Pellet for injection molding and pellet manufacturing method
By blending polylactic acid resin with wood grains of 50 μm or less, the resin material achieves high tensile strength and improved mold fluidity, addressing the limitations of existing injection molding technologies.
Patent Information
- Application Number
- JP2023065811
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-13
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-04-13
AI Technical Summary
Existing injection molding technologies using biodegradable plastics, such as those mixing wood flour with polylactic acid resin, face issues of low tensile strength and poor fluidity, particularly in small gates, leading to impaired mold flow and production challenges.
A resin material for injection molding is developed by blending polylactic acid resin with wood grains of 50 μm or less, using a crusher, classification screen, and a two-type blending mechanism to create pellets with high tensile strength and improved mold fluidity.
The solution results in pellets that maintain high tensile strength and ensure smooth flow through small gates, reducing production costs and enhancing the manufacturing process efficiency.
Smart Images

Figure 2024151958000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to granular pellet technology for injection molding. [Background technology]
[0002] It is known that waste plastic flows into the ocean, breaks down into micron-sized particles, and causes harm to fish and other marine life. If the waste plastic is biodegradable, it will not harm marine life. Therefore, it is desirable to replace plastics with biodegradable plastics.
[0003] However, biodegradable plastics are more expensive than other ordinary plastics. As a countermeasure, it is known to mix waste wood such as sawdust with biodegradable plastics to increase the volume and reduce costs, and devices for this purpose have been proposed (see, for example, Patent Document 1 (Figure 1)).
[0004] The technology of Patent Document 1 will be described with reference to FIG. As shown in Fig. 11, wood flour 102 and polylactic acid resin 103 are put into a hopper 101 and stirred with a stirring blade 104. The stirred mixture 105 is extruded while being kneaded in a molding machine 106 to obtain a molded product. The grain size of the wood powder 102 is 300 μm or more (Patent Document 1, paragraph 0025).
[0005] However, the technique of Patent Document 1 has the following drawbacks. First, the molded article produced by the technique of Patent Document 1 has low tensile strength. Secondly, the flowability of the resin material inside the mold is poor.
[0006] As the applications of molded products become more diverse, there is a demand for improved tensile strength. In addition, in a mold for injection molding small or ultra-small molded products, the gate diameter is inevitably small. Polylactic acid resin 103 becomes close to liquid through kneading, but wood powder 102 remains solid. When the gate diameter becomes small, wood powder 102 may hinder fluidization, and measures to prevent this are required.
[0007] Therefore, there is a demand for a resin material for injection molding, which is made by blending polylactic acid resin with wood flour, and which produces molded products with high tensile strength and good fluidity within a mold. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Patent No. 5321254 Summary of the Invention [Problem to be solved by the invention]
[0009] The present invention has an object to provide a resin material for injection molding, which is made by blending wood flour with polylactic acid resin, and which produces molded products with high tensile strength and good fluidity within a mold. [Means for solving the problem]
[0010] The invention according to claim 1 is a granular pellet to be subjected to injection molding, The pellets are characterized in that the base material is polylactic acid resin, and wood grains with a particle size not exceeding 50 μm are mixed into the base material. In addition, pellet means a small ball or a small grain in Japanese.
[0011] The invention according to claim 2 is a granular pellet to be subjected to injection molding, The pellets are characterized in that the base material is a polylactic acid resin, and wood granules having a particle size not exceeding 30 μm are mixed into the base material.
[0012] The invention according to claim 3 is a pellet manufacturing method for manufacturing the injection molding pellets according to claim 1, A step of preparing wood chips, a crusher, polylactic acid resin granules, a two-type blending mechanism, and a pellet manufacturing device; A step of feeding the wood chips into the crusher and crushing them with the crusher to obtain wood grains having a particle size of 50 μm or less; A step of feeding the wood grains and the polylactic acid resin grains into the two-type blending mechanism and obtaining blended grains in the two-type blending mechanism; The process comprises the steps of feeding the blended grains into the pellet manufacturing apparatus, kneading and extruding the blended grains in the pellet manufacturing apparatus, and cutting the resulting strands to obtain pellets.
