Method for manufacturing thermally conductive silicone resin sheet
A thermosetting silicone resin composition with specific components and a pulsed magnetic field orientation process addresses the need for higher thermal conductivity and productivity in electronic device heat dissipation, producing a sheet with enhanced thermal conductivity.
Patent Information
- Application Number
- JP2023065560
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-13
- Publication Date
- 2024-10-25
AI Technical Summary
Existing thermally conductive resin compositions do not meet the increasing thermal conductivity demands of smaller and more sophisticated electronic devices, and there is a need for higher productivity in orienting thermally conductive fillers.
A method involving a thermosetting silicone resin composition containing specific components (A1-A3) and a diamagnetic inorganic filler, oriented using a pulsed magnetic field followed by heating, to produce a thermally conductive silicone resin sheet with enhanced thermal conductivity.
The method results in a thermally conductive silicone resin sheet with excellent thermal conductivity in the thickness direction, suitable for heat dissipation from electronic components, and achieves high productivity through efficient filler orientation.
Smart Images

Figure 2024151828000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a thermally conductive silicone resin sheet. [Background technology]
[0002] In electronic devices such as computers and automobile parts, heat sinks and other heat dissipators are used to dissipate heat generated by heat-generating bodies such as semiconductor elements and machine parts. In order to increase the efficiency of heat transfer to the heat dissipating body, a thermally conductive sheet is sometimes placed between the heat generating body and the heat dissipating body.
[0003] As such a thermally conductive sheet, Patent Document 1 discloses a thermally conductive sheet in which carbon fibers are filled and oriented as a thermally conductive material. Patent Document 2 discloses a thermally conductive sheet in which carbon powder is oriented in the thickness direction of the sheet. Patent Document 3 discloses a thermally conductive sheet in which thermally conductive fillers are oriented in the thickness direction and have flexibility. Patent Document 4 discloses a thermally conductive sheet that is multi-layered with a flexible layer and a thermally conductive layer to reduce contact thermal resistance. In addition, a low-hardness, high-thermal-conductivity sheet is disclosed, although it is pressure-oriented. In addition, as an inexpensive high-magnetic-field generating device, there is a magnetic field generating device that accumulates electric charge in an electric double-layer capacitor as disclosed in Patent Document 5, and supplies a discharge current to an electromagnet to generate a magnetic field.
[0004] In recent years, electronic devices have become smaller and more sophisticated, and the amount of heat generated by them is constantly increasing. This has led to a demand for thermally conductive resin compositions with higher thermal conductivity than conventional thermally conductive resin compositions. In addition, in order to improve productivity, there is a demand for the orientation of thermally conductive fillers to be performed in a short period of time. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2005-146057 A [Patent Document 2] JP 2014-001388 A [Patent Document 3] JP 2019-186555 A [Patent Document 4] International Publication No. WO2021 / 166370 [Patent Document 5] Patent Publication No. 2022-881 Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention has been made to solve the above-mentioned problems, and has an object to provide a method for producing a thermally conductive silicone resin sheet that has excellent thermal conductivity in the thickness direction and in which a thermally conductive filler is highly oriented. [Means for solving the problem]
[0007] In order to solve the above problems, the present invention provides (A) a thermosetting silicone resin containing the following components (A1) to (A3): 100 parts by mass (A1) an organopolysiloxane having two or more alkenyl groups bonded to silicon atoms in each molecule; (A2) an organohydrogenpolysiloxane having two or more hydrosilyl groups per molecule: an amount such that the molar ratio of hydrosilyl groups in the component (A2) to alkenyl groups bonded to silicon atoms in the component (A1) is 0.5 to 2; and (A3) Platinum group metal hydrosilylation catalyst: 0.1 to 2,000 ppm by mass of platinum group metal element relative to the component (A) and, (B) a thermally conductive inorganic filler that is a diamagnetic material having an aspect ratio of the major axis to the minor axis of 5 or more, a major axis of 30 μm or more and 300 μm or less, and a specific gravity of 2.0 or more and less than 3.5: 30 to 150 parts by mass; A method for producing a thermally conductive silicone resin sheet, which is a cured product of the thermally conductive thermosetting silicone resin composition, by curing a thermally conductive thermosetting silicone resin composition containing The present invention provides a method for producing a thermally conductive silicone resin sheet, which comprises applying a pulse magnetic field of 30 T or more to the thermally conductive thermosetting silicone resin composition for 0.5 to 60 seconds, and then heating the thermally conductive thermosetting silicone resin composition at 90 to 150°C for 1 to 2 hours to cure the composition.
[0008] According to such a method for producing a thermally conductive silicone resin sheet, a thermally conductive silicone resin sheet having excellent thermal conductivity in the thickness direction can be produced with good productivity.
[0009] In this case, it is particularly preferable that the component (A1) is an organopolysiloxane represented by the following average composition formula (1). R 1 m R 2 n SiO (4-m-n) / 2 (1) (In the formula, R 1 are independently selected from an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, and an aralkyl group having 7 to 10 carbon atoms; R 2 are independently an alkenyl group having 2 to 6 carbon atoms. m is a positive number of 0.5 to 2.5, and n is a positive number of 0.0001 to 0.2, with the proviso that m+n is a positive number of 0.8 to 2.7.
[0010] The component (A2) is preferably an organohydrogenpolysiloxane represented by the following average composition formula (2). R 3 p1 H q1 SiO (4-p1-q1) / 2 (2) (In the formula, R 3 are independently a group selected from an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, and an aralkyl group having 7 to 10 carbon atoms. p1 is a positive number of 1.0 to 3.0, and q1 is a positive number of 0.05 to 2.0, with the proviso that p1+q1 is a positive number of 0.5 to 3.0.
