Composite granule and method for producing microfiber cellulose composite resin
By compressing resin powder with microfiber cellulose to form granules with defects, the handling and mixing issues of microfiber cellulose are addressed, resulting in improved productivity and uniformity of composite resins.
Patent Information
- Application Number
- JP2023065814
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-13
- Publication Date
- 2024-10-25
AI Technical Summary
Microfiber cellulose is bulky and difficult to handle, leading to inefficiencies in transportation, feeding to kneading machines, and incomplete mixing with resin, resulting in non-homogeneous composite resins.
Forming composite granules by compressing a mixture of resin powder and microfiber cellulose with specific properties, including defects on the surface and/or inside, to improve dispersibility and handling.
The composite granules facilitate stable feeding, reduce bulkiness, and enhance uniform dispersion, leading to improved productivity and quality of microfiber cellulose composite resins.
Smart Images

Figure 2024151961000001_ABST
Abstract
Description
[Technical field]
[0001] In recent years, nanotechnology has been attracting attention as it aims to reduce the size of substances to the nano level and obtain new physical properties that differ from those of the substances themselves. Microfiber cellulose, which is produced by subjecting pulp, a cellulose-based raw material, to chemical processing, pulverization, and other processes, has excellent strength, elasticity, and other properties. Molded products produced by processing this microfiber cellulose are expected to be used in various applications as a high-strength material derived from biomass. Patent Document 1 discloses that by taking advantage of the properties of this microfiber cellulose and mixing it with resin to produce a molded product, a composite resin with strength exceeding that of the original resin is produced.
[0002] This patent document discloses a composite resin that can be used as a high-strength material and that contains microfiber cellulose as a main component, and makes various proposals specifying the physical properties of this composite resin. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2019-131774 A Summary of the Invention [Problem to be solved by the invention]
[0004] Cellulose composite resins are usually produced by feeding microfiber cellulose as the main raw material into a kneader, kneading it, and then injection molding it. If the moisture content of the microfiber cellulose is high, steam explosion will occur during kneading, which will reduce productivity, so it is desirable for the moisture content to be low.
[0005] However, since microfiber cellulose is bulky not only in a slurry state but also in a dry state, it may take time to transport it, and it may be difficult to increase the amount of the microfiber cellulose fed to the kneader per unit time, making it impossible to increase the productivity of the composite resin. Furthermore, if the microfiber cellulose and the resin fed to the kneader are not mixed sufficiently, the composite resin produced may not be homogeneous, which may cause problems in the application of the composite resin to various applications. Therefore, the main problem to be solved by the present invention is to provide a composite granulated product that is suppressed in bulk, is unlikely to leave relatively large fragments when disintegrated, and has excellent dispersibility. [Means for solving the problem]
[0006] In the technical field related to obtaining microfibrous cellulose, cellulose nanofibers, etc. by defibrating raw pulp, research and development has been conducted focusing on defibration techniques, such as how to defibrate and to what extent. However, defibrated cellulose fibers are bulky, and therefore require special care in storage and handling. The present invention aims to solve the above problem by mixing cellulose fibers that have been finely defibrated once with a powdered resin to form blocks. The following embodiment can be said to be one embodiment that solves this problem. (First aspect) A composite granule formed by compressing a mixture containing resin powder and microfiber cellulose having an average fiber length of 0.1 to 1 mm. having surface and / or internal defects; A composite granule characterized by:
[0007] Conventionally, microfiber cellulose obtained by defibrating raw pulp aggregates randomly with each other in a dry state and becomes powdery, and when these are collected in one place, they become bulky and difficult to handle. For example, when transporting dry microfiber cellulose, some of the microfiber cellulose may fly away and be lost. In addition, when supplying the microfiber cellulose to a kneader, for example, if the microfiber cellulose powder contains excessive moisture, it may aggregate and become entangled or stuck at the supply port, or form bridges, making it difficult to supply the microfiber cellulose to the kneader stably.
[0008] In addition, even if a material consisting of only microfiber cellulose is agglomerated by applying pressure to reduce bulkiness, it is brittle and easily crumbles. On the other hand, it is known that when a mixture of microfiber cellulose and resin powder is pressurized to produce a granulated product, the shape of the granulated product is maintained, the handling during operation is facilitated, the transportability is improved, entanglement and sticking are unlikely to occur when fed to a kneader, and the amount of material fed to the kneader per unit time can be increased. It is also known that the granulated product has a certain hardness, but crumbles when a shear force is applied in the kneader.
[0009] However, there is another problem in producing a microfiber cellulose composite resin by supplying the above granules to a kneader. That is, the microfiber cellulose composite resin may not be produced uniformly. As a result of analyzing the produced microfiber cellulose composite resin to see whether the composite granules in the trial stage were sufficiently disintegrated and dispersed, it was found that the disintegration was insufficient and relatively large fragments remained in the produced microfiber cellulose composite resin. This is probably because the degree of compression of the composite granules in the trial stage was too strong during kneading, so that they were not completely disintegrated partially, and the dispersion was also insufficient.
[0010] Specifically, when a composite granule containing resin powder and microfibrous cellulose is fed into a kneader, the composite granule is sheared inside the kneader and falls apart. Some of the composite granules fall apart immediately while others fall apart after a period of time, and some of the granules fall apart finely while others fall apart only gradually. It is presumed that the difference in time for fall apart and the difference in the degree of fall apart prevent the resin powder and microfibrous cellulose from being uniformly dispersed.
[0011] Therefore, the present inventors have conducted intensive research and have completed the invention of the composite granules of the above-mentioned embodiment. In the first place, microfiber cellulose alone is not compressed to form granules, but a mixture having both resin powder and microfiber cellulose as in this embodiment can be compressed to form granules. Moreover, the composite granules of this embodiment are not firmly granulated, and are easily disintegrated when a certain degree of shear force is applied. In particular, since the composite granules of this embodiment have a defect, when a shear force is applied, the collapse easily occurs from the defect. Furthermore, when the composite granules of this embodiment collapse, fragments are unlikely to remain and the composite granules of this embodiment are easily broken up, so that the composite granules are more uniformly dispersed. Furthermore, the composite granules of this embodiment are compressed, so they are easy to handle, are unlikely to become entangled or stuck when fed to a kneader, and the amount of material fed to the kneader per unit time can be increased.
[0012] In addition to the above-mentioned aspects, the following aspects are also preferred. (Second aspect) The defect has at least a surface thereof, The composite granule according to the first embodiment.
[0013] (Third aspect) The composite granule is The cylindrical shape has a plurality of the missing portions on the side surface, The ratio (Rmin / Rmax) of the maximum diameter Rmax of the composite granule to the minimum diameter Rmin of the approximately cylindrical diameters in each of the missing portions is 0.5 or more and 0.9 or less. The composite granule according to the first embodiment.
[0014] If the ratio is within the above range, when the composite granules fed to the kneader are subjected to a shear force, they will crumble into pieces from the defective parts, and relatively large fragments are unlikely to remain.
[0015] (Fourth aspect) The mixture has an average fiber length of 0.1 to 1 mm and contains microfibrous cellulose in which all or a part of the hydroxyl groups are substituted with carbamate groups. The composite granule according to the first embodiment.
[0016] The cellulose fibers are easily agglomerated by hydrogen bonding due to the action of the hydroxyl groups that they have, but when the hydroxyl groups are substituted with carbamate groups, the hydrophilicity is suppressed, and the carbamate groups, which are bulkier than the hydroxyl groups, make it easier to disperse between the fibers (hereinafter, microfiber cellulose substituted with carbamate groups is also referred to as "carbamate-modified microfiber cellulose" in particular). When raw pulp is defibrated, if the microfiber cellulose is not substituted with carbamate groups, some of the defibration remains insufficient, whereas substituted microfiber cellulose is easily defibrated overall. The more defibrated the microfiber cellulose is overall, the more uniformly it disperses in the resin powder, so there is less bias when it is mixed with the resin powder. In a mixture in which the microfiber cellulose is uniformly dispersed, the microfiber cellulose easily enters the gaps formed between the resin powders, and by applying pressure in a state in which the microfiber cellulose is sufficiently dispersed, a composite granule in which the uneven distribution of the microfiber cellulose is suppressed is obtained.
[0017] (Fifth aspect) The substitution rate of the microfiber cellulose with a carbamate group is 0.05 mmol / g or more and 2.0 mmol / g or less. The composite granule according to the fourth embodiment.
[0018] If the substitution rate is within the above range, the dispersibility of the macrofibrous cellulose is improved, and the microfibrous cellulose is less likely to aggregate with itself.
[0019] (Sixth aspect) The resin powder is an acid-modified resin. The composite granule according to the first embodiment.
[0020] If the resin powder is an acid-modified resin, it is suitable as a matrix when the resin powder is made into a microfiber cellulose composite resin, and has the effect of improving the interfacial adhesion and improving the physical properties as a composite material.
[0021] (Seventh aspect) The resin powder contains a polymer having a polyolefin main chain and an organic acid anhydride group in a side chain. The composite granule according to the first embodiment.
[0022] The improved interfacial adhesion and physical properties as a composite material are even more pronounced.
[0023] (Eighth aspect) Bulk density: 0.10 to 0.40 g / cm 3 That is, The composite granule according to the first embodiment.
[0024] When the material has such a bulk density, it is less likely to leave relatively large fragments when it is broken down.
[0025] (Ninth aspect) The mass ratio of the resin powder to the microfiber cellulose is 50:50 to 1:99 based on the solid content. The composite granule according to the first embodiment.
[0026] The resin powder and the microfiber cellulose have good compressibility, and this has the effect of providing a composite granule with an appropriate hardness.
[0027] (Tenth Aspect) Volume is 5~800mm 3 That is, The composite granule according to the first embodiment.
[0028] This provides excellent transportability and other operability, making it easy to supply to a kneader.
[0029] (Eleventh aspect) a compression step of compressing a mixture containing a resin powder and microfiber cellulose having an average fiber length of 0.1 to 1 mm to obtain a composite granule having defects on the surface and / or inside; A kneading step of kneading the composite granules with resin pellets to obtain a microfiber cellulose composite resin, The total area of the foreign matter in the microfiber cellulose composite resin is 3000 to 1 mm 2 / m 2 That is, Manufacturing method of microfiber cellulose composite resin
[0030] As a composite granule, the same effects as in the first embodiment can be expected, and since the total area of the foreign matter is within the above range, the microfiber cellulose composite resin has uniform physical properties as a whole. Effect of the Invention
[0031] According to the present invention, there is provided a composite granule which is suppressed in bulk, is less likely to leave relatively large fragments when disintegrated, and has excellent dispersibility, and a method for producing a microfiber cellulose composite resin using the composite granule. [Brief description of the drawings]
[0032] [Figure 1] FIG. 2 is a diagram illustrating an example of a composite granule. [Diagram 2] FIG. 2 is a schematic diagram showing an example of a composite granule. [Diagram 3] FIG. 2 is a schematic diagram showing an example of a composite granule. [Figure 4] FIG. 2 is a diagram showing a production example of a microfiber cellulose composite resin. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0033] Next, an embodiment of the present invention will be described. Note that the embodiment is an example of the present invention. The scope of the present invention is not limited to the scope of the embodiment.
[0034] The composite granule 110 of this embodiment is a composite granule 110 formed by compressing a mixture containing resin powder and microfibrous cellulose having an average fiber length of 0.1 to 1 mm, and is characterized by having defective parts 111 on the surface and / or inside.
[0035] The composite granulated material 110 of this embodiment is formed by compressing a mixture of resin powder and microfiber cellulose. Although it is difficult to describe, if one imagines, for example, a wood pellet formed by compressing a large amount of finely ground wood under pressure, the composite granulated material 110 of this embodiment can be understood.
[0036] However, the compression conditions are completely different between wood pellets and the composite granulated material 110 of this embodiment, and in the case of wood pellets, finely ground wood is easily compressed when pressure is applied, but this is due to the adhesive properties of lignin, hemicellulose, etc. contained in the wood. In the case of microfiber cellulose, since some of the substances having such adhesive properties are removed during the fiberization process, even if pressure is applied to compress the microfibers together, the compressed state is not maintained when the pressure is removed, and the microfibers easily collapse.
