Millable silicone rubber composition and cured product thereof

A millable silicone rubber composition using specific components enables primary vulcanization to achieve low compression set, addressing energy inefficiencies and vulcanization issues in existing technologies, suitable for gaskets and packings.

JP2024151709AActive Publication Date: 2024-10-25SHIN ETSU CHEMICAL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023065283
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-13
Publication Date
2024-10-25
Estimated Expiration
2043-04-13

AI Technical Summary

Technical Problem

Existing silicone rubber compositions require secondary vulcanization to achieve a sufficiently small compression set, which is inefficient in terms of energy usage, and using sulfur-containing compounds can lead to vulcanization property deterioration and addition cure inhibition.

Method used

A millable silicone rubber composition comprising organopolysiloxane, surface-treated reinforcing silica, chain aliphatic alcohol, organohydrogenpolysiloxane, and a hydrosilylation reaction catalyst, which allows for primary vulcanization to achieve a low compression set without secondary vulcanization.

Benefits of technology

The composition results in a silicone rubber cured product with a low compression set after primary vulcanization, suitable for applications like gaskets and packings, with improved mechanical properties and reduced energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024151709000001
    Figure 2024151709000001
  • Figure 2024151709000002
    Figure 2024151709000002
  • Figure 2024151709000003
    Figure 2024151709000003
Patent Text Reader

Abstract

To provide a millable silicone rubber composition that yields a silicone rubber cured product with low compression set using only primary vulcanization.SOLUTION: A millable silicone rubber composition includes (A) an organopolysiloxane with a weight-average degree of polymerization of 1,000-100,000, including two or more alkenyl groups bonded to silicon atoms in one molecule, in an amount of 100 pts.mass, (B) surface-treated reinforcing silica with a BET-based specific surface area of 50 m2 / g or more in an amount of 10-100 pts.mass, (C) an open-chain aliphatic alcohol with a boiling point of 170°C or higher in an amount of 0.1-10 pts.mass, (D) an organohydrogenpolysiloxane including two or more hydrogen atoms (hydrosilyl groups) bonded to silicon atoms in one molecule, in such an amount that the molar ratio of hydrosilyl groups in component (D) to silicon atom-bonded alkenyl groups in component (A) is 0.5-10, and (E) a catalyst for hydrosilylation in a catalytic amount.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a millable silicone rubber composition and a cured product thereof. [Background technology]

[0002] Silicone rubber has excellent properties such as weather resistance, electrical properties, low compression set, heat resistance, and cold resistance.

[0003] The silicone rubber composition can be molded and cured by a conventional method, and the molding method can be selected from injection molding, transfer molding, injection molding, compression molding, etc., which is the most suitable method for the purpose. The curing method can adopt heat treatment (primary vulcanization) conditions at 40 to 230°C for about 3 seconds to 160 minutes. Furthermore, in order to reduce compression set, secondary vulcanization (post cure) is performed at 40 to 230°C for about 10 minutes to 24 hours.

[0004] In recent years, there has been a demand for reducing electricity consumption in order to achieve carbon neutrality. However, there is a problem that if post-vulcanization is not performed, it is difficult to obtain a product with a sufficiently small compression set.

[0005] Patent Document 1 describes that the inclusion of cerium oxide hydrate and zirconium oxide hydrate improves the heat resistance and compression set of silicone rubber. However, there is no specific description that good compression set properties can be obtained by primary vulcanization alone, and the above problem remains unresolved.

[0006] Patent Document 2 describes that the use of a sulfur-containing compound makes it possible to obtain a silicone rubber cured product with excellent compression set properties even with only primary vulcanization. However, the use of a sulfur-containing compound can cause addition cure inhibition, which can deteriorate the vulcanization properties.

[0007] Patent Document 3 describes that silicone rubber cured products containing reinforcing fillers that have been surface-treated with benzotriazole derivatives have low compression set. It also describes that the deterioration of vulcanization properties can be suppressed, but none of these results have reached a level that can withstand practical use. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2014-031408 A [Patent Document 2] JP 2016-196591 A [Patent Document 3] JP 2017-165931 A Summary of the Invention [Problem to be solved by the invention]

[0009] Therefore, an object of the present invention is to provide a millable type silicone rubber composition which, upon primary vulcanization alone, produces a cured silicone rubber product with small compression set. [Means for solving the problem]

[0010] As a result of extensive research into the above-mentioned problems, the present inventors have discovered that by adding a specific alcohol, a millable type silicone rubber composition can be obtained that can reduce the compression set of the cured product even when only the primary vulcanization is performed. That is, the present invention provides the following millable type silicone rubber composition and cured product thereof.

