A laminated decorative sheet with biomass-derived resin layers addresses the lack of plant-derived materials in decorative sheets, reducing petroleum dependence and carbon emissions while maintaining high design quality.

JP2024151821AInactive Publication Date: 2024-10-25TOPPAN HOLDINGS INC
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023065546
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-13
Publication Date
2024-10-25
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

There is a lack of plant-derived materials for decorative sheets, leading to high petroleum dependence and carbon dioxide emissions, which hinders the transition to an environmentally friendly and sustainable society.

Method used

A decorative sheet is designed with a laminated structure comprising a colored thermoplastic resin layer, pattern printing layer, transparent thermoplastic resin layer, and surface protective layer, where at least one of the resin layers is made from a biomass-derived resin composition, and includes a gloss adjustment layer synchronized with the pattern printing layer, enhancing design quality and reducing petroleum dependence.

Benefits of technology

The solution reduces petroleum dependence, conserves resources, and contributes to a more sustainable society by using biomass-derived materials while maintaining high design quality and functionality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024151821000001_ABST
    Figure 2024151821000001_ABST
Patent Text Reader

Abstract

To provide a decorative sheet and a decorative material capable of reducing petroleum dependency in materials and conserving petroleum resources.SOLUTION: A decorative sheet comprises: a colored thermoplastic resin layer 2; a pattern printed layer 3; a transparent thermoplastic resin layer 5; and a surface protective layer 6 laminated in this order, and further comprises a gloss adjustment layer 7 provided on a surface opposite to the transparent thermoplastic resin layer 5 of the surface protective layer 6 and coordinated with the pattern of the pattern printed layer 3, wherein at least one of the colored thermoplastic resin layer 2 and the transparent thermoplastic resin layer 5 is formed using a biomass-derived resin composition.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a decorative sheet and a decorative material. [Background technology]

[0002] As an alternative to decorative sheets made of polyvinyl chloride, decorative sheets using olefin resins, as disclosed in Patent Document 1, for example, have been proposed. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2014-188941 A Summary of the Invention [Problem to be solved by the invention]

[0004] In recent years, against the backdrop of environmental issues, there has been a demand to reduce dependency on petroleum, conserve petroleum resources, and reduce carbon dioxide emissions by switching decorative sheet materials from conventional petroleum-derived materials to plant-derived materials, thereby contributing to an environmentally friendly and sustainable society. However, there are few plant-derived materials that can be used in decorative sheets, and there has been an issue in that it has not been possible to reduce dependency on petroleum in decorative sheet materials.

[0005] In view of the above-mentioned problems, the present disclosure has an object to provide a decorative sheet and a decorative material that can reduce the dependency on petroleum in the materials and conserve petroleum resources. [Means for solving the problem]

[0006] According to one aspect of the present invention, a decorative sheet is provided in which a colored thermoplastic resin layer, a pattern printed layer, a transparent thermoplastic resin layer, and a surface protective layer are laminated in this order, and further a gloss adjusting layer is provided on the side of the surface protective layer opposite the transparent thermoplastic resin layer, the gloss adjusting layer being in harmony with the pattern of the pattern printed layer, and at least one of the colored thermoplastic resin layer and the transparent thermoplastic resin layer is formed using a biomass-derived resin composition.

[0007] In addition, according to another aspect of the present invention, there is provided a decorative sheet in which at least a colored thermoplastic resin layer, a picture-printed layer, and a transparent thermoplastic resin layer are laminated in this order, and further which has a concave-convex pattern provided on the transparent thermoplastic resin layer side that is in harmony with the pattern of the picture-printed layer, and at least one of the colored thermoplastic resin layer and the transparent thermoplastic resin layer is formed using a biomass-derived resin composition.

[0008] Furthermore, according to another aspect of the present invention, there is provided a decorative material comprising a substrate and the decorative sheet of the above aspect attached to at least one surface of the substrate. Effect of the Invention

[0009] According to one aspect of the present invention, it is possible to provide a decorative sheet and a decorative material that can reduce dependency on petroleum in the materials and conserve petroleum resources. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a cross-sectional view showing a schematic diagram of an example of a decorative material according to the present invention. [Diagram 2] FIG. 2 is a configuration diagram that illustrates an example of a transparent thermoplastic resin layer forming apparatus. [Diagram 3] FIG. 2 is a schematic diagram showing an example of a gloss adjusting layer forming device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Next, an embodiment of the present invention will be described below with reference to the drawings. Here, the drawings are schematic, and the relationship between thickness and planar dimensions, the thickness ratio of each layer, etc. differ from the actual ones. Furthermore, the embodiments shown below are examples of configurations for embodying the technical idea of ​​the present invention, and the technical idea of ​​the present invention is not limited to the materials, shapes, structures, etc. of the components described below. The technical idea of ​​the present invention can be modified in various ways within the technical scope defined by the claims.

[0012] 1 is a cross-sectional view that shows a schematic diagram of a decorative material 10 according to one embodiment of the present invention. The decorative material 10 is formed by providing a substrate 9 on the surface of a decorative sheet 1 that faces a primer layer 8, which will be described later. <Composition of decorative sheet> The decorative sheet 1 is formed by laminating, in the stated order, a colored thermoplastic resin layer 2, a pattern printed layer 3, an adhesive layer 4, a transparent thermoplastic resin layer 5, a surface protective layer 6, and a gloss adjusting layer 7, with a primer layer 8 laminated on the side of the colored thermoplastic resin layer 2 opposite the pattern printed layer 3, so that an uneven pattern 5a is formed from the surface protective layer 6 to the transparent thermoplastic resin layer 5.

[0013] The decorative sheet 1 according to this embodiment may include a colored thermoplastic resin layer 2, a pattern printed layer 3, an adhesive layer 4, a transparent thermoplastic resin layer 5, a surface protective layer 6, and a gloss adjusting layer 7 in this order. In the decorative sheet 1 according to this embodiment, at least one of the colored thermoplastic resin layer 2 and the transparent thermoplastic resin layer 5 is a resin layer formed using a resin composition containing a resin material derived from a biomass plant. This allows the decorative sheet 1 according to this embodiment to reduce the dependency on petroleum in the material and conserve petroleum resources. Therefore, it is possible to reduce carbon dioxide emissions and contribute to an environmentally friendly and sustainable society.

[0014] Here, we will explain the case where both the colored thermoplastic resin layer 2 and the transparent thermoplastic resin layer 5 are formed using a resin composition containing a resin material derived from a biomass plant, but only one of the colored thermoplastic resin layer 2 and the transparent thermoplastic resin layer 5 may be formed using a resin composition containing a resin material derived from a biomass plant. Furthermore, the decorative sheet 1 may have both the uneven pattern 5a and the gloss-adjusting layer 7, or may have only the uneven pattern 5a or only the gloss-adjusting layer 7. In addition, the uneven pattern 5a may be provided on the surface of the surface protection layer 6 after the surface protection layer 6 is formed, and in that case, the recesses may or may not reach the transparent thermoplastic resin layer 5.

[0015] <Colored thermoplastic resin layer> The colored thermoplastic resin layer 2 is a resin formed using a thermoplastic resin, and is a resin layer formed using a resin composition containing a biomass-derived (plant-derived) resin material. In this embodiment, the colored thermoplastic resin layer 2 contains a biomass-derived polyolefin formed by polymerizing a monomer containing a biomass-derived olefin as the main material of the resin composition. For example, the colored thermoplastic resin layer 2 in the decorative sheet 1 according to this embodiment is a colored thermoplastic resin layer formed from a resin composition containing biomass-derived polyethylene as the biomass-derived resin material.

[0016] The composition of the colored thermoplastic resin layer 2 will be described in detail below. <Biomass-derived polyethylene> In this embodiment, the biomass-derived polyethylene is obtained by polymerizing a monomer containing biomass-derived ethylene. The biomass-derived ethylene is not particularly limited, and ethylene produced by a conventionally known method can be used. Since biomass-derived ethylene is used as the raw material monomer, the polymerized polyethylene is derived from biomass.

[0017] The raw material monomer for polyethylene does not necessarily contain 100% by mass of ethylene derived from biomass. The monomer that is the raw material of the biomass-derived polyethylene may further contain at least one of ethylene derived from a fossil fuel and an α-olefin derived from a fossil fuel, or may further contain an α-olefin derived from a biomass.

[0018] The number of carbon atoms of the α-olefin is not particularly limited, but one having 3 to 20 carbon atoms can usually be used, and butylene, hexene, or octene is preferable. This is because butylene, hexene, or octene can be produced by polymerization of ethylene, which is a raw material derived from biomass. In addition, by including such an α-olefin, the polyethylene obtained by polymerization has an alkyl group as a branched structure, and therefore can be more flexible than a simple linear one.

[0019] By using ethylene, a raw material derived from biomass, it is theoretically possible to produce polypropylene from components derived 100% from biomass. The biomass-derived ethylene concentration in the polyethylene (hereinafter sometimes referred to as "biomass degree") is a value obtained by measuring the content of biomass-derived carbon by radiocarbon (C14) measurement. Carbon dioxide in the atmosphere contains a certain proportion of C14 (105.5 pMC), and it is known that the C14 content in plants that grow by absorbing carbon dioxide from the atmosphere, such as corn, is also about 105.5 pMC. It is also known that fossil fuels contain almost no C14. Therefore, the proportion of biomass-derived carbon can be calculated by measuring the proportion of C14 contained in the total carbon atoms in the polyethylene. In this embodiment, the content of biomass-derived carbon Pbio can be calculated as follows when the content of C14 in the polyethylene is PC14.

[0020] Pbio(%)=PC14 / 105.5×100 In the present embodiment, theoretically, if all biomass-derived ethylene is used as the raw material for polyethylene, the concentration of biomass-derived ethylene is 100%, and the biomass degree of the biomass-derived polyethylene is 100. Moreover, the concentration of biomass-derived ethylene in fossil fuel-derived polyethylene produced only from fossil fuel-derived raw materials is 0%, and the biomass degree of the fossil fuel-derived polyethylene is 0.

[0021] In this embodiment, the biomass-derived polyethylene or the decorative sheet 1 comprising this polyethylene does not necessarily have a biomass degree of 100. In this embodiment, the polymerization method of the ethylene-containing monomer derived from biomass is not particularly limited, and can be carried out by a conventionally known method. The polymerization temperature and polymerization pressure are preferably adjusted appropriately depending on the polymerization method and polymerization apparatus. The polymerization apparatus is also not particularly limited, and a conventionally known apparatus can be used. An example of the polymerization method of the ethylene-containing monomer will be described below.

[0022] The polymerization method for the ethylene polymer or the ethylene-α-olefin copolymer can be appropriately selected depending on the type of polyethylene to be produced, for example, differences in density and branching such as high density polyethylene (HDPE), medium density polyethylene (MDPE), low density polyethylene (LDPE), linear low density polyethylene (LLDPE), etc. For example, it is preferable to use a multi-site catalyst such as a Ziegler-Natta catalyst or a single-site catalyst such as a metallocene catalyst as the polymerization catalyst, and carry out the polymerization in one stage or in two or more stages by any of the methods of gas phase polymerization, slurry polymerization, solution polymerization, and high pressure ion polymerization. As the biomass-derived polyethylene, an ethylene polymer or an ethylene-α-olefin copolymer may be used alone or in combination of two or more kinds.

[0023] <Resin composition containing biomass-derived polyethylene> In this embodiment, the resin composition contains the above-mentioned polyethylene as a main component. The resin composition forming the colored thermoplastic resin layer 2, i.e., the colored thermoplastic resin layer 2, contains 5% by mass or more of biomass-derived ethylene relative to the entire resin composition, preferably in the range of 5% by mass or more and less than 99% by mass, and more preferably in the range of 25% by mass or more and 90% by mass or less. If the concentration of biomass-derived ethylene in the resin composition is 5% by mass or more, the amount of fossil fuel used can be reduced more reliably than when conventional fossil fuels are used, and a carbon-neutral decorative sheet can be realized.

