Method for peeling off skin material and polyurethane foam, and liquid peeling agent used in the method
The method of using a low-SP-value liquid to separate polyurethane foam from laminates under ambient conditions addresses the complexity and cost of existing peeling methods, enhancing recyclability and reducing equipment needs.
Patent Information
- Application Number
- JP2023065159
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-12
- Publication Date
- 2024-10-25
AI Technical Summary
Existing methods for peeling polyurethane foam from laminates require high temperatures and pressures, necessitating costly and complex equipment, which is not suitable for efficient recycling of automobile shredder residue.
A method involving the use of a liquid with an SP value of 15 or less to contact the interface between the skin material and polyurethane foam under non-heating and non-pressurized conditions, allowing for the separation of laminates without adhesives, even in thermally welded or integrally molded structures.
This approach simplifies the peeling process, reduces equipment costs, and improves peelability, enabling efficient recycling of polyurethane foam without quality deterioration.
Smart Images

Figure 2024151646000001 
Figure 2024151646000002
Abstract
Description
[Technical field]
[0001] The present technology relates to a method for peeling a skin material from a polyurethane foam, and more particularly to a method for peeling a skin material from a polyurethane foam in a laminate in which the skin material and the polyurethane foam are laminated, and a peeling solution used in the peeling method. [Background technology]
[0002] The residue that remains after airbags, fluorocarbons, doors, engines, and other parts are removed from used automobiles and then shredded to recover useful metals is called Automotive Shredder Residue (ASR), and the recycling of this ASR determines the final disposal volume of automobile-related waste generated from scrapped vehicles.
[0003] ASR is made up of 70% combustible materials such as resin and urethane by weight, and is recycled as thermal energy at incineration facilities, but recent efforts to reduce greenhouse gas emissions have called for a reduction in the proportion of ASR burned for heat and an increase in the proportion reused as a resource. Many parts used in vehicle seats and interior materials in particular are made up of multiple materials, and technology is being developed to separate these laminates for recycling.
[0004] For example, Patent Document 1 proposes a method for peeling a polyurethane foam from a polyurethane foam composite having a polyurethane foam and a laminated portion such as a resin, sheet or metal plate bonded to at least one surface thereof, in which the polyurethane foam composite is heat-treated in a treatment liquid whose main component is water at a temperature of 180°C or less in a closed space to peel the laminated portion from the polyurethane foam composite, thereby enabling the peeled and regenerated materials to be reused as they are without any deterioration. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 6-220245 Summary of the Invention [Problem to be solved by the invention]
[0006] The peeling technique of Patent Document 1 involves heat treatment in a treatment solution at a temperature of 180°C or less for 20 to 80 minutes under high pressure, but it is believed that a strong, airtight container is required to achieve the specified temperature and pressure. On the other hand, in recycling, there is a demand for cost reduction and for the process to be carried out using as simple equipment and conditions as possible.
[0007] Therefore, the main object of this technology is to provide a technology that enables peeling of a skin material and a polyurethane foam in a low-cost and simple manner. [Means for solving the problem]
[0008] In the present technology, first, a method for peeling a skin material and a polyurethane foam from a laminate in which the skin material and the polyurethane foam are laminated, comprising the steps of: A liquid having a solubility parameters (SP) value of 15 or less is brought into contact with the interface between the skin material and the polyurethane foam. Or, bringing a liquid into contact with the interface between the skin material and the polyurethane foam under non-heating conditions; A method of stripping is provided, comprising the step of contacting. In the peeling method according to the present technology, the contacting step can be performed under a non-pressurized condition. The peeling method according to the present technology makes it possible to peel off a laminate in which no adhesive material is present between the skin material and the polyurethane foam layers. Moreover, the peeling method according to the present technology makes it possible to peel off a laminate in which the skin material and the polyurethane foam are thermally welded or integrally molded.
