19 (see Fig. 4). The foam-molded product 19 is not limited to a seat pad, and may be, for example, a cushion material of furniture.

[0013] The reinforcing material 10 may have a back portion 12 corresponding to the surface of the backrest, two side portions 13 extending from the left and right sides of the back portion 12 toward the front of the vehicle, and two through holes 14 corresponding to the attachment points of a headrest. The reinforcing material 10 is obtained, for example, by molding or sewing a nonwoven fabric 11 shown in Fig. 2. Molding can be performed by any method, such as press molding or vacuum molding.

[0014] As shown in Fig. 2, nonwoven fabric 11 is obtained by cutting nonwoven fabric sheet 33 (see Fig. 7) into a desired shape, for example, the shape of a backrest of an automobile seat. Nonwoven fabric 11 may have a central wrap-around portion 15 and two side wrap-around portions 16. Central wrap-around portion 15 is a portion that wraps around the back surface of back portion 12 during molding. Side wrap-around portions 16 are portions that wrap around the back surfaces of side portions 13 during molding.

[0015] The nonwoven fabric 11 of the present disclosure is a single layer material produced by a needle punch method. More specifically, a plurality of webs formed from staple fibers are overlapped, and the fibers of the layers are entangled with each other by the reciprocating motion of a metal needle to form a single layer material. The number of layers of the overlapped webs is, for example, seven layers, but is not limited to this and can be changed as desired. For example, the single layer material may be formed by folding the web 3 to 12 times.

[0016] The weight of the nonwoven fabric 11 is, for example, 50 to 500 g / m 2 Alternatively, 80 to 250 g / m 2 and 90 to 200 g / m 2 and 110 to 180 g / m 2 and 130 to 160 g / m 2 More specifically, 140 g / m 2 The apparent density of the nonwoven fabric 11 may be 0.02 to 0.05 g / m 2 and may be 0.025 to 0.045 g / m 2 and may be 0.03 to 0.04 g / m 2 may be also possible.

[0017] As shown in FIG. 3, the reinforcing material 10 may be molded using a mold 20. In this mold 20, the reinforcing material 10 may be joined to the foam molding material 18. The mold 20 may include an upper mold 21, a core mold 22, and a lower mold 23. The reinforcing material 10 is set, for example, so as to cover the core mold 22. Thereafter, a foaming material 17 containing a foaming agent, for example, urethane, is injected into the mold 20. This causes the foam molding material 18 to be foam molded. The reinforcing material 10 provides a gap for releasing gas from within the mold 20 during foam molding of the foam molding material 18.

[0018] As shown in Fig. 4, the foam molded product 19 may include a foam molded material 18 and a reinforcing material 10 bonded to the foam molded material 18. The reinforcing material 10 may be arranged so as to protect the surface of the foam molded material 18. The reinforcing material 10 may be arranged in a portion of the foam molded product 19 that comes into contact with a metal part, such as a pipe frame or a spring. The presence of the reinforcing material 10 suppresses abnormal noise caused by the foam molded material 18 rubbing against the metal part.

[0019] [Nonwoven fabric manufacturing method] FIG. 5 shows an example of a method for producing the nonwoven fabric 11. First, in a web forming process in step S11, a web 31 (see FIG. 6) is formed. The web 31 is formed by arranging short fibers, which are at least one of polyethylene terephthalate fibers and polypropylene fibers, by a machine or air flow.

[0020] The web 31 may contain 20% to 60% by weight of polyethylene terephthalate (PET) fibers and 40% to 80% by weight of polypropylene (PP) fibers. As an example, the web may contain 55% by weight of PP fibers and 45% by weight of PET fibers. Polypropylene (PP) has a smaller specific gravity than polyethylene terephthalate (PET). Therefore, by including PP, the number of fibers can be increased without increasing the weight. By increasing the number of fibers constituting the nonwoven fabric, the passage of the foaming material can be suppressed.

[0021] The PP fibers may be a mixture of fibers of different thicknesses. By using thin fibers, the number of fibers can be increased without changing the weight, so that the passage of the foaming material 17 can be suppressed. The PET fibers may have a core-sheath structure. This core-sheath structure may include a core and a sheath having a melting point lower than that of the core. The melting point of the sheath material may be, for example, about 110°C. The melting point of these fibers can be changed depending on the processing method, such as molding. By providing a core-sheath structure, the sheath melts when heated to bond the fibers together, while the core, which is difficult to melt, maintains the strength of the fibers.

[0022] The weight per layer of the web 31 is 10 to 30 g / m 2 is appropriate, but 15 to 25 g / m 2 The weight per layer of the web 31 may be 10 g / m 2 The lower it goes, the more difficult it becomes to function as a layer.