[0013] The invention according to claim 4 is a pellet manufacturing method for manufacturing the injection molding pellets according to claim 2, A step of preparing wood chips, a crusher, a classification net, polylactic acid resin particles, a two-type blending mechanism, and a pellet manufacturing device; A step of feeding the wood pieces into the crusher and crushing them with the crusher to obtain wood grains; A step of obtaining fine wood particles having a particle size of 30 μm or less by classifying the obtained wood particles with the classification net; A step of feeding the wood fine particles and the polylactic acid resin particles into the two-type blending mechanism and obtaining blended particles in the two-type blending mechanism; The process comprises the steps of feeding the blended grains into the pellet manufacturing apparatus, kneading and extruding the blended grains in the pellet manufacturing apparatus, and cutting the resulting strands to obtain pellets. Effect of the Invention
[0014] In the invention according to claim 1, the granular pellets are fed into an injector and kneaded and plasticized in the injector. The plasticization causes the polylactic acid resin to become fluid, but the wood grains remain solid. The diameter of the gate inside the mold varies, but the minimum diameter of the tunnel gate is said to be about 0.50 mm. With conventional technology, wood powder is 300 μm (0.30 mm), so it is difficult for it to pass through a 0.50 mm tunnel gate. In contrast, the wood grains of the present invention are 50 μm (0.05 mm) which is significantly smaller than the minimum diameter (0.50 mm) of the tunnel gate, so the resin material passes through the 0.50 mm tunnel gate without delay.
[0015] Furthermore, as will be described in more detail later, 50 μm wood grains are expected to produce a structure with approximately 1.4 times the tensile strength compared to 300 μm wood powder. Therefore, according to claim 1, a resin material (pellets for injection molding) is provided which gives a molded product with high tensile strength and good fluidity within a mold.
[0016] In the invention according to claim 2, the wood grains have a diameter of 30 μm (0.03 mm), which is significantly smaller than the minimum diameter (0.50 mm) of the tunnel gate, so that the resin material passes through the 0.50 mm tunnel gate more smoothly.
[0017] Furthermore, as will be described in more detail later, 30 μm wood grains are expected to produce a structure with approximately 1.5 times the tensile strength compared to 300 μm wood powder. Therefore, according to claim 2, a resin material (pellets for injection molding) is provided which gives a molded product with high tensile strength and good fluidity within a mold.
[0018] The invention according to claim 3 is a pellet manufacturing method, which manufactures pellets using a crusher, a two-kind blending mechanism, and a pellet manufacturing device. The crusher, the two-component blending mechanism, and the pellet manufacturing device are relatively simple in structure and inexpensive, so that pellets for injection molding can be manufactured at a relatively low cost.