[0009] Next, the present technology provides a peeling liquid for peeling off a skin material and a polyurethane foam in a laminate in which the skin material and the polyurethane foam are laminated, the peeling liquid comprising: Liquids with a Solubility Parameters value of 15 or less, Or, a liquid for contacting the interface between the skin material and the polyurethane foam under non-heated conditions; The present invention provides a liquid peeling agent containing the above as an active ingredient. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] A preferred embodiment for carrying out the present technology will be described below. The embodiments described below are examples of typical embodiments of the present technology, and any of the embodiments can be combined. In addition, the scope of the present technology is not narrowly interpreted by these.
[0011] 1. Peeling method The peeling method according to the present technology is a method for peeling a skin material from a polyurethane foam in a laminate in which the skin material and the polyurethane foam are laminated, and is a method that performs a contacting step. More specifically, the peeling method according to the present technology is a method that performs a contacting step of contacting the interface between the skin material and the polyurethane foam with a liquid having an SP (Solubility Parameters) value of 15 or less, or a contacting step of contacting the interface between the skin material and the polyurethane foam with a liquid under non-heating conditions.
[0012] In the present technology, "contacting the interface between the skin material and the polyurethane foam with a liquid" includes all manners in which the liquid reaches a part or the whole of the interface between the skin material and the polyurethane foam. Examples of methods for contacting the interface between the skin material and the polyurethane foam with a liquid include a method of immersing a part or the whole of the laminate in a liquid, a method of immersing a part or the whole of the skin material and / or the polyurethane foam in a liquid, and a method of applying the liquid from the skin material side and / or the polyurethane foam side by spraying or the like and allowing it to permeate and reach the interface between the skin material and the polyurethane foam.
[0013] As the liquid that can be used in the peeling method according to the present technology, one or more liquids that can permeate polyurethane foam can be freely selected and used, such as water, methanol, ethanol, isopropanol, acetone, methylene chloride, ethyl acetate, ethyl ether, hexane, tetrahydrofuran, etc.
[0014] Of these, it is preferable to use water from the viewpoint of reducing costs.
[0015] From the viewpoint of improving the releasability, it is preferable to use a liquid having an SP value of 25 or less, more preferably to use a liquid having an SP value of 20 or less, and even more preferably to use a liquid having an SP value of 15 or less. The lower limit of the SP value of the liquid used is not particularly limited as long as it does not impair the action and effect of the present technology, but is, for example, 5.0 or more, preferably 5.5 or more, more preferably 6.0 or more, even more preferably 6.5 or more, even more preferably 7.0 or more, and particularly preferably 7.5 or more. A liquid having an SP value in this range has high wettability into polyurethane foam, and can further improve the releasability between the skin material and the polyurethane foam.
[0016] From the viewpoint of improving the releasability, it is preferable to use a liquid having a relative dielectric constant of 1.8 or more, more preferably a liquid having a relative dielectric constant of 2.0 or more, and even more preferably a liquid having a relative dielectric constant of 5.0 or more. The upper limit of the relative dielectric constant of the liquid used is not particularly limited as long as it does not impair the action and effect of the present technology, but is, for example, 80 or less, preferably 60 or less, more preferably 40 or less, even more preferably 35 or less, and particularly preferably 30 or less. A liquid having a relative dielectric constant in this range has high wettability into polyurethane foam, and can further improve the releasability between the skin material and the polyurethane foam.
[0017] For reference, the SP values and relative dielectric constants of the liquids exemplified above are shown in Table 1 below.
