Method for producing polymer compound
By using a twin-screw extruder and specific additives, the method enhances the tensile strength and elongation of thermoplasticized crosslinked polyethylene, addressing the limitations of existing methods and producing compounds suitable for demanding applications.
Patent Information
- Application Number
- JP2023065078
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-12
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-04-12
Smart Images

Figure 2024151606000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a polymeric compound having high tensile strength and tensile elongation by thermoplasticizing crosslinked polyethylene. [Background technology]
[0002] Cross-linked polyethylene is polyethylene that has been treated with a cross-linking agent to form intermolecular bonds between the polymer chains in a three-dimensional mesh structure, improving its heat resistance and impact resistance. Cross-linked polyethylene is broadly classified into peroxide cross-linked polyethylene, which is cross-linked with organic peroxides, and silane cross-linked polyethylene, which is cross-linked with a silanol condensation catalyst.
[0003] Cross-linked polyethylene does not melt even when heated, making it extremely difficult to recycle. However, in recent years, much research has been done on methods to recycle cross-linked polyethylene by thermoplasticizing it. Thermoplasticization is a technology that applies appropriate heat and shear stress to cross-linked polyethylene to destroy the cross-linked structure and reduce the molecular weight, resulting in a thermoplastic recycled material. However, cross-linked polyethylene has a large bond energy, making it difficult to properly cut the cross-linking points, and it is difficult to obtain a polymer compound with high tensile strength and tensile elongation.
[0004] Various methods of thermoplasticization for reusing cross-linked polyethylene have been investigated. For example, a method for processing polymer compounds that can obtain a high-quality product with little molecular weight loss by adding a small amount of virgin polyethylene and thermoplasticizing a mixture of cross-linked polyethylenes with different cross-linking methods (Patent Document 1) and a material recycling method in which polyethylene resins containing silane cross-linked polyethylene are thermoplasticized by adding an aliphatic compound (Patent Document 2) are known.
[0005] In the method for treating a polymer compound described in the claims of Patent Document 1, the polymer compound and a chemical agent are fed into a reactive extruder and reacted at 240 to 380° C. in a shear kneading zone provided inside the extruder to perform the treatment. The polymer compound and the chemical agent are reacted in the reactive extruder to thermoplasticize the polymer compound, thereby producing a treated polymer product.
[0006] In the material recycling method described in Patent Document 2, a silane-crosslinked polyethylene resin is mixed with an additive selected from aliphatic compounds having 16 or more carbon atoms, one or more hydroxyl groups, and a boiling point of 300°C or higher, and then a shear stress is applied to thermoplasticize the mixture, thereby obtaining a polymer compound that can be recycled.
[0007] [Patent Document 1] JP 2009-197138 A [Patent Document 2] Patent Publication No. 2021-024904 Summary of the Invention [Problem to be solved by the invention]
[0008] However, in the method described in Patent Document 1, a polymer compound and a drug are supplied to a reaction extruder and reacted at 240 to 380°C in a shear kneading zone provided inside the extruder. As a result, according to the data in Table 3, the tensile property Tb (referred to as tensile strength in this application) of the obtained polymer compound was less than 15 MPa, and the tensile property Eb (referred to as tensile elongation in this application) was also 450% or less.
[0009] As shown in Table 1, the polymer compound obtained by the method described in Patent Document 2 had a tensile strength of 17 MPa or more, but the tensile elongation was a low value of 320% at most.
[0010] As described above, the polymer compounds obtained by the conventional thermoplasticization method of crosslinked polyethylene have low values of tensile strength and tensile elongation, and are not suitable for materials requiring high tensile strength and tensile elongation, such as blow molding materials and foam molding materials.
