Method of molding precast concrete, hydraulic composition to be used in the method, and precast concrete

The precast concrete forming method using an oxyalkylene-modified rosin derivative and dispersants effectively reduces surface bubble occupancy, improving aesthetics and reducing repair work, addressing the limitations of existing methods.

JP2024152022APending Publication Date: 2024-10-25TAKEMOTO OIL & FAT CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2023065919
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-13
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Existing precast concrete methods fail to adequately improve surface aesthetics, leading to increased repair work due to high surface bubble occupancy, which is exacerbated by the declining number of construction and civil engineering workers.

Method used

A precast concrete forming method involving a hydraulic composition mixed with an oxyalkylene-modified rosin derivative, along with specific dispersants, is used to reduce surface bubble occupancy and enhance aesthetics.

Benefits of technology

The method results in precast concrete with reduced surface bubble occupancy and improved aesthetics, minimizing the need for post-manufacturing repairs and enhancing work efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024152022000001
    Figure 2024152022000001
  • Figure 2024152022000002
    Figure 2024152022000002
  • Figure 2024152022000003
    Figure 2024152022000003
Patent Text Reader

Abstract

To provide a method of molding precast concrete with improved beautiful surface appearance.SOLUTION: The method of molding precast concrete comprises a hydraulic composition production step of mixing hydraulic powder, aggregate and water to produce a hydraulic composition, and a vibration step of filling a concrete form with the hydraulic composition and vibration-molding the hydraulic composition. In the hydraulic composition production step, 0.0001 to 0.01 pt.mass of an oxyalkylene modified rosin derivative is mixed with 100 pts.mass of the hydraulic powder.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for molding precast concrete, a hydraulic composition used in the method, and precast concrete. More specifically, the present invention relates to a method for molding precast concrete with improved surface aesthetics on the surface (surface) of a concrete product, a hydraulic composition used in the method, and precast concrete which is a hardened product of the hydraulic composition. [Background technology]

[0002] Conventionally, the cast-in-place method and the precast method are known as methods for constructing concrete structures. The cast-in-place method is a method in which concrete is poured directly into a formwork assembled at a predetermined location (on-site) where the concrete structure will be placed. The precast method is a method in which concrete that has already been molded into a predetermined shape in a factory or the like (precast concrete) is transported to the site and joined together to assemble the structures.

[0003] The cast-in-place method requires a long construction period on-site, as it requires the installation of formwork, pouring of concrete, and a curing period.On the other hand, the precast method can shorten the construction period because precast concrete is manufactured in a factory and the installation is relatively simple, so it has tended to be adopted in cases where construction in a short period of time is required.

[0004] Furthermore, in recent years, the precast construction method has come to be widely adopted due to the decrease in the number of construction and civil engineering workers caused by the decline in population.

[0005] There are two known precast methods: a method of producing precast concrete using a centrifugal molding device, and a casting method in which a hydraulic composition is poured into a molding formwork and then removed after the hydraulic composition has hardened (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2020-172429 A Summary of the Invention [Problem to be solved by the invention]

[0007] However, even with the method described in Patent Document 1, there is still room for improvement in the aesthetic surface of the precast concrete (hardened product). In particular, further improving the aesthetic surface of the surface of the precast concrete (hardened product) would make it possible to omit repair work on the surface of the precast concrete. As a result, the efficiency of the work can be improved, which is of great value in light of the recent decline in the number of construction and civil engineering workers mentioned above. For these reasons, there is a demand for the development of a molding method for precast concrete that improves the aesthetic surface of precast concrete (reducing the air bubble occupancy rate (surface air bubble occupancy rate) on the surface).

[0008] In view of the above-mentioned circumstances, an object of the present invention is to provide a method for forming precast concrete which improves the aesthetic appearance of the surface of the precast concrete (reducing the occupancy rate of air bubbles on the surface), a hydraulic composition to be used in this method, and precast concrete which is the hardened product of the hydraulic composition. [Means for solving the problem]

[0009] As a result of intensive research into solving the above problems, the present inventors have found that the above problems can be solved by using a specific ratio of component (A) in a method for forming precast concrete. According to the present invention, there are provided the following method for forming precast concrete, a hydraulic composition for use in the method, and precast concrete which is a hardened product thereof.

[0010] [1] A hydraulic composition production process in which a hydraulic powder, an aggregate and water are mixed to prepare a hydraulic composition; A vibration process of filling the hydraulic composition into a form and vibrating and molding it, A method for forming precast concrete, characterized in that in the hydraulic composition production step, 0.0001 to 0.01 parts by mass of component (A), which is an oxyalkylene-modified rosin derivative, is mixed with 100 parts by mass of the hydraulic powder.

[0011] [2] The method for molding precast concrete according to the above item [1], further comprising mixing at least one component (B) selected from component (B1) represented by the following general formula (2) and component (B2) represented by the following general formula (3) in the hydraulic composition production process:

[0012] [ka] (However, in the general formula (2), R 3 is an alkyl group having 4 to 22 carbon atoms or an alkenyl group having 4 to 22 carbon atoms, R 4 A is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. 2 O is an oxyalkylene group having 2 to 4 carbon atoms (however, when a plurality of oxyalkylene groups are present, one type may be used alone or two or more types may be used), and m is A 2 is the average number of moles of O added, and is a number from 1 to 150.

[0013] [ka] (However, in the general formula (3), R 5 is an alkyl group having 1 to 22 carbon atoms or an alkenyl group having 2 to 22 carbon atoms, 3 O, A 4 O is an oxyalkylene group having 2 to 4 carbon atoms (however, when a plurality of oxyalkylene groups are present, one type may be used alone or two or more types may be used), and p is A 3 is the average number of moles of O added, and is a number from 1 to 100; 4 is the average number of moles of O added, and is a number from 0 to 100 (with the proviso that p+q=2 to 150 is satisfied).

[0014] [3] The method for molding precast concrete according to [1] or [2], wherein in the hydraulic composition production process, component (C) which is at least one selected from a polycarboxylic acid-based dispersant and a naphthalene-based dispersant is further mixed.

[0015] [4] The method for forming precast concrete according to [1] or [2] above, wherein the hydraulic composition in the hydraulic composition production step has a slump of 5 to 25 cm.

[0016] [5] A hydraulic composition for use in the method for forming precast concrete according to [1] or [2] above, A hydraulic composition comprising: a hydraulic powder; a component (A) which is an oxyalkylene-modified rosin derivative in an amount of 0.0001 to 0.01 parts by mass relative to 100 parts by mass of the hydraulic powder; an aggregate; and water.

[0017] [6] A precast concrete composition comprising the hydraulic composition described in [5] above. Effect of the Invention

[0018] According to the method for molding precast concrete of the present invention, it is possible to reduce the surface air bubble occupancy rate of the precast concrete, thereby achieving the effect of improving the aesthetic appearance of the surface.

[0019] The hydraulic composition of the present invention, when used in a method for molding precast concrete, has the effect of enabling the production of precast concrete having a low surface air bubble occupancy on the skin surface (front surface) and improved surface aesthetics.

[0020] The precast concrete of the present invention is a hardened product of the hydraulic composition of the present invention, and has the effect of having a low surface air bubble occupancy rate on its surface (front surface) and improved surface aesthetics. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] Hereinafter, the embodiments of the present invention will be described. However, the present invention is not limited to the following embodiments. Therefore, it should be understood that appropriate modifications, improvements, etc. can be made to the following embodiments based on the ordinary knowledge of those skilled in the art without departing from the spirit of the present invention. In the following examples, etc., % means % by mass, and parts means parts by mass, unless otherwise specified.