[0018] [Table 1]
[0019] Furthermore, from the viewpoint of recycling, it is preferable to use methanol, ethanol, isopropanol, acetone, methylene chloride, tetrahydrofuran, ethyl acetate, ethyl ether, etc. The reason is as follows. After separation into the skin material and the polyurethane foam, the polyurethane foam is widely studied for decomposing its resin and regenerating it into the constituent alcohol compounds. Polyurethane foam contains many additives such as flame retardants depending on its application, and these additives are avoided in the process of regenerating the constituents into alcohol compounds. However, in peeling the skin material and the polyurethane foam, in addition to improving the peelability, the additives in the polyurethane foam are extracted, making it easier to regenerate the polyurethane foam into alcohol compounds and contributing to improving the quality of the regenerated alcohol compounds by contacting the polyurethane foam with a liquid such as methanol, ethanol, isopropanol, acetone, methylene chloride, tetrahydrofuran, ethyl acetate, ethyl ether, etc.
[0020] In this technology, the contact step can be performed under non-heating conditions. As will be demonstrated in the examples described later, this technology has succeeded in sufficiently increasing the peelability between the skin material and the polyurethane foam even under non-heating conditions. As a result, it is possible to simplify the equipment required for the peeling operation and also contribute to reducing the cost required for the peeling operation.
[0021] In this technology, "under non-heating conditions" means conditions under which active heating is not performed. For example, cases where the temperature of the liquid rises due to differences in temperature between the storage location or container of the liquid and the location or container in which the contacting step is performed, where the temperature of the liquid rises due to seasonal or weather changes, and where the temperature of the liquid or polyurethane foam rises due to some chemical reaction proceeding in the contacting step are all included in the "under non-heating conditions" of this technology.
[0022] In the contact step in the peeling method according to the present technology, it is possible to achieve sufficient improvement in peelability even under non-heating conditions, but there is no intention to exclude heating. Depending on the type of liquid used, it is possible to adjust the temperature of the liquid to a temperature that provides the optimum viscosity for contact, or to adjust the temperature of the liquid or laminate to a temperature condition suitable for contact work. Specifically, in the contact step, the liquid and / or laminate can be adjusted to, for example, 0°C or higher, preferably 5°C or higher, and more preferably 10°C or higher. In addition, in the contact step, the liquid and / or laminate can be adjusted to, for example, 95°C or lower, preferably 80°C or lower, more preferably 70°C or lower, and even more preferably 50°C or lower.
[0023] In this technology, the contact step can be performed under non-pressurized conditions. As will be demonstrated in the examples described later, this technology has succeeded in sufficiently improving the peelability between the skin material and the polyurethane foam even under non-pressurized conditions. As a result, it is possible to simplify the equipment required for the peeling operation and also contribute to reducing the cost required for the peeling operation.
[0024] In this technology, "under non-pressurized conditions" means conditions under which no active pressurization is performed. For example, the following are included in the "non-pressurized conditions" of this technology: a case where the pressure in the contact process increases due to differences in the atmospheric pressure between the storage location or container of the liquid and the location or container in which the contact process is performed; a case where the pressure in the contact process increases due to seasonal or weather changes; a case where the pressure in the container increases due to evaporation of the liquid; a case where the pressure in the contact process increases due to the progress of some chemical reaction in the contact process; and the like.
[0025] In the contact step in the peeling method according to the present technology, it is possible to achieve sufficient improvement in peelability even under non-pressurized conditions, but there is no intention to exclude the use of pressure. Depending on the type of liquid used, it is possible to adjust the pressure in the contact step to, for example, obtain the optimum viscosity for contact, or to adjust the pressure in the contact step to suit the contact work. Specifically, the pressure in the contact step can be adjusted to, for example, 0.7 atm or more, preferably 0.8 atm or more, more preferably 0.85 atm or more. In addition, the pressure in the contact step can be adjusted to, for example, 1.4 atm or less, preferably 1.3 atm or less, more preferably 1.2 atm or less.