[0023] As shown in Fig. 6, in the lamination process of step S12, the web 31 is laminated into a plurality of layers, for example, seven layers, to form the laminated material 30. The number of folded layers of the web may be 3 to 12 layers, 5 to 11 layers, or 7 to 10 layers. The web 31 may be laminated by folding a continuously extending long web 31. The web 31 may be continuously laminated while transporting the laminated material 30 in the transport direction, so that the web 31 is continuously subjected to processing.

[0024] As shown in Fig. 7, in the needle punching process of step S13, the laminate 30 is repeatedly pierced with a plurality of needles 40 to perform needle punching. In the needle punching process, the punch density of the needle punch is set low so that the interlayer peel strength is 0.05 to 2.45 N / cm. The interlayer peel strength is the value of the tensile force required to peel the bonded webs 31 from each other. The method for measuring the interlayer peel strength will be described later.

[0025] As shown in FIG. 8, each needle 40 has a number of protrusions 41 . 7, the needle 40 repeatedly moves back and forth, penetrating the laminate 30 in the forward movement and being pulled out of the laminate 30 in the return movement. As the needle 40 moves back and forth, a plurality of protrusions 41 (see FIG. 8) catch the fibers, so that the fibers between the webs 31 become entangled, and the laminated webs 31 are bonded to each other to form a single layer material 32.

[0026] One or more support beds 45 and one or more moving devices 44 arranged opposite the support beds 45 may be arranged on the conveying path of the laminated material 30. Each moving device 44 may hold a plurality of needles 40. For example, two moving devices 44 may be arranged on the conveying path.

[0027] The needles 40 may be inserted from only one side of the laminate 30 transported on the support bed 45. A plurality of needle groups, for example, two needle groups 42 and 43, may be arranged on the transport path of the laminate 30. The needle groups 42 and 43 may be held by corresponding moving devices 44. The needle groups 42 and 43 may operate differently from each other. For example, the needle groups 42 and 43 may have different insertion depths or penetration numbers.

[0028] For example, the needle density (penetration number) of the first needle group 42 is set to 50 needles / cm 2 The needle density (penetration number) of the second needle group 43 is set to 75 needles / cm 2 Alternatively, the needle depth of the first needle group 42 may be 9 mm, and the needle depth of the second needle group 43 may be 3 mm. The needle depth is the length that the tip of the needle 40 passes through the support bed 45. If the needle depth is shallow, the number of protrusions 41 that pass through the web 31 is reduced. Therefore, the second needle group 43, which has a shallow needle depth, is less effective at entangling the fibers than the first needle group 42. The needle depth of the second needle group 43 may be shallow enough that the protrusions 41 do not catch the fibers. This reduces the effect of entangling the fibers.

[0029] In the heat treatment step shown in step S14, the calender roll 46 is used to 2Only the surface of the single layer material 32 is heat treated so that the thickness under load is 1 to 8 mm. The calender roll 46 may include rolls 47, 48 that sandwich the single layer material 32, and one or more heating devices 49 that heat the rolls 47, 48. The two heating devices 49 may be arranged to heat the rolls 47, 48, respectively. The surface temperature of the heating rolls 47, 48 is, for example, 130°C. The distance between the rolls 47, 48 is set so as not to crush the single layer material 32. The distance between the rolls 47, 48 is, for example, 4 mm. The transport speed of the single layer material 32 transported between the rolls 47, 48 is, for example, 5 m / min.

[0030] By subjecting the single layer material 32 to a heat treatment process, the single layer material 32 becomes a nonwoven fabric sheet 33. The nonwoven fabric sheet 33 includes a first surface 33a that has been heat treated, a second surface 33b opposite the first surface 33a that has been heat treated, and internal fibers 33c that are not heat treated and are located between the first surface 33a and the second surface 33b.

[0031] The purpose of the heat treatment is to remove the fluff from the surface of the single layer material 32, not to heat the internal fibers 33c. Therefore, the heating temperature, the distance between the rolls 47 and 48, and the conveying speed in the heat treatment step are set to 7 g / cm or less, so long as the heat treatment does not reach the inside of the single layer material 32. 2 The thickness of the nonwoven fabric 11 can be arbitrarily changed to 1 to 8 mm under load. 2 The thickness under load may be 2 to 7.5 mm, 2.5 to 6.5 mm, or 3 to 5.5 mm.

[0032] Through steps S11 to S14, nonwoven fabric sheet 33 is manufactured as a single layer material having an interlayer peel strength of 0.05 to 2.45 N / cm. Nonwoven fabric sheet 33 may be wound into a roll. The winding direction at this time is the same as the conveying direction during production. When nonwoven fabric sheet 33 is cut into a desired shape, nonwoven fabric 11 (see FIG. 2) is obtained. Nonwoven fabric 11 has substantially the same properties as nonwoven fabric sheet 33.