[0022] (1) Precast concrete molding method: The method for forming precast concrete of the present invention includes a hydraulic composition preparation step of mixing hydraulic powder, aggregate, and water to prepare a hydraulic composition, and a vibration step of filling a formwork with the hydraulic composition and vibrating and molding it. In the hydraulic composition preparation step, 0.0001 to 0.01 parts by mass of component (A), which is an oxyalkylene-modified rosin derivative, is mixed with 100 parts by mass of the hydraulic powder.

[0023] According to this method of forming precast concrete, it is possible to reduce the surface air bubble occupancy rate of the precast concrete, and improve the aesthetic appearance of the surface. In other words, air bubble marks (cavities) appear on the surface of the hardened concrete. If the area occupied by these air bubble marks is large, the aesthetic appearance of the concrete surface is judged to be poor. On the other hand, if the area occupied by the air bubble marks is small, i.e., if the concrete surface is smooth, the aesthetic appearance of the concrete surface is judged to be good.

[0024] If the surface appearance of the precast concrete is good in this way, the work of repairing the surface of the precast concrete after its production (repair work) can be omitted. In other words, by omitting this work, the work efficiency in the production of the precast concrete can be improved.

[0025] Here, there are two methods for forming precast concrete (precast construction methods): a method for producing precast concrete using a centrifugal molding device (centrifugal molding), and a pouring molding method in which a hydraulic composition is poured into a molding form and the hydraulic composition is removed after hardening. Of these, centrifugal molding is less likely to cause air bubble marks on the surface of the precast concrete. On the other hand, pouring molding is more likely to cause air bubble marks on the surface of the precast concrete than centrifugal molding. Therefore, repair work is required, and it is important to improve the surface aesthetics of the precast concrete to the extent that repair work is not necessary, especially in a situation where the number of workers is decreasing as described above.

[0026] "Precast" refers to the manufacturing of products and components in advance in a location other than the actual site, such as a factory or production yard. "Precast concrete" refers to concrete manufactured using this precast method.

[0027] (1-1) Hydraulic composition manufacturing process: The hydraulic composition production step is a step of preparing a hydraulic composition by mixing hydraulic powder, aggregate, and water. In this step, 0.0001 to 0.01 parts by mass of component (A), which is an oxyalkylene-modified rosin derivative, is mixed with 100 parts by mass of the hydraulic powder.

[0028] (1-1a) Component (A): Component (A) is an oxyalkylene-modified rosin derivative. Here, the term "oxyalkylene-modified rosin derivative" refers to a rosin component (mainly resin acid) modified with an oxyalkylene (polyoxyalkylene).

[0029] Rosin includes diterpene acid compounds called resin acids (rosin acids). Examples of such rosins include natural rosin, modified rosin, and polymerized rosin.

[0030] Natural rosin is a mixture of resin acids present in the residue obtained after volatile substances such as essential oils are distilled off from resin oil obtained from pine plants, and is classified into gum rosin, wood rosin, and tall oil rosin (tall rosin) depending on the production method.

[0031] Gum rosin is obtained by making cuts in pine trees, filtering and refining the raw rosin that flows out, and removing the turpentine by steam distillation. Wood rosin is obtained by solvent extraction of pine stump chips. Tall oil rosin is obtained by distilling and refining crude tall oil, a by-product of the process of making pulp from pine wood using the kraft pulp method.

[0032] Modified rosin refers to natural rosin that has been modified. Examples of modified rosin include hydrogenated rosin, which is obtained by hydrogenating natural rosin under high pressure using a precious metal catalyst such as a nickel catalyst, a platinum catalyst, a palladium catalyst, or the like to eliminate or reduce the double bonds in the molecule, and disproportionated rosin, which is obtained by heating natural rosin at high temperature in the presence of a precious metal catalyst or a halogen catalyst to eliminate unstable conjugated double bonds in the molecule.

[0033] The resin acid contained in rosin is mainly abietic acid, but in addition to this abietic acid, there are also neoabietic acid, dehydroabietic acid, tetrahydroabietic acid, palustric acid, pimaric acid, isopimaric acid, sandaracopimaric acid, levopimaric acid, etc. Thus, rosin is generally a mixture of various compounds mainly containing resin acids.

[0034] Thus, rosin contains carboxylic acids such as resin acids, and the amount of carboxylic acids in rosin is quantified by measuring the acid value, which can be determined by measuring according to the Japanese Industrial Standard JIS K 0070.

[0035] As described above, the "oxyalkylene-modified rosin derivative" which is component (A) is a compound in which a component of rosin (mainly a resin acid) is modified with an oxyalkylene, and specifically, it can be said to be a compound having an acyl residue of a resin acid (e.g., abietic acid) constituting rosin and an oxyalkylene group. This compound may have a substituent at the end of the terminal oxyalkylene group.

[0036] There is no particular limitation on the method of production of "a rosin component (mainly resin acid) modified with oxyalkylene", and it may be a compound obtained by adding oxyalkylene to a rosin component, or a compound obtained by esterifying a rosin component with polyalkylene glycol (PAG). The PAG terminal formed may have a substituent.

[0037] Since rosin is used in the production of component (A), natural rosin is preferred from the viewpoint of ease of availability during production. Among natural rosins, gum rosin and tall rosin are more preferred.

[0038] If expressed using a chemical formula, "a rosin component (mainly resin acid) modified with oxyalkylene" can be expressed by general formula (1). The compound represented by general formula (1) can also be called a rosin polyoxyalkylene adduct.

[0039] In general formula (1), "acyl residue of a carboxylic acid constituting rosin" means an acyl residue of a carboxylic acid such as a resin acid constituting rosin. In other words, compounds represented by general formula (1) include, for example, a compound having an acyl residue of abietic acid, a compound having an acyl residue of palustric acid, and the like. For this reason, an oxyalkylene-modified rosin derivative (component (A)) usually contains two or more compounds represented by general formula (1), but may also contain one type of compound (for example, a compound having an acyl residue of abietic acid).

[0040] [ka] (However, in the general formula (1), R 1 is the acyl residue of the carboxylic acid that constitutes rosin, and R 2 is a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, or an alkenyl group having 2 to 20 carbon atoms, 1 O is an oxyalkylene group having 2 to 4 carbon atoms (however, when a plurality of oxyalkylene groups are present, one type may be used alone or two or more types may be used), and n is A 1 is the average number of moles of O added, and is a number from 1 to 150.

[0041] R in general formula (1) 1 is an acyl residue of a carboxylic acid constituting rosin. The carboxylic acid constituting this rosin is, for example, a resin acid, and specific examples of the resin acid include abietic acid, neoabietic acid, dehydroabietic acid, tetrahydroabietic acid, palustric acid, pimaric acid, isopimaric acid, sandaracopimaric acid, and levopimaric acid.

[0042] R in general formula (1) 2 is a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, or an alkenyl group having 2 to 20 carbon atoms. Among these, a hydrogen atom or an alkyl group having 1 to 4 carbon atoms is preferable. In such a case, the air bubble occupancy rate is lower.

[0043] A in general formula (1) 1 O is an oxyalkylene group having 2 to 4 carbon atoms (however, when a plurality of such oxyalkylene groups are present, one type may be used alone or two or more types may be used). 1 When there are two or more types of O, they may be in the form of a random adduct, a block adduct, or an alternating adduct.

[0044] In the general formula (1), A 1Of the total O, the oxyalkylene group having 2 carbon atoms is preferably 50 mol % or more, more preferably 80 mol % or more, and particularly preferably 90 mol % or more. In this way, the air bubble occupancy rate becomes lower.