[0024] The above resin composition may contain two or more types of polyethylene with different biomass contents, and it is sufficient that the concentration of biomass-derived ethylene in the entire resin composition is within the above range. The resin composition may further contain fossil fuel-derived ethylene and fossil fuel-derived polyethylene obtained by polymerizing a monomer containing at least one of fossil fuel-derived ethylene and α-olefin. That is, in this embodiment, the resin composition may be a mixture of biomass-derived polyethylene and fossil fuel-derived polyethylene. The mixing method is not particularly limited, and mixing can be performed by a conventionally known method. For example, dry blending or melt blending may be used.

[0025] In the present embodiment, when a mixture with fossil fuel-derived polyethylene is used, the colored thermoplastic resin layer 2 contains 5% by mass or more, preferably 5 to 90% by mass, and more preferably 25 to 75% by mass of biomass-derived polyethylene. The resin composition may contain a mixture of biomass-derived polyethylene and, for example, fossil fuel-derived polyethylene, and even when such a resin composition of a mixture is used, the concentration of biomass-derived ethylene in the entire resin composition should be within the range of 5% by mass or more, preferably 5 to 90% by mass, and more preferably 25 to 75% by mass.

[0026] <Nucleating agent> The biomass-derived polyethylene that is the main material of the resin composition that forms the colored thermoplastic resin layer 2 may contain a nucleating agent (nucleating agent). The nucleating agent is preferably nanosized, for example. That is, the nucleating agent is preferably nanosized. In addition, in the colored thermoplastic resin layer 2, the nucleating agent is preferably added to the biomass-derived polyethylene in a range of 500 ppm or more and 2000 ppm or less, based on the mass of the biomass-derived polyethylene, and more preferably added to the biomass-derived polyethylene in a range of 1500 ppm or more and 2000 ppm or less. By including the nucleating agent in the colored thermoplastic resin layer 2 within the above range, the effect of high crystallinity is achieved.

[0027] <Additives> In addition to the polyethylene, which is the main component, various additives may be added to the resin composition forming the colored thermoplastic resin layer 2 produced in the above-mentioned resin composition production process, within a range in which the characteristics are not impaired. In other words, the colored thermoplastic resin layer 2 may contain various additives. Examples of additives (additives) include fillers, plasticizers, ultraviolet absorbers, light stabilizers, heat stabilizers, coloring inhibitors, matting agents, deodorants, flame retardants, weather resistance agents, antistatic agents, thread friction reducers, slip agents, mold release agents, antioxidants (antioxidants), ion exchange agents, and colorants (coloring pigments), antistatic agents, lubricants, antibacterial agents, antiviral agents, antifungal agents, antifriction agents, light scattering agents, and gloss adjusters. In addition, it is preferable to add one or more of the above-mentioned additives, particularly antibacterial agents, antiviral agents, and ultraviolet absorbers, as functional additives to the resin composition forming the colored thermoplastic resin layer 2. This can impart excellent functionality to the colored thermoplastic resin layer 2. These additives are added in an amount of preferably 1 to 20% by mass, more preferably 1 to 10% by mass, based on the total mass of the resin composition.

[0028] <Inorganic substances> The colored thermoplastic resin layer 2 may contain an inorganic substance. In other words, the resin composition forming the colored thermoplastic resin layer 2 may be configured to contain an inorganic substance. By adding an inorganic substance, it is possible to suitably control the specific gravity of the colored thermoplastic resin layer 2. As the inorganic substance, for example, any one or a plurality of calcium carbonate, titanium oxide, carbon black, silica, chromium, antimony, titanium composites, other oxides, and the like can be applied.

[0029] Furthermore, the colored thermoplastic resin layer 2 is preferably configured so that its specific gravity is within the range of 0.9 to 1.6. By adding an inorganic substance, the specific gravity of the colored thermoplastic resin layer 2 can be controlled within the above range. By adding an inorganic substance to the colored thermoplastic resin layer 2 so that its specific gravity is 0.9 to 1.6, the concealing property of the colored thermoplastic resin layer 2 can be improved.

[0030] As described above, the colored thermoplastic resin layer 2 contains 5% by mass or more, preferably 5% by mass or more and less than 99% by mass, of biomass-derived ethylene relative to the entire colored thermoplastic resin layer 2. If the concentration of biomass-derived ethylene in the colored thermoplastic resin layer 2 is 5% by mass or more, it is possible to reliably reduce the amount of fossil fuel used compared to conventional methods, and to realize a carbon-neutral decorative sheet.

[0031] The colored thermoplastic resin layer 2 may be any of those containing biomass-derived high-density polyethylene and biomass-derived low-density polyethylene, those containing biomass-derived high-density polyethylene and fossil fuel-derived polyethylene, and those containing fossil fuel-derived high-density polyethylene and biomass-derived low-density polyethylene, and the biomass degree of the entire colored thermoplastic resin layer 2 may be within the range of 10% or more and 90% or less.

[0032] Biomass-derived high-density polyethylene refers to polyethylene with a density exceeding 0.94, while biomass-derived low-density polyethylene refers to polyethylene with a density of 0.94 or less. The biomass-derived polyethylene for the colored thermoplastic resin layer 2 is preferably a blend of biomass-derived high-density polyethylene and low-density polyethylene (which may be derived from biomass or fossil fuels) in the range of 95:5 to 70:30. If the content of low-density polyethylene is low, the film formation stability is poor, and if the content of low-density polyethylene is high, the film becomes too soft.

[0033] The method for producing the colored thermoplastic resin layer 2 is not particularly limited, and the layer can be produced by a conventionally known method. In the present embodiment, the layer is preferably formed by calendar molding. The thickness of the colored thermoplastic resin layer 2 is preferably in the range of 30 μm to 150 μm, more preferably 51 μm to 150 μm, and even more preferably 55 μm to 100 μm. When the thickness of the colored thermoplastic resin layer 2 is 30 μm or more, it can absorb unevenness and steps of the floor material that serves as the base, improving the finish of the applied decorative sheet 1. In addition, when the thickness of the colored thermoplastic resin layer 2 is 150 μm or less, the colored thermoplastic resin layer 2 is not formed thicker than necessary, and the manufacturing cost of the decorative sheet 1 can be reduced.

[0034] In this embodiment, biomass-derived polyethylene has been described as the biomass-derived resin constituting the colored thermoplastic resin layer 2, but the present invention is not limited thereto. For example, biomass-derived polypropylene or biomass-derived polybutylene may be used instead of the above-mentioned biomass-derived polyethylene. In other words, in this embodiment, a wide variety of biomass-derived polyolefins can be used as the biomass-derived resin constituting the colored thermoplastic resin layer 2.

[0035] <Pattern printing layer> The pattern-printed layer 3 is laminated on one surface (the upper surface in FIG. 1) of the colored thermoplastic resin layer 2, and is intended to add a pattern that imparts design. Any pattern can be used as the pattern, and for example, a wood grain pattern, a stone pattern, a cloth pattern, an abstract pattern, a geometric pattern, letters, a light solid color, or a combination thereof can be applied.

[0036] The pattern-printed layer 3 is formed using, for example, printing ink or paint in which a colorant such as a dye or pigment is dissolved or dispersed in a diluting solvent together with an appropriate binder resin. As the binder resin, for example, urethane-based resin, acrylic-based resin, vinyl chloride acetate-based resin, polyimide-based resin, nitrocellulose, or a mixture thereof can be used, but is not limited to these. The printing ink or paint forming the pattern-printed layer 3 is applied using, for example, various printing methods such as gravure printing or offset printing, or various coating methods such as gravure coating or roll coating.

[0037] The pattern-printed layer 3 preferably has a thickness in the range of 1 μm to 10 μm. When the pattern-printed layer 3 has a thickness of 1 μm or more, the printing can be made clear. On the other hand, when the pattern-printed layer 3 has a thickness of 10 μm or less, the printing workability can be improved and an increase in manufacturing costs can be suppressed. The pattern printed layer 3 may also contain functional additives that do not require various functions, such as extender pigments, plasticizers, dispersants, surfactants, tackifiers, adhesive aids, drying agents, hardeners, hardening accelerators, and hardening retarders.

[0038] In order to improve the concealing properties of the decorative sheet 1, a concealing layer can be provided between the colored thermoplastic resin layer 2 and the pattern-printed layer 3. This concealing layer can be formed, for example, using an opaque printing ink or paint that contains a large amount of opaque pigments such as titanium dioxide or iron oxide. In addition, the pattern-printed layer 3 can be omitted when it can be substituted by the coloring of the colored thermoplastic resin layer 2.

[0039] <Adhesive layer> The adhesive layer 4 is laminated on one surface of the pattern-printed layer 3 (the upper surface in FIG. 1) and serves to bond the pattern-printed layer 3 and the transparent thermoplastic resin layer 5. As the adhesive layer 4, for example, a transparent adhesive made of a resin such as a urethane-based, acrylic-based, ethylene-vinyl acetate copolymer, vinyl chloride-vinyl acetate copolymer, polyester, or polyolefin-based adhesive can be applied. In particular, from the viewpoint of adhesion to the transparent thermoplastic resin layer 5, it is highly preferable that the adhesive layer is made of a polyolefin-based resin. The adhesive layer 4 may or may not be provided. If the adhesion between the pattern-printed layer 3 and the transparent thermoplastic resin layer 5 is sufficient, the adhesive layer 4 may not be provided.

[0040] <Transparent thermoplastic resin layer> The transparent thermoplastic resin layer 5 is laminated on one surface (the upper surface in FIG. 1) of the adhesive layer 4, and is a resin layer formed using a thermoplastic resin. More specifically, in this embodiment, the transparent thermoplastic resin layer 5 is a resin layer formed using a resin composition containing a biomass-derived (plant-derived) resin material. In this embodiment, the transparent thermoplastic resin layer 5 contains, as the main material of the resin composition, a biomass-derived polyolefin obtained by polymerizing a monomer containing a biomass-derived olefin, similar to the colored thermoplastic resin layer 2. For example, the transparent thermoplastic resin layer 5 in the decorative sheet 1 according to this embodiment is a transparent thermoplastic resin layer formed from a resin composition containing biomass-derived polypropylene as the biomass-derived resin material.

[0041] <Biomass-derived polypropylene> In this embodiment, the biomass-derived polypropylene is obtained by polymerizing a monomer containing biomass-derived propylene. The biomass-derived propylene is not particularly limited, and propylene produced by a conventionally known method can be used. Since biomass-derived propylene is used as the raw material monomer, the polymerized polypropylene is derived from biomass.

[0042] The raw material monomer for polypropylene does not necessarily have to contain 100% by mass of biomass-derived propylene. The monomers that are the raw material for biomass-derived polypropylene may further include propylene derived from fossil fuels. By using propylene, a raw material derived from biomass, it is theoretically possible to produce polypropylene from 100% biomass-derived components.

[0043] The biomass-derived propylene concentration in the polypropylene (hereinafter sometimes referred to as "biomass degree") is a value obtained by measuring the amount of biomass-derived carbon by the radiocarbon (C14) measurement, and the amount of biomass-derived carbon can be calculated by measuring the amount of C14 in the total carbon atoms in the polypropylene. In this embodiment, the amount of biomass-derived carbon Pbio can be calculated as follows, assuming that the amount of C14 in the polypropylene is PC14.

[0044] Pbio(%)=PC14 / 105.5×100 In this embodiment, theoretically, if all biomass-derived propylene is used as the raw material for polypropylene, the concentration of biomass-derived propylene is 100%, and the biomass degree of the biomass-derived polypropylene is 100. Moreover, the concentration of biomass-derived propylene in fossil fuel-derived polypropylene produced only from fossil fuel-derived raw materials is 0%, and the biomass degree of the fossil fuel-derived polypropylene is 0.

