Adhesive, fuel cell, and method for manufacturing fuel cell

A pressure-sensitive adhesive with acid-modified polypropylene enhances fuel cell assembly by providing high adhesive strength in high-temperature conditions, addressing the inefficiencies of traditional gasketing methods and adhesive requirements.

JP2024151809AInactive Publication Date: 2024-10-25TOYOTA JIDOSHA KK
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023065530
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-13
Publication Date
2024-10-25
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing fuel cell sealing methods using thermoset rubber gaskets are time-consuming, and adhesives with acrylic copolymers require high-temperature heat treatment for sufficient adhesiveness, which is not suitable for high-temperature applications.

Method used

A pressure-sensitive adhesive comprising a specific amount of acid-modified polypropylene relative to a base polymer, such as maleic anhydride-modified or maleic acid-modified polypropylene, is used to achieve high adhesive strength even in high-temperature conditions.

Benefits of technology

The adhesive provides strong bonding between fuel cells even in high-temperature environments, enabling efficient and rapid assembly of fuel cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024151809000001_ABST
    Figure 2024151809000001_ABST
Patent Text Reader

Abstract

To provide an adhesive that has high adhesive strength even in high-temperature water, a fuel cell including the adhesive, and a method for manufacturing the fuel cell.SOLUTION: An adhesive according to an embodiment includes a base polymer, a tackifier, and an acid-modified polypropylene, the acid-modified polypropylene is at least one acid-modified polypropylene selected from maleic anhydride-modified polypropylene and maleic acid-modified polypropylene, and the mass ratio of the acid-modified polypropylene to the base polymer (acid-modified polypropylene / base polymer) is 0.1 or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to an adhesive, a fuel cell, and a method for manufacturing a fuel cell. [Background technology]

[0002] In a fuel cell, hydrogen, air, cooling water, etc. are supplied between the fuel cell cells to generate electricity. To prevent leakage of these substances, it is necessary to seal between the fuel cell cells. Rubber gaskets are widely used to seal between the fuel cell cells. As gaskets are usually made of thermosetting materials, it takes a long time to produce fuel cells.

[0003] Incidentally, Patent Document 1 discloses an adhesive film having a base film and an adhesive layer formed on at least one surface of the base film, the adhesive layer being formed from an adhesive composition containing a (meth)acrylic copolymer obtained by living radical polymerization, the (meth)acrylic copolymer containing a structural unit (a-1) having a cyclic ether group and a structural unit (a-2) having an acidic group, a molecular weight distribution (Mw / Mn) of 3.0 or less, and a gel fraction of the adhesive layer of 30 mass% or more. The adhesive film disclosed in Patent Document 1 has a cyclic ether group such as an epoxy group, and requires high-temperature heat treatment to exhibit sufficient adhesiveness. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent Publication No. 2022-61158 Summary of the Invention [Problem to be solved by the invention]

[0005] The inventors investigated the use of a pressure-sensitive adhesive instead of a gasket to quickly bond fuel cell cells together, but found that typical pressure-sensitive adhesives have low adhesive strength in the environments in which fuel cell cells are used, such as in high-temperature water.

[0006] An object of the present disclosure is to provide a pressure-sensitive adhesive that has high adhesive strength even in high-temperature water, a fuel cell including the pressure-sensitive adhesive, and a method for manufacturing a fuel cell. [Means for solving the problem]

[0007] The present inventors conducted intensive research to solve the above problems and discovered that an adhesive containing a specific acid-modified polypropylene in a specific amount relative to the base polymer has high adhesive strength even in high-temperature water, leading to the present disclosure.

[0008] An example aspect of this embodiment is described as follows.

[0009] (1) A composition comprising a base polymer, a tackifier, and an acid-modified polypropylene; The acid-modified polypropylene is at least one acid-modified polypropylene selected from maleic anhydride-modified polypropylene and maleic acid-modified polypropylene, A pressure-sensitive adhesive, in which the mass ratio of acid-modified polypropylene to base polymer (acid-modified polypropylene / base polymer) is 0.1 or more. (2) The pressure-sensitive adhesive according to (1), which is in the form of a sheet. (3) A fuel cell, in which the adhesive according to (1) or (2) is disposed between fuel cell cells. (4) A step of placing an adhesive between the fuel cell cells and bonding the fuel cell cells by applying pressure, The process is carried out at a temperature of 23 to 95° C. The pressure-sensitive adhesive comprises a base polymer, a tackifier, and an acid-modified polypropylene; The acid-modified polypropylene is at least one acid-modified polypropylene selected from maleic anhydride-modified polypropylene and maleic acid-modified polypropylene, A method for producing a fuel cell, wherein the mass ratio of the acid-modified polypropylene to the base polymer (acid-modified polypropylene / base polymer) is 0.1 or more. (5) The method for producing a fuel cell according to (4), wherein the steps are carried out at a temperature of 30 to 95°C. Effect of the Invention