[0045] In the general formula (1), n ​​is A 1 It represents the average number of moles of O added, and is a number from 1 to 150. n is preferably a number from 5 to 150, and more preferably a number from 10 to 100.

[0046] The proportion of component (A) used is 0.0001 to 0.01 parts by mass, and more preferably 0.0001 to 0.005 parts by mass, per 100 parts by mass of hydraulic powder. By using such an amount, the air bubble occupancy rate is reduced.

[0047] (1-1b) Component (B): In the hydraulic composition production process, at least one component (B) selected from component (B1) represented by the following general formula (2) and component (B2) represented by the following general formula (3) can be further mixed. By further mixing this component (B), the air bubble occupancy rate on the surface of the precast concrete is further reduced. As a result, the surface aesthetics are further improved.

[0048] [ka] (However, in the general formula (2), R 3 is an alkyl group having 4 to 22 carbon atoms or an alkenyl group having 4 to 22 carbon atoms, R 4 A is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. 2 O is an oxyalkylene group having 2 to 4 carbon atoms (however, when a plurality of oxyalkylene groups are present, one type may be used alone or two or more types may be used), and m is A 2 is the average number of moles of O added, and is a number from 1 to 150.

[0049] [ka] (However, in the general formula (3), R 5 is an alkyl group having 1 to 22 carbon atoms or an alkenyl group having 2 to 22 carbon atoms, 3 O, A 4 O is an oxyalkylene group having 2 to 4 carbon atoms (however, when a plurality of oxyalkylene groups are present, one type may be used alone or two or more types may be used), and p is A 3 is the average number of moles of O added, and is a number from 1 to 100; 4 is the average number of moles of O added, and is a number from 0 to 100 (with the proviso that p+q=2 to 150 is satisfied).

[0050] (1-1b1) Component (B1): R in general formula (2) 3 is an alkyl group having 4 to 22 carbon atoms or an alkenyl group having 4 to 22 carbon atoms.

[0051] R in general formula (2) 4 is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and among these, a hydrogen atom or a methyl group is preferred.

[0052] A in general formula (2) 2 O is an oxyalkylene group having 2 to 4 carbon atoms (however, when a plurality of such oxyalkylene groups are present, one type may be used alone or two or more types may be used). 2 When there are two or more types of O, they may be in the form of a random adduct, a block adduct, or an alternating adduct.

[0053] In the general formula (2), A 2 Of all O, oxyalkylene groups having 2 carbon atoms account for preferably 50 mol % or more, more preferably 80 mol % or more, and particularly preferably 90 mol % or more.

[0054] In the general formula (2), m is A 2 This is the average number of moles of O added, which is a number from 1 to 150, preferably a number from 2 to 100, and more preferably a number from 5 to 90.

[0055] (1-1b2) Component (B2): R in general formula (3) 5 is an alkyl group having 1 to 22 carbon atoms or an alkenyl group having 2 to 22 carbon atoms, and among these, an alkyl group having 4 to 22 carbon atoms or an alkenyl group having 4 to 22 carbon atoms is preferred. These alkyl groups and alkenyl groups may be linear or branched, and may be of one type or two or more types.

[0056] A in general formula (3) 3 O, A 4 O is an oxyalkylene group having 2 to 4 carbon atoms (however, when a plurality of such oxyalkylene groups are present, one type may be used alone or two or more types may be used). 3 O, A 4 When two or more types of O are present, they may be in the form of a random adduct, a block adduct, or an alternating adduct.

[0057] In the general formula (3), A 3 O, A 4 Of the total amount of O, oxyalkylene groups having 2 carbon atoms account for preferably 50 mol % or more, more preferably 80 mol % or more, and particularly preferably 90 mol % or more.

[0058] In the general formula (3), p is A 3 This is the average number of moles of O added, which is a number from 1 to 100, preferably a number from 1 to 80, and more preferably a number from 2 to 50.

[0059] In the general formula (3), q is A 4 This is the average number of moles of O added, which is a number from 0 to 100, preferably a number from 0 to 80, and more preferably a number from 0 to 50.

[0060] However, the sum of p and q (p+q) is from 2 to 150, preferably from 2 to 100, and more preferably from 3 to 80.

[0061] The proportion of component (B) used is preferably 0.00001 to 0.01 parts by mass per 100 parts by mass of the hydraulic powder. By using such an amount, the air bubble occupancy rate becomes low.

[0062] (1-1c) Component (C): In the hydraulic composition manufacturing process, component (C), which is at least one selected from a polycarboxylic acid-based dispersant and a naphthalene-based dispersant, can be further mixed. By further mixing this component (C), the air bubble occupancy rate on the surface of the precast concrete is further reduced. As a result, the surface aesthetics are further improved.

[0063] As the polycarboxylic acid dispersant, known ones can be used. As the polycarboxylic acid dispersant, for example, a copolymer of a monoester of polyalkylene glycol and (meth)acrylic acid and a carboxylic acid (salt) such as (meth)acrylic acid (salt), a copolymer of an unsaturated alcohol having polyalkylene glycol and a carboxylic acid (salt) such as (meth)acrylic acid (salt), a copolymer of an unsaturated alcohol having polyalkylene glycol and a dicarboxylic acid (salt) such as maleic acid (salt), etc. can be used. Here, (meth)acrylic acid (salt) means a carboxylic acid selected from acrylic acid and methacrylic acid or a salt thereof.

[0064] As the naphthalene-based dispersant, known ones can be used, and examples thereof include naphthalenesulfonic acid (salt) formaldehyde condensation products.

[0065] The polycarboxylic acid-based dispersant and the naphthalene-based dispersant may be commercially available as a high-performance water reducing agent for products and may be used as they are.

[0066] The proportion of component (C) used is preferably 0.01 to 3 parts by mass, more preferably 0.01 to 2.5 parts by mass, and particularly preferably 0.02 to 2 parts by mass, per 100 parts by mass of the hydraulic powder. By using such an amount, the air bubble occupancy rate is reduced.

[0067] (1-1d) Hydraulic powder, aggregates, and other ingredients: Hydraulic powder is a powder that is mixed into hydraulic compositions such as concrete, reacts with water added to the hydraulic composition together with the hydraulic powder, and hardens in air or water, and is also called a binder. Examples of such hydraulic powder include cement, gypsum, ground granulated blast furnace slag, fly ash, silica fume, volcanic glass, etc.

[0068] Examples of cement include various Portland cements such as ordinary Portland cement, moderate heat Portland cement, low heat Portland cement, high early strength Portland cement, and sulfate resistant Portland cement, as well as various blended cements such as blast furnace cement, fly ash cement, and silica fume cement.

[0069] In addition, the hydraulic powder may be not only cement, but also various hydraulic powders such as gypsum, ground granulated blast furnace slag, fly ash, silica fume, volcanic glass, expansive materials, etc., and various admixtures such as stone powder and limestone powder.

[0070] The aggregate may be fine aggregate, coarse aggregate, etc. One or both of these may be used as the aggregate in this step.

[0071] Examples of fine aggregate include river sand, mountain sand, land sand, sea sand, silica sand, crushed sand, various types of slag fine aggregate, recycled aggregate, and the like, and may include those containing fine particles such as clay.

[0072] Examples of coarse aggregate include river gravel, mountain gravel, land gravel, crushed stone, various types of slag coarse aggregate, lightweight aggregate, and recycled aggregate.

[0073] In this step, it is preferable to further mix the above-mentioned components (B) and (C) in addition to the hydraulic powder, aggregate, water, and component (A). Furthermore, other components may be further included as appropriate within the range in which the effects of the present invention are not impaired.