[0011] [1] (A) an organopolysiloxane having two or more alkenyl groups bonded to silicon atoms in each molecule and a weight average degree of polymerization of 1,000 to 100,000; 100 parts by mass, (B) The specific surface area by the BET method is 50 m 2 / g or more of surface-treated reinforcing silica; 10 to 100 parts by mass, (C) a chain aliphatic alcohol having a boiling point of 170° C. or higher; 0.1 to 10 parts by mass, (D) an organohydrogenpolysiloxane containing two or more silicon-bonded hydrogen atoms (hydrosilyl groups) per molecule; an amount such that the molar ratio of hydrosilyl groups in component (D) to silicon-bonded alkenyl groups in component (A) is 0.5 to 10; and (E) a hydrosilylation catalyst; a catalytic amount; A millable type silicone rubber composition comprising: [2] The millable type silicone rubber composition according to [1], wherein component (C) is one or more selected from the group consisting of 1-octanol, 1-nonanol, 1-dodecanol, 2-ethyl-1-hexanol, 2,6-dimethyl-4-heptanol, 3,5,5-trimethyl-1-hexanol, and ethylene glycol. [3] A cured product of the millable silicone rubber composition according to [1] or [2]. Effect of the Invention

[0012] The present invention can provide a millable silicone rubber composition that can be cured into a silicone rubber with small compression set after only primary vulcanization. Therefore, the cured product of the millable silicone rubber composition of the present invention is useful for applications such as gaskets, such as O-rings and packings. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The present invention will be described in detail below, but the present invention is not limited thereto.

[0014] In this specification, the mixture of components (A), (B), and (C) described below before components (D) and (E) are blended is referred to as the (millable type) silicone rubber compound, and the mixture of this silicone rubber compound with components (D) and (E) is referred to as the (millable type) silicone rubber composition.

[0015] [Component (A)] In the present invention, component (A) is an organopolysiloxane having a weight average degree of polymerization of 1,000 to 100,000 and containing two or more alkenyl groups bonded to silicon atoms in each molecule, and is the base polymer (main component) of the composition according to the present invention.

[0016] The organopolysiloxane used as component (A) has at least two alkenyl groups in one molecule, preferably from 2 to 50, and more preferably from 2 to 20. The alkenyl groups may be bonded to silicon atoms at the molecular chain terminals, or may be bonded to silicon atoms in the middle of the molecular chain (non-terminal molecular chain), or may be both, but are preferably bonded to silicon atoms at the molecular chain terminals.

[0017] The alkenyl group bonded to the silicon atom in component (A) typically has 2 to 8 carbon atoms, and preferably has 2 to 4 carbon atoms. Examples of alkenyl groups include vinyl, allyl, propenyl, butenyl, and hexenyl groups; and cycloalkenyl groups such as cyclohexenyl groups. Of these, vinyl and allyl groups are preferred, and vinyl groups are particularly preferred. Examples of groups other than the alkenyl group include an alkyl group having 1 to 10 carbon atoms, a cycloalkyl group having 5 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, and an aralkyl group having 7 to 10 carbon atoms. Specific examples include alkyl groups such as a methyl group, an ethyl group, a propyl group, a butyl group, a hexyl group, and an octyl group; cycloalkyl groups such as a cyclopentyl group and a cyclohexyl group; aryl groups such as a phenyl group and a tolyl group; and aralkyl groups such as a benzyl group and a 2-phenylethyl group. Of the above, a methyl group and a phenyl group are preferred, and a methyl group is particularly preferred.

[0018] The molecular structure of the organopolysiloxane of component (A) is preferably linear or partially branched. Specifically, the repeating structure of the diorganosiloxane unit constituting the main chain of the organopolysiloxane is preferably composed of only repeating dimethylsiloxane units, or the like in which diorganosiloxane units having phenyl groups, vinyl groups, or the like as substituents, such as diphenylsiloxane units, methylphenylsiloxane units, or methylvinylsiloxane units, are introduced as part of the dimethylpolysiloxane structure composed of repeating dimethylsiloxane units constituting the main chain.

[0019] In addition, both molecular chain terminals are preferably blocked with triorganosiloxy groups such as trimethylsiloxy groups, dimethylphenylsiloxy groups, vinyldimethylsiloxy groups, divinylmethylsiloxy groups, and trivinylsiloxy groups.