[0011] The present invention has been made to overcome the above-mentioned disadvantages, and has an object to provide a method for producing a polymer compound that can be suitably used even in applications requiring both high tensile strength and high tensile elongation (e.g., blow molding or foam molding). [Means for solving the problem]
[0012] The method for producing a polymer compound according to the present invention is a method for producing a polymer compound by thermoplasticizing a crosslinked polyethylene with an extruder, the method comprising the steps of: a mixing step of mixing the crosslinked polyethylene, a first non-crosslinked polyethylene, and an additive to produce a mixture; a thermoplasticizing step of feeding the mixture from a first input section of the extruder and applying heat and shear stress to thermoplasticize the crosslinked polyethylene; and a kneading step of feeding a second non-crosslinked polyethylene from a second input section of the extruder to the mixture after the thermoplasticizing step and kneading the mixture, wherein the amount of the first non-crosslinked polyethylene in the mixing step is 1 to 5 parts by weight relative to 100 parts by weight of the crosslinked polyethylene, the additive comprises at least one non-crosslinked polymer compound selected from an ethylene-vinyl acetate copolymer, an ethylene-methyl acrylate copolymer, an ethylene-ethyl acrylate copolymer, an ethylene-methyl methacrylate copolymer, or an ethylene-ethyl methacrylate copolymer, the amount of the additive is 0.1 to 3 parts by weight relative to 100 parts by weight of the crosslinked polyethylene, and the shear stress in the thermoplasticizing step is 10,000 to 15,000 s -1 The method is characterized in that the shear rate is generated at 5 to 30 seconds at a shear rate of 50 to 150 parts by weight of the second non-crosslinked polyethylene per 100 parts by weight of the crosslinked polyethylene.
[0013] Furthermore, the additive may have a melt flow index of 1 to 30 g / 10 min.
[0014] The polymer compound after the kneading step may have a tensile strength of 18 MPa or more and a tensile elongation of more than 450%. Effect of the Invention
[0015] According to the present invention, a polymer compound having high tensile strength and tensile elongation can be obtained by using an additive containing at least one non-crosslinked polymer compound selected from ethylene-vinyl acetate copolymer, ethylene-methyl acrylate copolymer, ethylene-ethyl acrylate copolymer, ethylene-methyl methacrylate copolymer, or ethylene-ethyl methacrylate copolymer. The obtained polymer compound can be used in applications requiring high tensile strength and tensile elongation, such as blow molding and foam molding. [Brief description of the drawings]
[0016] [Figure 1] 1 is a schematic cross-sectional view showing an internal structure of a twin-screw extruder according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a partial cross-sectional plan view of two screws arranged inside a cylinder of a twin-screw extruder according to an embodiment of the present invention. [Diagram 3] FIG. 1 is a process diagram of a method for producing a polymer compound according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, an embodiment of the present invention will be described with reference to the drawings.
[0018] <Description of the device> The thermoplasticization of cross-linked polyethylene is carried out using an extruder, which can be broadly divided into single-screw extruders with only one screw and twin-screw extruders with two screws. Compared to single-screw extruders, twin-screw extruders have the following advantages: they are more efficient at uniformly mixing different components such as additives and fillers, they are less affected by frictional heat and therefore generate less heat, and the internal material flow is more complex, allowing greater shear stress to be applied to the material. For this reason, tests were carried out using a twin-screw extruder in the present invention.
[0019] Fig. 1 is a schematic cross-sectional view showing the internal structure of a twin-screw extruder 10 according to an embodiment of the present invention. Fig. 2 is a partial cross-sectional view showing two screws 13 arranged inside a cylinder 12 of the twin-screw extruder 10 in a plan view.
[0020] As shown in FIG. 1, the twin-screw extruder 10 has a cylinder 12 extending from a drive section 14, and further includes a first input section 16 and a second input section 24 for inputting polyethylene or the like. A first transport section 18, a first kneading section 20, a second transport section 26, a second kneading section 28, and a third transport section 32 are provided in the cylinder 12 in this order. Each of the first transport section 18, the first kneading section 20, the second transport section 26, the second kneading section 28, and the third transport section 32 has two pairs of screws 13. Here, the screws of the first transport section 18, the second transport section 26, and the third transport section 32 are configured as screws having shapes suitable for transport, and the screws of the first kneading section 20 and the second kneading section 28 are configured as screws having shapes suitable for thermoplasticization.
[0021] A motor (not shown) is provided in the drive unit 14, and the motor of the drive unit 14 is connected to the screw of the first transport unit 18, and each screw is further connected to an adjacent screw. Therefore, when the motor in the drive unit 14 is driven, each screw of the first transport unit 18, the first kneading unit 20, the second transport unit 26, the second kneading unit 28, and the third transport unit 32 rotates simultaneously. Furthermore, a heating means such as a heater (not shown) is provided to keep the inside of the cylinder 12 at a predetermined temperature.
[0022] A first input section 16 is provided above the first transport section 18, and the mixture mixed outside the twin-screw extruder 10 is input from the first input section 16, heated and melted in the first transport section 18 heated by a heater or the like, and transferred to the first kneading section 20.