[0074] Examples of such other components include setting retarders made of sugars, oxycarboxylates, etc., various water reducing agents, AE agents made of anionic surfactants, etc., defoamers made of polyoxyalkylene compounds, etc., hardening accelerators made of alkanolamines, etc., shrinkage reducers made of polyoxyalkylene alkyl ethers, thickeners made of cellulose ether compounds, preservatives made of isothiazolinone compounds, and rust inhibitors made of nitrites, etc.

[0075] The content of the other components may be, for example, 0 to 10 parts by mass relative to 100 parts by mass of the hydraulic powder.

[0076] The hydraulic composition may have a slump of 5 to 25 cm, and preferably 15 to 25 cm. By setting the slump in this range, the aesthetic appearance of the surface can be improved. The slump is a value measured in accordance with JIS A1101:2020.

[0077] The fluidity of a hydraulic composition may be indicated by slump flow instead of slump. In the case of a hydraulic composition having a slump of more than 21 cm and high fluidity, it may be managed by slump flow. The slump flow is a value measured in accordance with JIS A1105:2020. The slump flow may be within a range in which no separation is observed, and may be, for example, 300 to 800 mm.

[0078] In the hydraulic composition in this step, the ratio of water to hydraulic powder (water / hydraulic powder ratio) may be any ratio known in the art, and may be, for example, 20 to 70 mass %.

[0079] (1-2) Vibration process: The vibration step is a step of filling a formwork with the hydraulic composition and vibrating and molding it. This step can be appropriately performed using a vibration step in a conventionally known method for molding precast concrete.

[0080] That is, a conventionally known form can be appropriately adopted. The form can be filled with the hydraulic composition by a conventionally known method. Furthermore, the vibration molding method includes an "internal vibration method" in which a vibrator is inserted inside the hydraulic composition, a "form vibration method" in which a vibrator is attached to the outside of the form and the vibrator is brought into contact with the form to give vibration, a "surface vibration method" in which a vibrator is applied to the surface of the hydraulic composition, and a "table vibration method" in which the form is placed on a table-like vibration table and the entire form is vibrated. These methods may be adopted alone, or two or more methods may be used in combination.

[0081] The conditions for vibration molding are not particularly limited, and vibration can be performed under conventionally known conditions. For example, the vibration frequency can be about 500 to 300,000 vpm, although the higher the frequency, the more effective it is, and the vibration time can be about 5 to 300 seconds.

[0082] (1-3) Other steps: The method for forming precast concrete of the present invention may include a curing step in addition to the hydraulic composition production step and the vibration step. In this curing step, a conventionally known method may be appropriately adopted, and steam curing may also be performed on the vibrated hydraulic composition.

[0083] (2) Hydraulic composition: The hydraulic composition of the present invention is a hydraulic composition used in the method for forming precast concrete of the present invention, and contains hydraulic powder, 0.0001 to 0.01 parts by mass of the above-mentioned component (A) relative to 100 parts by mass of the hydraulic powder, aggregate, and water.

[0084] By using such a hydraulic composition in a method for forming precast concrete, it is possible to obtain precast concrete having a low surface air bubble occupancy on the skin surface (surface) and improved surface appearance.

[0085] As the component (A), the same component (A) as that explained in the above-mentioned method for molding precast concrete of the present invention can be used.

[0086] Hydraulic powder is a powder that is mixed into hydraulic compositions such as concrete, reacts with water added to the hydraulic composition together with the hydraulic powder, and hardens in air or water, and is also called a binder. Examples of such hydraulic powder include cement, gypsum, ground granulated blast furnace slag, fly ash, silica fume, volcanic glass, etc.

[0087] Examples of cement include various Portland cements such as ordinary Portland cement, moderate heat Portland cement, low heat Portland cement, high early strength Portland cement, and sulfate resistant Portland cement, as well as various blended cements such as blast furnace cement, fly ash cement, and silica fume cement.

[0088] The hydraulic powder may be used in combination with various hydraulic powders such as gypsum, finely divided blast furnace slag, fly ash, silica fume, volcanic glass, and expansive materials, as well as various admixtures such as stone powder and fine limestone powder.

[0089] The aggregate includes fine aggregate, coarse aggregate, etc.

[0090] Examples of fine aggregate include river sand, mountain sand, land sand, sea sand, silica sand, crushed sand, various types of slag fine aggregate, recycled aggregate, and the like, and may include those containing fine particles such as clay.

[0091] Examples of coarse aggregate include river gravel, mountain gravel, land gravel, crushed stone, various types of slag coarse aggregate, lightweight aggregate, and recycled aggregate.

[0092] In addition to the hydraulic powder, aggregate, water, and component (A), the hydraulic composition preferably further contains the above-mentioned components (B) and (C). Furthermore, the hydraulic composition may further contain other components as appropriate within the range in which the effects of the present invention are not impaired.

[0093] Examples of such other components include setting retarders made of sugars, oxycarboxylates, etc., various water reducing agents, AE agents made of anionic surfactants, etc., defoamers made of oxyalkylene compounds, etc., hardening accelerators made of alkanolamines, etc., shrinkage reducers made of polyoxyalkylene alkyl ethers, thickeners made of cellulose ether compounds, preservatives made of isothiazolinone compounds, and rust inhibitors made of nitrites, etc.

[0094] The content of the other components may be, for example, 0 to 10 parts by mass relative to 100 parts by mass of the hydraulic powder.

[0095] The hydraulic composition may have a slump of 5 to 25 cm, and preferably 15 to 25 cm. By setting the slump in this range, the aesthetic appearance of the surface can be improved. The slump is a value measured in accordance with JIS A1101:2020.

[0096] The fluidity of a hydraulic composition may be indicated by slump flow instead of slump. In other words, in the case of a hydraulic composition having a high fluidity with a slump exceeding 21 cm, it may be managed by the slump flow. The slump flow is a value measured in accordance with JIS A1105:2020. The slump flow of the hydraulic composition of the present invention may be within a range in which no separation is observed, for example, 300 to 800 mm, and the upper limit may be equivalent to a slump of 25 cm.

[0097] In the hydraulic composition in this step, the ratio of water to hydraulic powder (water / hydraulic powder ratio) may be any ratio known in the art, and may be, for example, 20 to 70 mass %.

[0098] (3) Precast concrete: The precast concrete of the present invention is a hardened product of the hydraulic composition of the present invention. This precast concrete has a low surface air bubble occupancy rate on its surface (surface), and has improved surface aesthetics. This precast concrete is produced by using the hydraulic composition of the present invention and employing the method for forming precast concrete of the present invention. EXAMPLES

[0099] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples.

[0100] First, the component (A) (compounds (A-1) to (A-8)), which is an oxyalkylene-modified rosin derivative, was synthesized according to the following Synthesis Examples 1 to 8. The obtained compounds (A-1) to (A-8) are shown in Table 1.

[0101] (Synthesis Example 1) Synthesis of compound (A-1): In a stainless steel pressure vessel, 328.1 g of X-grade "gum rosin" (acid value: 171 mgKOH / g) from the People's Republic of China (hereinafter simply referred to as "China") and 2.0 g of potassium hydroxide were charged and heated to 120°C. After that, dehydration under reduced pressure was performed for 1 hour while maintaining this temperature and stirring. After that, the pressure was returned to normal pressure with nitrogen, and 660 g of ethylene oxide and 58 g of propylene oxide were simultaneously injected under 0.4 MPa at a temperature range of 150 to 160°C (set temperature 155°C), and then aging was performed for 1 hour at that temperature. After that, it was cooled and 20 g of an adsorbent (trade name: Kyoward 600 manufactured by Kyowa Chemical Industry Co., Ltd.) was added. Furthermore, dehydration under reduced pressure was performed at 120°C, and pressure filtration was performed to obtain compound (A-1).