[0020] Such organopolysiloxanes can be obtained, for example, by (co)hydrolyzing and condensing one or more organohalogenosilanes, or by ring-opening polymerization of a cyclic polysiloxane (e.g., a siloxane trimer or tetramer) using an alkaline or acidic catalyst.

[0021] The degree of polymerization of the organopolysiloxane is 1,000 to 100,000, preferably 2,000 to 100,000, more preferably 2,000 to 50,000, and particularly preferably 3,000 to 20,000. The organopolysiloxane is characterized by being in a raw rubber state (non-liquid state) without self-flowability at room temperature (25°C). If the degree of polymerization is less than 1,000, problems such as roll adhesion will occur when the organopolysiloxane is made into a silicone rubber compound, and roll workability will deteriorate. The degree of polymerization in the present invention is determined as the weight-average degree of polymerization from the weight-average molecular weight in terms of polystyrene by gel permeation chromatography (GPC) analysis measured under the following conditions. [Measurement conditions] Developing solvent: toluene Flow rate: 0.35mL / min Detector: Refractive index detector (RI) Column: TSK Guardcolumn SuperH-L TSKgel SuperH4000(6.0mmI.D.×15cm×1) TSKgel SuperH3000(6.0mmI.D.×15cm×1) TSKgel SuperH2000(6.0mmI.D.×15cm×2) (All manufactured by Tosoh Corporation) Column temperature: 40℃ Sample injection volume: 10 μL (toluene solution with a concentration of 0.5% by mass)

[0022] The component (A) may be a single type, or a mixture of two or more types differing in molecular weight (degree of polymerization) or molecular structure.

[0023] [(B) Component] The surface-treated reinforcing silica of component (B) acts as a component that imparts excellent mechanical properties to the resulting silicone rubber composition. The reinforcing silica may be either precipitated silica (wet silica) or fumed silica (dry silica). In the present invention, the surface-treated reinforcing silica of component (B) has a specific surface area of ​​50 m2 or less as measured by the BET method. 2 / g or more, and preferably 100 to 400m 2 / g. This specific surface area is 50m 2 If it is less than 1 / g, the reinforcing effect of component (B) will be insufficient.

[0024] The reinforcing silica of component (B) is surface-treated with an organosilicon compound such as silanol-containing organopolysiloxane, organopolysilazane, chlorosilane, alkoxysilane, etc. These reinforcing silicas may be used alone or in combination of two or more.

[0025] The amount of reinforcing silica (B) added is 10 to 100 parts by mass, preferably 15 to 80 parts by mass, and more preferably 20 to 70 parts by mass, per 100 parts by mass of the organopolysiloxane (A). If the amount added is outside the above range, not only will the processability of the silicone rubber composition decrease, but the mechanical properties of the cured silicone rubber will also be insufficient.

[0026] [(C) component] Component (C) is a chain aliphatic alcohol with a boiling point of 170° C. or higher, and is a component for reducing the compression set of the cured product after primary vulcanization. The alcohol of component (C) has a boiling point of 170° C. or higher, and preferably has a boiling point of 170 to 300° C. As long as the boiling point is within this range, the structure does not matter, but a chain aliphatic alcohol having 2 to 24 carbon atoms is preferred, and a monovalent chain aliphatic alcohol having 2 to 24 carbon atoms is particularly preferred. It should be noted that, since alcohols having an alkynyl group containing a C≡C triple bond are used as hydrosilylation reaction inhibitors, acetylene alcohol-based inhibitors described below are not considered to be included in component (C).

[0027] Examples of the chain aliphatic alcohols having a boiling point of 170°C or higher as component (C) include 1-octanol (194-195°C), 1-nonanol (215°C), 1-dodecanol (259°C), 2-ethyl-1-hexanol (184-185°C), 2,6-dimethyl-4-heptanol (176°C), 3,5,5-trimethyl-1-hexanol (193-202°C), and ethylene glycol (197.3°C) (the boiling points of each substance are shown in parentheses). These alcohols may be used alone or in combination of two or more. The boiling point of component (C) of the present invention is the value listed on the Ministry of Health, Labor and Welfare's "Workplace Safety Site" (https: / / anzeninfo.mhlw.go.jp / anzen_pg / GHS_MSD_FND.aspx).