[0037] Regarding this point, the inventors of the present invention have found that when resin powder is mixed with microfiber cellulose to form a mixture and pressure is applied to this mixture, a composite granulated product 110 is formed in which the compressed state is maintained. The mechanism by which the compressed state is maintained is not clear, but is roughly thought to be as follows. First, the size of the resin powder mixed with the microfiber cellulose to disperse the microfiber cellulose is relatively small compared to the size of the microfiber cellulose. Second, the microfiber cellulose and the resin powder are each well dispersed without bias. Third, it is thought that the resin powder has an adhesive effect similar to that of lignin and hemicellulose in wood pellets, and is easily granulated when compressed under pressure.
[0038] Since the composite granules 110 of this embodiment are compressed and granulated, they do not scatter and the amount lost can be reduced. In addition, even if the composite granules 110 contain excess moisture, they are unlikely to become entangled with each other at the feed port of the kneader, or to form sticking or bridges. Furthermore, the bulk density of the composite granules 110 is higher than that of powdered microfiber cellulose, and more raw material can be supplied to the kneader per unit time, which is expected to improve the productivity of the microfiber cellulose composite resin.
[0039] Generally, microfiber cellulose has the property of agglomerating together when dried, but this "aggregation" is a different concept from "compression" in this embodiment. In this embodiment, "compression" of microfiber cellulose formed by compression means that a mixture of resin powder and microfiber cellulose is compressed, and is different from the microfiber cellulose alone agglomerating together. In addition, the composite granule 110 is formed by compressing a mixture containing resin powder and a large number of microfiber celluloses.
[0040] In this specification, the molded body obtained by kneading and molding the composite granules 110 of this embodiment will be referred to as a "microfiber cellulose composite resin" or the like.
[0041] (Microfiber cellulose) Microfiber cellulose is a fiber made by finely pulverizing cellulose. In addition to microfiber cellulose, the category of finely pulverized cellulose fibers includes cellulose nanofibers with smaller fiber widths. Composite resins can be produced using microfiber cellulose, cellulose nanofibers, or a mixture of both. In particular, the reinforcing effect of the resin is significantly improved when the fiber is microfiber cellulose. In addition, in a washing process for the purpose of removing unreacted residual reagents, urea, etc. after the carbamate reaction, if the fiber to be washed is cellulose nanofiber, the dehydration is very poor. On the other hand, microfiber cellulose is easier to modify with carbamate groups (carbamation) than cellulose nanofiber from the viewpoint of dehydration. However, for cellulose fibers to be carbamate-converted, it is more preferable to carbamate the cellulose raw material before finely pulverizing it from the viewpoint of promoting the chemical reaction.
[0042] The microfiber cellulose used in the composite granule 110 of this embodiment has an average fiber width of, for example, 20 to 5 μm, preferably 18 to 8 μm, and more preferably 15 to 10 μm. If the average fiber width of the microfiber cellulose falls below 5 μm, it becomes no different from cellulose nanofiber, and there is a risk that the effect of improving the strength of the resin (particularly the bending modulus) may not be sufficiently obtained. In addition, a lot of time and a large amount of energy are required for defibration. Furthermore, dehydration is deteriorated. If the dehydration is deteriorated, a large amount of energy is required for drying, and if the energy consumed for drying is large, the fibers of the microfiber cellulose deteriorate, and there is a risk of the strength decreasing. On the other hand, if the average fiber width of the microfiber cellulose exceeds 20 μm, it becomes no different from pulp, and there is a risk of the reinforcing effect becoming insufficient.
[0043] Microfiber cellulose can be obtained by defibrating (refining) a cellulose raw material (hereinafter also referred to as "raw pulp"). As the raw pulp, one or more types can be selected from wood pulp made from broadleaf trees, coniferous trees, etc., non-wood pulp made from straw, bagasse, cotton, hemp, bast fiber, etc., and waste paper pulp (DIP) made from recycled waste paper, broke paper, etc. The above various raw materials may be in the form of a pulverized material (powdered material), for example, called cellulose-based powder.
[0044] However, in order to prevent impurities from being mixed in as much as possible, it is preferable to use wood pulp as the raw material pulp. As the wood pulp, for example, one or more types may be selected from chemical pulps such as hardwood kraft pulp (LKP) and softwood kraft pulp (NKP), and mechanical pulp (TMP), etc.
[0045] The hardwood kraft pulp may be bleached hardwood kraft pulp, unbleached hardwood kraft pulp, or semi-bleached hardwood kraft pulp. Similarly, the softwood kraft pulp may be bleached softwood kraft pulp, unbleached softwood kraft pulp, or semi-bleached softwood kraft pulp.
[0046] As the mechanical pulp, for example, one or more types can be selected and used from stone ground pulp (SGP), pressed stone ground pulp (PGW), refiner ground pulp (RGP), chemi-ground pulp (CGP), thermo-ground pulp (TGP), ground pulp (GP), thermo-mechanical pulp (TMP), chemi-thermomechanical pulp (CTMP), refiner mechanical pulp (RMP), bleached thermo-mechanical pulp (BTMP), etc.
[0047] For the microfiber cellulose, it is preferable to use pulp with a lignin content of 1.0% or less as the raw material pulp, and more preferably pulp with a lignin content of 0.8% or less. When carbamate-treated microfiber cellulose is used, for example, heat treatment of cellulose fibers so that the substitution rate of the carbamate group is 0.05 mmol / g or more tends to cause coloring. However, if the lignin content of the raw material pulp is within the above range, coloring caused by lignin can be suppressed, and coloring can also be suppressed when the composite granule 110 or microfiber cellulose composite resin is used. In addition, when the cellulose raw material is carbamate-treated, the lignin coexisting with the cellulose is also carbamate-treated. That is, the reagent used in the carbamate reaction reacts not only with the cellulose portion of the raw material pulp, but also with the lignin. When the carbamate reaction is completed and the remaining reagent is washed off from the cellulose, the carbamate-treated lignin also flows out and is removed. In this series of operations, the reagents for the carbamate reaction are consumed not only for cellulose but also for lignin, so that the carbamate conversion rate of the cellulose remaining in the fiber may decrease as a result. From this viewpoint, if the lignin content in the composite granules 110 is the above-mentioned content, the amount of carbamate compounds that flow out and do not contribute to fiber reinforcement can be suppressed, and the strength of the composite resin when made into the composite resin can be improved.
[0048] The lignin content is a value measured in accordance with the Lignin Content Test Method (JAPAN-TAPPI-No. 61 (2000)).
[0049] From the viewpoint of preventing discoloration, the kappa number of the raw material pulp is preferably 2 or less, and more preferably 1 or less.
[0050] The kappa number is a value measured in accordance with the kappa number test method (JIS-P-8211 (2011)).
[0051] The lignin content and the kappa number can be adjusted, for example, by the selection of the raw pulp, cooking, bleaching, and the like.
[0052] In this embodiment, the whiteness of the raw material pulp is preferably 50% or more, more preferably 80% or more, and particularly preferably 82% or more. If the whiteness of the raw material pulp itself is less than 50%, it will be further colored during melt-kneading of the composite granules 110, and the whiteness of the composite resin itself will be low.
[0053] The whiteness value is a value measured in accordance with JIS-P-8148:2001.
[0054] The raw pulp can be pretreated by a chemical method prior to defibration. Examples of pretreatment by a chemical method include hydrolysis of polysaccharides by acid (acid treatment), hydrolysis of polysaccharides by enzymes (enzyme treatment), swelling of polysaccharides by alkali (alkali treatment), oxidation of polysaccharides by an oxidizing agent (oxidation treatment), reduction of polysaccharides by a reducing agent (reduction treatment), and the like. As a pretreatment by a chemical method, an enzyme treatment is preferably carried out, and in addition, one or more treatments selected from an acid treatment, an alkali treatment, and an oxidation treatment are more preferably carried out. The enzyme treatment will be described in detail below.
[0055] As the enzyme used in the enzymatic treatment, it is preferable to use at least one of cellulase enzymes and hemicellulase enzymes, and more preferably to use both in combination. The use of these enzymes makes it easier to defibrate the cellulose raw material. Note that cellulase enzymes cause the decomposition of cellulose in the presence of water. Also, hemicellulase enzymes cause the decomposition of hemicellulose in the presence of water.
[0056] Examples of cellulase enzymes that can be used include enzymes produced by the genera Trichoderma (filamentous fungi), Acremonium (filamentous fungi), Aspergillus (filamentous fungi), Phanerochaete (basidiomycetes), Trametes (basidiomycetes), Humicola (filamentous fungi), Bacillus (bacteria), Schizophyllum (basidiomycetes), Streptomyces (bacteria), and Pseudomonas (bacteria). These cellulase enzymes are available as reagents or commercially available products. Examples of commercially available products include Cellulose T2 (manufactured by HPI), Meicerase (manufactured by Meiji Seika Kaisha), Novozym 188 (manufactured by Novozym), Multifect CX10L (manufactured by Genencor), and cellulase enzyme GC220 (manufactured by Genencor).
[0057] As the cellulase enzyme, either EG (endoglucanase) or CBH (cellobiohydrolase) can be used. EG and CBH can be used alone or in combination. They can also be used in combination with a hemicellulase enzyme.
[0058] Examples of hemicellulase enzymes that can be used include xylanase, which is an enzyme that breaks down xylan, mannase, which is an enzyme that breaks down mannan, and arabanase, which is an enzyme that breaks down araban. Also, pectinase, which is an enzyme that breaks down pectin, can be used.
[0059] Hemicellulose is a polysaccharide, excluding pectins, found between cellulose microfibrils in plant cell walls. Hemicellulose is diverse and differs depending on the type of wood and between the layers of the cell wall. In the secondary walls of softwoods, glucomannan is the main component, while in the secondary walls of hardwoods, 4-O-methylglucuronoxylan is the main component. Therefore, when obtaining fine fibers from softwood bleached kraft pulp (NBKP), it is preferable to use mannase. Also, when obtaining fine fibers from hardwood bleached kraft pulp (LBKP), it is preferable to use xylanase.
[0060] The amount of enzyme added to the cellulose raw material is determined by, for example, the type of enzyme, the type of wood used as the raw material (coniferous or broadleaf), the type of mechanical pulp, etc. However, the amount of enzyme added to the cellulose raw material is preferably 0.1 to 3 mass%, more preferably 0.3 to 2.5 mass%, and particularly preferably 0.5 to 2 mass%. If the amount of enzyme added is less than 0.1 mass%, the effect of adding the enzyme may not be sufficiently obtained. On the other hand, if the amount of enzyme added is more than 3 mass%, cellulose may be saccharified, and the yield of fine fibers may decrease. There is also a problem that the effect improvement corresponding to the increase in the amount added may not be observed.
[0061] When a cellulase enzyme is used as the enzyme, the pH during the enzyme treatment is preferably in the weak acidic range (pH = 3.0 to 6.9) from the viewpoint of the reactivity of the enzyme reaction, whereas when a hemicellulase enzyme is used as the enzyme, the pH during the enzyme treatment is preferably in the weak alkaline range (pH = 7.1 to 10.0).
[0062] The temperature during the enzyme treatment is preferably 30 to 70° C., more preferably 35 to 65° C., and particularly preferably 40 to 60° C., regardless of whether a cellulase enzyme or a hemicellulase enzyme is used as the enzyme. If the temperature during the enzyme treatment is 30° C. or higher, the enzyme activity is less likely to decrease, and it is possible to prevent the treatment time from being prolonged. On the other hand, if the temperature during the enzyme treatment is 70° C. or lower, it is possible to prevent the enzyme from being deactivated.
[0063] The time for the enzyme treatment depends on, for example, the type of enzyme, the temperature of the enzyme treatment, the pH during the enzyme treatment, etc. However, the time for the enzyme treatment is generally 0.5 to 24 hours.
[0064] After the enzyme treatment, it is preferable to inactivate the enzyme. Examples of methods for inactivating the enzyme include a method of adding an alkaline aqueous solution (preferably pH 10 or higher, more preferably pH 11 or higher) and a method of adding hot water at 80 to 100°C.
[0065] In addition, the enzyme treatment breaks down cellulose into oligosaccharides and monosaccharides, which turn brown and discolor when heated, like caramelized sugar. Therefore, after the enzyme treatment, it is preferable to thoroughly wash the raw pulp with water.
[0066] Next, the alkali treatment method will be described. When the pulp is treated with alkali prior to defibration, the hydroxyl groups of the hemicellulose and cellulose contained in the pulp are partially dissociated and the molecules are anionized, weakening the intra- and intermolecular hydrogen bonds and promoting the dispersion of the cellulose raw material during defibration.
[0067] Examples of the alkali used in the alkali treatment include organic alkalis such as sodium hydroxide, lithium hydroxide, potassium hydroxide, an aqueous ammonia solution, tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrabutylammonium hydroxide, and benzyltrimethylammonium hydroxide. However, from the viewpoint of production costs, it is preferable to use sodium hydroxide.