[0102] (Synthesis Example 2) Synthesis of compound (A-2): In a stainless steel pressure vessel, 328.1 g of grade X of "gum rosin" produced in China (acid value: 171 mgKOH / g) and 1.6 g of potassium hydroxide were charged and heated to 120°C. After that, dehydration under reduced pressure was performed for 1 hour while maintaining this temperature and stirring. After that, the pressure was returned to normal with nitrogen, and 1320 g of ethylene oxide was pressurized under 0.4 MPa at a temperature range of 150 to 160°C (set temperature 155°C), and then aging was performed for 1 hour at that temperature. After that, it was cooled, and after cooling, the pH was adjusted to 6 using 85% phosphoric acid. After that, dehydration under reduced pressure was performed at 120°C, and pressure filtration was performed to obtain compound (A-2).

[0103] (Synthesis Example 3) Synthesis of compound (A-3): Compound (A-3) was obtained in the same manner as compound (A-1), except that propylene oxide was changed to 1,2-butylene oxide and the amounts of ethylene oxide and 1,2-butylene oxide charged were changed.

[0104] (Synthesis Example 4) Synthesis of compound (A-4): Compound (A-4) was obtained in the same manner as compound (A-2), except that gum rosin was changed to tall rosin grade X (Harima Chemicals, acid value 169 mg / g) and the amount added was changed.

[0105] (Synthesis Example 5) Synthesis of compound (A-5): In a 1L glass reaction vessel, 692.0g of α-methoxy-ω-hydroxy-poly(n=15)oxyethylene, 328.0g of X-grade Chinese "gum rosin" (acid value: 171mgKOH / g), and 9.6g of methanesulfonic acid were charged and substituted with nitrogen. After that, dehydration was carried out under reduced pressure at 150°C and 0.5kPa, and an esterification reaction was carried out. The reaction was terminated when the esterification rate reached 99% or more. After that, the mixture was purified to obtain compound (A-5).

[0106] (Synthesis Example 6) Synthesis of compound (A-6): Compound (A-6) was obtained in the same manner as compound (A-5), except that α-methoxy-ω-hydroxy-poly(n=15)oxyethylene was changed to 1-butanol with 4 moles of propylene oxide and 30 moles of ethylene oxide block-added thereto, and the amounts of the charged materials were changed.

[0107] (Synthesis Examples 7 and 8) Synthesis of Compounds (A-7) and (A-8): Compounds (A-7) and (A-8) were obtained in the same manner as compound (A-1), except that the amounts of ethylene oxide and propylene oxide charged were changed.

[0108] [Table 1]

[0109] In Table 1, “R 1 "Gum rosin acyl residue" in the "Compound" column indicates an acyl residue of a carboxylic acid constituting gum rosin, and "tall rosin acyl residue" indicates an acyl residue of a carboxylic acid constituting tall rosin. The carboxylic acids constituting gum rosin and tall rosin include abietic acid, palustric acid, isopimaric acid, dehydroabietic acid, and neoabietic acid. Note that gum rosin and tall rosin differ in the composition ratio of the carboxylic acids constituting these. Compounds (A-1) to (A-8) are of multiple types, such as those having an acyl residue of abietic acid and those having an acyl residue of palustric acid.

[0110] Next, component (B1) (compounds (B1-1) to (B1-3), compounds (B1-5) to (B1-10)) and component (B2) (compounds (B2-1) to (B2-7)) which are component (B) were synthesized in the following Synthesis Examples 9 to 25. The obtained compounds (B1-1) to (B1-10) are shown in Table 2, and the obtained compounds (B2-1) to (B2-7) are shown in Table 3. As for compound (B1-4), Softanol 90 (manufactured by Nippon Shokubai Co., Ltd.) was used as it was.

[0111] (Synthesis Example 9) Synthesis of compound (B1-1): In a stainless steel pressure vessel, 332.0 g of Softanol 30 (manufactured by Nippon Shokubai Co., Ltd.) and 2.0 g of potassium hydroxide were charged and heated to 120°C. After that, while maintaining this temperature, dehydration under reduced pressure was performed for 1 hour while stirring. After that, the pressure was returned to normal with nitrogen, and 1188 g of ethylene oxide was pressurized under 0.4 MPa at a temperature range of 110 to 130°C (set temperature 120°C), and aging was performed for 1 hour at that temperature. After that, it was cooled, and an adsorbent (manufactured by Kyowa Chemical Industry Co., Ltd., product name: Kyoward 600) was added, and dehydration under reduced pressure was further performed at 120°C. After that, pressure filtration was performed to obtain compound (B1-1).

[0112] (Synthesis Example 10) Synthesis of compound (B1-2): Compound (B1-2) was obtained in the same manner as compound (B1-1), except that the type of raw material alcohol and the amount of ethylene oxide, etc. were changed. In the synthesis of compound (B1-2), ISOFOL16 (manufactured by Sasol) was used as the raw material alcohol.

[0113] (Synthesis Example 11) Synthesis of compound (B1-3): In a stainless steel pressure vessel, 134.3 g of oleyl alcohol (Angecol 85AN, Nippon Rika Co., Ltd.) and 1.9 g of potassium hydroxide were charged and heated to 120°C. While maintaining this temperature, dehydration under reduced pressure was performed for 1 hour while stirring. After that, the pressure was returned to normal with nitrogen, and 1760 g of ethylene oxide was injected under 0.4 MPa at a temperature range of 110 to 130°C (set temperature 120°C), and aging was performed for 1 hour at that temperature. After that, it was cooled and 28.1 g of potassium hydroxide was added. After dehydration under reduced pressure at 120°C, 26 g of methyl chloride was further injected at 120°C to perform methylation. After that, desalting and filtration were performed to obtain compound (B1-3).

[0114] (Synthesis Example 12) Synthesis of compound (B1-5): Compound (B1-5) was obtained in the same manner as compound (B1-1), except that the type of raw material alcohol and the amount of ethylene oxide, etc. were changed. In the synthesis of compound (B1-5), EXXAL9S (manufactured by ExxonMobil Corp.) was used as the raw material alcohol.

[0115] (Synthesis Example 13) Synthesis of compound (B1-6): In a stainless steel pressure vessel, 193.0 g of SAFOL23 (manufactured by Sasol) and 1.0 g of potassium hydroxide were charged and heated to 120°C. Dehydration under reduced pressure was performed for 1 hour while maintaining this temperature and stirring. Then, the pressure was returned to normal with nitrogen, and 660 g of ethylene oxide was injected under 0.4 MPa at a temperature range of 110 to 130°C (set temperature 120°C), and aging was performed for 1 hour at that temperature. Then, 116 g of propylene oxide was injected under 0.4 MPa at a temperature range of 150 to 160°C (set temperature 155°C), and aging was performed for 1 hour at that temperature. Then, the mixture was cooled, and an adsorbent (trade name: Kyoward 600 manufactured by Kyowa Chemical Industry Co., Ltd.) was added, and dehydration under reduced pressure was performed at 120°C. Then, pressure filtration was performed to obtain compound (B1-6).