[0019] The invention according to claim 4 is a pellet manufacturing method, which manufactures pellets using a crusher, a classifying net, a two-kind mixing mechanism, and a pellet manufacturing device. The crusher, the two-type blending mechanism, and the pellet manufacturing device are relatively simple in structure and inexpensive, and the classification screen is also extremely inexpensive. Therefore, it is possible to manufacture pellets for injection molding at a relatively low cost. [Brief description of the drawings]
[0020] [Figure 1] FIG. 2 is a diagram showing the principle of a pulverizer used in the present invention. [Diagram 2] FIG. 1 is a diagram illustrating the principle of a classification net. [Diagram 3] (a) is a plan view of the two-type mixing mechanism, (b) is a cross-sectional view taken along line bb of (a), and (c) is a cross-sectional view taken along line cc of (b). [Figure 4] FIG. 2 is a plan view of the pellet manufacturing apparatus. [Diagram 5] FIG. [Figure 6] 1(a) to 1(c) are diagrams explaining the principle of the direct gate. [Figure 7] 1 is a graph showing the correlation between grain size and tensile strength of wood grains. [Figure 8] 1 is a graph showing the correlation between the blending ratio of wood grains and tensile strength. [Figure 9] Graph (a) shows the relationship between grain size and pressure fluctuation, and graphs (b) to (e) are diagrams explaining the principle of fluidity. [Figure 10] FIG. 1 is a flow diagram illustrating a pellet production method of the present invention. [Figure 11] FIG. 1 is a diagram illustrating a conventional technique. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS An embodiment of the present invention will now be described with reference to the accompanying drawings. EXAMPLES
[0022] [Crusher] As shown in FIG. 1, the crusher 10 comprises legs 12 placed on a floor 11, a main chamber 13 supported by the legs 12, a crushing blade 14 built into the main chamber 13, a motor 15 for rotating the crushing blade 14 at high speed, a conical cylinder 16 extending upward from the main chamber 13, a vertical cylinder 17 extending upward from the conical cylinder 16, and a sub-chamber 18 surrounding the conical cylinder 16. The conical cylinder 16 has a plurality of holes 19 that connect the main chamber 13 and the sub-chamber 18, and the sub-chamber 18 is provided with an outlet 21.
[0023] The crushing blade 14 is rotated at a speed of 1000 to 20000 revolutions per minute (16.7 to 333 revolutions per second). When wood chips 23 are fed into the vertical tube 17, the wood chips 23 are crushed by the crushing blades 14. While the crushed wood chips remain in the main chamber 13, they are repeatedly crushed by the crushing blades 14 and the centrifugal force caused by the rotation, becoming wood grains 25 with a grain size of 50 μm or less. These wood grains 25 are carried by a tornado-shaped swirling flow 26 upwards into the sub-chamber 18 and are then discharged from the outlet 21. As a result of the above, wood grains 25 having a grain size of 50 μm or less are obtained.
[0024] [Classification network] The wood grains 25 obtained from the grinder 10 of FIG. 1 are used when further classification is required. 2, the classification net 28 is, for example, a wire net having mesh that allows particles of 30 μm or less to pass and does not allow particles of more than 30 μm to pass. The wire net is moved back and forth in a fine motion.
[0025] When wood grains 25 are dropped onto a classification net 28 from above, wood grains 25 with a diameter exceeding 30 μm remain on the net and are discharged as shown by the arrow (1). The material that passes through the classification net 28 and falls becomes fine wood particles 29 of 30 μm or less.
[0026] [Two types of combination mechanism] As shown in Figure 3(a), the two-type blending mechanism 30 comprises a measure 31, a first tube 32 extending horizontally from the measure 31, a first spiral coil 33 rotatably stored in the first tube 32, a first motor 34 for rotating the first spiral coil 33, a first hopper 35 provided midway along the first tube 32, a second tube 36 extending horizontally from the measure 31, a second spiral coil 37 rotatably stored in the second tube 36, a second motor 38 for rotating the second spiral coil 37, and a second hopper 39 provided midway along the second tube 36.
[0027] As shown in Fig. 3(b), the polylactic acid resin granules 40 fed into the first hopper 35 drop into the first pipe 32, are transported by the first spiral coil 33, and reach the measure 31. The rotation speed of the first spiral coil 33 is controlled by the first motor 34, and the amount of polylactic acid resin granules 40 transported (mixed amount) is controlled.
[0028] Preferably, the tip of the first tube 32 protrudes from the wall of the measure 31 to the center of the measure 31. This allows the polylactic acid resin particles 40 to reach the drop opening without adhering to the wall of the measure 31. At this time, the measure 31 does not perform a blending function but prevents the polylactic acid resin particles 40 from scattering.
[0029] As shown in Figure 3 (c), the wood grains 25 or fine wood granules 29 fed into the second hopper 39 drop into the second pipe 36, are transported by the second spiral coil 37, and reach the measure 31. The rotation speed of the second spiral coil 37 is controlled by the second motor 38, and the amount (mixture) of the wood grains 25 or fine wood granules 29 fed is controlled.