[0028] The amount of alcohol (C) blended is 0.1 to 10 parts by mass, and preferably 0.3 to 5 parts by mass, per 100 parts by mass of the organopolysiloxane (A). If it is less than 0.1 part by mass, the effect of improving compression set cannot be obtained, and if it is more than 10 parts by mass, the hardness of the cured product of the obtained silicone rubber composition may be too low, and it is also economically undesirable.

[0029] [(D) component] The (D) component is an organohydrogenpolysiloxane containing two or more hydrogen atoms (hydrosilyl groups) bonded to silicon atoms in one molecule. The organohydrogenpolysiloxane may have a linear, cyclic, branched, or three-dimensional network structure, so long as it contains two or more, preferably three or more, more preferably 3 to 200, and even more preferably 4 to 100 hydrosilyl groups in one molecule, and any organohydrogenpolysiloxane known as a crosslinking agent for addition reaction curing silicone rubber compositions can be used, and for example, an organohydrogenpolysiloxane represented by the following average composition formula (1) can be used. R 1 a H b SiO (4-a-b) / 2 (1)

[0030] In the above average composition formula (1), R 1 are each independently a monovalent hydrocarbon group having 1 to 12 carbon atoms, preferably 1 to 8 carbon atoms, and preferably having no aliphatic unsaturated bonds. Specific examples include alkyl groups such as methyl, ethyl, and propyl groups; cycloalkyl groups such as cyclohexyl groups; aryl groups such as phenyl and tolyl groups; aralkyl groups such as benzyl, 2-phenylethyl, and 2-phenylpropyl groups; and groups in which some or all of the hydrogen atoms of these groups have been substituted with halogen atoms or the like, for example, 3,3,3-trifluoropropyl group.

[0031] In addition, a satisfies 0 < a < 3, preferably 0.5 ≤ a ≤ 2.2, more preferably 1.0 ≤ a ≤ 2.0. Also, b satisfies 0 < b ≤ 3, preferably 0.002 ≤ b ≤ 1.1, more preferably 0.005 ≤ b ≤ 1. Further, it is a positive number that satisfies 0 < a + b ≤ 3, preferably 1 ≤ a + b ≤ 3, more preferably 1.002 ≤ a + b ≤ 2.7.

[0032] The organohydrogenpolysiloxane of component (D) has two or more, preferably three or more hydrosilyl groups in one molecule, and these may be at the molecular chain ends, in the middle of the molecular chain, or both. Also, as this organohydrogenpolysiloxane, the viscosity at 25°C is preferably 0.5 to 10,000 mPa·s, particularly 1 to 300 mPa·s.

[0033] Specific examples of such organohydrogenpolysiloxanes include 1,1,3,3-tetramethyldisiloxane, 1,3,5,7-tetramethylcyclotetrasiloxane, tris(hydrogendimethylsiloxy)methylsilane, tris(hydrogendimethylsiloxy)phenylsilane, methylhydrogencyclopolysiloxane, methylhydrogensiloxane-dimethylsiloxane cyclic copolymer, methylhydrogenpolysiloxane capped with trimethylsiloxy groups at both ends, dimethylsiloxane-methylhydrogensiloxane copolymer capped with trimethylsiloxy groups at both ends, dimethylpolysiloxane capped with dimethylhydrogensiloxy groups at both ends, dimethylsiloxane-methylhydrogensiloxane copolymer ... Methylsiloxane-methylhydrogensiloxane copolymer, methylhydrogensiloxane-diphenylsiloxane copolymer with trimethylsiloxy groups at both ends, methylhydrogensiloxane-diphenylsiloxane-dimethylsiloxane copolymer with trimethylsiloxy groups at both ends, methylhydrogensiloxane-methylphenylsiloxane-dimethylsiloxane copolymer with trimethylsiloxy groups at both ends, methylhydrogensiloxane-dimethylsiloxane-diphenylsiloxane copolymer with dimethylhydrogensiloxy groups at both ends, methylhydrogensiloxane-dimethylsiloxane-methylphenylsiloxane copolymer with dimethylhydrogensiloxy groups at both ends, (CH3)2HSiO 1 / 2 Units and (CH3)3SiO 1 / 2 Units and SiO 4 / 2 A copolymer consisting of (CH3)2HSiO units. 1 / 2 Units and SiO 4 / 2 A copolymer consisting of (CH3)2HSiO units. 1 / 2 Units and SiO 4 / 2 Units and (C6H5)3SiO 1 / 2 and copolymers consisting of these units, and compounds in which part or all of the methyl groups in the above exemplary compounds have been substituted with other alkyl groups, phenyl groups, or the like. The organohydrogenpolysiloxane of the component (D) may use either a single compound, or a combination of two or more different compounds.