[0116] (Synthesis Example 14) Synthesis of compound (B1-7): In a stainless steel pressure vessel, 200.4 g of tridecyl alcohol (KH Neochem) and 2.5 g of potassium hydroxide were charged and heated to 120°C. Dehydration was carried out under reduced pressure for 1 hour while maintaining this temperature and stirring. Thereafter, the pressure was returned to normal with nitrogen, and 1496 g of ethylene oxide and 696 g of propylene oxide were simultaneously charged under 0.4 MPa at a temperature range of 140 to 160°C (set temperature 150°C), and aging was carried out at that temperature for 1 hour. Thereafter, the mixture was cooled, and an adsorbent (Kyowa Chemical Industry Co., Ltd., product name: Kyoward 600) was added, followed by dehydration under reduced pressure at 120°C. Thereafter, pressure filtration was carried out to obtain compound (B1-7).

[0117] (Synthesis Examples 15 and 16) Synthesis of Compounds (B1-8) and (B1-9): Compounds (B1-8) and (B1-9) were obtained in the same manner as compound (B1-6), except that the type of raw material alcohol and the amount of ethylene oxide and propylene oxide were changed. In the synthesis of compound (B1-8), 1-decanol (reagent, manufactured by Tokyo Chemical Industry Co., Ltd.) was used as the raw material alcohol, and in the synthesis of compound (B1-9), Angecol 85AN (manufactured by New Japan Chemical Co., Ltd.) was used as the raw material alcohol.

[0118] (Synthesis Example 17) Synthesis of compound (B1-10): Compound (B1-10) was obtained in the same manner as compound (B1-6), except that the raw material alcohol was changed to 2-ethylhexanol and the amounts of ethylene oxide, propylene oxide, and the like charged were changed.

[0119] (Synthesis Example 18) Synthesis of compound (B2-1): In a stainless steel pressure vessel, 185.4 g of Farmin CS (manufactured by Kao Corporation) was charged, and a nitrogen atmosphere was created by depressurizing and replacing with nitrogen. Then, 88 g of ethylene oxide was added under pressure at 0.4 MPa in a temperature range of 150 to 160 ° C (set temperature 155 ° C), and aging was performed for 1 hour at that temperature. Then, 1.9 g of potassium hydroxide was charged, and dehydration was performed under reduced pressure at 120 ° C for 1 hour while stirring. Then, the pressure was returned to normal pressure with nitrogen, and 1672 g of ethylene oxide was added under pressure at 0.4 MPa in a temperature range of 120 to 140 ° C (set temperature 130 ° C), and aging was performed for 1 hour at that temperature. Then, the mixture was cooled, and an adsorbent (manufactured by Kyowa Chemical Industry Co., Ltd., product name: Kyoward 600) was added, and dehydration was performed under reduced pressure at 120 ° C. Then, pressure filtration was performed to obtain compound (B2-1).

[0120] (Synthesis Example 19) Synthesis of compound (B2-2): In a stainless steel pressure vessel, 539.0 g of Fentamine AHT (manufactured by Solvay) and 1.4 g of potassium hydroxide were charged, and dehydration was carried out under reduced pressure at 120°C for 1 hour while stirring. After that, the pressure was returned to normal with nitrogen, and 880 g of ethylene oxide was added under pressure of 0.4 MPa in the temperature range of 120 to 140°C (set temperature 130°C), and aging was carried out at that temperature for 1 hour. After that, it was cooled, and an adsorbent (manufactured by Kyowa Chemical Industry Co., Ltd., product name: Kyoward 600) was added, and dehydration was carried out under reduced pressure at 120°C. After that, pressure filtration was carried out to obtain compound (B2-2).

[0121] (Synthesis Example 20) Synthesis of compound (B2-3): Compound (B2-3) was obtained in the same manner as compound (B2-1), except that the raw material amine was changed to the reagent stearylamine and the charged amounts of ethylene oxide and the like were changed.

[0122] (Synthesis Example 21) Synthesis of compound (B2-4): In a stainless steel pressure vessel, 269.5 g of Fentamine AHT (manufactured by Solvay) was charged, and a nitrogen atmosphere was created by depressurizing and replacing with nitrogen. Then, 88 g of ethylene oxide was charged under 0.4 MPa at a temperature range of 150 to 160 ° C (set temperature 155 ° C), and aging was performed for 1 hour at that temperature. Then, 1.7 g of potassium hydroxide was charged, and dehydration under reduced pressure was performed at 120 ° C for 1 hour while stirring. Then, the pressure was returned to normal pressure with nitrogen, and 968 g of ethylene oxide and 348 g of propylene oxide were simultaneously charged under 0.4 MPa at a temperature range of 140 to 150 ° C (set temperature 145 ° C), and aging was performed for 1 hour at that temperature. Then, 116 g of propylene oxide was charged under the same conditions, and aging was performed for 1 hour at that temperature. Then, it was cooled, an adsorbent (manufactured by Kyowa Chemical Industry Co., Ltd., product name: Kyoward 600) was added, and dehydration under reduced pressure was performed at 120 ° C. Then, pressure filtration was performed to obtain compound (B2-4).

[0123] (Synthesis Example 22) Synthesis of compound (B2-5): Compound (B2-5) was obtained in the same manner as compound (B2-4), except that the raw material amine was changed to a reagent hexylamine and the amounts of ethylene oxide, propylene oxide, and the like charged were changed.

[0124] (Synthesis Example 23) Synthesis of compound (B2-6): In a stainless steel pressure vessel, 267.5 g of oleylamine (Tokyo Chemical Industry Co., Ltd., reagent) was charged, and a nitrogen atmosphere was created by depressurizing and replacing with nitrogen. Then, 88 g of ethylene oxide was charged under 0.4 MPa at a temperature range of 150 to 160 ° C (set temperature 155 ° C), and aging was performed for 1 hour at that temperature. Then, 1.7 g of potassium hydroxide was charged, and dehydration was performed under reduced pressure at 120 ° C for 1 hour while stirring. Then, the pressure was returned to normal pressure with nitrogen, and 440 g of ethylene oxide was charged under 0.4 MPa at a temperature range of 110 to 130 ° C (set temperature 120 ° C), and aging was performed for 1 hour at that temperature. Then, 348 g of propylene oxide was charged under 0.4 MPa at a temperature range of 150 to 160 ° C (set temperature 155 ° C), and aging was performed for 1 hour at that temperature. Then, the mixture was cooled, an adsorbent (manufactured by Kyowa Chemical Industry Co., Ltd., product name: Kyoward 600) was added, and dehydration was performed under reduced pressure at 120° C. Then, pressure filtration was performed to obtain compound (B2-6).

[0125] (Synthesis Example 24) Synthesis of compound (B2-7): Compound (B2-7) was obtained in the same manner as compound (B2-6), except that the raw material amine was Fentamine AHT (manufactured by Solvay) and the amounts of ethylene oxide, propylene oxide, and the like charged were changed.

[0126] [Table 2]

[0127] In Table 2, "EO%" stands for A 2 The percentage of EO (ethylene oxide) in O is also shown. 2 The addition form of O is A 2O indicates whether it is a random addition or a block addition.

[0128] [Table 3]

[0129] In Table 3, "EO%" stands for A 3 O and A 4 The percentage of EO (ethylene oxide) in the total of O is also shown. 3 O / A 4 The addition form of O is A 3 O and A 4 O indicates whether it is a random addition or a block addition.

[0130] (Examples 1 to 34, Comparative Examples 1 to 9) Next, the methods of forming the precast concrete in Examples 1 to 34 and Comparative Examples 1 to 9 will be described below.

[0131] (Hydraulic composition manufacturing process) First, hydraulic compositions were prepared based on the following formulations 1 to 4 (hydraulic composition manufacturing process).