[0068] By subjecting the microfibrous cellulose to an enzyme treatment, acid treatment, or oxidation treatment prior to defibration, the water retention of the microfibrous cellulose can be reduced, the crystallinity can be increased, and the homogeneity can be improved. In this regard, microfibrous cellulose with low water retention is preferable because it is less likely to cause steam explosion during kneading and produces a high-strength composite resin.
[0069] When raw pulp is treated with enzymes, acids, or oxidation, the hemicellulose and amorphous regions of cellulose contained in the pulp are decomposed. As a result, the energy required for defibration can be reduced, and the uniformity and dispersibility of the cellulose fibers can be improved. However, since pretreatment reduces the aspect ratio of microfiber cellulose, excessive pretreatment is preferably avoided when using it as a reinforcing material for resins.
[0070] The raw material pulp can be defibrated by beating the raw material pulp using, for example, a homogenizer such as a beater, a high-pressure homogenizer, or a high-pressure homogenizer, a stone mill-type friction machine such as a grinder or a grinding machine, a single-shaft kneader, a multi-shaft kneader, a kneader refiner, a jet mill, etc. However, it is preferable to use a refiner or a jet mill.
[0071] The average fiber length (average length of single fibers) of the microfiber cellulose is preferably 0.1 to 1.0 mm, more preferably 0.2 to 0.8 mm, and particularly preferably 0.3 to 0.6 mm. If the average fiber length is less than 0.1 mm, a three-dimensional network cannot be formed between the fibers, and the flexural modulus of the composite resin may decrease, and the reinforcing effect may not be improved. On the other hand, if the average fiber length exceeds 1.0 mm, the reinforcing effect may be insufficient because the length is the same as that of the raw pulp.
[0072] The average fiber length of the cellulose raw material that is the raw material for the microfiber cellulose is preferably 0.50 to 5.00 mm, more preferably 1.00 to 3.00 mm, and particularly preferably 1.50 to 2.50. If the average fiber length of the cellulose raw material is less than 0.50 mm, the reinforcing effect of the resin may not be sufficiently obtained when the fiberization process is performed. On the other hand, if the average fiber length exceeds 5.00 mm, there is a risk of being disadvantageous in terms of production costs during fiberization.
[0073] The average fiber length of the microfibrous cellulose can be adjusted as desired by, for example, selecting the raw pulp, pre-treating, defibrating, and the like.
[0074] The fine A ratio of the microfiber cellulose is preferably 5% or more and 80% or less, more preferably 10% or more and 70% or less, and particularly preferably 15% or more and 60% or less. If the fine A ratio is less than 5%, the proportion of heterogeneous fibers is high, and a composite resin with low strength may be produced. On the other hand, if the fine A ratio exceeds 80%, the bending modulus may be insufficient, and some fibers are considered to be too low molecular weight, and these fibers are likely to produce oligosaccharides and monosaccharides that cause coloring when exposed to heat.
[0075] In addition, the fine A ratio of the microfiber cellulose is preferably within the above range, and the fine B ratio of the microfiber cellulose is preferably 15 to 50%, more preferably 16 to 40%. When the fine B ratio is within the above range, the strength of the composite resin is further increased.
[0076] The above is the fineness ratio of the microfiber cellulose, but it is more preferable if the fineness ratio of the cellulose raw material that is the raw material for the microfiber cellulose is also within a specified range. Specifically, the fine A ratio of the cellulose raw material that is the raw material for the microfiber cellulose is preferably 1% or more, more preferably 3 to 20%, and particularly preferably 5 to 18%. If the fine A ratio of the cellulose raw material before defibration is within the above range, it is considered that even if the microfiber cellulose is defibrated so that the fine A ratio is 30% or more, the damage to the fibers is small and the reinforcing effect of the resin is improved.
[0077] The fine A rate and the fine B rate can be adjusted by pretreatment such as enzyme treatment. However, especially when enzyme treatment is performed, the fiber itself may become tattered, and the reinforcing effect of the resin may decrease. Therefore, from this viewpoint, the amount of enzyme added is preferably 2% by mass or less, more preferably 1% by mass or less, and particularly preferably 0.5% by mass or less. Also, not performing enzyme treatment (addition amount 0% by mass) is also an option.
[0078] In this embodiment, "fine A rate" refers to the percentage of the total mass of pulp fibers with a fiber width of 75 μm or less and a fiber length of 0.2 mm or less to the total mass of pulp fibers. "Fine B rate" refers to the percentage of the total mass of pulp fibers with a fiber width of 10 μm or less and a fiber length of 0.2 mm or more to the total mass of pulp fibers.
[0079] The aspect ratio of the microfibrous cellulose is preferably 200 to 5, more preferably 100 to 10, and particularly preferably 60 to 20. If the aspect ratio is less than 5, a three-dimensional network cannot be sufficiently constructed, and therefore even if the average fiber length is 0.1 mm or more, the reinforcing effect may be insufficient. On the other hand, if the aspect ratio is more than 200, the microfibrous cellulose may be entangled more frequently, resulting in insufficient dispersion in the resin.
[0080] The fibrillation rate of the microfibrous cellulose is preferably 0.1 to 3.0%, more preferably 0.3 to 2.8%, and particularly preferably 0.5 to 2.5%. If the fibrillation rate exceeds 3.0%, the contact area with water becomes too large, so that dehydration may become difficult even if the cellulose is defibrated to an average fiber width of 0.1 μm or more. On the other hand, if the fibrillation rate is less than 0.1%, there may be few hydrogen bonds between fibrils, making it impossible to form a strong three-dimensional network.
[0081] In this embodiment, the fibrillation rate refers to the value obtained by disintegrating cellulose fibers in accordance with JIS-P-8220:2012 "Pulp Disintegration Method" and measuring the resulting disintegrated pulp using a fiber analyzer "FS5" manufactured by Valmet.
[0082] The crystallinity of the microfiber cellulose is preferably 50% or more, more preferably 55% or more, and particularly preferably 60% or more. If the crystallinity is less than 50%, the mixability with other fibers such as pulp and cellulose nanofibers is improved, but the strength of the fiber itself is reduced, so that the composite granule 110 may become excessively brittle or the strength of the resin may not be improved. On the other hand, the crystallinity of the microfiber cellulose is preferably 95% or less, more preferably 90% or less, and particularly preferably 85% or less. If the crystallinity is more than 95%, the proportion of strong hydrogen bonds formed within the molecule increases, the fiber itself becomes rigid, and dispersibility becomes poor.
[0083] The crystallinity of the microfibrous cellulose can be adjusted as desired, for example, by selecting the raw pulp, pre-treating it, and refining it.
[0084] The pulp viscosity of the microfiber cellulose is preferably 2 cps or more, more preferably 4 cps or more. If the pulp viscosity of the microfiber cellulose is less than 2 cps, it may be difficult to suppress the aggregation of the microfiber cellulose.
[0085] The freeness of the microfiber cellulose is preferably 500 ml or less, more preferably 300 ml or less, and particularly preferably 100 ml or less. If the freeness of the microfiber cellulose exceeds 500 ml, the effect of improving the strength of the resin may not be sufficiently obtained.
[0086] The zeta potential of the microfibrous cellulose is preferably -150 to 20 mV, more preferably -100 to 0 mV, and particularly preferably -80 to -10 mV. If the zeta potential is less than -150 mV, the compatibility with the resin may be significantly reduced, resulting in insufficient reinforcing effect. On the other hand, if the zeta potential is more than 20 mV, the dispersion stability may be reduced.
[0087] The water retention of the microfiber cellulose is preferably 400 to 80%, more preferably 350 to 90%, and particularly preferably 300 to 100%. If the water retention is less than 80%, the composite granule 110 may be excessively brittle. On the other hand, if the water retention is more than 400%, the composite granule 110 tends to have poor dewaterability and is prone to aggregation. On the other hand, if the water retention is 300 to 100%, the moisture content of the composite granule 110 can be easily adjusted and the fibers are less likely to be damaged, which contributes to improving the strength of the composite resin. The water retention of the microfiber cellulose can be further reduced by substituting the hydroxyl group of the fiber with a carbamate group, and the dewaterability and drying properties can be improved.
[0088] The water retention of the microfiber cellulose can be adjusted as desired by, for example, selecting the raw pulp, pre-treating it, defibrating it, and the like.
[0089] The microfiber cellulose can be modified by substituting a part of the cellulose with a functional group in order to impart another property to the inherent properties of the cellulose. Examples of the modification of the microfiber cellulose include carbamate, esterification, etherification, amidation, and sulfidation. In particular, carbamate is preferable because it improves the dispersibility of the microfiber cellulose. The microfiber cellulose constituting the composite granule 110 may be modified by carbamate to have a carbamate group, or may not be modified at all.
[0090] In the process of producing the composite granule 110, the timing of substituting the hydroxyl group of the microfibrous cellulose with the carbamate group is not particularly limited, as long as it is before the mixture containing the resin powder and the microfibrous cellulose is subjected to a compression treatment. For example, the cellulose raw material may be subjected to a carbamate reaction to have a carbamate group, or the microfibrous cellulose (finely divided cellulose raw material) may be subjected to a carbamate reaction to have a carbamate group.
[0091] Incidentally, having a carbamate group means that a carbamate group (an ester of carbamic acid) is introduced into the microfiber cellulose. The carbamate group can be represented by the following structural formula (Chemical Formula 1), and is, for example, represented by -O-CO-NH-, and examples thereof include -O-CO-NH2, -O-CONHR, and -O-CO-NR2.
[0092] [ka]
[0093] Here, n represents an integer of 1 or more. Each R is independently at least one of a saturated linear hydrocarbon group, a saturated branched hydrocarbon group, a saturated cyclic hydrocarbon group, an unsaturated linear hydrocarbon group, an unsaturated branched hydrocarbon group, an aromatic group, and a group derived therefrom.
[0094] Examples of the saturated linear hydrocarbon group include linear alkyl groups having 1 to 10 carbon atoms, such as a methyl group, an ethyl group, and a propyl group.
[0095] Examples of the saturated branched hydrocarbon group include branched alkyl groups having 3 to 10 carbon atoms, such as an isopropyl group, a sec-butyl group, an isobutyl group, and a tert-butyl group.
[0096] Examples of the saturated cyclic hydrocarbon group include cycloalkyl groups such as a cyclopentyl group, a cyclohexyl group, and a norbornyl group.
[0097] Examples of the unsaturated linear hydrocarbon group include linear alkenyl groups having 2 to 10 carbon atoms, such as ethenyl group (vinyl group), propen-1-yl group, and propen-3-yl group, and linear alkynyl groups having 2 to 10 carbon atoms, such as ethynyl group, propyn-1-yl group, and propyn-3-yl group.
[0098] Examples of the unsaturated branched hydrocarbon group include branched alkenyl groups having 3 to 10 carbon atoms, such as a propen-2-yl group, a buten-2-yl group, and a buten-3-yl group, and branched alkynyl groups having 4 to 10 carbon atoms, such as a butyn-3-yl group.
[0099] Examples of the aromatic group include a phenyl group, a tolyl group, a xylyl group, and a naphthyl group.
[0100] Examples of derivative groups include groups in which one or more hydrogen atoms in the above-mentioned saturated linear hydrocarbon groups, saturated branched hydrocarbon groups, saturated cyclic hydrocarbon groups, unsaturated linear hydrocarbon groups, unsaturated branched hydrocarbon groups, and aromatic groups are substituted with substituents (e.g., hydroxy groups, carboxy groups, halogen atoms, etc.).
[0101] In microfiber cellulose having a carbamate group (introduced with a carbamate group), some or all of the highly polar hydroxyl groups are replaced with carbamate groups having relatively low polarity. Therefore, microfiber cellulose having a carbamate group has low hydrophilicity and high affinity with resins having low polarity. As a result, microfiber cellulose having a carbamate group has excellent uniform dispersion with resins having similarly low polarity. In addition, the slurry of microfiber cellulose having a carbamate group has low viscosity and good handling properties.