[0011] The component (B) is preferably one or more diamagnetic materials selected from carbon fiber, graphite, graphene, carbon nanotubes, silicon carbide, and boron nitride.
[0012] By using each of these components, the thermally conductive silicone resin sheet produced in the present invention can be made to have superior thermal conductivity in the thickness direction. Effect of the Invention
[0013] According to the present invention, a method for producing a thermally conductive silicone resin sheet having excellent thermal conductivity in the thickness direction can be provided. In addition, the method for producing the thermally conductive silicone resin sheet has good productivity. The thermally conductive silicone resin sheet is suitable for removing heat from electric and electronic components that generate heat during use. [Brief description of the drawings]
[0014] [Figure 1] FIG. 2 is a diagram showing an example of a profile of a pulsed magnetic field applied to a thermally conductive thermosetting silicone resin composition in the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] As a result of extensive research in order to achieve the above object, the present inventors have found that (A) a thermosetting silicone resin containing the following components (A1) to (A3): 100 parts by mass (A1) an organopolysiloxane having two or more alkenyl groups bonded to silicon atoms in each molecule; (A2) an organohydrogenpolysiloxane having two or more hydrosilyl groups per molecule: an amount such that the molar ratio of hydrosilyl groups in the component (A2) to alkenyl groups bonded to silicon atoms in the component (A1) is 0.5 to 2; and (A3) Platinum group metal hydrosilylation catalyst: 0.1 to 2,000 ppm by mass of platinum group metal element relative to the component (A) and, (B) a thermally conductive inorganic filler that is a diamagnetic material having an aspect ratio of the major axis to the minor axis of 5 or more, a major axis of 30 μm or more and 300 μm or less, and a specific gravity of 2.0 or more and less than 3.5: 30 to 150 parts by mass; A method for producing a thermally conductive silicone resin sheet, which is a cured product of the thermally conductive thermosetting silicone resin composition, by curing a thermally conductive thermosetting silicone resin composition containing It has been found that a method for producing a thermally conductive silicone resin sheet having excellent thermal conductivity in the thickness direction can be achieved by subjecting the thermally conductive thermosetting silicone resin composition to a step of applying a pulse magnetic field of 30 T or more for 0.5 to 60 seconds, and then curing the thermally conductive thermosetting silicone resin composition by heating at 90 to 150°C for 1 to 2 hours.
[0016] The present invention will be described in detail below. [(A) Thermosetting silicone resin] The thermosetting silicone resin which is the component (A) of the present invention contains the following components (A1) to (A3). (A1) an organopolysiloxane having two or more alkenyl groups bonded to silicon atoms in each molecule; (A2) an organohydrogenpolysiloxane having two or more hydrosilyl groups per molecule: an amount such that the molar ratio of hydrosilyl groups in component (A2) to alkenyl groups bonded to silicon atoms in component (A1) is 0.5 to 2; and (A3) Platinum group metal hydrosilylation catalyst: 0.1 to 2,000 ppm by mass of platinum group metal element relative to the component (A) Each component will be described in detail below.
[0017] [Component (A1)] The alkenyl-containing organopolysiloxane, which is the component (A1), has two or more alkenyl groups bonded to silicon atoms in one molecule. The number of alkenyl groups bonded to silicon atoms in one molecule is preferably 2 to 20, more preferably about 2 to 10. These (A1) components can be used alone or in appropriate combination of two or more. The (A1) component can be a polymer made of a single siloxane unit or a copolymer made of two or more kinds of siloxane units. Furthermore, the position of the alkenyl group bonded to the silicon atom in the (A1) component is not particularly limited, and the alkenyl group can be bonded to either the silicon atom at the molecular chain terminal or the silicon atom at a non-terminal of the molecular chain (in the middle of the molecular chain), or can be bonded to both.
[0018] The molecular structure of component (A1) is not particularly limited, and examples thereof include a linear structure, a partially branched linear structure, a branched structure, a cyclic structure, and a branched cyclic structure. Of these, a substantially linear organopolysiloxane is usually preferred, and specifically, a linear diorganopolysiloxane whose molecular chain is mainly composed of repeating diorganosiloxane units and whose molecular chain is terminated at both ends with triorganosiloxy groups is preferred.
[0019] The viscosity of the (A1) component at 25°C is preferably 1 to 20,000 mPa·s, more preferably 10 to 1,000 mPa·s. The alkenyl-containing organopolysiloxane of the (A1) component preferably has 3 to 700 silicon atoms (or degree of polymerization) per molecule, more preferably about 4 to 300. If the viscosity is 1 mPa·s or more, the sedimentation of the thermally conductive inorganic filler, which is the (B) component in the resulting silicone resin composition, can be suppressed, and long-term storage stability can be maintained in a good condition. If the viscosity is 20,000 mPa·s or less, the thermally conductive inorganic filler, which is the diamagnetic material, which is the (B) component in the resulting silicone resin composition, can be easily oriented in a magnetic field, making it easier to increase the thermal conductivity and to improve the thermal conductivity. The viscosity in the present invention is a value measured by a rotational viscometer described in JIS K 7117-1:1999.
[0020] As the component (A1), in particular, a compound represented by the following average composition formula (1) R 1 m R 2 n SiO (4-m-n) / 2 (1) (In the formula, R 1 are independently selected from an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, and an aralkyl group having 7 to 10 carbon atoms; R 2 are independently an alkenyl group having 2 to 6 carbon atoms. m is a positive number of 0.5 to 2.5, and n is a positive number of 0.0001 to 0.2, with the proviso that m+n is a positive number of 0.8 to 2.7. and having two or more alkenyl groups bonded to silicon atoms in one molecule.