[0132] In addition, the hydraulic composition obtained in Mixture 1 has a target slump of 18±1 cm and a target air content of 4.5±0.5%. In Mixture 2, the target slump is 15±1.5 cm and the target air content is 2.0% or less. In Mixture 4, the target slump is 8±1 cm and the target air content is 4.5±0.5%. The slump was measured in accordance with JIS A1101:2020. The air content was measured in accordance with JIS A1128:2019. In Mixture 3, the target slump flow (20°C) was 650±25 mm, which was measured in accordance with JIS A 1150:2020. In Mixture 3, the target air content was 2.0% or less. The temperature of the hydraulic composition was also measured when the slump and air content were measured. The temperature of the hydraulic composition was measured in accordance with JIS A1156:2014.

[0133] (Formulation 1) In a thermostatic room at 20°C and 80% humidity, the components shown in Table 4 and the components (A) to (C) shown in Table 8 were added to a 55L pan-type forced mixing mixer in the prescribed ratios and mixed for 90 seconds. At this time, 0.7% by mass of "PCE1", an aqueous solution of a commercially available polycarboxylic acid dispersant (Chupol NV-80) with a solid content of 20%, 0.0025% by mass of an AE agent (AE-200), and 0.0005% by mass of an antifoaming agent (AFK-2) were used as part of the mixing water.

[0134] In this way, 30 L of hydraulic composition (concrete) was prepared. The temperature of the prepared concrete was 20° C. The prepared concrete was filled into a steel form within 15 minutes after mixing, and subjected to a vibration step described later.

[0135] [Table 4]

[0136] In Table 4, "cement" refers to hydraulic powder, and is ordinary Portland cement (an equal mixture of products manufactured by Taiheiyo Cement Corporation, UBE Mitsubishi Cement Corporation, and Sumitomo Osaka Cement Co., Ltd.) with a density of 3.16 g / cm 3 The "water" is the water supply of Gamagori City. The "fine aggregate" is the Oi River water system land sand (density 2.58 g / cm 3 The "coarse aggregate" is crushed stone from Okazaki (density 2.68g / cm 3 ).

[0137] (Formulation 2) In a thermostatic room at 20°C and 80% humidity, the components shown in Table 5 and the components (A) to (C) shown in Table 9 were added together in the prescribed ratios to a 55L pan-type forced mixing mixer and mixed for 45 seconds. At this time, "NSF", an aqueous solution containing 40% solids of a commercially available naphthalene-based dispersant (Polfine 510AN), was used, and 1.0% by mass of cement was used as part of the mixing water.

[0138] In this way, 30 L of hydraulic composition (concrete) was prepared. The temperature of the prepared concrete was 20° C. The prepared concrete was filled into a steel form within 15 minutes after mixing, and subjected to a vibration step described later.

[0139] [Table 5]

[0140] In Table 5, "cement" refers to hydraulic powder, and is ordinary Portland cement (an equal mixture of products manufactured by Taiheiyo Cement Corporation, UBE Mitsubishi Cement Corporation, and Sumitomo Osaka Cement Co., Ltd.) with a density of 3.16 g / cm 3 The "water" is the water supply of Gamagori City. The "fine aggregate" is the Oi River water system land sand (density 2.58 g / cm 3 The "coarse aggregate" is crushed stone from Okazaki (density 2.66 g / cm 3 ).

[0141] (Formulation 3) 1.5m 3 The components shown in Table 6 and the components (A) to (C) shown in Table 9 were added in the specified ratios to a forced twin-shaft mixer with a capacity of 1000 ml, and mixed for 60 seconds. At this time, "PCE2", an aqueous solution containing 20% ​​polycarboxylic acid dispersant (Chupol NV-80E) in solid content, was used as 1.2% by mass relative to the cement, and an antifoaming agent (AFK-2) was used as 0.001% by mass relative to the cement as part of the mixing water.

[0142] In this way, 0.5m 3 The outdoor air temperature was 23° C., and the temperature of the prepared concrete was 21° C. The prepared concrete was filled into a steel form within 15 minutes after mixing, and subjected to the vibration step described below.

[0143] [Table 6]

[0144] In Table 6, "cement" refers to hydraulic powder, and is ordinary Portland cement (manufactured by Taiheiyo Cement Corporation) with a density of 3.16 g / cm 3 "Limestone powder" is a type of admixture, and has a density of 2.72 g / cm3 for Tankal 200 mesh (manufactured by Inasasu Co., Ltd.). 3 The "fine aggregate" is crushed sand with a density of 2.57 g / cm 3 "Coarse aggregate" is crushed stone 2005 density 2.66g / cm 3 It is.

[0145] (Formulation 4) In a thermostatic room at 20°C and 80% humidity, the components shown in Table 7 and the components (A) to (C) shown in Table 9 were added to a 55L pan-type forced mixing mixer in the prescribed ratios and mixed for 90 seconds. At this time, 0.60% by mass of "PCE3", an aqueous solution of a commercially available polycarboxylic acid dispersant (Chupol NV-G5) with a solid content of 20%, and 0.0015% by mass of an air-entraining agent (AE-300) were used as part of the mixing water.

[0146] In this way, 30 L of hydraulic composition (concrete) was prepared. The temperature of the prepared concrete was 20° C. The prepared concrete was filled into a steel form within 15 minutes after mixing, and subjected to a vibration step described later.

[0147] [Table 7]

[0148] In Table 7, "cement" refers to hydraulic powder, and is ordinary Portland cement (an equal mixture of products manufactured by Taiheiyo Cement Corporation, UBE Mitsubishi Cement Corporation, and Sumitomo Osaka Cement Co., Ltd.) with a density of 3.16 g / cm 3 The "water" is the water supply of Gamagori City. The "fine aggregate" is the Oi River water system land sand (density 2.58 g / cm 3 The "coarse aggregate" is crushed stone from Okazaki (density 2.66 g / cm 3 ).

[0149] (vibration process) Next, a vibration step was carried out using the prepared hydraulic composition.

[0150] Specifically, using a mug, concrete (hydraulic composition) was poured into a cylindrical steel specimen mold with a diameter of 10 cm and a height of 20 cm, the inner surface of which was coated with a concrete release agent (Polyzone S: manufactured by Takemoto Yushi Co., Ltd.) in one operation so that the mold was filled. Then, using a table vibrator (table vibrator "CF-1033" manufactured by Maruto Seisakusho), vibration molding was performed on the mold filled with the hydraulic composition. The vibration conditions were a vibration frequency of 2800 vpm, a total amplitude of 0.8 mm, and a vibration time of 30 seconds. Then, the mold was left standing in a thermostatic room at 20°C and a humidity of 80%. Then, after 24 hours, the mold was removed to obtain a cylindrical concrete hardened product, which was a test product of precast concrete.

[0151] In the case of Blend 3, the vibration step was carried out as follows.

[0152] First, concrete (hydraulic composition) was poured into a steel formwork of a U-shaped gutter 300B (width 500 mm × depth 2000 mm × height 400 mm) with a release agent applied thereto, using a concrete bucket. Then, this steel formwork was vibrated for 30 seconds with a formwork vibrator (150 W, vibration frequency 60 Hz), and steam curing was performed as it was. The conditions for this steam curing were as follows. Specifically, after pouring, the concrete was left to stand at outside temperature for 2 hours, and then the temperature was raised to 50°C at a rate of 15°C per hour. Then, the concrete was held at 50°C for 30 minutes. Then, the temperature was slowly returned to room temperature. Next, the formwork was removed 15 hours after pouring, and a hardened concrete product, which was a test product of precast concrete, was obtained.