[0045] In this embodiment, the biomass-derived polypropylene or the decorative sheet 1 comprising this polypropylene does not necessarily have a biomass degree of 100. In this embodiment, the polymerization method of the monomer containing propylene derived from biomass is not particularly limited, and can be carried out by a conventionally known method. The polymerization temperature and polymerization pressure are preferably adjusted appropriately depending on the polymerization method and polymerization apparatus. The polymerization apparatus is also not particularly limited, and a conventionally known apparatus can be used. An example of the polymerization method of the monomer containing propylene will be described below.

[0046] The polymerization method for the propylene polymer can be appropriately selected depending on the type of the desired polypropylene, such as homopolypropylene, random polypropylene, block polypropylene, etc. For example, it is preferable to use a multi-site catalyst such as a Ziegler-Natta catalyst or a single-site catalyst such as a metallocene catalyst as a polymerization catalyst, and carry out the polymerization in one stage or in two or more stages by any of gas phase polymerization, slurry polymerization, solution polymerization, and high pressure ion polymerization.

[0047] As the biomass-derived polypropylene, homopolypropylene, random polypropylene, and block polypropylene may be used alone or in combination of two or more kinds.

[0048] <Resin composition containing biomass-derived polypropylene> In this embodiment, the resin composition contains the above-mentioned polypropylene as a main component. The resin composition forming the transparent thermoplastic resin layer 5, i.e., the transparent thermoplastic resin layer 5, contains biomass-derived propylene in an amount of 5% by mass or more, preferably 5% by mass or more and less than 99% by mass, and more preferably 25% by mass or more and 75% by mass or less, based on the entire resin composition. If the concentration of biomass-derived propylene in the resin composition is in the range of 5% by mass or more and less than 99% by mass, the amount of fossil fuel used can be reduced more reliably than before, and a carbon-neutral decorative sheet can be realized.

[0049] The above resin composition may contain two or more types of polypropylene having different biomass degrees, and it is sufficient that the concentration of biomass-derived propylene in the entire resin composition is within the above range. The resin composition may further contain propylene derived from a fossil fuel. That is, in this embodiment, the resin composition may be a mixture of biomass-derived polypropylene and fossil fuel-derived polypropylene. The mixing method is not particularly limited, and the materials may be mixed by a conventionally known method. For example, dry blending or melt blending may be used.

[0050] According to this embodiment, when the resin composition is a mixture with fossil fuel-derived polypropylene, it contains biomass-derived polypropylene in a range of preferably 5% by mass or more and less than 99% by mass, more preferably 25% by mass or more and 75% by mass or less, and fossil fuel-derived polypropylene in a range of preferably 1% by mass or more and 95% by mass or less, more preferably 25% by mass or more and 75% by mass or less. Even when such a resin composition of the mixture is used, it is sufficient that the concentration of biomass-derived propylene in the entire resin composition is within the above range.

[0051] <Nucleating agent> The biomass-derived polypropylene that is the main material of the resin composition that forms the transparent thermoplastic resin layer 5 may contain a nucleating agent (nucleating agent).

[0052] The nucleating agent is preferably nano-sized. That is, the nucleating agent is preferably nano-sized. In addition, in the transparent thermoplastic resin layer 5, the nucleating agent is preferably added to the biomass-derived polypropylene in a range of 500 ppm to 2000 ppm based on the mass of the biomass-derived polypropylene, and more preferably in a range of 1500 ppm to 2000 ppm based on the mass of the biomass-derived polypropylene. By adding a nucleating agent within the above range to the transparent thermoplastic resin layer 5, the haze (cloudiness value) can be reduced and the transparency of the transparent thermoplastic resin layer 5 can be improved.

[0053] In the decorative sheet 1 according to this embodiment, the nucleating agent may be added to at least one of the colored thermoplastic resin layer 2 or the transparent thermoplastic resin layer 5. In other words, in the colored thermoplastic resin layer 2 and the transparent thermoplastic resin layer 5 of the decorative sheet 1, the nucleating agent may be contained in both the colored thermoplastic resin layer 2 and the transparent thermoplastic resin layer 5, only the colored thermoplastic resin layer 2, or only the transparent thermoplastic resin layer 5.

[0054] <Additives> In addition to the polypropylene, which is the main component, various additives may be added to the resin composition forming the transparent thermoplastic resin layer 5 produced in the above-mentioned resin composition production process, as long as the characteristics are not impaired. That is, the transparent thermoplastic resin layer 5 may contain various additives. As the additives (additives), for example, as in the colored thermoplastic resin layer 2, fillers, plasticizers, ultraviolet absorbers, light stabilizers, heat stabilizers, coloring inhibitors, matting agents, deodorants, flame retardants, weather resistance agents, antistatic agents, thread friction reducing agents, slip agents, mold release agents, antioxidants (antioxidants), ion exchange agents, and colorants (coloring pigments), antistatic agents, lubricants, antibacterial agents, antiviral agents, antifungal agents, antifriction agents, light scattering agents, and gloss adjusting agents may be added. As in the colored thermoplastic resin layer 2, it is preferable to add one or more of the above-mentioned additives, particularly antibacterial agents, antiviral agents, and ultraviolet absorbers, as functional additives. This can impart excellent functionality to the transparent thermoplastic resin layer 5. These additives are added in an amount of preferably 1 to 20% by mass, more preferably 1 to 10% by mass, based on the total mass of the resin composition.

[0055] <Inorganic substances> As with the colored thermoplastic resin layer 2, the transparent thermoplastic resin layer 5 may contain an inorganic substance. In other words, the resin composition forming the transparent thermoplastic resin layer 5 may be configured to contain an inorganic substance. By adding an inorganic substance, the specific gravity of the transparent thermoplastic resin layer 5 can be suitably controlled. As with the colored thermoplastic resin layer 2, the inorganic substance in the transparent thermoplastic resin layer 5 may be, for example, any one or more of calcium carbonate, titanium oxide, carbon black, silica, chromium, antimony, titanium composites, and other oxides.

[0056] In the decorative sheet 1 according to this embodiment, it is sufficient that at least one of the colored thermoplastic resin layer 2 and the transparent thermoplastic resin layer 5 contains an inorganic substance or the above-mentioned functional additive. In other words, in the colored thermoplastic resin layer 2 and the transparent thermoplastic resin layer 5 of the decorative sheet 1, the inorganic substance may be contained in both the colored thermoplastic resin layer 2 and the transparent thermoplastic resin layer 5, or may be contained only in the colored thermoplastic resin layer 2, or may be contained only in the transparent thermoplastic resin layer 5. Furthermore, the above-mentioned functional additive may be contained in both the colored thermoplastic resin layer 2 and the transparent thermoplastic resin layer 5, or may be contained only in the colored thermoplastic resin layer 2, or may be contained only in the transparent thermoplastic resin layer 5.

[0057] Furthermore, the transparent thermoplastic resin layer 5 is preferably configured so that its specific gravity is within the range of 0.9 to 0.99. By adding an inorganic substance, the specific gravity of the transparent thermoplastic resin layer 5 can be controlled within the above range. By adding an inorganic substance to the transparent thermoplastic resin layer 5 so that the specific gravity is 0.9 to 0.99, the concealing property of the transparent thermoplastic resin layer 5 can be improved.

[0058] As described above, the transparent thermoplastic resin layer 5 contains biomass-derived propylene in an amount of 5% by mass or more, preferably 5% by mass or more and less than 99% by mass, and more preferably 25% by mass or more and 75% by mass or less, based on the entire transparent thermoplastic resin layer 5. If the concentration of biomass-derived propylene in the transparent thermoplastic resin layer 5 is 5% by mass or more, the amount of fossil fuel used can be more reliably reduced compared to conventional methods, and a carbon-neutral decorative sheet can be realized.

[0059] The transparent thermoplastic resin layer 5 may have a biomass content in the range of 10% to 90% throughout the entire transparent thermoplastic resin layer 5. The transparent thermoplastic resin layer 5 may contain polypropylene derived from fossil fuels in addition to the biomass-derived polypropylene. The method for producing the transparent thermoplastic resin layer 5 is not particularly limited, and the layer can be produced by a conventionally known method. In this embodiment, the layer is preferably formed by calendar molding.

[0060] The thickness of the transparent thermoplastic resin layer 5 is preferably in the range of 60 μm to 150 μm, more preferably in the range of 61 μm to 150 μm, and even more preferably in the range of 61 μm to 100 μm. If the thickness is within the above range, the wear resistance and scratch resistance are sufficiently within the practical range. Alternatively, in terms of design, the presence of the transparent thermoplastic resin layer 5, in combination with the picture print layer 3, has the effect of making the depth and depth feel greater. Specifically, if the thickness of the transparent thermoplastic resin layer 5 is less than 60 μm, the surface hardness may be reduced and the wear resistance and scratch resistance may not be sufficiently obtained. On the other hand, if the thickness of the transparent thermoplastic resin layer 5 exceeds 150 μm, the productivity during production may be poor, which may be disadvantageous in terms of cost.

[0061] In this embodiment, biomass-derived polypropylene has been described as the biomass-derived resin constituting the transparent thermoplastic resin layer 5, but the present invention is not limited thereto. For example, in addition to the above-mentioned biomass-derived polypropylene, biomass-derived polybutylene, etc. may be used. In other words, in this embodiment, a wide variety of biomass-derived polyolefins can be used as the biomass-derived resin constituting the transparent thermoplastic resin layer 5.

[0062] Furthermore, the biomass-derived resin constituting the transparent thermoplastic resin layer 5 is not limited to biomass-derived polyolefin. The transparent thermoplastic resin layer 5 may be composed of a biomass plastic other than biomass-derived polyolefin. In this case, the transparent thermoplastic resin layer 5 composed of the biomass plastic is preferably configured so that the specific gravity is within the range of 0.9 to 1.4. By adding an inorganic substance, the specific gravity of the transparent thermoplastic resin layer 5 composed of the biomass plastic can be controlled within the above range, thereby enhancing the concealing property of the transparent thermoplastic resin layer 5.

[0063] Furthermore, a concave-convex pattern 5a that is in harmony with the pattern of the picture-printed layer 3 is formed on the surface of the transparent thermoplastic resin layer 5 opposite the adhesive layer 4. This allows the pattern of the picture-printed layer 3 and the concave-convex pattern 5a of the transparent thermoplastic resin layer 5 to be in harmony with each other, improving the tactile feel and three-dimensional effect, and improving the realism of patterns such as wood grain, stone grain, fabric grain, and abstract patterns. In addition, the concave-convex pattern 5a can improve scratch resistance.

[0064] <Surface protective layer> The surface protection layer 6 is laminated on one surface of the transparent thermoplastic resin layer 5 (the upper surface in FIG. 1), through which the pattern of the picture print layer 3 can be seen, and is a sheet-like layer made of a transparent resin that protects the surface of the transparent thermoplastic resin layer 5. There is no particular limitation on the transparent resin, and any known transparent resin can be used. For example, a (meth)acrylate-based cured resin can be used. This makes the resin hard and tough. In particular, a urethane transparent thermoplastic resin layer is more preferable in terms of improving bending processability.

[0065] Furthermore, the resin constituting the surface protective layer 6 penetrates into the unevenness of the uneven pattern 5a of the transparent thermoplastic resin layer 5. That is, the surface protective layer 6 is formed with unevenness that follows the surface shape of the uneven pattern 5a. In this way, by forming the surface protective layer 6 with unevenness that follows the surface shape of the uneven pattern 5a and allowing the resin constituting the surface protective layer 6 to penetrate into the recesses of the uneven pattern 5a, the surface protective layer 6 can be firmly fixed to the transparent thermoplastic resin layer 5.