[0021] Above R 1 Specific examples of the alkyl group include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, hexyl, octyl, and decyl; aryl groups such as phenyl, tolyl, xylyl, and naphthyl; cycloalkyl groups such as cyclopentyl and cyclohexyl; aralkyl groups such as benzyl, 2-phenylethyl, and 3-phenylpropyl; and groups in which some of the hydrogen atoms bonded to carbon atoms in these hydrocarbon groups have been substituted with halogen atoms such as chlorine atoms and bromine atoms, for example, chloromethyl, 2-bromoethyl, and 3,3,3-trifluoropropyl.
[0022] Among these, a methyl group, a phenyl group, or a combination of these is preferred. 1 In the case of component (A1) in which R is a methyl group, a phenyl group, or a combination of these two, synthesis is easy and the chemical stability is good. Furthermore, when an organopolysiloxane with particularly good solvent resistance is used as component (A1), R 1 More preferably, is a combination of a 3,3,3-trifluoropropyl group with a methyl group, a phenyl group, or a combination of both.
[0023] Above R 2 Specific examples of R include vinyl, allyl, isopropenyl, 1-butenyl, isobutenyl, and hexenyl groups. Among these, vinyl is preferred. 2 The component (A1) in which is a vinyl group is easy to synthesize and has good chemical stability.
[0024] Specific examples of component (A1) include dimethylsiloxane-methylvinylsiloxane copolymers capped at both molecular chain terminals with trimethylsiloxy groups, methylvinylpolysiloxanes capped at both molecular chain terminals with trimethylsiloxy groups, dimethylsiloxane-methylvinylsiloxane-methylphenylsiloxane copolymers capped at both molecular chain terminals with trimethylsiloxy groups, dimethylsiloxane-methylvinylsiloxane-diphenylsiloxane copolymers capped at both molecular chain terminals with trimethylsiloxy groups, dimethylpolysiloxanes capped at both molecular chain terminals with dimethylvinylsiloxy groups, and dimethylvinylsiloxanes capped at both molecular chain terminals with dimethylvinylsiloxy groups. Examples of the organopolysiloxane include methylvinylpolysiloxane capped with dimethylvinylsiloxy groups at both molecular chain terminals, dimethylsiloxane-methylvinylsiloxane copolymer capped with dimethylvinylsiloxy groups at both molecular chain terminals, dimethylsiloxane-methylvinylsiloxane-methylphenylsiloxane copolymer capped with dimethylvinylsiloxy groups at both molecular chain terminals, dimethylsiloxane-methylvinylsiloxane-diphenylsiloxane copolymer capped with dimethylvinylsiloxy groups at both molecular chain terminals, dimethylpolysiloxane capped with divinylmethylsiloxy groups at both molecular chain terminals, and dimethylpolysiloxane capped with trivinylsiloxy groups at both molecular chain terminals. These organopolysiloxanes may be used alone or in combination of two or more, or one or more types with different degrees of polymerization may be used in combination.
[0025] [(A2) component] The (A2) component is characterized by being an organohydrogenpolysiloxane having two or more hydrosilyl groups in one molecule. The (A2) component may be used alone or in combination of two or more. The (A2) component is a curing agent in a silicone resin composition, and preferably has three or more hydrosilyl groups in one molecule, more preferably four or more (usually about 4 to 300), and even more preferably five or more (usually about 5 to 200). The molecular structure of the (A2) component is not particularly limited, and may be, for example, any of straight-chain, branched, cyclic, or three-dimensional network structure resinous materials, but it is preferable to use one represented by the following average composition formula (2).
[0026] R 3 p1 H q1 SiO (4-p1-q1) / 2 (2) (In the formula, R 3 are independently a group selected from an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, and an aralkyl group having 7 to 10 carbon atoms. p1 is a positive number of 1.0 to 3.0, and q1 is a positive number of 0.05 to 2.0, with the proviso that p1+q1 is a positive number of 0.5 to 3.0.
[0027] R in Equation (2) 3 Examples of the alkyl group include unsubstituted or halogen-substituted monovalent hydrocarbon groups, typically having 1 to 10 carbon atoms, preferably about 1 to 8 carbon atoms, excluding aliphatic unsaturated bonds, such as alkyl groups, such as methyl, ethyl, propyl, butyl, pentyl, hexyl, isopropyl, isobutyl, tert-butyl, and cyclohexyl; aryl groups, such as phenyl, tolyl, and xylyl; aralkyl groups, such as benzyl and phenethyl; and halogenated alkyl groups, such as 3-chloropropyl and 3,3,3-trifluoropropyl. Methyl, ethyl, propyl, phenyl, and 3,3,3-trifluoropropyl groups are preferred, with methyl being more preferred.
[0028] Specific examples of the organohydrogenpolysiloxane of component (A2) include 1,1,3,3-tetramethyldisiloxane, 1,3,5,7-tetramethylcyclotetrasiloxane, methylhydrogencyclopolysiloxane, methylhydrogensiloxane-dimethylsiloxane cyclic copolymer, tris(dimethylhydrogensiloxy)methylsilane, tris(dimethylhydrogensiloxy)phenylsilane, dimethylsiloxane-methylhydrogensiloxane copolymer capped at both molecular chain ends with dimethylhydrogensiloxy groups, methylhydrogenpolysiloxane capped at both molecular chain ends with dimethylhydrogensiloxy groups, and copolymers thereof. Methylhydrogenpolysiloxane capped at both molecular chain ends with trimethylsiloxy groups, dimethylpolysiloxane capped at both molecular chain ends with dimethylhydrogensiloxy groups, dimethylsiloxane-diphenylsiloxane copolymer capped at both molecular chain ends with dimethylhydrogensiloxy groups, dimethylsiloxane-methylhydrogensiloxane copolymer capped at both molecular chain ends with trimethylsiloxy groups, dimethylsiloxane-diphenylsiloxane-methylhydrogensiloxane copolymer capped at both molecular chain ends with trimethylsiloxy groups, dimethylsiloxane-methylhydrogensiloxane copolymer capped at both molecular chain ends with dimethylhydrogensiloxy groups, H(CH3)2SiO 1 / 2 Copolymer of SiO2 units and H(CH3)2SiO 1 / 2 Units and (CH3)3SiO 1 / 2 Examples of the organohydrogenpolysiloxane include copolymers of SiO2 units and SiO2 units, and mixtures of two or more of these organohydrogenpolysiloxanes.