[0034] The amount of the organohydrogenpolysiloxane is such that the molar ratio of the hydrosilyl groups in the (D) component to the alkenyl groups bonded to silicon atoms in the (A) component is in the range of 0.5 to 10, preferably 0.7 to 5. If the molar ratio of the hydrosilyl groups in the (D) component to the alkenyl groups bonded to silicon atoms in the (A) component is less than 0.5, crosslinking is not sufficient, and sufficient mechanical strength is not obtained, which is not preferable. If the molar ratio exceeds 10, the physical properties after curing are reduced, particularly the heat resistance is deteriorated, and the compression set is large. In addition, the amount of the (D) component is preferably 0.1 to 40 parts by mass per 100 parts by mass of the silicone rubber compound (the total amount of the (A), (B), and (C) components).

[0035] [(E) component] The hydrosilylation catalyst of component (E) is a catalyst that causes a hydrosilylation addition reaction between the alkenyl group of component (A) and the hydrosilyl group of the organohydrogenpolysiloxane. Examples of the hydrosilylation catalyst include platinum group metal catalysts, such as simple platinum group metals and their compounds, and any of the catalysts known in the art for use in addition reaction curing silicone rubber compositions can be used. Examples include particulate platinum metal adsorbed on a carrier such as silica, alumina, or silica gel; platinic chloride, chloroplatinic acid, or a reaction product of chloroplatinic acid with a monohydric alcohol; a complex of chloroplatinic acid with an olefin; a complex of chloroplatinic acid with a vinyl group-containing (poly)siloxane; a complex of chloroplatinic acid with a phosphite ester; a palladium catalyst; and a rhodium catalyst. Of these, a complex of chloroplatinic acid with a vinyl group-containing (poly)siloxane is preferred. The hydrosilylation reaction catalyst of the component (E) may use either a single compound, or a combination of two or more different compounds.

[0036] The amount of catalyst added may be any amount sufficient to promote the hydrosilylation reaction, and is usually used in the range of 1 ppm by mass to 1% by mass, calculated as the amount of platinum group metal relative to the silicone rubber compound, with a range of 10 to 500 ppm by mass being preferred. If the amount added is 1 ppm by mass or more, the addition reaction is sufficiently promoted and curing is sufficient, while if it is 1% by mass or less, sufficient reactivity is maintained and it is not uneconomical.

[0037] In addition to the above catalysts, an addition reaction inhibitor may be used according to the purpose of the present invention in order to adjust the curing rate. Specific examples of such an inhibitor include acetylene alcohol inhibitors such as 1-ethynyl-1-cyclohexanol and 2-methyl-3-butyn-2-ol, and vinyl siloxanes such as 1,3,5,7-tetramethyl-1,3,5,7-tetravinylcyclotetrasiloxane and 1,3-divinyl-1,1,3,3-tetramethyldisiloxane. The addition reaction inhibitor may be used alone or in combination of two or more.

[0038] [Other ingredients] In addition to the above-mentioned components, the millable silicone rubber composition of the present invention may optionally contain, as necessary, fillers such as crushed quartz, crystalline silica, diatomaceous earth, calcium carbonate, etc., colorants, tear strength improvers, acid acceptors, thermal conductivity improvers such as alumina and boron nitride, release agents, and filler dispersants such as various alkoxysilanes, particularly phenyl-containing alkoxysilanes and their hydrolysates, diphenylsilanediol, carbon functional silane, and other fillers and additives known in thermosetting silicone rubber compositions.

[0039] In addition, the millable silicone rubber composition of the present invention may contain an organopolysiloxane that is liquid at 25°C, contains two or more alkenyl groups per molecule, and has a degree of polymerization of less than 1,000, for the purpose of adjusting the viscosity of the composition and the rubber properties. The degree of polymerization of the liquid organopolysiloxane is preferably 100 or more and less than 1,000, and more preferably 100-800. Examples of the alkenyl group and non-alkenyl group in the liquid organopolysiloxane include the same groups as those exemplified for component (A). The organopolysiloxane preferably has a viscosity at 25° C. of 10 to 120,000 mPa·s, and more preferably 100 to 100,000 mPa·s. In the present invention, the viscosity is a value measured at 25° C. using a rotational viscometer as described in JIS K 7117-1:1999. The amount of the liquid organopolysiloxane blended is preferably 0 to 20 parts by mass per 100 parts by mass of the component (A).