[0102] The substitution rate of the carbamate group for the hydroxyl group of the microfiber cellulose is preferably 0.05 mmol / g or more and 2.0 mmol / g or less, more preferably 0.1 mmol / g or more and 1.8 mmol / g or less, and particularly preferably 0.2 mmol / g or more and 1.6 mmol / g or less. When the substitution rate exceeds 0.05 mmol / g, the hydrogen bonds between cellulose caused by the hydroxyl groups of cellulose are weakened (aggregation relaxation effect), and in addition, the affinity with the resin powder is increased (affinity improvement effect) by the introduction of the carbamate group, which is more hydrophobic than the hydroxyl group, so that the resin powder and the microfiber cellulose are mutually entangled, and the microfiber cellulose is less likely to aggregate, and the effect of resin reinforcement is enhanced. On the other hand, when the substitution rate of the carbamate group is high, especially when it exceeds 2.0 mmol / g, the heat resistance of the composite resin is reduced. In this regard, when the cellulose fiber is subjected to heat, the detachment of the hydroxyl group usually occurs, and the molecular chain may be shortened from the point where the detachment occurs. If some of the hydroxyl groups are modified by carbamate or the like, the elimination of the hydroxyl groups is more likely to occur. Therefore, if the substitution rate of the carbamate group is too high, the molecular chain becomes too short, the decomposition temperature decreases, and the heat resistance decreases. If the substitution rate of the carbamate group exceeds 2.0 mmol / g, the average fiber length of the pulp becomes short when the cellulose fiber is carbamate-modified, and there is a risk that the resin reinforcement effect is not sufficient. If the substitution rate exceeds 10.0 mmol / g, the cellulose fiber cannot maintain the fiber shape.
[0103] In this embodiment, the carbamate group substitution rate (mmol / g) refers to the amount of carbamate groups contained in 1 g of cellulose raw material having carbamate groups. The carbamate group substitution rate is calculated by measuring the N atoms present in the carbamate-treated pulp by the Kjeldahl method and calculating the carbamate rate per unit weight. Cellulose is a polymer with anhydroglucose as a structural unit, and has three hydroxyl groups per structural unit.
[0104] Examples of methods for obtaining carbamate-treated microfibrous cellulose include a method in which a cellulose raw material is subjected to a carbamate reaction and then finely divided (fibrillated) to obtain carbamate-treated microfibrous cellulose, and a method in which the cellulose raw material is finely divided (fibrillated) and then subjected to a carbamate reaction to obtain carbamate-treated microfibrous cellulose. Here, the defibration of the cellulose raw material is explained first, and then the carbamate reaction (modification) is explained. However, either the defibration or the carbamate reaction may be carried out first. In particular, it is preferable to carry out the carbamate reaction first, and then defibration. This is because the cellulose raw material before defibration has a high dehydration efficiency, and the cellulose raw material is easily defibrated by the heating accompanying the carbamate reaction.
[0105] The process of carbamate conversion of microfiber cellulose and the like (which may be a cellulose raw material as mentioned above; the same applies below) can be mainly divided into, for example, a mixing process, a removal process, and a heat treatment. The mixing process and the removal process can be collectively referred to as a conditioning process for preparing a mixture to be subjected to a heat treatment. Carbamate conversion also has the advantage that the reactants can be chemically modified without using an organic solvent.
[0106] In the mixing treatment, the microfiber cellulose or the like and urea or a derivative of urea (hereinafter simply referred to as "urea or the like") are mixed in a dispersion medium.
[0107] Examples of urea and urea derivatives that can be used include urea, thiourea, biuret, phenylurea, benzylurea, dimethylurea, diethylurea, tetramethylurea, and compounds in which the hydrogen atoms of urea are substituted with alkyl groups. These urea and urea derivatives can be used alone or in combination. However, it is preferable to use urea.
[0108] The upper limit of the mixture mass ratio of urea etc. to microfiber cellulose etc. (urea etc. / microfiber cellulose etc.) is preferably 300 / 100, more preferably 200 / 100. On the other hand, the lower limit is preferably 10 / 100, more preferably 20 / 100. By making the mixture mass ratio 10 / 100 or more, the efficiency of carbamate formation is improved. On the other hand, even if the mixture mass ratio exceeds 300 / 100, the carbamate formation is not further promoted.
[0109] The dispersion medium is usually water, although other dispersion media such as alcohols, ethers, and mixtures of water with other dispersion media may also be used.
[0110] In the mixing process, for example, microfibrous cellulose, etc. and urea, etc. may be added to water, microfibrous cellulose, etc. may be added to an aqueous solution of urea, etc., or urea, etc. may be added to a slurry containing microfibrous cellulose, etc. Furthermore, in order to mix uniformly, stirring may be performed after addition. Furthermore, the dispersion containing microfibrous cellulose, etc. and urea, etc. may contain other components. When the microfibrous cellulose, etc. is a sheet-shaped cellulose raw material, a method may be adopted in which the cellulose raw material is impregnated in a mixed liquid of urea, etc. and a dispersion medium and mixed. When the cellulose raw material is in a sheet shape, heat is conducted within the sheet, so that the heating temperature in the heat treatment can be lowered and the heating time can be shortened.
[0111] In the removal treatment, the dispersion medium is removed from the dispersion liquid containing the microfibrous cellulose etc. and urea etc. obtained in the mixing treatment. By removing the dispersion medium, the urea etc. can be reacted efficiently in the subsequent heat treatment.
[0112] The dispersion medium is preferably removed by volatilizing it by heating, which makes it possible to efficiently remove only the dispersion medium while leaving behind the components such as urea.
[0113] When the dispersion medium is water, the lower limit of the heating temperature in the removal treatment is preferably 50°C, more preferably 70°C, and particularly preferably 90°C. By setting the heating temperature at 50°C or higher, the dispersion medium can be efficiently volatilized (removed). On the other hand, the upper limit of the heating temperature is preferably 120°C, more preferably 100°C. If the heating temperature exceeds 120°C, the dispersion medium and urea may react, and the urea may independently decompose.
[0114] The heating time in the removal treatment can be appropriately adjusted depending on the solid content concentration of the dispersion liquid, etc. Specifically, it is, for example, 6 to 24 hours.
[0115] In the heat treatment following the removal treatment, a mixture of the microfiber cellulose and urea is heat-treated. In this heat treatment, some or all of the hydroxyl groups of the microfiber cellulose react with urea and are replaced with carbamate groups. More specifically, when urea is heated, it is decomposed into isocyanic acid and ammonia as shown in the following reaction formula (1). Isocyanic acid is very reactive, and for example, carbamate groups are formed on the hydroxyl groups of cellulose as shown in the following reaction formula (2). NH2-CO-NH2→ HN=C=O + NH3…(1) Cell-OH + HN=C=O → Cell-O-CO-NH2…(2)
[0116] The lower limit of the heating temperature in the heat treatment is preferably 120°C, more preferably 130°C, particularly preferably the melting point of urea (about 134°C) or higher, even more preferably 140°C, and most preferably 150°C. By setting the heating temperature at 120°C or higher, carbamate formation is efficiently carried out. The upper limit of the heating temperature is preferably 200°C, more preferably 180°C, and particularly preferably 170°C. If the heating temperature exceeds 200°C, the microfiber cellulose and the like may decompose, resulting in insufficient reinforcing effect.
[0117] The lower limit of the heating time in the heat treatment is preferably 1 minute, more preferably 5 minutes, particularly preferably 30 minutes, even more preferably 1 hour, and most preferably 2 hours. By setting the heating time to 1 minute or more, the carbamate reaction can be carried out reliably. On the other hand, the upper limit of the heating time is preferably 5 hours, more preferably 3 hours. If the heating time exceeds 5 hours, it is not economical, and carbamate reaction can be sufficiently carried out in 5 hours.
[0118] However, prolonged heating time leads to deterioration of cellulose fibers. Therefore, it is desirable to adjust the pH of the reaction system so as not to deteriorate cellulose fibers as much as possible even during heat treatment. Specifically, the pH is preferably 9 or more, more preferably 9 to 13, and particularly preferably 10 to 12 under alkaline conditions. As a second best option, the pH is 7 or less, preferably 3 to 7, and particularly preferably 4 to 7 under acidic or neutral conditions. Under neutral conditions of pH 7 to 8, the average fiber length of cellulose fibers may be shortened, and the reinforcing effect of the resin may be inferior. On the other hand, under alkaline conditions of pH 9 or more, the reactivity of cellulose fibers is increased, the reaction to urea, etc. is promoted, and the carbamate reaction occurs efficiently, so that the average fiber length of cellulose fibers can be sufficiently secured. On the other hand, under acidic conditions of pH 7 or less, the reaction of decomposing urea, etc. into isocyanic acid and ammonia proceeds, the reaction to cellulose fibers is promoted, and the carbamate reaction occurs efficiently, so that the average fiber length of cellulose fibers can be sufficiently secured. However, if possible, it is preferable to perform heat treatment under alkaline conditions. This is because acidic conditions may cause acid hydrolysis of cellulose to proceed.
[0119] The pH can be adjusted by adding an acidic compound (eg, acetic acid, citric acid, etc.) or an alkaline compound (eg, sodium hydroxide, calcium hydroxide, etc.) to the mixture.
[0120] As a heating device in the heat treatment, for example, a hot air dryer, a papermaking machine, a dry pulp machine, etc. can be used.
[0121] The mixture after the heat treatment may be washed. This washing may be performed with water or the like. By this washing, the unreacted remaining urea and the like can be removed.
[0122] (slurry) If necessary, the microfiber cellulose is dispersed in an aqueous medium to form a dispersion (slurry). The aqueous medium is particularly preferably entirely water, but an aqueous medium containing other liquids that are partially compatible with water can also be used. As the other liquid, lower alcohols having 3 or less carbon atoms can be used.
[0123] The solid content of the slurry is preferably 0.1 to 10.0% by mass, more preferably 0.5 to 5.0% by mass. If the solid content is less than 0.1% by mass, excessive energy may be required for dehydration or drying. On the other hand, if the solid content is more than 10.0% by mass, the fluidity of the slurry itself may decrease, and when a dispersant is used, the slurry may not be mixed uniformly.
[0124] (Resin powder) Microfiber cellulose may aggregate depending on storage conditions, and once aggregated, it takes time to redisperse it. In order to suppress the aggregation of microfiber cellulose and to facilitate redispersion, it is advisable to mix resin powder with the microfiber cellulose. If microfiber cellulose and resin powder are mixed to form a mixture, the microfiber cellulose remains dispersed and stable, making it less likely to aggregate. In particular, when microfiber cellulose is dried, aggregation of the microfiber cellulose is likely to occur, so by dispersing and mixing the resin powder, aggregation can be suppressed.
[0125] The resin powder is preferably a resin that is the matrix of the fiber master batch. When this resin is compounded with other general-purpose resins, such as polyolefin resins, it is possible to improve the interfacial adhesion between the polyolefin resin and the fiber, and improve the physical properties of the composite material. From this viewpoint, the resin powder is preferably an acid-modified resin powder. The acid-modified resin is a polymer having a polymer main chain and a side chain of an anhydrous organic acid group, and the polymer main chain is selected from polyolefin resins, polyester resins, AS resins, polyamide resins, etc. When it is assumed that the general-purpose resin is compounded with a polyolefin resin, it is preferable that the polymer main chain of the acid-modified resin powder is a polyolefin resin. The side chain may be an organic acid capable of forming an acid anhydride, but in consideration of the cost, an unsaturated carboxylic acid is preferable. In the acid-modified resin powder, the acid group is ionically bonded to part or all of the carbamate group of the microfiber cellulose. This ionic bond improves the reinforcing effect of the resin.
[0126] As the polyolefin component, for example, one or more types may be selected from alkene polymers such as ethylene, propylene, butadiene, isoprene, etc. However, it is preferable to use a polypropylene resin, which is a propylene polymer.
[0127] As the unsaturated carboxylic acid component, for example, one or more selected from maleic anhydrides, phthalic anhydrides, itaconic anhydrides, citraconic anhydrides, citric anhydrides, etc. can be used. However, it is preferable to use maleic anhydrides, and it is suitable to use maleic anhydride-modified polypropylene resin.
[0128] In view of the above, it is preferable that the resin powder contains, for example, a polymer whose main chain is polyolefin and whose side chain has an organic anhydride group.
[0129] The resin powder to be mixed with the microfiber cellulose may be a mixture of an acid-modified resin powder and a non-acid-modified resin powder, or the entire amount of the resin powder may be an acid-modified resin powder, or the entire amount of the resin powder may be a non-acid-modified resin powder. When the acid-modified resin powder and the non-acid-modified resin powder are mixed, the amount of the non-acid-modified resin powder mixed is preferably 0 to 200 parts by mass, more preferably 1 to 100 parts by mass, and particularly preferably 10 to 70 parts by mass, relative to 100 parts by mass of the acid-modified resin powder.