[0030] Preferably, the tip of the second pipe 36 protrudes from the wall of the measure 31, protruding to near the center of the measure 31. This allows the wood grains 25 or fine wood granules 29 to reach the drop opening without adhering to the wall of the measure 31. At this time, the measure 31 does not perform a mixing function, but prevents the wood grains 25 or fine wood granules 29 from scattering.
[0031] The first helical coil 33 may be a screw having a helical blade attached to a shaft. However, since the first helical coil 33 is obtained by processing a steel wire into a helical coil shape, it is much cheaper than a screw. The same is true for the second helical coil 37. By employing the first spiral coil 33 and the second spiral coil 37, the manufacturing cost of the two-kind blending mechanism 30 can be reduced.
[0032] By the above steps, a blended pellet (FIG. 4, reference numeral 63) is obtained in which an appropriate amount of polylactic acid resin pellets 40 is blended with an appropriate amount of wood pellets 25 or fine wood pellets 29.
[0033] [Pellet manufacturing equipment] As shown in FIG. 4, the pellet manufacturing apparatus 50 comprises a first screw 51, a second screw 52 arranged alongside the first screw 51, a barrel 53 housing the first screw 51 and the second screw 52 so as to be freely rotatable, a heater 54 surrounding the barrel 53, a drop block 55 arranged at one end of the barrel 53, a converter 56 and a drive motor 57 for rotating the first screw 51 and the second screw 52, a die 58 arranged at the other end of the barrel 53, a strand cooling conveyor 61 arranged outside the die 58 and in series with the barrel 53, and a stride cutter 62 arranged at the outlet of the strand cooling conveyor 61.
[0034] The converter 56 is a device that distributes the power of the drive motor 57 to the rotational force of the first screw 51 and the rotational force of the second screw 52. The converter 56 can rotate the first screw 51 and the second screw 52 at the same speed in the same direction. By changing the internal structure of the converter 56, it is also possible to rotate the second screw 52 in the opposite direction to the first screw 51. Therefore, the rotational directions of the first screw 51 and the second screw 52 can be set arbitrarily.
[0035] The bucket 31 is bolted to the drop hole block 55. That is, the two-kind blending mechanism 30 is mounted on the pellet manufacturing device 50. By mounting it, it is not necessary to place the two-kind blending mechanism 30 on the floor, and the blended granules 63 immediately after blending can be fed into the barrel 53, thereby suppressing deterioration of the blended granules 63 over time.
[0036] In addition, when deterioration over time is acceptable, the two-kind blending mechanism 30 may be located away from the pellet manufacturing device 50. In this case, the blended granules 63 are transported from the two-kind blending mechanism 30 to the pellet manufacturing device 50 in a bag or bucket. Since the blended granules 63 can be prepared and stored, there is an advantage in that the flexibility of production is increased.
[0037] The particle size of the polylactic acid resin particles 40 fed into the first hopper 35 is, for example, 3.0 mm. The grain size of the wood grains 25 fed into the second hopper 39 is, for example, 50 μmm or less. Alternatively, the grain size of the fine wood grains 29 fed into the second hopper 39 is, for example, 30 μmm or less.
[0038] The ratio of the mixture in the portion of the measure 31 is, for example, polylactic acid resin particles 40:wood particles 25 (or fine wood particles 29)=70-99% by mass:30-1.0% by mass.
[0039] The blended granules 63 are kneaded by the rotation of the first screw 51 and the second screw 52, melted by the heat of the heater 54, and discharged from the die 58 in the form of thin rod-like strands 64. The strand 64 is cooled and solidified while being conveyed by the strand cooling conveyor 61, and is cut by a stride cutter 62 into pellets 66 for injection molding. The particle size of the pellets 66 for injection molding is, for example, 2.0 to 3.0 mm.