[0153] <Surface bubble occupancy rate (%)> (Formulation 1, 2, 4) For the cylindrical hardened concrete products in Mixes 1, 2, and 4, the surface air void occupancy rate (%) was calculated as follows.

[0154] Specifically, the side (curved surface) of the cylindrical cured concrete was scanned with a handy scanner (Sanwa Direct's "400-SCN032", resolution 900 dpi), and the scanned image was binarized using the bitmap image editing and processing software "GIMP 2.10.20". The threshold value for binarization was set so that the number of air bubble marks in the original scanned image was equal to the number of air bubble marks in the processed image. Note that when binarizing, the boundaries of the formwork remaining in the cured concrete and color unevenness such as blackening due to poor curing or oil stains may be recognized as "black". Therefore, these parts were deleted and made "white". In this way, the air bubble marks recognized as black were separated from the parts other than the air bubble marks recognized as white.

[0155] Thereafter, the air bubble occupancy, i.e., the ratio (%) of the area corresponding to the air bubble marks to the entire side surface of the hardened concrete product in the scanned image, was calculated. Then, the ratio of the air bubble occupancy of each hardened concrete product to the air bubble occupancy of each hardened concrete product (reference product) of Comparative Examples 1, 5, and 8, which were the reference test products, was calculated (formula: air bubble occupancy of each hardened concrete product / air bubble occupancy of reference product×100(%)). The surface aesthetics (i.e., the degree of occurrence of air bubble marks) were evaluated based on the calculated numerical values ​​(%). The evaluation criteria are shown below. Note that the column for the evaluation of the surface aesthetics of the reference product is marked as "reference".

[0156] (Formulation 3) In addition, for the hardened concrete of Mix 3, the surface air bubble occupancy rate (%) was calculated as follows.

[0157] Specifically, a photograph of the side (curved surface) of the hardened concrete was taken at 16M size (4608 x 3456 pixels) and divided into 7 parts on one side, for a total of 14 images. The obtained images were binarized using the bitmap image editing and processing software "GIMP 2.10.20". The threshold value for the binarization process was set so that the number of air bubble marks in the original image was equal to the number of air bubble marks in the processed image. Note that when binarizing, color unevenness such as the boundaries of the formwork remaining in the hardened concrete, and blackening due to poor hardening or oil stains may be recognized as "black". These parts were deleted and made "white". Then, the image was divided into air bubble marks recognized as black and parts other than air bubble marks recognized as white.

[0158] Thereafter, the air bubble occupancy, i.e., the ratio (%) of the area corresponding to the air bubble marks to the entire side surface of the hardened concrete product in the scanned image, was calculated. Then, the ratio of the air bubble occupancy of each hardened concrete product to the air bubble occupancy of the hardened concrete product of Comparative Example 7 (reference product), which was the reference test product, was calculated (formula: air bubble occupancy of each hardened concrete product / air bubble occupancy of reference product×100(%)). The surface aesthetics (i.e., the degree of occurrence of air bubble marks) were evaluated based on the calculated numerical values ​​(%). The evaluation criteria are shown below. Note that the column for evaluation of surface aesthetics of the reference product (Comparative Example 7) is marked with "reference".

[0159] (Evaluation Criteria) S: When the ratio of air voids in each concrete hardened material to the air voids in the standard product is less than 30% A: When the ratio of air voids in each hardened concrete product to the air voids in the standard product is 30% or more and less than 50%. B: When the ratio of air voids in each hardened concrete product to the air voids in the standard product is 50% or more and less than 70%. C: When the ratio of air voids in each concrete hardened material to the air voids in the standard product is 70% or more and less than 90%. D: When the ratio of air voids in each hardened concrete to the air voids in the standard product is 90% or more

[0160] [Table 8]

[0161] [Table 9]

[0162] In Table 8, "PCE1" is an aqueous solution containing a commercially available polycarboxylic acid dispersant (Chupol NV-80) at 20% solids. In Table 9, "PCE2" is an aqueous solution containing a commercially available polycarboxylic acid dispersant (Chupol NV-80E) at 20% solids. "PCE3" is an aqueous solution containing a commercially available polycarboxylic acid dispersant (Chupol NV-G5) at 20% solids. "NSF" is an aqueous solution containing a commercially available naphthalene dispersant (Polfine 510AN) at 40% solids. Under the conditions of Mix 3, the hydraulic composition had high fluidity, so the slump flow was measured and the slump was also measured.

[0163] (result) As shown in Tables 8 and 9, it was confirmed that the precast concrete molding method of this embodiment can reduce the surface air bubble occupancy rate, i.e., improve the surface appearance. [Industrial Applicability]

[0164] The method for forming precast concrete of the present invention can be adopted as a method for forming precast concrete. The hydraulic composition of the present invention can be used to form precast concrete. The precast concrete of the present invention can be used as a concrete product.

Claims

1. A hydraulic composition production process in which a hydraulic powder, an aggregate, and water are mixed to prepare a hydraulic composition; A vibration process of filling the hydraulic composition into a form and vibrating and molding it, The method for forming precast concrete is characterized in that in the hydraulic composition production step, 0.0001 to 0.01 parts by mass of component (A), which is an oxyalkylene-modified rosin derivative, is mixed with 100 parts by mass of the hydraulic powder.

2. 2. The method for molding precast concrete according to claim 1, wherein in the hydraulic composition production step, at least one component (B) selected from component (B1) represented by the following general formula (2) and component (B2) represented by the following general formula (3) is further mixed: 【Chemistry 1】 (However, in the general formula (2), R 3 is an alkyl group having 4 to 22 carbon atoms or an alkenyl group having 4 to 22 carbon atoms, R 4 is a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. 2 O is an oxyalkylene group having 2 to 4 carbon atoms (however, when a plurality of oxyalkylene groups are present, one type may be used alone or two or more types may be used), and m is A 2 is the average number of moles of O added, which is a number from 1 to 150. 【Chemistry 2】 (However, in the general formula (3), R 5 is an alkyl group having 1 to 22 carbon atoms or an alkenyl group having 2 to 22 carbon atoms; A 3 O.A. 4 O is an oxyalkylene group having 2 to 4 carbon atoms (however, when a plurality of oxyalkylene groups are present, one type may be used alone or two or more types may be used), and p is A 3 is the average number of moles of O added, and is a number from 1 to 100; 4 is the average number of moles of O added, and is a number from 0 to 100 (with the proviso that p+q=2 to 150 is satisfied).

3. 3. The method for forming precast concrete according to claim 1 or 2, wherein in the hydraulic composition production step, a component (C) which is at least one selected from a polycarboxylic acid-based dispersant and a naphthalene-based dispersant is further mixed.

4. 3. The method for forming precast concrete according to claim 1, wherein the hydraulic composition in the hydraulic composition production step has a slump of 5 to 25 cm.

5. A hydraulic composition used in the method for forming precast concrete according to claim 1 or 2, A hydraulic composition comprising: a hydraulic powder; a component (A) which is an oxyalkylene-modified rosin derivative in an amount of 0.0001 to 0.01 parts by mass relative to 100 parts by mass of the hydraulic powder; an aggregate; and water.

6. A precast concrete composition comprising the hydraulic composition according to claim 5 as a hardened product.

Citation Information

Patent Citations

  • Novel concrete cracking-resistant modifier

    CN104591580A

  • Method of decreasing bubble on surface of concrete secondary product

    JP1981129108A

  • Air-entraining composition for cement composition

    JP1997511977A

  • Method for producing hardened body of hydraulic composition

    JP2018095537A

  • Precast molding method

    JP2020172429A