[0010] The present disclosure makes it possible to provide a pressure-sensitive adhesive having high adhesive strength even in high-temperature water, a fuel cell having the pressure-sensitive adhesive, and a method for producing a fuel cell. [Brief description of the drawings]

[0011] [Figure 1] The peel strength in high-temperature water for Material 2 and Material 3 is shown. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The adhesive, fuel cell, and method for producing the fuel cell according to the present embodiment are described in detail below. The adhesive according to the present embodiment includes a base polymer, a tackifier, and an acid-modified polypropylene, the acid-modified polypropylene being at least one acid-modified polypropylene selected from maleic anhydride-modified polypropylene and maleic acid-modified polypropylene, and the mass ratio of the acid-modified polypropylene to the base polymer (acid-modified polypropylene / base polymer) is 0.1 or more.

[0013] (Base polymer) The base polymer is not particularly limited, including conventionally known polymers, as long as it can be used as the base polymer of the adhesive. Examples of the base polymer include styrene-based polymers, acrylic-based polymers, rubber-based polymers, polyester-based polymers, urethane-based polymers, polyether-based polymers, and silicone-based polymers. The base polymer is preferably at least one base polymer selected from styrene-based polymers, acrylic-based polymers, and rubber-based polymers. The base polymer may be used alone or in combination of two or more. The base polymer may be a block copolymer of a monovinyl compound and a conjugated diene compound.

[0014] The styrene-based polymer may be a styrene-based block copolymer. For example, a styrene-isoprene-styrene block copolymer or a styrene-butadiene-styrene block copolymer may be used as the styrene-based block copolymer. The styrene-based block copolymer preferably has a styrene content of 50% by mass or less, more preferably 40% by mass or less. The styrene content means the amount (% by mass) of a styrene-derived structural unit in 100% by mass of the copolymer.

[0015] Examples of acrylic polymers include polymers whose main constituent units are structural units derived from alkyl (meth)acrylates, where the main constituent units refer to structural units that account for more than 50% by mass of 100% by mass of the polymer.

[0016] The alkyl(meth)acrylate is preferably an alkyl(meth)acrylate represented by the following general formula (1). CH2=C(R 1 )COOR 2 (1) Here, R in the above formula (1) 1 is a hydrogen atom or a methyl group, R 2 is an alkyl group having 1 to 20 carbon atoms.

[0017] The acrylic polymer may have a structural unit other than the structural unit derived from the alkyl (meth) acrylate. Examples of the structural unit other than the structural unit derived from the alkyl (meth) acrylate include a structural unit derived from a functional group-containing monomer such as a carboxy group-containing monomer, a hydroxyl group-containing monomer, an acid anhydride group-containing monomer, or an amide group-containing monomer.

[0018] The rubber-based polymer may be, for example, a rubber other than a styrene-based polymer, and may be a natural rubber or a synthetic rubber, for example, polyisoprene, polybutadiene, polyisobutylene, and butyl rubber.

[0019] (tackifier) The tackifier is not particularly limited, including conventionally known tackifiers, as long as it can be used as a tackifier. Examples of the tackifier include rosin-based resins, terpene-based resins, petroleum-based resins, coumarone-indene resins, alkylphenol resins, xylene resins, etc. As the tackifier, at least one tackifier selected from rosin-based resins, terpene-based resins, and petroleum-based resins is preferred. The tackifier may be used alone or in combination of two or more.

[0020] Examples of rosin-based resins include rosin, hydrogenated rosin, rosin ester, hydrogenated rosin ester, rosin phenol resin, and polymerized rosin.

[0021] Examples of the terpene resin include terpene resin, terpene phenol resin, aromatic modified terpene resin, and hydrogenated terpene resin.

[0022] Examples of petroleum resins include aliphatic petroleum resins, hydrogenated petroleum resins, alicyclic petroleum resins, aromatic petroleum resins, and copolymer petroleum resins.

[0023] (Acid-modified polypropylene) The acid-modified polypropylene is at least one acid-modified polypropylene selected from maleic anhydride-modified polypropylene and maleic acid-modified polypropylene.