[0033] [Method of forming reinforcement material] An example of a method for producing the reinforcing material 10, particularly a method for molding the same, will be described below. The molding device 50 for the reinforcing material 10 shown in Fig. 9 includes, for example, a molding die 51, legs 53 and 54, a base 60, and an air supply / exhaust unit 61. The molding die 51 has an internal space and a plurality of air vents 51a communicating with the internal space. The molding die 51 may have two tube portions 52 at positions corresponding to the headrest. The molding die 51 may be supported on the base 60 via the air supply legs 53 and the exhaust legs 54.

[0034] Base 60 has therein an air supply passage 60a and an exhaust passage 60b. Air supply passage 60a and exhaust passage 60b may communicate with the internal space of molding die 51 through air supply leg portion 53 and exhaust leg portion 54, respectively. Air supply passage 60a and exhaust passage 60b may communicate with air supply and exhaust unit 61 through air supply pipe 62 and exhaust pipe 63, respectively. Air supply and exhaust unit 61 may be configured to supply heated steam or heated air through air supply pipe 62. Air supply and exhaust unit 61 may also be configured to take in air through exhaust pipe 63.

[0035] In the covering step shown in FIG. 10, the nonwoven fabric 11 to be molded is covered on a mold 51 . 11, the molding apparatus 50 may further include a cover material 64, a first auxiliary cover 70, and two second auxiliary covers 56. The first auxiliary cover 70 may be disposed between the air supply leg portion 53 and the air exhaust leg portion 54.

[0036] As shown in FIG. 12, the first auxiliary cover 70 includes two cover bodies 71, four magnets 72, and a connecting bar 73. The connecting bar 73 connects the two cover bodies 71. Each cover body 71 has an edge region 71a curved to fit along the lower end of the mold 51. Two magnets 72 are attached to each cover body 71 so as to face each other. A magnet (not shown) may be disposed in the lower end region of the mold 51. The first auxiliary cover 70 may be fixed to the mold 51 by the magnets 72 in the first auxiliary cover fixing step so as to fix the lower end of the nonwoven fabric 11 covering the mold 51 to the mold 51.

[0037] 11 , in the second auxiliary cover fixing step, the two second auxiliary covers 56 are fixed to the sides of the forming die 51 by fasteners (not shown), such as magnets or screws, so as to press the sides 13 of the nonwoven fabric 11. Furthermore, the nonwoven fabric 11 may be fixed to the forming die 51 by a plurality of strings 58. In the space forming step, the cover material 64 forms a closed space 65 by having its edge fixed to the base 60 while covering the forming die 51. At this time, the auxiliary covers 56, 70 are disposed in the closed space 65.

[0038] After the space forming step, in the air supply step or heating step, the air supply and exhaust unit 61 supplies heated steam or heated air to the inside of the mold 51 through the air supply pipe 62, the air supply path 60a, the air supply leg portion 53, and the air vent 51a. This heats the nonwoven fabric 11 and the mold 51. At this time, the supplied heated steam causes the cover material 64 to expand.

[0039] Then, in the exhaust step, the supply and exhaust unit 61 exhausts air from the closed space 65 by sucking through the exhaust pipe 63, the exhaust path 60b, the exhaust leg portion 54, and the ventilation hole 51a. This causes the inflated covering material 64 to contract as if being drawn into the forming die 51. As a result, the nonwoven fabric 11, which has been heated and has high plasticity, adheres closely to the forming die 51 and is formed into a shape that matches the outer shape of the forming die 51. The reinforcing material 10 shown in FIG. 1 is formed by the molding method including the covering step, the first auxiliary cover fixing step, the second auxiliary cover fixing step, the space forming step, the air supply step (heating step), and the exhaust step.

[0040] The covered portion of the nonwoven fabric 11 covered with the auxiliary covers 56, 70 is not only less likely to be heated, but is also not pressed against the mold 51 by the cover material 64. Therefore, this covered portion has a lower rigidity and is softer than the other portions. That is, the reinforcing material 10 has a first portion (the portion not covered with the auxiliary covers 56, 70) having a first rigidity, and a second portion (the portion covered with the auxiliary covers 56, 70) having a second rigidity lower than the first rigidity. By arranging the second portion in a location of the foam-molded product 19 where abnormal noise is likely to occur, the generation of abnormal noise can be suppressed.

[0041] The molding device 50 does not have to include at least one of the first auxiliary cover 70 and the second auxiliary cover 56. In other words, the molding method of the reinforcing material 10 does not have to include at least one of the first auxiliary cover fixing step and the second auxiliary cover fixing step.

[0042] [Method for measuring interlayer peel strength] The method for measuring the interlayer peel strength will be described below. As shown in Fig. 13, the nonwoven fabric sheet 33 (see Fig. 7) is cut to prepare a test piece 80 having a width of 3 cm and a length of 30 cm. The width and length of the test piece 80 can be changed, but the width is preferably 1 cm or more.

[0043] Next, as a preparation step, about 50 mm of the end region in the longitudinal direction of the test piece 80 is peeled off. The length of the end region to be peeled off in the preparation step can be changed as desired within a range in which the peel length required for the test can be secured.