[0040] [Method of producing the composition] The millable silicone rubber composition of the present invention can be obtained by mixing the components constituting the composition with a known mixer such as a kneader, a Banbury mixer, a two-roll mill, etc. It is preferable to mix components (A), (B), and (C) to obtain a mixture, and then add components (E) and (D) to the mixture. When the composition containing the components (A) to (E) further contains other components, it is preferable to first mix the components (A), (B), and (C) with the other components to obtain a mixture, and then add the components (E) and (D) to the mixture.

[0041] [Curing conditions] The millable silicone rubber composition of the present invention can be cured by a known curing method under known curing conditions. Specifically, the composition can be cured by heating at 25 to 200° C., preferably 80 to 160° C. The heating time may be about 0.5 minutes to 5 hours, and particularly about 1 minute to 3 hours. The millable silicone rubber composition of the present invention may be cured under pressure. EXAMPLES

[0042] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to these.

[0043] The hardness (Durometer A), tensile strength and elongation at break of the cured products of the silicone rubber compositions prepared in the following Examples and Comparative Examples were measured according to JIS K 6249:2003. In addition, according to JIS K 6262:2013, the compression set (150°C / 22 hours, 25% compression) was measured using a large test piece (disk-shaped with a diameter of 29.0±0.5 mm and a thickness of 12.5±0.5 mm). The viscosity was measured using a rotational viscometer at 25°C as described in JIS K 7117-1:1999.

[0044] The following components were used as component (A): (A): A rubber-like dimethylsiloxane-methylvinylpolysiloxane copolymer with 10 methylvinylsiloxane units and a weight-average degree of polymerization of approximately 8,000, both ends of which are capped with dimethylvinylsiloxy groups.

[0045] The following components were used as component (B): (B-1): Specific surface area is 110m 2 / g of dimethyldichlorosilane-surface-treated fumed silica (product name: Aerosil R972, manufactured by Nippon Aerosil Co., Ltd.) (B-2): Specific surface area is 180m 2 / g of dimethyldichlorosilane-treated fumed silica (product name: Reolosil DM-20S, manufactured by Tokuyama Corporation)

[0046] The following components were used as component (C): (C-1): 1-dodecanol (boiling point: 259°C) (C-2): 2-ethyl-1-hexanol (boiling point: 184-185°C) (C-3): Cyclohexanol (boiling point: 161°C, for comparison) (C-4): 1-hexanol (boiling point: 156.5°C, for comparison) (C-5): Ethylene glycol (boiling point: 197.3°C) (C-6): 1-pentanol (boiling point: 138°C, for comparison)

[0047] The following components were used as component (D): (D-1): Methylhydrogen-dimethylpolysiloxane having hydrosilyl groups in the side chains (both ends of the molecular chain are blocked with trimethylsiloxy groups, weight average degree of polymerization is 38, in the above formula (1), a = 1.55, b = 0.5, R 1 =CH3, Number of hydrosilyl groups: 20, Viscosity: 17 mPa s) (D-2): 2,5-dimethyl-2,5-bis(t-butylperoxy)hexane (for comparison)

[0048] The following components were used as component (E): Platinum catalyst (a dimethylpolysiloxane solution containing 1% by mass of chloroplatinic acid / 1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex as platinum atom content)

[0049] As an optional addition reaction inhibitor other than the components (A) to (E), the following components were used. 1-Ethynyl-1-cyclohexanol (Ethynylcyclohexanol)

[0050] [Example 1] 100 parts by mass of component (A), 35 parts by mass of component (B-1), and 1 part by mass of component (C-1) were mixed in a kneader to prepare base compound (1). The base compound (1) was mixed with 1.22 parts by mass of component (D-1) (the amount of hydrosilyl groups per mole of alkenyl groups in component (A) is 4.4 moles), 0.05 parts by mass of ethynylcyclohexanol as an addition reaction inhibitor, and 0.07 parts by mass of component (E) using a twin roll to obtain a silicone rubber composition. The obtained composition was subjected to a 120°C, 70 kgf / cm 2 The test sheets were then subjected to measurements of hardness (Durometer A), tensile strength and elongation at break. The results are shown in Table 1. The obtained composition was then subjected to a test at 120°C and 70 kgf / cm 2The test pieces were press cured for 15 minutes under the above conditions to prepare cured products for measuring compression set, and the compression set was measured. The results are shown in Table 1.