[0029] There are no particular limitations on the viscosity of component (A2) at 25°C, but it is preferably 0.5 to 1,000,000 mPa s, and more preferably 1 to 100,000 mPa s. Furthermore, the organohydrogenpolysiloxane of component (A2) preferably has 3 to 500 silicon atoms (or degree of polymerization) per molecule, and more preferably has about 4 to 300 silicon atoms.
[0030] The amount of component (A2) blended is an amount such that the molar ratio of hydrosilyl groups in component (A2) to alkenyl groups bonded to silicon atoms in component (A1) is 0.5 to 2. The above molar ratio is more preferably an amount of 0.7 to 1.8, and even more preferably an amount of 0.8 to 1.7.
[0031] [(A3) component] The thermosetting silicone resin of the present invention contains (A3) a platinum group metal-based hydrosilylation catalyst, which is an addition reaction catalyst for promoting the above reaction. Examples of the (A3) component include catalysts well known as catalysts used in hydrosilylation reactions. These can be used alone or in appropriate combination of two or more. Among them, a hydrosilylation catalyst in which a platinum complex such as chloroplatinic acid or chloroplatinate is diluted with an organopolysiloxane having a vinyl group such as an alkenyl group is preferred. This can be obtained by mixing a platinum complex with an organopolysiloxane having a vinyl group. If the platinum complex contains a solvent such as toluene, it is recommended to remove the solvent after mixing.
[0032] The platinum group metal hydrosilylation catalyst, component (A3), is present in an amount of 0.1 to 2,000 ppm, calculated as the platinum group metal element mass relative to component (A). This content is preferably 0.5 to 1,000 ppm. If the amount of platinum group metal hydrosilylation catalyst added is within this range, sufficient curability can be ensured and costs can be reduced.
[0033] [(B) Component] The component (B) is a thermally conductive inorganic filler selected from diamagnetic materials, with an aspect ratio of major axis to minor axis of 5 or more, preferably 30 to 300, a major axis of 30 μm or more and 300 μm or less, preferably 50 μm or more and 250 μm or less, and a specific gravity of 2.0 or more and less than 3.5, preferably 2.0 or more and 3.0 or less. The component (B) is a component for improving the thermal conductivity of the silicone composition. By using such a thermally conductive inorganic filler, the component (B) in the thermally conductive thermosetting silicone resin composition is easily oriented by application of a magnetic field, and the thermal conductivity in the thickness direction of the produced thermally conductive silicone resin sheet can be improved.
[0034] Among these, it is preferable that the component (B) is one or more diamagnetic materials selected from carbon fiber, graphite, graphene, carbon nanotubes, silicon carbide, and boron nitride.
[0035] The amount of component (B) is 30 to 150 parts by mass, and preferably 35 to 145 parts by mass, per 100 parts by mass of the thermosetting silicone resin (A). If the amount of component (B) is less than 30 parts by mass, the thermal conductivity will be poor, and if it is more than 150 parts by mass, the viscosity of the thermally conductive thermosetting silicone resin composition will be significantly high, which may make magnetic field orientation difficult.
[0036] In the present invention, a thermally conductive inorganic filler other than the component (B) may be blended. Examples include aluminum oxide powder, zinc oxide powder, magnesium oxide, aluminum nitride, boron nitride powder, aluminum, silver, nickel, silicon oxide, magnesium oxide, aluminum nitride, silicon nitride, silicon carbide, and metal silicon. These may be used alone or in appropriate combination of two or more. When a thermally conductive inorganic filler other than the component (B) is blended, the content of the filler in the thermally conductive thermosetting silicone resin composition is preferably 100 parts by mass or less per 100 parts by mass of the component (A1).
[0037] [Other ingredients] The heat conductive thermosetting silicone resin composition of the present invention may further contain a viscosity modifier consisting of a hydrolyzable organopolysiloxane as another component in order to reduce the viscosity before heat curing. One type may be used alone, or two or more types may be used in appropriate combination. The viscosity modifier maintains the fluidity of the heat conductive thermosetting silicone resin composition even when the silicone resin of the component (A) is highly filled with the heat conductive filler (B), and imparts good handleability to the composition. The viscosity modifier preferably contains an organopolysiloxane represented by the following general formula (3), in particular a trifunctional (g=0 in the following formula (4)) hydrolyzable organopolysiloxane. [ka] (In the formula, R 4 are independently selected from an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, and an aralkyl group having 7 to 10 carbon atoms. 4 Or a group represented by the following formula (4), at least one of which is a group represented by the following formula (4). [ka] (In the formula, Q is an oxygen atom or an alkylene group having 1 to 4 carbon atoms, and R 5 are independently selected from an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, and an aralkyl group having 7 to 10 carbon atoms; R 6 are independently a group selected from an alkyl group having 1 to 4 carbon atoms, an alkoxyalkyl group having 1 to 4 carbon atoms, or an acyl group having 1 to 4 carbon atoms, and g is an integer of 0 to 2. a is 1≦a≦100, and b is 0≦b≦100.
[0038] The viscosity modifier may be a compound represented by the following general formula (5): [ka] (In the formula, R 4 , R 6 g is the same as above, and c is an integer of 5 to 100. In particular, organopolysiloxanes having a viscosity at 25° C. of 0.005 to 100 mPa·s are preferred.