[0026] The contact time in the contact step can be appropriately adjusted according to the type of skin material or polyurethane foam to be peeled off, the type of liquid, etc., as long as it does not impair the action and effect of the present technology. The lower limit of the contact time in the contact step is, for example, 10 seconds or more, preferably 15 seconds or more, more preferably 20 seconds or more, and even more preferably 30 seconds or more. By setting the lower limit of the contact time in this range, it is possible to reliably improve the peelability. The upper limit of the contact time in the contact step is, for example, 24 hours or less, preferably 12 hours or less, more preferably 6 hours or less, even more preferably 1 hour or less, particularly preferably 30 minutes or less, 10 minutes or less, or 5 minutes or less. By setting the upper limit of the contact time in the contact step in this range, it is possible to shorten the time required for peeling and prevent deterioration of the quality of the polyurethane foam after peeling.
[0027] 2.Laminate to be peeled As for the laminate that can be peeled off by the peeling method according to the present technology, if the laminate is a laminate in which a skin material and a polyurethane foam are laminated, the skin material and the polyurethane foam can be peeled off.
[0028] The peeling method according to the present technology is very suitable for peeling a laminate in which no adhesive material is present between the layers of a skin material and a polyurethane foam. In this technology, "no adhesive material is present" means that no adhesive components other than the skin material and the polyurethane foam are present between the layers. In other words, when the skin material and the polyurethane foam are thermally welded, the surface of the skin material and / or the polyurethane foam melts and the skin material itself and / or the polyurethane foam itself are present between the layers as adhesive components, which is included in the "no adhesive material is present" of the present technology.
[0029] The peeling method according to the present technology is very suitable for peeling off a laminate in which a skin material and a polyurethane foam are heat-welded or integrally molded. An example of a heat-welding method is frame lamination. Frame lamination is a technique in which the surface of the polyurethane foam is melted with a flame and heat-welded to the skin material. An integral molding method is a method in which an unfoamed composition, which is the raw material of the polyurethane foam, is foamed and molded while attached to the skin material.
[0030] The polyurethane foam has a cellular structure, and is bonded to the skin material at the points where the cellular structure comes into contact. Although the bond is small, the adhesive strength is sufficient, so that when an attempt is made to peel the polyurethane foam off, the polyurethane foam breaks because the adhesive strength is stronger than the strength of the polyurethane foam, and the laminate cannot be separated. However, by carrying out the contact step of the peeling method according to the present technology and bringing a liquid into contact with the interface between the skin material and the polyurethane foam, the strength of the bonded points is reduced, and it becomes possible to easily peel the polyurethane foam off of the skin material without breaking it.
[0031] The peeling method according to the present technology can perform peeling even when an adhesive material is interposed between the layers of the skin material and the polyurethane foam, depending on the type of adhesive material. For example, when a type of polyurethane foam different from the polyurethane foam constituting the laminate is used as the adhesive material, or when an adhesive material that is permeable to the liquid used and whose adhesive strength can be reduced by the liquid used is used, peeling can be performed using the peeling method according to the present technology even when an adhesive material is interposed between the layers of the skin material and the polyurethane foam.
[0032] The material and structure of the skin material constituting the laminate that can be peeled off are not particularly limited as long as they do not impair the action and effect of the present technology. Examples of the material of the skin material include polyester resin, vinyl chloride resin, urethane resin, acrylic resin, nylon, rayon, natural fiber, etc., and examples of the structure of the skin material include knitted fabric, woven fabric, resin sheet, film material, etc. In particular, even skin materials that have been coated with resin such as acrylic as a backing material, or that have been treated to provide functional additives such as flame retardants and deodorants, or to improve durability, can be peeled off by the peeling method according to the present technology.
[0033] The material and structure of the polyurethane foam constituting the laminate that can be the subject of peeling are not particularly limited as long as they do not impair the action and effect of the present technology. Flexible polyurethane foam, rigid polyurethane foam, and semi-rigid polyurethane foam manufactured using materials used in the manufacture of general polyurethane foam, as well as flexible polyurethane foam, rigid polyurethane foam, and semi-rigid polyurethane foam having known or future functions can be the subject of peeling by the peeling method according to the present technology.