[0023] The first kneading section 20 has a narrow screw and cylinder width so that high shear stress is generated. A first degassing section 22 is provided above the first kneading section 20, and the mixture transferred from the first conveying section 18 is subjected to shear stress and heat in the first kneading section 20, thereby thermoplasticizing the cross-linked polyethylene. The gas generated at that time is discharged to the outside of the twin-screw extruder 10 through the first degassing section 22. The thermoplasticized mixture is then transferred to the second conveying section 26.
[0024] Here, shear stress τ is the stress that acts when one surface inside an object and another surface inside the object are deformed in alternate parallel directions. If the force applied to deform is F and the area of the deformed is A, the shear stress is expressed as F / A, and its unit is τ (Pa pascal) = F (N newton) / A (area m 2 )
[0025] In addition, the shear stress τ (Pa) is proportional to the shear rate γ (s -1 ) and the viscosity of polyethylene μ (Pa s). In other words, τ = μγ. The unit of shear rate γ is expressed in reciprocal seconds (1 / s). Here, since the viscosity μ of polyethylene is determined by the type of polyethylene and the temperature, the shear stress τ is generally controlled by the shear rate.
[0026] Here, the shear rate γ(s -1 ) is expressed as γ=v / t, where t (mm) is the clearance between the extruder cylinder and the screw, and v (mm / s) is the speed at the top of the screw tip. Note that the speed v at the top of the screw tip is v=πND / 60, where N (rpm) is the screw rotation speed and D (mm) is the diameter. In other words, the shear rate is expressed as γ=πND / 60t. Note that π represents the constant pi.
[0027] The second transport section 26 is connected to the first kneading section 20 and the second kneading section 28, and the second input section 24 is provided above the second transport section 26. The solid material input from the second input section 24 is melted in the second transport section 26 heated by a heater or the like, and is transferred to the second kneading section 28 together with the mixture transferred from the first kneading section 20.
[0028] The second kneading section 28 is connected to the second transport section 26 and the third transport section 32, and has two screws that perform mixing and kneading. In the second kneading section 28, the thermoplastic mixture transferred from the second transport section 26 and the input material can be uniformly kneaded. Then, the kneaded polymer compound is transferred to the third transport section 32.
[0029] The third transport section 32 is connected to the second kneading section 28 and the discharge section 34. A second degassing section 30 is provided above the third transport section 32, and is structured so that gas generated inside the cylinder 12 is discharged to the outside. The polymer compound transferred from the second kneading section 28 passes through the third transport section 32 and is discharged from the discharge section 34 to the outside.
[0030] <Process Description> Next, a method for producing a polymer compound according to an embodiment of the present invention will be described with reference to Fig. 3. Fig. 3 is a process diagram of the method for producing a polymer compound according to an embodiment of the present invention.
[0031] (Preparation process: S1) At the start, the twin-screw extruder 10 is powered on. This causes the motor in the drive section 14 of the twin-screw extruder 10 to rotate, causing the screws of the first conveying section 18, the first kneading section 20, the second conveying section 26, the second kneading section 28, and the third conveying section 32 connected to the drive section 14 to rotate. At the same time, the inside of the cylinder 12 is heated to a predetermined temperature by the heating mechanism, and this is maintained for a predetermined time until the device is sufficiently stabilized.
[0032] As mentioned above, the shear rate is expressed by the formula γ = πND / 60t, and the shear rate in the first kneading section is 10,000 to 15,000 s -1, preferably 10,000s -1 The screw rotation speed is set so that the shear stress in the first kneading section is 10,000s -1 At shear rates below 15,000s, thermoplasticity does not progress sufficiently. -1 At shear rates above this level, thermoplasticization proceeds too far, resulting in a marked decrease in the physical properties of the resulting polymer compound.
[0033] Moreover, it is preferable to apply the shear stress for 5 to 30 seconds. If the shear stress is applied for less than 5 seconds, the thermoplasticization does not proceed sufficiently, and if the shear stress is applied for more than 30 seconds, the physical properties of the obtained polymer compound are significantly reduced.
[0034] The temperature in the first kneading section 20 is set to 300 to 400° C., preferably 350° C. The shear rate in the first kneading section 20 is 10,000 s -1 Below 15,000s, sufficient shear stress is not obtained and the cross-linked polyethylene does not undergo sufficient thermoplasticization. -1 If the temperature is above 250°C, the shear stress becomes too high, and the physical properties of the thermoplastic polymer compound are significantly reduced. Furthermore, if the temperature in the first kneading section 20 is below 250°C, the thermoplastic reaction does not proceed, and if it is above 400°C, the polymer compound is thermally deteriorated, and the physical properties are significantly reduced.