[0066] The surface protective layer 6 may contain various additives, such as weathering agents, plasticizers, stabilizers, fillers, dispersants, colorants such as dyes and pigments, solvents, ultraviolet absorbers, heat stabilizers, light stabilizers, antiblocking agents, catalyst scatterers, light scattering agents, gloss adjusters, etc. Furthermore, the surface protective layer 6 may contain functional additives, such as antibacterial agents, antifungal agents, and antiviral agents, if necessary.

[0067] <Gloss adjustment layer> The gloss adjusting layer 7 is a sheet-like layer made of a transparent resin through which the pattern of the picture printed layer 3 and the uneven pattern 5a of the transparent thermoplastic resin layer 5 can be seen through and which has a pattern due to the gloss state that is in harmony with the pattern pattern of the picture printed layer 3 and the uneven pattern 5a. The transparent resin is not particularly limited, and any known transparent resin can be used. For example, a composition in which a gloss adjusting agent is added to a two-liquid curing urethane resin can be used. As the gloss adjusting agent, for example, fine particles of inorganic substances such as silica, alumina (α-alumina, etc.), calcium carbonate, barium sulfate, kaolinite, aluminosilicate, etc., or organic substances (resins) such as polycarbonate, nylon, and urethane resin can be used. The average particle size of the gloss adjusting agent is preferably in the range of 1 μm or more and 10 μm or less. The amount of gloss adjusting agent added is appropriately selected depending on the pattern due to the desired gloss state, but it is usually preferable to set it to a maximum of 30 mass%. As the two-component curing urethane resin, for example, a urethane resin containing polyol as a main component and isocyanate as a crosslinking agent (curing agent) can be used. In addition, by forming a surface protection layer 6 and a gloss adjustment layer 7 on the transparent thermoplastic resin layer 5, it is possible to improve the tactile feel, the three-dimensional effect due to reflection, and the durability.

[0068] <Primer layer> The primer layer 8 is a base layer for improving adhesion and corrosion resistance between the colored thermoplastic resin layer 2 and the substrate 9. The primer layer 8 is provided on the surface of the colored thermoplastic resin layer 2 opposite the picture-printed layer 3. The primer layer 8 is formed using, for example, polyester resin, organic additives, pigments, etc. The primer layer 8 may contain an anti-rust pigment for the purpose of improving corrosion resistance. The thickness of the primer layer 8 is, for example, in the range of 1 μm to 10 μm.

[0069] <Base material> The substrate 9 is a plate-shaped member made of metal, wood, etc. There are no particular limitations on the metal, wood, etc., and any known metal, wood, etc. can be used. For example, aluminum, steel, stainless steel, MDF (medium density fiberboard), particle board, etc. can be used. <Decorative sheet manufacturing equipment> Next, a transparent thermoplastic resin layer forming apparatus 101 for forming the transparent thermoplastic resin layer 5 and a gloss adjusting layer forming apparatus 102 for forming the gloss adjusting layer 7 will be described. <Transparent thermoplastic resin layer forming device> In FIG. 2, (a) is a schematic diagram showing an example of a transparent thermoplastic resin layer forming apparatus 101, and (b) is an enlarged view of a portion where lamination is performed by rollers 14a and 14b.

[0070] The transparent thermoplastic resin layer forming apparatus 101 includes a feeding section 12, an extrusion section 13, a bonding section 14, and a winding section 15. In this embodiment, the formation of the picture printed layer 3 and the formation of the transparent thermoplastic resin layer 5 are performed in separate apparatuses. The unwinding unit 12 holds a first unwinding roll 19 rotatably about its axis, the first unwinding roll 19 having a laminate (hereinafter also referred to as "first laminate 18") wound thereon, in which a picture-printed layer 3 is laminated on one side of a colored thermoplastic resin layer 2. The unwinding unit 12 then unwinds the first laminate 18 from the held first unwinding roll 19 at a predetermined set speed and transfers it to the laminating unit 14.

[0071] The extrusion unit 13 melts a transparent resin for forming the transparent thermoplastic resin layer 5. Then, the extrusion unit 13 extrudes the molten resin to form it into a film shape, and supplies it to the lamination unit . The laminating section 14 sandwiches the first laminate 18 transferred from the unwinding section 12 and the film-like resin supplied from the extrusion section 13 between a pair of rollers 14a, 14b to laminate them together (extrusion lamination). As a result, the transparent thermoplastic resin layer 5 is laminated on the first laminate 18 by extrusion lamination, and a laminate 18a for forming a concave-convex pattern is formed in which the picture print layer 3 and the transparent thermoplastic resin layer 5 are laminated in this order on one side of the colored thermoplastic resin layer 2. Here, the roller 14a is driven to rotate so as to pull the first laminate 18 by the frictional force between the roller 14a and the first laminate 18. The roller 14b is also biased toward the roller 14a, increasing the frictional force between the roller 14a and the first laminate 18, and is pulled and rotated by the first laminate 18.

[0072] A printing plate (embossing plate) is provided on the outer peripheral surface of the roller 14a that comes into contact with the transparent thermoplastic resin layer 5 to form an uneven pattern 5a in harmony with the design pattern of the picture printed layer 3 on the transparent thermoplastic resin layer 5. Therefore, after the uneven pattern forming laminate 18a is formed by the first laminate 18 passing through the laminating section 14, the uneven pattern 5a is formed on the surface of the uneven pattern forming laminate 18a.

[0073] The winding section 15 forms a second delivery roll 21 by winding a laminate (hereinafter also referred to as a "second laminate 20") that is formed by extrusion lamination and on which the uneven pattern 5a is formed. In addition, when an adhesive layer 4 is provided between the picture-printed layer 3 and the transparent thermoplastic resin layer 5, adhesive can be applied to the surface on the picture-printed layer 3 side while the first laminate 18 is being transported to the lamination section 14.

[0074] <Gloss adjustment layer forming device> As shown in FIG. 3, the gloss adjusting layer forming device 102 includes a feeding section 22, a coating section 23, and a winding section 24. The unwinding section 22 holds a third unwinding roll 28 rotatably around its axis, around which a laminate (hereinafter also referred to as "third laminate (laminate for forming gloss adjusting layer) 27") is wound, in which a picture-printed layer 3, a transparent thermoplastic resin layer 5, and a surface protective layer 6 are laminated in this order on one surface of a colored thermoplastic resin layer 2. The unwinding section 22 then unwinds the third laminate 27 from the held third unwinding roll 28 and transfers it to the coating section 23.

[0075] The coating section 23 sandwiches the third laminate 27 transferred from the pay-out section 22 between a pair of rollers 23a, 23b, and coats the resin for forming the gloss-adjusting layer 7, forming the gloss-adjusting layer 7 having a pattern with a gloss state that is in tune with the pattern design of the picture-printed layer 3. As a result, the gloss-adjusting layer 7 is laminated on the surface protective layer 6 of the third laminate 27, and a laminate (hereinafter also referred to as "fourth laminate 29") is formed in which the picture-printed layer 3, the transparent thermoplastic resin layer 5, the surface protective layer 6 and the gloss-adjusting layer 7 are laminated on one side of the colored thermoplastic resin layer 2.

[0076] A printing plate is provided on the outer peripheral surface of the roller 23a that applies the resin, for forming a glossy pattern (hereinafter also referred to as a "pattern with a desired glossy state") on the surface protective layer 6 that is in tune with the design of the picture printed layer 3. The winding section 24 winds the fourth laminate 29 formed in the coating section 23 to form a fourth delivery roll 30.

[0077] <Characteristics of laminate> Next, the characteristics of the laminate will be described. <Laminate for forming uneven patterns> The laminate 18a for forming a concave-convex pattern has an elasticity characteristic (hereinafter also referred to as an elasticity characteristic for synchronizing a concave-convex pattern) such that when the laminate 18a for forming a concave-convex pattern is transported and a concave-convex pattern 5a is formed on the surface of the transparent thermoplastic resin layer 5, the laminate 18a for forming a concave-convex pattern stretches in the transport direction within a range of 0.02% to 3.0% of a preset basic length in the transport direction of the laminate 18a for forming a concave-convex pattern, and shrinks in the orthogonal direction within a range of 0.02% to 0.9% of a preset basic length in the orthogonal direction perpendicular to the transport direction.

[0078] In other words, as shown in Figure 2, when the gloss adjusting layer 7 is formed while transporting the first laminate 18 and the laminate 18a for forming the uneven pattern, as the first laminate 18 is transported, a force that stretches it in the transport direction is applied to the first laminate 18, so that the first laminate 18 expands in the transport direction and contracts in the perpendicular direction, and the laminate 18a for forming the uneven pattern may also deform in the same manner. Here, in this embodiment, in order to synchronize the uneven pattern 5a with the pattern of the picture-printed layer 3, for example, positioning marks are set in advance on the picture-printed layer 3, and in the transparent thermoplastic resin layer forming device 101, the uneven pattern 5a is formed on the uneven pattern forming laminate 18a using the marks on the picture-printed layer 3 as a guide so that the pattern of the picture-printed layer 3 and the gloss adjusting layer 7 overlap in a planar view.

[0079] Since the embossed pattern 5a is formed using the marks on the picture-printed layer 3 as a guide, if the first laminate 18, i.e., the laminate 18a for forming the embossed pattern, expands in the transport direction during transport and shrinks in the perpendicular direction, deforming the pattern. Even if the embossed pattern 5a is formed so that the pattern pattern of the picture-printed layer 3 and the embossed pattern 5a overlap using the marks on the picture-printed layer 3 as a guide, depending on the part of the laminate 18a for forming the embossed pattern, the embossed pattern 5a may be formed in a location other than the intended location, and as a result, the pattern pattern of the picture-printed layer 3 and the embossed pattern 5a may be misaligned when viewed in a planar view.

[0080] In this case, if the expansion rate of the first laminate 18, i.e., the laminate 18a for forming the concave-convex pattern, in the transport direction is 3.0% or less, the concave-convex pattern 5a can be regarded as being synchronized even if a deviation occurs between the pattern pattern of the picture-printed layer 3 and the concave-convex pattern 5a by forming the concave-convex pattern 5a on the laminate 18a for forming the concave-convex pattern in a state in which the laminate is deformed in the transport direction. Similarly, if the contraction rate of the laminate 18a for forming the concave-convex pattern in the orthogonal direction is 0.9% or less, the laminate 18a for forming the concave-convex pattern can be regarded as being synchronized even if a deviation occurs between the pattern pattern of the picture-printed layer 3 and the concave-convex pattern 5a by the laminate 18a for forming the concave-convex pattern deforming in the orthogonal direction. If the expansion rate of the laminate 18a for forming the concave-convex pattern in the transport direction is greater than 3.0%, or if the contraction rate in the orthogonal direction is greater than 0.9%, the deviation between the pattern pattern of the picture-printed layer 3 and the concave-convex pattern 5a caused by the laminate 18a for forming the concave-convex pattern deforming in the transport direction or the orthogonal direction is large, and it is difficult to say that they are synchronized. In addition, in order to transport the uneven pattern-forming laminate 18a, the expansion rate in the transport direction and the contraction rate in the perpendicular direction of the uneven pattern-forming laminate 18a are preferably 0.02% or more.

[0081] From the above, by using a laminate having an elastic property for synchronizing the concave-convex pattern as the concave-convex pattern forming laminate 18a, i.e., the first laminate 18, it is possible to suppress synchronization failure caused by the deformation of the concave-convex pattern forming laminate 18a during transportation. In other words, when forming the concave-convex pattern 5a on the surface of the transparent thermoplastic resin layer 5 side while transporting the concave-convex pattern forming laminate 18a, the stretch rate of the concave-convex pattern forming laminate 18a in the transport direction relative to a preset basic length in the transport direction of the concave-convex pattern forming laminate 18a is within a range of 0.02% to 3.0%, and the shrink rate of the concave-convex pattern forming laminate 18a in the orthogonal direction relative to a preset basic length in the orthogonal direction perpendicular to the transport direction is within a range of 0.02% to 0.9%, thereby suppressing synchronization failure between the design pattern of the picture-printed layer 3 and the concave-convex pattern 5a.