[0024] Maleic anhydride modified polypropylene is a polymer obtained by modifying polypropylene with maleic anhydride, and maleic acid modified polypropylene is a polymer obtained by modifying polypropylene with maleic acid. There is no particular limitation on the modification method, and any known method may be used. For example, there is a method in which polypropylene is dissolved in a solvent, a polar monomer and a radical generator are added, and the mixture is heated and stirred, a method in which the above components are fed into an extruder to be graft-copolymerized, and a solid-phase modification method.

[0025] The amount of structural units derived from polar monomers in the acid-modified polypropylene (e.g., graft amount) is preferably 0.1% by mass or more, more preferably 0.3% by mass or more, even more preferably 0.5% by mass or more, and is preferably 20% by mass or less, more preferably 15% by mass or less, even more preferably 10% by mass or less. The amount of the structural units can be determined, for example, by infrared absorption spectroscopy.

[0026] The maleic anhydride-modified polypropylene may have a structure derived from a substance other than propylene and maleic anhydride, such as a structure derived from at least one selected from ethylene, an olefin having 4 to 6 carbon atoms, and maleic acid. The maleic acid-modified polypropylene may have a structure derived from a substance other than propylene and maleic acid, such as a structure derived from at least one selected from ethylene, an olefin having 4 to 6 carbon atoms, and maleic anhydride.

[0027] (Adhesive) The pressure-sensitive adhesive of the present embodiment includes the above-mentioned base polymer, tackifier, and acid-modified polypropylene. The mass ratio of the acid-modified polypropylene contained in the pressure-sensitive adhesive to the base polymer (acid-modified polypropylene / base polymer) is 0.1 or more. The mass ratio of the acid-modified polypropylene to the base polymer (acid-modified polypropylene / base polymer) may be 0.5 or less, or may be 0.4 or less. This range is preferable because the pressure-sensitive adhesive can exhibit high adhesive strength even under high-temperature conditions such as in high-temperature water.

[0028] The mass ratio of the tackifier to the base polymer contained in the pressure-sensitive adhesive (tackifier / base polymer) is, for example, 0.7 to 1.3, and may be 0.8 to 1.2.

[0029] The shape of the adhesive is not particularly limited. For example, an adhesive having no specific shape may be used by coating. The adhesive may also be in a sheet shape. When the adhesive is in a sheet shape, the adhesive can be used as an adhesive sheet. The sheet-shaped adhesive preferably has a thickness of, for example, 50 to 300 μm.

[0030] The adhesive may contain components other than the base polymer, tackifier, and acid-modified polypropylene, such as additives. Examples of additives include crosslinkers, plasticizers, fillers, antioxidants, conductive materials, release regulators, softeners, surfactants, flame retardants, antioxidants, solvents, etc. The additives are contained in an amount of, for example, 0.1 to 30% by mass in 100% by mass of the adhesive.

[0031] The method for preparing the adhesive is not particularly limited, and the adhesive can be obtained by, for example, mixing the above-mentioned raw materials using a kneader such as a twin-screw kneader. In addition, for example, the adhesive obtained by mixing can be processed into a sheet by a method such as press molding, and cut or punched as necessary to obtain a desired shape, thereby obtaining a sheet-shaped adhesive, i.e., an adhesive sheet.

[0032] (fuel cell) In the fuel cell of this embodiment, the above-mentioned adhesive is disposed between the fuel cell cells. As long as the above-mentioned adhesive is disposed between the fuel cell cells, the other members of the fuel cell are not particularly limited.

[0033] From the viewpoint of adhesive strength, the material of the portion of the fuel cell that comes into contact with the adhesive, i.e., the adherend, is preferably at least one selected from stainless steel, titanium, and aluminum.

[0034] The fuel cell is composed of at least two fuel cells, and the above-mentioned adhesive is disposed between the fuel cells, and the cells are bonded by the adhesive. The above-mentioned adhesive has high adhesive strength even in high-temperature water, so that the fuel cell can be used stably. In a fuel cell, the fuel cells are generally stacked in series. The number of stacks is, for example, 2 to 400, preferably 50 to 370, and more preferably 70 to 340.

[0035] (Fuel Cell Manufacturing Method) The method for producing a fuel cell of this embodiment includes a step of placing an adhesive between fuel cell cells and bonding the fuel cell cells by applying pressure, the step being carried out at a temperature of 23 to 95°C, the adhesive includes a base polymer, a tackifier, and an acid-modified polypropylene, the acid-modified polypropylene is at least one acid-modified polypropylene selected from maleic anhydride-modified polypropylene and maleic acid-modified polypropylene, and the mass ratio of the acid-modified polypropylene to the base polymer (acid-modified polypropylene / base polymer) is 0.1 or more. That is, the above-mentioned adhesive of this embodiment is used in the method for producing a fuel cell. The method for producing a fuel cell only needs to include the above steps, and there are no particular limitations on the other steps.