[0040] [Injection molding equipment] As shown in FIG. 5, the injection molding apparatus 70 includes a bed 71, and an injection mechanism 72 and a mold clamping mechanism 82 that are placed on the bed 71. In the clamping mechanism 82, a mold 83 is clamped by a fixed platen 84, a movable platen 85, and a toggle mechanism 86. The mold 83 is composed of, for example, a fixed mold 87 and a movable mold 88.
[0041] In the injection mechanism 72, the pellets 66 for injection molding are fed into a heating barrel 74 via a hopper 73. The fed pellets 66 for injection molding are kneaded by the rotation of a screw 75 contained in the heating barrel 74 and the heat from the heating barrel 74, and become plasticized.
[0042] The injection mechanism 72 is moved horizontally so that the nozzle 89 at the tip of the heating barrel 74 comes into contact with a sprue provided on the fixed platen 84 (or the fixed mold 87). The injection molding pellets 66 in a plasticized state (hereinafter referred to as molten resin material) accumulate on the nozzle 89 side inside the heating barrel 74. As the amount of accumulated material increases, the screw 75 retreats. When the retreat distance reaches a predetermined value, the screw 75 is advanced at high speed. As a result of this advancement, the molten resin material is injected into the mold 83.
[0043] The internal state of the mold 83 and the subsequent operations will be explained with reference to FIG. 6(a), inside the mold 83, the molten resin material 94 flows in the order of the runner 91, the tunnel gate 92, and the product cavity 93, and the molten resin material 94 fills the runner 91, the tunnel gate 92, and the product cavity 93. In this state, the molten resin material 94 is cooled. After cooling is completed, the movable mold 88 is separated from the fixed mold 87.
[0044] 6(b), the solidified product portion 96, the gate portion 97, and the runner portion 98 remain on the movable mold 88. In this state, the ejection pin 99 is advanced.
[0045] 6(c), the product part 96 is released from the movable die 88 by the ejector pin 99. A gate mark 97a remains in this product part 96, but the gate mark 97a is small. A molded product is obtained by finishing the product part 96 including the gate mark 97a.
[0046] In the direct gate method, the product portion 96 is separated from the movable mold 88 with the gate portion 97 connected to it. A process of cutting the gate portion 97 from the product portion 96 with a gate cutter (gate cutting process) is essential.
[0047] On the other hand, in the tunnel gate method, as explained in FIGS. 6(b) and 6(c), the gate portion 97 is cut in the product ejection process, so there is an advantage that the gate cutting process using a gate cutter is not required.
[0048] On the other hand, in order to cut the gate portion 97 in the product ejection process, it is necessary to reduce the gate diameter at the tip of the tunnel gate 92 in Fig. 6(a) The minimum gate diameter is, for example, 0.50 mm.
[0049] (experiment) The object of the present invention is to provide a resin material for injection molding, which is made by mixing wood powder with polylactic acid resin, and which has a high tensile strength of the molded product and good fluidity in the mold. For this purpose, a pellet manufacturing device (Fig. 4, reference number 50) and an injection molding device (Fig. 5, reference number 70) were used to prepare test pieces, and the tensile strength of the test pieces was examined. The mold (Fig. 5, reference number 93) was replaced with a mold that can obtain test pieces.
[0050] (material) Polylactic acid resin granules: FY201 manufactured by HighChem Wood chips: Larch
[0051] (wood grain) Wood grain: For comparison, three types of grains were prepared: 300 μm, 212 μm, and 2 μm.
[0052] (composition ratio) The mixture ratio was 90% by mass of polylactic acid resin granules and 10% by mass of wood grains.
[0053] (Test piece) Test specimen: Dumbbell tensile test specimen Number of test specimens: Five test specimens were prepared in consideration of the reliability of the measurements.
[0054] (Test Equipment) Testing equipment: Shimadzu Corporation precision universal testing machine AG-IS 250KN
[0055] The tensile strengths thus obtained are shown in Table 1.