[0082] <Second laminate> The second laminate 20 has a characteristic that, when the concave-convex pattern 5a is formed on the concave-convex pattern forming laminate 18a, the deviation amount in the transport direction of the concave-convex pattern forming laminate 18a between a reference position previously set on the picture-printed layer 3 and a reference position previously assumed for the concave-convex pattern 5a as a position overlapping with the reference position set on the picture-printed layer 3 in a plan view is 10 mm or less, and the deviation amount in the orthogonal direction perpendicular to the transport direction is 3 mm or less (hereinafter, also referred to as a deviation characteristic for concave-convex pattern synchronization). If the deviation amount in the transport direction between the pattern pattern of the picture-printed layer 3 and the concave-convex pattern 5a is 10 mm or less, it can be considered that the pattern pattern of the picture-printed layer 3 and the concave-convex pattern 5a are synchronized even if a deviation occurs. Similarly, if the deviation amount in the orthogonal direction is 3 mm or less, it can be considered that the pattern pattern of the picture-printed layer 3 and the concave-convex pattern 5a are synchronized even if a deviation occurs. If the amount of deviation in the transport direction between the pattern of the picture-printed layer 3 and the uneven pattern 5a is greater than 10 mm, or if the amount of deviation in the perpendicular direction is greater than 3 mm, it is difficult to say that the deviation between the pattern of the picture-printed layer 3 and the uneven pattern 5a is significantly synchronized.

[0083] From the above, by using a laminate having a shift characteristic for synchronizing the uneven pattern as the second laminate 20, synchronization failure caused by the deformation of the uneven pattern forming laminate 18a can be suppressed. In other words, by forming the second laminate 20 so that in the second laminate 20 after the uneven pattern 5a is formed on the uneven pattern forming laminate 18a, the amount of shift in the transport direction of the uneven pattern forming laminate 18a between a reference position previously set on the picture-printed layer 3 and a reference position previously assumed for the uneven pattern 5a as a position overlapping the reference position set on the picture-printed layer 3 in a plan view is 10 mm or less, and the amount of shift in the orthogonal direction perpendicular to the transport direction is 3 mm or less, synchronization failure between the pattern pattern of the picture-printed layer 3 and the uneven pattern 5a can be suppressed.

[0084] In addition, when the uneven pattern 5a is formed not on the laminate 18a for forming the uneven pattern, but on a laminate A (not shown) in which the colored thermoplastic resin layer 2, the picture printed layer 3, the transparent thermoplastic resin layer 5, and the surface protective layer 6 are laminated in this order after the surface protective layer 6 has been formed, a laminate is used as the laminate A in which the expansion and contraction rates in the transport direction and orthogonal direction of the laminate A when forming the uneven pattern 5a have expansion and contraction characteristics for synchronizing with the uneven pattern, and in laminate B (not shown), which is the laminate A after the uneven pattern 5a has been formed, a laminate is used as the laminate B in which the amount of deviation between the reference position set on the picture printed layer 3 and the reference position previously set on the uneven pattern 5a has deviation characteristics for synchronizing with the uneven pattern, thereby obtaining an effect equivalent to that described above.

[0085] In addition, each of the laminate 18a for forming the uneven pattern and the second laminate 20 may have stretch characteristics or shift characteristics for synchronizing the uneven pattern in order to synchronize the pattern of the picture printed layer 3 with the uneven pattern 5a, or only the laminate 18a for forming the uneven pattern may have stretch characteristics for synchronizing the uneven pattern, or only the second laminate 20 may have shift characteristics for synchronizing the uneven pattern.

[0086] <Third laminate> The third laminate 27, which is formed by laminating the colored thermoplastic resin layer 2, the picture print layer 3, the transparent thermoplastic resin layer 5, and the surface protection layer 6 in this order, has the following properties when the third laminate 27 is unwound from the third unwound roll 28 in the gloss adjusting layer forming device 102 and transferred to the coating section 23 to form the gloss adjusting layer 7. That is, the third laminate 27 has an expansion and contraction property (hereinafter also referred to as the expansion property for synchronizing the gloss adjusting layer) that when it is stretched in the transport direction within a range of 0.02% to 3.0% of a preset basic length in the transport direction of the third laminate 27, it shrinks in the orthogonal direction within a range of 0.02% to 0.9% of a preset basic length in the orthogonal direction perpendicular to the transport direction.

[0087] That is, in this embodiment, in order to synchronize the gloss-adjusting layer 7 with the pattern pattern of the picture-printed layer 3, for example, a mark for positioning is set in advance on the picture-printed layer 3, and in the transparent thermoplastic resin layer forming device 101, the gloss-adjusting layer 7 is formed on the third laminate 27 so that the pattern pattern of the picture-printed layer 3 and the gloss-adjusting layer 7 overlap in a planar view, using the mark on the picture-printed layer 3 as a clue. Therefore, even when the gloss-adjusting layer 7 is formed so that the pattern pattern of the picture-printed layer 3 and the gloss-adjusting layer 7 overlap using the mark on the picture-printed layer 3 as a clue, depending on the part of the gloss-adjusting layer 7, it may be formed in a place different from the expected place on the third laminate 27, and as a result, the pattern pattern of the picture-printed layer 3 and the gloss-adjusting layer 7 may be misaligned in a planar view.

[0088] In this embodiment, the third laminate 27 has an expansion and contraction characteristic (hereinafter also referred to as an expansion and contraction characteristic for synchronizing the gloss adjustment layer) in which, when the third laminate 27 is expanded in the transport direction within a range of 0.02% to 3.0% of a preset basic length in the transport direction of the third laminate 27 when the gloss adjustment layer 7 is formed on the surface of the surface protective layer 6 side while the third laminate 27 is being transported, the third laminate 27 shrinks in the orthogonal direction within a range of 0.02% to 0.9% of a preset basic length in the orthogonal direction perpendicular to the transport direction. If the expansion and contraction rate of the third laminate 27 in the transport direction is 3.0% or less, it can be considered that the pattern of the picture-printed layer 3 and the gloss adjustment layer 7 are synchronized even if a deviation occurs between them by forming the gloss adjustment layer 7 on the third laminate 27 in a state deformed in the transport direction. Similarly, if the contraction rate of the third laminate 27 in the orthogonal direction is 0.9% or less, it can be considered that the pattern of the picture-printed layer 3 and the gloss adjustment layer 7 are synchronized even if a deviation occurs between them by the deformation of the third laminate 27 in the orthogonal direction. If the expansion rate of the third laminate 27 in the transport direction is greater than 3.0%, or the shrinkage rate in the orthogonal direction is greater than 0.9%, the third laminate 27 deforms in the transport direction or the orthogonal direction, causing a large misalignment between the pattern of the picture-printed layer 3 and the gloss-adjusting layer 7, making it difficult to say that they are in harmony. In addition, in order to transport the third laminate 27, the expansion rate of the third laminate 27 in the transport direction and the shrinkage rate in the orthogonal direction are preferably 0.02% or more.

[0089] From the above, by using a laminate having elastic properties for synchronizing the gloss-adjusting layer as the third laminate 27, it is possible to suppress synchronization failure between the pattern pattern of the picture-printed layer 3 and the gloss-adjusting layer 7 caused by deformation of the third laminate 27 during transportation. In other words, when the gloss-adjusting layer 7 is formed on the surface of the third laminate 27 on the surface protective layer 6 side while transporting the third laminate 27, the third laminate 27 is transported so that the extension rate of the third laminate 27 in the transport direction relative to a preset basic length in the transport direction of the third laminate 27 is within a range of 0.02% to 3.0%, and the contraction rate of the third laminate 27 in the orthogonal direction relative to a preset basic length in the orthogonal direction perpendicular to the transport direction is within a range of 0.02% to 0.9%, thereby suppressing synchronization failure between the pattern pattern of the picture-printed layer 3 and the gloss-adjusting layer 7.

[0090] <Fourth laminate> The fourth laminate 29 has a misalignment characteristic (hereinafter also referred to as a misalignment characteristic for synchronizing the gloss-adjusting layer) in which, when the gloss-adjusting layer forming device 102 unwinds the third laminate 27 from the third unwinding roll 28 and transports it to the coating section 23 to form the gloss-adjusting layer 7, the misalignment in the laminate transport direction between a reference position previously set for the pattern-printed layer 3 and a reference position previously set for the gloss-adjusting layer 7 as a position overlapping with this reference position in a plan view is 6 mm or less, and the misalignment in the orthogonal direction perpendicular to the transport direction is 1.5 mm or less. If the misalignment in the transport direction between the pattern of the pattern-printed layer 3 and the gloss-adjusting layer 7 is 6 mm or less, it can be considered that the pattern of the pattern-printed layer 3 and the gloss-adjusting layer 7 are synchronized even if a misalignment occurs. Similarly, if the misalignment in the orthogonal direction is 1.5 mm or less, it can be considered that the pattern of the pattern-printed layer 3 and the gloss-adjusting layer 7 are synchronized even if a misalignment occurs. If the deviation between the pattern of the picture-printed layer 3 and the gloss-adjusting layer 7 in the transport direction is greater than 6 mm, or if the deviation in the perpendicular direction is greater than 1.5 mm, the deviation between the pattern of the picture-printed layer 3 and the gloss-adjusting layer 7 is large and it is difficult to say that they are synchronized.

[0091] Therefore, since the fourth laminate 29 has a misalignment characteristic for synchronizing the gloss adjusting layer, it is possible to suppress synchronization failure between the pattern pattern of the picture-printed layer 3 and the gloss adjusting layer 7, which is caused by deformation of the third laminate 27 during transport. In other words, by forming the fourth laminate 29 on which the gloss adjusting layer 7 is formed, such that the misalignment amount in the transport direction of the third laminate 27 between a reference position previously set on the picture-printed layer 3 and a reference position previously assumed for the gloss adjusting layer 7 as a position overlapping the reference position set on the picture-printed layer 3 in a plan view is 10 mm or less, and the misalignment amount in the orthogonal direction perpendicular to the transport direction is 3 mm or less, it is possible to suppress synchronization failure between the pattern pattern of the picture-printed layer 3 and the uneven pattern 5a.

[0092] In addition, each of the third laminate 27 and the fourth laminate 29 may have stretch characteristics or shift characteristics for synchronizing the gloss adjusting layer 7 with the pattern of the picture printed layer 3, or only the third laminate 27 may have stretch characteristics for synchronizing the gloss adjusting layer, or only the fourth laminate 29 may have shift characteristics for synchronizing the gloss adjusting layer.

[0093] <Method of manufacturing decorative sheets> Next, a method for producing the decorative sheet 1 having the above-mentioned configuration will be described. In the production of the decorative sheet 1, the first to fifth steps are carried out in this order.

[0094] <1st process: Pattern printing layer formation process> A pay-out roll around which the colored thermoplastic resin layer 2 is wound is prepared. Next, the colored thermoplastic resin layer 2 is paid out from the prepared pay-out roll, and the paid-out colored thermoplastic resin layer 2 is passed between a plate cylinder and an impression cylinder, and patterns are sequentially printed on one surface side of the colored thermoplastic resin layer 2 to form a pattern-printed layer 3. This forms a first laminate 18 in which the pattern-printed layer 3 is laminated on one surface side of the colored thermoplastic resin layer 2. Next, the formed first laminate 18 is wound to form a first pay-out roll 19.