[0039] In the above formulas (3) and (5), R 4 are independently selected from an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, and an aralkyl group having 7 to 10 carbon atoms, and examples thereof include a linear alkyl group, a branched alkyl group, a cyclic alkyl group, an aryl group, an aralkyl group, and a halogenated alkyl group. Examples of linear alkyl groups include a methyl group, an ethyl group, a propyl group, a hexyl group, and an octyl group. Examples of branched alkyl groups include an isopropyl group, an isobutyl group, a tert-butyl group, and a 2-ethylhexyl group. Examples of cyclic alkyl groups include a cyclopentyl group and a cyclohexyl group. Examples of aryl groups include a phenyl group and a tolyl group. Examples of aralkyl groups include a 2-phenylethyl group and a 2-methyl-2-phenylethyl group. Examples of halogenated alkyl groups include a 3,3,3-trifluoropropyl group, a 2-(nonafluorobutyl)ethyl group, and a 2-(heptadecafluorooctyl)ethyl group. 4 As the alkyl group, a methyl group and a phenyl group are preferable.
[0040] Above R 5 is a group selected from an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, and an aralkyl group having 7 to 10 carbon atoms; R 5 As a specific example of R 1 Examples of the above are given below.
[0041] Above R 6 are independently selected from an alkyl group having 1 to 4 carbon atoms, an alkoxyalkyl group having 1 to 4 carbon atoms, or an acyl group having 1 to 4 carbon atoms. Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, and a butyl group. Examples of the alkoxyalkyl group include a methoxyethyl group and a methoxypropyl group. Examples of the acyl group include an acetyl group. R6 is preferably an alkyl group, and particularly preferably a methyl group or an ethyl group.
[0042] a is 1≦a≦100, b is 0≦b≦100, and preferably a+b is 10 to 50. c is an integer of 5 to 100, and preferably 10 to 50. g is an integer of 0 to 2, and preferably 0. In addition, when OR 6 It is preferable that the group has 1 to 6 groups, and particularly 3 or 6 groups.
[0043] Specific examples of suitable viscosity modifiers include the following: [ka]
[0044] The amount of the viscosity modifier is preferably 50 to 300 parts by mass relative to 100 parts by mass of the (A1) component. The amount of the viscosity modifier is preferably 60 to 250 parts by mass. When the amount of the viscosity modifier is 50 parts by mass or more, the viscosity of the thermally conductive thermosetting silicone resin composition becomes more appropriate, and the dischargeability can be improved. On the other hand, when the amount of the viscosity modifier is 300 parts by mass or less, the viscosity becomes more appropriate, and the risk of bleeding of the viscosity modifier and the risk of settling when a thermally conductive inorganic filler other than the (B) component is blended can be suppressed.
[0045] The thermally conductive thermosetting silicone resin composition of the present invention may contain any components other than those mentioned above.
[0046] In addition to the above-mentioned thermally conductive inorganic fillers, other fillers may be used. These other fillers may be used alone or in combination of two or more. Examples of these other fillers include clays such as wollastonite, talc, aluminum oxide, calcium sulfate, magnesium carbonate, and kaolin; copper carbonates such as aluminum hydroxide, magnesium hydroxide, barite, and malachite; nickel carbonates such as zarakite; barium carbonates such as witherite; strontium carbonates such as strontianite; silicates such as forsterite, sillimanite, mullite, pyrophyllite, kaolinite, and vermiculite; non-reinforcing fillers such as diatomaceous earth; and fillers whose surfaces are treated with organic silicon compounds. When such other fillers are blended, the content of the fillers in the thermally conductive thermosetting silicone resin composition is preferably 5 parts by mass or less per 100 parts by mass of the (A1) component.
[0047] In order to improve the adhesiveness of the thermally conductive silicone resin sheet, which is the cured product of the thermally conductive thermosetting silicone resin composition of the present invention, an adhesion promoter may be blended in. The adhesion promoter may be used alone or in appropriate combination of two or more kinds.Specific examples of adhesion promoters include alkyl alkenyl dialkoxy silanes such as methyl vinyl dimethoxy silane, ethyl vinyl dimethoxy silane, methyl vinyl diethoxy silane, and ethyl vinyl diethoxy silane; alkyl alkenyl dioxime silanes such as methyl vinyl dioxime silane and ethyl vinyl dioxime silane; alkyl alkenyl diacetoxy silanes such as methyl vinyl diacetoxy silane and ethyl vinyl diacetoxy silane; alkenyl alkyl dihydroxy silanes such as methyl vinyl dihydroxy silane and ethyl vinyl dihydroxy silane; organo trialkoxy silanes such as methyl trimethoxy silane, vinyl trimethoxy silane, allyl trimethoxy silane, 3-methacryloxypropyl trimethoxy silane, 3-glycidoxypropyl trimethoxy silane, 3-aminopropyl trimethoxy silane, N-(2-aminoethyl)-3-aminopropyl trimethoxy silane, bis(trimethoxysilyl)propane, and bis(trimethoxysilyl)hexane; triallyl isocyanurate, diaryl isocyanurate compounds such as tris(3-trimethoxysilyl)isocyanurate, tris(3-trimethoxysilylpropyl)isocyanurate, tris(3-triethoxysilylpropyl)isocyanurate, and tris(3-tripoxysilylpropyl)isocyanurate; titanium compounds such as tetraethyl titanate, tetrapropyl titanate, tetrabutyl titanate, tetra(2-ethylhexyl)titanate, titanium ethylacetonate, and titanium acetylacetonate; aluminum compounds such as ethylacetoacetate aluminum diisopropylate, aluminum tris(ethylacetoacetate), alkylacetoacetate aluminum diisopropylate, aluminum tris(acetylacetonate), and aluminum monoacetylacetonate bis(ethylacetoacetate); and zirconium compounds such as zirconium acetylacetonate, zirconium butoxyacetylacetonate, zirconium bisacetylacetonate, and zirconium ethylacetoacetate.