[0034] The physical properties of the polyurethane foam constituting the laminate that can be peeled off are not particularly limited as long as they do not impair the action and effect of the present technology. 3 , preferably with a density of 20 to 60 kg / m 3 , and more preferably, the density is 25 to 45 kg / m 3The polyurethane foams described above can be preferable targets for the peeling method according to the present technology. Note that the density in the present technology is a value measured in accordance with JIS K 7222:2005.
[0035] The polyurethane foam constituting the laminate that can be peeled off is produced using a composition for producing polyurethane foam that contains polyol, a blowing agent, a catalyst, a foam stabilizer, isocyanate, and other additives as necessary. The raw materials for polyurethane foam will be described below.
[0036] <Polyol> The polyol used in the polyurethane foam production composition can be one or more polyols that can be used in the production of polyurethane foam, as long as the action and effect of the present technology are not impaired. Examples of the polyol include polyether polyols obtained by adding alkylene oxides such as ethylene oxide (EO) and propylene oxide (PO) to polyhydric alcohols such as ethylene glycol, diethylene glycol, propylene glycol, dipropylene glycol, butylene glycol, neopentyl glycol, glycerin, pentaerythritol, trimethylolpropane, sorbitol, and sucrose; polyester polyols obtained by polycondensation of aliphatic carboxylic acids such as malonic acid, succinic acid, and adipic acid, or aromatic carboxylic acids such as phthalic acid, and aliphatic glycols such as ethylene glycol, diethylene glycol, and propylene glycol; polyether ester polyols obtained by reacting the polyether polyols with polybasic acids to form polyesters; and polyether ester polyols having both polyether and polyester segments in one molecule. Among these, the target to be peeled by the peeling method according to the present technology is preferably a polyurethane foam produced using a polyol having an ester group, specifically a polyester polyol and / or a polyether ester polyol.
[0037] <Foaming agent> The blowing agent used in the polyurethane foam-producing composition can be one or more blowing agents that can be used in the production of polyurethane foam, as long as the action and effect of the present technology is not impaired. Examples of the blowing agent include water, methylene chloride, carbon dioxide gas, and hydrocarbons such as pentane. The amount of the blowing agent used is not particularly limited as long as the action and effect of the present technology is not impaired, but it is preferable to use, for example, 1 to 8 parts by mass of the blowing agent per 100 parts by mass of polyol.
[0038] <Catalyst> The catalyst used in the polyurethane foam producing composition can be one or more catalysts that can be used in the production of polyurethane foam, as long as the action and effect of the present technology is not impaired. Examples of the catalyst include amine-based catalysts such as triethylamine, dimethylaminohexanol, triethylenediamine, and tetramethylguanidine; tin-based catalysts such as stannous octoate; and metal catalysts (also called organometallic catalysts) such as phenylmercury propionate and lead octenate. The amount of the catalyst used is not particularly limited as long as the action and effect of the present technology is not impaired. For example, it is preferable to use 0.1 to 2 parts by mass of the catalyst per 100 parts by mass of polyol.
[0039] <Foam stabilizer> The foam stabilizer used in the polyurethane foam-producing composition may be one or more foam stabilizers that can be used in the production of polyurethane foam, as long as the action and effect of the present technology is not impaired. Examples of the foam stabilizer include silicone-based foam stabilizers, fluorine-containing compound-based foam stabilizers, and surfactants. The amount of the foam stabilizer used is not particularly limited as long as the action and effect of the present technology is not impaired, but it is preferable to use, for example, 0.5 to 3 parts by mass of the foam stabilizer per 100 parts by mass of polyol.