[0035] (Mixing process: S2) Next, the crosslinked polyethylene, the first non-crosslinked polyethylene, and the additives are mixed outside the twin-screw extruder 10 to produce a mixture. At this time, it is preferable to mix the first non-crosslinked polyethylene in an amount of 1 to 5 parts by weight and the additives in an amount of 0.1 to 3 parts by weight relative to 100 parts by weight of the crosslinked polyethylene.
[0036] Since the first non-crosslinked polyethylene acts as a lubricant, if the amount is less than 1 part by weight, the lubricating effect is lost and a load is placed on the twin-screw extruder, which is not preferable. Also, if the amount of the first non-crosslinked polyethylene is more than 5 parts by weight, the thermoplastic reaction is inhibited.
[0037] Furthermore, if the amount of the additive is less than 0.1 parts by weight, the thermoplastic reaction does not proceed, whereas if it is more than 3 parts by weight, the physical properties of the final polymer compound decrease.
[0038] The additive contains at least one non-crosslinked polymer compound selected from ethylene-vinyl acetate copolymer, ethylene-methyl acrylate copolymer, ethylene-ethyl acrylate copolymer, ethylene-methyl methacrylate copolymer, and ethylene-ethyl methacrylate copolymer. Among these, it is preferable to contain at least one of ethylene-vinyl acetate copolymer (EVA) and ethylene-ethyl acrylate copolymer (EEA).
[0039] Ethylene-vinyl acetate copolymer (EVA) is a copolymer of ethylene and vinyl acetate, with the weight percentage of vinyl acetate usually being 10-50% and the remainder being ethylene. The vinyl acetate content of the ethylene-vinyl acetate copolymer (EVA) used in the present invention is preferably 20-40%. If it is less than 20%, the effect of thermoplasticization decreases, and if it is more than 40%, the ethylene-vinyl acetate copolymer (EVA) does not mix well with polyethylene.
[0040] Ethylene ethyl acrylate copolymer (EEA) is a resin synthesized by polymerization of ethylene and ethyl acrylate, and the ethyl acrylate content of the ethylene ethyl acrylate copolymer (EEA) used in the present invention is preferably 10 to 30%. If it is less than 10%, the effect of thermoplasticization decreases, and if it is more than 30%, EEA does not mix well with polyethylene, which is not preferable.
[0041] Furthermore, the melt flow index of ethylene vinyl acetate copolymer (EVA) and ethylene ethyl acrylate copolymer (EEA) is preferably 1 to 30 g / 10 min. If the melt flow index is 1 g / 10 min, it will not mix well with the cross-linked polyethylene and thermoplasticization will not proceed. If the melt flow index is 30 g / 10 min or more, the physical properties of the resulting polymer compound will decrease.
[0042] The melt flow index is an index that indicates the fluidity of a thermoplastic resin when melted. It is calculated by extruding the resin from a metal cylinder with a small hole at a certain temperature and pressure, and converting it into grams per 10 minutes.
[0043] (First input process: S3) The mixture of the cross-linked polyethylene, the first non-cross-linked polyethylene and the additives is fed into the first feeding section 16, heated and melted while rotating around the twin screws in the first conveying section 18, and introduced into the first kneading section 20.
[0044] (Thermoplasticization process: S4) The mixture is subjected to shear stress and heat in the first kneading section 20, whereby the crosslinking points of the crosslinked polyethylene are broken and the mixture is thermoplasticized. The gas generated as the thermoplasticization progresses is discharged to the outside of the cylinder 12 from the first degassing section 22 located above the first kneading section 20. As the generated gas is discharged, the pressure in the first kneading section 20 becomes close to atmospheric pressure.
[0045] (Second input process: S5) The second non-crosslinked polyethylene is fed from the second feeding section 24 and introduced into the second kneading section 28 from the second transport section 26 together with the mixture heat plasticized in the first kneading section 20. The second non-crosslinked polyethylene is preferably 50 to 150 parts by weight per 100 parts by weight of the crosslinked polyethylene fed from the first feeding section. The first non-crosslinked polyethylene and the second non-crosslinked polyethylene may be made of the same material or different materials.
[0046] If the amount of the second non-crosslinked polyethylene fed from the second feeding portion 24 is less than 50 parts by weight, the physical properties of the resulting polymeric compound are low, and molded products are likely to be defective. If the amount is more than 150 parts by weight, the physical properties of the resulting polymeric compound are low, and molded products are likely to be defective.