[0130] The ratio of the average particle diameter of the resin powder to the average fiber width of the microfiber cellulose to be mixed (average particle diameter of the resin powder (μm) / average fiber width of the microfiber cellulose (μm)) is preferably 50 to 80,000, more preferably 500 to 60,000. If the ratio is less than 50, the resin powder is too small relative to the microfiber cellulose, so that the fibers may come into contact with each other during the drying process, and the effect of preventing aggregation due to the presence of the resin powder may not be exhibited. If the ratio exceeds 60,000, the resin powder is too large relative to the microfiber cellulose, so that the resin powder cannot get between the fibers during the drying process, and the effect of preventing aggregation due to the presence of the resin powder may not be exhibited. In the case of the microfiber cellulose of this embodiment, the average particle diameter of the resin powder is preferably 0.1 to 1000 μm, more preferably 1 to 800 μm, and even more preferably 10 to 600 μm. If it is within this range, aggregation of the dried microfiber cellulose can be suppressed, which is preferable.
[0131] The weight average molecular weight of the maleic anhydride modified polypropylene is, for example, 1,000 to 100,000, and preferably 3,000 to 50,000.
[0132] The acid value of the maleic anhydride modified polypropylene is preferably 0.5 mgKOH / g or more and 100 mgKOH / g or less, and more preferably 1 mgKOH / g or more and 50 mgKOH / g or less.
[0133] Furthermore, the MFR (melt flow rate) of the acid-modified resin powder is preferably 2000 g / 10 min (190° C. / 2.16 kg) or less, more preferably 1500 g / 10 min or less, and particularly preferably 500 g / 10 min or less. If the MFR exceeds 2000 g / 10 min, the dispersibility of the cellulose fibers may decrease.
[0134] The acid value is measured in accordance with JIS-K2501 by titration with potassium hydroxide, and the MFR is measured in accordance with JIS-K7210 by placing a load of 2.16 kg at 190°C and measuring the weight of the sample that flows out in 10 minutes.
[0135] The resin powder used to mix with the microfiber cellulose to form the composite granules 110 has a different average particle size from the resin pellets mixed when kneading the composite granules 110, and it is preferable that the resin powder has a smaller average particle size than the resin pellets. The resin powder and the resin pellets may use the same resin compound or different resin compounds.
[0136] (Dispersant) The mixture containing the resin powder and the cellulose fiber solid of this embodiment can preferably contain a dispersant. As the dispersant, a compound having an amine group and / or a hydroxyl group in an aromatic group, or a compound having an amine group and / or a hydroxyl group in an aliphatic group is preferable.
[0137] Examples of compounds having an amine group and / or a hydroxyl group in an aromatic group include anilines, toluidines, trimethylanilines, anisidines, tyramines, histamines, tryptamines, phenols, dibutylhydroxytoluenes, bisphenol A, cresols, eugenols, gallic acids, guaiacols, picric acids, phenolphthaleins, serotonins, dopamines, adrenalines, noradrenalines, thymols, tyrosines, salicylic acids, methyl salicylates, a Examples of such alcohols include varnish alcohols, salicylic alcohols, sinapyl alcohols, diphenidols, diphenylmethanols, cinnamyl alcohols, scopolamines, tryptophols, vanillyl alcohols, 3-phenyl-1-propanols, phenethyl alcohols, phenoxyethanols, veratryl alcohols, benzyl alcohols, benzoins, mandelic acids, mandelonitriles, benzoic acids, phthalic acids, isophthalic acids, terephthalic acids, mellitic acids, and cinnamic acids.
[0138] Examples of compounds having an amine group and / or a hydroxyl group in an aliphatic group include capryl alcohols, 2-ethylhexanols, pelargonic alcohols, capric alcohols, undecyl alcohols, lauryl alcohols, tridecyl alcohols, myristyl alcohols, pentadecyl alcohols, cetanols, stearyl alcohols, elaidyl alcohols, oleyl alcohols, linoleyl alcohols, methylamines, dimethylamines, trimethylamines, ethylamines, diethylamines, and ethylenediamines. , triethanolamines, N,N-diisopropylethylamines, tetramethylethylenediamines, hexamethylenediamines, spermidines, spermines, amantadines, formic acids, acetic acids, propionic acids, butyric acids, valeric acids, caproic acids, enanthic acids, caprylic acids, pelargonic acids, capric acids, lauric acids, myristic acids, palmitic acids, margaric acids, stearic acids, oleic acids, linoleic acids, linolenic acids, arachidonic acids, eicosapentaenoic acids, docosahexaenoic acids, and sorbic acids.
[0139] The above dispersants inhibit hydrogen bonding between cellulose fibers. Therefore, when a dispersant is contained in a mixture containing powdered resin and microfibrous cellulose, the microfibrous cellulose in the mixture is dispersed while being prevented from agglomerating with each other, so that even when the composite granule 110 is formed, the microfibrous cellulose and the resin powder remain uniformly mixed.
[0140] It is possible to add a separate compatibilizing agent (drug) when kneading the composite granules 110 and the resin pellets, but rather than adding the drug at this stage, it is better to mix the microfiber cellulose and the dispersing agent (drug) in advance to form the composite granules 110, as this will allow the drug to adhere more uniformly to the microfiber cellulose and will be more effective in improving compatibility with the resin.
[0141] Also, for example, polypropylene has a melting point of 160°C, so the composite granules 110 and the resin pellets are kneaded at a temperature higher than that. If the temperature is high, the resin component melts, and if a dispersant (liquid) is added in this state, the dispersion medium evaporates in an instant and dries up. Therefore, a method can be adopted in which a master batch (composite resin with a high concentration of microfiber cellulose) is produced using resin pellets with a low melting point, and then normal resin pellets are fed to the kneader to reduce the concentration of microfiber cellulose. However, resins with low melting points generally have low strength. Therefore, this method may reduce the strength of the composite resin.
[0142] The amount of the dispersant mixed is preferably 0.1 to 1,000 parts by mass, more preferably 1 to 500 parts by mass, and particularly preferably 10 to 200 parts by mass, relative to 100 parts by mass of the microfiber cellulose. If the amount of the dispersant mixed is less than 0.1 parts by mass, the improvement in resin strength may be considered insufficient. On the other hand, if the amount mixed is more than 1,000 parts by mass, the resin strength tends to decrease due to excessive use.
[0143] In this respect, the acid-modified resin powder described above is intended to improve compatibility by ionic bonding between the acid group and the carbamate group of the microfibrous cellulose, thereby enhancing the reinforcing effect, and is considered to be compatible with resin pellets due to its large molecular weight, thereby contributing to improving strength. On the other hand, the dispersant described above is intended to intervene between the hydroxyl groups of the microfibrous cellulose to prevent aggregation, thereby improving dispersibility in the resin, and since its molecular weight is smaller than that of the acid-modified resin, it can enter narrow spaces between the microfibrous cellulose that the acid-modified resin cannot enter, thereby improving dispersibility and improving strength. From the above viewpoint, the molecular weight of the acid-modified resin described above is preferably 2 to 2,000 times, preferably 5 to 1,000 times, the molecular weight of the dispersant.
[0144] (Non-interacting powder) The composite granule 110 of this embodiment can contain a powder that does not interact with the resin powder and the microfiber cellulose. By containing the powder that does not interact with the composite granule 110, the microfiber cellulose can be made to have a form that can exhibit the reinforcing properties of the resin. In this regard, in this embodiment, before the microfiber cellulose is composited with the resin pellets, the composite granule 110 may be dried so that the moisture content is within a predetermined range. However, when drying, the cellulose may irreversibly aggregate due to hydrogen bonding, and the reinforcing effect as a fiber may not be fully exhibited. Therefore, by containing the powder that does not interact with the composite granule 110, there is an advantage that the hydrogen bonding between the cellulose is physically inhibited. The powder that does not interact with the resin may be added to a mixture having the resin and the microfiber cellulose in an aqueous dispersion system and blended to form a mixture.
[0145] Here, "not interacting" means that there is no strong bond with cellulose through covalent bonds, ionic bonds, or metallic bonds (that is, the concept of "not interacting" includes bonds through hydrogen bonds and van der Waals forces.) Preferably, the strong bond is a bond with a bond energy of more than 100 kJ / mol.
[0146] The non-interacting powder is preferably an inorganic powder that has little effect of dissociating the hydroxyl group of the cellulose fiber into hydroxide ions when it coexists in a mixture containing resin powder and microfiber cellulose. If the powder has such physical properties, the cellulose fiber and the powder that does not interact with the cellulose fiber can be easily dispersed in the resin or the like when the composite granule 110 is made and then composited with resin pellets or the like. In addition, inorganic powders are particularly advantageous in terms of operation. Specifically, the moisture content of the composite granule 110 can be adjusted, for example, by directly applying the aqueous dispersion (a mixture of microfiber cellulose, resin powder, and non-interacting powder) to a metal drum as a heat source to dry (e.g., drying with a Yankee dryer or cylinder dryer, etc.), or by heating the aqueous dispersion without directly contacting the heat source, that is, drying in the air (e.g., drying with a thermostatic dryer, etc.).
[0147] The average particle size of the non-interacting powder is preferably 1 to 10,000 μm, more preferably 10 to 5,000 μm, and particularly preferably 100 to 1,000 μm. If the average particle size exceeds 10,000 μm, there is a risk that the powder will not enter the gaps between the cellulose fibers and inhibit aggregation when the aqueous medium is removed from the slurry-like microfibrous cellulose. On the other hand, if the average particle size is less than 1 μm, there is a risk that the powder will be too fine to inhibit hydrogen bonding between the microfibrous cellulose.
[0148] In this specification, the average particle size of a non-interacting powder is a median diameter calculated from a volume-based particle size distribution measured using a particle size distribution measuring device (e.g., a laser diffraction / scattering particle size distribution measuring device manufactured by Horiba, Ltd.) for the powder as it is or in the form of an aqueous dispersion.
[0149] Examples of inorganic powders include simple substances, oxides, hydroxides, carbonates, sulfates, silicates, sulfites, and various clay minerals made of compounds of metal elements in Groups I to VIII of the periodic table, such as Fe, Na, K, Cu, Mg, Ca, Zn, Ba, Al, Ti, and silicon. Specific examples include barium sulfate, calcium sulfate, magnesium sulfate, sodium sulfate, calcium sulfite, zinc oxide, heavy calcium carbonate, light calcium carbonate, aluminum borate, alumina, iron oxide, calcium titanate, aluminum hydroxide, magnesium hydroxide, calcium hydroxide, sodium hydroxide, magnesium carbonate, calcium silicate, clay, wollastonite, glass beads, glass powder, silica gel, dry silica, colloidal silica, silica sand, silica stone, quartz powder, diatomaceous earth, white carbon, and glass fiber. A plurality of these inorganic fillers may be contained. In addition, the filler may be one contained in waste paper pulp, or may be a so-called regenerated filler obtained by regenerating inorganic matter in papermaking sludge.
[0150] However, it is preferable to use at least one inorganic powder selected from calcium carbonate, talc, white carbon, clay, calcined clay, titanium dioxide, aluminum hydroxide, and regenerated fillers, which are preferably used as fillers or pigments for papermaking, more preferably at least one selected from calcium carbonate, talc, and clay, and particularly preferably at least one of light calcium carbonate and heavy calcium carbonate. When calcium carbonate, talc, and clay are used, it is easy to form a composite with a matrix such as a resin. In addition, since they are general-purpose inorganic materials, there is an advantage that there are few restrictions on use. Furthermore, calcium carbonate is particularly preferable for the following reasons. When light calcium carbonate is used, it is easy to control the size and shape of the powder to a constant value. For this reason, there is an advantage that the size and shape can be adjusted to fit the size and shape of the cellulose fibers so that the effect of entering the gaps and suppressing the aggregation of the cellulose fibers can be easily exerted, and the effect can be easily pinpointed. In addition, the use of heavy calcium carbonate has the advantage that, since the heavy calcium carbonate is amorphous, even if fibers of various sizes are present in the slurry, the heavy calcium carbonate can penetrate into the gaps during the process of the fibers agglomerating when the aqueous medium is removed and suppress the aggregation of the cellulose fibers.
[0151] The blending amount of the non-interacting powder is preferably 1 to 9900% by mass, more preferably 5 to 1900% by mass, and particularly preferably 10 to 900% by mass, based on the microfiber cellulose. If the blending amount is less than 1% by mass, the effect of entering the gaps between the cellulose fibers and suppressing aggregation may be insufficient. On the other hand, if the blending amount exceeds 9900% by mass, the function of the cellulose fibers may not be exerted. It is preferable to blend the non-interacting powder in a ratio that does not interfere with thermal recycling.