[0095] <Second step: Transparent thermoplastic resin layer formation step> As shown in FIG. 2, the unwinding section 12 of the transparent thermoplastic resin layer forming device 101 unwinds the first laminate 18 from the first unwinding roll 19 and transfers the unwound first laminate 18 to the laminating section 14. The extrusion section 13 melts the transparent resin for forming the transparent thermoplastic resin layer 5, extrudes the molten resin to form a film, and supplies it to the laminating section 14. The laminating section 14 then sandwiches the first laminate 18 transferred from the unwinding section 12 and the film-like resin supplied from the extrusion section 13 between a pair of rollers 14a and 14b to bond them together. As a result, the transparent thermoplastic resin layer 5 is laminated on the picture-printed layer 3 of the first laminate 18 by extrusion lamination, and a laminate (a laminate 18a for forming a concave-convex pattern) in which the picture-printed layer 3 and the transparent thermoplastic resin layer 5 are laminated on one side of the colored thermoplastic resin layer 2 is formed. At the same time, the roller 14a forms, on the transparent thermoplastic resin layer 5, a concave-convex pattern 5a that is in sync with the design pattern of the picture-printed layer 3. At this time, in the transparent thermoplastic resin layer forming device 101, the transport speeds of the first laminate 18 and the concave-convex pattern forming laminate 18a and each part of the laminating unit 14 are controlled so that the reference position of the design pattern of the picture-printed layer 3 and the reference position of the concave-convex pattern 5a overlap in a plan view.

[0096] Furthermore, the winding section 15 winds up the laminate (second laminate 20) formed by the extrusion lamination process to form a second delivery roll 21. At this time, the laminate 18a for forming the uneven pattern and the second laminate 20 are formed so that the laminate 18a for forming the uneven pattern has an expansion and contraction characteristic for synchronizing with the uneven pattern, and the second laminate 20 has a shift characteristic for synchronizing with the uneven pattern.

[0097] <3rd step: Surface protective layer formation step> The second laminate 20 is unwound from the second unwinding roll 21, and the resin for forming the surface protective layer 6 is applied onto the transparent thermoplastic resin layer 5 of the unwound second laminate 20. This forms a third laminate 27 in which the surface protective layer 6 is laminated onto the second laminate 20. At this time, the resin for forming the surface protective layer 6 is applied onto the transparent thermoplastic resin layer 5 along the surface shape of the uneven pattern 5a, so that the resin forming the surface protective layer 6 is in a state in which it penetrates into the unevenness of the uneven pattern 5a of the transparent thermoplastic resin layer 5, that is, in a state in which it penetrates into the recesses of the uneven pattern 5a. This causes the surface protective layer 6 to be firmly fixed to the transparent thermoplastic resin layer 5. Next, the formed third laminate 27 is wound to form a third unwinding roll 28.

[0098] <4th step: gloss adjustment layer formation step> 3, the unwinding section 22 of the gloss-adjusting layer forming device 102 unwinds the third laminate 27 from the third unwinding roll 28, and transfers the unwound third laminate 27 to the coating section 23. The coating section 23 then coats the third laminate 27 transferred from the unwinding section 22 with a resin for forming the gloss-adjusting layer 7 to form the gloss-adjusting layer 7 having a pattern based on a gloss state that is in tune with the pattern of the picture-printed layer 3. At this time, the gloss-adjusting layer forming device 102 controls the transfer speed of the third laminate 27 and each section of the coating section 23 so that a reference position set for the pattern of the picture-printed layer 3 coincides with a reference position previously set for the gloss-adjusting layer 7.

[0099] As a result, the gloss adjusting layer 7 is laminated on the surface protective layer 6 of the third laminate 27, and a fourth laminate 29 is formed in which the picture printed layer 3, the transparent thermoplastic resin layer 5, the surface protective layer 6 and the gloss adjusting layer 7 are laminated on one side of the colored thermoplastic resin layer 2. At this time, the third laminate 27 and the fourth laminate 29 are formed so that the third laminate 27 has an expansion and contraction characteristic for forming a gloss adjusting layer, and the fourth laminate 29 has a displacement characteristic for forming a gloss adjusting layer.

[0100] Moreover, the winding section 24 winds up the laminate (fourth laminate 29) formed by the pair of rollers 23a, 23b to form a fourth pay-out roll 30. As a result, a decorative sheet 1 can be obtained in which the colored thermoplastic resin layer 2, the picture printed layer 3, the transparent thermoplastic resin layer 5, the surface protective layer 6, and the gloss adjusting layer 7 are laminated. <5th step: Primer layer formation step> Furthermore, a fourth laminate 29 is fed from a fourth feed roll 30, and a resin for forming a primer layer 8 is applied to the other surface side of the fed fourth laminate 29. This makes it possible to obtain a decorative sheet 1 in which the primer layer 8 is laminated on the fourth laminate 29.

[0101] <Effects of this embodiment> The decorative sheet 1 according to this embodiment can achieve the effects described below. (1) The decorative sheet 1 according to this embodiment is formed by laminating a colored thermoplastic resin layer 2, a pattern printed layer 3, a transparent thermoplastic resin layer 5, and a surface protective layer 6 in this order, and further includes a gloss adjusting layer 7 on the surface protective layer 6 side that matches the pattern of the pattern printed layer 3, and has an uneven pattern 5a across the surface protective layer 6 and the transparent thermoplastic resin layer 5, and at least one of the colored thermoplastic resin layer 2 and the transparent thermoplastic resin layer 5 is formed using a resin composition derived from biomass. Therefore, it is possible to provide a decorative sheet 1 that can reduce dependency on petroleum as a material and conserve petroleum resources.

[0102] (2) The third laminate 27, which is formed by laminating the colored thermoplastic resin layer 2, the pattern-printed layer 3, the transparent thermoplastic resin layer 5, and the surface protective layer 6 in this order, has an elasticity characteristic for forming a gloss-adjusting layer, in which when the third laminate 27 is stretched in the transport direction within a range of 0.02% to 3.0% of a preset basic length while the third laminate 27 is being transported and the gloss-adjusting layer 7 is formed on the surface of the surface protective layer 6, the third laminate 27 shrinks in the orthogonal direction perpendicular to the transport direction within a range of 0.02% to 0.9% of a preset basic length. Therefore, even if the third laminate 27 is deformed in the transport direction or the orthogonal direction by transporting the third laminate 27, it is possible to suppress the occurrence of a mismatch between the gloss-adjusting layer 7 formed on the deformed third laminate 27 and the pattern of the pattern-printed layer 3.

[0103] Similarly, the fourth laminate 29, which is a laminate obtained after the gloss adjusting layer 7 is formed on the surface of the third laminate 27 on the surface protective layer 6 side while the third laminate 27 is being transported, has a shift characteristic for forming a gloss adjusting layer in which the shift amount in the transport direction between a reference position previously set on the picture-printed layer 3 and a reference position previously set on the gloss adjusting layer 7 as a position overlapping with this reference position in a plan view is 6 mm or less, and the shift amount in the orthogonal direction perpendicular to the transport direction is 1.5 mm or less. Therefore, even if the third laminate 27 is deformed in the transport direction or the orthogonal direction by transporting the third laminate 27, it is possible to suppress the occurrence of mismatch between the gloss adjusting layer 7 formed on the deformed third laminate 27 and the pattern of the picture-printed layer 3.

[0104] (3) Furthermore, since the pattern of the picture-printed layer 3 and the gloss-adjusting layer 7 are synchronized, and the pattern of the picture-printed layer 3 and the uneven pattern 5a are synchronized, a decorative sheet 1 with a more attractive design can be obtained.

[0105] (4) The uneven pattern-forming laminate 18a, which is formed by laminating the colored thermoplastic resin layer 2, the picture-printed layer 3, and the transparent thermoplastic resin layer 5 in this order, has an expansion and contraction characteristic for forming an uneven pattern, in which when the uneven pattern-forming laminate 18a is transferred and the uneven pattern 5a is formed on the surface of the transparent thermoplastic resin layer 5, the uneven pattern-forming laminate 18a expands in the transfer direction within a range of 0.02% to 3.0% of a preset basic length, and contracts in the orthogonal direction perpendicular to the transfer direction within a range of 0.02% to 0.9% of a preset basic length. Therefore, even if the uneven pattern-forming laminate 18a is deformed in the transfer direction or the orthogonal direction by transferring the first laminate 18 and the uneven pattern-forming laminate 18a, it is possible to suppress poor synchronization between the uneven pattern 5a formed on the deformed uneven pattern-forming laminate 18a and the pattern of the picture-printed layer 3.

[0106] Similarly, the second laminate 20, which is a laminate obtained after the uneven pattern 5a is formed on the transparent thermoplastic resin layer 5 of the uneven pattern forming laminate 18a while the uneven pattern forming laminate 18a is being transported, has a shift characteristic for forming an uneven pattern in which the shift amount in the transport direction between a reference position preset on the picture-printed layer 3 and a reference position preset on the uneven pattern 5a as a position overlapping with this reference position in a plan view is 10 mm or less, and the shift amount in the orthogonal direction perpendicular to the transport direction is 3 mm or less. Therefore, even if the uneven pattern forming laminate 18a is deformed in the transport direction or the orthogonal direction by transporting the first laminate 18 and the uneven pattern forming laminate 18a, it is possible to suppress the occurrence of a mismatch between the uneven pattern 5a formed on the deformed uneven pattern forming laminate 18a and the pattern of the picture-printed layer 3.

[0107] (5) The uneven pattern 5a is formed on the surface of the transparent thermoplastic resin layer 5 opposite the picture-printed layer 3, and the surface protective layer 6 is formed such that the resin forming the surface protective layer 6 penetrates into the unevenness of the uneven pattern 5a. Therefore, the surface protective layer 6 can be firmly fixed to the transparent thermoplastic resin layer 5.

[0108] (6) The colored thermoplastic resin layer 2 and the transparent thermoplastic resin layer 5 contain, as the main material of the resin composition, a biomass-derived polyolefin formed by polymerizing a monomer containing a biomass-derived olefin, which reduces dependency on petroleum and makes it possible to obtain an environmentally friendly decorative sheet 1.

[0109] (7) The transparent thermoplastic resin layer 5 is laminated by extrusion lamination to the laminate (first laminate 18) of the colored thermoplastic resin layer 2 and the picture-printed layer 3. Therefore, the amount of adhesive between the transparent thermoplastic resin layer 5 and the picture-printed layer 3 can be reduced, and the picture of the picture-printed layer 3 can be seen more clearly through the transparent thermoplastic resin layer 5.

[0110] (8) The decorative material 10 according to this embodiment is formed by attaching a substrate to the primer layer 8 side of the decorative sheet 1. Therefore, a decorative material with a high design quality can be obtained in which the uneven pattern 5a and the gloss adjusting layer 7 are in harmony with the design of the picture printed layer 3. EXAMPLES

[0111] Examples 1 to 7 and Comparative Examples 1 to 9 of the decorative sheet according to the present invention will be described below. However, the present invention is not limited to the following examples.

[0112] Example 1 In Example 1, a decorative sheet was produced using the following materials and procedures. First, a wood grain pattern was printed on the colored thermoplastic resin layer 2 to form a pattern-printed layer 3, thereby forming a first laminate 18. A transparent thermoplastic resin layer 5 was laminated by extrusion lamination on the pattern printed layer 3 side of this first laminate 18 to form a laminate 18a for forming a concave-convex pattern, and a concave-convex pattern 5a was formed on the transparent thermoplastic resin layer 5 side of the laminate 18a for forming a concave-convex pattern to obtain a second laminate 20. Next, a surface protection layer 6 made of a urethane resin was laminated on the surface of the second laminate 20 on the transparent thermoplastic resin layer 5 side, to obtain a third laminate 27. Next, a gloss-adjusting layer 7 having a pattern depending on the gloss state that is in harmony with the pattern of the picture-printed layer 3 was provided on the surface protective layer 6, thereby obtaining a fourth laminate 29, i.e., a decorative sheet in which the colored thermoplastic resin layer 2, the picture-printed layer 3, the transparent thermoplastic resin layer 5, the surface protective layer 6 and the gloss-adjusting layer 7 are laminated.