[0047] (Kneading process: S6) The heat-plasticized mixture and the second non-crosslinked polyethylene fed from the second feeding section 24 are then mixed and kneaded in the second kneading section 28 to obtain a uniform polymer compound. (Discharge process: S7) Thereafter, the polymer compound passes through the third transport section and is discharged from the discharge section 34 to the outside of the twin-screw extruder 10, thereby obtaining the polymer compound.
[0048] The polymer compound obtained as described above has excellent moldability, and can have a tensile strength of 18 MPa or more and a tensile elongation of more than 450%, and therefore can be used in applications requiring physical strength, such as blow molding and foam molding.
[0049] Furthermore, the polymer compound obtained by the present invention can be used for both press molding and injection molding, and can give molded products having high strength, high heat resistance and high impact resistance.
[0050] The results of the polymer compound according to the present invention will be shown below by way of examples and comparative examples, but the present invention is not limited to these examples.
[0051] [Tensile test and elongation test] Tensile and elongation tests were performed on the polymer compounds. The tensile and elongation test equipment used was the Shimadzu Autograph AGS System. The tensile tests were performed using a tensile tester at a speed of 50 mm / min using a tensile tester that was punched into a dumbbell No. 3 shape from a polymer compound press-molded into a 1 mm thick sheet in accordance with JIS K6922-2.
[0052] [Gel fraction] The gel fraction was measured by extracting the sample in boiling hot xylene for 8 hours in accordance with JIS-K6796. The sample was then vacuum dried at 140°C for 3 hours, after which it was weighed, and the gel fraction was calculated from the ratio of the weight before extraction to the weight before extraction using the following formula. Gel fraction (%) = (weight after extraction (g) / weight before extraction (g)) x 100 The gel fraction of the cross-linked polyethylene used as the raw material was 65 to 85%.
[0053] Next, Examples 1 to 14 and Comparative Examples 1 to 8 will be described in detail.
[0054] [Table 1] EVA: Ethylene vinyl acetate copolymer, EEA: Ethylene ethyl acrylate copolymer, 100*: Uses peroxide cross-linked polyethylene
[0055] Examples 1 to 5 are explained below. In Examples 1 to 5, 100 parts by weight of silane crosslinked polyethylene was mixed with 2 parts by weight of a first non-crosslinked polyethylene and non-crosslinked ethylene-vinyl acetate copolymer (EVA) as an additive in the ratios shown in Table 1 to prepare a mixture. After that, the mixture was subjected to thermal plasticization using a twin-screw extruder according to the above-mentioned process, and a polymer compound was obtained, and the gel fraction, tensile strength, and tensile elongation were measured.
[0056] Example 1 Using the twin-screw extruder 10 of FIG. 1, the temperature of the first kneading section was 350° C., and the maximum shear rate was 10,000 s -1 The maximum shear time was set to 15 s (Fig. 3 S1: Preparation step). Then, a mixture was obtained by mixing 100 parts by weight of the silane crosslinked polyethylene with 2 parts by weight of the first non-crosslinked polyethylene (non-crosslinked PE) and 0.1 parts by weight of ethylene vinyl acetate copolymer (EVA) as an additive (Fig. 3 S2: Mixing step). After that, the mixture was fed from the first feeding section 16 to the twin-screw extruder 10 (Fig. 3 S3: Feeding step). Then, the mixture was kneaded for 15 seconds in the first kneading section 20 to generate a mixture in which the silane crosslinked polyethylene was thermoplasticized (Fig. 3 S4: Thermoplasticization step). Next, 100 parts by weight of the second non-crosslinked polyethylene was fed from the second feeding section 24 (Fig. 3 S5: Second feeding step). The thermoplastic mixture and the second non-crosslinked polyethylene fed from the second feed section were transferred from the second transport section 26 to the second kneading section 28, where they were kneaded to form a homogeneous polymer compound (Fig. 3 S6: kneading process), passed through the third transport section 32 and discharged from the discharge section 34, obtaining a polymer compound (Fig. 3 S7: discharge process). The gel fraction of the obtained polymer compound was 19%, the tensile strength was 20 MPa, and the elongation was 545%.
[0057] Example 2 A polymer compound was obtained by carrying out the same test as in Example 1, except that 0.5 parts by weight of ethylene vinyl acetate copolymer (EVA) was used as an additive. The gel fraction of the obtained polymer compound was 13%, the tensile strength was 21 MPa, and the elongation was 576%.