[0044] 14, "interlayer delamination" refers to peeling the webs of nonwoven fabric that have been made into a single layer by needle punching to separate them into a first layer 81 and a second layer 82. The first layer 81 includes a first surface 33a, and the second layer 82 includes a second surface 33b.

[0045] Next, in a peeling step, the peeled first layer 81 and second layer 82 are held separately in a tensile tester (not shown) and peeled between the layers. The maximum force required for this peeling is the peel strength. As an example, the test piece 80 may be peeled about 20 cm at a tensile speed of 970 mm / min. The tensile speed and peel length can be changed as desired. Any device can be used as the tensile tester as long as it is capable of measuring the tensile strength.

[0046] Table 1 shows the results of the interlayer peel strength test using the nonwoven fabrics of Examples 1 to 4. The nonwoven fabrics of Examples 1 to 4 contain, as materials, 35% by weight of polypropylene staple fibers (fineness: 1.7 dtex, cut length: 51 mm), 20% by weight of polypropylene staple fibers (fineness: 7.7 dtex, cut length: 64 mm), and 45% by weight of heat-adhesive polyester staple fibers having a core-sheath structure (fineness: 2.2 dtex, cut length: 51 mm, sheath melting point: 110°C). These staple fibers were mixed and carded to obtain the webs of Examples 1 to 4. Seven layers of this web were laminated, and then needle punched to obtain a single-layer material with an interlayer peel strength of 0.104 to 1.2 N / cm. Thereafter, the single-layer material was subjected to heat treatment processing only on the surface at a roll distance of 4 mm, a roll temperature of 130°C, and a speed of 5 m / min. As a result, a 7 g / cm2 non-fuzzed ... 2 Thickness under load: 3.6-4.5mm, actual weight: 143-156g / m 2 A nonwoven fabric sheet 33 was obtained.

[0047] Examples 1 to 4 are test pieces 80 made of nonwoven fabrics formed using the same web, and have different punch densities. Example 2 has a higher punch density than Example 1, and Example 3 has an even higher punch density than Example 2. Example 4 has a lower punch density than Example 1. For each example, the same test was performed 10 times. The test results of each of the 10 times, i.e., the tensile force, were averaged, and the average value was divided by 3 to convert it into strength per unit width (1 cm width). The value calculated in this way is the interlayer peel strength.

[0048] [Table 1]

[0049] As is clear from the interlayer peel strengths of Examples 1 to 4, a higher punch density strengthens the bond between the webs (layers), and therefore increases the tensile force required for interlayer peeling. In other words, the interlayer peel strength increases. The interlayer peel strengths of Examples 1 to 4 are all in the range of 0.05 to 2.45 N / cm. In order to calculate a stable value for the measurement of interlayer peel strength, the test can be performed multiple times and the average value can be calculated, but the number of tests can be changed as desired.

[0050] Table 1 shows a number of physical property values ​​for each of Examples 1 to 4 as well as Comparative Examples 1 and 2. In Comparative Examples 1 and 2, the two layers did not peel off even when subjected to a peel strength test, so the value of the peel strength could not be calculated.

[0051] Comparative Example 1 is a conventional single-layer nonwoven fabric. This single-layer material contains 35% by weight of polyester staple fibers (fineness: 2.2 dtex, cut length: 51 mm), 20% by weight of polyester staple fibers (fineness: 7.7 dtex, cut length: 64 mm), and 45% by weight of thermally adhesive polyester staple fibers having a core-sheath structure (fineness: 2.2 dtex, cut length: 51 mm, sheath melting point: 110°C). These staple fibers were mixed and carded to obtain the web of Comparative Example 1. Seven layers of this web were laminated, and then needle punched to obtain a 7 g / cm2 non-peeling web. 2 The thickness under load is 2.6 mm, and the actual weight is 145 g / m 2 Thus, a nonwoven fabric sheet of Comparative Example 1 was obtained.

[0052] Comparative Example 2 is a reinforcing base fabric having a three-layer structure disclosed in JP 2016-132228 A. The reinforcing base fabric of Comparative Example 3 includes a surface layer, a back layer, and an intermediate layer disposed between the surface layer and the back layer. The surface layer and the back layer are nonwoven fabrics. The intermediate layer is made of a foam (slab urethane). The surface layer has a basis weight of 20 g / m 2 or more, and the back layer has a basis weight of 30 g / m 2 The weight of the middle layer is 30 to 100 g / m 2The nonwoven fabric (front layer and back layer) contained in the reinforcing base fabric of Comparative Example 2 was obtained by mixing polyester staple fibers and thermal adhesive polyester staple fibers and subjecting the mixture to needle punch processing.

[0053] The "actual weight" in Table 1 is the weight converted into weight after measuring the material weight of 100 x 100 mm. The "no-load thickness" in Table 1 is a reference value, as it varies depending on the place where it is measured.