[0152] (Manufacturing method) As described in detail below, the mixture containing microfiber cellulose and resin powder (when the dispersibility of microfiber cellulose is adjusted, the mixture further contains a dispersant, a non-interacting powder, etc.) is preferably dried to a moisture content of 10% or less before kneading with resin pellets. This dried mixture is usually in the form of pellets. This pellet-like mixture is preferably pulverized into a powder in order to process it into the desired composite granules 110. When made into a powder, the substances constituting the mixture are not biased with each other, so that the composite granules 110 are uniformly kneaded when kneaded with the resin pellets, and the coloring of the obtained microfiber cellulose composite resin is reduced. In addition, there is no need to heat excessively to remove moisture from the microfiber cellulose when kneading with the resin pellets, and the thermal efficiency is good. Furthermore, when the mixture contains a non-interacting powder or a dispersant, there is a low risk that the microfiber cellulose will not be redispersed even if the mixture is dried.
[0153] The mixture may be dehydrated as necessary prior to drying to obtain a dehydrated product, which may be carried out using one or more dehydration devices selected from the group consisting of a belt press, a screw press, a filter press, a twin roll, a twin wire former, a valveless filter, a center disk filter, a membrane treatment device, and a centrifuge.
[0154] The mixture or the dehydrated product can be dried using one or more selected from, for example, rotary kiln drying, disc drying, air flow drying, media fluidized drying, spray drying, drum drying, screw conveyor drying, paddle drying, uniaxial kneading drying, multiaxial kneading drying, vacuum drying, stirring drying, and the like.
[0155] The dried mixture (dried product) is preferably pulverized to obtain a powder product. The pulverization of the dried product can be carried out, for example, by using one or more selected from a bead mill, a kneader, a disperser, a twist mill, a cut mill, a hammer mill, and the like.
[0156] The average particle size of the powdery material is preferably 1 to 2000 μm, more preferably 10 to 1500 μm, and particularly preferably 100 to 1000 μm. If the average particle size of the powdery material exceeds 2000 μm, the composite granulated material 110 formed by compression easily crumbles when subjected to an external force. On the other hand, if the average particle size of the powdery material is less than 1 μm, the bulk density of the formed composite granulated material 110 becomes too small.
[0157] The average particle size of the powdery material can be controlled by controlling the degree of pulverization, as well as by classification using a classifying device such as a filter or a cyclone.
[0158] The moisture content of the mixture (a mixture containing resin powder and microfiber cellulose) is 10% or less, preferably 8 to 0.5%, and more preferably 5 to 1%. If the moisture content exceeds 10%, the compression treatment in the next step becomes difficult.
[0159] The moisture content was calculated using the following formula by holding a sample at 105°C for 6 hours or more in a constant temperature dryer and measuring the mass after drying at the point where no change in mass was observed. Moisture content (%) = [(mass before drying - mass after drying) ÷ mass before drying] × 100
[0160] (composite granules) The composite granulated material 110 is formed by compressing a mixture containing resin powder and microfiber cellulose. The compression process refers to a process of applying external pressure to the mixture, and can be performed, for example, using a granulation device that applies external pressure to a powdery material to compress it and granulate it into pellets. Examples of such devices include a biomass pellet manufacturing device from Earth Engineering Co., Ltd., a press pelleter from Chiyoda Machinery Co., Ltd., a wood pellet manufacturing device from Apte Japan Co., Ltd., a biomass pellet manufacturing device from Shinko Koki Co., Ltd., a pelletizer from Tosa Tech Co., Ltd., a briquette from WELHOUSE Co., Ltd., and a briquette machine from Nippon Steel Corporation. The mixture is compressed into a pellet-shaped composite granulated material 110 by being put into the device.
[0161] The granulation device is a device in which a (ring) die is provided with a large number of cylindrical through holes that are perpendicular to and substantially parallel to the ring surface, and a mixture containing resin powder and microfiber cellulose is compressed into the through holes from one end of the through holes by using a roller while applying pressure, and the mixture is compressed into a granule and discharged from the other end. To manufacture the composite granule 110 of this embodiment, for example, the through holes may have a shape in which multiple holes with different diameters are connected in the axial direction. In addition, the through holes may have the same diameter from one end to the other end. The compression rate of the composite granule can be adjusted by changing the pressure transmitted from the roller, the shape of the through holes, the speed at which the mixture passes through the through holes, and the amount of the mixture introduced into the through holes.
[0162] The composite granules 110 each have a volume of 5 to 800 mm 3 , and the bulk density is 0.10 to 0.40 g / cm 3 Preferably, the volume is 20 to 500 mm 3 , and the bulk density is 0.20 to 0.37 g / cm 3 More preferably, the volume is 50 to 200 mm 3 , and the bulk density is 0.25 to 0.35 g / cm 3 It is more preferable that the volume and bulk density of the composite granule 110 are correlated, and if either the volume or the bulk density is out of the above range, the effect of improving the productivity of the microfiber cellulose composite resin may not be achieved. For example, even if the bulk density of the composite granule 110 is within the above range, if the volume is 5 mm 3 If the volume is less than 800 mm, the composite granules 110 are too small to achieve the desired effect of compressing and granulating the mixture. 3 If the bulk density exceeds 0.40 g / cm3, when a large number of composite granules 110 are packed in a container, gaps are formed relatively, making the composite granules bulky, and it becomes difficult to put the composite granules 110 into a kneader. 3 If the temperature exceeds this range, the composite granules 110 will be hard when kneaded, will leave fragments when broken down, and will be difficult to mix with each other, or even if they do mix, it will take a lot of time and energy to mix them homogeneously.
[0163] The bulk density is a value measured in accordance with JIS K7365.
[0164] The shape of the composite granulated material 110 is not particularly limited, but examples thereof include geometric three-dimensional shapes such as an approximately cylindrical shape, an approximately rectangular prism, an approximately cube, an approximately rectangular prism, or a shape similar to these or a combination of these shapes, but are not limited to these.
[0165] In particular, it is preferable that the composite granules 110 have a generally cylindrical shape, since they easily come into contact with the screw of the kneader and are easily broken down. Also, referring to FIG. 2, in the case of a composite granule 110 having an approximately cylindrical shape having one or more of the missing portions 111 on its side, in which the minimum diameter of the approximately cylindrical diameters (R1, R2, R3, R4, ...) in each of the missing portions 111 is Rmin (R4 in FIG. 2) and the maximum diameter of the composite granule 110 is Rmax, the ratio (Rmin / Rmax) of the minimum diameter Rmin of the approximately cylindrical diameters in each of the missing portions 111 to the maximum diameter Rmax of the composite granule 110 is preferably 0.50 or more and 0.94 or less, more preferably 0.70 or more and 0.92 or less, and even more preferably 0.80 or more and 0.90 or less, is preferable because when the composite granule 110 is disintegrated by shear between adjacent screw blades of a kneading machine or between the screw and the inner wall, the missing portion 111 becomes the starting point of disintegration and disintegrates easily, and the composite granule 110 is less likely to remain at an incomplete size.
[0166] The composite granulated material 110 may be roughly cylindrical and have a defect 111 on the side. In this case, the side is concave at the location of the defect 111, so that the diameter of the side of the composite granulated material 110 at the defect 111 is smaller than the diameter at the location without the defect 111.
[0167] A specific method for measuring the diameter is not particularly limited, but may be, for example, the following method. The missing portion 111 of the composite granulated product 110 is defined as a point on the side surface of the approximately cylinder, and the length of the shortest line segment drawn from the point through the center line of the approximately cylinder to the opposite side surface is defined as the diameter. When there are multiple missing portions 111 on the side surface, the diameter of each missing portion 111 is measured, and the shortest diameter is defined as the minimum diameter Rmin. The point is defined as the position of the specific missing portion 111 that is closest to the center line of the approximately cylinder.
[0168] In addition, a point on the side surface of the composite granule 110 where the diameter is the largest is determined, and the diameter of the composite granule 110 at the point is measured and taken as the maximum diameter Rmax. The measurement can be performed using a measuring device such as a digital microscope with a scale bar.
[0169] The surface of the approximately cylinder can be represented by a pair of opposing bottom surfaces and side surfaces, and the distance from the first bottom surface to the second bottom surface of the pair of bottom surfaces is called the height of the approximately cylinder, and the imaginary line extending from the center of the first bottom surface to the center of the second bottom surface is called the center line 114. Here, as shown in Fig. 3, the approximately cylinder is divided into a first bottom surface portion B1, a central portion C, and a second bottom surface portion B2 from the first bottom surface toward the second bottom surface. Then, for the central portion C of this approximately cylinder, the ratio (Rmin / Rmax) of the minimum diameter Rmin of the diameters of the approximately cylinder in each of the cutout portions 111 can also be obtained. In this case, it is also preferable that the ratio (Rmin / Rmax) of the minimum diameter Rmin of the diameter of the approximately cylindrical in each of the defects 111 on the side surface of the central part C in the approximately cylindrical composite granule 110 having one or more defects 111 on the side surface of the central part C to the maximum diameter Rmax is preferably 0.50 or more and 0.94 or less, more preferably 0.70 or more and 0.92 or less, and even more preferably 0.80 or more and 0.90 or less. Here, the ratio of the heights of the first bottom surface part B1, the central part C, and the second bottom surface part B2 is, for example, the height of the first bottom surface part B1:the height of the central part C:the height of the second bottom surface part B2=1:8:1. This is because a pair of bottom surface portions may be chipped depending on the amount of the mixture of materials fed to the granulator and the degree of compression, and in the case of a roughly cylindrical composite granule 110 chipped in this way, it is preferable that the composite granule 110 has the above-mentioned ratio (Rmin / Rmax) at the center C, since it can be fed to the kneader without any problems. Note that the first bottom surface when a portion of the first bottom surface portion B1 is chipped refers to a virtual plane (first virtual bottom surface 112' (if a portion of the first bottom surface portion B1 is not chipped, this portion corresponds to the "first bottom surface")) in which the edge 112 on the first surface side in the direction of the center line 114 of the composite granule 110 is a part on the surface (the surface perpendicular to the center line 114). Similarly, when a portion of the second bottom surface portion B2 is missing, the second bottom surface refers to a virtual plane (second virtual bottom surface 113' (if a portion of the second bottom surface portion B2 is not missing, this portion corresponds to the "second bottom surface")) in which the edge 113 on the second surface side in the direction of the center line 114 of the composite granulated material 110 is part of the surface (a surface perpendicular to the center line 114).
[0170] The composite granules 110 may have a moisture content of 20% or less, preferably 0-20%, more preferably 1-15%, and even more preferably 2-10%. If the moisture content exceeds 20%, there is a risk of steam explosion occurring frequently during heating in a kneader. When the microfiber cellulose mixture is compressed, the moisture contained in the microfiber cellulose is squeezed out, so that the moisture content of the composite granules 110 is lower than that of the mixture containing the resin powder and the microfiber cellulose mixture.
[0171] If the moisture content exceeds 20%, when exposed to high temperatures, for example, 180°C or higher during melt kneading, the microfibrous cellulose frequently comes into contact with high-temperature water, causing a low-molecular-weight reaction of the microfibrous cellulose, generating low-molecular-weight compounds that cause coloring, and it is believed that coloring due to the low-molecular-weight compounds progresses during the kneading process. However, when carbamate is added so that the carbamate group substitution rate is 1 mmol / g or more, for example, the color-causing substances are removed in the washing process of the carbamate pulp, and further, by setting the moisture content to 10% or less, it becomes possible to evaporate the high-temperature water before it comes into contact with the microfibrous cellulose, thereby preventing coloring.
[0172] Incidentally, when the originally existing discoloration-causing substances (hemicellulose, etc.) are broken down into smaller molecules, they become water-soluble, making it possible to remove the discoloration-causing substances during the carbamate pulp washing process. If the discoloration-causing substances remain in the microfiber cellulose, they come into contact with the high-temperature water described above, causing noticeable discoloration.
[0173] In the composite granule 110 of the present embodiment, the mass ratio of the resin powder to the microfibrous cellulose is preferably 50:50 to 1:99, more preferably 45:55 to 10:90, and even more preferably 40:60 to 20:80, based on the solid content. If the mass ratio is outside this range, the resin powder and the microfibrous cellulose are difficult to granulate, and the strength of the microfibrous cellulose composite resin may not be sufficient.