[0058] Example 3 A polymer compound was obtained by carrying out the same test as in Example 1, except that 1 part by weight of ethylene vinyl acetate copolymer (EVA) was used as the additive. The gel fraction of the obtained polymer compound was 18%, the tensile strength was 22 MPa, and the elongation was 528%.
[0059] Example 4 A polymer compound was obtained by carrying out the same test as in Example 1, except that 2 parts by weight of ethylene vinyl acetate copolymer (EVA) was used as an additive. The gel fraction of the obtained polymer compound was 14%, the tensile strength was 21 MPa, and the elongation was 504%.
[0060] Example 5 A polymer compound was obtained by carrying out the same test as in Example 1, except that 3 parts by weight of ethylene vinyl acetate copolymer (EVA) was used as an additive. The gel fraction of the obtained polymer compound was 19%, the tensile strength was 20 MPa, and the elongation was 556%.
[0061] From the results of Examples 1 to 5, by mixing 0.1 to 3 parts by weight of ethylene vinyl acetate copolymer (EVA) as an additive and performing thermal plasticization, a polymer compound with a gel fraction of 13 to 19%, a tensile strength of 20 to 22 MPa, and a tensile elongation of 504 to 576% was obtained.
[0062] Examples 6 to 10 are explained below. In Examples 6 to 10, a mixture was prepared by mixing a silane crosslinked polyethylene, a first non-crosslinked polyethylene, and 0.1 to 3 parts by weight of an ethylene ethyl acrylate copolymer (EEA) as an additive. The silane crosslinked polyethylene was then thermoplasticized, and the gel fraction, tensile strength, and elongation of the resulting polymer compound were measured.
[0063] Example 6 A polymer compound was obtained by carrying out the same test as in Example 1, except that 0.1 parts by weight of ethylene ethyl acrylate copolymer (EEA) was used as the additive. The gel fraction of the obtained polymer compound was 18%, the tensile strength was 20 MPa, and the elongation was 534%.
[0064] Example 7 A polymer compound was obtained by carrying out the same test as in Example 1, except that 0.5 parts by weight of ethylene ethyl acrylate copolymer (EEA) was used as the additive. The gel fraction of the obtained polymer compound was 15%, the elongation was 540%, and the tensile strength was 21 MPa.
[0065] Example 8 A polymer compound was obtained by carrying out the same test as in Example 1, except that 1 part by weight of ethylene ethyl acrylate copolymer (EEA) was used as the additive. The gel fraction of the obtained polymer compound was 17%, the tensile strength was 22 MPa, and the elongation was 536%.
[0066] Example 9 A polymer compound was obtained by carrying out the same test as in Example 1, except that 2 parts by weight of ethylene ethyl acrylate copolymer (EEA) was used as the additive. The gel fraction of the obtained polymer compound was 15%, the tensile strength was 22 MPa, and the elongation was 564%.
[0067] Example 10 A polymer compound was obtained by carrying out the same test as in Example 1, except that 3 parts by weight of ethylene ethyl acrylate copolymer (EEA) was used as the additive. The gel fraction of the obtained polymer compound was 19%, the tensile strength was 21 MPa, and the elongation was 568%.
[0068] As shown in Examples 6 to 10, by mixing 0.1 to 3 parts by weight of ethylene ethyl acrylate copolymer (EEA) as an additive to the polymer compound and performing thermal plasticization, a polymer compound with a gel fraction of 15 to 19%, a tensile strength of 20 to 22 MPa, and an elongation of 534 to 568% was obtained.
[0069] Examples 11 to 13 are explained below. In Examples 11 to 13, a mixture was prepared by mixing a peroxide-crosslinked polyethylene, a first non-crosslinked polyethylene, and 1 to 3 parts by weight of an ethylene-vinyl acetate copolymer (EVA) as an additive. The peroxide-crosslinked polyethylene was then thermoplasticized, and the gel fraction, tensile strength, and elongation of the resulting polymer compound were measured.
[0070] Example 11 A mixture was obtained by mixing 100 parts by weight of peroxide cross-linked polyethylene, 2 parts by weight of a first non-cross-linked polyethylene, and 1 part by weight of ethylene vinyl acetate copolymer (EVA) as an additive (FIG. 3: S2). Otherwise, the test was performed in the same manner as in Example 1 to obtain a polymer compound. The gel fraction of the obtained polymer compound was 5%, the tensile strength was 19 MPa, and the elongation was 754%.
[0071] Example 12 A polymer compound was obtained by carrying out the same test as in Example 1, except that 2 parts by weight of ethylene vinyl acetate copolymer (EVA) was used as the additive. The gel fraction of the obtained polymer compound was 9%, the tensile strength was 18 MPa, and the elongation was 530%.