[0054] The results of the bleeding test using Examples 1 to 4 and Comparative Examples 1 and 2 are shown in Table 1. The bleeding degree was calculated by preparing a 30 cm x 30 cm test piece from each of the fabrics of Examples 1 to 4 and Comparative Examples 1 and 2, joining each test piece with a foam material in a test mold, and then visually calculating the percentage of the area (%) of the foam material that had leaked through the test piece and was exposed. The visual inspection was performed by multiple people, and the numerical value was determined in 5% increments.

[0055] The exudation rates of Examples 1 to 4 were 40%, 60%, 65%, and 30%, respectively, and it can be seen that the lower the interlayer peel strength, i.e., the lower the punch density, the smaller the exudation rate. In addition, the exudation rate of the conventional nonwoven fabric, which is a single-layer material in Comparative Example 1, was 85%.

[0056] As a simple method for judging the interlayer peel strength, nonwoven fabric 11 may be pinched by hand and peeled. That is, when nonwoven fabric 11 is manually pulled in the thickness direction, if it can be peeled into two layers while maintaining the layered shape without being partially torn, it can be judged that nonwoven fabric 11 has the necessary interlayer peel strength. In other words, a nonwoven fabric that does not have interlayer peel strength cannot be peeled into two layers, and a nonwoven fabric that cannot be peeled into two layers cannot even obtain a numerical value for interlayer peel strength.

[0057] [Function of nonwoven fabric] The function of the nonwoven fabric 11 (or nonwoven fabric sheet 33) of the present disclosure will now be described. Nonwoven fabrics used as reinforcement materials for foam-molded products are required to have at least the shielding properties of the foam material (urethane), the ability to conform to the shape of the mold during molding, and workability. In addition, the economic viability of the product must also be taken into consideration.

[0058] Workability can also be said to be the ease of handling in operations including storage, transportation, and processing. For example, the nonwoven fabric 11 of the present disclosure is heated only on the surface to remove fuzz from the surface. This prevents the nonwoven fabrics 11 from sticking to each other when stacked for storage or transportation. In addition, the nonwoven fabric 11 has appropriate rigidity, flexibility, and appropriate elongation required as a foam molding reinforcement material. The appropriate elongation means an elongation that allows the material to conform to a mold while suppressing unnecessary elongation of the entire material.

[0059] In the nonwoven fabric 11 of the present disclosure, only the surface is heat-treated for workability, but the heat does not reach the inside of the layers, so the short fibers constituting the nonwoven fabric 11 are not thermally bonded to each other, and as a result, the nonwoven fabric 11 maintains its original flexibility.

[0060] Here, the nonwoven fabric 11 shields the foaming material by the following mechanism. That is, the nonwoven fabric 11 is a thick bulky material that maintains the layer structure as much as possible by stacking webs in which short fibers are aligned so as to be oriented in one direction. The nonwoven fabric 11 can also be said to have a coarse structure. Therefore, the nonwoven fabric 11 does not shield the foaming material on the surface, but impregnates the foaming material from the surface to a certain extent, while delaying the impregnation of the foaming material with the multiple overlapping webs. The nonwoven fabric 11 is designed to stop the impregnation of the foaming material before the foaming material seeps out from the opposite side due to the increase in viscosity caused by the foaming reaction.

[0061] However, a nonwoven fabric cannot be used as a reinforcing material unless the overlapping webs are bonded together. Therefore, in the manufacturing method of nonwoven fabric 11 of the present disclosure, the short fibers are entangled by needle punching to the extent that the webs maintain the shape of a single layer, in other words, to the extent that the webs are bonded together to a minimum extent. The degree of entanglement of the fibers varies in various ways depending on the processing conditions of the needle punching, the type of needle used, the fiber diameter, the fiber shape, the friction coefficient of the fibers (type of oil), and the working environment (humidity and temperature). Therefore, in the present disclosure, interlayer peel strength is introduced as a unique index to easily quantify the degree of entanglement of the short fibers.

[0062] For example, when a nonwoven fabric is manufactured by needle punching, the fibers are entangled with a plurality of needles having protrusions, thereby bonding the laminated webs together. The higher the interlayer peel strength, the stronger the bond between the fibers, and the higher the punch density in the needle punching process, the higher the interlayer peel strength. A nonwoven fabric with a high punch density contains many through holes created by the penetration of the needles. Therefore, a nonwoven fabric with a high punch density is more likely to pass through the foaming material when it is joined to the foaming material. Therefore, the foaming material is more likely to be exposed on the surface of the molded product.

[0063] The nonwoven fabric of the present disclosure has an interlayer peel strength of 0.05 to 2.45 N / cm by bonding the webs to such an extent that the webs peel off from each other when pulled. Here, the lower limit of the interlayer peel strength of 0.05 N / cm is the minimum strength required to maintain the shape of the nonwoven fabric, and the upper limit of the interlayer peel strength of 2.45 N / cm is the maximum value at which the nonwoven fabric can be peeled off while maintaining the layer shape. In other words, an interlayer peel strength of less than the lower limit of 0.05 N / cm means that it is difficult to use as a nonwoven fabric, and an interlayer peel strength of more than the upper limit of 2.45 N / cm means that the webs cannot be peeled off in layers. Therefore, with conventional nonwoven fabrics, even if you try to peel the webs off from each other, you cannot peel the webs off in the thickness direction while maintaining the layer shape.