[0113] At this time, when forming the uneven pattern 5a, the elongation rate in the transport direction of the laminate 18a for forming the uneven pattern with respect to the preset basic length in the transport direction was 0.02%, and the contraction rate in the perpendicular direction with respect to the preset basic length in the perpendicular direction was 0.02%. Furthermore, when forming the gloss adjusting layer 7, the third laminate 27 had an elongation rate in the transport direction of 0.02% relative to a preset basic length in the transport direction of the third laminate 27, and a shrinkage rate in the orthogonal direction of 0.02% relative to a preset basic length in the orthogonal direction.

[0114] Further, the deviation between the reference position preset for the design pattern of the picture-printed layer 3 and the reference position preset for the concave-convex pattern 5a was 0 mm in both the conveying direction and the perpendicular direction. Furthermore, the deviation between the reference position preset for the pattern of the picture-printed layer 3 and the reference position preset for the gloss-adjusting layer 7 was 0 mm in both the conveying direction and the perpendicular direction. Colored thermoplastic resin layer Material: Plant-derived polyethylene Thickness: 55μm Transparent thermoplastic resin layer Material: Plant-derived polyethylene Thickness: 70μm

[0115] Example 2 The transparent thermoplastic resin layer 5 was formed by the same procedure as in Example 1, except that petroleum-derived polyethylene was used instead of plant-derived polyethylene. Example 3 The colored thermoplastic resin layer 2 was produced in the same manner as in Example 1, except that petroleum-derived polyethylene was used instead of plant-derived polyethylene. Example 4 In Example 1, when forming the uneven pattern 5a, the elongation rate in the transport direction of the laminate 18a for forming the uneven pattern with respect to a preset basic length in the transport direction was 3.0%, and the contraction rate in the perpendicular direction with respect to a preset basic length in the perpendicular direction was 0.9%. The deviation between the reference position preset for the design pattern of the picture-printed layer 3 and the reference position preset for the concave-convex pattern 5a was 10 mm in the conveying direction and 3 mm in the perpendicular direction. Other than this, the same procedure as in Example 1 was used for preparation.

[0116] Example 5 In Example 1, when forming the gloss adjusting layer 7, the elongation rate in the transport direction of the third laminate 27 relative to the preset basic length in the transport direction was 3.0%, and the shrinkage rate in the perpendicular direction relative to the preset basic length in the perpendicular direction was 0.9%. The deviation between the reference position preset for the pattern of the picture-printed layer 3 and the reference position preset for the gloss-adjusting layer 7 was 6 mm in the conveying direction and 1.5 mm in the perpendicular direction. Other than this, the same procedure as in Example 1 was used for preparation.

[0117] Example 6 In Example 1, when forming the uneven pattern 5a, the elongation rate in the transport direction of the laminate 18a for forming the uneven pattern with respect to a preset basic length in the transport direction was 3.0%, and the contraction rate in the perpendicular direction with respect to a preset basic length in the perpendicular direction was 0.9%. The deviation between the reference position preset for the design pattern of the picture-printed layer 3 and the reference position preset for the concave-convex pattern 5a was 10 mm in the transport direction and 3 mm in the perpendicular direction. In addition, no gloss adjusting layer 7 was provided. Other than this, the same procedure as in Example 1 was followed to produce the film.

[0118] Example 7 In Example 1, when forming the gloss adjusting layer 7, the elongation rate in the transport direction of the third laminate 27 relative to the preset basic length in the transport direction was 3.0%, and the shrinkage rate in the perpendicular direction relative to the preset basic length in the perpendicular direction was 0.9%. The deviation between the reference position preset for the pattern of the picture-printed layer 3 and the reference position preset for the gloss-adjusting layer 7 was 6 mm in the conveying direction and 1.5 mm in the perpendicular direction. In addition, the uneven pattern 5a was not provided. Other than this, the same procedure as in Example 1 was followed to produce the film.

[0119] Comparative Example 1 The same procedure was followed as in Example 1, except that both the colored thermoplastic resin layer 2 and the transparent thermoplastic resin layer 5 were formed using petroleum-derived polyethylene instead of plant-derived polyethylene. Comparative Example 2 The same procedure as in Example 1 was followed, except that the thickness of the transparent thermoplastic resin layer 5 was changed to 200 μm. Comparative Example 3 The same procedure as in Example 1 was followed, except that the thickness of the transparent thermoplastic resin layer 5 was 50 μm.

[0120] Comparative Example 4 In Example 1, the deviation between the reference position preset for the pattern of the picture-printed layer 3 and the reference position preset for the gloss-adjusting layer 7 was 10 mm in the conveying direction and 0 mm in the perpendicular direction. Other than this, the same procedure as in Example 1 was used for preparation. Comparative Example 5 In Example 1, the deviation between the reference position preset for the pattern of the picture-printed layer 3 and the reference position preset for the gloss-adjusting layer 7 was 0 mm in the conveying direction and 6 mm in the perpendicular direction. Other than this, the same procedure as in Example 1 was used for preparation. Comparative Example 6 In Example 1, the deviation between the reference position preset for the design pattern of the picture-printed layer 3 and the reference position preset for the concave-convex pattern 5a was 15 mm in the transport direction and 0 mm in the perpendicular direction. Other than this, the same procedure as in Example 1 was used for production.

[0121] Comparative Example 7 In Example 1, the deviation between the reference position preset for the design pattern of the picture-printed layer 3 and the reference position preset for the concave-convex pattern 5a was 0 mm in the transport direction and 8 mm in the perpendicular direction. Other than this, the same procedure as in Example 1 was used for production. Comparative Example 8 In Example 1, when forming the uneven pattern 5a, the elongation rate of the uneven pattern forming laminate 18a in the transport direction relative to a preset basic length was 4.0%, and the contraction rate in the perpendicular direction relative to the preset basic length was 1.5%. The deviation between the reference position preset for the design pattern of the picture-printed layer 3 and the reference position preset for the concave-convex pattern 5a was 20 mm in the transport direction and 5 mm in the perpendicular direction. Other than this, the same procedure as in Example 1 was used to prepare the product.

[0122] Comparative Example 9 In Example 1, when forming the gloss adjusting layer 7, the elongation rate in the transport direction of the third laminate 27 relative to a preset basic length in the transport direction was 4.5%, and the shrinkage rate in the orthogonal direction relative to a preset basic length in the orthogonal direction was 2.5%. The deviation between the reference position preset for the pattern of the picture-printed layer 3 and the reference position preset for the gloss-adjusting layer 7 was 18 mm in the conveying direction and 5 mm in the perpendicular direction. Other than this, the same procedure as in Example 1 was used for preparation.

[0123] <Evaluation method and criteria> Performance evaluation was carried out for each of the decorative sheets produced as described above in Examples 1 to 7 and Comparative Examples 1 to 9. The evaluation method and evaluation criteria were as follows. (Productivity of transparent thermoplastic resin layer) The transparent thermoplastic resin layer 5 of the produced decorative sheet was visually inspected for the presence or absence of fish eyes and unevenness in thickness, and the degree of defects such as film formability, including the surface condition. "◎": Same as current product, with almost no defects. "○": Inferior to current product, but no effect on production. "△": Defects exist, but production is not affected. "X": Defects severe enough to affect production. (Printability) The decorative sheets produced were visually inspected for the occurrence of heat wrinkles when the ink was drying. If the occurrence of heat wrinkles was judged to affect productivity, for example, it was judged that the winding / unwinding tension needed to be adjusted. "◎": The printing suitability is comparable to that of the current product. "○": Inferior to current product, but no effect on production. "△": There is a printing defect, but it does not affect production. "X": There is a printing defect that affects production. (Pencil hardness test) The pencil hardness of the prepared decorative sheets was measured in accordance with JIS K5600. "◎": Equivalent to the current product. "○": Inferior to current product, but no effect on production. "△": Inferior to the current product and below the quality standard. "X": Hardness that affects production. (Processing suitability) The prepared decorative sheets were visually inspected for the presence or absence of whitening or cracks when folded. "◎": Equivalent to the current product. "○": Inferior to current product, but no effect on production. "△": Significant whitening is present. "X": Significant cracks are present. (pattern matching) The degree of matching between the picture print layer and the gloss control layer 7 or the uneven pattern 5a was judged by visual inspection. "Excellent": The gloss adjusting layer 7 and the uneven pattern 5a completely match the pattern of the picture printed layer. "◯": The gloss adjusting layer 7 and the uneven pattern 5a do not completely match the pattern of the picture printed layer, but there is no sense of incongruity. "△": Misalignment between the gloss adjusting layer 7 and the uneven pattern 5a and the pattern of the picture printed layer can be visually confirmed. "X": A deviation has occurred that affects production. (Evaluation Results) The evaluation results for each decorative sheet are as shown in Table 1 below.

[0124] [Table 1]

[0125] The decorative sheets of Examples 1 to 7 were good in all evaluation items, and although in Examples 2 and 3, only one of the colored thermoplastic resin layer 2 and the transparent thermoplastic resin layer 5 was formed from a biomass material, it was confirmed that the decorative sheets of Examples 2 and 3 exhibited performance equivalent to that of the decorative sheet of Example 1, in which both the colored thermoplastic resin layer 2 and the transparent thermoplastic resin layer 5 were formed from a biomass material. It was also confirmed that the decorative sheets of Examples 1 to 3 exhibited performance equivalent to that of the decorative sheet of Comparative Example 1, which is a current product in which both the colored thermoplastic resin layer 2 and the transparent thermoplastic resin layer 5 were formed from petroleum-derived polyethylene. In addition, even if the stretch rate of the laminate 18a for forming a concave-convex pattern during the formation of the concave-convex pattern was 3.0% in the transport direction and 0.9% in the orthogonal direction, the deviation between the reference position of the pattern pattern of the picture-printed layer 3 and the reference position of the concave-convex pattern was 10 mm in the transport direction and 3 mm in the orthogonal direction, and it was confirmed that the pattern pattern of the picture-printed layer 3 and the concave-convex pattern were in sync (Example 4). Similarly, when forming the gloss-adjusting layer 7, even if the elongation rate of the third laminate 27 in the transport direction is 3.0% and the shrinkage rate in the orthogonal direction is 0.9%, the deviation between the reference position of the pattern of the picture-printed layer 3 and the reference position of the gloss-adjusting layer 7 is 6 mm in the transport direction and 1.5 mm in the orthogonal direction, and it was confirmed that the pattern of the picture-printed layer 3 and the gloss-adjusting layer 7 are synchronized (Example 5).

[0126] Furthermore, even when only a rugged pattern is provided without a gloss adjusting layer 7 (Example 6), or conversely, when only a gloss adjusting layer 7 is provided without a rugged pattern (Example 7), it was confirmed that the pattern of the picture printed layer 3 can be synchronized with the rugged pattern 5a or the gloss adjusting layer 7 by using a laminate having stretching and shearing characteristics for synchronizing with the rugged pattern or stretching and shearing characteristics for synchronizing with the gloss adjusting layer.

[0127] On the other hand, in Example 1, when the thickness of the transparent thermoplastic resin layer 5 is 200 μm (Comparative Example 2), the transparent thermoplastic resin layer 5 is too thick, so the productivity of the transparent thermoplastic resin layer 5 decreases and bending workability decreases. Conversely, when the thickness of the transparent thermoplastic resin layer 5 is 50 μm (Comparative Example 3), it is too thin, so the productivity decreases and the surface strength is small. In addition, because the transparent thermoplastic resin layer 5 is too thin, it picks up the unevenness of the substrate 9, making it impossible to maintain the smoothness of the surface of the decorative sheet 1.