[0048] When an adhesion promoter is added, the content of the adhesion promoter in the thermally conductive thermosetting silicone resin composition is not particularly limited, but is preferably 0.01 to 10 parts by mass per 100 parts by mass of component (A1).
[0049] [Manufacturing method] The method for producing a thermally conductive silicone resin sheet of the present invention is a method for producing a thermally conductive silicone resin sheet, which is a cured product, by curing a thermally conductive thermosetting silicone resin composition containing the above-mentioned component (A) (thermosetting silicone resin containing components (A1) to (A3)) and the above-mentioned component (B). In this case, the present invention is characterized in that a step of applying a pulse magnetic field of 30 T or more to the thermally conductive thermosetting silicone resin composition for 0.5 to 60 seconds is carried out, and then the thermally conductive thermosetting silicone resin composition is heated at 90 to 150°C for 1 to 2 hours to be cured.
[0050] A more specific example of the method for producing a thermally conductive silicone resin sheet includes the following steps (I) to (IV).
[0051] [Process (I)] The above components (A1) and (B) are mixed using a mixer such as a Trimix, Twinmix, or Planetary Mixer (all of which are registered trademarks of mixers manufactured by Inoue Seisakusho Co., Ltd.), an Ultramixer (registered trademark of mixers manufactured by Mizuho Kogyo Co., Ltd.), or a Hivis Dispermix (registered trademark of mixers manufactured by Tokushu Kika Kogyo Co., Ltd.). The temperature and time for mixing components (A1) and (B) are not particularly limited, but are preferably mixed at 20°C to 150°C for 30 minutes to 3 hours, and from the viewpoint of the stability of the physical properties of the thermally conductive thermosetting silicone resin composition, are preferably mixed at 100°C to 150°C for 1 hour to 2 hours.
[0052] [Process (II)] The mixture obtained in step (I) is mixed with a platinum group metal hydrosilylation catalyst (A3) and component (A2), and mixed at room temperature to 40°C for 10 minutes to 1 hour to produce a thermosetting silicone thermally conductive composition.
[0053] [Process (III)] As a step of magnetically orienting the thermally conductive inorganic filler of the thermally conductive thermosetting silicone resin composition, a pulse magnetic field having a magnetic field strength (magnetic flux density) of 30 T or more, preferably 30 T to 40 T, is applied for a duration of 0.5 seconds to 60 seconds, preferably 0.5 to 10 seconds, at a temperature of 60°C to 90°C, preferably 65 to 85°C during magnetic field application. FIG. 1 shows an example of a profile of the pulse magnetic field applied to the thermally conductive thermosetting silicone resin composition. This is a profile of the pulse magnetic field applied in Example 1 described later. The horizontal axis of FIG. 1 is the elapsed time, and the starting point of 0 seconds is arbitrary. The vertical axis is the measured value of the magnetic flux density. In the description of the present invention, a magnetic field strength (magnetic flux density) of 30 T or more means that the peak strength of the pulse magnetic field is 30 T or more. In the description of the present invention, the duration of the magnetic field means the elapsed time during which the magnetic field strength is 5 T or more when the peak strength of the pulse magnetic field is 30 T or more as described above. In Fig. 1, the magnetic field strength (i.e., peak magnetic field strength) is 39.1 T. Also, the time during which the magnetic field strength is 5 T or more is 1.0 second.
[0054] [Process (IV)] The magnetically oriented thermally conductive thermosetting silicone resin composition is thermally cured at 90° C. to 150° C. for 1 to 2 hours.
[0055] [Pulse magnetic field generator] A pulsed magnetic field generating device that can be used in the present invention is, for example, configured as follows. 1) DC generator with flywheel 2) Electromagnet 3) Controller 4) Temperature chamber
[0056] In the following, each component of the pulsed magnetic field generator will be described in accordance with the embodiment used in the examples described later, but in the present invention, any pulsed magnetic field generator can be used as long as it can apply a pulsed magnetic field of 30 T or more for 0.5 seconds or more and 60 seconds or less to the thermally conductive thermosetting silicone resin composition.
[0057] [DC generator with flywheel] A DC generator with a flywheel combines a DC motor with a disk (flywheel) that has a large moment of inertia. Energy can be stored by rotating the flywheel with a DC motor, and the rotational energy can be extracted as electrical energy by using the DC motor as a dynamo. The DC generator with a flywheel used in the examples of this invention has a maximum output of 2.7 kV, 19 kA, and 51.3 MW. The output of this DC generator with a flywheel is adjusted by a controller, and a large current is passed through the electromagnets connected in series, generating a magnetic field proportional to the current in the electromagnets described below.
[0058] [electromagnet] In the embodiment of the present invention, a solenoid made of 4 mm x 6 mm copper wire was used as the electromagnet. The electrical resistance of this solenoid was 42 mΩ at 77 K and 330 mΩ at room temperature, and the inductance was 100 mH. The space in which a constant magnetic field can be generated is the inner diameter size of the electromagnet, 27 mm in diameter and 40 mm in length.
[0059] [Controller] In an embodiment of the present invention, the controller supplied a current of 10 kA to an electromagnet cooled to 77 K by liquid nitrogen with a discharge voltage of 2,400 V.
[0060] [Thermostatic machine] In the embodiment of the present invention, a double tube made of stainless steel was inserted as a thermostatic device to thermally insulate the electromagnet cooled by liquid nitrogen from the sample space. The inside size of this double tube is 20 mm in diameter, and a vacuum is maintained between the inner tube and the outer tube of the double tube, and a heater made of manganin wire with a diameter of 0.1 mm is attached to this space. As a result, even if the double tube is placed in liquid nitrogen, the temperature of the sample space can be semi-permanently maintained between 77 K and 373 K. Under this constant temperature condition, a pulse magnetic field of up to 39 T was applied to harden the silicone composition.