[0064] The interlayer peel strength may be 0.05 to 1.8 N / cm, 0.05 to 1.3 N / cm, or 0.1 to 1.2 N / cm. The lower the peel strength, the higher the foam shielding performance, and the higher the peel strength, the higher the strength of the nonwoven fabric.

[0065] In the nonwoven fabric 11, the webs 31 are bonded together at a punch density low enough to allow delamination. As a result, the nonwoven fabric 11 has a delamination strength of 0.05 to 2.45 N / cm. Such a nonwoven fabric 11 has fewer holes penetrated by the needles 40 than a conventional nonwoven fabric in which the webs are bonded together at a punch density high enough not to cause delamination. Therefore, the foaming material 17 is less likely to pass through the nonwoven fabric 11 (reinforcing material 10) during foam molding. Therefore, exposure or seepage of the foaming material 17 to the surface of the foam-molded product 19 is suppressed. Therefore, even if the foam-molded material 18 rubs against a metal part via the reinforcing material 10, abnormal noise is less likely to be generated.

[0066] In addition, the nonwoven fabric of the present disclosure has a density of 7 g / cm 2 The thickness under load may be 1 to 8 mm, 2 to 7.5 mm, or 2.5 to 6 mm. If the nonwoven fabric is made thicker, the passage of the foaming material can be suppressed, but the processability during molding deteriorates. More specifically, if the thickness is less than 1 mm, the foaming material easily passes through, and if the thickness exceeds 8 mm, the processability deteriorates. In this regard, the thickness of the nonwoven fabric having the above interlayer peel strength is set to 7 g / cm 2 If the load is set to 1 to 8 mm, it is possible to suppress the exposure of the foaming material and to achieve good processability. 2 More suitable performance can be achieved by setting the thickness under load to 2 to 7.5 mm. The apparent density of the nonwoven fabric 11 is 0.02 to 0.05 g / m 2 It becomes.

[0067] Although a nonwoven fabric that is a multilayer material can suppress the passage of a foaming material, the processability during molding is deteriorated. Therefore, if the nonwoven fabric has the above-mentioned interlayer peel strength, even if it is a single-layer material, it can appropriately suppress the passage of a foaming material, and since it is a single layer, it has excellent processability. In addition, since a single-layer material is generally cheaper than a multilayer material, it has excellent economical properties.

[0068] Conventionally, it was thought that a single layer having a bulky and coarse structure such as the nonwoven fabric 11 of the present disclosure alone would not be able to provide a foam shielding effect. Therefore, conventionally, the foam was shielded by a long fiber layer or a dense layer. In contrast, the nonwoven fabric 11 of the present disclosure is configured so that the PET fibers act as a binder and thermally bond the fibers together under the heat and pressure during foaming, thereby increasing the strength of the parts not impregnated with the foaming material. In this way, the nonwoven fabric 11 made from a coarse material has low strength of the material itself, but the fibers are thermally bonded together by the heat and pressure generated by the foaming reaction. Therefore, when the nonwoven fabric 11 is in the form of a foam-molded product, it is possible to obtain a strength that does not cause any practical problems.

[0069] The web used to manufacture such nonwoven fabrics is not limited to needle punching, but can also be formed using an air-laying machine that aligns short fibers with airflow. When using an air-laying machine, the nonwoven fabric of the present disclosure can be manufactured by adjusting at least one of the heating temperature, compression distance, and compression time.

[0070] Nonwoven fabric 11 of the present disclosure can provide the following effects. (1) Nonwoven fabrics are processed so that the web bonds are not strong, and therefore the surface is prone to fluffing. In this regard, nonwoven fabric 11 has been heat-treated on the surface, which suppresses fluffing caused by low punch density. When the nonwoven fabric is heated to the inside, the internal fibers of the nonwoven fabric are altered by the heat, and the rigidity of the nonwoven fabric increases. Nonwoven fabrics with increased rigidity have poor processability. In this regard, nonwoven fabric 11 of the present disclosure has been heat-treated only on the surface, which suppresses fluffing. In addition, the internal fibers between the first and second surfaces are not heat-treated, so good processability can be maintained.

[0071] (2) A reinforcing material with high molding accuracy can be obtained by molding the highly moldable nonwoven fabric 11. In particular, the high processability of the nonwoven fabric 11 is useful when the reinforcing material is molded three-dimensionally by a molding process involving heating.