[0174] The bulk density of the composite granules of the present invention is preferably 0.50 to 0.10 g / cm 3 and more preferably 0.40 to 0.20 g / cm 3 The bulk density is the upper limit of 0.50 g / cm 3 If the bulk density exceeds the lower limit of 0.10 g / cm, the fiber aggregates in the granules will increase, the load during extrusion kneading will increase, and operability may deteriorate. 3 If the temperature is lower than this, the pellets will lose a certain degree of hardness, which may cause them to lose their disintegratability during kneading, making it difficult to alleviate the aggregation of the fibers. In addition, the mixture will become powdery, which may blow out from the kneader vent together with steam, which may cause poor operability.
[0175] (Kneading process) The kneading process is a process of kneading a composite granule or kneading a composite granule with a resin pellet to obtain a microfiber cellulose composite resin. Conventionally, when cellulose fine fibers are mixed with a resin as a reinforcing material for the resin and kneaded, a process of defibrating raw pulp into cellulose fine fibers and feeding them to a kneader together with the resin has been performed as a preliminary step. However, since the defibrated and dried cellulose fine fibers are in the form of powder, they are bulky and have a so-called poor swallowing, making it difficult to feed a large amount. For this reason, in the case of a conventional powder sample, for example, when a twin-screw extruder with a diameter of 15 mm is used, the discharge speed was about 0.1 kg / h. In addition, the composite resin containing cellulose fine fibers and resin discharged from the kneader is discharged in the form of strands, for example, but it may be difficult to stabilize the supply amount, and as a result, the strands may be brittle, not discharged as stable strands, or may be colored.
[0176] On the other hand, in this embodiment, the sample supplied to the kneader is a composite granule 110 having resin powder and microfibrous cellulose, so the amount supplied to the kneader is stable, the thermal conductivity to the sample during kneading is excellent, the strands formed by kneading are stable, and there is little discoloration, which was previously observed.
[0177] In order to adjust the blending amount of microfiber cellulose contained in the finally produced microfiber cellulose composite resin, resin pellets can be added and supplied in the mixing process and kneaded together with the composite granules 110. The resin pellets to be kneaded preferably have an average particle diameter of 1 to 10 mm, more preferably 2 to 5 mm. If the average particle diameter is less than 1 mm, the resin may melt before reaching the axis and adhere to the wall surface, etc., and the adhered resin may hinder the supply of subsequent resin pellets, and may not be quantitatively kneaded. Furthermore, the thermal conductivity between the resin pellets is poor, and a lot of energy is consumed until the resin pellets are melted. If the average particle diameter exceeds 10 mm, the thermal conductivity between the resin pellets is poor, and a lot of energy is consumed until the resin pellets are melted, it is difficult to supply to the kneader, and heat conduction is biased, and it takes time to melt.
[0178] The temperature of the kneading treatment in this embodiment is equal to or higher than the glass transition point of the resin pellets, and differs depending on the type of resin pellets, but is preferably 80 to 280° C., more preferably 90 to 260° C., and particularly preferably 100 to 240° C. In the kneading treatment, in addition to melting the resin pellets, the resin powder contained in the composite granules 110 also melts.
[0179] In the present embodiment, the kneading process is carried out by supplying the composite granules 110 and the resin to a twin-screw extruder having a diameter of, for example, φ15 mm, so that the extrusion rate is preferably 1.0 to 10.0 kg / h, more preferably 1.5 to 7.0 kg / h, and even more preferably 2.0 to 5.0 kg / h.
[0180] For the kneading process, for example, one or more of a single-screw or multi-screw kneader having two or more screws, a multi-screw kneading extruder, a mixing roll, a kneader, a roll mill, a Banbury mixer, a screw press, a disperser, etc. can be selected and used. Among these, it is preferable to use a multi-screw kneader having two or more screws. Two or more multi-screw kneaders having two or more screws may be used in parallel or in series.
[0181] The resin used for the resin pellets is preferably at least one of a thermoplastic resin and a thermosetting resin.
[0182] As the thermoplastic resin, for example, one or more selected from polyolefins such as polypropylene (PP) and polyethylene (PE), polyester resins such as aliphatic polyester resins and aromatic polyester resins, polyacrylic resins such as polystyrene, methacrylate and acrylate, polyamide resins, polycarbonate resins, polyacetal resins, etc. can be used.
[0183] However, it is preferable to use at least one of polyolefin and polyester resin. As the polyolefin, it is preferable to use polypropylene. As the polyester resin, examples of the aliphatic polyester resin include polylactic acid and polycaprolactone, and examples of the aromatic polyester resin include polyethylene terephthalate, but it is preferable to use a biodegradable polyester resin (also simply called "biodegradable resin").
[0184] As the biodegradable resin, for example, one or more types may be selected from hydroxycarboxylic acid-based aliphatic polyesters, caprolactone-based aliphatic polyesters, dibasic acid polyesters, and the like and used.
[0185] As the hydroxycarboxylic acid-based aliphatic polyester, one or more selected from homopolymers of hydroxycarboxylic acids such as lactic acid, malic acid, glucose acid, 3-hydroxybutyric acid, etc., and copolymers using at least one of these hydroxycarboxylic acids, etc. However, it is preferable to use polylactic acid, copolymers of lactic acid and the above hydroxycarboxylic acids other than lactic acid, polycaprolactone, and copolymers of at least one of the above hydroxycarboxylic acids and caprolactone, and it is particularly preferable to use polylactic acid.
[0186] As the lactic acid, for example, L-lactic acid, D-lactic acid, etc. can be used, and these lactic acids may be used alone or in combination of two or more kinds.
[0187] As the caprolactone-based aliphatic polyester, for example, one or more types may be selected from homopolymers of polycaprolactone and copolymers of polycaprolactone or the like with the above-mentioned hydroxycarboxylic acids and the like.
[0188] As the dibasic acid polyester, for example, one or more types may be selected from polybutylene succinate, polyethylene succinate, polybutylene adipate, and the like and used.
[0189] The biodegradable resin may be used alone or in combination of two or more kinds.
[0190] Examples of the thermosetting resin that can be used include phenol resins, urea resins, melamine resins, furan resins, unsaturated polyesters, diallyl phthalate resins, vinyl ester resins, epoxy resins, urethane resins, silicone resins, thermosetting polyimide resins, etc. These resins can be used alone or in combination of two or more.
[0191] The resin pellets may contain an inorganic filler, preferably in a proportion that does not impede thermal recycling.
[0192] Examples of inorganic fillers include simple substances, oxides, hydroxides, carbonates, sulfates, silicates, and sulfites of metal elements in Groups I to VIII of the periodic table, such as Fe, Na, K, Cu, Mg, Ca, Zn, Ba, Al, Ti, and silicon, as well as various clay minerals composed of these compounds.
[0193] Specific examples include barium sulfate, calcium sulfate, magnesium sulfate, sodium sulfate, calcium sulfite, zinc oxide, silica, heavy calcium carbonate, light calcium carbonate, aluminum borate, alumina, iron oxide, calcium titanate, aluminum hydroxide, magnesium hydroxide, calcium hydroxide, sodium hydroxide, magnesium carbonate, calcium silicate, clay wollastonite, glass beads, glass powder, silica sand, silica stone, quartz powder, diatomaceous earth, white carbon, glass fiber, etc. A plurality of these inorganic fillers may be contained. Also, it may be one contained in waste paper pulp.
[0194] The blending ratio of the resin pellets to the microfiber cellulose is preferably 0 to 50, more preferably 0 to 20, and even more preferably 0 to 10, parts by mass of the resin pellets per part by mass of the microfiber cellulose. When the blending ratio is within the above range, the strength of the resin composition, particularly the bending strength and tensile modulus, can be significantly improved.
[0195] The content ratio of the microfiber cellulose and the resin contained in the finally obtained microfiber cellulose composite resin is usually the same as the blending ratio of the microfiber cellulose and the resin (resin powder and resin pellets).
[0196] Solubility parameters (cal / cm) of microfiber cellulose and resin 3 ) 1 / 2 The difference in SP value is the SP value of microfiber cellulose. MFC Value, resin SP POL value, the difference in SP value = SP MFC Value − SP POL The difference in SP value is preferably 0.1 to 10.0, more preferably 0.5 to 8.0, and particularly preferably 1.0 to 5.0. If the difference in SP value exceeds 10.0, the microfiber cellulose may not disperse in the resin, and the reinforcing effect may not be obtained. On the other hand, if the difference in SP value is less than 1.0, the microfiber cellulose will dissolve in the resin, will not function as a filler, and the reinforcing effect will not be obtained. In this regard, the SP of the resin (solvent)POL Value and SP of microfiber cellulose (solute) MFC The smaller the difference in the values, the greater the reinforcing effect.
[0197] The solubility parameter (cal / cm 3 ) 1 / 2 The SP value is a measure of the intermolecular force acting between a solvent and a solute, and the closer the SP values of the solvent and solute are, the greater the solubility.
[0198] The total area of the foreign matter in the microfiber cellulose composite resin is preferably 3000 mm 2 / m 2 Less than or equal to 2800~1mm, more preferably 2 / m 2 , and more preferably 2500 to 5 mm 2 / m 2 The total area of the foreign object is 10,000 mm 2 / m 2 Microfiber cellulose composite resins exceeding this limit may have scattered fragments of incompletely disintegrated composite granules, resulting in uneven strength.
[0199] (Molding process) The kneaded mixture of the composite granules 110 and the resin can be molded into a desired shape after being kneaded again as necessary. The size, thickness, shape, etc. of the molded product are not particularly limited, and can be, for example, a sheet, pellet, powder, fiber, etc.
[0200] The temperature during the molding process is equal to or higher than the glass transition point of the resin, and differs depending on the type of resin, but is, for example, 90 to 260°C, and preferably 100 to 240°C.
[0201] The kneaded material can be molded by, for example, mold molding, injection molding, extrusion molding, hollow molding, foam molding, etc. The kneaded material can also be spun into fibers and mixed with the above-mentioned plant materials to form a mat or board. The mixed fibers can be simultaneously deposited by air laying, for example.
[0202] As the apparatus for molding the kneaded product, for example, one or more types may be selected from an injection molding machine, a blow molding machine, a hollow molding machine, a blow molding machine, a compression molding machine, an extrusion molding machine, a vacuum molding machine, a pressure molding machine, etc., and may be used.
[0203] The above molding can be carried out following kneading, or the kneaded mixture can be cooled once and then chipped using a crusher or the like, and the chips can be fed into a molding machine such as an extrusion molding machine or an injection molding machine. Of course, molding is not an essential requirement of the present invention.
[0204] (Other compositions) The microfiber cellulose may contain cellulose nanofibers together with the microfiber cellulose. The cellulose nanofibers are fine fibers like the microfiber cellulose, and play a role in complementing the microfiber cellulose in improving the strength of the resin. However, if possible, it is preferable to use only microfiber cellulose as the fine fibers without including cellulose nanofibers. The average fiber width of the cellulose nanofibers (average fiber width; average diameter of a single fiber) is preferably 4 to 100 nm, more preferably 10 to 80 nm.
[0205] The microfiber cellulose may also contain pulp. Pulp plays a role in significantly improving the dewaterability of the cellulose fiber slurry. However, as with the cellulose nanofiber, it is most preferable not to include pulp, i.e., the content is 0 mass%.
[0206] The composite granulated material 110 can contain, or may contain, in addition to fine fibers and pulp, fibers derived from plant materials obtained from various plants such as kenaf, jute, Manila hemp, sisal, gampi, mitsumata, paper mulberry, banana, pineapple, coconut, corn, sugarcane, bagasse, palm, papyrus, reed, esparto, sabai grass, wheat, rice, bamboo, various coniferous trees (such as cedar and cypress), broad-leaved trees, and cotton.
[0207] For example, one or more of antistatic agents, flame retardants, antibacterial agents, colorants, radical scavengers, foaming agents, etc. may be added to the composite granules 110 within a range that does not impair the effects of the present invention. These raw materials may be added to the dispersion liquid of microfibrous cellulose, added to the mixture of resin powder and microfibrous cellulose during the granulation process, or added by other methods. However, from the viewpoint of production efficiency, it is preferable to add them to the dispersion liquid of microfibrous cellulose.
[0208] An ethylene-α-olefin copolymer elastomer or a styrene-butadiene block copolymer may be contained as a rubber component in the composite granule 110. Examples of α-olefins include butene, isobutene, pentene, hexene, methyl-pentene, octene, decene, and dodecene.