[0056] [Table 1]
[0057] The average tensile strengths shown in Table 1 are graphed in Figure 7. As shown in FIG. 7, the smaller the grain size of the wood, the greater the tensile strength. The particle size of 300 μm in Comparative Example 1 corresponds to that of Patent Document 1 described in the prior art. One of the objectives of the present invention is to increase the tensile strength compared to conventional methods, and the degree of increase (expected value) is set to 1.5 times. If the horizontal axis is 30 μm or less, 1.5 times is achieved. Even if the particle size is 50 μm or less, it is almost achieved. Therefore, it was confirmed that the grain size of wood should be 50 μm or less, and even better, 30 μm or less.
[0058] (Additional Experiments) Next, additional experiments were carried out on the compounding ratio.
[0059] (composition ratio) The composition was 80% by mass of polylactic acid resin granules and 20% by mass of wood grains.
[0060] (wood grain) ·Wood grain: 2μm
[0061] The other conditions were the same as those in the above experiment. The results are shown in Table 2.
[0062] [Table 2]
[0063] The average tensile strengths shown in Table 2 are plotted in Figure 8. Example 1 and Comparative Example 1 are also included in FIG. 8 for comparison. According to FIG. 8, the higher the proportion of wood grain, the lower the tensile strength.
[0064] Although it is an estimated value, when the proportion of wood grains is 40 mass %, it becomes 0.95 times that of Comparative Example 1, and the object of the present invention cannot be achieved. When the proportion of wood grains is 30 mass %, the tensile strength is 1.16 times that of Comparative Example 1, which is somewhat unsatisfactory, but an improvement in the tensile strength is expected. Therefore, the blend should preferably contain 30% by mass or less of wood grain, even better 20% by mass or less, and if it is 10% by mass or less, a further increase in tensile strength can be expected.
[0065] (Liquidity considerations) The minimum diameter of the tunnel gate was 0.50 mm, i.e., 500 μm, and the wood grain content was 10 mass %, and the pressure (internal pressure) at the time of injection from the nozzle 89 shown in FIG. 5 was examined. As a result, the tendency shown in Figure 9(a) was confirmed.
[0066] FIG. 9(a) is a graph in which the horizontal axis indicates grain size (μm) of wood grains and the vertical axis indicates pressure fluctuation. As shown in Fig. 9(a), when the grain size exceeds 50 μm, the pressure fluctuation becomes large. On the other hand, when the grain size is 50 μm or less, the pressure fluctuation is small.
[0067] The reason for the occurrence of pressure fluctuations is presumed based on Figs. 9(b) to (e). As shown in Fig. 9(b), a grain 25 of 150 µm is approximately 1 / 3 of the minimum diameter of the gate (500 µm), which is smaller than the minimum diameter of the gate, so it flows as indicated by the arrow (←). At this time, the pressure becomes a predetermined pressure.
[0068] As shown in Figure 9(c), even if the grains are 150 μm, when multiple grains of wood 25 are packed together, they block the gate and the pressure rises sharply. After a short time, the mass collapses. That is, Figures 9(b) and 9(c) are repeated, and the pressure fluctuation becomes larger.
[0069] As shown in Fig. 9(d), a 50μm grain 25 is 1 / 10 of the minimum diameter of the gate (500μm), which is much smaller than the minimum diameter of the gate, so it flows as shown by the arrow (←). At this time, the pressure becomes a predetermined pressure. Although the frequency of occurrence is very low, when a large number of 50 μm grains 25 are aggregated, they block the gate in FIG. 9(e). However, this aggregate collapses immediately and returns to FIG. 9(d). As a result, the pressure fluctuation becomes smaller.
[0070] From the above, it was confirmed that even in the case of a tunnel gate, if the grain size of the wood is 50 μm or less, preferably 30 μm or less, a stable flow as shown in Figure 9(d) can be maintained and fluidity can be increased.