[0072] (3) By adjusting the punch density when the laminated webs are bonded to each other by needle punching, a single-layer material with an interlayer peel strength of 0.05 to 2.45 N / cm can be formed. In addition, by subjecting only the surface of the single-layer material to heat treatment, a single-layer material with an interlayer peel strength of 7 g / cm can be formed. 2 Thickness under load is 2-7.5mm, apparent density is 0.02-0.05g / m 2 It can be adjusted so that

[0073] (4) Nonwoven fabric 11 having interlayer peel strength does not allow foaming material to pass through easily. In addition, such nonwoven fabric 11 has appropriate flexibility, is a single-layer material, and is relatively thin (e.g., 2 to 7.5 mm), and therefore has excellent formability. More specifically, nonwoven fabric 11 has appropriate stretchability, making it easy to set in mold 20 or forming mold 51 or to sew, and has good conformability to molds 20, 51.

[0074] (5) The web 31 containing 40 to 80% by weight of PP fiber can have a larger number of fibers without increasing the weight, compared to a web consisting of only PET fiber. Since the nonwoven fabric 11 has a larger number of fibers than conventional nonwoven fabrics, it can suppress the passage of the foaming material 17.

[0075] (6) The PET fibers contained in the nonwoven fabric 11 have a core-sheath structure. When heated, the sheath melts, bonding the fibers together, while the core, which does not melt easily, maintains the strength of the fibers.

[0076] (7) Since the heat treatment does not extend to the internal fibers 33c of the nonwoven fabric 11, the flexibility of the nonwoven fabric 11 is maintained. Therefore, the nonwoven fabric 11 has excellent processability, for example, in a shaping process that involves heating. In addition, when the reinforcing material 10 is molded by heating, the effect of reducing molding wrinkles due to shrinkage can be more effectively achieved.

[0077] (8) The reinforcing material 10 is produced by molding the nonwoven fabric 11, which has excellent processability, and therefore the molding precision is high. [Modifications of the present disclosure] This embodiment can be modified as follows: This embodiment and the following modifications can be combined with each other to the extent that there is no technical contradiction.

[0078] The nonwoven fabric 11 may be shaped by sewing. A group of needles that pierce the first surface 33a and a group of needles that pierce the second surface 33b may be arranged on the transport path of the laminate 30.

[0079] The nonwoven fabric 11, which is a single-layer material, may be used as a multilayer structure material by combining it with other single-layer materials or multilayer materials. The layers to be combined are not limited to nonwoven fabrics, and may be, for example, cloth, cushioning materials, or leather. When combined with other nonwoven fabrics, for example, in order to increase the strength of the nonwoven fabric 11, one or more nonwoven fabric layers that do not delaminate may be bonded to the nonwoven fabric 11. In this case, the nonwoven fabric layer may be formed from short fibers. Alternatively, in order to increase the rigidity of the nonwoven fabric 11, a nonwoven fabric layer mainly made of core-sheath fibers may be bonded to the nonwoven fabric 11. In this case, the nonwoven fabric layer may contain 70% or more of core-sheath fibers, and may be formed from long or short fibers. In addition, leather or cloth having any pattern or color may be bonded to the nonwoven fabric 11 as a decorative material when used as a seat pad for a seat. Alternatively, in order to increase the cushioning property of the seat pad, a cushioning material (for example, a slab urethane sheet) may be bonded to the nonwoven fabric 11. In order to obtain desired properties, any other material can be combined with the nonwoven fabric 11. The method of bonding such other layers to the nonwoven fabric 11 can be changed as desired depending on the application.

[0080] Aspects grasped based on the above embodiment and modified examples are listed below. [1] A nonwoven fabric used as a reinforcing material for a foam-molded product that is bonded to a foam-molded material in order to reinforce the foam-molded product, the nonwoven fabric comprising: A single-layer material is formed by folding a web formed from staple fibers and laminating the web, and the staple fibers of the web are bonded to each other by needle punching, 7g / cm 2 The thickness under load is 2 to 7.5 mm. Apparent density: 0.02~0.05g / m 2 and The interlayer peel strength is 0.05 to 2.45 N / cm, and the interlayer peel strength is a value of a tensile force required to peel the laminated webs from each other. A nonwoven fabric used as a reinforcing material for foam moldings. [2] The weight per layer of the web is 10 to 30 g / m 2 and The monolayer material is formed by folding the web 3 to 12 times. A nonwoven fabric used as a reinforcing material for foam moldings described in [1] above. [3] The basis weight of the single layer material is 90 to 200 g / m 2 That is, The nonwoven fabric used as a reinforcing material for foam moldings according to the above [1] or [2]. [4] A heat-treated first surface; a second surface opposite the first surface, the second surface being heat treated; and an internal fiber between the first surface and the second surface that is not heat treated; Including, The nonwoven fabric used for a reinforcing material for foam-molded products according to any one of the above [1] to [3]. [5] The web contains 20% to 60% by weight of polyethylene terephthalate fibers and 40 to 80% by weight of polypropylene fibers. The nonwoven fabric used for a reinforcing material for foam-molded products according to any one of the above [1] to [4]. [6] The polyethylene terephthalate fiber has a core-sheath structure, The core-sheath structure includes a core and a sheath having a melting point lower than that of the core. A nonwoven fabric used as a reinforcing material for foam moldings described in [5] above. [7] A multilayer structure comprising the nonwoven fabric according to any one of [1] to [4] above. [8] A reinforcing material for foam-molded products, formed from the nonwoven fabric according to any one of [1] to [4] above. [9] A method for producing a nonwoven fabric used as a reinforcing material for foam molding, comprising the steps of: laminating a web formed from staple fibers by folding said web; bonding the staple fibers of the laminated webs together by needle punching to form a single layer material; and applying a heat treatment to only the surface of the monolayer material; The nonwoven fabric is 7g / cm 2 The thickness under load is 2 to 7.5 mm. Apparent density: 0.02~0.05g / m 2 and The interlayer peel strength is 0.05 to 2.45 N / cm, and the interlayer peel strength is a value of a tensile force required to peel the laminated webs from each other. A method for manufacturing nonwoven fabrics used as reinforcing materials for foam moldings. [Explanation of symbols]