[0209] The composite granules 110 (resin reinforcing material) obtained as described above are kneaded with resin pellets to finally obtain a microfiber cellulose composite resin. This kneading can be performed, for example, by mixing the pellet-shaped resin with the reinforcing material, or by melting the resin pellets first and adding the reinforcing material to the melt. Note that acid-modified resins, dispersants, etc. can also be added at this stage.
[0210] (Example of manufacturing method) An example of a method for producing a microfiber cellulose composite resin will be described with reference to Fig. 4. First, a microfiber cellulose 1 is prepared. In the microfiber cellulose 1, all or a part of the cellulose may or may not be substituted with a carbamate group.
[0211] The microfiber cellulose 1 is subjected to a mixing step s50. In the mixing step s50, the microfiber cellulose 1 and the resin 2 are charged into a mixer 52 and mixed together to obtain a mixture. To obtain a uniform mixture, it is preferable to arrange two mixers (mixers 52 and 53) in series.
[0212] The mixture is subjected to a pulverization step s60. In the pulverization step s60, the mixture is supplied to a pulverizer 62. The mixture is pulverized in the pulverizer 62 to become powder having a diameter of about 1 mm.
[0213] This powder is subjected to a compression step s70. In the compression step s70, the powder is compressed by a pelletizer 72 and formed into composite granules 110.
[0214] The composite granules 110 are subjected to a kneading and pelletizing step s80. In the kneading and pelletizing step s80, the composite granules 110 are fed to a kneader 81 and kneaded to become a microfiber cellulose composite resin. In addition to the composite granules 110, resin pellets 82 can also be fed to the kneader 81 and kneaded. The resin pellets 82 may be fed at the beginning of the kneading process by the kneader 81, or may be fed at a stage where the kneading process has progressed to a certain degree. Here, the kneading process having progressed to a certain degree can be, for example, half the total time required from when the composite granules 110 are fed to the initial sample feed section of the kneader 81 until they are kneaded and discharged from the discharge section of the kneader 81 as a microfiber cellulose composite resin. The microfiber cellulose composite resin discharged from the kneader 81 is processed into pellets (microfiber cellulose composite resin) by a pelletizing step 84, sent to a packaging step 91, and packaged to become a final product.
[0215] In the kneading / pelletizing step s80, when the resin pellets 82 are newly supplied to the kneader 81 in addition to the composite granules 110 and kneaded, the newly supplied pellet resin 82 is preferably 0 to 10,000 parts by mass, more preferably 0 to 1000 parts by mass, per 100 parts by mass of the microfiber cellulose. By newly supplying the resin pellets 82, the blending ratio of the microfiber cellulose can be adjusted as desired.
[0216] The kneading and pelletizing step s80 may be repeated two or more times. For example, when the first kneading and pelletizing step s80 is repeated twice, in the first kneading and pelletizing step s80, the composite granules 110 are supplied to the kneader 81 and kneaded without newly supplying the resin pellets 82 to obtain a microfiber cellulose composite resin. Then, in the second kneading and pelletizing step s80, the obtained microfiber cellulose composite resin is supplied to the kneader 81 again, and newly supplied resin pellets 82 are kneaded during the kneading process to obtain a microfiber cellulose composite resin (kneaded twice).
[0217] (Definition, measurement method, etc.) (average fiber width) The method for measuring the average fiber width of fine fibers (microfiber cellulose and cellulose nanofiber) is as follows. First, 100 ml of an aqueous dispersion of fine fibers with a solid content concentration of 0.01 to 0.1% by mass is filtered through a Teflon (registered trademark) membrane filter, and the solvent is replaced once with 100 ml of ethanol and three times with 20 ml of t-butanol. Next, the sample is freeze-dried and osmium-coated to obtain a sample. This sample is observed using an electron microscope SEM image at a magnification of 3,000 to 30,000 times depending on the width of the fibers that constitute it. Specifically, two diagonal lines are drawn on the observed image, and three straight lines passing through the intersection of the diagonal lines are arbitrarily drawn. Furthermore, the widths of a total of 100 fibers that intersect with these three straight lines are visually measured. The median diameter of the measured values is then taken as the average fiber width.
[0218] (Aspect Ratio) The aspect ratio is the average fiber length divided by the average fiber width. The larger the aspect ratio, the more points at which snagging occurs, and therefore the greater the reinforcing effect. However, on the other hand, the more snagging occurs, and this is thought to reduce the ductility of the resin.
[0219] (Water retention) The water retention is a value measured in accordance with JAPAN TAPPI No. 26 (2000).
[0220] (Fiber Analysis) The fine rate, fibrillation rate, average fiber length, etc. were measured using a fiber analyzer "FS5" manufactured by Valmet.
[0221] (Crystallization degree) The crystallinity is a value measured in accordance with JIS K 0131 (1996).
[0222] (viscosity) The pulp viscosity is a value measured in accordance with TAPPI T 230.
[0223] (Freeness) The freeness is a value measured in accordance with JIS P8121-2 (2012). EXAMPLES
[0224] In the examples, composite granules and microfiber cellulose composite resin were produced using resin and pulp as raw materials, and evaluation tests were carried out. The results are shown in Table 1.
[0225] <Production of Test Example> The manufacturing procedure for the test example was as follows. Step (1) A predetermined sizing agent was added to the pulp slurry, and the pulp was made into paper in the wire part so as to have a predetermined Cobb sizing degree, and then sent to the press part and the pre-dryer part to obtain a paper base material with a predetermined basis weight. The pulp used was a mixture of bleached hardwood kraft pulp and bleached softwood kraft pulp.
[0226] Step (2) Next, the obtained paper base material was impregnated with an aqueous urea solution of a predetermined concentration in a coater part and coated, and then dried in a subsequent after-dryer part to obtain a urea-coated paper.
[0227] Step (3) The obtained urea-coated paper was reacted in a roll-to-roll reactor at a predetermined temperature for a predetermined residence time to obtain a carbamate-modified paper.
[0228] Step (4) The resulting carbamate-modified paper was then diluted with water to a solids concentration of 5% using a disintegrator and disintegrated. The disintegration liquid was dehydrated and washed twice to obtain washed carbamate-modified pulp. The carbamate-modified pulp was beaten in a refiner to obtain carbamate-modified microfibrous cellulose with a fine A ratio of 40% or more. The average fiber length of the carbamate-modified microfibrous cellulose was 0.5 mm.
[0229] Step (5) 15 g of maleic anhydride-modified polypropylene (MAPP) powder was added in terms of bone dry weight to 1000 g of a carbamate-modified microfiber cellulose aqueous dispersion adjusted to a solid content concentration of 3.0% by mass, and after stirring, the mixture was heated and dried using a contact dryer set at 140 ° C. to obtain a mixture containing MAPP powder and microfiber cellulose. The maleic anhydride-modified polypropylene powder used was one of the following: Riken Vitamin's product "MG400W" (average particle size: about 500 μm), Mitsui Chemicals' product "Admer AT2606" (average particle size: about 700 μm), and Mitsubishi Chemical's product "Modic P928" (average particle size: about 500 μm).
[0230] Step (6) The resulting mixture was compressed with a compressor (TS-55, manufactured by Tosa Tech Co., Ltd.) to obtain a composite granule containing resin powder and microfiber cellulose. Each composite granule was approximately cylindrical with a diameter of 3 to 5 mm and a height of 3 to 5 mm, with defects on the surface and / or inside, and a volume of 50 to 170 mm. 3 , Bulk density 0.2~0.5g / cm 3 The moisture content was 3 to 10%. The substitution rate of the carbamate group of the microfiber cellulose constituting the composite granule was 0.8 mmol / g. The mass ratio of the resin powder to the microfiber cellulose in the composite granule was 33.3:66.7 on a solid content basis.
[0231] Step (7) The obtained composite granules were melt-kneaded using a φ15 mm twin-screw extruder at 160°C to 180°C and 200 rpm to obtain a microfiber cellulose composite resin. The obtained microfiber cellulose composite resin was cut into a cylindrical shape with a diameter of 2 mm and a height of 2 mm using a pelleter.
[0232] Step (8) The microfiber cellulose composite resin and the prepared PP pellets were mixed, further heated and mixed, and fed into a twin-screw kneader and kneaded under conditions of 180°C and 200 rpm to obtain a microfiber cellulose composite resin (containing MAPP and PP). The obtained microfiber cellulose composite resin (containing MAPP and PP) was cut into a cylindrical shape with a diameter of 2 mm and a height of 2 mm using a pelleter. The microfiber cellulose composite resin (containing MAPP and PP) had a microfiber cellulose blending ratio of 10.0%. The microfiber cellulose composite resin (containing MAPP and PP) was injection molded at a setting of 180°C to obtain a rectangular parallelepiped test piece (length 59 mm, width 9.6 mm, thickness 3.8 mm). The prepared PP pellets were "MA3" products manufactured by Novatec.
[0233] In the above series of steps, the microfiber cellulose is modified to carbamate to produce the test examples 1 to 11, but the test examples can also be produced without the modification. In this case, the following procedure is recommended.
[0234] Step (1)' The prepared pulp is refined in a refiner to obtain unmodified microfiber cellulose with a fine A ratio of 40% or more. The average fiber length of the microfiber cellulose is 0.5 mm.
[0235] Step (2)' The obtained microfiber cellulose is subjected to the same procedures as those (5) to (8) described above to prepare a test piece.
[0236] <Evaluation Test 1> The side diameters (maximum diameter Rmax and minimum diameter Rmin) of the composite granules produced by the above procedure were measured. In addition, the ratio of the minimum diameter Rmin to the maximum diameter Rmax (Rmin / Rmax) was calculated.
[0237] Furthermore, the bulk density of the composite granules was measured.
[0238] <Evaluation Test 2> The operability of the composite granules was evaluated according to the following criteria. ◯: The composite granules maintained an approximately cylindrical shape and were easy to feed into the twin-screw extruder. ×: The composite granules could not maintain the approximately cylindrical shape and turned into powder, making it difficult to feed the composite granules into the twin-screw extruder.
[0239] <Evaluation Test 3> 1 g of the microfiber cellulose composite resin obtained in step (8) above was pressed in a press at 180°C and processed into a circular sheet with a diameter of about 9 cm, which was then subjected to a foreign matter measurement. The foreign matter measurement was performed in accordance with JIS-P8145:2011 "Paper and paperboard - Evaluation method for foreign matter" (threshold value 150), and the total area of foreign matter (mm 2 / m 2 ) was measured.
[0240] [Table 1] [Industrial Applicability]
[0241] The present invention can be used as a composite granule or a microfiber cellulose composite resin. [Explanation of symbols]
[0242] 110 Composite granules 111 Missing part
Claims
1. A composite granule formed by compressing a mixture containing a resin powder and microfiber cellulose having an average fiber length of 0.1 to 1 mm, Having defects on the surface and / or inside, A composite granule characterized by:
2. The defect has at least a surface thereof, The composite granule according to claim 1.
3. The composite granule is The cylindrical shape has a plurality of the missing portions on the side surface, The ratio (Rmin / Rmax) of the maximum diameter Rmax of the composite granule to the minimum diameter Rmin of the approximately cylindrical diameters in each of the missing portions is 0.5 or more and 0.9 or less. The composite granule according to claim 1.
4. The mixture has a microfiber cellulose having an average fiber length of 0.1 to 1 mm, and all or a part of the hydroxyl groups are substituted with carbamate groups. The composite granule according to claim 1.
5. The substitution rate of the microfiber cellulose with a carbamate group is 0.05 mmol / g or more and 2.0 mmol / g or less. The composite granule according to claim 4.
6. The resin powder is an acid-modified resin. The composite granule according to claim 1.
7. The resin powder contains a polymer having a polyolefin main chain and an organic acid anhydride group in a side chain. The composite granule according to claim 1.
8. Bulk density is 0.1 to 0.4 g / cm 3 That is, The composite granule according to claim 1.
9. The mass ratio of the resin powder to the microfiber cellulose is 50:50 to 1:99 based on the solid content. The composite granule according to claim 1.
10. Volume is 5 to 800 mm 3 That is, The composite granule according to claim 1.
11. a compression step of compressing a mixture containing a resin powder and microfiber cellulose having an average fiber length of 0.1 to 1 mm to obtain a composite granule having defects on the surface and / or inside; A kneading step of kneading the composite granules with resin pellets to obtain a microfiber cellulose composite resin, The total area of the foreign matter in the microfiber cellulose composite resin is 10,000 to 0 mm 2 / m 2 That is, A method for producing microfiber cellulose composite resin.
Citation Information
Patent Citations
Cellulose nanofiber-containing resin composition
JP2019131774A