[0072] Example 13 A polymer compound was obtained by carrying out the same test as in Example 1, except that 3 parts by weight of ethylene vinyl acetate copolymer (EVA) was used as an additive. The gel fraction of the obtained polymer compound was 8%, the tensile strength was 18 MPa, and the elongation was 650%.
[0073] Example 14 will be described below. In Example 14, 100 parts by weight of silane crosslinked polyethylene, 2 parts by weight of a first non-crosslinked polyethylene, 1 part by weight of ethylene vinyl acetate copolymer (EVA) and 1 part by weight of ethylene ethyl acrylate copolymer (EEA) as additives were mixed to obtain a mixture. Except for this, the test was carried out in the same manner as in Example 1 to obtain a polymer compound. The gel fraction of the obtained polymer compound was 15%, the tensile strength was 20 MPa, and the elongation was 600%.
[0074] As shown in Examples 1 to 14, by adding 0.1 to 3 parts by weight of ethylene vinyl acetate copolymer (EVA) and / or ethylene ethyl acrylate copolymer (EEA) as an additive to 100 parts by weight of crosslinked polyethylene and then performing heat plasticization, a polymer compound with a tensile strength of 18 MPa or more and an elongation rate of more than 450% was obtained. The gel fraction was 20% or less in all cases.
[0075] Comparative Examples 1 to 8 are explained below. Comparative Example 1 was conducted under the condition of no additives in the silane cross-linked polyethylene, and Comparative Examples 2 and 3 were conducted under the condition of 0.05 parts by weight and 5 parts by weight of ethylene vinyl acetate copolymer (EVA) as an additive. Comparative Examples 4 and 5 were conducted under the condition of 0.05 parts by weight and 5 parts by weight of ethylene ethyl acrylate copolymer (EEA) as an additive. Comparative Examples 6 to 8 were conducted under the condition of no additives in the peroxide cross-linked polyethylene, and mixtures were produced using 2, 5, and 10 parts by weight of a first non-cross-linked polyethylene (non-cross-linked PE), respectively, and polymer compounds were produced under the same conditions as in Example 1.
[0076] Comparative Example 1 No additive was used, and 100 parts by weight of silane cross-linked polyethylene and 2 parts by weight of the first non-cross-linked polyethylene were mixed to obtain a mixture (FIG. 3: S2). Otherwise, the test was performed in the same manner as in Example 1 to obtain a polymer compound. The gel fraction of the obtained polymer compound was 45%, the tensile strength was 15 MPa, and the elongation was 84%.
[0077] Comparative Example 2 A polymer compound was obtained by carrying out the same test as in Example 1, except that 0.05 parts by weight of EVA was used as the additive. The gel fraction of the obtained polymer compound was 40%, the tensile strength was 14 MPa, and the elongation was 119%.
[0078] Comparative Example 3 A polymer compound was obtained by carrying out the same test as in Example 1, except that 5 parts by weight of EVA was used as the additive. The gel fraction of the obtained polymer compound was 35%, the tensile strength was 16 MPa, and the elongation was 332%.
[0079] Comparative Example 4 A polymer compound was obtained by carrying out the same test as in Example 1, except that 0.05 parts by weight of EEA was used as the additive. The gel fraction of the obtained polymer compound was 41%, the tensile strength was 15 MPa, and the elongation was 348%.
[0080] Comparative Example 5 A polymer compound was obtained by carrying out the same test as in Example 1 except that 5 parts by weight of EEA was used as the additive. The gel fraction of the obtained polymer compound was 34%, the tensile strength was 15 MPa, and the elongation percentage was 358%.
[0081] Comparative Example 6 A mixture was obtained by mixing 100 parts by weight of peroxide-crosslinked polyethylene and 2 parts by weight of a first non-crosslinked polyethylene without using any additives (FIG. 3: S2). Otherwise, the test was carried out in the same manner as in Example 1 to obtain a polymer compound. The gel fraction of the obtained polymer compound was 29%, the tensile strength was 16 MPa, and the elongation was 350%.
[0082] Comparative Example 7 A mixture was obtained by mixing 100 parts by weight of peroxide-crosslinked polyethylene and 5 parts by weight of a first non-crosslinked polyethylene without using any additives (FIG. 3: S2). Otherwise, the test was carried out in the same manner as in Example 1 to obtain a polymer compound. The gel fraction of the obtained polymer compound was 35%, the tensile strength was 13 MPa, and the elongation was 250%.