[0051] [Examples 2 to 7] A silicone rubber composition was prepared in the same manner as in Example 1 using the formulation shown in Table 1. Test sheets and cured products were made from the resulting compositions, and various physical properties were evaluated. The results are shown in Table 1.

[0052] [Comparative Examples 1 to 3] A silicone rubber composition was prepared in the same manner as in Example 1 using the formulation shown in Table 2. Test sheets and cured products were made from the resulting compositions, and various physical properties were evaluated. The results are shown in Table 2.

[0053] [Comparative Example 4] 100 parts by mass of component (A) and 35 parts by mass of component (B-1) were mixed in a kneader to prepare base compound (2). The base compound (2) was mixed with 0.14 parts by mass of component (D-2) using a twin roll mill to obtain a silicone rubber composition. The obtained composition was subjected to a test at 165°C and 70 kgf / cm 2 The test sheets were then subjected to measurements of hardness (Durometer A), tensile strength and elongation at break. The results are shown in Table 2. The obtained composition was then subjected to a test at 165°C and 70 kgf / cm 2 The test pieces were press cured for 15 minutes under the above conditions to prepare cured products for measuring compression set, and the compression set was measured. The results are shown in Table 2.

[0054] [Comparative Examples 5 to 6] A silicone rubber composition was prepared using the formula shown in Table 2 in the same manner as in Comparative Example 4. Test sheets and cured products were prepared from the resulting composition, and various physical properties were evaluated. The results are shown in Table 2.

[0055] [Examples 8 to 9, Comparative Examples 7 to 8] A silicone rubber composition was prepared in the same manner as in Example 1 using the formulation shown in Table 3. Test sheets and cured products were made from the resulting compositions, and various physical properties were evaluated. The results are shown in Table 3.

[0056] [Example 10, Comparative Example 9] A silicone rubber composition was prepared in the same manner as in Example 1 using the formulation shown in Table 4. Test sheets and cured products were made from the resulting compositions, and various physical properties were evaluated. The results are shown in Table 4.

[0057] [Table 1] In the table, "H / Vi" indicates the ratio of hydrosilyl groups in component (D-1) to vinyl groups in component (A).

[0058] [Table 2] In the table, "H / Vi" indicates the ratio of hydrosilyl groups in component (D-1) to vinyl groups in component (A).

[0059] [Table 3] In the table, "H / Vi" indicates the ratio of hydrosilyl groups in component (D-1) to vinyl groups in component (A).

[0060] [Table 4] In the table, "H / Vi" indicates the ratio of hydrosilyl groups in component (D-1) to vinyl groups in component (A).

Claims

1. (A) 100 parts by mass of an organopolysiloxane having two or more alkenyl groups bonded to silicon atoms in each molecule and a weight average degree of polymerization of 1,000 to 100,000; (B) A material with a specific surface area of ​​50 m2 measured by the BET method 2 / g or more of surface-treated reinforcing silica; 10 to 100 parts by mass, (C) a chain aliphatic alcohol having a boiling point of 170° C. or higher; 0.1 to 10 parts by mass, (D) an organohydrogenpolysiloxane containing two or more silicon-bonded hydrogen atoms (hydrosilyl groups) per molecule; an amount such that the molar ratio of hydrosilyl groups in component (D) to silicon-bonded alkenyl groups in component (A) is 0.5 to 10; and (E) a hydrosilylation reaction catalyst; a catalytic amount; A millable type silicone rubber composition comprising:

2. 2. The millable silicone rubber composition according to claim 1, wherein component (C) is one or more selected from the group consisting of 1-octanol, 1-nonanol, 1-dodecanol, 2-ethyl-1-hexanol, 2,6-dimethyl-4-heptanol, 3,5,5-trimethyl-1-hexanol, and ethylene glycol.

3. A cured product of the millable type silicone rubber composition according to claim 1 or 2.

Citation Information

Patent Citations

  • Silicone rubber composition and its molding

    JP1996269339A

  • Silicone rubber composition and silicone rubber

    JP2019143047A

  • Silicone rubber composition and silicone rubber

    JP2019194293A

  • Thermosetting silicone rubber composition

    JP2014031408A

  • Silicone rubber composition

    JP2016196591A