[0081] 10...reinforcing material, 11...nonwoven fabric, 12...back portion, 13...side portion, 14...through hole, 15...central wrap-around portion, 16...side wrap-around portion, 17...foaming material, 18...foaming molding material, 19...foaming molding product, 20...mold, 21...upper mold, 22...core mold, 23...lower mold, 30...laminate material, 31...web, 32...single layer material, 33...nonwoven fabric sheet, 33a...first surface, 33b...second surface, 33c...internal fiber, 40...needle, 41...projection, 42...first needle group, 43...second needle group, 44...moving device, 45...support bed, 4 6...calendar roll, 47...heating roll, 48...roll, 49...heating device, 50...molding device, 51...molding mold, 51a...ventilation hole, 52...tubular portion, 53...air intake leg portion, 54...exhaust leg portion, 56...second auxiliary cover, 58...string, 60...base, 60a...air intake passage, 60b...exhaust passage, 61...air intake and exhaust unit, 62...air intake pipe, 63...exhaust pipe, 64...cover material, 65...closed space, 70...first auxiliary cover, 71...cover body, 71a...edge region, 72...magnet, 73...connecting bar, 80...test piece, 81...first layer, 82...second layer.

Claims

1. A nonwoven fabric used as a reinforcing material for a foam-molded product that is bonded to a foam-molded material in order to reinforce the foam-molded product, the nonwoven fabric comprising: A single-layer material is formed by folding a web formed from staple fibers and laminating the web, and the staple fibers of the web are bonded to each other by needle punching, 7 g / cm 2 The thickness under load is 2 to 7.5 mm; Apparent density: 0.02 to 0.05 g / m 2 and The interlayer peel strength is 0.05 to 2.45 N / cm, and the interlayer peel strength is a value of a tensile force required to peel the laminated webs from each other. A nonwoven fabric used as a reinforcing material for foam moldings.

2. The weight per layer of the web is 10 to 30 g / m 2 and The monolayer material is formed by folding the web 3 to 12 times. The nonwoven fabric used in the reinforcing material for foam-molded products according to claim 1.

3. The weight of the single layer material is 90 to 200 g / m 2 That is, The nonwoven fabric used in the reinforcing material for foam-molded products according to claim 2.

4. a heat treated first surface; a second surface opposite the first surface, the second surface being heat treated; and non-heat treated internal fibers between the first surface and the second surface; Including, The nonwoven fabric used in the reinforcing material for foam-molded products according to claim 1.

5. A multi-layer structure comprising the nonwoven fabric according to any one of claims 1 to 4.

6. A reinforcing material for foam-molded products, which is formed from the nonwoven fabric according to any one of claims 1 to 4.

7. A method for producing a nonwoven fabric used as a reinforcing material for a foam-molded product, comprising the steps of: laminating a web formed from staple fibers by folding said web; bonding the staple fibers of the laminated webs together by needle punching to form a single layer material; and applying a heat treatment to only the surface of the monolayer material; The nonwoven fabric is 7 g / cm 2 The thickness under load is 2 to 7.5 mm; Apparent density: 0.02 to 0.05 g / m 2 and The interlayer peel strength is 0.05 to 2.45 N / cm, and the interlayer peel strength is a value of a tensile force required to peel the laminated webs from each other. A method for manufacturing nonwoven fabrics used as reinforcing materials for foam moldings.

Citation Information

Patent Citations

  • Nonwoven fabric for reinforcing material for foamed molded article and method for producing the same

    JP2012082548A

  • Nonwoven fabric for reinforcement of foam molded article

    JP2013076179A

Cited By

  • Production method for seat pad reinforcement fabric, production device for seat pad reinforcement fabric, and sheet member

    WO2025211461A1