[0061] [Thermal conductive silicone resin sheet] The thermal conductivity of the thermally conductive silicone resin sheet obtained by the manufacturing method of the present invention is preferably 20 W / m·K or more, and more preferably 30 W / m·K or more. There is no particular upper limit, but it can be 50 W / m·K or less. Because of such excellent thermal conductivity, it is suitable for heat dissipation. In the present invention, the thermal conductivity is measured by a xenon flash analyzer manufactured by NETZSCH. EXAMPLES
[0062] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to the following examples.
[0063] The components used in the examples and comparative examples are described below.
[0064] [Preparation Example: Preparation of Addition Reaction Catalyst (Component (A3))] First, component (A3) was prepared as follows. 8.0 g of chloroplatinic acid HPtCl6·6H2O (37.6 mass% in terms of platinum atoms) was placed in a 100 mL reaction flask equipped with a reflux condenser, thermometer, and stirrer, and then 40.0 g of ethanol and 16.0 g of divinyltetramethyldisiloxane were added. After heating and reacting at 70°C for 50 hours, the reaction mixture was neutralized for 2 hours by gradually adding 16 g of sodium bicarbonate while stirring at room temperature (25°C). The reaction mixture was filtered under suction, and the filtrate was distilled under reduced pressure to substantially remove the ethanol and excess divinyltetramethyldisiloxane, and then diluted with toluene to make the total amount 600 g (containing 0.5 mass% in terms of platinum atoms).
[0065] To the above-mentioned toluene solution of platinum-vinylsiloxane complex, 290 g of dimethylpolysiloxane terminated at both molecular chain terminals with dimethylvinylsiloxy groups and a viscosity of 600 mPa s was added and stirred, and the toluene was removed under reduced pressure at 60°C / 27 hPa. The product from which the toluene had essentially been removed was used as the hydrosilylation catalyst (containing 1.0 mass% platinum atoms).
[0066] [Component (A1)] Dimethylpolysiloxane terminated at both ends with dimethylvinylsiloxy groups, with a viscosity of 600 mPa s (vinyl group content: 0.015 mol / 100 g, equivalent to m = 2.000 and n = 0.011 in formula (1))
[0067] [(A2) component] Organohydrogenpolysiloxane represented by the following formula: [ka] (Hydrosilyl group content: 0.00128 mol / g, corresponding to p1=1.969 and q1=0.098 in formula (2)) The bonding order of each siloxane unit is not limited to the above.
[0068] [(A3) component] Platinum group metal-based hydrosilylation catalysts prepared in the above Preparation Examples
[0069] [Component (B): Diamagnetic, thermally conductive inorganic filler] B-1: XN-100-15M (average diameter 1 μm, average length 150 μm): manufactured by Nippon Graphite Fiber Co., Ltd. B-2: XN-100-25M (average diameter 1 μm, average length 250 μm): manufactured by Nippon Graphite Fiber Co., Ltd.
[0070] [Other ingredients] A viscosity modifier represented by the following formula: [ka]
[0071] A thermally conductive silicone resin sheet having the composition shown in Table 1 was produced by the method described below.
[0072] [Examples 1 to 5, Comparative Examples 1 and 2] Preparation of Thermally Conductive Silicone Composition The (A1) component and the (B) component were blended at room temperature (25°C) and mixed for 10 to 30 minutes using a planetary mixer. The resulting mixture was heated to 150°C and stirred and mixed under reduced pressure for 120 minutes. After that, the heating was stopped and the mixture was cooled to 50°C or less under room temperature air blowing conditions. After cooling, the platinum metal-based hydrosilylation reaction catalyst components (A2) and (A3) were added and stirred and mixed at room temperature (25°C). In this way, a thermally conductive thermosetting silicone resin composition was obtained.
[0073] [Preparation of thermally conductive silicone resin sheet] The composition was molded into a sheet, subjected to a magnetic field under the conditions shown in Table 1, and then heat-cured to produce a thermally conductive silicone resin sheet. The magnetic flux density profile of the magnetic field applied in Example 1 is shown in Figure 1. The heat-curing temperature and heating time were 120°C and 1.5 hours in all of Examples 1 to 5 and Comparative Examples 1 and 2.
[0074] The properties of the produced thermally conductive silicone resin sheets were measured by the methods described below. The results are shown in Table 1.
[0075] [Thermal conductivity measurement] Measurement was carried out at 25° C. using a xenon flash analyzer LFA447 manufactured by NETZSCH.
[0076] [Table 1]
[0077] The results in Table 1 show that the thermally conductive silicone resin sheet obtained by the manufacturing method of the present invention has excellent thermal conductivity. This excellent thermal conductivity is due to the high orientation of the thermally conductive inorganic filler. The thermally conductive silicone resin sheet obtained by the manufacturing method of the present invention not only has excellent thermal conductivity, but also demonstrates excellent productivity because it is oriented by application of a magnetic field for a very short time. That is, Examples 1 to 5, which contain components (A1) to (A3) and component (B) and apply a pulse magnetic field of 30 T or more for 0.5 to 60 seconds before curing, have excellent thermal conductivity compared to Comparative Examples 1 and 2, even when the magnetic field application time is as short as 0.017 minutes (about 1.0 second).