[0040] <Isocyanate> The isocyanate used in the polyurethane foam production composition can be freely selected from one or more isocyanates that can be used in the production of polyurethane foam, as long as the action and effect of the present technology are not impaired. Examples of isocyanates include aliphatic isocyanates such as hexamethylene diisocyanate, isophorone diisocyanate, and dicyclohexamethane diisocyanate; aromatic isocyanates such as toluene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), naphthalene diisocyanate, xylylene diisocyanate, and polymeric polyisocyanate (crude MDI); and modified polyisocyanates obtained by modifying these. Among these, polyurethane foam produced using toluene diisocyanate (TDI) is preferred as the target of the peeling method according to the present technology.
[0041] The isocyanate index of the polyurethane foam to be peeled is not particularly limited as long as it does not impair the action and effect of the present technology, but for example, a polyurethane foam having an isocyanate index of 90 to 120 can be a preferred target for peeling by the peeling method according to the present technology. Note that, in the present technology, the isocyanate index is a value calculated by [(isocyanate equivalent in the composition for producing polyurethane foam / active hydrogen equivalent in the composition for producing polyurethane foam)×100].
[0042] <Other> In the composition for producing polyurethane foam, one or more of various other components that can be used in the production of polyurethane foam can be freely selected according to the purpose, as long as the action and effect of the present technology are not impaired. For example, flame retardants, stabilizers, plasticizers, colorants, pigments, antioxidants, crosslinking agents, antibacterial agents, dispersants, ultraviolet absorbers, etc. can be mentioned. In addition, it is preferable that the other components used in the composition for producing polyurethane foam are components that are soluble in the stripping solution described below. If the components are soluble in the stripping solution, they can be dissolved from the polyurethane foam in the contact step, which contributes to improving the recyclability of the polyurethane foam.
[0043] 3. Stripping solution The stripping solution according to the present technology is a stripping solvent for stripping a skin material and a polyurethane foam in a laminate in which the skin material and the polyurethane foam are laminated, and is a liquid having an SP (Solubility Parameters) value of 15 or less as an active ingredient, or a liquid for contacting the interface between the skin material and the polyurethane foam under non-heating conditions. Details of the liquid that is the active ingredient of the stripping solution are the same as the liquid used in the contact step of the stripping method according to the present technology described above, and therefore will not be described here.
[0044] In addition to the liquid, other components can be used in the stripping solution according to the present technology, as long as the action and effect of the present technology are not impaired. As other components, for example, preservatives, pH adjusters, colorants, stabilizers, and other components that are normally used in liquid formulations can be used. Furthermore, components having known or future functions can be used in combination depending on the purpose.
[0045] In addition, the present technology can also have the following configuration. (1) A method for peeling a skin material from a polyurethane foam in a laminate having the skin material and the polyurethane foam laminated therein, comprising the steps of: A liquid having a solubility parameters (SP) value of 15 or less is brought into contact with the interface between the skin material and the polyurethane foam. Or, bringing a liquid into contact with the interface between the skin material and the polyurethane foam under non-heating conditions; A peeling method comprising a contacting step. (2) The peeling method according to (1), wherein the contacting step is carried out under a non-pressurized condition. (3) The peeling method according to (1) or (2), wherein no adhesive material is interposed between the skin material and the polyurethane foam. (4) The peeling method according to any one of (1) to (3), wherein the skin material and the polyurethane foam are heat-welded or integrally molded. (5) A peeling liquid for peeling a skin material and a polyurethane foam from a laminate in which the skin material and the polyurethane foam are laminated, comprising: Liquids with a Solubility Parameters value of 15 or less, Or, a liquid for contacting the interface between the skin material and the polyurethane foam under non-heated conditions; A peeling liquid containing the following as an active ingredient. EXAMPLES
[0046] The present technology will be described in more detail below based on examples. Note that the examples described below are representative examples of the present technology, and the scope of the present technology is not to be interpreted narrowly by these examples.
[0047] <Experimental Example 1> In Experimental Example 1, in a laminate in which a skin material and a polyurethane foam are laminated, the influence on separation of the skin material and the polyurethane foam due to differences in the type of liquid used for separating the skin material and the polyurethane foam was examined.