[0083] Comparative Example 8 A mixture was obtained by mixing 100 parts by weight of peroxide-crosslinked polyethylene and 10 parts by weight of a first non-crosslinked polyethylene without using any additives (FIG. 3: S2). Otherwise, the test was carried out in the same manner as in Example 1 to obtain a polymer compound. The gel fraction of the obtained polymer compound was 40%, the tensile strength was 14 MPa, and the elongation was 220%.
[0084] As shown in Comparative Examples 1 and 6 to 8, when thermal plasticization was performed using only silane-crosslinked polyethylene or peroxide-crosslinked polyethylene and a first non-crosslinked polyethylene without using any additives, the tensile strength was 16 MPa or less and the elongation was 350% or less, which were lower values compared to the Examples.
[0085] In addition, as shown in Comparative Examples 2 to 5, when the amount of ethylene vinyl acetate copolymer (EVA) or ethylene ethyl acrylate copolymer (EEA) added was less than 0.1 parts by weight or more than 3 parts by weight, the tensile strength was 16 MPa or less and the elongation was 358% or less, which were lower values than those in the Examples. Also, the gel fraction was 29% or more in all cases.
[0086] From the above results, it was found that by producing a polymer compound using 0.1 to 3 parts by weight of ethylene-vinyl acetate copolymer (EVA) and / or ethylene-ethyl acrylate copolymer (EEA) as an additive per 100 parts by weight of cross-linked polyethylene, it is possible to obtain a polymer compound that exhibits high physical properties, such as a tensile strength of 18 MPa or more and an elongation of over 450%. [Industrial Applicability]
[0087] According to the present invention, a polymer compound with high physical properties can be produced by using a twin-screw extruder and additives such as ethylene vinyl acetate copolymer (EVA) and ethylene ethyl acrylate copolymer (EEA), which can be used in blow molding and foam molding, which require high tensile strength and elongation. [Explanation of symbols]
[0088] 10 Twin screw extruder 12 cylinders 13 Screw 14 Drive unit 16 First input section 18 First Transportation Department 20 First kneading section 22 First degassing section 24 Second input section 26 Second Transport Department 28 Second kneading section 30 Second degassing section 32 Third Transport Department 34 Discharge section
Claims
1. A method for producing a polymer compound by thermoplasticizing crosslinked polyethylene in an extruder, comprising the steps of: a mixing step of mixing the crosslinked polyethylene, a first non-crosslinked polyethylene, and an additive to form a mixture; a thermoplasticizing step of feeding the mixture through a first feeding portion of the extruder and applying heat and shear stress to thermoplasticize the crosslinked polyethylene; and a kneading step of feeding a second non-crosslinked polyethylene from a second feeding portion of the extruder into the mixture after the thermal plasticizing step and kneading the mixture, the amount of the first non-crosslinked polyethylene in the mixing step is 1 to 5 parts by weight based on 100 parts by weight of the crosslinked polyethylene; The additive comprises at least one non-crosslinked polymer compound selected from ethylene-vinyl acetate copolymer, ethylene-methyl acrylate copolymer, ethylene-ethyl acrylate copolymer, ethylene-methyl methacrylate copolymer, or ethylene-ethyl methacrylate copolymer; The amount of the additive is 0.1 to 3 parts by weight based on 100 parts by weight of the crosslinked polyethylene, The shear stress in the thermoplastic process is 10,000 to 15,000 s -1 for 5 to 30 seconds, A method for producing a polymer compound, characterized in that the amount of the second non-crosslinked polyethylene added in the kneading step is 50 to 150 parts by weight per 100 parts by weight of the crosslinked polyethylene.
2. The method for producing a polymer compound according to claim 1, The method for producing a polymer compound is characterized in that the additive has a melt flow index of 1 to 30 g / 10 min.
3. The method for producing a polymer compound according to claim 1 or 2, A method for producing a polymer compound, characterized in that the polymer compound after the kneading step has a tensile strength of 18 MPa or more and a tensile elongation of more than 450%.
Citation Information
Patent Citations
Method for preparing regenerated product from waste phosphogypsum and waste crosslinked polyethylene
CN114106441A
Reclaiming process for crosslinked polyethylene resin
JP2001131331A
Method for recycling crosslinked polymer, recycling apparatus thereof and wax
JP2005200573A
Regeneration method of crosslinked polyolefin resin
JP2018035247A
Granulator and granulating method
JP2019065092A
Cited By
Polyolefin materials and molded products
JP2026123644A