[0036] The adhesive may be disposed between the fuel cells by coating the adhesive on the fuel cells or by disposing an adhesive sheet between the fuel cells.

[0037] In the above process, the pressure is usually 0.5 to 5 MPa, and preferably 1 to 3 MPa. In the above process, the pressing time is usually 1 to 15 seconds, and preferably 2 to 10 seconds. The above process is also carried out at a temperature of 23 to 95°C. By carrying out the process under the above conditions, the fuel cell units can be bonded with sufficient strength. From the viewpoint of adhesive strength stability, a temperature of 30 to 95°C is more preferable. EXAMPLES

[0038] The present embodiment will be described below with reference to examples, but the present disclosure is not limited to these examples.

[0039] The following materials were used in the examples and comparative examples. Base polymer: Quintac® 3421 (Zeon Corporation), Tackifier: Quintone® M100 (Zeon Corporation), Maleic anhydride modified polypropylene: Modic P512VB (Mitsubishi Chemical Corporation) In Table 1, maleic anhydride modified polypropylene is referred to as m-PP.

[0040] (Examples and Comparative Examples) Quintac® 3421, Quintone® M100, and Modic P512VB were mixed in the amounts shown in Table 1 using a twin-screw kneader. The resulting mixed material (adhesive) was formed into a sheet by rolling it out to a thickness of 150 μm using a press. The resulting sheet was sandwiched between two 0.1 mm thick SUS plates and pressed using the press at a pressure of 3 MPa, a press time of 10 seconds, and a temperature shown in Table 1 to prepare an adhesion test specimen.

[0041] A peel test was carried out on the adhesion test pieces in water at 95°C, and the peel strength was calculated. The peel strength is shown in Table 1 as high-temperature water peel strength. Note that material 1 in Table 1 corresponds to the comparative example, and materials 2 and 3 correspond to the examples. The high-temperature water peel strengths of materials 2 and 3 are shown in Figure 1.

[0042] [Table 1]

[0043] It can be seen from Table 1 that the adhesive of the present embodiment containing a predetermined amount of maleic anhydride-modified polypropylene has excellent peel strength in high-temperature water, and therefore the adhesive of the present embodiment can be suitably used for bonding between fuel cell units.

[0044] The upper limit and / or lower limit of the numerical ranges described in this specification can be arbitrarily combined to define a preferred range. For example, the upper limit and lower limit of the numerical range can be arbitrarily combined to define a preferred range, the upper limit of the numerical range can be arbitrarily combined to define a preferred range, and the lower limit of the numerical range can be arbitrarily combined to define a preferred range.

[0045] Although the present embodiment has been described in detail above, the specific configuration is not limited to this embodiment, and even if there are design changes within the scope that does not deviate from the gist of this disclosure, they are included in this disclosure.

Claims

1. The composition includes a base polymer, a tackifier, and an acid-modified polypropylene. The acid-modified polypropylene is at least one acid-modified polypropylene selected from maleic anhydride-modified polypropylene and maleic acid-modified polypropylene, A pressure-sensitive adhesive, in which the mass ratio of acid-modified polypropylene to base polymer (acid-modified polypropylene / base polymer) is 0.1 or more.

2. The pressure-sensitive adhesive according to claim 1 , which is in the form of a sheet.

3. A fuel cell comprising the adhesive according to claim 1 disposed between fuel cell cells.

4. The method includes a step of placing an adhesive between the fuel cell cells and bonding the fuel cell cells by applying pressure, The process is carried out at a temperature between 23 and 95° C. The pressure-sensitive adhesive comprises a base polymer, a tackifier, and an acid-modified polypropylene; The acid-modified polypropylene is at least one acid-modified polypropylene selected from maleic anhydride-modified polypropylene and maleic acid-modified polypropylene, A method for producing a fuel cell, wherein the mass ratio of the acid-modified polypropylene to the base polymer (acid-modified polypropylene / base polymer) is 0.1 or more.

5. The method for producing a fuel cell according to claim 4, wherein said steps are carried out at a temperature of 30 to 95°C.

Citation Information

Patent Citations

  • Alkali-dispersible hot-melt adhesive composition, method for producing the same, method for attaching label, and container

    JP2010090185A

  • Adhesive sealing member

    JP2011213767A

  • Thermoplastic polymer composition and molded article

    WO2012026501A1

  • Assembly for fuel cell, and laminate

    WO2021060000A1

  • Adhesive film

    JP2022061158A