[0048] (1) Preparation of test specimens The test subject was a product made by laminating a surface material "Aperto" (woven polyester resin fabric) manufactured by Suminoe Teijin Techno Co., Ltd. and polyurethane foam "EL-67F" manufactured by Inoac Corporation using a frame laminate. A product with a thickness of 5 mm was cut to a size of 25.4 mm wide and 150 mm long to prepare a test specimen.
[0049] (2) Test method The test piece prepared above was immersed in the liquid shown in Table 2 below for 1 minute, squeezed, and then subjected to the following peel strength test before the liquid dried. When no liquid was used, the test piece prepared above was subjected to the following peel strength test without any treatment. The appearance after peeling was evaluated according to the following evaluation criteria.
[0050] [Peel strength test] The peel strength of the skin material and urethane foam of a laminate made by frame laminating "Aperto" manufactured by Suminoe Teijin Techno Co., Ltd. and urethane foam "EL-67F" manufactured by Inoac Corporation was measured using a tensile tester "ZTA-50N" manufactured by Imada Co., Ltd. Specifically, the laminate with a thickness of 5 mm was cut into a size of 25.4 mm wide and 150 mm long to prepare a test piece, and only the skin material was peeled off from the short side of the test piece. The urethane foam part that had been peeled off from the skin material was attached to the tensile tester and peeled off at a tensile speed of 200 mm / min, and the maximum load at this time was measured.
[0051] [Appearance evaluation] ◎: The polyurethane foam peels off cleanly from the skin. ○: Small pieces of polyurethane foam remain on part of the surface of the skin material. △: Small pieces of polyurethane foam remain on the entire surface of the skin material ×: The polyurethane foam broke during the process and could not be peeled off from the skin.
[0052] (3) Results The results are shown in Table 2. Table 2 also shows the SP value and relative dielectric constant of each solution.
[0053] [Table 2]
[0054] (4) Discussion As shown in Table 2, when no liquid was contacted, the peel strength during peeling was high, the polyurethane foam broke midway, and it was impossible to peel it off from the skin material. On the other hand, by contacting the liquid under non-heated and non-pressurized conditions, the peel strength during peeling decreased, and the appearance after peeling was good.
[0055] When comparing by type of liquid, liquids with an SP value of 15 or less had lower peel strength during peeling and better appearance after peeling than water with an SP value of over 15. When comparing by dielectric constant, liquids with a dielectric constant of 60 or less had lower peel strength during peeling and better appearance after peeling than water with a high dielectric constant. On the other hand, liquids with a dielectric constant of 1.9 or more had lower peel strength during peeling and better appearance after peeling than hexane with a very low dielectric constant.
Claims
1. A method for peeling a skin material from a polyurethane foam in a laminate having the skin material and the polyurethane foam laminated therein, comprising the steps of: A liquid having an SP (Solubility Parameters) value of 15 or less is brought into contact with the interface between the skin material and the polyurethane foam. Or, bringing a liquid into contact with the interface between the skin material and the polyurethane foam under non-heating conditions; A peeling method comprising a contacting step.
2. The peeling method according to claim 1 , wherein the contacting step is carried out under a non-pressurized condition.
3. The peeling method according to claim 1 , wherein no adhesive material is interposed between the skin material and the polyurethane foam.
4. The peeling method according to claim 1 , wherein the skin material and the polyurethane foam are heat-welded or integrally molded.
5. A peeling liquid for peeling a skin material and a polyurethane foam from a laminate in which the skin material and the polyurethane foam are laminated, comprising: Liquids with a SP (Solubility Parameters) value of 15 or less; Or, a liquid for contacting the interface between the skin material and the polyurethane foam under non-heated conditions; A peeling liquid containing the following as an active ingredient.
Citation Information
Patent Citations
Method for separating polyurethane composite foam
JP1994220245A