[0128] In addition, when there is a shift in the transport direction between the reference position of the pattern of the pattern-printed layer and the reference position of the gloss-adjusting layer 7 (Comparative Example 4), when there is a shift in the perpendicular direction (Comparative Example 5), when there is a shift in the transport direction between the reference position of the pattern of the pattern-printed layer and the reference position of the uneven pattern (Comparative Example 6), and when there is a shift in the perpendicular direction (Comparative Example 7), the shift is large in all cases, and the degree of synchronization is low. Furthermore, when the stretch rate in the transport direction of the uneven pattern-forming laminate 18a during the uneven pattern formation is 4.0% and the shrink rate in the perpendicular direction is 1.5% (Comparative Example 8), and when the stretch rate in the transport direction of the third laminate 27 during the gloss-adjusting layer 7 is 4.5% and the shrink rate in the perpendicular direction is 2.5%, it was confirmed that the shift between the pattern of the pattern-printed layer and the uneven pattern or gloss-adjusting layer 7 becomes large and the degree of synchronization is low.

[0129] The present invention can have the following configurations, for example. (1) A colored thermoplastic resin layer, a picture print layer, a transparent thermoplastic resin layer, and a surface protective layer are laminated in this order, Further, a gloss adjusting layer is provided on the surface of the surface protective layer opposite to the transparent thermoplastic resin layer, and the gloss adjusting layer is in harmony with the pattern of the picture print layer, A decorative sheet, characterized in that at least one of the colored thermoplastic resin layer and the transparent thermoplastic resin layer is formed using a biomass-derived resin composition. (2) A gloss-adjusting layer-forming laminate having the colored thermoplastic resin layer, the pattern printed layer, the transparent thermoplastic resin layer, and the surface protective layer laminated in this order, The decorative sheet described in (1) above, characterized in that when the gloss adjustment layer is formed on the surface of the gloss adjustment layer forming laminate on the surface protection layer side of the gloss adjustment layer forming laminate while the gloss adjustment layer forming laminate is transported, the gloss adjustment layer forming laminate has an elasticity property such that when the gloss adjustment layer forming laminate stretches in the transport direction of the gloss adjustment layer forming laminate within a range of 0.02% to 3.0% of a preset basic length in the transport direction, the gloss adjustment layer forming laminate shrinks in the perpendicular direction perpendicular to the transport direction within a range of 0.02% to 0.9% of a preset basic length in the perpendicular direction. (3) a gloss-adjusting layer-forming laminate in which the colored thermoplastic resin layer, the picture-printed layer, the transparent thermoplastic resin layer, and the surface protective layer are laminated in this order; The decorative sheet described in (2) above, characterized in that after the gloss adjustment layer is formed on the surface of the gloss adjustment layer forming laminate on the surface protection layer side while the gloss adjustment layer forming laminate is being transported, the gloss adjustment layer forming laminate has a shift characteristic in which the amount of shift in the transport direction of the gloss adjustment layer forming laminate between a reference position previously set on the picture printed layer and a reference position previously set on the gloss adjustment layer as a position that overlaps with the reference position in a planar view is 6 mm or less, and the amount of shift in a perpendicular direction perpendicular to the transport direction is 1.5 mm or less. (4) A decorative sheet according to any one of (1) to (3) above, characterized in that it is provided on the surface protective layer side and has a concave-convex pattern that is in harmony with the pattern pattern of the picture printed layer. (5) At least a colored thermoplastic resin layer, a picture print layer, and a transparent thermoplastic resin layer are laminated in this order, Further, a concave-convex pattern is provided on the transparent thermoplastic resin layer side and is in harmony with the pattern pattern of the picture print layer, A decorative sheet, characterized in that at least one of the colored thermoplastic resin layer and the transparent thermoplastic resin layer is formed using a biomass-derived resin composition. (6) A laminate for forming a concave-convex pattern, which is obtained by laminating the colored thermoplastic resin layer, the picture printed layer, and the transparent thermoplastic resin layer in this order, The decorative sheet according to (4) or (5) above, characterized in that when the uneven pattern is formed on the surface of the transparent thermoplastic resin layer side of the uneven pattern forming laminate while the uneven pattern forming laminate is being transported, the uneven pattern forming laminate has an elasticity property such that when the uneven pattern forming laminate stretches in the transport direction of the uneven pattern forming laminate within a range of 0.02% to 3.0% of a preset basic length in the transport direction, the uneven pattern forming laminate shrinks in the orthogonal direction perpendicular to the transport direction within a range of 0.02% to 0.9% of a preset basic length in the orthogonal direction perpendicular to the transport direction. (7) A laminate for forming a concave-convex pattern, which is obtained by laminating the colored thermoplastic resin layer, the picture printed layer, and the transparent thermoplastic resin layer in this order, The decorative sheet described in (6) above, characterized in that after the uneven pattern is formed on the surface of the transparent thermoplastic resin layer side of the uneven pattern forming laminate while the uneven pattern forming laminate is being transported, the uneven pattern forming laminate has a shift characteristic in which the amount of shift in the transport direction of the uneven pattern forming laminate between a reference position previously set on the picture printed layer and a reference position previously set on the uneven pattern as a position that overlaps with the reference position in a planar view is 10 mm or less, and the amount of shift in a perpendicular direction perpendicular to the transport direction is 3 mm or less. (8) the uneven pattern is formed on the surface of the transparent thermoplastic resin layer opposite to the picture print layer, and a surface protective layer is formed on the surface of the transparent thermoplastic resin layer; The decorative sheet according to any one of (4) to (7) above, wherein the resin forming the surface protective layer penetrates into the projections and recesses of the projection and recess pattern. (9) The decorative sheet according to any one of (1) to (8) above, characterized in that the colored thermoplastic resin layer and the transparent thermoplastic resin layer contain a biomass-derived polyolefin formed by polymerizing a monomer containing a biomass-derived olefin as a main material of the resin composition. (10) A decorative sheet according to any one of (1) to (9) above, characterized in that the transparent thermoplastic resin layer is laminated by extrusion lamination to a laminate of the colored thermoplastic resin layer and the picture printed layer. (11) The decorative sheet according to any one of (1) to (10) above, wherein the design is a wood grain pattern. (12) A substrate; A decorative material comprising: a decorative sheet according to any one of (1) to (11) above, attached to at least one surface of the substrate. [Explanation of symbols]

[0130] 1 Decorative sheet 2 Colored thermoplastic resin layer 3. Pattern printing layer 4 Adhesive layer 5 Transparent thermoplastic resin layer 6 Surface protective layer 7. Gloss Adjustment Layer 8 Primer layer 9 Base material 101 Transparent thermoplastic resin layer forming device 102 Gloss adjustment layer forming device

Claims

1. A colored thermoplastic resin layer, a picture print layer, a transparent thermoplastic resin layer, and a surface protective layer are laminated in this order, Further, a gloss adjusting layer is provided on the surface of the surface protective layer opposite to the transparent thermoplastic resin layer, and the gloss adjusting layer is in harmony with the pattern of the picture print layer, A decorative sheet, characterized in that at least one of the colored thermoplastic resin layer and the transparent thermoplastic resin layer is formed using a biomass-derived resin composition.

2. The decorative sheet according to claim 1, characterized in that the gloss adjustment layer forming laminate, which is formed by laminating the colored thermoplastic resin layer, the pattern printed layer, the transparent thermoplastic resin layer, and the surface protective layer in this order, has an elasticity characteristic in which, when the gloss adjustment layer is formed on the surface of the gloss adjustment layer forming laminate while being transported, the gloss adjustment layer forming laminate stretches in the transport direction within a range of 0.02% to 3.0% of a predetermined basic length in the transport direction of the gloss adjustment layer forming laminate, and shrinks in the perpendicular direction within a range of 0.02% to 0.9% of a predetermined basic length in the perpendicular direction perpendicular to the transport direction.

3. The decorative sheet described in claim 2, characterized in that the gloss adjustment layer forming laminate, which is formed by laminating the colored thermoplastic resin layer, the pattern printed layer, the transparent thermoplastic resin layer, and the surface protective layer in this order, has a displacement characteristic in which, after the gloss adjustment layer is formed on the surface of the gloss adjustment layer forming laminate while being transported, the gloss adjustment layer forming laminate has a displacement characteristic in which the displacement amount in the transport direction of the gloss adjustment layer forming laminate between a reference position preset on the pattern printed layer and a reference position preset on the gloss adjustment layer as a position that overlaps with the reference position in a planar view is 6 mm or less, and the displacement amount in the perpendicular direction perpendicular to the transport direction is 1.5 mm or less.

4. 3. The decorative sheet according to claim 1, further comprising a concave-convex pattern provided on said surface protective layer side and in harmony with the pattern of said picture print layer.

5. At least a colored thermoplastic resin layer, a picture print layer, and a transparent thermoplastic resin layer are laminated in this order, Further, a concave-convex pattern is provided on the transparent thermoplastic resin layer side and is in harmony with the pattern pattern of the picture print layer, A decorative sheet, characterized in that at least one of the colored thermoplastic resin layer and the transparent thermoplastic resin layer is formed using a biomass-derived resin composition.

6. The decorative sheet according to claim 5, characterized in that the laminate for forming a concave-convex pattern, which is formed by laminating the colored thermoplastic resin layer, the picture printed layer, and the transparent thermoplastic resin layer in this order, has an elasticity characteristic in which, when the laminate for forming a concave-convex pattern is transported and the concave-convex pattern is formed on the surface of the transparent thermoplastic resin layer side of the laminate for forming a concave-convex pattern, the laminate for forming a concave-convex pattern stretches in the transport direction of the laminate for forming a concave-convex pattern within a range of 0.02% to 3.0% of a predetermined basic length in the transport direction, and shrinks in the perpendicular direction perpendicular to the transport direction within a range of 0.02% to 0.9% of a predetermined basic length in the perpendicular direction perpendicular to the transport direction.

7. The decorative sheet according to claim 6, characterized in that the laminate for forming a concave-convex pattern, which is formed by laminating the colored thermoplastic resin layer, the picture printed layer, and the transparent thermoplastic resin layer in this order, has a shift characteristic in which, after the concave-convex pattern is formed on the surface of the laminate for forming a concave-convex pattern on the transparent thermoplastic resin layer side while the laminate for forming a concave-convex pattern is transported, the laminate for forming a concave-convex pattern has a shift characteristic in which the amount of shift in the transport direction of the laminate for forming a concave-convex pattern between a reference position preset on the picture printed layer and a reference position preset on the concave-convex pattern as a position that overlaps with the reference position in a planar view is 10 mm or less, and the amount of shift in an orthogonal direction perpendicular to the transport direction is 3 mm or less.

8. the uneven pattern is formed on the surface of the transparent thermoplastic resin layer opposite to the picture print layer, and a surface protective layer is formed on the surface of the transparent thermoplastic resin layer; 8. The decorative sheet according to claim 5, wherein the resin forming the surface protective layer penetrates into the projections and recesses of the projection and recess pattern.

9. The decorative sheet according to claim 1 or claim 5, characterized in that the colored thermoplastic resin layer and the transparent thermoplastic resin layer contain a biomass-derived polyolefin formed by polymerizing a monomer containing a biomass-derived olefin as a main material of the resin composition.

10. 6. The decorative sheet according to claim 1, wherein the transparent thermoplastic resin layer is laminated by extrusion lamination onto a laminate of the colored thermoplastic resin layer and the picture printed layer.

11. 6. The decorative sheet according to claim 1, wherein the design is a wood grain design.

12. A substrate; A decorative material comprising: the decorative sheet according to claim 1 or 5 attached to at least one surface of the substrate.

Citation Information

Patent Citations

  • Decorative sheet and decorative material

    JP2014188941A