[0071] From the above findings, the following pellet production method is derived. In step number (hereinafter, referred to as ST) 01 in FIG. 10, wood chips, a crusher, a classification net, polylactic acid resin particles, a two-kind blending mechanism, and a pellet manufacturing device are prepared. In ST02, the wood chips are fed into a crusher and crushed. This crushing process produces wood grains of 1 to 50 μm (i.e., less than 50 μm).
[0072] In ST03, it is decided whether or not to classify. If classification is not required, preparation of a classification net can be omitted in ST01. Furthermore, if wood fines of 40 μm or less (or 30 μm or less) can be obtained by increasing the rotation speed of the crushing blades (FIG. 1, reference numeral 14) in the crusher, the classification step can be omitted.
[0073] If classification is necessary, classification is performed using a classification net in ST04. By this classification, wood fine particles of 1 to 30 μm (i.e., 30 μm or less) are obtained. In ST05, wood particles (or fine wood particles) and polylactic acid resin particles are fed into the two-component blending mechanism and blended. As a result, blended particles are obtained. In ST06, the compounded grains are fed into the pellet manufacturing device, kneaded, extruded, and the resulting strands are cut to obtain pellets for injection molding.
[0074] The crusher 10, the two-kind blending mechanism 30, and the pellet manufacturing device 50 described in the embodiment are merely examples, and the structure and principle may be changed.
[0075] Although the pellets for injection molding according to the present invention are suitable for a tunnel gate, they may be used for injection into a mold having other gates, such as a direct gate, a side gate, and a pin gate. [Industrial Applicability]
[0076] The present invention is suitable for injection molding pellets made of polylactic acid resin and wood grains (or wood granules). [Explanation of symbols]
[0077] 10...crusher, 23...wood chips, 25...wood grains, 29...fine wood grains, 30...two-type blending mechanism, 40...polylactic acid resin grains, 50...pellet manufacturing device, 63...blended grains, 66...pellets for injection molding.
Claims
1. A granular pellet to be subjected to injection molding, The pellets are injection molding pellets, characterized in that the base material is a polylactic acid resin, and wood grains having a particle size not exceeding 50 μm are mixed into the base material.
2. A granular pellet to be subjected to injection molding, The pellets are injection molding pellets, characterized in that the base material is a polylactic acid resin, and wood grains having a particle size not exceeding 30 μm are mixed into the base material.
3. A method for producing the injection molding pellets according to claim 1, comprising the steps of: A step of preparing wood chips, a crusher, polylactic acid resin granules, a two-type blending mechanism, and a pellet manufacturing device; A step of feeding the wood chips into the crusher and crushing them with the crusher to obtain wood grains having a particle size of 50 μm or less; A step of feeding the wood grains and the polylactic acid resin grains into the two-type blending mechanism and obtaining blended grains in the two-type blending mechanism; feeding the blended grains into the pellet manufacturing apparatus, kneading and extruding the blended grains in the pellet manufacturing apparatus, and cutting the resulting strands to obtain pellets.
4. A method for producing the injection molding pellets according to claim 2, comprising the steps of: A step of preparing wood chips, a crusher, a classification net, polylactic acid resin particles, a two-type blending mechanism, and a pellet manufacturing device; A step of feeding the wood pieces into the crusher and crushing them with the crusher to obtain wood grains; A step of classifying the obtained wood grains using the classification net to obtain fine wood grains with a particle size of 30 μm or less; A step of feeding the wood fine particles and the polylactic acid resin particles into the two-type blending mechanism and obtaining blended particles in the two-type blending mechanism; feeding the blended grains into the pellet manufacturing apparatus, kneading and extruding the blended grains in the pellet manufacturing apparatus, and cutting the resulting strands to obtain pellets.
Citation Information
Patent Citations
Porous film and its production
JP1996027296A
Resin composition and molding therefrom
JP2003286402A
Wood powder-containing material, method of manufacturing the same, and compact
JP2013067681A
Fiber-reinforced flame-retardant resin composition and molding
JP2018154725A