[0078] The present specification includes the following aspects. [1]: (A) a thermosetting silicone resin containing the following components (A1) to (A3): 100 parts by mass (A1) an organopolysiloxane having two or more alkenyl groups bonded to silicon atoms in each molecule; (A2) an organohydrogenpolysiloxane having two or more hydrosilyl groups per molecule: an amount such that the molar ratio of hydrosilyl groups in the component (A2) to alkenyl groups bonded to silicon atoms in the component (A1) is 0.5 to 2; and (A3) Platinum group metal hydrosilylation catalyst: 0.1 to 2,000 ppm by mass of platinum group metal element relative to the component (A) and, (B) a thermally conductive inorganic filler that is a diamagnetic material having an aspect ratio of the major axis to the minor axis of 5 or more, a major axis of 30 μm or more and 300 μm or less, and a specific gravity of 2.0 or more and less than 3.5: 30 to 150 parts by mass; A method for producing a thermally conductive silicone resin sheet, which is a cured product of the thermally conductive thermosetting silicone resin composition, by curing a thermally conductive thermosetting silicone resin composition containing A method for producing a thermally conductive silicone resin sheet, comprising applying a pulse magnetic field of 30 T or more to the thermally conductive thermosetting silicone resin composition for 0.5 to 60 seconds, and then heating the thermally conductive thermosetting silicone resin composition at 90 to 150°C for 1 to 2 hours to cure the composition. [2]: The method for producing a thermally conductive silicone resin sheet according to the above [1], wherein the component (A1) is an organopolysiloxane represented by the following average composition formula (1): R 1 m R 2 n SiO (4-m-n) / 2 (1) (In the formula, R 1 are independently selected from an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, and an aralkyl group having 7 to 10 carbon atoms; R 2 are independently an alkenyl group having 2 to 6 carbon atoms. m is a positive number of 0.5 to 2.5, and n is a positive number of 0.0001 to 0.2, with the proviso that m+n is a positive number of 0.8 to 2.7. [3]: The method for producing a thermally conductive silicone resin sheet according to the above [1] or [2], wherein the component (A2) is an organohydrogenpolysiloxane represented by the following average composition formula (2): R 3 p1 H q1 SiO (4-p1-q1) / 2 (2) (In the formula, R 3 are independently a group selected from an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, and an aralkyl group having 7 to 10 carbon atoms. p1 is a positive number of 1.0 to 3.0, and q1 is a positive number of 0.05 to 2.0, with the proviso that p1+q1 is a positive number of 0.5 to 3.0. [4]: The method for producing a thermally conductive silicone resin sheet according to any one of the above [1] to [3], wherein the component (B) is one or more diamagnetic materials selected from carbon fiber, graphite, graphene, carbon nanotubes, silicon carbide, and boron nitride.
[0079] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention. [Industrial Applicability]
[0080] The method for producing a thermally conductive silicone resin sheet of the present invention is not only excellent in productivity, but also provides a thermally conductive silicone resin sheet that has excellent thermal conductivity.
Claims
1. (A) A thermosetting silicone resin containing the following components (A1) to (A3): 100 parts by mass (A1) an organopolysiloxane having two or more alkenyl groups bonded to silicon atoms in each molecule; (A2) an organohydrogenpolysiloxane having two or more hydrosilyl groups per molecule: an amount such that the molar ratio of hydrosilyl groups in component (A2) to alkenyl groups bonded to silicon atoms in component (A1) is 0.5 to 2; and (A3) Platinum group metal hydrosilylation catalyst: 0.1 to 2,000 ppm by mass of platinum group metal element relative to the component (A) and, (B) a thermally conductive inorganic filler that is a diamagnetic material having an aspect ratio of the major axis to the minor axis of 5 or more, a major axis of 30 μm or more and 300 μm or less, and a specific gravity of 2.0 or more and less than 3.5: 30 to 150 parts by mass; A method for producing a thermally conductive silicone resin sheet, which is a cured product of the thermally conductive thermosetting silicone resin composition, by curing a thermally conductive thermosetting silicone resin composition containing A method for producing a thermally conductive silicone resin sheet, comprising the steps of: applying a pulse magnetic field of 30 T or more to the thermally conductive thermosetting silicone resin composition for 0.5 seconds or more and 60 seconds or less; and then heating the thermally conductive thermosetting silicone resin composition at 90 to 150°C for 1 to 2 hours to cure the composition.
2. 2. The method for producing a thermally conductive silicone resin sheet according to claim 1, wherein the component (A1) is an organopolysiloxane represented by the following average composition formula (1): R 1 m R 2 n SiO (4-m-n)/2 (1) (In the formula, R 1 are independently selected from an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, and an aralkyl group having 7 to 10 carbon atoms; R 2are independently an alkenyl group having 2 to 6 carbon atoms; m is a positive number of 0.5 to 2.5, and n is a positive number of 0.0001 to 0.2, provided that m+n is a positive number of 0.8 to 2.
7.
3. 3. The method for producing a thermally conductive silicone resin sheet according to claim 1, wherein the component (A2) is an organohydrogenpolysiloxane represented by the following average composition formula (2): R 3 p1 H q1 SiO (4-p1-q1)/2 (2) (In the formula, R 3 are independently a group selected from an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, and an aralkyl group having 7 to 10 carbon atoms. p1 is a positive number of 1.0 to 3.0, and q1 is a positive number of 0.05 to 2.0, provided that p1+q1 is a positive number of 0.5 to 3.
0.
4. 3. The method for producing a thermally conductive silicone resin sheet according to claim 1, wherein the component (B) is one or more diamagnetic materials selected from the group consisting of carbon fiber, graphite, graphene, carbon nanotubes, silicon carbide, and boron nitride.
Citation Information
Patent Citations
High-thermal-conductivity molding and method for producing the same
JP2005146057A
Thermally conductive sheet, method for producing the same, and heat radiation device using thermally conductive sheet
JP2014001388A
Heat conductive sheet and manufacturing method of heat conductive sheet
JP2019186555A
Magnetic field generation device
JP2022000881A